Production method for recycled polyester and production method for polyester composite material
The method addresses the challenges of recycling polyester by using solvent-based purification and flocculation techniques to produce high-quality recycled polyester with enhanced mechanical strength and color tone, while reducing environmental impact and costs.
Patent Information
- Application Number
- PCT/JP2024/013204
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for recycling polyester, such as chemical recycling and material recycling, face challenges including high environmental impact, high manufacturing costs, and poor quality of recycled polyester due to contamination from impurities, especially in textile products and polyester composite materials, which affect the color tone and mechanical strength of the recycled material.
A method involving the use of specific cleaning and dissolution solvents, followed by filtration and precipitation steps, to remove impurities like colorants and surfactants, and treat the polyester composite material with flocculants and filter aids to achieve high-quality recycled polyester with excellent color tone and mechanical strength without extensive thermal energy or environmental impact.
The method produces recycled polyester with improved color tone and mechanical strength, achieving a narrow molecular weight distribution and reducing the environmental footprint by minimizing thermal energy usage and solvent volatility.
Smart Images

Figure JP2024013204_03102024_PF_FP_ABST
Abstract
Description
Method for producing recycled polyester and method for producing polyester composite material
[0001] The present invention relates to a method for producing recycled polyester and a method for producing a polyester composite material.
[0002] Polyesters (hereinafter sometimes referred to as "PEs") have excellent mechanical strength, heat resistance, chemical resistance, and moisture resistance, and are easy to mold and inexpensive, and are therefore used in a variety of applications, such as fibers, films, and resin molded products. However, because they are inexpensive, mass production and mass consumption have expanded, and the life cycle per product is short, leading to large amounts of waste, incineration, and landfill disposal. In addition, because these are petroleum-derived products, they pose a significant environmental burden, which has become an issue.
[0003] Therefore, there is a need to establish a method for recycling polyester. Chemical recycling (e.g., Patent Document 1) and material recycling (e.g., Patent Documents 2 and 3) have been proposed as methods for recycling polyester. In recent years, PET bottle recycling has progressed, and products using recycled polyester have also been produced.
[0004] JP-A-2002-60369 JP-A-11-60795 Patent No. 6708642
[0005] However, in recent years, advances in bottle-to-bottle horizontal recycling technology have made it possible to remanufacture PET bottles from used PET bottles, making it difficult to use used PET bottles as recycled raw materials for other polyester products. For these reasons, there is a need to establish technology for obtaining recycled polyester from textile products such as clothing and other apparel, household goods, and automobile interior parts, as well as polyester composite materials such as injection-molded and extrusion-molded products that contain other resins.
[0006] On the other hand, chemical recycling methods such as those described in Patent Document 1 can remove impurities and other resins, thereby producing recycled polyester of the same quality as petroleum-derived virgin products. However, chemical recycling involves many processes, and requires a large amount of thermal energy for depolymerization (decomposition down to the monomer), transesterification of the monomer, and repolymerization, which results in issues such as a large environmental impact and high production costs.
[0007] While material recycling can be inexpensive, if various impurities are present in the recycled raw materials, the resulting recycled polyester will also contain these impurities, resulting in a deterioration in quality. For example, in the case of textile products, textile products colored with dyes of various colors are mixed in, so there is a high possibility that the recycled polyester will be mixed with coloring components, resulting in black recycled polyester, and it will be very difficult to color textile products manufactured using this polyester to the desired color. Furthermore, in the case of polyester composite materials, since they contain not only polyester but also other resins, it is difficult to recover only polyester through material recycling.
[0008] Patent Documents 2 and 3 report methods for obtaining recycled polyester by dissolving polyester, separating other fiber materials and impurities, and using a polyester precipitation solvent.
[0009] However, Patent Document 2 recommends hexafluoroisopropanol (HFIP) as a dissolving solvent for polyester, but HFIP is corrosive and unsuitable for industrial use, and is also highly volatile and toxic, making it an unsuitable solvent. Furthermore, this method does not adequately address the dyes absorbed in the fibers or the impurities contained in the fibers. In particular, since no decolorization process is performed on colored textile products, it is believed that the color tone of the recycled polyester will deteriorate.
[0010] In fact, as shown in Comparative Example 1 described later, when the present inventors dissolved a polyester fiber product and recovered recycled polyester without performing a decolorizing operation, they were unable to sufficiently remove the colored components in the fiber.
[0011] Patent Document 3 reports a method in which decolorization is performed before dissolving a polyester fiber product, the polyester is dissolved using the same solvent but at a higher temperature than for decolorization, and the solvent is then removed by distillation. A cyclic amide is selected as the dissolving solvent, but because cyclic amides have a high boiling point, there is a high possibility that the cyclic amide will remain in the recycled polyester. This requires the use of a large amount of energy in the distillation operation, making this a suboptimal process. Furthermore, when removing the solvent from the recycled polyester, the recycled polyester is distilled at a high temperature, which may result in depolymerization of the recycled polyester.
[0012] In fact, as shown in Comparative Example 2 described below, when the present inventors obtained recycled polyester using a method similar to that described in Patent Document 3, the colored components could not be sufficiently removed, and even after drying at high temperature and reduced pressure for a long period of time, a large amount of the dissolving solvent remained, and the molecular weight was also reduced due to the heat load.
[0013] Under these circumstances, there is a need to recover recycled polyester with excellent color tone and mechanical strength from polyester composite materials and process it again into polyester composite materials. The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing recycled polyester that can obtain recycled polyester with excellent color tone and mechanical strength using a method with little environmental impact, without requiring the extensive steps such as depolymerization, transesterification, and repolymerization, or the thermal energy required in chemical recycling. Another aim is to provide a method for producing a polyester composite material using the obtained recycled polyester.
[0014] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that recycled polyester having excellent color tone and mechanical strength and a narrow molecular weight distribution can be recovered without decomposing down to the monomer by washing a polyester composite material with a specific washing solvent to remove impurities such as colorants and surfactants, dissolving the polyester in a solvent that can dissolve it, removing impurities such as fibers and resins other than polyester and metal impurities by filtration, and then contacting the resulting material with a solvent that cannot dissolve polyester to precipitate the polyester, which has led to the completion of the invention of the following method for producing recycled polyester.
[0015] The present inventors have also discovered that by dissolving the polyester in a polyester composite material in a specific dissolution solvent, treating the mixture with a flocculant or a flocculant and a filter aid, and then performing solid-liquid separation to precipitate the polyester, it is possible to recover recycled polyester that has excellent color tone and mechanical strength and a narrow molecular weight distribution, without decomposing the polyester down to the monomer, and have thus completed the invention of the following method for producing recycled polyester.
[0016] That is, the present invention relates to the following inventions. [1] A method for producing recycled polyester from a polyester composite material, comprising the following steps (A) to (D): step (A): washing a polyester composite material with a washing solvent comprising a mixture of a solvent (X1) consisting of a phenolic solvent and / or a chlorine-based organic solvent and one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water; step (B): mixing the washed polyester composite material with a dissolution solvent comprising a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved, and then subjecting the solution in which the polyester is dissolved to solid-liquid separation to obtain a liquid component (L) in which the polyester is dissolved; step (C): mixing the liquid component (L) with a poor solvent (PS) having a boiling point of 130°C or less to precipitate the polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; and (D): a step of drying the solid polyester to obtain a recycled polyester. [2] A method for producing a recycled polyester according to [1] above, wherein in step (B), the polyester in the polyester composite material is dissolved in the dissolution solvent, and then mixed with a nonpolar solvent having a dielectric constant of 1 or more and 3 or less to obtain a solution in which the polyester is dissolved. [3] The method for producing a recycled polyester according to [1] above or [2] above, wherein the polyester is one or more selected from the group consisting of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, copolymers thereof, and copolymers with other resins.[4] The method for producing recycled polyester according to any one of [1] to [3], wherein the polyester composite material contains polyester and one or more other components selected from the group consisting of low-molecular-weight organic compounds, metal compounds, inorganic fine particles, non-polyester fibers, and non-polyester resins, and the recycled polyester is polyester from which the other components have been removed. [5] The method for producing recycled polyester according to [4], wherein the low-molecular-weight organic compounds contain one or more selected from the group consisting of colorants, surfactants, antistatic agents, and flame retardants, the metal compounds contain matting agents and / or ultraviolet absorbers, the inorganic fine particles contain pigments, the non-polyester fibers contain one or more selected from the group consisting of natural fibers, acrylic fibers, rayon fibers, polyurethane fibers, nylon fibers, polyethylene fibers, polypropylene fibers, and glass fibers, and the non-polyester resins contain one or more selected from the group consisting of polyethylene resins, polypropylene resins, polyurethane resins, polystyrene resins, nylon resins, polyvinyl chloride resins, and acrylic resins. [6] The method for producing recycled polyester according to any one of [1] to [5], wherein the polyester composite material is polyester-containing fibers. [7] The method for producing recycled polyester according to [6], wherein the polyester-containing fiber contains at least a colorant and titanium oxide and / or fibers other than polyester, and the polyester-containing fiber is decolorized in step (A), and the titanium oxide and / or fibers other than polyester are removed in step (B). [8] The method for producing recycled polyester according to any of [1] to [7], wherein the pH of the washing solvent is less than 13.0. [9] The method for producing recycled polyester according to any of [1] to [8], wherein the washing temperature in step (A) is 30°C or higher and 150°C or lower, and the dissolution temperature in step (B) is 30°C or higher and 150°C or lower.
[10] The method for producing recycled polyester according to any of [1] to [9], wherein the boiling point of the solvent (Y1) is 250°C or lower.
[11] The method for producing recycled polyester according to any one of [1] to
[10] above, wherein the dissolution temperature in step (B) is higher than the washing temperature in step (A).
[12] The method for producing recycled polyester according to any one of [1] to
[11] above, wherein the content of solvent (X2) in the dissolution solvent in step (B) is higher than the content of solvent (X1) in the washing solvent in step (A).
[13] The method for producing recycled polyester according to any one of [1] to
[12] above, wherein the poor solvent (PS) is one or more selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water.
[14] The method for producing recycled polyester according to any one of [1] to
[13] , wherein the solvent (Y1) is one or more selected from the group consisting of toluene, xylene, heptane, hexane, acetone, methanol, ethanol, ethylene glycol, propylene glycol, and water, and the poor solvent (PS) is one or more selected from the group consisting of acetone, toluene, methanol, ethanol, and water.
[15] The method for producing recycled polyester according to any one of [1] to
[14] , wherein the Ti content in the polyester composite is 500 ppm or more and the Ti content of the recycled polyester is 100 ppm or less.
[16] The method for producing recycled polyester according to any one of [1] to
[15] , wherein the N content in the polyester composite is 400 ppm or more and the N content of the recycled polyester is 80 ppm or less.
[17] The method for producing recycled polyester according to any one of [1] to
[16] , wherein the solution in which the polyester is dissolved is contacted with a filter aid before performing the solid-liquid separation in step (B).
[18] The method for producing recycled polyester according to any one of [1] to
[17] , wherein the solution in which the polyester is dissolved is brought into contact with a flocculant before the solid-liquid separation in the step (B).
[19] A method for producing recycled polyester, which produces recycled polyester from a polyester composite material, comprising the following steps (B2), (Z2), (C2), and (D2): step (B2): mixing the polyester composite material with a dissolution solvent containing a solvent (X2) made of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved; step (Z2): bringing the solution in which the polyester is dissolved into contact with a flocculant, followed by solid-liquid separation to obtain a liquid component (L2) in which the polyester is dissolved; step (C2): mixing the liquid component (L2) with a poor solvent (PS) having a boiling point of 130°C or less to precipitate the polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; and step (D2): drying the solid polyester to obtain a recycled polyester.
[20] The method for producing recycled polyester according to
[19] , wherein the solution containing dissolved polyester is contacted with a filter aid before the solid-liquid separation in step (Z2).
[21] The method for producing recycled polyester according to any one of
[18] to
[20] , wherein the flocculant is one or more selected from the group consisting of inorganic salts other than alkali metals and alkaline earth metals and polymeric compounds.
[22] The method for producing recycled polyester according to any one of
[18] to
[21] , wherein the flocculant is an inorganic salt other than alkali metals and alkaline earth metals.
[23] The method for producing recycled polyester according to
[22] , wherein the inorganic salt other than alkali metals and alkaline earth metals is one or more selected from the group consisting of iron(III) chloride, iron(II) sulfate, iron(III) sulfate, aluminum sulfate, and aluminum chloride.
[24] The method for producing recycled polyester according to
[21] , wherein the solution containing dissolved polyester is contacted with the flocculant consisting of the inorganic salt other than alkali metals and alkaline earth metals, and then contacted with the flocculant consisting of the polymeric compound.
[25] The method for producing recycled polyester according to
[21] or
[24] above, wherein the polymer compound is one or more selected from the group consisting of polyacrylamide and polyethylene oxide.
[26] The method for producing recycled polyester according to
[17] ,
[18] , or
[20] above, wherein the filter aid is one or more selected from the group consisting of activated carbon, activated clay, celite, silica gel, synthetic adsorbents, bentonite, alumina, and zeolite.
[27] A method for producing a polyester composite material, comprising the steps of obtaining a recycled polyester by the method for producing recycled polyester according to any one of [1] to
[26] above, and producing a polyester composite material using the obtained recycled polyester.
[0017] According to the present invention, there is provided a method for producing recycled polyester, which can produce recycled polyester excellent in color tone and mechanical strength by a method with little environmental impact, without requiring a large number of steps or thermal energy.
[0018] Fig. 1 is a flow chart of an example of a method for producing a first recycled polyester (recycled PEs) of the present invention. Fig. 2 is a flow chart for explaining step (B) of the method for producing a first recycled polyester of the present invention. Fig. 3 is a flow chart of an example of a method for producing a first recycled polyester of the present invention when a polyester-containing fiber (PEs-containing fiber) is used as a polyester composite material (PEs composite material).
[0019] The following describes in detail an embodiment of the present invention, but the following description of the constituent elements is one example (typical example) of an embodiment of the present invention, and the present invention is not limited to the following content unless the gist of the present invention is changed. Note that when the expression "~" is used in this specification, it is used as an expression including the numerical values or physical property values before and after it.
[0020] <Method for Producing Recycled Polyester> (First Method for Producing Recycled Polyester) The first method for producing recycled polyester according to the present invention is a method for producing recycled polyester from a polyester composite material, and includes the following steps (A) to (D): step (A): washing a polyester composite material with a washing solvent obtained by mixing a solvent (X1) consisting of a phenolic solvent and / or a chlorine-based organic solvent with one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water, step (B): mixing the washed polyester composite material with a dissolution solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved (hereinafter, may be referred to as a "PEs solution"), and then subjecting the PEs solution to solid-liquid separation to obtain a liquid component (L) in which the polyester is dissolved, The method for producing recycled polyester (hereinafter, may be referred to as "first method for producing recycled polyester of the present invention") includes: step (C): a step of mixing the liquid component (L) with a poor solvent (PS) having a boiling point of 130°C or less to precipitate a polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; and step (D): a step of drying the solid polyester to obtain a recycled polyester.
[0021] One of the features of the first recycled polyester production method of the present invention is that impurities are removed in multiple steps (i.e., steps (A), (B), and (C)) by utilizing differences in solubility. The inventors have found that impurities such as low-molecular-weight organic compounds (e.g., colorants and surfactants) that may be contained in the polyester composite material can be dissolved and removed by washing the polyester composite material with a specific washing solvent (step (A)) before dissolving the polyester in the polyester composite material. They have also found that fibers, resins, and metal impurities other than polyester can be removed by washing the polyester composite material with a specific washing solvent and then dissolving and filtering the polyester (step (B)). The polyester can then be recovered by reprecipitation (step (C)). This makes it possible to recover recycled polyester with excellent color tone and mechanical strength without requiring numerous steps or thermal energy, as is the case with chemical recycling. By using the first recycled polyester production method of the present invention, recycled polyester can be produced inexpensively and with low energy, without decomposing the polyester into monomers.
[0022] (Second method for producing recycled polyester) The second method for producing recycled polyester according to the present invention is a method for producing recycled polyester from a polyester composite material, and includes the following steps (B2), (Z2), (C2), and (D2): step (B2): mixing the polyester composite material with a dissolution solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved (PEs solution); step (Z2): bringing the PEs solution into contact with a flocculant, followed by solid-liquid separation to obtain a liquid component (L2) in which the polyester is dissolved; step (C2): mixing the liquid component (L2) with a poor solvent (PS) having a boiling point of 130°C or less to precipitate the polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; and step (D2): drying the solid polyester to obtain a recycled polyester. The second recycled polyester production method of the present invention includes the steps of:
[0023] One of the features of the second recycled polyester production method of the present invention is that impurities are removed in multiple steps (i.e., steps (B2), (Z2), and (C2)). The inventors' studies have shown that dissolving the polyester in a polyester composite material in a specific solvent allows components insoluble in the solvent (such as fibers and resins other than polyester, metal impurities, and inorganic fine particles) to be separated from the polyester. However, they have found that small inorganic fine particles, despite being insoluble in the solvent, tend not to be captured as a solid during solid-liquid separation and to be mixed into the liquid. They have also found that treating the PEs solution with a flocculant before solid-liquid separation allows small inorganic fine particles to adsorb and flocculate, enabling the small inorganic fine particles to be separated during solid-liquid separation. Therefore, in the second recycled polyester production method of the present invention, the PEs solution is treated with a flocculant in step (Z2) before solid-liquid separation. Furthermore, by recovering the polyester through reprecipitation (step (C)), the polyester can be separated from impurities soluble in the poor solvent (PS).
[0024] In this application, the "first method for producing recycled polyester of the present invention" and the "second method for producing recycled polyester of the present invention" may be collectively referred to as the "method for producing recycled polyester of the present invention."
[0025] <Polyester Composite Material (PEs Composite Material)> Hereinafter, a polyester composite material common to the "first method for producing recycled polyester of the present invention" and the "second method for producing recycled polyester of the present invention" will be described.
[0026] The polyester composite material used in the present invention is a waste material containing polyester and components other than polyester, and is a pre-consumer material or a post-consumer material.
[0027] (Polyesters (PEs)) The type of polyester contained in the polyester composite material is not limited. Polyester is a polymer or copolymer obtained by dehydration condensation of dicarboxylic acid and diol to form an ester bond. Polyester may be a homopolymer or a copolymer. Examples of polyester include polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), and copolymers thereof. Polyester may also be a copolymer with other resins.
[0028] (Components other than polyester) Components other than polyester contained in the polyester composite material are impurities that are removed in any step of the method for producing recycled polyester of the present invention.
[0029] The non-polyester components include compounds used as additives in various products, non-polyester fibers, and non-polyester resins. For example, a composite material containing polyester and one or more other components selected from the group consisting of low-molecular-weight organic compounds, metal compounds, inorganic fine particles, non-polyester fibers, and non-polyester resins can be used as a polyester composite material. The method for producing recycled polyester of the present invention can remove other components, thereby producing a polyester from which the other components have been removed. Examples of low-molecular-weight organic compounds include compounds used as colorants, antistatic agents, flame retardants, surfactants, antioxidants, and light-resistant agents, and typically have a molecular weight of 2,000 or less. Examples of metal compounds include metal oxides and metal salts used as matting agents and UV absorbers. Examples of inorganic fine particles include pigments such as carbon black. Examples of fibers other than polyester include natural fibers, acrylic fibers, rayon fibers, polyurethane fibers, nylon fibers, polyethylene fibers, polypropylene fibers, acetate fibers, glass fibers, and carbon fibers. Examples of resins other than polyester include polyethylene resin, polypropylene resin, polyurethane resin, polystyrene resin, nylon resin, polyvinyl chloride resin, and acrylic resin.
[0030] The first method for producing recycled polyester of the present invention can efficiently remove colorants (dyes), and therefore, it is more effective to apply the first method for producing recycled polyester of the present invention to materials that contain at least a colorant as a component other than polyester.
[0031] Furthermore, the second method for producing recycled polyester of the present invention can efficiently remove pigments, and therefore, it is more effective to apply the second method for producing recycled polyester of the present invention to materials that contain at least pigments as a component other than polyester.
[0032] The form of the polyester composite material is not particularly limited, and fibers, resin molded products, laminated products, etc. may be used. For example, polyester-containing fibers are composite materials that contain, in addition to polyester fibers, natural fibers (cotton, linen, silk, etc.), synthetic fibers (acrylic, rayon, etc.), various additives (dyes, pigments, titanium oxide, etc.), etc. Furthermore, polyester-containing injection-molded products and polyester-containing laminated products are composite materials that contain, in addition to polyester, resins other than polyester (polypropylene, polyethylene, polyurethane, acrylic, etc.), glass fibers, various additives, etc. Furthermore, products that have been subjected to metal loading, dyeing, surface treatment with organic substances, etc. to improve the functionality and design of polyester composite materials are also polyester composite materials.
[0033] The content of polyester in the polyester composite material is not particularly limited, but a material containing 10% by mass or more of polyester in the polyester composite material is preferred, and a material containing 30% by mass or more of polyester is more preferred. Furthermore, the polyester composite material may contain one type of material or two or more types of materials.
[0034] Specific examples of polyester composite materials include polyester fiber products such as clothing, bedding, sofas, curtains, carpets, cushions, mats, automobile interior seats, and aircraft interior seats; blow-molded products such as PET bottles; and waste materials from injection-molded and extrusion-molded products used in electric and electronic parts, automobile parts, etc.
[0035] The polyester composite material used in the present invention is preferably fragmented. By using a finely divided polyester composite material, the efficiency of impurity removal is improved and handling in subsequent steps is also facilitated. The polyester composite material can be fragmented (finely divided) by any method, such as cutting, pulverization, crushing, or cutting, in combination of one or more methods depending on the form of the polyester composite material. The fragmented polyester composite material may be cut, crushed, broken, or cut.
[0036] The fragmented polyester composite material is preferably 5 cm square or less, more preferably 3 cm square or less, and even more preferably 2 cm square or less. If the size of the polyester composite material is too large, impurity removal in step (A) may not proceed sufficiently, or the polyester dissolution time in step (B) may become longer, which is undesirable. Note that "5 cm square or less" means a size that can pass through a sieve with 5 cm openings, "3 cm square or less" means a size that can pass through a sieve with 3 cm openings, and "2 cm square or less" means a size that can pass through a sieve with 2 cm openings. There is no particular lower limit, but it is 1 cm square or more.
[0037] The fragmented polyester composite material may be used directly in step (A) or step (B2). However, since some impurities adhering to the surface of the polyester composite material can be easily removed by washing with water, the fragmented polyester composite material may be washed with water before being used in step (A) or step (B2). For example, step (A) or step (B2) may be carried out after a step of fragmenting the polyester composite material and a step of washing the fragmented polyester composite material with water. Examples of the water washing method include a method in which the fragmented polyester composite material is immersed in water and then the water is removed. Considering the boiling point of water, the temperature of the water used for washing is usually 80°C or lower.
[0038] <Method for producing first recycled polyester> Hereinafter, the first method for producing recycled polyester according to the present invention will be described. FIG. 1 is a flow diagram of an example of the method for producing the first recycled polyester (recycled PEs) of the present invention. FIG. 2 is a flow diagram for explaining an example of step (B) of the method for producing the first recycled polyester of the present invention. Hereinafter, the method for producing the first recycled polyester of the present invention will be described with reference to FIGS. 1 and 2.
[0039] <Step (A)> Step (A) is a step of washing a polyester composite material with a washing solvent obtained by mixing a solvent (X1) consisting of a phenol-based solvent and / or a chlorine-based organic solvent with one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon-based solvents, aliphatic hydrocarbon-based solvents, ketone-based solvents, aldehyde-based solvents, alcohol-based solvents, ether-based solvents, and water.
[0040] In step (A), impurities (hereinafter sometimes referred to as "impurities (α)") contained in the polyester composite material and soluble in the washing solvent are dissolved and removed, thereby obtaining a polyester composite material from which the impurities (α) have been removed. The impurities (α) removed in step (A) are components soluble in the washing solvent used, and include low-molecular-weight organic compounds (e.g., low-molecular-weight organic compounds having a molecular weight of 2000 or less) containing one or more selected from the group consisting of colorants, surfactants, antistatic agents, antioxidants, light stabilizers, and flame retardants, nylon fibers, thermoplastic polyurethane fibers, nylon resins, and thermoplastic polyurethane resins.
[0041] By the step (A), colorants, among the impurities (α), can be efficiently removed, and the colorant content in the polyester composite material can be significantly reduced. Currently, low molecular weight organic compounds containing nitrogen (N), such as azo dyes, are widely used as colorants, and the step (A) is particularly effective in removing low molecular weight organic compounds containing nitrogen.
[0042] The polyester composite material can be washed by contacting the polyester composite material with a washing solvent for a predetermined time, followed by solid-liquid separation. The solid component recovered by solid-liquid separation is the polyester composite material from which the impurity (α) has been removed.
[0043] The method for contacting the polyester composite material with the washing solvent is not particularly limited, but a method in which the polyester composite material is immersed in the washing solvent is preferred. The order in which the polyester composite material and the washing solvent are supplied to the reaction vessel is not particularly limited, and the polyester composite material may be supplied followed by the washing solvent, or the polyester composite material may be supplied followed by the washing solvent, or the polyester composite material and the washing solvent may be supplied in parallel. During the immersion, the washing solvent may be allowed to stand, but it is preferable to dissolve the impurities (α) while stirring.
[0044] (Contact between Polyester Composite Material and Washing Solvent) The washing temperature (the temperature of the washing solvent when the polyester composite material is brought into contact with the washing solvent) is preferably 30°C or higher. Furthermore, in order to weaken the intermolecular interactions of the polyester and elute the impurities (α) from the amorphous portions, it is more preferable to dissolve the impurities (α) while heating. Therefore, washing is preferably carried out by heating at a temperature of 30°C or higher, more preferably at a temperature of 60°C or higher. Heating also facilitates the dissolution of the impurities (α) adhering to the surface of the polyester composite material. On the other hand, since excessive heat may dissolve the polyester, washing is preferably carried out at 150°C or lower, and more preferably at 90°C or lower in order to avoid using a large amount of heat energy. For example, the washing temperature can be 30°C to 150°C or 60°C to 90°C.
[0045] The cleaning time (contact time between the polyester composite material and the cleaning solvent) is appropriately set depending on the cleaning temperature, etc., but is preferably 5 minutes or more, more preferably 30 minutes or more, and is preferably 2 hours or less, more preferably 1 hour or less. For example, the cleaning time can be 5 minutes to 2 hours or 30 minutes to 1 hour.
[0046] The amount of washing solvent is not particularly limited, but if the amount of washing solvent is too small, the impurity (α) may not be sufficiently dissolved, so the amount of washing solvent added is preferably 5 times by mass or more, more preferably 10 times by mass or more, relative to the amount of polyester composite material to be treated. Furthermore, if the amount of washing solvent is too large, a lot of thermal energy is required for solvent recovery, so the amount of washing solvent added is preferably 20 times by mass or less, more preferably 15 times by mass or less, relative to the amount of polyester composite material to be treated. For example, the amount of washing solvent can be 5 to 20 times by mass or 10 to 15 times by mass relative to the amount of polyester composite material.
[0047] (Washing Solvent) The washing solvent is a mixed solvent obtained by mixing a solvent (X1) consisting of a phenol-based solvent and / or a chlorine-based organic solvent with one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon-based solvents, aliphatic hydrocarbon-based solvents, ketone-based solvents, aldehyde-based solvents, alcohol-based solvents, ether-based solvents, and water.
[0048] The pH of the washing solvent is preferably less than 13.0, preferably 12.5 or less, more preferably 12.0 or less, more preferably 11.5 or less, and even more preferably 11.0 or less.
[0049] In step (A), impurities (α) soluble in the cleaning solvent in the polyester composite material are dissolved and removed without substantially dissolving or decomposing the polyester. Therefore, it is preferable not to dissolve the polyester in step (A). It is generally considered best to dissolve the impurities using a solvent in which the polyester has low solubility. However, the inventors' investigations revealed that even when step (A) is performed using a solvent in which the polyester has low solubility, impurities (α) such as colorants and surfactants cannot be sufficiently removed. This is believed to be because the impurities (α) such as colorants and surfactants also penetrate between the polyester molecules. Therefore, they investigated the importance of weakening the intermolecular interactions in the amorphous portions of the polyester in order to elute the intermolecular impurities (α). They found that using a phenolic solvent and / or a chlorine-based organic solvent, which has high solubility for polyester, as part of the cleaning solvent weakens the intermolecular interactions in the amorphous portions and effectively elutes the intermolecular impurities (α) without substantially dissolving the polyester. Thus, one of the features of the first method for producing recycled polyester of the present invention is the use, as the washing solvent in step (A), of a mixed solvent obtained by mixing a solvent (X1) consisting of a phenolic solvent and / or a chlorine-based organic solvent with one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water.
[0050] The solvent (X1), consisting of a phenolic solvent and / or a chlorine-based organic solvent, is effective in weakening the intermolecular interactions of the polyester. By including the solvent (X1) as part of the cleaning solvent, the impurities (α) inside the polyester are also more easily dissolved in the cleaning solvent. Examples of phenolic solvents include phenol, cresol, xylenol, ethylphenol, propylphenol, butylphenol, methoxyphenol, ethoxyphenol, propoxyphenol, butoxyphenol, benzylphenol, phenylphenol, chlorophenol, dichlorophenol, and chloromethylphenol. Examples of chlorine-based organic solvents include methylene chloride, chloroform, chlorohexane, chloropropane, tetrachloroethane, chloropropenyl, chlorobutene, chloromethoxypropane, dichloroethylene, trichloroethylene, bromochloroethane, chlorobenzene, dichlorobenzene, chlorotoluene, bromochlorobenzene, chloropentane, chloroethoxybenzene, and tetrachloroacetic acid. One or more of these solvents may be selected. Among these, the solvent (X1) is preferably one or more selected from the group consisting of phenol, cresol, methylene chloride, and chloroform.
[0051] The one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents, and water dissolve the impurities (α), but have low solubility for polyester. Therefore, by including solvent (Y1) as part of the washing solvent, it is possible to elute the impurities (α) that are soluble in the washing solvent without dissolving the polyester.Examples of the solvent (Y1) include aromatic hydrocarbon solvents such as toluene, xylene, ethylbenzene, diethylbenzene, 1-methylethylbenzene, and mesitylene; aliphatic hydrocarbon solvents such as hexane, heptane, octane, hexene, heptene, octene, cyclopentane, cyclohexane, cycloheptane, cyclohexene, cycloheptene, nonane, decane, and cyclooctane; acetone, methyl ethyl ketone, pentanone, hexanone, diethyl ketone, methyl isobutyl ketone, 3-pentene-2-one, 2,4-pentanedione, cyclopropane, and the like. Ketone solvents such as propanone, cyclobutanone, heptanone, octanone, nonanone, decanone, hexanedione, 3-methyl-3-penten-2-one, cycloheptanone, cyclohexanone, 4-methylcyclohexanone, acetophenone, isophorone, and dimethylacetophenone; propionaldehyde, butyraldehyde, pentanal, hexanal, vinyl aldehyde, glyoxal, glyceraldehyde, isobutyraldehyde, succinaldehyde, heptanal, octanal, nonanal, decanal, benzaldehyde, and phenanthroline; Aldehyde solvents such as nylpropenal, perillaldehyde, and isopropylbenzaldehyde; alcohol solvents such as methanol, ethanol, propanol, isopropanol, isobutyl alcohol, tert-butyl alcohol, pentanol, hexanol, pentanediol, hexanediol, 3-ethyl-3-pentanol, ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, cyclohexanol, methylcyclohexanol, and benzyl alcohol; ether solvents such as diethyl ether, 1,4-dioxane, tetrahydrofuran, isopropyl methyl ether, methyl propyl ether, furan, p-dimethoxybenzene, cyclopentyl methyl ether, ethyl isopropyl ether, tert-butyl propyl ether, ethylene glycol diethyl ether, methyl phenyl ether, ethyl phenyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl ether, cyclohexyl ethyl ether, dihexyl ether, benzyl ethyl ether, and benzofuran; and water can be used.These solvents may be used alone or in combination of two or more. The boiling point of the solvent (Y1) is preferably 250°C or lower. From an industrial viewpoint, the boiling point is more preferably 145°C or lower so as to reduce the heat load caused by distillation during solvent recovery. The solvent (Y1) is preferably one capable of dissolving low-molecular-weight organic compounds such as colorants and surfactants, and is more preferably one or more selected from the group consisting of toluene, xylene, heptane, hexane, acetone, methanol, ethanol, ethylene glycol, propylene glycol, and water.
[0052] The mixing ratio of solvent (X1) to solvent (Y1) may be adjusted within a range in which the polyester does not substantially dissolve. For example, when the temperature of the cleaning solvent is high (e.g., 90°C or higher, or 90°C to 150°C), the proportion of solvent (X1) may be reduced, and when the temperature of the cleaning solvent is low (e.g., 50°C or lower, or 30°C to 50°C), the proportion of solvent (X1) may be increased. This can be adjusted as needed depending on the temperature and time required for eluting the impurities (α). On the other hand, if the proportion of solvent (X1) is too high, the polyester tends to dissolve easily, and if the proportion of solvent (Y1) is too high, the elution of the impurities (α) tends to be insufficient. Therefore, a mass ratio of solvent (X1):solvent (Y1) of approximately 20:80 to 80:20 is preferred, and a mass ratio of solvent (X1):solvent (Y1) of 40:60 to 60:40, 45:55 to 55:45, or 50:50 is more preferred.
[0053] (Solid-Liquid Separation) In step (A), the impurities (α) in the polyester composite material are dissolved in a washing solvent, and then solid-liquid separation is performed to recover the polyester composite material from the washing solvent. When recovering the polyester composite material by evaporating the washing solvent, the impurities (α) dissolved in the washing solvent may precipitate and remain in the solid. Therefore, solid-liquid separation is preferably performed by a method other than evaporating the washing solvent. For example, known methods such as filtration and centrifugation, or methods using a mesh container such as a basket or colander, can be used as the solid-liquid separation method. When filtration is performed, the method is not particularly limited, and any of filter paper, centrifugal filtration, cyclone filtration, glass filters, bag filters, candle filters, etc. can be used, with the filter material preferably having a mesh size of 1 cm or more. When a mesh container is used, it is preferable to dissolve the impurities (α) in the polyester composite material in the washing solvent in the mesh container attached to the reaction vessel in which step (A) is performed, and then remove the mesh container containing the polyester composite material and transfer it to a reaction apparatus in which the next step is performed. Furthermore, when a mesh container is used, the mesh container containing the polyester composite material may be attached to a reaction vessel in which step (A) is performed, or the mesh container may be attached to a reaction vessel in which step (A) is performed, and then the polyester composite material may be added.
[0054] <Step (A0) (Post-Washing of Step (A))> The polyester composite material recovered by solid-liquid separation may be used directly in step (B). However, because impurities (α) are likely to remain on the surface of the polyester composite material, it is preferable to further wash (post-wash) the polyester composite material after step (A) before using it in step (B). Therefore, step (A0) of further washing the polyester composite material may be performed after step (A). Specifically, the polyester composite material recovered by solid-liquid separation is mixed with a solvent for post-washing, stirred, and then the solvent for post-washing is removed. This removes the impurities (α) adhering to the surface of the polyester composite material.
[0055] In step (A0), it is preferable to use an organic solvent and / or water that does not contain phenolic solvents or chlorinated organic solvents so as not to dissolve the polyester composite material. Examples of organic solvents that can be used include aromatic hydrocarbon solvents such as toluene and xylene; aliphatic hydrocarbons such as hexane; alcohol solvents such as methanol and ethanol; ketone solvents such as acetone; aldehyde solvents such as propionaldehyde; and ether solvents such as diethyl ether. These organic solvents may be used in combination. Furthermore, the organic solvent used as the post-washing solvent preferably has a boiling point of 210°C or less. From an industrial perspective, this is because it reduces the heat load caused by distillation during solvent recovery. A boiling point of 130°C or less is more preferable, and 80°C or less is even more preferable. Among these, the post-washing solvent is preferably one or more selected from the group consisting of acetone, toluene, hexane, methanol, ethanol, and water. The temperature of the solvent during post-washing can be set appropriately depending on the boiling point of the solvent used, but is preferably 20 to 80°C. The amount of the post-washing solvent used is preferably at least 2 times, and more preferably at least 5 times, the amount of the polyester composite material.
[0056] Step (A0) may be performed multiple times. When step (A0) is performed multiple times, the type of solvent used, the temperature, the amount of solvent, and the like may be the same or may be different for each step. For example, washing with an organic solvent may be performed multiple times, followed by washing with water.
[0057] <Step (B)> Step (B) is a step of mixing the washed polyester composite material with a dissolution solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a PEs solution, and then subjecting the PEs solution to solid-liquid separation to obtain a liquid component (L) in which the polyester is dissolved.
[0058] The polyester composite material obtained after step (A) typically contains impurities (hereinafter sometimes referred to as "impurities (β)") that are insoluble in the dissolution solvent used in step (B). These impurities (β) remain as solids in the PEs solution. Therefore, the PEs solution is a suspension in which these impurities (β) are dispersed. By subjecting this suspension, the PEs solution, to solid-liquid separation, the liquid component containing the dissolved polyester can be separated from the solid component containing the impurities (β). The impurities (β) are components that are insoluble in the washing solvent used in step (A) and the dissolution solvent used in step (B), and include natural fibers such as cotton, linen, and silk; rayon fibers; acrylic fibers; polyethylene fibers; polypropylene fibers; acetate fibers; glass fibers; polyethylene resins; polypropylene resins; polystyrene resins; thermosetting polyurethane resins; polyvinyl chloride resins; acrylic resins; metal compounds such as titanium oxide and silicon oxide; and inorganic fine particles such as carbon black.
[0059] (Mixing of polyester composite material and dissolving solvent) The order of mixing the polyester composite material and dissolving solvent is not particularly limited, and the polyester composite material may be supplied to the reaction vessel after the dissolving solvent is supplied, or the polyester composite material may be supplied to the reaction vessel after the dissolving solvent is supplied, or the polyester composite material and the dissolving solvent may be supplied in parallel. Furthermore, after mixing the polyester composite material and the dissolving solvent, the mixture may be left to stand to dissolve the polyester, but it is preferable to dissolve the polyester by stirring the liquid.
[0060] The dissolution temperature (the temperature at which the polyester is dissolved) is preferably 30°C or higher, more preferably 60°C or higher, and even more preferably 90°C or higher. While there are no particular limitations on the upper limit, it is preferable to carry out the dissolution at 150°C or lower, and more preferably 130°C or lower in order to avoid using a large amount of thermal energy. For example, the dissolution temperature can be 30°C to 150°C, 60°C to 150°C, or 90°C to 130°C. Furthermore, although this depends on the composition of the washing solvent and dissolution solvent, it is preferable that the dissolution temperature in step (B) be higher than the washing temperature in step (A), particularly when the compositions of the washing solvent and dissolution solvent are similar. By carrying out the dissolution at a temperature higher than that in step (A), the intermolecular interactions of the polyester are weakened, which makes it easier to separate and remove intermolecular impurities in subsequent steps, which is preferable.
[0061] The time for dissolving the polyester is preferably 30 minutes or more, more preferably 1 hour or more, preferably 4 hours or less, and more preferably 2 hours or less. For example, the dissolution time can be 30 minutes to 4 hours, or 1 hour to 2 hours.
[0062] The amount of dissolution solvent added is not particularly limited, but if the amount of dissolution solvent is too small, it will take a long time to dissolve the polyester, so the amount of dissolution solvent added is preferably 5 times by mass or more, more preferably 10 times by mass or more, relative to the amount of polyester composite material to be treated. Furthermore, if the amount of dissolution solvent is too large, a lot of thermal energy will be required for solvent recovery, so the amount of dissolution solvent added is preferably 30 times by mass or less, more preferably 20 times by mass or less, relative to the amount of polyester composite material to be treated. For example, the amount of dissolution solvent added can be 5 to 30 times by mass or 10 to 20 times by mass relative to the amount of polyester composite material to be treated.
[0063] (Dissolution Solvent) The dissolution solvent is a solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent. Examples of phenolic solvents include phenol, cresol, xylenol, ethylphenol, propylphenol, butylphenol, methoxyphenol, ethoxyphenol, propoxyphenol, butoxyphenol, benzylphenol, phenylphenol, chlorophenol, dichlorophenol, and chloromethylphenol. Examples of chlorine-based organic solvents include methylene chloride, chloroform, chlorohexane, chloropropane, tetrachloroethane, chloropropenyl, chlorobutene, chloromethoxypropane, dichloroethylene, trichloroethylene, bromochloroethane, chlorobenzene, dichlorobenzene, chlorotoluene, bromochlorobenzene, chloropentane, chloroethoxybenzene, and tetrachloroacetic acid. One or more of these solvents may be selected. Among these, it is preferable that the solvent (X2) be one or more selected from the group consisting of phenol, cresol, methylene chloride, and chloroform. The solvent (X2) in the dissolution solvent may be the same as or different from the solvent (X1) in the washing solvent. The dissolution solvent may consist of the solvent (X2) or may contain a solvent other than the solvent (X2) (hereinafter referred to as "solvent (Y2)"), as long as it can dissolve the polyester.
[0064] When the dissolution solvent contains solvent (Y2) (a solvent other than solvent (X2)), the boiling point of solvent (Y2) is preferably 250°C or lower, and more preferably 145°C or lower from the viewpoint of solvent recovery. For example, since the viscosity of the solution increases when the polyester dissolves, solvent (Y2) may be added to solvent (X2) for the purpose of improving the fluidity of the polyester dissolution solvent. Examples of solvent (Y2) include aromatic hydrocarbon solvents such as toluene and xylene; aliphatic hydrocarbons such as hexane; ketone solvents such as acetone; aldehyde solvents such as propionaldehyde; alcohol solvents such as methanol, ethanol, ethylene glycol, and propylene glycol; and ether solvents such as diethyl ether. Preferably, solvent (Y2) is one or more selected from the group consisting of toluene, xylene, hexane, ethanol, ethylene glycol, and propylene glycol, and more preferably toluene.
[0065] When the dissolution solvent includes solvent (Y2) in addition to solvent (X2), the order of mixing with the polyester composite material is not particularly limited. The polyester composite material, solvent (X2), and solvent (Y2) may be mixed in parallel to dissolve the polyester. Alternatively, a mixture of solvent (X2) and solvent (Y2) may be mixed with the polyester composite material to dissolve the polyester. Alternatively, the polyester composite material may be mixed with solvent (X2) to dissolve the polyester to a certain extent, and then solvent (Y2) or a mixture of solvent (X2) and solvent (Y2) may be mixed.
[0066] Since it is necessary to dissolve the polyester in step (B), the content of solvent (X2) in the dissolution solvent is usually equal to or greater than the content of solvent (X1) in the washing solvent used in step (A), and preferably greater than the content of solvent (X1) in the washing solvent used in step (A), although this depends on the dissolution temperature, etc. Note that the content of solvent (X1) and solvent (X2) refers to the total content of phenol and chlorine-based organic solvent, but when only a phenol-based solvent is contained, it is the same as the content of the phenol-based solvent, and when only a chlorine-based organic solvent is contained, it is the same as the content of the chlorine-based organic solvent.
[0067] Furthermore, if the proportion of solvent (X2) in the dissolution solvent is too low, it may be difficult to dissolve the polyester or high temperatures may be required, and therefore the content of solvent (X2) in the dissolution solvent is preferably greater than the content of solvent (X1) in the washing solvent used in step (A) and is 60% by mass or greater. In order to improve the solubility of the polyester, it is preferable to increase the content of solvent (X2) in the dissolution solvent to 65% by mass or greater, 70% by mass or greater, 75% by mass or greater, 80% by mass or greater, 85% by mass or greater, 90% by mass or greater, or 95% by mass or greater.
[0068] As shown in FIG. 2, the liquid obtained by dissolving the polyester in the polyester composite material in a dissolution solvent may be used as the PEs solution, or the liquid obtained may be subjected to operations such as washing with water or mixing with a nonpolar solvent, and the resulting liquid may be used as the PEs solution.
[0069] (Water washing after dissolving polyester) By dissolving polyester in a dissolving solvent and then washing with water, the efficiency of removing impurities such as titanium oxide, alkali metals, and alkaline earth metals can be improved. Specifically, the water washing after dissolving polyester involves dissolving the polyester in the polyester composite material in a dissolving solvent, mixing with water, stirring for a predetermined time, and then allowing to stand to separate into two phases, removing the aqueous phase, and obtaining an organic phase, a PEs solution. Typically, the stirring time is 10 minutes or more, and the standing time is 10 minutes or more. Furthermore, if the amount of water is too large, the polyester may precipitate, while if it is too small, the impurity removal effect is reduced. Therefore, the mass of water is preferably 0.1 to 0.5 times the mass of the dissolving solvent. The water washing process may be repeated multiple times, such as three or more times.
[0070] (Mixing with Nonpolar Solvent) Metal compounds that may be contained as UV absorbers or matting agents have small particle sizes (particle diameters) and may not be captured by filter media during filtration. However, mixing with a nonpolar solvent having a dielectric constant of 1 to 3 can cause the metal compounds to aggregate and become smaller in size, making them easier to remove by solid-liquid separation. Therefore, it is preferable to dissolve polyester in a dissolution solvent and then mix the resulting liquid with a nonpolar solvent having a dielectric constant of 1 to 3 to form a PEs solution. Examples of nonpolar solvents having a dielectric constant of 1 to 3 include toluene, xylene, hexane, cyclohexane, octane, styrene, benzene, biphenyl, 1,4-dioxane, 1,3-cyclohexanediene, and naphthalene, with toluene and / or xylene being preferred. The mixing temperature is preferably 50 to 130°C, and may be the same as or different from the dissolution temperature. Furthermore, after mixing with the nonpolar solvent, it is preferable to stir for 10 minutes to 1 hour. If the amount of nonpolar solvent is too small, there is little aggregation effect, and if it is too large, the polyester may precipitate. Therefore, the lower limit of the mass of the nonpolar solvent is preferably 0.5 times or more, more preferably 1 time or more, and even more preferably 1.5 times or more, the mass of the dissolving solvent. The upper limit is preferably 5 times or less, more preferably 4 times or less, even more preferably 3 times or less, and may be 2.5 times or less, or 2 times or less, the mass of the dissolving solvent. For example, the mass of the nonpolar solvent can be 0.5 to 5 times, 1 to 4 times, or 2 to 3 times the mass of the dissolving solvent.
[0071] (Contact with filter aid and / or flocculant) Further, when preparing the PEs solution, or after preparing the PEs solution, a step (Z) of treating with a filter aid and / or flocculant may be included. When the particle size of the impurities (β) that are not dissolved in the dissolution solvent used in step (B) is small, the impurities (β) cannot be captured by solid-liquid separation despite being solid, and the impurities (β) tend to remain in the liquid component (L). In particular, pigments with small particle sizes such as carbon black tend to remain. Therefore, in order to improve the removal efficiency of impurities with small particle sizes such as pigments, it is preferable to contact the PEs solution with a filter aid and / or contact the PEs solution with a flocculant before the solid-liquid separation in step (B). Before the solid-liquid separation in step (B), the PEs solution is contacted with a filter aid and / or a flocculant to adsorb or aggregate coloring components such as pigments, making it easier to capture by filtration or the like.
[0072] The method for contacting the PEs solution with the filter aid and / or flocculant is not particularly limited as long as the filter aid and / or flocculant comes into contact with the PEs solution, but examples include a method in which the filter aid and / or flocculant is added and mixed into a reactor containing the PEs solution after obtaining the PEs solution, a method in which the filter aid is packed into a column and the PEs solution is passed through it, and a method in which the filter aid and / or flocculant is added and mixed when obtaining the PEs solution. These methods may be combined.
[0073] Examples of filter aids include activated carbon, activated clay, bentonite, celite, alumina, silica gel, zeolite, and synthetic adsorbents. If the amount of filter aid added when mixing in a reactor is small, adsorption of pigments and the like does not proceed sufficiently. Therefore, it is preferable to add 1% by mass or more of the filter aid relative to the mass of the polyester composite material, more preferably 5% by mass or more, and even more preferably 15% by mass or more. If the amount added is small, adsorption does not proceed sufficiently. On the other hand, if the amount of filter aid added is large, for example, when performing filtration as solid-liquid separation in step (B), the filter aid may leak through the mesh. Therefore, the amount of filter aid added relative to the mass of the polyester composite material is preferably 500% by mass or less, more preferably 250% by mass or less. For example, the amount of filter aid relative to the polyester composite material can be 1% by mass to 500% by mass, 5% by mass to 500% by mass, or 15% by mass to 250% by mass.
[0074] When using a flocculant, the lower limit of the amount added is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, relative to the mass of the polyester composite material, because a small amount is sufficient to achieve the desired effect. On the other hand, if too much flocculant is added, impurities derived from the flocculant may remain in the PEs solution, potentially deteriorating the color tone and mechanical strength of the final recycled polyester. Therefore, the amount of flocculant added is preferably 20% by mass or less, more preferably 10% by mass or less, relative to the mass of the polyester composite material. For example, the amount of flocculant relative to the polyester composite material can be 0.1% by mass to 20% by mass or 0.5% by mass to 10% by mass.
[0075] The flocculant neutralizes the charge of impurities, such as pigments, dispersed in the PEs solution, promoting adsorption and aggregation of the impurities and increasing the particle size to a size that can be captured by solid-liquid separation. Usable flocculants include one or more selected from the group consisting of inorganic salts other than alkali metal salts and alkaline earth metal salts that decompose polyesters, and polymer compounds. For example, inorganic salts other than alkali metal salts and alkaline earth metal salts include iron(III) chloride, iron(II) sulfate, iron(III) sulfate, aluminum chloride, aluminum sulfate, titanium oxide, copper(I) sulfate, copper(II) sulfate, copper(I) chloride, copper(II) chloride, and zinc sulfate. One or more selected from the group consisting of iron(III) chloride, iron(II) sulfate, iron(III) sulfate, aluminum sulfate, and aluminum chloride are preferred. Alternatively, a mixture of commercially available inorganic salts may be used as the flocculant. In particular, when promoting adsorption and aggregation of pigments with small particle sizes, such as carbon black, using inorganic salts with relatively similar molecular sizes is more likely to promote adsorption and aggregation.
[0076] Inorganic salts can neutralize electric charges, but if the particle size of the aggregated particles is small, it is recommended to add a polymer compound such as an anionic polymer compound, a cationic polymer compound, or a nonionic polymer compound. That is, it is preferable to contact the PEs solution with a flocculant consisting of an inorganic salt other than an alkali metal salt or an alkaline earth metal salt, and then contact it with a flocculant consisting of a polymer compound. The particles dispersed in the PEs solution adhere to the polymer chains, allowing for an increase in particle size. For these reasons, when removing relatively small impurities such as pigments, adding an inorganic salt first and then a polymer flocculant effectively increases the particle size to a size that can be captured by the solid-liquid separation in step (B). Representative examples of polymer compounds include polyacrylamide and polyethylene oxide.
[0077] It is preferable to use a filter aid and a flocculant in combination, and it is preferable to contact the PEs solution with the filter aid and the PEs solution with the flocculant before the solid-liquid separation in step (B). When using a filter aid and a flocculant in combination, the PEs solution may be treated with the filter aid and then with the flocculant, or may be treated with the flocculant and then with the filter aid, or may be treated using the filter aid and the flocculant simultaneously. Moreover, the contact method between the PEs solution and the filter aid and the contact method between the PEs solution and the flocculant may be different methods.
[0078] If the contact time is too short, adsorption and coagulation do not proceed sufficiently, so it is preferably 20 minutes or more, more preferably 30 minutes or more. On the other hand, if it is too long, impurities will be eluted from the added filter aid and coagulant, so it is preferably 180 minutes or less, more preferably 120 minutes or less. For example, the contact time can be 20 to 180 minutes or 30 to 120 minutes.
[0079] In addition to step (A), in step (B), treatment with a filter aid and / or a flocculant can be performed to sufficiently remove impurities that could not be removed in step (A).
[0080] (Solid-Liquid Separation) The method of solid-liquid separation is not particularly limited, and known methods such as filtration and centrifugation can be used, but filtration is preferred. The method of filtering the PEs solution is not particularly limited, and any of filter paper, centrifugal filtration, cyclone filtration, glass filters, bag filters, candle filters, etc. may be used. Furthermore, multiple stages of filtering and multiple methods may be used. The smallest mesh size of the filter medium is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. Furthermore, the smallest mesh size of the filter medium is preferably 0.1 μm or more, more preferably 0.5 μm or more. If the mesh size is too large, removal of foreign matter will be insufficient, and if it is too small, filterability will tend to be poor.
[0081] Solid-liquid separation may be carried out at room temperature or under heated conditions. Filtration may be performed at room temperature or under heated conditions, but heated filtration is preferred to prevent precipitation of the polyester. The temperature of the filtrate is preferably maintained at 50°C or higher, more preferably 80°C or higher. In addition, to prevent deterioration of the polyester due to heat load, the upper limit is preferably 110°C or lower, more preferably 100°C or lower. For example, the temperature of the filtrate during solid-liquid separation can be 50°C to 110°C or 80°C to 100°C.
[0082] <Step (C)> Step (C) is a step of mixing the liquid component (L) with a poor solvent (PS) having a boiling point of 130°C or less to obtain a slurry by precipitating a polyester, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester.
[0083] By mixing the poor solvent (PS), the polyester precipitates as a solid, while impurities that dissolve in the poor solvent (PS) remain dissolved without precipitating. By appropriately selecting the poor solvent (PS), the polyester can be precipitated while the impurities remain dissolved in the liquid component (L), and the impurities dissolved in the poor solvent (PS) can be removed by solid-liquid separation. Impurities that can be removed by leaving them dissolved without precipitating in step (C) include impurities (β) such as acrylic fibers and acrylic resins that were slightly dissolved in step (B) and could not be fully removed, and impurities (α) that could not be fully removed in step (A).
[0084] Furthermore, when the boiling point of the poor solvent (PS) is 130°C or lower, the solvent can be easily removed in step (D), and from an industrial viewpoint, the heat load due to distillation when recovering the solvent can be reduced. The boiling point of the poor solvent (PS) is preferably 100°C or lower.
[0085] (Poor Solvent) The poor solvent (PS) used in step (C) is a poor solvent having a boiling point of 130° C. or lower and having low solubility for polyester. The poor solvent (PS) is not particularly limited as long as it has a boiling point of 130° C. or lower and is capable of precipitating polyester, but typically, a solvent having a boiling point of 130° C. or lower other than a phenol-based solvent or a chlorine-based organic solvent is used, and preferably at least one selected from the group consisting of an aromatic hydrocarbon-based solvent, an aliphatic hydrocarbon-based solvent, a ketone-based solvent, an aldehyde-based solvent, an alcohol-based solvent, an ether-based solvent, and water. Examples of the poor solvent (PS) include aromatic hydrocarbon solvents such as toluene; aliphatic hydrocarbon solvents such as hexane, heptane, octane, hexene, heptene, octene, cyclopentane, cyclohexane, cycloheptane, cyclohexene, and cycloheptene; ketone solvents such as acetone, methyl ethyl ketone, pentanone, hexanone, diethyl ketone, methyl isobutyl ketone, 3-penten-2-one, cyclopropanone, cyclobutanone, and dimethylacetophenone; and propionaldehyde, butylaldehyde, pentanal, and hexanone. Examples of suitable solvents include aldehyde solvents such as ethanol, vinyl aldehyde, glyoxal, isobutyraldehyde, and succinaldehyde; alcohol solvents such as methanol, ethanol, propanol, isopropanol, isobutyl alcohol, and tert-butyl alcohol; ether solvents such as diethyl ether, 1,4-dioxane, tetrahydrofuran, isopropyl methyl ether, methyl propyl ether, furan, cyclopentyl methyl ether, ethyl isopropyl ether, and tert-butyl propyl ether; and water. These solvents may be used alone or in combination of two or more. Among these, it is preferable to use one or more poor solvents (PS) selected from the group consisting of acetone, toluene, methanol, ethanol, and water.
[0086] The mixing ratio of the liquid component (L) and the poor solvent (PS) is not particularly limited as long as the polyester can be precipitated, but if the amount of the poor solvent is too small or too large relative to the amount of solvent (X2) in the liquid component (L), the polyester cannot be sufficiently precipitated. Therefore, the mass ratio of solvent (X2) to poor solvent in the liquid component (L) is preferably 1:0.5 to 1:10, and more preferably 1:1 to 1:5. Since the content of solvent (X2) in the liquid component (L) is approximately the same as that of solvent (X2) in the dissolution solvent, the amount of poor solvent (PS) may be appropriately set depending on the amount of solvent (X2) in the dissolution solvent, and the mass ratio of poor solvent (PS) to solvent (X2) in the dissolution solvent is preferably 0.5 to 10, and more preferably 1 to 5.
[0087] (Precipitation of Polyester) In step (C), the liquid component (L) and the poor solvent (PS) are usually mixed, and then the mixture is stirred for a predetermined time to precipitate the polyester and obtain a slurry. The precipitated polyester is usually a polyester crystal having a crystalline structure at least in part. The method for mixing the liquid component (L) and the poor solvent (PS) is not particularly limited, and the poor solvent (PS) may be supplied to the liquid component (L), or the liquid component (L) may be supplied to the poor solvent (PS). From the viewpoint of being able to slowly precipitate the polyester and making it difficult for impurities to be incorporated into the polyester, a method of supplying the poor solvent (PS) to the liquid component (L) is preferred, and a method of supplying the poor solvent (PS) dropwise to the liquid component (L) is more preferred. When two or more types of poor solvents (PS) are supplied to the liquid component (L), two or more types of poor solvents (PS) may be mixed and supplied, or supplied separately.
[0088] As the polyester precipitates, the ratio of solid (polyester) to liquid increases, and therefore the stirring efficiency tends to decrease. In order to suppress this decrease in stirring efficiency associated with the precipitation of polyester, the polyester is gradually precipitated and the particle diameter of each solid particle is uniform, so that the liquid component (L) and the poor solvent (PS) are preferably mixed while controlling the temperature, and more preferably mixed by dropwise supply while controlling the temperature.
[0089] In order to gradually precipitate the polyester, the mixing of the liquid component (L) and the poor solvent (PS) is preferably carried out at a temperature of more than 20°C and less than 100°C in the reaction vessel in which step (C) is carried out. When the liquid component (L) is supplied to the poor solvent (PS), the temperature of the poor solvent (PS) is preferably more than 20°C, more preferably 30°C or more, and more preferably 50°C or more, depending on the boiling points of the poor solvent (PS) and the liquid component (L). In addition, in order to suppress deterioration of the polyester, the lower limit is preferably 100°C or less, more preferably 80°C or less. In addition, when the poor solvent (PS) is supplied to the liquid component (L), the temperature of the liquid component (L) is preferably 50°C or more and less than 100°C, and more preferably 60°C or more and less than 80°C, depending on the boiling points of the poor solvent (PS) and the liquid component (L).
[0090] The supply rate can be appropriately set depending on the size of the reaction vessel, the amount of liquid, etc., as long as it does not exceed the above-mentioned temperature, but it is preferable to set it to a rate that allows the entire amount to be supplied within 2 hours. Furthermore, if the supply rate is too fast, the growth of solid particles will proceed rapidly, making it easier for impurities to be incorporated, so it is preferable to set it to a rate that allows the entire amount to be supplied in 0.25 hours or more. That is, the supply time is preferably 0.25 to 2 hours, and more preferably 0.5 to 1.5 hours. The supply time refers to the time required to supply the entire amount of liquid component (L) when supplying liquid component (L) to poor solvent (PS), and to supply the entire amount of poor solvent (PS) when supplying poor solvent (PS) to liquid component (L).
[0091] In step (C), it is preferable to mix the liquid component (L) and the poor solvent (PS), cool the mixture to a predetermined aging temperature of 20°C or less, and then maintain the aging temperature to precipitate the polyester. The aging temperature is preferably 20°C or less, more preferably 10°C or less. The cooling rate is preferably 5°C / min or less, more preferably 3°C / min or less, and even more preferably 1°C / min or less. If the time for maintaining the aging temperature (aging time) is too short, the polyester may not precipitate sufficiently, which may reduce the yield of recycled polyester. Therefore, the time for maintaining the aging temperature (aging time) is preferably 0.5 hours or more, more preferably 1.5 hours or more. Furthermore, since the increase in the amount of precipitated polyester is small beyond a certain time, the upper limit of the aging time is usually 3 hours or less.
[0092] (Separation of Polyester) In step (C), after obtaining a slurry in which the polyester has precipitated, the slurry is subjected to solid-liquid separation to recover the solid polyester. Solid-liquid separation of the slurry can be performed by known methods such as filtration or centrifugation, but filtration is preferred. Low-molecular-weight polyesters are often present in polyester composite materials. Filtration can be performed by preferentially removing low-molecular-weight polyesters, resulting in a recycled polyester with a narrow molecular weight distribution. Filtration can be performed using filter paper, centrifugal filtration, cyclone filtration, glass filters, bag filters, candle filters, etc. Multiple stages and multiple methods of filtering may also be used. If the mesh size of the filter medium is too large, foreign matter removal will be insufficient. If the mesh size is too small, filtering performance tends to be poor. Therefore, the smallest mesh size of the filter medium is preferably 15 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. Furthermore, the smallest mesh size of the filter medium is preferably 1 μm or more, more preferably 3 μm or more.
[0093] <Step (C0) (Post-Washing of Step (C))> The solid polyester recovered by solid-liquid separation may be dried directly in step (D). However, since impurities may be attached to the surface of the polyester, it is preferable to further wash (post-wash) the polyester and then dry it in step (D). Therefore, step (C0) of further washing the polyester may be performed after step (C). Specifically, in step (C0), the solid polyester recovered by solid-liquid separation is mixed with a solvent for post-washing, stirred, and then the solvent for post-washing is removed. This removes impurities attached to the surface of the polyester.
[0094] The solvent for post-washing can be any solvent that can be used as the poor solvent (PS) in step (C), and it is preferable to use one or more selected from the group consisting of acetone, toluene, methanol, ethanol, and water. The solvent for post-washing and the poor solvent (PS) in step (C) may be the same or different. To facilitate solvent removal in step (D), the solvent for post-washing preferably has a boiling point of 100°C or less, more preferably 60°C or less. The temperature of the solvent during post-washing may be appropriately set depending on the boiling point of the solvent used, but is preferably 25 to 80°C. The amount of solvent used for post-washing is preferably at least 2 times, more preferably at least 5 times, the mass of the solid polyester. Step (C0) may also be performed multiple times. When step (C0) is performed multiple times, the type of solvent used, the temperature, the amount of solvent, and other conditions may be the same or different for each iteration.
[0095] <Step (D)> Step (D) is a step of drying the solid polyester to obtain recycled polyester. The drying method is not particularly limited, and a known method can be used, and drying under reduced pressure or atmospheric pressure can be used. The drying temperature can be appropriately determined, and for example, drying can be performed at 50 to 120°C for 2 to 15 hours.
[0096] <Recycling of Solvent> When recycled polyester is obtained on an industrial scale, the solvent used in each step may be separated from impurities by distillation, recovered, and reused. For example, the washing solvent used in step (A) may be separated from impurities by distillation, and the recovered solvent may be reused in step (A). Similarly, the liquid separated from the polyester by solid-liquid separation in step (C) also contains the dissolving solvent and poor solvent (PS), so it may be recovered by distillation and reused in step (B) or step (C).
[0097] <Production of recycled polyester from polyester-containing fibers> Figure 3 is a flow diagram of an example of the first method for producing recycled polyester (recycled PEs) of the present invention when polyester-containing fibers (PEs-containing fibers) are used as a polyester composite material. The production method shown in Figure 3 includes a step (S10) of washing the polyester-containing fibers with a washing solvent, a step (S20) of post-washing the polyester-containing fibers, a step (S30) of dissolving the polyester in the polyester-containing fibers in a dissolution solvent, a step (S31) of mixing the liquid in which the polyester has been dissolved with a nonpolar solvent having a dielectric constant of 1 to 3, a step (S32) of performing solid-liquid separation of the PEs solution mixed with the nonpolar solvent to obtain a liquid component (L) in which the polyester has been dissolved, a step (S40) of mixing the liquid component (L) with a poor solvent (PS) to precipitate the polyester, and then obtaining the polyester by solid-liquid separation, a step (S50) of post-washing the polyester, and a step (S60) of drying the polyester.
[0098] Most polyester-containing fibers are dyed or colored with dyes or pigments. They also contain additives such as antistatic agents, UV absorbers, matting agents, flame retardants, surfactants, antioxidants, and light-fastening agents. Metal oxides, particularly titanium oxide, are often incorporated into the fibers as UV absorbers or matting agents. When producing recycled polyester from polyester-containing fibers, decolorization (removal of colorants) and removal of metal oxides from the polyester-containing fibers are particularly important. If the recycled polyester is colored, more dye than conventional methods is required to process the recycled polyester into the desired color. Therefore, the recycled polyester must be sufficiently dye-free and decolorized. Furthermore, if the recycled polyester contains metal oxides, particularly titanium oxide, the metal oxides act as nucleating agents, facilitating crystallization and resulting in reduced mechanical strength. Therefore, the metal oxides must be thoroughly removed. The inventors discovered that dyed polyester-containing fibers can be efficiently removed and decolorized by treating the polyester in the dyed polyester-containing fibers with the specific cleaning solvent described above before dissolving the polyester. The present inventors have also discovered that dissolving the polyester in a polyester-containing fiber in the specific dissolution solvent described above and then mixing with a non-polar solvent having a dielectric constant of 1 to 3 can cause the metal oxide to aggregate and become a size that makes it easy to capture by filtration. Based on these findings, it is preferable to produce recycled polyester from a polyester-containing fiber using the production method shown in Figure 3.
[0099] (S10) S10 is a step of washing the polyester-containing fiber with a washing solvent. S10 is step (A) of the first recycled polyester production method of the present invention and can be carried out in the same manner as step (A) above. The polyester-containing fiber may be polyester fiber alone or may contain polyester fiber and fibers other than polyester. It is preferable to use cut material cut with a cutting machine. In S10, impurities (α) such as low-molecular-weight organic compounds such as colorants, antistatic agents, flame retardants, surfactants, antioxidants, and light-resistant agents, as well as nylon fibers and polyurethane fibers, can be dissolved and removed in the washing solvent.
[0100] In particular, in order to remove the colorant more efficiently, it is preferable to heat the washing solvent in S10, and the washing temperature is more preferably 30 to 150°C, and even more preferably 60 to 90°C. Because polyester is highly crystalline, a dispersion dyeing method is often used to dye fibers, in which heat is applied to the fibers to weaken the intermolecular forces of the amorphous polyester, the colorant is poured in, and the dye is diffused into the interior of the fibers by using a carrier or applying pressure, etc. As in the dyeing process, in removing the colorant (bleaching), applying heat to the fibers weakens the intermolecular interactions of the polyester without substantially dissolving the polyester, making it easier for the colorant molecules to elute from the amorphous parts.
[0101] (S20) S20 is a step of post-washing the polyester-containing fiber. S20 is step (A0) of the first method for producing recycled polyester of the present invention, and can be carried out in the same manner as step (A0) above.
[0102] (S30 to S32) S30 is a step of dissolving the polyester in the polyester-containing fiber in a dissolution solvent, S31 is a step of mixing the liquid in which the polyester has been dissolved with a nonpolar solvent having a dielectric constant of 1 to 3, and S32 is a step of performing solid-liquid separation on the PEs solution mixed with the nonpolar solvent to obtain a liquid component (L) in which the polyester has been dissolved. S30 to S32 are step (B) of the first method for producing recycled polyester of the present invention, and can be performed in the same manner as the corresponding steps of step (B) above.
[0103] By performing steps S30 to S32, impurities (β) such as natural fibers, rayon fibers, acrylic fibers, polyethylene fibers, polypropylene fibers, and metal compounds can be removed. In particular, by performing steps S30 to S32, titanium oxide can be removed. As described above, polyester-containing fibers often have metal oxides, particularly titanium oxide, kneaded into the fibers. Because these metal oxides have small particle sizes, if a solution in which the polyester in the polyester-containing fibers is dissolved in a solvent is filtered as is, the metal oxides may pass through the filter material and become mixed into the liquid component (L). In the manufacturing method shown in FIG. 3 , in step S31, the solution in which the polyester is dissolved is mixed with a nonpolar solvent having a dielectric constant of 1 to 3, and the metal oxides are coagulated. Then, in step S32, solid-liquid separation is performed, thereby further reducing the contamination of the liquid component (L) with metal oxides, particularly titanium oxide.
[0104] (S40) S40 is a step of mixing the liquid component (L) with the poor solvent (PS) to precipitate a solid polyester, and then obtaining the polyester by solid-liquid separation. S40 is step (C) of the first recycled polyester production method of the present invention, and can be performed in the same manner as step (C) above.
[0105] (S50) S50 is a step of post-washing the polyester. S50 is step (C0) of the first method for producing recycled polyester of the present invention, and can be carried out in the same manner as step (C0) above.
[0106] (S60) S60 is a step of drying the polyester. S60 is step (D) of the first method for producing recycled polyester of the present invention, and can be performed in the same manner as step (D) above.
[0107] The production method shown in FIG. 3 is particularly suitable for polyester-containing fibers containing a colorant and titanium oxide and / or fibers other than polyester. Furthermore, as described above, low-molecular-weight organic compounds containing nitrogen (N) are widely used as colorants, so the production method shown in FIG. 3 is even more suitable for polyester-containing fibers containing a low-molecular-weight organic compound containing nitrogen and titanium oxide and / or fibers other than polyester. By using the production method shown in FIG. 3, the polyester-containing fibers can be decolorized (the colorant can be removed) in S10, and titanium oxide and / or fibers other than polyester can be removed in S30 to S32. From the viewpoint of the color tone and mechanical strength of the resulting recycled polyester, it is preferable that the colorant and titanium oxide content of the recycled polyester be sufficiently reduced. As described below, decolorization can be measured using the N content of the recycled polyester as an indicator, and titanium oxide removal can be measured using the Ti (titanium) content of the recycled polyester as an indicator.
[0108] The production method shown in FIG. 3 is one example of a method for producing recycled polyester from polyester-containing fibers, and the method for producing recycled polyester from polyester-containing fibers is not limited to this.
[0109] <Second method for producing recycled polyester> The second method for producing recycled polyester of the present invention is described below. The second method for producing recycled polyester of the present invention does not involve step (A) of the first method for producing recycled polyester, but instead requires that the polyester composite material be contacted with a flocculant when or after being dissolved in a specific dissolution solvent.
[0110] <Step (B2)> Step (B2) is a step of mixing a polyester composite material with a dissolution solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a PEs solution. Step (B2) is similar to the preparation of the PEs solution in step (B) of the first recycled polyester production method of the present invention, except that a polyester composite material is used without performing step (A), and the preferred embodiments are also the same.
[0111] <Step (Z2)> Step (Z2) is a step of contacting the PEs solution with a flocculant, followed by solid-liquid separation to obtain a liquid component (L2) in which the polyester has been dissolved. The method for contacting the PEs solution with the flocculant, the type of flocculant, the contact conditions, and the like are the same as those described for the flocculant in step (B), and preferred embodiments are also the same.
[0112] By carrying out step (B2) and step (Z2), components insoluble in the dissolution solvent can be removed. Components insoluble in the dissolution solvent include natural fibers such as cotton, linen, and silk, rayon fibers, acrylic fibers, polyethylene fibers, polypropylene fibers, acetate fibers, glass fibers, polyethylene resins, polypropylene resins, polystyrene resins, thermosetting polyurethane resins, polyvinyl chloride resins, acrylic resins, metal compounds such as titanium oxide and silicon oxide, and inorganic fine particles such as carbon black. In particular, by carrying out step (B2) and step (Z2), inorganic fine particles with small particle sizes such as pigments can be effectively separated.
[0113] In addition, in the second recycled polyester production method, it is preferable to contact the PEs solution with a filter aid before performing the solid-liquid separation in step (Z2). By using a coagulant and a filter aid in combination, impurities can be removed more efficiently. The contact between the PEs solution and the filter aid may be simultaneous with the contact between the PEs solution and the coagulant, before the contact between the PEs solution and the coagulant, or after the contact between the PEs solution and the coagulant. The contact method between the PEs solution and the filter aid, the type of filter aid, the contact conditions, etc. are the same as those described for the filter aid in step (B), and the preferred embodiments are also the same.
[0114] <Step (C2)> Step (C2) is a step of mixing liquid component (L2) with a poor solvent (PS) having a boiling point of 130°C or less to obtain a slurry by precipitating a polyester, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester. Step (C2) is the same as step (C) in the first method for producing recycled polyester of the present invention, except that liquid component (L2) is used instead of liquid component (L), and preferred embodiments are also the same.
[0115] Impurities dissolved in the dissolution solvent in step (B2) remain in liquid component (L2). Impurities that may remain in liquid component (L2) include low-molecular-weight organic compounds (e.g., low-molecular-weight organic compounds having a molecular weight of 2000 or less) containing one or more selected from the group consisting of colorants, surfactants, antistatic agents, antioxidants, light stabilizers, and flame retardants, as well as nylon fibers, thermoplastic polyurethane fibers, acrylic fibers, nylon resins, thermoplastic polyurethane resins, and acrylic resins. These impurities do not precipitate as a solid even when a poor solvent (PS) is added, and therefore can be separated from the polyester and removed in step (C2).
[0116] Furthermore, since impurities may be attached to the surface of the polyester recovered by solid-liquid separation in step (C2), it is preferable to further wash the polyester (post-washing) and then dry it in step (D2). The post-washing in step (C2) (step (C0)) can be carried out in the same manner as the post-washing in step (C) in the first method for producing recycled polyester of the present invention.
[0117] <Step (D2)> Step (D2) is a step of drying the solid polyester to obtain a recycled polyester. Step (D2) is the same as step (D) in the first method for producing recycled polyester of the present invention, except that the polyester obtained in step (C2) is used as is or after post-washing, and preferred embodiments are also the same.
[0118] <Recycled Polyester (Recycled PEs)> The recycled polyester obtained by the recycled polyester production method of the present invention is polyester regenerated from a polyester composite material by material recycling. The recycled polyester has a weight-average molecular weight equivalent to that of the raw material or virgin product, a molecular weight distribution equal to or smaller than that of the raw material or virgin product, and excellent color tone and mechanical strength.
[0119] The difference between the weight average molecular weight of the recycled polyester and the weight average molecular weight of the polyester in the raw polyester composite material is preferably not more than 1000. The weight average molecular weight of the recycled polyester is 10,000 to 12,000.
[0120] The molecular weight distribution of the recycled polyester is equal to or less than that of the raw material or virgin product, and is preferably 1.8 to 2.5. Note that a lower molecular weight distribution value means less variation in molecular weight, which is preferable, for example, when using the recycled polyester to regenerate fibers, etc.
[0121] The color tone of the recycled polyester is preferably the same as that of virgin polyester, and the color difference from virgin polyester measured with a color difference meter is preferably 10 or less. The color b value of the recycled polyester measured with a color difference meter is preferably 5 or less.
[0122] Furthermore, in order to make the color tone of recycled polyester equivalent to that of virgin polyester, it is preferable that the content of N-containing compounds, which are widely used as colorants, is low, and the N content can be used as an indicator of this. The N content in the recycled polyester is preferably 80 ppm or less, more preferably 50 ppm or less, and even more preferably 5 ppm or less. The N content can be measured by the method described in the Examples. Therefore, in the method for producing recycled polyester of the present invention, it is preferable that the N content in the polyester composite is 400 ppm or more, and the N content of the recycled polyester is 80 ppm or less.
[0123] From the viewpoint of the mechanical strength of the recycled polyester, it is preferable that the content of metal compounds in the recycled polyester is small. Many raw polyester composite materials contain metal compounds as additives, and a high content of metal compounds tends to deteriorate the mechanical strength. For example, the Ti (titanium) content of the recycled polyester is preferably 100 ppm or less, more preferably 50 ppm or less. Therefore, in the method for producing recycled polyester of the present invention, it is preferable that the Ti content in the polyester composite is 500 ppm or more, and the Ti content of the recycled polyester is 100 ppm or less.
[0124] As will be described later in the Examples, it is preferable that the recycled polyester has a crystallization peak between 120° C. and 170° C. in DSC measurement. The heat of the crystallization peak between 120° C. and 170° C. is preferably 50% or more, more preferably 80% or more, of the heat of fusion of virgin polyester.
[0125] <Method for producing polyester composite material> The present invention also relates to a method for producing a polyester composite material (hereinafter, sometimes referred to as "method for producing a polyester composite material of the present invention"), which includes a step of producing a recycled polyester by the method for producing a recycled polyester of the present invention, and a step of producing a polyester composite material using the obtained recycled polyester.
[0126] The process for producing recycled polyester is as described above. The process for producing a polyester composite material can be carried out by a known production method, except that recycled polyester is used as the raw polyester. Examples of methods for producing a polyester composite material include a method of processing the recycled polyester into a polyester fiber product by spinning it using a spinneret, and a method of molding the recycled polyester into various polyester products such as polyester films and polyester molded articles by melt extrusion or injection molding using a mold.
[0127] In the process for producing a polyester composite material, the raw material polyester may contain recycled polyester, and recycled polyester alone may be used, or recycled polyester and virgin polyester may be used in combination.
[0128] The form of the polyester composite material to be produced is not particularly limited, and polyester-containing fibers, polyester-containing molded articles, polyester-containing laminated articles, etc. can be produced by the method for producing a polyester composite material of the present invention.
[0129] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not changed.
[0130] <Analysis Method> = Molecular Weight Measurement = The sample to be measured was dissolved in 1,1,1,3,3,3-hexafluoro-2-propanol (HFIP), filtered through a 0.45 μm syringe filter, and then measured by size exclusion chromatography under the following conditions: Apparatus: Waters "ACQUITY" Mobile phase: HFIP with 0.01 M trifluoroacetic acid Na salt added Flow rate: 0.2 mL / min Column: ACQUITY APC XT900+ XT450+ XT125 Column temperature: 50°C Injection volume: 10 μL Detector: Differential refractometer Molecular weight calculation: Polymethyl methacrylate (PMMA) equivalent
[0131] = Analysis of N contained in samples before and after recycling = Whether or not decolorization had occurred was determined by analyzing the amount of N. The recycled polyester was combusted under an argon and oxygen atmosphere, and the generated combustion gas was measured using a trace nitrogen analyzer ("TN-2100H" manufactured by Nitto Seiko Analytech Co., Ltd.) that uses the reduced pressure chemiluminescence method. A sample prepared by dissolving aniline in toluene was used as a standard sample.
[0132] = Color Tone Measurement of Recycled Polyester = Using a color difference meter ("ZE-6000" manufactured by Nippon Denshoku Industries Co., Ltd.), the L value, a value, and b value of the recycled polyester were measured. Measurements were also carried out on virgin polyester ("GG500D" manufactured by Mitsubishi Chemical Engineering Plastics Corporation). L1, a1, and b1 are the L value, a value, and b value of the recycled polyester, respectively, and L0, a0, and b0 are the L value, a value, and b value of the virgin polyester, respectively. The color difference ΔEa*b* was calculated using the following formula:
[0133]
[0134] =Analysis of Ti contained in samples before and after recycling= Sulfuric acid was added to the recycled polyester, and after white fume treatment on a hot plate, it was dry ashed at 650°C in an electric furnace (Yamato Co., Ltd.'s "Muffle Furnace FP410"). Pure water and sulfuric acid were added to the remaining ash, white fume treatment was performed, and after dissolution, the volume was adjusted to a constant level with pure water. The amount of Ti contained in the recycled polyester was then quantified using an ICP light emitting device (Agilent Technologies Inc.'s "5800 ICP-OES").
[0135] =Molding Test= 3 g of recycled polyester was melted at 290°C and molded into a size of 7 cm length x 7 cm width x 0.5 mm thickness using a hot press. Some samples were so brittle that they broke immediately after molding, so the molded products were evaluated as follows: ⊚: A sample that maintained its strength without breaking in all 10 moldings out of 10 moldings; ◯: A sample that maintained its strength without breaking in 7 to 9 of 10 moldings out of 10 moldings; △: A sample that maintained its strength without breaking in 3 to 6 of 10 moldings out of 10 moldings; ×: A sample that maintained its strength without breaking in 2 or less of 10 moldings out of 10 moldings out of 10 moldings
[0136] = Crystallinity Measurement = In order to confirm the thermal history during molding of the samples obtained in the above molding test, crystallinity measurement was performed. The crystallinity measurement was performed using a DSC ("EXSTAR6000" manufactured by Hitachi High-Tech Science Corporation). 8 mg of a molded product molded using recycled polyester was measured and heated from 30°C to 360°C at a rate of 10°C / min.
[0137] Polyester is characterized by its slow crystallization rate, which allows the production of molded articles with excellent transparency and mechanical strength. Therefore, when many molded articles are subjected to DSC analysis, a crystallization peak is observed between 120°C and 170°C. However, if impurities are present in the molded article, the impurities act as nucleating agents, accelerating the crystallization rate. As a result, the molded article has a high degree of crystallization and poor mechanical strength. When such molded articles are subjected to DSC analysis, no crystallization peak is observed between 120°C and 170°C. Therefore, in the present invention, measurements were conducted to confirm the crystallization rate of the recycled polyester molded articles obtained in the molding test. Evaluation was performed as follows: virgin molded articles were measured 10 times, the average heat of fusion at 260°C was calculated, and the average heat of fusion was compared with the heat of fusion value of each crystallization peak of the recycled polyester molded articles obtained in the molding test. Excellent: A crystallization peak was observed between 120°C and 170°C, and the heat of fusion value was 80-100% of the heat of fusion of the virgin product. ◯: A crystallization peak was observed between 120°C and 170°C, and the calorific value was 50-80% of that of the virgin product. △: A crystallization peak was observed between 120°C and 170°C, and the calorific value was 50% or less of that of the virgin product. ×: No crystallization peak was observed between 120°C and 170°C.
[0138] =Melt Point Measurement of Raw Materials= In order to confirm the type of polyester in the raw polyester composite material, the melting points were measured using a DSC ("EXSTAR6000" manufactured by Hitachi High-Tech Science Corporation) to identify the type of polyester. In the case of polyethylene terephthalate (PET), a melting peak is observed near 260°C, and in the case of polybutylene terephthalate, a melting peak is observed near 220°C, so the type of polyester can be confirmed.
[0139] <Raw Materials> The following raw materials A to E were used. Raw material A: 100% polyester clothing (1) Raw material B: 100% polyester clothing (2) Raw material C: 100% polyester clothing (3) Raw material D: Polyester and cotton blend clothing (1) Raw material E: Polyester and cotton blend clothing (2) Raw material F: Automotive interior fiber Raw material G: Polybutylene terephthalate resin containing 30% glass fiber (GF) (containing carbon black (CB))
[0140] The raw materials were cut into 2 cm x 2 cm pieces using a cutter. Table 1 shows the polyester content, type of polyester, color, weight-average molecular weight Mw, number-average molecular weight Mn, Mw / Mn, N content, and Ti content of raw materials A to G.
[0141]
[0142] [Example 1] (Step A) 300 g of cut sample A was placed in a 5 L separable flask, and 3,000 g of a solution prepared by adjusting toluene and phenol at a mass ratio of 50:50 as a washing solvent was added. The mixture was heated at 80°C for 1 hour with stirring under a nitrogen atmosphere to decolorize the fibers and remove other impurities. Thereafter, the solution was removed by filtration, and decolorized sample A was obtained.
[0143] (Step (A0)) 2000 g of toluene heated to 80° C. was added to the mixture, and the mixture was stirred and the toluene was removed. This operation was repeated twice to wash away colorants and the like adhering to the fibers.
[0144] (Step (B)) Next, 3,000 g of phenol was added as a dissolution solvent, and the mixture was heated at 110° C. for 1 hour with stirring under a nitrogen atmosphere to dissolve the polyester fibers. The mixture was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a filtrate in which the polyester fibers were dissolved was obtained.
[0145] (Step (C)) While the filtrate was kept at 50° C., 3,000 g of acetone as a poor solvent (PS) was added dropwise to the filtrate little by little so that the temperature did not exceed the controlled temperature of 50° C., thereby precipitating PET. After the entire amount of acetone was added, the temperature was lowered to 20° C. over 30 minutes, and then the mixture was stirred for 1 hour at 20° C. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered.
[0146] (Step (C0)) 2000 g of acetone was added to the filtered product (PET), followed by washing and filtering again. This procedure was repeated three times to remove impurities, thereby obtaining a wet cake (washed PET).
[0147] (Step (D)) The obtained wet cake was dried at 80° C. under reduced pressure using an evaporator to obtain a recycled polyester.
[0148] The obtained recycled polyester was evaluated according to the above procedures. The experimental conditions are shown in Table 2, and the evaluation results are shown in Table 4. The recovery rate of polyester was calculated based on the recovery rate of polyester contained in the raw material.
[0149] [Example 2] A recycled polyester was obtained in the same manner as in Example 1, except that 300 g of cut sample B was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0150] [Example 3] A recycled polyester was obtained in the same manner as in Example 1, except that 300 g of cut sample C was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0151] [Example 4] A recycled polyester was obtained in the same manner as in Example 1, except that 300 g of cut sample D was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0152] [Example 5] A recycled polyester was obtained in the same manner as in Example 1, except that 300 g of cut sample E was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0153] [Example 6] (Step A) 300 g of the cut sample A was placed in a 5 L separable flask, and 3,000 g of a solution prepared by adjusting toluene and methylene chloride at a ratio of 50:50 (by mass) as a washing solvent was added. The mixture was heated at 40°C for 1 hour while stirring under a nitrogen atmosphere, thereby decolorizing the fibers and removing other impurities. Thereafter, the solution was removed by filtration, and a decolorized sample A was obtained.
[0154] (Step (A0)) 2000 g of toluene at room temperature was added to the mixture, and the mixture was stirred and the toluene was removed. This procedure was repeated twice to wash away colorants and other substances adhering to the fibers.
[0155] (Step (B)) Next, 600 g of phenol and 2,400 g of methylene chloride were added as dissolution solvents, and the mixture was heated at 45° C. for 1 hour under a nitrogen atmosphere while stirring to dissolve the polyester fibers. The mixture was filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a filtrate in which the polyester fibers were dissolved was obtained.
[0156] (Step (C)) While the filtrate was kept at 40° C., 3,000 g of acetone as a poor solvent (PS) was added dropwise to the filtrate little by little so that the temperature did not exceed the controlled temperature of 40° C., thereby precipitating PET. After the entire amount of acetone was added, the temperature was lowered to 20° C. over 30 minutes, and then the mixture was stirred for 1 hour at 20° C. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered.
[0157] (Step (C0)) 2000 g of acetone was added to the filtered product (PET), followed by washing and filtering again. This procedure was repeated three times to remove impurities, thereby obtaining a wet cake (washed PET).
[0158] (Step (D)) The obtained wet cake was dried at 80° C. under reduced pressure using an evaporator to obtain a recycled polyester.
[0159] The obtained recycled polyester was evaluated according to the above procedures. The experimental conditions are shown in Table 2, and the evaluation results are shown in Table 4. The recovery rate of polyester was calculated based on the recovery rate of polyester contained in the raw material.
[0160] [Example 7] A recycled polyester was obtained in the same manner as in Example 1, except that in step (B), 3,000 g of phenol was added as a dissolution solvent, and the mixture was heated at 110°C for 1 hour to dissolve the polyester fibers. 4,500 g of toluene was then added, the mixture was stirred for 30 minutes, and then filtered using a filter paper with a pore size of 0.5 µm to obtain a filtrate. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0161] [Example 8] A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample B was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0162] [Example 9] A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample C was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0163] [Example 10] A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample D was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0164] [Example 11] A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample E was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0165] [Example 12] A recycled polyester was obtained in the same manner as in Example 7, except that PET was precipitated in water, and various evaluations were carried out. Table 2 shows the experimental conditions, and Table 4 shows the evaluation results.
[0166] [Example 13] (Step A) 100 g of the cut sample D was placed in a 5 L separable flask, and 1000 g of a solution prepared by adjusting toluene and phenol at a mass ratio of 50:50 as a washing solvent was added. The mixture was heated at 80°C for 1 hour while stirring under a nitrogen atmosphere, thereby decolorizing the fibers and removing other impurities. Thereafter, the solution was removed by filtration, and a decolorized sample A was obtained.
[0167] (Step (A0)) 700 g of room temperature toluene was added to the mixture, and the mixture was stirred and the toluene was removed. This procedure was repeated twice to wash away colorants and other substances adhering to the fibers.
[0168] (Step (B)) Next, 1,000 g of phenol was added as a dissolution solvent, and the mixture was heated at 110° C. for 1 hour with stirring under a nitrogen atmosphere to dissolve the polyester fibers. After dissolution, 10 g of activated carbon was added, and the mixture was stirred for 60 minutes. The mixture was then filtered using filter paper with a pore size of 0.5 μm to remove impurities, and a filtrate in which the polyester fibers were dissolved was obtained.
[0169] (Step (C)) While the filtrate was kept at 40° C., 1000 g of acetone as a poor solvent (PS) was added dropwise to the filtrate little by little so that the temperature did not exceed the controlled temperature of 40° C., thereby precipitating PET. After the entire amount of acetone was added, the temperature was lowered to 20° C. over 30 minutes, and then the mixture was stirred at 20° C. for 1 hour. The mixture was filtered using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered.
[0170] (Step (C0)) 700 g of acetone was added to the filtered product (PET), followed by washing and filtering again. This procedure was repeated three times to remove impurities, thereby obtaining a wet cake (washed PET).
[0171] (Step (D)) The obtained wet cake was dried at 80° C. under reduced pressure using an evaporator to obtain a recycled polyester.
[0172] The obtained recycled polyester was evaluated according to the above procedures. The experimental conditions are shown in Table 2, and the evaluation results are shown in Table 4. The recovery rate of polyester was calculated based on the recovery rate of polyester contained in the raw material.
[0173] [Example 14] A recycled polyester was obtained in the same manner as in Example 13, except that in step (B), after dissolving the polyester fibers, 5 g of activated carbon and 3 g of iron (II) sulfate were added instead of 10 g of activated carbon, and various evaluations were carried out. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0174] [Example 15] A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample F was added to a 5 L separable flask instead of cut sample A, and various evaluations were carried out. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0175] Example 16 A recycled polyester was obtained in the same manner as in Example 1, except that 300 g of cut sample F was added to a 5 L separable flask instead of cut sample A, and step (B) was changed to "add 3,000 g of phenol as a dissolution solvent, heat at 110°C for 1 hour to dissolve the polyester fibers, add 30 g of activated carbon and 10 g of iron (II) sulfate, stir at 80°C for 60 minutes, and then filter using filter paper with a pore size of 0.5 μm to obtain a filtrate." Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0176] Example 17 A recycled polyester was obtained in the same manner as in Example 7, except that 300 g of cut sample F was added to a 5 L separable flask instead of cut sample A, and step (B) was changed to "add 3,000 g of phenol as a dissolution solvent, heat at 110°C for 1 hour to dissolve the polyester fibers, add 4,500 g of toluene, stir for 30 minutes, add 30 g of iron (III) chloride, stir at 80°C for 60 minutes, and then filter using filter paper with a pore size of 0.5 μm to obtain a filtrate." Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0177] [Example 18] A recycled polyester (PBT) was obtained and evaluated in the same manner as in Example 1, except that 300 g of cut sample G was added to a 5 L separable flask instead of cut sample A. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0178] Example 19 A recycled polyester (PBT) was obtained in the same manner as in Example 1, except that 300 g of cut sample G was added to a 5 L separable flask instead of cut sample A, and step (B) was changed to "add 3,000 g of phenol as a dissolution solvent, heat at 90°C for 1 hour to dissolve the polyester fibers, add 15 g of iron (III) chloride, stir at 80°C for 60 minutes, and then filter using filter paper with a pore size of 0.5 μm to obtain a filtrate." Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0179] Example 20: A 5-L separable flask was charged with 300 g of cut sample G instead of cut sample A, and step (B) was changed to "add 3,000 g of phenol as a dissolution solvent, heat at 100°C for 1 hour to dissolve the polyester fibers, add 30 g of activated clay and 15 g of iron (III) sulfate, stir at 80°C for 60 minutes, and then filter using a filter paper with a pore size of 0.5 μm to obtain a filtrate." Except for this, a recycled polyester (PBT) was obtained in the same manner as in Example 1, and various evaluations were performed. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0180] [Example 21] The same procedure as in Example 16 was carried out except that steps (A) and (A0) were not carried out, and steps (B2), (Z2), (C2), (C0), and (D2) were carried out to obtain a recycled polyester. The obtained recycled polyester was evaluated. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0181] Example 22: Instead of the cut sample A, 300 g of the cut sample G was added to a 5 L separable flask. Steps (A) and (A0) were not performed. Step (B) was changed to "adding 3,000 g of phenol as a dissolution solvent, heating at 80°C for 1 hour to dissolve the polyester fibers, adding 15 g of activated carbon and 15 g of iron (II) sulfate, stirring at 60°C for 60 minutes, and then filtering using a filter paper with a pore size of 0.5 μm to obtain a filtrate." The same procedures as in Example 1 were carried out, except that steps (B2), (Z2), (C2), (C0), and (D2) were carried out to obtain a recycled polyester (PBT). The obtained recycled polyester was evaluated. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0182] Comparative Example 1: 10 g of cut sample A was placed in a 500 mL recovery flask. Without performing the decolorization operation (step (A)), 100 g of hexafluoroisopropanol (HFIP) was added, and the polyester fibers were dissolved at room temperature for 1 hour. This was filtered using filter paper with a pore size of 0.5 μm to remove impurities, yielding a filtrate (corresponding to step (B)). The filtrate was gradually added dropwise to 100 g of water to precipitate PET. Filtration was performed using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered (corresponding to step (C)). 70 g of water was added to the filtrate, which was then washed and filtered three times to remove impurities, yielding a wet cake (washed PET) (corresponding to step (C0)). The resulting wet cake was dried to yield a recycled polyester (corresponding to step (D)). The resulting recycled polyester was evaluated according to the procedures described above. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0183] Comparative Example 2: 50 g of the cut sample A was placed in a 1-L separable flask, and 500 g of 1,3-dimethyl-2-imidazolidinone (DMI) was added. The fibers were decolorized by heating at 120°C for 1 hour under a nitrogen atmosphere. The solution was then removed to obtain decolorized sample A (corresponding to step (A)). 350 g of 1,3-dimethyl-2-imidazolidinone heated to 120°C was added to the sample, and the mixture was stirred twice to wash away any colored components adhering to the fibers (corresponding to step (A0)). Next, 500 g of 1,3-dimethyl-2-imidazolidinone was added, and the mixture was heated at 170°C for 1 hour to dissolve the polyester fibers. This was then filtered using filter paper with a pore size of 0.5 μm to remove impurities, yielding a filtrate (corresponding to step (B)). The filtrate was gradually added dropwise to 500 g of ethanol to precipitate PET. Filtration was performed using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered (corresponding to step (C)). 350 g of ethanol was added to the filtrate, and the filtrate was washed and filtered again. This operation was repeated three times to remove impurities, yielding a wet cake (washed PET) (corresponding to step (C0)). The resulting wet cake was dried at 80°C under reduced pressure for 3 hours, but was not dry. Therefore, the temperature was increased to 120°C, and the pressure was reduced to 3 kPa for another 3 hours, but the solvent remained on the walls of the flask, and the solvent could not be sufficiently removed from the recycled polyester (corresponding to step (D)). The recycled polyester was recovered in a solvent-containing state, and each evaluation was performed using the above procedures. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results. From the evaluation results shown in Table 5, it can be seen that since DMI is a solvent containing N, the N content was higher than before treatment, and DMI was not sufficiently removed.
[0184] Comparative Example 3 300 g of the cut sample A was added to a 5-L separable flask, and without performing the decolorization operation (step (A)), 3,000 g of phenol was added. The mixture was heated at 110°C for 1 hour to dissolve the polyester fibers. This was then filtered using filter paper with a pore size of 0.5 μm to remove impurities and obtain a filtrate (corresponding to step (B)). The filtrate was recovered, and while maintaining the filtrate at 50°C, the filtrate was gradually added dropwise to 3,000 g of acetone so as not to exceed the controlled temperature of 50°C, thereby precipitating PET. After the addition of all the acetone, the temperature was lowered to 20°C over 30 minutes, and then the mixture was stirred at 20°C for 1 hour. Filtration was performed using filter paper with a pore size of 7 μm, and the filtrate (PET) was recovered (corresponding to step (C)). The filtered product was added with 2000 g of acetone, washed, and filtered again. This procedure was repeated three times to remove impurities, yielding a wet cake (washed PET) (corresponding to step (C0)). The obtained wet cake was dried under reduced pressure at 80°C using an evaporator to yield a recycled polyester (corresponding to step (D)). The obtained recycled polyester was evaluated according to the procedures described above. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0185] [Comparative Example 4] 300 g of cut sample G was added to a 5 L separable flask, and 3000 g of phenol was added without decolorization (step (A)). The mixture was heated at 110 ° C. for 1 hour. This was filtered using filter paper with a pore size of 0.5 μm to remove impurities and obtain a filtrate (corresponding to step (B)). The filtrate was recovered, and while keeping the filtrate at 50 ° C., the filtrate was gradually added dropwise to 3000 g of acetone so as not to exceed the control temperature of 50 ° C., thereby precipitating PBT. After the addition of all the acetone, the temperature was lowered to 20 ° C. over 30 minutes, and then stirred at 20 ° C. for 1 hour. Filtration was performed using filter paper with a pore size of 7 μm, and the filtrate (PBT) was recovered (corresponding to step (C)). 2000 g of acetone was added to the filtrate, and the mixture was washed and filtered again. This operation was repeated three times to remove impurities and obtain a wet cake (washed PET) (corresponding to step (C0)). The obtained wet cake was dried under reduced pressure at 80°C using an evaporator to obtain a recycled polyester (corresponding to step (D)). The obtained recycled polyester was evaluated according to the procedures described above. Table 3 shows the experimental conditions, and Table 5 shows the evaluation results.
[0186] Table 4 shows the evaluation results for Examples 1 to 13, and Table 5 shows the evaluation results for Examples 15 to 22 and Comparative Examples 1 to 4. Items that were not evaluated are indicated as N.T. From the results of Examples 1 to 20 and Comparative Examples 1 to 4, it can be seen that by going through the processes of step (A) (washing with a washing solvent), step (B) (dissolving and filtering the polyester), and step (C) (reprecipitation of the polyester), it is possible to obtain recycled polyester with excellent color tone and a molecular weight distribution of approximately 1.85 to 2.1 without chemically decomposing the polyester. In particular, it can be seen that by performing a titanium oxide coagulation operation in step (B), recycled polyester with excellent color tone and mechanical strength can be obtained. Furthermore, from the results of Examples 21 and 22 and Comparative Examples 1 to 4, it can be seen that recycled polyester with excellent color tone and mechanical strength can be obtained by using a coagulant and / or filter aid (performing step (Z2)) even without performing step (A).
[0187]
[0188]
[0189]
[0190]
Claims
1. A method for producing recycled polyester from a polyester composite material, comprising the following steps (A) to (D): step (A): washing a polyester composite material with a washing solvent comprising a mixture of a solvent (X1) consisting of a phenolic solvent and / or a chlorine-based organic solvent and one or more solvents (Y1) selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents and water; step (B): mixing the washed polyester composite material with a dissolution solvent comprising a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved, and then subjecting the solution in which the polyester is dissolved to solid-liquid separation to obtain a liquid component (L) in which the polyester is dissolved; step (C): mixing the liquid component (L) with a poor solvent (PS) having a boiling point of 130° C. or less to precipitate the polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; step (D): drying the solid polyester to obtain a recycled polyester.
2. A method for producing recycled polyester as described in claim 1, in which in step (B), the polyester in the polyester composite material is dissolved in the dissolution solvent, and then mixed with a non-polar solvent having a dielectric constant of 1 to 3 to obtain a solution in which the polyester is dissolved.
3. The method for producing recycled polyester according to claim 1 or 2, wherein the polyester is one or more selected from the group consisting of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, copolymers thereof, and copolymers with other resins.
4. A method for producing recycled polyester as described in claim 1 or 2, wherein the polyester composite material contains polyester and one or more other components selected from the group consisting of low molecular weight organic compounds, metal compounds, inorganic fine particles, fibers other than polyester, and resins other than polyester, and the recycled polyester is polyester from which the other components have been removed.
5. The method for producing recycled polyester described in claim 4, wherein the low molecular weight organic compound comprises one or more selected from the group consisting of colorants, surfactants, antistatic agents and flame retardants, the metal compound comprises a matting agent and / or an ultraviolet absorber, the inorganic microparticles comprise a pigment, the fibers other than polyester comprise one or more selected from the group consisting of natural fibers, acrylic fibers, rayon fibers, polyurethane fibers, nylon fibers, polyethylene fibers, polypropylene fibers and glass fibers, and the resins other than polyester comprise one or more selected from the group consisting of polyethylene resins, polypropylene resins, polyurethane resins, polystyrene resins, nylon resins, polyvinyl chloride resins and acrylic resins.
6. The method for producing recycled polyester according to claim 1 or 2, wherein the polyester composite material is a polyester-containing fiber.
7. The method for producing recycled polyester according to claim 6, wherein the polyester-containing fiber contains at least a colorant and titanium oxide and / or fibers other than polyester, the polyester-containing fiber is decolorized in the step (A), and the titanium oxide and / or fibers other than polyester are removed in the step (B).
8. The method for producing recycled polyester according to claim 1 or 2, wherein the pH of the washing solvent is less than 13.
0.
9. The method for producing recycled polyester according to claim 1 or 2, wherein the washing temperature in step (A) is 30°C or higher and 150°C or lower, and the dissolution temperature in step (B) is 30°C or higher and 150°C or lower.
10. A method for producing recycled polyester according to claim 1 or 2, wherein the boiling point of the solvent (Y1) is 250°C or lower.
11. The method for producing recycled polyester according to claim 9, wherein the dissolution temperature in step (B) is higher than the washing temperature in step (A).
12. A method for producing recycled polyester as described in claim 1 or 2, wherein the content of the solvent (X2) in the dissolution solvent in step (B) is greater than the content of the solvent (X1) in the washing solvent in step (A).
13. A method for producing recycled polyester according to claim 1 or 2, wherein the poor solvent (PS) is one or more selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, aldehyde solvents, alcohol solvents, ether solvents and water.
14. A method for producing recycled polyester according to claim 1 or 2, wherein the solvent (Y1) is one or more selected from the group consisting of toluene, xylene, heptane, hexane, acetone, methanol, ethanol, ethylene glycol, propylene glycol and water, and the poor solvent (PS) is one or more selected from the group consisting of acetone, toluene, methanol, ethanol and water.
15. A method for producing recycled polyester according to claim 1 or 2, wherein the Ti content in the polyester composite is 500 ppm or more, and the Ti content of the recycled polyester is 100 ppm or less.
16. A method for producing recycled polyester according to claim 1 or 2, wherein the N content in the polyester composite is 400 ppm or more, and the N content of the recycled polyester is 80 ppm or less.
17. A method for producing recycled polyester according to claim 1, wherein the solution in which the polyester is dissolved is contacted with a filter aid before the solid-liquid separation in step (B).
18. A method for producing recycled polyester according to claim 1 or 17, wherein the solution in which the polyester is dissolved is contacted with a flocculant before the solid-liquid separation in step (B) is carried out.
19. A method for producing recycled polyester, comprising the steps of: producing recycled polyester from a polyester composite material, the method comprising the steps of: step (B2), step (Z2), step (C2), and step (D2) below; step (B2): mixing the polyester composite material with a dissolution solvent containing a solvent (X2) consisting of a phenolic solvent and / or a chlorine-based organic solvent to obtain a solution in which the polyester in the polyester composite material is dissolved; step (Z2): contacting the solution in which the polyester is dissolved with a flocculant, followed by solid-liquid separation to obtain a liquid component (L2) in which the polyester is dissolved; step (C2): mixing the liquid component (L2) with a poor solvent (PS) having a boiling point of 130°C or less to precipitate the polyester to obtain a slurry, and then subjecting the slurry to solid-liquid separation to obtain a solid polyester; and step (D2): drying the solid polyester to obtain a recycled polyester.
20. A method for producing recycled polyester according to claim 19, wherein the solution in which the polyester is dissolved is contacted with a filter aid before the solid-liquid separation in step (Z2).
21. The method for producing recycled polyester according to claim 19, wherein the flocculant is one or more selected from the group consisting of inorganic salts other than alkali metals and alkaline earth metals, and polymeric compounds.
22. The method for producing recycled polyester according to claim 19 or 20, wherein the flocculant comprises an inorganic salt other than an alkali metal or an alkaline earth metal.
23. The method for producing recycled polyester according to claim 22, wherein the inorganic salt other than an alkali metal or an alkaline earth metal is one or more selected from the group consisting of iron (III) chloride, iron (II) sulfate, iron (III) sulfate, aluminum sulfate, and aluminum chloride.
24. A method for producing recycled polyester as described in claim 21, in which a solution in which the polyester is dissolved is contacted with the coagulant consisting of an inorganic salt other than the alkali metal and alkaline earth metal, and then contacted with the coagulant consisting of the polymer compound.
25. A method for producing recycled polyester according to claim 21 or 24, wherein the polymer compound is one or more selected from the group consisting of polyacrylamide and polyethylene oxide.
26. A method for producing recycled polyester according to claim 17 or 20, wherein the filter aid is one or more selected from the group consisting of activated carbon, activated clay, celite, silica gel, synthetic adsorbents, bentonite, alumina and zeolite.
27. A method for producing a polyester composite material, comprising the steps of obtaining a recycled polyester by the method for producing a recycled polyester according to any one of claims 1, 2, 17, 19, 20, 21 and 24, and producing a polyester composite material using the obtained recycled polyester.
Citation Information
Patent Citations
Recycling of polyester-containing polymer waste and apparatus therefor
JP1999060795A
Method for recycling polyester waste
JP2002060369A
Recycling Process
JP6708642B2
Process for recovering and recycling dyed polyester fiber
JP1976115577A