Ferrite powder

A ferrite powder with controlled composition and particle structure addresses the issue of decreasing magnetic permeability over time, ensuring stability and performance in high-frequency applications by optimizing iron, manganese, and zinc content and spinel phase characteristics.

WO2024204618A1PCT designated stage expired Publication Date: 2024-10-03POWDERTECH CO LTD

Patent Information

Application Number
PCT/JP2024/012842
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional ferrite powders used in composite materials experience a decrease in magnetic permeability over time, known as disaccommodation, which affects their stability and performance in high-frequency applications like inductors.

Method used

A ferrite powder composition with specific ranges of iron (Fe), manganese (Mn), and zinc (Zn) content, along with a spinel phase and controlled vacancy rate, is developed to maintain high magnetic permeability and low loss, featuring spherical or polyhedral particles with a step structure to enhance moldability and adhesion.

Benefits of technology

The ferrite powder exhibits excellent temporal stability of magnetic permeability, high filling properties, and low loss, making it suitable for high-frequency applications without impairing formability and fillability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012842_03102024_PF_FP_ABST
    Figure JP2024012842_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a ferrite powder having excellent stability of magnetic permeability over time while maintaining high chargeability and high magnetic permeability and low loss at high frequencies. This ferrite powder contains 56.0-63.0 mass% inclusive of iron (Fe), 7.0-3.0 mass% inclusive of manganese (Mn), and 1.0-3.0 mass% inclusive of zinc (Zn).
Need to check novelty before this filing date? Find Prior Art

Description

ferrite powder

[0001] The present invention relates to a ferrite powder.

[0002] Composite materials made of ferrite powder and resin are widely used in a variety of applications, including inductors. These composite materials are produced by kneading ferrite powder and resin together. The composite material is then molded into a sheet or other shape to form a composite (molded body). When the particles that make up the ferrite powder are close to spherical, the fluidity during molding increases, and the filling rate of the ferrite powder in the composite increases. This results in good moldability and improved magnetic properties. From this perspective, ferrite powder (particles) made of spherical or polyhedral particles have been proposed.

[0003] For example, Patent Document 1 discloses an Mn-Zn ferrite powder containing at least spherical or polyhedral ferrite particles having a spinel phase as the main phase, the ferrite particles having a stepped structure with a convex polygonal outline on the surface, and the ferrite powder has a BET specific surface area of ​​0.35 m 2 / g or more 10.00m 2 / g or less and a zinc oxide (ZnO) phase content of 0 mass % or more and 0.8 mass % or less is disclosed (claim 1 of Patent Document 1). Patent Document 1 also describes that the ferrite powder can suppress magnetic loss at high frequencies and can suppress particle shedding without impairing moldability and packability when applied to composite materials or composites (paragraph

[0024] of Patent Document 1).

[0004] International Publication No. 2022 / 209640

[0005] As described above, it has been proposed to improve the moldability and packing properties of composite materials and composite bodies by using spherical or polyhedral ferrite powder. However, the inventors have found that when conventional ferrite powder is combined with a resin and then heated and molded to produce a resin molded body (composite body), a problem occurs in which the magnetic permeability of the resin molded body gradually decreases over time (disaccommodation).

[0006] As a result of further investigations by the inventors, it was found that the time change in magnetic permeability is due to the γ-Fe oxide, which has a vacant lattice, among the ferromagnetic iron (Fe) oxides contained in ferrite. 2 O 3 It was found that the effect of γ-Fe was significant. 2 O 3 The present inventors have found that by suppressing the generation of ferrite powder and controlling the vacancy rate, it is possible to obtain a ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0007] Therefore, an object of the present invention is to provide a ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0008] The present invention includes the following aspects (1) to (4). In this specification, the expression "to" includes the numerical values ​​at both ends. In other words, "X to Y" is synonymous with "at least X and at most Y."

[0009] (1) Ferrite powder containing iron (Fe) in an amount of 56.0 mass% or more and 63.0 mass% or less, manganese (Mn) in an amount of 7.0 mass% or more and 13.0 mass% or less, and zinc (Zn) in an amount of 1.0 mass% or more and 3.0 mass% or less.

[0010] (2) The ferrite powder according to (1), wherein the ferrite powder contains spherical ferrite particles mainly composed of a spinel phase, the spinel phase has an iron (Fe) amount in excess of the stoichiometric ratio and a vacancy rate of 0 mol % or more and 90 mol % or less, and the ferrite powder has a shape factor SF-1 of 100 or more and 110 or less and a volume average particle size (D50) of 2.0 μm or more and 20 μm or less.

[0011] (3) α-iron oxide (α-Fe 2 O 3 The ferrite powder according to (1) or (2), wherein the content of (I) is 0.0 mass % or more and 3.0 mass % or less.

[0012] (4) The ferrite powder according to any one of (1) to (3) above, wherein the copper (Cu) content is 0.0 mass% or more and 0.5 mass% or less.

[0013] According to the present invention, there is provided a ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0014] 1 shows the change over time of the real part of magnetic permeability (μ') of ferrite powder (Example 1). 1 shows the change over time of the real part of magnetic permeability (μ') of ferrite powder (Example 5).

[0015] A specific embodiment of the present invention (hereinafter referred to as the "present embodiment") will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.

[0016] <<1. Ferrite Powder>> The ferrite powder of the present embodiment contains 56.0 mass% or more and 63.0 mass% or less of iron (Fe), 7.0 mass% or more and 13.0 mass% or less of manganese (Mn), and 1.0 mass% or more and 3.0 mass% or less of zinc (Zn).

[0017] Ferrite powder (hereinafter sometimes simply referred to as "powder") is composed of multiple ferrite particles (hereinafter sometimes simply referred to as "particles"). That is, ferrite powder is an aggregate of multiple ferrite particles. Furthermore, the ferrite particles that make up ferrite powder are basically independent. Therefore, ferrite powder exhibits fluidity as a whole by itself. However, as long as it exhibits fluidity as a whole, this does not exclude ferrite powders in which some particles are bonded together to form agglomerated particles (secondary particles).

[0018] The ferrite powder (particles) of this embodiment has a spinel phase as the main phase. That is, the content of the spinel phase is 50.0 mass % or more. The spinel phase is MFe 2 O 4 (where M is a metal element such as a transition metal element or a vacancy), and many of them are ferromagnetic. Therefore, ferrite powders with a spinel phase as the main phase exhibit excellent magnetic properties.

[0019] The ferrite powder of this embodiment has a composition of Mn-Zn ferrite containing iron (Fe), manganese (Mn), and zinc (Zn). Mn-Zn ferrite is generally characterized by high magnetic permeability. Therefore, when the ferrite powder is applied to elements such as inductors, it is possible to obtain excellent magnetic properties.

[0020] The iron (Fe) content of the ferrite powder is 56.0% by mass or more and 63.0% by mass or less. When the Fe content is below 56.0% by mass, the Mn content and / or Zn content become relatively high. In this case, depending on the composition ratio, the loss factor (tan δ) tends to increase from relatively low frequencies around 50 MHz. Due to the large loss, it is unsuitable for use in high-frequency applications such as inductors. The Fe content is preferably 57% by mass or more, more preferably 58% by mass or more. On the other hand, when the Fe content exceeds 63.0% by mass, the Mn content and / or Zn content become relatively low. The real part of the complex permeability (real part of permeability; μ') is low, and a high saturation magnetic flux density cannot be obtained. Therefore, it is still unsuitable for use in applications such as inductors. The Fe content is preferably 62.5% by mass or less, more preferably 62% by mass or less. The Fe content is preferably 57% by mass or more and 62.5% by mass or less, and more preferably 58% by mass or more and 62% by mass or less.

[0021] The manganese (Mn) content of the ferrite powder is 7.0% by mass or more and 13.0% by mass or less. If the Mn content is less than 7.0% by mass, the Fe content and / or Zn content will be relatively high. In this case, the real part of the magnetic permeability (μ') will be low, making it unsuitable for use in applications such as inductors. The Mn content is preferably 7.3% by mass or more, more preferably 7.5% by mass or more. On the other hand, if the Mn content exceeds 13.0% by mass, the Fe content and / or Zn content will be relatively low. Depending on the composition ratio, the loss factor (tan δ) tends to increase from relatively low frequencies around 50 MHz. Therefore, it is still unsuitable for use in high-frequency applications such as inductors. The Mn content is preferably 12% by mass or less, more preferably 11% or less. The Mn content is preferably 7.3% by mass or more and 12% by mass or less, more preferably 7.5% by mass or more and 11% by mass or less.

[0022] The zinc (Zn) content of the ferrite powder is 1.0% by mass or more and 3.0% by mass or less. If the Zn content is less than 1.0% by mass, the effect of adding Zn is less pronounced, resulting in a low magnetic permeability real part (μ'). On the other hand, if the Zn content exceeds 3.0% by mass, the loss factor (tan δ) at 50 MHz increases. Furthermore, excessive Zn content can cause fine zinc oxide (ZnO) to adhere to the surfaces of the ferrite particles constituting the ferrite powder. This is because some of the excess Zn volatilizes during the high-temperature heat treatment process (such as the thermal spraying process) during the production of the ferrite powder, and reprecipitates as fine ZnO on the surfaces of the ferrite particles. If ZnO adheres to the surfaces of the ferrite particles, the viscosity of the composition may increase rapidly when the ferrite powder and a resin are mixed and kneaded to produce a composite material, making production difficult.

[0023] The ferrite powder preferably contains iron (Fe) in an amount of 57% by mass or more and 62.5% by mass or less, manganese (Mn) in an amount of 7.3% by mass or more and 12% by mass or less, and zinc (Zn) in an amount of 1.0% by mass or more and 3.0% by mass or less, and more preferably contains iron (Fe) in an amount of 58% by mass or more and 62% by mass or less, manganese (Mn) in an amount of 7.5% by mass or more and 11% by mass or less, and zinc (Zn) in an amount of 1.0% by mass or more and 3.0% by mass or less.

[0024] Preferably, the ferrite powder contains spherical-like ferrite particles mainly composed of a spinel phase. Here, spherical-like ferrite particles include not only spherical particles but also polyhedral particles. By controlling the shape of the particles contained in the ferrite powder to be spherical (spherical, polyhedral), the moldability and packing properties of the ferrite powder can be improved. This is because the spherical-like particles can smoothly avoid contact with other particles during molding. Therefore, fluidity during molding is improved and dense packing is possible. In contrast, particles having an anisotropic or irregular shape, such as a plate or needle shape, are inferior in moldability and packing properties.

[0025] The ferrite particles constituting the ferrite powder may be partly or entirely spherical ferrite particles. However, from the viewpoint of improving moldability and packing properties, a higher proportion of spherical ferrite particles is preferable. Specifically, the proportion of spherical ferrite particles is preferably 50% by number or more.

[0026] Polyhedral particles basically have a shape in which multiple polygons are three-dimensionally combined. The polygons constituting the polyhedrons are typically triangles, squares, hexagons, octagons, decagons, or combinations thereof, reflecting the crystal structure of the ferrite particles. Examples of such polyhedrons include rhombic truncated cuboctahedrons, which are combinations of squares, hexagons, and octagons. Furthermore, the greater the number of faces a polyhedron has, the closer it is to a sphere. Therefore, polyhedral particles preferably have a shape of 10 or more, more preferably 12 or more, and even more preferably 14 or more. Furthermore, polyhedral particles typically have a shape of 100 or less, more typically 72 or less, and even more typically 24 or less.

[0027] Particles in which one or more of the lines constituting the polygon are broken, or particles in which some of the lines are curved, are also considered to be polyhedral particles, as long as they are recognizable as polyhedral when viewed as a whole. Particles in which the lines constituting the polygon are finely jagged are also considered to be polyhedral particles. Furthermore, spherical-like stepped particles may have a step structure on their surface. In this case, strictly speaking, they may not be perfectly spherical or polyhedral. However, this step structure is significantly smaller than the particle dimensions. Therefore, particles that have such a microscopic step structure but have a spherical or polyhedral shape when viewed macroscopically are considered spherical or polyhedral particles.

[0028] Preferably, the ferrite powder contains ferrite particles (spherical-like stepped particles) that have a step structure on their surface. By including particles with such a step structure, when the ferrite powder is applied to a composite material or composite, adhesion to the resin is improved and particle shedding is suppressed. While the detailed mechanism is unknown, it is speculated that the presence of the step structure increases the particle surface area, i.e., the contact area with the resin, resulting in a stronger chemical bond between the particle and the resin. It is also speculated that the interlocking of the particles and the resin at the steps of the step structure creates an anchor effect of the resin, thereby strengthening the physical bond between the particles and the resin.

[0029] The step structure has a convex polygonal outline on the ferrite particle surface. That is, when the particle is viewed from the surface, the step structure has a convex polygonal outline. In other words, the step structure is provided so that a region of the particle surface is surrounded by a combination of straight lines. By providing such a step structure, it is possible to more effectively prevent particle shedding. Here, a convex polygon is a polygon in which any interior angle is 180° or less. It can also be said to be a polygon in which a line segment connecting any two points inside or on the boundary does not extend outside. In other words, it is not a concave polygon (non-convex polygon) such as a star. The outline of the step structure is not limited as long as it is a convex polygon. However, reflecting the crystal structure of ferrite, the outline is typically a triangle, a rectangle, a hexagon, an octagon, or a decagon. Furthermore, ferrite particles may have multiple step structures on their surfaces. This can more effectively prevent particle shedding.

[0030] Preferably, the spinel phase contained in the ferrite powder has an amount of iron (Fe) in excess of the stoichiometric composition. That is, the spinel phase has a composition in which iron (Fe) is in excess of the stoichiometric composition. As described above, the spinel phase has a composition in which MFe 2 O 4(where M is a metal element such as a transition metal element or a vacancy). Therefore, in a stoichiometric composition where M is an element other than Fe, the molar ratio of the amount of Fe to the total amount of M and Fe contained in the spinel phase is 2 / 3. When the ratio of the amount of Fe is more than 2 / 3, Fe is incorporated into the M site, and the composition of the spinel phase becomes (M, Fe)Fe 2 O 4 By increasing the amount of Fe contained in the spinel phase compared to the stoichiometric composition, the loss factor (tan δ) at high frequencies can be reduced, resulting in low loss of the ferrite powder.

[0031] Preferably, the spinel phase has a vacancy rate of 0 mol % or more and 90 mol % or less. 3 O 4 (Magnetite) and γ-Fe 2 O 3 γ-Fe relative to the total mole number of (maghematite) 2 O 3の Ratio of mole number (γ-Fe 2 O 3 Number of moles / (Fe 3 O 4 Number of moles + γ-Fe 2 O 3 The vacancy rate is defined as the number of mols (mol). By suppressing the vacancy rate, it is possible to reduce the change in magnetic permeability of the ferrite powder over time. In contrast, if the vacancy rate exceeds 90 mol%, the change in magnetic permeability over time becomes significant. Therefore, when ferrite powder is used as a filler in an inductor core, the performance of the inductor changes over time. In this case, it becomes difficult to achieve the performance originally designed, which can lead to malfunctions of electronic devices.

[0032] To explain this point, as mentioned above, the iron (Fe)-excess spinel phase is (M, Fe)Fe 2 O 4 In other words, a large amount of Fe is contained in the crystals of the spinel phase, which is an oxide. 2 O 3 (hematite), γ-Fe 2 O3 (maghematite), and Fe 3 O 4 There are various forms of α-Fe, such as α-Fe (magnetite). 2 O 3 and FeO are antiferromagnetic materials and do not exhibit ferromagnetic properties. In addition, they do not have a spinel structure.

[0033] In contrast, Fe 3 O 4 (Magnetite) and γ-Fe 2 O 3 (Maghemite) is a ferromagnetic material. 3 O 4 The composition formula is Fe 3+ (Fe 2+ , Fe 3+ ) 2 O 4 can be rewritten as γ-Fe 2 O 3 The composition formula is Fe 3+ (Fe 3+ 5/6 V 1/6 ) 2 O 4 (where V is a vacancy). Therefore, they have a spinel structure. Therefore, the iron (Fe)-excess spinel phase is 3 O 4 (Magnetite) and γ-Fe 2 O 3 (maghematite) or both.

[0034] Fe with spinel structure 3 O 4 (Magnetite) has no vacancies in its crystal structure, whereas γ-Fe 2 O 3 (Maghemite) has vacancies (V). Therefore, γ-Fe 2 O 3 The ferrite powder containing γ-Fe has vacancies (V) in the spinel phase. 2 O 3 The more the amount, the more vacant lattices there are. 2 O 3The greater the amount, the greater the change in magnetic permeability over time. This is thought to be due to the interaction between the vacancies in the ferrite crystal lattice moving within the crystal lattice over time and settling into an energetically stable state (position), and the presence of the vacancies hindering the movement of the domain walls.

[0035] Therefore, γ-Fe in the spinel phase 2 O 3 By lowering the amount of vacancy, i.e., the vacancy rate, the change in magnetic permeability over time can be reduced. From the viewpoint of suppressing the change in magnetic permeability over time, a small vacancy rate is desirable. The vacancy rate is more preferably 90 mol% or less, and even more preferably 85 mol% or less. On the other hand, by increasing the vacancy rate to a certain extent, the loss factor (tan δ) can be kept low. The vacancy rate is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more. The vacancy rate is more preferably 20 mol% or more to 90 mol% or less, more preferably 30 mol% or more to 90 mol% or less, and particularly preferably 40 mol% or more to 85 mol% or less.

[0036] As mentioned above, the vacancy rate is Fe 3 O 4 and γ-Fe 2 O 3 γ-Fe relative to the total number of moles 2 O 3 The ferromagnetic Fe oxide is Fe 3 O 4 and γ-Fe 2 O 3 These two types of Fe oxides are thought to exist as non-stoichiometric compounds in the spinel. 3 O 4 , γ-Fe 2 O 3 vacancy-containing Fe oxide (γ-Fe 2 O 3 ) as an index, the spinel hollow lattice fraction can be estimated.

[0037] The vacancy rate can be determined as follows: First, the ferrite powder is subjected to chemical analysis to determine the amounts of Fe, Mn, Zn, and Cu in the powder as mass percentages (mass%). Separately, the divalent iron (Fe 2+ Furthermore, the ferrite powder is subjected to X-ray diffraction (XRD) analysis to determine the amount of α-Fe in the powder. 2 O 3 (Hematite) Calculate the amount.

[0038] Next, the atomic weight of Fe (55.85), the atomic weight of Mn (54.94), the atomic weight of Zn (65.39), the atomic weight of Cu (63.55), and α-Fe 2 O 3 Using the formula weight (159.70), the amount of Fe A, the amount of Mn B, the amount of Zn C, and the amount of Fe were converted into moles according to the following formulas (1) to (6). 2+ Amount D, α-Fe 2 O 3 Then, the excess Fe amount G (mol number) and the amount of Fe compounds with vacancies (γ-Fe) are calculated according to the following formulas (7) and (8): 2 O 3 Finally, the vacancy rate I (mol %) is calculated according to the following formula (9):

[0039]

[0040]

[0041] The ferrite powder is α-Fe 2 O 3 In addition, when the ferrite powder contains copper (Cu), it may contain CuOFe 5 O 8 (copper-iron complex oxide) may be formed. 2 O 3 and CuOFe 5 O 8 is not a ferromagnetic material with a spinel structure. Therefore, when calculating the amount of excess Fe in the spinel phase using the above formula (7), 2 O 3 and CuOFe 5 O 8The Fe content contained in the Fe 3 O 4 (Magnetite) is a divalent iron ion (Fe 2+ ) while γ-Fe 2 O 3 (Maghemite) is Fe 2+ Therefore, in the above formula (8), γ-Fe is not included. 2 O 3 When calculating the amount of Fe 3 O 4 Fe contained in 2+ minutes are excluded.

[0042] The amount of excess Fe calculated according to the above formula (7) should be greater than zero (0). In this case, the amount of iron (Fe) in the spinel phase contained in the ferrite powder is in excess of the stoichiometric composition.

[0043] Preferably, the excess iron (Fe) ratio of the ferrite powder is 25 mol% or more and 70 mol% or less. If the excess Fe ratio is below 25 mol%, the real part of magnetic permeability (μ') increases, but the loss factor (tan δ) increases. Therefore, the ferrite powder is unsuitable for use as a filler for inductor cores. Furthermore, if the excess Fe ratio exceeds 70 mol%, the loss factor (tan δ) decreases, but the real part of magnetic permeability (μ') also decreases. Therefore, the ferrite powder is also unsuitable for use as a filler for inductor cores. The excess Fe ratio is more preferably 35 mol% or more and 70 mol% or less, and even more preferably 40 mol% or more and 70 mol% or less. The excess Fe ratio is the ratio of the amount of excess Fe to the total amount of Fe, and is calculated according to the following formula (10):

[0044]

[0045] Preferably, the mass ratio of iron (Fe) to manganese (Mn) contained in the ferrite powder (Fe / Mn mass ratio) is 5.5 to 8.0. If the Zn content is in the range of 1% by mass to 3% by mass and the Fe / Mn mass ratio is 5.5 to 8.0, the ferrite powder can achieve a good balance between high magnetic permeability and low loss. Therefore, it is possible to increase the μ′Q product.

[0046] Preferably, the copper (Cu) content of the ferrite powder is 0% by mass or more and 1.0% by mass or less. Cu tends to segregate in ferrite particles. If segregation occurs, the magnetic properties of the ferrite powder may deteriorate. By limiting the Cu content to 1.0% by mass or less, it is possible to suppress the generation of segregation that leads to deterioration of magnetic properties. On the other hand, Cu has the effect of stabilizing the valence of Fe. Depending on the manufacturing method of the ferrite powder, adding an appropriate amount of Cu can suppress the generation of vacancies and suppress changes in magnetic permeability over time over a long period of time. The Cu content is more preferably 0% by mass or more and 0.50% by mass or less, and even more preferably 0% by mass or more and 0.35% by mass or less.

[0047] The ferrite powder may have a composition containing iron (Fe), manganese (Mn), zinc (Zn), copper (Cu), and oxygen (O), with the remainder being unavoidable impurities. Alternatively, it may contain other component elements in addition to Fe, Mn, Zn, Cu, and O. Examples of such component elements include lithium (Li), magnesium (Mg), aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), and nickel (Ni). However, from the viewpoint of utilizing the excellent magnetic properties of Mn-Zn ferrite, it is preferable that the powder does not contain large amounts of other component elements in addition to Fe, Mn, Zn, Cu, and O. The content of other component elements is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0048] Preferably, the spinel phase content in the ferrite powder (ferrite particles) is 80.0% by mass or more. The spinel phase, which is a ferromagnetic material, is the crystalline phase that is the main component responsible for the magnetic properties of the ferrite powder. Increasing the spinel phase proportion makes it possible to increase the saturation magnetization (σs) and magnetic permeability (μ) of the ferrite powder. The spinel phase proportion is more preferably 85.0% by mass or more, even more preferably 90.0% by mass or more, particularly preferably 95.0% by mass or more, and most preferably 99.0% by mass or more. The spinel phase proportion is 100.0% by mass or less.

[0049] Preferably, the zinc oxide (ZnO) content in the ferrite powder is 0.0% by mass or more and 1.0% by mass or less. Zinc oxide (ZnO) is a heterophase derived from zinc (Zn) that has not been ferritized. Ferrite powder containing a large amount of ZnO has poor magnetic properties. Furthermore, when this ferrite powder is applied to a resin composition, it can cause the problem of increasing the viscosity of the composition. Therefore, the less ZnO that is a heterophase, the better. The ZnO content is more preferably 0.0% by mass or more and 0.8% by mass or less, and even more preferably 0.0% by mass or more and 0.5% by mass or less.

[0050] Preferably, the α-iron oxide (α-Fe 2 O 3 ) content is 0.0 mass % or more and 3.0 mass % or less. 2 O 3 is a heterogeneous phase that is an antiferromagnetic material. 2 O 3 If the amount is too large, the magnetic properties of the ferrite powder will be reduced. 2 O 3 If the amount is within the above range, the effect on magnetic properties is small. 2 O 3 By keeping the amount within this range, it is possible to prevent a decrease in magnetic properties, particularly saturation magnetization (σs), and a decrease in saturation magnetic flux density when used in an inductor.

[0051] The particles constituting the ferrite powder may be either single crystal or polycrystalline. However, polycrystalline is preferred. The average crystallite diameter of the particles constituting the ferrite powder is preferably 150 nm or more and 220 nm or less.

[0052] Preferably, the volume average particle size (D50) of the ferrite powder is 2.0 μm or more and 20 μm or less. Here, the volume average particle size refers to the cumulative 50% diameter (D50) in the volume particle size distribution. By increasing D50 to 2.0 μm or more, it is possible to suppress aggregation of the ferrite powder, and it is possible to further improve the moldability and packability. Furthermore, although it depends on the manufacturing conditions, by increasing the particle size to a certain extent, it is possible to control the vacancy rate of the ferrite powder. In other words, ferrite particles with a small particle size have a large specific surface area. Therefore, oxidation is easily promoted during high-temperature heat treatment processes such as thermal spraying during the manufacturing of ferrite powder, and γ-Fe with vacancies 2 O 3 tends to be easily generated. From the viewpoint of improving moldability and packing property and controlling the vacancy rate, D50 is more preferably 2.3 μm or more, even more preferably 2.5 μm or more, particularly preferably 2.8 μm or more, and most preferably 3.0 μm or more. On the other hand, by suppressing D50 to 20 μm or less, the generation of interparticle voids can be suppressed, resulting in better packing property. From the viewpoint of improving packing property, D50 is more preferably 12 μm or less, even more preferably 10 μm or less, particularly preferably 8.0 μm or less, and most preferably 7.0 μm or less. D50 is more preferably 2.3 μm or more and 12 μm or less, even more preferably 2.5 μm or more and 10 μm or less, particularly preferably 2.8 μm or more and 8.0 μm or less, and most preferably 3.0 μm or more and 7.0 μm or less.

[0053] Preferably, the shape factor SF-1 of the ferrite powder is 100 or more and 110 or less. SF-1 is an index of the sphericity of the particles constituting the powder. For a perfect sphere, SF-1 is 100, and the further away from a sphere, the larger it becomes. By keeping SF-1 at 110 or less, the fluidity of the powder is improved, regardless of whether the particles are spherical or polyhedral, and the moldability and packability are improved. SF-1 is more preferably 105 or less, and even more preferably 103 or less. SF-1 is more preferably 100 or more and 105 or less, and even more preferably 100 or more and 103 or less.

[0054] Preferably, the shape factor SF-2 of the ferrite powder is 100 or more and 110 or less. SF-2 is an index that indicates the degree of roughness of the particle surfaces that make up the powder. If there are no surface roughness, SF-2 is 100, and the deeper the roughness, the higher the SF-2 becomes. If the ferrite powder has a microscopic step structure on the particle surface, this improves adhesion with resin when made into a composite material or composite, thereby suppressing particle shedding. Therefore, SF-2 should be moderately high, specifically, 101 or more is more preferable. On the other hand, if SF-2 is excessively high, the flowability of the powder decreases, which may lead to a decrease in moldability and packability. SF-2 is more preferably 105 or less, and even more preferably 103 or less. SF-2 is more preferably 101 or more and 105 or less, and even more preferably 101 or more and 103 or less.

[0055] Preferably, the ferrite powder has a BET specific surface area of ​​0.2 m 2 / g or more 2.0m 2 / g or less. 2 By increasing the BET specific surface area to 0.3 m / g or more, the generation of interparticle voids is suppressed, and the packing property can be further improved. Furthermore, by keeping the BET specific surface area within the above range, the adhesion to resins can be improved when the ferrite powder is applied to composite materials or composites. From the viewpoint of improving packing property and adhesion, the BET specific surface area is set to 0.3 m 2 On the other hand, the BET specific surface area is preferably 2.0 m / g or more. 2 By suppressing the BET specific surface area to 1.5 m / g or less, aggregation of the ferrite powder is suppressed, which leads to improved compactibility and packing properties. Furthermore, although it depends on the manufacturing conditions, by reducing the BET specific surface area to a certain extent, it becomes possible to control the vacancy rate of the ferrite powder within an appropriate range. From the viewpoint of improving compactibility and packing properties and controlling the vacancy rate, the BET specific surface area is set to 1.5 m / g or less. 2 / g or less is more preferable, and 1.0m 2 The BET specific surface area is more preferably 0.2 m / g or less. 2 / g or more 1.5m 2 / g or less is more preferable, and 0.3m 2 / g or more 1.0m 2 / g or less is more preferable.

[0056] Preferably, the tap density of the ferrite powder is 0.50 g / cm 3 3.50g / cm or more 3 By mixing small and large particles, the tap density can be increased, resulting in better overall packing of the ferrite powder. The tap density is 1.00 g / cm 3 3.00g / cm or more 3 The following is more preferred:

[0057] Preferably, the true specific gravity of the ferrite powder is 5.00 g / cm 3 That's all. By increasing the true specific gravity, it is possible to improve the magnetic properties of the ferrite powder, particularly the saturation magnetization (σs) and magnetic permeability (μ). The true specific gravity is 5.05 g / cm 3 The above is more preferable.

[0058] Preferably, the real part of magnetic permeability (μ') of the ferrite powder at 50 MHz is 7.0 or more. By increasing μ', the magnetic properties of elements such as inductors containing the ferrite powder can be improved. μ' is more preferably 7.5 or more, and even more preferably 8.0 or more.

[0059] Preferably, the μ'Q product of the ferrite powder at 50 MHz is 400 or more. Increasing the μ'Q product makes it possible to achieve a good balance between high magnetic permeability and low loss in the ferrite powder. The μ'Q product is more preferably 450 or more, and even more preferably 500 or more. The μ'Q product is calculated according to the following formula (11) using the real part (μ') of the complex permeability and the loss factor (tan δ) of the ferrite powder. The loss factor (tan δ) is calculated according to the following formula (12) using the real part (μ') and imaginary part (μ'') of the complex permeability.

[0060]

[0061] Preferably, the permeability change rate of the ferrite powder at 50 MHz is 0.040 or less. The permeability change rate is an index of the degree of change in permeability over time, and the smaller this index, the smaller the change in permeability over time, meaning better stability over time. The change in permeability over a long period of time is considered a relaxation phenomenon and is approximated by a power law. Therefore, the permeability μ'(t) after an elapsed time t (unit: hr) has an approximate linear relationship with the natural logarithm ln(t) of time t, as shown in the following equation (13). In the following equation (13), A represents the slope of the line and B represents the intercept. Then, as shown in the following equation (14), the absolute value of the slope A of the line is defined as the permeability change rate.

[0062]

[0063] If the rate of change of magnetic permeability is 0.040 or less, it can be determined that the change in magnetic permeability over time is small over a long period of time. On the other hand, if the rate of change of magnetic permeability is greater than 0.040, when the ferrite powder is used as a magnetic core filler for an inductor, the performance of the inductor changes over time. This makes it difficult to achieve the performance (output) originally designed, which may lead to malfunction of the electronic device.

[0064] <<2. Method for Producing Ferrite Powder>> The ferrite powder of this embodiment may be produced by any method as long as it satisfies the above-described requirements. However, it is preferably produced by thermally spraying a mixture of ferrite raw materials under predetermined conditions, followed by quenching, as described below.

[0065] <Mixing of Raw Materials> First, ferrite raw materials are mixed to prepare a raw material mixture. Known ferrite raw materials such as oxides, carbonates, hydroxides, and / or chlorides can be used as the ferrite raw materials. The raw materials can be mixed using a known mixer such as a Henschel mixer in either a dry or wet manner, or both.

[0066] <Pre-calcination and pulverization> Next, the resulting raw material mixture is pre-calcined to form a pre-calcined product. Pre-calcination may be performed by a known method. For example, it may be performed using a furnace such as a rotary kiln, a continuous furnace, or a batch furnace under known conditions. For example, the pre-calcination may be performed under an atmosphere such as air at a temperature of 700°C to 1300°C for 2 hours to 12 hours.

[0067] <Granulation> The resulting calcined product is then pulverized and granulated to form a granulated product. The pulverization method is not particularly limited. For example, a known pulverizer such as a vibration mill, ball mill, or bead mill may be used, and either or both of a dry method and a wet method may be used. The granulation method may also be a known method. For example, water and, if necessary, a binder such as polyvinyl alcohol (PVA), a dispersant, and / or an additive such as an antifoaming agent may be added to the pulverized calcined product to adjust the viscosity, and the mixture is then granulated using a granulator such as a spray dryer.

[0068] In the production of ordinary ferrite powder (particles), the binder component is generally removed before sintering. In contrast, in the production method of this embodiment, it is preferable not to perform the binder removal process. By performing thermal spraying while the binder component is contained and controlling the carbon content in the granulated material, the vacancy rate of the finally obtained ferrite powder can be adjusted to fall within an appropriate range.

[0069] Preferably, the carbon content of the granules is 0.08% by mass or more and 0.20% by mass or less. Although it depends on the thermal spraying conditions, by limiting the carbon content of the granules to the above-mentioned range, the vacancy rate of the ferrite powder can be controlled to a desired value. On the other hand, if the carbon content is too low, the oxygen concentration in the surrounding environment of the particles passing through the flame in the subsequent thermal spraying process becomes high. As a result, oxidation of the ferrite powder progresses, and the γ-Fe 2 O 3 On the other hand, if the carbon content is too high, the decomposition of the binder component of the granulated material does not proceed sufficiently, which may result in particles with excessively large particle sizes and irregular shapes.

[0070] <Thermal Spraying> The resulting granules are then thermally sprayed to form a thermal spray material. In thermal spraying, the granules transported by gas pass through a thermal spray flame, melting and converting to ferrite. The ferrite particles are then rapidly cooled and solidified with a cooling gas and collected using a cyclone or filter. The cooling gas may be air at room temperature, or air or an inert gas (nitrogen gas, helium gas, argon gas, etc.) at a temperature lower than room temperature to prevent rapid cooling and oxidation. If necessary, the collected ferrite particles may be classified. For classification, the particle size is adjusted to the desired particle size using existing techniques such as air classification (air flow classification), mesh filtration, sieve classification, and sedimentation. It is also possible to separate and collect large particles in a single process using air flow classification such as a cyclone.

[0071] In order to obtain ferrite particles with a step structure (spherical-like step particles), it is important to thermally spray the granulated material under specified conditions. During thermal spraying, the entire granulated material is melted and then rapidly cooled. Although the detailed mechanism is unknown, it is speculated that a polygonal step structure that reflects the ferrite's crystal structure is formed on the particle surface during high-temperature melting, and that this structure is maintained by rapid cooling. In contrast, if the granulated material is sintered at a temperature below the melting temperature to produce ferrite particles, it is thought that the polygonal step structure is difficult to form, and even if it does form, it will disappear upon slow cooling.

[0072] In thermal spraying, a mixture of combustion gas and oxygen can be used as a combustible gas combustion flame source. The volume ratio of combustion gas to oxygen is preferably 1:3.5 to 1:6.0, more preferably 1:4.9 to 1:6.0, and even more preferably 1:4.9 to 1:5.3. This allows the volatilized raw material to condense, and the formation of small-diameter particles can be favorably promoted. For example, a combustion gas flow rate of 7 Nm 3 Total oxygen flow rate 35 Nm / hr 3 / hour (volume ratio of combustion gas to oxygen is 1:5).

[0073] If there is an excessive amount of combustion gas or oxygen during combustion, the gas not used in combustion may absorb heat during combustion, causing the flame temperature to drop. The amount of excess combustion gas not used in combustion is preferably 20% or less of the amount of supplied combustion gas. Also, the amount of excess oxygen not used in combustion is preferably 20% or less of the amount of supplied oxygen.

[0074] The amount of combustion gas relative to the amount of raw material supplied is also important. Specifically, the net fuel gas ratio is 1.05 Nm 3 / kg or more 2.00Nm 3 / kg or less is preferable. Here, the net gas amount ratio is the ratio of the net combustion gas amount to the raw material supply amount, and is calculated according to the following formula (15). The net combustion gas amount is the amount of combustion gas used for net combustion, and is calculated according to the following formula (16) or (17).

[0075]

[0076] Examples of combustion gases used in thermal spraying include flammable gases such as propane gas, propylene gas, and acetylene gas, with propane gas being preferred. A carrier gas such as nitrogen, oxygen, or air can be used to transport the granules into the flammable gas. The flow rate of the transported granules is preferably 20 m / s or more and 60 m / s or less. The thermal spraying temperature is preferably 1000°C or more and 3500°C or less, more preferably 2000°C or more and 3500°C or less.

[0077] The amount of raw material supplied during thermal spraying is also important. That is, the mechanism of step structure development changes depending on the time it takes for the raw material to cool down from the temperature (amount of heat given to the raw material particles) when passing through the thermal spray flame to room temperature. In particular, the step structure is developed by the rapid cooling of the primary raw material particles that have passed through the high-temperature flame. Even with the same flame temperature, the step structure is less likely to develop if the number of passes per unit time of the primary raw material particles (the amount of processing per hour) increases. From the perspective of developing a step structure, it is preferable to supply a small amount of raw material for thermal spraying. For example, the supply amount is preferably 20 kg / hour or less, more preferably 10 kg / hour or less, and most preferably 7 kg / hour or less.

[0078] The step structure is effectively developed in ferrite powder by including elements with high vapor pressure, such as zinc (Zn). However, not only the included elements but also the conditions during thermal spraying are important. That is, the step structure is easily developed when the sprayed material passes through the thermal spray flame and cools from a high temperature at an appropriate rate. Unlike thermal spraying, the cooling rate is relatively slow in sintering. Therefore, as the grain boundaries of the particles grow, the periphery of the step structure becomes non-linear.

[0079] The cooling rate also has a significant effect on magnetic properties, particularly the frequency characteristics of magnetic permeability. Particles that are rapidly cooled during thermal spraying have relatively small grain sizes. This results in a small loss factor (tan δ) at frequencies above 10 MHz. On the other hand, particles that are slowly cooled during firing have large grain sizes, resulting in a large loss factor at high frequencies.

[0080] In this way, by controlling the thermal spraying conditions, it is possible to adjust the properties of the ferrite powder. By performing thermal spraying under preferred conditions, it is possible to suitably adjust the shape of the obtained ferrite particles. In addition, it is possible to control the vacancy rate of the ferrite particles within a desired range.

[0081] <<3. Ferrite Resin Composite Material>> The ferrite resin composite material of this embodiment includes the above-described ferrite powder and a resin. This composite material prevents ferrite particles from falling off without impairing moldability and fillability.

[0082] Examples of resins constituting the composite material include epoxy resins, urethane resins, acrylic resins, silicone resins, polyamide resins, polyimide resins, polyamideimide resins, fluororesins, and combinations thereof. The silicone resin may be a modified silicone resin modified with acrylic, urethane, epoxy, and / or fluorine.

[0083] The composite material may contain components other than the ferrite powder and the resin, such as a solvent, a filler (organic filler or inorganic filler), a plasticizer, an antioxidant, a dispersant, a colorant such as a pigment, and / or thermally conductive particles.

[0084] The ratio of the ferrite powder to the total solid content in the composite material is preferably 50% by mass to 95% by mass, more preferably 80% by mass to 95% by mass. The ratio of the resin to the total solid content in the composite material is preferably 5% by mass to 50% by mass, more preferably 5% by mass to 20% by mass. By setting the ratios of the ferrite powder and resin within the above ranges, the dispersion stability of the ferrite powder in the composite material, as well as the storage stability and moldability of the composite material, are improved, and the properties such as the mechanical strength and magnetic properties of the composite (molded body) obtained by molding the composite material are improved.

[0085] <<4. Ferrite Resin Composite>> The ferrite resin composite of this embodiment includes a molded product of the above-described ferrite resin composition. That is, the composite is produced by molding the ferrite resin composition. The molding method is not particularly limited, and examples thereof include compression molding, extrusion molding, injection molding, blow molding, and calendar molding. Alternatively, a method of forming a coating film of the composite material on a substrate may be used.

[0086] <<5. Electronic Component>> The electronic component of this embodiment includes the ferrite resin composite described above. The electronic component may be a known component that utilizes the magnetic properties of ferrite. Examples of such components include inductors such as transformers and communication coils. The electronic component of this embodiment includes ferrite powder with small time-dependent change in magnetic permeability, and therefore has the advantage of excellent stability over time.

[0087] The present embodiment will be described in more detail using the following examples and comparative examples, but the present invention is not limited to the following examples.

[0088] (1) Preparation of ferrite powder [Examples 1 to 10] <Mixing of raw materials> α-iron oxide (α-Fe 2 O 3 ), manganese tetroxide (Mn 3 O 4 ), zinc oxide (ZnO) and copper oxide (CuO) were used as raw materials, which were weighed and mixed using a Henschel mixer. 2 O 3The raw materials were weighed so that the blending amounts of the raw materials calculated as MnO, ZnO and CuO were the molar amounts shown in Table 1 below.

[0089] <Pre-firing and pulverization> The obtained mixture was pre-firing using a rotary kiln. The pre-firing was carried out by holding the mixture for 4 hours under the conditions (temperature and atmosphere) shown in Table 1 below. Next, the obtained pre-firing product was coarsely pulverized using a dry bead mill (3 / 16 inch steel ball beads). After that, water was added and the mixture was finely pulverized using a wet bead mill (0.65 mm zirconia beads), thereby obtaining a slurry. The particle size of the pulverized powder in the slurry is shown in Table 1 below.

[0090] <Granulation> Polyvinyl alcohol (PVA, 10% aqueous solution) was added as a binder to the obtained slurry. At this time, the amount of PVA added was adjusted. The amount of PVA added in terms of solid content relative to the pulverized powder is shown in Table 1 below. Thereafter, the slurry to which the binder had been added was granulated using a spray dryer.

[0091] <Thermal spraying> The obtained granules were thermally sprayed and quenched in a combustible gas combustion flame. The thermal spraying was carried out under the conditions (propane gas flow rate, total oxygen flow rate, raw material supply oxygen flow rate, combustion oxygen flow rate, raw material supply amount, air flow rate, and thermal spraying temperature) shown in Table 1 below. In addition, air for cooling was introduced into the combustion gas immediately after thermal spraying to quench the product. Furthermore, the product was recovered using a cyclone installed downstream to obtain a thermal sprayed product. Coarse particles were removed from the obtained thermal sprayed product using a sieve, and fine particles were further removed using a classifier to obtain a ferrite powder consisting of Mn-Zn ferrite particles.

[0092] The manufacturing conditions for the ferrite powders of Examples 1 to 10 are summarized in the following Table 1. Examples 1 and 7 to 10 are embodiment samples, and Examples 2 to 6 are comparative examples.

[0093]

[0094]

[0095] (2) Evaluation The ferrite powders produced in Examples 1 to 10 were evaluated for various properties as follows.

[0096] <Chemical Analysis> The ferrite powder was subjected to chemical analysis to determine the metal component content. First, 0.2 g of ferrite powder was weighed, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added thereto, followed by heating to prepare an aqueous solution in which the sample was completely dissolved. The obtained aqueous solution was placed in an ICP analyzer (Shimadzu Corporation, ICPS-10001V), and the metal component content was measured.

[0097] <Oxidation-reduction titration> The divalent iron (Fe) contained in the ferrite powder was determined by oxidation-reduction titration. 2+ The oxidation-reduction titration was carried out in accordance with JIS M 8213, using potassium permanganate instead of potassium dichromate.

[0098] <XRD> The ferrite powder was analyzed by X-ray diffraction (XRD) under the following conditions.

[0099] - X-ray diffraction equipment: PANalytical X'pert MPD (including high-speed detector) - Radiation source: Co-Kα - Tube voltage: 45 kV - Tube current: 40 mA - Scan speed: 0.002° / sec (continuous scan) - Scan range (2θ): 15 to 90°

[0100] Based on the obtained X-ray diffraction profile, the spinel phase, ZnO phase, and α-Fe phase contained in the ferrite powder were identified. 2 O 3 The content ratio of each phase was determined. The X-ray diffraction profile was subjected to Rietveld analysis to estimate the lattice constant of the spinel phase, and the crystallite size of the spinel phase was determined according to Scherrer's formula.

[0101] Furthermore, the amounts of Fe, Mn, Zn, and Cu (unit: mass%) determined by chemical analysis, and the amount of divalent iron (Fe 2+ ) (unit: mass%), and the amount of α-Fe determined by XRD analysis 2 O 3 The amount (unit: mass %) of the spinel phase was used to calculate the vacancy rate and the Fe excess ratio, etc. Specifically, the calculations were performed according to the above formulas (1) to (10).

[0102] <Particle Shape and Surface Structure> The shape and surface structure of particles in the ferrite powder were evaluated as follows. First, the ferrite powder was observed using a scanning electron microscope (SEM; Hitachi High-Technologies Corporation, SU-8020). During the observation, the magnification was set to 50,000 times. Then, an image was taken with 1 to 30 particles, preferably 1 to 10 particles, in the field of view. Photographs were taken of 10 fields of view at random to confirm the presence or absence of a polygonal step structure.

[0103] <Shape Factor> The shape factors (SF-1 and SF-2) of the ferrite powder were determined using a particle image analyzer (Malvern Panalytical, Morphologi G3). First, the ferrite powder was analyzed using the particle image analyzer. During the analysis, image analysis was performed on each of 30,000 particles in the powder, and the circularity, perimeter, and circle equivalent diameter (CE diameter) were automatically measured. In this case, a 10x objective lens was used, and the sample size was 3 mm. 3 The particles were dispersed on a slide glass under a dispersion pressure of 5 bar using a dispersion tool attached to the apparatus.

[0104] Of the obtained data, the averages of data for particles within ±5% of the volume average particle size were calculated as the average circularity, average perimeter, and average circle equivalent diameter (CE diameter), and these were used to calculate SF-1 and SF-2 according to the following formulas (18) and (19).

[0105]

[0106] <Tap Density> The tap density of the ferrite powder was measured using a USP tap density measuring device (Powder Tester PT-X, manufactured by Hosokawa Micron Corporation) in accordance with JIS Z 2512-2012.

[0107] <True Specific Gravity> The true specific gravity of the ferrite powder was measured using a gas displacement method in accordance with JIS Z8807: 2012. Specifically, the measurement was performed using a fully automatic true density measuring device (Macpycno, Mountec Co., Ltd.).

[0108] <BET Specific Surface Area> The BET specific surface area of ​​the ferrite powder was measured using a specific surface area measurement device (Mountec Co., Ltd., Macsorb HM model-1208). First, approximately 10 g of ferrite powder was placed on a medicine wrapping paper and degassed in a vacuum dryer. After confirming that the degree of vacuum was 0.1 MPa or less, the powder was heated at 200°C for 2 hours to remove moisture adhering to the particle surface. The ferrite powder from which moisture had been removed (approximately 0.5 to 4 g) was then placed in a standard sample cell dedicated to the measurement device and accurately weighed using a precision balance. The weighed ferrite powder was then placed in the measurement port of the measurement device, and measurement was performed using the single-point method. The measurement atmosphere was a temperature of 10 to 30°C and a relative humidity of 20 to 80% (no condensation).

[0109] <Particle Size Distribution> The particle size distribution of the ferrite powder was measured as follows. First, 10 g of ferrite powder and 80 ml of water were placed in a 100 ml beaker, and two drops of sodium hexametaphosphate were added as a dispersant. The mixture was then dispersed using an ultrasonic homogenizer (UH-150 model, SMT Corporation). The output level of the ultrasonic homogenizer was set to 4, and dispersion was performed for 20 seconds. Bubbles formed on the surface of the homogenizer were then removed, and the resulting dispersion was introduced into a laser diffraction particle size distribution analyzer (SALD-7500nano, Shimadzu Corporation) for measurement. The measurement conditions were a pump speed of 7, built-in ultrasonic irradiation time of 30, and a refractive index of 1.70-050i. From this measurement, the 10% diameter (D10), 50% diameter (volume average particle size, D50), and 90% diameter (D90) in the volume particle size distribution were determined.

[0110] <Magnetic Properties - Saturation Magnetization, Remanent Magnetization, and Coercive Force> The magnetic properties (saturation magnetization, remanent magnetization, and coercive force) of the ferrite powder were measured as follows. First, the ferrite powder was packed into a cell with an inner diameter of 5 mm and a height of 2 mm, and the cell was set in a vibrating sample magnetometer (VSM-C7-10A, Toei Kogyo Co., Ltd.). A magnetic field was applied and swept up to 5 kOe, and then the applied magnetic field was reduced to draw a hysteresis curve. From the data of this curve, the saturation magnetization σs, remanent magnetization σr, and coercive force Hc of the ferrite powder were determined.

[0111] <Magnetic Permeability> The magnetic permeability of the ferrite powder was measured using an RF impedance / material analyzer (Agilent Technologies, Inc., E4991B) and a magnetic material measurement electrode (16454A). First, 9 g of ferrite powder and 1 g of binder resin (Kynar 301F: polyvinylidene fluoride) were placed in a polyethylene container (100 ml capacity) and stirred and mixed using a ball mill at a rotation speed of 100 rpm. Next, the resulting mixture (approximately 0.6 g) was filled into a die (inner diameter 4.5 mm, outer diameter 13 mm) and pressed at a pressure of 40 MPa for 1 minute using a press to produce a molded body. The resulting molded body was heat-cured at 180°C for 1 hour using a hot air dryer to prepare a measurement sample. The resulting measurement sample was placed in the RF impedance / material analyzer, and the outer diameter, inner diameter, and height of the measurement sample, which had been measured in advance, were entered. During the measurement, the amplitude was set to 100 mV, and the measurement frequency range was swept from 1 MHz to 3 GHz on a logarithmic scale.The real part (μ') and imaginary part (μ'') of the complex permeability at a frequency of 50 MHz were then determined.

[0112] In addition, the loss factor (tan δ) and μ′Q product were calculated according to the above formulas (11) and (12) using the real part (μ′) and imaginary part (μ″) of the complex permeability after 72 hours at 50 MHz.

[0113] Furthermore, the change in the real part of magnetic permeability (μ′) at 50 MHz over time was measured up to an elapsed time of 17,520 hours, and the rate of change in magnetic permeability was calculated using the obtained data according to the above equations (13) and (14).

[0114] (3) Evaluation Results The evaluation results obtained for the ferrite powders of Examples 1 to 10 are shown in the following Tables 2 to 6. The time changes in the real part of magnetic permeability (μ') of the ferrite powders of Examples 1 and 5 are shown in Figure 1 (Example 1) and Figure 2 (Example 5).

[0115] The ferrite powders of Comparative Examples 2 and 3 had a low Fe content of 54.53 mass% or less and a high Zn content of 3.64 mass% or more (Table 2). As a result, the loss factor (tan δ) at 50 MHz was high, 0.028 or more, and the μ′Q product was low, 330 or less (Table 5). These ferrite powders had high loss and were therefore unsuitable for use in high-frequency applications such as inductors.

[0116] The ferrite powder of Example 4, a comparative example, had a high Fe content of 63.11 mass % and a Zn content of zero (0) (Table 2). Therefore, the real part of magnetic permeability (μ') was low at 6.45 (Table 5). This ferrite powder had low magnetic permeability and was therefore unsuitable for use in inductors and other applications.

[0117] The ferrite powder of Example 5, a comparative example, had a high Zn content of 3.30 mass% (Table 2). As a result, the loss factor (tan δ) was high at 0.024 and the μ′Q product was low at 379 (Table 5). The vacancy rate was also high at 100.0% and the rate of change in magnetic permeability was high at 0.061 (Tables 3 and 6). This ferrite powder was found to have high loss and poor stability of magnetic permeability over time.

[0118] The ferrite powder of Comparative Example 6 contained aggregates (Table 4). As a result, the shape factors SF-1 and SF-2 were large, ranging from 126 to 130, and the volume average particle size (D50) was large, ranging from 23.11 μm (Table 4). Furthermore, no step structure was observed on the particle surface (Table 4). This ferrite powder had a large loss factor (tan δ) of 0.084 and a small μ'Q product of 107 (Table 5). Furthermore, the rate of change in magnetic permeability was large, ranging from 0.081 (Table 6). This ferrite powder exhibited high loss and poor stability of magnetic permeability over time. Furthermore, this ferrite powder was considered to have poor filling properties when used in a composite material (composite).

[0119] In contrast, the ferrite powders of Examples 1 and 7 to 10, which are working examples, were spherical (Table 4). Therefore, SF-1 and SF-2 were small, ranging from 101 to 102, had polygonal step structures on the surface, and had relatively small D50 values ​​of 9.92 μm or less (Table 4). Furthermore, the vacancy fraction was 80.5 mol% or less (Table 3). These ferrite powders had real permeability parts (μ') of 8.23 ​​or more and μ'Q products of 439 or more (Table 5). Furthermore, the rate of change in permeability was small, ranging from 0.038 or less, and the rate of change in permeability of the ferrite powder of Example 9 in particular was very small, at 0.005 (Table 6). Therefore, these ferrite powders were found to have high permeability, low loss, and small time-dependent change in permeability.

[0120] From the above results, it can be seen that according to this embodiment, a ferrite powder can be obtained that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0121]

[0122]

[0123]

[0124]

[0125]

Claims

1. Ferrite powder containing iron (Fe) in an amount of 56.0% by mass or more and 63.0% by mass or less, manganese (Mn) in an amount of 7.0% by mass or more and 13.0% by mass or less, and zinc (Zn) in an amount of 1.0% by mass or more and 3.0% by mass or less.

2. The ferrite powder according to claim 1, wherein the ferrite powder comprises spherical ferrite particles mainly composed of a spinel phase, the spinel phase has an iron (Fe) amount in excess of the stoichiometric ratio and a vacancy rate of 0 mol% or more and 90 mol% or less, and the ferrite powder has a shape factor SF-1 of 100 or more and 110 or less and a volume average particle size (D50) of 2.0 μm or more and 20 μm or less.

3. α-iron oxide (α-Fe 2 O 3 The ferrite powder according to claim 1 or 2, wherein the content of said element (I) is 0.0 mass % or more and 3.0 mass % or less.

4. The ferrite powder according to claim 1 or 2, wherein the copper (Cu) content is 0.0 mass % or more and 0.5 mass % or less.

Citation Information

Patent Citations

  • Ferrite powder, ferrite resin composite material, and electromagnetic shielding material, electronic material, or electronic component

    WO2022209640A1

  • Low-loss soft magnetic ferrite material for 5G and preparation method thereof

    CN113200741A

  • Mn-zn ferrite magnetic material

    JP1994290926A

  • Ferrite powder and method for producing the same

    JP2021066648A

  • Composite particle, powder, resin composition, and molded article

    WO2019159799A1

Cited By

  • Ferrite powder and production method for same

    WO2026211661A1