Solid titanium catalyst component, catalyst for polymerizing olefin, and method for polymerizing olefin

The solid titanium catalyst component with a polyamide structure addresses the challenge of producing olefin polymers with wide molecular weight distribution and high heat of fusion, enhancing the heat resistance and rigidity of the polymers, suitable for diverse applications.

WO2024204845A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC

Patent Information

Application Number
PCT/JP2024/013472
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-04-01
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current olefin polymerization catalysts struggle to produce olefin polymers with a wide molecular weight distribution and high heat of fusion, which are essential for achieving optimal heat resistance and rigidity in materials like polypropylene.

Method used

A solid titanium catalyst component containing a polyamide compound with a specific structure, comprising magnesium, titanium, and halogen, is used in olefin polymerization to produce polymers with a wide molecular weight distribution and high heat of fusion, enhancing the heat resistance and rigidity of the resulting polymers.

Benefits of technology

The use of this catalyst component results in olefin polymers with improved moldability, rigidity, and high heat resistance, characterized by a wide molecular weight distribution and high heat of fusion, making them suitable for various applications including injection molded bodies and lithium ion battery separators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013472_03102024_PF_FP_ABST
    Figure JP2024013472_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This solid titanium catalyst component includes magnesium, titanium, halogen, and an amide compound specified by formula (1). This catalyst for polymerizing olefin includes the solid titanium catalyst component (I) and an organometallic compound catalyst component (II) containing a metal element selected from Group 1, Group 2, and Group 13 of the periodic table. This method for polymerizing olefin involves polymerizing olefin in the presence of the catalyst for polymerizing olefin.
Need to check novelty before this filing date? Find Prior Art

Description

Solid titanium catalyst component, catalyst for olefin polymerization, and method for polymerizing olefins

[0001] The present invention relates to a solid titanium catalyst component, an olefin polymerization catalyst containing the solid titanium catalyst component, and an olefin polymerization process using the olefin polymerization catalyst.

[0002] Catalysts containing a titanium compound supported on an active magnesium halide have been known as catalysts used to produce olefin polymers such as homopolymers of ethylene or α-olefins or ethylene-α-olefin copolymers. Hereinafter, "homopolymerization" and "copolymerization" may be collectively referred to as "polymerization."

[0003] Widely known examples of such olefin polymerization catalysts include catalysts called Ziegler-Natta catalysts, which contain titanium tetrachloride or titanium trichloride, and catalysts which contain a solid titanium catalyst component comprising magnesium, titanium, a halogen, and an electron donor, and an organometallic compound.

[0004] The latter catalyst exhibits high activity in the polymerization of ethylene as well as α-olefins such as propylene and 1-butene, and the resulting α-olefin polymers may have high stereoregularity.

[0005] Among the above catalysts, it has been reported that excellent polymerization activity and stereospecificity are exhibited when a catalyst comprising a solid titanium catalyst component supported with an electron donor selected from carboxylic acid esters, a typical example of which is phthalic acid ester, an aluminum-alkyl compound as a co-catalyst component, and a silicon compound having at least one Si—OR group (wherein R is a hydrocarbon group) is used (for example, Patent Document 1). In addition to phthalic acid esters, many other electron donors, such as polyvalent ether compounds, have also been investigated.

[0006] As a study on using an ester compound as an electron donor, a catalyst containing a carboxylic acid ester having a divalent or higher ester group has been disclosed (for example, Patent Document 2). The present applicant has also reported that an ester compound having a special cyclic structure can give polyolefins with a wide molecular weight distribution with high activity (Patent Document 3).

[0007] Catalysts containing substituted succinic acid esters as electron donors have been reported to produce polyolefins with broad molecular weight distributions. The present applicant has also reported catalysts containing polycarboxylic acid esters with special cyclic structures (Patent Documents 4 to 6).

[0008] Japanese Patent Application Laid-Open No. 57-63310 Special Publication No. 2005-517746 International Publication No. 2008 / 010459 International Publication No. 2006 / 077945 International Publication No. 2022 / 045232 International Publication No. 2022 / 138634

[0009] Polypropylene (propylene polymer), a representative example of polymers of olefins with three or more carbon atoms, is known to have the potential to exhibit heat resistance and rigidity comparable to that of general-purpose engineering plastics, despite its hydrocarbon structure. Furthermore, polyolefins, which have a hydrocarbon structure, are also materials with a relatively low environmental impact, since they emit fewer toxic gases when disposed of by combustion or when thermally recycled (a recycling method in which combustion heat energy is recovered as electricity or the like).

[0010] It is well known that the heat resistance of propylene polymers depends on their stereoregularity, but it also appears to depend on the relationship between stereoregularity and molecular weight and their distribution. It is also known that rigidity is affected not only by stereoregularity but also by molecular weight distribution. Technologies have been developed that allow for fairly high control of the stereoregularity, but with the recent advances in molding technology, it is thought that polymers with higher stereoregularity may exhibit unexpected physical properties. Having a wider molecular weight distribution may also further improve the balance of physical properties. From the viewpoint of heat resistance and heat-resistant rigidity, it is preferable that the polymer has a high melting point and a high heat of fusion.

[0011] In view of the above, an object of the present invention is to provide a solid titanium catalyst component, an olefin polymerization catalyst, and an olefin polymerization method which are capable of producing an olefin polymer having a broad molecular weight distribution, a high melting point, and a large heat of fusion.

[0012] As a result of extensive research, the present inventors have found that a solid titanium catalyst component containing a polyamide compound with a special structure can produce olefin polymers having a wide molecular weight distribution, a high melting point, and a large heat of fusion with high activity, and have thus completed the present invention. Examples of the present invention are shown below.

[0013] [1] A solid titanium catalyst component comprising magnesium, titanium, a halogen, and an amide compound specified by the following formula (1):

[0014] [In formula (1), C, C 1 and C 2 is a carbon atom, N is a nitrogen atom, R 1 and R 2 are each a hydrocarbon group, and R 3 ~R 6 are groups containing carbon, hydrogen, and an element selected from the group 15, 16, and 17 elements of the periodic table, 11 and R 12 are each a hydrogen atom or a hydrocarbon group, m is an integer of 0 to 10, A is a linking group selected from an aliphatic group, an alicyclic group, and an aromatic group, and when there are multiple As, they may all be groups having the same structure, or some or all of them may be groups having different structures.

[0015] [2] The solid titanium catalyst component according to item [1], wherein the amide compound is specified by the following formula (2):

[0016] [In formula (2), R 1 ~R 6 , R 11 , R 12 , C, C 1 , C 2 and N are the same as those in formula (1), m is an integer of 1 to 10, and a plurality of R x is a group containing carbon, hydrogen, and an element selected from the elements of Groups 15, 16, and 17 of the periodic table; R x can be bonded to each other to form a ring structure.

[0017] [3] R 11 and R 12[4] The solid titanium catalyst component according to item [1] or [2], wherein R is a hydrogen atom. 3 , R 4 , R 5 and R 6

[0013] [1] - [3], wherein is a hydrogen atom.

[0018] [5] An olefin polymerization catalyst comprising the solid titanium catalyst component (I) according to any one of items [1] to [4] and an organometallic compound catalyst component (II) containing a metal element selected from Groups 1, 2, and 13 of the periodic table.

[0019] [6] The olefin polymerization catalyst according to item [5], further comprising an electron donor (III). [7] An olefin polymerization method, comprising polymerizing an olefin in the presence of the olefin polymerization catalyst according to item [5] or [6].

[0020] According to the solid titanium catalyst component, olefin polymerization catalyst and olefin polymerization method of the present invention, it is possible to produce olefin polymers having a wide molecular weight distribution and particularly a high heat of fusion.

[0021] Therefore, it is expected that the use of the solid titanium catalyst component, olefin polymerization catalyst, and olefin polymerization method of the present invention will enable the production of olefin polymers that have not only moldability and rigidity but also high heat resistance.

[0022] The solid titanium catalyst component (I), the olefin polymerization catalyst, the process for producing an olefin polymer, and the propylene polymer according to the present invention will be described in detail below.

[0023] [Solid Titanium Catalyst Component (I)] The solid titanium catalyst component (I) according to the present invention is characterized by containing titanium, magnesium, a halogen, and an amide compound having a special structure (hereinafter sometimes simply referred to as "amide compound").

[0024] <Amide Compound> The amide compound is represented by the following formula (1).

[0025] In the above formula (1), C, C 1 , C2 is a carbon atom, and N is a nitrogen atom. A line like "-" indicates a covalent bond.

[0026] R 1 and R 2 are hydrocarbon groups. More specifically, they are each substituted or unsubstituted hydrocarbon groups having 1 to 20 carbon atoms, and are preferably substituted or unsubstituted hydrocarbons having 6 to 20 carbon atoms and having an aryl group, and may have a structure containing a heteroatom as described below. Examples of heteroatom-containing aryl groups include those having a basic skeleton in which the aryl structure itself contains a heteroatom, such as a pyrrole ring or a pyran ring, and those in which a substituent such as a heteroatom-containing hydrocarbon group, such as an alkoxy group, is bonded to a benzene ring.

[0027] The structure containing a hetero atom is typically a structure having a substituent containing a hetero atom, and a preferred example of such a substituent is a heteroatom-containing aryl group, and a particularly preferred example is an aryl group containing oxygen. 1 and R 2 is preferably a structure in which one of the carbon atoms contained therein is covalently bonded to the adjacent carbonyl carbon.

[0028] The above R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 11 , R 12 and A may be bonded to each other to form a ring structure. Preferred embodiments of these will be described later.

[0029] The R 1 and R 2 can bond with each other to form a ring structure. 1 , R 11 , R 3 , R 4 The substituents selected from can be bonded to each other to form a ring structure. 2 , R, which will be described later 12 , R 5 , R 6The substituents selected from can be bonded to each other to form a ring structure.

[0030] The R 3 and R 4 and a substituent selected from the group consisting of R 5 and R 6 The substituents selected from the above may be bonded to each other to form a ring structure. In this case, m, which will be described later, is preferably 1 or more.

[0031] The ring structure formed by these substituents and the linking group A described later is C in formula (1) as described later. 1 Carbon or C 2 Considering the mobility around the carbon, an alicyclic structure having 5 or more members is preferred, and a 6 or more membered ring is more preferred. On the other hand, the upper limit of the number of members in the ring structure is arbitrary, but is preferably a 10-membered ring, and more preferably an 8-membered ring. 1 carbon, C 2 It may be preferred that at least one of the carbon-containing structures is other than a cyclic structure.

[0032] R 3 ~R 6 is a group containing carbon, hydrogen, and an element selected from the elements of Groups 15, 16, and 17 of the periodic table. 3 ~R 6 are each a group selected from a hydrogen atom, a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a halogen atom.

[0033] The above R 3 ~R 6 In the formula (I), hydrogen atoms, carbon atoms, or both may be partially substituted with atoms selected from the group consisting of elements in Groups 15 to 17 of the periodic table, such as nitrogen atoms, oxygen atoms, phosphorus atoms, and halogen atoms. 3 ~R 6 includes embodiments of hydrocarbon groups containing atoms selected from the group consisting of elements in Groups 15 to 17 of the periodic table, such as nitrogen, oxygen, phosphorus, halogens, etc. The atoms may be substituted at one or more positions.

[0034] In the present invention, the expression "atom" such as a halogen atom or a hydrogen atom in the description of a substituent may naturally refer to an embodiment having a bond, such as "H-" or "Cl-", as represented by a structural formula.

[0035] In addition, the above R 3 and R 4 Ya, R 5 and R 6 When R forms a ring structure, it also includes an embodiment in which a carbon-carbon double bond is formed (in this case, the carbon-carbon double bond is considered to be a two-membered ring). 3 ~R 6 may bond with a linking group A described later to form a ring structure, but in that case, the embodiment in which a double bond is formed is excluded from the scope of the present invention. The reason why such a structure is suitable for the present invention will be described later.

[0036] The aforementioned R 3 ~R 6 is preferably a relatively low bulky substituent, and is particularly preferably a hydrogen atom. In solid titanium catalyst components containing organic compounds (generally referred to as internal donors), bulky compounds tend to be preferred in many cases. The reason why such low bulky substituents tend to be preferred in the present invention is currently unclear, but as will be described later, it is likely that the amide compound of the present invention tends to stably adopt a relatively suitable conformation as, for example, a component of an olefin polymerization catalyst, and therefore, the substituent R on the opposite side of the amide group 3 ~R 6 This is probably because a smaller bulky structure makes it more difficult for the coordination of olefins to be disturbed with titanium in the solid titanium catalyst component.

[0037] R 11 and R 12 is a hydrogen atom or a hydrocarbon group. The hydrocarbon group is 1 , R 2 This is the same as the aspect explained in R 11 and R 12 is preferably a hydrogen atom. 11 , R 12is hydrogen, i.e., a structure represented by "-NH", is considered to have active hydrogen, and it is known that as an internal donor component contained in a solid titanium catalyst component, it may function as a catalyst poison. In the present invention, the reason why even such an "-NH" structure exhibits a favorable effect is currently unknown, but the inventors speculate as follows.

[0038] The two "-NH" structures shown above are relatively close to each other, and are therefore expected to have a relatively strong interaction, such as a hydrogen bond. Furthermore, the "-NH" structure is also expected to have a relatively strong interaction with the carbonyl group of other amide groups for similar reasons. This may reduce its catalytic poisoning effect. Furthermore, this interaction suppresses the rotation of the amide group, favoring a "slightly stable" conformation with relatively little change, such as a pseudocyclic structure, which exhibits a relatively large twist. Therefore, it is thought that this interaction with titanium in the solid titanium catalyst component facilitates the formation of highly stereoregular active sites.

[0039] Based on the same idea as above, R 11 and R 12 and R are bonded to each other to form a ring structure, which is also expected to be a preferred embodiment of the present invention. 11 and R 12 In some cases, a hydrocarbon group is preferred, including the case where the ring structure is formed as described above.

[0040] From this viewpoint, the nitrogen atoms of at least two amide groups in the amide compound of the present invention are preferably bonded via 2 to 10 atoms including carbon (—C 1 -A m -C 2 It is preferable that the two amide groups are separated by 2 to 8 atoms, and more preferably 3 to 6 atoms. In this way, it is sometimes preferable that the two amide groups are neither too close nor too far apart.

[0041] In the amide compound of the present invention, A is a linking group selected from an aliphatic group, an alicyclic group, and an aromatic group, and when there are multiple A's, they may all be groups having the same structure, or some or all of them may be groups having different structures. The linking group can also be interpreted as a divalent substituent.

[0042] The above-mentioned linking group is preferably a substituent having an aliphatic structure, an alicyclic structure, or an aromatic structure. Among these, a substituent selected from an alicyclic structure or an aromatic structure is preferred, and a substituent having an alicyclic structure is more preferred. Such a substituent is preferably, for example, a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms. Examples of the hydrocarbon group having the above-mentioned substituent include the substituent having a heteroatom-containing substituent described above.

[0043] The amide compound of the present invention is more clearly a compound having a structure specified by the following formula (2).

[0044] Among the above, R 1 ~R 6 , R 11 , R 12 , C, C 1 , C 2 , N, and m are the same as in formula (1). x is R 3 ~R 6 When m is an integer of 1 to 10, the number of R x may be preferably bonded to each other to form a ring structure such as an alicyclic structure or an aromatic structure, and such a ring structure is more preferably an alicyclic structure.

[0045] In addition, within the scope of the present invention, the above (CR x 2) The chain structure may contain heteroatoms such as oxygen or nitrogen-containing groups between carbon atoms.

[0046] The amide compound of the present invention is a compound in which the linking group A and the nitrogen of the amide group are separated by one carbon atom (C 1 , C 2One of its characteristics is that it has a structure in which the bond is made via a bond bond. This type of structure is considered to be a structure with relatively little rigidity, and it is speculated that it easily adopts a relatively unstable (e.g., twisted) conformation with the titanium in the solid titanium catalyst component, as described above, thereby exhibiting the favorable effects described above.

[0047] In the amide compound of the present invention, m is an integer of 0 to 10. The preferred lower limit, depending on the structure of A, is 1, and more preferably 2. On the other hand, the preferred upper limit is 8, more preferably 7, and even more preferably 6. Within this range, the distance between at least two amide groups falls within an appropriate range, and it can be expected that the olefin polymerization performance of the present invention will be exhibited. When m is 0, the above-mentioned C 1 and C 2 The structure is such that the and are connected by a single bond.

[0048] The above R 1 ~R 12 Specific examples of hydrocarbon groups include monovalent hydrocarbon groups having 1 to 20 carbon atoms, preferably 1 to 10, more preferably 2 to 8, even more preferably 3 to 8, still more preferably 4 to 8, and particularly preferably 4 to 6 carbon atoms. Examples of such hydrocarbon groups include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups, such as substituted or unsubstituted aryl groups and substituted or unsubstituted cycloalkenyl groups, including methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, hexyl, heptyl, octyl, 2-ethylhexyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclohexyl, and phenyl groups. The alicyclic hydrocarbon groups and aromatic hydrocarbon groups may contain a substituent. Among these, n-butyl, isobutyl, hexyl, octyl, and phenyl groups are preferred, with n-butyl, isobutyl, and phenyl being even more preferred.

[0049] Furthermore, in the case of a hydrocarbon group containing an element of Groups 15 to 17 of the periodic table, such as nitrogen, oxygen, phosphorus, or a halogen, specific preferred examples include a carboxylic acid ester group, an aldehyde group, an acetyl group, a carbonyl structure-containing group such as an oxycarbonylalkyl group, an alkoxy group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted alkenyloxy group, a substituted or unsubstituted cycloalkyloxy group, a substituted or unsubstituted cycloalkenyloxy group, a substituted or unsubstituted aryloxy group, a substituted or unsubstituted heteroaryl group, a substituted or unsubstituted heteroaryloxy group, and a siloxy group. The heteroatom is preferably nitrogen or oxygen, more preferably oxygen.

[0050] Among the heteroatom-containing substituents, aryl groups containing oxygen-containing substituents are preferred, and specifically, preferred examples are structures in which an oxygen-containing substituent, such as an alkoxy group, an aryloxy group, an alkoxyalkyl group, an aryloxyalkyl group, or a substituent in which the oxygen of the above-mentioned substituent is substituted with a carbonyl group or a carboxyl group, is bonded to an aromatic skeleton. Among the above, substituents in which an alkoxy group or an aryloxy group is bonded to an aromatic skeleton are preferred, and more preferred are substituents in which an alkoxy group is bonded to an aromatic skeleton. The number of carbon atoms in the oxygen-containing substituent is preferably 1 to 10, more preferably 1 to 8, and even more preferably 1 to 6. More specifically, in addition to the above-mentioned methoxyphenyl group, ethoxyphenyl group, propyloxyphenyl group, isopropyloxyphenyl group, butoxyphenyl group, phenoxyphenyl group, etc. are preferred examples. Aryl groups containing such oxygen-containing substituents can be formed by R 1 , R 2 It may be particularly preferably used in the following cases.

[0051] Among the above, R 3 ~R 6 , R 11 , R 12can be exemplified by hydrocarbon groups such as a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted cycloalkyl group, a substituted or unsubstituted cycloalkenyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted alkenyloxy group, or a substituted or unsubstituted aryl group; or heteroatom-containing hydrocarbon groups such as a substituted or unsubstituted cycloalkyloxy group, a substituted or unsubstituted cycloalkenyloxy group, a substituted or unsubstituted aryloxy group, a substituted or unsubstituted heteroaryl group, or a substituted or unsubstituted heteroaryloxy group. Among these, as mentioned above, a hydrogen atom is preferred. The hydrocarbon group is preferably a substituent having 1 to 8 carbon atoms, more preferably 1 to 7, and particularly preferably 1 to 6 carbon atoms. Furthermore, among the above, alkyl groups not containing heteroatoms are preferred.

[0052] Specific examples of the linking group A of the present invention include divalent substituents corresponding to the structure of the monovalent substituents described above. Among them, preferred are methylene, ethylene, 1,3-propylene, 1,2-propylene, 1,4-butylene, 1-3 butylene, 2-3 butylene, 2,4 pentylene, 1,2-cyclopentylene, 1,3-cyclopentylene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, 1,2-cycloheptalene, 1,3-cycloheptalene, 1,4-cycloheptalene, 1,2-phenylene, and 1,3-phenylene.

[0053] Examples of such amide compounds include the following structures: The structural formulas of the exemplary compounds below may have stereoisomers, and although some of the isomeric structures are specified, they may also include isomeric structures not shown as examples.

[0054]

[0055]

[0056]

[0057]

[0058]

[0059]

[0060]

[0061]

[0062]

[0063]

[0064]

[0065]

[0066]

[0067]

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

[0074]

[0075]

[0076]

[0077]

[0078]

[0079]

[0080]

[0081]

[0082]

[0083]

[0084]

[0085]

[0086]

[0087]

[0088]

[0089] In the above structural formula, the methyl group is represented as "Me," the ethyl group as "Et," the butyl group as "Bu," and the phenyl group as "Ph." Also, "i" stands for "iso" and "t" stands for "tertiary."

[0090] These compounds may be used alone or in combination of two or more. Furthermore, these amide compounds may be used in combination with the catalyst component (b) or the catalyst component (c) described below, as long as the object of the present invention is not impaired.

[0091] The amide compound may also be formed during the preparation of the solid titanium catalyst component (I).

[0092] The method for producing an olefin polymer of the present invention tends to easily produce a polymer having a wide molecular weight distribution and a high melting point and heat of fusion with high activity. The reason for this is unclear at present, but the present inventors, taking into account the above-mentioned facts, believe that the amide moiety of the amide compound of the present invention tends to be relatively easily coordinated with titanium and magnesium of the solid titanium catalyst component, while the C bonded to the nitrogen of the amide group in the structural formula (1) in particular tends to be easily coordinated with titanium and magnesium of the solid titanium catalyst component. 1 carbon, C 2 In terms of rigidity around the carbon, the amide compound of the present invention is considered to have a loose structure, and therefore assumes a conformation with limited range of motion, which is thought to facilitate the production of olefin polymers with high stereoregularity and a wide molecular weight distribution (wider toward the high molecular weight side).In this case, since the stereoregularity of the polymer, particularly on the high molecular weight side, is high, it is likely to crystallize relatively easily for its molecular weight, and the nucleating agent effect is also exhibited, which is thought to facilitate the production of polymers with high melting points and heats of fusion.

[0093] The olefin polymers obtained by the process of the present invention are polymers obtained using a catalyst capable of adopting a wide range of conformations to some extent, and therefore can be polymers with a wide range of molecular weights even on the low molecular weight side. Therefore, there may be a large amount of components soluble in hydrocarbon solvents such as decane. Although such soluble components are usually feared to weaken the crystalline structure of the olefin polymer, the heat of fusion of the olefin polymers of the present invention tends to be high. This is probably because the nucleating effect of the high molecular weight components takes precedence.

[0094] In preparing the solid titanium catalyst component (I) of the present invention, in addition to the above-mentioned amide compound, a magnesium compound and a titanium compound are used.

[0095] <Magnesium Compound> Specific examples of such magnesium compounds include known magnesium compounds such as: magnesium halides such as magnesium chloride and magnesium bromide; alkoxymagnesium halides such as methoxymagnesium chloride, ethoxymagnesium chloride and phenoxymagnesium chloride; alkoxymagnesiums such as ethoxymagnesium, isopropoxymagnesium, butoxymagnesium and 2-ethylhexoxymagnesium; aryloxymagnesiums such as phenoxymagnesium; and magnesium carboxylates such as magnesium stearate.

[0096] These magnesium compounds may be used alone or in combination of two or more kinds. Furthermore, these magnesium compounds may be complex compounds or double compounds with other metals, or mixtures with other metal compounds.

[0097] Among these, halogen-containing magnesium compounds are preferred, and magnesium halides, especially magnesium chloride, are preferably used. Other preferred magnesium compounds include alkoxymagnesium compounds such as ethoxymagnesium. The magnesium compounds may also be derived from other substances, such as those obtained by contacting an organomagnesium compound, such as a Grignard reagent, with a titanium halide, a silicon halide, or a halogenated alcohol.

[0098] <Titanium Compound> Examples of titanium compounds include those represented by the general formula: Ti(OR') g X 4-g (wherein R' is a hydrocarbon group, X is a halogen atom, and g is 0≦g≦4) More specific examples include titanium tetrahalides such as TiCl4 and TiBr4; alkoxytitanium trihalides such as Ti(OCH3)Cl3, Ti(OC2H5)Cl3, Ti(O-n-C4H9)Cl3, Ti(OC2H5)Br3, and Ti(O-iso-C4H9)Br3; alkoxytitanium dihalides such as Ti(OCH3)2Cl2 and Ti(OC2H5)2Cl2; alkoxytitanium monohalides such as Ti(OCH3)3Cl, Ti(O-n-C4H9)3Cl, and Ti(OC2H5)3Br; and tetraalkoxytitanium such as Ti(OCH3)4, Ti(OC2H5)4, Ti(OC4H9)4, and Ti(O-2-ethylhexyl)4.

[0099] Among these, titanium tetrahalides are preferred, with titanium tetrachloride being particularly preferred. These titanium compounds may be used alone or in combination of two or more. Examples of the magnesium compounds and titanium compounds described above include compounds described in detail in Patent Documents 1 and 2.

[0100] <Method for preparing solid titanium catalyst component (I)> The solid titanium catalyst component (I) used in the present invention can be prepared by any known method without limitation, except for using the above-mentioned amide compound. Specific preferred methods include, for example, the following methods (P-1) to (P-4).

[0101] (P-1) A method in which a solid adduct consisting of a magnesium compound and the catalyst component (b) described below is contacted with an amide compound and a liquid titanium compound in the presence of an inert hydrocarbon solvent in a suspended state.

[0102] (P-2) A method in which a solid adduct consisting of a magnesium compound and the catalyst component (b) is contacted with an amide compound and a liquid titanium compound in multiple batches.

[0103] (P-3) A method in which a solid adduct consisting of a magnesium compound and catalyst component (b) is contacted with an amide compound and a liquid titanium compound in the presence of an inert hydrocarbon solvent in a suspension state, and the contact is carried out in multiple batches.

[0104] (P-4) A method of contacting a liquid magnesium compound comprising a magnesium compound and catalyst component (b), a liquid titanium compound, and an amide compound.

[0105] The reaction temperature is preferably in the range of -30°C to 150°C, more preferably -25°C to 130°C, and even more preferably -25°C to 120°C.

[0106] The production of the solid titanium catalyst component can also be carried out in the presence of a known medium, if necessary. Examples of the medium include slightly polar aromatic hydrocarbons such as toluene, and known aliphatic and alicyclic hydrocarbon compounds such as heptane, octane, decane, and cyclohexane. Among these, aliphatic hydrocarbons are preferred.

[0107] When the reaction is carried out within the above range, it is possible to obtain a polymer having a wide molecular weight distribution, and at the same time, it is possible to achieve a higher level of activity and stereoregularity of the obtained polymer.

[0108] <Catalyst Component (b)> The catalyst component (b) used to form the solid adduct or liquid magnesium compound is preferably a known compound capable of solubilizing the magnesium compound in a temperature range of room temperature to about 300° C., such as an alcohol, an aldehyde, an amine, a carboxylic acid, or a mixture thereof. Examples of such compounds include those described in detail in Patent Document 1 and Patent Document 2.

[0109] More specific examples of the alcohol capable of solubilizing the magnesium compound include aliphatic alcohols such as methanol, ethanol, propanol, butanol, isobutanol, ethylene glycol, 2-methylpentanol, 2-ethylbutanol, n-heptanol, n-octanol, 2-ethylhexanol, decanol, and dodecanol; alicyclic alcohols such as cyclohexanol and methylcyclohexanol; aromatic alcohols such as benzyl alcohol and methylbenzyl alcohol; and aliphatic alcohols having an alkoxy group, such as n-butyl cellosolve.

[0110] Examples of the carboxylic acid include organic carboxylic acids having 7 or more carbon atoms, such as caprylic acid and 2-ethylhexanoic acid. Examples of the aldehyde include aldehydes having 7 or more carbon atoms, such as capric aldehyde and 2-ethylhexyl aldehyde.

[0111] Examples of the amine include amines having 6 or more carbon atoms, such as heptylamine, octylamine, nonylamine, laurylamine, and 2-ethylhexylamine.

[0112] As the catalyst component (b), the above alcohols are preferred, with ethanol, propanol, butanol, isobutanol, hexanol, 2-ethylhexanol, decanol and the like being particularly preferred.

[0113] The amounts of magnesium compound and catalyst component (b) used when preparing the solid adduct or liquid magnesium compound vary depending on the type and contact conditions, but the magnesium compound is used in an amount of 0.1 to 20 mol / L, preferably 0.5 to 5 mol / L, per unit volume of catalyst component (b). If necessary, a medium inert to the solid adduct can also be used in combination. Preferred examples of the medium include known hydrocarbon compounds such as heptane, octane, and decane.

[0114] The composition ratio of magnesium to catalyst component (b) in the resulting solid adduct or liquid magnesium compound varies depending on the type of compound used and cannot be generally defined. However, the amount of catalyst component (b) relative to 1 mole of magnesium in the magnesium compound is preferably 2.0 moles or more, more preferably 2.2 moles or more, even more preferably 2.6 moles or more, particularly preferably 2.7 moles or more, and is preferably in the range of 5 moles or less.

[0115] <Aromatic carboxylic acid ester and / or compound having two or more ether bonds via multiple carbon atoms> The solid titanium catalyst component (I) of the present invention may further contain an aromatic carboxylic acid ester and / or a compound having two or more ether bonds via multiple carbon atoms (hereinafter also referred to as "catalyst component (c)"). When the solid titanium catalyst component (I) of the present invention contains catalyst component (c), it may be possible to increase activity and stereoregularity and further broaden the molecular weight distribution.

[0116] As this catalyst component (c), known aromatic carboxylic acid esters and polyether compounds that are preferably used in conventional olefin polymerization catalysts, such as the compounds described in Patent Document 2 and JP-A-2001-354714, can be used without limitation.

[0117] Specific examples of the aromatic carboxylic acid ester include aromatic carboxylic acid monoesters such as benzoic acid esters and toluic acid esters, as well as aromatic polycarboxylic acid esters such as phthalic acid esters. Among these, aromatic polycarboxylic acid esters are preferred, and phthalic acid esters are more preferred. Preferred phthalic acid esters include alkyl phthalates such as ethyl phthalate, n-butyl phthalate, isobutyl phthalate, hexyl phthalate, and heptyl phthalate, with diisobutyl phthalate being particularly preferred.

[0118] More specifically, the polyether compound includes a compound represented by the following formula (3).

[0119]

[0120] In the above formula (3), m is an integer of 1≦m≦10, more preferably an integer of 3≦m≦10, and R 11 , R 12 , R 31 ~R 36 are each a hydrogen atom or a substituent having at least one element selected from carbon, hydrogen, oxygen, fluorine, chlorine, bromine, iodine, nitrogen, sulfur, phosphorus, boron and silicon.

[0121] When m is 2 or more, there are multiple R 11 and R 12 may be the same or different. 11 , R 12 , R 31 ~R 36 , preferably R 11 and R 12 may combine to form a ring other than a benzene ring.

[0122] Specific examples of such compounds include 2-isopropyl-1 , 3-Dimethoxypropane, 2-s-butyl-1 , 3-Dimethoxypropane, 2-cumyl-1 , 1-substituted dialkoxypropanes such as 3-dimethoxypropane; 2-isopropyl-2-isobutyl-1 , 3-dimethoxypropane, 2 , 2-Dicyclohexyl-1 , 3-Dimethoxypropane, 2-methyl-2-isopropyl-1 , 3-Dimethoxypropane, 2-methyl-2-cyclohexyl-1 , 3-Dimethoxypropane, 2-methyl-2-isobutyl-1 , 3-dimethoxypropane, 2 , 2-diisobutyl-1 , 3-dimethoxypropane, 2 , 2-bis(cyclohexylmethyl)-1 , 3-dimethoxypropane, 2 , 2-diisobutyl-1 , 3-diethoxypropane, 2 , 2-diisobutyl-1 ,3-dibutoxypropane, 2 , 2-di-s-butyl-1 , 3-dimethoxypropane, 2 , 2-dineopentyl-1 , 3-Dimethoxypropane, 2-isopropyl-2-isopentyl-1 , 3-Dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1 , 2-substituted dialkoxypropanes such as 3-dimethoxypropane; , 3-Dicyclohexyl-1 , 4-diethoxybutane, 2 , 3-Dicyclohexyl-1 , 4-diethoxybutane, 2 , 3-diisopropyl-1 , 4-diethoxybutane, 2 , 4-diphenyl-1 , 5-dimethoxypentane, 2 , 5-diphenyl-1 , 5-dimethoxyhexane, 2 , 4-diisopropyl-1 , 5-dimethoxypentane, 2 , 4-diisobutyl-1 , 5-dimethoxypentane, 2 , 4-Diisoamyl-1 , Dialkoxyalkanes such as 5-dimethoxypentane; 2-methyl-2-methoxymethyl-1 , 3-Dimethoxypropane, 2-cyclohexyl-2-ethoxymethyl-1 , 3-diethoxypropane, 2-cyclohexyl-2-methoxymethyl-1 , trialkoxyalkanes such as 3-dimethoxypropane; 2 , 2-diisobutyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-isopropyl-2-isoamyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-cyclohexyl-2-methoxymethyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-isopropyl-2-methoxymethyl-1 ,3-Dimethoxy-4-cyclohexenyl, 2-isobutyl-2-methoxymethyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-cyclohexyl-2-ethoxymethyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-isopropyl-2-ethoxymethyl-1 , 3-Dimethoxy-4-cyclohexenyl, 2-isobutyl-2-ethoxymethyl-1 , Examples include dialkoxycycloalkanes such as 3-dimethoxy-4-cyclohexenyl.

[0123] Of these, 1 , 3-Diethers are preferred, particularly 2-isopropyl-2-isobutyl-1 , 3-dimethoxypropane, 2 , 2-diisobutyl-1 , 3-Dimethoxypropane, 2-isopropyl-2-isopentyl-1 , 3-dimethoxypropane, 2 , 2-Dicyclohexyl-1 , 3-dimethoxypropane, 2 , 2-bis(cyclohexylmethyl) 1 , 3-Dimethoxypropane is preferred. These compounds may be used alone or in combination of two or more.

[0124] The above-mentioned amide compound, catalyst component (b), and catalyst component (c) may be considered to be components known as electron donors by those skilled in the art. The above-mentioned electron donor components are known to have the effect of increasing the stereoregularity of the resulting polymer while maintaining high catalyst activity, the effect of controlling the composition distribution of the resulting copolymer, and the effect of acting as a flocculant to control the particle shape and particle size of the catalyst particles.

[0125] It is believed that the amide compound of the present invention also exhibits the effect of being able to further control the molecular weight distribution by the electron donor.

[0126] In the solid titanium catalyst component (I) used in the present invention, the halogen / titanium (atomic ratio) (i.e., the number of moles of halogen atoms / the number of moles of titanium atoms) is desirably 2 to 100, preferably 4 to 90; the amide compound / titanium (molar ratio) (i.e., the number of moles of amide compound / the number of moles of titanium atoms) is desirably 0.01 to 100, preferably 0.2 to 10; and in catalyst component (b) and catalyst component (c), the catalyst component (b) / titanium (molar ratio) is desirably 0 to 100, preferably 0 to 10, and the catalyst component (c) / titanium (molar ratio) is desirably 0 to 100, preferably 0 to 10. The magnesium / titanium (atomic ratio) (i.e., the number of moles of magnesium atoms / the number of moles of titanium atoms) is desirably 2 to 100, preferably 4 to 50.

[0127] Furthermore, the content of components that may be contained other than the above-mentioned amide compound, such as catalyst component (b) and catalyst component (c), is preferably 20% by weight or less, more preferably 10% by weight or less, based on 100% by weight of the amide compound.

[0128] As more detailed preparation conditions for the solid titanium catalyst component (I), the conditions described in, for example, EP585869A1 (European Patent Application Publication No. 0585869) and Patent Document 2 can be preferably used, except for the use of an amide compound.

[0129] [Olefin polymerization catalyst] The olefin polymerization catalyst according to the present invention is characterized by comprising the above-mentioned solid titanium catalyst component (I) according to the present invention and an organometallic compound catalyst component (II) containing a metal element selected from Groups 1, 2 and 13 of the periodic table.

[0130] <Organometallic Compound Catalyst Component (II)> As the organometallic compound catalyst component (II), compounds containing a Group 13 metal, such as organoaluminum compounds, alkylated complexes of Group 1 metals and aluminum, and organometallic compounds of Group 2 metals can be used. Among these, organoaluminum compounds are preferred. Specific preferred examples of the organometallic compound catalyst component (II) include the organometallic compound catalyst components described in known documents such as EP585869A1.

[0131] <Electron Donor (III)> The olefin polymerization catalyst of the present invention may contain, if necessary, an electron donor (III) in addition to the organometallic compound catalyst component (II). A preferred example of the electron donor (III) is an organosilicon compound. An example of this organosilicon compound is a compound represented by the following general formula (4): R S n Si(OR") 4-n ...(4) In formula (4), R S and R″ is a hydrocarbon group, and n is an integer of 0<n<4.

[0132] Specific examples of the organosilicon compound represented by the general formula (4) include diisopropyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldiethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, t-butyltriethoxysilane, phenyltriethoxysilane, cyclohexyltrimethoxysilane, cyclopentyltrimethoxysilane, 2-methylcyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, dicyclopentyldimethoxysilane, dicyclopentyldiethoxysilane, tricyclopentylmethoxysilane, dicyclopentylmethylmethoxysilane, dicyclopentylethylmethoxysilane, and cyclopentyldimethylethoxysilane.

[0133] Of these, vinyltriethoxysilane, diphenyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, and dicyclopentyldimethoxysilane are preferably used.

[0134] Furthermore, a silane compound represented by the following formula (5), which is described in International Publication No. 2004 / 016662, is also a preferred example of the organosilicon compound: Si(OR a ) 3 (NR b R c ) ... (5)

[0135] In formula (5), R a is a hydrocarbon group having 1 to 6 carbon atoms, and R a Examples of the alkyl group include unsaturated or saturated aliphatic hydrocarbon groups having 1 to 6 carbon atoms, and particularly preferred are hydrocarbon groups having 2 to 6 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, an n-pentyl group, an isopentyl group, a cyclopentyl group, an n-hexyl group, and a cyclohexyl group, and among these, an ethyl group is particularly preferred.

[0136] In formula (5), R b is a hydrocarbon group having 1 to 12 carbon atoms or hydrogen, and R b Examples of the alkyl group include hydrogen and unsaturated or saturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms. Specific examples include a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, an n-pentyl group, an isopentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group, with an ethyl group being particularly preferred.

[0137] In formula (5), R c is a hydrocarbon group having 1 to 12 carbon atoms, and R cExamples of the alkyl group include hydrogen and unsaturated or saturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, an n-pentyl group, an isopentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group, with an ethyl group being particularly preferred.

[0138] Specific examples of the compound represented by the above formula (5) include dimethylaminotriethoxysilane, diethylaminotriethoxysilane, diethylaminotrimethoxysilane, diethylaminotriethoxysilane, diethylaminotri-n-propoxysilane, di-n-propylaminotriethoxysilane, methyl-n-propylaminotriethoxysilane, t-butylaminotriethoxysilane, ethyl-n-propylaminotriethoxysilane, ethyl iso-propylaminotriethoxysilane, and methylethylaminotriethoxysilane.

[0139] Another example of the organosilicon compound is a compound represented by the following formula (6): N NSi(OR a ) 3 ... (6)

[0140] In formula (6), R N N is a cyclic amino group, and examples of this cyclic amino group include a perhydroquinolino group, a perhydroisoquinolino group, a 1,2,3,4-tetrahydroquinolino group, a 1,2,3,4-tetrahydroisoquinolino group, and an octamethyleneimino group.

[0141] Specific examples of the compound represented by formula (6) include (perhydroquinolino)triethoxysilane, (perhydroisoquinolino)triethoxysilane, (1,2,3,4-tetrahydroquinolino)triethoxysilane, (1,2,3,4-tetrahydroisoquinolino)triethoxysilane, octamethyleneiminotriethoxysilane, etc. These organosilicon compounds can also be used in combination of two or more.

[0142] Other preferred examples of compounds useful as the electron donor (III) include the aromatic carboxylic acid esters and / or the polyether compounds described as examples of compounds having two or more ether bonds via a plurality of carbon atoms (the catalyst component (c)).

[0143] Among these polyether compounds, 1 , 3-Diethers are preferred, particularly 2-isopropyl-2-isobutyl-1 , 3-dimethoxypropane, 2 , 2-diisobutyl-1 , 3-Dimethoxypropane, 2-isopropyl-2-isopentyl-1 , 3-dimethoxypropane, 2 , 2-Dicyclohexyl-1 , 3-dimethoxypropane, 2 , 2-bis(cyclohexylmethyl) 1 , 3-Dimethoxypropane is preferred. These compounds can be used alone or in combination of two or more.

[0144] The combined use of the electron donor (III) as described above often makes it possible to adjust the stereoregularity and molecular weight in particular. Specifically, increasing the ratio of the electron donor (III) used relative to the organometallic compound catalyst component tends to make it easier to obtain a polymer with high stereoregularity and a high molecular weight. On the other hand, decreasing the ratio of the electron donor (III) used tends to make it easier to obtain a polymer with low stereoregularity (for example, a high content of decane-soluble components, as described below) and a low molecular weight.

[0145] In addition to the above-mentioned components, the olefin polymerization catalyst of the present invention may contain other components useful for olefin polymerization, as needed, such as a carrier such as silica, an antistatic agent, a particle flocculant, a storage stabilizer, etc.

[0146] [Olefin Polymerization Method] The olefin polymerization method according to the present invention is characterized by carrying out olefin polymerization using the olefin polymerization catalyst of the present invention. In the present invention, the term "polymerization" may include not only homopolymerization but also copolymerization such as random copolymerization and block copolymerization.

[0147] In the olefin polymerization method of the present invention, it is also possible to carry out main polymerization in the presence of a prepolymerization catalyst obtained by prepolymerizing an α-olefin in the presence of the olefin polymerization catalyst of the present invention. This prepolymerization is carried out by prepolymerizing an α-olefin in an amount of 0.1 to 1000 g, preferably 0.3 to 500 g, particularly preferably 1 to 200 g, per 1 g of the olefin polymerization catalyst.

[0148] In the prepolymerization, the catalyst can be used at a higher concentration than that in the main polymerization system. The concentration of the solid titanium catalyst component (I) in the prepolymerization is desirably set to be in the range of usually about 0.001 to 200 mmol, preferably about 0.01 to 50 mmol, and particularly preferably 0.1 to 20 mmol, calculated as titanium atom per liter of the liquid medium.

[0149] The amount of the organometallic compound catalyst component (II) in the prepolymerization may be such that 0.1 to 1,000 g, preferably 0.3 to 500 g, of polymer is produced per gram of the solid titanium catalyst component (I), and it is desirable that the amount is usually about 0.1 to 300 mol, preferably about 0.5 to 100 mol, particularly preferably 1 to 50 mol, per mol of titanium atom in the solid titanium catalyst component (I).

[0150] In the prepolymerization, the electron donor (III) and the like can be used as needed, and in this case, these components are used in an amount of 0.1 to 50 mol, preferably 0.5 to 30 mol, and more preferably 1 to 10 mol, per mol of titanium atom in the solid titanium catalyst component (I). By adjusting the amount of the electron donor (III), it may be possible to adjust the stereoregularity of the resulting olefin polymer.

[0151] The prepolymerization can be carried out under mild conditions by adding an olefin and the above-mentioned catalyst components to an inert hydrocarbon medium.

[0152] In this case, specific examples of the inert hydrocarbon medium to be used include: aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cycloheptane, methylcycloheptane, 4-cycloheptane, and methyl 4-cycloheptane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride and chlorobenzene, and mixtures thereof.

[0153] Among these inert hydrocarbon media, it is particularly preferable to use aliphatic hydrocarbons. When an inert hydrocarbon medium is used, it is preferable to carry out the prepolymerization in a batch system.

[0154] On the other hand, the prepolymerization can be carried out using the olefin itself as a solvent, or in the substantial absence of a solvent. In this case, it is preferable to carry out the prepolymerization continuously.

[0155] The olefin used in the prepolymerization may be the same as or different from the olefin used in the main polymerization described below, and specifically, it is preferably propylene.

[0156] The temperature during the prepolymerization is usually in the range of about -20 to +100°C, preferably about -20 to +80°C, and more preferably 0 to +40°C.

[0157] Next, the main polymerization, which is carried out after the above-mentioned prepolymerization or without prepolymerization, will be explained.

[0158] Olefins that can be used (i.e., polymerized) in this polymerization include α-olefins having 3 to 20 carbon atoms, such as linear olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene, and branched olefins such as 4-methyl-1-pentene, 3-methyl-1-pentene, and 3-methyl-1-butene, with propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, and 3-methyl-1-butene being preferred. Furthermore, from the viewpoint that the advantages of polymers with a wide molecular weight distribution are easily realized in highly rigid resins, propylene, 1-butene, 4-methyl-1-pentene, and 3-methyl-1-butene are particularly preferred.

[0159] These α-olefins can also be used in combination with aromatic vinyl compounds such as ethylene, styrene, and allylbenzene; and alicyclic vinyl compounds such as vinylcyclohexane and vinylcycloheptane. Furthermore, compounds having polyunsaturated bonds, such as conjugated or non-conjugated dienes, including dienes such as cyclopentene, cycloheptene, norbornene, tetracyclododecene, isoprene, and butadiene, can also be used as polymerization raw materials in combination with ethylene and the α-olefin. These compounds can be used alone or in combination with two or more (hereinafter, olefins used in combination with the above-mentioned ethylene or "α-olefins having 3 to 20 carbon atoms" will also be referred to as "other olefins").

[0160] Among the other olefins, ethylene and aromatic vinyl compounds are preferred. Furthermore, other olefins such as ethylene may be used in combination in a small amount, for example, 10% by weight or less, preferably 5% by weight or less, based on 100% by weight of the total amount of olefins.

[0161] In the present invention, the prepolymerization and main polymerization can be carried out by any of liquid phase polymerization methods such as bulk polymerization, solution polymerization, and suspension polymerization, or gas phase polymerization methods.

[0162] When the main polymerization is carried out in the form of a slurry polymerization reaction, the inert hydrocarbon used in the prepolymerization described above can be used as the reaction solvent, or an olefin that is liquid at the reaction temperature can be used.

[0163] In the main polymerization of the polymerization method of the present invention, the solid titanium catalyst component (I) is typically used in an amount of about 0.0001 to 0.5 millimoles, preferably about 0.005 to 0.1 millimoles, calculated as titanium atoms per liter of polymerization volume. The organometallic compound catalyst component (II) is typically used in an amount of about 1 to 2,000 moles, preferably about 5 to 500 moles, more preferably 10 to 350 moles, even more preferably 30 to 350 moles, and particularly preferably 50 to 350 moles, per mole of titanium atoms in the prepolymerized catalyst component in the polymerization system. The electron donor (III), if used, is typically used in an amount of 0.001 to 50 moles, preferably 0.01 to 30 moles, and particularly preferably 0.05 to 20 moles, per mole of metal atoms in the organometallic compound catalyst component (II). As mentioned above, the stereoregularity and molecular weight can sometimes be adjusted by adjusting the amount of electron donor (III) used.

[0164] If the polymerization is carried out in the presence of hydrogen, the molecular weight of the resulting polymer can be controlled, and a polymer having a high melt flow rate can be obtained.

[0165] In the present invention, the polymerization temperature of the olefin is usually about 20 to 200°C, preferably about 30 to 100°C, and more preferably 50 to 90°C. The pressure is usually set at atmospheric pressure to 10 MPa, preferably 0.20 to 5 MPa. In the polymerization method of the present invention, the polymerization can be carried out by any of batch, semi-continuous, and continuous methods. Furthermore, the polymerization can be carried out in two or more stages by changing the reaction conditions. By carrying out such multi-stage polymerization, it is possible to further broaden the molecular weight distribution of the olefin polymer.

[0166] The olefin polymer thus obtained may be any of a homopolymer, a random copolymer, a block copolymer, etc. When olefin polymerization, particularly propylene polymerization, is carried out using the above-mentioned olefin polymerization catalyst, a highly stereoregular propylene polymer having a decane-insoluble component content of 70% or more, preferably 85% or more, particularly preferably 90% or more can be obtained.

[0167] Furthermore, according to the olefin polymerization method of the present invention, polyolefins, particularly polypropylene, having a broad molecular weight distribution can be obtained even with a small number of polymerization stages, for example, single-stage polymerization, without requiring multistage polymerization. The olefin polymerization method of the present invention is characterized in that it often produces olefin polymers having a higher proportion of high molecular weight components and a lower proportion of low molecular weight components (particularly so-called solid components) than conventional olefin polymers having the same melt flow rate (MFR). This characteristic can be confirmed by gel permeation chromatography (GPC) measurements, which will be described later, and polymers having high Mw / Mn and Mz / Mw values ​​can be obtained.

[0168] Polypropylene obtained using a conventional solid titanium catalyst component containing magnesium, titanium, a halogen, and an electron donor generally has an Mw / Mn value of 5 or less and an Mz / Mw value of less than 4, which are indicators of molecular weight distribution determined by GPC measurement, in the MFR region of 1 to 10 g / 10 min. However, by using the olefin polymerization method of the present invention, it is possible to obtain olefin polymers having an Mw / Mn value of 6 to 30, preferably 7 to 20, under the same polymerization conditions as above. Also, it is possible to obtain olefin polymers having an Mz / Mw value of 4 to 15, more preferably 4.5 to 10. In particular, the olefin polymerization method of the present invention often produces polymers with high Mz / Mw values.

[0169] It is common knowledge among those skilled in the art that polypropylene with a high Mw / Mn value has excellent moldability and rigidity. On the other hand, a high Mz / Mw value indicates a high content of high molecular weight components, and it is expected that the resulting polypropylene will likely have a high melt tension and excellent moldability.

[0170] The olefin polymerization method of the present invention can produce polymers with a broad molecular weight distribution without multi-stage polymerization, which may allow for the simplification of polymer production equipment. Furthermore, when applied to conventional multi-stage polymerization methods, it is expected that polymers with superior melt tension and moldability can be obtained.

[0171] Other methods for obtaining polymers with a wide molecular weight distribution include dissolving and mixing polymers of different molecular weights or melt-kneading them. However, the polymers obtained by these methods may not have sufficient improvements in melt tension and moldability, despite the relatively complicated procedures. This is presumably because polymers of different molecular weights are fundamentally difficult to mix. On the other hand, the polymers obtained by the olefin polymerization method of the present invention are blended at the catalyst level, i.e., at the nano-level, with polymers of extremely wide ranges of different molecular weights, and are therefore expected to have high melt tension and excellent moldability.

[0172] As described above, the polymer obtained by the olefin polymerization method of the present invention has high stereoregularity. Therefore, the olefin polymer obtained by the method of the present invention tends to have a high melting point. The melting point is usually determined by differential scanning calorimetry (DSC).

[0173] Propylene-based polymers such as those obtained by the olefin polymerization method of the present invention (e.g., having a content of propylene-derived structural units of 99 mol % or more) are polymers that surprisingly exhibit an unexpected tendency to have a high heat of fusion as described above, despite having a high content of decane-soluble components.

[0174] It is known that the decane-soluble component of a propylene homopolymer generally has a tendency to have not only low stereoregularity but also low molecular weight, and that polymers with low stereoregularity such as the decane-soluble component are sometimes used as elastomers for shoe sole materials, etc.

[0175] The present inventors have found that the propylene-based polymers obtained by the olefin polymerization method of the present invention tend to have a high molecular weight of the decane-soluble component. Therefore, the above-mentioned propylene-based polymers (containing 99 mol% or more of propylene-derived structural units, a high content of decane-soluble components, and a high molecular weight of the decane-soluble components) may be novel polymers.

[0176] The content of structural units derived from propylene in the propylene-based polymer is preferably 99.3 mol % or more, more preferably 99.5 mol % or more, even more preferably 99.7 mol % or more, and particularly preferably 99.8 mol % or more, with the upper limit being, of course, 100 mol %.

[0177] The decane-soluble component content of the propylene polymer is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, while the upper limit is preferably 15% by mass, more preferably 14% by mass, and even more preferably 13% by mass.

[0178] The molecular weight of the decane-soluble component of the propylene polymer is, in terms of weight average molecular weight, 20% or more, more preferably 25% or more, and even more preferably 27% or more of the entire propylene polymer.

[0179] The stereoregularity of the decane soluble component is 13 This is a specific component in which the stereoregularity (pentad tacticity) derived from methyl groups measured by C NMR shows almost the same values ​​for the mmmm value and the rrrr value. The mmmm value and the rrrr value are both preferably 10 to 30%. A more preferred lower limit is 13%, and even more preferably 15%. On the other hand, a more preferred upper limit is 27%, and even more preferably 25%.

[0180] Propylene polymers containing such high molecular weight decane-soluble components are expected to have not only a high heat of fusion but also flexibility, despite their structure consisting almost entirely of structural units derived from propylene.

[0181] The above-mentioned propylene polymers can be obtained, for example, by polymerizing propylene using the olefin polymerization catalyst of the present invention. The reason why such propylene polymers can be obtained is unclear at present, but it is thought that the catalyst, which is an active species that can have various stereoconformations like the above-mentioned olefin polymers, is less likely to cause chain transfer and can also form active species with low stereospecificity.

[0182] As described above, the olefin polymers, particularly propylene polymers, obtained by the method of the present invention tend to have a broad molecular weight distribution, particularly a large Mz, and therefore tend to have a distribution that is broadened toward the high molecular weight side. Since the molecular mobility of olefin polymers varies depending on the molecular weight, in the case of polymers with a broad molecular weight distribution, the chart obtained by DSC measurement may not have a unimodal shape but may have a multimodal shape or a broad shape. In other words, since ultrahigh molecular weight polymers are more difficult to crystallize, the broad shape toward the low temperature side in DSC measurement may be due to the ultrahigh molecular weight. Therefore, ΔH, measured as the heat of fusion (heat of crystallization), may also tend to be low.

[0183] It is said that the components in the ultra-high molecular weight region may cause problems such as fish eyes in applications where transparency and visibility are important, such as film applications. As described above, the olefin polymer obtained by the method of the present invention tends to achieve a fine dispersion state at the level of catalytic active species, i.e., even at the nano-level, and therefore tends to be less susceptible to the above problems. Furthermore, by selecting the structure of the amide compound used in the catalyst of the present invention, it is possible to adjust the balance between the molecular weight and content of the components in the ultra-high molecular weight region and the molecular weight and melt flow rate (MFR) of the entire polymer.

[0184] The propylene polymer obtained by the method of the present invention can be used in various known applications. In particular, because of its expected high heat resistance and rigidity, it is suitable for use in various injection-molded articles, more specifically, automobile components and home appliance components. Furthermore, because of its wide molecular weight distribution, it can also be used in various sheets and films. In particular, it is suitable for use as separators for lithium-ion batteries and capacitors. It can also be used suitably in stamping molded articles, calendered articles, rotational molded articles, and the like.

[0185] The present invention will be described below with reference to examples, but is not limited to these examples. In the following examples, the bulk density, melt flow rate, amount of decane-soluble (insoluble) components, molecular weight distribution, final melting point, melting point, crystallization temperature, and heat of fusion of the propylene polymer were measured by the following methods.

[0186] (1) Bulk specific gravity: Measured in accordance with JIS K-6721. (2) Melt flow rate (MFR): Measured in accordance with ASTM D1238E, with a load of 2.16 kg and a measurement temperature of 230° C. for propylene polymers.

[0187] (3) Amount of decane-soluble (insoluble) components: About 3 g (10 -4 The weight was measured to the nearest gram. This weight was represented as b (grams) in the formula below. ), 500 ml of decane, and a small amount of a heat stabilizer soluble in decane were added, and the mixture was heated to 150°C over 2 hours while stirring with a stirrer under a nitrogen atmosphere to dissolve the propylene polymer. After maintaining the temperature at 150°C for 2 hours, the mixture was slowly cooled to 23°C over 8 hours. The resulting liquid containing a precipitate of the propylene polymer was filtered under reduced pressure using a 25G-4 standard glass filter manufactured by Tokyo Glass Instruments Co., Ltd. 100 ml of the filtrate was collected and dried under reduced pressure to obtain a portion of the decane-soluble component, and the weight of this was reduced to 10 -4The weight was measured to the nearest gram (this weight is represented as a (gram) in the formula below). After this operation, the amount of decane-soluble components was determined using the following formula: Content of decane-soluble components = 100 × (500 × a) / (100 × b) Content of decane-insoluble components = 100 - 100 × (500 × a) / (100 × b)

[0188] <Method for recovering decane-soluble component: Example 7, Comparative Example 2> A five-fold amount of acetone (poor solvent) was added to the filtrate at room temperature to precipitate the dissolved polymer, which was then filtered using a 350-mesh metal filter to obtain a precipitate. The recovered precipitate was then dried under reduced pressure at 80°C for 1 hour to obtain the decane-soluble component of the propylene polymer. The molecular weight of this decane-soluble component was measured by the GPC method described below, and 13 The stereoregularity was measured by C NMR.

[0189] (4) Molecular Weight Distribution (MWD): Gel Permeation Chromatograph: HLC-8321 GPC / HT Model, manufactured by Tosoh Corporation. Detector: Differential Refractometer. Column: Two TSKgel GMH6-HT columns and two TSKgel GMH6-HTL columns, manufactured by Tosoh Corporation, were connected in series. Mobile Phase: o-Dichlorobenzene. Flow Rate: 1.0 mL / min. Measurement Temperature: 140°C. Calibration Curve Preparation Method: A standard polystyrene sample was used. Measurements were performed under the following conditions: sample concentration: 0.1% (w / w) and sample solution volume: 0.4 mL. The resulting chromatograms were analyzed using known methods to calculate the weight-average molecular weight (Mw), number-average molecular weight (Mn), Z-average molecular weight (Mz), and the Mw / Mn and Mz / Mw values, which are indicators of molecular weight distribution (MWD). The measurement time per sample was 60 minutes.

[0190] (5) Melting Point (Tm) of Polymer: The melting point (Tm), crystallization temperature (Tc), and heat of fusion (ΔH) of the polymer in the present invention were measured by differential scanning calorimetry (DSC) using a PerkinElmer DSC8000 device. 3 to 10 mg of sample was sealed in an aluminum pan and heated from room temperature to 200°C at 100°C / min. The sample was held at 200°C for 5 minutes and then cooled to 30°C at 10°C / min. The peak temperature observed in this cooling test was taken as the crystallization temperature (Tc), and the calorific value determined by the area of ​​the peak was taken as ΔH. After being left at 30°C for 5 minutes, the sample was heated a second time to 200°C at 10°C / min. The peak temperature observed in this second heating test was taken as the melting point (Tm).

[0191] The final melting point (Tmf) of the polymer in the present invention was measured by differential scanning calorimetry (DSC) using a PerkinElmer DSC8000 instrument. 3 to 10 mg of sample was sealed in an aluminum pan and heated from room temperature to 240°C at 80°C / min. The sample was held at 240°C for 1 minute and then cooled to 0°C at 80°C / min. After holding at 0°C for 1 minute, the sample was heated to 150°C at 80°C / min and held for 5 minutes. Finally, the sample was heated to 180°C at 1.35°C / min, and the intersection of the tangent to the inflection point on the high-temperature side of the peak obtained in this final heating test and the baseline was taken as the final melting point (Tmf).

[0192] Tmf can be considered as one parameter for evaluating the crystal structure of a component that exhibits very high stereoregularity, or the ease of crystallization and crystal structure of a polymer in the ultra-high molecular weight range that is thought to be difficult to crystallize. More specifically, it can be considered that the higher the Tmf value, the more likely the ultra-high molecular weight polymer component is to form crystals with high heat resistance.

[0193] (6) Stereoregularity of propylene polymer ( 13C NMR measurement): 50 mg of sample was dissolved in 0.6 ml of a 4 / 1 mixed solvent of o-dichlorobenzene and deuterated benzene (o-dichlorobenzene / deuterated benzene; volume ratio), and measured using a Bruker Biospin AVANCE NEO cryo-500 nuclear magnetic resonance spectrometer at 120°C with a 45° pulse, a repetition time of 5.5 seconds, and 256 accumulations. The reference value for the chemical shift was set to 21.59 ppm, the signal derived from the mmmm methyl group. The peak of the methyl group derived from propylene was assigned in the usual manner, and the proportions of various stereostructures were determined.

[0194] The structural formulas of the compounds used in the following examples and comparative examples may have stereoisomeric structures. The structural formulas showing the stereoisomers of the exemplified compounds indicate the isomers that are the main components of the compounds used in the examples and comparative examples. In the present invention, the "main component" refers to an isomer that accounts for more than 50 mol %, preferably 70 mol % or more.

[0195] Example 1 Preparation of solid titanium catalyst component [α1] After thoroughly replacing the atmosphere in a 1 L glass vessel with nitrogen, 85.8 g of anhydrous magnesium chloride, 321 g of decane, and 352 g of 2-ethylhexyl alcohol were placed in the vessel and reacted by heating at 130° C. for 3 hours to obtain a homogeneous solution. 241 g of this solution and 6.43 g of ethyl benzoate were added to the vessel and mixed with stirring at 50° C. for 1 hour.

[0196] The homogeneous solution thus obtained was cooled to room temperature, and 38.3 ml of this homogeneous solution was added dropwise over 45 minutes with stirring to 100 ml of titanium tetrachloride maintained at -20°C. After the addition was complete, the temperature of this mixture was raised to 80°C over 3.8 hours. When the temperature reached 80°C, 1.77 g of Compound 1 below was added to the mixture. The temperature was again raised to 120°C over 40 minutes and maintained at the same temperature for 35 minutes with stirring. After the reaction was completed, the solid was collected by hot filtration, resuspended in 100 ml of titanium tetrachloride, and then heated to 120°C for 35 minutes with stirring. After the reaction was completed, the solid was again collected by hot filtration and thoroughly washed with decane at 100°C and room temperature until no free titanium compound was detected in the washings. The solid titanium catalyst component [α1] prepared by the above procedure was stored as a decane slurry, and a portion of this was dried for the purpose of examining the catalyst composition. The solid titanium catalyst component [α1] thus obtained had a composition of 0.42 mass % of titanium, 1.2 mass % of magnesium, and 0.07 mass % of 2-ethylhexyl alcohol residue.

[0197]

[0198] <Main Polymerization> 500 g of propylene and 1 NL of hydrogen were added to a 2-liter polymerization vessel at room temperature, followed by a mixture of 7 ml of heptane, 0.50 mmol of triethylaluminum, 0.10 mmol of cyclohexylmethyldimethoxysilane, and 0.0040 mmol (titanium atom equivalent) of the solid titanium catalyst component [α1] mixed for 10 minutes at 25°C. The mixture was then added, and the temperature inside the polymerization vessel was rapidly raised to 70°C with stirring. After polymerization at 70°C for 1.5 hours, the reaction was terminated with a small amount of methanol, and the propylene was purged. The resulting polymer particles were then dried under reduced pressure at 80°C overnight. The activity, bulk density, MFR, amount of decane-insoluble component, Tm, Tmf, and MWD are shown in Table 1.

[0199] Example 2 Preparation of solid titanium catalyst component [α2] After thoroughly replacing the atmosphere in a 1 L glass vessel with nitrogen, 85.8 g of anhydrous magnesium chloride, 321 g of decane, and 352 g of 2-ethylhexyl alcohol were placed in the vessel and reacted by heating at 130° C. for 3 hours to obtain a homogeneous solution. 241 g of this solution and 6.43 g of ethyl benzoate were added to the vessel and mixed with stirring at 50° C. for 1 hour.

[0200] The homogeneous solution thus obtained was cooled to room temperature, and 30.6 ml of this homogeneous solution was added dropwise over 45 minutes with stirring to 80 ml of titanium tetrachloride maintained at -20°C. After the addition was complete, the temperature of this mixture was raised to 80°C over 3.8 hours. Once the temperature reached 80°C, 0.63 g of Compound 2 below was added to the mixture. The temperature was again raised to 120°C over 40 minutes and maintained at the same temperature for 35 minutes with stirring. After the reaction was completed, the solid was collected by hot filtration, resuspended in 80 ml of titanium tetrachloride, and then heated to 120°C for 35 minutes with stirring. After the reaction was completed, the solid was again collected by hot filtration and thoroughly washed with decane at 100°C and room temperature until no free titanium compound was detected in the washings. The solid titanium catalyst component [α2] prepared by the above procedure was stored as a decane slurry, and a portion of this was dried for the purpose of examining the catalyst composition. The solid titanium catalyst component [α2] thus obtained had a composition of 0.36% by mass of titanium, 1.7% by mass of magnesium, and 0.11% by mass of 2-ethylhexyl alcohol residue.

[0201]

[0202] <Main Polymerization> 500 g of propylene and 1 NL of hydrogen were added to a 2-liter polymerization vessel at room temperature, followed by a mixture of 7 ml of heptane, 0.40 mmol of triethylaluminum, 0.08 mmol of cyclohexylmethyldimethoxysilane, and 0.0032 mmol (titanium atom equivalent) of the solid titanium catalyst component [α2] mixed for 10 minutes at 25°C. The mixture was then added, and the temperature inside the polymerization vessel was rapidly raised to 70°C with stirring. After polymerization at 70°C for 1.5 hours, the reaction was terminated with a small amount of methanol, and the propylene was purged. The resulting polymer particles were then dried under reduced pressure at 80°C overnight. The activity, bulk density, MFR, amount of decane-insoluble component, Tm, Tmf, and MWD are shown in Table 1.

[0203] [Example 3] <Preparation of solid titanium catalyst component [α3]> A solid titanium catalyst component [α3] was obtained in the same manner as in Example 1, except that 1.64 g of the following compound 3 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α3] thus obtained was 0.44 mass % of titanium, 1.4 mass % of magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0204]

[0205] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α3] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0206] Example 4 Preparation of solid titanium catalyst component [α4] A solid titanium catalyst component [α4] was obtained in the same manner as in Example 1, except that 1.74 g of the following compound 4 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α4] thus obtained was 0.33 mass % titanium, 1.5 mass % magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0207]

[0208] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α4] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0209] Example 5 Preparation of solid titanium catalyst component [α5] A solid titanium catalyst component [α5] was obtained in the same manner as in Example 1, except that 1.47 g of the following compound 5 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α5] thus obtained was 0.28 mass % titanium, 1.7 mass % magnesium, and 0.06 mass % of 2-ethylhexyl alcohol residue.

[0210]

[0211] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that 0.0032 mmol (equivalent to titanium atom) of the solid titanium catalyst component [α5] was used instead of the solid titanium catalyst component [α1], the amount of triethylaluminum used was changed from 0.50 mmol to 0.40 mmol, and the amount of cyclohexylmethyldimethoxysilane used was changed from 0.10 mmol to 0.08 mmol. The results are shown in Table 1.

[0212] [Example 6] <Preparation of solid titanium catalyst component [α6]> A solid titanium catalyst component [α6] was obtained in the same manner as in Example 1, except that 1.88 g of the following compound 6 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α6] thus obtained was 0.43 mass % titanium, 1.6 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0213]

[0214] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α6] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0215] Example 7 Preparation of solid titanium catalyst component [α7] A solid titanium catalyst component [α7] was obtained in the same manner as in Example 1, except that 1.71 g of the following compound 7 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α7] thus obtained was 0.66 mass % titanium, 1.3 mass % magnesium, and 0.05 mass % of 2-ethylhexyl alcohol residue.

[0216]

[0217] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α7] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1. Separately, the decane-soluble component was recovered and subjected to GPC measurement and 13 The results are shown in Table 2.

[0218] Example 8 Preparation of solid titanium catalyst component [α8] A solid titanium catalyst component [α8] was obtained in the same manner as in Example 1, except that 1.37 g of the following compound 8 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α8] thus obtained was 0.64 mass % titanium, 1.4 mass % magnesium, and 0.07 mass % of 2-ethylhexyl alcohol residue.

[0219]

[0220] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α8] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0221] [Comparative Example 1] <Preparation of solid titanium catalyst component [β1]> A solid titanium catalyst component [β1] was obtained in the same manner as in Example 1, except that 1.12 g of the following compound-c1 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [β1] thus obtained was 0.57 mass % titanium, 1.5 mass % magnesium, and 0.03 mass % of 2-ethylhexyl alcohol residue.

[0222]

[0223] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [β1] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0224] [Comparative Example 2] <Preparation of solid titanium catalyst component [β2]> A solid titanium catalyst component [β2] was obtained in the same manner as in Example 1, except that 1.60 g of the following compound-c2 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [β2] thus obtained was 0.25 mass % titanium, 1.9 mass % magnesium, and 0.08 mass % of 2-ethylhexyl alcohol residue.

[0225]

[0226] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [β2] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1. Separately, the decane-soluble component was recovered and subjected to GPC measurement and 13 The results are shown in Table 2.

[0227] [Comparative Example 3] <Preparation of solid titanium catalyst component [β3]> A solid titanium catalyst component [β3] was obtained in the same manner as in Example 1, except that 1.85 g of the following compound-c3 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [β3] thus obtained was 0.77 mass % titanium, 1.1 mass % magnesium, and 0.18 mass % of 2-ethylhexyl alcohol residue.

[0228]

[0229] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [β3] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 1.

[0230]

[0231]

[0232] Example 9 Preparation of solid titanium catalyst component [α9] A solid titanium catalyst component [α9] was obtained in the same manner as in Example 1, except that 1.57 g of the following compound 9 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α9] thus obtained was 0.58 mass % titanium, 1.3 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0233]

[0234] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α9] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0235] [Example 10] <Preparation of solid titanium catalyst component [α10]> A solid titanium catalyst component [α10] was obtained in the same manner as in Example 1, except that 1.28 g of the following compound 10 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α10] thus obtained was 0.61 mass % titanium, 1.4 mass % magnesium, and 0.15 mass % of 2-ethylhexyl alcohol residue.

[0236]

[0237] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α10] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0238] [Example 11] <Preparation of solid titanium catalyst component [α11]> A solid titanium catalyst component [α11] was obtained in the same manner as in Example 1, except that 1.77 g of the following compound 11 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α11] thus obtained was 0.87 mass % titanium, 1.1 mass % magnesium, and 0.15 mass % of 2-ethylhexyl alcohol residue.

[0239]

[0240] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α11] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0241] [Example 12] <Preparation of solid titanium catalyst component [α12]> A solid titanium catalyst component [α12] was obtained in the same manner as in Example 1, except that 1.64 g of the following compound 12 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α12] thus obtained was 0.64 mass % titanium, 1.5 mass % magnesium, and 0.09 mass % of 2-ethylhexyl alcohol residue.

[0242]

[0243] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α12] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0244] [Example 13] <Preparation of solid titanium catalyst component [α13]> A solid titanium catalyst component [α13] was obtained in the same manner as in Example 1, except that 1.64 g of the following compound 13 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α13] thus obtained was 0.91 mass % titanium, 1.0 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0245]

[0246] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α13] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0247] [Example 14] <Preparation of solid titanium catalyst component [α14]> A solid titanium catalyst component [α14] was obtained in the same manner as in Example 1, except that 1.94 g of the following compound 14 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α14] thus obtained was 0.67 mass % titanium, 1.2 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0248]

[0249] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α14] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0250] [Example 15] <Preparation of solid titanium catalyst component [α15]> A solid titanium catalyst component [α15] was obtained in the same manner as in Example 1, except that 2.17 g of the following compound 15 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α15] thus obtained was 0.29 mass % titanium, 1.4 mass % magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0251]

[0252] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α15] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0253] Example 16 Preparation of solid titanium catalyst component [α16] A solid titanium catalyst component [α16] was obtained in the same manner as in Example 1, except that 2.43 g of the following compound 16 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α16] thus obtained was 0.28 mass % titanium, 1.3 mass % magnesium, and 0.03 mass % of 2-ethylhexyl alcohol residue.

[0254]

[0255] <Main Polymerization> Propylene polymerization was carried out in the same manner as in Example 1, except that the solid titanium catalyst component [α16] was used instead of the solid titanium catalyst component [α1]. The results are shown in Table 3.

[0256]

[0257] [Example 17] <Preparation of solid titanium catalyst component [α17]> A solid titanium catalyst component [α17] was obtained in the same manner as in Example 1, except that 1.57 g of the following compound 17 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α17] thus obtained was 0.95 mass % titanium, 1.0 mass % magnesium, and 0.03 mass % of 2-ethylhexyl alcohol residue.

[0258]

[0259] [Example 18] <Preparation of solid titanium catalyst component [α18]> A solid titanium catalyst component [α18] was obtained in the same manner as in Example 1, except that 1.50 g of the following compound 18 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α18] thus obtained was 0.85 mass % titanium, 1.1 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0260]

[0261] [Example 19] <Preparation of solid titanium catalyst component [α19]> A solid titanium catalyst component [α19] was obtained in the same manner as in Example 1, except that 0.98 g of the following compound 19 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α19] thus obtained was 0.57 mass % titanium, 1.2 mass % magnesium, and 0.16 mass % of 2-ethylhexyl alcohol residue.

[0262]

[0263] [Example 20] <Preparation of solid titanium catalyst component [α20]> A solid titanium catalyst component [α20] was obtained in the same manner as in Example 1, except that 1.77 g of the following compound 20 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α20] thus obtained was 0.80 mass % titanium, 1.0 mass % magnesium, and 0.14 mass % of 2-ethylhexyl alcohol residue.

[0264]

[0265] [Example 21] <Preparation of solid titanium catalyst component [α21]> A solid titanium catalyst component [α21] was obtained in the same manner as in Example 1, except that 1.49 g of the following compound 21 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α21] thus obtained was 0.71 mass % titanium, 1.2 mass % magnesium, and 0.18 mass % of 2-ethylhexyl alcohol residue.

[0266]

[0267] Example 22 Preparation of solid titanium catalyst component [α22] A solid titanium catalyst component [α22] was obtained in the same manner as in Example 1, except that 1.20 g of the following compound 22 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α22] thus obtained was 0.38 mass % titanium, 1.6 mass % magnesium, and 0.07 mass % of 2-ethylhexyl alcohol residue.

[0268]

[0269] [Example 23] <Preparation of solid titanium catalyst component [α23]> A solid titanium catalyst component [α23] was obtained in the same manner as in Example 1, except that 1.64 g of the following compound 23 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α23] thus obtained was 0.47 mass % titanium, 1.2 mass % magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0270]

[0271] [Example 24] <Preparation of solid titanium catalyst component [α24]> A solid titanium catalyst component [α24] was obtained in the same manner as in Example 1, except that 1.68 g of the following compound 24 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α24] thus obtained was 0.57 mass % titanium, 1.3 mass % magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0272]

[0273] Example 25 Preparation of solid titanium catalyst component [α25] A solid titanium catalyst component [α25] was obtained in the same manner as in Example 1, except that 1.94 g of the following compound 25 was used instead of 1.77 g of compound 1. The composition of the solid titanium catalyst component [α25] thus obtained was 0.47 mass % titanium, 1.3 mass % magnesium, and 0.02 mass % of 2-ethylhexyl alcohol residue.

[0274]

[0275] [Example 26] <Preparation of solid titanium catalyst component [α26]> A solid titanium catalyst component [α26] was obtained in the same manner as in Example 2, except that 2.43 g of the following compound 26 was used instead of 0.63 g of compound 1. The composition of the solid titanium catalyst component [α26] thus obtained was 0.55 mass % titanium, 1.5 mass % magnesium, and 0.04 mass % of 2-ethylhexyl alcohol residue.

[0276]

Claims

1. A solid titanium catalyst component comprising magnesium, titanium, a halogen and an amide compound specified by the following formula (1): [In formula (1), C, C 1 and C 2 is a carbon atom, N is a nitrogen atom, R 1 and R 2 are each a hydrocarbon group, R 3 ~R 6 are groups containing carbon, hydrogen, and an element selected from the group consisting of elements in groups 15, 16, and 17 of the periodic table; R 11 and R 12 are each a hydrogen atom or a hydrocarbon group, m is an integer of 0 to 10, A is a linking group selected from an aliphatic group, an alicyclic group, and an aromatic group, and when there are multiple As, they may all be groups having the same structure, or some or all of them may be groups having different structures.

2. The solid titanium catalyst component according to claim 1, wherein the amide compound is specified by the following formula (2): [In formula (2), R 1 ~R 6 , R 11 , R 12 , C, C 1 , C 2 and N are the same as those in formula (1), m is an integer of 1 to 10, and a plurality of R x is a group containing carbon, hydrogen, and an element selected from the group 15, 16, and 17 elements of the periodic table; R x can be bonded together to form a ring structure.

3. R 11 and R 12 2. The solid titanium catalyst component according to claim 1, wherein is a hydrogen atom.

4. R 3 , R 4 , R 5 and R 6 2. The solid titanium catalyst component according to claim 1, wherein is a hydrogen atom.

5. An olefin polymerization catalyst comprising the solid titanium catalyst component (I) according to claim 1 and an organometallic compound catalyst component (II) containing a metallic element selected from Groups 1, 2 and 13 of the periodic table.

6. The olefin polymerization catalyst according to claim 5, further comprising an electron donor (III).

7. A process for olefin polymerization, which comprises carrying out polymerization of an olefin in the presence of the olefin polymerization catalyst according to claim 5 or 6.

Citation Information

Patent Citations

  • Solid titanium catalyst component for olefin polymerization, process for preparing the same, catalyst for olefin polymerization and process for olefin polymerization

    EP0585869A1

  • Ingredient and catalyst for olefin polymerization

    JP1982063310A

  • Solid titanium catalyst component for olefin polymerization, olefin polymerization catalyst, and method for polymerizing olefin

    JP2001354714A

  • CATALYSTS FOR POLYMERIZATION OR COPOLYMERIZATION OF &agr -OLEFINS, CATALYST COMPONENTS THEREOF, AND PROCESSES FOR POLYMERIZATION OF &agr -OLEFINS WITH THE CATALYSTS

    WO2004016662A1

  • Solid titanium catalyst component, catalyst for olefin polymerization, and process for producing olefin polymer

    WO2006077945A1

Cited By

  • Solid titanium catalyst component, catalyst for polymerizing olefin, and method for polymerizing olefin

    WO2026173054A1