Optical laminate and method for manufacturing same
The optical laminate with a specific pigment and binder resin composition addresses the challenge of achieving high infrared transmittance and matching visible light color, improving sensor accuracy and design aesthetics by ensuring high infrared transmittance and synchronous color reproduction.
Patent Information
- Application Number
- PCT/JP2024/013246
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-14
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Current optical laminates used in infrared sensors and display-type automobile panels face challenges in achieving high infrared transmittance while maintaining a black appearance and ensuring that the color of transmitted visible light matches the irradiated light, which affects sensor accuracy and design aesthetics.
An optical laminate with an optical functional layer containing multiple types of pigments and a binder resin, optimized to have specific spectral transmittance ratios and a black ink composition, is developed to achieve high infrared transmittance and a black appearance, while ensuring that the transmitted visible light maintains the same color as the irradiated light.
The optical laminate achieves excellent infrared transmittance, a high degree of blackness, and synchronous color reproduction in the visible light range, enhancing sensor accuracy and design aesthetics by minimizing interference and maintaining visibility of indicator lights.
Smart Images

Figure JP2024013246_03102024_PF_FP_ABST
Abstract
Description
Optical laminate and method for producing the same
[0001] FIELD OF THE INVENTION An embodiment of the present invention relates to an optical laminate and a method for producing the same.
[0002] In various optical devices, there is a demand for technologies to control optical properties, for example, technologies to selectively transmit or block light of specific wavelengths. Optical laminates such as dichroic mirrors, bandpass filters, AR coatings, UV cut filters, IR cut filters, and UVIR cut filters are used for such technologies. For example, in infrared sensors, which are an example of optical devices, wavelengths in the infrared region are often used as light sources. LEDs with maximum wavelengths of 850 nm, 905 nm, or 940 nm are typically used. In particular, the light from LEDs with a maximum wavelength of 850 nm contains some visible light. Therefore, in order to improve sensor accuracy, there is a demand for optical laminates for sensors that can be used in technologies that block visible light and transmit only infrared light.
[0003] One example of the use of an optical laminate for sensors (hereinafter sometimes referred to as a laminate) is a driver monitoring system that detects a driver's behavior using infrared rays. This system detects the driver's condition by irradiating the driver with infrared rays from an LED built into the automobile panel (Patent Document 1). A sensor laminate is provided within the automobile panel, and by blocking visible light, the sensor accuracy is improved. In recent years, development has been underway on display-type automobile panels that incorporate LEDs of various colors in addition to infrared sensors and use each LED as an indicator light. In such display-type automobile panels, the LED indicator lights are illuminated from behind the laminate as a backlight, and it is expected that the design of the automobile panel will be improved.
[0004] The optical laminate is installed at a position corresponding to at least the sensor sensing portion of an optical component constituting an optical device. If the optical laminate is transparent or translucent, the sensor sensing portion will be visible, resulting in poor design. Therefore, from the perspective of the appearance of the optical component, it is preferable that the laminate installed at the position corresponding to the sensor sensing portion be in a color that matches the surrounding components. In many cases, the appearance of the optical component is black, and in order to match the color of the surrounding components as described above, the appearance of the optical laminate is preferably black. For these reasons, there is a demand for an optical laminate that is infrared-transparent and has a black appearance. However, the use of black pigments such as carbon black tends to reduce the infrared transmittance of the laminate and decrease sensor accuracy. Furthermore, while laminates can be manufactured using inks containing a colorant such as a pigment and a binder resin, the dispersion state of the pigment in the ink affects the haze value (cloudiness) of the coating film. It is preferable that the haze value in the infrared region of the coating film be low. A high haze value in the infrared region of the coating film tends to reduce the infrared transmittance of the coating film and decrease sensor accuracy. For these reasons, development of a laminate that has a black appearance and excellent infrared transmittance is desired.
[0005] Furthermore, in display-type automotive panels, it is necessary to view the light of the indicator light through the optical laminate. However, if a laminate that completely blocks visible light is used to increase infrared transmittance, the light of the indicator light cannot be seen through the laminate. Therefore, laminates used in display-type optical devices such as display-type automotive panels need to balance infrared transmittance and visible light blocking properties.
[0006] Furthermore, for example, when a white LED indicator light is turned on as a backlight from behind the laminate, it is desirable that the driver should be able to see the indicator light as a white color. However, the light that passes through the laminate including the infrared-transmitting layer is often colored a different color from the light of the indicator light. Such coloring of light by the laminate significantly reduces visibility and design.
[0007] For this reason, there is a strong demand for the development of an optical laminate that has excellent transmittance in the infrared region and in which the irradiated light and the transmitted light in the visible light region are in the same color.
[0008] Japanese Patent Application Laid-Open No. 2022-170958
[0009] Based on the above, the present invention provides an optical laminate having excellent infrared transmittance and a black appearance. The present invention also provides an optical laminate having excellent infrared transmittance and a black appearance, in which irradiated light and transmitted light in the visible light region have the same color.
[0010] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by the following optical laminate, and have thus completed the present invention. That is, the embodiments of the present invention include the following. However, the present invention is not limited to the following and includes various embodiments.
[0011] <1> An optical laminate having an optical functional layer on at least one surface of a substrate, the optical functional layer comprising a colorant containing multiple types of pigments and a binder resin, the optical laminate having an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm, and an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfying at least one of the following formulas (1A) and (2A), where T1 is the maximum spectral transmittance at wavelengths of 350 nm or more but less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm or more but less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm or more but less than 750 nm: 0.1≦T1 / T2≦10 (1A) 1≦T3 / T2≦20 (2A)
[0012] <2> An optical laminate having an optical functional layer on at least one surface of a substrate, the optical functional layer comprising a colorant containing a plurality of types of pigments and a binder resin, the optical laminate having an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm, and an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfying the following formulas (1) and (2), where T1 is the maximum spectral transmittance at wavelengths of 350 nm or more but less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm or more but less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm or more but less than 750 nm: 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)
[0013] <3> The optical laminate according to <1> or <2>, wherein the colorant containing multiple pigments includes a combination of yellow pigment / red pigment / indigo pigment, red pigment / indigo pigment / green pigment, or yellow pigment / indigo pigment / purple pigment.
[0014] <4> The optical laminate according to any one of the above <1> to <3>, wherein the colorant containing multiple types of pigments contains a combination of yellow pigment / red pigment / indigo pigment.
[0015] <5> The optical laminate according to any one of <1> to <4> above, which is for transmission viewing.
[0016] <6>L * a * b * In the color coordinates of the display system, the color coordinates of the light irradiated from the light source to the optical laminate (a * 1, b * 1) and the color coordinates (a * 2, b * 2) and the color difference (a * 2-a * 1), and (b * 2-b * <1> <5>, wherein 1) satisfies the following formulas (3) and (4): * 2-a * 1)<10 (3) -10<(b * 2-b * 1) <10 (4)
[0017] <7> The optical laminate according to any one of <1> to <6>, wherein the optical functional layer further contains a dispersant.
[0018] <8> The optical laminate according to any one of the above <1> to <7>, wherein the binder resin contains at least one resin selected from the group consisting of an acrylic resin, a polyester resin, and an epoxy resin.
[0019] <9> A method for producing the optical laminate according to the above item <1> or <2>, comprising a step of applying a colorant containing multiple pigments and a black ink containing a binder resin onto a substrate to form an optical functional layer. The disclosure of the present application is related to the subject matter described in Japanese Patent Application No. 2023-097565, filed on June 14, 2023, the entire disclosure of which is incorporated herein by reference.
[0020] According to the present invention, an optical laminate having excellent infrared transmittance and a black appearance can be provided. Also, according to the present invention, an optical laminate having excellent infrared transmittance and a black appearance, in which irradiated light and transmitted light in the visible light region have the same color, can be provided.
[0021] 1 is a graph showing the transmission spectrum of the optical laminate of Example 1 at wavelengths of 320 nm to 800 nm.
[0022] The following describes in detail an embodiment of the present invention, but the following description of the constituent elements is one example (typical example) of the present invention. The present invention is not limited to the contents of the embodiment described below, and various modifications can be made without departing from the gist of the present invention.
[0023] <Optical Laminate> An optical laminate according to one embodiment of the present invention has at least a substrate and an optical functional layer. The optical laminate may have an optical functional layer on at least one surface of the substrate. The optical functional layer may be formed so as to cover the entire surface or a portion of the substrate. In the optical laminate of the embodiment, the optical functional layer contains a colorant containing multiple types of pigments and a binder resin. The optical functional layer can be formed by printing (coating) an ink containing at least a colorant and a binder resin on the substrate. That is, the optical functional layer may be a coating (printed layer) of the ink.
[0024] The optical laminate of the above embodiment is characterized in that it has an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm, an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfies at least one of the following formulas (1A) and (2A), where T1 is the maximum spectral transmittance at wavelengths of 350 nm or more but less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm or more but less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm or more but less than 750 nm. In one embodiment, it is preferable that both of the following formulas (1A) and (2A) are satisfied: 0.1≦T1 / T2≦10 (1A) 1≦T3 / T2≦20 (2A)
[0025] By including multiple pigments in the optical functional layer, the multiple pigments can complement each other to absorb visible light that cannot be absorbed by a single pigment. Furthermore, by setting the average spectral transmittance at wavelengths of 350 nm to 750 nm to 25% or less, an optical laminate with high blackness can be obtained, making it possible to match the color of the optical laminate with the surrounding components used in combination (seamless). Furthermore, by setting the average spectral transmittance at wavelengths of 850 nm to 2500 nm to 85% or more, the laminate covering the infrared light source or infrared receiver can be easily matched with the surrounding components without impairing the infrared sensor sensitivity.
[0026] In the optical laminate of the above embodiment, the average spectral transmittance in the wavelength range of 350 nm to 750 nm may be adjusted to a value of 25% or less. In one embodiment, the average spectral transmittance is preferably 20% or less, and more preferably 15% or less. By adjusting the average spectral transmittance to 25% or less, the OD value (optical density) of the optical laminate is increased, and a black appearance can be easily obtained.
[0027] The lower limit of the average spectral transmittance for wavelengths of 350 nm to 750 nm varies depending on the application of the optical laminate. For example, when the optical laminate is used for transmissive viewing, the lower limit of the average spectral transmittance may be 0.01%. An average spectral transmittance of 0.01% or more allows the minimum amount of light required for transmissive viewing to be transmitted. Therefore, in one embodiment, the average spectral transmittance for wavelengths of 350 nm to 750 nm of the optical laminate may be 0.01% to 25%. When the average spectral transmittance is adjusted to 0.01% to 25%, the optical laminate can be suitably used for transmissive viewing applications, and an optical laminate having a black appearance can be easily provided. Here, transmissive viewing means that light irradiated from a light source can be viewed as transmitted light through the optical laminate. More preferably, it means that the color tone of the transmitted light visible through the optical laminate is identical to that of the light irradiated from the light source. Specific examples of applications for transmissive viewing include transmissive viewing components in display-type optical devices such as display-type automobile panels.
[0028] On the other hand, when the optical laminate is used for purposes other than transmission viewing, the average spectral transmittance may be less than 0.01%, for example, 0.00001%, or may be a value as close to 0 as possible. By bringing the average spectral transmittance closer to 0, the visible light blocking ability can be improved, and a black appearance with a high degree of blackness can be easily obtained. Examples of uses other than transmission viewing include a cover member that covers a sensor part in an optical device. More specifically, the laminate can be suitably used, for example, as part of a cover member that covers a side-view camera of an automobile. Since the laminate has a black appearance with a high degree of blackness, it is easy to enhance the decorative properties of the laminate.
[0029] The black appearance of the optical laminate can be evaluated by optical density (OD value). The OD value of the optical laminate is preferably 1 or more, more preferably 1.4 or more, and even more preferably 2 or more. The OD value is a logarithmic value of the absorbance measured by a transmission densitometer after irradiating the optical laminate with light in the visible light range. The higher the OD value, the higher the degree of blackness.
[0030] In the optical laminate of the above embodiment, the average spectral transmittance in the wavelength range of 850 nm to 2500 nm may be adjusted to a value of 85% or more. In one embodiment, the average spectral transmittance is preferably 87% or more, and more preferably 90% or more. When used as a decorative member for an infrared sensor, the average spectral transmittance of 85% or more can minimize interference with infrared transmission and reception, and the sensitivity of the sensor can be easily improved.
[0031] The optical laminate of the above embodiment is characterized in that the average spectral transmittance at wavelengths of 350 nm to 750 nm and at wavelengths of 850 nm to 2500 nm is within the above range, and in addition, at least one of the above formulas (1A) and (2A) is satisfied. By satisfying the above formulas (1A) and / or (2A), the lightness (L * value) to approach 0. As a result, the laminate has a blackish color tone, and it is easy to obtain a good black appearance.
[0032] In one embodiment, the maximum spectral transmittance "T1" of 350 nm or more and less than 460 nm may be present in a wavelength range of preferably 360 nm or more and less than 440 nm, more preferably 380 nm or more and less than 420 nm. The maximum spectral transmittance "T2" of 460 nm or more and less than 570 nm may be present in a wavelength range of preferably 480 nm or more and less than 560 nm, more preferably 500 nm or more and less than 540 nm. The maximum spectral transmittance "T3" of 570 nm or more and less than 750 nm may be present in a wavelength range of preferably 660 nm or more and less than 740 nm, more preferably 680 nm or more and less than 720 nm.
[0033] In one embodiment of the optical laminate, the maximum spectral transmittance "T1" of 350 nm or more and less than 460 nm, the maximum spectral transmittance "T2" of 460 nm or more and less than 570 nm, and the maximum spectral transmittance "T3" of 570 nm or more and less than 750 nm may be within ranges that satisfy the following formulas (A1) and (A2): 0.1≦T1 / T2<1 (A1) 1≦T3 / T2<2 (A2)
[0034] In one embodiment of the optical laminate, the maximum spectral transmittance "T1" of 350 nm or more but less than 460 nm, the maximum spectral transmittance "T2" of 460 nm or more but less than 570 nm, and the maximum spectral transmittance "T3" of 570 nm or more but less than 750 nm preferably satisfy the following formulas (1) and (2): 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2) When T1, T2, and T3 satisfy the ranges (1) and (2), blue, green, and red light can be transmitted in a suitable balance, and the irradiated light and the transmitted light in the visible light region are in the same color. Therefore, the transmitted light that has passed through the laminate can directly reproduce the color tone of the irradiated light from the light source. For example, when white light is used as the light source, the transmitted light is visually perceived as white, and when green light is used as the light source, the transmitted light is visually perceived as green.
[0035] In the above embodiment, T1, T2, and T3 may more preferably be in the following ranges: 1.2≦T1 / T2≦7 2.5≦T3 / T2≦15 T1, T2, and T3 may even more preferably be in the following ranges: 1.5≦T1 / T2≦5 3≦T3 / T2≦10
[0036] <Optical Functional Layer> The optical functional layer is preferably formed from a colorant containing multiple types of pigments and a black ink containing a binder resin. For example, the optical functional layer is obtained by applying the colorant containing multiple types of pigments and the black ink containing a binder resin to a substrate and drying it, and the resulting printed matter becomes an optical laminate. The film thickness of the optical functional layer can be adjusted appropriately depending on its purpose and application. In one embodiment, the film thickness is preferably 3 to 20 μm, more preferably 5 to 15 μm, and even more preferably 5 to 10 μm. When the film thickness is adjusted within the above range, the light blocking properties in the visible light region are improved, and an appearance with a higher degree of blackness can be easily obtained.
[0037] Ink that can be used to form the optical functional layer will be described below. The ink includes a colorant containing multiple pigments and a binder resin. From the viewpoint of obtaining a coating film with a black appearance, the colorant containing multiple pigments preferably has a black color tone. In one embodiment, the combination of multiple pigments may be, for example, a blue pigment, a yellow pigment, and a red pigment. In this way, by combining at least three pigments, a black ink that can easily achieve a black appearance in the optical laminate can be constructed. Specific examples of black inks will be described below.
[0038] [Black Ink] The black ink contains a colorant containing a plurality of types of pigments and a binder resin.
[0039] (Colorant) The colorant contains multiple types of pigments, and multiple types of pigments are mixed together to be used. By containing multiple types of pigments, the blackness of the appearance of the optical laminate is ensured, making it possible to create a seamless design with the same color as the surrounding components, and providing design features.
[0040] Examples of colorants include various organic pigments, inorganic pigments, dyes, etc. Pigments with high color development and heat resistance are preferred, and organic pigments are preferable. Among organic pigments, combinations of yellow pigment / red pigment / indigo pigment, red pigment / indigo pigment / green pigment, and yellow pigment / indigo pigment / purple pigment can be mentioned. From the viewpoint of uniform shielding properties in the visible light region, it is preferable that the combination of multiple pigments contains at least one of yellow pigment, red pigment, and indigo pigment. In addition to the above pigments, complementary color pigments such as orange pigment, green pigment, and purple pigment may be used as long as they do not interfere with the effects of the present invention.
[0041] Specific examples of organic pigments that can be used as colorants are shown below by color index numbers. Note that "C.I." in this specification stands for Color Index (C.I.).
[0042] Yellow pigments include C.I. Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35: 1, 36, 36: 1, 37, 37: 1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 125, 12 Suitable examples of the yellow pigment that can be used include C.I. 6, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 198, 199, 213, 214, 218, 219, 220, 221, and 231. Although not particularly limited, in one embodiment, the yellow pigment is C.I. Pigment Yellow 110, 150, and 139.
[0043] As red pigments, C.I. Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 57:1, 81, 81:1, 81:2, 81:3, 81:4, 97, 122, 123, 146, 149, 150, 168, 169, 176, 177, 178, 180, 184, 185, 187, 192, 200, 202, 208, 209, 210, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, 242, 246, 254, 255, 264, 268, 270, 272, 273, 274, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, etc. can be suitably used. Although not particularly limited, in one embodiment, the red pigment may include at least one selected from the group consisting of C.I. Pigment Red 122, 254, and 264.
[0044] Suitable indigo pigments include C.I. Pigment Blue 1, 1:2, 1:3, 2, 2:1, 2:2, 3, 8, 9, 10, 10:1, 11, 12, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 18, 19, 22, 24, 24:1, 53, 56, 56:1, 57, 58, 59, 60, 61, 62, and 64. Although not particularly limited, in one embodiment, the yellow pigment may include at least one selected from the group consisting of C.I. Pigment Blue 15:3, 15:4, and 15:6.
[0045] As the orange pigment, C.I. Pigment Orange 36, 38, 43, 51, 55, 59, 61, 71, 73, etc. can be suitably used. Although not particularly limited, in one embodiment, the orange pigment may include at least one selected from the group consisting of C.I. Pigment Orange 43, 71, and 73.
[0046] As the green pigment, C.I. Pigment Green 7, 10, 36, 37, 58, 62, 63, etc. can be suitably used. Although not particularly limited, in one embodiment, the green pigment may include at least one selected from the group consisting of C.I. Pigment Green 7, 10, and 36.
[0047] As the purple pigment, C.I. Pigment Violet 1, 19, 27, 29, 30, 32, 37, 40, 42, 50, etc. can be suitably used. Although not particularly limited, in one embodiment, the purple pigment may include at least one selected from the group consisting of C.I. Pigment Violet 23, 27, and 29.
[0048] Examples of inorganic pigments include titanium oxide, carbon black, aluminum paste, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, and iron black. Examples of extender pigments include silica, alumina, talc, calcium carbonate, precipitated barium, and the like. Inorganic pigments are preferably used in combination with organic pigments to ensure good coatability, sensitivity, developability, and the like while maintaining a balance between saturation and brightness.
[0049] When a black ink containing carbon black is used, a black coating film can be easily obtained. However, as the carbon black content in the optical functional layer increases, the transmittance in the infrared region decreases. From this perspective, the carbon black content in the optical functional layer is preferably less than 2.5% by mass, based on the total mass of the optical functional layer. When the carbon black content is adjusted to less than 2.5% by mass, the transmittance in the infrared region can be easily adjusted to 85% or more. The content may more preferably be 1.0% by mass or less, and even more preferably 0.5% by mass or less. In one embodiment, it is preferable that the optical functional layer is substantially free of carbon black. Here, "substantially free" means that carbon black is not intentionally used, and the content may be 0.1% by mass or less, or even 0% by mass.
[0050] The content of the colorant in the total solid components of the black ink (total mass of the optical functional layer) is preferably 10 to 45 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 35 mass%. By adjusting the colorant content within the above range, good light-blocking properties are achieved, and an appearance with a higher degree of blackness can be obtained. Here, the content of the colorant in the optical functional layer corresponds to the proportion of the colorant content based on the total mass of the solid components in the black ink. The same applies to the content of solid components such as pigments and binder resins described below.
[0051] In the optical laminate of the present invention, from the viewpoint of satisfying the above-mentioned transmittance, in the case of a combination of yellow pigment / red pigment / indigo pigment, the total solid components of the black ink (total mass of the optical functional layer) preferably contain 0.1 to 10 mass% yellow pigment, 0.1 to 10 mass% red pigment, and 0.1 to 10 mass% indigo pigment. It is more preferable to contain 0.1 to 4 mass% yellow pigment, 0.1 to 8 mass% red pigment, and 0.1 to 8 mass% indigo pigment. It is even more preferable to contain 0.1 to 3 mass% yellow pigment, 0.1 to 6 mass% red pigment, and 0.1 to 6 mass% indigo pigment. The blending ratio of the pigments is preferably yellow pigment / red pigment / indigo pigment = 5 to 40 / 5 to 60 / 5 to 60, more preferably 10 to 30 / 10 to 50 / 10 to 50, and even more preferably 10 to 30 / 25 to 50 / 25 to 50. The yellow pigment is C. When C.I. Pigment Yellow 139 is used as the red pigment, C.I. Pigment Red 264 is used as the crimson pigment, and C.I. Pigment Blue 15:6 is used as the indigo pigment, excellent shielding properties can be exhibited in the visible light region, which is preferable.
[0052] In the case of a combination of red pigment / indigo pigment / green pigment, the red pigment is preferably contained in an amount of 0.1 to 10% by mass, the indigo pigment in an amount of 0.1 to 10% by mass, and the green pigment in an amount of 0.1 to 10% by mass, based on the total solid components of the black ink (total mass of the optical functional layer). It is more preferable to contain the red pigment in an amount of 0.1 to 8% by mass, the indigo pigment in an amount of 0.1 to 4% by mass, and the green pigment in an amount of 0.1 to 8% by mass. It is even more preferable to contain the red pigment in an amount of 0.1 to 6% by mass, the indigo pigment in an amount of 0.1 to 3% by mass, and the green pigment in an amount of 0.1 to 6% by mass. The blending ratio of the pigments is preferably red pigment / indigo pigment / green pigment = 5 to 60 / 5 to 40 / 5 to 60, more preferably 10 to 50 / 10 to 30 / 10 to 50, and even more preferably 30 to 50 / 20 to 30 / 30 to 50. The red pigment is preferably C.I. It is preferable to use C.I. Pigment Red 264 as the blue pigment, C.I. Pigment Blue 15:6 as the indigo pigment, and C.I. Pigment Green 7 as the green pigment.
[0053] Furthermore, in the case of a combination of yellow pigment / indigo pigment / violet pigment, the yellow pigment is preferably contained in an amount of 0.1 to 10% by mass, the indigo pigment in an amount of 0.1 to 10% by mass, and the violet pigment in an amount of 0.1 to 10% by mass, based on the total solid components of the black ink (total mass of the optical functional layer). It is more preferable to contain the yellow pigment in an amount of 0.1 to 8% by mass, the indigo pigment in an amount of 0.1 to 4% by mass, and the violet pigment in an amount of 0.1 to 8% by mass. It is even more preferable to contain the yellow pigment in an amount of 0.1 to 6% by mass, the indigo pigment in an amount of 0.1 to 3% by mass, and the violet pigment in an amount of 0.1 to 6% by mass. The blending ratio of the pigments is preferably yellow pigment / indigo pigment / violet pigment = 5 to 60 / 5 to 40 / 5 to 60, more preferably 10 to 50 / 10 to 30 / 10 to 50, and even more preferably 30 to 50 / 20 to 30 / 30 to 50. C.I. is used as the yellow pigment. It is preferable to use C.I. Pigment Yellow 139 as the indigo pigment, C.I. Pigment Blue 15:6 as the blue pigment, and C.I. Pigment Violet 23 as the violet pigment.
[0054] Furthermore, in the case of a combination of yellow pigment / red pigment / violet pigment, the yellow pigment is preferably contained in an amount of 0.1 to 10% by mass, the red pigment in an amount of 0.1 to 10% by mass, and the violet pigment in an amount of 0.1 to 10% by mass, based on the total solid components of the black ink (total mass of the optical functional layer). It is more preferable to contain the yellow pigment in an amount of 0.1 to 8% by mass, the red pigment in an amount of 0.1 to 4% by mass, and the violet pigment in an amount of 0.1 to 8% by mass. It is even more preferable to contain the yellow pigment in an amount of 0.1 to 6% by mass, the red pigment in an amount of 0.1 to 3% by mass, and the violet pigment in an amount of 0.1 to 6% by mass. The blending ratio of the pigments is preferably yellow pigment / red pigment / violet pigment = 5 to 60 / 5 to 40 / 5 to 60, more preferably 10 to 50 / 10 to 30 / 10 to 50, and even more preferably 30 to 50 / 20 to 30 / 30 to 50. The yellow pigment is preferably C.I. It is preferable to use C.I. Pigment Yellow 139 as the red pigment, C.I. Pigment Red 264 as the crimson pigment, and C.I. Pigment Violet 23 as the violet pigment.
[0055] (Binder Resin) The binder resin refers to a resin that can function as a binder in the colored ink. It may be a thermoplastic resin or a thermosetting resin, and is preferably a thermoplastic resin. Examples of thermoplastic resins include acrylic resins, polyester resins, epoxy resins, styrene-based resins, rosin-based resins, styrene-maleic acid resins, dammar resins, polycarbonate resins, rosin-modified maleic acid resins, rosin ester resins, terpene resins, and urethane resins. These resins may be used in combination as long as the effects of the present invention are not impaired. Thermoplastic resins that can react with crosslinking agents such as isocyanates can also be used as thermosetting resins.
[0056] From the viewpoint of adhesion to the substrate during the formation of the coating film (optical functional layer), the binder resin preferably contains at least one thermoplastic resin selected from the group consisting of acrylic resin, polyester resin, and epoxy resin. The binder resin more preferably contains an acrylic resin. When the binder resin contains an acrylic resin, the content of the acrylic resin in the binder resin is preferably 70% by mass or more, more preferably 80% by mass or more, based on the total mass of the binder resin.
[0057] When the binder resin contains an acrylic resin, the acid value of the acrylic resin is preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, even more preferably 10 mgKOH / g or less, still more preferably 5 mgKOH / g or less, and particularly preferably 1 mgKOH / g or less.
[0058] When the binder resin contains an acrylic resin, the hydroxyl value of the acrylic resin is preferably 1 mgKOH / g or more, more preferably 10 mgKOH / g or more, even more preferably 20 mgKOH / g or more, and particularly preferably 25 mgKOH / g or more.
[0059] When the binder resin contains an acrylic resin, the reactive functional group value (the sum of the acid value and the hydroxyl value) of the acrylic resin is preferably 1 to 50 mgKOH / g, more preferably 5 to 40 mgKOH / g, and even more preferably 10 to 35 mgKOH / g.
[0060] As used herein, "acrylic resin" refers to a copolymer of (meth)acrylic acid and a (meth)acrylic acid derivative such as a (meth)acrylic acid ester. A monomer having an ethylenically unsaturated bond other than (meth)acrylic acid and a (meth)acrylic acid derivative may also be used as a monomer for forming the copolymer. Examples include styrene. In one embodiment, the (meth)acrylic acid derivative may be a compound in which the hydrogen atom of the carboxyl group is substituted with an alkyl group or a hydroxyalkyl group. The alkyl group may have 1 to 8 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably 1 to 4 carbon atoms. Examples include ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. The same applies to the alkyl group of the hydroxyalkyl group. Examples of such compounds include 2-hydroxyethyl (meth)acrylate.
[0061] Although not particularly limited, the acrylic resin may be a copolymer of (meth)acrylic acid / (meth)acrylic acid alkyl ester / (meth)acrylic acid hydroxyalkyl ester / styrene, more specifically, a copolymer of (meth)acrylic acid / stearyl (meth)acrylate / methyl (meth)acrylate / 2-hydroxyethyl (meth)acrylate / styrene.
[0062] The weight average molecular weight of the binder resin is preferably 5,000 to 120,000, more preferably 20,000 to 100,000, and even more preferably 30,000 to 80,000. When a binder resin having a weight average molecular weight within the above range is used, printability can be easily improved.
[0063] The content of the binder resin in the total solid components of the black ink (total mass of the optical functional layer) is preferably 40 to 80 mass%, more preferably 45 to 75 mass%, and even more preferably 50 to 70 mass%, because this improves dispersion stability.
[0064] The mass ratio of the total amount of colorants to the binder resin in the total solid components of the black ink (total mass of the optical functional layer) is preferably 85 / 15 to 60 / 40, more preferably 80 / 20 to 65 / 35. This ratio improves the light-blocking properties and provides an appearance with a higher degree of blackness.
[0065] The black ink used to form the optical functional layer may further contain a photocurable resin as a binder resin in addition to the thermoplastic resin. However, when a photocurable resin is used, curing tends to be insufficient, resulting in poor lightfastness. Furthermore, the presence of a curable resin, such as an acrylic monomer, in the ink system can disrupt the compatibility balance and cause the pigment dispersion to become unstable. Unstable pigments tend to stabilize themselves through aggregation. Aggregated pigment particles diffuse light, resulting in a high haze value. For this reason, when a photocurable resin is used, the transmittance in the near-infrared region decreases, which may contribute to a decrease in sensor sensitivity. From this perspective, the content of the thermoplastic resin in the binder resin is preferably 60% by mass or more. Based on the total mass of the binder resin, the content of the thermoplastic resin is more preferably 70% by mass or more, and even more preferably 80% by mass or more. In one embodiment, the content of the thermoplastic resin may be 100% by mass.
[0066] (Dispersant) The black ink used to form the optical functional layer preferably further contains a dispersant. The dispersant has the effect of suppressing pigment aggregation in the black ink and improving dispersion stability, and more preferably has a comb structure. In this specification, the term "comb structure" refers to a (co)polymer structure in which repeating units are bonded as side chains to the main chain. When the dispersant has a comb structure, dispersion stability is improved.
[0067] The dispersant preferably has an acidic group, and more preferably has an acid value of 0.1 to 100 mgKOH / g. When the dispersant has an acidic group, it does not transmit light in the visible region, and exhibits excellent shielding properties.
[0068] The content of the dispersant is preferably 1 to 25 mass %, more preferably 2 to 20 mass %, and even more preferably 3 to 15 mass %, of the total solid content of the black ink (total mass of the optical functional layer). By adjusting the content of the dispersant within the above range, compatibility with the binder resin can be maintained, and the transparency of the coating film can be maintained without causing turbidity in the coating film.
[0069] The weight-average molecular weight of the dispersant is preferably 10,000 to 100,000, more preferably 10,000 to 50,000, and even more preferably 10,000 to 30,000. When the weight-average molecular weight is 10,000 or more, steric repulsion that contributes to dispersion stability is obtained, and aggregation of the pigment can be prevented. When the weight-average molecular weight is 100,000 or less, compatibility with the solvent can be maintained, and dispersion stability of the pigment can be maintained. For example, NOF Corporation's "Marialim SC-1015F" (comb structure, weight-average molecular weight 20,000) can be suitably used.
[0070] (Organic Solvent) The black ink may contain an organic solvent. Examples of the organic solvent include glycol ether organic solvents, ester organic solvents, aliphatic organic solvents, aromatic organic solvents, alcohol organic solvents, and cyclic ketone organic solvents. Among these, cyclic ketone organic solvents are preferred because of their good printability.
[0071] (Antifoaming Agent) The black ink preferably contains an antifoaming agent. The content of the antifoaming agent is preferably 0.1 to 5 mass %, and more preferably 0.3 to 4 mass %, relative to the total mass of the black ink.
[0072] In one embodiment, the viscosity of the black ink used to form the optical functional layer may be preferably 0.1 to 60 Pa s, more preferably 0.3 to 30 Pa s, and even more preferably 0.5 to 10 Pa s at 25° C. When the viscosity of the ink is adjusted to be within the above range, the printability is improved.
[0073] <Formation of Optical Functional Layer> In the optical laminate of the above embodiment, the optical functional layer can be formed by applying the black ink to the substrate. The application method may be, for example, screen printing, roll coater, dispenser coating, dip coating, brush coating, etc. Among these, screen printing, dispenser coating, or dip coating is preferred. It is preferable to use a cylinder press printing machine or a semi-automatic printing machine as the printing machine, and to use a resin material such as nylon or polyester, or a resin material such as stainless steel as the printing plate.
[0074] Although not particularly limited, screen printing is preferred from the viewpoints of film thickness and printability on molded products. Screen printing is a technique in which a screen made of synthetic fibers such as polyester or nylon or stainless steel is used as a printing plate, and a photosensitive emulsion is used to pattern areas where the ink is transparent and areas where it is not transparent, and then the ink is transferred to the substrate by pressing and moving the ink against the inner surface of the screen with a spatula-shaped rubber plate called a squeegee. The film thickness of the printed ink can be adjusted by the film thickness of the photosensitive emulsion applied to the substrate surface. After printing, the ink can be fixed to the substrate by volatilizing the solvent in the ink using a hot air oven.
[0075] <Substrate> The substrate used to form the optical laminate is not particularly limited, and a transparent substrate is preferred. Examples include inorganic substrates such as glass, polyester substrates such as polyethylene terephthalate, polyolefin substrates such as polyethylene, polypropylene, ethylene-vinyl acetate, and other polyolefin substrates, nylon substrates such as polyamide, acrylic substrates such as polymethyl methacrylate, polyvinyl chloride substrates, polycarbonate substrates, polyurethane substrates, epoxy substrates, and cyclic olefin substrates such as cycloolefin polymer (COP) and cycloolefin copolymer (COC). Laminates of these may also be used. Vapor-deposited substrates in which inorganic compounds such as silica, alumina, and aluminum are vapor-deposited onto the substrate can also be used, and the vapor-deposited surface may be further coated with polyvinyl alcohol or the like. Corona treatment, frame treatment, or stretching treatment may also be performed. Among the above, inorganic material substrates such as glass, polyester substrates such as polyethylene terephthalate, acrylic substrates such as polymethyl methacrylate (PMMA), and polycarbonate substrates are preferred.
[0076] The optical laminate of the above embodiment may further include a protective layer for protecting the optical functional layer in addition to the substrate and the optical functional layer. The presence of the protective layer improves resistance to light, weather resistance, scratch resistance, etc. It is preferable that the protective layer does not inhibit the desired effects of the present invention, such as infrared transmittance and visible light blocking ability. For example, the protective layer may be formed by coating a transparent resin such as a thermoplastic resin on the upper surface of the optical functional layer. Alternatively, the above-mentioned transparent substrate may be attached to the upper surface of the optical functional layer with an adhesive.
[0077] <Method for manufacturing optical laminate> The optical laminate of the above embodiment can be manufactured by a manufacturing method including a step of forming an optical functional layer by applying a colorant containing multiple types of pigments and a black ink containing a binder resin onto a substrate. The optical laminate has an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm and an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfies the following formulas (1A) and (2A), where T1 is the maximum spectral transmittance at wavelengths of 350 nm to less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm to less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm to 750 nm. 0.1≦T1 / T2≦10 (1A) 1≦T3 / T2≦20 (2A)
[0078] The method for producing the black ink is not particularly limited, and known methods can be applied. For example, a method can be used in which a colorant, a binder resin, and an organic solvent are uniformly stirred in a stirrer, then dispersed in a bead mill, and filtered through a filter. The printing conditions for the black ink are not particularly limited, but preferred coating methods are screen printing, dispenser coating, and dip coating. Preferred printing machines are cylinder press printing machines or semi-automatic printing machines. Preferred printing plates are made of resin materials such as nylon, polyester, and stainless steel.
[0079] <Use form of optical laminate> The use of the optical laminate according to one embodiment of the present invention is not particularly limited as long as it is an optical device. Examples include components for automobiles and home appliances. The optical laminate is also suitable as an optical component such as an optical filter used in infrared sensors of smartphones and the like. In particular, it can be suitably used as the above-mentioned transmission viewing component. In this specification, transmission viewing means viewing light irradiated onto the optical laminate from the side opposite the light source across the optical laminate.
[0080] More specifically, since the optical laminate has a black appearance, it can be used to form a cover member that also serves as an optical filter for an infrared sensor. An example of such a use is an infrared sensor cover including the optical laminate.
[0081] Furthermore, a sensor unit including an infrared sensor and a light source can be combined with the optical laminate of the above embodiment to form a display-type sensor panel. The optical laminate is installed in front of the sensor unit and transmits light from the light source to make it visible. In the above embodiment, the light source for irradiating the optical laminate is not particularly limited, but it is preferable to use an incandescent lamp, an EL lamp such as an organic EL lamp, or a light-emitting diode (LED).
[0082] Due to the optical properties of the optical laminate of this embodiment, it is preferable that the color tone of the irradiated light (incident light) irradiated onto the optical laminate from a light source and the color tone of the light (transmitted light) visible through the optical laminate are the same or do not differ significantly. In other words, it is preferable that the color difference between the irradiated light and the transmitted light is small.
[0083] In one embodiment, L * a * b * In the color coordinates of the display system, the color coordinates of the light irradiated from the light source to the optical laminate (a * 1, b * 1) and the color coordinates (a * 2, b * 2) and the color difference (a * 2-a * 1), and (b * 2-b * 1) can satisfy the following formulas (3) and (4): −10<(a * 2-a * 1)<10 (3) -10<(b * 2-b * 1) <10 (4)
[0084] When the color difference satisfies the above formulas (3) and (4), the color difference between the irradiated light and the transmitted light is small, and it is therefore easy to make the color tone of the light from the light source and the color tone of the light visible through the optical laminate the same. From this perspective, it is preferable that the color difference is as small as possible, and in one embodiment, it is preferable that the color difference is in the range of the following formulas (5) and (6). -5<(a * 2-a * 1)<5 (5) -5<(b * 2-b * 1) <5 (6)
[0085] The above L * a * b * Color coordinate a of the display system * , b * is a value expressed as color coordinates in the CIE (1976) display system based on values measured by a spectrophotometer after irradiating the optical laminate with light. The measurement can be carried out in accordance with JIS Z8781-4.
[0086] The present invention will be specifically described below using examples, but the present invention is not limited to the following examples. In the present invention, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0087] <1> Ink Preparation Examples <1-1> Synthesis of Binder Resin <Synthesis Example 1> (Synthesis of Acrylic Resin 1) 300 g of methyl ethyl ketone (MEK) was placed in a four-necked flask equipped with a stirrer, a reflux condenser, a nitrogen inlet pipe, an inlet pipe, and a thermometer, and the container was heated to 80°C while injecting nitrogen gas into the container. At the same temperature, a mixture of 38 g of methyl methacrylate (MMA), 53 g of butyl methacrylate (BMA), 16 g of 2-hydroxyethyl methacrylate (HEMA), 13 g of styrene (St), and 0.8 g of 2,2'-azobisisobutyronitrile (AIBN) was added dropwise over 1 hour to carry out a polymerization reaction. After the dropwise addition was completed, the mixture was further reacted at 80°C for 3 hours, and then a solution of 1.2 parts of 2,2'-azobisisobutyronitrile in 100 g of isophorone was added, and the mixture was reacted at 80°C for 1 hour to obtain acrylic resin 1 (weight average molecular weight 40,000, acid value 0.3 mgKOH / g, hydroxyl value 30 mgKOH / g).
[0088] <3-2> Preparation of Black Inks <Preparation Example 1> (Black Ink S1) The following ink ingredients, i.e., each color's finely divided pigment, dispersing resin, and isophorone, were stirred and mixed to homogeneity. This mixture was dispersed for 5 hours in an Eiger mill (Eiger Japan Co., Ltd., "Mini Model M-250 MKII") using zirconia beads with a diameter of 0.5 mm, and then filtered through a 5 μm filter to obtain a mixed color pigment dispersion. (Ink ingredients) - Yellow finely divided pigment C.I. Pigment Yellow 139 (LIONOGEN YELLOW 1090) 2 parts - Red finely divided pigment C.I. Pigment Red 264 (Cinilex DPP Rubine SR6T) 4 parts - Indigo finely divided pigment C.I. Pigment Blue 15:6 (LIONOGEN BLUE 7703) 4 parts Dispersant (NOF Corporation "Marialim SC-1015F", comb structure, weight average molecular weight 20,000) 5 parts Isophorone 35 parts
[0089] To the mixed pigment dispersion obtained above, 49 parts of the previously prepared acrylic resin 1 solution (resin / isophorone=24 / 25) and 1 part of an antifoaming agent (BYK-054, manufactured by BYK Japan KK) were added. These were mixed uniformly using a mixer rotary stirrer to obtain black ink S1.
[0090] Preparation Examples 2 to 21 (Preparation of Black Inks S2 to S14, T1 to T7) Using the same method as in Preparation Example 1, black inks S2 to S14 and T1 to T7 were obtained using the raw materials and blending ratios shown in Tables 1 and 2, respectively.
[0091] The abbreviations in Tables 1 and 2 are shown below. Unless otherwise specified, the numerical values in the tables represent "parts", and blanks indicate that no values are used.
[0092] (Pigments) C.I. Pigment Yellow 139 (product name "LIONOGEN YELLOW 1090" manufactured by Toyocolor Co., Ltd.) C.I. Pigment Red 264 (product name "Cinilex DPP Rubine SR6T" manufactured by Kikuchi Color Co., Ltd.) C.I. Pigment Blue 15:6 (product name "LIONOGEN BLUE 770" manufactured by Toyocolor Co., Ltd.) C.I. Pigment Violet 23 (product name "LIONOGEN VIOLET FG-6240" manufactured by Toyocolor Co., Ltd.) C.I. Pigment Green 7 (product name "LIONOGEN GREEN 8944" manufactured by Toyocolor Co., Ltd.) C.I. Pigment Black 10 (Mitsubishi Chemical Corporation product name: Mitsubishi Carbon Black MA8)
[0093] (Binder resin) Ultraviolet (UV) curable resin: EBECRYL8606 (manufactured by Daicel Allnex Corporation, weight average molecular weight 1400) Polyester resin: VYLON GK250 (manufactured by Toyobo Co., Ltd., number average molecular weight 10000, acid value <2 mg KOH / g, hydroxyl value 11 mg KOH / g) Epoxy resin: JER1010 (manufactured by Mitsubishi Chemical Corporation, number average molecular weight 5000, acid value <2 mg KOH / g) Urethane resin: Polylite OD-X-2523 (manufactured by DIC Corporation, molecular weight 3500, acid value 0.5 mg KOH / g, hydroxyl value 32 mg KOH / g)
[0094] (Photopolymerization initiator) Omnirad TPO (manufactured by IGM, 2,4,6-trimethylbenzoyldiphenylphosphine oxide)
[0095] <2> Production of Optical Laminate Production Example 1 (Production of Optical Laminate SS1) MICRO SLIDE GLASS (manufactured by Matsunami Glass Co., Ltd., large slide glass S9213, film thickness 1 mm) was used as a substrate, and the above black ink S1 was screen-printed onto this substrate using a screen printing plate (manufactured by NBC Meshtec, L-SCREEN, 250-015 / 255PW) to form a pattern, thereby forming an optical functional layer with a film thickness of 7 μm, and an optical laminate SS1 was obtained.
[0096] <Production Examples 2 to 25> (Production of Optical Laminates SS2 to SS14, TT1 to TT7, and UU1 to UU4) Optical laminates SS2 to SS14, TT1 to TT7, and UU1 to UU3 were obtained in the same manner as in Production Example 1, except that the black ink S1 used in Example 1 was replaced with the black inks listed in Tables 1 and 2. Furthermore, black ink U4 containing a UV-curable resin was used, and screen printing was performed in the same manner as in Production Example 1. The coating was then cured by irradiation with UV light (light source: metal halide lamp), yielding optical laminate UU4. The ultraviolet light irradiation was performed at a conveyor speed of 10 m / min, 120 W / cm, and an irradiation distance of 15 mm.
[0097] <3> Evaluation of Optical Laminates The optical laminates (optical functional layer thickness 7 μm) obtained in Production Examples 1 to 25 were evaluated for various properties as follows. <Spectral Transmittance of Optical Laminates> The spectral transmittance of the optical laminates was measured in the following wavelength range using a UV3600 ultraviolet-visible-near-infrared spectrophotometer manufactured by Shimadzu Corporation. The obtained measured values were evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Average spectral transmittance for wavelengths of 350 nm to 750 nm) A: 10% or less B: More than 10% and 25% or less C: More than 25% (Average spectral transmittance for wavelengths of 850 nm to 2500 nm) A: 90% or more B: 85% or more and less than 90% C: Less than 85%
[0098] <Evaluation 1 of Optical Properties of Optical Laminate> For the optical laminate, T1, T2, and T3 described below were measured using a UV3600 ultraviolet-visible-near-infrared spectrophotometer manufactured by Shimadzu Corporation. Maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm: T1 Maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm: T2 Maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm: T3 From the obtained measured values, the values of T1 / T2 and T2 / T3 were calculated and further evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Criteria for Evaluation 1 of T1 / T2) ◯: 0.1≦T1 / T2≦10 (Meets formula (1A)) ×: T1 / T2<0.1, or 10<T1 / T2 (Does not satisfy formula (1A)) (Criteria for Evaluation 1 of T3 / T2) ◯: 1≦T3 / T2≦20 (Meets formula (2A)) ×: T3 / T2<1, 20<T3 / T2 (Does not satisfy formula (2A))
[0099] <OD Value (Optical Density) of Optical Laminate> The OD value of the optical laminate in the visible light region was measured using a transmission densitometer Gretag Macbeth TD-931. The obtained measured values were evaluated according to the following criteria. The results are shown in Tables 1 and 2. The higher the OD value, the deeper the black color. A rating of "B" or higher is at a practical level. A: OD value of 1.4 or higher B: OD value of 1 or higher, but less than 1.4 C: OD value less than 1
[0100] <Haze Value> The haze value of the optical laminate in the infrared region (wavelength 850 nm) was measured using a haze meter HSP-150VIR manufactured by Murakami Color Research Laboratory Co., Ltd. The measurement was carried out in accordance with the method described in JIS K7361. The obtained measured values were evaluated according to the following criteria. The results are shown in Tables 1 and 2. A rating of "B" or higher is at a practical level. A: Haze value 3% or less B: Haze value greater than 3% and less than 10% C: Haze value greater than 10%
[0101]
[0102]
[0103] As can be seen from Tables 1 and 2, the optical laminates SS1 to SS14, TT2 to TT5, and UU1 to UU4, whose T1 / T2 and T3 / T2 values fall within the ranges defined by formula (1A) and / or formula (2A), are black with high OD values, have excellent transmittance in the infrared region (wavelengths of 850 nm to 2500 nm), and are also excellent in terms of haze value. In particular, compared with the optical laminates SS11 to SS14 and UU1 to UU4, the optical laminates SS1 to SS10 and TT2 to TT5 have good haze evaluation results using light with a wavelength of 850 nm. The optical laminate SS11 uses an ink that does not contain a dispersant, and the optical laminates SS12 to SS14 use an ink that contains a thermoplastic resin other than an acrylic resin as the binder resin. Furthermore, the optical laminates UU1 to UU3 use ink containing acrylic resin and a resin other than acrylic resin as the binder resin. The optical laminate UU4 uses ink containing acrylic resin and a UV-curable resin as the binder resin. These findings demonstrate that a good optical laminate with a low haze value can be easily constructed by adding a dispersant to the ink or increasing the acrylic resin content in the binder resin. On the other hand, the optical laminate TT1, which had an average spectral transmittance of more than 25% in the wavelength range of 350 nm to 750 nm, had a low OD value and poor optical density. Furthermore, the optical laminate TT7, which used carbon black, showed poor transmittance in the infrared region (wavelengths of 850 nm to 2500 nm).
[0104] <Evaluation 2 of Optical Properties of Optical Laminate> The values of T1 / T2 and T3 / T2 calculated in Evaluation 1 described above were evaluated according to the following criteria as Evaluation 2. The results are shown in Tables 3 and 4. For reference, Tables 3 and 4 also show the evaluation results of the average spectral transmittance at wavelengths of 350 nm to 750 nm, the average spectral transmittance at wavelengths of 850 nm to 2500 nm, and the OD value (optical density) shown above. (Criteria for T1 / T2 evaluation 2) A: 1.5≦T1 / T2≦5 B: 1≦T1 / T2<1.5, 5<T1 / T2≦10 C: T1 / T2<1, 10<T1 / T2 (Criteria for T3 / T2 evaluation 2) A: 3≦T3 / T2≦10 B: 2≦T3 / T2<3, 10<T3 / T2≦20 C: T3 / T2<2, 20<T3 / T2
[0105] <Color of transmitted light> The optical laminate was irradiated with white light or green light from a light source, and the color of the light transmitted through the optical laminate was visually confirmed and evaluated. The evaluation criteria are as follows. The results are shown in Tables 3 and 4. A rating of "B" or higher is at a practical level. A: Same color as the irradiated light (no discoloration) B: Slightly different color from the irradiated light (slight discoloration) C: Different color from the irradiated light (discoloration)
[0106] <Color Difference> According to the method described in JIS Z8781-4, the optical laminate was irradiated with light at an incident angle of 90 degrees, and the color difference was measured using a Spectral Haze Meter SH7000 manufactured by Nippon Denshoku Industries Co., Ltd., based on the L of CIE (1976). * a * b * Color coordinates (a * 2, b * On the other hand, the color coordinates (a 2) of the substrate of the optical laminate (MICRO SLIDE GLASS (manufactured by Matsunami Glass Co., Ltd., large slide glass S9213, film thickness 1 mm) were measured in the same manner as above. * 1, b * Next, the color difference was calculated from the above color coordinates by (a * 2-a * 1), and (b * 2-b * 1) was calculated and evaluated according to the following criteria. The results are shown in Tables 3 and 4. In the following evaluation criteria, (a* 2-a * 1) to a * , (b * 2-b * 1) to b * A rating of "B" or higher is a practical level. A: -5<a * <5, -5<b * <5 B:-10<a * <10, -10<b * <10 C: a * ≦-10, or 10≦a * , b * ≦-10, or 10≦b *
[0107]
[0108]
[0109] The optical laminates SS1 to SS14 and UU1 to UU4, in which the values of T1 / T2 and T3 / T2 fall within the ranges defined by formulas (1) and (2), are preferred embodiments of the present invention. As can be seen from Tables 3 and 4, the optical laminates SS1 to SS14 and UU1 to UU4 have a color-matched relationship between the irradiated light and the transmitted light in the visible light region (for example, the transmitted light when irradiated with white light is white). Furthermore, they have a high OD value and are black, have excellent transmittance in the infrared region, and have a color-matched relationship between the irradiated light and the transmitted light in the visible light region (the transmitted light when irradiated with white light is white). This demonstrates that they can be suitably used as a transmission-visible component.
[0110] On the other hand, the optical laminate TT1, which has an average spectral transmittance of more than 25% at wavelengths of 350 nm to 750 nm, has excellent visible light transmittance but a low OD value. Furthermore, the optical laminates TT2 to TT6, in which the values of T1 / T2 and T3 / T2 are outside the ranges defined by formulas (1) and (2), did not have the same color for the irradiated light and the transmitted light in the visible light region, resulting in poor visibility. Furthermore, the optical laminate TT7, which used carbon black, did not transmit much visible light, making it impossible to confirm the color of the transmitted light, and also resulted in poor infrared transmittance.
Claims
1. An optical laminate having a substrate and an optical functional layer on at least one surface of the substrate, the optical functional layer comprising a colorant containing a plurality of types of pigments and a binder resin, the optical laminate having an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm and an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfying at least one of the following formulas (1A) and (2A), where T1 is the maximum spectral transmittance at wavelengths of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm or more and less than 750 nm. 0.1≦T1 / T2≦10 (1A) 1≦T3 / T2≦20 (2A) 2. The optical laminate according to claim 1, wherein T1, T2, and T3 satisfy the following formulas (1) and (2): 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2) 3. The optical laminate according to claim 1 or 2, wherein in the colorant, the plurality of pigments include any one of the combinations of yellow pigment / red pigment / indigo pigment, red pigment / indigo pigment / green pigment, and yellow pigment / indigo pigment / violet pigment.
4. The optical laminate according to any one of claims 1 to 3, wherein in the colorant, the plurality of pigments include a combination of a yellow pigment, a red pigment, and a blue pigment.
5. The optical laminate according to any one of claims 1 to 4, which is for transmission viewing.
6. L * a * b * In the color coordinates of the display system, the color coordinates of the light irradiated from the light source to the optical laminate (a * 1, b * 1) and the color coordinate (a * 2, b * 2) and the color difference (a * 2-a * 1), and (b * 2-b * The optical laminate according to any one of claims 1 to 5, wherein -10<(a * 2-a *1)<10 (3) -10<(b * 2-b * 1) <10 (4) 7. The optical laminate according to any one of claims 1 to 6, wherein the optical functional layer further contains a dispersing agent.
8. The optical laminate according to any one of claims 1 to 7, wherein the binder resin contains at least one resin selected from the group consisting of acrylic resins, polyester resins, and epoxy resins.
9. A method for producing an optical laminate, comprising the step of applying a colorant containing multiple types of pigments and a black ink containing a binder resin onto a substrate to form an optical functional layer, wherein the optical laminate has an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm, an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfies at least one of the following formulas (1A) and (2A), where T1 is the maximum spectral transmittance at wavelengths of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at wavelengths of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at wavelengths of 570 nm or more and less than 750 nm. 0.1≦T1 / T2≦10 (1A) 1≦T3 / T2≦20 (2A)
Citation Information
Patent Citations
Curable composition, cured film, infrared transmission filter, and solid state image pickup device
JP2016177079A
Curable composition, cured film, infrared transmission filter, and solid state image pickup device
JP2016177273A
Photosensitive coloring composition, and cured film, light-shielding filter, color filter, image display device, solid-state imaging element, and infrared sensor, using photosensitive coloring composition
JP2022097344A
Cited By
Leather-like seat
JP2026138490A
Leather-like seat
JP7909640B1