Thermally conductive sheet and method for manufacturing same

The thermally conductive sheet with an acrylic adhesive layer and reactive double bonds addresses adhesion issues during high-temperature processes, enhancing both adhesion and thermal conductivity for semiconductor applications.

WO2024204753A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013141
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermally conductive sheets used in semiconductor packages face challenges in maintaining adhesion to adherends during high-temperature processes like reflow, as existing solutions either compromise thermal conductivity or peel off due to decreased tack force.

Method used

A thermally conductive sheet with a polymer matrix and anisotropic filler, featuring an acrylic adhesive layer with reactive double bonds, which enhances adhesion and maintains strength even at high temperatures by crosslinking with the adherend and organopolysiloxane hydrosilyl groups.

Benefits of technology

The sheet achieves improved adhesion and thermal conductivity while preventing peeling during high-temperature processes, maintaining die shear strength and ensuring effective heat dissipation in semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000052_0000
    Figure 00000052_0000
Patent Text Reader

Abstract

This thermally conductive sheet comprising: a thermally conductive layer containing a polymer matrix and a thermally conductive filler; and an acrylic adhesive layer provided on the surface of the thermally conductive layer, wherein the acrylic adhesive layer has a reactive double bond.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive sheet and manufacturing method thereof

[0001] The present invention relates to a thermally conductive sheet and a method for producing the same.

[0002] In recent years, with the increasing density of wiring in multilayer wiring boards, the increasing density of wiring in semiconductor packages, the increased mounting density of electronic components, and the increased heat generation per unit area due to the high integration of semiconductor elements themselves, there has been a demand for improved heat dissipation from semiconductor packages. It is known that semiconductor packages dissipate heat by sandwiching a heat dissipation material between a heat-generating body such as a semiconductor chip and a heat dissipating body called a heat spreader. Thermally conductive grease has traditionally been widely used as the heat dissipation material placed between the semiconductor chip and the heat spreader.

[0003] Semiconductor packages are generally heated above a certain temperature during use. Because each component, such as the substrate, semiconductor chip, and heat spreader, has a different thermal expansion coefficient, warping can occur when heated. As chips have become larger in recent years, the gaps caused by warping have also become larger. Thermally conductive grease cannot accommodate this warping, resulting in gaps. Therefore, the use of thermally conductive sheets instead of thermally conductive grease is being considered.

[0004] Thermally conductive sheets used in the above applications are required to have improved flexibility to accommodate warpage while also improving heat dissipation. However, when attempting to improve both heat dissipation and flexibility, the thermally conductive sheet's adhesion to surrounding components decreases, raising concerns that it may not be able to accommodate warpage as with thermally conductive grease and may peel off from the semiconductor chip or heat spreader. For this reason, for example, Patent Document 1 attempts to increase tack by blending a thermally conductive sheet with liquid polybutene, an acrylic ester polymer, an ethylene-α-olefin copolymer, a hot melt agent, or the like to increase the sheet's tackiness and prevent peeling from the semiconductor chip or heat spreader.

[0005] Patent No. 7067571

[0006] Semiconductor packages are generally manufactured through a reflow process that involves high-temperature heating. Therefore, thermally conductive sheets placed between a semiconductor chip and a heat spreader are often required to maintain adhesion to the semiconductor chip, heat spreader, or other adherends even after high-temperature heating. However, as described in Patent Document 1, simply improving the tack strength of thermally conductive sheets can result in a decrease in tack strength during high-temperature heating, such as in the reflow process, which can cause the sheets to peel off from the adherend.

[0007] Therefore, an object of the present invention is to provide a thermally conductive sheet that can adhere closely to an adherend and can prevent peeling from the adherend even after high-temperature heating such as reflow.

[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by incorporating a reactive double bond into a thermally conductive sheet comprising a thermally conductive layer containing a polymer matrix and a thermally conductive filler, and an acrylic adhesive layer provided on the surface of the thermally conductive layer, and have completed the present invention as described below.

[0009] That is, the present invention provides the following [1] to

[14] . [1] A thermally conductive sheet comprising a thermally conductive layer containing a polymer matrix and a thermally conductive filler, and an acrylic adhesive layer provided on the surface of the thermally conductive layer, wherein the acrylic adhesive layer has a reactive double bond. [2] The thermally conductive sheet according to [1] above, wherein the acrylic adhesive layer has a Raman spectrum intensity ratio A / B of the peak intensity A of C=C stretching vibration to the peak intensity B of C=O stretching vibration, of 0.2 or more. [3] The thermally conductive sheet according to [1] or [2] above, wherein the polymer matrix is ​​organopolysiloxane. [4] The thermally conductive sheet according to any of [1] to [3] above, wherein the thermally conductive layer contains an anisotropic filler oriented in the thickness direction of the thermally conductive layer. [5] The thermally conductive sheet according to any of [1] to [4] above, wherein the surface of the thermally conductive layer is a sliced ​​surface. [6] The thermally conductive sheet according to any of [1] to [5] above, wherein the acrylic adhesive layer is impregnated into the thermally conductive layer. [7] A method for producing a thermally conductive sheet, comprising: mixing at least a curable polymer composition and a thermally conductive filler to obtain a mixed composition; curing the mixed composition by heating to obtain a cured product; and applying an adhesive to the surface of the cured product, wherein the adhesive is an acrylic adhesive having a reactive double bond. [8] A method for producing a thermally conductive sheet as described in [7] above, comprising heating the mixed composition to obtain a molded product, slicing the molded product, and forming the cured product into a sheet. [9] A method for producing a thermally conductive sheet as described in [7] or [8] above, comprising mixing a compatible substance in addition to the curable polymer composition and the thermally conductive filler to obtain the mixed composition, and volatilizing at least a portion of the compatible substance by heating.

[10] A method for producing a thermally conductive sheet as described in any of [7] to [9] above, comprising allowing the applied adhesive to penetrate into the cured product.

[11] A bonding method comprising: a bonding step of sandwiching the thermally conductive sheet according to any one of [1] to [6] above between a semiconductor chip and a heat spreader to bring them into close contact; and a bonding step of bonding the semiconductor chip and the heat spreader, which are heated to 200°C or higher after the bonding step.

[12] The bonding method according to

[11] above, wherein in the adhering step, the thermally conductive sheet is sandwiched between the semiconductor chip and the heat spreader, and then pressure is applied at 50° C. or higher and 200° C. or lower to adhere them together.

[13] The bonding method according to

[11] or

[12] above, wherein the adhering step is performed without applying pressure.

[14] Use of a thermally conductive sheet for adhering a semiconductor chip and a heat spreader in a reflow step, the thermally conductive sheet comprising: a thermally conductive layer containing a polymer matrix and a thermally conductive filler; and an acrylic adhesive layer provided on the surface of the thermally conductive layer, the acrylic adhesive layer having a reactive double bond.

[0010] According to the present invention, it is possible to provide a thermally conductive sheet that can adhere closely to an adherend and that is prevented from peeling off from the adherend even after undergoing high-temperature heating such as a reflow process.

[0011] 1 is a schematic diagram of a thermal resistance measuring machine. FIG. 2 is a schematic diagram showing a method for measuring die shear strength.

[0012] [Thermal Conductive Sheet] The thermal conductive sheet of the present invention comprises a thermal conductive layer containing a polymer matrix and a thermally conductive filler, and an acrylic adhesive layer provided on the surface of the thermal conductive layer. The thermal conductive sheet will be described in detail below.

[0013] (Acrylic Adhesive Layer) In the present invention, the acrylic adhesive layer has a reactive double bond. The reactive double bond allows the acrylic adhesive layer to maintain its adhesion to an adherend, such as a heat spreader or a semiconductor chip, even when heated to high temperatures during a reflow process or the like, preventing peeling from the adherend. Furthermore, the acrylic adhesive layer can maintain high adhesion even when used in a relatively high-temperature environment, such as about 150°C, in actual use. It is generally known that acrylic adhesives significantly reduce their adhesive strength when heated to high temperatures. However, in the present invention, the acrylic adhesive layer has a reactive double bond, which allows it to maintain or improve its adhesive strength to an adherend, contrary to the properties of conventional acrylic adhesives. Although the mechanism behind this is unclear, it is believed that the reactive double bonds in the acrylic adhesive layer react upon heating, for example, to bond to the adherend, or crosslink between the reactive double bonds, thereby improving the mechanical strength of the adhesive layer. Furthermore, in some cases, the reactive double bonds may also react with unreacted hydrosilyl groups in the organopolysiloxane constituting the polymer matrix, and these combined effects are thought to improve adhesion.

[0014] The acrylic adhesive layer is formed from an acrylic adhesive. The acrylic adhesive preferably contains an acrylic polymer as the adhesive's main component, and the acrylic polymer preferably has the reactive double bond described above. The acrylic adhesive layer can exhibit adhesiveness by containing the acrylic polymer. Furthermore, it is believed that the acrylic polymer having the reactive double bond described above dramatically improves the mechanical strength of the adhesive layer due to crosslinking between the reactive double bonds.

[0015] The acrylic adhesive layer of the present invention preferably has an intensity ratio A / B of 0.2 or more of the peak intensity A of the C=C stretching vibration to the peak intensity B of the C=O stretching vibration in the Raman spectrum. Here, the peak intensity A is a peak generated by a reactive double bond (C=C double bond). Furthermore, the peak intensity B is a peak generated by a C=O bond contained in the acrylic polymer. Therefore, the intensity ratio A / B of the peak intensity A to the peak intensity B can be said to be an index showing the proportion of reactive double bonds in the acrylic polymer.

[0016] The acrylic adhesive layer has a sufficient amount of reactive double bonds when the intensity ratio A / B is 0.2 or more, and can maintain adequate adhesion to the adherend even when heated to high temperatures in a reflow process or the like while in close contact with the adherend.The intensity ratio A / B is more preferably 0.3 or more, even more preferably 0.4 or more, and even more preferably 0.5 or more.In addition, the intensity ratio A / B is not particularly limited, but is, for example, 1.0 or less, preferably 0.8 or less, and more preferably 0.7 or less.The peak of the C=O stretching vibration is typically at a wave number of 1720 cm -1 The peak of the C=C stretching vibration typically appears around the wavenumber 1636 cm -1 However, these peaks may be slightly shifted depending on the structure of the acrylic polymer, etc.

[0017] The acrylic polymer used in the acrylic adhesive layer may contain an acrylic polymer having a reactive double bond (a reactive double bond-containing acrylic polymer). The reactive double bond-containing acrylic polymer preferably has a reactive double bond in a side chain. The reactive double bond is a saturated carbon-carbon double bond that does not constitute an aromatic ring, and is typically H 2 C=CH-* or H 2 C=CCH 3 It is constituted by a group having a structure represented by -* (* represents a bond), and specific examples include a vinyl group, an acryloyl group, a methacryloyl group, etc. Furthermore, the reactive double bond-containing acrylic polymer may have a functional group such as a hydroxyl group, a carboxyl group, an epoxy group, an amino group, etc. in the side chain in addition to the group having the reactive double bond, but it is preferable for it to have at least one of a hydroxyl group and a carboxyl group in the side chain, and it is more preferable for it to have both a hydroxyl group and a carboxyl group.

[0018] The weight-average molecular weight of the reactive double bond-containing acrylic polymer is not particularly limited, but is, for example, about 100,000 to 1,200,000, preferably about 200,000 to 1,000,000.The weight-average molecular weight is measured by gel permeation chromatography (GPC) and calculated as a polystyrene equivalent value.By adjusting the molecular weight, the solid content concentration and viscosity of the adhesive containing the organic solvent described below can be adjusted.Specifically, if you want to adjust the solid content concentration to a high viscosity while adjusting it to a low viscosity, you can reduce the molecular weight.If you want to adjust the solid content concentration to a low viscosity while adjusting it to a high viscosity, you can increase the molecular weight.

[0019] The reactive double bond-containing acrylic polymer can be obtained, for example, by reacting an acrylic polymer having a functional group such as a hydroxyl group, a carboxyl group, an epoxy group, or an amino group in a side chain (hereinafter also referred to as an acrylic polymer (X)) with a reactive double bond-containing compound having a reactive group that reacts with the functional group and a reactive double bond (hereinafter also referred to as a reactive double bond-containing compound (Y)).

[0020] The acrylic polymer (X) may be any polymer containing a structural unit derived from (meth)acrylate, but typically contains a structural unit derived from alkyl(meth)acrylate as the main component. More specifically, the acrylic polymer (X) may be a copolymer of alkyl(meth)acrylate and a functional group-containing monomer, or a copolymer of alkyl(meth)acrylate, a functional group-containing monomer, and a monomer other than these. The term "(meth)acrylate" is used to mean either or both of acrylate and methacrylate, and the same applies to other similar terms.

[0021] Alkyl (meth)acrylates are esters of (meth)acrylic acid and alkyl alcohols. The alkyl group in the alkyl (meth)acrylate may be linear, branched, or cyclic. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. One type of alkyl (meth)acrylate may be used alone, or two or more types may be used in combination. The alkyl (meth)acrylate is preferably an alkyl (meth)acrylate in which the alkyl group has 1 to 12 carbon atoms, and more preferably includes an alkyl acrylate in which the alkyl group has 2 to 8 carbon atoms. The structural unit derived from the alkyl acrylate in which the alkyl group has 2 to 8 carbon atoms may be the main component in the acrylic polymer (X), and may account for, for example, 50% by mass or more, preferably 60% by mass or more and 95% by mass or less, and more preferably 70% by mass or more and 90% by mass or less.

[0022] As described above, examples of the functional group in the functional group-containing monomer include a carboxyl group, a hydroxyl group, an amino group, and an epoxy group. Of these, a carboxyl group and a hydroxyl group are preferred. Examples of monomers containing a carboxyl group include (meth)acrylic acid and crotonic acid. Of these, (meth)acrylic acid is more preferred. Examples of monomers containing a hydroxyl group include (meth)acrylates having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, and allyl alcohol. Of these, a (meth)acrylate having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, is preferred. The content of the structural units derived from the functional group-containing monomer in the acrylic polymer (X) is, for example, about 1% by mass to 35% by mass, preferably 5% by mass to 30% by mass, and more preferably 10% by mass to 25% by mass. The functional group-containing monomers may be used alone or in combination of two or more.

[0023] Examples of other monomers include alkyl (meth)acrylates and monomers other than the functional group-containing monomers described above, and are not particularly limited as long as they are copolymerizable with the alkyl (meth)acrylates and functional group-containing monomers. Specific examples include styrene derivatives such as styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and divinylbenzene; compounds having a vinyl ester group such as vinyl acetate and vinyl propionate; N-vinylpyrrolidone, N-vinylmorpholine, (meth)acrylonitrile, N-cyclohexylmaleimide, N-phenylmaleimide, N-laurylmaleimide, N-benzylmaleimide, n-propyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, and tert-butyl vinyl ether. One type of other monomer may be used alone, or two or more types may be used in combination.

[0024] The reactive double bond-containing compound (Y) is a compound having a reactive group that reacts with the above-mentioned functional group and a reactive double bond. Examples of the reactive group include an isocyanate group, an epoxy group, a carboxyl group, and a hydroxyl group. Among these, an isocyanate group and an epoxy group are preferred, and an isocyanate group is more preferred. The content of the reactive double bond contained in the acrylic adhesive layer can be adjusted by the amount of functional groups contained in the acrylic polymer (X) and the ratio of the functional groups that react with the reactive double bond-containing compound (Y). The amount of functional groups contained in the acrylic polymer (X) can be adjusted by the ratio of functional group-containing monomers used in synthesizing the acrylic polymer (X).

[0025] The acrylic polymer contained in the acrylic adhesive layer may be an acrylic polymer containing a reactive double bond, or may contain an acrylic polymer without a reactive double bond in addition to the acrylic polymer containing a reactive double bond. Examples of the acrylic polymer without a reactive double bond include the acrylic polymer (X) described above. In addition to the acrylic polymer described above, the acrylic adhesive may contain components generally blended in adhesives, and may appropriately contain additives such as a crosslinker, a tackifier, a filler, an antioxidant, an ultraviolet protection agent, a plasticizer, and a viscosity adjuster.

[0026] The acrylic adhesive layer may be provided on one surface of the thermally conductive layer or on both surfaces of the thermally conductive layer. Here, "one surface" or "both surfaces" refers to the surface perpendicular to the thickness direction of the thermally conductive layer, also known as the "main surface." By providing the acrylic adhesive layer on both surfaces of the thermally conductive layer, the adhesion of both surfaces of the thermally conductive sheet to the substrate can be improved. Therefore, when the thermally conductive sheet is used in semiconductor applications, it can adhere to both the semiconductor chip and the heat spreader with relatively high adhesive strength. Furthermore, even when the thermally conductive sheet is heated at high temperatures through a reflow process or the like while in close contact with these, peeling of the thermally conductive sheet from both the semiconductor chip and the heat spreader is easily prevented.

[0027] The weight per unit area of ​​the acrylic adhesive layer on each surface is, for example, 0.05 mg / cm 2 or more, preferably 0.1 mg / cm 2 More preferably, 0.2 mg / cm 2 More preferably, 0.3 mg / cm 2 or more, and for example, 1.0 mg / cm 2 or less, preferably 0.75 mg / cm 2 or less, more preferably 0.5 mg / cm 2 More preferably, 0.45 mg / cm 2 The acrylic adhesive layer can ensure sufficient adhesive strength to the adherend by setting the basis weight to a certain amount or more. Furthermore, by setting the basis weight to a certain amount or less, it is possible to prevent the acrylic adhesive layer from lowering the thermal resistance value, making it easier to ensure good thermal conductivity.

[0028] The acrylic adhesive layer preferably permeates into the thermally conductive layer. Typically, a portion of the acrylic adhesive layer permeates into the thermally conductive layer. However, the entire acrylic adhesive layer may permeate into the thermally conductive layer as long as the acrylic adhesive layer can exert adhesive strength to the adherend. By permeating the thermally conductive layer, the amount of adhesive present on the surface of the thermally conductive layer can be reduced, thereby preventing a decrease in thermal conductivity due to the acrylic adhesive layer. Furthermore, the thermally conductive sheet can ensure high adhesion even if the adhesive permeates into the thermally conductive layer. While the mechanism behind this is unclear, it is presumed that the permeated adhesive seeps out to the surface due to the pressure applied during use, thereby enhancing adhesion.

[0029] As described below, the acrylic adhesive layer can be impregnated into bubbles formed by the evaporation of the volatile substance, allowing an appropriate amount of the acrylic adhesive layer to penetrate into the thermally conductive layer. The acrylic adhesive layer may be formed to cover the entire surface of the thermally conductive layer, or may be formed to cover only a portion of the surface as long as it can exert adhesive force on the adherend. The bubbles described above are spaces partitioned by the polymer matrix or thermally conductive filler in the thermally conductive layer, and are continuous spaces that serve as evaporation paths for the volatile substance. This continuity allows the adhesive to penetrate into the thermally conductive layer.

[0030] [Thermal Conductive Layer] The thermal conductive layer of the present invention comprises a polymer matrix and a thermally conductive filler. The polymer matrix is ​​a matrix made of an organic polymer, such as an elastomer or rubber, and is preferably formed by curing a liquid polymer composition (curable polymer composition) consisting of a mixture of a base resin and a curing agent. The curable polymer composition may be, for example, a composition made of uncrosslinked rubber and a crosslinking agent, or a composition containing a monomer, prepolymer, or the like and a curing agent. The curing reaction may be room temperature curing or heat curing.

[0031] The polymer matrix is ​​preferably an organopolysiloxane. In the present invention, the use of an organopolysiloxane makes the polymer matrix flexible after curing, improving the filling ability of the thermally conductive filler. The organopolysiloxane is preferably silicone rubber. Furthermore, the organopolysiloxane is preferably a curable silicone, and more preferably an addition reaction silicone. In the case of an addition reaction silicone, the curable polymer composition is composed of an alkenyl group-containing organopolysiloxane (base) and a hydrogen organopolysiloxane (curing agent), and the polymer matrix may be formed by curing these components. When an addition reaction silicone is used, the reactive double bonds contained in the acrylic adhesive layer react with unreacted hydrosilyl groups upon high-temperature heating, such as during a reflow process, which is thought to improve adhesion to the adherend. In particular, since organopolysiloxane is also used as a release layer, it has traditionally been common knowledge that acrylic adhesives do not adhere to silicones. However, it was unexpected that the acrylic adhesive layer contains reactive double bonds as described above, and that adhesion is enhanced by undergoing a predetermined heating step.

[0032] In addition to silicone rubber, various synthetic rubbers can be used as rubber. Specific examples include acrylic rubber, nitrile rubber, isoprene rubber, urethane rubber, ethylene propylene rubber, styrene-butadiene rubber, butadiene rubber, fluororubber, and butyl rubber. When using these rubbers, the synthetic rubbers may be crosslinked or left uncrosslinked (i.e., uncured) in the thermally conductive sheet. Uncrosslinked rubbers are primarily used in flow orientation. Furthermore, when crosslinked (i.e., cured), as described above, the polymer matrix may be formed by curing a curable polymer composition comprising an uncrosslinked synthetic rubber and a crosslinking agent. Furthermore, thermoplastic elastomers such as polyester-based thermoplastic elastomers and polyurethane-based thermoplastic elastomers, as well as thermosetting elastomers formed by curing a liquid polymer composition containing a base resin and a curing agent, can also be used. For example, a polyurethane-based elastomer formed by curing a polymer composition containing a hydroxyl-containing polymer and an isocyanate can be used.

[0033] Furthermore, the polymer composition for forming the polymer matrix may consist of an organic polymer alone, or may consist of an organic polymer and a plasticizer. Plasticizers are preferably used when synthetic rubber is used, and the inclusion of a plasticizer can increase the flexibility of the polymer matrix when uncrosslinked. For example, when the polymer matrix is ​​an organopolysiloxane, silicone oil is preferably used as the plasticizer. That is, the curable polymer composition may consist of a base agent and a curing agent, or may consist of a base agent, a curing agent, and a plasticizer. The content of the polymer matrix, expressed as a volume-based filling rate (volume filling rate), is preferably 15% by volume or more and 50% by volume or less, more preferably 17% by volume or more and 45% by volume or less, and even more preferably 20% by volume or more and 40% by volume or less, based on the total amount of the thermal conductive sheet.

[0034] (Thermal Conductive Filler) The thermal conductive filler contained in the thermal conductive layer is preferably dispersed in a polymer matrix and held in the polymer matrix. Examples of the thermal conductive filler include anisotropic fillers and non-anisotropic fillers, but it is preferable to use at least anisotropic fillers.

[0035] The anisotropic filler is preferably oriented in the thickness direction of the thermally conductive sheet. This makes it easier for the thermally conductive layer to increase its thermal conductivity. When the anisotropic filler is oriented in the thickness direction, its long axis direction does not need to be strictly parallel to the thickness direction; even if the long axis direction is slightly tilted relative to the thickness direction, it is still considered to be oriented in the thickness direction. Specifically, anisotropic fillers whose long axis direction is tilted by less than 20° are also considered to be oriented in the thickness direction, and if such anisotropic fillers constitute the majority of the thermally conductive sheet (for example, more than 60%, preferably more than 80% of the total number of anisotropic fillers), they are considered to be oriented in the thickness direction.

[0036] The content of the thermally conductive filler is preferably 150 parts by mass or more and 3,000 parts by mass or less, more preferably 200 parts by mass or more and 1,800 parts by mass or less, and even more preferably 300 parts by mass or more and 1,000 parts by mass or less, per 100 parts by mass of the polymer matrix. By setting the content of the thermally conductive filler to 150 parts by mass or more, a certain level of thermal conductivity can be imparted to the thermally conductive layer. Furthermore, by setting the content to 3,000 parts by mass or less, the thermally conductive filler can be properly dispersed in the polymer matrix. Furthermore, it is possible to prevent the viscosity of the mixed composition described below from becoming unnecessarily high. Furthermore, the volume filling rate of the thermally conductive filler relative to the total amount of the thermally conductive layer is preferably 30% by volume or more and 85% by volume or less, more preferably 50% by volume or more and 83% by volume or less, and even more preferably 60% by volume or more and 80% by volume or less. By setting the volume filling rate at or above the lower limit, a certain level of thermal conductivity can be imparted to the thermally conductive layer. Furthermore, by setting the content to or below the upper limit, the thermally conductive layer can be easily manufactured.

[0037] (Anisotropic Filler) An anisotropic filler is a filler that has an anisotropic shape and can be oriented. Examples of anisotropic fillers include fibrous materials and scaly materials. An anisotropic filler has a high aspect ratio, specifically, an aspect ratio of greater than 2, preferably 5 or greater. By increasing the aspect ratio to greater than 2, the anisotropic filler is more easily oriented in one direction, such as the thickness direction, and the thermal conductivity of the thermally conductive layer in one direction, such as the thickness direction, is easily increased. The upper limit of the aspect ratio is not particularly limited, but is practically 100. The aspect ratio is the ratio of the major axis length to the minor axis length of the anisotropic filler. In the case of fibrous materials, it means the fiber length / fiber diameter, and in the case of scaly materials, it means the major axis length / thickness of the scaly material.

[0038] The content of the anisotropic filler in the thermally conductive layer is preferably 10 parts by mass or more and 500 parts by mass or less, more preferably 30 parts by mass or more and 300 parts by mass or less, and even more preferably 50 parts by mass or more and 250 parts by mass or less, relative to 100 parts by mass of the polymer matrix. By setting the content of the anisotropic filler to 10 parts by mass or more, thermal conductivity is easily improved. Furthermore, by setting the content to 500 parts by mass or less, the viscosity of the mixed composition described below is easily adjusted, resulting in good orientation of the anisotropic filler. Furthermore, the dispersibility of the anisotropic filler in the polymer matrix is ​​also improved.

[0039] When the anisotropic filler is a fibrous material, its average fiber length is preferably 10 μm or more and 300 μm or less, more preferably 20 μm or more and 200 μm or less, and even more preferably 30 μm or more and 100 μm or less. When the average fiber length is 10 μm or more, the anisotropic fillers are in proper contact with each other within the thermally conductive layer, ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive layer. On the other hand, when the average fiber length is 500 μm or less, the bulk of the anisotropic filler is reduced, allowing it to be highly loaded into the binder component. Furthermore, the average fiber length of the fibrous material is preferably shorter than the thickness of the thermally conductive sheet. Being shorter than the thickness prevents the fibrous material from protruding more than necessary from the surface of the thermally conductive sheet. The above average fiber length can be calculated by observing the anisotropic filler under a microscope. More specifically, the fiber lengths of 50 arbitrary anisotropic fillers can be measured using, for example, an electron microscope or an optical microscope, and the average value (arithmetic mean value) can be used as the average fiber length.

[0040] Furthermore, when the anisotropic filler is a scaly material, its average particle size is preferably 10 μm or more and 300 μm or less, more preferably 15 μm or more and 200 μm or less, and even more preferably 20 μm or more and 100 μm or less. By setting the average particle size to 10 μm or more, the anisotropic fillers in the thermally conductive layer are more likely to come into contact with each other, ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive layer. On the other hand, setting the average particle size to 400 μm or less reduces the bulk of the thermally conductive sheet, allowing the anisotropic filler to be highly loaded into the binder component. The average particle size of the scaly filler is D50, which can be calculated by observing the scaly filler under a microscope and using the long diameter as the diameter. More specifically, for example, using an electron microscope or optical microscope, the long diameter of 500 or more random scaly fillers is measured, and the particle size corresponds to a cumulative frequency of 50%. Specifically, using a scaly filler as a sample, the particle size distribution curve can be determined by plotting the particle size on the horizontal axis and the cumulative frequency on the vertical axis. The particle size distribution curve is a numerical particle size distribution curve obtained by integrating the particle sizes of the scaly filler starting from the smallest particle size.

[0041] The anisotropic filler may be any known material having thermal conductivity. However, when oriented by magnetic field orientation as described below, it is preferable for the filler to have diamagnetic properties. On the other hand, when oriented by flow orientation or when the anisotropic filler is not oriented, it does not need to have diamagnetic properties. Specific examples of anisotropic fillers include carbon-based materials such as carbon fiber or flake carbon powder, metal materials such as metal fiber and metal oxides, boron nitride, metal nitrides, metal carbides, metal hydroxides, and polyparaphenylene benzoxazole fibers. Among these, carbon-based materials are preferred due to their low specific gravity and good dispersibility in binder components, and graphitized carbon materials with high thermal conductivity are more preferred. Graphitized carbon materials have diamagnetic properties due to the alignment of graphite planes in a specific direction. Boron nitride is also a preferred anisotropic filler. While not particularly limited, boron nitride is preferably used as a flake material. The flake-like boron nitride may be agglomerated or not, but it is preferable that it is not agglomerated in part or in whole. Note that boron nitride also has diamagnetic properties when its crystal planes are aligned in a specific direction.

[0042] Furthermore, the anisotropic filler is not particularly limited, but its thermal conductivity along the anisotropic direction (i.e., the long axis direction) is generally 30 W / m K or more, preferably 60 W / m K or more, more preferably 100 W / m K or more, and even more preferably 200 W / m K or more. The upper limit of the thermal conductivity of the anisotropic filler is not particularly limited, but is, for example, 2000 W / m K or less. The thermal conductivity can be measured by a laser flash method or the like.

[0043] The anisotropic filler may be used alone or in combination of two or more. For example, the anisotropic filler may be an anisotropic filler having at least two different average particle sizes or average fiber lengths. When anisotropic fillers of different sizes are used, the smaller anisotropic fillers are embedded between the relatively larger anisotropic fillers, which is thought to enable the anisotropic fillers to be densely packed in the binder component and to improve heat conduction efficiency.

[0044] Furthermore, among the above, the anisotropic filler preferably contains a fibrous material. As described below, when a thermally conductive layer containing a fibrous material is sliced, the fibrous material falls off, creating unevenness on the surface and reducing adhesion. However, in the present invention, the acrylic adhesive layer penetrates into the recesses, thereby sufficiently improving adhesion even with a thermally conductive layer containing a fibrous material. Furthermore, from the viewpoint of improving thermal conductivity, the thermally conductive layer preferably contains a scaly material in addition to the fibrous material as an anisotropic filler. In this case, the content ratio of the scaly material to the fibrous material (scaly material / fibrous material) is, for example, 0.01 to 1, preferably 0.02 to 0.5, and more preferably 0.1 to 0.3, by mass.

[0045] The carbon fiber used as the anisotropic filler is preferably graphitized carbon fiber. Furthermore, the scaly carbon powder is preferably scaly graphite powder. It is also preferable to use a combination of graphitized carbon fiber and scaly graphite powder as the anisotropic filler. Graphitized carbon fiber has graphite crystal planes aligned in the fiber axis direction, providing high thermal conductivity in the fiber axis direction. Therefore, by aligning the fiber axis direction in a predetermined direction, thermal conductivity in a specific direction can be increased. Furthermore, scaly graphite powder has graphite crystal planes aligned in the in-plane direction of the scaly surfaces, providing high thermal conductivity in the in-plane direction. Therefore, by aligning the scaly surfaces in a predetermined direction, thermal conductivity in a specific direction can be increased. The graphitized carbon fiber and scaly graphite powder preferably have a high degree of graphitization.

[0046] The graphitized carbon materials, such as the graphitized carbon fiber and flake graphite powder, can be obtained by graphitizing the following raw materials. Examples include condensed polycyclic hydrocarbon compounds such as naphthalene, condensed heterocyclic compounds such as PAN (polyacrylonitrile), and pitch. However, it is particularly preferable to use graphitized mesophase pitch, polyimide, or polybenzazole, which have a high degree of graphitization. For example, by using mesophase pitch, the pitch is anisotropically oriented in the fiber axis direction during the spinning process described below, thereby producing graphitized carbon fibers with excellent thermal conductivity in the fiber axis direction. The use of mesophase pitch in graphitized carbon fibers is not particularly limited as long as it can be spun. Mesophase pitch may be used alone or in combination with other raw materials. However, using mesophase pitch alone, i.e., graphitized carbon fibers with a 100% mesophase pitch content, is most preferable in terms of high thermal conductivity, spinnability, and quality stability.

[0047] The graphitized carbon fiber can be one that has been subjected to spinning, infusibilization, and carbonization in sequence, and then pulverized or cut to a predetermined particle size before graphitization, or one that has been carbonized, pulverized, or cut and then graphitized. When pulverization or cutting is performed before graphitization, condensation polymerization reactions and cyclization reactions are more likely to proceed on the newly exposed surface during the graphitization treatment, thereby increasing the degree of graphitization and enabling the production of graphitized carbon fibers with even improved thermal conductivity. On the other hand, when spun carbon fiber is pulverized after graphitization, the graphitized carbon fiber is stiff and therefore easy to pulverize, and carbon fiber powder with a relatively narrow fiber length distribution can be obtained by pulverization for a short period of time.

[0048] As described above, the average fiber length of the graphitized carbon fiber is preferably 10 μm or more and 300 μm or less, more preferably 20 μm or more and 200 μm or less, and even more preferably 30 μm or more and 100 μm or less. Furthermore, as described above, the aspect ratio of the graphitized carbon fiber is greater than 2, preferably 5 or more. The thermal conductivity of the graphitized carbon fiber is not particularly limited, but the thermal conductivity in the fiber axis direction is preferably 400 W / m·K or more, more preferably 800 W / m·K or more.

[0049] When the thermally conductive layer contains an anisotropic filler, it may or may not be exposed on the surface of the thermally conductive layer, but it is preferable that it be exposed. When the anisotropic filler is exposed, the anisotropic filler comes into contact with an adherend such as a heat generating body or a heat dissipating body, which makes it easier to reduce the thermal resistance value. Furthermore, when the anisotropic filler is exposed, it is difficult to improve adhesion to the adherend. However, in such cases, in the present invention, the provision of an acrylic adhesive layer makes it easier to improve adhesion.

[0050] (Non-anisotropic filler) The thermally conductive filler of the present invention may contain a non-anisotropic filler, and it is preferable to use the above-mentioned anisotropic filler in combination with a non-anisotropic filler. When the non-anisotropic filler is used in combination with an anisotropic filler oriented in one direction, such as the thickness direction, the non-anisotropic filler is interposed in the gaps between the oriented anisotropic fillers, thereby further increasing thermal conductivity. The non-anisotropic filler is a filler that has substantially no anisotropy in shape, and is a filler that does not orient in a predetermined direction even under environments in which the anisotropic filler orients in a predetermined direction, such as under the generation of magnetic field lines or under the action of shear force, as described below.

[0051] The aspect ratio of the non-anisotropic filler is 2 or less, and preferably 1.5 or less. When used in combination with an anisotropic filler, a non-anisotropic filler with such a low aspect ratio is more likely to be arranged in the gaps between the anisotropic filler, making it easier to improve thermal conductivity. Furthermore, by setting the aspect ratio to 2 or less, an increase in the viscosity of the mixed composition described below can be prevented, enabling high filling.

[0052] Specific examples of non-anisotropic fillers include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, and oxides, nitrides, and carbides other than metals. The shapes of the non-anisotropic fillers include spherical, polyhedral, and irregularly shaped powders. Examples of metals in non-anisotropic fillers include aluminum, copper, and nickel. Examples of metal oxides include aluminum oxide (e.g., alumina), magnesium oxide, and zinc oxide. Examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Examples of carbon materials include spherical graphite. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, aluminum oxide and aluminum are preferred because of their high thermal conductivity and the ease of obtaining spherical fillers. The non-anisotropic fillers may be used alone or in combination of two or more of the above.

[0053] The average particle size of the non-anisotropic filler is, for example, 0.1 μm or more and 200 μm or less, preferably 0.5 μm or more and 100 μm or less, and more preferably 1 μm or more and 70 μm or less. Furthermore, when the non-anisotropic filler is used in combination with an anisotropic filler, the average particle size of the non-anisotropic filler is preferably 0.1 μm or more and 50 μm or less, more preferably 0.5 μm or more and 35 μm or less, and even more preferably 1 μm or more and 15 μm or less. By setting the average particle size to 50 μm or less, problems such as disturbance of the orientation of the anisotropic filler are less likely to occur even when used in combination with an anisotropic filler. Furthermore, by setting the average particle size to 0.1 μm or more, the specific surface area of ​​the non-anisotropic filler does not become larger than necessary, and even when a large amount is blended, the viscosity of the mixed composition is less likely to increase, making it easier to highly fill the non-anisotropic filler. The non-anisotropic filler may be, for example, a non-anisotropic filler having at least two different average particle sizes. The average particle size of the non-anisotropic filler can be measured by observation with an electron microscope or the like. More specifically, the particle sizes of 500 or more particles of any non-anisotropic filler can be measured using, for example, an electron microscope or an optical microscope, and the D50 can be calculated in the same manner as for the scaly filler.

[0054] The content of the non-anisotropic filler is preferably 50 parts by mass or more and 2500 parts by mass or less, more preferably 100 parts by mass or more and 1500 parts by mass or less, and even more preferably 200 parts by mass or more and 750 parts by mass or less, relative to 100 parts by mass of the polymer matrix. By setting the content at 50 parts by mass or more, the thermal conductivity of the thermal conductive sheet can be improved. On the other hand, by setting the content at 1500 parts by mass or less, the non-anisotropic filler can be properly dispersed in the binder component, thereby achieving the effect of increasing the thermal conductivity according to the content. In addition, an unnecessary increase in the viscosity of the mixed composition can be prevented.

[0055] The mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler is not particularly limited, but is preferably from 0.5 to 15, more preferably from 1 to 10, and more preferably from 1.1 to 7. By setting the mass ratio within the above range, the non-anisotropic filler is appropriately filled between the anisotropic fillers, forming efficient heat transfer paths, thereby further improving the thermal conductivity of the thermally conductive sheet.

[0056] In the thermally conductive layer, the polymer matrix may further contain components other than those described above, provided that the functionality of the thermally conductive layer is not impaired. Specific examples include at least one selected from dispersants, flame retardants, antioxidants, colorants, anti-settling agents, etc. Furthermore, when the curable polymer composition is to be crosslinked or cured as described above, additives such as crosslinking accelerators, curing accelerators, and curing catalysts that accelerate crosslinking and curing may be added. When the polymer matrix is ​​an organopolysiloxane, a platinum catalyst may be used as the curing catalyst.

[0057] The surface of the thermally conductive layer is preferably a sliced ​​surface. By having the surface of the thermally conductive layer as a sliced ​​surface, the anisotropic filler and the like can be easily exposed to the surface of the thermally conductive layer, as described above, and the thermal resistance value can be effectively reduced. The thermally conductive sheet may have one or both surfaces as sliced ​​surfaces, but it is preferable that the surface on which the acrylic adhesive layer is provided be a sliced ​​surface. As will be described later, a sliced ​​surface is a surface formed by cutting with a shearing blade, laser, or the like. Sliced ​​surfaces often have large irregularities due to the protrusion or detachment of the anisotropic filler. However, by filling the recesses with an acrylic adhesive layer, the air gap can be reduced during use, improving the thermal resistance value while also increasing adhesion.

[0058] It is also preferable that the thermally conductive sheet has a polished surface. By having at least one surface of the thermally conductive sheet be a polished surface, the thermal resistance value can be more effectively reduced. The thermally conductive sheet may have one surface or both surfaces polished, but it is preferable that the surface on which the acrylic adhesive layer is provided is a polished surface, and it is particularly preferable that the surface on which the acrylic adhesive layer is provided is a sliced ​​surface and a polished surface. The polished surface has relatively high smoothness, and therefore, when the acrylic adhesive layer is provided, it is easy to increase adhesion to the adherend.

[0059] The thickness of the thermally conductive layer is not particularly limited, but is, for example, approximately 1200 μm or less. However, from the viewpoint of suitable use in semiconductor applications and from the viewpoint of preventing an increase in thermal resistance, it is preferable to make it relatively thin, preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less. The thickness of the thermally conductive layer is also not particularly limited, but in practical terms, it is, for example, 10 μm or more, preferably 20 μm or more, more preferably 70 μm or more. The thickness of the thermally conductive layer is the initial thickness measured without applying a load in the thickness direction.

[0060] (Arithmetic mean height (Sa)) The arithmetic mean height (Sa) of the surface of the thermally conductive sheet on which the acrylic adhesive layer is provided is, for example, 20 μm or less, preferably 12 μm or less, more preferably 6 μm or less, and even more preferably 5 μm or less. By reducing the arithmetic mean height of the surface on which the acrylic adhesive layer is provided, the thermal resistance value of the thermally conductive sheet can be more effectively reduced. Furthermore, the acrylic adhesive layer enables the thermally conductive sheet to be more effectively adhered to the adherend. Note that, for example, when the surface of the thermally conductive sheet is sliced ​​as described above, the arithmetic mean height tends to be relatively large. However, by polishing after slicing, the arithmetic mean height (Sa) can be reduced as described above. The arithmetic mean height (Sa) of the surface on which the acrylic adhesive layer of the thermally conductive sheet is provided is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more. By setting the arithmetic mean height (Sa) at or above these lower limits, it can be relatively easily obtained by polishing even the sliced ​​surface.

[0061] (E Hardness) The thermally conductive layer of the present invention preferably has a Type E hardness (hereinafter also referred to as "E hardness") defined in JIS K6253 of 10 or more and 80 or less, more preferably 20 or more and 70 or less, and even more preferably 30 or more and 65 or less. When the E hardness is equal to or more than the above lower limit, the mechanical strength of the thermally conductive sheet is easily increased. On the other hand, when the E hardness is equal to or less than the above upper limit, a certain degree of flexibility is imparted to the thermally conductive sheet, and adhesion to the adherend is also easily improved.

[0062] (Thermal Resistance of Thermally Conductive Sheet) The thermally conductive sheet of the present invention has a thermal resistance of, for example, 0.5°C cm 2 / W or less, but 0.25°C cm 2 / W or less, and 0.2°C cm 2 / W or less, and more preferably 0.16°C cm 2 When the thermal resistance is equal to or less than the upper limit, the efficiency of heat transfer from the heat generating body to the heat dissipating body via the thermal conductive sheet is improved, and excellent thermal conductivity can be obtained. In the present invention, the lower the thermal resistance is, the better.2 / W or more, but in practice, for example, 0.01°C cm 2 / W or more, preferably 0.05°C cm 2 The thermal resistance value is a thermal resistance value measured when a pressure of 20 psi (138 kPa) is applied in the thickness direction, and specifically, can be obtained by the measurement method described in the examples.

[0063] [Method for manufacturing thermally conductive sheet] The thermally conductive sheet of the present invention can be manufactured by a method comprising at least the following steps 1 to 3. However, the thermally conductive sheet of the present invention may also be manufactured by a method other than the following manufacturing method. Step 1: A step of mixing at least a curable polymer composition and a thermally conductive filler to obtain a mixed composition. Step 2: A step of curing the mixed composition by heating to obtain a cured product. Step 3: A step of applying an adhesive to the surface of the cured product. In addition, the present invention preferably comprises the following step 4. Step 4: A step of allowing the applied adhesive to soak into the cured product.

[0064] (Step 1) In step 1, a mixed composition is obtained by mixing at least a curable polymer composition and a thermally conductive filler, and it is preferable to further mix a volatile substance into the mixed composition. In addition, other components such as additives may be appropriately added to the mixed composition as needed.

[0065] In step 1, the mixing method and order of the above components are not particularly limited as long as they can be mixed to obtain a mixed composition. The curable polymer composition, the thermally conductive filler, the volatile substance added as needed, and other components added as needed can be mixed in any order to obtain the mixed composition. As described above, the curable polymer composition may be composed of, for example, a base agent and a curing agent (e.g., an alkenyl group-containing organopolysiloxane and a hydrogen organopolysiloxane in the case of an addition reaction type silicone). In such cases, the base agent, the curing agent, the thermally conductive filler, the volatile substance added as needed, and other components added as needed can be mixed in any order to obtain the mixed composition. The mixed composition may be in the form of a one-component type or a two-component type consisting of a first component and a second component. A two-component type is a type in which the first component and the second component are mixed together to obtain the mixed composition at the time of use.

[0066] (Volatile Substance) The volatile substance used in the present invention may be any component that volatilizes in step 2, which will be described later. The volatile substance volatilizes when heated during curing, thereby increasing the content of the thermally conductive filler in the thermally conductive sheet. Furthermore, the viscosity of the mixed composition decreases when the volatile substance is contained. This makes it easier to increase the amount of thermally conductive filler incorporated, and furthermore, makes it easier to orient the anisotropic filler in a predetermined direction by magnetic field orientation, which will be described later. Furthermore, the volatilization of the volatile substance forms a large number of fine bubbles in the cured product, which makes it easier for the adhesive to penetrate into the thermally conductive layer in step 4, which will be described later.

[0067] Furthermore, the volatile substance is preferably a compatible substance that is compatible or soluble in the curable polymer composition. If the volatile substance is a compatible substance, the curable polymer composition and the volatile substance can be mixed uniformly, making it easier to reduce viscosity and increase the amount of thermally conductive filler added. Furthermore, the bubbles formed by the evaporation of the volatile substance can be made fine and uniform.

[0068] The volatile substance is preferably a substance that is liquid at room temperature (25°C) and 1 atmosphere. Examples of the volatile substance include alkoxysilane compounds, hydrocarbon solvents, and alkoxysiloxane compounds. These compounds can increase the solubility or compatibility with the curable polymer composition, making it easier to reduce the viscosity of the mixed composition and increase the amount of thermally conductive filler added. Furthermore, the evaporation of the volatile substance makes it easier to form fine and uniform bubbles. The volatile substance may be used alone or in combination of two or more.

[0069] An alkoxysilane compound is preferably used as the volatile substance. The use of an alkoxysilane compound results in a cured thermally conductive sheet with a good appearance and no surface roughness. The alkoxysilane compound used as the volatile substance is a compound having a structure in which one to three of the four bonds possessed by a silicon atom (Si) are bonded to alkoxy groups, and the remaining bond is bonded to an organic substituent. The alkoxysilane compound possesses an alkoxy group and an organic substituent, thereby enhancing compatibility with curable polymer compositions, particularly curable polymer compositions composed of organopolysiloxanes. Examples of alkoxy groups possessed by alkoxysilane compounds include methoxy, ethoxy, protoxy, butoxy, pentoxy, and hexatoxy groups. The alkoxysilane compound may be contained in the curable polymer composition as a dimer.

[0070] Among alkoxysilane compounds, from the viewpoint of easy availability, alkoxysilane compounds having at least one of a methoxy group and an ethoxy group are preferred. From the viewpoint of compatibility with the curable polymer composition, solubility, etc., the number of alkoxy groups in the alkoxysilane compound is preferably 2 or 3, more preferably 3. Specifically, the alkoxysilane compound is preferably at least one selected from a trimethoxysilane compound, a triethoxysilane compound, a dimethoxysilane compound, and a diethoxysilane compound.

[0071] Examples of functional groups contained in the organic substituents of alkoxysilane compounds include acryloyl groups, alkyl groups, carboxyl groups, vinyl groups, methacrylic groups, aromatic groups, amino groups, isocyanate groups, isocyanurate groups, epoxy groups, hydroxyl groups, and mercapto groups. When a platinum catalyst is used as a curing catalyst for a curable polymer composition composed of an organopolysiloxane, it is preferable to select and use an alkoxysilane compound that is less likely to affect the curing reaction of the organopolysiloxane. Specifically, when an addition reaction-type organopolysiloxane using a platinum catalyst is used, it is preferable that the organic substituents of the alkoxysilane compound do not contain amino groups, isocyanate groups, isocyanurate groups, hydroxyl groups, or mercapto groups.

[0072] From the viewpoint of compatibility with the curable polymer composition composed of organopolysiloxane, the alkoxysilane compound preferably includes an alkylalkoxysilane compound having an alkyl group bonded to a silicon atom, i.e., an alkoxysilane compound having an alkyl group as an organic substituent. Therefore, dialkyldialkoxysilane compounds and alkyltrialkoxysilane compounds are preferred, with alkyltrialkoxysilane compounds being particularly preferred. The number of carbon atoms in the alkyl group bonded to the silicon atom may be, for example, 1 to 16. Furthermore, in trialkoxysilane compounds such as trimethoxysilane compounds and triethoxysilane compounds, the number of carbon atoms in the alkyl group is preferably 6 or more, more preferably 8 or more, and preferably 12 or less, more preferably 10 or less. Meanwhile, in dialkoxysilane compounds such as dimethoxysilane compounds and triethoxysilane compounds, the number of carbon atoms in the alkyl group may be 1 or more, and preferably 10 or less, more preferably 6 or less, and even more preferably 4 or less.

[0073] Examples of alkyl group-containing alkoxysilane compounds include methyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, di-n-propyldimethoxysilane, di-n-propyldiethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, and n-decyltriethoxysilane. Among the alkyl group-containing alkoxysilane compounds, n-decyltrimethoxysilane and n-octyltriethoxysilane are even more preferred from the viewpoint of compatibility with the organopolysiloxane that constitutes the curable polymer composition.

[0074] The alkoxysiloxane compound used as the volatile substance has two or more siloxane bonds and a structure in which an alkoxy group is bonded to at least one silicon atom. The alkoxysiloxane compound has a structure in which an organic substituent is bonded to at least one of the silicon atoms constituting the siloxane bond. The alkoxysiloxane compound can improve compatibility with the organopolysiloxane constituting the curable polymer composition by having an alkoxy group and an organic substituent. Examples of the alkoxy group and organic substituent possessed by the alkoxysiloxane compound include those exemplified in the description of the alkoxysilane compound above. From the viewpoint of compatibility with the organopolysiloxane constituting the curable polymer composition, it is preferable that the alkoxysiloxane compound has at least an alkyl group.

[0075] Examples of the alkoxysiloxane compound include methyl methoxy siloxane oligomer, methyl phenyl methoxy siloxane oligomer, methyl epoxy methoxy siloxane oligomer, methyl mercapto methoxy siloxane oligomer, and methyl acryloyl methoxy siloxane oligomer, etc. One or more types of alkoxy siloxane compounds can be used.

[0076] Examples of hydrocarbon solvents used as volatile substances include aromatic hydrocarbon solvents. Among these, aromatic hydrocarbon solvents are preferred from the viewpoint of compatibility with the curable polymer composition. Examples of aromatic hydrocarbon solvents include aromatic hydrocarbon solvents having about 6 to 10 carbon atoms, such as toluene, xylene, mesitylene, ethylbenzene, propylbenzene, butylbenzene, and t-butylbenzene, with toluene and xylene being preferred.

[0077] In the mixed composition, the content of the volatile substance per 100 parts by mass of the curable polymer composition is preferably 6 parts by mass or more and 60 parts by mass or less. When the content is 6 parts by mass or more, the effect of the volatile substance is easily exerted, for example, an appropriate amount of fine bubbles can be formed in the polymer matrix. Furthermore, when the content is 60 parts by mass or less, an effect commensurate with the amount of volatile substance used can be obtained. From these viewpoints, the content of the volatile substance is more preferably 8 parts by mass or more and 50 parts by mass or less, and even more preferably 10 parts by mass or more and 35 parts by mass or less. It is preferable that the volatile substance is partially or completely volatilized by heating in step 2. Therefore, the volatile substance does not need to be contained in the thermally conductive sheet, but may be contained in the thermally conductive sheet in an amount less than the content in the mixed composition.

[0078] The detailed description of the components other than the volatile substance in the mixed composition (i.e., the curable polymer composition, the thermally conductive filler, other additives, etc.) is as described above. The content of the thermally conductive filler in the mixed composition is also as described above. However, while the content of each component is shown above as an amount based on 100 parts by mass of the polymer matrix, in the mixed composition, the amount is based on 100 parts by mass of the curable polymer composition.

[0079] (Step 2) Step 2 is a step of curing the mixed composition by heating. The temperature at which the mixed composition is heated is not particularly limited as long as the curable polymer composition can be cured by heating. It is sufficient to heat the mixed composition at a temperature higher than room temperature (25°C), but preferably at 50°C or higher, more preferably at 70°C or higher. The heating temperature is also not particularly limited, but may be any temperature that does not cause thermal degradation of the thermally conductive layer or the mixed composition, for example, 200°C or lower, preferably 180°C or lower, more preferably 160°C or lower. The heating may be performed in one stage or in two or more stages. When performing the heating in two or more stages, the heating temperature may be within the above range in at least one stage, but it is preferable that the heating temperature be within the above range in all stages. Furthermore, it is preferable that at least the first heating stage is heated at a temperature lower than the boiling point of the volatile compound. The total heating time is, for example, about 10 minutes to 24 hours. When the curing is carried out in two or more stages, for example, the mixed composition may be partially cured in the first stage (primary curing) and fully cured by heating in the second or subsequent stage (secondary curing). Alternatively, the curing may be such that the mixed composition is fully cured by the primary curing and the heating in the second or subsequent stage does not involve curing.

[0080] As described below, when a molded product obtained from the mixed composition is sliced ​​into a sheet-like molded product, it is also preferable to perform a first-stage heating before slicing to perform primary curing, and then further heating after slicing to perform a second-stage or subsequent heating (secondary curing). By heating after slicing, volatile substances are more likely to volatilize by the second-stage or subsequent heating. When curing in two or more stages, the heating in the first stage (primary curing) may be performed at a temperature of, for example, 50°C to 120°C, preferably 60°C to 100°C, and more preferably 70°C to 90°C. Furthermore, the heating in the second stage or subsequent (secondary curing) may be performed at a temperature higher than that of the primary curing, for example, 100°C to 200°C, preferably 120°C to 180°C, and more preferably 140°C to 160°C. The heating time in the first stage may be, for example, from 5 minutes to 20 hours, and preferably from 30 minutes to 12 hours. The heating time in the second and subsequent stages is, for example, about 10 minutes to 15 hours, preferably about 1 hour to 10 hours. By performing the first heating stage on the molded body obtained from the mixed composition at a relatively low temperature as described above, the volatile compound is less likely to foam and generate large bubbles, and the molded body can be cured so that the volatile compound remains within the molded body. Furthermore, if the molded body is sliced ​​and then heated in the second stage at a relatively high temperature, the molded body will harden, preventing foaming and generating large bubbles even at high temperatures, and the spaces where the volatile compound was present will become fine bubbles. The size of the bubbles is, for example, 1 μm or less, preferably 0.2 μm or less. There is no particular lower limit to the size of the bubbles, but it is, for example, 0.001 μm or more.

[0081] In step 2, the mixed composition may be formed into a predetermined shape such as a block or sheet, and then heated to harden. Furthermore, in step 2, if the mixed composition contains an anisotropic filler as the thermally conductive filler, the anisotropic filler may be oriented in one direction before being hardened by heating. The anisotropic filler can be oriented by a magnetic field orientation method or a flow orientation method, but magnetic field orientation is preferred.

[0082] In the magnetic field orientation method, the mixed composition is injected into a mold or the like and placed in a magnetic field to orient the anisotropic filler along the magnetic field. The curable polymer composition is then cured to obtain an oriented molded body. The mixed composition is preferably cured under the heating conditions described above. The oriented molded body is preferably in the form of a block, but may also be in the form of a sheet. By using a sheet, the oriented molded body may be coated with an adhesive directly in step 3 without slicing. On the other hand, by using a block, the orientation of the anisotropic filler is enhanced.

[0083] In the magnetic field orientation method, a release film may be placed inside the mold in the portion that comes into contact with the mixed composition. For example, a resin film with good releasability or a resin film whose one side has been treated with a release agent or the like is used as the release film. By using the release film, the oriented molded body can be easily released from the mold.

[0084] The viscosity of the mixed composition used in the magnetic field orientation method is preferably 10 Pa·s or more and 300 Pa·s or less in order to achieve magnetic field orientation. By setting the viscosity at 10 Pa·s or more, the thermally conductive filler is less likely to settle. Furthermore, by setting the viscosity at 300 Pa·s or less, the fluidity is improved, the anisotropic filler is properly oriented in the magnetic field, and problems such as excessive time required for orientation do not occur. Note that the viscosity is measured using a rotational viscometer (Brookfield viscometer DV-E, spindle SC4-14) at 25°C and a rotation speed of 10 rpm. However, when using a thermally conductive filler that is less likely to settle or when combining with additives such as anti-settling agents, the viscosity of the mixed composition may be less than 10 Pa·s.

[0085] In the magnetic field orientation method, magnetic field line generating sources for applying magnetic field lines include superconducting magnets, permanent magnets, electromagnets, etc., but superconducting magnets are preferred because they can generate a magnetic field with a high magnetic flux density. The magnetic flux density of the magnetic field generated from these magnetic field line generating sources is preferably 1 to 30 Tesla. If the magnetic flux density is 1 Tesla or higher, it becomes possible to easily orient the above-mentioned anisotropic filler made of a carbon material, etc. Furthermore, if the magnetic flux density is 30 Tesla or lower, practical production becomes possible.

[0086] In the flow orientation method, a primary sheet is produced in which the anisotropic filler is oriented in the plane direction by applying a shear force to the mixed composition. More specifically, in the flow orientation method, the mixed composition prepared in step 1 is first stretched flat while applying a shear force to form a sheet (primary sheet). Applying a shear force can orient the anisotropic filler in the shear direction. Examples of sheet forming methods include applying the mixed composition to a substrate film using a coating applicator such as a bar coater or doctor blade, or by extrusion molding or nozzle discharge, and then drying, semi-curing, or fully curing the mixed composition as needed. The thickness of the primary sheet is preferably approximately 50 μm to 5,000 μm. In the primary sheet, the anisotropic filler is oriented in one direction along the plane direction of the sheet. The mixed composition used in the flow orientation method has a relatively high viscosity so that a shear force is applied when stretched into a sheet. Specifically, the viscosity of the mixed composition is preferably 3 Pa·s to 500 Pa·s.

[0087] The primary sheet may be used as a thermally conductive sheet without being formed into a block, as described below. Alternatively, a laminated block (a block-shaped oriented molded product) may be formed by stacking multiple primary sheets so that they are oriented in the same direction, and then bonding the primary sheets together using a heat press or the like while curing them by heating as needed. To form a laminated block, at least one of the surfaces of the primary sheets to be stacked may be irradiated with vacuum ultraviolet light, and then the primary sheets may be stacked. By stacking the primary sheets via the surface irradiated with vacuum ultraviolet light, the primary sheets can be firmly bonded to each other. When irradiating with vacuum ultraviolet light, the mixed composition may be fully cured when preparing the primary sheet; curing by heating or the like is not necessary when stacking the primary sheets to form the laminated block. Even in the flow orientation method, the mixed composition may be cured under the heating conditions described above.

[0088] As described above, when forming a block-shaped oriented molded body, the obtained oriented molded body may be cut perpendicular to the orientation direction of the anisotropic filler by slicing or the like to form a sheet-shaped molded body. Slicing may be performed, for example, using a shear blade or a laser. When the sheet-shaped molded body is cut by slicing or the like, a portion of the fibrous filler may be exposed from the matrix at each surface, i.e., the cut surface. Most of the exposed fibrous filler will be oriented in the thickness direction without collapsing. However, in step 2, when the oriented molded body is cut by slicing or the like, the fibrous filler contained in the oriented molded body may be cut to a degree that does not impair the effects of the present invention.

[0089] The sheet-like molded body obtained by cutting may be directly coated with an adhesive in step 3 described below, or may be further processed. For example, each surface, i.e., the sliced ​​surface, may be polished. Furthermore, as described above, secondary curing may be performed. The secondary curing may be performed after or before polishing. By polishing the sheet-like molded body, the surface condition of the sheet-like molded body is improved, making it easier to further reduce the thermal resistance value. By polishing the sheet-like molded body, the sheet surface can be made smooth while leaving a certain amount of anisotropic filler, such as a fibrous filler, exposed on the surface. The fibrous filler can also be made to be in a collapsed state. This makes it easier to adhere the surface of the thermally conductive sheet to other components, and also makes it easier to cover the sheet surface with the fibrous filler over a certain area or more, making it easier to reduce the thermal resistance value.

[0090] The polishing may be performed by polishing at least one surface of the obtained sheet-like molded body, but it is preferable to polish both surfaces of the sheet-like molded body. The surface polishing may be performed using, for example, abrasive paper, abrasive film, abrasive cloth, abrasive belt, or the like. The properties of the abrasive paper are preferably those containing abrasive grains with an average particle size (D50) of 0.1 μm or more and 100 μm or less, more preferably 1 μm or more and 60 μm or less. The grain size of the abrasive grains in the abrasive paper is preferably #120 to 20,000, more preferably #300 to 15,000, and more preferably #320 to 4,000.

[0091] The polishing method can be, for example, polishing the surface of the sheet-like molded body by continuously contacting abrasive paper in the same linear direction, or by polishing by reciprocating a certain distance, by polishing by rotating in the same direction, or by polishing by contacting in various directions. The degree of polishing can be determined, for example, while observing the surface condition. For example, in the case of reciprocating polishing, one to 300 reciprocating strokes is preferred, two to 200 strokes is more preferred, and three to 50 strokes is even more preferred. The surface of the sheet-like molded body may be polished in two separate polishing steps. For example, after the first polishing using abrasive paper with a larger average particle size of abrasive grains, a second polishing using abrasive paper with a smaller average particle size of abrasive grains than that used in the first polishing may be performed.

[0092] (Step 3) In step 3, an adhesive is applied to the surface of the cured product, such as the sheet-like molded product, obtained in step 2, as described above. In the present invention, the adhesive to be applied is preferably an acrylic adhesive having a reactive double bond, as described above. In addition, in this manufacturing method, it is preferable to impregnate the thermally conductive layer with the adhesive in step 4, but it is also preferable that the adhesive penetrates into the thermally conductive layer simply by applying the adhesive. In other words, it is preferable that steps 3 and 4 proceed simultaneously.

[0093] The adhesive may be diluted with a diluent and applied to the surface of the sheet-shaped molded body as a diluted adhesive solution. Diluting the adhesive with a diluent makes it easier for the adhesive to penetrate into the thermal conductive layer. The diluent is not particularly limited as long as it is a liquid at 25°C and 1 atmosphere, has solubility or compatibility with the adhesive, and is a component that volatilizes upon drying as described below, but an organic solvent is preferably used.

[0094] The organic solvent to be used is not particularly limited, but examples thereof include ketone compounds such as acetone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbon compounds such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, tripropylene glycol monomethyl ether, and polyethylene glycol monoethyl ether; ester compounds such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; and aliphatic hydrocarbon compounds such as hexane, octane, and decane. In order to properly penetrate the adhesive into the thermally conductive layer when spray-coating as described below, it is preferable to use an organic solvent that does not volatilize too quickly, such as cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, or polyethylene glycol monoethyl ether. In addition to the organic solvents listed above, it is also preferable to use an organic solvent with a lower boiling point than these. Specific examples include methyl ethyl ketone, methyl isobutyl ketone, hexane, ethyl acetate, butyl acetate, and toluene.

[0095] The dilution concentration with the diluent is not particularly limited, but it is recommended to adjust the solids concentration of the adhesive to, for example, 5% by mass or more and 50% by mass or less, preferably 8% by mass or more and 35% by mass or less, and more preferably 10% by mass or more and 25% by mass or less. A solids concentration of 5% by mass or more can prevent excessive heating during drying and allow a predetermined amount of adhesive, together with the organic solvent, to properly penetrate into the thermally conductive layer. Furthermore, by adjusting the solids concentration to 50% by mass or less, the basis weight is not increased more than necessary and the viscosity can be adjusted to facilitate penetration, allowing the adhesive to properly penetrate into the thermally conductive layer. The amount of adhesive that penetrates into the thermally conductive layer can be adjusted by adjusting the viscosity, solids concentration, type of solvent, etc. For example, if you want to increase the amount of adhesive that penetrates, you can adjust the solids concentration to a high concentration with a low viscosity. If you want to reduce the amount of adhesive that penetrates, you can adjust the solids concentration to a high concentration with a high viscosity.

[0096] The adhesive application method is not particularly limited, and known application methods may be employed, although spray application is preferred. Spray application prevents the basis weight from becoming excessively high and facilitates the adhesive to properly penetrate the thermally conductive layer. Furthermore, spray application and reduced application volume can provide areas with and without an adhesive layer on the thermally conductive layer surface. When spray application is employed, it is preferable to spray an adhesive containing a fast-drying organic solvent such as ethyl acetate and a slow-drying organic solvent such as polyethylene glycol monoethyl ether or propylene glycol monomethyl ether acetate. More specifically, the inclusion of a slow-drying organic solvent prevents excessive evaporation of the organic solvent when the adhesive is applied to the thermally conductive layer surface from the sprayer, thereby facilitating penetration of the adhesive into the thermally conductive layer. On the other hand, the inclusion of a fast-drying solvent preferably adjusts the viscosity to a level suitable for spray application.

[0097] The applied adhesive may then be dried to volatilize the diluent. The drying temperature may be a temperature at which the reaction of the reactive double bonds in the adhesive does not substantially proceed, for example, 80°C or less, preferably 70°C or less, and more preferably 60°C or less. The drying temperature is not particularly limited in terms of its lower limit, and may be around room temperature, for example, 20°C or more. From the viewpoint of shortening the drying time, however, 30°C or more is preferred, 40°C or more is more preferred, and 45°C or more is even more preferred. The drying time may be a time sufficient to volatilize substantially all of the diluent contained in the applied adhesive, for example, 1 minute or more, preferably 2 minutes or more, and more preferably 3 minutes or more. The drying time is not particularly limited, but from the viewpoint of workability, it is better to have a shorter drying time, for example, 24 hours or less, preferably 3 hours or less, and more preferably 1 hour or less.

[0098] [Uses of Thermally Conductive Sheets] Thermally conductive sheets are interposed between a heat-generating element and a heat sink, transferring heat generated by the heat-generating element to the heat sink via thermal conduction and dissipating the heat from the heat sink. Thermally conductive sheets are used in electronic devices, semiconductor applications, and the like, and are preferably used in semiconductor applications. In semiconductor applications, thermally conductive sheets may be used in any application, but are preferably used in applications called TIM1, where they are directly applied to semiconductor chips such as silicon dies, for example, between semiconductor chips and heat spreaders. Of course, thermally conductive sheets may also be used in applications called TIM2, where they are not directly applied to semiconductor chips. In this case, the thermally conductive sheet may be used, for example, between a heat spreader and a cooling unit such as a heat sink or heat pipe. In addition to the above, thermally conductive sheets may also be used between various electronic components that generate heat and heat sinks, heat pipes, heat pumps, metal housings of electronic devices, and other heat sinks. The thermally conductive sheet is preferably placed between two members (adherends) such as a heat sink or a heat generator, and is preferably used in a state of being in close contact with and compressed against each member (adherend).

[0099] The thermally conductive sheet is preferably used in applications where it is heated to high temperatures, for example, between 200°C and 300°C, preferably between 220°C and 270°C, while in close contact with an adherend via an acrylic adhesive layer. The thermally conductive sheet of the present invention maintains, or in some cases even improves, its adhesive strength to the adherend even when heated to high temperatures while in close contact with the adherend. Therefore, even when heated to high temperatures as described above while in close contact with the adherend, peeling from the adherend is prevented. It is preferable to heat the sheet without applying pressure. For semiconductor applications, the thermally conductive sheet is preferably subjected to a reflow process while in close contact with the adherend via an acrylic adhesive layer, and is preferably heated within the above-mentioned temperature range during the reflow process. The thermally conductive sheet is preferably heated during the reflow process while in close contact with one or both of the adherends, for example, a semiconductor chip or a heat spreader, via an acrylic adhesive layer. Thus, the thermally conductive sheet of the present invention can be used to bond a semiconductor chip and a heat spreader during the reflow process. Before heating to 200°C or higher, it is preferable to carry out a bonding step in which the thermally conductive sheet is bonded to the adherend via the acrylic adhesive layer. The bonding step is carried out, for example, by heating the thermally conductive sheet sandwiched between the adherends to a temperature of 50°C to 180°C and applying pressure. The heating temperature is preferably 120°C to 160°C.

[0100] As described above, the present invention can also provide a bonding method that sequentially performs a bonding step of sandwiching a thermally conductive sheet between a semiconductor chip and a heat spreader to bond them together, and a bonding step of heating the semiconductor chip and heat spreader to 200°C or higher after the bonding step. In the bonding step, after sandwiching the thermally conductive sheet between the semiconductor chip and the heat spreader, the sheets are preferably pressed together at a temperature of 50°C or higher and 200°C or lower, more preferably 50°C or higher and 180°C or lower, and even more preferably 120°C or higher and 160°C or lower. The heating temperature in the bonding step is preferably 220°C or higher, and preferably 300°C or lower, more preferably 270°C or lower. The bonding step is preferably performed without pressure.

[0101] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0102] The measurement and evaluation methods in the present examples are as follows.

[0103] [A / B ratio] A drop of adhesive coating solution prepared in the same manner as the adhesive used in each Example and Comparative Example was applied to a gold-plated stainless steel plate, and after application, the plate was thoroughly dried to volatilize the solvent, and an acrylic adhesive layer was formed on the plate. Note that drying was performed by leaving the plate coated with the adhesive in an 80°C environment for 15 minutes. The acrylic adhesive layer formed on the plate was analyzed by Raman analysis, and the A / B value was determined using the following equipment and measurement conditions. Note that in each Example and Comparative Example, a wave number of 1636.1 cm was used. -1 The intensity is "A", and the wave number is 1724.4 cm -1 The intensity of the laser beam was designated as "B". (Device used) "inVia Qcontrol", manufactured by Renishaw (Measurement conditions) Laser power: 50 Number of times of integration: 1 Laser wavelength: 785 nm Grating: 1200 l / mm Magnification: 50 times Focus: Aligned with the surface of the sample on which the acrylic adhesive layer was formed

[0104] [Confirming Penetration into the Acrylic Adhesive Layer] The diluted adhesive solution used in each Example and Comparative Example further contained 0.5 parts by mass of the fluorescent agent Nikka Flow OB (manufactured by Nippon Chemical Industry Co., Ltd.) per 100 parts by mass of adhesive. Using the diluted solution prepared in this manner, a thermally conductive sheet was produced using the same method as in each Example and Comparative Example. The thermally conductive sheet was sliced ​​in the thickness direction to form a cross section (observation surface), which was then observed using a fluorescence microscope. The areas where fluorescence from the fluorescent agent was observed were areas where the adhesive had penetrated, confirming whether the adhesive had penetrated into the thermally conductive layer. The fluorescence microscope conditions were as follows: Fluorescence microscope device: Olympus "Polarizing Microscope BX51" Light source: Olympus "U-RFL-T" mercury lamp Measurement conditions: The observation surface was irradiated with 365 nm light, and the focus was adjusted using a 10x objective lens through an optical filter that transmits visible light and absorbs ultraviolet light of 400 nm or less. Next, the distribution of light emission (blue light emission) from the fluorescent agent was observed using the software "Stream Basic" with an exposure time of 800 ms. The exposure time is not limited to 800 ms, but may be any time that allows the distribution of light emission from the fluorescent agent to be recognized. For example, the exposure time can be adjusted according to the width of the field of view and the intensity of the light source.

[0105] [Initial Sheet Thickness] The thickness (initial thickness) of the thermally conductive sheet before compression was measured using a thickness gauge.

[0106] [E Hardness] The type E hardness of the thermally conductive sheet was measured in accordance with Japanese Industrial Standard JIS K 6253. Specifically, the oriented molded article produced in each example was measured using a type E durometer.

[0107] [Arithmetic Mean Height (Sa)] The arithmetic mean height (Sa) of the surface of the thermally conductive sheet was measured in accordance with ISO 25178 by surface quality analysis using a laser microscope (Keyence Corporation, VK-X150). Specifically, the surface profile of a two-dimensional area with a surface area of ​​1000 μm × 1000 μm was measured using a laser method at a lens magnification of 10x. The average value obtained by measuring three locations on the same sample was used as the arithmetic mean height (Sa) of the peaks. For thermally conductive sheets provided with an acrylic adhesive layer, the arithmetic mean height (Sa) of the surface of the thermally conductive sheet provided with the acrylic adhesive layer was measured.

[0108] [Thermal Resistance Value] The thermal resistance value was measured using a thermal resistance measuring instrument as shown in FIG. 1 by the following method. Specifically, for each sample, a test piece S measuring 30 mm × 30 mm was prepared for this test. Each test piece S was then attached to a copper block 22 with a measurement surface of 25.4 mm × 25.4 mm and sides covered with a thermal insulator 21, and sandwiched between upper copper blocks 23. A load of 10 psi was applied by a load cell 26. Here, the lower copper block 22 was in contact with a heater 24. The upper copper block 23 was also covered with a thermal insulator 21 and connected to a heat sink 25 equipped with a fan. Next, the heater 24 was heated to 80°C, and after 10 minutes when the temperature reached a substantially steady state, the temperature (θ j0 ), the temperature of the lower copper block 22 (θ j1 ), and the heat generation amount (Q) of the heater were measured, and the thermal resistance value of each sample was calculated using the following formula (1). At the same time as measuring the thermal resistance value, the thickness of the thermally conductive sheet at the time of measuring the thermal resistance value was also measured. Thermal resistance = (θ j1 -θ j0 ) / Q Formula (1) In formula (1), θ j1 is the temperature of the lower copper block 22, θ j0 is the temperature of the upper copper block 23, and Q is the amount of heat generated.

[0109] Similar measurements were performed with the pressure applied by the load cell 26 changed to 20 psi, 30 psi, and 40 psi, and the results are shown in Table 2. Regarding the thermal resistance value at a pressure of 20 psi, the thermal resistance change rate was calculated as the ratio of the thermal resistance value when the thermal resistance value of a blank thermal conductive sheet was set as the reference (100%). The blank was a thermal conductive sheet with the same configuration except that it did not have an acrylic adhesive layer.

[0110] [Die Shear Strength] As shown in Figure 2, a 3 mm x 3 mm thermally conductive sheet 11 obtained in each Example and Comparative Example was placed on a nickel-plated copper plate 10 having an outer dimension of 50 mm x 50 mm and a thickness of 2 mm. A 3 mm x 3 mm, 600 μm-thick silicon die 12 was then placed on the thermally conductive sheet 11. The resulting laminate was pressed in the thickness direction at a pressure of 1 MPa for 60 seconds in a room temperature environment to bond the thermally conductive sheet 11 to the nickel-plated copper plate 10 and the silicon die 12, thereby obtaining a measurement sample 15. The measurement sample 15 was placed on a hot plate with the nickel-plated copper plate side 11 facing down and heated at 250 °C for 3 minutes. Note that heating at 250 °C for 3 minutes simulates a reflow process. Thereafter, in a 25°C environment, a die shear tester ("Dage-S4000", manufactured by Nordson Corporation) was used to adjust the height so that the tip of the tool 17 was 300 μm above the surface of the thermally conductive sheet 10. The tool 17 was then applied to the silicon die 12 at a speed of 150 μm / s along the shear direction S, and the load required to break the joint was taken as the die shear strength. The die shear strength was also measured in a 25°C environment for the measurement sample without heating at 250°C for 3 minutes. The die shear strength measured in a 25°C environment without heating at 250°C for 3 minutes was used as the blank.

[0111] Measurement of die shear strength using a die shear tester was also performed on measurement samples prepared in the same manner in an 80°C environment and an 150°C environment. The die shear strengths measured in 25°C, 80°C, and 150°C environments are shown in Table 2. The die shear strength measured in 25°C, 80°C, and 150°C environments when heated at 250°C for 3 minutes (i.e., reflow treatment) is expressed as a percentage (%) relative to the blank, and is shown in Table 2 as the rate of change in die shear strength. Note that a rate of change in die shear strength of 75% or more can be considered a good result.

[0112] The following components were used as raw materials for the thermally conductive sheet. (Polymer composition) Curable silicone: an addition reaction type organopolysiloxane consisting of an alkenyl group-containing organopolysiloxane as the base material and a hydrogen organopolysiloxane as the curing agent (but containing a catalytic amount of platinum catalyst). (Volatile substance) n-decyltrimethoxysilane

[0113] (Thermal conductive filler) Aluminum oxide 1: spherical, average particle size (D50) = 3 μm, aspect ratio 1.0 Aluminum oxide 2: polyhedral, average particle size (D50) = 0.5 μm, aspect ratio 1.0 Aluminum: spherical, average particle size (D50) = 3 μm, aspect ratio 1.0 to 1.5 Graphitized carbon fiber: average fiber length (arithmetic mean) 85 μm, diameter 10 μm, aspect ratio 8.5, thermal conductivity 900 W / m·K Flake boron nitride: average particle size (D50) = 50 μm, aspect ratio 20 to 50, thermal conductivity 200 W / m·K Flake graphite powder: average particle size (D50) = 15 μm, aspect ratio 10, thermal conductivity 550 W / m·K

[0114] (Adhesives) Adhesive 1: An adhesive whose main adhesive agent is an acrylic polymer whose main component is a structural unit derived from 2-ethylhexyl acrylate and has hydroxyl groups, carboxyl groups, and vinyl groups in its side chains. A / B = 0.588 Adhesive 2: An adhesive whose main adhesive agent is an acrylic polymer whose main component is a structural unit derived from 2-ethylhexyl acrylate and has hydroxyl groups, carboxyl groups, and vinyl groups in its side chains. A / B = 0.405 Adhesive 3: An adhesive whose main adhesive agent is an acrylic polymer whose main component is a structural unit derived from 2-ethylhexyl acrylate and butyl acrylate and has hydroxyl groups and carboxyl groups in its side chains but no reactive double bonds. A / B = 0.138 Adhesive 4: An adhesive whose main adhesive agent is an acrylic polymer whose main component is a structural unit derived from butyl acrylate and has hydroxyl groups and carboxyl groups in its side chains but no reactive double bonds. A / B=0.138 *100 parts by mass of a diluted solution of the adhesive diluted with ethyl acetate to a solid content concentration of 33% by mass was further diluted with 120 parts by mass of propylene glycol monomethyl ether acetate (solvent) to prepare a coating solution with a solid content concentration of 15% by mass, which was used in each of the Examples and Comparative Examples.

[0115] Example 1: The components in accordance with Recipe 1 in Table 1 were mixed using a planetary mixer at 25°C for 50 minutes to obtain a mixed composition. The mixed composition was then poured into a mold set to a thickness sufficiently greater than that of the thermally conductive sheet, and an 8 T magnetic field was applied in the thickness direction to orient the carbon fibers and flake graphite in the thickness direction. The curable silicone was then primarily cured by heating at 80°C for 8 hours to obtain a block-shaped oriented molded product. Next, the block-shaped oriented molded product was sliced ​​into sheets approximately 120 μm thick using a shearing blade to obtain a sheet-shaped molded product with exposed carbon fibers. The sheet-shaped molded product was then heated at 150°C for 6 hours to undergo secondary curing. The sheet-shaped molded product was then reciprocally polished 25 times with coarse abrasive paper A (grain size #800) having an average abrasive grain size (D50) of 20 μm, and then further reciprocally polished 10 times with coarse abrasive paper B (grain size #4000) having an average abrasive grain size (D50) of 3 μm.

[0116] The adhesive 1 coating solution was sprayed onto both surfaces of the resulting sheet-like molded article, adjusting the discharge rate so that the dried basis weight was the amount listed in Table 1. The sheet was then dried at 50°C for 3 minutes to obtain a thermally conductive sheet with an acrylic adhesive layer on both surfaces of the thermally conductive layer. Fine bubbles were present within the thermally conductive layer, and it was confirmed that the acrylic adhesive had penetrated into the fine bubbles near both surfaces. The thermally conductive layer had a filling rate of 64.0% by volume, and the anisotropic filler was oriented in the thickness direction. The thickness of the thermally conductive sheet was as listed in the table.

[0117] Examples 2, 3, and 7 The same procedures as in Example 1 were carried out, except that the spray application conditions were changed so that the basis weight of the acrylic adhesive layer after drying was as shown in Table 2.

[0118] [Example 4] The same procedure as in Example 1 was carried out, except that the type of adhesive was changed as shown in Table 2 and the spray application conditions were changed so that the basis weight of the acrylic adhesive layer after drying was as shown in Table 2.

[0119] Example 5 The same procedure as in Example 1 was carried out, except that the block-shaped oriented molded product was sliced ​​into sheets having a thickness of about 80 μm.

[0120] [Example 6] According to formulation 3 in Table 1, the components were mixed using a planetary mixer at 25°C for 50 minutes to obtain a mixed composition. The mixed composition was applied unidirectionally to a polyethylene terephthalate (PET) substrate film at 25°C using a bar coater as an applicator. The anisotropic filler was oriented such that its major axis was aligned with the application direction and its minor axis was aligned with one direction along the sheet surface and perpendicular to the application direction. Next, the applied mixed composition was heated at 80°C for 8 hours to harden the liquid composition, thereby obtaining a primary sheet having a thickness of 2 mm.

[0121] Both sides of each of the obtained primary sheets were exposed to a VUV irradiation device (trade name Excimer MINI, manufactured by Hamamatsu Photonics K.K.) at room temperature (25°C) in the atmosphere with an integrated light dose of 20 mJ / cm 2 on the surface of the primary sheet. 2VUV irradiation was performed under the conditions of . Next, 100 VUV-irradiated primary sheets were stacked and pressed with a roller at a pressure of 1.6 kgf / 50 mm in an environment of 25 °C to obtain a laminated block. The obtained laminated block was sliced ​​with a cutter blade parallel to the stacking direction and perpendicular to the direction along the long axis of the scale-like filler, obtaining a sheet-like molded product with a thickness of 2 mm for each unit layer and a sheet thickness of approximately 0.30 mm. In the sheet-like molded product, the anisotropic filler was oriented in the thickness direction. The sheet-like molded product was then further heated at 150 °C for 6 hours for secondary curing. The same procedure as in Example 1 was then performed, except that the spray application conditions were changed so that the basis weight of the acrylic adhesive layer after drying was as shown in Table 2, to obtain a thermally conductive sheet having an acrylic adhesive layer on both surfaces of the thermally conductive layer. The filling rate of the thermally conductive filler in the thermally conductive layer was 70.2 vol%, and the anisotropic filler was oriented in the thickness direction.

[0122] [Example 8] A thermally conductive sheet having an acrylic adhesive layer on both surfaces of the thermally conductive layer was obtained in the same manner as in Example 1, except that the formulation of the mixed composition was changed to Formulation 2 shown in Table 1 and the spray application conditions were changed so that the basis weight of the acrylic adhesive layer after drying was as shown in Table 2. No fine bubbles were found inside the thermally conductive layer, and it was not possible to confirm that the acrylic adhesive had penetrated into the fine bubbles. The filling rate of the thermally conductive filler in the thermally conductive layer was 59.9% by volume, and the anisotropic filler was oriented in the thickness direction.

[0123] [Comparative Examples 1 and 2] The same procedures as in Example 1 were carried out, except that the type of adhesive was changed as shown in Table 2 and the spray application conditions were changed so that the basis weight of the acrylic adhesive layer after drying was as shown in Table 2.

[0124] Comparative Example 3 The same procedure as in Example 1 was carried out, except that the adhesive coating liquid was not applied to the sheet-shaped molding.

[0125] Comparative Example 4 The same procedure as in Example 8 was carried out, except that the adhesive coating liquid was not applied to the sheet-shaped molding.

[0126] Comparative Example 5 The same procedure as in Example 6 was carried out, except that the adhesive coating liquid was not applied to the sheet-shaped molding.

[0127] *The values ​​for each component are parts by mass in each formulation. *The sheet hardness values ​​were measured for the cured products obtained from formulations 1, 2, and 3 in each example and comparative example.

[0128] *In Comparative Example 3, the thermally conductive sheet could not be adhered to the silicon die or the nickel-plated copper plate, so the die shear strength could not be measured.

[0129] In the above examples, the provision of an acrylic adhesive layer having a reactive double bond on the surface of the thermally conductive sheet improved die shear strength and adhesion to the adherend. Furthermore, even after the thermally conductive sheet was heated to a high temperature of approximately 250°C while in close contact with the adherend, high die shear strength was maintained, preventing peeling of the adhered thermally conductive sheet even after a reflow process. These results were also obtained when the die shear strength was measured at 80°C or 150°C, assuming a typical usage environment. In contrast, in Comparative Examples 1 and 2, the provision of an acrylic adhesive layer on the surface of the thermally conductive sheet improved die shear strength. However, because the acrylic adhesive layer does not contain a reactive double bond, when heated to a high temperature (250°C) while in close contact with the adherend, high die shear strength cannot be maintained, raising concerns about peeling during a reflow process. Furthermore, in Comparative Examples 3 to 5, the absence of an acrylic adhesive layer on the surface of the thermally conductive sheet prevented improvement in die shear strength.

Claims

1. A thermally conductive sheet comprising: a thermally conductive layer including a polymer matrix and a thermally conductive filler; and an acrylic adhesive layer provided on a surface of the thermally conductive layer, the acrylic adhesive layer having a reactive double bond.

2. The thermally conductive sheet according to claim 1, wherein the intensity ratio A / B of the peak intensity A of the C=C stretching vibration to the peak intensity B of the C=O stretching vibration in the Raman spectrum of the acrylic adhesive layer is 0.2 or more.

3. The thermally conductive sheet according to claim 1 or 2, wherein the polymer matrix is ​​an organopolysiloxane.

4. The thermally conductive sheet according to claim 1 or 2, wherein the thermally conductive layer contains an anisotropic filler oriented in the thickness direction of the thermally conductive layer.

5. A thermally conductive sheet according to claim 1 or 2, wherein the surface of the thermally conductive layer is a sliced ​​surface.

6. The thermally conductive sheet according to any one of claims 1 to 5, wherein the acrylic adhesive layer is permeated into the thermally conductive layer.

7. A method for producing a thermally conductive sheet, comprising: a step of mixing at least a curable polymer composition and a thermally conductive filler to obtain a mixed composition; a step of curing the mixed composition by heating to obtain a cured product; and a step of applying an adhesive to a surface of the cured product, wherein the adhesive is an acrylic adhesive having a reactive double bond.

8. The method for producing a thermally conductive sheet according to claim 7, further comprising heating the mixed composition to obtain a molded body, slicing the molded body, and forming the cured product into a sheet.

9. A method for producing a thermally conductive sheet as described in claim 7 or 8, wherein in addition to the curable polymer composition and the thermally conductive filler, a compatible substance is further mixed to obtain the mixed composition, and at least a portion of the compatible substance is volatilized by the heating.

10. A method for producing a thermally conductive sheet according to claim 7 or 8, wherein the applied adhesive is allowed to soak into the cured product.

11. A bonding method comprising the steps of: sandwiching the thermally conductive sheet according to claim 1 or 2 between a semiconductor chip and a heat spreader to bring them into close contact; and, following the bonding step, bonding the semiconductor chip and the heat spreader by heating them to 200°C or higher.

12. The bonding method according to claim 11, wherein in the bonding step, the thermally conductive sheet is sandwiched between the semiconductor chip and the heat spreader, and then pressure is applied at 50° C. or higher and 200° C. or lower to bond them together.

13. The bonding method according to claim 11 or 12, wherein the bonding step is carried out without applying pressure.

14. Use of a thermally conductive sheet for bonding a semiconductor chip and a heat spreader in a reflow process, the thermally conductive sheet comprising a thermally conductive layer containing a polymer matrix and a thermally conductive filler, and an acrylic adhesive layer provided on the surface of the thermally conductive layer, the acrylic adhesive layer having a reactive double bond.

Citation Information

Patent Citations

  • Thermally conductive material

    JP2002194232A

  • Heat conducting sheet, method for producing heat conducting sheet, and heat radiator

    JP2012109312A