Aqueous coating material composition and method for forming multilayer coating film
The water-based coating composition, with its unique viscosity behavior and additive combination, addresses the adhesion and drying issues of traditional water-based paints, resulting in improved appearance and strength of the paint film through a multilayer coating film formation method.
Patent Information
- Application Number
- PCT/JP2024/013057
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-27
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Water-based paints face challenges with low adhesion to plastic surfaces, poor drying properties, and reduced workability due to low solid content and high volatility, which affects the appearance and strength of the paint film.
A water-based coating composition with a specific viscosity behavior, containing a resin, bright or colored pigments, and an extender pigment, along with a thixotropic agent, to achieve improved adhesion, drying properties, and workability, including a multilayer coating film formation method.
The composition and method result in a water-based coating with enhanced appearance, workability, and strength, addressing the limitations of traditional water-based paints by optimizing viscosity and pigment distribution.
Smart Images

Figure JP2024013057_03102024_PF_FP_ABST
Abstract
Description
Water-based paint composition and method for forming multi-layer paint film
[0001] The present invention relates to a water-based coating composition and a method for forming a multi-layer coating film.
[0002] Conventionally, organic solvent-based paints have generally been used to paint plastic materials (see, for example, Patent Document 1). Organic solvent-based paints contain organic solvents that etch the surface of plastic materials, and the resulting coating film adheres well to the etched surface due to its anchoring effect, making them suitable for use on plastics. However, organic compounds (hereinafter also referred to as VOCs) in paints are released into the atmosphere during painting and drying, causing air pollution and becoming a major environmental problem. Along with the trend toward stricter VOC regulations, various industries are actively moving toward solvent-free (VOC-free) paints.
[0003] Therefore, in recent years, the paint industry has been shifting from organic solvent-based paints to water-based paints that contain little or no VOCs, against the backdrop of these global environmental issues. Also, in the field of automotive interiors, the introduction of water-based paints is being promoted, taking into consideration the effects on the human body of organic solvents released from coatings and adhesives applied to interior materials in rooms that tend to be enclosed spaces, and the concerns of people who suffer from chemical hypersensitivity.
[0004] Plastic materials are primarily used in automotive interior parts and home appliances, but water-based paints do not contain sufficient organic solvents that etch the surfaces of plastic materials as described above, and therefore tend to have lower adhesion to plastic surfaces than organic solvent-based paints.
[0005] For example, Patent Document 2 discloses an aqueous coating composition, which is a glitter pigment dispersion containing water, a scaly aluminum pigment, and a cellulose-based viscosity modifier, and a method for forming a multilayer coating film using the same.
[0006] Patent Document 3 also discloses an aqueous multi-component coating composition comprising a main component (I) and a curing agent (II), wherein the main component (I) contains a hydroxyl-containing resin (A), the hydroxyl-containing resin (A) comprises a colloidal dispersion type acrylic resin (A1) and a water-soluble acrylic resin (A2), and the colloidal dispersion type acrylic resin (A1) is contained in an amount of 50% by mass or more relative to the total resin solids contained in the main component (I). This aqueous multi-component coating composition discloses that a coating film having excellent drying properties, paint handling properties, storage properties, weather resistance, and gloss finish suitable for large substrates can be obtained.
[0007] Japanese Patent Application Laid-Open No. 2018-069185 International Publication No. 2017 / 175468 Japanese Patent Application Laid-Open No. 2021-130812
[0008] However, the invention described in Patent Document 2 is limited to a metallic water-based paint containing a cellulose-based viscosity modifier. Furthermore, the invention described in Patent Document 3 improves the coating film appearance, coating workability, etc. of a two-component water-based coating composition, but does not propose solutions to the problems associated with one-component water-based coating compositions. Water-based coating compositions use a hydrophilic resin suitable for aqueous coating compositions, and because water is the primary solvent and has low volatility, they tend to drip easily and have poor coating workability. Furthermore, when water is the primary solvent, the solids content tends to be low during coating, which can result in poor coating film drying. Considering the impact of coating film drying on the coating film appearance and strength after coating, there is still room for improvement in the coating film appearance and strength after coating. The present invention was made in consideration of the above circumstances, and aims to provide a water-based coating composition and a method for forming a multilayer coating film that are excellent in at least one of coating film appearance, coating workability, coating film drying, and coating film strength.
[0009] The above-mentioned object of the present invention is achieved by the following means: [1] A water-based coating composition containing water, a resin, and at least one of a bright pigment and a color pigment, which exhibits the following viscosity behaviors (a) and (b) when the viscosity is adjusted to 430 mPa·s at a measurement temperature of 25°C. (a) When the shear rate is 1000 sec -1 The shear viscosity V1 at time T1 after 60 seconds has elapsed since the shear rate was set to 0.1 sec. -1 (b) The ratio V2 / V1 of the shear viscosity V2 at time T2, which is one second after time T1, to the shear viscosity V2 at time T2, which is one second after time T2, is 10 or more. (b) The ratio V3 / V2 of the shear viscosity V2 at time T2, which is one second after time T2, to the shear viscosity V3 at time T3, which is one second after time T2, is 1.3 or more. [2] The composition further contains an extender pigment, the resin is at least one of an acrylic resin and a urethane resin, and the extender pigment has a particle size D50 of 0.5 μm or more and a density of 4.2 g / cm 3
[0013] The aqueous coating composition according to [1], wherein the acrylic resin has a solid hydroxyl value of 2% or less, and the content of the extender pigment in the aqueous coating composition is 0.1% by mass or more but less than 25% by mass. [3] The aqueous coating composition according to [2], wherein the acrylic resin has a solid hydroxyl value of 2% or less. [4] The aqueous coating composition according to [2], wherein the extender pigment has an oil absorption of 21 ml / g or less. [5] The aqueous coating composition according to [2], wherein the extender pigment is barium sulfate. [6] The aqueous coating composition according to [1] or [2], further comprising a thixotropic agent, and wherein, when the viscosity of the aqueous coating composition at a measurement temperature of 25°C is adjusted to 430 mPa s, the solids content of the thixotropic agent in the aqueous coating composition is 0.1% by mass or more but less than 1.5% by mass. [7] The aqueous coating composition according to [1] or [2], wherein the solids concentration of the aqueous coating composition is 5% by mass or more and 50% by mass or less when the viscosity of the aqueous coating composition is adjusted to 430 mPa s at a measurement temperature of 25° C. [8] A method for forming a multilayer coating film, comprising: a base coating film-forming step of applying the aqueous coating composition according to any one of [1] to [7] onto an object to be coated to form a wet base coating film; a topcoat coating film-forming step of applying a topcoat coating composition onto the obtained wet base coating film to form a wet topcoat coating film; and a drying step of simultaneously drying the obtained wet base coating film and the wet topcoat coating film to form a multilayer coating film.
[0010] According to the present invention, it is possible to obtain a water-based coating composition and a method for forming a multi-layer coating film that are excellent in at least one of the appearance of the coating film, workability during application, drying properties of the coating film, and coating strength.
[0011] 1 is a graph showing the shear viscosity of one embodiment of the aqueous coating composition of the present invention.
[0012] The water-based coating composition of the present invention will be described in detail below.
[0013] [Water-based coating composition] The water-based coating composition of the present invention is a coating composition containing water, a resin, and at least one of a bright pigment and a color pigment, and when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU (approximately 430 mPa·s in mPa equivalent), the water-based coating composition has the following viscosity behaviors (a) and (b): (a) at a shear rate of 1000 sec -1 The shear viscosity V1 at time T1 after 60 seconds has elapsed since the shear rate was set to 0.1 sec. -1 and (b) V2 / V1, which is the ratio of shear viscosity V2 at time T2, one second after time T1, to shear viscosity V2 at time T2, is 10 or more. (c) V3 / V2, which is the ratio of shear viscosity V2 at time T2 to shear viscosity V3 at time T3, one second after time T2, is 1.3 or more. Here, "measurement temperature 25°C" refers to a state in which both the ambient temperature and the liquid temperature of the composition are 25°C. First, the components of the water-based paint composition will be described below.
[0014] <Water> In this specification, the term "water-based coating composition" refers to a coating composition containing water as the main solvent. "Main solvent" means that the proportion of the solvent used, i.e., water, is at least 50% by mass. The water used in the water-based coating composition of the present invention is not particularly limited, and examples include pure water such as ion-exchanged water and distilled water, groundwater, tap water, and industrial water. Furthermore, when storing the water-based coating composition for a long period of time, water that has been sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria.
[0015] (Organic Solvent) The aqueous coating composition of the present invention may contain an organic solvent. The content of the organic solvent in the aqueous coating composition is preferably 15% by mass or less, most preferably 10% by mass. From the viewpoint of VOC reduction, a low content of organic solvent is preferable. However, by using a small amount of organic solvent, for example, adhesion to plastic substrates can be improved, and in the case of an aqueous metallic coating composition, the dispersibility of the scaly metal pigment in the composition and the film-forming properties of the aqueous metallic coating composition can be maintained well. The organic solvent that can be used in the aqueous coating composition of the present invention is not particularly limited, and various hydrophilic or hydrophobic organic solvents can be used.
[0016] As the hydrophilic organic solvent, for example, an alcohol solvent or a glycol ether solvent is preferably used. Examples of the alcohol solvent include isobutyl alcohol, n-butyl alcohol, isoamyl alcohol, n-amyl alcohol, hexyl alcohol, 2-ethylbutyl alcohol, methylamyl alcohol, cyclohexanol, 2-ethylhexyl alcohol, octyl alcohol, benzyl alcohol, dimethylaminoethanol, and butanol. Examples of the glycol ether solvent include ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, and tetraethylene glycol dimethyl ether.
[0017] Examples of hydrophobic organic solvents include 2-ethylhexanol, dipropylene glycol monobutyl ether, and ethylene glycol monobutyl ether acetate. The ratio of hydrophilic organic solvents to hydrophobic organic solvents in the aqueous coating composition is preferably 100:0 or more and 33:67 or less.
[0018] When the aqueous coating composition of the present invention is applied directly to a plastic substrate, it is preferable that the coating composition contain 0.5% by mass or more and 5.0% by mass or less of an organic solvent having a high boiling point and high solubility in the substrate. In the case of aqueous coating, the organic solvent content is lower than in organic solvent-based coating, and therefore it is considered that the etching effect on the surface of plastic substrates is small. However, by using an organic solvent having a high boiling point and high solubility in the substrate, the highly soluble solvent remains on the substrate for a longer period after coating, and therefore it is thought that even a small amount of addition will show a high etching effect.
[0019] The high-boiling organic solvent preferably has a boiling point of 160° C. or higher, particularly preferably in the range of 180 to 300° C. Examples of such organic solvents include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, butyl glycol acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monopropyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, dipropylene glycol monomethyl ether, triethylene glycol monomethyl ether, triethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tetraethylene glycol dimethyl ether, and polyethylene glycol dimethyl ether.
[0020] An organic solvent that has high solubility in a substrate is an organic solvent that can dissolve the surface of a plastic substrate when dropped onto the substrate, and has an SP value (solubility parameter) of 20.0 (J / cm 3 ) 1/2 It is preferable that the saturation voltage is 18.0 (J / cm 3 ) 1/2It is more preferable that the organic solvent is not more than 100% by mass %. Furthermore, the type of organic solvent is preferably a glycol-based organic solvent, and more preferably a water-soluble glycol-based organic solvent. Examples of organic solvents having a high boiling point and high solubility in the substrate include triethylene glycol butyl methyl ether (boiling point: 261°C, SP value: 16.6), diethylene glycol diethyl ether (boiling point: 189°C, SP value: 17.8), diethylene glycol dimethyl ether (boiling point: 162°C, SP value: 18.2), diethylene glycol butyl methyl ether (boiling point: 212°C, SP value: 16.1), and tetraethylene glycol dimethyl ether (boiling point: 275°C, SP value: 17.5).
[0021] The SP value is a guideline for determining compatibility, and there are various calculation and measurement methods. In this specification, the SP value is the value of the Hansen solubility parameter, and is calculated using the Y-MB method.
[0022] -Method of calculating average SP value- When a plastic substrate is composed of n types of polymerizable compounds, the SP values of the polymerizable compounds are respectively SP1, SP2, ..., SPn, and the mass fractions of the polymerizable compounds are respectively W1, W2, ..., Wn (W1+W2+ ... +Wn=1), and the average SP value can be calculated using the following formula: average SP value=SP1×W1+SP2×W2+ ... +SPn×Wn
[0023] -Solids concentration of water-based coating composition- The solids concentration of the water-based coating composition of the present invention is preferably 5% by mass or more and 30% by mass or less when the viscosity is adjusted to 65 KU (approximately 430 mPa s in mPa equivalent). Furthermore, when a luster pigment is contained, it is particularly preferably 8% by mass or more and 20% by mass or less. By setting the solids concentration of the water-based coating composition within the above range, it is possible to improve the orientation of the pigment and the sagging properties during coating.
[0024] <Resin> The resin used in the aqueous coating composition of the present invention is appropriately selected taking into consideration the intended use, etc., and is not particularly limited, but examples thereof include acrylic resins, epoxy resins, urethane resins, alkyd resins, polyester resins, silicone resins, etc., and known resins such as amino resins, melamine resins, isocyanate resins, urea resins, etc. as crosslinking components. When a one-component aqueous coating composition is prepared, it is preferable to use acrylic resins, urethane resins, etc., taking into consideration the orientation of the pigment and coating workability. The resins in the present invention may be used alone or in combination of two or more.
[0025] (Acrylic Resin) The acrylic resin contained in the aqueous coating composition of the present invention may be any resin containing one or more (meth)acrylic monomers as constituent units, and may contain monomers other than (meth)acrylic monomers as constituent units as long as the effects of the present invention are not impaired. (Meth)acrylic monomer refers to a monomer having a (meth)acryloyl group, such as (meth)acrylic acid or a (meth)acrylic acid ester. For example, the constituent monomer of the acrylic resin used in the present invention is preferably an alkyl ester of (meth)acrylic acid, and the alkyl group in this ester preferably has 1 to 10 carbon atoms, particularly preferably 1 to 8 carbon atoms. A functional group may be introduced into this alkyl group, and this alkyl group may be a cyclic group. Examples of such constituent monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate.
[0026] Examples of the resin form of the acrylic resin include an acrylic emulsion resin that can be produced by emulsion polymerization, and an aqueous acrylic dispersion resin that can be produced by solution polymerization in a common organic solvent.
[0027] -Weight Average Molecular Weight Mw of Acrylic Resin- The weight average molecular weight Mw of the acrylic resin is not particularly limited, but is preferably 50,000 or more, and more preferably 100,000 or more. The weight average molecular weight Mw of the acrylic resin can be measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation). SEC conditions include using tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C, and using TSK standard polystyrene (manufactured by Tosoh Corporation) as the standard substance. Generally, emulsion resins obtained by emulsion polymerization tend to have large molecular weights, and emulsion resins having a crosslinked structure in particular cannot be accurately measured by gel permeation chromatography; therefore, in this specification, the molecular weight is set to 100,000 or more.
[0028] -Hydroxyl value of acrylic resin- When the aqueous coating composition of the present invention is used as a one-component coating, the hydroxyl value of the acrylic resin solid content is preferably 2% or less. If the hydroxyl value of the acrylic resin solid content exceeds 2%, many hydroxyl groups will remain in the coating film, resulting in reduced water resistance.
[0029] (Urethane Resin) The urethane resin used in the aqueous coating composition of the present invention can be any conventionally known urethane resin without any particular limitation. Examples include urethane resins obtained by reacting at least one diisocyanate compound selected from the group consisting of aliphatic diisocyanate compounds, alicyclic diisocyanate compounds, and aromatic diisocyanate compounds with at least one polyol compound selected from the group consisting of polyether polyols, polyester polyols, and polycarbonate polyols; and urethane resins obtained by reacting the above-mentioned acrylic resins, polyester resins, or epoxy resins with dipolyisocyanate compounds to obtain high molecular weight urethane resins.
[0030] <Brightening Pigment or Coloring Pigment> The aqueous coating composition of the present invention contains at least one of a brightening pigment or a coloring pigment. The brightening pigment and the coloring pigment are appropriately selected depending on the color and gloss of the coating film, coating workability, strength, physical properties, etc.
[0031] (Luminous pigment) Luminous pigment means a pigment that imparts metallic luster to the coating film by light reflection or interference, and examples thereof include aluminum powder pigment, nickel powder pigment, gold powder, silver powder, bronze powder, copper powder, stainless steel powder pigment, mica pigment, graphite pigment, glass flake pigment, metal-coated glass powder, metal-coated mica powder, metal-coated plastic powder, and scaly iron oxide pigment, with aluminum pigment being particularly preferred. Luminous pigments may be used alone or in combination of two or more, and are preferably present in an amount of 5% by mass or more and 30% by mass or less, more preferably 7% by mass or more and 20% by mass or less, of the solid content of the coating composition.
[0032] (Coloring Pigment) The coloring pigment is not particularly limited, and pigments commonly used in the paint industry can be used. Specific examples include inorganic pigments such as titanium dioxide, iron oxide, and carbon black, and organic pigments such as phthalocyanine pigments and azo pigments. The coloring pigment may be used alone or in combination of two or more, and is preferably present in an amount of 30% by mass or more and 70% by mass or less, and more preferably 40% by mass or more and 60% by mass or less, of the solid content of the paint composition.
[0033] (Extender Pigment) The water-based paint composition of the present invention may contain a body pigment. In this case, the body pigment has a particle diameter D50 of 0.5 μm or more and a density of 4.2 g / cm 3 By using an extender pigment having a particle size and density within the above ranges, it is possible to suppress an increase in the viscosity of the paint and increase the NV value (Nonvolatile content) during application. In addition, the particle size D50 of the extender pigment is 5.0 μm or less, and the density is 4.2 g / cm. 3 It is more preferable that the particle size D50 is 5.0 μm or less. By keeping the particle size D50 at 5.0 μm or less, it is possible to prevent unevenness caused by the pigment from appearing on the coating surface and to prevent the arrangement of other pigments from being disturbed, thereby achieving a good appearance. The particle size D50 is measured using an X-ray transmission sedimentation method particle size distribution analyzer in accordance with JIS Z 8825 "Particle size analysis - laser diffraction and scattering method."
[0034] The content of the extender pigment in the aqueous paint composition of the present invention is 0.1% by mass or more and less than 25% by mass. When the content of the extender pigment is 0.1% by mass or more, the drying properties of the paint film are good. Furthermore, when the content of the extender pigment is less than 25% by mass, the appearance of the paint film is good. The content of the extender pigment in the aqueous paint composition is preferably 5% by mass or more and 15% by mass or less, and more preferably 5% by mass or more and 10% by mass or less. The extender pigment may be used alone or in combination of two or more types.
[0035] The oil absorption of the extender pigment is preferably 5 ml / g or more and 30 ml / g or less, and more preferably 10 ml / g or more and 20 ml / g or less. When the oil absorption of the extender pigment is within the above range, the NV value can be increased while suppressing an increase in the viscosity of the paint, thereby improving workability during application and drying properties. The oil absorption of the extender pigment is a value determined in accordance with ISO-787-5 "General test methods for pigments and extender pigments - Part 5: Determination of oil absorption."
[0036] Examples of extender pigments include silica, talc, mica, calcium carbonate, barium sulfate, clay, etc. Among these, barium sulfate is preferred.
[0037] <Other Components> The aqueous coating composition of the present invention may contain various additives commonly used in the field of coatings, such as crosslinking components, thixotropic agents, dispersants, thickeners, neutralizing agents, antifoaming agents, surface conditioners, emulsifiers, surfactants, silane coupling agents, pH adjusters, and preservatives, within the scope of the present invention.
[0038] (Crosslinking component) When the substrate to be coated is metal, the aqueous coating composition of the present invention can be baked at high temperatures, so it may contain an acrylic resin, amino resin, melamine resin, urea resin, etc. with a high hydroxyl value. In addition, a blocked polyisocyanate can be used in the aqueous coating composition of the present invention when improving the storage stability of the coating at room temperature or when coating and drying on a plastic material such as polyimide with excellent heat resistance. From the viewpoints of storage stability and workability, such as ease of uniform mixing with the aqueous acrylic resin, it is more preferable to use a water-dispersible blocked polyisocyanate.
[0039] (Thixitropic Agent) The aqueous coating composition of the present invention can use any conventionally known thixotropic agent as the thixotropic agent, without any particular limitation. Examples include polymer association type thixotropic agents, alkali thickening type thixotropic agents, polyamide type thixotropic agents, polyethylene type thixotropic agents, and bentonite type thixotropic agents. Among these, it is preferable to contain at least one of polymer association type thixotropic agents, alkali thickening type thixotropic agents, and polyamide type thixotropic agents. A thixotropic agent imparts thixotropy to the coating, thereby reducing sagging during application, enabling a thicker film thickness per coat, and is added for the purposes of further improving workability by reducing the viscosity of the coating during application. A single thixotropic agent may be used alone, or two or more types may be used in combination.
[0040] -Solids content of thixotropic agent-When the viscosity of the aqueous coating composition at a measurement temperature of 25°C is adjusted to 65 KU (approximately 430 mPa s in mPa equivalent), the solids content of the thixotropic agent in the aqueous coating composition is preferably 0.1% by mass or more and 1.0% by mass or less, and more preferably 0.3% by mass or more and 0.9% by mass or less. When the content of the thixotropic agent is within the above range, the viscosity behavior described below is more easily obtained, and therefore a coating film with excellent coating workability and excellent appearance can be formed.
[0041] Commercially available thixotropic agents include, for example, trade names "AS1130", "AS1137", and "AS1180" (all manufactured by BASF), trade names "RHEOBYK H7625VF", "RHEOBYK L1400VF", "RHEOBYK-420", and "RHEOBYK-425" (all manufactured by BYK-Chemie), trade names "ACRYSOL RM-8W" and "ACRYSOL RM-12W" (all manufactured by The Dow Chemical Company), trade names "Thixol 53L", "Viscoatex 46", "Viscoatex 146", "Viscoatex 730", "Viscoatex 146", "Lheotech 4800", "Coapur XS83", and "Coapur XS83". 6050," "Coapur 830W," and "BR100P" (all manufactured by COATEX Co., Ltd.), trade name "Nopal 3303" (manufactured by San Nopco Ltd.), trade name "Disparlon 4200-20" (manufactured by Kusumoto Chemicals Co., Ltd.), and the like.
[0042] (Dispersant) The dispersant is not particularly limited, and commercially available dispersants for water-based paints such as the BYK series (manufactured by BYK-Chemie), the EFKA series (manufactured by EFKA Chemical Co., Ltd.), and the FLOWLEN series (manufactured by Kyoeisha Chemical Co., Ltd.) can be used.
[0043] (Neutralizing Agent) The aqueous coating composition of the present invention is preferably neutralized with ammonia or an amine-based neutralizing agent in terms of water resistance, dispersion stability, reactivity, weather resistance, contamination resistance, etc. The amine-based neutralizing agent is not particularly limited as long as it is capable of neutralizing acidic groups, and examples thereof include diethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, dimethylethanolamine, diethylethanolamine, isopropylethanolamine, diisopropanolamine, 2-amino-2-methylpropanol, 2-(dimethylamino)-2-methylpropanol, morpholine, N-methylmorpholine, and N-ethylmorpholine. The neutralizing agent is preferably added in an amount such that the pH of the aqueous coating composition after neutralization is about 6.5 to 9.0.
[0044] (Antifoaming Agent) The aqueous coating composition of the present invention may contain an antifoaming agent. Commercially available antifoaming agents can be used as appropriate, but it is preferable to use those with little odor. Antifoaming agents are generally classified into mineral oil-based, silicone-based, polyether-based, etc. depending on the carrier oil, and usually contain, in addition to the carrier, a nucleating agent such as hydrophobic silica, wax, amide, or metal soap as a constituent component. The amount of antifoaming agent in the aqueous coating composition of the present invention is preferably 0.01% by mass or more and 5% by mass or less. The antifoaming agents may be used alone or in combination of two or more.
[0045] (Surface Conditioner) Examples of the surface conditioner include silicone-based, acrylic-based, vinyl-based, and fluorine-based surface conditioners. From the viewpoint of the metallic luster and water resistance of the resulting coating film, silicone-based surface conditioners are preferred. Examples of silicone-based surface conditioners include polydimethylsiloxane and modified silicones obtained by modifying polydimethylsiloxane. Examples of modified silicones include polyether-modified silicone, acrylic-modified silicone, and polyester-modified silicone. One type of surface conditioner may be used alone, or two or more types may be used in combination. Examples of commercially available surface conditioners include the product name "SURFYNOL SF104BC" (acetylene dialcohol-based surface conditioner, manufactured by EVONIK).
[0046] <Solids concentration in water-based coating composition> The solids concentration in the water-based coating composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU (approximately 430 mPa·s in mPa equivalent). Furthermore, the solids concentration of the water-based coating composition of the present invention is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less, when the viscosity at a measurement temperature of 25°C is adjusted to 430 mPa·s. By setting the solids concentration in the water-based coating composition within the above range, it is possible to improve the orientation of the pigment and the sagging properties during coating.
[0047] <Viscosity> The viscosity of the aqueous coating composition of the present invention varies depending on the coating method and coating conditions. For example, in the case of rotary disk coating using a bell-type coating gun, it can be suitably used in a range of 60 KU to 70 KU (in mPa equivalent, about 300 mPa·s to about 580 mPa·s) at a measurement temperature of 25°C. In the case of air spray coating, it can be suitably used in a range of 40 KU to 50 KU (in mPa equivalent, about 100 mPa·s to about 180 mPa·s) at a measurement temperature of 25°C. A diluent such as water can be used to adjust the viscosity. When the viscosity of the aqueous coating composition during coating is 40 KU to 70 KU (in mPa equivalent, about 100 mPa·s to about 580 mPa·s), particularly about 430 mPa·s or higher, it is suitable for coating uneven or flow-shaped substrates such as automobile parts. The viscosity of the water-based coating composition is a value measured in accordance with JIS K 5600-2-2:1999 at a measurement temperature of 25°C using a Stormer viscometer.
[0048] <Viscosity behavior> The viscosity behavior of the aqueous coating composition of the present invention will be described. The aqueous coating composition of the present invention exhibits the following viscosity behaviors (a) and (b) when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU (approximately 430 mPa·s in mPa equivalent). (a) Shear rate: 1000 sec -1 The shear viscosity V1 at time T1 after 60 seconds has elapsed since the shear rate was set to 0.1 sec. -1 and V2 / V1, which is the ratio of the shear viscosity V2 at time T2, which is one second after time T1, to V2, is equal to or greater than 10. (b) V3 / V2, which is the ratio of the shear viscosity V2 at time T2 to V3 at time T3, which is one second after time T2, is equal to or greater than 1.3.
[0049] The shear viscosity at each time is a value measured using a rheometer (MCR rheometer manufactured by Anton Parr) or the like after adjusting the liquid temperature to 25°C.
[0050] "Shear rate 1000 sec -1"The shear rate is 1000 sec" means a high shear rate during application. When the viscosity at a measurement temperature of 25°C is adjusted to 65 KU (approximately 430 mPa·s in mPa equivalent), -1 In this case, the shear viscosity V1 of the aqueous coating composition at time T1 is preferably 0.01 Pa s or more and 0.5 Pa s or less, and more preferably 0.01 Pa s or more and 0.2 Pa s or less. In the case of such a high shear rate, a low shear viscosity V1 within the above range means that the workability during coating is good.
[0051] Next, "shear rate 1000 sec -1 At time T1, 60 seconds after the shear rate was increased to 0.1 sec -1 "When the shear rate is 0.1 sec" means a state of low shear rate such as when the coating is left to stand. -1 The shear viscosity V2 at time T2, 1 second after time T1, is preferably 1.5 Pa s or more and 10 Pa s or less, and more preferably 1.5 Pa s or more and 6 Pa s or less. When the shear viscosity V2 is in the above range, the pigments tend to align uniformly in the wet coating film immediately after application, and the appearance of the formed coating film is good.
[0052] Furthermore, the shear viscosity V3 at time T3, 1 second after time T2, is preferably 2 Pa s or more and 15 Pa s or less, and more preferably 2 Pa s or more and 8 Pa s or less. When the shear viscosity V3 is in the above range, the sagging resistance after painting and the paint appearance are good.
[0053] The aqueous coating composition of the present invention has a shear viscosity V2 / V1 ratio (V2 / V1) of 10 or more (above (a)), which significantly increases the viscosity within 1 second after application, making it easier for the pigments to align uniformly and enabling the production of a coating film with excellent appearance. V2 / V1 is more preferably 15 or more, and even more preferably 20 or more.
[0054] The aqueous coating composition of the present invention has a ratio of shear viscosity V2 to shear viscosity V3, V3 / V2, of 1.3 or more (above (b)), which prevents sagging of the coating and allows the production of a coating film with good appearance. V3 / V2 is more preferably 1.4 or more and 3.0 or less.
[0055] The aqueous coating composition of the present invention can be prepared by mixing various components appropriately selected as needed. The aqueous coating composition of the present invention may be a one-component or two-component type, but is preferably used as a one-component type from the viewpoint that it is not necessary to take into account the labor of mixing during application and the usable time.
[0056] [Method for forming a multilayer coating film] The method for forming a multilayer coating film of the present invention comprises a base coating film forming step of applying the aqueous coating composition of the present invention onto an object to be coated to form a wet base coating film, a top coating film forming step of applying a top coating composition onto the obtained wet base coating film to form a wet top coating film, and a drying step of simultaneously drying the obtained base coating film and top coating film to form a multilayer coating film.
[0057] <Substrate> The substrates to be coated with the aqueous coating composition of the present invention include plastic substrates such as epoxy resins, ABS resins, polycarbonates, polyvinyl chloride, polystyrene, acrylic resins, such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyolefins, such as polypropylene (PP), metal substrates such as steel, zinc-plated steel, tin-plated steel, stainless steel, magnesium alloys, aluminum, aluminum alloys, titanium, titanium alloys, inorganic substrates other than metals, such as cement, mortar, concrete, slate, gypsum, calcium silicate, glass, ceramics, calcium carbonate, marble, artificial marble, wood substrates, and composite substrates combining two or more of these substrates. Examples of composite substrates include composite substrates such as wood fiber-reinforced cement boards, fiber-reinforced cement boards, and fiber-reinforced cement / calcium silicate boards, metal substrates that have been subjected to various surface treatments, such as oxidation treatments, and plastic substrates whose surfaces are coated with inorganic substances (for example, plastic substrates coated with glass). Furthermore, the substrate may be subjected to various surface treatments, and at least a portion of the substrate surface may have a primer coating film such as a conductive primer or an old coating film (a coating film that has already been formed before the coating composition of the present invention is applied).
[0058] <Top Coat Paint Composition> The top coat paint composition is not particularly limited, and a commonly used top coat paint can be used. Examples of resins used in the top coat paint include acrylic resins, fluorine-based resins, urethane resins, epoxy resins, organically modified silicone resins (e.g., acrylic silicone resins), polyester resins, and melamine resins, and it is particularly preferable to use acrylic resins and urethane resins. Furthermore, in order to make the most of the appearance of the coating film formed from the aqueous paint composition of the present invention, it is preferable that the top coat paint composition is a clear paint.
[0059] The method for applying the water-based paint composition and topcoat paint composition is not particularly limited, and known methods such as air spray coating, airless spray coating, rotary disk coating, etc. Alternatively, a method in which electrostatic charge is applied during coating to increase the coating efficiency may be used.
[0060] The dry film thickness of the aqueous coating composition of the present invention is, for example, preferably 5 μm to 40 μm, more preferably 5 μm to 30 μm. A dry coating film of 5 μm or more makes it easy to obtain a continuous, uniform film that is not too thin and can completely conceal the color of the base. On the other hand, a dry coating film of 40 μm or less makes it less likely to develop defects such as popping or sagging during drying, so a normal dry coating film can be obtained.
[0061] The base coating film forming step of the present invention may be preceded by a step of forming a primer on the substrate. For example, a conductive primer is preferably used as the primer from the viewpoint of the coating efficiency of electrostatic coating. When the coating composition of the present invention is applied as a base coat paint, it is preferable to apply the conductive primer so that the dry film thickness is 10 to 100 μm.
[0062] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto.
[0063] [Examples 1 to 17, Comparative Examples 1 to 8] The preparation of the coating compositions of the Examples and Comparative Examples will be described. The raw materials used in the coating compositions and their blending amounts are shown in Tables 1 to 3. The values in the tables are in mass %. Here, the solid content refers to the components remaining in the coating film when the coating film is formed. Each of the raw materials shown in Tables 1 to 3 was mixed using a disperser so as to be uniformly dispersed, to obtain each coating composition.
[0064] Details of the raw materials listed in Table 1 are as follows: (1) Resins Acrylic resin: NeoCry A639 (manufactured by DSM, solid content: 45%, hydroxyl value: less than 1.0%) Urethane resin 1: DAOTAN TW6450 / 30WA (manufactured by Daicel Allnex, solid content: 35%) Urethane resin 2: Bayhydrol UH2606 (manufactured by Covestro, solid content: 35%) Urethane resin 3: Watersol WTW-315 (manufactured by DIC, solid content: 41.5%) Melamine resin: Maprenal MF 927 / 70IB (manufactured by Prefere Resins, solid content: 70%)
[0065] (2) Pigments Luminescent pigment: EMR-DZ460 (manufactured by Toyo Aluminum, NV: 56%, silica-coated aluminum pigment) Coloring pigment: R960 (manufactured by DuPont, titanium dioxide) Extender pigment: BF-21 (manufactured by Sakai Chemical Industry Co., Ltd., barium sulfate)
[0066] (3) Thixotropic Agents Alkali-thickening thixotropic agent 1: AS1137 (manufactured by BASF, NV: 30%) Alkali-thickening thixotropic agent 2: AS1180 (manufactured by BASF, NV: 30%) Alkali-thickening thixotropic agent 3: Viscoatex 146 (manufactured by COATEX, NV: 28%) Hydrophobic urethane association type: Coapur 6050 (manufactured by COATEX, NV: 50%) Urethane association type: RHEOBYK-425 (manufactured by BYK-Chemie, NV: 50%)
[0067] (4) Other additives Dispersant 1: XL250 (manufactured by Allnex, NV: 47%) Dispersant 2: DISPERBYK-190 (manufactured by BYK, NV: 40%) Defoamer: BYK024 (manufactured by BYK, NV: 96%) Surface conditioner: SURFYNOL SF104BC (manufactured by EVONIK, NV: 49%)
[0068] (5) Solvents Water-soluble organic solvent 1: ethylene glycol monobutyl ether (boiling point: 171°C, SP value: 20.8) Water-soluble organic solvent 2: dimethylaminoethanol Water-soluble organic solvent 3: butanol Water-soluble organic solvent 4: triethylene glycol butyl methyl ether (boiling point: 261°C, SP value: 16.6) Water-soluble organic solvent 5: diethylene glycol diethyl ether (boiling point: 189°C, SP value: 17.8) Non-water-soluble organic solvent 1: diethylene glycol butyl methyl ether (boiling point: 212°C, SP value: 16.1) Water-soluble organic solvent 6: ethylene glycol monomethyl ether (boiling point: 124°C, SP value: 24.8) Water-soluble organic solvent 7: ethylene glycol dimethyl ether (boiling point: 85°C, SP value: 17.6)
[0069] [Evaluation of Paint Properties and Coating Appearance] The following evaluations were carried out for each of the paint compositions obtained in the above Examples and Comparative Examples. The evaluation results are shown in Tables 1 to 3. Note that "paint properties after viscosity adjustment (65 KU)" refers to the paint properties when water was added to 100 parts by mass of each paint composition until the Stormer viscosity reached 65 KU, and the amount of water added was taken as the dilution amount. The viscosity at the time of viscosity adjustment was measured at 25°C using a digital Stormer viscometer (KU2, manufactured by Brookfield). The shear viscosity at each time point was measured using a rheometer (such as an MCR rheometer manufactured by Anton Parr) after adjusting the liquid temperature to 25°C.
[0070] (Appearance of coating film in bell coating) After adjusting the viscosity of each coating composition obtained in the above Examples and Comparative Examples to 65 KU, the coating was applied to a polypropylene plate using a "Mighty Robo Bell 21 rotary atomizer electrostatic coater" (manufactured by CFT Ransberg) under the following coating conditions so that the dry film thickness was 10 μm. <Coating conditions> Temperature / humidity: 25°C / 70RH% Bell cup diameter: Φ70 mm Discharge rate: 168 cc / min Bell rotation speed: 40,000 rpm Shaving air (in): 200 kPa Shaving air (out): 200 kPa Applied voltage: -60 KV Number of coating passes: 6 passes (after 3 passes, an interval of 82 seconds was allowed, followed by another 3 passes)
[0071] The finished appearance of the coating film was visually observed and rated according to the following criteria. <Evaluation criteria> A: The coating film has no uneven color and no visible irregularities on the surface, giving an excellent coating appearance. B: The coating film has some uneven color but no visible irregularities on the surface, giving no practical problems with the coating appearance. C: The coating film has uneven color and visible irregularities on the surface.
[0072] (Sagging immediately after bell coating) Each of the coating compositions obtained in the above Examples and Comparative Examples was coated under the coating conditions described above, and after leaving to stand for 180 seconds, a polypropylene plate was placed upright and sagging was evaluated according to the following criteria. <Evaluation criteria> A: No sagging, smooth and uniform surface. B: Slight sagging of the paint not resulting in sagging was observed. C: Sagging occurred, and the base coat was partially visible.
[0073] (Appearance of coating film in spray coating) Each of the coating compositions obtained in the above Examples and Comparative Examples was diluted with water to a viscosity that allowed coating with an air spray, and coated onto a polypropylene plate using an air spray at 25°C / 70% RH to a dry film thickness of 10 μm. The finished appearance was evaluated based on the results of observation of the coating appearance and using the following criteria. <Evaluation criteria> A: The coating film has no uneven color when visually inspected, and no irregularities can be detected on the coating film surface, resulting in an excellent coating appearance. B: Some unevenness in the coating film is visible when visually inspected, but no irregularities can be detected on the coating film surface, resulting in no practical problems with the coating appearance. C: The coating film has uneven color when visually inspected, and irregularities can be detected on the coating film surface.
[0074] (Adhesion test to substrate) Each coating composition obtained in the above Examples and Comparative Examples was diluted with water to a viscosity suitable for application by air spray, and then applied to an ABS plate (150 mm x 70 mm x 2 mm) using an air spray under conditions of 25 ° C / 70% RH to a dry film thickness of 20 μm, and then dried at 100 ° C for 30 minutes to prepare a test specimen. In accordance with JIS K5600-5-6:1999, the coating surface of each test specimen was cut with a cutter to create 100 2 mm square grids, and adhesive tape was applied thereto, followed by a forced peel test. The number of remaining grids out of the 100 grids was counted and evaluated according to the following criteria. 100 / 100 indicates a coating film peeling area of 0%, and for example, 80 / 100 indicates a coating film peeling area of 20%. <Evaluation criteria> AA: 100 / 100 A: 90 / 100 to 99 / 100 B: 70 / 100 to 89 / 100 C: 69 / 100 or less
[0075]
[0076]
[0077]
[0078] As shown in Tables 1 to 3, in the examples where V2 / V1 was 10 or more and V3 / V2 was 1.3 or more, good results were obtained in all of the coating appearance (bell coating), sagging immediately after coating (bell coating), and coating appearance (air spray coating). Furthermore, in Examples 15 to 17, in which an organic solvent with a high boiling point and high solubility in the substrate was added, excellent adhesion to the ABS substrate was obtained.
[0079] [Examples 1A to 18A, Comparative Examples 1A to 6A] The preparation of coating compositions 1A to 24A of Examples 1A to 18A and Comparative Examples 1A to 6A will be described. The raw materials and blending amounts used in coating compositions 1A to 24A are shown in Tables 4 to 7. The values in the tables are in mass %. Here, the solid content refers to the components remaining in the coating film when the coating film is formed. Each of the raw materials shown in Tables 4 to 7 was mixed using a disperser to uniformly disperse them, thereby obtaining each coating composition.
[0080] Details of the raw materials listed in the table are as follows: (1) Resins Acrylic resin: NeoCryl A639 (manufactured by DSM Corporation, solid content: 45%, hydroxyl value: less than 1.0%) Urethane resin 1: DAOTAN TW6450 / 30WA (manufactured by Daicel Allnex Corporation, solid content: 35%) Urethane resin 2: Bayhydrol UH2606 (manufactured by Covestro, solid content: 35%) Urethane resin 3: Watersol WTW-315 (manufactured by DIC Corporation, solid content: 41.5%)
[0081] (2) Curing agent Isocyanate: Duranate WR80-70P (manufactured by Asahi Kasei Corporation, solid content: 70%) Melamine resin: Maprenal MF 927 / 70IB (manufactured by Prefere Resins, solid content: 70%)
[0082] (3) Pigments (i) Luster pigment: (Silica-coated aluminum pigment (trade name "EMR-DZ460", solid content 56%, manufactured by Toyo Aluminum K.K.) (ii) Colored pigments Colored pigment 1: White pigment (titanium dioxide, trade name "R960", manufactured by DuPont) Colored pigment 2: Black pigment, carbon black, trade name "COLOUR BLACK FW200 BEADS", manufactured by Orion Engineered) Colored pigment 3: Red pigment, DPP Red, trade name "Irgazin Rubine L 4030", manufactured by BASF) (iii) Extender pigments Extender pigment 1: Barium sulfate (trade name "Ultrafine Precipitated Barium Sulfate", particle size D50: 0.50 to 0.70 μm, oil absorption: 10 to 15 g / cm 3 , Density: 4.5g / cm 3 , manufactured by Shaanxi Fuhua Chemical Co., Ltd.) Extender pigment 2: Barium sulfate (trade name "BARIFINE BF-21", particle size D50: 0.05 μm, oil absorption: 15 to 19 g / cm) 3 , Density: 3.9g / cm 3 , manufactured by Sakai Chemical Industry Co., Ltd.) Extender pigment 3: calcium carbonate (trade name "Sunlight 1000", particle size D50: 2.5 to 5.5 μm, oil absorption: 25 to 29 g / cm 3 , density 2.71g / cm 3 , manufactured by Takehara Chemical Industry Co., Ltd.)
[0083] (4) Thixotropic Agents Alkali-thickening thixotropic agent 1: trade name "AS1137", manufactured by BASF, solid content 30% Alkali-thickening thixotropic agent 2: trade name "Viscoatex 146", manufactured by COATEX, NV: 28% Urethane associative type: trade name "BYK-425", manufactured by BYK-Chemie, solid content 50%
[0084] (5) Other additives Dispersant 1: trade name "XL250", manufactured by Allnex Co., Ltd., anionic wetting agent, solid content 47% Dispersant 2: trade name "DISPERBYK-190", manufactured by BYK-Chemie Co., Ltd., dispersant, solid content 40% Defoamer: trade name "BYK024", manufactured by BYK-Chemie Co., Ltd., solid content 96% Surface conditioner: trade name "SURFYNOL SF104BC", acetylene dialcohol-based surface conditioner, manufactured by EVONIK Co., Ltd., solid content 49%
[0085] (6) Solvents Water-soluble organic solvent 1: ethylene glycol monobutyl ether (boiling point: 171°C, SP value: 20.8) Water-soluble organic solvent 2: dimethylaminoethanol Water-soluble organic solvent 3: butanol Water-soluble organic solvent 4: triethylene glycol butyl methyl ether (boiling point: 261°C, SP value: 16.6) Water-soluble organic solvent 5: diethylene glycol diethyl ether (boiling point: 189°C, SP value: 17.8) Non-water-soluble organic solvent 1: diethylene glycol butyl methyl ether (boiling point: 212°C, SP value: 16.1) Water-soluble organic solvent 6: ethylene glycol monomethyl ether (boiling point: 124°C, SP value: 24.8) Water-soluble organic solvent 7: ethylene glycol dimethyl ether (boiling point: 85°C, SP value: 17.6)
[0086] [Evaluation of Paint Properties and Coating Appearance] The following evaluations were carried out for each of the paint compositions obtained in the above Examples and Comparative Examples. The evaluation results are shown in Tables 4 to 7. Note that "paint properties after viscosity adjustment" refers to the paint properties when water was added to 100 parts by mass of each paint composition until the Stormer viscosity reached 430 mPa·s, and the amount of water added was taken as the dilution amount. The viscosity at the time of viscosity adjustment was measured at a measurement temperature of 25°C using a digital Stormer viscometer (KU2, manufactured by Brookfield). The measurement temperature refers to the liquid temperature at the time of viscosity measurement. The shear viscosity at each time was measured using a rheometer (such as an MCR rheometer manufactured by Anton Parr) after adjusting the liquid temperature to 25°C.
[0087] (Appearance of coating film in bell coating) After adjusting the viscosity of each coating composition obtained in the above Examples and Comparative Examples to 430 mPa·s, the coating was applied to a polypropylene plate using a "Mighty Robo Bell 21 rotary atomizer electrostatic coating machine" (manufactured by CFT Ransberg) under the following coating conditions so that the dry film thickness would be 10 μm or 20 μm. <Coating conditions> Temperature / humidity: 25°C / 70 RH% Bell cup diameter: Φ70 mm Bell rotation speed: 40,000 rpm Shaving air (in): 200 kPa Shaving air (out): 200 kPa Applied voltage: -60 KV
[0088] (Appearance of coating film by bell coating) The finished appearance of a coating film with a thickness of 20 μm was visually observed and evaluated according to the following evaluation criteria. <Evaluation criteria> A: The coating film has no unevenness in color when visually observed, and no irregularities can be seen on the coating film surface, resulting in an excellent coating appearance. B: The coating film has some unevenness in color when visually observed, but no irregularities can be seen on the coating film surface, resulting in no practical problems with the coating appearance. C: The coating film has unevenness in color when visually observed, and irregularities can also be seen on the coating film surface.
[0089] (Coating film drying properties 1) Each of the coating compositions obtained in the above Examples and Comparative Examples was coated to a film thickness of 10 μm under the coating conditions described above, and immediately afterwards the plate was stood upright and left to stand for 180 seconds, after which sagging was evaluated according to the following criteria. <Evaluation criteria> A: No sagging, surface is smooth and uniform. B: Slight sagging of the paint that does not amount to sagging is observed. C: Sagging occurs, and the base is partially visible.
[0090] (Coating film drying properties 2) Each of the coating compositions obtained in the above Examples and Comparative Examples was coated to a film thickness of 20 μm under the coating conditions described above, and immediately afterwards the plate was stood upright and left to stand for 180 seconds, after which sagging was evaluated according to the following criteria. <Evaluation criteria> A: No sagging, surface is smooth and uniform. B: Sagging has occurred, and sagging of the paint is observed. C: Sagging has occurred, and the base is visible through.
[0091] (Appearance of coating film in spray coating) Each of the coating compositions obtained in the above Examples and Comparative Examples was diluted with water to a viscosity that allowed coating with an air spray, and then coated onto a polypropylene plate using an air spray at 25°C / 70% RH to a dry film thickness of 20 μm. The finished appearance was observed and rated according to the following criteria. <Evaluation criteria> A: The coating film has no uneven color when visually inspected, and no irregularities are visible on the coating film surface, resulting in an excellent coating appearance. B: Some unevenness in the coating film is visible when visually inspected, but no irregularities are visible on the coating film surface, resulting in no practical problems with the coating appearance. C: The coating film has uneven color when visually inspected, and irregularities are visible on the coating film surface.
[0092] (Adhesion to Substrate) Each coating composition obtained in the above Examples and Comparative Examples was diluted with water to a viscosity that allowed application by air spray. Using an air spray, the coating was applied to an ABS (acrylonitrile butadiene styrene resin) plate (150 mm x 70 mm x 2 mm) to a dry film thickness of 20 μm under conditions of 25°C / 70% RH, and then dried at 100°C for 30 minutes to prepare a test specimen. According to JIS K5600-5-6:1999, the coating surface of each test specimen was cut with a cutter to create 100 2 mm square grids, and adhesive tape was applied to the grids, followed by a forced peel test. The number of remaining grids out of the 100 grids was counted and evaluated according to the following criteria. 100 / 100 indicates a 0% peeled area of the coating film, and for example, 80 / 100 indicates a 20% peeled area of the coating film. <Evaluation criteria> AA: 100 / 100 A: 90 / 100 to 99 / 100 B: 70 / 100 to 89 / 100 C: 69 / 100 or less
[0093] (Coating strength) Evaluation was carried out according to item 6 of JIS K 5600-5-3 (DuPont method). AA: 500g 50cm, no cracks A: 500g 40cm, no cracks B: 500g 30cm, no cracks C: 500g 30cm, cracks
[0094]
[0095]
[0096]
[0097]
[0098] As shown in Tables 4 to 7, the aqueous coating compositions of Examples 1A to 18A of the present invention gave good results in all evaluation items, including coating appearance by bell coating, coating drying properties, coating appearance by spray coating, adhesion to substrate, and coating strength.
Claims
1. A water-based coating composition containing water, a resin, and at least one of a glittering pigment and a coloring pigment, which has the following viscosity behaviors (a) and (b) when the viscosity is adjusted to 430 mPa·s at a measurement temperature of 25°C. (a) A shear rate of 1000 sec -1 The shear viscosity V1 at time T1 after 60 seconds has elapsed since the shear rate was set to 0.1 sec at the time T1. -1 and V2 / V1, which is a ratio of the shear viscosity V2 at time T2, which is one second after time T1, is equal to or greater than 10. (b) V3 / V2, which is a ratio of the shear viscosity V2 at time T2 to the shear viscosity V3 at time T3, which is one second after time T2, is equal to or greater than 1.
3.
2. The ink further contains a body pigment, the resin being at least one of an acrylic resin and a urethane resin, and the body pigment has a particle diameter D50 of 0.5 μm or more and a density of 4.2 g / cm 3 2. The aqueous coating composition according to claim 1, wherein the content of the extender pigment in the aqueous coating composition is 0.1% by mass or more and less than 25% by mass.
3. The water-based coating composition according to claim 2, wherein the acrylic resin has a solid hydroxyl value of 2% or less.
4. The water-based paint composition according to claim 2, wherein the oil absorption of said body pigment is 21 ml / g or less.
5. The water-based paint composition according to claim 2, wherein the body pigment is barium sulfate.
6. The aqueous coating composition according to claim 1 or 2, further comprising a thixotropic agent, and when the viscosity of the aqueous coating composition is adjusted to 430 mPa·s at a measurement temperature of 25°C, the solid content of the thixotropic agent in the aqueous coating composition is 0.1 mass % or more and 1.5 mass % or less.
7. The aqueous coating composition according to claim 1 or 2, wherein when the viscosity of the aqueous coating composition is adjusted to 430 mPa·s at a measurement temperature of 25° C., the aqueous coating composition has a solids concentration of 5 mass % or more and 50 mass % or less.
8. A method for forming a multi-layer coating film, comprising: a base coating film forming step of applying an aqueous coating composition according to any one of claims 1 to 7 onto an object to be coated, and forming a wet base coating film; a topcoat coating film forming step of applying a topcoat coating composition onto the obtained wet base coating film, and forming a wet topcoat coating film; and a drying step of simultaneously drying the obtained wet base coating film and the wet topcoat coating film to form a multi-layer coating film.
Citation Information
Patent Citations
Coating composition for forming pattern and coated article
JP2007291144A
Multilayer coating film forming method and coating material composition
JP2018069185A
Method for applying to substrate, one liquid type aqueous coating composition using high transfer efficiency applicator
JP2022171643A