Composition for forming resist underlayer film

A resist underlayer film composition with an aromatic hydrocarbon ring and phenolic hydroxyl group addresses defects in semiconductor pattern formation by enhancing sensitivity and preventing intermixing, effectively supporting advanced lithography techniques in semiconductor manufacturing.

WO2024204764A1PCT designated stage expired Publication Date: 2024-10-03NISSAN CHEM CORP
View PDF 64 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013182
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In semiconductor manufacturing, defects in resist pattern formation due to influences from semiconductor substrates have become a major issue as devices become more highly integrated, and existing methods for resist underlayer films do not effectively prevent intermixing with the resist film or achieve high sensitivity in pattern formation, especially with the use of advanced lithography techniques like EUV and electron beam lithography.

Method used

A composition for forming a resist underlayer film containing a compound with an aromatic hydrocarbon ring bonded to a phenolic hydroxyl group and a solvent, which includes a crosslinking agent, is used to create a film with an atomic percentage of oxygen in the phenolic hydroxy group of 2.00% or more, ensuring high sensitivity and preventing intermixing with the resist film.

Benefits of technology

The composition enables the formation of a resist underlayer film that achieves high sensitivity and prevents intermixing, leading to improved pattern formation and manufacturing of semiconductor elements using EUV or electron beam lithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
  • Figure JPOXMLDOC01-APPB-C000004
    Figure JPOXMLDOC01-APPB-C000004
Patent Text Reader

Abstract

Disclosed is a composition for forming a resist underlayer film, the composition containing a compound (A) that contains an aromatic hydrocarbon ring to which a phenolic hydroxy group is bonded, and a solvent (B), wherein the atomic percentage of oxygen in the phenolic hydroxy group in a cured film of the composition is 2.00% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Composition for forming resist underlayer film

[0001] The present invention relates to a composition for forming a resist underlayer film, a resist underlayer film, a laminate, a method for producing a semiconductor element, and a method for forming a pattern.

[0002] In the manufacture of semiconductor devices, microfabrication by lithography using a resist composition has traditionally been performed. This microfabrication process involves forming a thin film of a photoresist composition on a semiconductor substrate, such as a silicon wafer, irradiating the substrate with actinic rays such as ultraviolet light through a mask pattern bearing a device pattern, developing the thin film, and etching the substrate using the resulting photoresist pattern as a protective film, thereby forming fine irregularities on the substrate surface corresponding to the photoresist pattern. In recent years, the integration density of semiconductor devices has increased, and in addition to the conventionally used i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), and ArF excimer laser (wavelength 193 nm), the practical use of EUV light (wavelength 13.5 nm) or EB (electron beam) is being considered for cutting-edge microfabrication. As a result, poor resist pattern formation due to influences from the semiconductor substrate, etc., has become a major problem. To address this issue, methods of providing a resist underlayer film between the resist and the semiconductor substrate have been widely investigated.

[0003] Patent Document 1 discloses a composition for forming an underlayer film for lithography, which contains a naphthalene ring having a halogen atom. Patent Document 2 discloses a halogenated antireflective film. Patent Document 3 discloses a composition for forming a resist underlayer film.

[0004] International Publication No. 2006 / 003850 Special Publication No. 2005-526270 International Publication No. 2020 / 111068

[0005]

[0009] The present invention has been made in view of the above circumstances, and aims to provide a composition for forming a resist underlayer film that can form a resist underlayer film that can form a resist pattern with high sensitivity, as well as methods for manufacturing a resist underlayer film, a laminate, and a semiconductor device, and a pattern formation method, all of which use the composition for forming a resist underlayer film.

[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.

[0007] That is, the present invention encompasses the following aspects. [1] A composition for forming a resist underlayer film, comprising a compound (A) containing an aromatic hydrocarbon ring to which a phenolic hydroxy group is bonded and a solvent (B), wherein the atomic percentage of oxygen in the phenolic hydroxy group in a cured film of the composition is 2.00% or more. [2] The composition for forming a resist underlayer film according to [1], wherein the compound (A) contains at least one of a phenol resin, a naphthol resin, a biphenol resin, a polyhydroxystyrene, and a polyhydroxyvinylnaphthalene. [3] The composition for forming a resist underlayer film according to [1], wherein the compound (A) is a low-molecular-weight compound (A-1) containing two or more phenolic hydroxy groups and having a molecular weight of 5,000 or less. [4] The composition for forming a resist underlayer film according to any of [1] to [3], further comprising a crosslinking agent (C). [5] The composition for forming a resist underlayer film according to any of [1] to [4], wherein the composition for forming a resist underlayer film is a composition for forming a resist underlayer film for EUV or electron beam lithography. [6] A resist underlayer film that is a cured product of the composition for forming a resist underlayer film according to any one of [1] to [5]. [7] The resist underlayer film according to [6], wherein the atomic percentage of oxygen in phenolic hydroxy groups in the resist underlayer film is 2.00% or more. [8] The resist underlayer film according to [6] or [7], wherein the resist underlayer film has a film thickness of 2 nm or more and 20 nm or less. [9] A laminate comprising: a semiconductor substrate; and the resist underlayer film according to any one of [6] to [8].

[10] A method for manufacturing a semiconductor device, comprising: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film according to any one of [1] to [5]; and forming a resist film on the resist underlayer film.

[11] A pattern forming method comprising: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film according to any one of [1] to [5]; forming a resist film on the resist underlayer film; irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern; and etching the resist underlayer film using the resist pattern as a mask.

[0008] According to the present invention, it is possible to provide a composition for forming a resist underlayer film that can form a resist underlayer film that can form a resist pattern with high sensitivity, as well as methods for producing a resist underlayer film, a laminate, and a semiconductor element, and a pattern formation method, all of which use the composition for forming a resist underlayer film.

[0009] (Composition for forming a resist underlayer film) The composition for forming a resist underlayer film of the present invention contains a compound (A) containing an aromatic hydrocarbon ring having a phenolic hydroxy group bonded thereto, and a solvent (B). The composition for forming a resist underlayer film may also contain a crosslinking agent (C), a curing catalyst (D), and the like.

[0010] The atomic percentage of oxygen in the phenolic hydroxy groups in the cured film of the composition is 2.00% or more, preferably 2.00% or more and 30.00% or less, and more preferably 3.00% or more and 20.00% or less. When the atomic percentage of oxygen in the phenolic hydroxy groups in the cured film of the composition is 2.00% or more, it is possible to form a resist underlayer film that can form a resist pattern with high sensitivity. The atomic percentage of oxygen in the phenolic hydroxy groups in the cured film of the composition can be determined, for example, by the following method.

[0011] The resist underlayer film-forming composition is applied to a silicon wafer using a spinner. The silicon wafer is baked on a hot plate at 205°C for 60 seconds to obtain a 5 nm thick resist underlayer film. The silicon wafer on which the resist underlayer film is formed is cut to a size of approximately 0.5 x 1 cm and dried under reduced pressure for 20 hours or more. The wafer is then sealed in a 6.0 x 7.5 cm weighing bottle with 3 ml of trifluoroacetic anhydride, and the hydrogen atoms of the phenolic hydroxy groups are substituted with trifluoroacetyl groups by gas-phase chemical modification at 25°C. The reaction time is determined based on the time required to reach reaction equilibrium for each composition. Further, unreacted trifluoroacetic anhydride and by-product trifluoroacetic acid are removed by drying under reduced pressure for 20 hours or more. The number of each atom constituting the film (excluding hydrogen) is then measured using X-ray photoelectron spectroscopy (Quanterar SXM) using an AlKa radiation source. The atomic percentage of oxygen in the phenolic hydroxy groups in the resist underlayer film (R ) is calculated using the following formula: OH [atom %]) is calculated. F: number of fluorine atoms A: total number of atoms (excluding hydrogen atoms) Note that, if the resist underlayer film contains fluorine atoms before being subjected to the vapor phase chemical modification method, the fluorine atoms are not included in F in the formula.

[0012] The atomic percentage of oxygen in the phenolic hydroxy groups in the cured film of the composition can be adjusted by appropriately selecting the amount of compound (A) and the type of compound (A) in the composition for forming a resist underlayer film.

[0013] <Compound (A)> The compound (A) contains an aromatic hydrocarbon ring to which a phenolic hydroxy group is bonded. The compound (A) may be a low molecular weight compound or a high molecular weight compound.

[0014] Examples of aromatic hydrocarbon rings include a benzene ring, a naphthalene ring, an anthracene ring, a pyrene ring, etc. That is, the term "phenolic hydroxy group" has the same meaning as a hydroxy group directly bonded to an aromatic hydrocarbon ring.

[0015] The number of phenolic hydroxy groups bonded to one aromatic hydrocarbon ring is not particularly limited, and may be one or two or more.

[0016] The number of aromatic hydrocarbon rings to which phenolic hydroxy groups are bonded that the compound (A) has is not particularly limited, and may be one or two or more.

[0017] As the compound (A), from the viewpoint of suitably obtaining the effects of the present invention, a phenol resin, a naphthol resin, a biphenol resin, a polyhydroxystyrene, a polyhydroxyvinylnaphthalene, or a low-molecular-weight compound (A-1) containing four or more phenolic hydroxy groups and having a molecular weight of 5,000 or less is preferred.

[0018] The molecular weight of the compound (A) is not particularly limited, but for example, the weight average molecular weight is preferably not more than 100,000, and more preferably not more than 70,000. The weight average molecular weight can be determined, for example, by gel permeation chromatography (GPC).

[0019] <<Phenol Resin, Naphthol Resin, Biphenol Resin>> Phenol resin, naphthol resin, and biphenol resin (hereinafter, these may be referred to as “phenolic resins”) are resins obtained, for example, by a condensation reaction of a phenolic compound with at least one of an aldehyde compound, a ketone compound, and a divinyl compound in the presence of an acid catalyst.

[0020] Examples of phenolic compounds include phenols, naphthols, anthrols, and hydroxypyrenes. Examples of phenols include phenol, cresol, xylenol, resorcinol, biphenol, bisphenol F, bisphenol A, p-tert-butylphenol, p-octylphenol, 9,9-bis(4-hydroxyphenyl)fluorene, and 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane. Examples of naphthols include 1-naphthol, 2-naphthol, 1,5-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, and 9,9-bis(6-hydroxynaphthyl)fluorene. Examples of anthrols include 9-anthrole. Examples of hydroxypyrenes include 1-hydroxypyrene and 2-hydroxypyrene. These compounds may be used alone or in combination of two or more. These compounds may have a substituent. For example, these compounds may have a substituent on the aromatic ring.

[0021] Examples of aldehyde compounds include saturated aliphatic aldehydes, unsaturated aliphatic aldehydes, heterocyclic aldehydes, aromatic aldehydes, etc. Examples of saturated aliphatic aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, propylaldehyde, butyraldehyde, isobutyraldehyde, valeraldehyde, capronaldehyde, 2-methylbutyraldehyde, hexylaldehyde, undecanoic aldehyde, 7-methoxy-3,7-dimethyloctyl aldehyde, cyclohexane aldehyde, 3-methyl-2-butyraldehyde, 2-ethylhexyl aldehyde, glyoxal, malonaldehyde, succinaldehyde, glutaraldehyde, adipic aldehyde, etc. Examples of unsaturated aliphatic aldehydes include acrolein and methacrolein. Examples of heterocyclic aldehydes include furfural and pyridine aldehyde. Examples of aromatic aldehydes include benzaldehyde, naphthyl aldehyde, anthryl aldehyde, phenanthryl aldehyde, salicyl aldehyde, phenylacetaldehyde, 3-phenylpropionaldehyde, tolyl aldehyde, (N,N-dimethylamino)benzaldehyde, and acetoxybenzaldehyde. Among these, saturated aliphatic aldehydes and aromatic aldehydes are preferred. Examples of ketone compounds include diaryl ketone compounds. Examples of diaryl ketone compounds include diphenyl ketone, phenyl naphthyl ketone, dinaphthyl ketone, phenyl tolyl ketone, and ditolyl ketone. Examples of divinyl compounds include divinylbenzene, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, 5-vinylnoborna-2-ene, divinylpyrene, limonene, 5-vinylnorbornadiene, etc. These can be used alone or in combination of two or more.

[0022] The phenolic resin preferably contains a structural unit represented by the following formula (1). In formula (1), R 1represents a substituent substituted on the ring, and each independently represents a halogen atom, a nitro group, a cyano group, an amino group, an optionally substituted alkyl group, an optionally substituted alkenyl group, or an optionally substituted aryl group. 2 represents a hydrogen atom, an optionally substituted aryl group, or an optionally substituted heteroaryl group. 3 represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted aryl group, or an optionally substituted heteroaryl group. 2 and R 3 The groups may be bonded to each other to form a divalent group. Examples of the substituents on the aryl group and heteroaryl group include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxy group, a carboxy group, an alkyl group, and an alkenyl group. 1 represents a benzene ring, a naphthalene ring, or a biphenyl structure. 1 Each of k independently represents an integer of 0 to 4. 1 Each independently represents an integer of 1 to 4. 1 When is a benzene ring, h 1 Tok 1 The sum of Ar is 4 or less, 1 When is a naphthalene ring, h 1 Tok 1 The sum of Ar is 6 or less, 1 When is a biphenyl structure, h 1 Tok 1 The sum of the above is 8 or less.

[0023] Specific examples of the structural unit represented by formula (1) are listed below, but the present invention is not limited to these.

[0024] Specific examples of phenols are listed below, but are not limited to these. n represents an integer of 0 to 4.

[0025] Examples of phenols include NeoFARIT 7177C (manufactured by Mitsubishi Gas Chemical Company, Inc.), NeoFARIT V002-EA2 (manufactured by Mitsubishi Gas Chemical Company, Inc.), and NeoFARIT V003 (manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0026] As described above, phenols are resins obtained by, for example, condensing a phenolic compound with at least one of an aldehyde compound, a ketone compound, and a divinyl compound in the presence of an acid catalyst. In this condensation reaction, for example, 0.1 to 10 equivalents of the aldehyde compound or ketone compound are typically used per equivalent of the benzene ring constituting the ring of the phenolic compound.

[0027] In the condensation reaction, an acid catalyst is usually used. Examples of the acid catalyst include, but are not limited to, mineral acids such as sulfuric acid, phosphoric acid, and perchloric acid; organic sulfonic acids such as p-toluenesulfonic acid and p-toluenesulfonic acid monohydrate; and carboxylic acids such as formic acid and oxalic acid. The amount of the acid catalyst cannot be generally specified because it is determined appropriately depending on the type of acid used, etc., but is usually determined appropriately in the range of 0.001 to 10,000 parts by mass per 100 parts by mass of the phenolic compound.

[0028] The condensation reaction can be carried out without a solvent if either the raw material compounds or the acid catalyst used are liquid, but is usually carried out using a solvent. The solvent is not particularly limited as long as it does not inhibit the reaction, but typically includes ether compounds, ether ester compounds, and the like. Examples of ether compounds include cyclic ether compounds such as tetrahydrofuran and dioxane. Examples of ether ester compounds include methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monomethyl ether propionate, propylene glycol monoethyl ether propionate, and propylene glycol monopropyl ether propionate.

[0029] The reaction temperature is usually appropriately set within the range of 40° C. to 200° C. The reaction time cannot be generally defined as it varies depending on the reaction temperature, but is usually appropriately set within the range of 30 minutes to 50 hours.

[0030] After the reaction is complete, if necessary, purification and isolation are carried out according to a standard method, and the resulting phenols are used for preparing a composition for forming a resist underlayer film. A person skilled in the art would be able to determine the production conditions of the phenols without undue burden based on the above explanation and common technical knowledge, and would therefore be able to produce the phenols.

[0031] <<Polyhydroxystyrenes>> Polyhydroxystyrenes include polyhydroxystyrene and polyhydroxystyrene derivatives.

[0032] Examples of polyhydroxystyrene or polyhydroxystyrene derivatives include poly-o-hydroxystyrene, poly-m-hydroxystyrene, poly-p-hydroxystyrene, poly-α-methyl-o-hydroxystyrene, poly-α-methyl-m-hydroxystyrene, and poly-α-methyl-p-hydroxystyrene.

[0033] The polyhydroxystyrene or polyhydroxystyrene derivative may be a homopolymer of hydroxystyrene which may have a substituent, or a copolymer obtained by copolymerizing hydroxystyrene which may have a substituent with another compound, such as (meth)acrylic acid or a (meth)acrylic acid derivative described below, acrylonitrile, methacrylonitrile, or a styrene derivative such as styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, p-methoxystyrene, or p-chlorostyrene.

[0034] Polyhydroxystyrenes are obtained by polymerizing hydroxystyrene which may have a substituent, and preferably have a structural unit represented by the following formula (2), for example.

[0035] (In formula (2), R represents a halogen atom, a carboxy group, a nitro group, a cyano group, a methylenedioxy group, an acetoxy group, a methylthio group, an amino group, or an alkoxy group having 1 to 9 carbon atoms. n represents an integer of 0 to 4. When n is 2 or more, the n Rs may be the same or different.)

[0036] In this specification, halogen atoms include fluorine atoms, chlorine atoms, bromine atoms and iodine atoms.

[0037] In this specification, examples of an alkoxy group having 1 to 9 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentyloxy group, a 2-methyl-n-pentyloxy group, and a 3-methyl-n-pentyloxy group. , 4-methyl-n-pentyloxy group, 1,1-dimethyl-n-butoxy group, 1,2-dimethyl-n-butoxy group, 1,3-dimethyl-n-butoxy group, 2,2-dimethyl-n-butoxy group, 2,3-dimethyl-n-butoxy group, 3,3-dimethyl-n-butoxy group, 1-ethyl-n-butoxy group, 2-ethyl-n-butoxy group, 1,1,2-trimethyl-n-propoxy group, 1,2,2-trimethyl-n-propoxy group, 1-ethyl-1-methyl-n-propoxy group, 1-ethyl-2-methyl-n-propoxy group, n-heptyloxy group, n-octyloxy group and n-nonyloxy group.

[0038] Examples of the (meth)acrylic acid derivative as a copolymerization component include (meth)acrylic acid alkyl esters such as (meth)acrylic acid methyl ester, (meth)acrylic acid ethyl ester, (meth)acrylic acid propyl ester, (meth)acrylic acid butyl ester, (meth)acrylic acid pentyl ester, (meth)acrylic acid hexyl ester, (meth)acrylic acid heptyl ester, (meth)acrylic acid octyl ester, (meth)acrylic acid 2-ethylhexyl ester, (meth)acrylic acid nonyl ester, (meth)acrylic acid decyl ester, (meth)acrylic acid undecyl ester, (meth)acrylic acid dodecyl ester, (meth)acrylic acid trifluoroethyl ester, and (meth)acrylic acid tetrafluoropropyl ester; acrylamides such as diacetone acrylamide; (meth)acrylic acid tetrahydrofurfuryl ester, (meth)acrylic acid dialkylaminoethyl ester, and (meth)acrylic acid glycidyl ester.

[0039] <<Polyhydroxyvinylnaphthalenes>> Polyhydroxyvinylnaphthalenes include polyhydroxyvinylnaphthalene and polyhydroxyvinylnaphthalene derivatives.

[0040] The polyhydroxyvinylnaphthalene or polyhydroxyvinylnaphthalene derivative may be a homopolymer of hydroxyvinylnaphthalene which may have a substituent, or a copolymer obtained by copolymerizing hydroxyvinylnaphthalene which may have a substituent with another compound, such as (meth)acrylic acid or the (meth)acrylic acid derivatives described above, acrylonitrile, methacrylonitrile, or a styrene derivative such as styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, p-methoxystyrene, or p-chlorostyrene.

[0041] Polyhydroxyvinylnaphthalenes are obtained by polymerizing hydroxyvinylnaphthalene which may have a substituent, and preferably have a structural unit represented by the following formula (3), for example.

[0042] (In formula (3), R represents a halogen atom, a carboxy group, a nitro group, a cyano group, a methylenedioxy group, an acetoxy group, a methylthio group, an amino group, or an alkoxy group having 1 to 9 carbon atoms. n represents an integer of 0 to 6. When n is 2 or more, the n Rs may be the same or different.)

[0043] <<Low Molecular Weight Compound (A-1)>> The low molecular weight compound (A-1) is not particularly limited as long as it is a compound containing two or more phenolic hydroxy groups and having a molecular weight of 5,000 or less.

[0044] The number of phenolic hydroxy groups in the low molecular weight compound (A-1) is 2 or more, preferably 3 to 50, and more preferably 4 to 30.

[0045] The molecular weight of the low molecular weight compound (A-1) is 5,000 or less, preferably 200 to 4,000, and more preferably 300 to 3,000.

[0046] As the low molecular weight compound (A-1), from the viewpoint of suitably obtaining the effects of the present invention, a compound represented by the following formula (A-1-1), a compound represented by the following formula (A-1-2), a compound represented by the following formula (A-1-3), or a compound represented by the following formula (A-1-4) is preferred.

[0047] <<<Compound represented by formula (A-1-1)>>> (In formula (A-1-1), Z 1 represents a p-valent group, and p represents an integer of 2 to 4. Each X independently represents an organic group represented by the following formula (X):

[0048] (In formula (X), R 1 represents an alkylene group having 1 to 4 carbon atoms. T represents a single bond or an (s+1)-valent hydrocarbon group having 1 to 8 carbon atoms. A 1 ~A 3 each independently represents a hydrogen atom, a methyl group, or an ethyl group. k represents 0 or 1. m represents an integer of 0 to 4. n represents 0 or 1. q represents 0 or 1. s represents 1 or 2. * represents Z in formula (A-1-1). 1However, when T is a single bond, n and q cannot be 1 at the same time.)

[0049] Z in formula (A-1-1) 1 Although there are no particular limitations on the group Z, as long as it is a p-valent group, it is preferably represented by the following formula (Z-1). (In formula (Z-1), Q 3 represents the following formula (Z-1-1), formula (Z-1-2), formula (Z-1-3), or formula (Z-1-4). * represents the bond to X in formula (A-1-1). (In formula (Z-1-1), formula (Z-1-2), formula (Z-1-3), and formula (Z-1-4), R 11 ~R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group, or a phenyl group, and the phenyl group may be substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms. * represents a bond. *1 represents a bond bonded to the nitrogen atom in formula (Z-1). *2 represents a bond bonded to a carbon atom in formula (Z-1). *3 represents the bond to X in formula (A-1-1).

[0050] In formula (Z-1), Q 3 represents formula (Z-1-1), R in formula (Z-1-1) 11 and R 12 are each preferably an alkyl group having 1 to 10 carbon atoms.

[0051] In formula (Z-1), Q 3 represents formula (Z-1-2), R in formula (Z-1-2) 13 and R 14 are each preferably an alkyl group having 1 to 10 carbon atoms.

[0052] Q in formula (Z-1) 3 is preferably represented by formula (Z-1-3) or formula (Z-1-4). 15 is preferably an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, or an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, and more preferably an alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms.

[0053] The compound represented by formula (A-1-1) can be obtained, for example, by reacting a compound represented by the following formulas (a) to (w) and (ac) to (aj) with a compound represented by the following formula (Y) by a known method, but is not limited thereto.

[0054]

[0055] (In formula (Y), m represents an integer of 0 to 4, and k represents 0 or 1.)

[0056] Examples of the compound represented by formula (Y) include the following compounds.

[0057] Examples of the compound represented by formula (A-1-1) include the following compounds:

[0058] <<<Compound represented by formula (A-1-2)>>> (In formula (A-1-2), Ar 1 ~Ar 3 each independently represents an aromatic hydrocarbon ring; n1 to n3 each independently represent an integer of 1 to 4.

[0059] Examples of aromatic hydrocarbon rings include a benzene ring, a naphthalene ring, an anthracene ring, etc. Among these, a benzene ring and a naphthalene ring are preferred.

[0060] n1 to n3 are preferably 1.

[0061] Examples of the compound represented by formula (A-1-2) include the following compounds:

[0062] The compound represented by formula (A-1-2) can be synthesized, for example, by reacting phloroglucinol represented by the following formula (A-1-2A) with a compound represented by the following formula (A-1-2B). In the reaction, a protecting group for the hydroxy group is used and deprotected as necessary. (In formula (A-1-2B), Ar represents an aromatic hydrocarbon ring. R represents a hydrogen atom or a protecting group for a hydroxy group. n1 represents an integer of 1 to 4.)

[0063] Examples of aromatic hydrocarbon rings include a benzene ring, a naphthalene ring, an anthracene ring, etc. Among these, a benzene ring and a naphthalene ring are preferred.

[0064] Examples of the compound represented by formula (A-1-2B) include tert-butoxystyrene and 2-tert-butoxyvinylnaphthalene.

[0065] <<<Compound represented by formula (A-1-3)>>> (In formula (A-1-3), T represents a single bond, an alkylene group having 1 to 10 carbon atoms, or an arylene group having 6 to 40 carbon atoms. X 1 and X 2 R each independently represents a hydrogen atom or a methyl group. 5 ~R 8 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms; and n1 to n4 each independently represent an integer of 0 to 3.

[0066] Examples of the compound represented by formula (A-1-3) include the following compounds: The compound represented by formula (A-1-3) may be a commercially available product, such as TEP-TPA (manufactured by Asahi Organic Chemicals Co., Ltd.).

[0067] <<<Compound Represented by Formula (A-1-4)>>> The compound represented by formula (A-1-4) is tannic acid.

[0068] The content of compound (A) in the composition for forming a resist underlayer film is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably 40% by mass to 99% by mass, more preferably 45% by mass to 95% by mass, and particularly preferably 50% by mass to 90% by mass, based on the film-constituting components. In the present invention, the film-constituting components refer to components other than the solvent contained in the composition.

[0069] <Solvent (B)> The solvent (B) is not particularly limited and may be water or an organic solvent. Examples of the organic solvent include alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers.

[0070] Examples of the alkylene group of the alkylene glycol monoalkyl ether include alkylene groups having 2 to 4 carbon atoms. Examples of the alkyl group of the alkylene glycol monoalkyl ether include alkyl groups having 1 to 4 carbon atoms. Examples of the number of carbon atoms of the alkylene glycol monoalkyl ether include 3 to 8. Examples of the alkylene glycol monoalkyl ether include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether.

[0071] Examples of the alkylene group of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include alkylene groups having 2 to 4 carbon atoms. Examples of the alkyl group of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include alkyl groups having 1 to 4 carbon atoms. Examples of the monocarboxylic acid of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include saturated monocarboxylic acids having 2 to 4 carbon atoms. Examples of saturated monocarboxylic acids having 2 to 4 carbon atoms include acetic acid, propionic acid, and butyric acid. Examples of the number of carbon atoms of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include those having 5 to 10 carbon atoms. Examples of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, and propylene glycol propyl ether acetate.

[0072] Other organic solvents include, for example, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0073] Among these solvents (B), alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers are preferred.

[0074] These solvents (B) may be used alone or in combination of two or more.

[0075] The mass proportion of the organic solvent in the solvent (B) is not particularly limited, but is preferably 50 mass % to 100 mass %.

[0076] The content of the solvent (B) in the composition for forming a resist underlayer film is not particularly limited, but is preferably 50% by mass to 99.99% by mass, more preferably 75% by mass to 99.95% by mass, and particularly preferably 90% by mass to 99.9% by mass.

[0077] <Crosslinking Agent (C)> The crosslinking agent (C) is not particularly limited. The crosslinking agent (C) has a structure different from that of the compound (A).

[0078] The crosslinking agent (C) is preferably an aminoplast crosslinking agent or a phenoplast crosslinking agent. The aminoplast crosslinking agent is an addition condensation product of a compound having an amino group, such as melamine or guanamine, with formaldehyde. The phenoplast crosslinking agent is an addition condensation product of a compound having a phenolic hydroxy group with formaldehyde.

[0079] Examples of the crosslinking agent (C) include compounds having two or more of the following structures. (In the structure, R 101 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxyalkyl group having 2 to 6 carbon atoms. * represents a bond.) The bond is bonded to, for example, a nitrogen atom or a carbon atom constituting an aromatic hydrocarbon ring.

[0080] R 101 is preferably a hydrogen atom, a methyl group, an ethyl group or a group represented by the following structure. (In the structure, R 102 represents a hydrogen atom, a methyl group, or an ethyl group. * represents a bond.

[0081] The crosslinking agent (C) is preferably a melamine compound, a guanamine compound, a glycoluril compound, a urea compound, or a compound having a phenolic hydroxy group, which may be used alone or in combination of two or more.

[0082] Examples of the melamine compound include hexamethylol melamine, hexamethoxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine have been methoxymethylated, or a mixture thereof, hexamethoxyethyl melamine, hexaacyloxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine have been acyloxymethylated, or a mixture thereof.

[0083] Examples of the guanamine compound include tetramethylolguanamine, tetramethoxymethylguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are methoxymethylated, or a mixture thereof; tetramethoxyethylguanamine, tetraacyloxyguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are acyloxymethylated, or a mixture thereof; and the like.

[0084] Examples of glycoluril compounds include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, compounds in which one to four methylol groups of tetramethylol glycoluril are methoxymethylated or mixtures thereof, and compounds in which one to four methylol groups of tetramethylol glycoluril are acyloxymethylated or mixtures thereof.

[0085] The glycoluril compound may be, for example, a glycoluril derivative represented by the following formula (1E). (In formula (1E), four R 1 each independently represents a methyl group or an ethyl group, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group.

[0086] Examples of the glycoluril derivative represented by the formula (1E) include compounds represented by the following formulas (1E-1) to (1E-6).

[0087] The glycoluril derivative represented by formula (1E) can be obtained, for example, by reacting a glycoluril derivative represented by the following formula (2E) with at least one compound represented by the following formula (3d).

[0088] (In formula (2E), R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group; R 4 each independently represents an alkyl group having 1 to 4 carbon atoms.

[0089] (In formula (3d), R 1 represents a methyl group or an ethyl group.

[0090] Examples of glycoluril derivatives represented by formula (2E) include compounds represented by formulas (2E-1) to (2E-4) below. Furthermore, examples of compounds represented by formula (3d) include compounds represented by formulas (3d-1) and (3d-2) below.

[0091] Examples of the urea compound include tetramethylol urea, tetramethoxymethyl urea, tetramethylol urea compounds in which one to four methylol groups are methoxymethylated, or mixtures thereof, and tetramethoxyethyl urea.

[0092] Examples of the compound having a phenolic hydroxy group include compounds represented by the following formula (G-1) or (G-2). (In formula (G-1) and formula (G-2), Q 1 represents a single bond or a monovalent organic group. 1 and R 4 R represents an alkyl group having 2 to 10 carbon atoms, or an alkyl group having 2 to 10 carbon atoms and an alkoxy group having 1 to 10 carbon atoms. 2 and R 5 R represents a hydrogen atom or a methyl group. 3 and R 6n represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. 1 is 1≦n 1 an integer ≦3, n 2 is 2≦n 2 n is an integer ≦5 3 is 0≦n 3 an integer ≦3, n 4 is 0≦n 4 an integer ≦3, 3≦(n 1 +n 2 +n 3 +n 4 ) represents an integer ≦6. 5 is 1≦n 5 an integer ≦3, n 6 is 1≦n 6 n is an integer ≦4 7 is 0≦n 7 an integer ≦3, n 8 is 0≦n 8 an integer ≦3, 2≦(n 5 +n 6 +n 7 +n 8 ) represents an integer of ≦5. m1 represents an integer of 2 to 10.

[0093] Examples of compounds having a phenolic hydroxy group include compounds represented by the following formula (G-3) or formula (G-4): The compound represented by formula (G-1) or formula (G-2) may be obtained by reacting a compound represented by the following formula (G-3) or formula (G-4) with a hydroxyl group-containing ether compound or an alcohol having 2 to 10 carbon atoms. (In formula (G-3) and formula (G-4), Q 2 represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 R represents a hydrogen atom or a methyl group. 7 and R 10 n represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. 9 is 1≦n 9 an integer ≦3, n 10 is 2≦n 10 an integer ≦5, n11 is 0≦n 11 an integer ≦3, n 12 is 0≦n 12 an integer ≦3, 3≦(n 9 +n 10 +n 11 +n 12 ) represents an integer ≦6. 13 is 1≦n 13 an integer ≦3, n 14 is 1≦n 14 n is an integer ≦4 15 is 0≦n 15 an integer ≦3, n 16 is 0≦n 16 an integer ≦3, 2≦(n 13 +n 14 +n 15 +n 16 ) represents an integer of ≦5. m2 represents an integer of 2 to 10. 2 In the above, the m2-valent organic group includes, for example, an m2-valent organic group having 1 to 4 carbon atoms.

[0094] Examples of the compound represented by formula (G-1) or formula (G-2) include the following compounds:

[0095] Examples of the compound represented by formula (G-3) or formula (G-4) include the following compounds: (In the above formula, Me represents a methyl group.)

[0096] The above compound is available as a product of Asahi Organic Chemicals Co., Ltd. and Honshu Chemical Industry Co., Ltd. An example of the product is TMOM-BP, a product name of Asahi Organic Chemicals Co., Ltd.

[0097] Among these, glycoluril compounds are preferred, specifically tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, tetramethylol glycoluril compounds in which one to four methylol groups have been methoxymethylated or mixtures thereof, and tetramethylol glycoluril compounds in which one to four methylol groups have been acyloxymethylated or mixtures thereof, with tetramethoxymethyl glycoluril being more preferred.

[0098] The molecular weight of the crosslinking agent (C) is not particularly limited, but is preferably 500 or less.

[0099] The content of the crosslinking agent (C) in the composition for forming a resist underlayer film is not particularly limited, but is, for example, 1% by mass to 70% by mass, and preferably 5% by mass to 60% by mass, relative to the compound (A).

[0100] <Curing Catalyst (D)> The curing catalyst (D) contained as an optional component in the composition for forming a resist underlayer film may be either a thermal acid generator or a photoacid generator, but it is preferable to use a thermal acid generator. Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium-p-toluenesulfonate (pyridinium-p-toluenesulfonic acid), pyridinium phenolsulfonic acid, pyridinium-p-hydroxybenzenesulfonic acid (pyridinium p-phenolsulfonate salt), pyridinium-trifluoromethanesulfonic acid, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid, N-methylmorpholine-p-toluenesulfonic acid, N-methylmorpholine-p-hydroxybenzenesulfonic acid, and N-methylmorpholine-5-sulfosalicylic acid.

[0101] Examples of the photoacid generator include an onium salt compound, a sulfonimide compound, and a disulfonyldiazomethane compound.

[0102] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-normal butanesulfonate, diphenyliodonium perfluoro-normal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-normal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.

[0103] Examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.

[0104] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0105] The curing catalyst (D) may be used alone or in combination of two or more.

[0106] When the curing catalyst (D) is used, the content of the curing catalyst (D) relative to the crosslinking agent (C) is, for example, 0.1% by mass to 50% by mass, and preferably 1% by mass to 30% by mass.

[0107] <Other Components> A surfactant may be further added to the composition for forming a resist underlayer film in order to prevent pinholes, striations, and the like from occurring and to further improve the coatability against surface irregularities.

[0108] Examples of surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate; nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorine-based surfactants such as Eftop EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, and R-30 (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by AGC Inc.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants to be added is usually 2.0 mass % or less, and preferably 1.0 mass % or less, based on the total solid content of the composition for forming a resist underlayer film. These surfactants may be added alone or in combination of two or more.

[0109] The solid content of the composition for forming a resist underlayer film of the present invention, that is, the content of components excluding the solvent, is, for example, 0.01% by mass to 10% by mass.

[0110] The composition for forming a resist underlayer film of the present invention is preferably a composition for forming a resist underlayer film for EUV (extreme ultraviolet) or electron beam lithography.

[0111] For example, the composition for forming a resist underlayer film does not contain a light absorber. Also, for example, the composition for forming a resist underlayer film does not contain a polymer having an —NH—C(═S)—O— bond. Also, for example, the composition for forming a resist underlayer film does not contain a polymer having a structural unit represented by the following formula (Z-1):

[0112] Furthermore, for example, the composition for forming a resist underlayer film does not contain a polymer having a structural unit represented by the following formula (Z-2). (In formula (Z-2), each R independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.)

[0113] (Resist Underlayer Film) The resist underlayer of the present invention is a cured product of the composition for forming a resist underlayer film described above. The resist underlayer film can be produced, for example, by applying the composition for forming a resist underlayer film described above onto a semiconductor substrate and baking it.

[0114] In the resist underlayer film, the atomic percentage of oxygen in the phenolic hydroxy groups is, for example, 2.00% or more, preferably 2.00% or more and 30.00% or less, and more preferably 3.00% or more and 20.00% or less. The atomic percentage of oxygen in the phenolic hydroxy groups in the resist underlayer film can be determined, for example, by the following method.

[0115] The silicon wafer on which the resist underlayer film is formed is cut to a size of approximately 0.5 x 1 cm and dried under reduced pressure for 20 hours or more. Then, the wafer is sealed in a 6.0 x 7.5 cm weighing bottle with 3 ml of trifluoroacetic anhydride, and the hydrogen atoms of the phenolic hydroxy groups are substituted with trifluoroacetyl groups by gas-phase chemical modification at 25°C. The reaction time is determined based on the time required for each composition to reach reaction equilibrium. Further, unreacted trifluoroacetic anhydride and by-product trifluoroacetic acid are removed by drying under reduced pressure for 20 hours or more. The number of each atom constituting the film (excluding hydrogen) is then measured using X-ray photoelectron spectroscopy (Quanterar SXM) using an AlKa radiation source. The atomic percentage of oxygen in the phenolic hydroxy groups in the resist underlayer film (R OH [atom %]) is calculated. F: number of fluorine atoms A: total number of atoms (excluding hydrogen atoms) Note that, if the resist underlayer film contains fluorine atoms before being subjected to the vapor phase chemical modification method, the fluorine atoms are not included in F in the formula.

[0116] Examples of semiconductor substrates onto which the resist underlayer film-forming composition can be applied include silicon wafers, germanium wafers, and wafers of compound semiconductors such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.

[0117] When a semiconductor substrate having an inorganic film formed on its surface is used, the inorganic film can be formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin coating (spin-on glass: SOG). Examples of the inorganic film include a polysilicon film, a silicon oxide film, a silicon nitride film, a BPSG (Boro-Phospho Silicate Glass) film, a titanium nitride film, a titanium nitride oxide film, a tungsten film, a gallium nitride film, and a gallium arsenide film.

[0118] The resist underlayer film-forming composition of the present invention is applied to such a semiconductor substrate by a suitable application method such as a spinner or coater. The composition is then baked using a heating means such as a hot plate to form a resist underlayer film. The baking conditions are appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 to 60 minutes. A baking temperature of 120°C to 350°C and a baking time of 0.5 to 30 minutes are preferred, and a baking temperature of 150°C to 300°C and a baking time of 0.8 to 10 minutes are more preferred.

[0119] The thickness of the resist underlayer film may be, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.004 μm (4 nm) to 0.05 μm (50 nm), 0.005 μm (5 nm) to 0.05 μm (5 0 nm), 0.003 μm (3 nm) to 0.03 μm (30 nm), 0.003 μm (3 nm) to 0.02 μm (20 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.003 μm (3 nm) to 0.01 μm (10 nm), 0.005 μm (5 nm) to 0.01 μm (10 nm), 0.003 μm (3 nm) to 0.006 μm (6 nm), or 0.005 μm (5 nm).

[0120] The thickness of the resist underlayer film is preferably 2 nm or more and 20 nm or less, from the viewpoint of suitably obtaining the effects of the present invention.

[0121] The method for measuring the film thickness of the resist underlayer film in this specification is as follows: Measurement device name: Ellipso film thickness measurement device RE-3100 (SCREEN Corporation) SWE (single wavelength ellipsometer) mode Arithmetic mean of 8 points (for example, measuring 8 points at 1 cm intervals in the X direction of the wafer)

[0122] (Laminate) The laminate of the present invention includes a semiconductor substrate and the resist underlayer film of the present invention. Examples of the semiconductor substrate include the semiconductor substrates described above. The resist underlayer film is disposed on the semiconductor substrate, for example.

[0123] (Method for manufacturing a semiconductor element, method for forming a pattern) The method for manufacturing a semiconductor element of the present invention includes at least the following steps: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film of the present invention, and forming a resist film on the resist underlayer film.

[0124] The pattern forming method of the present invention includes at least the following steps: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film of the present invention, forming a resist film on the resist underlayer film, irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern, and etching the resist underlayer film using the resist pattern as a mask.

[0125] Typically, a resist layer is formed on the resist underlayer film. The film thickness of the resist layer is, for example, 3,000 nm or less, 2,000 nm or less, 1,800 nm or less, 1,500 nm or less, or 1,000 nm or less. The lower limit is 100 nm, 80 nm, 50 nm, 30 nm, 20 nm, or 10 nm.

[0126] The resist film formed on the resist underlayer film by a known method (e.g., coating and baking a resist composition) is not particularly limited as long as it is responsive to light or electron beam (EB) irradiation. Both negative and positive photoresists can be used. In this specification, resists responsive to EB are also referred to as photoresists. Examples of photoresists include positive photoresists composed of a novolak resin and a 1,2-naphthoquinone diazide sulfonic acid ester; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate and a photoacid generator; chemically amplified photoresists composed of a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate, a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator; and resists containing metal elements. Examples of such photoresists include V146G (trade name) manufactured by JSR Corporation, APEX-E (trade name) manufactured by Shipley Co., Ltd., PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 (trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Further examples include fluorine-containing polymer photoresists such as those described in Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000).

[0127] Also, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO201 9 / 172054, WO2019 / 021975, WO2018 / 230334, WO2018 / 194123, JP 2018-180525, WO2018 / 190088, JP 2018-070596, JP 2018-028090, JP 2016-153409, JP 2016-130240, JP 2016-108325, JP 2016-047920, JP 2016-035570, JP 2016-035567, JP 2016-035565, JP 2019-101417, JP 2019-117373, JP 2019-052294, JP 2019-008280, JP 2019-008279, JP 2019-003176, JP 2019-003175, JP 2018-197853, JP 2019-191298, JP 2019-061217, JP 2018-045152, JP 2018-022039, JP 2016-090441, JP 2015-10878, JP 2012-168279, JP 2012-022261, JP 2012-022258, JP 2011-043749, JP 2010-18 1857, JP 2010-128369, WO2018 / 031896, JP 2019-113855, WO2017 / 156388, WO2017 / 066319, JP 2018-41099, WO2016 / 065120, WO2015 / 026482, JP 2016-29498, JP 2011-253185, etc., radiation-sensitive resin compositions, so-called resist compositions such as high-resolution patterning compositions based on organometallic solutions, and metal-containing resist compositions can be used, but are not limited to these.

[0128] Examples of the resist composition include the following compositions.

[0129] An actinic ray-sensitive or radiation-sensitive resin composition comprising: Resin A having a repeating unit having an acid-decomposable group in which a polar group is protected with a protecting group that is cleaved by the action of an acid; and a compound represented by the following general formula (121):

[0130] In the general formula (121), m represents an integer of 1 to 6. 1 and R 2 each independently represents a fluorine atom or a perfluoroalkyl group. 1 is -O-, -S-, -COO-, -SO 2 - or -SO 3 - represents. 2 represents an alkylene group which may have a substituent or a single bond. 1 represents a cyclic organic group which may have a substituent. + represents a cation.

[0131] A metal-containing film-forming composition for extreme ultraviolet or electron beam lithography, comprising a compound having a metal-oxygen covalent bond and a solvent, wherein the metal element constituting the compound belongs to Periods 3 to 7 of Groups 3 to 15 of the periodic table.

[0132] A radiation-sensitive resin composition comprising: a polymer having a first structural unit represented by the following formula (31) and a second structural unit represented by the following formula (32) containing an acid-dissociable group; and an acid generator.

[0133] In formula (31), Ar is a group obtained by removing (n+1) hydrogen atoms from an arene having 6 to 20 carbon atoms. 1 is a hydroxy group, a sulfanyl group, or a monovalent organic group having 1 to 20 carbon atoms. n is an integer of 0 to 11. When n is 2 or more, multiple R 1 are the same or different. 2 is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. 3 is a monovalent group having 1 to 20 carbon atoms containing the above acid-dissociable group. Z is a single bond, an oxygen atom, or a sulfur atom. R 4is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group.

[0134] A resist composition comprising: a resin (A1) containing a structural unit having a cyclic carbonate structure, a structural unit represented by the following formula, and a structural unit having an acid labile group; and an acid generator.

[0135] [In the formula, R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom; X 1 represents a single bond, —CO—O—*, or —CO—NR 4 -*, * represents a bond to -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from the group consisting of a hydroxy group and a carboxyl group.]

[0136] Examples of the resist film include the following.

[0137] A resist film comprising a base resin comprising a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit that generates an acid bonded to a polymer main chain upon exposure:

[0138] (In formula (a1) and formula (a2), R A are each independently a hydrogen atom or a methyl group. 1 and R 2 are each independently a tertiary alkyl group having 4 to 6 carbon atoms. 3 are each independently a fluorine atom or a methyl group, and m is an integer of 0 to 4. 1 X is a single bond, a phenylene group, or a naphthylene group, or a linking group having 1 to 12 carbon atoms and containing at least one selected from an ester bond, a lactone ring, a phenylene group, and a naphthylene group. 2 is a single bond, an ester bond, or an amide bond.

[0139] Examples of resist materials include the following:

[0140] A resist material comprising a polymer having a repeating unit represented by the following formula (b1) or (b2):

[0141] (In formula (b1) and formula (b2), R A is a hydrogen atom or a methyl group. 1 is a single bond or an ester group. 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group, an ester group or a lactone ring-containing group; and X 2 At least one hydrogen atom contained in X is substituted with a bromine atom. 3 Rf is a single bond, an ether group, an ester group, or a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group. 1 ~Rf 4 are each independently a hydrogen atom, a fluorine atom, or a trifluoromethyl group, but at least one is a fluorine atom or a trifluoromethyl group. 1 and Rf 2 may combine to form a carbonyl group. 1 ~R 5 are each independently a linear, branched, or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched, or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an aryloxyalkyl group having 7 to 12 carbon atoms, in which some or all of the hydrogen atoms may be substituted with a hydroxy group, a carboxy group, a halogen atom, an oxo group, a cyano group, an amide group, a nitro group, a sultone group, a sulfone group, or a sulfonium salt-containing group, and in which some of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group, or a sulfonate ester group. 1 and R 2may be bonded to form a ring together with the sulfur atom to which they are attached.

[0142] A resist material comprising a base resin containing a polymer containing a repeating unit represented by the following formula (a):

[0143] (In formula (a), R A is a hydrogen atom or a methyl group. 1 is a hydrogen atom or an acid labile group. 2 is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine. 1 X is a single bond, a phenylene group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring. 2 is -O-, -O-CH 2 - or -NH-. m is an integer of 1 to 4. u is an integer of 0 to 3. However, m+u is an integer of 1 to 4.

[0144] A resist composition that generates an acid upon exposure, and whose solubility in a developer changes due to the action of the acid, comprising: a base component (A) whose solubility in a developer changes due to the action of the acid; and a fluorine additive component (F) that exhibits decomposition in an alkaline developer, wherein the fluorine additive component (F) comprises a fluororesin component (F1) that has a structural unit (f1) that includes a base dissociable group, and a structural unit (f2) that includes a group represented by the following general formula (f2-r-1):

[0145] [In formula (f2-r-1), Rf 21 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxy group, a hydroxyalkyl group, or a cyano group. n" is an integer of 0 to 2. * is a bond.

[0146] The structural unit (f1) includes a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2).

[0147] [In formulas (f1-1) and (f1-2), each R is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. X is a divalent linking group that does not have an acid-dissociable site. A aryl represents a divalent aromatic cyclic group which may have a substituent. 01 is a single bond or a divalent linking group. 2 are each independently an organic group having a fluorine atom.

[0148] Coatings, coating solutions, and coating compositions include, for example:

[0149] A coating comprising a metal oxo-hydroxo network having organic ligands with metal carbon and / or metal carboxylate bonds.

[0150] Inorganic oxo / hydroxo-based compositions.

[0151] a coating solution comprising an organic solvent; a first organometallic composition having the formula R z SnO (2-(z/2)-(x/2)) (OH) x (where 0<z≦2 and 0<(z+x)≦4), formula R′ n SnX 4-n wherein n=1 or 2, or mixtures thereof, where R and R′ are independently hydrocarbyl groups having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn, or a combination thereof; and a hydrolyzable metal compound having the formula MX′ v wherein M is a metal selected from groups 2 to 16 of the periodic table of the elements, v is a number from 2 to 6, and X' is a ligand having a hydrolyzable M-X bond or a combination thereof.

[0152] an organic solvent and a solution of the formula RSnO (3/2-x/2) (OH) xand a first organometallic compound of the formula: wherein 0<x<3, wherein the solution contains from about 0.0025M to about 1.5M tin, and R is an alkyl or cycloalkyl group having from 3 to 31 carbon atoms, the alkyl or cycloalkyl group being bonded to the tin at a secondary or tertiary carbon atom.

[0153] An aqueous inorganic patterning precursor solution comprising a mixture of water, metal suboxide cations, polyatomic inorganic anions, and radiation-sensitive ligands comprising peroxide groups.

[0154] Irradiation with light or electron beams is carried out, for example, through a mask (reticle) for forming a predetermined pattern. For example, i-line, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet), or EB (electron beam) can be used. The composition for forming a resist underlayer film of the present invention is preferably applied for EB (electron beam) or EUV (extreme ultraviolet: 13.5 nm) irradiation, more preferably for EUV (extreme ultraviolet) exposure. The irradiation energy of the electron beam and the exposure dose of light are not particularly limited.

[0155] After irradiation with light or electron beams and before development, baking (PEB: Post Exposure Bake) may be performed. The baking temperature is not particularly limited, but is preferably 60° C. to 150° C., more preferably 70° C. to 120° C., and particularly preferably 75° C. to 110° C. The baking time is not particularly limited, but is preferably 1 second to 10 minutes, more preferably 10 seconds to 5 minutes, and particularly preferably 30 seconds to 3 minutes.

[0156] For example, an alkaline developer is used for development. The development temperature can be, for example, 5°C to 50°C. The development time can be, for example, 10 seconds to 300 seconds. Examples of alkaline developers that can be used include aqueous solutions of alkalis such as inorganic alkalis (e.g., sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia); primary amines (e.g., ethylamine and n-propylamine); secondary amines (e.g., diethylamine and di-n-butylamine); tertiary amines (e.g., triethylamine and methyldiethylamine); alcohol amines (e.g., dimethylethanolamine and triethanolamine); quaternary ammonium salts (e.g., tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline); and cyclic amines (e.g., pyrrole and piperidine). Furthermore, the aqueous solutions of the alkalis can be used by adding an appropriate amount of alcohols (e.g., isopropyl alcohol) or a nonionic surfactant. Among these, preferred developers are aqueous solutions of quaternary ammonium salts, more preferably aqueous solutions of tetramethylammonium hydroxide and choline. Furthermore, surfactants and the like can also be added to these developers. Alternatively, development may be carried out with an organic solvent such as butyl acetate instead of an alkaline developer, and the portions of the photoresist where the alkaline dissolution rate is not improved may be developed.

[0157] Next, the resist underlayer film is etched using the formed resist pattern as a mask. The etching may be dry etching or wet etching, but dry etching is preferred. If the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed. If the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed. Thereafter, the semiconductor substrate is processed by a known method (e.g., dry etching), thereby manufacturing a semiconductor device.

[0158] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples.

[0159] The weight-average molecular weights of the polymers shown in Synthesis Examples 1 to 7 and Comparative Synthesis Examples 1 to 3 below in this specification are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). A GPC device manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions were as follows: GPC column: TSKgel Super-Multipore HZ-N (2 columns) Column temperature: 40°C Solvent: tetrahydrofuran (THF) Flow rate: 0.35 ml / min Standard sample: polystyrene (manufactured by Tosoh Corporation)

[0160] Synthesis Example 1 Under nitrogen, 15.00 g of 2,2'-biphenol (manufactured by Tokyo Chemical Industry Co., Ltd.), 8.55 g of 1-benzaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.77 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to a reaction vessel, and 24.32 g of propylene glycol monomethyl ether acetate was further charged. The reaction vessel was purged with nitrogen, and then the reaction was carried out at 140°C for 3 hours. After cooling, the mixture was reprecipitated in methanol, and the resulting precipitate was filtered and dried in a vacuum dryer at 60°C for 12 hours to obtain the target polymer 1. GPC analysis showed that the resulting polymer 1 had a weight average molecular weight of 4,600 and a polydispersity of 2.3, calculated as standard polystyrene. The structure present in polymer 1 is shown in the following formula.

[0161]

[0162] Synthesis Example 2 Under nitrogen, 15.00 g of 2,2'-biphenol (manufactured by Tokyo Chemical Industry Co., Ltd.), 12.58 g of 1-naphthaldehyde (manufactured by Aldrich Chemical Co., Ltd.), and 1.94 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to a reaction vessel, and 29.52 g of propylene glycol monomethyl ether acetate was further charged. After the reaction vessel was purged with nitrogen, the reaction was carried out at 140°C for 3 hours. After cooling, the mixture was reprecipitated in methanol, and the resulting precipitate was filtered and dried in a vacuum dryer at 60°C for 12 hours to obtain the target polymer 2. GPC analysis showed that the resulting polymer 2 had a weight average molecular weight of 51,500 and a polydispersity of 29.6, calculated as standard polystyrene. The structure present in polymer 2 is shown in the following formula.

[0163]

[0164] Synthesis Example 3 Under nitrogen, a reaction vessel was charged with 25.00 g of 2,2'-biphenol (manufactured by Tokyo Chemical Industry Co., Ltd.), 10.48 g of 1-naphthaldehyde (manufactured by Aldrich Chemical Industry Co., Ltd.), 15.46 g of 1-pyrenecarboxaldehyde (manufactured by Tokyo Chemical Industry Co., Ltd.), and 3.87 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 54.81 g of propylene glycol monomethyl ether was further charged. The reaction vessel was purged with nitrogen, and then the reaction was carried out at 120°C for 24 hours. After cooling, the mixture was reprecipitated in methanol, and the resulting precipitate was filtered and dried in a vacuum dryer at 50°C for 10 hours to obtain the target polymer 3. GPC analysis showed that the resulting polymer 3 had a weight average molecular weight of 5,000 and a polydispersity of 4.8, calculated as standard polystyrene. The structure present in polymer 3 is shown in the following formula.

[0165]

[0166] Synthesis Example 4 4.00 g of 1,3,5-tris(2,3-epoxypropyl)isocyanuric acid (product name: TEPIC-SS, manufactured by Nissan Chemical Industries, Ltd.), 8.19 g of 3,7-dihydroxy-2-naphthoic acid (manufactured by Midori Chemical Industry Co., Ltd.), and 0.36 g of ethyltriphenylphosphonium bromide (manufactured by Hokko Chemical Industry Co., Ltd.) were added to 29.29 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. The atmosphere in the reaction vessel was replaced with nitrogen, and the reaction was carried out at 140°C for 24 hours to obtain a solution containing polymer 4. GPC analysis showed that the obtained polymer 4 had a weight average molecular weight of 1,000 and a dispersity of 4.8, calculated as standard polystyrene. The structure present in polymer 4 is shown in the following formula.

[0167]

[0168] Synthesis Example 5 Under nitrogen, 6.00 g of phloroglucinol (anhydrous) (manufactured by Tokyo Chemical Industry Co., Ltd.), 17.15 g of 4-tert-butoxystyrene (manufactured by Tokyo Chemical Industry Co., Ltd.), and 2.74 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to a reaction vessel, and 23.15 g of propylene glycol monomethyl ether was further charged, followed by a reaction at 140°C for 24 hours. After cooling, the mixture was reprecipitated in heptane, and the resulting precipitate was filtered and dried in a vacuum dryer at 60°C for 12 hours to obtain the target polymer 5. GPC analysis showed that the resulting polymer 5 had a weight average molecular weight of 1,300 and a dispersity of 1.6, calculated in terms of standard polystyrene. The structure present in polymer 5 is shown in the following formula.

[0169]

[0170] Synthesis Example 6 Under nitrogen, a reaction vessel was charged with 6.00 g of phloroglucinol (anhydrous) (manufactured by Tokyo Chemical Industry Co., Ltd.), 32.30 g of 2-tert-butoxy-6-vinylnaphthalene (product name: , manufactured by Tosoh Corporation), and 6.86 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 38.30 g of propylene glycol monomethyl ether was further charged, and the reaction was carried out at 140°C for 24 hours. After cooling, the mixture was reprecipitated in hexane, and the obtained precipitate was filtered and dried in a vacuum dryer at 60°C for 12 hours to obtain the target polymer 6. GPC analysis showed that the obtained polymer 6 had a weight average molecular weight of 970 and a dispersity of 1.7, calculated as standard polystyrene. The structure present in polymer 6 is shown in the following formula.

[0171]

[0172] Synthesis Example 7: 8.00 g of 2-tert-butoxy-6-vinylnaphthalene (product name: manufactured by Tosoh Corporation) and 0.48 g of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 19.79 g of propylene glycol monomethyl ether acetate (hereinafter abbreviated as PGMEA in this specification), and then added to 14.13 g of PGMEA in a reaction vessel heated and maintained at 140°C. The reaction was allowed to proceed for 3 hours to obtain a polymer solution. After cooling, the solution was reprecipitated in ultrapure water / methanol, and the obtained precipitate was filtered and dried in a vacuum dryer at 60°C for 12 hours to obtain a polymer. Furthermore, 38.51 g of propylene glycol monomethyl ether acetate and 2.22 g of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to 7.41 g of the obtained polymer, and the mixture was allowed to react at 80°C for 7 hours. After cooling, the mixture was reprecipitated in ultrapure water / methanol, and the resulting precipitate was filtered and dried in a vacuum dryer at 40°C for 24 hours to obtain the target polymer 7. GPC analysis showed that the weight average molecular weight of the resulting polymer 7 was 8,300 and the dispersity was 2.3, calculated in terms of standard polystyrene. The structure present in polymer 7 is shown in the following formula.

[0173]

[0174] Comparative Synthesis Example 1 100.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemicals Corporation), 66.4 g of 5,5-diethylbarbituric acid, and 4.1 g of benzyltriethylammonium chloride were added to 682.00 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the reaction was carried out at 130°C for 24 hours to obtain a solution containing Comparative Polymer 1. GPC analysis showed that the obtained Comparative Polymer 1 had a weight average molecular weight of 6,800 and a dispersity of 4.8, calculated as standard polystyrene. The structure present in Comparative Polymer 1 is shown in the following formula.

[0175] Comparative Synthesis Example 2 6.00 g of styrene (manufactured by Tokyo Chemical Industry Co., Ltd.), 2.50 g of 2-hydroxyethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.43 g of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 20.82 g of PGMEA, and the solution was added to 14.87 g of PGMEA in a reaction vessel heated and maintained at 140°C, and the reaction was carried out for 24 hours to obtain a solution containing comparative polymer 2. GPC analysis showed that the obtained comparative polymer 2 had a weight average molecular weight of 7,700 and a polydispersity of 2.6, calculated as standard polystyrene. The structure present in comparative polymer 2 is shown in the following formula.

[0176]

[0177] Comparative Synthesis Example 3 5.00 g of 4-hydroxyphenyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.38 g of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 20.82 g of PGMEA, and the solution was added to 12.54 g of PGMEA in a reaction vessel heated and maintained at 80°C, and the reaction was carried out for 24 hours to obtain a solution containing Comparative Polymer 3. GPC analysis showed that the obtained Comparative Polymer 3 had a weight average molecular weight of 3,900 and a polydispersity of 1.8, calculated as standard polystyrene. The structure present in Comparative Polymer 3 is shown in the following formula.

[0178]

[0179] Examples and Comparative Examples Each of the compounds or polymers obtained in Synthesis Examples 1 to 7 and Comparative Synthesis Examples 1 to 3 above, and the following polymers, crosslinking agents, curing catalysts, and solvents were mixed in the proportions shown in Table 1-1 or Table 1-2, and filtered through a 0.1 μm fluororesin filter to prepare a composition for forming a resist underlayer film.

[0180] The following polymers were used, and the abbreviations in Tables 1-1 and 1-2 are also shown. PSF-2808: Cresol novolac resin (product name: PSF-2808, manufactured by Gunei Chemical Co., Ltd.) TA: Tannic acid (product name: Tannic acid AL, manufactured by Fuji Chemical Industry Co., Ltd.) TEP-TPA: Polyphenol resin-1 (product name: TEP-TPA, manufactured by Honshu Chemical Co., Ltd.) NF7177C: Polyphenol resin-2 (product name: NeoFARIT 7177C, manufactured by Mitsubishi Gas Chemical Company, Inc.) NFV002-EA2: Polyphenol resin-3 (product name: NeoFARIT V002-EA2, manufactured by Mitsubishi Gas Chemical Company, Inc.) NFV003: Polyphenol resin-4 (product name: NeoFARIT V003, manufactured by Mitsubishi Gas Chemical Company, Inc.) VP-8000: Phenolic resin (product name: VP-8000, manufactured by Nippon Soda Co., Ltd.)

[0181] Other abbreviations in Tables 1-1 and 1-2 are as follows: PL-LI: Tetramethoxymethyl glycoluril PGME-PL: Imidazo[4,5-d]imidazole-2,5(1H,3H)-dione,tetrahydro-1,3,4,6-tetrakis[(2-methoxy-1-methylethoxy)methyl]- TMOM-BP: 3,3',5,5'-tetrakis(methoxymethyl)-[1,1'-biphenyl]-4,4'-diol PyPSA: Pyridinium-p-hydroxybenzenesulfonic acid R-30N: Surfactant PGMEA: Propylene glycol monomethyl ether acetate PGME: Propylene glycol monomethyl ether The amount of each additive is shown in parts by mass, and the amount of the solvent is shown in composition ratio.

[0182]

[0183]

[0184] (Elution test into photoresist solvent) Each of the resist underlayer film-forming compositions of Examples 1 to 14 and Comparative Examples 1 to 4 was applied onto a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a film with a thickness of 5 nm. These resist underlayer films were immersed in a mixed solution of propylene glycol monomethyl ether / propylene glycol monomethyl ether acetate = 70 / 30 (mass ratio), which is a solvent used in photoresists, and the results are shown in Table 2, with a film thickness change of 5 Å or less being rated as "good" and a film thickness change of more than 5 Å being rated as "poor."

[0185]

[0186] (Measurement of atomic percentage (atom %) of oxygen of phenolic hydroxy groups in resist underlayer film) Each resist underlayer film-forming composition was applied to a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a resist underlayer film with a thickness of 5 nm. The silicon wafer on which the resist underlayer film was formed was cut into a size of approximately 0.5 x 1 cm and dried under reduced pressure for 20 hours or more. The resulting product was then sealed in a 6.0 x 7.5 cm weighing bottle together with 3 ml of trifluoroacetic anhydride, and the hydrogen atoms of the phenolic hydroxy groups were substituted with trifluoroacetyl groups by a gas-phase chemical modification method at 25°C. The reaction time was determined based on the time required to reach reaction equilibrium for each composition. Unreacted trifluoroacetic anhydride and by-product trifluoroacetic acid were then removed by drying under reduced pressure for 20 hours or more. Thereafter, the number of atoms constituting the film (excluding hydrogen) was measured using X-ray photoelectron spectroscopy (Quanterar SXM) using an AlKa radiation source. The atomic percentage of oxygen in phenolic hydroxy groups in the resist underlayer film (R OH The atomic percentage of oxygen in the phenolic hydroxy groups in the resist underlayer films of Examples 1 to 5, 7 to 14, and Comparative Examples 1 to 4 is shown in Table 4. It was confirmed that the atomic percentage of oxygen in the phenolic hydroxy groups in the resist underlayer films of Examples 1 to 5 and 7 to 14 was higher than that of Comparative Examples 1 to 4. F: Number of fluorine atoms A: Total number of atoms (excluding hydrogen atoms)

[0187]

[0188] (Resist Patterning Evaluation) [Resist Pattern Formation Test Using Electron Beam Lithography Apparatus] Each of the resist underlayer film-forming compositions of Examples 1 to 14 and Comparative Examples 1 to 4 was applied to a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a 5 nm-thick resist underlayer film. An EUV positive resist solution was spin-coated onto the resist underlayer film and heated at 130°C for 60 seconds to form an EUV resist film. The resist film was exposed under specified conditions using an electron beam lithography apparatus (ELS-G130). After exposure, the resist was baked at 100°C for 60 seconds (PEB), cooled to room temperature on a cooling plate, and puddle developed for 30 seconds using a 2.38% aqueous solution of tetramethylammonium hydroxide (manufactured by Tokyo Ohka Kogyo Co., Ltd., product name NMD-3) as a photoresist developer. Resist patterns with hole sizes of 16 nm to 26 nm were formed. A scanning electron microscope (CG4100, manufactured by Hitachi High-Technologies Corporation) was used to measure the resist pattern. The photoresist patterns thus obtained were examined for the possibility of forming 23 nm contact holes (C / H). Formation of 23 nm C / H patterns was confirmed in all cases of Examples 1 to 14. The optimum irradiation energy was defined as the charge amount required to form a 23 nm contact hole, and the irradiation energy (μC / cm) when the charge amount in Comparative Example 1 was set to 1.00 was used. 2 ) are shown in Table 4. In Examples 1 to 14, a reduction in the optimum irradiation energy was confirmed compared with Comparative Examples 1 to 4.

[0189]

[0190] The composition for forming a resist underlayer film according to the present invention can provide a composition for forming a resist underlayer film for forming a resist underlayer film that can form a desired resist pattern, as well as a method for producing a substrate having a resist pattern and a method for producing a semiconductor device using the composition for forming a resist underlayer film.

Claims

1. A composition for forming a resist underlayer film, comprising a compound (A) containing an aromatic hydrocarbon ring having a phenolic hydroxy group bonded thereto, and a solvent (B), wherein the atomic percentage of oxygen in the phenolic hydroxy group in a cured film of the composition is 2.00% or more.

2. The composition for forming a resist underlayer film according to claim 1, wherein the compound (A) includes at least one of a phenol resin, a naphthol resin, a biphenol resin, a polyhydroxystyrene, and a polyhydroxyvinylnaphthalene.

3. The composition for forming a resist underlayer film according to claim 1, wherein the compound (A) is a low molecular weight compound (A-1) containing two or more phenolic hydroxy groups and having a molecular weight of 5,000 or less.

4. The composition for forming a resist underlayer film according to claim 1, further comprising a crosslinking agent (C).

5. The composition for forming a resist underlayer film according to claim 1, which is a composition for forming a resist underlayer film for EUV or electron beam lithography.

6. A resist underlayer film which is a cured product of the composition for forming a resist underlayer film according to any one of claims 1 to 5.

7. The resist underlayer film according to claim 6, wherein the atomic percentage of oxygen in phenolic hydroxy groups in said resist underlayer film is 2.00% or more.

8. The resist underlayer film according to claim 6, which has a film thickness of 2 nm or more and 20 nm or less.

9. A laminate comprising: a semiconductor substrate; and the resist underlayer film according to claim 6.

10. A method for manufacturing a semiconductor device, comprising: a step of forming a resist underlayer film on a semiconductor substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 5; and a step of forming a resist film on the resist underlayer film.

11. A pattern forming method comprising the steps of: forming a resist underlayer film on a semiconductor substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 5; forming a resist film on the resist underlayer film; irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern; and etching the resist underlayer film using the resist pattern as a mask.

Citation Information

Patent Citations

  • Halogenated anti-reflective coating

    JP2005526270A

  • Positive resist composition and resist pattern forming method

    JP2010128369A

  • Positive resist composition, resist pattern forming method, and polymer compound

    JP2010181857A

  • Positive resist composition, resist pattern forming method and polymeric compound

    JP2011043749A

  • Patterned inorganic layers, radiation based patterning compositions and corresponding methods

    JP2011253185A