Grain-oriented electrical steel sheet and wound core

The use of a grain-oriented electrical steel sheet with a forsterite undercoating and controlled inclusion density addresses the bending accuracy and iron loss issues in conventional wound cores, resulting in high-efficiency and manufacturally advantageous wound cores with improved magnetic properties.

WO2024204623A1PCT designated stage expired Publication Date: 2024-10-03JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012849
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional wound cores for transformers suffer from poor bending accuracy during manufacturing, leading to suboptimal iron loss characteristics and assembly issues due to strain introduction during the winding process, which complicates the lamination of steel plates and affects the magnetic properties of grain-oriented electrical steel sheets.

Method used

A grain-oriented electrical steel sheet with a surface undercoating of forsterite, optimized composition, and controlled inclusion density (0.5 μm to 3.0 μm diameter and 1.0 to 20.0 pieces/mm²) to enhance bending accuracy and magnetic properties, reducing iron loss and stress relief annealing needs.

Benefits of technology

The solution achieves excellent bending accuracy and magnetic properties, enabling the production of high-efficiency wound cores with improved manufacturability and reduced iron loss, while minimizing the risk of insulation failure and core loss deterioration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012849_03102024_PF_FP_ABST
    Figure JP2024012849_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a grain-oriented electrical steel sheet which has a component composition that contains 0.0050 mass% or less of C, 2.0-8.0 mass% of Si, and 0.02-1.0 mass% of Mn, with the balance being made up of Fe and unavoidable impurities, and which has a base coating film that is mainly composed of forsterite on the surface of a base material steel sheet, wherein the number density of inclusions having a diameter of 0.5-3.0 μm present inside the base material steel sheet is 1.0-20.0 inclusions / mm2. This grain-oriented electrical steel sheet has excellent magnetic characteristics and achieves excellent accuracy when bent. Also provided is a wound core which uses this grain-oriented electrical steel sheet.<sp / >
Need to check novelty before this filing date? Find Prior Art

Description

Grain-oriented electrical steel sheets and wound cores

[0001] The present invention relates to a grain-oriented electrical steel sheet suitable for use as a transformer core material, and a wound core manufactured using the steel sheet.

[0002] Grain-oriented electrical steel sheets are soft magnetic materials primarily used as iron core materials for transformers and large generators, and are characterized by a texture in which the crystallographic <001> axis, which is the axis of easy magnetization of iron, is highly aligned in the rolling direction of the steel sheet. Such a texture can be obtained by inducing secondary recrystallization and preferentially growing crystal grains with the {110}<001> orientation, known as the Goss orientation.

[0003] For grain-oriented electrical steel sheets, iron loss characteristics are of utmost importance due to their applications. Iron loss indicates the amount of energy lost, primarily as heat, when the steel sheet is magnetized; the lower the iron loss value, the less loss there is, and the better the material is considered to be. Known methods for reducing the iron loss include reducing the variation in the Goss orientation to approach the ideal Goss orientation, and applying a special process known as magnetic domain refinement. Furthermore, grain-oriented electrical steel sheets are generally used in laminated form, and therefore have an insulating coating formed on the surface of the steel sheet. Applying tensile force to the steel sheet surface through this coating can also reduce iron loss.

[0004] Transformer cores using grain-oriented electromagnetic steel sheets are broadly divided into wound cores and stacked cores. Wound cores are made by winding steel sheets one on top of the other and are used in relatively small transformers. For example, Patent Document 1 discloses a method for creating a three-phase, three-limbed transformer using a wound core. Patent Document 2 discloses a method for manufacturing a wound core that achieves low iron loss. Patent Document 3 describes a technology for extending tool life during slitting by applying an organic substance to the surface of grain-oriented electromagnetic steel sheets for wound cores. On the other hand, stacked cores are made by stacking cut sheets cut into rectangular or trapezoidal shapes and are often used in relatively large transformers. For example, Patent Documents 4 and 5 disclose technologies related to reducing iron loss in three-phase stacked transformers. Patent Document 6 describes a manufacturing technology for a three-phase stacked transformer that achieves low iron loss and low noise.

[0005] JP 05-101943 JP 61-15309 JP 62-14405 JP 06-251966 JP 10-261536 JP 2000-114064

[0006] Recently, wound cores have been gaining attention, and demand for so-called "Unicore" wound cores, in which steel sheets are individually folded and then stacked in multiple layers to form a rectangular wound core, is increasing. Conventionally, wound cores are assembled by preparing a mold for winding electromagnetic steel sheets and then winding the steel sheets around it. However, Unicore-type wound cores do not require a mold, making assembly and design modifications easier, and are expected to reduce costs and improve manufacturability. Furthermore, conventional wound cores have a problem in that strain is introduced into the steel sheets when they are wound around the mold, significantly degrading their core loss characteristics. However, with Unicore, strain is introduced only at the folded portions during core processing, minimizing core loss degradation and potentially eliminating strain relief annealing.

[0007] The grain-oriented electrical steel sheets used in the wound cores are bent during the manufacturing process, but the poor accuracy of this bending process has been recognized as a problem. For example, the steel sheets used in Unicore are slit to a specified width and then bent at several locations, as shown in Figure 1. However, as shown in Figure 2, after the bending process, the two sides of the butted steel sheet ends often do not become parallel. This makes it difficult to stack the steel sheets, resulting in the inability to construct the core.

[0008] The present invention has been made in view of the above-mentioned problems associated with the prior art, and its object is to provide a grain-oriented electrical steel sheet that exhibits excellent bending accuracy without causing deterioration in magnetic properties, and a wound core manufactured using the steel sheet.

[0009] To achieve the above object, the inventors conducted extensive research focusing on the influence of inclusions present inside a steel sheet product on magnetic properties and bending accuracy. As a result, they discovered that in order to improve bending accuracy without deteriorating magnetic properties, it is important to have fine inclusions present inside the steel sheet and to optimize their number density, which led to the development of the present invention.

[0010] Based on the above findings, the present invention provides a grain-oriented electrical steel sheet having a base coating mainly composed of forsterite on the surface of a base steel sheet, the base steel sheet having a chemical composition containing C: 0.0050 mass% or less, Si: 2.0 to 8.0 mass%, Mn: 0.02 to 1.0 mass%, and the balance consisting of Fe and unavoidable impurities, and the number density of inclusions having a diameter of 0.5 μm or more and 3.0 μm or less present inside the base steel sheet is 1.0 pieces / mm 2 20.0 pieces / mm or more 2 The grain-oriented electrical steel sheet is characterized by the following:

[0011] The grain-oriented electrical steel sheet of the present invention, with a base coating, contains S: 0.0005 to 0.0100 mass% and Se: 0.0005 to 0.0100 mass%, and when the concentration distributions of Se and S in the thickness direction from the surface of the steel sheet are measured by glow discharge optical emission spectroscopy, peaks in the emission intensity profiles of Se and S are present at the interface between the base coating and the base steel sheet, and the peak value I of the emission intensity of Se is Se and the peak value of the emission intensity of S, I S is represented by the following formula (1): Se / I S ≦1.0 (1) is satisfied.

[0012] In addition, the grain-oriented electrical steel sheet of the present invention has a number density of inclusions having a diameter of more than 5.0 μm present inside the base steel sheet of 2.0 pieces / mm 2 The present invention is characterized by the following:

[0013] Furthermore, the base steel sheet in the grain-oriented electrical steel sheet of the present invention further contains, in addition to the above components, Sn: 0.005 to 0.500 mass%, Cr: 0.005 to 0.500 mass%, Cu: 0.01 to 0.50 mass%, Ag: 0.001 to 0.050 mass%, Au: 0.001 to 0.050 mass%, Ni: 0.01 to 0.50 mass%, Bi: 0. 005 to 0.500 mass%, P: 0.005 to 0.50 mass%, Sb: 0.005 to 0.50 mass%, Mo: 0.005 to 0.50 mass%, B: 0.0000 1 to 0.00250 mass%, Nb: 0.001 to 0.020 mass%, Ti: 0.0005 to 0.0400 mass%, V: 0.001 to 0.020 mass%, As: 0 .. 0010 to 0.0200 mass%, Zn: 0.001 to 0.020 mass%, Pb: 0.0001 to 0.0100 mass%, W: 0.0010 to 0.0100 mass% , Co: 0.002 to 0.050 mass%, Ga: 0.0001 to 0.0050 mass%, Ge: 0.0001 to 0.0050 mass%, Ca: 0.001 to 0.020 mass%, Nd: 0.001 to 0.020 mass%, La: 0.001 to 0.020 mass%, Ce: 0.001 to 0.020 mass%, Pr: 0.001 to 0.020 mass%, Dy: 0.001 to 0.020 mass%, and Hf: 0.001 to 0.020 mass%.

[0014] The present invention also provides a wound core made of any of the grain-oriented electrical steel sheets described above.

[0015] According to the present invention, it is possible to provide a grain-oriented electrical steel sheet that not only has excellent magnetic properties but also has excellent bending accuracy, making it possible to manufacture wound cores with high efficiency.

[0016] 1 is a schematic diagram illustrating the bending process of steel sheets when manufacturing Unicore; 2 is a schematic diagram illustrating defects in the bending process of steel sheets when manufacturing Unicore; 3 is a diagram illustrating θ and H, which are parameters for evaluating the processing accuracy; and 4 is a graph showing the influence of the number density of inclusions with a diameter of 0.5 to 3.0 μm on the processing accuracy and iron loss of the bending process.

[0017] First, we will describe the experiments that inspired the development of the present invention. <Experiment 1> Molten iron tapped from a blast furnace was subjected to primary refining, in which it was decarburized, dephosphorized, and desulfurized in a converter during steelmaking. It was then subjected to secondary refining in a vacuum degassing treatment device to produce steel with a chemical composition containing 0.031-0.051 mass% C, 3.20-3.35 mass% Si, 0.07-0.11 mass% Mn, 0.005-0.011 mass% Al, 0.0011-0.0044 mass% N, and 0.0008-0.0023 mass% S, with the balance being Fe and unavoidable impurities. During this secondary refining, the nitrogen partial pressure and treatment time were adjusted to vary the amount and size of inclusions contained in the molten steel. Furthermore, in order to change the state of inclusions in the steel, the casting speed was changed in the range of 0.4 to 1.5 m / min when the molten steel was continuously cast to produce a slab. The slab obtained as described above was then reheated to a temperature of 1230°C and hot-rolled to a hot-rolled sheet having a thickness of 2.4 mm. Scale on the surface of the hot-rolled sheet was removed by pickling, and the hot-rolled sheet was then cold-rolled to a final thickness of 0.23 mm. Next, the cold-rolled sheet was treated with 60 vol% H 2 +40vol%N 2 The steel sheet was subjected to decarburization annealing, which also served as primary recrystallization annealing, at 850°C for 200 seconds in an atmosphere with a dew point of 45°C to obtain a decarburized annealed steel sheet. Next, an annealing separator mainly composed of MgO was applied to the surface of the decarburized annealed steel sheet and dried. After completing the secondary recrystallization, the steel sheet was subjected to H 2 The steel sheets were subjected to finish annealing in which they were held at a temperature of 1200°C for 5 hours in an atmosphere for purification, to obtain grain-oriented electrical steel sheets (product sheets) having a base coating mainly composed of forsterite.

[0018] For the product sheets obtained as described above, a base coating mainly composed of forsterite formed on the surface of the steel sheet was removed and then the composition of the base steel sheet was analyzed. The composition was found to contain C: 0.0008 to 0.0021 mass%, Si: 3.20 to 3.35 mass%, Mn: 0.07 to 0.11 mass%, and the balance being Fe and unavoidable impurities.

[0019] Further, a test piece of 100 mm wide x 300 mm long, with the rolling direction as the length direction, was taken from the product sheet, and the iron loss W was measured by the single sheet magnetic property test method described in JIS C 2556. 17/50 In the present invention, the iron loss W 17/50 If the value is 0.85 W / kg or less, the core loss characteristics are evaluated as being good.

[0020] Similarly, a sample measuring 150 mm wide x 1000 mm long was cut from the product sheet, with the rolling direction as the length direction. As shown in FIG. 1, eight locations in the length direction were bent at 45° with a radius of curvature r of 3 mm. Next, the processing accuracy of the ring-shaped sample after the bending process was evaluated using the two parameters θ and H shown in FIG. 3. Here, θ is the angle between the two butted sides (A and B in FIG. 3), and H is the vertical deviation distance between the two butted sides A and B. When an ideal shape is obtained, θ is 0° and H is 0 mm. The greater the deviation from these values, the worse the processing accuracy. In this experiment, if each parameter was within the range of θ: 0 to 3.0° and H: 0 to 5.0 mm, respectively, the processing accuracy was judged to be acceptable. If both parameters were acceptable, it was indicated as ◯, if only one parameter was acceptable, it was indicated as △, and if both parameters were unacceptable, it was indicated as ×.

[0021] In addition, in order to investigate inclusions present in the steel plate, one side of a sample taken from the above product plate was pickled with hydrochloric acid and removed down to the center of the plate thickness, and a plane passing through the center of the plate thickness parallel to the rolled surface (steel plate surface) was revealed. After that, the size and number of inclusions present in the surface were measured using a scanning electron microscope (Personal SEM: ASPEX) equipped with an automatic particle measurement mechanism. 2 The measurements were carried out over a range of

[0022] FIG. 4 shows the number density (number / mm) of inclusions having a diameter of 0.5 μm or more and 3.0 μm or less measured as described above. 2 ) and iron loss W 17/50 The figure shows the relationship between the number density of inclusions of the above size and the evaluation results of machining accuracy. 2 20.0 pieces / mm or more 2 Iron loss W in the following range 17/50It can be seen that both the diameter and processing accuracy are good. Here, the diameter of the inclusions refers to the average value of the Feret diameter in the rolling direction and the plate width direction read from the SEM image.

[0023] The reason why the processing accuracy is good when the number density of inclusions is in the above range is not yet fully understood, but the inventors believe it to be as follows. As mentioned above, grain-oriented electrical steel sheets are characterized by the crystal orientation of the base steel sheet being highly aligned in a specific direction and by the presence of coarse crystal grains. Therefore, there are few locations where stress concentrates during bending, and the starting points of processing become uneven, which makes deformation prone to be uneven. However, as obtained in this experiment, it is believed that when inclusions of a certain size are present in the steel sheet at a certain density, stress concentrates on the inclusions and they become the starting points of deformation. Furthermore, when the inclusions are uniformly distributed, the starting points of deformation also become uniform, which improves processing accuracy. However, when the size of the inclusions is less than 0.5 μm or the number density of the inclusions is less than 1.0 pieces / mm 2 On the other hand, if the number density is less than 20.0 pieces / mm, the effect of improving the processing accuracy cannot be sufficiently obtained. 2 If the density exceeds this, the inclusions will hinder the domain wall movement, resulting in a deterioration in iron loss. The force that hinders the domain wall movement depends on the average particle size and the amount of inclusions present, but when considering a single inclusion, the larger the particle size, the greater the force, and when the particle size exceeds 3.0 μm, the force becomes particularly significant. Therefore, as revealed by this experiment, by having relatively small inclusions with an average particle size of about 0.5 to 3.0 μm present at the above density, it is possible to obtain a steel sheet with good processing accuracy without causing a deterioration in magnetic properties. Based on this concept, the number of inclusions exceeding 5.0 μm, which have a particularly large force that hinders the domain wall movement, is 2.0 / mm 2 It is desirable that the following:

[0024] Furthermore, bending can cause the forsterite-based undercoating formed on the steel sheet surface to peel off at the bent portion, exposing the base steel sheet and resulting in insulation failure. Separate experiments and studies into countermeasures to prevent this peeling have revealed that it is preferable to have soft compounds such as sulfides or selenides present between the undercoating and the base steel sheet (at the interface). The present invention was developed based on the above-mentioned novel findings.

[0025] Next, the chemical composition of the grain-oriented electrical steel sheet (product sheet) of the present invention will be described. C: 0.0050 mass% or less If the C content in the product sheet exceeds 0.0050 mass%, magnetic aging occurs, leading to iron loss deterioration, so the C content is limited to 0.0050 mass% or less. Preferably, it is 0.0030 mass% or less.

[0026] Si: 2.0 to 8.0 mass% Si is an element necessary for increasing the resistivity of steel and reducing iron loss. However, if the Si content is less than 2.0 mass%, the above effect cannot be sufficiently obtained. On the other hand, if the Si content exceeds 8.0 mass%, the workability of the steel decreases, making slitting and bending of the steel sheet difficult. Therefore, the Si content is set to the range of 2.0 to 8.0 mass%. Preferably, it is set to the range of 3.0 to 6.5 mass%.

[0027] Mn: 0.02 to 1.0 mass% Mn is an element effective in improving hot workability and stabilizing secondary recrystallization. However, if the Mn content is less than 0.02 mass%, the above effects are poor, and reducing it requires significant costs. On the other hand, if it exceeds 1.0 mass%, the magnetic flux density of the finished sheet decreases. Therefore, Mn is set to the range of 0.02 to 1.0 mass%. Preferably, it is in the range of 0.05 to 0.50 mass%.

[0028] The grain-oriented electrical steel sheet (product sheet) of the present invention essentially consists of Fe and unavoidable impurities other than the above-mentioned C, Si, and Mn. However, for the purpose of improving magnetic properties, the following elements are added: Sn: 0.005 to 0.500 mass%, Cr: 0.005 to 0.500 mass%, Cu: 0.01 to 0.50 mass%, Ag: 0.001 to 0.050 mass%, Au: 0.001 to 0.050 mass%, Ni: 0.01 to 0.50 mass%, Bi: 0.005 to 0.500 mass% , P: 0.005 to 0.50 mass%, Sb: 0.005 to 0.50 mass%, Mo: 0.005 to 0.50 mass%, B: 0.00001 to 0.00250 ma ss%, Nb: 0.001-0.020 mass%, Ti: 0.0005-0.0400 mass%, V: 0.001-0.020 mass%, As: 0.0010-0. 0200 mass%, Zn: 0.001 to 0.020 mass%, Pb: 0.0001 to 0.0100 mass%, W: 0.0010 to 0.0100 mass%, Co: 0.002 to 0.050 mass%, Ga: 0.0001 to 0.0050 mass%, Ge: 0.0001 to 0.0050 mass%, Ca: 0.001 to 0.020 m At least one element selected from the group consisting of 0.001 to 0.020 mass%, Nd: 0.001 to 0.020 mass%, La: 0.001 to 0.020 mass%, Ce: 0.001 to 0.020 mass%, Pr: 0.001 to 0.020 mass%, Dy: 0.001 to 0.020 mass%, and Hf: 0.001 to 0.020 mass% may be appropriately contained. If the content of each element is less than the above lower limit, the effect of improving the magnetic properties cannot be sufficiently obtained. Conversely, if the content exceeds the above upper limit, the development of secondary recrystallized grains is suppressed, and the magnetic properties will deteriorate.

[0029] Next, the grain-oriented electrical steel sheet of the present invention will be described. The grain-oriented electrical steel sheet of the present invention has inclusions with a diameter of 0.5 μm to 3.0 μm present inside the steel sheet (base steel sheet) after removing the undercoat mainly composed of forsterite from the steel sheet surface, and the number density of the inclusions is 1.0 pieces / mm 2 20.0 pieces / mm or more 2The number density is a value measured in a plane parallel to the steel sheet surface including the center of the sheet thickness. 2 If it is less than 20.0 pieces / mm, the effect of improving the processing accuracy described above cannot be obtained sufficiently. 2 If the number of particles exceeds 1.0, the iron loss will increase significantly. 2 10.0 pieces / mm or more 2 The range is as follows:

[0030] In order to suppress the deterioration of iron loss due to inclusions, the number density of inclusions exceeding 5.0 μm in diameter, which are a major obstacle to the movement of the domain walls, must be 2.0 pieces / mm 2 It is preferable that the number of particles is 1.0 or less per mm. 2 More preferably, it is:

[0031] Next, a method for producing the grain-oriented electrical steel sheet of the present invention will be described. The steel material (slab) used for producing the grain-oriented electrical steel sheet of the present invention is produced by refining molten pig iron obtained by a blast furnace process or molten steel obtained by an electric furnace process using a conventionally known refining process, adjusting the components, and melting steel having the above-described component composition, and then using a continuous casting method or an ingot casting-slabbing method or the like to produce the molten steel.

[0032] The steel material preferably contains C in the range of 0.010 to 0.090 mass%. C is an element that is reduced to 0.0050 mass% or less in the decarburization annealing process so that the product sheet does not undergo magnetic aging. However, if the C content exceeds 0.090 mass%, decarburization may be insufficient, and the C content in the product sheet may exceed 0.0050 mass%. On the other hand, C is an element that has the effect of strengthening the grain boundaries of the steel material and improving the texture through the α-γ transformation of the hot-rolled sheet, and in order to obtain such effects, it is preferable that the C content be 0.010 mass% or more.

[0033] Furthermore, when an inhibitor is used to induce secondary recrystallization during the finish annealing described below, the steel material preferably contains, in addition to the above-described composition, inhibitor-forming components Al, N, S, and Se. Specifically, when AlN is used as the inhibitor, it is preferable that Al be contained in the range of 0.010 to 0.040 mass% and N be contained in the range of 0.005 to 0.020 mass%. When MnS and / or MnSe are used as the inhibitor, it is preferable that S be contained in the range of 0.005 to 0.040 mass% and / or Se be contained in the range of 0.005 to 0.040 mass%. The inhibitor-forming components are reduced to the impurity level by the purification treatment during the finish annealing described below. The inhibitors AlN and MnS and / or MnSe may be used alone or in combination.

[0034] On the other hand, when no inhibitor is used to induce secondary recrystallization, it is preferable to reduce the inhibitor-forming elements Al, N, S, and Se as much as possible. Specifically, Al: less than 0.010 mass%, N: less than 0.005 mass%, S: less than 0.005 mass%, and Se: less than 0.005 mass%. As will be described later, the inhibitor-forming elements S and Se are elements that contribute to improving the adhesion of a forsterite base coating, and therefore it is preferable to include them appropriately within the above-mentioned ranges.

[0035] Of the above-mentioned components, C can be reduced in a decarburization annealing process, and N can be nitrided in a finish annealing process. However, since it is difficult to change the content of components other than C and N in processes subsequent to hot rolling, it is preferable to adjust the components at the stage of producing molten steel.

[0036] In the present invention, in addition to adjusting the steel composition to the above-mentioned ranges during the refining process, it is also important to control the morphology of inclusions present in the steel. In general, grain-oriented electrical steel sheets have inclusions that deteriorate iron loss, so it is desirable to minimize their presence. However, in the present invention, in order to improve the processing accuracy of the bending process, it is necessary to have inclusions of an appropriate size and density in the steel that do not adversely affect the magnetic properties.

[0037] As a method for controlling the shape of the inclusions, for example, a method of shortening the time of primary refining in a converter, a method of limiting the discharge of slag, a method of reducing the flow rate of blown gas during secondary refining, a method of shortening the blown gas time, etc. However, in the present invention, there is no particular limitation on the method.

[0038] Next, the steel material (slab) in which the steel composition and inclusions have been appropriately controlled is heated to a predetermined temperature by a conventional method and conditions, and then hot-rolled to form a hot-rolled sheet of a predetermined thickness. When the slab contains an inhibitor-forming component, the slab is preferably heated to a temperature of 1350°C or higher before hot rolling in order to completely dissolve the inhibitor. On the other hand, when the slab does not contain an inhibitor-forming component, the slab is preferably heated to a temperature of 1250°C or lower, which is a temperature at which hot rolling is possible, in order to reduce thermal energy costs.

[0039] Next, the steel sheet (hot-rolled sheet) after the hot rolling may be subjected to hot-rolled sheet annealing depending on the required properties. In order to obtain good magnetic properties, the annealing temperature is preferably in the range of 800°C or higher and 1150°C or lower. If the hot-rolled sheet annealing temperature is lower than 800°C, the band structure formed by hot rolling will remain, making it difficult to obtain a uniformly sized primary recrystallized structure, and there is a risk that the development of secondary recrystallized grains will be hindered. On the other hand, if the hot-rolled sheet annealing temperature exceeds 1150°C, the grain size after the hot-rolled sheet annealing will become too coarse, making it difficult to obtain a uniformly sized primary recrystallized structure.

[0040] Next, the hot-rolled sheet or the hot-rolled sheet after the hot-rolled sheet annealing is subjected to one cold rolling or two or more cold rollings with intermediate annealing in between to produce a cold-rolled sheet of the final thickness (product thickness). When intermediate annealing is performed, the annealing temperature is preferably in the range of 900°C or higher and 1200°C or lower. If the annealing temperature is lower than 900°C, the recrystallized grains become finer, and the Goss nuclei in the primary recrystallized structure decrease, which may result in deterioration of magnetic properties. On the other hand, if the annealing temperature exceeds 1200°C, the grain size becomes too coarse, as with hot-rolled sheet annealing, making it difficult to obtain a uniformly sized primary recrystallized structure.

[0041] In the final cold rolling to obtain the final sheet thickness, it is preferable to employ warm rolling in which the steel sheet temperature during cold rolling is increased to 100°C to 300°C, or interpass aging in which aging is performed between rolling passes. This can improve the recrystallization texture and enhance the magnetic properties.

[0042] Next, the cold-rolled sheet having the final thickness is subjected to decarburization annealing, which also serves as primary recrystallization annealing. In order to ensure sufficient decarburization, the decarburization annealing is preferably performed at a temperature in the range of 800°C to 900°C, and in a humid atmosphere with a dew point of 30°C or higher. Similarly, in order to promote decarburization, the atmosphere contains H 2 It is preferable that the content of Cr is in the range of 5 vol% to 70 vol%. Furthermore, the heating rate to the annealing temperature is preferably 100°C / s or more from the viewpoint of improving iron loss characteristics. However, since the higher the heating rate, the higher the cost of the equipment required to achieve it, the upper limit is preferably about 2000°C / s.

[0043] Next, the steel sheet after the decarburization annealing is coated with an annealing separator on its surface, dried, wound into a coil, and subjected to finish annealing. The annealing separator is mainly composed of MgO, which prevents the steel sheets from fusing together during annealing and allows the formation of a base coating mainly composed of forsterite on the steel sheet surface. Here, "mainly composed of MgO" means that the annealing separator contains 75 mass% or more of MgO. Furthermore, "mainly composed of forsterite" means that the base coating contains 80 mass% or more of forsterite.

[0044] The above-mentioned finish annealing is preferably carried out at 800°C or higher in order to induce secondary recrystallization, and is preferably maintained at a temperature of 800°C or higher for 20 hours or more in order to complete the secondary recrystallization. Furthermore, in order to purify impurities in the steel and form a forsterite film, after the secondary recrystallization is completed, H 2 It is preferable to heat the material to a high temperature of about 1200° C. in an atmosphere containing impurities. 2 It is preferable to maintain the temperature at 1180° C. or higher for 3 hours or more in an atmosphere.

[0045] Next, the steel sheet after the above-mentioned finish annealing is preferably subjected to flattening annealing in order to remove unreacted annealing separator by washing with water, brushing, pickling, or the like, correct the shape of the steel sheet, and improve the iron loss characteristics.

[0046] Furthermore, when product sheets are stacked for use, it is preferable to form an insulating coating on the surface of the steel sheet during planarization annealing or a process before or after planarization annealing in order to further improve iron loss. From the viewpoint of enhancing the iron loss reduction effect, it is preferable to apply a tension-applying insulating coating that can apply tensile tension to the steel sheet. Furthermore, by employing a method of forming a tension coating via a binder or forming an inorganic coating on the surface of the steel sheet by physical vapor deposition or chemical vapor deposition, a coating with excellent adhesion can be obtained and a significant iron loss reduction effect can be achieved.

[0047] One method for evaluating the adhesion strength of a coating on a grain-oriented electrical steel sheet is to measure the bend peeling diameter. This method involves wrapping small pieces of the grain-oriented electrical steel sheet around the surfaces of several round bars of different diameters to determine the limiting value (bend peeling diameter) of the round bar diameter at which defects and peeling occur in the coating. It is generally considered that the smaller the bend peeling diameter, the better the peeling resistance. However, since Unicore-type wound cores are made by bending the steel sheet at several locations, the curvature radius of each bend may be 10 mm or less. In areas bent with such small curvature radii, the forsterite base coating formed on the steel sheet surface is subjected to large strain, which poses a problem of increased susceptibility to coating peeling, even if the evaluation test for determining the bend peeling diameter above is satisfactory.

[0048] In order to make such peeling of the base coating less likely to occur, it is effective to have soft sulfides or selenides present at the interface between the base steel sheet and the base coating. Means for having sulfides or selenides present at the interface include, for example, a method of including S or Se as a component of the steel material, or a method of using an annealing separator to which a compound containing S or Se has been added, as described in the Examples, but the latter method is preferred in terms of flexibility in implementation.

[0049] Here, in order to reliably obtain the above-mentioned effect of preventing peeling of the coating, when the composition of the entire steel sheet including the base coating is analyzed, the S content must be within the range of 0.0005 to 0.0100 mass%, and the Se content must be within the range of 0.0005 to 0.0100 mass%, and when the concentration distributions of Se and S in the thickness direction from the surface of the steel sheet are measured by glow discharge optical emission spectroscopy, peaks of the emission intensity profiles of Se and S are present at the interface between the base coating and the base steel sheet, and further, the peak value I of the emission intensity of Se must be within the range of 0.0005 to 0.0100 mass%. Se and the peak value of the emission intensity of S, I S Relative to I Se / I S More preferably, the S content is in the range of 0.0020 to 0.0090 mass%, the Se content is in the range of 0.0030 to 0.0090 mass%, and the ratio I Se / I S is less than or equal to 0.8.

[0050] The above ratio I Se / I S The reason why it is preferable that the ratio is 1.0 or less is that sulfides are softer than selenides and have a higher effect of suppressing peeling, so it is preferable to have a large amount of sulfides present.

[0051] Furthermore, to obtain even lower iron loss, the grain-oriented electrical steel sheet of the present invention may be subjected to magnetic domain refinement, which has a significant effect of reducing iron loss. While wound cores are generally subjected to stress relief annealing, stress relief annealing may not be performed for unicore-type cores. Therefore, as a method for the magnetic domain refinement, in addition to heat-resistant magnetic domain refinement treatments such as providing grooves on the steel sheet surface, non-heat-resistant magnetic domain refinement treatments in which a laser or electron beam is irradiated onto the steel sheet surface may also be applied.

[0052] The grain-oriented electrical steel sheet of the present invention manufactured to satisfy the above conditions not only has excellent magnetic properties but also has excellent processing accuracy when bent, making it suitable for use in wound cores. In particular, the grain-oriented electrical steel sheet of the present invention, which has appropriate amounts of S and Se present at the interface between the base coating and the base steel sheet, also has excellent coating peeling resistance, making it suitable for use in "Unicore" type wound cores having bent sections with a small radius of curvature.

[0053] Molten steel that had been primarily refined in an electric furnace was then secondary refined by ladle refining (LF) to produce a steel having a composition containing 0.034 to 0.085 mass% C, 3.11 to 3.40 mass% Si, 0.07 to 0.12 mass% Mn, 0.004 to 0.007 mass% Al, 0.003 to 0.004 mass% N, 0 to 0.022 mass% S, 0 to 0.007 mass% Se, 0.022 to 0.031 mass% Sb, and 0.045 to 0.055 mass% Sn, with the balance being Fe and unavoidable impurities. The amount and particle size of inclusions in the steel were adjusted by changing the amount of Ar gas blown in from the hearth and the refining time. Next, when the molten steel after the above-mentioned composition adjustment was made into a slab by a continuous casting method, the casting speed was changed in the range of 0.6 to 1.6 m / min in order to further change the state of inclusions in the steel. Next, the slab obtained as described above was reheated to a temperature of 1200°C, and then hot-rolled to a hot-rolled sheet having a thickness of 2.4 mm. The scale on the surface of the hot-rolled sheet was removed by pickling, and then cold-rolled to a cold-rolled sheet having a final thickness of 0.23 mm. Next, the above-mentioned cold-rolled sheet was subjected to a 60 vol% H 2 +40vol%N 2 The decarburization annealing, which also served as primary recrystallization annealing, was performed at 840°C for 100 seconds in an atmosphere with a dew point of 60°C to obtain a decarburization annealed sheet. Next, an annealing separator mainly composed of MgO was applied to the surface of the decarburization annealed sheet, and the sheet was dried. Next, after the secondary recrystallization was completed, the sheet was subjected to H 2 The steel sheet was subjected to finish annealing in which it was purified by holding it at a temperature of 1200°C for 5 hours in an atmosphere, to obtain a grain-oriented electrical steel sheet (product sheet) having an undercoat mainly composed of forsterite.

[0054] The product sheets thus obtained were subjected to a component analysis of the steel sheets (base steel sheets) after removing the undercoating. All of the steel sheets had a component composition containing C: 0.0008 to 0.0015 mass%, Si: 3.11 to 3.40 mass%, Mn: 0.07 to 0.12 mass%, Sb: 0.022 to 0.031 mass%, and Sn: 0.045 to 0.055 mass%, with the balance being Fe and unavoidable impurities.

[0055] Next, a test piece with a width of 100 mm and a length of 300 mm, with the rolling direction as the length direction, was taken from the product sheet, and the iron loss W was measured by the single sheet magnetic property test method described in JIS C 2556. 17/50 The results were measured. Furthermore, a sample measuring 150 mm wide x 1000 mm long, with the rolling direction as the length direction, was cut out from the product sheet, and was bent at 45° at eight locations in the length direction with a radius of curvature r of 3 mm, as shown in Figure 1 . The two parameters θ and H shown in Figure 3 were measured for the resulting ring-shaped sample after bending to evaluate the processing accuracy. If the parameters θ were within the ranges of 0 to 3.0° and H were within the ranges of 0 to 5.0 mm, the product sheet was evaluated as having good processing accuracy (accepted). Furthermore, to evaluate inclusions in the product sheet, a test specimen was taken from the product sheet, and one side was pickled with hydrochloric acid to reveal a plane parallel to the steel sheet surface, including the center of the steel sheet thickness. Then, a scanning electron microscope equipped with an automatic particle measurement mechanism was used to measure the surface at 50 mm from the surface. 2 The number density (pieces / mm 2 ) was measured.

[0056] The results of the above measurements are shown in Table 1. It can be seen from the table that when the number density of inclusions with a diameter of 0.5 μm or more and 3.0 μm or less is within the range that satisfies the conditions of the present invention, both the magnetic properties and the processing accuracy are good.

[0057]

[0058] The molten iron tapped from the blast furnace is subjected to primary refining in a converter to decarburize, dephosphorize, and desulfurize, and then secondary refining and final composition adjustment are carried out by vacuum degassing to obtain the following composition: C: 0.006-0.153 mass%, Si: 1.1-8.5 mass%, Mn: 0.01-1.5 mass%, Al: 0-0.032 mass%, N: 0.0005-0.0112 mass%, S: 0-0.012 mass%, and Se: 0-0.021 mass%. Steels having various compositional compositions were produced, each containing s% of Sn, Cr, Cu, Ag, Au, Ni, Bi, P, Sb, Mo, B, Nb, Ti, V, As, Zn, Pb, W, Co, Ga, Ge, Ca, Nd, La, Ce, Pr, Dy, and Hf, with the balance being Fe and unavoidable impurities, as shown in Table 2. The amount of slag discharged in the primary refining step and the treatment time in the secondary refining step were adjusted to adjust the amount and particle size of inclusions contained in the steel to fall within the ranges of the present invention. The molten steel was then continuously cast into a steel material (slab). The slab was then reheated to 1230°C and hot-rolled to a hot-rolled sheet having a thickness of 2.7 mm. Next, the scale on the surface of the hot-rolled sheet was removed by pickling, and then the sheet was cold-rolled to an intermediate thickness of 1.6 mm, and then subjected to intermediate annealing at 1000°C for 100 seconds, followed by a second cold rolling to obtain a cold-rolled sheet with a final thickness of 0.23 mm. 2 +40vol%N 2 The steel sheet was subjected to decarburization annealing, which also served as primary recrystallization annealing, at 850°C for 200 seconds in an atmosphere with a dew point of 45°C to obtain a decarburized annealed steel sheet. Next, an annealing separator mainly composed of MgO was applied to the surface of the decarburized annealed steel sheet and dried. After completing the secondary recrystallization, the steel sheet was subjected to H 2 The steel sheet was subjected to finish annealing in which it was held at 1200°C for 5 hours in an atmosphere for purification, to obtain a grain-oriented electrical steel sheet (product sheet) having a forsterite coating.

[0059] The resulting product sheets were subjected to a chemical analysis of the base steel sheet after removing the undercoat. Test pieces measuring 100 mm wide and 300 mm long, with the rolling direction as the length direction, were cut from the product sheets and their magnetic properties were measured using the single sheet magnetic property test method described in JIS C 2556. To evaluate processing accuracy, samples measuring 150 mm wide and 1000 mm long, with the rolling direction as the length direction, were cut from the product sheets and bent at 45° angles at eight locations along the length, with a curvature radius r of 3 mm, as shown in Figure 1 . The resulting ring-shaped samples after bending were measured for the two parameters θ and H shown in Figure 3 . A sample with a θ of 0 to 3.0° and an H of 0 to 5.0 mm was evaluated as having good processing accuracy (acceptable). Furthermore, in order to evaluate the inclusions in the product plate, a test piece was taken from the product plate, and one side was pickled with a mixed solution of hydrofluoric acid and hydrogen peroxide to reveal a plane parallel to the steel plate surface including the center of the steel plate thickness. Then, a scanning electron microscope equipped with an automatic particle measuring mechanism was used to measure the inclusions in a 50 mm area of ​​the surface. 2 The number density (pieces / mm) of inclusions with diameters of 0.5 μm or more and 3.0 μm or less and over 5.0 μm that exist within the range 2 ) was measured.

[0060] The results of the above measurements are also shown in Table 2. From this table, it can be seen that steel sheets satisfying the conditions of the present invention have both good magnetic properties and processing accuracy. Steel sheet No. 4 is an example in which the C content of the slab was too high, resulting in insufficient decarburization during decarburization annealing. Steel sheet No. 9, an example of the present invention, had many inclusions with diameters exceeding 5.0 μm, resulting in slightly deteriorated magnetic properties. It can also be seen that the fewer large inclusions, the better for magnetic properties. The contents of the inhibitor-forming elements Al, N, S, and Se in the base steel sheet are not shown in Table 2, but in all steel sheets, these elements were reduced to the level of unavoidable impurities.

[0061]

[0062] The steel sheet No. 1 after decarburization annealing produced in Example 2 was used as a base material, and an annealing separator containing MgO as a main component was applied to the surface of the steel sheet and dried. The steel base material for the steel sheet No. 1 contained 0.0050 mass% S and 0.0040 mass% Se. In this case, five types of annealing separators were used: one containing neither magnesium sulfate nor sodium selenate per 100 parts by mass of MgO (No. 1-1); one containing 3 parts by mass of magnesium sulfate per 100 parts by mass of MgO (No. 1-2); one containing 4 parts by mass of sodium selenate per 100 parts by mass of MgO (No. 1-3); one containing 3 parts by mass of magnesium sulfate and 5 parts by mass of sodium selenate per 100 parts by mass of MgO (No. 1-4); and one containing 2 parts by mass of magnesium sulfate and 6 parts by mass of sodium selenate per 100 parts by mass of MgO (No. 1-5). Next, the steel sheets were subjected to completion of secondary recrystallization, and then subjected to H 2 The steel sheets were subjected to finish annealing in a purification treatment by holding them at a temperature of 1200°C for 5 hours in an atmosphere, to obtain grain-oriented electrical steel sheets (product sheets) having a forsterite coating.

[0063] Samples were taken from the product sheet thus obtained, and the contents of C, Si, and Mn in the base steel sheet from which the forsterite-based undercoating had been removed, and the contents of S and Se in the steel sheet including the undercoating were analyzed. Furthermore, the concentration distributions of Se and S in the samples from the steel sheet surface to the thickness direction were measured by glow discharge optical emission spectroscopy, and it was confirmed that the peaks of the emission intensity profiles of Se and S existed at the interface between the undercoating and the base steel sheet. The peak values ​​I of the emission intensities of Se and S were also measured. Se , I S Ratio I Se / I SThe magnetic properties were measured using the single sheet magnetic property test method described in JIS C 2556. Furthermore, test pieces measuring 100 mm wide x 300 mm long, with the rolling direction as the length direction, were taken from the product sheet. The magnetic properties were measured using the single sheet magnetic property test method described in JIS C 2556. To evaluate processing accuracy, samples measuring 150 mm wide x 1000 mm long, with the rolling direction as the length direction, were cut from the product sheet. As shown in Figure 1, eight samples were bent at 45° angles with a curvature radius r of 3 mm at each end along the length. The two parameters θ and H shown in Figure 3 were measured for the resulting ring-shaped samples after bending. A sample with θ between 0 and 3.0° and H between 0 and 5.0 mm was evaluated as having good processing accuracy (pass). The surface of the bent portion was visually inspected for peeling of the undercoat. In addition, a hoop-shaped coil with a width of 150 mm and a length of 100 m was made from the above product plate, and 100 ring-shaped samples were folded using a steel plate bending and cutting machine for Unicore. 100 sheets were stacked to make Unicores with an outer diameter of long side: 300 mm x short side: 200 mm. Then, the iron loss W of the core was measured. 17/50 In the present invention, the iron loss W of Unicore using a steel plate with a thickness of 0.23 mm was measured. 17/50 Furthermore, in order to evaluate the inclusions in the product sheet, a test piece was taken from the product sheet, one side of which was pickled with a mixed solution of hydrofluoric acid and hydrogen peroxide solution to expose a plane parallel to the surface of the steel sheet including the center of the steel sheet thickness, and then a 50 mm diameter specimen of the surface was measured using a scanning electron microscope equipped with an automatic particle measurement mechanism. 2 The number density (pieces / mm 2 ) was measured.

[0064] The results of the above measurements are shown in Table 3. From this table, it can be seen that the steel sheet satisfying the conditions of the present invention has good magnetic properties and processing accuracy. In addition, the peak intensity ratio I of Se to S at the interface between the undercoat and the base steel sheet is Se / I S It can be seen that steel sheets with a coefficient of resistance of 1.0 or less also have excellent resistance to peeling of the coating at the bent portion. Incidentally, in a "coating peeling test" in which the steel sheets are wrapped around a round bar with a diameter of 20 mm, it was confirmed that no peeling occurred in any of the steel sheets.

[0065]

Claims

1. A grain-oriented electrical steel sheet having a base coating mainly composed of forsterite on the surface of a base steel sheet, the base steel sheet having a composition containing C: 0.0050 mass% or less, Si: 2.0 to 8.0 mass%, Mn: 0.02 to 1.0 mass%, with the balance being Fe and unavoidable impurities, the number density of inclusions having a diameter of 0.5 μm or more and 3.0 μm or less present inside the base steel sheet being 1.0 pieces / mm 2 20.0 pieces / mm or more 2 A grain-oriented electrical steel sheet characterized in that:

2. The grain-oriented electrical steel sheet, with a base coating, contains S: 0.0005-0.0100 mass% and Se: 0.0005-0.0100 mass%, and when the concentration distribution of Se and S in the thickness direction from the steel sheet surface is measured by glow discharge optical emission spectrometry, the peaks of the emission intensity profiles of Se and S are present at the interface between the base coating and the base steel sheet, and the peak value I of the emission intensity of Se is Se and the peak value of the emission intensity of S I S The grain-oriented electrical steel sheet according to claim 1, characterized in that the following formula (1) is satisfied: Se / I S ≦1.0 (1) 3. The density of inclusions having a diameter of more than 5.0 μm present inside the base steel plate is 2.0 pieces / mm 2 3. The grain-oriented electrical steel sheet according to claim 1, wherein:

4. In addition to the above components, the base steel plate further contains Sn: 0.005 to 0.500 mass%, Cr: 0.005 to 0.500 mass%, Cu: 0.01 to 0.50 mass%, Ag: 0.001 to 0.050 mass%, Au: 0.001 to 0.050 mass%, Ni: 0.01 to 0.50 mass%, Bi: 0.005 to 0.500 mass%, P:

0. 005 to 0.50 mass%, Sb: 0.005 to 0.50 mass%, Mo: 0.005 to 0.50 mass%, B: 0.00001 to 0.00250 mass%, Nb:

0. 001 to 0.020 mass%, Ti: 0.0005 to 0.0400 mass%, V: 0.001 to 0.020 mass%, As: 0.0010 to 0.0200 mass%, Zn: 0.001 to 0.020 mass%, Pb: 0.0001 to 0.0100 mass%, W: 0.0010 to 0.0100 mass%, Co: 0.002 to 0.050 mass%, Ga: 0.0001 to 0.0050 mass%, Ge: 0.0001 to 0.0050 mass%, Ca: 0.001 to 0.020 mass%, Nd: 0.001 to 0.020 mass% 4. The grain-oriented electrical steel sheet according to claim 1, further comprising at least one component selected from the group consisting of 0.001 to 0.020 mass% of La, 0.001 to 0.020 mass% of Ce, 0.001 to 0.020 mass% of Pr, 0.001 to 0.020 mass% of Dy, and 0.001 to 0.020 mass% of Hf.

5. A wound core made of the grain-oriented electrical steel sheet according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Wound core for transformer with low iron loss

    JP1986015309A

  • Directional electromagnetic steel plate for wound core having superior cutting property

    JP1987014405A

  • Three-phase wound core

    JP1993101943A

  • Low loss and low noise loaded iron core and manufacture thereof

    JP2000114064A

  • Production method of oriented silicon steel slab and oriented silicon steel slab

    CN115896602A