Inkjet recording method
By applying ultraviolet curable ink and active energy rays to an absorbent medium at controlled temperatures, the inkjet recording method enhances film strength and environmental safety, addressing the low film strength issue in inkjet recording.
Patent Information
- Application Number
- PCT/JP2024/012747
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Inkjet recording methods using ultraviolet curable water-based inks face challenges with low coating film strength, especially when applied to absorbent media like cloth, and require pretreatment, which complicates the process and affects environmental safety.
Applying ultraviolet curable aqueous ink to an absorbent recording medium while simultaneously irradiating with active energy rays, maintaining the surface temperature of the recording medium within a specific range (35°C or higher) to promote immediate curing and prevent ink penetration, thus enhancing film strength without the need for pretreatment.
This method produces a printed coating film with sufficient strength and improved environmental safety by reducing the number of process steps and eliminating the need for pretreatment, while maintaining high-quality image formation.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Inkjet recording method
[0001] The present invention relates to an inkjet recording method.
[0002] The inkjet recording method has the advantages of being easy to achieve full color, being quiet, being able to obtain high-resolution images at low cost, being capable of high-speed printing, being able to print on curved surfaces as well as flat surfaces, being able to print on large areas easily, etc. Therefore, the inkjet recording method is not limited to personal use, and in recent years has been rapidly spreading as an inkjet printer for commercial use for signage, window films, posters, car wrapping, wallpaper, etc.
[0003] Known inkjet recording methods include those using solvent-free UV inks. While these methods offer excellent coating film strength and substrate versatility, they are environmentally and safety-intensive, resulting in thick inks due to their high viscosity and poor surface smoothness. In recent years, recording methods using UV-curable water-based inks have also been developed. While UV-curable water-based inks are environmentally and safety-intensive, they must be dried before curing, resulting in weak coating film strength. Furthermore, a pretreatment liquid must be applied before applying the ink (see, for example, Patent Documents 1 and 2). The problem of weak coating film strength is particularly pronounced when an absorbent recording medium, such as a fabric, is used as the recording medium.
[0004] JP 2022-067314 A JP 2011-218571 A
[0005] An object of the present invention is to provide an inkjet recording method using an ultraviolet-curable water-based ink, which does not require pretreatment and can increase the strength of the printed coating film.
[0006] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by simultaneously performing an inkjet application step of applying an ultraviolet-curable water-based ink to an absorbent recording medium and an actinic energy ray irradiation step, and by controlling the surface temperature of the recording surface of the absorbent recording medium during these steps within a specific range. The present invention was achieved based on this finding, and is summarized as follows.
[0007] [1] An inkjet recording method comprising: an ink application step of applying an inkjet ink containing at least a polymerizable compound, a polymerization initiator, and water to an absorbent recording medium; and an irradiation step of irradiating the absorbent recording medium with active energy rays simultaneously with the application of the inkjet ink, wherein the surface temperature of the recording surface of the absorbent recording medium is 35°C or higher at the start of the ink application step.
[0008] [2] The inkjet recording method according to [1], wherein the surface temperature of the recording surface of the absorbent recording medium is 120° C. or less.
[0009] [3] The inkjet recording method according to [2], wherein the surface temperature of the recording surface of the absorbent recording medium is 100° C. or less.
[0010] [4] The inkjet recording method according to any one of [1] to [3], wherein the absorbent recording medium is heated by a heating means at the start of the ink application step.
[0011] [5] The inkjet recording method according to [4], wherein the absorbent recording medium is heated from the side opposite to the recording surface.
[0012] [6] The inkjet recording method according to [4] or [5], wherein the heating means is a hot plate.
[0013] [7] The inkjet recording method according to any one of [1] to [6], wherein the absorbent recording medium is a fabric.
[0014] [8] The inkjet recording method according to any one of [1] to [7], wherein the inkjet ink contains 70% by mass or more of a volatile component based on the total amount of the inkjet ink.
[0015] [9] The inkjet recording method according to any one of [1] to [8], wherein the content of the water relative to the total amount of the inkjet ink is 40% by mass or more.
[0016]
[10] The inkjet recording method according to any one of [1] to [9], wherein the light source of the actinic energy rays is a light-emitting diode having an emission peak wavelength in the range of 350 to 420 nm.
[0017]
[11] The inkjet recording method according to any one of [1] to
[10] , wherein the inkjet ink contains a sensitizer and / or a surfactant.
[0018]
[12] The inkjet recording method according to any one of [1] to
[11] , wherein a pretreatment agent is not applied to the absorbent recording medium before the ink application step.
[0019]
[13] The inkjet recording method according to any one of [1] to
[12] , wherein the polymerizable compound is present in the inkjet ink as particles.
[0020]
[14] The inkjet recording method according to
[13] , wherein the particles have an average particle size of 10 nm or more and 200 nm or less.
[0021]
[15] The inkjet recording method according to any one of [1] to
[14] , wherein the polymerizable compound contains a (meth)acrylate compound.
[0022]
[16] The inkjet recording method according to any one of [1] to
[15] , wherein the inkjet ink contains a pigment.
[0023]
[17] The irradiation energy of the active energy ray is 0.1 J / cm 2 The inkjet recording method according to any one of [1] to
[16] above.
[0024]
[18] The inkjet recording method according to any one of [1] to
[17] , wherein the inkjet ink is applied to the absorbent recording medium by a shuttle system.
[0025]
[19] The inkjet recording method according to any one of [1] to
[18] , wherein the actinic energy ray irradiation method is a shuttle method.
[0026]
[20] The inkjet recording method according to any one of [1] to
[19] , wherein the inkjet ink contains a water-soluble organic solvent.
[0027]
[21] The inkjet recording method according to any one of [1] to
[20] , wherein the viscosity of the inkjet ink at 25° C. is 1 mPa·sec or more and 25 mPa·sec or less.
[0028] According to the inkjet recording method of the present invention, a printed coating film having sufficient strength can be formed without pretreatment in inkjet recording using an ultraviolet-curable water-based ink that is excellent in environmental friendliness and safety. Therefore, by reducing the number of steps in inkjet recording and improving the coating film strength, high-quality printed images can be efficiently obtained.
[0029] An embodiment of the present invention will be described below, but the present invention is not limited to this embodiment.
[0030] In the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" and "preferably smaller than Y".
[0031] The inkjet recording method of the present invention comprises an ink application step of applying an inkjet ink containing at least a polymerizable compound, a polymerization initiator, and water (hereinafter sometimes referred to as "the inkjet ink of the present invention") to an absorbent recording medium, and an irradiation step of irradiating the absorbent recording medium with active energy rays simultaneously with the application of the inkjet ink, wherein the surface temperature of the recording surface of the absorbent recording medium is 35° C. or higher at the start of the ink application step. Hereinafter, irradiation of active energy rays simultaneously with the application of ink will sometimes be referred to as "simultaneous irradiation."
[0032] The inkjet recording method of the present invention may further include other steps as necessary. For example, it may further include a drying step of drying and removing the solvent in the inkjet ink applied to an absorbent recording medium such as a fabric. Furthermore, the inkjet recording method of the present invention may also include a pretreatment agent application step of applying a pretreatment agent to the recording medium before the ink application step. However, it is preferable that the inkjet recording method of the present invention does not include the pretreatment agent application step. That is, in the present invention, by performing simultaneous irradiation, a printed coating film having sufficient strength can be formed without performing the pretreatment agent application step before the ink application step. Therefore, the ability to omit the pretreatment agent application step is one of the features of the present invention.
[0033] [Mechanism] The mechanism by which the ink jet recording method of the present invention, which employs simultaneous irradiation, can increase the strength of the printed coating film is believed to be as follows.
[0034] In the conventional method, when an inkjet ink is applied to an absorbent recording medium such as fabric and then irradiated with active energy rays, the ink penetrates the absorbent recording medium before being irradiated with active energy rays, and the curing components in the ink (polymerizable compound and polymerization initiator) separate, preventing the curing reaction from proceeding sufficiently even when irradiated with active energy rays, resulting in a printed coating film that does not have sufficient strength.
[0035] In the inkjet recording method of the present invention, the ink is applied with active energy rays simultaneously, which immediately promotes the ink curing reaction. The heat from the curing reaction facilitates the volatilization of the ink solvent, resulting in increased viscosity and reduced penetration of the ink into the absorbent recording medium. Furthermore, during this simultaneous irradiation, by setting the surface temperature of the recording surface of the absorbent recording medium to 35°C or higher at the start of the ink application process, the ink curing reaction and the volatilization of the ink solvent are promoted, thereby more effectively suppressing penetration of the ink into the absorbent recording medium. Therefore, it is believed that the present invention can suppress separation of the curable components in the ink and increase the strength of the printed coating film. Therefore, it is believed that the present invention is particularly effective when the polymerizable compound is present in the ink as particles. Furthermore, it is believed that the above-mentioned problem caused by ink penetration into the absorbent recording medium is particularly problematic in ink systems containing a solvent (water-based inks or solvent-based inks).
[0036] [Ink Application Step] In the ink application step of the inkjet recording method of the present invention, the inkjet ink of the present invention contained in the ink set is applied onto an absorbent recording medium such as fabric from, for example, an inkjet head of an inkjet printer. The method for applying the inkjet ink of the present invention is not particularly limited as long as it is a method that can apply the inkjet ink in the desired image pattern. The inkjet method employed in the present invention is a preferred method from the viewpoints of compactness of the recording apparatus and high-speed recording.
[0037] In image formation by the inkjet method, inkjet ink is ejected onto a recording medium by applying energy to form a colored image. Although it depends on the image to be formed, the amount of ink used for image formation is usually 30 g / m. 2 For example, when printing is performed with eight passes, the amount of ink ejected per pass is one-eighth of the ink amount, i.e., 3.75 g / m 2 It will be about the following.
[0038] The inkjet method is not particularly limited, and may be any of known methods, such as a charge control method that uses electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, or an acoustic inkjet method that converts an electric signal into an acoustic beam and irradiates the ink with the acoustic beam to eject the ink using radiation pressure. The inkjet head used in the inkjet method may be either an on-demand method or a continuous method. Furthermore, there are no particular limitations on the ink nozzles used when recording using the inkjet method, and they can be appropriately selected depending on the purpose. The inkjet method also includes a method that ejects a large number of low-density inks in a small volume, known as photo inks, a method that uses multiple inks of substantially the same hue but different densities to improve image quality, and a method that uses colorless and transparent ink.
[0039] Inkjet methods include a shuttle method that uses a short serial head and performs printing by scanning the head in the width direction of the recording medium, and a line method that uses a line head in which recording elements are arranged to correspond to the entire area of one side of the recording medium.
[0040] In the line method, an image can be recorded on the entire surface of a recording medium by scanning the recording medium in a direction perpendicular to the direction in which the recording elements are arranged, eliminating the need for a transport system such as a carriage for scanning a short head. Furthermore, since complex scanning control of the carriage movement and the recording medium is not required and only the recording medium moves, a higher recording speed can be achieved compared to the shuttle method.
[0041] However, since multiple passes allow a certain amount or more of active energy rays to be irradiated even to the layer below the ink layer printed on the recording medium, it is easy to obtain a significant effect of simultaneous irradiation in the present invention, and therefore it is preferable to adopt the shuttle method in the present invention.
[0042] In the present invention, the surface temperature of the recording surface of the absorbent recording medium is set to 35° C. or higher at least at the start of the ink application process, and the temperature conditions will be described later.
[0043] [Irradiation Step] The irradiation step in the inkjet recording method of the present invention is a step carried out simultaneously with the ink application step described above, in which the absorbent recording medium onto which the inkjet ink has been applied is irradiated with active energy rays.
[0044] In the present invention, "simultaneous irradiation" means that irradiation of active energy rays is started simultaneously with the start of the inkjet ink application process, or within 10 seconds after the start of the inkjet ink application process. "Simultaneous with the start of the inkjet ink application process" more specifically means that the inkjet ink ejection operation and the active energy ray irradiation operation are performed simultaneously. For example, simultaneous irradiation in the present invention refers to a case where the inkjet recording apparatus is of a shuttle system, as described below, and has a configuration in which an inkjet head and an active energy ray irradiation unit are provided on a carriage, and the carriage is scanned while ejecting the inkjet ink and irradiating with active energy rays are performed simultaneously.
[0045] When exposed to actinic energy rays, the polymerizable compound contained in the inkjet ink of the present invention is polymerized by the action of the polymerization initiator to form a cured film of the inkjet ink, thereby more effectively improving the abrasion resistance and blocking resistance of the image.
[0046] The inkjet ink of the present invention undergoes a curing reaction when irradiated with actinic energy rays. This reaction is a reaction in which the polymerization initiator contained in the inkjet ink of the present invention decomposes upon irradiation with actinic energy rays to generate radicals, which then initiate and accelerate the polymerization reaction of the polymerizable compound, thereby curing the inkjet ink.
[0047] When the ink-jet ink is treated with a pretreatment agent containing an acidic compound, the acid supplied from the acidic compound further aggregates (fixes) the ink-jet ink during irradiation with active energy rays, thereby improving the image quality (abrasion resistance, blocking resistance, etc.). However, as described above, in the present invention, the treatment with a pretreatment agent can be omitted.
[0048] Examples of usable actinic energy rays include α-rays, γ-rays, electron beams, X-rays, ultraviolet light, visible light, infrared light, etc. As will be described later, the polymerization initiator preferably used in the inkjet ink of the present invention has high absorption, particularly for light in the ultraviolet region, and from this viewpoint, the emission peak wavelength of the actinic energy ray source to be irradiated is preferably in the range of 200 to 600 nm, more preferably in the range of 300 to 450 nm, and even more preferably in the range of 350 to 420 nm.
[0049] The emission peak wavelength may be one or more within the above wavelength range.
[0050] The irradiation energy of the active energy rays is 0.1 J / cm 2 or more, for example, 0.5 to 10 J / cm 2 When the irradiation energy is equal to or greater than the above lower limit, the polymerization reaction of the polymerizable compound can proceed smoothly, and a more excellent effect of improving the coating strength can be obtained.
[0051] Mercury lamps and gas / solid-state lasers are mainly used as sources of actinic radiation. Mercury lamps, halogen lamps, and metal halide lamps are widely known light sources used to cure UV-curable water-based inks. However, from the perspective of environmental protection, there is currently a strong demand for mercury-free devices. Replacing these light sources with GaN-based semiconductor UV-light-emitting devices would be extremely useful from both an industrial and environmental perspective. Furthermore, LEDs and laser diodes (LDs) are small, have a long lifespan, are highly efficient, and are low-cost, and are therefore expected to be light sources for photocurable inkjet printers.
[0052] In the present invention, LEDs and LDs can be used as active energy ray sources. In particular, UV-LEDs and UV-LDs can be used as ultraviolet light sources. For example, Nichia Corporation has marketed a purple LED whose main emission spectrum has wavelengths between 365 nm and 420 nm.
[0053] In the present invention, a particularly preferred active energy ray source is a UV-LED, and a UV-LED having a peak emission wavelength in the range of 350 to 420 nm is particularly preferred. In the present invention, from the viewpoints of cost and curability, it is preferred to use a light-emitting diode having a peak emission wavelength in the range of 350 to 420 nm.
[0054] For the same reason as in the ink application step, it is preferable that the irradiation method in the irradiation step carried out simultaneously with the ink application step is also carried out by the shuttle method.
[0055] In the present invention, the surface temperature of the recording surface of the absorbent recording medium is set to 35° C. or higher at least at the start of the ink application step, which is carried out simultaneously with the irradiation step. The temperature conditions are described below.
[0056] [Surface Temperature of Recording Surface at Start of Simultaneous Irradiation] In the inkjet recording method of the present invention, the surface temperature of the recording surface of the absorbent recording medium (hereinafter sometimes simply referred to as "surface temperature") is set to 35°C or higher at the start of the ink application process. If the surface temperature of the absorbent recording medium is 35°C or higher, the solvent (e.g., water, aqueous medium, etc.) in the ink applied to an absorbent recording medium such as fabric is effectively volatilized and removed, thereby improving curing properties. From this perspective, the surface temperature of the absorbent recording medium at the start of simultaneous irradiation is preferably 40°C or higher, more preferably 45°C or higher. On the other hand, the surface temperature is preferably 120°C or lower, more preferably 100°C or lower. On the other hand, the surface temperature of the absorbent recording medium at the start of simultaneous irradiation is preferably below the boiling point of the solvent contained in the ink with the largest content. Specifically, the temperature is preferably 120°C or lower, more preferably 100°C or lower. If the surface temperature is 120° C. or less, it is possible to prevent ink from drying on the surface of the ink ejection nozzle due to the influence of the surface temperature of the absorbent recording medium, thereby preventing ink ejection defects.
[0057] In order to make the surface temperature of the absorptive recording medium fall within the above range at the start of simultaneous irradiation, it is preferable to heat the absorptive recording medium with a heating means at the start of simultaneous irradiation.
[0058] The heating means is not particularly limited, but examples thereof include a hot air heater and an infrared heater, and more specifically, examples thereof include a ceramic heater, a halogen heater, and a quartz tube heater. A hot plate can also be used as the heating means. A hot plate is preferred because it can maintain a uniform temperature over the recording medium.
[0059]
[0033] Heating of the absorbent recording medium by a heating means is preferably carried out from the side opposite to the recording surface of the absorbent recording medium, since this has little effect on the recording surface of the absorbent recording medium. In the inkjet recording method of the present invention, it is sufficient that the surface temperature of the absorbent recording medium is 35°C or higher at the start of the ink application step of simultaneous irradiation, i.e., at the start of application of inkjet ink to the absorbent recording medium, but the above surface temperature may also be achieved before or after application of the inkjet ink to the absorbent recording medium, i.e., before or after simultaneous irradiation, and it is preferable to maintain the above surface temperature throughout all processes before, during, and after application.
[0060] [Recording Medium] In the inkjet recording method of the present invention, an absorbent recording medium is used as the recording medium. In the present invention, the absorbent recording medium refers to a recording medium having a surface with high ink absorption. More quantitatively, in the Bristow method, the ink is absorbed within 30 msec from the start of contact. 1/2 Water absorption up to 0.3g / m 2 On the other hand, a recording medium having a water absorption capacity of 0.3 g / m or more is called an absorbent recording medium. 2 The smaller recording medium is a non-absorbent recording medium.
[0061] Examples of the absorbent recording medium include paper, fabric, nonwoven fabric, leather, wood, and composite materials thereof. Among the absorbent recording media, fabric is preferred because it can provide a significant effect of simultaneous irradiation according to the present invention.
[0062] The material constituting the fabric is not particularly limited, and examples thereof include natural fibers such as cotton, linen, wool, and silk; synthetic fibers such as polypropylene, polyester, acetate, triacetate, polyamide, and polyurethane; and biodegradable fibers such as polylactic acid. The material constituting the fabric may be a blend of these fibers. Of these, cotton and polyester are preferred, and cotton is more preferred.
[0063] On the other hand, examples of non-absorbent recording media include plastic materials such as polyesters such as polyethylene terephthalate (PET), polyolefins such as polyvinyl chloride (PVC), polyethylene (PE), and polypropylene (PP), glass, ceramics, metals, and composites of these. As will be shown in the comparative examples and reference examples described later, the effects of simultaneous irradiation according to the present invention cannot be obtained with non-absorbent recording media.
[0064] [Inkjet Recording Apparatus] The inkjet recording apparatus for carrying out the inkjet recording method of the present invention may be any of various recording apparatuses using an inkjet recording system. For example, the inkjet recording method of the present invention can be suitably used in printers, facsimile machines, copying machines, printer / fax / copier combination machines, three-dimensional modeling apparatuses, etc.
[0065] In the present invention, a recording device is a device capable of ejecting ink, various treatment liquids, etc. onto a recording medium. This recording device may include not only a head portion that ejects ink, but also means related to feeding, transporting, and discharging the recording medium, as well as other devices called pre-processing devices and post-processing devices.
[0066] The recording apparatus may have a heating means or drying means for heating the absorptive recording medium, and an irradiation means for irradiating the absorptive recording medium with active energy rays. The heating means and drying means include, for example, means for heating and drying the printing surface and back surface of the recording medium.
[0067] As described above, examples of the irradiation means for irradiating the active energy rays include means using a light source such as a halogen lamp, a metal halide lamp, an LED lamp, etc. The light source for curing the ink irradiates the ink with active energy rays from the side of the head to cure the ink, thereby forming a printed image.
[0068] The recording device is not limited to a device that visualizes meaningful images such as letters and figures using ink. For example, it also includes a device that forms patterns such as geometric designs and a device that creates three-dimensional images.
[0069] Recording devices include not only desktop types, but also wide-width recording devices that can print on A0-sized recording media, and continuous feed printers that can use continuous paper wound into a roll as the recording medium.
[0070] Unless otherwise specified, the recording method or active energy ray irradiation method of the recording device includes both a shuttle method in which recording or irradiation is performed while moving a serial head, and a line method in which recording is performed using a line head. For shuttle-type recording devices, see, for example, JP 2022-181182 A and JP 2010-280828 A. Among these, the recording method or active energy ray irradiation method of the recording device is preferably the shuttle method, since, as described above, the remarkable effect of simultaneous irradiation according to the present invention can be obtained. More specifically, it is preferable that the carriage is configured to include an inkjet head and an active energy ray irradiation unit.
[0071] [Inkjet Ink] The inkjet ink of the present invention contains at least a polymerizable compound, a polymerization initiator, and water. That is, in the inkjet recording method of the present invention, an ultraviolet-curable water-based ink can be used.
[0072] [Polymerizable Compound] The polymerizable compound contained in the inkjet ink of the present invention is not particularly limited as long as it is a compound having polymerizability, and known polymerizable monomers, polymerizable resins, polymerizable oligomers, etc. Among these, polymerizable oligomers are preferred, and ultraviolet-curable oligomers are more preferred.
[0073] Specific examples of polymerizable compounds include (meth)acrylamide compounds, (meth)acrylate compounds, vinyl compounds, maleimide compounds, vinyl sulfone compounds, N-vinylamide compounds, and derivatives thereof. These compounds are more preferably bifunctional or higher. The polymerizable compounds are more preferably (meth)acrylamide compounds, (meth)acrylate compounds, and vinyl compounds, and particularly preferably bifunctional or higher (meth)acrylamide compounds. In the present invention, "(meth)acrylate" means acrylate or methacrylate. The same applies to "(meth)acryloyl" and "(meth)acryl."
[0074] These polymerizable compounds may be used alone or in combination of two or more. When two or more types are used in combination, it is preferable to use a mixture of two or more types selected from (meth)acrylamide compounds, (meth)acrylate compounds, vinyl compounds, maleimide compounds, vinyl sulfone compounds, and N-vinylamide compounds, and it is more preferable that at least one of them is a (meth)acrylamide compound.
[0075] The polymerizable compound may have a poly(ethyleneoxy) chain, a poly(propyleneoxy) chain, an ionic group (such as a carboxyl group or a sulfo group), a hydroxyl group, or the like in the molecule in order to improve water solubility.
[0076] As the (meth)acrylate compound, either a monofunctional (meth)acrylate compound (a compound having one (meth)acryloyl group) or a polyfunctional (meth)acrylate compound can be used, and polyfunctional (meth)acrylate compounds are preferred.
[0077] The ultraviolet-curable oligomer is not particularly limited as to whether it is ionic or not, and may be nonionic or ionic (anionic, cationic, or amphoteric). Here, "nonionic" means, for example, that the hydrophilic group of the ultraviolet-curable oligomer is composed of an ether bond or a hydroxyl group that does not ionically dissociate in water. "Ionic" (anionic, cationic, or amphoteric) means, for example, that the ultraviolet-curable oligomer has a carboxyl group or an amino group that can ionically dissociate in water.
[0078] The ultraviolet-curable oligomer is preferably any one of the following <1> to <3>.
[0079] <1> Having a structural unit derived from a compound represented by the following formula (1):
[0080]
[0081] (In formula (1), X is an alkylene group, Y is a (meth)acryloyl group, an allyl group, an acyl group, or a hydrogen atom, and n is an integer of 2 or more.)
[0082] <2> A compound having a structural unit derived from a polyisocyanate compound (A), wherein the compound (A) has three or more isocyanate groups in one molecule.
[0083] <3> A compound having a structural unit derived from the polyisocyanate compound (A), a structural unit derived from the compound (B') shown below, and a structural unit derived from the compound (C') shown below.
[0084] The ultraviolet-curable oligomer <3> is usually produced by reacting a polyisocyanate compound (A), a compound (B') and a compound (C').
[0085] Compound (B'): A compound containing two or more polymerizable unsaturated bonds and capable of bonding with the polyisocyanate compound (A). Compound (C'): A water-soluble compound capable of bonding with the polyisocyanate compound (A).
[0086] The ultraviolet-curable oligomer preferably contains a structural unit derived from a (meth)acrylate, particularly a structural unit derived from a polyfunctional (meth)acrylate. Furthermore, a structural unit derived from a polyfunctional (meth)acrylate and a structural unit derived from a polyalkylene glycol are preferred. That is, from the viewpoint of reactivity, the compound (B') is preferably a hydroxyl group-containing polyfunctional (meth)acrylate (B). From the viewpoint of water dispersibility, the compound (C') is preferably a polyalkylene glycol (C). Such an ultraviolet-curable oligomer is usually produced by reacting a polyisocyanate compound (A), a hydroxyl group-containing polyfunctional (meth)acrylate (B), and a polyalkylene glycol (C).
[0087] In the present invention, the term "structural unit derived from X" refers to a structural unit that is incorporated into the molecular structure of an ultraviolet-curable oligomer by using compound X as a raw material and reacting compound X with another compound. The "structural unit derived from X" is not necessarily limited to using compound X as a raw material. In other words, even if the structural unit is formed from a raw material other than X, it is considered to be an "structural unit derived from X" as long as the chemical structure is the same.
[0088] As described above, a preferred embodiment of the compound (B') is the hydroxyl group-containing polyfunctional (meth)acrylate (B). A preferred embodiment of the compound (B') may be "a compound (B") containing a hydroxyl group and two or more polymerizable unsaturated bonds."
[0089] The "compound capable of bonding to the polyisocyanate compound (A)" in the compound (B') may be a compound in which the hydroxyl group of the compound (B") is substituted with a carboxy group, an amino group, or the like. Examples of the polymerizable unsaturated bond include a carbon-carbon double bond and a carbon-carbon triple bond, and among these, a carbon-carbon double bond is preferable. More specific examples of the polymerizable unsaturated bond include carbon-carbon double bonds derived from a vinyl group, a (meth)acryloyl group, or the like.
[0090] The water-soluble compound in compound (C') includes a water-soluble polymer, and specific examples thereof include polyglycerin, polyhydroxy(meth)acrylate, polyamine, quaternary aminated polystyrene, sulfonated polystyrene, polyether, polyalkylene glycol, etc. Among these, nonionic water-soluble compounds such as polyglycerin, polyhydroxy(meth)acrylate, and polyalkylene glycol are preferred, with polyalkylene glycol being particularly preferred. Each of these water-soluble compounds may be a copolymer. Compound (C') has the structure of such a water-soluble compound and the structure of a "compound capable of bonding to polyisocyanate compound (A)." Here, the structure of the "compound capable of bonding to polyisocyanate compound (A)" can be selected from structures similar to those exemplified for compound (B') above.
[0091] The structural unit derived from the polyisocyanate compound (A) forms a urethane bond by bonding with the structural unit derived from the hydroxyl group-containing polyfunctional (meth)acrylate (B) and the structural unit derived from the polyalkylene glycol (C). This urethane bond may be substituted with a urea bond or an amide bond.
[0092] In the present invention, when the hydroxyl group-containing polyfunctional (meth)acrylate (B) is converted into the above-mentioned compound (B') or compound (B"), or when the polyalkylene glycol (C) is converted into the above-mentioned compound (C'), the preferred embodiments or specific embodiments in such cases can be similarly applied to the embodiments or specific embodiments that are preferred in the case of using the hydroxyl group-containing polyfunctional (meth)acrylate (B) or polyalkylene glycol (C) described below.
[0093] Each compound constituting the ultraviolet-curable oligomer will be described below. In the present invention, the term "oligomer" is not limited to a specific molecular weight range, etc., and it is sufficient if it has the structure shown below. The inkjet ink may contain only one type of ultraviolet-curable oligomer, or may contain two or more types.
[0094] <Polyisocyanate Compound (A)> The polyisocyanate compound (A) is a compound having a total of two or more isocyanate groups in one molecule.
[0095] The type of polyisocyanate compound (A) is not particularly limited, and examples thereof include chain aliphatic polyisocyanates, aromatic polyisocyanates, alicyclic polyisocyanates, etc. Among these, it is preferable that the polyisocyanate compound (A) contains a polyisocyanate trimer compound from the viewpoints of weather resistance and hardness.
[0096] The chain aliphatic polyisocyanate is a compound having a chain aliphatic structure and two or more isocyanate groups. The chain aliphatic polyisocyanate is preferred from the viewpoints of weather resistance and stretchability. The chain aliphatic structure in the chain aliphatic polyisocyanate is not particularly limited, but is preferably a linear or branched alkylene group having 1 to 12 carbon atoms, preferably 1 to 6 carbon atoms. Examples of the chain aliphatic polyisocyanate include aliphatic diisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and dimer acid diisocyanate, as well as trimer compounds of these polyisocyanates.
[0097] Aromatic polyisocyanates are compounds having an aromatic structure and two or more isocyanate groups. Aromatic polyisocyanates are preferred from the viewpoint of coating film strength. The aromatic structure in aromatic polyisocyanates is not particularly limited, but aromatic structures having 6 to 13 carbon atoms are preferred. Examples of aromatic polyisocyanates include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, and naphthalene diisocyanate, as well as trimer compounds of these polyisocyanates.
[0098] Alicyclic polyisocyanates are compounds having an alicyclic structure and two or more isocyanate groups. The alicyclic structure in the alicyclic polyisocyanate is not particularly limited, but the carbon number thereof is usually 5 or more, preferably 6 or more, and usually 15 or less, preferably 14 or less, more preferably 13 or less. The alicyclic structure is particularly preferably a cycloalkylene group. Examples of alicyclic polyisocyanates include diisocyanates having an alicyclic structure such as bis(isocyanatomethyl)cyclohexane, cyclohexane diisocyanate, bis(isocyanatocyclohexyl)methane, and isophorone diisocyanate, as well as trimer compounds of these polyisocyanates.
[0099] The ultraviolet-curable oligomer may contain only one of these polyisocyanate compounds (A) or two or more of them in combination. As the polyisocyanate compound (A), a polyisocyanate having two or more structures selected from a chain aliphatic structure, an aromatic structure, and an alicyclic structure may also be used.
[0100] From the viewpoint of adhesion to a substrate, the polyisocyanate compound (A) preferably has 3 to 6 isocyanate groups. The polyisocyanate compound (A) is preferably a trimer obtained by trimerization of hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, phenylene diisocyanate, or the like, and particularly preferably a trimer of hexamethylene diisocyanate.
[0101] <Compound containing a polymerizable unsaturated bond> In the compound containing a polymerizable unsaturated bond, the number of polymerizable unsaturated bonds is preferably 1 or more, more preferably 2 or more, even more preferably 4 or more, and is preferably 8 or less, more preferably 6 or less. The compound containing a polymerizable unsaturated bond is preferably a compound that can bond to the polyisocyanate compound (A).
[0102] (Compound (B')) The compound (B') is a compound containing two or more polymerizable unsaturated bonds and capable of bonding to the polyisocyanate compound (A). Examples of the compound (B') include compounds having a hydroxyl group, an amino group, or a carboxy group. Examples of the compound (B') include polyfunctional vinyl monomers, polyfunctional allyl monomers, and polyfunctional (meth)acrylates. Among these, the hydroxyl group-containing polyfunctional (meth)acrylate (B) is preferred as the compound (B').
[0103] <Hydroxyl Group-Containing Polyfunctional (Meth)acrylate (B)> The hydroxyl group-containing polyfunctional (meth)acrylate (B) has one or more hydroxyl groups and two or more (meth)acryloyl groups. Specific examples include (meth)acrylic acid partial esters of polyhydric alcohols. The hydroxyl group-containing polyfunctional (meth)acrylate forms a good crosslinked structure due to the involvement of multiple (meth)acryloyl groups in the curing reaction, and can provide good physical properties such as contamination resistance and abrasion resistance.
[0104] The number of hydroxyl groups in the hydroxyl group-containing polyfunctional (meth)acrylate (B) is preferably 3 or less, more preferably 2 or less, and even more preferably 1. The number of (meth)acryloyl groups in the hydroxyl group-containing polyfunctional (meth)acrylate (B) is preferably 8 or less, and more preferably 6 or less.
[0105] Examples of the hydroxyl group-containing polyfunctional (meth)acrylate (B) include pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified dipentaerythritol penta(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, 2-hydroxy-1,3-dimethacryloxypropane, and 2-hydroxy-3-acryloyloxypropyl methacrylate.
[0106] In producing the ultraviolet-curable oligomer, these hydroxyl group-containing polyfunctional (meth)acrylates (B) may be used alone or in combination of two or more.
[0107] As the hydroxyl group-containing polyfunctional (meth)acrylate (B), those having one hydroxyl group and 3 to 5 (meth)acryloyl groups are preferred, particularly from the viewpoint of the coating film strength of the resulting cured film. For example, dipentaerythritol penta(meth)acrylate and pentaerythritol tri(meth)acrylate are preferred. Dipentaerythritol penta(meth)acrylate is particularly preferred because it forms a good crosslinked structure and increases the mechanical strength of the cured film.
[0108] <Water-soluble compound> (Compound (C')) The compound (C') is a water-soluble compound that can bond with the polyisocyanate compound (A). The compound (C') is preferably a compound containing one terminal hydroxyl group, as this provides good water dispersibility.
[0109] As mentioned above, the compound (C') may be a water-soluble polymer, and among these, polyalkylene glycol (C) is particularly preferred.
[0110] The polyalkylene glycol (C) is not limited, but preferably has a mono-substituted structure. That is, it is preferable that one of the hydroxyl groups of the glycol is substituted. The substituted structure is preferably a structure that does not bond with isocyanate. The polyalkylene glycol (C) may be a mixture of a compound having a mono-substituted structure and a compound having a non-mono-substituted structure.
[0111] The mono-substituted structure is not limited, but from the viewpoint of making the ultraviolet-curable oligomer nonionic, polyalkylene glycol mono-substituted ether is preferred, polyethylene glycol mono-substituted ether, polytrimethylene glycol mono-substituted ether or polypropylene glycol mono-substituted ether is more preferred, and polyethylene glycol mono-substituted ether is even more preferred.
[0112] The molecular weight of the polyalkylene glycol (C) (if it is not a single molecule, it means the number average molecular weight) is not limited, but is usually 100 or more, preferably 200 or more, and usually 5000 or less, preferably 2000 or less.
[0113] Among polyalkylene glycol mono-substituted ethers, polyalkylene glycol mono-substituted ethers that do not contain an ionic substituent in the ether moiety are more preferred, for example, those represented by the following formula (1):
[0114]
[0115] (In formula (1), X is an alkylene group, Y is an alkyl group, a (meth)acryloyl group, an allyl group, an acyl group, or a hydrogen atom, and n is an integer of 2 or more.)
[0116] Specific examples of the polyalkylene glycol mono-substituted ether represented by the above formula (1) include the following: Those where Y is an alkyl group: polyethylene glycol monomethyl ether, polyethylene glycol lauryl ether, polyethylene glycol cetyl ether, polyethylene glycol stearyl ether, polyethylene glycol tridecyl ether, polyethylene glycol oleyl ether, polyethylene glycol octylphenyl ether, polyoxyethylene oleyl cetyl ether, polypropylene glycol monomethyl ether, etc. Those where Y is a (meth)acryloyl group: polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, etc. Those where Y is an allyl group: polyethylene glycol monoallyl ether, polypropylene glycol monoallyl ether, poly(ethylene glycol-propylene glycol) monoallyl ether, etc. Those where Y is an acyl group: polyethylene glycol monolaurate, polypropylene glycol monolaurate, poly(ethylene glycol-propylene glycol) monolaurate, polyethylene glycol monostearate, polyethylene glycol monooleate, etc.
[0117] Among these, X in formula (1) is preferably an alkylene group having 1 to 3 carbon atoms, more preferably an ethylene group, a trimethylene group, or a propylene group. From the viewpoint of pigment dispersion stability or high-temperature storage stability, X is even more preferably an ethylene group. From the viewpoint of coating film strength, Y is preferably a (meth)acryloyl group, an allyl group, or an acyl group, more preferably an allyl group.
[0118] In formula (1), n is usually 2 or more, preferably 5 or more, more preferably 6 or more, from the viewpoint of the coating film strength of the obtained cured film, and is usually 500 or less, preferably 100 or less, more preferably 50 or less.
[0119] In producing the ultraviolet-curable oligomer, only one of these polyalkylene glycols (C) may be used, or two or more of them may be used in combination. The polyalkylene glycol (C) may be a mixture of compounds having different molecular weights (compounds having different n in formula (1)).
[0120] <Average particle size> In the inkjet ink, the polymerizable compound preferably exists as particles, more preferably as particles having an average particle size of 10 nm or more and 200 nm or less, and even more preferably as particles having an average particle size of 20 nm or more and 150 nm or less. When the average particle size of the polymerizable compound is within the above range, the dispersion stability is improved. Here, the average particle size of the polymerizable compound is, for example, the volume average particle size (D 50 )
[0121] In the examples described later, the average particle size of the polymerizable compound particles in the aqueous dispersion of the polymerizable compound is measured, and the average particle size of the polymerizable compound particles in this aqueous dispersion is almost the same as the average particle size of the polymerizable compound particles in the ink.
[0122] In the present invention, as long as the polymerizable compound exists as particles, it is included in the above-mentioned state of "existing as particles" even if there is aggregation or other substances are contained within the particles.
[0123] The average particle size of the polymerizable compound means the particle size (primary particle size) of the polymerizable compound particles.
[0124] Components other than the polymerizable compound contained in the inkjet ink of the present invention will be described below.
[0125] [Colorant] The inkjet ink used in the inkjet recording method of the present invention may contain a colorant. As the colorant used in the inkjet ink, various dyes or pigments known as colorants used in inks can be used, but from the viewpoints of irradiation with actinic energy rays and long-term storage durability of printed images, it is preferable to use a pigment.
[0126] <Dye> Dyes that can be used in the present invention are not particularly limited, and examples thereof include water-soluble dyes such as acid dyes, direct dyes, and reactive dyes, disperse dyes, etc. Among these, anionic dyes are preferred.
[0127] (Water-Soluble Dyes) Examples of water-soluble dyes include azo dyes, methine dyes, azomethine dyes, xanthene dyes, quinone dyes, phthalocyanine dyes, triphenylmethane dyes, and diphenylmethane dyes.
[0128] <Pigment> Conventional organic and inorganic pigments can be used as the pigment. Examples include azo pigments such as azo lakes, insoluble azo pigments, condensed azo pigments, and chelate azo pigments; polycyclic pigments such as phthalocyanine pigments, perylene and perylene pigments, anthraquinone pigments, quinacridone pigments, dioxandine pigments, thioindigo pigments, isoindolinone pigments, and quinophthaloni pigments; dye lakes such as basic dye lakes and acid dye lakes; organic pigments such as nitro pigments, nitroso pigments, aniline black, and daylight fluorescent pigments; and inorganic pigments such as carbon black, titanium oxide, and iron oxide pigments. Among these, anionic pigments are preferred.
[0129] These dyes and pigments may be used alone or in combination of two or more.
[0130] [Aqueous Medium] The inkjet ink of the present invention is an aqueous ink. "Aqueous ink" means an ink containing an aqueous medium. The aqueous medium is water and / or a water-soluble organic solvent. The aqueous medium used in the present invention is preferably water or a mixture of water and a water-soluble organic solvent.
[0131] Water-soluble organic solvents include those that function as moisturizing solvents to increase the moisture retention and wettability of the ink, and those that are used as aqueous media to adjust the viscosity of the ink and improve its handling and ejection properties. The two are not clearly distinguished, and water-soluble organic solvents used as moisturizing solvents also function as aqueous media.
[0132] In the present invention, the term "water-soluble organic solvent" refers to a compound that is soluble in water. The solubility of the water-soluble organic solvent in water is not limited, but a compound that can dissolve in water at any ratio is preferred. Furthermore, even if a compound is difficult to exhibit the properties of a solvent by itself (for example, a compound that is solid or has high viscosity at room temperature), the compound is included in the water-soluble organic solvent as long as it can be used as a solvent by being uniformly mixed with water.
[0133] Examples of the water-soluble organic solvent include polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds.
[0134] Specific examples of the water-soluble organic solvent include the following: ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, polyhydric alcohols such as ethanol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol; Polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol; Propylene carbonate, ethylene carbonate:
[0135] As the water-soluble organic solvent, it is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a moisturizing solvent but also provides good drying properties.
[0136] As the water-soluble organic solvent, polyol compounds having 8 or more carbon atoms and glycol ether compounds are also suitably used. Specific examples of polyol compounds having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol. Specific examples of glycol ether compounds include polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monoisobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.
[0137] These water-soluble organic solvents may be used alone or in combination of two or more.
[0138] [Polymerization initiator] The inkjet ink of the present invention contains a polymerization initiator. The polymerization initiator is a photoradical polymerization initiator that generates radicals, which are active species, by the energy of light (ultraviolet rays) received when irradiated with active energy rays, and initiates photopolymerization of the polymerizable compound. This causes the ink present on the surface of the recording medium to cure, thereby forming an image.
[0139] The polymerization initiator may be contained in the ink in a state where it is not encapsulated in the polymerizable compound, or in a state where it is encapsulated in particles of the polymerizable compound, or may be contained in both of these states.
[0140] The polymerization initiator may be a fat-soluble polymerization initiator (hereinafter may be referred to as a "fat-soluble initiator") or a water-soluble polymerization initiator (hereinafter may be referred to as a "water-soluble initiator"). Here, the term "fat-soluble initiator" refers to a polymerization initiator that is compatible with a polymerizable compound such as an ultraviolet-curable oligomer or that is soluble in an organic solvent. The term "water-soluble initiator" refers to an initiator that is soluble in water at a concentration of 1% by mass or more. The same applies to the "fat-soluble sensitizer" and "water-soluble sensitizer" described below.
[0141] The polymerization initiator used in the present invention is not limited to the following, but examples thereof include aromatic ketones, acylphosphine oxide compounds, aromatic onium salt compounds, organic peroxides, thio compounds (thioxanthone compounds, thiophenyl group-containing compounds), α-aminoalkylphenone compounds, hexaarylbiimidazole compounds, ketoxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds.
[0142] Among these, the polymerization initiator preferably contains at least one of an acylphosphine oxide compound and a thioxanthone compound. Use of such a polymerization initiator tends to improve the curability of the ink.
[0143] Examples of the fat-soluble polymerization initiator include, but are not limited to, acetophenone, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, benzophenone, 2-chlorobenzophenone, p,p'-dichlorobenzophenone, p,p'-bisdiethylaminobenzophenone, Michler's ketone, benzil, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-propyl ether, benzoin isobutyl ether, benzoin-n-butyl ether, benzyl methyl ketal, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}2-methylpropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1,2-dione, Methylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)butan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]2-morpholinopropan-1-one, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methylbenzofilformate, azobisisobutyronitrile, benzoyl peroxide, and di-tert-butyl peroxide.
[0144] Examples of the water-soluble polymerization initiator include, but are not limited to, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, sodium phenyl(2,4,6-trimethylbenzoyl)phosphinate, and 2-(3-dimethylamino-2-hydroxypropoxy)-3,4-dimethyl-9H-thioxanthone-9-one methochloride.
[0145] Examples of commercially available polymerization initiators include GENOPOL TX-2 manufactured by RAHN, and Irgacure (registered trademark) 369, Irgacure (registered trademark) 500, and Irgacure (registered trademark) 2959 manufactured by BASF Japan Ltd.
[0146] The polymerization initiator may be used alone or in combination of two or more. For example, a fat-soluble initiator and a water-soluble initiator may be used in combination, the fat-soluble initiator may be encapsulated in particles of a polymerizable compound such as an ultraviolet-curable oligomer, and the water-soluble initiator may be dissolved in an aqueous medium.
[0147] As the polymerization initiator, in addition to the above-mentioned photoradical polymerization initiator, a thermal radical polymerization initiator may be used in combination.
[0148] [Surfactant] The inkjet ink of the present invention preferably contains a surfactant in order to improve the flatness of the coating film formed and the wettability with the substrate.
[0149] As the surfactant, any of silicone surfactants, fluorine surfactants, amphoteric surfactants, nonionic surfactants and anionic surfactants can be used.
[0150] The silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. Among them, those that do not decompose even at high pH are preferred, and examples thereof include side-chain modified polydimethylsiloxane, both-end modified polydimethylsiloxane, one-end modified polydimethylsiloxane, and both-end modified polydimethylsiloxane of the side chain. Those having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as the modifying group are particularly preferred because they exhibit good properties as aqueous surfactants. Polyether-modified silicone surfactants can also be used as the silicone surfactant. Examples of polyether-modified silicone surfactants include compounds in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane.
[0151] As the fluorine-based surfactant, a compound having 2 to 16 fluorine-substituted carbon atoms is preferred, and a compound having 4 to 16 fluorine-substituted carbon atoms is more preferred. As the fluorine-based surfactant, for example, perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate ester compounds, perfluoroalkyl alkylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain are preferred because of their low foaming properties. Examples of perfluoroalkyl sulfonic acid compounds include perfluoroalkyl sulfonic acid and perfluoroalkyl sulfonate salts. Examples of perfluoroalkyl carboxylic acid compounds include perfluoroalkyl carboxylic acids and perfluoroalkyl carboxylate salts. Examples of perfluoroalkyl phosphate ester compounds include perfluoroalkyl phosphate esters and perfluoroalkyl phosphate ester salts. Examples of perfluoroalkyl alkylene oxide adducts include perfluoroalkyl ethylene oxide adducts. Examples of polyoxyalkylene ether polymer compounds having a perfluoroalkyl ether group on the side chain include sulfate salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain, and salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain. Counter ions of the salts in these fluorine-based surfactants include Li, Na, K, NH 4 , N.H. 3 CH 2 CH 2 OH, NH 2 (CH 2 CH 2 OH) 2 , NH(CH 2 CH 2 OH) 3 etc.
[0152] Among these, polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in the side chains are more preferred because they have particularly low foaming properties, and fluorine-based surfactants represented by the following formulas (3A) and (3B) are particularly preferred.
[0153] CF 3 CF 2 (CF 2 CF 2 ) s -CH 2 CH 2 O (CH 2 CH 2 O) t H (3A) In the compound represented by formula (3A), s is preferably an integer of 0 or more and 10 or less, and t is preferably an integer of 0 or more and 40 or less, in order to impart water solubility.
[0154] C r F 2r+1 -CH 2 CH(OH)CH 2 -O-(CH 2 CH 2 O) c -Z (3B) In the compound represented by formula (3B), Z is H, C d F 2d+1 (d is an integer of 1 or more and 6 or less), CH 2 CH(OH)CH 2 -C e F 2e+1 (e is an integer of 4 or more and 6 or less), or C f H 2f+1 (f is an integer of 1 or more and 19 or less). r is an integer of 1 or more and 6 or less. c is an integer of 4 or more and 14 or less.
[0155] Commercially available fluorine-based surfactants can be used, such as Surflon (registered trademark) S-111, S-112, S-113, S-121, S-131, S-132, S-141, and S-145 (all manufactured by Asahi Glass Co., Ltd.); Fullard FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430, and FC-431 (all manufactured by Sumitomo 3M Limited); Megafac F-470, F-1405, and F-474 (all manufactured by DIC Corporation); and Zonyl TBS, FSP, FSA, FSN-100, FSN, and FSO-1. 00, FSO, FS-300, UR (all manufactured by DuPont); FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW (all manufactured by Neos Co., Ltd.), Polyfox PF-136A, PF-156A, PF-151N, PF-154, PF-159 (manufactured by Omnova), Noigen FN-1287 (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), Unidyne DSN-403N (manufactured by Daikin Industries, Ltd.), LE-604, LE-605, LE-606, LE-607 (manufactured by Kyoeisha Chemical Co., Ltd.), and the like.
[0156] Examples of amphoteric surfactants include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine.
[0157] Examples of nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, acetylene alcohol derivatives, and acetylene glycol derivatives.
[0158] Examples of anionic surfactants include polyoxyethylene alkyl ether acetates, dodecylbenzenesulfonates, laurates, and salts of polyoxyethylene alkyl ether sulfates.
[0159] These may be used alone or in combination of two or more.
[0160] As described above, the silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. Polyether-modified silicone surfactants having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modifying group are particularly preferred because they exhibit good properties as aqueous surfactants.
[0161] Such surfactants may be synthesized appropriately or commercially available products, such as those available from BYK Co., Ltd., Shin-Etsu Chemical Co., Ltd., Dow Corning Toray Silicone Co., Ltd., Nippon Emulsion Co., Ltd., and Kyoeisha Chemical Co., Ltd.
[0162] The polyether-modified silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be a surfactant represented by the following formula (2) in which a polyalkylene oxide structure is introduced into the Si moiety side chain of dimethylpolysiloxane.
[0163]
[0164] (In formula (2), p, q, a, and b represent integers. R and R′ represent hydrocarbon groups.)
[0165] Commercially available polyether-modified silicone surfactants can be used, such as KF-618, KF-642, and KF-643 (Shin-Etsu Chemical Co., Ltd.), SAG001, SAG002, SAG003, SAG005, SAG503, and SAG008 (Nissin Chemical Industry Co., Ltd.), EMALEX-SS-5602 and SS-1906EX (Nihon Emulsion Co., Ltd.), FZ-2105, FZ-2118, FZ-2154, FZ-2161, FZ-2162, FZ-2163, and FZ-2164 (Dow Corning Toray Silicone Co., Ltd.), BYK-33 and BYK-387 (BYK-Chemie Co., Ltd.), and TSF4440, TSF4452, and TSF4453 (Toshiba Silicon Co., Ltd.).
[0166] [Sensitizer] The inkjet ink of the present invention may contain a sensitizer. When a sensitizer is present in the ink together with a polymerization initiator, the sensitizer in the system absorbs actinic energy rays to become excited, and upon contact with the polymerization initiator, promotes decomposition of the polymerization initiator, thereby enabling a curing reaction with higher sensitivity.
[0167] The sensitizer may be either fat-soluble or water-soluble, similar to the polymerization initiator. If the sensitizer is fat-soluble, it can be encapsulated in particles of a polymerizable compound such as an ultraviolet-curable oligomer.
[0168] Examples of the sensitizer that can be used include aliphatic amines, amines having an aromatic group, and cyclic amine compounds such as piperidine; urea compounds such as thioxanthone compounds, alkoxyanthracene compounds, and o-tolylthiourea; sulfur compounds such as sodium diethylthiophosphate and soluble salts of aromatic sulfinic acids; nitrile compounds such as N,N'-disubstituted-p-aminobenzonitrile; phosphorus compounds such as tri-n-butylphosphine and sodium diethyldithiophosphate; Michler's ketone, N-nitrosohydroxylamine derivatives; and nitrogen compounds such as oxazolidine compounds, tetrahydro-1,3-oxazine compounds, and condensates of formaldehyde or acetaldehyde with diamines.
[0169] These sensitizers may be used alone or in combination of two or more.
[0170] [Other Resin Components] In addition to the above components, the inkjet ink of the present invention may contain, as necessary, any oligomer component other than the polymerizable compound, any resin component, or any monomer component (collectively referred to as "other resin components"). The other resin components may be encapsulated in particles of the polymerizable compound or dissolved in the aqueous medium. The other resin components may be dispersed alone in the ink or may be in a composite state with other components.
[0171] [Other Additives] In addition to the above-mentioned components, the inkjet ink of the present invention may contain other additives as needed. Examples of other additives include known additives such as anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, antifungal agents, rust inhibitors, pH adjusters, viscosity adjusters, dispersants, dispersion stabilizers, antifoaming agents, solid wetting agents, and chelating agents. These various additives may be added directly after preparing the ink, or may be added during the preparation of the ink.
[0172] For other additives, reference can be made to the descriptions in paragraphs 0088 to 0096 of JP-A No. 2010-65205 and paragraphs 0083 to 0090 of JP-A No. 2010-70669, as appropriate.
[0173] [Content of Each Component] The content of water in the inkjet ink of the present invention is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the drying property and ejection reliability of the ink, the content of water in the inkjet ink of the present invention is usually 10% by mass or more, preferably 20% by mass or more, and more preferably 40% by mass or more, and is usually 90% by mass or less, preferably 80% by mass or less.
[0174]
[0043] When the inkjet ink of the present invention contains a water-soluble organic solvent, its content (the total content of the water-soluble organic solvent that also serves as a moisturizing solvent and the water-soluble organic solvent that serves as an aqueous medium) is not particularly limited and can be appropriately selected depending on the type of water-soluble organic solvent used and the purpose. From the viewpoints of drying property, ejection reliability, wettability with the substrate, etc., the content of the water-soluble organic solvent is usually 10% by mass or more and usually 50% by mass or less, preferably 40% by mass or less.
[0175] The content of volatile components relative to the total amount of the inkjet ink of the present invention is preferably 70% by mass or more, more preferably 75% by mass or more, and preferably 95% by mass or less, and more preferably 90% by mass or less. If the content of volatile components is equal to or greater than the above lower limit, ejection reliability is high, and if it is equal to or less than the above upper limit, coating strength can be increased. The volatile components in the inkjet ink of the present invention refer to components that have decreased by 90% or more compared to before drying after 1 g of the inkjet ink is placed on an aluminum dish with a diameter of 10 cm and dried at 80°C for 4 hours.
[0176] From the viewpoint of drying properties and ejection reliability, the inkjet ink of the present invention is prepared so that the total solids concentration, which is the concentration of components other than the aqueous medium, i.e., water and / or a water-soluble organic solvent, is usually 5% by mass or more, preferably 7% by mass or more, more preferably 9% by mass or more, and usually 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less.
[0177] When a mixture of water and a water-soluble organic solvent is used as the aqueous medium, the ratio of water to the water-soluble organic solvent (the total of the water-soluble organic solvent that also serves as a moisturizing solvent and the water-soluble organic solvent used as the aqueous medium) is preferably such that the ratio of water to water-soluble organic solvent is usually 1:0.05 to 1:1.5 (mass ratio), preferably 1:0.1 to 1:1.2 (mass ratio), and more preferably 1:0.15 to 1:1.1 (mass ratio), from the viewpoint of improving drying properties and ejection properties.
[0178]
[0044] The content of the polymerizable compound in the inkjet ink of the present invention is usually 3% by mass or more, preferably 5% by mass or more, and more preferably 7% by mass or more, from the viewpoint of the performance of the resulting printed coating film and actinic energy ray curability. On the other hand, from the viewpoint of ejection stability, the content of the polymerizable compound in the inkjet ink of the present invention is usually 20% by mass or less, preferably 15% by mass or less, and more preferably 12% by mass or less. From the same viewpoint, the content of the polymerizable compound in the total solid content of the inkjet ink of the present invention is usually 30% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more, and is usually 90% by mass or less, preferably 85% by mass or less, and more preferably 80% by mass or less.
[0179]
[0044] From the viewpoints of improving image density, good fixability, and ejection stability, the content of the colorant in the inkjet ink of the present invention is usually 0.1% by mass or more, preferably 1% by mass or more, and usually 8% by mass or less, preferably 6% by mass or less. From the same viewpoints, the content of the colorant in the total solid content of the inkjet ink of the present invention is usually 1% by mass or more, preferably 5% by mass or more, and usually 40% by mass or less, preferably 30% by mass or less.
[0180] The content of the polymerization initiator in the inkjet ink of the present invention is usually 0.05% by mass or more, preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.4% by mass or more, and usually 8% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. Having the content of the polymerization initiator within this range sufficiently improves the curing rate and prevents residual polymerization initiator and coloration caused by the polymerization initiator. From the same perspective, the content of the polymerization initiator in the total solids content of the inkjet ink of the present invention is usually 0.5% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and usually 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less.
[0181]
[0033] When the inkjet ink of the present invention contains a surfactant, its content is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of achieving excellent wettability and ejection stability and improving image quality, the content of the surfactant in the ink is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and usually 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less. From the same viewpoint, the content of the surfactant in the total solid content of the inkjet ink of the present invention is usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and usually 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less.
[0182]
[0043] When the inkjet ink of the present invention contains a sensitizer, the content thereof is usually 0.01% by mass or more, preferably 0.03% by mass or more, more preferably 0.05% by mass or more, and usually 4% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.7% by mass or less. When the content of the sensitizer is within the above range, the effect of the sensitizer can be sufficiently obtained. From the same viewpoint, the content of the sensitizer in the total solid content of the inkjet ink of the present invention is usually 0.05% by mass or more, preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, and usually 8% by mass or less, preferably 6% by mass or less, and more preferably 5% by mass or less.
[0183] [Viscosity of Inkjet Ink] The viscosity of the inkjet ink of the present invention at 25° C. is preferably 25 mPa sec or less, more preferably 20 mPa sec or less, and even more preferably 10 mPa sec or less. The lower limit of the viscosity of the inkjet ink of the present invention at 25° C. is not particularly limited, but is preferably 1 mPa sec or more, more preferably 2 mPa sec or more, and even more preferably 5 mPa sec or more.
[0184] The viscosity of the inkjet ink can be measured using a digital viscometer DV-I+ manufactured by BROOKFIELD.
[0185] [Applications] The inkjet ink of the present invention used in the inkjet recording method of the present invention is water-based and therefore has excellent environmental and safety properties. According to the inkjet recording method of the present invention, a printed coating film with excellent coating properties can be formed using such an environmentally and safety-friendly water-based ink. Therefore, the inkjet recording method of the present invention can be suitably used for various applications such as fabrics for clothing such as T-shirts, textiles, wallpaper for interior decoration, and home furnishings.
[0186] An embodiment of the present invention will be described below, but the present invention is not limited to this embodiment.
[0187] [Ink Preparation] <Preparation of Polymerizable Compound Aqueous Dispersion> A polymerizable compound (nonionic UV-curable oligomer) was produced by reacting 0.4 mol of a hexamethylene diisocyanate trimer, 0.8 mol of dipentaerythritol pentaacrylate, and 0.4 mol of polyethylene glycol monoallyl ether (n = 30 to 40 in the above formula (1)). 2 parts by mass of an oil-soluble initiator (GENOPOL TX-2, manufactured by RAHN) were added to 20 parts by mass of the polymerizable compound. The mixture was kept at 60°C and stirred. Ion-exchanged water preheated to 60°C was added dropwise to the mixture until the solids concentration reached 20% by mass, thereby obtaining an aqueous dispersion with a solids concentration of 20% by mass. The average particle size (D 50 ) was measured using a particle size distribution analyzer, MICROTRAC WAVE II-EX150 (manufactured by Microtrac Bell Co., Ltd.) and found to be 29 nm.
[0188] <Preparation of Ink 1> Ion-exchanged water, the polymerizable compound aqueous dispersion (solids concentration 20% by mass), propylene glycol (PG) and diethylene glycol ethyl methyl ether (EM) as water-soluble organic solvents, water-soluble initiator 1, water-soluble sensitizer 1, BYK-347 manufactured by BYK Japan K.K. as a surfactant, and EMACOL SF CYAN AE2034F manufactured by Sanyo Pigment Co., Ltd. as a pigment dispersion (shown as "Cy" in Table 1), were added and mixed to obtain the composition shown in Table 1, thereby obtaining Ink 1. The viscosity of Ink 1 at 25°C was 6.5 mPa s. The water content and volatile component content in Ink 1 were 65% by mass and 85% by mass, respectively.
[0189] <Preparation of Inks 2 to 4> Inks 2 to 4 were obtained in the same manner as Ink 1, except that the following pigment dispersions were used and the type and blending ratio of the pigment dispersion and the blending ratio of the water-soluble sensitizer were changed as shown in Table 1 below. Pigment dispersion: EMACOL SF MAGENTA AG2172F manufactured by Sanyo Pigment (represented as "Ma" in Table 1) Pigment dispersion: EMACOL SF YELLOW AG2242F manufactured by Sanyo Pigment (represented as "Ye" in Table 1) Pigment dispersion: EMACOL SF BLACK AE2078F manufactured by Sanyo Pigment (represented as "Bk" in Table 1)
[0190] The viscosity, water content, and volatile component content of Inks 2 to 4 at 25°C were as follows: Ink 2: Viscosity = 7.2 mPa·s Water content = 64% by mass Volatile component content = 84% by mass Ink 3: Viscosity = 6.4 mPa·s Water content = 66% by mass Volatile component content = 86% by mass Ink 4: Viscosity = 6.2 mPa·s Water content = 65% by mass Volatile component content = 85% by mass
[0191] The content ratio of each component in Table 1 indicates the content of the component in the aqueous dispersion or solution when the component is in the form of an aqueous dispersion or solution.
[0192]
[0193] [Example 5] Ink 1 was used as the inkjet ink and cotton fabric was used as the recording medium in a commercially available shuttle-type UV inkjet printer. A hot plate was installed on the flatbed, and the recording medium was placed on the hot plate. The printing settings were as follows, and the recording medium was applied with ink 1 and simultaneously irradiated with active energy rays to obtain a printed coating film. (Printing settings) Resolution: 600 x 720 dpi Number of passes: 16 passes Image: 5 x 16.5 cm solid image
[0194] An LED with an emission peak wavelength of 385 nm was used as the active energy ray source. The illuminance, integrated light amount, and heater temperature were set as shown in Table 2. The illuminance and integrated light amount were measured using an ultraviolet integrating actinometer (H12684 manufactured by Hamamatsu Photonics KK).
[0195] Examples 6 to 8, Comparative Examples 1 to 20, Reference Examples 1 to 7 Printed coating films were obtained in the same manner as in Example 5, except that the type of ink, the type of recording medium, the illuminance and integrated light amount of the active energy rays, the timing of the active energy ray irradiation, and the heater temperature were changed as shown in Table 2. The (illuminated) PET used as the recording medium was a non-absorbent, illuminated transparent film made of surface-treated polyethylene terephthalate. The heater temperature corresponds to the surface temperature of the recording medium. Room temperature is a temperature of 20 to 30°C. In Table 2, "simultaneous with printing" indicates that simultaneous irradiation was performed according to the present invention. "After printing" indicates that the active energy ray irradiation was performed after the ink application process was completed.
[0196] [Evaluation of Coating Strength] The coating strength of the printed coating films obtained in the Examples, Comparative Examples and Reference Examples was evaluated by the following method.
[0197] <Evaluation of Coating Strength (Cotton)> For the cotton printed coatings obtained in Examples 5 to 8 and Comparative Examples 1 to 8 and 17 to 20, the substrate was scrubbed while wetting the printed coating with running water, and the change in density before and after washing was visually observed and evaluated as follows. The evaluation results are shown in Table 2. ◯: Little change in image density, no practical problem. Δ: Large change in image density, but few white spots. ×: Large change in image density and many white spots, so practical problem.
[0198] <Evaluation of Coating Strength (Illuminated PET)> The printed coating films of the illuminated PET obtained in Comparative Examples 9 to 16 and Reference Examples 1 to 7 were visually observed for color transfer to a cotton swab when the cotton swab was dipped in water and rubbed, and were evaluated as follows. The evaluation results are shown in Table 2. ◯: No color transfer occurred even when rubbed with water. ×: Color transfer occurred when rubbed with water. Or, the printed coating film peeled off.
[0199]
[0200] Table 2 demonstrates that the inkjet recording method of the present invention can produce printed images with excellent coating strength. In contrast, Comparative Examples 1 to 8, in which actinic energy rays were irradiated after ink application, and Comparative Examples 17 to 20, in which the surface temperature of the recording surface of the absorbent recording medium was less than 35°C, exhibited inferior coating strength. Comparative Examples 9 to 16, in which actinic energy rays were irradiated simultaneously with ink application to a non-absorbent recording medium such as (illuminated) PET, did not exhibit separation of the cured components due to penetration, and therefore the effect of simultaneous irradiation according to the present invention was not achieved. Reference Examples 1 to 7 demonstrate that in the case of a non-absorbent recording medium such as (illuminated) PET, the problem of reduced coating strength does not occur even when actinic energy rays are irradiated after printing. In other words, the problem of the present invention is considered to be unique to printing on an absorbent recording medium such as fabric.
[0201] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese Patent Application No. 2023-055780, filed on March 30, 2023, and is incorporated by reference in its entirety.
Claims
1. An inkjet recording method comprising: an ink application step of applying an inkjet ink containing at least a polymerizable compound, a polymerization initiator and water to an absorbent recording medium; and an irradiation step of irradiating the absorbent recording medium with active energy rays simultaneously with the application of the inkjet ink, wherein at the start of the ink application step, the surface temperature of the recording surface of the absorbent recording medium is 35°C or higher.
2. The ink-jet recording method according to claim 1, wherein the surface temperature of the recording surface of said absorbent recording medium is 120° C. or lower.
3. The ink-jet recording method according to claim 2, wherein the surface temperature of the recording surface of the absorbent recording medium is 100° C. or lower.
4. The ink-jet recording method according to claim 1 or 2, wherein the absorbent recording medium is heated by a heating means at the start of the ink application step.
5. The ink-jet recording method according to claim 4, wherein the absorbent recording medium is heated from the side opposite to the recording surface.
6. The ink-jet recording method according to claim 4, wherein the heating means is a hot plate.
7. The ink-jet recording method according to claim 1 or 2, wherein the absorbent recording medium is a fabric.
8. The inkjet recording method according to claim 1 or 2, wherein the inkjet ink contains 70% by mass or more of a volatile component based on the total amount of the inkjet ink.
9. The inkjet recording method according to claim 1 or 2, wherein the content of the water relative to the total amount of the inkjet ink is 40% by mass or more.
10. The ink-jet recording method according to claim 1 or 2, wherein the light source of the active energy rays is a light-emitting diode having an emission peak wavelength in the range of 350 to 420 nm.
11. The ink-jet recording method according to claim 1 or 2, wherein the ink-jet ink contains a sensitizer and / or a surfactant.
12. The ink jet recording method according to claim 1 or 2, wherein a pretreatment agent is not applied to the absorbent recording medium prior to the ink application step.
13. The ink-jet recording method according to claim 1 or 2, wherein the polymerizable compound is present as particles in the ink-jet ink.
14. The ink-jet recording method according to claim 13, wherein the particles have an average particle size of 10 nm or more and 200 nm or less.
15. The ink jet recording method according to claim 1 or 2, wherein the polymerizable compound includes a (meth)acrylate compound.
16. The ink-jet recording method according to claim 1 or 2, wherein the ink-jet ink contains a pigment.
17. The irradiation energy of the active energy ray is 0.1 J / cm 2 The inkjet recording method according to claim 1 or 2, 18. The ink-jet recording method according to claim 1 or 2, wherein the method for applying the ink-jet ink to the absorbent recording medium is a shuttle method.
19. The ink-jet recording method according to claim 1 or 2, wherein the active energy ray irradiation method is a shuttle method.
20. The ink-jet recording method according to claim 1 or 2, wherein the ink-jet ink contains a water-soluble organic solvent.
21. The ink-jet recording method according to claim 1 or 2, wherein the viscosity of the ink-jet ink at 25° C. is from 1 mPa·sec to 25 mPa·sec.
Citation Information
Patent Citations
Ink-jet recording liquid
JP2010065205A
Inkjet recording liquid
JP2010070669A
Ink, inkjet printer and printing method
JP2010280828A
Inkjet recording method and inkjet recording device
JP2011218571A
Process liquid, set of process liquid and ink, image forming method, and image forming apparatus
JP2022067314A