Curable resin composition, cured article and printed wiring board including cured article
The curable resin composition with a tailored (meth)acrylic group concentration addresses the inefficiencies in direct imaging by enhancing sensitivity and resolution, enabling faster high-resolution pattern formation on printed wiring boards, thus improving the manufacturing efficiency of electronic components.
Patent Information
- Application Number
- PCT/JP2024/013058
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current curable resin compositions used in direct imaging for forming high-resolution patterns on printed wiring boards are inefficient, requiring longer times due to the need for high precision control, which hampers their adoption despite the cost and time advantages of this method.
A curable resin composition with a specific formulation including a carboxyl group-containing resin, inorganic filler, thermosetting resin, photopolymerization initiator, and photopolymerizable monomer, where the concentration of (meth)acrylic groups is adjusted between 0.00070 to 0.00170 equivalent/g, enhancing sensitivity and resolution while reducing exposure time.
The optimized curable resin composition achieves high-resolution pattern formation in shorter times, improving the efficiency of direct imaging by balancing sensitivity and resolution, making it suitable for high-speed manufacturing of precise electronic components.
Smart Images

Figure JPOXMLDOC01-APPB-I000003 
Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Curable resin composition, cured product, and printed wiring board comprising the cured product
[0001] The present invention relates to a curable resin composition, more specifically to a curable resin composition suitable for forming an insulating layer by a direct imaging method that requires high-precision control, a cured product thereof, and a printed wiring board including the cured product. The present invention also relates to a method for producing a printed wiring board including an insulating layer using the curable resin composition.
[0002] In recent years, electronic devices have become lighter, thinner, shorter, and smaller, leading to higher precision and higher density of electronic components such as printed wiring boards. Currently, insulating layers such as solder resist layers are mainly formed by photolithography, in which a curable resin composition is applied to a substrate, dried, exposed to light, and developed to form a pattern, and the patterned resin is then fully cured by heating or light irradiation. In the manufacture of such electronic components, there is a demand for high-speed formation of fine patterns.
[0003] With the remarkable progress in exposure technology in recent years, new exposure methods and devices for realizing exposure using such new exposure methods have been developed, and today there are a variety of exposure methods and exposure devices. One of these exposure methods, called direct imaging, is attracting attention as a method that is more economical than conventional exposure methods that use a mask because it does not require a mask and can shorten the time from designing the exposure pattern to exposure.
[0004] On the other hand, while conventional exposure methods using masks are usually performed in a stationary state, direct imaging exposes while scanning, i.e., while in motion, so extremely high-precision control is required to achieve high-resolution developed patterns, and as patterns become finer, the time required for exposure increases, resulting in an increase in the time required to manufacture electronic components (takt time).For this reason, although direct imaging has many advantages, its widespread adoption has not progressed from a technical standpoint.
[0005] However, as demand for electronic devices is expected to increase further in the future, direct imaging is expected to become even more widespread, and various research and development efforts are being carried out to achieve this.
[0006] Under these circumstances, a technical problem exists to provide a highly sensitive curable resin composition that can form a high-resolution cured product pattern in a short period of time.
[0007] Therefore, an object of the present invention is to provide a highly sensitive curable resin composition that can form a high-resolution cured product pattern in a short time compared to conventional curable resin compositions. Another object of the present invention is to provide a high-resolution cured product obtained by curing such a curable resin composition, a printed wiring board including the cured product, and a method for producing the printed wiring board.
[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by adjusting the concentration of (meth)acrylic groups relative to the total mass of solids in a curable resin composition containing a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer to 0.00070 to 0.00170 equivalents / g. The present invention is based on this finding. Specifically, the gist of the present invention is as follows.
[0009] [1] A curable resin composition comprising a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer, wherein the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid contents of the curable resin composition is 0.00070 to 0.00170 equivalents / g. [2] The curable resin composition according to [1], wherein 30 to 60% of the total concentration of (meth)acrylic groups relative to the total mass of the solid contents of the curable resin composition are (meth)acrylic groups derived from the photopolymerizable monomer. [3] The curable resin composition according to [1] or [2], wherein the inorganic filler comprises an inorganic filler having (meth)acrylic groups on its surface, and wherein 30 to 60% of the total concentration of (meth)acrylic groups relative to the total mass of the solid contents of the curable resin composition are derived from the carboxyl group-containing resin, 5 to 30% are derived from the inorganic filler having (meth)acrylic groups, and 30 to 60% are derived from the photopolymerizable monomer. [4] The curable resin composition according to any one of [1] to [3], wherein the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is 0.00070 to 0.00140 equivalents / g. [5] The curable resin composition according to any one of [1] to [4], wherein the (meth)acrylic groups derived from the photopolymerizable monomer account for 40 to 55% of the total concentration of the (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition. [6] The curable resin composition according to any one of [1] to [5], wherein the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is 0.00080 to 0.00110 equivalents / g. [7] The curable resin composition according to any one of [1] to [6], wherein the (meth)acrylic groups derived from the photopolymerizable monomer account for 45 to 55% of the total concentration of the (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition. [8] A cured product obtained by curing the curable resin composition according to any one of [1] to [7]. [9] A printed wiring board comprising the cured product according to [8].
[10] A method for producing a printed wiring board having an insulating layer, the method comprising a step of forming the insulating layer by curing the curable resin composition according to any one of [1] to [7].
[0010] According to the present invention, there is provided a highly sensitive curable resin composition that can form a high-resolution cured product pattern in a short time compared to conventional curable resin compositions. Furthermore, according to the present invention, there are provided a high-resolution cured product obtained by curing such a curable resin composition, a printed wiring board including the cured product, and a method for producing the printed wiring board.
[0011] [Curable Resin Composition] According to one aspect of the present invention, a curable resin composition (hereinafter also referred to as the "curable resin composition of the present invention") is provided. The curable resin composition of the present invention comprises a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer, and is characterized in that the concentration of (meth)acrylic groups relative to the total mass of the solids of the curable resin composition is adjusted to 0.00070 to 0.00170 equivalents / g. Because the concentration of (meth)acrylic groups relative to the total mass of the solids is adjusted within a predetermined range, the curable resin composition of the present invention has higher sensitivity to exposure than conventional curable resin compositions and can form a cured product pattern with high resolution. Because the curable resin composition of the present invention has high sensitivity to exposure, a high-resolution cured product pattern can be formed with a short exposure time. Therefore, even with a moving exposure method such as direct imaging, a high-resolution cured product pattern can be formed in a short time.
[0012] In a curable resin composition containing a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer, adjusting the concentration of (meth)acrylic groups relative to the total mass of the solids of the curable resin composition to 0.00070 to 0.00170 equivalents / g is unclear, but the reason for this is speculated as follows: Radicals generated by the photopolymerization initiator absorbing ultraviolet light undergo radical polymerization with the (meth)acrylic groups present in the curable resin composition, but it is thought that polymerization inhibition by atmospheric oxygen also occurs in a countervailing manner. In this case, by keeping the concentration of (meth)acrylic groups in the curable resin composition within the above range, inhibition by oxygen of the radical polymerization between the radicals generated from the photopolymerization initiator and the (meth)acrylic groups in the curable resin composition can be suppressed, allowing the reaction to propagate, while also suppressing excessive halation in unexposed areas, resulting in a high level of balance between sensitivity (photocurability) and resolution. In the curable resin composition, the concentration of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is more preferably adjusted to 0.00070 to 0.00140 equivalents / g, and even more preferably 0.00080 to 0.00110 equivalents / g. In this specification, the "(meth)acrylic group concentration" in the "curable resin composition" refers to a value calculated based on the following formula. In the following formula, the "content of resin" and the "content of components other than resin" are each values converted into mass.
[0013] In the above formula, "(meth)acrylic group concentration of the resin" refers to the concentration of the total amount of (meth)acrylic groups in the resin components (carboxyl group-containing resin, thermosetting resin, photopolymerizable monomer, and other polymerizable components), and is calculated as follows. First, 0.1 g (mass equivalent) of a sample of each resin component is precisely weighed and dissolved in 10 ml of morpholine using ultrasound. 7 ml of a 1:1 acetic acid:water mixed solution is added, and the mixture is heated to 98°C in an oil bath for 30 minutes to react with the morpholine. The reaction solution is then left at room temperature, and 25 ml of methyl cellosolve and 20 ml of acetic anhydride are added to react with the unreacted morpholine. The mixture is then left at room temperature to prepare a solution for measurement. The resulting solution is titrated with 0.1 N perchloric acid solution to calculate the (meth)acrylic group concentration.
[0014] In addition, in the above formula, "the (meth)acrylic group concentration of components other than the resin" refers to the concentration of the total amount of (meth)acrylic groups in components other than the above-mentioned resin component, and the concentration of each component other than the resin component used in preparing the curable resin composition is calculated based on the (meth)acrylic group concentration of the component used in preparing the component.
[0015] The concentration of (meth)acrylic groups in the curable resin composition can be adjusted by appropriately selecting the types, concentrations, compounding ratios, etc. of the resin components and components other than the resins described above. In one embodiment, the concentration of (meth)acrylic groups in the curable resin composition can be adjusted by appropriately selecting the types, concentrations, compounding ratios, etc. of the carboxyl group-containing resin, inorganic filler, and photopolymerizable monomer.
[0016] Each component constituting the curable resin composition of the present invention is described in detail below. (Carboxyl Group-Containing Resin) The curable resin composition of the present invention contains a carboxyl group-containing resin. As the carboxyl group-containing resin, various conventionally known resins having carboxyl groups in the molecule can be used. By including a carboxyl group-containing resin in the curable resin composition, alkali developability can be imparted to the curable resin composition. In particular, from the viewpoint of the photocurability and development resistance of the curable resin composition, a photosensitive carboxyl group-containing resin having an ethylenically unsaturated double bond in the molecule is preferred. The ethylenically unsaturated double bond in the molecule constituting the carboxyl group-containing resin is preferably derived from acrylic acid, methacrylic acid, or a derivative thereof. When using only a carboxyl group-containing resin without an ethylenically unsaturated double bond, the curable resin composition can be made photocurable by using a compound having multiple ethylenically unsaturated groups in the molecule, i.e., a photopolymerizable monomer, as described below. Specific examples of carboxyl group-containing resins include the following compounds (which may be either oligomers or polymers): In this specification, "(meth)acrylate" is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to similar expressions such as "(meth)acrylic acid."
[0017] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, or isobutylene.
[0018] (2) Carboxyl group-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0019] (3) Carboxylic acid group-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A epoxy resins, hydrogenated bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bixylenol epoxy resins, and biphenol epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds, and diol compounds.
[0020] (4) A carboxyl group-containing photosensitive urethane resin that is (meth)acrylated at the terminal by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3) described above.
[0021] (5) A carboxyl group-containing photosensitive urethane resin that has been (meth)acrylated at its terminal by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reaction product of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3) described above.
[0022] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl group present in the side chain.
[0023] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin in which the hydroxyl groups of a bifunctional (solid) epoxy resin are further epoxidized with epichlorohydrin with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0024] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin, and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0025] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl groups of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, or adipic acid.
[0026] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.
[0027] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.
[0028] (12) A carboxyl group-containing photosensitive resin obtained by adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any of the resins (1) to (11).
[0029] The carboxyl group-containing resin is not limited to those mentioned above, and may be one type of carboxyl group-containing resin used alone or a combination of two or more types.
[0030] The acid value of the carboxyl group-containing resin is preferably 30 to 150 mgKOH / g, more preferably 50 to 120 mgKOH / g. When the acid value of the carboxyl group-containing resin is 30 mgKOH / g or more, the alkali developability of the curable resin composition is improved. On the other hand, when the acid value of the carboxyl group-containing resin is 150 mgKOH / g or less, dissolution of the exposed area by a developer and the resulting indiscriminate dissolution and peeling of the exposed area from the unexposed area can be suppressed, making it easier to draw a good cured product pattern.
[0031] The weight-average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 100,000, more preferably 5,000 to 50,000, even more preferably 6,000 to 30,000, and particularly preferably 8,000 to 15,000. A weight-average molecular weight of 2,000 or more of the carboxyl group-containing resin can suppress a decrease in the moisture resistance of the coating film of the curable resin composition after exposure and the accompanying film loss during development, thereby suppressing a decrease in the resolution of the cured product of the curable resin composition. On the other hand, a weight-average molecular weight of 100,000 or less of the carboxyl group-containing resin can improve the developability and storage stability of the curable resin composition. The weight-average molecular weight of the carboxyl group-containing resin can be measured by gel permeation chromatography (GPC) (polystyrene standard). Specifically, it can be measured by GPC using the following measuring device and measurement conditions. Measurement apparatus: Waters 2695 Detector: Waters 2414, RI (differential refractometer) Column: Waters HSPgel Column, HRMB-L, 3 μm, 6 mm × 150 mm × 2 + Waters HSPgel Column, HR1, 3 μm, 6 mm × 150 mm × 2 Column temperature: 40°C RI detector set temperature: 35°C Developing solvent: tetrahydrofuran Flow rate: 0.5 ml / min Sample amount: 10 μl Sample concentration: 0.7 wt%
[0032] The acrylic group concentration of the carboxyl group-containing resin is not particularly limited, but is, for example, 0.00050 to 0.00500 equivalents / g in terms of solid content.
[0033] The content of the carboxyl group-containing resin in the curable resin composition is not particularly limited as long as the effects of the present invention are achieved, but is preferably 5 to 60 mass %, more preferably 10 to 50 mass %, calculated as solid content. By setting the content of the carboxyl group-containing resin to 5 mass % or more, the coating strength of the curable resin composition can be improved. Furthermore, by setting the content of the carboxyl group-containing resin to 60 mass % or less, the viscosity of the curable resin composition becomes appropriate, improving processability.
[0034] In one preferred embodiment, the content of the carboxyl group-containing resin in the curable resin composition is adjusted so that 30 to 60%, preferably 40 to 50%, of the total amount of (meth)acrylic groups in the curable resin composition is derived from the carboxyl group-containing resin.
[0035] (Inorganic Filler) The curable resin composition of the present invention contains an inorganic filler. By including an inorganic filler in the curable resin composition, it is expected that the physical strength of the coating film of the curable resin composition will be improved. As the inorganic filler, barium sulfate, spherical silica, hydrotalcite, or talc is preferably used. Furthermore, in order to obtain a white appearance and flame retardancy in the cured product of the curable resin composition, an extender pigment made of a metal oxide such as titanium oxide or a metal hydroxide such as aluminum hydroxide can also be used as the inorganic filler. One type of inorganic filler may be used alone, or two or more types may be used in combination.
[0036] As the inorganic filler, spherical silica is preferably used. Any spherical silica that can be used as an inorganic filler for electronic materials can be used. The shape of the spherical silica is not limited to a true sphere, as long as it is spherical. Suitable spherical silica includes, for example, one having a sphericity of 0.8 or more as measured as follows, but is not limited thereto.
[0037] The sphericity of spherical silica is measured as follows: First, a photograph of spherical silica is taken with a scanning electron microscope (SEM), and the sphericity is calculated from the area and perimeter of the particles observed on the photograph using the following formula: (sphericity) = {4π × (area) ÷ (perimeter)} 2 Specifically, the sphericity of 100 particles is calculated using an image processing device, and the average value thereof is adopted.
[0038] The particle diameter of the spherical silica contained in the curable resin composition of the present invention is determined by measuring the specific surface area diameter (BET(N 2The particle diameter is expressed by the particle diameter based on the equivalent spherical particle diameter calculated from the specific surface area diameter (BET(N 2 The equivalent spherical particle diameter D (nm) calculated from the specific surface area S (m 2 From the specific surface area (D / g), the specific surface area is given by the formula D(nm) = 2720 / S. The specific surface area can be measured, for example, using a fully automatic specific surface area measuring device (Macsorb (registered trademark) HM model-1201) manufactured by Mountech Co., Ltd. The particle size of the spherical silica is not particularly limited, but is preferably on the order of nanometers (nm), for example, 1 to 1000 nm.
[0039] As the spherical silica, commercially available products may be used, or appropriately manufactured products may be used. The method for manufacturing spherical silica is not particularly limited, and methods known to those skilled in the art may be used. For example, spherical silica can be manufactured by burning silicon powder using the VMC (Vaporized Metal Combustion) method. The VMC method is a method in which a chemical flame is formed by a burner in an oxygen-containing atmosphere, and metal powder that constitutes a part of the target oxide particles is introduced into this chemical flame in an amount sufficient to form a dust cloud, causing a deflagration to occur and obtaining oxide particles.
[0040] Examples of commercially available spherical silica products include ADMAFINE SO-C2, SO-E2, and Admanano series manufactured by Admatechs Co., Ltd., SFP-20M, SFP-30M, and UFP-30 manufactured by Denka Co., Ltd., Organosilica sol PGM-ST manufactured by Nissan Chemical Co., Ltd., SEAHOSTAR (registered trademark) series manufactured by Nippon Shokubai Co., Ltd., Sciqas series manufactured by Sakai Chemical Industry Co., Ltd., SG-SO100 manufactured by Kyoritsu Material Co., Ltd., HPS series (HPS-0500, HPS-1000, HPS3500, etc.) manufactured by Toagosei Co., Ltd., and MUF-1BV and MSS-T7 manufactured by Tatsumori Co., Ltd.
[0041] The inorganic filler is preferably an inorganic filler whose surface has been treated to have (meth)acrylic groups. By using an inorganic filler whose surface has been treated to have (meth)acrylic groups, the bond at the organic-inorganic interface in the curable resin composition can be strengthened by a covalent bond formed by a photoreaction, thereby improving the strength of the cured product of the curable resin composition.
[0042] The method for treating the surface of the inorganic filler is not particularly limited, and any known or commonly used method may be used. However, it is preferable to treat the surface of the inorganic filler with a surface treatment agent having a (meth)acrylic group, for example, a coupling agent having a (meth)acrylic group as an organic group.
[0043] Examples of coupling agents that can be used include silane-based, titanate-based, aluminate-based, and zircoaluminate-based coupling agents. A single coupling agent may be used alone, or two or more may be used in combination. A silane-based coupling agent is preferably used. Examples of silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. These silane-based coupling agents are preferably immobilized on the surface of the inorganic filler in advance by adsorption or reaction. Here, the amount of the coupling agent to be used per 100 parts by mass of the inorganic filler is preferably 0.5 to 30 parts by mass. In the present invention, the reactive functional group derived from the coupling agent applied to the inorganic filler is not included in the compound having a photocurable reactive group or a thermosetting functional group.
[0044] The surface-treated inorganic filler may be blended into the curable resin composition of the present invention in a surface-treated state. An untreated inorganic filler and a surface treatment agent may be blended separately to surface-treat the inorganic filler in the composition, but blending a pre-surface-treated inorganic filler is preferred. Blending a pre-surface-treated inorganic filler can suppress a decrease in crack resistance, etc., due to the surface treatment agent that may remain unconsumed during the surface treatment if blended separately. When surface-treating the inorganic filler in advance, it is preferred to blend a pre-dispersion in which the inorganic filler is pre-dispersed in a solvent or curable component. The surface-treated inorganic filler is pre-dispersed in a solvent, and this pre-dispersion is blended into the composition. Alternatively, it is more preferred to pre-disperse the untreated inorganic filler in a solvent, thoroughly surface-treat it, and then blend this pre-dispersion into the composition.
[0045] In one preferred embodiment, the inorganic filler includes an inorganic filler having (meth)acrylic groups on its surface, and particularly preferably includes spherical silica (nanosilica) having (meth)acrylic groups on its surface and having a particle size of 100 nanometers (nm) or less.
[0046] The (meth)acrylic group concentration of the inorganic filler is not particularly limited, but is, for example, 0.00003 to 0.00300 equivalents / g, and more preferably 0.00005 to 0.00100 equivalents / g. By ensuring that the amount of surface treatment is within the above range, the inorganic filler can be well dispersed in the carboxyl group-containing resin, and the strength of the cured product of the curable resin composition can be improved.
[0047] The content of the inorganic filler in the curable resin composition is preferably 20 to 70 mass% and more preferably 30 to 60 mass% in terms of solid content, relative to the total mass of the curable resin composition. By having the inorganic filler content of 70 mass% or less, an excessive increase in viscosity of the curable resin composition can be suppressed, and a decrease in the coatability and moldability of the curable resin composition can be suppressed, thereby suppressing the brittleness of the cured product. Furthermore, by having the inorganic filler content of 20 mass% or more, the thermal expansion coefficient of the cured product of the curable resin composition can be reduced, thereby mitigating the difference in thermal expansion coefficient between the cured product and surrounding substrates such as wiring copper.
[0048] In one preferred embodiment, the content of the inorganic filler in the curable resin composition is adjusted so that 5.0 to 30%, preferably 5.5 to 10%, of the total amount of (meth)acrylic groups in the curable resin composition is derived from the inorganic filler.
[0049] (Thermosetting Resin) The curable resin composition of the present invention contains a thermosetting resin. By including a thermosetting resin in the curable resin composition, it is expected that the heat resistance of the curable resin composition will be improved. Any known and commonly used thermosetting resin can be used, for example, amino resins such as melamine resins, benzoguanamine resins, melamine derivatives, and benzoguanamine derivatives, isocyanate compounds, blocked isocyanate compounds, cyclocarbonate compounds, epoxy compounds, oxetane compounds, episulfide resins, bismaleimides, carbodiimide resins, etc. As the thermosetting resin, a thermosetting resin having multiple cyclic ether groups or cyclic thioether groups (hereinafter abbreviated as cyclic (thio)ether groups) in the molecule is particularly preferred. One type of thermosetting resin may be used alone, or two or more types may be used in combination.
[0050] The above-mentioned thermosetting resin having a plurality of cyclic (thio)ether groups in the molecule is a compound having a plurality of 3-, 4-, or 5-membered cyclic (thio)ether groups in the molecule, and examples thereof include a compound having a plurality of epoxy groups in the molecule, i.e., a polyfunctional epoxy compound; a compound having a plurality of oxetanyl groups in the molecule, i.e., a polyfunctional oxetane compound; and a compound having a plurality of thioether groups in the molecule, i.e., an episulfide resin.
[0051] Examples of polyfunctional epoxy compounds include epoxidized vegetable oils; bisphenol A type epoxy resins; hydroquinone type epoxy resins; bisphenol type epoxy resins; thioether type epoxy resins; brominated epoxy resins; novolac type epoxy resins; biphenol novolac type epoxy resins; bisphenol F type epoxy resins; hydrogenated bisphenol A type epoxy resins; glycidylamine type epoxy resins; hydantoin type epoxy resins; alicyclic epoxy resins; trihydroxyphenylmethane type epoxy resins; bixylenol type or biphenol type epoxy resins, or mixtures thereof. ; bisphenol S type epoxy resin; bisphenol A novolac type epoxy resin; tetraphenylolethane type epoxy resin; heterocyclic epoxy resin; diglycidyl phthalate resin; tetraglycidyl xylenoyl ethane resin; naphthalene group-containing epoxy resin; epoxy resin having a dicyclopentadiene skeleton; glycidyl methacrylate copolymer epoxy resin; cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin; epoxy-modified polybutadiene rubber derivative; CTBN-modified epoxy resin, etc., but are not limited to these.
[0052] Examples of polyfunctional oxetane compounds include bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, and (3-ethyl-3-oxetanyl)methyl acrylate. Examples of suitable oxetane compounds include polyfunctional oxetanes such as acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and oligomers or copolymers thereof, as well as ethers of oxetane alcohols with novolak resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or hydroxyl group-containing resins such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring with alkyl (meth)acrylates.
[0053] Examples of compounds having multiple cyclic thioether groups in the molecule include bisphenol A episulfide resins, etc. Also, episulfide resins in which the oxygen atoms of the epoxy groups of novolac epoxy resins are replaced with sulfur atoms using a similar synthesis method can be used.
[0054] Examples of amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.
[0055] The isocyanate compound may be a polyisocyanate compound, such as aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate, and 2,4-tolylene dimer; aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), and isophorone diisocyanate; alicyclic polyisocyanates such as bicycloheptane triisocyanate; and adducts, biuret compounds, and isocyanurates of the above-mentioned isocyanate compounds.
[0056] The blocked isocyanate compound can be an addition reaction product of an isocyanate compound and an isocyanate blocking agent. Examples of isocyanate compounds that can react with an isocyanate blocking agent include the polyisocyanate compounds described above. Examples of the isocyanate blocking agent include phenol-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, oxime-based blocking agents, mercaptan-based blocking agents, acid amide-based blocking agents, imide-based blocking agents, amine-based blocking agents, imidazole-based blocking agents, and imine-based blocking agents.
[0057] As the thermosetting resin, an epoxy resin is preferably used. Examples of commercially available epoxy resins include phenol novolac epoxy resin RE-306-SA9 manufactured by Nippon Kayaku Co., Ltd., phenol novolac epoxy resin EPICLON (registered trademark) N770-75EA manufactured by DIC Corporation, and biphenyl epoxy resin YX4000 manufactured by Mitsubishi Chemical Corporation.
[0058] The content of the thermosetting resin in the curable resin composition is preferably an amount such that the number of functional groups in the thermosetting resin that reacts with 1 mol of carboxyl groups contained in the carboxyl group-containing resin is 0.5 to 4.5 mol, more preferably 1.0 to 3.0 mol. When the content of the thermosetting resin is 0.5 mol or more, the amount of carboxyl groups remaining in the cured coating of the curable resin composition can be reduced, thereby achieving good heat resistance, alkali resistance, electrical insulation, etc. On the other hand, when the content of the thermosetting resin is 3.0 mol or less, the amount of low-molecular-weight cyclic (thio)ether groups remaining in the dried coating can be reduced, thereby ensuring good strength of the cured product of the curable resin composition.
[0059] (Photopolymerization initiator) The curable resin composition of the present invention contains a photopolymerization initiator. Any known photopolymerization initiator can be used as the photopolymerization initiator. One photopolymerization initiator may be used alone, or two or more photopolymerization initiators may be used in combination.
[0060] Examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Sphingoic acid, bisacylphosphine oxides such as bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenyl Monoacylphosphine oxides such as isopropyl phosphinate and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one hydroxyacetophenones such as 2-hydroxy-2-methyl-1-phenylpropan-1-one; benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ethers; benzophenones such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1- Acetophenones such as butanone and N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone anthraquinones such as acetophenone dimethyl ketal and 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O- oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium and titanocenes such as bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyr-1-yl)ethyl)phenyl]titanium; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like;
[0061] Examples of commercially available photopolymerization initiators include Omnirad 379 (2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one) manufactured by IGM Resins B.V. and IRGACURE (registered trademark) OXE02 manufactured by BASF Japan Ltd.
[0062] When a photopolymerization initiator other than an oxime ester-based photopolymerization initiator is used as the photopolymerization initiator, its content in the curable resin composition is not particularly limited as long as the effects of the present invention are achieved. However, it is preferably 0.5 to 5 mass% and more preferably 1 to 4 mass% in terms of solids content relative to the total mass of the curable resin composition. By setting the content of photopolymerization initiators other than oxime ester-based photopolymerization initiators to 0.5 mass% or more, the photocurability of the curable resin composition is improved, the cured coating is less likely to peel, and coating properties such as chemical resistance are also improved. On the other hand, by setting the content of photopolymerization initiators other than oxime ester-based photopolymerization initiators to 5 mass% or less, the effect of reducing outgassing is achieved, and further, light absorption at the surface of the curable resin composition layer is improved, preventing a decrease in deep curability. Furthermore, when an oxime ester-based photopolymerization initiator is used as the photopolymerization initiator, its content in the curable resin composition is preferably 0.005 to 1 mass% and more preferably 0.05 to 0.5 mass% in terms of solids content relative to the total mass of the curable resin composition. By setting the content of the oxime ester-based photopolymerization initiator to 0.005% by mass or more, the photocurability of the curable resin composition is improved, and the cured product thereof also has good properties such as heat resistance and chemical resistance. On the other hand, by setting the content of the oxime ester-based photopolymerization initiator to 1 part by mass or less, light absorption at the surface of the curable resin composition layer is improved, and deep curing is less likely to decrease.
[0063] A photoinitiator aid or sensitizer may be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator aid or sensitizer include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. In particular, it is preferable to use thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone. By including a thioxanthone compound as a photoinitiator aid or sensitizer, the deep curing properties of the layer of the curable resin composition can be improved. While these compounds may be used as photopolymerization initiators, it is preferable to use them in combination with a photopolymerization initiator. One type of photoinitiator aid or sensitizer may be used alone, or two or more types may be used in combination.
[0064] The above-mentioned photopolymerization initiator, photoinitiator assistant, and sensitizer each absorb light of a specific wavelength, and therefore, in some cases, the sensitivity may be reduced and they may function as ultraviolet absorbers. However, these are not used solely for the purpose of improving the sensitivity of the curable resin composition. If necessary, they can absorb light of a specific wavelength to increase the photoreactivity of the surface, change the line shape and opening of the resist to a vertical, tapered, or reverse tapered shape, and improve the accuracy of the line width and opening diameter.
[0065] (Photopolymerizable Monomer) The curable resin composition of the present invention contains a photopolymerizable monomer. When the above-mentioned carboxyl group-containing resin is a carboxyl group-containing resin that does not have an ethylenically unsaturated double bond, the curable resin composition can be made photocurable by using a photopolymerizable monomer in combination. The photopolymerizable monomer may be used alone or in combination of two or more.
[0066] The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond, and examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specific examples include alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Examples of suitable photopolymerizable monomers include polyhydric alcohols, alkylene oxide adducts, and ε-caprolactone adducts thereof; phenols, such as phenoxy acrylate and bisphenol A diacrylate, and polyhydric acrylates, such as alkylene oxide adducts thereof; glycidyl ether acrylates, such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and, without limitation, acrylates and melamine acrylates obtained by directly or via diisocyanate urethane acrylate of polyols, such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadienes, and polyester polyols, as well as methacrylates corresponding to the above acrylates. Such photopolymerizable monomers can also be used as reactive diluents. Dipentaerythritol hexaacrylate (DPHA) or the like is preferably used as the photopolymerizable monomer.
[0067] The (meth)acrylic group concentration of the photopolymerizable monomer is not particularly limited, but is, for example, 0.00100 to 0.01000 equivalents / g.
[0068] The content of the photopolymerizable monomer in the curable resin composition is not particularly limited as long as the effects of the present invention are achieved, but is preferably 5 to 50 parts by mass relative to 100 parts by mass of the carboxyl group-containing resin. When the content of the photopolymerizable monomer is 5 parts by mass or more, the photocurability of the curable resin composition is good, and pattern formation is easy in alkaline development after irradiation with active energy rays. On the other hand, when the content of the photopolymerizable monomer is 50 parts by mass or less, halation is less likely to occur during exposure, and good resolution can be obtained.
[0069] In one preferred embodiment, the content of the photopolymerizable monomer in the curable resin composition is adjusted so that 30 to 60%, preferably 40 to 55%, and even more preferably 45 to 55%, of the total amount of (meth)acrylic groups in the curable resin composition is derived from the photopolymerizable monomer.
[0070] (Thermosetting Catalyst) The curable resin composition of the present invention may contain a thermosetting catalyst as needed. Any known thermosetting catalyst can be used. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. The thermosetting catalyst is not limited to these, and may be a thermosetting catalyst for an epoxy resin or an oxetane compound, or one that promotes the reaction between at least one of an epoxy group and an oxetanyl group and a carboxyl group. Furthermore, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine-isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine-isocyanuric acid adduct can also be used as the thermosetting catalyst. These compounds that also function as adhesion promoters are preferably used in combination with the thermosetting catalyst. The thermosetting catalyst may be used alone or in combination of two or more. Dicyandiamide (DICY), melamine, etc. are preferably used as the thermosetting catalyst.
[0071] The content of the thermosetting catalyst in the curable resin composition is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the carboxyl group-containing resin. When the content of the thermosetting catalyst is 0.1 part by mass or more, the heat resistance of the curable resin composition is excellent. Furthermore, when the content of the thermosetting catalyst is 30 parts by mass or less, the storage stability of the curable resin composition is improved.
[0072] (Organic Solvent) The curable resin composition may contain an organic solvent for the purpose of adjusting the viscosity when preparing the curable resin composition or when applying the composition to a substrate or film, etc. As the organic solvent, known and commonly used organic solvents can be used. Examples of organic solvents include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. The organic solvent may be used alone or in combination of two or more. As the organic solvent, carbitol acetate (e.g., Dukisol CA manufactured by The Dow Chemical Company) is preferably used.
[0073] The organic solvent can be evaporated and dried using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which a dryer equipped with a heat source of an air heating type using steam is used, and hot air in the dryer is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0074] The content of the organic solvent in the curable resin composition can be appropriately changed depending on the materials constituting the curable resin composition and the method for applying the curable resin composition to a substrate. For example, when the curable resin composition is applied to a substrate by a screen printing method, it is preferable to adjust the content of the solvent so that the viscosity of the curable resin composition is 30 to 300 mPa·s. In the present invention, the viscosity of the resin composition is measured by taking 0.2 ml of the resin composition and measuring the viscosity at 25°C, 5 rpm (shear rate 10) using a cone-plate viscometer TV-33H (rotor 3°' x R9.7, manufactured by Toki Sangyo Co., Ltd.). -1 The viscosity is the value measured after rotating the sample at 1000 kJ / min for 30 seconds.
[0075] (Other Components) The curable resin composition may further contain, as necessary, components such as colorants, photoinitiator assistants, cyanate compounds, elastomers, mercapto compounds, urethane catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based antifoaming agents and leveling agents, silane coupling agents such as imidazole-based, thiazole-based, and triazole-based, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be those known in the field of electronic materials.
[0076] [Cured Product] According to another aspect of the present invention, a cured product of the curable resin composition of the present invention (hereinafter also referred to as the "cured product of the present invention") is provided. The cured product of the present invention is a cured product formed by curing the above-mentioned curable resin composition, and can have high resolution. Therefore, it can be suitably used as an insulating layer in electronic components such as printed wiring boards, where a fine cured product pattern is required.
[0077] [Dry Film] According to yet another aspect of the present invention, a dry film (hereinafter also referred to as "dry film of the present invention") comprising a layer of the curable resin composition of the present invention is provided. That is, the curable resin composition of the present invention can be in the form of a dry film comprising a first film and a resin layer comprising the curable resin composition formed on the first film. The first film in the dry film of the present invention refers to a film that is at least adhered to the resin layer when the dry film is integrally formed by laminating the resin layer formed on the dry film onto a substrate or other base material by heating or the like so that the resin layer side of the dry film is in contact with the resin layer side. The first film may be peeled from the resin layer in a step after lamination. In particular, in the dry film of the present invention, it is preferable to peel the first film from the resin layer in a step after exposure of the resin layer. When forming the curable resin composition of the present invention into a dry film, the curable resin composition is diluted with an organic solvent as needed to adjust the viscosity to an appropriate level, and then coated to a uniform thickness on a first film using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and typically dried for 1 to 30 minutes at a temperature of 50 to 130° C. to obtain a coating film. There are no particular restrictions on the film thickness when the curable resin composition is applied, but it is generally adjusted appropriately so that the film thickness after drying is in the range of 1 to 150 μm, preferably 10 to 60 μm.
[0078] The first film can be any known film without particular limitation, and examples of suitable films include polyester films such as polyethylene terephthalate and polyethylene naphthalate, and films made of thermoplastic resins such as polyimide films, polyamideimide films, polypropylene films, and polystyrene films. Among these, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. A laminate comprising a combination of multiple films can also be used as the first film.
[0079] Moreover, from the viewpoint of improving mechanical strength, the film made of the above-mentioned thermoplastic resin is preferably a film stretched in a uniaxial or biaxial direction.
[0080] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0081] After forming a resin layer of the curable resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer. The second film refers to a film that is peeled from the resin layer before lamination when the resin layer side of the laminate of the first film and the resin layer is in contact with a substrate or other base material by heating or the like to form an integral structure. Examples of such a second film include polyethylene film, polytetrafluoroethylene film, polypropylene film, surface-treated paper, etc. Furthermore, the relationship between the adhesive strength of the first film and the second film is such that, when the second film is peeled off, the adhesive strength between the resin layer and the second film is smaller than the adhesive strength between the resin layer and the first film.
[0082] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0083] In the production of the dry film of the present invention, the curable resin composition of the present invention may be applied to the second film described above and dried to form a resin layer, and the first film may be laminated on the surface of the resin layer. That is, in the production of the dry film of the present invention, the film to which the curable resin composition of the present invention is applied may be either the first film or the second film.
[0084] [Printed Wiring Board] According to yet another aspect of the present invention, there is provided a printed wiring board (hereinafter also referred to as "printed wiring board of the present invention") comprising the cured product of the present invention. The printed wiring board of the present invention comprises a cured product obtained by curing the curable resin composition of the present invention or the resin layer of the dry film.
[0085] The printed wiring board of the present invention can be manufactured, for example, according to the following procedure. First, the curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using an organic solvent as needed, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating. Next, the organic solvent contained in the curable resin composition is evaporated and dried (pre-dried) at a temperature of 60 to 100°C to form a tack-free resin layer. When a dry film is used, it is attached to the substrate using a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.
[0086] Substrates constituting printed wiring boards include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as copper-clad laminates for high-frequency circuits made from materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, polyphenylene oxide / cyanate, etc., and include copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.
[0087] The dry film is preferably bonded to the substrate under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, the dry film adheres tightly to the circuit substrate even if the circuit substrate surface is uneven, preventing the inclusion of air bubbles and improving the filling of recesses in the substrate surface. The pressure conditions are preferably about 0.1 to 2.0 MPa, and the heating conditions are preferably 40 to 120°C.
[0088] The volatilization drying carried out after the curable resin composition of the present invention is applied to a substrate can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating type using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0089] After forming a resin layer on a substrate, if necessary, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed areas are developed with a dilute alkaline aqueous solution (e.g., a 0.3 to 3% by weight aqueous solution of sodium carbonate) to form a cured product pattern. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is carried out to form a patterned cured product on the substrate. Note that, as long as the properties are not impaired, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed. Furthermore, a cured film with excellent properties such as adhesion and hardness can be formed by irradiating the cured product with active energy rays and then heat-curing (e.g., 100 to 220°C), or by irradiating active energy rays after heat-curing, or by heat-curing alone to perform final finish curing (main curing).
[0090] The exposure device used for the above-mentioned active energy ray irradiation may be a device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging device (for example, a laser direct imaging device that draws an image directly with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging device may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for image formation varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0091] The exposure method for the curable resin composition of the present invention is not particularly limited, and various conventionally employed exposure methods can be appropriately selected. However, since the curable resin composition of the present invention has high sensitivity to exposure and can form a high-resolution cured product pattern in a short exposure time, it can be suitably used in a moving exposure method such as direct imaging.
[0092] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or an amine.
[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all by mass unless otherwise specified.
[0094] [Preparation of Curable Resin Composition] (Synthesis of Carboxyl Group-Containing Resin A-1) Prior to preparing the curable resin composition, the carboxyl group-containing resin A-1 used in this example was prepared according to the procedure described below. First, 220 parts (1 equivalent) of cresol novolac epoxy resin (manufactured by Nippon Kayaku Co., Ltd., ECON-104S, epoxy equivalent: 220) was placed in a four-neck flask equipped with a stirrer and a reflux condenser, and 218 parts of carbitol acetate was added and heated to dissolve. Next, 0.46 parts of methylhydroquinone as a polymerization inhibitor and 1.38 parts of triphenylphosphine as a reaction catalyst were added. The resulting mixture was heated to 95-105°C, and 50.4 parts (0.7 equivalents) of acrylic acid and 41.5 parts (0.3 equivalents) of p-hydroxyphenethyl alcohol were slowly added dropwise, followed by a 16-hour reaction. The resulting reaction product (hydroxyl group: 1.3 equivalents) was cooled to 80-90°C, 91.2 parts (0.6 equivalents) of tetrahydrophthalic anhydride was added, and the mixture was reacted for 8 hours. After cooling, the mixture was removed and a solution of carboxyl group-containing resin A-1 was obtained. The resulting carboxyl group-containing resin A-1 had a weight average molecular weight of 14,000, a solids content of 65%, and an acid value of the solids of 83 mgKOH / g.
[0095] (Synthesis of Carboxyl Group-Containing Resin A-2) Prior to the preparation of the curable resin composition, the carboxyl group-containing resin A-2 used in this example was prepared according to the procedure described below. First, 456 parts of bisphenol A, 228 parts of water, and 649 parts of 37% formalin were placed in a flask equipped with a cooling tube and a stirrer, and 228 parts of a 25% aqueous sodium hydroxide solution was added while maintaining the temperature at 40°C or below. After the addition was completed, the mixture was reacted at 50°C for 10 hours. After the reaction was completed, the mixture was cooled to 40°C, and a 37.5% aqueous phosphoric acid solution was added while maintaining the temperature at 40°C or below to neutralize the mixture to pH 4. The reaction solution was then allowed to stand, and the aqueous layer was separated. After the aqueous layer was separated, 300 parts of methyl isobutyl ketone was added and uniformly dissolved, washed three times with 500 parts of distilled water, and the water, solvent, etc. were removed under reduced pressure at a temperature of 50°C or below. The obtained polymethylol compound was dissolved in 550 parts of methanol, yielding 1,230 parts of a methanol solution of the polymethylol compound. A portion of the resulting methanol solution of the polymethylol compound was dried at room temperature in a vacuum dryer, revealing a solids content of 55.2%. Next, 500 parts of the resulting methanol solution of the polymethylol compound and 440 parts of 2,6-xylenol were uniformly dissolved at 50°C. After uniform dissolution, the methanol was removed under reduced pressure at a temperature of 50°C or less. Next, 8 parts of oxalic acid was added, and the reaction was carried out at 100°C for 10 hours. After completion of the reaction, the distillate was removed under reduced pressure at 180°C and 50 mmHg, yielding 550 parts of novolak resin A. Next, 130 parts of the resulting novolak resin A, 2.6 parts of a 50% aqueous sodium hydroxide solution, and 100 parts of toluene / methyl isobutyl ketone (mass ratio = 2 / 1) were placed in an autoclave equipped with a thermometer, a nitrogen / alkylene oxide introducing device, and a stirrer. The system was purged with nitrogen while stirring, and then heated to 150°C and 8 kg / cm. 2 45 parts of ethylene oxide was gradually introduced and the reaction was carried out under a reaction gauge pressure of 0.0 kg / cm. 2The reaction mixture was stirred for about 4 hours until the reaction mixture reached a concentration of 0.01% and then cooled to room temperature. 3.3 parts of a 36% aqueous hydrochloric acid solution was added to the reaction solution and mixed to neutralize the sodium hydroxide. The resulting neutralized reaction product was diluted with toluene, washed with water three times, and the solvent was removed using an evaporator to obtain an ethylene oxide adduct of novolak resin A with a hydroxyl value of 175 g / eq. This means that the resulting ethylene oxide adduct of novolak resin A had an average of 1 mole of ethylene oxide added per equivalent of phenolic hydroxyl group. Next, 175 parts of the obtained ethylene oxide adduct of novolak resin A, 50 parts of acrylic acid, 3.0 parts of p-toluenesulfonic acid, 0.1 parts of hydroquinone monomethyl ether, and 130 parts of toluene were placed in a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and the mixture was stirred while blowing in air, heated to 115°C, and reacted for an additional 4 hours while distilling off water produced by the reaction as an azeotrope with toluene, and then cooled to room temperature. The resulting reaction solution was washed with a 5% aqueous NaCl solution, and the toluene was removed by distillation under reduced pressure. Then, diethylene glycol monoethyl ether acetate was added to obtain an acrylate resin solution with a solids content of 68%. Next, 312 parts of the obtained acrylate resin solution, 0.1 parts of hydroquinone monomethyl ether, and 0.3 parts of triphenylphosphine were placed in a four-neck flask equipped with a stirrer and a reflux condenser, and the mixture was heated to 110°C, 45 parts of tetrahydrophthalic anhydride was added, and the mixture was reacted for 4 hours. After cooling, the mixture was removed and a solution of carboxyl group-containing resin A-2 was obtained. The obtained carboxyl group-containing resin A-2 had a weight average molecular weight of 12,000, a solids content of 70%, and an acid value of the solids of 65 mgKOH / g.
[0096] (Synthesis of Carboxyl Group-Containing Resin A-3) Prior to the preparation of the curable resin composition, the carboxyl group-containing resin A-3 used in this example was prepared according to the procedure shown below. First, 119.4 parts of a novolac cresol resin (Showa Denko K.K.'s Shownol CRG951, OH equivalent: 119.4), 1.19 parts of potassium hydroxide, and 119.4 parts of toluene were placed in an autoclave equipped with a thermometer, a nitrogen introducing device / alkylene oxide introducing device, and a stirrer, and the system was purged with nitrogen while stirring, and the temperature was raised by heating. Next, 63.8 parts of propylene oxide were slowly added dropwise, and the temperature was raised to 125 to 132°C and the pressure to 0 to 4.8 kg / cm. 2The reaction was carried out at 100°C for 16 hours. The system was then cooled to room temperature, and 1.56 parts of 89% by weight phosphoric acid was added to the resulting reaction solution and mixed to neutralize the potassium hydroxide, yielding a propylene oxide reaction solution of novolac cresol resin with a nonvolatile content of 62.1% and a hydroxyl value of 182.2 g / eq. The resulting novolac cresol resin had an average of 1.08 moles of alkylene oxide added per equivalent of phenolic hydroxyl group. Next, 293.0 parts of the resulting alkylene oxide reaction solution of novolac cresol resin, 43.2 parts of acrylic acid, 11.53 parts of methanesulfonic acid, 0.18 parts of methylhydroquinone, and 252.9 parts of toluene were placed in a reactor equipped with a stirrer, thermometer, and air inlet tube, and the mixture was reacted at 110°C for 12 hours with stirring and air blown in at a rate of 10 ml / min. The water produced by the reaction was distilled as an azeotrope with toluene, and 12.6 parts of water were distilled off. The system was then cooled to room temperature, and the resulting reaction solution was neutralized with 35.35 parts of a 15% aqueous sodium hydroxide solution and washed with water. The toluene was then distilled off using an evaporator while being replaced with 118.1 parts of diethylene glycol monoethyl ether acetate (carbitol acetate), yielding a novolac acrylate resin solution. Next, 332.5 parts of the resulting novolac acrylate resin solution and 1.22 parts of triphenylphosphine were placed in a reactor equipped with a stirrer, thermometer, and air inlet tube, and air was blown in at a rate of 10 ml / min. While stirring, 60.8 parts of tetrahydrophthalic anhydride was gradually added, and the mixture was allowed to react at a temperature of 95 to 101°C for 6 hours. After cooling, the mixture was removed and a solution of carboxyl group-containing resin A-3 was obtained. The resulting carboxyl group-containing resin A-3 had a weight average molecular weight of 3,000, a solid content of 65%, and an acid value of the solid content of 88 mgKOH / g.
[0097] (Preparation of (meth)acrylic group-containing surface-treated inorganic filler B'-1) The (meth)acrylic group-containing surface-treated inorganic filler B'-1 used in this example was prepared according to the procedure shown below. Specifically, 70 g of spherical silica (SFP-30M manufactured by Denka Corporation, solids content 100%), 27 g of PMA (propylene glycol monomethyl ether acetate) as a solvent, and 3 g of KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd. as a silane coupling agent were uniformly dispersed to obtain a silica solvent-dispersed (meth)acrylic group-containing surface-treated inorganic filler B'-1.
[0098] (Preparation of (meth)acrylic group-containing surface-treated inorganic filler B'-2) The (meth)acrylic group-containing surface-treated inorganic filler B'-2 used in this example was prepared according to the procedure shown below. Specifically, 233 g of spherical silica (organosilica sol PGM-ST manufactured by Nissan Chemical Industries, Ltd., solids content 30%) and 3 g of silane coupling agent KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd. were uniformly dispersed to obtain a silica solvent-dispersed (meth)acrylic group-containing surface-treated inorganic filler B'-2.
[0099] (Preparation of (meth)acrylic group-containing surface-treated inorganic filler B'-3) The (meth)acrylic group-containing surface-treated inorganic filler B'-3 used in this example was prepared according to the procedure shown below. Specifically, 233 g of spherical silica (organosilica sol PGM-ST manufactured by Nissan Chemical Industries, Ltd., solids content 30%) and 36 g of silane coupling agent KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd. were uniformly dispersed to obtain a silica solvent-dispersed (meth)acrylic group-containing surface-treated inorganic filler B'-3.
[0100] The components shown in Table 1 below were mixed in the amounts shown in the table, pre-mixed using a mixer, and then kneaded using a three-roll mill to prepare the curable resin compositions of Examples 1 to 13 and Comparative Examples 1 and 2. Details of each component in Table 1 are as follows. The (meth)acrylic group concentration of all components other than each carboxyl group-containing resin and each inorganic filler was 0 equivalents / g. Carboxyl group-containing resin A-1: A carboxyl group-containing resin obtained by synthesizing the above-described carboxyl group-containing resin A-1. Carboxyl group-containing resin A-2: A carboxyl group-containing resin obtained by synthesizing the above-described carboxyl group-containing resin A-2. Carboxyl group-containing resin A-3: A carboxyl group-containing resin obtained by synthesizing the above-described carboxyl group-containing resin A-3. Inorganic filler B-1: Organosilica sol PGM-ST (particle diameter 12 nm, (meth)acrylic group concentration 0 equivalents / g) manufactured by Nissan Chemical Industries Co., Ltd. that was not surface-treated. Inorganic filler B-2: Barium sulfate B-30 (acrylic group concentration 0 equivalents / g) manufactured by Sakai Chemical Industry Co., Ltd. Inorganic filler B'-1: Solvent dispersion B'-1 of silica surface-treated with methacrylsilane prepared above (particle diameter 550 nm, (meth)acrylic group concentration 0.00011 equivalents / g). Inorganic filler B'-2: Solvent dispersion B'-2 of silica surface-treated with methacrylsilane prepared above (particle diameter 12 nm, (meth)acrylic group concentration 0.00005 equivalents / g). Inorganic filler B'-3: Solvent dispersion B'-3 of silica surface-treated with methacrylsilane prepared above (particle diameter 12 nm, (meth)acrylic group concentration 0.00050 equivalents / g). Thermosetting resin C-1: Phenol novolac epoxy resin RE-306-SA9 (solid content epoxy group equivalent 180) manufactured by Nippon Kayaku Co., Ltd. Thermosetting resin C-2: Phenol novolac epoxy resin EPICLON (registered trademark) N770-75EA (solid content epoxy group equivalent 190) manufactured by DIC Corporation. Thermosetting resin C-3: Biphenyl epoxy resin YX4000 (solid content epoxy group equivalent 190) manufactured by Mitsubishi Chemical Corporation. Photopolymerization initiator D-1: Omnirad 379 (2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one) manufactured by IGM Resins B.V.Photopolymerization initiator D-2: IRGACURE (registered trademark) OXE02 manufactured by BASF Japan Ltd. Photopolymerizable monomer E-1: dipentaerythritol hexaacrylate (DPHA) Colorant F-1: Firstgen Blue 5380 Colorant F-2: Yellow S1515 / AGR Heat curing catalyst G-1: dicyandiamide (DICY) Heat curing catalyst G-2: melamine Additive H-1: oil compound type defoamer KS-66 manufactured by Shin-Etsu Chemical Co., Ltd. Organic solvent I-1: Jukisol CA (carbitol acetate) manufactured by Dow Chemical Japan Ltd.
[0101] [Measurement of (meth)acrylic group concentration of carboxyl group-containing resin and photopolymerizable monomer] The (meth)acrylic group concentration of each of the above-mentioned carboxyl group-containing resins and photopolymerizable monomers was measured according to the following procedure. First, 0.1 g of each carboxyl group-containing resin and photopolymerizable monomer sample was precisely weighed and dissolved in 10 ml of morpholine using ultrasound. 7 ml of a 1:1 acetic acid:water mixed solution was added, and the mixture was heated at 98°C in an oil bath for 30 minutes to react with the morpholine. The reaction solution was then left at room temperature, and 25 ml of methyl cellosolve and 20 ml of acetic anhydride were added to react with the unreacted morpholine. The mixture was then left at room temperature to prepare a solution for measurement. The resulting solution was titrated with 0.1 N perchloric acid solution to calculate the (meth)acrylic group concentration.
[0102]
[0103] For each of the obtained curable resin compositions, the “total amount of solids in the curable resin composition,” “(meth)acrylic group concentration relative to the total amount of solids in the curable resin composition,” “(E) (meth)acrylic group concentration ratio in the solids derived from the polymerizable monomer,” “(A) (meth)acrylic group concentration ratio in the solids derived from the carboxyl group-containing resin,” and “(B′) (meth)acrylic group concentration ratio in the solids derived from the acrylic group-containing surface-treated inorganic filler” are shown in Table 1.
[0104] [Evaluation of Photocurability (Sensitivity)] The photocurability (sensitivity) of each curable resin composition was evaluated according to the following procedure. First, each curable resin composition was applied by screen printing to the entire surface of a copper-plated substrate (a copper-plated FR-4 copper-clad laminate substrate having a size of 15 cm x 9.5 cm, a thickness of 0.8 mm, and a circuit thickness of 18 μm) that had been surface-treated (CZ8101B chemical solution, CZ roughening treatment at an etching rate of 1.0 μm) so that the film thickness after drying would be 15 μm, and the composition was dried for 20 minutes in a hot air circulation drying oven at 80 ° C. Next, exposure was performed using a DI exposure machine (exposure device Mms-60 manufactured by Oak Corporation) via a Kodak Photographic Step Tablet No. 2 manufactured by Eastman Kodak Company. Next, a 1 wt % aqueous sodium carbonate solution was used, and the coating was applied at a spray pressure of 2 kg / cm 2 The photocurability (sensitivity) of each curable resin composition was evaluated according to the following evaluation criteria, based on the exposure dose at which the number of remaining steps after development was 10. The evaluation results are shown in Table 1. ⊚: The exposure dose at which the number of remaining steps after development was 10 was 150 mJ cm 2 ○: The exposure amount at which the number of remaining steps after development is 10 is less than 150 mJ / cm 2 More than 300mJ / cm 2 ×: The exposure amount at which the number of remaining steps after development is 10 is less than 300 mJ / cm 2 That's all.
[0105] [Evaluation of Resolution] The resolution of the cured product of each curable resin composition was evaluated according to the following procedure. First, a copper-plated substrate (a copper-plated FR-4 copper-clad laminate substrate having a size of 15 cm x 9.5 cm, a thickness of 0.8 mm, and a circuit thickness of 18 μm) that had been surface-treated (CZ8101B chemical solution, CZ roughening treatment at an etching rate of 1.0 μm) was coated with each curable resin composition by screen printing to a film thickness of 15 μm after drying, and dried for 20 minutes in a hot air circulation drying oven at 80 ° C. Next, using a Kodak Photographic Step Tablet No. 2 manufactured by Eastman Kodak Co., a DI exposure machine (an exposure device Mms-60 manufactured by Oak Corporation) was used to expose the substrate to various opening patterns (openings of Φ30 to 150 μm (every Φ10 μm) formed at 200 μm intervals) at an exposure dose such that the number of remaining steps after the existing step was 10. Next, a 1 wt % aqueous solution of sodium carbonate was used at a spray pressure of 2 kg / cm 2 Then, the film was developed in a UV conveyor oven at an integrated exposure dose of 1000 mJ / cm. 2 and heated at 150°C for 60 minutes to obtain a substrate for resolution evaluation. The aperture diameter of the obtained substrate for resolution evaluation was observed at 500x magnification using a JEOL Ltd. electron microscope JSM-6610LV, and the resolution of the cured product was evaluated based on the size of the smallest aperture diameter at which no halation or undercut occurred, according to the following evaluation criteria: ⊚: The smallest aperture diameter at which no halation or undercut occurred was less than 60 μm. ◯: The smallest aperture diameter at which no halation or undercut occurred was 60 μm or more and less than 90 μm. △: The smallest aperture diameter at which no halation or undercut occurred was 90 μm or more and less than 120 μm. ×: The smallest aperture diameter at which no halation or undercut occurred was 120 μm or more.
[0106] [Evaluation of Breaking Strength of Cured Product] The breaking strength of the cured product of each curable resin composition was evaluated according to the following procedure. First, each curable resin composition was applied by screen printing to the entire glossy surface of a 18 μm thick copper foil cut to a size of 150 mm x 100 mm, so that the film thickness after drying would be 30 μm, and the composition was dried for 20 minutes in a hot air circulation drying oven at 80°C. Next, a strip pattern of 10 mm wide x 80 mm long was exposed using a DI exposure machine (exposure device Mms-60 manufactured by Oak Corporation) with an exposure amount equivalent to 10 steps using Kodak Photographic Step Tablet No. 2 manufactured by Eastman Kodak Company. Next, a 1 wt % aqueous sodium carbonate solution was used, sprayed at a pressure of 2 kg / cm 2 Then, the film was developed in a UV conveyor oven at an integrated exposure dose of 1000 mJ / cm. 2 The specimen was irradiated with ultraviolet light under the conditions of 0.1 to 1.0 V and heated at 150°C for 60 minutes to obtain a cured product. The copper foil was peeled off from the obtained cured product to obtain a sample for evaluation of breaking strength. A tensile test was performed on the sample for evaluation of breaking strength at a gripping distance of 40 mm and a pulling rate of 1 mm / min to measure the maximum point stress. The measurement was performed using a tensile tester AGS-G100N manufactured by Shimadzu Corporation, and the maximum point stress was evaluated. The breaking strength of the evaluation sample was evaluated according to the following evaluation criteria: ⊚: Maximum point stress is 80 MPa or more; ○: Maximum point stress is 60 MPa or more and less than 80 MPa; ×: Maximum point stress is less than 60 MPa.
[0107] [Evaluation of Solder Heat Resistance] The solder heat resistance of the cured product of each curable resin composition was evaluated according to the following procedure. First, each curable resin composition was applied by screen printing to the entire surface of an FR-4 copper-clad laminate substrate having a length of 15 cm, a width of 9.5 cm, a thickness of 0.8 mm, and a circuit thickness of 18 μm, so that the film thickness on the copper after drying would be 15 μm, and the substrate was dried for 20 minutes in a hot air circulation drying oven at 80°C. Next, exposure was performed using a DI exposure machine (exposure device Mms-60 manufactured by Oak Corporation) at an exposure amount equivalent to 10 steps using Kodak Photographic Step Tablet No. 2 manufactured by Eastman Kodak Company. Next, a 1 wt % aqueous sodium carbonate solution was used, and the coating was sprayed at a pressure of 2 kg / cm. 2Then, the film was developed in a UV conveyor oven at an integrated exposure dose of 1000 mJ / cm. 2 and heated at 150°C for 60 minutes to obtain a substrate for evaluation of soldering heat resistance. A rosin-based flux was applied to the obtained substrate for evaluation of soldering heat resistance, and then the substrate was immersed for 10 seconds in a solder bath previously set to 260°C. The flux was then washed off with ethanol, and the cured product was visually inspected for swelling and peeling, and evaluated according to the following criteria: ⊚: No peeling was observed in the cured product even after 10-second immersion was repeated five or more times. ○: Peeling was observed in the cured product after 10-second immersion was repeated three to five times. ×: Swelling and peeling were observed in the cured product within three 10-second immersions.
[0108] [Evaluation of Dryness to Touch] The dryness to touch of each curable resin composition was evaluated according to the following procedure. First, each curable resin composition was applied by screen printing to the entire surface of a substrate (size 15 cm × 9.5 cm, thickness 1.6 mm, FR-4 copper-clad laminate substrate) having a circuit pattern with a copper thickness of 18 μm, so that the film thickness on the copper after drying would be 15 μm, and the composition was dried in a hot air circulation drying oven at 80°C for 20 minutes to form a resin layer. The surface of the resin layer was directly touched with the index finger for 1 minute with enough strength to touch the entire fingertip, and the presence or absence of stickiness was confirmed. The dryness to touch was evaluated according to the following criteria: ⊚: No stickiness at all. ○: Slight stickiness. ×: Stickiness.
[0109] From the results shown in Table 1, it can be seen that the curable resin compositions of Examples 1 to 13, which contain a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer and have a (meth)acrylic group concentration adjusted to 0.00070 to 0.00170 equivalents / g relative to the total mass of the solids of the curable resin composition, have excellent photocurability (sensitivity) and resolution. On the other hand, the curable resin compositions of Comparative Examples 1 and 2, which contain a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator, and a photopolymerizable monomer but have a (meth)acrylic group concentration not adjusted to 0.00070 to 0.00170 equivalents / g relative to the total mass of the solids of the curable resin composition, have poor photocurability (sensitivity) and resolution.
[0110] Furthermore, it can be seen that each of the curable resin compositions of Examples 1 to 13 is excellent in not only photocurability (sensitivity) and resolution, but also in the dryness to the touch of the curable resin composition, and the breaking strength and solder heat resistance of the cured product.
Claims
1. A curable resin composition comprising a carboxyl group-containing resin, an inorganic filler, a thermosetting resin, a photopolymerization initiator and a photopolymerizable monomer, characterized in that the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is 0.00070 to 0.00170 equivalents / g.
2. The curable resin composition according to claim 1, wherein the (meth)acrylic group is derived from the photopolymerizable monomer in an amount of 30 to 60% of the total amount of (meth)acrylic groups relative to the total mass of solids in the curable resin composition.
3. The curable resin composition according to claim 1, wherein the inorganic filler comprises an inorganic filler having a (meth)acrylic group on a surface thereof, and of the concentration of the total amount of (meth)acrylic groups relative to the total mass of solids in the curable resin composition, 30 to 60% is derived from the carboxyl group-containing resin, 5 to 30% is derived from the inorganic filler having a (meth)acrylic group, and 30 to 60% is derived from the photopolymerizable monomer.
4. The curable resin composition according to claim 1, wherein the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is 0.00070 to 0.00140 equivalents / g.
5. The curable resin composition according to claim 1, wherein the (meth)acrylic group is derived from the photopolymerizable monomer in an amount of 40 to 55% of the total amount of (meth)acrylic groups relative to the total mass of solids in the curable resin composition.
6. The curable resin composition according to claim 1, wherein the concentration of the total amount of (meth)acrylic groups relative to the total mass of the solid content of the curable resin composition is 0.00080 to 0.00110 equivalents / g.
7. The curable resin composition according to claim 1, wherein the (meth)acrylic group is derived from the photopolymerizable monomer in an amount of 45 to 55% of the total amount of (meth)acrylic groups relative to the total mass of solids in the curable resin composition.
8. A cured product obtained by curing the curable resin composition according to claim 1.
9. A printed wiring board comprising the cured product according to claim 8.
10. A method for manufacturing a printed wiring board having an insulating layer, comprising the step of forming the insulating layer by curing the curable resin composition according to claim 1.
Citation Information
Patent Citations
Photosensitive resin composition and hardened product
JP2004294882A
Photocurable resin composition, photosensitive thermosetting resin composition and its cured product
JP2004359890A
Photo-solder resist dry film and resin composition for producing the same, and solder resist film
JP2007316545A
Curable resin composition, dry film, cured product and electronic component
JP2020140065A
Dry film, cured product and electronic component
JP2020166215A