Semiconductor device substrate and method for producing semiconductor device substrate

The semiconductor device substrate addresses thermal cycle durability by employing a gradient crystal grain size in copper plates bonded to a ceramic substrate, ensuring peeling is suppressed through stress dispersion, resulting in improved thermal cycle performance.

WO2024204805A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD

Patent Information

Application Number
PCT/JP2024/013282
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Semiconductor device substrates face durability issues in thermal cycles, leading to peeling of copper plates due to temperature changes, which existing technologies fail to adequately address.

Method used

A substrate design featuring a ceramic substrate with copper plates bonded via a gradient crystal grain size profile, where the average crystal grain size increases with distance from the interface, and a manufacturing method involving heating and pressure treatment to form a bonding layer, ensuring the copper plates are made of oxygen-free copper and subjected to specific temperature and cooling profiles.

Benefits of technology

The solution provides a substrate with enhanced thermal cycle durability, effectively suppressing copper plate peeling by dispersing stress through a gradient crystal grain size, thereby maintaining structural integrity under temperature fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013282_03102024_PF_FP_ABST
    Figure JP2024013282_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A semiconductor device substrate according to the present invention includes: a silicon nitride ceramic substrate that has a first surface and a second surface; a bonding layer that is disposed on the first surface and the second surface; and a copper plate that is disposed on the bonding layer. In the copper plate, the average crystal grain size of copper increases toward the side away from an interface between the bonding layer and the copper plate, and the copper plate has a region in which the average crystal grain size of copper at a first position separated from the interface by 20 μm is at least 25 μm and less than 100 μm, and in which the average crystal grain size of copper at a second position separated from the interface by 250 μm is at least 100 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Substrate for semiconductor device and method for manufacturing substrate for semiconductor device

[0001] The present invention relates to a substrate for a semiconductor device and a method for manufacturing a substrate for a semiconductor device.

[0002] BACKGROUND ART As a substrate for a semiconductor device used in a power transistor module or the like, a substrate in which a copper plate is provided on the surface of a silicon nitride ceramic substrate via a bonding agent is known (for example, Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2022-173209

[0004] However, durability under thermal cycling has been an issue for substrates for semiconductor devices, and there has been a demand for a substrate for semiconductor devices that can prevent peeling of the copper plate even under such an environment. The present invention has been made to solve this problem, and an object of the present invention is to provide a substrate for semiconductor devices that can prevent peeling of the copper plate even under thermal cycling, and a method for manufacturing the same.

[0005] Item 1. A substrate for a semiconductor device comprising: a ceramic substrate having a first surface and a second surface; a bonding layer disposed on the first surface and the second surface; and a copper plate disposed on the bonding layer, wherein the thickness of the copper plate is 0.3 mm or more, and the copper plate has a region in which the average crystal grain size of copper increases with increasing distance from the interface between the bonding layer and the copper plate, and the average crystal grain size of copper at a first position 20 μm away from the interface is 25 μm or more and less than 100 μm, and the average crystal grain size of copper at a second position 250 μm away from the interface is 100 μm or more.

[0006] Item 2. The substrate for a semiconductor device according to Item 1, wherein the copper plate has an average crystal grain size of copper at the second position of 100 μm or more and 600 μm or less.

[0007] Item 3. The substrate for a semiconductor device according to Item 1 or 2, wherein the copper plate has an average crystal grain size of copper at a third position 100 μm away from the interface, of 50 μm or more and less than 150 μm.

[0008] Item 4. The substrate for a semiconductor device according to any one of Items 1 to 3, wherein the copper plate is made of oxygen-free copper.

[0009] Item 5. A method for manufacturing a substrate for a semiconductor device, comprising: a first step of preparing a ceramic substrate having a first surface and a second surface; a second step of forming a brazing filler metal layer on the first surface and the second surface; a third step of arranging a copper plate on the brazing filler metal layer to obtain an intermediate product having the ceramic substrate, the brazing filler metal layer, and the copper plate; and a fourth step of arranging the intermediate product in a furnace and performing a heating and pressurizing treatment, wherein in the fourth step, the temperature of the intermediate product is raised to 800 to 900°C, and then cooled to the softening point of copper constituting the copper plate at a first average cooling rate of 2.8 to 12°C / min.

[0010] Item 6. The method for manufacturing a substrate for a semiconductor device according to Item 5, wherein in the fourth step, after the intermediate product is cooled to the softening point, the intermediate product is cooled at a second average cooling rate lower than the first average cooling rate.

[0011] Item 7. The method for manufacturing a substrate for a semiconductor device according to Item 5 or 6, wherein in the fourth step, the pressure in the heating and pressurizing treatment is 0.2 to 22 MPa.

[0012] Item 8. The method for manufacturing a substrate for a semiconductor device according to any one of Items 5 to 7, wherein cooling is performed in an inert gas atmosphere in at least a portion of the fourth step.

[0013] Item 9. The substrate for a semiconductor device according to any one of Items 5 to 8, wherein in the fourth step, the copper plate is formed of oxygen-free copper.

[0014] According to the present invention, a bonded substrate having high durability against thermal cycles can be obtained, and peeling of the copper plate due to temperature changes can be suppressed.

[0015] 1 is a cross-sectional view showing an embodiment of a semiconductor device having a substrate for a semiconductor device according to the present invention; FIG. 1 is a cross-sectional view showing the interface between a copper plate and a bonding layer; FIG. 2 is a flowchart showing a method for manufacturing a substrate for a semiconductor device; FIG. 3 is a cross-sectional view showing the manufacturing process of a substrate for a semiconductor device; FIG. 4 is a cross-sectional view showing the manufacturing process of a substrate for a semiconductor device; FIG. 5 is a cross-sectional view showing the manufacturing process of a substrate for a semiconductor device; FIG. 6 is a temperature profile in the manufacturing process of a substrate for a semiconductor device; FIG. 7 is a graph showing a general tendency showing the relationship between stress when a force is applied in a direction to peel the plate from the bonding layer and the distance in a planar direction from an end of a circuit pattern; and FIG. 8 is a cross-sectional view explaining the horizontal axis of FIG.

[0016] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of a substrate for a semiconductor device according to the present invention will now be described with reference to the accompanying drawings. Fig. 1 is a cross-sectional view of an example of a semiconductor device having a substrate for a semiconductor device according to this embodiment.

[0017] <1. Overview of Semiconductor Device> The semiconductor device according to this embodiment is used as a power module in various electronic devices such as smartphones, personal computers, large home appliances, railways, electric vehicles, power generation (wind power generation, solar power generation, fuel cells, etc.), air conditioners, industrial robots, commercial elevators, home microwave ovens, induction electric rice cookers, and UPS (uninterruptible power supplies).

[0018] As shown in FIG. 1, the semiconductor device 1 according to this embodiment includes a substrate 2 for a semiconductor device, a first bonding material 5, a second bonding material 5', a semiconductor chip 6, bonding wires 7, and a heat sink 8.

[0019] The substrate 2 for a semiconductor device includes a plate-shaped ceramic substrate 3 which is an insulator, a first copper plate 4 bonded to the upper surface (first surface) of the ceramic substrate 3 via a bonding layer 9, and a second copper plate 4′ bonded to the lower surface (second surface) via a bonding layer 9. The ceramic substrate 3 may be, for example, an aluminum oxide substrate, an aluminum nitride substrate, or a silicon nitride substrate.

[0020] The bonding layer 9 may contain an active metal. The active metal may be, for example, at least one active metal selected from the group consisting of titanium and zirconium. Alternatively, the bonding layer 9 may contain a metal other than the active metal. The metal other than the active metal contained in the bonding layer 9 may be, for example, at least one metal selected from the group consisting of silver, copper, indium, and tin. The bonding layer 9 may also contain nitrogen and / or silicon supplied from the ceramic substrate 3, and the supplied nitrogen and / or silicon may form a compound with the active metal. Furthermore, the bonding layer 13 may contain copper supplied from the copper plate 12.

[0021] The first copper plate 4 is patterned to form a transmission circuit, while the second copper plate 4' is formed in a flat plate shape. The copper plates 4, 4' can be made of, for example, oxygen-free copper.

[0022] A semiconductor chip 6 is bonded to the upper surface of the semiconductor device substrate 2, i.e., to a part of the upper surface of the first copper plate 4, via a first bonding material 5. The semiconductor chip 6 and the first copper plate 4 are also connected by bonding wires 7.

[0023] On the other hand, a heat sink 8 is bonded to the lower surface of the semiconductor device substrate 2, i.e., the lower surface of the second copper plate 4′, via a second bonding material 5′. The heat sink 8 is a known material and can be made of a metal such as copper.

[0024] The thicknesses of the ceramic substrate 3, the copper plates 4, 4', and the bonding layer 9 are not particularly limited, but for example, the thickness of the ceramic substrate is preferably 0.2 to 0.5 mm, the thickness of the copper plate is preferably 0.3 to 2 mm, more preferably 0.5 to 1.5 mm, and particularly preferably 0.7 to 1.3 mm. The thickness of the bonding layer is preferably 0.1 to 20 μm.

[0025] 2. Features of the Substrate for a Semiconductor Device The substrate 2 for a semiconductor device according to this embodiment is characterized in that it has a region in which the average crystal grain size of copper increases from the interface between the bonding layer 9 and each copper plate 4, 4′ along the thickness direction of each copper plate 4, 4′, as shown in Fig. 2. The profile of the average crystal grain size is configured as follows.

[0026] (1) In the copper plates 4, 4', the average crystal grain size of copper is 25 μm or more and less than 100 μm at a first position 20 μm away in the thickness direction from the interface with the bonding layer 9. (2) In the copper plates 4, 4', the average crystal grain size of copper is 100 μm or more at a second position 250 μm away in the thickness direction from the interface with the bonding layer 9.

[0027] In (2), it is preferable that the upper limit of the average crystal grain size is 600 μm. It is also preferable to specify the following (3): (3) In the copper plates 4, 4′, the average crystal grain size of copper at a third position 100 μm away from the interface with the bonding layer 9 in the thickness direction is 50 μm or more and less than 150 μm.

[0028] In this embodiment, the average crystal grain size of copper increases with increasing distance from the interface, at least in the region from the interface to 250 μm, but it is sufficient if this tendency is present at least in the region from the interface to 250 μm.

[0029] The average crystal grain size can be calculated as follows. First, a region on the surface of the copper plates 4, 4' of the substrate 2 for a semiconductor device is selected where a length of 10 mm or more can be ensured. In other words, a region on the copper plates 4, 4' that is not divided by patterning and where a length of 10 mm or more can be ensured is selected. Next, a length of 10 mm is selected, and the substrate 2 for a semiconductor device is cut so that a cross section including the midpoint of the selected length is exposed. Subsequently, the cut surface is polished by wide-area cross-section polishing.

[0030] Next, EBSD analysis is performed on the polished cross section to obtain an image. The obtained image is then magnified 50 times. Next, the number of intersections between 1 mm long reference lines 1 to 3 and the copper grain boundaries is counted, and the reference line length is divided by the number of intersections to calculate the average crystal grain size. Figure 2 shows an example, where the black circles on reference line 2 represent the intersections. In this example, there are eight intersections on reference line 2, so the average crystal grain size is 1000 μm / 8 = 125 μm.

[0031] The above measurement method and measurement results can be applied to both substrates for semiconductor devices in which the copper plates 4, 4' are patterned as shown in FIG. 1, and substrates for semiconductor devices in which no patterning is applied.

[0032] 3. Manufacturing Method of Substrate for Semiconductor Device> Next, a manufacturing method of a substrate for a semiconductor device will be described. Fig. 3 is a flowchart showing the manufacturing method of a substrate for a semiconductor device according to this embodiment. Figs. 4, 5, and 6 are cross-sectional views schematically showing intermediate products obtained during the manufacturing of the substrate for a semiconductor device.

[0033] First, a ceramic substrate 3 is prepared (Step S1). Next, as shown in FIG. 4, brazing filler metal layers 9i are formed on the upper and lower surfaces of the ceramic substrate 3 (Step S1). At this time, a paste containing an active metal brazing filler metal, a binder, and a solvent is prepared as the brazing filler metal layer 9i. This paste may further contain a dispersant, an antifoaming agent, etc. Next, the prepared paste is screen-printed on the upper and lower surfaces of the ceramic substrate 3. As a result, a screen-printed film is formed on each surface of the ceramic substrate 3. Next, the solvent contained in the formed screen-printed film is volatilized. As a result, the screen-printed film is transformed into a brazing filler metal layer 9i (Step S2). The brazing filler metal layer 9i contains an active metal brazing filler metal and a binder. However, the brazing filler metal layer 9i may be formed by a method other than this method.

[0034] The active metal brazing material includes a hydrogenation active metal powder and a metal powder. The hydrogenation active metal powder includes a hydride of at least one active metal selected from the group consisting of titanium and zirconium. The metal powder includes silver. The metal powder may include a metal other than silver. The metal other than silver is at least one metal selected from the group consisting of copper, indium, and tin. When at least one metal selected from the group consisting of copper, indium, and tin is included in the active metal brazing material, the melting point of the active metal brazing material decreases.

[0035] The active metal brazing material is preferably made of a powder having an average particle size of 0.1 μm or more and 20 μm or less. The average particle size can be obtained by measuring the particle size distribution using a commercially available laser diffraction particle size distribution measuring device and calculating the D50 (median diameter) from the measured particle size distribution. By using a powder having such a small average particle size for the active metal brazing material, the brazing material layer 9i can be made thin.

[0036] The brazing material layer 9i preferably has a thickness of 0.1 μm or more and 20 μm or less, and more preferably has a thickness of 0.1 μm or more and 5 μm or less.

[0037] 5, the copper plates 4, 4' are placed on the formed brazing material layer 9i (step S3), thereby obtaining an intermediate product 2i including the ceramic substrate 3, the copper plates 4, 4', and the brazing material layer 9i.

[0038] Next, the obtained intermediate product 2i is placed in a heating furnace and subjected to a heating and pressurizing treatment (step S4). This produces a bonding layer 9 as shown in Fig. 6. As a result, a substrate 2 for a semiconductor device is obtained, which includes a ceramic substrate 3, copper plates 4, 4', and a bonding layer 9, as shown in Fig. 6. The copper plates 4, 4' are bonded to the ceramic substrate 3 by the bonding layer 9.

[0039] When the intermediate product 2i is subjected to the heating and pressurizing treatment, heating is performed according to the temperature profile shown in Fig. 7. As shown in Fig. 7, the temperature inside the furnace is raised in a vacuum atmosphere so that the temperature of the intermediate product 1i reaches a maximum of 800 to 900°C (hereinafter referred to as the upper limit temperature). The temperature rise rate at this time can be set to, for example, 2 to 10°C / min. In this process, the vacuum atmosphere inside the furnace is maintained at 10°C / min in the temperature range in which the bonding layer is formed, that is, the time range from approximately 750°C or higher until cooling begins. -2 The pressure is adjusted to be equal to or less than 0.2 Pa. Pressurization is applied to the intermediate product 2i during the temperature increase process and until cooling is completed. At this time, the surface pressure applied to the intermediate product 2i can be adjusted to, for example, 0.2 Pa to 22 MPa. By applying pressure, the ceramic substrate 3, the brazing material layer 9i, and the copper plates 4, 4' can be reliably contacted and reacted with each other, thereby forming the bonding layer 9.

[0040] Next, the temperature of the intermediate product 2i is maintained at 800 to 900°C for a predetermined time (for example, 15 to 120 minutes), and then the intermediate product 2i is cooled. Cooling methods that can be applied include, for example, injecting an inert gas such as nitrogen into the furnace to lower the temperature in an inert gas atmosphere, or cooling in a vacuum atmosphere. When cooling in an inert gas atmosphere, the pressure is preferably equal to or higher than atmospheric pressure. Note that FIG. 7 shows a profile for cooling using an inert gas such as nitrogen.

[0041] In the process of cooling the intermediate product 2i, the intermediate product 2i is rapidly cooled from 800-900°C to the softening point of copper at a first average cooling rate of 2.8-12°C / min (preferably 5.0-9.0°C / min). After cooling to the softening point of copper, the intermediate product 2i is cooled at a second average cooling rate that is lower than the first average cooling rate. The second average cooling rate can be, for example, 1.5-2.8°C / min. The softening point of copper is approximately 200-300°C (250°C in FIG. 7 as an example), depending on the copper material.

[0042] Next, the copper plate 4 and the bonding layer 9 are patterned by etching or the like. As a result, the copper plate 4 is transformed into the patterned copper plate 4 shown in Fig. 1. The bonding layer 9 is also transformed into the patterned bonding layer 13 shown in Fig. 1.

[0043] <4. Features> As described above, in this embodiment, there is a region where the average crystal grain size of copper increases from the interface between the bonding layer 9 and the copper plates 4, 4' along the thickness direction of the copper plates 4, 4', and since the above (1) and (2) are particularly satisfied, peeling of the copper plates 4, 4' can be suppressed. If the average crystal grain size at the first position is small as in the above (1), peeling can be easily suppressed. This point will be explained with reference to FIGS. 8 and 9.

[0044] FIG. 8 shows the stress distribution at the bonding interface during thermal cycling. FIG. 9 is a diagram illustrating the horizontal axis of FIG. 8. During thermal cycling, high stress is generated at the bonding interface due to the difference in thermal expansion between the copper 4, 4' and the ceramic substrate 3. As shown in FIG. 8, if there is a gradient in the copper plates 4, 4' that increases the average crystal grain size of the copper, the force is dispersed, and the peak value of the stress generated at the interface is reduced. Therefore, the peak value of the stress is reduced below the threshold at which peeling occurs, and peeling can be suppressed.

[0045] On the other hand, when the cooling rate is low, the average crystal grain size tends to be approximately the same or to increase in size in the thickness direction.

[0046] Furthermore, as described above, if the temperature of the intermediate product is raised to 800 to 900°C and then cooled to the softening point at a first average cooling rate of 2.8 to 12°C / min, a gradient in the average copper crystal grain size can be formed in the copper plate. This is because cooling at a temperature above the softening point makes the copper crystals more mobile, making it possible to control the crystal grain size. Therefore, it is possible to manufacture a substrate for a semiconductor device that can suppress the above-mentioned copper peeling.

[0047] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0048] 1. Fabrication of a Substrate for a Semiconductor Device A 0.32 mm thick silicon nitride ceramic substrate and a 0.8 mm thick copper plate were prepared. A brazing filler metal was also prepared, having a thickness of 0.1 μm to 20 μm, and containing 40 wt % to 95 wt % silver and titanium hydride. The brazing filler metal was then applied to the top and bottom surfaces of the silicon nitride ceramic substrate by screen printing. A copper plate, made of oxygen-free copper for example, was then placed on top of the silicon nitride ceramic substrate to form an intermediate product. The softening point of the oxygen-free copper was 250°C.

[0049] Next, this intermediate product was placed in a furnace and heated according to the temperature profile shown in Figure 7. In the temperature-raising process, the temperature was raised to approximately 850°C at approximately 5°C / min, and pressure was applied to approximately 20 MPa at the maximum temperature. Thereafter, cooling was performed at the cooling rate shown in Tables 1 to 4, and when the temperature dropped to approximately 250°C, it was slowly cooled to room temperature. In this way, the substrates for semiconductor devices according to Examples 1 to 9 and Comparative Examples 1 to 3 were completed. In other words, three substrates for semiconductor devices were produced at one cooling temperature. Note that copper plate patterning was not performed on these substrates for semiconductor devices.

[0050] <2. Evaluation> The average crystal grain size of copper was measured at the first to third positions described above for the substrates for semiconductor devices according to Examples 1 to 9 and Comparative Examples 1 to 3. The results are shown in Tables 1 to 4. The measurement conditions were as described above.

[0051] Next, a thermal cycle test was conducted on the semiconductor device substrates according to Examples 1 to 9 and Comparative Examples 1 to 3. That is, after 3,000 cycles of temperature increase and decrease between -40°C and 175°C, an ultrasonic flaw detection test was conducted to check for peeling at the edge of the copper plate. The ultrasonic flaw detection test was conducted using a Hitachi Power Solutions ultrasonic flaw detection device FSesIII, using the reflection method. The results are as follows: those in which no peeling was confirmed were rated as OK, and those in which no peeling was confirmed were rated as NO. In the images obtained by the ultrasonic flaw detection test, gaps are generated between the copper plate and the bonding layer in the areas where peeling has occurred, and these gaps appear white, allowing the peeling to be confirmed.

[0052] The results in Table 5 confirm that copper plates having a region in which the average crystal grain size of copper increases with increasing distance from the interface between the copper plate and the bonding layer do not peel off in the thermal cycle test. On the other hand, in Comparative Examples 1 and 2, the average crystal grain size was the same regardless of the position from the interface. Furthermore, in Comparative Example 3, the average crystal grain size of copper increased with increasing distance from the interface, but the average crystal grain size at the first position exceeded 100 μm. Therefore, peeling of the copper plate occurred in Comparative Examples 1 to 3. Therefore, it was found that peeling of the copper plate can be suppressed if the copper plate has the above-described average crystal grain size gradient and the average crystal grain size at the first position is less than 100 μm.

[0053] 2... Substrate for semiconductor device 3... Ceramic substrate 4, 4'... Copper plate 9... Bonding layer

Claims

1. A substrate for a semiconductor device comprising: a ceramic substrate having a first surface and a second surface; a bonding layer disposed on the first surface and the second surface; and a copper plate disposed on the bonding layer, wherein the thickness of the copper plate is 0.3 mm or more, and the copper plate has a region in which the average crystal grain size of copper increases with increasing distance from the interface between the bonding layer and the copper plate, and the average crystal grain size of copper at a first position 20 μm away from the interface is 25 μm or more and less than 100 μm, and the average crystal grain size of copper at a second position 250 μm away from the interface is 100 μm or more.

2. The substrate for a semiconductor device according to claim 1, wherein the average crystal grain size of copper in the copper plate at the second position is 100 μm or more and 600 μm or less.

3. The substrate for a semiconductor device according to claim 1 or 2, wherein the average crystal grain size of copper in the copper plate at a third position 100 μm away from the interface is 50 μm or more and less than 150 μm.

4. The substrate for semiconductor device according to claim 1 or 2, wherein the copper plate is made of oxygen-free copper.

5. A method for manufacturing a substrate for a semiconductor device, comprising: a first step of preparing a ceramic substrate having a first surface and a second surface; a second step of forming a brazing material layer on the first surface and the second surface; a third step of arranging a copper plate on the brazing material layer to obtain an intermediate product having a ceramic substrate, the brazing material layer, and the copper plate; and a fourth step of arranging the intermediate product in a furnace and subjecting it to a heating and pressurizing treatment, wherein in the fourth step, the temperature of the intermediate product is raised to 800 to 900°C, and then cooled to the softening point of copper constituting the copper plate at a first average cooling rate of 2.8 to 12°C / min.

6. A method for manufacturing a substrate for a semiconductor device as described in claim 5, wherein in the fourth step, after the intermediate product is cooled to the softening point, it is cooled at a second average cooling rate lower than the first average cooling rate.

7. The method for manufacturing a substrate for a semiconductor device according to claim 5 or 6, wherein in the fourth step, the pressure in the heating and pressurizing treatment is 0.2 to 22 MPa.

8. The method for manufacturing a substrate for a semiconductor device according to claim 5 or 6, wherein cooling is performed in an inert gas atmosphere during at least a portion of the fourth step.

9. The method for manufacturing a substrate for a semiconductor device according to claim 5 or 6, wherein the copper plate is made of oxygen-free copper.

Citation Information

Patent Citations

  • Bonded substrate

    JP2022173209A

  • Power module substrate and manufacturing method therefor

    JP2019110223A

  • Ceramic circuit board and its manufacturing method

    JP2021143120A

  • Copper / ceramic joint and insulated circuit board

    JP2021190702A

  • Bonded substrate and method for manufacturing bonded substrate

    WO2021112187A1

Cited By

  • Semiconductor device substrate and method for producing semiconductor device substrate