Hot-dipped steel sheet, frame, and method for producing hot-dipped steel sheet
The hot-dip plated steel sheet with a controlled chemical composition and manufacturing process addresses the adhesion and oxide formation issues in high-strength sheets, achieving improved workability and corrosion resistance for industrial applications.
Patent Information
- Application Number
- PCT/JP2024/012894
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
High-strength hot-dip Zn-Al-Mg plated steel sheets face issues with poor plating adhesion and appearance due to high Si content, leading to oxide formation and reduced corrosion resistance, which affects their workability and industrial applications.
A hot-dip plated steel sheet with a specific chemical composition and manufacturing process using an all-radiant tube type continuous hot-dip galvanizing equipment, suppressing Si oxide formation by controlling the plating bath and steel sheet temperatures, and incorporating an Al-Fe based interfacial alloy layer for improved adhesion and corrosion resistance.
The solution results in a steel sheet with enhanced workability, appearance, and corrosion resistance, suitable for applications like solar cell frames, with improved plating adhesion and reduced oxide formation, thereby increasing industrial applicability and reducing manufacturing costs.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Hot-dip galvanized steel sheet, frame, and method for manufacturing hot-dip galvanized steel sheet
[0001] The present invention relates to a hot-dip galvanized steel sheet, a frame, and a method for manufacturing the hot-dip galvanized steel sheet. This application claims priority to Japanese Patent Application No. 2023-055729, filed on March 30, 2023, the contents of which are incorporated herein by reference.
[0002] Steel sheets having a hot-dip Zn-coated layer containing Al and Mg formed on the surface thereof (hot-dip Zn-Al-Mg-coated steel sheets) have excellent corrosion resistance, and are therefore widely used as materials for structural members that require corrosion resistance, such as building materials.
[0003] For example, Patent Document 1 discloses a Si-containing high-strength hot-dip galvanized steel sheet having good coating adhesion and good corrosion resistance after painting, which comprises a high-strength steel sheet having an Si content of 0.4 to 2.0 mass%, a steel layer having an internal oxide content of SiO of 0.4 to 2.0 mass% and a thickness of 3 μm or less, and a hot-dip galvanized layer containing Al: 0.2 to 10 mass%, the balance being Zn and unavoidable impurities, formed thereon as a first layer.
[0004] Japanese Patent Application Publication No. 2001-323355
[0005] There is a demand for even higher strength in hot-dip Zn-Al-Mg-plated steel sheets. However, because high-strength steel sheets have a high Si content and low plating wettability, conventional plating methods often result in poor plating, poor appearance, and peeling of the coating during processing. For example, the technology disclosed in Patent Document 1 uses continuous hot-dip plating equipment with an oxidation zone for plating, which oxidizes Si, Mn, and Fe in the surface layer together in the oxidation zone and reduces only Fe in the reduction zone. While this improves plating wettability, it also creates problems such as the formation of Si oxides in the surface layer of the steel sheet, which reduces the carbon concentration in the surface layer of the steel sheet and alters the surface layer of the steel sheet.
[0006] The present invention has been made in consideration of the above problems, and provides a method for manufacturing a ceramic substrate having excellent workability and appearance, and ... 2The present invention aims to provide a hot-dip galvanized steel sheet, a frame, and a method for manufacturing the hot-dip galvanized steel sheet, in which oxide formation is suppressed.
[0007] In order to solve the above problems, the present invention proposes the following means. <1> A hot-dip galvanized steel sheet according to Aspect 1 of the present invention comprises: a steel sheet; and a coating layer provided on the steel sheet, wherein a first chemical composition of the steel sheet contains, in mass %, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, Si: 0.40% to 2.00%, P: 0.001% to 0.100%, S: 0.0001% to 0.0100%, and Al: 0.001% to 1.500%, with the balance being Fe and impurities, the tensile strength of the steel sheet is 740 MPa or more, and SiO is contained in a region of the steel sheet from the surface to 3 μm in the sheet thickness direction. 2 and a second chemical composition that is a chemical composition of the coating layer contains, in mass%, Al: 10% to 13%, Mg: 3% to 5%, and Si: 0.5% or less, with the balance being Zn and impurities, the coating layer includes an Al-Fe-based interface alloy layer in contact with the steel sheet surface, and the Al-Fe-based interface alloy layer has a thickness of 1.0 to 3.0 μm. <2> Aspect 2 of the present invention is the hot-dip coated steel sheet of Aspect 1, wherein the first chemical composition may further contain, in mass%, one or more selected from Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V: 0.001% to 0.300%. <3> Aspect 3 of the present invention relates to the hot-dip galvanized steel sheet of Aspect 1 or Aspect 2, wherein the first chemical composition may further contain, in mass %, one or more elements selected from: Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, Mo: 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00%. <4> Aspect 4 of the present invention relates to the hot-dip galvanized steel sheet of any one of Aspects 1 to 3, wherein SiO 2<5> Aspect 5 of the present invention is the hot-dip galvanized steel sheet of any one of Aspects 1 to 4, wherein the first chemical composition may further contain, in mass %, 0.0001% to 0.0100% in total of one or more of Ca, Mg, Zr, and REM. <6> A method for producing a hot-dip galvanized steel sheet according to Aspect 6 of the present invention includes a continuous plating step of plating a base steel sheet having a first chemical composition using an all-radiant tube type continuous hot-dip galvanizing facility, wherein in the continuous plating step, the base steel sheet is reduction-annealed in an atmosphere of 2 to 10 vol% hydrogen and 0.002 vol% to 0.05 vol% steam under reducing conditions where the maximum surface temperature of the base steel sheet is 775°C or higher and the residence time at 750°C or higher is 30 seconds or longer, and the base steel sheet after the reduction annealing is immersed in a plating bath at a plating bath temperature of 470°C to 520°C and an entry temperature of 470°C to 520°C, or at a plating bath temperature of 450°C to less than 470°C and an entry temperature of 490°C to 520°C for 3 seconds or longer, wherein the first chemical composition is, in mass%, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, The coating bath has a chemical composition, by mass%, of Al: 10% to 13%, Mg: 3% to 5%, and Si: 0.5% or less, with the balance consisting of Zn and impurities. <7> A mounting base according to aspect 7 of the present invention uses the hot-dip galvanized steel sheet according to aspect 1.
[0008] According to the above aspect of the present invention, it is possible to provide a ceramic material having excellent processability and appearance, and having SiO 2 It is possible to provide a hot-dip galvanized steel sheet, a frame, and a method for manufacturing a hot-dip galvanized steel sheet in which oxide formation is suppressed.
[0009] The present inventors have developed a method for producing a ceramic substrate having excellent processability and appearance, and containing SiO 2After extensive research into hot-dip galvanized steel sheets in which oxide formation is suppressed, the inventors have found that the formation of Si oxides in the surface layer of the steel sheet can be suppressed by using an all-radiant tube continuous hot-dip galvanizing system that does not have an oxidation zone. Furthermore, the inventors have found that by coating this steel sheet in which the formation of Si oxides in the surface layer is suppressed while controlling the temperature of the coating bath and the temperature of the steel sheet entering the coating bath within a predetermined range, a hot-dip galvanized steel sheet with excellent workability and appearance can be obtained, leading to the completion of the present invention. In this specification, the workability of a hot-dip galvanized steel sheet refers to the adhesion between the steel sheet and the coating layer at the bent portion of the hot-dip galvanized steel sheet, which is evaluated after bending the hot-dip galvanized steel sheet. Furthermore, the appearance refers to the coverage of the coating layer.
[0010] Hereinafter, a hot-dip galvanized steel sheet according to an embodiment of the present invention will be described. The hot-dip galvanized steel sheet according to this embodiment includes a steel sheet and a coating layer provided on the steel sheet, and a first chemical composition of the steel sheet contains, in mass %, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, Si: 0.40% to 2.00%, P: 0.001% to 0.100%, S: 0.0001 to 0.0100%, and Al: 0.001 to 1.500%, with the balance being Fe and impurities. The tensile strength of the steel sheet is 740 MPa or more, and SiO 2 the area ratio of the Al-Fe-based interfacial alloy layer to the surface of the steel sheet is less than 0.4%, and a second chemical composition that is a chemical composition of the plating layer contains, in mass %, 10% to 13% Al, 3% to 5% Mg, and 0.5% or less Si, with the balance being Zn and impurities, the plating layer includes an Al-Fe-based interfacial alloy layer in contact with the surface of the steel sheet, and the thickness of the Al-Fe-based interfacial alloy layer is 1.0 to 3.0 μm.
[0011] In the following description, the "%" designation for the content of each element in the chemical composition means "mass %." The content of an element in the chemical composition may be expressed as an element concentration (e.g., Zn concentration, Mg concentration, etc.). In this specification, the term "plated layer" refers to a plated film produced by a so-called hot-dip galvanizing process.
[0012] (Steel Sheet) A first chemical composition of the steel sheet contains, in mass %, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, Si: 0.40% to 2.00%, P: 0.001% to 0.100%, S: 0.0001% to 0.0100%, and Al: 0.001% to 1.500%, with the balance being Fe and impurities. Each element will be described below.
[0013] [C: 0.05% to 0.20%] C is an element added to increase the strength of steel sheets. However, if the C content exceeds 0.20%, weldability deteriorates, so the C content is set to 0.20% or less. From the viewpoint of weldability, the C content is preferably 0.15% or less. On the other hand, if the C content is less than 0.05%, the strength decreases and it becomes difficult to ensure sufficient tensile strength, so the C content is set to 0.05% or more. In order to further increase the strength, the C content is preferably 0.06% or more, and more preferably 0.07% or more.
[0014] [Mn: 1.00% to 3.00%] Mn is added to improve the hardenability of steel sheets and thereby increase their strength. However, if the Mn content exceeds 3.00%, coarse Mn-enriched areas form in the center of the steel sheet's thickness, making it more susceptible to embrittlement and problems such as cracking of the cast slab. Therefore, the Mn content is set to 3.00% or less. Furthermore, an increase in Mn content also deteriorates weldability. For this reason, the Mn content is preferably set to 2.80% or less, and more preferably set to 2.70% or less. On the other hand, if the Mn content is less than 1.00%, a large amount of soft tissue is formed during cooling after annealing, making it difficult to ensure sufficiently high tensile strength. Therefore, the Mn content is set to 1.00% or more. To further increase strength, the Mn content is preferably set to 1.20% or more, and more preferably set to 1.40% or more.
[0015] [Si: 0.40% to 2.00%] Si is an element that suppresses the formation of iron-based carbides in steel sheets and improves their strength and formability. However, Si also embrittles steel sheets, and if its content exceeds 2.00%, problems such as cracking of cast slabs become more likely. For this reason, the Si content is set to 2.00% or less. Furthermore, Si forms oxides on the surface of the base steel sheet during the annealing process, significantly impairing the adhesion of the coating. From this perspective, the Si content is preferably set to 1.90% or less, and more preferably set to 1.60% or less. On the other hand, if the Si content is less than 0.40%, a large amount of coarse iron-based carbides are generated during the coating process of hot-dip galvanized steel sheets, resulting in deterioration of their strength and formability. For this reason, the Si content is set to 0.40% or more. From the perspective of suppressing the formation of iron-based carbides, the Si content is preferably set to 0.50% or more, and more preferably set to 0.60% or more.
[0016] [P: 0.001% to 0.100%] P is an element that embrittles steel sheets. Furthermore, if the P content exceeds 0.100%, problems such as cracking of cast slabs become more likely to occur. For this reason, the P content is set to 0.100% or less. Furthermore, P is an element that embrittles the molten zone formed by spot welding. In order to obtain sufficient welded joint strength, the P content is preferably set to 0.040% or less, and more preferably set to 0.020% or less. On the other hand, setting the P content to less than 0.001% results in a significant increase in manufacturing costs. For this reason, the P content is set to 0.001% or more, and preferably 0.010% or more.
[0017] [S: 0.0001% to 0.0100%] S is an element that combines with Mn to form coarse MnS, reducing formability. For this reason, the S content is set to 0.0100% or less. S is also an element that deteriorates spot weldability. For this reason, the S content is preferably set to 0.0060% or less, and more preferably set to 0.0035% or less. On the other hand, setting the S content to less than 0.0001% results in a significant increase in manufacturing costs. For this reason, the S content is set to 0.0001% or more, preferably 0.0005% or more, and more preferably 0.0010% or more.
[0018] [Al: 0.001% to 1.500%] Al is an element that embrittles steel sheets. If the Al content exceeds 1.500%, problems such as cracking of the cast slab become more likely to occur, so the Al content is set to 1.500% or less. Furthermore, since an increase in the Al content deteriorates weldability, the Al content is preferably set to 1.200% or less, and more preferably to 1.000% or less. Al is an impurity present in trace amounts in raw materials, and reducing its content to less than 0.001% significantly increases manufacturing costs, so the Al content is set to 0.001% or more. Furthermore, Al is also an effective element as a deoxidizer, but to more fully obtain the deoxidizing effect, the Al content is preferably set to 0.010% or more.
[0019] The steel sheet according to this embodiment may contain the above elements, with the balance being Fe and impurities. Here, the impurities are elements that are mixed in during industrial steel production due to raw materials such as ore and scrap, and various factors in the production process, and whose presence is permitted to the extent that they do not impair the properties of the steel sheet according to this embodiment. They also include elements that are not intentionally added to the steel sheet.
[0020] Furthermore, the hot-dip galvanized steel sheet according to an embodiment of the present invention may contain the following elements as needed. Specifically, in addition to the above chemical components, the steel sheet may contain one or more elements selected from Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V: 0.001% to 0.300%. These elements do not necessarily have to be contained, and the lower limit of the content of each element is 0%.
[0021] [Ti: 0.001% to 0.150%] Ti is an element that contributes to increasing the strength of steel sheets by precipitation strengthening, grain refinement due to suppression of ferrite grain growth, and dislocation strengthening through suppression of recrystallization. However, if the Ti content exceeds 0.150%, the precipitation of carbonitrides increases, deteriorating formability. Therefore, the Ti content is preferably 0.150% or less. From the viewpoint of formability, the Ti content is more preferably 0.080% or less. In order to fully obtain the strength-increasing effect of Ti addition, the Ti content is preferably 0.001% or more. In order to further increase the strength of steel sheets, the Ti content is more preferably 0.010% or more.
[0022] [Nb: 0.001% to 0.100%] Nb is an element that contributes to increasing the strength of steel sheets by strengthening precipitates, strengthening fine grains by inhibiting ferrite grain growth, and strengthening dislocations by inhibiting recrystallization. However, if the Nb content exceeds 0.100%, the precipitation of carbonitrides increases, deteriorating formability. Therefore, the Nb content is more preferably 0.100% or less. From the viewpoint of formability, the Nb content is more preferably 0.060% or less. To fully obtain the strength-increasing effect of Nb addition, the Nb content is preferably 0.001% or more. To further increase the strength of steel sheets, the Nb content is more preferably 0.005% or more.
[0023] [V: 0.001% to 0.300%] V is an element that contributes to increasing the strength of steel sheets by strengthening precipitates, strengthening fine grains by inhibiting ferrite grain growth, and strengthening dislocations by inhibiting recrystallization. However, if the V content exceeds 0.300%, the precipitation of carbonitrides increases, deteriorating formability. For this reason, the V content is preferably 0.300% or less, and more preferably 0.200% or less. In order to fully obtain the strength-increasing effect of adding V, the V content is preferably 0.001% or more, and more preferably 0.010% or more.
[0024] Furthermore, the steel sheet according to this embodiment may further contain one or more elements selected from Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, Mo: 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00%. These elements do not necessarily have to be contained, and therefore the lower limit of the content of each element is 0%.
[0025] [Cr: 0.01% to 2.00%] Cr is an element that suppresses phase transformation at high temperatures and is effective in increasing strength, and may be added. However, if the Cr content exceeds 2.00%, hot workability is impaired, resulting in a decrease in productivity. For this reason, the Cr content is preferably 2.00% or less, and more preferably 1.20% or less. In order to fully obtain the effect of increasing strength due to the addition of Cr, the Cr content is preferably 0.01% or more, and more preferably 0.10% or more.
[0026] [Ni: 0.01% to 2.00%] Ni is an element that suppresses phase transformation at high temperatures and is effective in increasing strength, and may be added. However, if the Ni content exceeds 2.00%, weldability is impaired. For this reason, the Ni content is preferably 2.00% or less, and more preferably 1.20% or less. To fully obtain the effect of increasing strength due to the addition of Ni, the Ni content is preferably 0.01% or more, and more preferably 0.10% or more.
[0027] [Cu: 0.01% to 2.00%] Cu is an element that increases strength by being present in steel as fine particles, and can be added. However, if the Cu content exceeds 2.00%, weldability is impaired. It can also cause cracking due to surface red shortness during hot rolling. For this reason, the Cu content is preferably 2.00% or less, and more preferably 1.20% or less. To fully obtain the effect of increasing strength by adding Cu, the Cu content is preferably 0.01% or more, and more preferably 0.10% or more.
[0028] [Mo: 0.01% to 2.00%] Mo is an element that suppresses phase transformation at high temperatures and is effective in increasing strength, and may be added. However, if the Mo content exceeds 2.00%, hot workability is impaired, resulting in a decrease in productivity. For this reason, the Mo content is preferably 2.00% or less, and more preferably 1.20% or less. In order to fully obtain the effect of increasing strength due to the addition of Mo, the Mo content is preferably 0.01% or more, and more preferably 0.05% or more.
[0029] [B: 0.0001% to 0.0100%] B is an element that suppresses phase transformation at high temperatures and is effective in increasing strength, and may be added. However, if the B content exceeds 0.0100%, hot workability is impaired and productivity decreases, so the B content is preferably 0.0100% or less. From the viewpoint of productivity, the B content is more preferably 0.0050% or less. In order to fully obtain the effect of increasing strength by adding B, the B content is preferably 0.0001% or more. In order to further increase strength, the B content is more preferably 0.0005% or more.
[0030] [W: 0.01% to 2.00%] W is an element that suppresses phase transformation at high temperatures and is effective in increasing strength, and may be added. However, if the W content exceeds 2.00%, hot workability is impaired, resulting in a decrease in productivity. For this reason, the W content is preferably 2.00% or less, and more preferably 1.20% or less. In order to fully obtain the increased strength due to W, the W content is preferably 0.01% or more, and more preferably 0.10% or more.
[0031] Furthermore, the steel sheet of this embodiment may contain one or more of Ca, Mg, Zr, and REM in a total amount of 0.0001% to 0.0100% as other elements. The reasons for adding these elements are as follows. REM is an abbreviation for Rare Earth Metal, and here refers to elements belonging to the lanthanoid series.
[0032] Ca, Mg, Zr, and REM are elements effective in improving formability, and one or more of them can be added. However, if the total content of one or more of Ca, Mg, Zr, and REM exceeds 0.0100%, ductility may be impaired. Therefore, the total content of each element is preferably 0.0100% or less, and more preferably 0.0070% or less. On the other hand, the effects of the present invention can be achieved even if the lower limit of the content of one or more of Ca, Mg, Zr, and REM is not particularly specified. In order to fully obtain the effect of improving the formability of the steel sheet, the total content of these elements is preferably 0.0001% or more. From the viewpoint of formability, it is more preferable that the total content of one or more of Ca, Mg, Zr, and REM is 0.0010% or more.
[0033] The chemical composition of the steel sheet according to this embodiment can be determined by the following method. For example, the chemical composition (first chemical composition) of the steel sheet can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). C and S can be measured using a combustion-infrared absorption method, N can be measured using an inert gas fusion-thermal conductivity method, and O can be measured using an inert gas fusion-non-dispersive infrared absorption method. The chemical composition of the steel sheet can be measured after removing the coating layer by mechanical grinding.
[0034] (Tensile strength of steel sheet is 740 MPa or more) In the steel sheet according to this embodiment, the tensile strength (TS) is set to 740 MPa or more. The strength of the steel sheet is preferably 780 MPa or more, and more preferably 1000 MPa or more. The tensile strength is preferably 1250 MPa or less. The tensile strength (TS) can be determined by taking a JIS No. 5 tensile test piece from the steel sheet in a direction perpendicular to the rolling direction and the sheet thickness direction, and performing a tensile test in accordance with JIS Z 2241:2011. The tensile strength is measured after removing the plating.
[0035] (SiO in the region up to 3 μm from the surface of the steel plate in the plate thickness direction 2In the steel sheet according to this embodiment, in the region from the surface of the steel sheet to 3 μm in the sheet thickness direction, SiO 2 The area ratio of SiO in the region from the surface of the steel sheet to 3 μm in the sheet thickness direction is less than 0.4%. 2 When the area ratio of SiO is 0.4% or more, the surface layer 2 Oxides are formed, and the coating is likely to peel off when the high-strength steel sheet is processed. More preferably, SiO is formed in the region up to 3 μm from the surface of the steel sheet in the sheet thickness direction. 2 The area ratio of SiO in the region from the surface of the steel sheet to 3 μm in the sheet thickness direction is 0.2% or less. 2 The area ratio of the above is preferably 0.1% or more.
[0036] (Plated Layer) The second chemical composition of the plated layer contains, in mass %, 10% to 13% Al, 3% to 5% Mg, and 0.5% or less Si, with the remainder consisting of Zn and impurities. The plated layer includes an Al-Fe-based interface alloy layer in contact with the surface of the steel sheet. The portion of the plated layer excluding the Al-Fe-based interface alloy layer is a Zn-Al-Mg alloy layer. That is, the plated layer includes a Zn-Al-Mg alloy layer and an Al-Fe-based interface alloy layer. Each element in the plated layer will be described below.
[0037] [Al: 10% to 13%] Al is an element that improves corrosion resistance and suppresses Mg oxide dross in the coating bath, thereby contributing to bath stability. Therefore, the Al content is set to 10% or more. The Al content may be set to 11% or more. On the other hand, if Al is excessive, the Mg content and Zn content may relatively decrease, resulting in deterioration of corrosion resistance. Therefore, the Al content is set to 13% or less. The Al content may be set to 12% or less.
[0038] [Mg: 3% to 5%] Mg is an essential element for ensuring corrosion resistance. Therefore, the Mg content is set to 3% or more. The Mg content may be set to 4% or more. On the other hand, if the Mg content is excessive, workability and corrosion resistance may be deteriorated. Therefore, the Mg content is set to 5% or less. The Mg content may be set to 4% or less.
[0039] [Si: 0.5% or less] The Si content may be 0%. On the other hand, Si contributes to improving corrosion resistance. It also suppresses excessive growth of a brittle Al-Fe alloy layer at the interface between the coating and the base material, thereby improving plating workability. Therefore, the Si content may be 0.05% or more. On the other hand, if the Si content is excessive, corrosion resistance may deteriorate. Therefore, the Si content is set to 0.5% or less. The Si content may also be set to 0.4% or less. The Si content is preferably 0.10% or more.
[0040] [Balance: Zn and Impurities] The balance of the chemical composition (second chemical composition) of the plating layer according to this embodiment is Zn and impurities. Zn is an element that provides corrosion resistance to the plating layer. Impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the plating layer as impurities due to mutual atomic diffusion between the base steel sheet and the plating bath.
[0041] The chemical composition of the plating layer according to this embodiment is measured by the following method. First, an acid containing an inhibitor that suppresses corrosion of the steel sheet is used to strip and dissolve the plating layer to obtain an acid solution. Next, the obtained acid solution is subjected to ICP analysis. This allows the chemical composition (second chemical composition) of the plating layer to be obtained. The acid species is not particularly limited as long as it is an acid that can dissolve the plating layer. Note that the chemical composition measured by the above-mentioned means is the average chemical composition of the entire plating layer. The formation reaction of the Al-Fe-based interface alloy layer is completed in the plating bath, and the thickness of the Al-Fe-based interface alloy layer is also sufficiently small compared to the thickness of the plating layer. Therefore, unless a special heat treatment such as a thermal alloying treatment is performed after plating, the average chemical composition of the entire plating layer is substantially equal to the chemical composition of the Zn-Al-Mg alloy layer, and components such as the Al-Fe-based interface alloy layer can be ignored.
[0042] [Al-Fe-based interface alloy layer] The plating layer according to this embodiment includes an Al-Fe-based interface alloy layer in contact with the surface of the steel sheet. The Al-Fe-based interface alloy layer is formed on the surface of the steel sheet, specifically between the steel sheet and the plating layer, and is a layer whose structure contains an Al-Fe intermetallic compound as a main component. For example, the Al-Fe-based interface alloy layer may be formed by5 Fe 2 The Al phase is the main phase layer. 5 Fe 2 The Al-Fe alloy layer is composed of an Al phase having an area ratio of 80% or more. 5 Fe 2 It means that it is a phase.
[0043] The Al-Fe-based interfacial alloy layer is formed by mutual atomic diffusion between the steel sheet and the plating bath. In this embodiment, the plating bath contains Al at a concentration equal to or higher than a certain level. 5 Fe 2 However, because atomic diffusion takes time, the Fe concentration in the Al-Fe system interface alloy layer is not uniform, and the Fe concentration may be higher in the area closer to the steel sheet. Therefore, the Al-Fe system interface alloy layer is partially composed of an AlFe phase, an Al 3 It may contain a small amount of Fe phase, etc. In addition, since the plating bath also contains a certain concentration of Zn, the Al-Fe-based interface alloy layer may also contain a small amount of Zn or Si, which tends to accumulate at the interface.
[0044] When Si is contained in the plating layer, the Si may be incorporated into the Al-Fe-based interfacial alloy layer and form an Al-Fe-Si intermetallic compound phase. The intermetallic compound phase that can be identified is the AlFeSi phase, and isomers such as α-, β-, q1-, and q2-AlFeSi phases exist. Therefore, these AlFeSi phases may be detected in the Al-Fe-based interfacial alloy layer.
[0045] The Al-Fe-based interfacial alloy layer ensures adhesion between the plating layer and the steel sheet during processing of the hot-dip galvanized steel sheet and affects processability. In this embodiment, the thickness of the Al-Fe-based interfacial alloy layer is 1.0 to 3.0 μm. If the Al-Fe-based interfacial alloy layer exceeds 3.0 μm, cracks may occur during processing. If the Al-Fe-based interfacial alloy layer is less than 1.0 μm, sufficient adhesion between the plating layer and the steel sheet may not be obtained.
[0046] The thickness of each layer of the plating layer according to this embodiment and the region from the surface of the steel sheet to 3 μm in the sheet thickness direction are 2 The area ratio can be evaluated by the following method.
[0047] First, a test piece is cut out by FIB (Focused Ion Beam) processing so that the cutting direction is parallel to the thickness direction and perpendicular to the width direction. The cross-sectional structure of this cut surface is observed using a scanning electron microscope with an electron beam microanalyzer (SEM-EPMA) at a magnification that allows each layer to fit within the observation field. If the Zn-Al-Mg alloy layer, the Al-Fe-based interfacial alloy layer, and the region extending from the surface of the steel sheet to 3 μm in the thickness direction are not included within the observation field, the cross-sectional structure is observed in multiple consecutive fields. For example, a field of view of approximately 1 μm x 1 μm or more may be used for observation. The width of the observation range in the thickness direction and width direction is confirmed by referring to the scale bar used during SEM photography. An acceleration voltage of 20 kV may also be used. Since it is difficult to obtain average information about the steel sheet when observing only one field of view, it is sufficient to observe 10 randomly selected, mutually separated locations within the field of view for judgment.
[0048] In order to identify each layer in the cross-sectional structure of the steel sheet according to this embodiment, a line analysis is performed along the sheet thickness direction using an electron probe microanalyzer (EPMA), and the chemical composition of each layer is quantitatively analyzed. The elements to be quantitatively analyzed are six elements: Fe, Si, O, Mg, Zn, and Al.
[0049] From the results of the SEM-EPMA quantitative analysis described above, the layered region located deepest in the sheet thickness direction and having an Fe content of 70 atomic % or more and an O content of less than 30 atomic % excluding measurement noise was determined to be a steel sheet, and the region having an Fe content of 10 atomic % or more but less than 70 atomic % and an O content of less than 30 atomic % was determined to be an Al-Fe-based interfacial alloy layer. The region having an Fe content of less than 10 atomic % was determined to be a Zn-Al-Mg alloy layer. The surface of the steel sheet was determined to be the interface between the steel sheet and the Al-Fe-based interfacial alloy layer. The thickness of the Al-Fe-based interfacial alloy layer was determined to be the length along the sheet thickness direction from the interface between the Zn-Al-Mg alloy layer and the Al-Fe-based interfacial alloy layer to the interface between the Al-Fe-based interfacial alloy layer and the steel sheet.
[0050] For example, a linear analysis of the precipitates observed in the steel sheet is performed in the thickness direction of the steel sheet identified by the above method using an electron probe microanalyzer (EPMA), and quantitative analysis of the chemical components is performed to determine SiO2 The elements to be quantitatively analyzed are six elements: Fe, Si, O, Mg, Zn, and Al. From the results of the quantitative analysis by EPMA described above, excluding measurement noise, it was found that the area where the Fe content is 15 atomic % or less, the Si content is 30 atomic % or more, and the O content is 55 atomic % or more is internally oxidized SiO 2 The total area of the region from the surface of the steel sheet to 3 μm in the sheet thickness direction and the obtained SiO 2 From the area of SiO 2 The area ratio of SiO 2 (area of the area of the steel plate from the surface to 3 μm in the thickness direction)
[0051] (Area ratio of plating layer) In the hot-dip plated steel sheet according to the present embodiment, the area ratio (coverage) of the plating layer to the steel sheet surface is preferably 99% or more. The area ratio of the plating layer can be evaluated using image analysis software on a surface observation image of the hot-dip plated layer.
[0052] (Adhesion weight of plating layer) The adhesion weight of the plating layer per side is, for example, 20 to 150 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 150 g / m or more, the corrosion resistance of the hot-dip galvanized steel sheet can be further improved. 2 By setting the following, the workability of the hot-dip galvanized steel sheet can be further improved.
[0053] The coating weight of the coating layer according to this embodiment is measured by the following method. First, the area of the coating layer of the hot-dip galvanized steel sheet and the weight of the hot-dip galvanized steel sheet are measured before the coating layer is peeled off. Next, the coating layer is peeled off using an acid containing an inhibitor that suppresses corrosion of the steel sheet. The weight of the hot-dip galvanized steel sheet after peeling is measured and calculated to determine the coating weight of the coating layer (g / m 2 ) is obtained.
[0054] <Method for manufacturing hot-dip galvanized steel sheet> Next, a method for manufacturing the hot-dip galvanized steel sheet according to the present embodiment will be described, but the method for manufacturing the hot-dip galvanized steel sheet according to the present embodiment is not particularly limited. For example, the hot-dip galvanized steel sheet according to the present embodiment can be obtained under the manufacturing conditions described below.
[0055] The method for producing a hot-dip galvanized steel sheet according to this embodiment includes a continuous plating step of plating a base steel sheet having the above-mentioned first chemical composition using all-radiant tube type continuous hot-dip galvanizing equipment, and in the continuous plating step, the base steel sheet is reduction-annealed in an atmosphere of 2 to 10 vol% hydrogen and 0.002 vol% to 0.05 vol% steam under reducing conditions where the maximum surface temperature of the base steel sheet is 775°C or higher and the residence time at 750°C or higher is 30 seconds or longer, and the base steel sheet after reduction annealing is immersed for 3 seconds or longer in a plating bath having a second chemical composition at a plating bath temperature of 470°C to 520°C and an entry temperature of 470°C to 520°C, or at a plating bath temperature of 450°C or higher but lower than 470°C and an entry temperature of 490°C to 520°C. Specifically, the chemical composition of the plating bath (second chemical composition) contains, in mass %, 10% to 13% Al, 3% to 5% Mg, and 0.5% or less Si, with the remainder consisting of Zn and impurities.
[0056] (Base Steel Sheet) As the base steel sheet, a steel sheet having the above-described first chemical composition and a tensile strength (for example, the tensile strength of the steel sheet after the above-described reduction annealing) of 740 MPa or more is used. The base steel sheet is not particularly limited as long as it has the above-described first chemical composition and, for example, a tensile strength of 740 MPa or more. As the base steel sheet, for example, a hot-rolled steel sheet obtained by steelmaking a slab having the above-described first chemical composition and hot-rolling the slab may be used. Alternatively, a cold-rolled steel sheet obtained by cold-rolling the obtained hot-rolled steel sheet may be used.
[0057] (All Radiant Tube Type Continuous Hot-Dip Galvanizing Equipment) The all radiant tube (ART: All Radiant Tube) type continuous hot-dip galvanizing equipment according to this embodiment does not have an oxidation zone in the continuous furnace. Therefore, by appropriately controlling the annealing dew point, it is possible to suppress the formation of internal oxides of Si in the surface layer of the steel sheet. As a result, in the region from the surface of the steel sheet to 3 μm in the sheet thickness direction, SiO2 The area ratio of the above can be set to less than 0.4%.
[0058] In the continuous plating process according to this embodiment, reduction annealing is performed in an atmosphere of 2 to 10 vol% hydrogen and 0.002 vol% to 0.05 vol% water vapor. During this process, the maximum surface temperature of the base steel sheet is set to 775°C or higher, and the residence time at 750°C or higher is set to 30 seconds or longer. By reducing the base steel sheet under these reduction conditions, SiO 2 The area ratio of the hot-dip galvanized steel sheet can be less than 0.4%. The maximum temperature may be 900°C or less. The residence time may be 150 seconds or less. By setting the maximum temperature to 775°C or more and the residence time at 750°C or more to 30 seconds or more, the tensile strength of the steel sheet can be 740 MPa or more. If the water vapor concentration exceeds 0.05 vol%, the plating wettability is improved, but workability is reduced, which is not preferable. In order to obtain the hot-dip galvanized steel sheet according to this embodiment, the water vapor concentration is set to 0.002 vol% or more.
[0059] The dew point during reduction annealing is preferably −30° C. or lower. By setting the dew point to −30° C. or lower, it is possible to prevent the formation of SiO in the region from the surface of the steel sheet to 3 μm in the sheet thickness direction. 2 The area ratio can be easily set to less than 0.4%.
[0060] log(PH) during reduction annealing 2 O / PH 2 ) is preferably −2.20 to −1.00. 2 O indicates the partial pressure of water vapor, and PH 2 indicates the partial pressure of hydrogen. 2 O / PH 2 ) is -2.20 to -1.00, SiO 2 The area ratio can be easily set to less than 0.4%.
[0061] The base steel sheet after reduction annealing is immersed for 3 seconds or more in a coating bath having the same composition as the second chemical composition under the following condition A or condition B. The immersion time may be 10 seconds or less. By immersing the base steel sheet having the first chemical composition under condition A or condition B for 3 seconds or more, the coating wettability can be improved. Fe diffuses into the coating bath and reacts with the coating bath, forming an Al-Fe-based interfacial alloy layer at the interface between the coating layer and the steel sheet. Furthermore, the Al-Fe-based interfacial alloy layer can be set to 1 to 3 μm. If the coating bath temperature exceeds 520°C, the thickness of the Al-Fe-based interfacial alloy layer will exceed 3 μm, and the workability of the hot-dip coated steel sheet according to this embodiment will decrease. Condition A: Coating bath temperature 470°C to 520°C and entry material temperature 470°C to 520°C. Condition B: Coating bath temperature 450°C to less than 470°C and entry material temperature 490°C to 520°C.
[0062] The immersion time in the plating bath is 3 seconds or more. If the immersion time in the plating bath is less than 3 seconds, the plating area ratio will not be 99% or more.
[0063] Next, the base steel sheet with the molten metal attached thereto is removed from the coating bath. The steel sheet with the molten metal attached thereto is subjected to gas wiping to control the coating weight of the coating layer. The coating weight of the coating layer is not particularly limited and can be, for example, within the above-mentioned range.
[0064] Next, after controlling the coating weight of the coating layer, the adhered molten metal is cooled to solidify. Cooling is continuously performed on the steel sheet with the molten metal attached immediately after being pulled up from the coating bath until the temperature of the molten metal drops from the bath temperature to 300°C. The cooling method may be spraying nitrogen, air, or a hydrogen-helium mixed gas, or mist cooling. The cooling conditions below 300°C are not particularly limited, and subsequent mist cooling may be performed, or the sheet may be air-cooled or allowed to cool naturally. The average cooling rate between the bath temperature and 300°C is, for example, 10°C / second or more.
[0065] The hot-dip galvanized steel sheet of the present disclosure has excellent workability and appearance, and is also excellent in the SiO 2Because oxide formation is suppressed, it can be used suitably for solar cell mounting, etc. Because the steel sheet has excellent plating adhesion, it can be processed more heavily than conventional steel sheets, and the number of parts can be reduced, which reduces the cost of manufacturing parts and the construction cost of assembling parts on site.
[0066] Examples of the present invention will be described below. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0067] The base steel sheet used had the chemical composition shown in Table 1. Next, the base steel sheet was subjected to reduction annealing under the conditions shown in Tables 2A and 2B. The base steel sheet after reduction annealing was then galvanized under the conditions shown in Tables 3A and 3B. The base steel sheet was removed from the galvanizing bath and gas wiped to adjust the coating weight, and then cooled with nitrogen gas. All radiant tube type continuous hot-dip galvanizing equipment without an oxidation zone was used for the galvanization except for Experiment No. 26. Experiment No. 26 was galvanized using continuous hot-dip galvanizing equipment with an oxidation zone.
[0068] (Chemical composition of the plating layer: thickness of the Al-Fe-based interface alloy layer and SiO in the region from the surface of the steel sheet to 3 μm in the thickness direction) 2 Evaluation of the area ratio of the obtained coating layer, the thickness of the Al-Fe-based interface alloy layer, and the area ratio of SiO in the region from the surface of the steel sheet to 3 μm in the thickness direction 2 The area ratios were evaluated by the methods described above. The results are shown in Tables 4A, 4B, 4C, and 4D.
[0069] (Tensile Strength) Tensile strength (TS) was evaluated for the steel sheet after peeling the coating layer from the obtained hot-dip plated steel sheet. Peeling was performed using the same method as used for analyzing the chemical composition of the coating layer described above. JIS No. 5 tensile test specimens were taken in a direction perpendicular to the rolling direction of the steel sheet, and tensile tests were performed in accordance with JIS Z 2241:2011 to determine the tensile strength. The results are shown in Tables 4A, 4B, 4C, and 4D. Similarly, the tensile strength was evaluated for the base steel sheet after reduction annealing. The results are shown in Table 1.
[0070] (Plating evaluation) The plating evaluation was carried out with the following criteria: an area ratio of the plating layer of 99% or more was rated as "good," an area ratio of the plating layer of 67% or more but less than 99% was rated as "fair," and an area ratio of the plating layer of less than 67% was rated as "poor." An area ratio of the plating layer of 99% or more was rated as "pass." The results are shown in Tables 4A, 4B, 4C, and 4D.
[0071] (Evaluation of Workability) Workability was evaluated based on the adhesion of the plating layer. Steel sheets with a plating layer area ratio of 99% or more were evaluated. Each steel sheet was bent 180 degrees in accordance with JIS G 3323:2019. The inner spacing between the bent steel sheets was 3T (number of sheets). Tape was applied to the bent steel sheet, and the steel sheet was evaluated based on the area ratio (remaining area ratio) of the plating layer remaining after the tape was peeled off. A remaining plating layer area ratio of 99% or more was evaluated as ◯, a remaining plating layer area ratio of 67% or more but less than 99% was evaluated as △, and a remaining plating layer area ratio of less than 67% was evaluated as ×. Steel sheets with a remaining plating layer area ratio of 99% or more were evaluated as excellent workability and passed. Steel sheets with bare areas that were not evaluated were evaluated as "-". The results are shown in Tables 4A, 4B, 4C, and 4D.
[0072] As shown in Tables 4A, 4B, 4C, and 4D, the chemical composition of the steel sheet, the chemical composition of the coating layer, the thickness of the Al-Fe-based interface alloy layer, and the SiO content in the region from the surface of the steel sheet to 3 μm in the thickness direction are 2 In Examples 4 to 7, 10 to 12, 16 to 19, 29, 32, 35, 38, 41, 44, 47, 50, 53, 56, 59, 62, 65, 67, and 68 according to the present invention, in which the area ratio of SiO was appropriately controlled, were excellent in both appearance and workability. In addition, because the galvanizing was performed using an all-radiant tube type continuous hot-dip galvanizing facility, the SiO in the region from the surface of the steel sheet to 3 μm in the thickness direction was 2 The area ratio of SiO 2 The formation of oxides was suppressed. The coating weight of the plating layer per side in the examples was, for example, 20 to 150 g / m 2 In Comparative Example 27, since the Si content in the steel sheet was low, even though the plating bath temperature and sheet temperature were outside the ranges, the area ratio of the plating layer was 99% or more, but the tensile strength was low.
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079]
[0080]
[0081]
[0082] The hot-dip galvanized steel sheet of the present disclosure has excellent workability and appearance, and is also excellent in the SiO 2 Since the formation of oxides is suppressed, the composition has high industrial applicability.
Claims
1. A steel sheet comprising: a steel sheet; and a plating layer provided on the steel sheet; wherein a first chemical composition of the steel sheet contains, in mass %, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, Si: 0.40% to 2.00%, P: 0.001% to 0.100%, S: 0.0001% to 0.0100%, and Al: 0.001% to 1.500%, with the balance being Fe and impurities; the steel sheet has a tensile strength of 740 MPa or more; and in a region from the surface of the steel sheet to 3 μm in the sheet thickness direction, 2 the area ratio of said Al-Fe-based interfacial alloy layer is less than 0.4%, a second chemical composition which is a chemical composition of said plating layer contains, in mass %, Al: 10% to 13%, Mg: 3% to 5%, and Si: 0.5% or less, with the balance being Zn and impurities, said plating layer includes an Al-Fe-based interfacial alloy layer in contact with the steel sheet surface, and a thickness of said Al-Fe-based interfacial alloy layer is 1.0 to 3.0 μm.
2. The hot-dip galvanized steel sheet according to claim 1, wherein the first chemical composition further contains, in mass%, one or more selected from the following: Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V: 0.001% to 0.300%.
3. The hot-dip galvanized steel sheet according to claim 1, wherein the first chemical composition further contains, in mass%, one or more elements selected from the following: Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, Mo: 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00%.
4. SiO 2 The hot-dip plated steel sheet according to claim 1 , wherein the area ratio of said hot-dip plated steel sheet is 0.1% or more.
5. The hot-dip galvanized steel sheet according to claim 1, wherein the first chemical composition further contains, in mass%, 0.0001% to 0.0100% in total of one or more of Ca, Mg, Zr and REM.
6. A method for manufacturing a galvanized steel sheet having a first chemical composition, comprising: a continuous plating process for plating a base steel sheet having a first chemical composition using an all-radiant tube type continuous hot-dip galvanizing facility; wherein, in the continuous plating process, the base steel sheet is reduction-annealed in an atmosphere of 2 to 10 vol% hydrogen and 0.002 vol% to 0.05 vol% steam under reducing conditions in which the maximum surface temperature of the base steel sheet is 775°C or higher and the residence time at 750°C or higher is 30 seconds or more; and the base steel sheet after the reduction annealing is immersed in a plating bath for 3 seconds or more at a plating bath temperature of 470°C to 520°C and an entry material temperature of 470°C to 520°C or at a plating bath temperature of 450°C to less than 470°C and an entry material temperature of 490°C to 520°C; and wherein the first chemical composition is, in mass%, C: 0.05% to 0.20%, Mn: 1.00% to 3.00%, Si: 0.40% to 2.00%, A method for producing a hot-dip galvanized steel sheet comprising: P: 0.001% to 0.100%, S: 0.0001% to 0.0100%, and Al: 0.001% to 1.500%, with the balance being Fe and impurities; and a chemical composition of the coating bath comprising, in mass%, Al: 10% to 13%, Mg: 3% to 5%, and Si: 0.5% or less, with the balance being Zn and impurities.
7. A stand using the hot-dip galvanized steel sheet according to claim 1.
Citation Information
Patent Citations
Zn-Al-Mg BASED HOT DIP PLATED STEEL HAVING EXCELLENT CORROSION RESISTANCE
JP2003003238A
Hot-dip galvanized steel sheet with excellent plating adhesion and method for manufacturing the same
JP2014505168A
Cited By
Hot-dip galvanized steel sheet
JP2026110914A
Hot-dip galvanized steel sheet
JP7849653B1
Hot-dip galvanized steel sheet
JP7849654B1
Hot-dip galvanized steel sheet
JP7935900B2
Hot-dip galvanized steel sheet
WO2026141047A1