Solid electrolyte material, solid electrolyte composite, electrode, and method for producing solid electrolyte material

A novel solid electrolyte material with a specific composition and production method enhances ionic conductivity and stability, addressing the performance gaps in existing lithium ion and all-solid-state batteries for electric vehicles and renewable energy systems.

WO2024204581A1PCT designated stage expired Publication Date: 2024-10-03PUBLIC UNIVERSITY CORPORATION OSAKA CITY UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012733
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current lithium ion secondary batteries and all-solid-state batteries require solid electrolytes with higher ionic conductivity to enhance their performance, particularly for applications in electric vehicles and renewable energy systems, where existing materials do not fully meet the demands for both conductivity and safety.

Method used

A novel solid electrolyte material with a composition of Li3PS4(a)·Li4SnS4(b)·LiX(c) is developed, exhibiting an LGPS-like crystal phase, achieved through a method involving a mixing step, amorphization, and heat treatment, which improves ionic conductivity and stability.

Benefits of technology

The new solid electrolyte material demonstrates significantly higher ionic conductivity and stability, outperforming previous LGPS-based materials, making it suitable for advanced battery applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012733_03102024_PF_FP_ABST
    Figure JP2024012733_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a solid electrolyte material exhibiting high ion conductivity. The present invention solves said problem by providing a solid electrolyte material which has an LGPS-type crystal phase represented by (I): (Li3PS4)a(Li4SnS4)b(LiX)c (in the formula, a>0, b>0, c>0, a+b+c=1.0, 2.0≤a / b≤9.0, c / (a+b)≥0.20, and X represents Cl, Br or I).
Need to check novelty before this filing date? Find Prior Art

Description

Solid electrolyte material, solid electrolyte composite, electrode, and method for producing solid electrolyte material

[0001] The present invention relates to a solid electrolyte material, a solid electrolyte composite containing the solid electrolyte material, an electrode containing the solid electrolyte material, and a method for producing the solid electrolyte material.

[0002] In recent years, there has been an increasing demand for lithium-ion secondary batteries to store power in automobiles such as electric vehicles and hybrid vehicles, and in power generation devices such as solar cells and wind power generators. Furthermore, from the perspective of ensuring safety, active research has been conducted into all-solid-state batteries that use solid electrolytes instead of liquid electrolytes in the electrolyte layer. Further improvements in the performance of these lithium-ion secondary batteries and all-solid-state batteries are being sought.

[0003] In order to improve the physical properties of all-solid-state lithium batteries, such as their discharge capacity, the solid electrolyte of the all-solid-state lithium battery is required to have a higher ionic conductivity. Therefore, various studies have been conducted. For example, Patent Document 1 discloses that a solid electrolyte having a relatively high ionic conductivity can be provided by using an LGPS-based solid electrolyte using SnS as a raw material.

[0004] International Publication No. WO2019 / 239949

[0005] In order to obtain an all-solid-state lithium battery with excellent charge / discharge capacity, it has been desired to provide a solid electrolyte that exhibits higher ionic conductivity.

[0006] The present inventors have conducted extensive research and discovered that a Li-P-Sn-SX solid electrolyte synthesized to contain a specific amount of the compound has an LGPS-like crystalline phase and exhibits excellent ionic conductivity, leading to the completion of the present invention. Thus, the present invention provides the following [Embodiment 1] to [Embodiment 13].

[0007] [Embodiment 1] (Li3PS4) a (Li4SnS4) b (LiX) c (I) A solid electrolyte material having an LGPS-like crystalline phase, represented by the formula (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, and X represents Cl, Br, or I).

[0008] [Embodiment 2] The solid electrolyte material according to [Embodiment 1], wherein X is I.

[0009] [Embodiment 3] The solid electrolyte material according to [Embodiment 1] or [Embodiment 2], wherein c / (a+b)≧0.25.

[0010] [Embodiment 4] The solid electrolyte material according to any one of [Embodiment 1] to [Embodiment 3], wherein c=0.33; 2.0≦a / b≦7.0.

[0011] [Embodiment 5] The solid electrolyte material according to any one of [Embodiments 1] to [Embodiments 3], wherein c=0.33; a / b=3; and c / (a+b)=0.5. [Embodiment 6] The LGPS-like crystalline phase is a crystalline phase having the following characteristics in an X-ray diffraction pattern using CuKα radiation: it has peaks at 2θ = 20.0° ± 0.5°, 23.5° ± 0.5°, 29.0° ± 0.5°, 41.0° ± 1.0°, and 47.0° ± 1.0°; the peak intensity of the peak at 20.0° ± 0.5° is greater than the peak intensity of the peak at 23.5° ± 0.5°; and the peak intensities of the peaks at 2θ = 20.0° ± 0.5° and 29.0° ± 0.5° are both greater than the peak intensities of the peaks at 41.0° ± 1.0° and 47.0° ± 1.0°. The solid electrolyte material according to any one of [Embodiments 1] to [Embodiments 5].

[0012] [Embodiment 7] A solid electrolyte composite comprising the solid electrolyte material according to any one of [Embodiment 1] to [Embodiment 6].

[0013] [Embodiment 8] An electrode comprising the solid electrolyte material according to any one of [Embodiment 1] to [Embodiment 6] or the solid electrolyte composite according to [Embodiment 7].

[0014] [Embodiment 9] A method for producing a semiconductor device having the following composition formula: (Li3PS4) using as raw materials a first substance containing Li and / or P, a second substance containing Sn and / or S, and a third substance containing X (X is Cl, Br, or I), the method comprising: a mixing step of selecting at least one substance from each of the first substance, the second substance, and the third substance and mixing the raw materials so as to contain all of Li, P, S, Sn, and X; an amorphization step of amorphizing the mixture obtained in the mixing step; and a heat treatment step of heat-treating the amorphous body obtained in the amorphization step. a (Li4SnS4) b (LiX) c (I) A method for producing a solid electrolyte material having an LGPS-like crystalline phase, represented by the formula (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, and X represents Cl, Br, or I.

[0015] [Embodiment 10] The method for producing a solid electrolyte material according to [Embodiment 9], wherein the amorphization step involves amorphizing the mixture using a mechanochemical method.

[0016] [Embodiment 11] The method for producing a solid electrolyte material according to [Embodiment 9] or [Embodiment 10], wherein the first substance is Li2S and P2S5, the second substance is SnS2, and the third substance is LiX.

[0017] [Embodiment 12] The method for producing a solid electrolyte material according to any one of [Embodiment 9] to [Embodiment 11], wherein X is I.

[0018] [Embodiment 13] The method for producing a solid electrolyte material according to any one of [Embodiments 9] to [Embodiments 12], wherein the heat treatment is performed at a temperature of 200 to 300°C in the heat treatment step.

[0019] According to the present invention, there is provided a novel solid electrolyte material which has an LGPS-like crystalline phase and exhibits excellent ionic conductivity.

[0020] 1 is a graph showing the X-ray diffraction patterns of the materials of Examples 1 to 4 and Reference Samples 1 and 2. 2 is a graph showing the X-ray diffraction patterns of the materials of Comparative Examples 1 to 8.

[0021] In this specification, "x to y" (x and y are specific values) means at least x and at most y, unless otherwise specified. In addition, each numerical value described includes values ​​rounded to the nearest significant digit (for example, if a numerical value is described as 100, this 100 includes 99.5 to 100.4. As another example, if a numerical value is 0.5, this 0.5 includes 0.45 to 0.54).

[0022] (Solid Electrolyte Material Having an LGPS-Like Crystal Phase) The solid electrolyte material having an LGPS-like crystal phase of the present invention (hereinafter also simply referred to as a solid electrolyte material) has the following composition formula (I) (Li3PS4) a (Li4SnS4) b (LiX) c (I) A Li-P-Sn-SX solid electrolyte material consisting of (I) (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, X represents Cl, Br, or I).

[0023] In the above formula (I), a, b, and c are any values ​​that satisfy the following: a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; and c / (a+b)≧0.20. Among these, the lower limit of a / b is preferably 2.0 or more from the viewpoint of increasing ionic conductivity, and more preferably 2.2 or more. From the viewpoint of water resistance, the upper limit of a / b is preferably 8.5 or less, more preferably 8.2 or less, even more preferably 8.0 or less, even more preferably 7.7 or less, even more preferably 7.4 or less, even more preferably 7.2 or less, and most preferably 7.0 or less. From the viewpoints of both high ionic conductivity and water resistance, the range of a / b is, for example, preferably 2.0≦a / b≦8.5, more preferably 2.0≦a / b≦8.2, more preferably 2.0≦a / b≦8.0, more preferably 2.0≦a / b≦7.7, more preferably 2.0≦a / b≦7.4, more preferably 2.0≦a / b≦7.2, more preferably 2.0≦a / b≦7.0, and most preferably 2.2≦a / b≦7.0. Furthermore, when c=0.33, a / b is more preferably in the range of 2.0≦a / b≦7.0, and even more preferably 2.2≦a / b≦7.0. From the viewpoint of promoting crystallization, c / (a+b) is preferably c / (a+b)≧0.25, and may be c / (a+b)≧0.30 or c / (a+b)≧0.40. From the viewpoint of providing a solid electrolyte material having superior ionic conductivity, it is preferable that a / b satisfies 2.0≦a / b≦7.0 and / or c / (a+b) satisfies c / (a+b)≧0.25, it is more preferable that 2.2≦a / b≦7.0 and / or c / (a+b)≧0.30, and it is most preferable that 2.2≦a / b≦7.0 and c / (a+b)≧0.4.

[0024] In the above formula (I), as long as the inequality in the above formula (I) is satisfied, for example, the lower limit of a is preferably 0.33 or more from the viewpoint of increasing the ionic conductivity. More preferably 0.35 or more, still more preferably 0.37 or more, still more preferably 0.40 or more, still more preferably 0.42 or more, still more preferably 0.43 or more, and most preferably 0.44 or more. The upper limit is preferably 0.74 or less from the viewpoint of the stability of the electrolyte. More preferably 0.72 or less, still more preferably 0.70 or less, still more preferably 0.66 or less, still more preferably 0.65 or less, still more preferably 0.63 or less, still more preferably 0.60 or less, and most preferably 0.59 or less. The range of a is preferably, for example, 0.33 ≤ a ≤ 0.74, more preferably 0.35 ≤ a ≤ 0.72, still more preferably 0.37 ≤ a ≤ 0.70, still more preferably 0.40 ≤ a ≤ 0.70, still more preferably 0.40 ≤ a ≤ 0.66, still more preferably 0.40 ≤ a ≤ 0.65, still more preferably 0.42 ≤ a ≤ 0.62, still more preferably 0.43 ≤ a ≤ 0.60, and most preferably 0.44 ≤ a ≤ 0.59, from the viewpoints of both high ionic conductivity and stability of the electrolyte.

[0025] In the above formula (I), as long as the inequality in the above formula (I) is satisfied, for example, the lower limit of b is preferably 0.01 or more from the viewpoint of improving water resistance. More preferably 0.05 or more, still more preferably 0.08 or more. The upper limit is preferably 0.27 or less in order not to decrease the ionic conductivity. More preferably 0.25 or less, still more preferably 0.24 or less, and most preferably 0.225 or less. The range of b is preferably, for example, 0 < b ≤ 0.27, more preferably 0 < b ≤ 0.25, still more preferably 0.01 ≤ b ≤ 0.25, still more preferably 0.05 ≤ b ≤ 0.25, still more preferably 0.05 ≤ b ≤ 0.24, still more preferably 0.05 ≤ b ≤ 0.225, and most preferably 0.08 ≤ b ≤ 0.225, from the viewpoints of both improving water resistance and high ionic conductivity.

[0026] As long as the inequality in formula (I) is satisfied, the range of c in formula (I) is preferably, for example, 0.167 or more in terms of promoting amorphization. It is more preferably 0.17 or more, even more preferably 0.18 or more, even more preferably 0.19 or more, even more preferably 0.199 or more, and most preferably 0.20 or more. It is preferably less than 1.0 in terms of suppressing the generation of halogen gas. It is more preferably 0.99 or less, even more preferably 0.95 or less, even more preferably 0.90 or less, even more preferably 0.80 or less, even more preferably 0.70 or less, even more preferably 0.60 or less, even more preferably 0.50 or less, even more preferably 0.40 or less, and most preferably 0.34 or less. From the viewpoints of both promoting amorphization and suppressing the generation of halogen gas, the range of c is, for example, preferably 0.167≦c<1.0, more preferably 0.17≦c<1.0, more preferably 0.17≦c≦0.99, more preferably 0.17≦c≦0.95, more preferably 0.18≦c≦0.90, more preferably 0.19≦c≦0.80, more preferably 0.199≦c≦0.80, more preferably 0.20≦c≦0.70, more preferably 0.20≦c≦0.60, more preferably 0.20≦c≦0.50, more preferably 0.20≦c≦0.40, and most preferably 0.2≦c≦0.34.

[0027] X in the above formula (I) is selected from Cl, Br, or I. X may be one of these, or a plurality of X may be selected. Among these, X preferably contains at least I, and more preferably is I. When X is I, a solid electrolyte material with better ion conductivity can be provided.

[0028] Specific examples of the solid electrolyte material represented by the above formula (I) include Li 7.25 P 1.75 Sn 0.25 S8I[(Li3PS4) 0.583 (Li4SnS4) 0.083 (LiI) 0.333 or (Li3PS4) 7 / 12 (Li4SnS4) 1 / 12 (LiI) 4 / 12 ], Li 7.25 P1.75 Sn 0.25 S8Cl[(Li3PS4) 0.583 (Li4SnS4) 0.083 (LiCl) 0.333 or (Li3PS4) 7 / 12 (Li4SnS4) 1 / 12 (LiCl) 4 / 12 ], Li 7.25 P 1.75 Sn 0.25 S8Br[(Li3PS4) 0.583 (Li4SnS4) 0.083 (LiBr) 0.333 or (Li3PS4) 7 / 12 (Li4SnS4) 1 / 12 (LiBr) 4 / 12 ], Li 7.5 P 1.5 Sn 0.5 S8I[(Li3PS4) 0.5 (Li4SnS4) 0.167 (LiI) 0.333 or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiI) 2 / 6 ], Li 7.5 P 1.5 Sn 0.5 S8Cl[(Li3PS4) 0.5 (Li4SnS4) 0.167 (LiCl) 0.333 or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiCl) 2 / 6 ], Li 7.5 P 1.5 Sn 0.5 S8Br[(Li3PS4) 0.5 (Li4SnS4) 0.167 (LiBr) 0.333 or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiBr) 2 / 6 ], Li 23 P4Sn2S 24 I3[(Li3PS4) 0.444 (Li4SnS4) 0.222 (LiI) 0.333 or (Li3PS4) 4 / 9(Li4SnS4) 2 / 9 (LiI) 3 / 9 ], Li 23 P4Sn2S 24 Cl3[(Li3PS4) 0.444 (Li4SnS4) 0.222 (LiCl) 0.333 or (Li3PS4) 4 / 9 (Li4SnS4) 2 / 9 (LiCl) 3 / 9 ], Li 23 P4Sn2S 24 Br3[(Li3PS4) 0.444 (Li4SnS4) 0.222 (LiBr) 0.333 or (Li3PS4) 4 / 9 (Li4SnS4) 2 / 9 (LiBr) 3 / 9 ], Li 14 P3SnS 16 I[(Li3PS4) 0.6 (Li4SnS4) 0.2 (LiI) 0.2 ], Li 14 P3SnS 16 Cl[(Li3PS4) 0.6 (Li4SnS4) 0.2 (LiCl) 0.2 ], Li 14 P3SnS 16 Br[(Li3PS4) 0.6 (Li4SnS4) 0.2 (LiBr) 0.2 ] etc.

[0029] In one embodiment, the solid electrolyte material of the present invention has the following composition formula (II) (Li3PS4): a (Li4SnS4) b (LiX) 0.33(II) (wherein a>0; b>0; a+b=0.67; 2.0≦a / b≦7.0; c / (a+b)≧0.20, X represents Cl, Br, or I). This formula is equivalent to formula I with c set to 0.33 and a / b set to 2.0≦a / b≦7.0. In the above formula (II), a, b, and c are any values ​​that satisfy a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; and c / (a+b)≧0.25, and can be selected from a, b, and c in the above formula (I). X is also as described above. When the solid electrolyte material of the present invention is represented by formula (II), a solid electrolyte material with better ionic conductivity can be provided.

[0030] In one embodiment, the solid electrolyte material of the present invention has the following composition formula (III) (Li3PS4): a (Li4SnS4) b (LiI) 0.33 (III) (wherein a>0; b>0; a+b=0.67; 2.0≦a / b≦7.0; c / (a+b)≧0.20). This formula is equivalent to formula I, where c is 0.33, a / b is 2.0≦a / b≦7.0, and X is I. In formula (III), a, b, and c are any values ​​that satisfy a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; and c / (a+b)≧0.25, and can be selected from a, b, and c in formula (I) described above. When the solid electrolyte material of the present invention is represented by formula (III), a solid electrolyte material with superior ionic conductivity can be provided.

[0031] In one embodiment, the solid electrolyte material of the present invention has the following composition formula (IV) (Li3PS4): a (Li4SnS4) b (LiX) c(IV) (wherein a>0; b>0; c>0; a+b+c=1.0; 2.8≦a / b≦3.2; 0.48≦c / (a+b)≦0.52, and X represents Cl, Br, or I). In the above formula (IV), a, b, and c are any values ​​that satisfy a>0; b>0; c>0; a+b+c=1.0; 2.8≦a / b≦3.2; and 0.48≦c / (a+b)≦0.52, and can be selected from a, b, and c in the above formula (I). X is also as described above. When the solid electrolyte material of the present invention is represented by formula (IV), a solid electrolyte material with better ion conductivity can be provided. Specific solid electrolyte materials represented by formula (V) include, for example, (Li3PS4) 0.5 (Li4SnS4) 0.167 (LiX) 0.333 [or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiX) 2 / 6 When the solid electrolyte material of the present invention is represented by formula (IV), a solid electrolyte material with even more excellent ion conductivity can be provided.

[0032] In one embodiment, the solid electrolyte material of the present invention has the following composition formula (V) (Li3PS4): a (Li4SnS4) b (LiI) c (V) (wherein a>0; b>0; c>0; a+b+c=1.0; 2.8≦a / b≦3.2; 0.48≦c / (a+b)≦0.52). In the above formula (IV), a, b, and c are any values ​​that satisfy a>0; b>0; c>0; a+b+c=1.0; 2.8≦a / b≦3.2; 0.48≦c / (a+b)≦0.52, and can be selected from a, b, and c in the above formula (I). Specific examples of solid electrolyte materials represented by formula (V) include (Li3PS4) 0.5 (Li4SnS4) 0.167 (LiI) 0.333 [or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiI) 2 / 6When the solid electrolyte material of the present invention is represented by formula (V), a solid electrolyte material with better ion conductivity can be provided.

[0033] The raw materials for the solid electrolyte material represented by the above formulas (I) to (V) [and formula (VI) described later] are not particularly limited as long as they can form the solid electrolyte material represented by the above formulas (I) to (V) [and formula (VI)] described later, and examples thereof include Li, S, P, Cl, Br, I, Li2S, LiCl, LiBr, LiI, P2S5, SnS2, Li3PS4, and Li4SnS4. Of these raw materials, it is preferable to select at least one from each of a first substance containing Li and / or P, a second substance containing Sn and / or S, and a third substance containing X (X is Cl, Br, or I), and select a substance so as to contain all of Li, P, S, Sn, and X.

[0034] The solid electrolyte materials represented by the above formulas (I) to (V) [and formula (VI) described below] have an LGPS-like crystalline phase. The LGPS-like crystalline phase can be confirmed by the following characteristics in an X-ray diffraction pattern using CuKα radiation: Characteristic peaks at 2θ = 20.0° ± 0.5°, 23.5° ± 0.5°, 29.0° ± 0.5°, 41.0° ± 1.0°, and 47.0° ± 1.0°. The peak intensity of the peak at 20.0° ± 0.5° is greater than the peak intensity of the peak at 23.5° ± 0.5°. The peak intensities of the peaks at 2θ = 20.0° ± 0.5° and 29.0° ± 0.5° are both greater than the peak intensities of the peaks at 41.0° ± 1.0° and 47.0° ± 1.0°.

[0035] The peak at 2θ = 20.0° ± 0.5° may be one peak or two peaks, but preferably one peak. The two peaks may partially overlap. Note that when two peaks are included at 2θ = 20.0° ± 0.5°, it is sufficient that the peak intensity of at least one of the two peaks is greater than the peak intensity of the peak at 23.5° ± 0.5°.

[0036] The peak intensities of the peaks at 2θ = 20.0° ± 0.5°, 23.5° ± 0.5°, and 29.0° ± 0.5° are greater than the peak intensities of the peaks at 20.0° ± 0.5°, 23.5° ± 0.5°, and 29.0° ± 0.5°, respectively. Note that the peak intensities here refer to the intensity of the peaks relative to the baseline, and the baseline of the X-ray diffraction pattern can be calculated using commercially available analysis software (e.g., SmartLab Studio II, manufactured by Rigaku Corporation).

[0037] The solid electrolyte of the present invention has a crystalline structure similar to that of previously known LGPS-based solid electrolytes, but the X-ray diffraction pattern results differ in some respects from those of previously known LGPS-based solid electrolytes. (For example, the LGPS-based solid electrolyte described in Patent Document 1 has characteristic peaks at 2θ = 19.80° ± 0.50°, 20.10° ± 0.50°, 26.60° ± 0.50°, and 29.10° ± 0.50° in its X-ray diffraction pattern using CuKα radiation, but this X-ray diffraction pattern is slightly different from the X-ray diffraction pattern of the LGPS-like crystalline phase of the present invention.) For example, previously known LGPS solid electrolytes have two peaks observed near 2θ = 20°, but the present invention has the characteristic that these peaks overlap and appear as a single peak. Therefore, the inventors believe that in the present invention, it is possible to determine whether the solid electrolyte phase has an LGPS-like crystalline phase from the X-ray diffraction pattern by the presence or absence of X-ray peaks and the intensity of the peaks, as described above.

[0038] In one embodiment, the solid electrolyte material of the present invention may be represented by the following composition formula (VI): (Li3PS4) a (Li4SnS4) b (LiX) c(VI) (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, X represents Cl, Br, or I), and in an X-ray diffraction pattern using CuKα radiation, has peaks at at least 2θ=20.0°±0.5°, 23.5°±0.5°, 29.0°±0.5°, 41.0°±1.0°, and 47.0°±1.0°, wherein the peak intensity at 20.0°±0.5° is greater than the peak intensity at 23.5°±0.5°, and the peak intensities at 2θ=20.0°±0.5° and 29.0°±0.5° are greater than the peak intensities at 41.0°±1.0° and 47.0°±1.0°, respectively.

[0039] (Method for Producing a Solid Electrolyte Material) The present invention uses as raw materials a first substance containing Li and / or P, a second substance containing Sn and / or S, and a third substance containing X (X is Cl, Br, or I), and includes a mixing step of selecting at least one substance from each of the first substance, the second substance, and the third substance and mixing the raw materials so as to contain all of Li, P, S, Sn, and X; an amorphization step of amorphizing the mixture obtained in the mixing step; and a heat treatment step of heat-treating the amorphous body obtained in the amorphization step, the solid electrolyte material having the following composition formula: (Li3PS4) a (Li4SnS4) b (LiX) c (I) (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20; X represents Cl, Br, or I) A method for producing a solid electrolyte material having an LGPS-like crystalline phase is provided. In the formula (I), a, b, c, and X are as described above. Each step is described below.

[0040] (Mixing Step) In the mixing step, a mixture is produced by mixing a first substance, a second substance, and a third substance. The first substance, the second substance, and the third substance used in the mixing step are as described above. The mixing ratio of the first substance, the second substance, and the third substance can be appropriately adjusted to suit each combination of a, b, and c in formula (I) above. For example, when Li2S or P2S5 is selected as the first substance, SnS2 is selected as the second substance, and LiX is selected as the third substance, the first substance, the second substance, and the third substance may be selected in a molar ratio of first substance:second substance:third substance=16:1:4, 8:1:1, 8:1:2, or 12:2:3. Among these, a combination of first substance:second substance:third substance=8:1:2 is preferred, and a combination of first substance:second substance:third substance=8:1:2 and LiX being LiI is more preferred.

[0041] The first substance, the second substance, and the third substance may be subjected to a heating or drying process before being mixed. By subjecting these substances to a heating or drying process before being mixed, moisture contained in each substance can be removed.

[0042] The mixing method is not particularly limited as long as it is usable in the relevant field, and examples thereof include a method using a mortar, a V-type mixer, a sand mill, a mixer (such as a homomixer or a planetary mixer), etc. The mixing step may be carried out by mechanochemical treatment, which will be described later. In this case, the mixing step and the mechanochemical treatment step are carried out simultaneously.

[0043] The mixing time is not particularly limited, but can be, for example, in the range of 1 minute to 120 hours, preferably in the range of 10 minutes to 96 hours. The lower limit of the mixing time can be, for example, 1 minute, 5 minutes, 10 minutes, 30 minutes, 35 minutes, or 1 hour. The upper limit of the mixing time can be, for example, 120 hours, 96 hours, 85 hours, 80 hours, 72 hours, 48 ​​hours, 36 hours, or 24 hours.

[0044] (Amorphization Process) The mixture is subjected to an amorphization process to become an amorphous body. The amorphous body is composed of an amorphous phase (glass phase). The amorphous phase refers to a phase that does not exhibit clear crystallinity. The absence of clear crystallinity can be confirmed, for example, by observing no clear crystallites using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). Alternatively, the solid electrolyte material can be subjected to X-ray diffraction (XRD) using CuKα radiation, and the obtained diffraction peaks can be subjected to crystal structure analysis using the Rietveld method. Specifically, the presence of a broad peak or halo pattern due to the amorphous phase can be confirmed. Here, a broad peak refers, for example, to a full width at half maximum of 0.5 or more, more specifically, 1.0 or more.

[0045] The method for amorphizing the mixture is not particularly limited as long as it can amorphize the mixture, but examples thereof include mechanochemical treatment. Alternatively, gas phase methods such as PVD (Physical Vapor Deposition) and CVD (Chemical Vapor Deposition) and liquid phase methods can be used, with mechanochemical treatment being preferred. The mechanochemical treatment may be a wet method or a dry method.

[0046] The treatment device for mechanochemical treatment is not particularly limited as long as it can mix while applying mechanical energy, and examples that can be used include a ball mill, a bead mill, a jet mill, a vibration mill, a disk mill, a turbo mill, and a mechanofusion. A ball mill is preferred because it can generate large mechanical energy. Among ball mills, a planetary ball mill is preferred because it can efficiently generate high impact energy by rotating the pot on its axis and revolving the base in the opposite direction to the rotation.

[0047] The duration of the mechanochemical treatment is not particularly limited and can be set appropriately depending on the scale and performance of the treatment equipment and the mixture. The treatment time can be, for example, 10 minutes to 120 hours, preferably 30 minutes to 80 hours. The lower limit of the treatment time may be, for example, 10 minutes, 30 minutes, 1 hour, or 5 hours, and the upper limit may be 120 hours, 100 hours, or 80 hours. From the viewpoint of productivity, a short duration of the mechanochemical treatment is preferable as long as the objective of amorphization can be achieved. When a planetary ball mill is used for the mechanochemical treatment, the diameter of the ball is not particularly limited and may be selected, for example, from the range of 0.1 to 20 mm. The rotation speed may be selected, for example, from 150 to 600 revolutions per minute. The output power is also not particularly limited and may be selected, for example, from conditions resulting in 1 to 100 kWh per kg of raw material.

[0048] (Heat Treatment Step) A solid electrolyte material having an LGPS-like crystalline phase can be obtained by heating the amorphous body obtained in the amorphization step. The solid electrolyte material having an LGPS-like crystalline phase may be a glass ceramic. Glass ceramic refers to a material having a glass phase and a crystalline phase dispersed (precipitated) in the glass phase. Glass ceramics can be formed, for example, by heating the glass phase at a temperature equal to or higher than its crystallization temperature to crystallize (at least a portion of) the material. The crystallization temperature can be measured, for example, by differential thermal analysis (DTA). The solid electrolyte material can be confirmed to be a glass ceramic by observing, for example, the presence of multiple crystalline phases in the glass phase using a TEM or SEM. Alternatively, the solid electrolyte material may be determined to be a glass ceramic when peaks not observed in the mixture before heating are observed in XRD using CuKα radiation.

[0049] The heating temperature can be set appropriately depending on the crystallization temperature of the amorphous body, but is preferably set in the range of 100°C to 500°C, more preferably in the range of 150°C to 400°C, more preferably in the range of 200°C to 300°C, more preferably in the range of 210°C to 280°C, and even more preferably in the range of 220°C to 250°C. When treated at a high temperature of 600°C or higher, the Li4PS4X phase (X is Cl, Br, or I) is preferentially formed.

[0050] The heating time is not particularly limited and can be set appropriately, but can be, for example, in the range of 1 minute to 24 hours, preferably in the range of 5 minutes to 12 hours, more preferably in the range of 30 minutes to 6 hours, and still more preferably in the range of 30 minutes to 3 hours.

[0051] Heating may be carried out once or multiple times. When heating is carried out multiple times, it is preferable that the heating temperature and heating time for each heating step are within the above-mentioned ranges.

[0052] The rate of temperature rise at the start of heating is not particularly limited and can be set appropriately, for example, within the range of 10°C / min to 1000°C / min.

[0053] The heating method is not particularly limited as long as the above-mentioned temperature rise rate can be realized. For example, an electric furnace, a hot plate, a muffle furnace, a high-frequency induction heating device, a rotary kiln, a sand bath, a salt bath, etc. can be used for heating. It is preferable that the heating device has a function of adjusting the temperature and time.

[0054] The method may include a step of cooling the heated material. The heated solid electrolyte material may be slowly cooled to room temperature, or may be rapidly cooled using any cooling device. The cooling method is not particularly limited, and cooling may be performed by natural cooling, or by slow or rapid cooling using any cooling device. Examples of cooling devices that can be used include a liquid quenching and solidification device, a quenching flake manufacturing device, a submerged spinning device, a gas atomizing device, a water atomizing device, and a rotating disk device.

[0055] Each treatment step is preferably carried out in an inert atmosphere (e.g., a nitrogen atmosphere, an argon atmosphere, a helium atmosphere, etc.). It is also preferable to carry out the treatment in an environment where the moisture concentration is 1000 ppm or less and the oxygen concentration is 1000 ppm or less. Each treatment step may be carried out under a pressure lower or higher than atmospheric pressure. Normal pressure refers to, for example, a range of 200 hPa around 1013 hPa. The pressure conditions may also be varied, such as gradually increasing the pressure, gradually decreasing the pressure, or using atmospheric pressure during heating but increasing the pressure during cooling.

[0056] (Solid Electrolyte Composite) The present invention provides a solid electrolyte composite containing a solid electrolyte material represented by any one of the above formulas (I) to (VI). In addition to the solid electrolyte material represented by any one of the above formulas (I) to (VI), the solid electrolyte composite may contain a mixture of a solid electrolyte other than the solid electrolyte material of the present invention, a binder, a conductive material, etc. The proportion of the solid electrolyte material of the present invention in the solid electrolyte composite can be, for example, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 95% by mass or more.

[0057] The binder is not particularly limited, and examples thereof include fluorine-based polymers, polyolefin-based polymers, poly(meth)acrylic polymers, polyvinyl-based polymers, polystyrene-based polymers, polyimide-based polymers, polyester-based polymers, cellulose-based polymers, and polyacrylonitrile-based polymers. Specific examples include polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polyvinyl alcohol, polyvinyl acetate, polymethyl methacrylate, polyethylene, polypropylene, styrene-butadiene rubber, acrylonitrile-butadiene rubber, polyimide, polyamide, carboxymethyl cellulose, polyacrylonitrile, and copolymers thereof. The binder may be a single type of binder or a combination of multiple binders. When mixing the solid electrolyte material of the present invention using a solvent, it is preferable to use a solvent that does not undergo side reactions with the solid electrolyte material of the present invention.

[0058] The content of the binder in the solid electrolyte composite is not particularly limited and may be appropriately selected from the range of, for example, 0 to 40% by mass, preferably 30% by mass or less, more preferably 20% by mass or less, still more preferably 10% by mass or less, and preferably 5% by mass or less.

[0059] Conductive materials are mainly classified into carbon-based conductive materials and metal-based conductive materials. Examples of carbon-based conductive materials include nanocarbon or fibrous carbon (e.g., vapor-grown carbon fiber (VGCF) or carbon nanofiber), and more specifically, natural graphite, artificial graphite, acetylene black, ketjen black, furnace black, etc. Examples of metal-based conductive materials include metals such as Cu, Ni, Al, Ag, Au, Pt, Zn, and Mn, or alloys thereof. Of these, it is preferable to use carbon-based conductive materials. The conductive material may be one type of conductive material or a combination of multiple conductive materials.

[0060] The content of the conductive material in the solid electrolyte composite is not particularly limited and may be appropriately selected from the range of, for example, 0 to 40 mass %. Of this range, it is preferably 30 mass % or less, and more preferably 20 mass % or less.

[0061] The solid electrolyte other than the solid electrolyte material represented by the above formulas (I) to (VI) contained in the solid electrolyte composite is not particularly limited, and examples thereof include sulfide-based solid electrolytes, oxide-based solid electrolytes, and halide solid electrolytes. The solid electrolyte other than the solid electrolyte material represented by the above formulas (I) to (VI) may be glass or glass ceramics.

[0062] Examples of sulfide-based solid electrolytes include Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 7-y PS 6-y Z y (Z=Cl or Br), Li6PS5I, Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiI-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S -SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-GeS2, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li7P3S 11 , Li3PS4, Li 3.25 P 0.75 S4, etc. These sulfide-based solid electrolytes may be used alone or in combination of two or more.

[0063] Examples of oxide-based solid electrolyte materials include Li2O-B2O3-P2O3, Li2O-SiO2, Li2O-P2O5, Li2O-B2O3-SiO2, and Li5La3Ta2O. 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 Si 0.6 P 0.4 O4 or Li3BO3-Li2SO4-Li2CO3, etc. These oxide-based solid electrolytes may be used alone or in combination of two or more.

[0064] Examples of halide-based solid electrolytes include Li6YCl6 and Li3YBr6. Among these, sulfide-based solid electrolytes are preferred, and Li6PS5I, Li 7-y PS 6-y Z y Argyrodite-type sulfide solid electrolytes such as (Z=Cl or Br) and Li 10 GeP2S 12 It is more preferable that the solid electrolyte is an LGPS-based sulfide solid electrolyte such as the above.

[0065] The content of the solid electrolyte other than the solid electrolyte material represented by the above formulas (I) to (VI) contained in the solid electrolyte composite is not particularly limited, but may be, for example, in the range of 0.1 to 50 mass %, more preferably 40 mass % or less, and even more preferably 30 mass % or less.

[0066] The solid electrolyte composite can be formed by mixing a solid electrolyte material represented by any of the above formulas (I) to (VI) with a solid electrolyte other than the solid electrolyte material represented by any of the above formulas (I) to (VI), a binder, a conductive material, etc. The mixing method is not particularly limited as long as it can be used in the relevant field, and for example, the methods used in the above-mentioned mixing method can be used.

[0067] The solid electrolyte composite or the solid electrolyte material represented by any one of the above formulas (I) to (VI) can be formed into a solid electrolyte layer by, for example, pressing it to a predetermined thickness. The pressing pressure can be selected from the range of, for example, 50 to 2000 MPa.

[0068] (Electrode) One embodiment of the present invention provides an electrode containing a solid electrolyte material represented by any of the above formulas (I) to (VI). The electrode may be a positive electrode or a negative electrode. The amount of the solid electrolyte material of the present invention contained in the electrode is not particularly limited, but may be, for example, in the range of 1 to 50 mass % of the electrode. The electrode may contain a positive electrode active material and a negative electrode active material commonly used in the relevant field, the above-mentioned binder, conductive material, and a solid electrolyte other than the solid electrolyte material of the present invention.

[0069] The positive electrode active material is, for example, Li4Ti5O 12 , LiCoO2, LiMnO2, LiVO2, LiCrO2, LiNiO2, Li2NiMn3O8, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Examples of the positive electrode active material include O2, FeS, Ti2S, LiFeO2, Li3V2(PO4)3, and LiMn2O4. These positive electrode active materials may be used alone or in combination of two or more.

[0070] Examples of the negative electrode active material include carbonaceous materials such as natural graphite, artificial graphite, acetylene black, ketjen black, denka black, carbon black, and VCGF; metals such as Si, Li alloys, Na alloys, Au, Pt, Pd, Ag, Al, Bi, Sn, Sb, Zn, Mg, K, Ca, and Na; and Li 4 / 3 Ti 5 / 3 Examples of the negative electrode active material include various transition metal oxides such as O4, Li3V2(PO4)3, and SnO. These negative electrode active materials may be used alone or in combination of two or more.

[0071] The electrode can be obtained in the form of a pellet or sheet by, for example, mixing an electrode active material and, optionally, a binder, a conductive material, an electrolyte, or the like, and pressing the resulting mixture.

[0072] (Electrode composite) The present invention also provides an electrode composite in which the electrode of the present invention is combined with a current collector. The current collector is not particularly limited in material, shape, etc., as long as it can be combined with the electrode of the present invention and functions as a current collector. The shape of the current collector may be a uniform alloy plate or a shape with holes. It may also be in the form of a foil, sheet, or film.

[0073] Examples of materials for the current collector include Al, Ni, Ti, Mo, Ru, Pd, stainless steel, and steel. In addition to the above materials, the current collector may be coated with Au, Al, or C. The thickness of the coating is not particularly limited, but is preferably 10 nm to 2 μm. Furthermore, it is preferable that the coating has a uniform thickness. The coating method is not particularly limited as long as it can coat the current collector. For example, it can be formed by vapor deposition on the surface using a sputter coater. The electrode composite of the present invention may be formed by combining the electrode and current collector formed separately, or the electrode may be formed directly on the current collector. When directly forming the electrode, the electrode active material may be applied to the surface of the current collector using a known method.

[0074] (All-Solid-State Secondary Battery) The present invention provides an all-solid-state secondary battery comprising the solid electrolyte composite of the present invention and / or the electrode of the present invention. The all-solid-state secondary battery may combine a solid electrolyte layer comprising the solid electrolyte composite of the present invention with a positive electrode and a negative electrode that are commonly used in the relevant field, or may combine a solid electrolyte layer comprising the solid electrolyte composite of the present invention with the electrode of the present invention, or may combine a solid electrolyte layer that is commonly used in the relevant field with the electrode of the present invention.

[0075] An all-solid-state secondary battery can be obtained, for example, by laminating a positive electrode, a solid electrolyte layer, a negative electrode, and a current collector, pressing the laminated layers together, and then fixing the laminated layers in a container. A metal layer selected from Au, Pt, In, Al, Sn, Si, or the like may be provided between the electrode and the solid electrolyte layer. The thickness of the metal layer is preferably 10 nm to 100 μm.

[0076] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following examples and comparative examples, Li2S (purity 99.9%, 200 mesh) from Mitsuwa Chemical Co., Ltd., P2S5 (purity 99.9%) from Sigma-Aldrich Co., Ltd., SnS2 (purity 99.5%) from Mitsuwa Chemical Co., Ltd., and LiI (anhydrous beads, purity 99.999%, -10 mesh) from Sigma-Aldrich Co., Ltd. were used. In the following examples and comparative examples, a Fritsch Planetary Ball Mill P-5 was used as the planetary ball mill. A Rigaku SmartLab fully automated multipurpose X-ray diffractometer was used as the X-ray diffractometer. Ionic and electronic conductivity were measured using an impedance analyzer (SI-1260) from Solartron Corporation. The differential thermal analyzer used was a TG-DTA (Termo plus EV02 TG-DTA8121) manufactured by Rigaku Corporation.

[0077] Example 1: Preparation of Li-P-Sn-SI-Based Solid Electrolyte Material 1 (Mixing Step) 3 g of LiS, P2S5, SnS2, and LiI were weighed out to a molar ratio of LiS:P2S5:SnS2:LiI = 25:7:2:8. These raw materials were weighed and placed in a zirconia pot (250 mL) in the order they were weighed, along with zirconia balls (4 mm diameter, 450 g), to obtain a mixture of LiS, P2S5, SnS2, and LiI. The operation was carried out in a glove box under an argon atmosphere, with a moisture content of -70°C or higher and an oxygen concentration of 10 ppm or less (all operations performed in the glove box hereinafter were carried out under these conditions).

[0078] (Amorphization step) The mixture obtained in the mixing step was subjected to mechanochemical treatment by a dry method using a planetary ball mill P-5 manufactured by Fritsch. The mechanochemical treatment conditions were a table rotation speed of 250 rpm and a treatment time of 80 hours. An amorphous body was obtained as a result.

[0079] (Heat Treatment Step) 0.13 g of the obtained amorphous body was placed in a rod with a diameter of 10 mm, and uniaxially pressed for 5 minutes at a pressure of 360 MPa using a hydraulic press to form pellets. The formed pellets were then heat-treated. For the heat treatment, the pellets were placed in an electric furnace under an argon atmosphere and treated at 250°C for 1 hour to obtain heat-treated pellets. The heat treatment temperature was measured using the temperature of the furnace core tube. The actual temperature of the pellets being heat-treated was within the range of the set temperature of the electric furnace to -20°C below that set temperature. This resulted in the formation of Li-P-Sn-SI-based solid electrolyte material. 7.25 P 1.75 Sn 0.25 S8I[(Li3PS4) 0.583 (Li4SnS4) 0.083 (LiI) 0.333 or (Li3PS4) 7 / 12 (Li4SnS4) 1 / 12 (LiI) 4 / 12 ] was produced and used as the material for Example 1.

[0080] Example 2: Production of Li-P-Sn-SI based solid electrolyte material 2 A Li-P-Sn-SI based solid electrolyte material, Li, was produced in the same manner as in Example 1, except that LiS, P, S, SnS, and LiI were weighed to obtain a mixture in a molar ratio of LiS:P:SnS:LiI=13:3:2:4, and 0.1277 g of the amorphous body obtained from the mixture was molded into pellets. 7.5 P 1.5 Sn 0.5 S8I[(Li3PS4) 0.5 (Li4SnS4) 0.167 (LiI) 0.333 or (Li3PS4) 3 / 6 (Li4SnS4) 1 / 6 (LiI) 2 / 6 ] was produced and used as the material for Example 2.

[0081] Example 3: Production 3 of Li-P-Sn-SI based solid electrolyte material A Li-P-Sn-SI based solid electrolyte material, Li, was produced in the same manner as in Example 1, except that LiS, P2S5, SnS2, and LiI were weighed to obtain a mixture in a molar ratio of LiS:P2S5:SnS2:LiI=10:2:2:3, and 0.1488 g of the amorphous body obtained from the mixture was molded into pellets. 23 P4Sn2S 24 I3[(Li3PS4) 0.444 (Li4SnS4) 0.222 (LiI) 0.333 or (Li3PS4) 4 / 9 (Li4SnS4) 2 / 9 (LiI) 3 / 9 The Li-P-Sn-SI solid electrolyte material was prepared in the same manner as in Example 1, except that Li2S, P2S5, SnS2, and LiI were weighed to obtain a mixture with a molar ratio of Li2S:P2S5:SnS2:LiI=13:3:2:2. 14 P3SnS 16 I[(Li3PS4) 0.6 (Li4SnS4) 0.2 (LiI) 0.2 ] was produced and used as the material for Example 4.

[0082] Comparative example 1: Li 7.25 P 1.75 Sn 0.25 Unheated Material of S8I 0.13 g of the Li-P-Sn-SI amorphous material of Example 1 was molded into a pellet, and the material of Comparative Example 1 was prepared in the same manner as in Example 1 except that it was not heated.

[0083] Comparative example 2: Li 7.5 P 1.5 Sn 0.5 Unheated Material of S8I 0.13 g of the Li-P-Sn-SI amorphous material of Example 2 was molded into a pellet, and the material of Comparative Example 2 was prepared in the same manner as in Example 1, except that it was not heated.

[0084] Comparative example 3: Li 23 P4Sn2S 24 Unheated Material for I3 0.13 g of the Li-P-Sn-SI amorphous material of Example 3 was molded into pellets, and the material for Comparative Example 3 was prepared in the same manner as in Example 1, except that it was not heated.

[0085] Comparative example 4: Li 14 P3SnS 16 Unheated Material of I 0.13 g of the Li-P-Sn-SI amorphous material of Example 1 was molded into pellets, and the material of Comparative Example 4 was prepared in the same manner as in Example 1, except that it was not heated.

[0086] Comparative Example 5: Amorphous Li8PSnS8I Amorphous Li8PSnS8I was obtained by the same processes as in the (mixing step) and (amorphization step) of Example 1, except that Li2S, P2S5, SnS2, and LiI were weighed out to a molar ratio of Li2S:P2S5:SnS2:LiI = 7:1:2:2. Pellets were molded from 0.13 g of this amorphous material to prepare the material for Comparative Example 5.

[0087] Comparative example 6: Li 8.5 P 0.5 Sn 1.5 Amorphous S8I was obtained by treating Li2S, P2S5, SnS2, and LiI in the same manner as in Example 1 (mixing step) and (amorphization step), except that Li2S, P2S5, SnS2, and LiI were weighed out in a molar ratio of Li2S:P2S5:SnS2:LiI=15:1:6:4. 8.5 P 0.5Sn 1.5 An amorphous body of S8I was obtained. 0.13 g of this amorphous body was molded into pellets to be used as the material for Comparative Example 6.

[0088] Comparative Example 7: Heat-treated material of Li8PSnS8I A pellet was molded from 0.13 g of the amorphous body of Li8PSnS8I obtained in Comparative Example 5. This pellet was treated in the same manner as in Example 1 (heat treatment step) to obtain the material of Comparative Example 7.

[0089] Comparative example 8: Li 8.5 P 0.5 Sn 1.5 Heat-treated material of S8I Li obtained in Comparative Example 5 8.5 P 0.5 Sn 1.5 A pellet was molded from 0.13 g of the amorphous body of S8I. This pellet was treated in the same manner as in Example 1 (heat treatment step) to obtain the material for Comparative Example 8.

[0090] Reference Sample 1: Li3PS4 As a reference sample, Li3PS4 was produced in the same manner as in Example 1, except that Li2S and P2S5 were weighed out to give a molar ratio of Li2S:P2S5 = 3:1, and this was used as the material for Reference Sample 1.

[0091] Reference Sample 2: Li4SnS4 As a reference sample, Li4SnS4 was produced in the same manner as in Example 1, except that Li2S and SnS2 were weighed out to have a molar ratio of Li2S:SnS2 = 1:1, and this was used as the material for Reference Sample 2.

[0092] (XRD Measurement) X-ray diffraction (XRD) measurement was carried out on each material of Examples 1 to 4, Comparative Examples 1 to 8, and Reference Samples 1 and 2. A SmartLab was used as the X-ray diffractometer, and CuKα radiation (= 1.54056 × 10 -10 m), the tube voltage was 45 kV, the tube current was 200 mA, the scanning angle 2θ = 10° to 80°, the sampling interval was 0.02°, and the scanning speed was 10° min -1Structural analysis was performed using the method described above. The measurement results are shown in Figures 1 and 2. Figure 1 shows the results for Examples 1 to 4 and Reference Samples 1 and 2, while Figure 2 shows the results for Comparative Examples 1 to 8. Figures 1 and 2 also show the X-ray diffraction patterns of the LGPS crystals. Figures 1 and 2 reveal that the materials of Examples 1 to 4 were converted to amorphous form by mechanochemical processing and then recrystallized by heating to form glass ceramics. Furthermore, Figure 1 reveals that the materials of Examples 1 to 4 have the following characteristics: - Characteristic peaks at 2θ = 20.0°±0.5°, 23.5°±0.5°, 29.0°±0.5°, 41.0°±1.0°, and 47.0°±1.0°. - The peak intensity of the peak at 20.0°±0.5° is greater than the peak intensity of the peak at 23.5°±0.5°. The peak intensities at 2θ = 20.0° ± 0.5° and 29.0° ± 0.5° are greater than those at 41.0° ± 1.0° and 47.0° ± 1.0°, respectively. The X-ray diffraction patterns of the materials in Examples 1 to 4 are similar to those of the LGPS crystals listed for reference, but have some differences in structure. For example, the peaks at 2θ = 20.0° ± 0.5°, 23.5° ± 0.5°, 29.0° ± 0.5°, 41.0° ± 1.0°, and 47.0° ± 1.0° of the materials in Examples 1 to 4 are different from those of the LGPS crystals. This indicates that the materials in Examples 1 to 4 have a crystalline phase similar to the LGPS crystal but with a different structure. These findings demonstrate that the Li-P-Sn-SI solid electrolyte materials described in Examples 1 to 4 have an LGPS-like crystalline phase.

[0093] (Measurement of Ionic Conductivity (σ)) The ionic conductivity (σ) was measured using each of the materials in Examples 1 to 4 and Comparative Examples 1 to 8. The AC impedance was measured using an impedance analyzer (SI-1260) at a measurement frequency of 0.1 Hz to 1×10 6 The impedance plot was measured at 100 Hz, with an AC amplitude of 10 mV. The intersection of the semicircle and the real axis of the obtained impedance plot was taken as the resistance R of the material, and the ionic conductivity σ was calculated using the following formula: σ = (1 / R) × (L / S) (1), where L is the pellet thickness (cm) and S is the electrode surface area (0.785 cm). 2 )

[0094] The ionic conductivity of each material in Examples 1 to 4 and Comparative Examples 1 to 8 is shown in Tables 1 and 2. Table 1 shows the results for each material in Examples 1 to 4, and Table 2 shows the results for each material in Comparative Examples 1 to 8.

[0095]

[0096]

[0097] It can be seen from Tables 1 and 2 that the solid electrolyte materials having an LGPS-like crystalline phase described in Examples 1 to 4 have excellent ionic conductivities. These ionic conductivities shown in Table 1 are significantly higher than those of previously known solid electrolytes having an LGPS-like phase. This demonstrates that the novel material of the present invention having an LGPS-like crystalline phase has extremely excellent properties as a solid electrolyte.

Claims

1. (Li3PS4) a (Li4SnS4) b (LiX) c (I) A solid electrolyte material having an LGPS-like crystal phase, represented by the formula: (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, X represents Cl, Br or I).

2. The solid electrolyte material according to claim 1, wherein X is I.

3. The solid electrolyte material according to claim 1, wherein c / (a+b) is ≧0.

25.

4. The solid electrolyte material according to claim 1, wherein c=0.33; 2.0≦a / b≦7.

0.

5. The solid electrolyte material of claim 1, wherein c=0.33; a / b=3; c / (a+b)=0.

5.

6. The solid electrolyte material according to claim 1, wherein the LGPS-like crystalline phase is a crystalline phase having the following characteristics in an X-ray diffraction pattern using CuKα radiation: having peaks at 2θ = 20.0° ± 0.5°, 23.5° ± 0.5°, 29.0° ± 0.5°, 41.0° ± 1.0°, and 47.0° ± 1.0°; the peak intensity of the peak at 20.0° ± 0.5° is greater than the peak intensity of the peak at 23.5° ± 0.5°; and the peak intensities of the peaks at 2θ = 20.0° ± 0.5° and 29.0° ± 0.5° are both greater than the peak intensities of the peaks at 41.0° ± 1.0° and 47.0° ± 1.0°.

7. A solid electrolyte composite comprising the solid electrolyte material according to any one of claims 1 to 6.

8. An electrode comprising the solid electrolyte material according to any one of claims 1 to 6.

9. A method for producing a semiconductor device having the following composition formula: (Li3PS4) comprising the steps of: a first substance containing Li and / or P; a second substance containing Sn and / or S; and a third substance containing X (X is Cl, Br, or I); a mixing step of selecting at least one substance from each of the first substance, the second substance, and the third substance, and mixing the raw materials so as to contain all of Li, P, S, Sn, and X; an amorphization step of amorphizing the mixture obtained in the mixing step; and a heat treatment step of heat treating the amorphous body obtained in the amorphization step. a (Li4SnS4) b (LiX) c (I) A method for producing a solid electrolyte material having an LGPS-like crystal phase, represented by the formula (I): (wherein a>0; b>0; c>0; a+b+c=1.0; 2.0≦a / b≦9.0; c / (a+b)≧0.20, X represents Cl, Br or I).

10. The method for producing a solid electrolyte material according to claim 9, wherein in the amorphization step, the mixture is amorphized using a mechanochemical method.

11. A method for producing a solid electrolyte material as described in claim 9, wherein the first material is Li2S and P2S5, the second material is SnS2, and the third material is LiX.

12. The method for producing a solid electrolyte material according to claim 9, wherein X is I.

13. The method for producing a solid electrolyte material according to claim 9, wherein the heat treatment is carried out at a temperature of 200 to 300° C. in the heat treatment step.

Citation Information

Patent Citations

  • LGPS-based solid electrolyte and production method

    WO2019239949A1

  • Sulfide solid electrolyte

    JP2019102263A

  • Microwave synthesis of lithium thiophosphate composite materials

    JP2020015661A

  • Method for manufacturing LGPS-based solid electrolyte

    JP2020027781A

  • Iodine-containing lithium tin sulfide and method for producing the same