Tungsten alloy, structure, and rhenium powder
The development of a tungsten alloy with controlled rhenium dispersibility and potassium doping addresses the non-uniformity issues in existing tungsten alloys, enhancing strength and high-temperature performance for applications requiring long-term discharge characteristics.
Patent Information
- Application Number
- PCT/JP2024/012902
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Tungsten alloys containing rhenium often fail to exhibit optimal electrical resistance, wear resistance, and tensile strength due to non-uniform dispersibility of rhenium, leading to issues with crack formation and reduced lifespan under high temperatures.
A tungsten alloy with rhenium is developed, ensuring a standard deviation of rhenium concentration of 1.0 wt% or less through precise dispersion of rhenium powder with a particle size of less than 0.5 μm, forming a solid solution with tungsten, and incorporating potassium as a dopant to enhance mechanical properties.
The solution achieves uniform strength, reduced crack occurrence, and long-term discharge characteristics by ensuring uniform rhenium dispersibility, improving the alloy's high-temperature performance and mechanical properties for applications like X-ray tubes and medical needles.
Smart Images

Figure JP2024012902_03102024_PF_FP_ABST
Abstract
Description
Tungsten alloys, structures and rhenium powder
[0001] SUMMARY OF THE INVENTION Embodiments of the present invention relate to tungsten alloys, structures, and rhenium powders.
[0002] Tungsten alloys containing rhenium are used in a variety of applications. For example, wires made of tungsten alloys containing rhenium have higher electrical resistance and wear resistance, and higher tensile strength or ductility than tungsten wires. Therefore, tungsten alloys containing rhenium are used in semiconductor inspection probe pins, heaters for electron tubes, filaments for earthquake-resistant light bulbs, thermocouples, filaments for fluorescent display tubes, medical needles, etc. In addition, tungsten has a high melting point and generates X-rays when irradiated with high-speed electron beams. By incorporating rhenium into tungsten, toughness is improved, roughness of the electron beam irradiated surface is suppressed, and the life span can be extended. Therefore, tungsten alloys containing rhenium are used as X-ray sources for X-ray tubes used in various applications such as medical and security.
[0003] However, if rhenium cannot be uniformly dispersed in tungsten, the above-mentioned characteristics cannot be fully exhibited.
[0004] Japanese Patent Laid-Open No. 7-204207 Japanese Patent Laid-Open No. 2002-75059
[0005] The problem to be solved is to provide a tungsten alloy containing rhenium, which has excellent rhenium dispersibility, a structure containing this tungsten alloy, and rhenium powder used as a raw material for this tungsten alloy.
[0006] According to an embodiment, a tungsten alloy containing rhenium is provided. Based on point analysis by scanning electron microscope / energy dispersive X-ray analysis for any six points on any cross section of the tungsten alloy, the standard deviation of the rhenium concentration is 1.0 wt% or less.
[0007] Also, according to the embodiment, a structure including the tungsten alloy of the embodiment is provided.
[0008] According to an embodiment, a structure is provided, comprising: a first member including at least one of molybdenum or a molybdenum alloy; and a second member stacked on the first member and including the tungsten alloy of the embodiment.
[0009] According to an embodiment, the rhenium powder is used as a raw material for a tungsten alloy, and when dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less, the number ratio of particles having a particle size of less than 0.5 μm is 20% or more. The rhenium powder has a frequency distribution.
[0010] 1 is a graph showing an example of a frequency distribution of particle diameters of a rhenium powder according to an embodiment; 2 is a schematic diagram showing an example of a rhenium powder according to an embodiment; 3 is a cross-sectional view showing an outline of an example of a structure according to an embodiment; 4 is a diagram showing an electron image of a tungsten alloy according to Example 1 by an electron probe microanalyzer (EPMA); 5 is a diagram showing an electron image of a tungsten alloy according to Comparative Example 1 by an electron probe microanalyzer;
[0011] The present inventors have focused on the relationship between the stability of discharge characteristics and the dispersibility of rhenium in tungstenalloy, and have found the following.Rhenium disperses in tungstenalloy in a state of solid solution with tungsten, and can improve the strength of tungstenalloy.By improving the dispersibility of rhenium, the strength of tungstenalloy can be made uniform, and therefore the existence of locally low strength parts of the material can be reduced.As a result, even when tungstenalloy is exposed to high temperatures, it is possible to reduce the occurrence of abnormal parts such as cracks.As a result, tungstenalloy can exhibit long-term discharge characteristics (electron emission characteristics).That is, in the tungstenalloy of the embodiment, the standard deviation of rhenium concentration based on the point analysis of any six points of any cross section by scanning electron microscope (SEM / EDX) / energy dispersive X-ray analysis is 1.0 wt% or less.
[0012] By making the standard deviation of rhenium concentration (wt%) less than 1.0 wt%, the dispersibility of rhenium in tungsten alloy can be improved.Therefore, rhenium can be dispersed uniformly in tungsten in a solid solution state, so the strength of tungsten alloy can be improved.As a result, even if tungsten alloy is exposed to high temperatures, it can reduce the occurrence of abnormal parts such as cracks, so it can exhibit long-term discharge characteristics.
[0013] The details of the point analysis using a scanning electron microscope / energy dispersive X-ray analysis (hereinafter referred to as SEM / EDX) are described below.
[0014] The shape of the tungsten alloy to be measured is not particularly important. For example, when the tungsten alloy has a disk-like, cylindrical or ring-like shape, the tungsten alloy is cut perpendicular to the diameter direction to take out small pieces.In addition, when the tungsten alloy has a cylindrical shape such as a wire rod, the tungsten alloy is cut parallel to the diameter direction to take out small pieces.The small pieces taken out are embedded in resin, and then mirror polished to obtain a sample.For the obtained sample, use SEM / EDX to observe three arbitrary fields of view at a magnification of 2000 times.Select two arbitrary positions for each field of view, and for each of a total of six positions, measure the rhenium concentration (wt%) in the tungsten alloy by a measuring method using energy dispersive X-ray analysis (EDX).That is, carry out point analysis to measure the rhenium concentration at only six positions selected from any one cross section of the tungsten alloy.It should be noted that the accelerating voltage during point analysis is preferably 15 kV. The average value (wt%) of the obtained rhenium concentrations (wt%) is calculated, and the standard deviation (wt%) is obtained.
[0015] As described in the above method, "any six locations on any cross section" means selecting six measurement regions from any one cross section.
[0016] In the tungstenalloy of the embodiment, confirmation that rhenium component and tungsten component form solid solution can be carried out for example by the following method.When observing the metal structure of tungstenalloy by SEM backscattered electron image, if Re region and W region are not clear, it is judged to be ReW solid solution.
[0017] The rhenium content of the tungstenalloy of the embodiment can be, for example, 2 wt% or more and 30 wt% or less. The rhenium content is a value analyzed by inductively coupled plasma-optical emission spectrometry (ICP-OES). By increasing the rhenium content of the tungstenalloy to 2 wt% or more, the elongation of tungsten at high temperatures can be improved, thereby enhancing workability. Furthermore, the strength of the tungstenalloy can be increased by solid solution strengthening. Furthermore, by increasing the rhenium content of the tungstenalloy to 30 wt% or less, the rhenium can be diffused and homogenized (solid-dissolved) in the tungsten matrix. As a result, the occurrence of a phase region with a locally high rhenium composition ratio (σ-phase segregation phase) can be suppressed. By increasing the rhenium content to 2 wt% or more and 30 wt% or less, the mechanical properties (strength and wear resistance) of structures such as probe pins and medical needles can be ensured. The rhenium content is preferably, for example, 2 wt % or more and 28 wt % or less, and more preferably, 2 wt % or more and 12 wt % or less.
[0018] The tungstenalloy of the embodiment may contain potassium (K) as a dopant in an amount of 30 wtppm or more and 90 wtppm or less. The potassium content is a value obtained by analysis using inductively coupled plasma optical emission spectroscopy (ICP-OES). By containing potassium, the tensile strength and creep strength at high temperatures can be improved due to the doping effect. By making the potassium content 30 wtppm or more, the doping effect can be sufficiently achieved. Furthermore, by making the potassium content 90 wtppm or less, the workability and yield of the tungstenalloy can be improved. By containing potassium in an amount of 30 wtppm or more and 90 wtppm or less as a dopant, for example, wires (e.g., thin wires) for thermocouples or electron tube heaters made from the tungstenalloy of the embodiment can be produced with high yield while ensuring high-temperature properties (preventing breakage and deformation during high-temperature use).
[0019] The tungstenalloy of the embodiment can be manufactured by the following method for example.<Regarding raw materials> As the raw material of tungstenalloy, tungsten powder and rhenium powder can be listed, but not limited to these, and necessary additives can be included in the raw material of tungstenalloy.
[0020] The rhenium powder preferably has an average particle size of less than 8 μm. The tungsten powder preferably has an average particle size of less than 16 μm. The tungsten powder is either pure tungsten powder excluding unavoidable impurities, or doped tungsten powder containing potassium (K) in an amount that takes into account the yield of the tungsten alloy. When the average particle size of the rhenium powder is 8 μm or more, or when the average particle size of the tungsten powder is 16 μm or more, the diffusion distance of the rhenium atoms or tungsten atoms increases, which facilitates the formation of a σ phase, in order to diffuse and homogenize (solid-solve) the rhenium into the tungsten matrix.
[0021] The average particle size of rhenium powder and tungsten powder is measured by laser diffraction. The amount of metal powder used for one measurement is the amount recommended for the measurement device. Generally, 0.02 g is recommended. The minimum amount is 0.01 g, and the maximum amount is 0.03 g. The measurement sample is thoroughly stirred before measurement and then weighed.
[0022] The ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder (average particle size of Re / average particle size of W) is preferably 0.1 or more and 2.0 or less. If the ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder is less than 0.1 or exceeds 2.0, the diffusion distance of the rhenium atoms to the center of the tungsten particle, or the diffusion distance of the tungsten atoms to the center of the rhenium particle, becomes long, and the σ phase may be easily generated.
[0023] The rhenium powder can be composed of rhenium particles having a frequency distribution in which the number ratio of particles having a particle size of less than 0.5 μm is 20% or more when dispersed at a vacuum level of -0.9 bar or more and -1.0 bar or less. If the number of particles having a particle size of less than 0.5 μm is 20% or more in the frequency distribution of the particle size of the rhenium powder, rhenium can be easily diffused into tungsten during alloying of rhenium and tungsten, allowing the rhenium component to be uniformly dispersed in the tungsten matrix. If the number of particles having a particle size of less than 0.5 μm is less than 20%, the dispersion of the rhenium component in the tungsten matrix may be non-uniform, or rhenium that is not solid-dissolved in tungsten may remain in the alloy. The number ratio of particles having a particle size of less than 0.5 μm in the frequency distribution is preferably 30% or more, and more preferably 50% or more.
[0024] Furthermore, for example, the rhenium powder can be composed of rhenium particles having a frequency distribution in which the proportion of particles with a particle size of less than 1 μm is 50% or more when dispersed at a vacuum of −0.9 bar or more and −1.0 bar or less.
[0025] Dispersion under the above vacuum can be carried out using a powder disperser. The measurement method using a powder disperser is described below.
[0026] The particle size of the rhenium powder is measured using a scanning electron microscope (SEM). Observation samples are prepared using a powder disperser, Nebula, manufactured by Pheno World, or a powder disperser with equivalent functionality. A pin stub with carbon tape attached is placed in the disperser, and the powder is dispersed onto the carbon tape. The vacuum level during dispersion can be, for example, -1.0 bar. If a powder disperser is not used, the rhenium particles will overlap, making accurate measurements impossible. Furthermore, if the vacuum level during dispersion is less than -0.9 bar, the dispersion force weakens, causing the rhenium powder to remain agglomerated, making accurate measurements impossible. The prepared samples are observed using a scanning electron microscope, ProX, manufactured by Pheno World, at a magnification of 20,000x, a field of view of 13.6 μm, and an accelerating voltage of 1.0 kV. Ten randomly selected fields are photographed, and the particle size of the photographed SEM images is measured using Phenom ParticleMetric Software manufactured by Phenom World. The observation position must be such that 100 or more particles can be captured in 10 fields of view. The number of captured particles is preferably 300 or more. The equivalent circular area diameter of all particles captured and measured by Phenom ParticleMetric Software is recorded, and the percentage of particles smaller than 0.5 μm in size relative to the total number of captured particles is calculated.
[0027] Figure 1 shows an example of a frequency distribution (histogram) of rhenium powder in which the number of particles with a particle size of less than 0.5 µm is 20% or more. The horizontal axis of Figure 1 represents the particle size (m) of the rhenium powder, and the vertical axis represents the frequency. In the frequency distribution shown in Figure 1, the total number of frequencies for the number of particles is about 400, and the number of particles with a particle size of 0.1 µm (0.1 x 10 ―6The frequency of the rhenium powder (m) exceeds 250. A schematic diagram of an example of an SEM image of the rhenium powder whose frequency distribution is shown in FIG. 1 is shown in FIG. 2. As shown in FIG. 2, rhenium particles 1 have a small particle size and little aggregation. <Mixing of Raw Powders> Tungsten powder and rhenium powder are mixed so that the rhenium content is 2 wt% or more and 30 wt% or less. The mixing method is not particularly limited, but examples include using an organic solvent-based solution that can suppress oxidation of the powder and achieve the desired effect at a low temperature in the drying process described below, and mixing the powder in a slurry form. This method is particularly preferred because it produces powder with good dispersibility. Furthermore, to ensure the homogeneity of the powder lot, it is even more preferable to dry-mix the same powder lot after drying the slurry. <Preparation of Compact> Next, the mixed powder is placed in a predetermined mold and press-molded to produce a compact. The pressing pressure at this time is preferably 150 MPa or more. The pressure is preferably 200 MPa or more and 500 MPa or less. If the pressure is less than 150 MPa, the density of the green body is insufficient, making it difficult to obtain a high-density sintered body, while if the pressure exceeds 500 MPa, cracks are likely to occur in the green body, which is undesirable. The green body obtained is sintered in a hydrogen atmosphere, an inert gas atmosphere such as argon, or in a vacuum. The sintering temperature is preferably 1900°C or higher, and more preferably 2100°C or higher. If the sintering temperature is less than 1900°C, the diffusion of rhenium atoms and atoms does not proceed sufficiently during sintering. The sintered body is forged as needed.
[0028] The tungstenalloy of the embodiment is not particularly limited in its application, but can be applied to the object that requires discharge characteristics (electron emission characteristics).The structure that includes the tungstenalloy of the embodiment can be exemplified as the target of X-ray tube, probe pin, heater for electron tube, filament, thermocouple, medical needle, wire etc.The probe pin of the embodiment includes the probe pin for semiconductor inspection.The filament of the embodiment includes the filament for earthquake-proof light bulb and the filament for fluorescent display tube.
[0029] The manufacturing method of rods and wires, such as thermocouples and wires, which are examples of the use of the tungsten alloy of the embodiment, will be described. The manufacturing method is not particularly limited, but the following method can be mentioned as an example. The processing is carried out until the required wire diameter is obtained.
[0030] Tungsten powder and rhenium powder are mixed so that the rhenium content is 2 wt% or more and 30 wt% or less. The mixing method is not particularly limited. A method of mixing the powders in a slurry form using water or an alcohol-based solution is particularly preferred because it produces a powder with good dispersibility. The rhenium powder to be mixed has an average particle size of, for example, less than 8 μm. The tungsten powder is either pure tungsten powder excluding unavoidable impurities, or doped tungsten powder containing a potassium amount that takes into account the yield of wire. The tungsten powder has an average particle size of, for example, less than 16 μm.
[0031] Next, the mixed powder is placed in a predetermined mold and press-molded. The pressing pressure is preferably 200 MPa or higher. To facilitate handling, the molded body may be pre-sintered in a hydrogen furnace at 1200°C to 1400°C. The resulting molded body is sintered in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum. The sintering temperature is preferably 1900°C or higher, more preferably 2100°C or higher, and even more preferably 2500°C or higher. If the sintering temperature is lower than 1900°C, the diffusion of rhenium and tungsten atoms during sintering will not proceed sufficiently. The upper limit of the sintering temperature is 3400°C (below the melting point of tungsten, 3422°C). If the upper limit of the sintering temperature exceeds the melting point of tungsten (3422°C), the molded body will not maintain its shape and may become defective. The relative density after sintering is preferably 90% or higher. By making the relative density of the sintered body 90% or more, it is possible to reduce the occurrence of cracks, chips, breaks, etc. in the subsequent swaging process.
[0032] Molding and sintering may be performed simultaneously by hot pressing in a hydrogen atmosphere, an inert gas atmosphere such as argon, or in a vacuum. The pressing pressure is preferably 100 MPa or more, and the heating temperature is preferably 1700°C to 2825°C. This hot pressing method can produce a dense sintered body even at a relatively low temperature.
[0033] As rhenium powder, use rhenium particles with a frequency distribution in which the number proportion of particles with particle diameter less than 0.5 μm is 20% or more when dispersed under the vacuum degree of -0.9 bar or more and -1.0 bar or less, can suppress the aggregation of rhenium particles, and reduce the generation of lumps of rhenium particles.Therefore, even in the manufacture of rod material and wire material such as wire, Re diffusion proceeds at a relatively low temperature, and can obtain the sintered body of the tungstenalloy of the embodiment at a sintering temperature of 1900 ° C or more.
[0034] The sintered body obtained in this sintering step is subjected to a first rolling and punching process (SW process). The first SW process is preferably carried out at a heating temperature of 1300°C or higher and 1600°C or lower. The reduction rate of the cross-sectional area (area reduction rate) in one heat treatment (one heat) is preferably 5% or higher and 15% or lower. After the first SW process, heat treatment is carried out to control the crystal orientation. Since the sintered body does not have a true density after the first SW process, strain in the sintered body is likely to become non-uniform. For this reason, non-uniformity is removed by heat treatment. Heat treatment can be carried out by direct resistance heating in a hydrogen atmosphere, for example. In the case of direct resistance heating, the current is 14 A / mm 2 More than 17A / mm 2 The current value is preferably 14 A / mm or less. 2 If the current is less than 17 A / mm, the strain relief in the first SW process will be insufficient. 2 If the strain exceeds this value, uneven strain will cause coarse recrystallization at the outer periphery of the cross section of the sintered body, making the structure uneven. This makes it difficult to control the crystal orientation.
[0035] After the first SW processing and heat treatment, rolling processing (RM (rolling machine) processing) is performed. The RM processing is preferably performed at a heating temperature of 1200°C or higher and 1600°C or lower. The area reduction rate per heat is preferably 40% or higher and 75% or lower. As the rolling mill, a two-way roller rolling mill, a four-way roller rolling mill, a die roll rolling mill, or the like can be used. RM processing makes it possible to significantly improve manufacturing efficiency.
[0036] The sintered body (rhenium tungsten rod) after RM is subjected to a second SW process. The second SW process is preferably performed at a heating temperature of 1200°C or higher and 1500°C or lower. The area reduction rate per heat is preferably about 5% or higher and 20% or lower.
[0037] The rhenium tungsten rod after the second SW process is then subjected to a recrystallization treatment. The recrystallization treatment is preferably carried out, for example, using a high-frequency heating device in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum, at a treatment temperature in the range of 1900 ° C or more and 2100 ° C or less. If the heat treatment temperature is below 1900 ° C, the recrystallization treatment is insufficient, and the processed structure and the recrystallized structure are likely to be mixed. If the heat treatment temperature exceeds 2100 ° C, coarse recrystallization occurs, and the structure is likely to become non-uniform. By carrying out the treatment in the range of 1900 ° C or more and 2100 ° C or less, it is possible to control the crystal orientation.
[0038] The rhenium-tungsten rod that has completed the recrystallization treatment is subjected to a third SW process. The third SW process is preferably carried out at a heating temperature of 1200°C or higher and 1500°C or lower. The area reduction rate per heat is preferably approximately 10% or higher and 30% or lower. The third SW process is carried out until the rhenium-tungsten rod has a diameter that can be drawn (preferably a diameter of 2 mm or higher and 4 mm or lower).
[0039] The rhenium-tungsten rod that has completed the third SW process is subjected to a first wiredrawing process from a diameter of 1.2 mm or less to 0.3 mm. The first wiredrawing process is preferably performed in a temperature range of 600 ° C or higher and 1100 ° C or lower. In the rhenium-tungsten wire of this embodiment, it is necessary to form a sufficient oxide film on the tungsten surface in order to allow the carbon-based lubricant to sufficiently penetrate the surface during the wiredrawing process, and it is desirable to perform annealing treatment multiple times at 900 ° C or higher and 1200 ° C or lower in an oxidizing atmosphere between a diameter of 1.2 mm or less and 0.3 mm. If the temperature is below 900 ° C, the oxide film is not sufficiently formed, the lubricating effect is insufficient, and the wire is prone to breakage. On the other hand, if the temperature exceeds 1200 ° C, the strength of the rhenium-tungsten wire itself decreases, causing breakage during wiredrawing, so the above temperature range is preferable.
[0040] The ReW wire that has undergone the first wiredrawing process is then subjected to a second wiredrawing process to reduce the diameter from 0.3 mm to 0.05 mm. The second wiredrawing process is preferably performed at a temperature of 500°C to 800°C. The workable temperature varies depending on the wire diameter, with the larger the diameter, the higher the temperature. If the temperature is lower than the workable temperature, cracks and wire breakage occur frequently. If the temperature is higher than the workable temperature, seizure occurs between the ReW wire and the die, and the deformation resistance of the rhenium-tungsten wire decreases, causing fluctuations in the diameter after wiredrawing (thinning) due to the drawing force. The area reduction rate is preferably 15% to 35%. If it is less than 15%, differences in the internal and external structure and residual stress occur during the process, causing cracks. If it is greater than 35%, the drawing force becomes excessive, causing large fluctuations in the diameter after wiredrawing and resulting in breakage. The wiredrawing speed is determined by the balance between the capacity of the heating device, the distance from the device to the die, and the area reduction rate. Polishing may be performed during the wiredrawing process.
[0041] Polishing can be performed by electrochemical polishing (electrolytic polishing) in a sodium hydroxide solution with a concentration of 7 wt% to 15 wt%. Heat treatment for strain relief (to prevent recrystallization) can also be performed. Rhenium-tungsten wire with a diameter of 0.05 mm to 0.3 mm can be produced by wire drawing. Mechanical grinding, such as centerless grinding, can also be used.
[0042] Another example of the structure that comprises the tungstenalloy of the embodiment can be a laminate that comprises a first member that comprises at least one of molybdenum or molybdenum alloy, and a second member that comprises the tungstenalloy of the embodiment, laminated on the first member.This laminate can be used for the target of X-ray tube, such as X-ray tube anode target.
[0043] The molybdenum alloy of the first member is not particularly limited, but in addition to Mo, it can contain, for example, at least one selected from the group consisting of oxygen, carbon, titanium, zirconium, titanium carbide, hafnium carbide, zirconium carbide, and tantalum carbide.
[0044] The shape of the first member is not particularly limited as long as it has a first surface onto which the second member is laminated.
[0045] The laminate may further include a third member containing carbon. The third member may be provided at a location on the first member different from the location on the first member where the second member is provided. For example, the third member may be laminated on the second surface of the first member. The second surface may be provided at a position facing the first surface of the first member across the first member.
[0046] A structure comprising a first member and a second member can be manufactured, for example, by the method described below. <Press molding> A mixed powder consisting of raw material powders is prepared according to the raw material powder mixing process in the production of a tungsten alloy. The prepared mixed powder is placed in a predetermined mold and press-molded to produce a compact. The pressing pressure at this time is desirably 200 MPa or more, preferably 200 MPa or more and 500 MPa or less. If the pressure is less than 200 MPa, the density of the compact is insufficient, making it difficult to obtain a high-density sintered body. On the other hand, if the pressure exceeds 500 MPa, cracks are likely to occur in the compact, which is not preferable. The first member containing a molybdenum alloy and the second member containing a tungsten alloy can be molded and sintered together, or they can be sintered separately and then integrated.
[0047] The obtained compact is sintered in a hydrogen atmosphere, an inert gas atmosphere such as argon, or a vacuum. The sintering temperature is preferably 1900°C or higher, and more preferably 2100°C or higher. If the sintering temperature is lower than 1900°C, the diffusion of rhenium atoms and tungsten atoms during sintering does not proceed sufficiently. The sintered compact is forged as needed. After processing into the product shape, a degassing treatment may be performed as needed.
[0048] Through the above steps, the structure of the embodiment can be obtained.
[0049] An example in which the structure of the embodiment is applied to an X-ray tube anode target will be described with reference to FIG. 3 . The X-ray tube anode target 3 shown in FIG. 3 can generate X-rays by irradiating an electron beam onto an electron beam irradiation surface. The X-ray tube anode target 3 includes a rotating shaft 4, a first member 5 attached to the rotating shaft 4 and having an electron beam irradiation surface, and a second member 7 attached to the first member 5. The first member 5 includes a first rotating body 6a containing a molybdenum alloy and a second rotating body 6b containing a molybdenum alloy. The molybdenum alloy of the first rotating body 6a may be the same as or different from the molybdenum alloy of the second rotating body 6b. The first rotating body 6a has a generally truncated cone shape and a through-hole near its center through which the rotating shaft 4 is inserted. The second rotating body 6b has a generally ring shape and is inclined near its outer periphery, with a through-hole near its center communicating with the through-hole of the first rotating body 6a. The second rotating body 6b is attached to the side of the first rotating body 6a with the inclined surface. The outer surface of the second rotor 6b functions as an electron beam irradiation surface. The second member 7 has a ring shape and is provided at a predetermined position on the electron beam irradiation surface of the second rotor 6b. The second member 7 can function as an electron impact buffer layer for buffering the impact received during electron beam irradiation.
[0050] Although not shown in Fig. 3, the X-ray tube anode target 3 may include a third member containing carbon. The third member containing carbon can be provided on the surface of the first rotor 6a opposite to the second rotor 6b side (the lower surface in Fig. 3).
[0051] According to the structure of the embodiment described above, since it contains the tungsten alloy of the embodiment, it can maintain the required performance such as discharge performance for a long period of time.
[0052] The examples will be described in detail below.
[0053] Example 1 A structure was fabricated by the method described below.
[0054] Rhenium powder with an average particle size of 2.9 μm and tungsten powder with an average particle size of 13 μm were used as raw material powders. The particle size distribution of the rhenium powder was measured using the method described above when the powder was dispersed at a vacuum of -1.0 bar using a powder disperser. Table 1 shows the measurement results, including the number of trapped particles (pcs (pieces)), the number of particles (pcs) with a particle size less than 1 μm, the proportion (%) of particles with a particle size less than 1 μm in the number of trapped particles, the number of particles (pcs) with a particle size less than 0.5 μm, and the proportion (%) of particles with a particle size less than 0.5 μm in the number of trapped particles. As shown in Table 1, the rhenium powder had a frequency distribution in which the proportion of particles with a particle size less than 0.5 μm was 20% or more when dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less.
[0055] The ratio of the average particle size of the rhenium powder to the average particle size of the tungsten powder (average particle size of Re / average particle size of W) was 0.22.
[0056] Rhenium powder and pure tungsten powder were mixed in a ketone solution to form a slurry containing 3 wt % rhenium, and the resulting slurry was dried to obtain a mixed powder made of the raw material powders.
[0057] The mixed powder and the molybdenum alloy were press-molded to obtain a compact having a two-layer structure of the mixed powder and the molybdenum alloy. The compact was sintered in a hydrogen atmosphere at 2100°C for 12 hours to obtain a sintered body. The sintered body was then hot-forged in a hydrogen atmosphere at a heating temperature of 1600°C, with a forging ratio of 10%, which is the rate of change in thickness of the forged body before and after forging. The forged body was then annealed in a hydrogen atmosphere at 1600°C for 30 minutes to remove strain.
[0058] The forged body was machined and the rhenium-tungsten alloy portion was ground to create the desired shape.
[0059] The processed product was subjected to VT treatment in a vacuum at a temperature of 1600°C for 5 hours to remove gas components, and a structure was obtained as a finished product, which had a disk-shaped first member containing a molybdenum alloy and a disk-shaped second member containing a tungsten alloy and was stacked on one end surface of the first member.
[0060] The second member of the structure was cut perpendicular to the radial direction (diameter direction) to extract small pieces. The extracted small pieces were embedded in resin and then mirror-polished to obtain samples. Three arbitrary fields of view were observed for the obtained samples at a magnification of 2000x using SEM / EDX. Two arbitrary locations were selected for each field of view, and the rhenium concentration (wt%) in the tungsten alloy was measured for a total of six locations by point analysis using EDX. The details of the point analysis are as described above. The average value (wt%) was calculated from the obtained rhenium concentration (wt%), and the standard deviation (wt%) was obtained. These results, the average particle size (μm) of the rhenium powder used as the raw material, the average particle size (μm) of the tungsten powder, and the ratio (Re average particle size / W average particle size) are shown in Tables 2 and 4.
[0061] Example 2 A rhenium-tungsten alloy and a structure were produced in the same manner as in Example 1, except that rhenium powder and pure tungsten powder were mixed so that the rhenium content was 2 wt %.
[0062] Example 3 A rhenium-tungsten alloy and a structure were produced in the same manner as in Example 1, except that rhenium powder and pure tungsten powder were mixed so that the rhenium content was 27.5 wt %.
[0063] Example 4 A rhenium-tungsten alloy and a structure were produced in the same manner as in Example 1, except that rhenium powder with an average particle size of 7.6 μm was used.
[0064] Example 5 A rhenium tungsten alloy and a structure were produced in the same manner as in Example 1, except that tungsten powder with an average particle size of 15.5 μm was used.
[0065] Example 6 A rhenium-tungsten alloy and a structure were produced in the same manner as in Example 1, except that rhenium powder having an average particle size of 7.6 μm and tungsten powder having an average particle size of 8.0 μm were used.
[0066] Example 7 A rhenium-tungsten alloy and a structure were produced in the same manner as in Example 1, except that rhenium powder having an average particle size of 1.6 μm and tungsten powder having an average particle size of 15.5 μm were used.
[0067] The particle size distribution of the rhenium powder used in Examples 4, 6, and 7 was measured by the method described above when the powder was dispersed at a vacuum of -1.0 bar using a powder disperser, as in Example 1. Table 3 shows the measurement results, including the number of trapped particles (pcs (pieces)), the number of particles (pcs) having a particle size less than 1 μm, the proportion (%) of particles having a particle size less than 1 μm in the number of trapped particles, the number of particles (pcs) having a particle size less than 0.5 μm, and the proportion (%) of particles having a particle size less than 0.5 μm in the number of trapped particles. As shown in Table 3, the rhenium powder used in Examples 4, 6, and 7 had a frequency distribution in which the proportion of particles having a particle size less than 0.5 μm was 20% or more when dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less. Table 3 also shows the results of Example 1.
[0068] In addition, for the second member of the structure according to embodiment 2 to embodiment 7, the rhenium concentration (wt%) in tungstenalloy is measured by the same method as embodiment 1, and standard deviation (wt%) is obtained.These results, the average particle diameter (μm) of the rhenium powder used as raw material, the average particle diameter (μm) of the tungsten powder, and Re / W (average particle diameter of Re / average particle diameter of W) are shown in table 4.In addition, table 4 also shows the results of embodiment 1.
[0069] Comparative Example 1 A structure was produced in the same manner as in Example 1, except that the rhenium powder described below was used as the raw material rhenium powder.
[0070] The rhenium powder used as the raw material had an average particle size of 13 μm. The particle size distribution of this rhenium powder was measured using the method described above when it was dispersed at a vacuum of -1.0 bar using a powder disperser. Among the measurement results, the number of trapped particles (pcs), the number of particles (pcs) having a particle size of less than 1 μm, the proportion (%) of particles having a particle size of less than 1 μm to the number of trapped particles, the number of particles (pcs) having a particle size of less than 0.5 μm, and the proportion (%) of particles having a particle size of less than 0.5 μm to the number of trapped particles are shown in Table 1. As shown in Table 1, the rhenium powder had a frequency distribution in which the proportion of particles having a particle size of less than 0.5 μm was less than 20% when it was dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less.
[0071] Comparative Example 2 A structure was produced in the same manner as in Example 1, using a rhenium powder having an average particle size of 2.9 μm as a raw material, different from the rhenium powder used in Example 1. The particle size distribution of this rhenium powder was measured using the method described above when it was dispersed at a vacuum of -1.0 bar using a powder disperser. Among the measurement results, the number of trapped particles (pcs), the number of particles (pcs) having a particle size of less than 1 μm, the proportion (%) of particles having a particle size of less than 1 μm to the number of trapped particles, the number of particles (pcs) having a particle size of less than 0.5 μm, and the proportion (%) of particles having a particle size of less than 0.5 μm to the number of trapped particles are shown in Table 3. As shown in Table 3, the rhenium powder had a frequency distribution in which the proportion of particles having a particle size of less than 0.5 μm was less than 20% when it was dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less.
[0072] For the tungstenalloy of the structure obtained in comparative example 1 and comparative example 2, the average value of rhenium concentration (weight%), standard deviation (weight%) is measured by the same method as in example 1, and the result, and the average particle size (μm) of the rhenium powder that is used as raw material, the average particle size (μm) of tungsten powder, and its ratio (average particle size of Re / average particle size of W) are shown in table 2 and table 4.
[0073]
[0074]
[0075]
[0076]
[0077] For the tungstenal alloy of embodiment 1 and comparative example 1, use electron probe microanalyzer (EPMA) to carry out elemental mapping analysis of Re, and the Re elemental mapping image of the tungstenal alloy of embodiment 1 is shown in Figure 4, and the Re elemental mapping image of the tungstenal alloy of comparative example 1 is shown in Figure 5.As shown in Figure 4, the Re elemental mapping image of the tungstenal alloy of embodiment 1 has little color unevenness, and it can be seen that Re exists relatively evenly.In addition, as shown in Figure 5, the Re elemental mapping image of the tungstenal alloy of comparative example 1 has a lot of color unevenness, such as partially existing dark colored part, and it can be seen that Re is unevenly distributed in specific location.
[0078] X-ray tubes were fabricated by using the target alloys of the structures of Examples 1 to 7, Comparative Examples 1 and 2 as targets, attaching shafts (rotating shafts), and incorporating them into X-ray tubes. The number of discharges while outputting 30,000 X-rays (rotation speed 8,000 rpm) using each X-ray tube was evaluated. The results are shown in Table 5.
[0079]
[0080] As can be seen from table 5, the target of embodiment 1 to embodiment 7 has 0 discharge times while outputting 30,000 times of X-ray (rotation speed 8,000 rpm), and can output 30,000 times or more of X-ray in one discharge.On the other hand, the target of comparative example 1 and 2 has 15 or more discharge times while outputting under the same conditions.The tungstenalloy used for the target of embodiment 1 to embodiment 7 has excellent dispersibility of rhenium, so can realize long-term electron emission characteristics.
[0081] Example 8 The same rhenium powder and pure tungsten powder as in Example 1 were mixed and molded to obtain a sintered body so that the rhenium content was 26 wt %. From this sintered body, a rhenium-tungsten wire rod with a diameter (φ) of 3 mm was produced using the above-mentioned method for processing rods and wires, and processed into a thermocouple.
[0082] Example 9 The same rhenium powder and pure tungsten powder as in Example 1 were mixed and molded to obtain a sintered body so that the rhenium content was 5 wt %. From this sintered body, a rhenium-tungsten wire rod with a diameter (φ) of 3 mm was produced using the above-mentioned method for processing rods and wires, and processed into a thermocouple.
[0083] Comparative Example 3 Using the same powder as in Comparative Example 2 as the raw material powder, a rhenium-tungsten wire rod having a diameter (φ) of 3 mm was produced in the same manner as in Example 8, and processed into a thermocouple.
[0084] The rhenium tungsten wire rods of Example 8 and Comparative Example 3 were cut parallel to the diameter direction to extract small pieces. The extracted small pieces were embedded in resin and then mirror-polished to obtain samples. Three arbitrary fields of view were observed for the obtained samples at a magnification of 2000x using SEM / EDX. Two arbitrary locations were selected for each field of view, and the rhenium concentration (wt%) in the tungsten alloy was measured for a total of six locations by point analysis using EDX. The details of the point analysis are as described above. The average value (wt%) was calculated from the obtained rhenium concentration (wt%), and the standard deviation (wt%) was obtained. These results, the average particle size (μm) of the rhenium powder used as the raw material, the average particle size (μm) of the tungsten powder, and the ratio (Re average particle size / W average particle size) are shown in Table 4.
[0085] Thermocouples consisting of Examples 8 and 9, and Comparative Examples 3 and 9 were fabricated. The resulting thermocouples are designated as the thermocouple of Example 8 and the thermocouple of Comparative Example 3, respectively. The electromotive force at 2000°C was measured simultaneously with a reference thermocouple conforming to ASTM E 230-11, and the error relative to the reference thermocouple was evaluated. The error relative to the reference is shown in Table 6.
[0086]
[0087] As can be seen from table 6, the thermocouple of embodiment 8 has smaller error than the thermocouple of comparative example 3.From this result, the tungsten alloy that is used for the thermocouple of embodiment 8 has excellent dispersibility of Re, so the Re content in wire becomes uniform, can output the thermoelectric power close to standard, and can reduce the measurement variation.
[0088] As shown in the above-mentioned results, the tungstenalloy of embodiment 1 to embodiment 8 improves the dispersibility of Re, so can improve the high-temperature discharge characteristics of tungstenalloy and the structure that contains it, and can reduce the measurement variation of the thermocouple that uses tungstenalloy.
[0089] According to the tungstenalloy of at least one of these embodiments, the standard deviation of the rhenium concentration based on the point analysis of any six places of any cross section by scanning electron microscope / energy dispersive X-ray analysis is 1.0wt% or less, therefore, can provide the tungstenalloy that improves the dispersibility of rhenium.
[0090] Although several embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents as defined in the claims.
[0091] The following are embodiments of the invention. <1> A tungsten alloy containing rhenium, wherein the standard deviation of the rhenium concentration based on point analysis by scanning electron microscope / energy dispersive X-ray analysis of any six locations on any cross section is 1.0 wt% or less. <2> The tungsten alloy according to <1>, wherein the rhenium content is 2 wt% or more and 30 wt% or less. <3> The tungsten alloy according to <1>, wherein the rhenium content is 2 wt% or more and 28 wt% or less. <4> The tungsten alloy according to <1>, wherein the rhenium content is 2 wt% or more and 12 wt% or less. <5> The tungsten alloy according to any one of <1> to <4>, wherein the rhenium is formed from rhenium powder having a frequency distribution in which the number ratio of particles having a particle size of less than 0.5 μm is 20% or more when dispersed at a vacuum level of -0.9 bar or more and -1.0 bar or less. <6> A structure comprising the tungstenalloy according to any one of <1> to <5>. <7> The structure according to <6>, which is at least one selected from the group consisting of an X-ray tube target, a probe pin, a heater for an electron tube, a filament, a thermocouple, a medical needle, and a wire. <8> A structure comprising: a first member containing at least one of molybdenum or a molybdenum alloy; and a second member laminated on the first member and containing the tungstenalloy according to any one of <1> to <5>. <9> The structure according to <8>, wherein the second member is laminated on a part of the first member, and further comprising a third member laminated on another part of the first member and containing carbon. <10> The structure according to <8>, which is a target for an X-ray tube. <11> A rhenium powder used as a raw material for the tungstenalloy according to any one of <1> to <5>, wherein the rhenium powder has a frequency distribution in which the number ratio of particles having a particle size of less than 0.5 μm is 20% or more when dispersed at a vacuum of -0.9 bar or more and -1.0 bar or less. <12> The rhenium powder according to <11>, wherein the dispersion is performed using a powder disperser. <13> The rhenium powder according to <11> or <12>, wherein the number ratio of particles having a particle size of less than 0.5 μm in the frequency distribution is 30% or more.
[0092] 1...Rhenium particle, 3...X-ray tube anode target, 4...rotating shaft, 5...first member, 6a...first rotating body, 6b...second rotating body, 7...second member.
Claims
1. A tungsten alloy containing rhenium, in which the standard deviation of the rhenium concentration based on point analysis by scanning electron microscope / energy dispersive X-ray analysis for any six points on any cross section is 1.0 wt% or less.
2. The tungsten alloy of claim 1, wherein the rhenium content is 2 wt.% or more and 30 wt.% or less.
3. The tungsten alloy of claim 1, wherein the rhenium content is from 2 to 28 wt.%.
4. The tungsten alloy of claim 1, wherein the rhenium content is greater than or equal to 2 wt.% and less than or equal to 12 wt.%.
5. The tungstenalloy of claim 1, wherein the rhenium is formed from rhenium powder having a frequency distribution in which the number ratio of particles having a particle size of less than 0.5 μm is 20% or more when the rhenium is dispersed under a vacuum of -0.9 bar or more and -1.0 bar or less.
6. A structure comprising the tungsten alloy according to any one of claims 1 to 5.
7. The structure according to claim 6, which is at least one selected from the group consisting of an X-ray tube target, a probe pin, a heater for an electron tube, a filament, a thermocouple, a medical needle, and a wire.
8. A structure comprising: a first member comprising at least one of molybdenum and a molybdenum alloy; and a second member laminated to the first member and comprising the tungsten alloy according to any one of claims 1 to 5.
9. The structure of claim 8, further comprising: a third member, the second member being laminated to a portion of the first member, and the third member being laminated to another portion of the first member, the third member comprising carbon.
10. The structure of claim 8 which is a target for an x-ray tube.
11. Rhenium powder used as a raw material for the tungsten alloy according to any one of claims 1 to 5, the rhenium powder having a frequency distribution in which the proportion of particles having a particle size of less than 0.5 μm is 20% or more when dispersed under a vacuum of -0.9 bar or more and -1.0 bar or less.
12. The rhenium powder of claim 11, wherein the dispersion is by a powder disperser.
13. The rhenium powder according to claim 11, wherein the number ratio of particles having a particle size of less than 0.5 μm in the frequency distribution is 30% or more.
Citation Information
Patent Citations
High modulus material for surgical needle
JP1995204207A
Rhenium tungsten wire, probe pin using it, charging wire for corona discharge and filament for fluorescent character tube, and their manufacturing methods
JP2002075059A
Preparation method of high-purity superfine rhenium powder
CN117620190A
Manufacture of powdered w-re mixture
JP1982023007A
Metal contained composition for electrical connection of electronic device
JP2004111254A