Composition for protective film for electroconductive layer
The protective film composition, featuring a crosslinked isobutene-isoprene copolymer and hydrotalcite, addresses the instability of conductive substrates in humid environments by forming a stable, flexible, and moisture-resistant barrier that maintains conductivity and prevents conductor migration.
Patent Information
- Application Number
- PCT/JP2024/012699
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conductive substrates with metal nanowires, metal mesh, and conductive polymers face corrosion and increased surface resistance in high-temperature, high-humidity environments, leading to instability in conductivity and migration of conductors, with existing protective layers failing to provide adequate long-term protection due to high water vapor permeability and lack of flexibility.
A protective film composition incorporating a crosslinked polymer with an isobutene-isoprene copolymer chain, combined with a liquid polyolefin resin and/or liquid rubber, and a hygroscopic inorganic filler like hydrotalcite, which forms a moisture-barrier film that suppresses surface resistivity changes and conductor migration while offering adhesion strength and bending resistance.
The composition effectively maintains stable conductivity and prevents conductor migration in high-temperature, high-humidity conditions, ensuring long-term reliability and flexibility of the conductive substrate.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Protective film composition for conductive layer
[0001] The present invention relates to a composition for protecting (sealing) a conductive layer that constitutes a conductive substrate.
[0002] Conductive substrates using metal nanowires, metal meshes, metal nanoparticles, and conductive polymers as conductors are being developed, and are expected to be used in display electrode materials, touch panel electrode materials, electromagnetic wave shielding materials, and the like. However, these conductors have the problem of corrosion due to moisture in high-temperature, high-humidity environments, resulting in increased surface resistance. Sealing with an encapsulating sheet is required to obtain substrates that exhibit stable conductivity even in high-temperature, high-humidity environments. For example, Patent Document 1 describes a method in which a protective layer containing a chelating agent is used on a silver nanowire-containing conductive layer. Patent Document 2 also describes an acrylic polymer resin composition as an adhesive layer for adhering a substrate on which metal mesh wiring and silver nanowires are formed.
[0003] However, in Patent Document 1, an acrylic resin composition is selected for forming the protective layer, and UV irradiation is required to ensure its functionality. Furthermore, the resin has a high water vapor permeability, so it cannot fully function as a protective layer in long-term high-temperature, high-humidity tests. Furthermore, Patent Document 2 achieves adhesion while suppressing metal migration into the adhesive layer, but does not mention flexibility.
[0004] Patent No. 7030277 JP 2021-195449 A
[0005] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a composition capable of forming a protective (sealing) film that can protect (seal) a conductive layer constituting a conductive substrate, while simultaneously achieving transparency, adhesion strength, and flex resistance, and suppressing changes in the surface resistivity of the conductive substrate and migration of conductors.
[0006] As a result of intensive research to solve the above-mentioned problems, the present inventors have found that by using a composition for protecting (sealing) a conductive layer constituting a conductive substrate with the following configuration, it is possible to form a protective (sealing) film that can suppress changes in the surface resistivity of the conductive substrate and migration of conductors while simultaneously achieving transparency, adhesion strength, and flex resistance, and have thus completed the present invention.
[0007] That is, the present invention has the following features. [1] A composition for a protective film of a conductive layer of a conductive substrate, comprising (A) a crosslinked polymer having an isobutene-isoprene copolymer chain, the conductive layer being composed of a conductive material containing at least one selected from the group consisting of metal nanowires, metal meshes, metal nanoparticles, and conductive polymers. [2] The composition according to [1], wherein (A) the crosslinked polymer having an isobutene-isoprene copolymer chain is at least one selected from the group consisting of a reaction product of an isobutene-isoprene copolymer having an epoxy group with an olefin-based polymer having a carboxy group and / or an acid anhydride group, and a reaction product of an isobutene-isoprene copolymer having a carboxy group and / or an acid anhydride group with an olefin-based polymer having an epoxy group. [3] The composition according to [1] or [2], wherein the content of component (A) is 10 to 75% by mass, based on 100% by mass of the nonvolatile content of the composition. [4] The resin composition according to any one of [1] to [3], further comprising (B) a liquid polyolefin-based resin and / or a liquid rubber. [5] The composition according to [4], wherein the content of component (B) is 5 to 50% by mass, based on 100% by mass of the non-volatile content of the composition. [6] The composition according to any one of [1] to [5], further comprising (C) a hygroscopic inorganic filler. [7] The composition according to [6], wherein the hygroscopic inorganic filler (C) is one or more selected from uncalcined hydrotalcite and semi-calcined hydrotalcite. [8] The composition according to [6] or [7], wherein the content of component (C) is 1 to 60% by mass, based on 100% by mass of the non-volatile content of the composition. [9] The composition according to any one of [1] to [8], wherein the metal constituting the metal nanowires, metal mesh, and / or metal nanoparticles is one or more selected from silver, copper, gold, nickel, platinum, palladium, iron, cobalt, and tin.
[10] The composition according to any one of [1] to [9], wherein the conductive polymer is at least one selected from poly(3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, graphene, polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.
[0008] According to the present invention, it is possible to provide a composition that can form a protective (sealing) film that can protect (seal) a conductive layer that constitutes a conductive substrate, while simultaneously achieving transparency, adhesion strength, and flex resistance, and suppressing changes in the surface resistivity of the conductive substrate and migration of conductors.
[0009] The present invention will be described below with reference to preferred embodiments. [Composition for Protective Film of Conductive Layer of Conductive Substrate] The composition of the present invention is for use in a protective film of a conductive layer of a conductive substrate, and comprises (A) a crosslinked polymer having an isobutene-isoprene copolymer chain, and the conductive layer is composed of a conductive material containing one or more selected from metal nanowires, metal meshes, metal nanoparticles, and conductive polymers.
[0010] <Component (A): Crosslinked Polymer Having Isobutene-Isoprene Copolymer Chains> The component (A) is a crosslinked polymer having an isobutene-isoprene copolymer (i.e., butyl rubber) chain. Only one type of component (A) may be used, or two or more types may be used in combination. The use of component (A) suppresses an increase in the surface resistivity of the conductive substrate (exhibiting low moisture permeability and preventing the intrusion of oxygen and ions, which cause an increase in surface resistivity), and also makes it possible to form a protective (sealing) film with excellent flex resistance.
[0011] Component (A) can be formed by reacting an isobutene-isoprene copolymer (i.e., a butyl rubber having a first reactive functional group) having a reactive functional group (hereinafter sometimes referred to as a "first reactive functional group") with an olefin polymer having a reactive functional group (hereinafter sometimes referred to as a "second reactive functional group") that can react with the first reactive functional group. Herein, "olefin polymer" refers to a polymer in which structural units derived from olefins (hereinafter sometimes abbreviated as "olefin units") are the main structural units (i.e., the amount of olefin units is the largest among all structural units). Note that, hereinafter, "structural units derived from butene," which are olefin units, may be abbreviated as "butene units," etc.
[0012] The olefin is preferably a monoolefin having one olefinic carbon-carbon double bond and / or a diolefin having two olefinic carbon-carbon double bonds. Examples of monoolefins include α-olefins such as ethylene, propylene, 1-butene, isobutene (isobutylene), 1-pentene, 1-hexene, 1-heptene, and 1-octene. Examples of diolefins include 1,3-butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethylbutadiene.
[0013] The olefin-based polymer may be a homopolymer or a copolymer. The copolymer may be a random copolymer or a block copolymer. The olefin-based polymer may also be a copolymer of an olefin and a monomer other than an olefin. Examples of the olefin-based copolymer include an ethylene-non-conjugated diene copolymer, an ethylene-propylene copolymer, an ethylene-propylene-non-conjugated diene copolymer, an ethylene-butene copolymer, a propylene-butene copolymer, a propylene-butene-non-conjugated diene copolymer, a styrene-isobutene copolymer, a styrene-isobutene-styrene copolymer, and an isobutylene-isoprene copolymer (i.e., butyl rubber).
[0014] The olefin polymer having a second reactive functional group is preferably a butene polymer having a second reactive functional group. Here, "butene polymer" means a polymer in which butene units are the main structural units (i.e., the amount of butene units is the largest among all structural units). Examples of butene include 1-butene and isobutene. Examples of butene polymers include polybutene and isobutene-isoprene copolymer. Polybutene may be a homopolymer (e.g., 1-butene homopolymer, isobutene homopolymer) or a copolymer (e.g., a copolymer of 1-butene and isobutene).
[0015] To form the component (A), the isobutene-isoprene copolymer having the first reactive functional group and the olefin polymer having the second reactive functional group may each be used alone or in combination of two or more.
[0016] Examples of combinations of the first reactive functional group and the second reactive functional group include a combination of an epoxy group and a carboxy group and / or an acid anhydride group (i.e., a carbonyloxycarbonyl group (—CO—O—CO—)), a combination of a carboxy group and / or an acid anhydride group and an epoxy group, a combination of an epoxy group and an amino group, a combination of an amino group and an epoxy group, a combination of a hydroxy group and an isocyanate group (i.e., an isocyanato group), a combination of an isocyanate group and a hydroxy group, and a combination of functional groups having double bonds (e.g., a vinyl group or a (meth)acryloyl group). Among these, from the viewpoint of moisture blocking properties, a combination of an epoxy group and a carboxy group and / or an acid anhydride group, and a combination of a carboxy group and / or an acid anhydride group and an epoxy group are preferred, and a combination of an epoxy group and an acid anhydride group and a combination of an acid anhydride group and an epoxy group are more preferred. In the above combinations, the former reactive functional group represents the first reactive functional group, and the latter reactive functional group represents the second reactive functional group.
[0017] In one embodiment of the present invention, component (A) is preferably at least one selected from the group consisting of a reaction product of an isobutene-isoprene copolymer having an epoxy group with an olefin polymer having a carboxy group and / or an acid anhydride group, and a reaction product of an isobutene-isoprene copolymer having a carboxy group and / or an acid anhydride group with an olefin polymer having an epoxy group. In this embodiment, the olefin polymer is preferably a butene polymer, more preferably polybutene or an isobutene-isoprene copolymer. In this embodiment, the carboxy group and / or the acid anhydride group is preferably an acid anhydride group.
[0018] In one embodiment of the present invention, component (A) is preferably a reaction product of an isobutene-isoprene copolymer having an epoxy group and a polybutene having a carboxy group and / or an acid anhydride group. In this embodiment, the carboxy group and / or the acid anhydride group is preferably an acid anhydride group.
[0019] In one embodiment of the present invention, component (A) is preferably a reaction product of an isobutene-isoprene copolymer having an epoxy group and an isobutene-isoprene copolymer having a carboxy group and / or an acid anhydride group. In this embodiment, the carboxy group and / or the acid anhydride group is preferably an acid anhydride group.
[0020] The amount of the isobutene-isoprene copolymer having a reactive functional group (e.g., an epoxy group, a carboxy group, and / or an acid anhydride group) used is preferably 15 to 100 mass%, more preferably 20 to 100 mass%, and even more preferably 30 to 100 mass%, based on the total amount of polymers used to form component (A) (e.g., the total amount of the isobutene-isoprene copolymer having a first reactive functional group and the olefin polymer having a second reactive functional group used). When an isobutene-isoprene copolymer having a first reactive functional group and an isobutene-isoprene copolymer having a second reactive functional group are used to form component (A), the term "amount of the isobutene-isoprene copolymer having a reactive functional group used" refers to the "total amount of the isobutene-isoprene copolymer having a first reactive functional group and the isobutene-isoprene copolymer having a second reactive functional group used."
[0021] The number average molecular weight of the isobutene-isoprene copolymer having reactive functional groups (e.g., epoxy groups, carboxy groups, and / or acid anhydride groups) used to form component (A) is preferably 5,000 to 500,000, more preferably 10,000 to 400,000, and even more preferably 20,000 to 300,000. The number average molecular weight in the present invention is measured by gel permeation chromatography (GPC) (polystyrene equivalent). Specifically, the number average molecular weight measured by GPC is measured using a Shimadzu Corporation "LC-9A / RID-6A" measuring device, a Showa Denko Corporation "Shodex K-800P / K-804L / K-804L" column, toluene or the like as the mobile phase, at a column temperature of 40°C, and can be calculated using a calibration curve of standard polystyrene.
[0022] The number average molecular weight of the olefin polymer (excluding isobutene-isoprene copolymer) having a second reactive functional group (for example, an epoxy group, a carboxy group, and / or an acid anhydride group) used to form component (A) is preferably 500 to 500,000, more preferably 1,000 to 300,000, and even more preferably 1,500 to 200,000.
[0023] From the viewpoint of flex resistance, the amount of isoprene units in the isobutene-isoprene copolymer having reactive functional groups (e.g., epoxy groups, carboxy groups, and / or acid anhydride groups) for forming component (A) is preferably 0.1 to 20 mass%, more preferably 0.3 to 10 mass%, and even more preferably 0.5 to 15 mass%, based on the total of isobutene units and isoprene units. The amount of isoprene units is based on the isobutene units and isoprene units excluding modified portions (e.g., portions derived from maleic anhydride for introducing acid anhydride groups).
[0024] The epoxy group concentration in the epoxy group-containing olefin polymer (e.g., epoxy group-containing isobutene-isoprene copolymer, epoxy group-containing polybutene) used to form component (A) is preferably 0.01 to 10 mmol / g, more preferably 0.05 to 5 mmol / g. The epoxy group concentration is determined from the epoxy equivalent obtained in accordance with JIS K 7236-1995.
[0025] The carboxy group concentration in the olefin polymer having a carboxy group (e.g., an isobutene-isoprene copolymer having a carboxy group, or a polybutene having a carboxy group) used to form component (A) is preferably 0.01 to 10 mmol / g, and more preferably 0.05 to 5 mmol / g. The carboxy group concentration is determined from the acid value, which is defined as the number of milligrams of potassium hydroxide required to neutralize the acid present in 1 g of resin, in accordance with JIS K 2501.
[0026] The concentration of acid anhydride groups in the olefin polymer having acid anhydride groups (e.g., an isobutene-isoprene copolymer having acid anhydride groups, or a polybutene having acid anhydride groups) used to form component (A) is preferably 0.01 to 10 mmol / g, more preferably 0.05 to 5 mmol / g. The concentration of acid anhydride groups is determined from the acid value, which is defined as the number of milligrams of potassium hydroxide required to neutralize the acid present in 1 g of resin, in accordance with JIS K 2501.
[0027] The sum of the concentration of carboxy groups and the concentration of acid anhydride groups in the olefin polymer having carboxy groups and acid anhydride groups (for example, an isobutene-isoprene copolymer having carboxy groups and acid anhydride groups, or a polybutene having carboxy groups and acid anhydride groups) used to form component (A) is preferably 0.01 to 10 mmol / g, and more preferably 0.05 to 5 mmol / g.
[0028] The amounts of the isobutene-isoprene copolymer having epoxy groups and the olefin polymer having carboxy groups (for example, an isobutene-isoprene copolymer having carboxy groups, or a polybutene having carboxy groups) used are not particularly limited as long as a crosslinked polymer, component (A), can be formed. However, the ratio of the amount (mol) of epoxy groups to the amount (mol) of carboxy groups (i.e., amount (mol) of epoxy groups: amount (mol) of carboxy groups) is preferably 100:10 to 100:500, more preferably 100:25 to 100:475, and even more preferably 100:40 to 100:450.
[0029] The amounts of the isobutene-isoprene copolymer having epoxy groups and the olefin polymer having acid anhydride groups (for example, an isobutene-isoprene copolymer having acid anhydride groups, or a polybutene having acid anhydride groups) used are not particularly limited as long as a crosslinked polymer, component (A), can be formed. However, the ratio of the amount (mol) of epoxy groups to the amount (mol) of acid anhydride groups (i.e., amount (mol) of epoxy groups: amount (mol) of acid anhydride groups) is preferably 100:10 to 100:500, more preferably 100:25 to 100:475, and even more preferably 100:40 to 100:450.
[0030] The amounts of the isobutene-isoprene copolymer having epoxy groups and the olefin polymer having carboxy groups and acid anhydride groups (for example, an isobutene-isoprene copolymer having carboxy groups and acid anhydride groups, or a polybutene having carboxy groups and acid anhydride groups) used are not particularly limited as long as a crosslinked polymer, component (A), can be formed. However, the ratio of the "amount (mol) of epoxy groups" to the "total amount (mol) of carboxy groups and amount (mol) of acid anhydride groups" (i.e., the ratio of the amount (mol) of epoxy groups:(amount (mol) of carboxy groups + amount (mol) of acid anhydride groups)) is preferably 100:10 to 100:500, more preferably 100:25 to 100:475, and even more preferably 100:40 to 100:450.
[0031] An olefin polymer having an epoxy group (for example, an isobutene-isoprene copolymer having an epoxy group, or a polybutene having an epoxy group) can be obtained by graft-modifying an olefin polymer with an unsaturated compound having an epoxy group (for example, glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, or allyl glycidyl ether) under radical reaction conditions.
[0032] Commercially available olefin polymers having epoxy groups may be used. Examples of commercially available isobutene-isoprene copolymers having epoxy groups include "ER866" (glycidyl methacrylate-modified butyl rubber, epoxy group concentration: 1.63 mmol / g, number average molecular weight: 113,000) manufactured by Seiko PMC Corporation and "ER850" (glycidyl methacrylate-modified butyl rubber, epoxy group concentration: 0.65 mmol / g, number average molecular weight: 99,200) manufactured by Seiko PMC Corporation. Commercially available examples of olefin polymers having epoxy groups (excluding isobutene-isoprene copolymers) include "T-YP341" manufactured by Seiko PMC Corporation (glycidyl methacrylate-modified propylene-butene random copolymer, epoxy group concentration: 0.64 mmol / g, number average molecular weight: 155,000), "T-YP276" manufactured by Seiko PMC Corporation (glycidyl methacrylate-modified propylene-butene random copolymer, epoxy group concentration: 0.64 mmol / g, number average molecular weight: 57,000), and "T-YP313" manufactured by Seiko PMC Corporation (glycidyl methacrylate-modified propylene-butene random copolymer, epoxy group concentration: 0.64 mmol / g, number average molecular weight: 155,000).
[0033] An olefin polymer having a carboxy group and / or an acid anhydride group (for example, an isobutene-isoprene copolymer having a carboxy group and / or an acid anhydride group, or a polybutene having a carboxy group and / or an acid anhydride group) can be obtained by graft-modifying an olefin polymer with an unsaturated compound having a carboxy group and / or an acid anhydride group (for example, maleic anhydride) under radical reaction conditions.
[0034] The olefin polymer having a carboxy group and / or an acid anhydride group may be a commercially available product. Examples of commercially available isobutene-isoprene copolymers having a carboxy group and / or an acid anhydride group include "ER661" manufactured by Seiko PMC Corporation (maleic anhydride-modified butyl rubber, acid anhydride group concentration: 0.77 mmol / g, number average molecular weight: 40,000) and "ER641" manufactured by Seiko PMC Corporation (maleic anhydride-modified butyl rubber, acid anhydride group concentration: 0.46 mmol / g, number average molecular weight: 57,000). Commercially available olefin polymers having carboxyl groups and / or acid anhydride groups (excluding isobutene-isoprene copolymers) include, for example, "HV-300M" manufactured by Toho Chemical Industry Co., Ltd. (maleic anhydride-modified polybutene, acid anhydride group concentration: 1.16 mmol / g, number average molecular weight: 2,100), "T-YP279" manufactured by Seiko PMC Co., Ltd. (maleic anhydride-modified propylene-butene random copolymer, acid anhydride group concentration: 0.46 mmol / g, number average molecular weight: 35,000), and "T-YP279" manufactured by Seiko PMC Co., Ltd. (maleic anhydride-modified propylene-butene random copolymer, acid anhydride group concentration: 0.46 mmol / g, number average molecular weight: 35,000). Examples include "T-YP312" manufactured by Hikari PMC Co., Ltd. (maleic anhydride-modified propylene-butene random copolymer, acid anhydride group concentration: 0.46 mmol / g, number average molecular weight: 60,900), and "Lucant A-5260" manufactured by Mitsui Chemicals, Inc. (maleic anhydride-modified ethylene-α-olefin random copolymer, acid anhydride group concentration: 0.44 mmol / g, number average molecular weight: 5,400), and "Lucant A-5320" (maleic anhydride-modified ethylene-α-olefin random copolymer).
[0035] From the viewpoint of flex resistance, the content of component (A) in the composition layer is preferably 10% by mass or more, more preferably 12.5% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the nonvolatile content of the composition, and from the viewpoint of moisture blocking property, it is preferably 75% by mass or less, more preferably 70% by mass or less, and even more preferably 65% by mass or less. In one embodiment of the present invention, the content of component (A) is preferably 10 to 75% by mass, and more preferably 12.5 to 70% by mass or less, relative to 100% by mass of the nonvolatile content of the composition.
[0036] <Component (B): Liquid Polyolefin Resin and / or Liquid Rubber> The composition of the present invention may contain a liquid polyolefin resin and / or liquid rubber. In the present invention, "liquid" means that the viscosity at 25°C is 5,000 Pa s or less. In addition, in the present invention, "viscosity at 25°C" means the viscosity calculated by multiplying the kinematic viscosity at 25°C measured with a dynamic viscoelasticity measuring device by the density. Examples of dynamic viscoelasticity measuring devices include a rheometer (product name: DISCOVERY HR-2) manufactured by TA Instruments.
[0037] With regard to component (B) of the present invention, "liquid polyolefin resin" refers to an olefin polymer having a viscosity of 5,000 Pa s or less at 25° C. and which is incapable of forming a rubbery elastomer by crosslinking, and "liquid rubber" refers to a polymer having a viscosity of 5,000 Pa s or less at 25° C. and which is capable of forming a rubbery elastomer by crosslinking. For example, liquid polyisoprene is classified as a liquid rubber because it can form a rubbery elastomer by crosslinking.
[0038] The viscosity of the liquid polyolefin resin and the liquid rubber at 40° C. is preferably 5 to 5,000 Pa·s, more preferably 10 to 4,000 Pa·s, and even more preferably 20 to 3,000 Pa·s.
[0039] The component (B) may be used alone or in combination of two or more. By using the component (B), good adhesion (particularly adhesion at high temperatures) can be achieved, and the viscoelasticity of the composition can be controlled. The composition of the present invention may also contain a hygroscopic inorganic filler, as described below. However, using a large amount of the hygroscopic inorganic filler reduces the adhesiveness of the protective (sealing) film. In this regard, by using the component (B), good adhesion can be achieved even when a large amount of the hygroscopic inorganic filler is used.
[0040] The number average molecular weight of the liquid polyolefin resin is preferably 500 to 15,000, more preferably 750 to 12,500, and even more preferably 1,000 to 10,000. The number average molecular weight of the liquid rubber is 500 to 15,000, more preferably 750 to 12,500, and even more preferably 1,000 to 10,000.
[0041] The liquid polyolefin resin and / or liquid rubber is preferably at least one selected from liquid polybutene, hydrogenated polybutadiene, butadiene-based liquid rubber, and liquid polyisoprene, more preferably at least one selected from liquid polybutene and hydrogenated polybutadiene, and even more preferably liquid polybutene. The liquid polybutene may be a homopolymer (e.g., 1-butene homopolymer, isobutene homopolymer) or a copolymer (e.g., a copolymer of 1-butene and isobutene).
[0042] Commercially available liquid polyolefin resins and / or liquid rubbers can be used. Commercially available liquid polyolefin resins include, for example, ENEOS "HV-300" (liquid polybutene), ENEOS "HV-1900" (liquid polybutene), ENEOS "HV-50" (liquid polybutene), ENEOS "HV-35" (liquid polybutene), Kothari "950MW" (liquid polybutene), Kothari "2400MW", INEOS "H-1900" (liquid polybutene), INEOS "H-6000" (liquid polybutene), and the like. Examples of suitable polybutenes include "H-18000" (liquid polybutene) manufactured by INEOS Corporation, "200N" (liquid polybutene) manufactured by NOF Corporation, "BI-2000" (hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd., "BI-3000" (hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd., "GI-3000" (hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd., "Lucant LX100" (liquid olefin polymer) manufactured by Mitsui Chemicals, Inc., and "Lucant LX400" (liquid olefin polymer) manufactured by Mitsui Chemicals, Inc.
[0043] Commercially available liquid rubbers include, for example, "Poly bd R-45HT" (butadiene-based liquid rubber) manufactured by Idemitsu Showa Shell Co., Ltd., "Poly bd R-15HT" (butadiene-based liquid rubber) manufactured by Idemitsu Showa Shell Co., Ltd., and "Poly bd R-15HT" (butadiene-based liquid rubber) manufactured by Idemitsu Showa Shell Co., Ltd. ip" (liquid polyisoprene), Nippon Soda's "B-1000" (liquid polybutadiene), Nippon Soda's "B-3000" (liquid polybutadiene), Nippon Soda's "G-3000" (liquid polybutadiene), Kuraray's "LIR-30" (liquid polyisoprene), Kuraray's "LIR-390" (liquid polyisoprene), Kuraray's "LIR-290" (liquid polyisoprene), Kuraray's "LBR-302" (liquid polybutadiene), Kuraray's "LBR-305" (liquid polybutadiene), Kuraray's "LBR-361" (liquid polybutadiene), Kuraray's "L-SBR-820" (liquid styrene-butadiene random copolymer), CRAY VALLEY's "Ricon" 154" (liquid butadiene), and CRAY VALLEY's "Ricon 184" (liquid styrene-butadiene random copolymer).
[0044] The content of component (B) in the composition (when both a liquid polyolefin resin and a liquid rubber are used, the total content of these) is preferably 5% by mass or more, more preferably 7.5% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the nonvolatile content of the composition, from the viewpoint of adhesiveness, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of adhesiveness at high temperatures. In one embodiment of the present invention, the content of component (B) is preferably 5 to 50% by mass, more preferably 7.5 to 40% by mass or less, based on 100% by mass of the nonvolatile content of the composition.
[0045] <Component (C): Hygroscopic Inorganic Filler> The composition of the present invention may contain a hygroscopic inorganic filler. The component (C) may be used alone or in combination of two or more. By using the component (C), good moisture blocking properties can be achieved, and by trapping ionic impurities, an increase in surface resistivity in high-temperature, high-humidity environments can be suppressed, and electrical conductivity can be maintained.
[0046] Examples of component (C) include uncalcined hydrotalcite, semi-calcined hydrotalcite, calcined hydrotalcite, calcium oxide, magnesium oxide, calcined dolomite (a mixture containing calcium oxide and magnesium oxide), calcium hydride, strontium oxide, aluminum oxide, barium oxide, molecular sieve, zeolite, silica, etc. Component (C) is preferably one or more selected from uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite, and more preferably one or more selected from uncalcined hydrotalcite and semi-calcined hydrotalcite.
[0047] Hydrotalcite can be classified into uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite.
[0048] Uncalcined hydrotalcite is, for example, natural hydrotalcite (Mg 6 Al 2 (OH) 16 CO 3 ・4H 2 O), and for example, the basic skeleton layer [Mg 1-X Al X (OH) 2 ] X+ and the intermediate layer [(CO 3 ) X/2 ・mH 2 O] X- The uncalcined hydrotalcite is a concept that includes hydrotalcite-like compounds such as synthetic hydrotalcite. Examples of hydrotalcite-like compounds include those represented by the following formula (I) and formula (II).
[0049] [M 2+ 1-x M 3+ x (OH) 2 ] x+ ・[(A n- ) x/n ・mH 2 O] x- (I) (wherein, M 2+ is Mg 2+ , Zn 2+ represents a divalent metal ion such as M 3+ is Al 3+ , Fe 3+ represents a trivalent metal ion such as A n- is CO 3 2- , Cl - , NO 3 - In formula (I), M represents an n-valent anion such as 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 2+ is preferably Mg 2+ and M 3+ is preferably Al 3+ and A n- is preferably CO 3 2- is.
[0050] M 2+ x Al 2 (OH) 2x+6-nz (A n- ) z ・mH 2 O (II) (wherein, M 2+ is Mg 2+ , Zn 2+ represents a divalent metal ion such as A n- is CO 3 2- , Cl - , NO 3 - In formula (II), M represents an n-valent anion such as , where x is a positive number of 2 or more, z is a positive number of 2 or less, m is a positive number, and n is a positive number. 2+ is preferably Mg 2+ and A n-is preferably CO 3 2- is.
[0051] Semi-calcined hydrotalcite refers to a metal hydroxide obtained by calcining uncalcined hydrotalcite and having a layered crystal structure in which the amount of interlayer water is reduced or eliminated. When explained using a composition formula, "interlayer water" refers to "H" in the composition formula of the uncalcined natural hydrotalcite and the hydrotalcite-like compound described above. 2 It refers to "O".
[0052] On the other hand, calcined hydrotalcite is obtained by calcining uncalcined or semi-calcined hydrotalcite, and refers to a metal oxide having an amorphous structure in which not only interlayer water but also hydroxyl groups have disappeared through condensation dehydration.
[0053] Uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite can be distinguished by their saturated water absorption. The saturated water absorption of semi-calcined hydrotalcite is 1% by mass or more and less than 20% by mass. On the other hand, the saturated water absorption of uncalcined hydrotalcite is less than 1% by mass, and the saturated water absorption of calcined hydrotalcite is 20% by mass or more.
[0054] The "saturated water absorption" refers to the rate of mass increase relative to the initial mass when 1.5 g of a measurement sample (for example, semi-calcined hydrotalcite) is weighed out on a balance, the initial mass is measured, and the sample is allowed to stand for 200 hours in a small environmental test chamber (SH-222 manufactured by Espec Corporation) set at atmospheric pressure, 60°C, and 90% RH (relative humidity), and can be calculated using the following formula (i): saturated water absorption (mass%) = 100 × (mass after moisture absorption - initial mass) / initial mass (i).
[0055] The saturated water absorption of the semi-calcined hydrotalcite is preferably 3% by mass or more and less than 20% by mass, and more preferably 5% by mass or more and less than 20% by mass.
[0056] Furthermore, uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite can be distinguished by the rate of weight loss on heat measured by thermogravimetric analysis. The rate of weight loss on heat of semi-calcined hydrotalcite at 280°C is less than 15% by mass, and the rate of weight loss on heat of semi-calcined hydrotalcite at 380°C is 12% by mass or more. On the other hand, the rate of weight loss on heat of uncalcined hydrotalcite at 280°C is 15% by mass or more, and the rate of weight loss on heat of calcined hydrotalcite at 380°C is less than 12% by mass.
[0057] Thermogravimetric analysis can be performed using a Hitachi High-Tech Science TG / DTA EXSTAR6300 by weighing 5 mg of hydrotalcite into an aluminum sample pan, leaving the pan open and uncovered, in an atmosphere of nitrogen at a flow rate of 200 mL / min, and raising the temperature from 30°C to 550°C at a rate of 10°C / min. The thermal weight loss rate can be calculated using the following formula (ii): Thermal weight loss rate (mass%) = 100 × (mass before heating - mass when the predetermined temperature is reached) / mass before heating (ii).
[0058] Furthermore, uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite can be distinguished by the peaks and relative intensity ratios measured by powder X-ray diffraction. Semi-calcined hydrotalcite exhibits a split peak or a peak with a shoulder formed by combining two peaks in powder X-ray diffraction at 2θ of approximately 8 to 18°, and the relative intensity ratio (low-angle diffraction intensity / high-angle diffraction intensity) of the diffraction intensity of the peak or shoulder appearing on the low-angle side (= low-angle diffraction intensity) to the diffraction intensity of the peak or shoulder appearing on the high-angle side (= high-angle diffraction intensity) is 0.001 to 1,000. On the other hand, uncalcined hydrotalcite has only one peak near 8 to 18°, or the relative intensity ratio of the diffraction intensity of the peak or shoulder appearing on the low-angle side to the peak or shoulder appearing on the high-angle side is outside the aforementioned range. Calcined hydrotalcite does not have a characteristic peak in the 8 to 18° region, but has a characteristic peak at 43°. Powder X-ray diffraction measurements were performed using a powder X-ray diffractometer (PANalytical, Empyrean) under the following conditions: CuKα (1.5405 Å) anticathode, voltage: 45 V, current: 40 mA, sampling width: 0.0260°, scan rate: 0.0657° / s, measurement diffraction angle range (2θ): 5.0131 to 79.9711°. Peak search was performed using the peak search function of the software provided with the diffractometer under the following conditions: minimum significance: 0.50, minimum peak tip: 0.01°, maximum peak tip: 1.00°, peak base width: 2.00°, method: minimum value of second derivative.
[0059] The BET specific surface area of semi-calcined hydrotalcite is 1 to 250 m 2 / g is preferred, and 5 to 200m 2 These BET specific surface areas can be calculated according to the BET method by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM Model 1210, manufactured by Mountech Co., Ltd.) and then using the BET multipoint method.
[0060] The particle size of the uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite is preferably 1 to 1,000 nm, more preferably 10 to 800 nm, from the viewpoint of transparency. These particle sizes are the median diameters of the particle size distributions determined on a volume basis by laser diffraction / scattering particle size distribution measurement (JIS Z8825).
[0061] Uncalcined hydrotalcite, semi-calcined hydrotalcite, and calcined hydrotalcite can be used after surface treatment with a surface treatment agent. Examples of the surface treatment agent that can be used for the surface treatment include higher fatty acids, alkylsilanes, and silane coupling agents, and among these, higher fatty acids and alkylsilanes are preferred. One or more types of surface treatment agents can be used.
[0062] Commercially available uncalcined hydrotalcites can be used. Examples of commercially available products include "DHT-4A" (particle diameter (median diameter): 370 nm), "Almakaiser" (particle diameter (median diameter): 620 nm), and "Magcera 1" (particle diameter (median diameter): 470 nm), all manufactured by Kyowa Chemical Industry Co., Ltd., and "STABIACE HT-1," "STABIACE HT-7," and "STABIACE HT-P" manufactured by Sakai Chemical Industry Co., Ltd.
[0063] Commercially available semi-calcined hydrotalcites can be used, such as "DHT-4C" (particle diameter (median diameter): 400 nm) and "DHT-4A-2" (particle diameter (median diameter): 400 nm) manufactured by Kyowa Chemical Industry Co., Ltd.
[0064] Commercially available calcined hydrotalcites can be used, such as "KW-2200" (particle diameter (median diameter): 400 nm) and "KW-2200" (particle diameter (median diameter): 400 nm) manufactured by Kyowa Chemical Industry Co., Ltd.
[0065] Commercially available calcium oxide products can be used, such as "QC-X" manufactured by Inoue Lime Industry Co., Ltd., "Moistop #10" manufactured by Sankyo Flour Milling Co., Ltd., "HAL-G," "HAL-J," and "HAL-F" manufactured by Yoshizawa Lime Industry Co., Ltd., and "CaO Nano Powder" manufactured by Filgen.
[0066] The particle size of calcium oxide and the particle size of the mixture containing calcium oxide are each preferably 0.03 to 10 μm, more preferably 0.05 to 5 μm, and even more preferably 0.1 to 3 μm. These particle sizes are the median diameters of the particle size distributions determined on a volume basis by laser diffraction / scattering particle size distribution measurement (JIS Z 8825).
[0067] The content of component (C) in the composition is preferably 1 mass % or more, more preferably 2.5 mass % or more, and even more preferably 5.0 mass % or more, based on 100 mass % of the nonvolatile content of the composition, from the viewpoint of moisture blocking properties, and is preferably 60 mass % or less, more preferably 55 mass % or less, and even more preferably 50 mass % or less, from the viewpoint of adhesion and flexibility.
[0068] The composition may contain components other than components (A) to (C) (hereinafter sometimes referred to as "other components") to the extent that the effects of the present invention are not impaired. Examples of other components include tackifiers, curing accelerators, antioxidants, plasticizers, and metal complexes in which a bidentate ligand in which both coordinating atoms are oxygen atoms and a monodentate ligand in which the coordinating atom is oxygen atom are bonded to a central metal. These may be used alone or in combination of two or more.
[0069] The tackifier is a component that imparts tackiness to the protective (sealing) film and improves adhesion. In the present invention, there are no particular limitations on the tackifier, and known tackifiers can be used.
[0070] From the viewpoint of the heat resistance of the protective (sealing) film, the softening point of the tackifier is preferably 50 to 200° C., more preferably 90 to 180° C., and even more preferably 100 to 150° C. The softening point is measured by the ring and ball method in accordance with JIS K2207.
[0071] Commercially available tackifiers can be used, such as Arakawa Chemical Industries, Ltd.'s "Arcon P-90," "Arcon P-100," "Arcon P-115," "Arcon P-125," "Arcon P-140," "Arcon M-90," "Arcon M-100," "Arcon M-115," and "Arcon M-135" (all of which are cyclohexane ring-containing hydrogenated petroleum resins).
[0072] From the viewpoint of the adhesiveness and sealing properties of the protective (sealing) film, the content of the tackifier is preferably 0 to 30 mass %, more preferably 0 to 25 mass %, and even more preferably 0 to 22.5 mass %, relative to 100 mass % of the nonvolatile content of the composition.
[0073] Examples of the curing accelerator include imidazole compounds, tertiary and quaternary amine compounds, dimethylurea compounds, and organic phosphine compounds.
[0074] Examples of the imidazole compound include 1H-imidazole, 2-methylimidazole, 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 2-phenyl-4,5-bis(hydroxymethyl)imidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2-phenylimidazole, 2-dodecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Specific examples of the imidazole compound include Curesol 2MZ, 2P4MZ, 2E4MZ, 2E4MZ-CN, C11Z, C11Z-CN, C11Z-CNS, C11Z-A, 2PHZ, 1B2MZ, 1B2PZ, 2PZ, C17Z, 1.2DMZ, 2P4MHZ-PW, 2MZ-A, and 2MA-OK (all manufactured by Shikoku Chemicals Corporation).
[0075] The tertiary and quaternary amine compounds are not particularly limited, and examples thereof include quaternary ammonium salts such as tetramethylammonium bromide and tetrabutylammonium bromide; diazabicyclo compounds such as DBU (1,8-diazabicyclo[5.4.0]undecene-7), DBN (1,5-diazabicyclo[4.3.0]nonene-5), DBU-phenol salt, DBU-octylate salt, DBU-p-toluenesulfonate, DBU-formate salt, and DBU-phenol novolac resin salt; tertiary amines or salts thereof such as benzyldimethylamine, 2-(dimethylaminomethyl)phenol, and 2,4,6-tris(dimethylaminomethyl)phenol (TAP); and dimethylurea compounds such as aromatic dimethylurea and aliphatic dimethylurea.
[0076] Examples of dimethylurea compounds include aromatic dimethylureas such as DCMU (3-(3,4-dichlorophenyl)-1,1-dimethylurea) and U-CAT3512T (manufactured by San-Apro Co., Ltd.); and aliphatic dimethylureas such as U-CAT3503N (manufactured by San-Apro Co., Ltd.). Among these, aromatic dimethylureas are preferably used from the viewpoint of curability.
[0077] Examples of the organic phosphine compound include triphenylphosphine, tetraphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tri-tert-butylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, triphenylphosphine triphenylborane, etc. Specific examples of the organic phosphine compound include TPP, TPP-MK, TPP-K, TTBuP-K, TPP-SCN, TPP-S (all manufactured by Hokko Chemical Industry Co., Ltd.), etc.
[0078] When a curing accelerator is used, the content thereof is preferably 0.0001 to 0.1 mass%, more preferably 0.0002 to 0.075 mass%, and even more preferably 0.0002 to 0.05 mass%, relative to 100 mass% of the nonvolatile content of the composition, in order to promote the formation of component (A) (i.e., a crosslinked polymer having an isobutene-isoprene copolymer chain), etc.
[0079] In the present invention, there are no particular limitations on the antioxidant, and known antioxidants can be used. When an antioxidant is used, the content thereof is preferably 0.01 to 0.5% by mass, more preferably 0.05 to 0.4% by mass, and even more preferably 0.1 to 0.3% by mass, relative to 100% by mass of the nonvolatile content of the composition.
[0080] Examples of plasticizers include mineral oils such as paraffinic process oil, naphthenic process oil, liquid paraffin, and vaseline, and vegetable oils such as castor oil, cottonseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, and olive oil.
[0081] In order to improve the adhesion and flex resistance of the protective (sealing) film, a metal complex may be used in which a bidentate ligand in which both coordinating atoms are oxygen atoms (hereinafter sometimes referred to as an "oxygen-bidentate ligand") and a monodentate ligand in which the coordinating atom is an oxygen atom (hereinafter sometimes referred to as an "oxygen-monodentate ligand") are bonded to a central metal.
[0082] The metal complex is preferably a metal complex represented by the following formula (1) (hereinafter referred to as "metal complex (1)").
[0083]
[0084] In formula (1), M is a central metal of the metal complex and represents a metal of the second to sixth periods of the periodic table; 1 and R 3 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkoxy group, an alkenyloxy group, an aryloxy group, or an aralkyloxy group; R 2represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkoxy group, an alkenyloxy group, an aryloxy group, an aralkyloxy group, an alkoxycarbonyl group, or an alkenyloxycarbonyl group; X represents a monodentate oxygen ligand; the solid line between the oxygen atom (O) and M in [ ] represents a covalent bond; the dashed line between the oxygen atom (O) and M in [ ] represents a coordinate bond; and m represents an integer of 3 or 4, and n represents an integer of 1 to 3, with m>n.
[0085] M in formula (1) is preferably a metal of the third to fifth periods, more preferably Al, Ti, Mn, Fe, Co, Ni, Cu, Zn, Ge, Zr, In, or Sn, and even more preferably Al, Ti, or Zr.
[0086] In this specification, examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0087] In this specification, the alkyl group may be either linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1,1-dimethylbutyl group, a 2,2-dimethylbutyl group, a 3,3-dimethylbutyl group, and a 2-ethylbutyl group. The alkyl group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0088] In this specification, the alkenyl group may be either linear or branched. The number of carbon atoms in the alkenyl group is preferably 2 to 20. Examples of the alkenyl group include ethenyl (i.e., vinyl group), 1-propenyl, 2-propenyl, 2-methyl-1-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 3-methyl-2-butenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 4-methyl-3-pentenyl, 1-hexenyl, 3-hexenyl, 5-hexenyl, and octadecenyl (e.g., 9-octadecenyl). Examples of substituents that the alkenyl group may have include halogen atoms, hydroxy groups, and amino groups which may have a substituent.
[0089] In this specification, the alkynyl group may be either linear or branched. The number of carbon atoms in the alkynyl group is preferably 2 to 10, and more preferably 2 to 6. Examples thereof include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, a 2-pentynyl group, a 3-pentynyl group, a 4-pentynyl group, a 1-hexynyl group, a 2-hexynyl group, a 3-hexynyl group, a 4-hexynyl group, a 5-hexynyl group, and a 4-methyl-2-pentynyl group. Examples of substituents that the alkynyl group may have include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0090] In this specification, the number of carbon atoms in the aryl group is preferably 6 to 18, and more preferably 6 to 14. Examples of the aryl group include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, and a 9-anthryl group. The aryl group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, and an optionally substituted amino group.
[0091] In this specification, the number of carbon atoms in the aralkyl group is preferably 7 to 16. Examples of the aralkyl group include a benzyl group, a phenethyl group, a naphthylmethyl group, and a phenylpropyl group. The aralkyl group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0092] In this specification, examples of the amino group which may have a substituent include an amino group, a mono- or di-alkylamino group (e.g., a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, a propylamino group, a dibutylamino group), a mono- or di-cycloalkylamino group (e.g., a cyclopropylamino group, a cyclohexylamino group), a mono- or di-arylamino group (e.g., a phenylamino group), a mono- or di-aralkylamino group (e.g., a benzylamino group, a dibenzylamino group), a heterocyclic amino group (e.g., a pyridylamino group) and the like.
[0093] In this specification, the alkyl group in an alkoxy group (i.e., an alkyloxy group) is the same as the alkyl group described above. The alkoxy group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0094] In this specification, the alkenyl group in the alkenyloxy group is the same as the above-mentioned alkenyl group. The alkenyloxy group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0095] In this specification, the explanation of the aryl group in the aryloxy group is the same as the explanation of the aryl group described above. The aryloxy group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, and an optionally substituted amino group.
[0096] In this specification, the description of the aralkyl group in the aralkyloxy group is the same as the description of the aralkyl group described above. The aralkyloxy group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0097] In this specification, the alkyl group in the alkoxycarbonyl group (i.e., alkyloxycarbonyl group) is the same as the alkyl group described above. The alkoxycarbonyl group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0098] In this specification, the alkenyl in the alkenyloxycarbonyl group is the same as the above-mentioned alkenyl. The alkenyloxycarbonyl group may have a substituent. Examples of the substituent include a halogen atom, a hydroxy group, and an amino group which may have a substituent.
[0099] The oxygen-monodentate ligand represented by X in formula (1) is usually the conjugate base of a Bronsted acid, for example, RO - (R: organic group), RCOO - (R: organic group), etc.
[0100] RO - In the formula (I), the organic group R may be either an aliphatic group or an aromatic group. The aliphatic group may be either a saturated aliphatic group or an unsaturated aliphatic group. The number of carbon atoms in the organic group R is preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6. - Examples of the oxide anion include methoxide anion, ethoxide anion, propoxide anion, isopropoxide anion, butoxide anion, isobutoxide anion, sec-butoxide anion, tert-butoxide anion, pentyloxide anion, and hexyloxide anion.
[0101] RCOO -In the formula, the organic group R may be either an aliphatic group or an aromatic group. The aliphatic group may be either a saturated aliphatic group or an unsaturated aliphatic group. The number of carbon atoms in the organic group R is preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6. RCOO - Examples of the anions include anions corresponding to carboxylic acids such as acetic acid, propionic acid, and benzoic acid.
[0102] The brackets in formula (1) represent an oxygen-bidentate ligand. Specific examples of the oxygen-bidentate ligand include acetylacetone, 3-methyl-2,4-pentanedione, acetylacetaldehyde, 2,4-hexanedione, 2,4-heptanedione, 5-methyl-2,4-hexanedione, 5,5-dimethyl-2,4-hexanedione, benzoylacetone, benzoylacetophenone, salicylaldehyde, 1,1,1-trifluoroacetylacetone, 1,1,1,5,5,5-hexafluoroacetylacetone, 3-methoxy-2,4-pentanedione, 3-cyano-2,4-pentanedione, 3-nitro-2,4-pentanedione, 3-chloro-2,4-pentanedione, acetoacetic acid, methyl acetoacetate, ethyl acetoacetate, propyl acetoacetate, salicylic acid, methyl salicylate, malonic acid, dimethyl malonate, and diethyl malonate. When coordinated to the central metal, the oxygen-bidentate ligand has a structure in which one or more protons have been removed.
[0103] Examples of the metal complex (1) in which the central metal M is Al include (octadecenylacetoacetate)aluminum diisopropylate, (ethylacetoacetate)aluminum diisopropylate, (ethylacetoacetate)aluminum di-n-butylate, (propylacetoacetate)aluminum diisopropylate, and (n-butylacetoacetate)aluminum diisopropylate.
[0104] Examples of the metal complex (1) in which the central metal M is Ti include titanium allylacetoacetate triisopropoxide, titanium di-n-butoxide (bis-2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), titanium methylphenoxide, and titanium oxide bis(pentanedionate).
[0105] Examples of the metal complex (1) in which the central metal M is Zr include zirconium allylacetoacetate triisopropoxide, zirconium di-n-butoxide (bis-2,4-pentanedionate), zirconium diisopropoxide (bis-2,4-pentanedionate), zirconium diisopropoxide bis(tetramethylheptanedionate), zirconium diisopropoxide bis(ethylacetoacetate), zirconium butoxide (acetylacetate) (bisethylacetoacetate), and zirconium tributoxymonoacetylacetonate.
[0106] When a metal complex in which an oxygen-bidentate ligand and an oxygen-monodentate ligand are bonded to a central metal (particularly, metal complex (1)) is used, the content thereof is preferably 0.05 to 5.0 mass%, more preferably 0.1 to 4.0 mass%, and even more preferably 0.15 to 3.0 mass%, relative to 100 mass% of the nonvolatile content of the composition.
[0107] <Conductive Layer of Conductive Substrate> The conductive layer of the conductive substrate protected (sealed) by the composition of the present invention is composed of a conductive material containing one or more metal nanowires, metal meshes, metal nanoparticles, and conductive polymers. The metal constituting the metal nanowires, metal meshes, and / or metal nanoparticles is not particularly limited and may be, for example, one or more metals selected from silver, copper, gold, nickel, platinum, palladium, iron, cobalt, and tin, with silver, copper, gold, and nickel being preferred. The conductive polymer is not particularly limited and may be, for example, one or more metals selected from poly(3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, graphene, polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline, with PEDOT being preferred. In a preferred embodiment of the present invention, the conductive layer of the conductive substrate is composed of a conductive material containing silver nanowires.
[0108] [Method for Producing Composition] The method for producing the composition of the present invention is not particularly limited, and examples thereof include a method in which the above-mentioned blended components are mixed, if necessary, with a solvent or the like, using a kneading roller or a rotary mixer.
[0109] [Method for forming protective (sealing) film] The method for forming a protective (sealing) film on the conductive layer of a conductive substrate (for protecting (sealing) the conductive layer) is not particularly limited, and examples thereof include: (1) a method of applying a varnish of a composition on the conductive layer and drying it to form a protective (sealing) film; (2) a method of preparing a sealing sheet having a composition layer on a support, laminating the composition layer of the sealing sheet on the conductive layer, and peeling off the support to form a protective (sealing) film; and the like.
[0110] Method (1) can be carried out, for example, by applying a varnish-like composition prepared by blending an organic solvent onto a conductive layer using a die coater or the like, and then drying the resulting coating by heating or blowing hot air onto the conductive layer to form a protective (sealing) film on the conductive layer.
[0111] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (hereinafter also abbreviated as "MEK"), and cyclohexanone, acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. Any of the organic solvents may be used alone, or two or more may be used in combination.
[0112] There are no particular restrictions on the drying conditions, but typically drying at about 50 to 100° C. for about 3 to 15 minutes is preferred.
[0113] The thickness of the protective (sealing) film after drying is usually in the range of 3 μm to 200 μm, preferably 5 μm to 100 μm, and more preferably 5 μm to 50 μm.
[0114] The method (2) can be carried out by, for example, applying a composition prepared by blending an organic solvent into a varnish onto a support using a die coater or the like, drying the resulting coating film by heating or by blowing hot air onto the support, or the like, to prepare a sealing sheet in which a composition layer is formed on a support, and then laminating the composition layer of the sealing sheet onto a conductive layer using a roll laminator, a vacuum laminator, or the like by a batch method, a continuous method with a roll, or the like, and peeling off the support to form a protective (sealing) film on the conductive layer.
[0115] Examples of the support include plastic films such as polyolefins such as polyethylene, polypropylene, and polyvinyl chloride; cycloolefin polymers; polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate; polycarbonate; and polyimides. PET is particularly preferred as a plastic film. The support may also be a metal foil such as aluminum foil, stainless steel foil, or copper foil. The surface of the support on which the composition layer is formed may be subjected to a release treatment using a silicone resin-based release agent, an alkyd resin-based release agent, a fluororesin-based release agent, or the like, a matte treatment, a corona treatment, or the like. In the present invention, when the support has a release layer, the release layer is also considered to be part of the support. The thickness of the support is not particularly limited, but from the viewpoint of handleability, etc., it is preferably 20 to 200 μm, more preferably 20 to 125 μm.
[0116] The organic solvent, drying conditions, and thickness of the protective (sealing) film after drying are the same as those in the above method (1).
[0117] [Uses] The composition of the present invention can be used for protecting (sealing) the conductive layer of a conductive substrate that uses metal nanowires, metal meshes, metal nanoparticles, or conductive polymers, particularly metal nanowires or metal nanoparticles, as the conductor.
[0118] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples and can be practiced with appropriate modifications within the scope of the above and below aims, all of which are included within the technical scope of the present invention. Note that "parts" and "%" in the amounts of components mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0119] <Components> The components used in the Production Examples are as follows. Component (A): "ER866" (manufactured by Seiko PMC Corporation, glycidyl methacrylate-modified butyl rubber (glycidyl methacrylate-modified isobutene-isoprene copolymer), epoxy group concentration: 1.63 mmol / g, number average molecular weight: 113,000, isobutene unit / isoprene unit: 98.9% / 1.1%) "ER661" (manufactured by Seiko PMC Corporation, maleic anhydride-modified butyl rubber (maleic anhydride-modified isobutene-isoprene copolymer), acid anhydride group concentration: 0.77 mmol / g, number average molecular weight: 40,000, isobutene unit / isoprene unit: 98.9% / 1.1%) (Component (B): "HV-300M" (manufactured by Toho Chemical Industry Co., Ltd., maleic anhydride-modified liquid polybutene, acid anhydride group concentration: 0.77 mmol / g, number average molecular weight: 2,100) "HV-1900" (manufactured by ENEOS Corporation, liquid polybutene, number average molecular weight: 2,900, viscosity at 25°C: 460 Pa·s) (C) component: semi-calcined hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd., "DHT-4C", particle diameter (median diameter): 400 nm, BET specific surface area: 15 m 2 / g) Uncalcined hydrotalcite (manufactured by Kyowa Chemical Industry Co., Ltd., "DHT-4A", particle diameter (median diameter): 370 nm, BET specific surface area: 11 m 2 / g) Other ingredients: "Arcon P-125" (tackifier: Arakawa Chemical Industries, Ltd., cyclohexane ring-containing hydrogenated petroleum resin, softening point: 125°C) "Plenact Al-M" (metal complex: Ajinomoto Fine-Techno Co., Ltd., (octadecenylacetoacetate)aluminum diisopropylate) 2,4,6-tris(dimethylaminomethyl)phenol (curing accelerator: hereinafter abbreviated as "TAP") (Kayaku Akzo Co., Ltd.) Comparative ingredients: "KR-3700" (Shin-Etsu Chemical Co., Ltd., solvent-added silicone adhesive) "CAT-PL-50T" (Shin-Etsu Chemical Co., Ltd., toluene solution of divinyltetramethylsiloxane complex of chloroplatinic acid) "PARACRON S-2012" (manufactured by Negami Chemical Industrial Co., Ltd., thermoplastic acrylic resin, weight average molecular weight: 900,000, hydroxyl value: 6.5 KOHmg / g, toluene solvent, solid content: 34.5% by weight), "STABIO D-376" (manufactured by Mitsui Chemicals, Inc., isocyanate curing agent, NCO%: 24%), "ZX-1059" (manufactured by Nippon Steel Chemical & Material Co., Ltd., liquid hydrogenated bisphenol A and F type epoxy resin, epoxy equivalent: 165 g / eq), "TOPR-300" (manufactured by Nippon Steel Chemical & Material Co., Ltd., solid epoxy resin), "YX7200B35" (manufactured by Mitsubishi Chemical Corporation, phenoxy resin solution, solvent: MEK, non-volatile content: 35%), "TBPDA" (manufactured by Hokko Chemical Industry Co., Ltd., ionic liquid curing agent).
[0120] <Substrate> Polyethylene terephthalate (PET) film: Lumirror R80 manufactured by Toray Industries, Inc., 38 μm thick, water vapor permeability 20 g / m 2 / day (40°C-90%RH, MOCON method) Barrier film: Reiko Co., Ltd. Beleal 38UD001, 38 μm, water vapor permeability 5 × 10 -4 g / m 2 / day (40℃-90%RH, MOCON method)
[0121] <Method for producing encapsulating sheet> <Production Example 1> A varnish having a blending ratio shown in Table 1 was produced by the following procedure, and an encapsulating sheet was produced using the obtained varnish. The amount (parts) of each component used in the table below indicates the amount of non-volatile content of each component in the varnish.
[0122] Specifically, a Swazol solution (non-volatile content: 60%) of cyclohexane ring-containing hydrogenated petroleum resin (tackifier, Arakawa Chemical Industries, Ltd.'s "Arcon P-125") was blended with maleic anhydride-modified liquid polybutene (Toho Chemical Industry Co., Ltd.'s "HV-300M"), polybutene (ENEOS Corporation's "HV-1900"), a toluene solution (non-volatile content: 25%) of glycidyl methacrylate-modified butyl rubber (Seiko PMC Corporation's "ER866"), a toluene solution (non-volatile content: 35%) of maleic acid-modified butyl rubber (Seiko PMC Corporation's "ER661"), a curing accelerator (TAP, Kayaku Nouryon Co., Ltd.), and toluene. The resulting mixture was uniformly dispersed in a high-speed rotary mixer to obtain a varnish composition. The obtained varnish was uniformly applied by a die coater onto a release-treated surface of a polyethylene terephthalate (PET) film ("SP4020" manufactured by Toyo Cross Co., Ltd., PET film thickness: 50 μm) that had been treated with a silicone-based release agent, and the applied film was heated at 130° C. for 30 minutes to obtain a sealing sheet having a composition layer with a thickness of 20 μm.
[0123] Production Example 2 A mixture was obtained by dispersing maleic anhydride-modified liquid polybutene ("HV-300M" manufactured by Toho Chemical Industry Co., Ltd.), polybutene ("HV-1900" manufactured by ENEOS Corporation), uncalcined hydrotalcite ("DHT-4A" manufactured by Kyowa Chemical Industry Co., Ltd.), and a metal complex ("Plenact Al-M" manufactured by Ajinomoto Fine-Techno Co., Ltd.) in a Swazol solution (non-volatile content: 60%) of cyclohexane ring-containing hydrogenated petroleum resin (tackifier, "Arcon P-125" manufactured by Arakawa Chemical Industries, Ltd.) using a three-roll mill. Glycidyl methacrylate-modified butyl rubber ("ER866" manufactured by Seiko PMC Corporation), maleic acid-modified butyl rubber ("ER661" manufactured by Seiko PMC Corporation), a curing accelerator (TAP, manufactured by Nouryon Chemical Industries, Ltd.), and toluene into the resulting mixture, which was then uniformly dispersed using a high-speed rotary mixer to obtain a varnish composition. The obtained varnish was uniformly applied by a die coater onto a release-treated surface of a polyethylene terephthalate (PET) film ("SP4020" manufactured by Toyo Cross Co., Ltd., PET film thickness: 50 μm) that had been treated with a silicone-based release agent, and the applied film was heated at 130° C. for 30 minutes to obtain a sealing sheet having a composition layer with a thickness of 20 μm.
[0124] <Production Example 3> A varnish of a composition and a sealing sheet having a composition layer with a thickness of 20 μm were obtained in the same manner as in Production Example 2, except that the uncalcined hydrotalcite was changed to semi-calcined hydrotalcite ("DHT-4C" manufactured by Kyowa Chemical Industry Co., Ltd.).
[0125] <Production Example 4> A divinyltetramethylsiloxane complex of chloroplatinic acid ("CAT-PL-50T" manufactured by Shin-Etsu Chemical Co., Ltd.) was added to a solvent-addition type silicone pressure-sensitive adhesive ("KR-3700" manufactured by Shin-Etsu Chemical Co., Ltd., a toluene solution with a solids content of 60 wt%), and the resulting mixture was stirred with a high-speed rotary mixer to obtain a varnish of the composition. The obtained varnish was uniformly applied with a die coater to the release-treated surface of a PET film ("SS1A" manufactured by Nippa Corporation) that had been treated with a fluorine-based release agent, and heated at 150°C for 1 minute to obtain a sealing sheet having a composition layer with a thickness of 20 μm.
[0126] <Production Example 5> An isocyanate curing agent ("STABIO D-376" manufactured by Mitsui Chemicals, Inc.) was added to a thermoplastic acrylic resin ("PARACRON S-2012" manufactured by Negami Chemical Industrial Co., Ltd., solid content: 34.5 wt%, toluene solvent), and the resulting mixture was stirred with a high-speed rotary mixer to obtain a varnish of the composition. The obtained varnish was uniformly applied with a die coater to the release-treated surface of a PET film ("SP4020" manufactured by Toyo Cross Co., Ltd., PET film thickness: 50 μm) that had been treated with a silicone-based release agent, and the resulting mixture was heated at 130°C for 30 minutes to obtain an encapsulating sheet having a composition layer with a thickness of 20 μm.
[0127] <Production Example 6> A mixture of liquid hydrogenated bisphenol A and F epoxy resins ("ZX-1059" manufactured by Mitsubishi Chemical Corporation) and a solid epoxy resin ("TOPR-300" manufactured by Nippon Steel Chemical & Material Co., Ltd.) was prepared, followed by blending with a phenoxy resin solution ("YX7200B35" manufactured by Mitsubishi Chemical Corporation, solvent: MEK, non-volatile content: 35%) and an ionic liquid curing agent ("TBPDA" manufactured by Hokko Chemical Industry Co., Ltd.) and uniformly dispersing the mixture in a high-speed rotary mixer to obtain a varnish of the composition. The obtained varnish was uniformly applied using a die coater to the release-treated surface of a PET film ("NS80A" manufactured by Fujimori Kogyo Co., Ltd., PET film thickness: 38 μm) that had been treated with an alkyd-based release agent, and the mixture was heated at 130°C for 30 minutes to obtain an encapsulating sheet having a composition layer with a thickness of 20 μm.
[0128] <Method for measuring haze and total light transmittance of composition layer> Haze (%) and total light transmittance (%) were measured in accordance with JIS 7136. Specifically, the sealing sheets of Production Examples 1 to 6 prepared by the above-mentioned method were processed into 40 mm × 40 mm squares, and the composition layer was bonded to a 50 mm × 50 mm square alkali-free glass ("OA-10G" manufactured by Nippon Electric Glass Co., Ltd., thickness: 700 μm) using a vacuum laminator ("V-160" manufactured by Nikko Materials Co., Ltd., temperature 80 ° C., 0.3 MPa, 30 seconds) to prepare a measurement sample. Note that, after bonding, the PET film was peeled off from the sealing sheet of Production Example 6, and the sheet was heated at 100 ° C. for 60 minutes for curing treatment. Next, the haze (%) and total light transmittance (%) of the prepared measurement sample were measured using a haze meter HZ-V3 (halogen lamp) manufactured by Suga Test Instruments Co., Ltd. under D65 light with air as a reference. The results are shown in Table 1.
[0129] <Method for measuring adhesion strength of composition layer> The sealing sheets produced in Production Examples 1 to 6 were cut to a length of 50 mm and a width of 20 mm. Next, using a batch vacuum laminator ("Morton-724" manufactured by Nichigo-Morton Co., Ltd.), a composite film comprising aluminum foil and a polyethylene terephthalate (PET) film ("PET-Tsuke AL1N30" manufactured by Tokai Toyo Aluminum Sales Co., Ltd., aluminum foil thickness: 30 μm, PET film thickness: 25 μm) was laminated onto the composition layer of the sealing sheet. The lamination was performed under conditions of a temperature of 80°C, a time of 30 seconds, and a pressure of 0.3 MPa. Next, the PET film was peeled off from the sealing sheet, and a polyimide film ("Upilex-S" manufactured by Ube Industries, Ltd., thickness: 50 μm) was laminated onto the exposed composition layer under the same conditions as above to obtain a laminate having a laminate structure of "composite film / composition layer / polyimide film". In addition, after lamination, the sealing sheet of Production Example 6 was peeled off, and the polyimide film was laminated under the same conditions as above, and then heated at 100 ° C for 60 minutes to perform a curing treatment. For the obtained laminate, the adhesive strength (room temperature adhesive strength) was measured when the "composite film / composition layer" was peeled from the polyimide film at room temperature in a direction 180 degrees to the longitudinal direction of the aluminum foil at a pulling rate of 300 mm / min. In addition, the adhesive strength (high temperature adhesive strength) was measured when the laminate produced in the same manner as above was similarly peeled under an environment of 60 ° C. The results are shown in Table 1.
[0130] <Evaluation of Surface Resistivity of Encapsulated Silver Nanowire-Laminated Conductive Film> A5-sized silver nanowire-laminated conductive film (NovaFilm-AgNW; silver nanowire-coated transparent conductive film (PET substrate)) manufactured by Novarials was prepared. The sealing sheets prepared in Production Examples 1 to 6 were processed to A5 size, and the composition layer was attached to the substrate listed in Table 2 using a vacuum laminator ("V-160" manufactured by Nikko Materials Co., Ltd., 80°C, 0.3 MPa, 30 seconds). Thereafter, the PET film was peeled off from the sealing sheet, and the exposed composition layer was attached to the silver nanowire layer of the silver nanowire-laminated conductive film under the same conditions as above to prepare an evaluation sample. Note that in Comparative Example 3 using Production Example 6, the composition layer was attached to the silver nanowire layer and then heated at 100°C for 60 minutes for curing treatment.
[0131] The initial surface resistivity (Ω / Sq.) of the encapsulated silver nanowire-laminated conductive film was measured using an eddy current sheet resistance meter (EddyCusTF Protable 1010 manufactured by SURAGUS Corporation). The encapsulated silver nanowire-laminated conductive film was then stored in a constant temperature and humidity tester (85°C, 85% RH), and after 100 hours, the surface resistivity (Ω / Sq.) was measured again using the eddy current sheet resistance meter. The change in surface resistivity was calculated as follows: Change (%) = [(Surface resistivity after 100 hours of storage at 85°C, 85% RH) / (Initial surface resistivity)] × 100 - 100, and evaluation was performed according to the following criteria. The results are shown in Table 2. (Evaluation criteria for surface resistivity) ◎ Change in surface resistivity is less than 0% ○ Change in surface resistivity is 0% or more but less than 20% × Change in surface resistivity is 20% or more
[0132] <Evaluation of Flex Resistance> The PET film was peeled off from each of the sealing sheets produced in Production Examples 1 to 6, and polyimide films (manufactured by Unitika Ltd., 25 μm) were attached to both sides of the composition layer by vacuum lamination (80° C., 0.3 MPa, 30 seconds) to produce evaluation samples having a structure of “polyimide (PI) film / composition layer / polyimide (PI) film.”
[0133] The obtained evaluation sample was placed in a clamshell-type bending tester "CL40R type-E02" (manufactured by Yuasa System Co., Ltd.), and the evaluation sample was bent 100,000 times under conditions of a temperature of 60°C, humidity of 90% RH, a radius of curvature (R) of 2.0 mm, and a speed of 60 rpm. After bending, the evaluation sample was observed using a Keyence digital microscope "VHX-5000" (magnification: 20x), and the bending resistance was evaluated according to the following criteria. The results are shown in Table 2. (Evaluation criteria for bending resistance) ○ (Acceptable): No peeling × (Unacceptable): Peeling and generation of bubbles
[0134]
[0135]
[0136] From the results in Tables 1 and 2, it can be seen that Examples 1 to 4 have good values for haze, total light transmittance and adhesion strength, and also have good evaluations for surface resistivity and flex resistance.
[0137] The composition of the present invention can form a protective (sealing) film that, when protecting (sealing) a conductive layer that constitutes a conductive substrate, can suppress changes in the surface resistivity of the conductive substrate and migration of the conductor while simultaneously achieving transparency, adhesion strength, and flex resistance. Therefore, the composition can be used to protect (seal) the conductive layer of a conductive substrate that uses metal nanowires, metal meshes, metal nanoparticles, or conductive polymers, particularly metal nanowires or metal nanoparticles, as the conductor.
[0138] This application is based on patent application No. 2023-052198 filed in Japan, the contents of which are incorporated in their entirety herein.
Claims
1. A composition for a protective film of a conductive layer of a conductive substrate, comprising: (A) a crosslinked polymer having an isobutene-isoprene copolymer chain; and the conductive layer is composed of a conductive material including one or more selected from metal nanowires, metal meshes, metal nanoparticles, and conductive polymers.
2. The composition according to claim 1, wherein (A) the crosslinked polymer having an isobutene-isoprene copolymer chain is at least one selected from the group consisting of a reaction product between an isobutene-isoprene copolymer having an epoxy group and an olefin polymer having a carboxy group and / or an acid anhydride group, and a reaction product between an isobutene-isoprene copolymer having a carboxy group and / or an acid anhydride group and an olefin polymer having an epoxy group.
3. The composition according to claim 1, wherein the content of component (A) is 10 to 75 mass % based on 100 mass % of the nonvolatile content of the composition.
4. The resin composition according to claim 1, further comprising (B) a liquid polyolefin resin and / or a liquid rubber.
5. The composition according to claim 4, wherein the content of component (B) is 5 to 50 mass % based on 100 mass % of the nonvolatile content of the composition.
6. The composition of claim 1, further comprising (C) a hygroscopic inorganic filler.
7. The composition according to claim 6, wherein the hygroscopic inorganic filler (C) is at least one selected from uncalcined hydrotalcite and semi-calcined hydrotalcite.
8. The composition according to claim 6, wherein the content of component (C) is 1 to 60 mass % based on 100 mass % of the nonvolatile content of the composition.
9. The composition according to claim 1, wherein the metal constituting the metal nanowires, metal mesh and / or metal nanoparticles is one or more selected from silver, copper, gold, nickel, platinum, palladium, iron, cobalt and tin.
10. The composition according to claim 1, wherein the conductive polymer is one or more selected from the group consisting of poly(3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, graphene, polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.
Citation Information
Patent Citations
Graphene structure, method for producing the same, photoelectric conversion element, solar cell, and image pickup apparatus
JP2013035699A
sealing film
JP2015502868A
Sealing film and organic electronic device including the same
JP2017513205A
Sealing sheet
JP2023007246A