Urethane-based heat-dissipating adhesive composition having long pot life and excellent thermal conductivity
The urethane-based heat dissipation adhesive composition extends pot life and maintains short complete curing time, enhancing process stability and thermal conductivity, addressing the limitations of conventional compositions for electronic and automotive applications.
Patent Information
- Application Number
- PCT/KR2023/004252
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional urethane heat dissipation adhesive compositions have a short pot life and complete curing time, which affects process stability and handleability, particularly in applications like electronic devices and electric vehicle batteries, where extended workability and thermal conductivity are crucial.
A urethane-based heat dissipation adhesive composition is developed with a main part containing a first polyol and a chain extender, and a curing agent portion with three types of aromatic isocyanates, optimizing the mixing ratio and components to achieve a longer pot life and shorter complete curing time, ensuring excellent thermal conductivity and mechanical properties.
The composition exhibits a pot life twice as long as conventional compositions, with a complete curing time comparable to existing technologies, significantly improving process stability, handleability, and thermal conductivity, making it suitable for electronic devices and electric vehicle batteries.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Urethane-based heat-dissipating adhesive composition with long working life and excellent thermal conductivity
[0001] The present invention relates to a urethane heat-resistant adhesive composition having a long working time and a short complete curing time, thereby improving the work stability and handling of the process, and at the same time having excellent thermal conductivity and mechanical properties.
[0002]
[0003] Recently, the issue of heat management generated by the miniaturization of electronic devices and the high integration of battery modules in electric vehicles has been receiving much attention.
[0004] One method for easily dissipating heat generated from electronic devices into the atmosphere is the development of Thermal Interface Materials (TIMs), which blend inorganic fillers into a polymer structure, extrude the material over a heat source, and then cure to seamlessly fill the heat source interface. Automotive batteries, in particular, are often exposed to extreme environmental changes. For these applications, TIMs are being developed using polyurethane materials that offer excellent adhesion to various materials and weather resistance.
[0005] Typically, polyurethane TIMs are manufactured by storing the main component and the curing agent separately in containers, and mixing them before dispensing them for actual use. The viscosity of the composition must not increase significantly for an appropriate amount of time after dispensing so that it can be molded into the desired shape and used. On the other hand, the composition must cure quickly after a certain amount of time has passed since dispensing. For example, the pot life of conventional urethane thermal adhesive compositions used for the same purpose is typically around 30 minutes, and the full cure time is approximately 24 hours. Since these pot life and full cure times are generally proportional, it is important to secure a technology that lengthens the pot life while shortening the full cure time, taking into account the workability and handling of the process.
[0006]
[0007] The present invention has been devised to solve the above-mentioned problems, and the technical task of the present invention is to provide a novel urethane heat-dissipating adhesive composition which has a long working life and an equivalent complete curing time compared to conventional urethane heat-dissipating adhesive compositions by controlling the components of the main part and the hardener part constituting the heat-dissipating adhesive composition, and the contents and properties therebetween, thereby ensuring process stability and excellent thermal conductivity.
[0008] Other objects and advantages of the present invention can be more clearly explained by the detailed description of the invention and the claims below.
[0009]
[0010] In order to achieve the above-mentioned technical task, the present invention provides a urethane-based heat-dissipating adhesive composition comprising a main part comprising a first polyol and a chain extender; and a curing agent part comprising a second polyol and at least three kinds of aromatic isocyanates, wherein the composition has a working time of 50 minutes or more until the initial viscosity formed by mixing the main part and the curing agent part becomes twice as high.
[0011] In one embodiment of the present invention, the urethane-based heat-dissipating adhesive composition is mixed with the main body and the curing agent, and then 2250 cm -1 The complete cure time, where the IR peak in the region disappears, can be within 24 hours.
[0012] In one embodiment of the present invention, the composition may have a working time of 50 to 65 minutes and a complete curing time of 21 to 24 hours.
[0013] In one embodiment of the present invention, the at least three aromatic isocyanates may include a first aromatic diisocyanate comprising at least two arylene groups; a second aromatic diisocyanate comprising one arylene group; and a third aromatic isocyanate having a polyfunctionality exceeding two.
[0014] In one embodiment of the present invention, the mixing ratio of the first aromatic diisocyanate, the second aromatic diisocyanate, and the third aromatic isocyanate may be a weight ratio of 1:1.1 to 2.0:0.1 to 0.9.
[0015] In one embodiment of the present invention, the curing agent may have an NCO content of 14 to 16 wt% and a viscosity of 1100 to 1500 cP (at 25°C).
[0016] In one embodiment of the present invention, the curing agent may include 56 to 66 parts by weight of a second polyol; and 34 to 45 parts by weight of at least three kinds of aromatic isocyanates.
[0017] In one embodiment of the present invention, the subject matter may have an OH value of 190 to 200 mg KOH / g; and a viscosity (at 25°C) of 1100 to 1400 cP.
[0018] In one embodiment of the present invention, the subject part may include 66 to 76 parts by weight of the first polyol; and 24 to 34 parts by weight of the chain extender.
[0019] In one embodiment of the present invention, the mixing ratio between the main body and the hardener may be 1:1.1 to 1.5 by weight.
[0020] In one embodiment of the present invention, the urethane-based heat-dissipating adhesive composition may further include at least one selected from the group consisting of a thermally conductive inorganic filler, a dispersant, a plasticizer, a pigment, and an antioxidant.
[0021]
[0022] According to one embodiment of the present invention, by optimizing the composition of a heat-dissipating adhesive composition by controlling the components constituting the main body and the hardener, and the content and properties therebetween, a working life approximately twice as long and a complete curing time equivalent to that of a conventional urethane heat-dissipating adhesive composition for the same purpose can be secured, thereby improving the work stability, handling, and product reliability of the process.
[0023] Accordingly, the urethane-based heat-dissipating adhesive composition of the present invention can be usefully applied to heat-emitting displays, various portable devices, and electric vehicle batteries.
[0024] The effects according to the present invention are not limited to those exemplified above, and more diverse effects are included in this specification.
[0025]
[0026] Hereinafter, the present invention will be described in detail.
[0027] All terms (including technical and scientific terms) used in this specification, unless otherwise defined, may be used in their common sense by those of ordinary skill in the art to which the present invention pertains. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined otherwise.
[0028] Additionally, throughout this specification, when a part is said to "include" a component, this does not exclude other components, but rather means that other components may be included, unless otherwise specifically stated. Furthermore, throughout this specification, "above" or "on" means not only when the target part is located above or below it, but also when there is another part in between, and does not necessarily mean that the target part is located above the direction of gravity.
[0029] Additionally, in this specification, "functional group" refers to an isocyanate (NCO) group. And "polyol" or a variation thereof broadly refers to a substance having an average number of two or more hydroxyl groups per molecule.
[0030]
[0031] <Urethane-based heat-dissipating adhesive composition>
[0032] One example of the present invention is a urethane-based heat-dissipating adhesive composition used to easily dissipate heat generated in displays, various mobile devices, and / or electric vehicle batteries. It is particularly differentiated by its approximately twice as long working life as existing compositions for the same purpose, while maintaining a comparable full curing time, thereby significantly improving process stability and handling.
[0033] Here, the working time means the time until the initial viscosity doubles after mixing the main component and the hardener. Also, the complete curing time is 2250 cm2, which represents the isocyanate (-NCO) functional group after mixing the main component and the hardener. -1 The IR peak in the region disappears completely, or 1730 cm, which means carbonyl group. -1 It refers to the time at which the peak of the region no longer expands compared to the initial mixture composition.
[0034] The above heat-dissipating adhesive composition is a two-component composition comprising a main component and a curing agent component, and for example, comprises a main component comprising a first polyol and a chain extender; and a curing agent comprising a second polyol and at least three kinds of aromatic isocyanates, wherein each component is composed at a predetermined mixing ratio. If necessary, at least one or more conventional additives in the art, such as an inorganic filler, an adhesion promoter, a plasticizer, a pigment, an antifoaming agent, and a solvent, may be further included.
[0035] Hereinafter, the composition of the urethane-based heat-dissipating adhesive composition will be specifically examined as follows.
[0036] <Theme>
[0037] The above-mentioned subject matter comprises a first polyol and a chain extender.
[0038] 1st polyol
[0039] The first polyol reacts with the isocyanate group of the curing agent part described below, specifically, the isocyanate terminal group of the urethane-based prepolymer, thereby forming a urethane bond, thereby curing the resin composition.
[0040] The first polyol may be any conventional polyol known in the art without limitation, and examples thereof include polycarbonate diol, polyether polyol, and low molecular weight glycols. In particular, as long as the hydroxyl value (OH value) of the main component including the polyol and the chain extender can satisfy 190 to 200 mg KOH / g, there are no particular limitations on the components, content, etc. of the first polyol.
[0041] For example, the first polyol may have two to three activated hydrogens and a number average molecular weight of 500 g / mol to 8,000 g / mol, specifically, a number average molecular weight of 3,000 g / mol to 7,000 g / mol. If the number average molecular weight of the first polyol is outside the above-mentioned range, the number of urethane bonds that realize the hardness of the coating film may be too small or too large, making it impossible to realize an appropriate hardness.
[0042] Non-limiting examples of the usable first polyol include at least one selected from the group consisting of polybutadiene diol, polytetramethylene ether glycol, polypropylene oxide glycol, polypropylene oxide triol, polybutylene oxide glycol, polybutylene oxide diol, polybutylene oxide triol, 1,6-hexanediol, neopentyl glycol, 1,4-butanediol, 1,3-butanediol, ethylene propylene glycol, diethylene glycol, dipropylene glycol, polyether polyol, polyester polyol, and polycaprolactone polyol.
[0043] In the present invention, the content of the first polyol is not particularly limited and depends on the amounts of other components used to form the urethane-based heat-radiating adhesive composition and the desired properties of the heat-radiating adhesive composition. For example, it may be 66 to 76 parts by weight, and specifically 68 to 75 parts by weight, based on the total weight of the subject matter (e.g., 100 parts by weight).
[0044] chain extender
[0045] The subject matter according to the present invention includes a chain extender.
[0046] These chain extenders regulate the rate of polymerization between hydroxyl and isocyanate groups during polyurethane polymerization, and enhance the bonding strength between molecules. Depending on their content and type, the synthesis time and physical properties of polyurethane vary. Therefore, they play a crucial role in the mixing and processing of the two-component main component and curing agent.
[0047] The above chain extender may be any one known in the art without limitation, and it is particularly preferred to use a chain extender containing a carboxyl group and / or a hydroxyl group. In particular, as long as the hydroxyl value (OH value) of the main component including the polyol and the chain extender can satisfy 190 to 200 mg KOH / g, there are no particular limitations on the components, content, etc. of the chain extender.
[0048] For example, the chain extender may be EG (Ethylene Glycol), tripropylene glycol, 1,2-PG (1,2-Propylene Glycol), 1,3-BG (1,3-Butandiol), 1,4-BG (1,4-Butandiol), NPG (Neopentyl glycol), DEG (Diethylene Glycol), MPD (3-Methyl-1,5-Pentandiol), 1,6-HD (1,6-Hexandiol), TMP (Trimethylol Propane), 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxymethyl)butyric acid, or a mixture thereof having a number average molecular weight of 50 to 200 g / mol.
[0049] The content of the chain extender is not particularly limited, and may be, for example, 24 to 34 parts by weight based on the total weight of the subject matter (e.g., 100 parts by weight), and specifically, 28 to 31 parts by weight.
[0050] Considering the long working life and short complete curing time that the present invention aims to achieve, it is preferable to adjust the above-mentioned main component to have an appropriate hydroxyl value (OH value). For example, the hydroxyl value (OH value) of the main component may be 190 to 200 mg KOH / g, and more specifically, 190 to 195 mg KOH / g.
[0051] In addition, the heat-dissipating adhesive composition of the present invention includes an inorganic filler to exhibit excellent thermal conductivity. At this time, if the viscosity of the composition is too low, the inorganic filler will quickly settle out when mixed, preventing it from exhibiting proper physical properties. On the other hand, if the viscosity is too high, uniform mixing with the inorganic filler will not occur. Accordingly, it is preferable to adjust the viscosity to an appropriate range that allows for proper mixing without causing the inorganic filler to settle out too quickly. For example, the viscosity of the main component (at 25°C) may be approximately 1000 to 1500 cP, and more specifically, 1050 to 1450 cP.
[0052] <Hardener Department>
[0053] The above curing agent comprises a second polyol and at least three kinds of aromatic isocyanates.
[0054] Second polyol
[0055] The second polyol is a component included in the curing agent portion, and may be the same as or different from the first polyol of the aforementioned subject portion. Specifically, it is preferable that the second polyol be the same as the first polyol.
[0056] The second polyol may be any conventional polyol known in the art without limitation, and examples thereof include polycarbonate diol, polyether polyol, and low molecular weight glycols. In particular, as long as the isocyanate content (NCO content) of the curing agent portion including the second polyol and at least three aromatic isocyanates satisfies 14 to 16 wt%, there are no particular limitations on the components, content, etc. of the second polyol.
[0057] For example, the second polyol may have two to three activated hydrogens and may have a number average molecular weight of 500 g / mol to 8,000 g / mol, specifically, a number average molecular weight of 3,000 g / mol to 7,000 g / mol.
[0058] Non-limiting examples of usable second polyols include at least one selected from the group consisting of polybutadiene diol, polytetramethylene ether glycol, polypropylene oxide glycol, polypropylene oxide triol, polybutylene oxide glycol, polybutylene oxide diol, polybutylene oxide triol, 1,6-hexanediol, neopentyl glycol, 1,4-butanediol, 1,3-butanediol, ethylene propylene glycol, diethylene glycol, dipropylene glycol, polyether polyol, polyester polyol, and polycaprolactone polyol.
[0059] In the present invention, the content of the second polyol is not particularly limited, and may be, for example, 56 to 66 parts by weight based on the total weight of the curing agent part (e.g., 100 parts by weight), and specifically, 57 to 65 parts by weight.
[0060] aromatic isocyanates
[0061] The curing agent according to the present invention is differentiated from the prior art in that it mixes at least three kinds of aromatic isocyanates and does not contain aliphatic isocyanates.
[0062] The above aromatic isocyanate may be one known in the art, and in particular, as long as the isocyanate content (NCO content) of the curing agent part can satisfy 14 to 16 wt%, there is no particular limitation on the components of the aromatic isocyanate, its content, etc.
[0063] For example, the at least three aromatic isocyanates may include a first aromatic diisocyanate comprising at least two arylene groups; a second aromatic diisocyanate comprising one arylene group; and a third polyfunctional aromatic isocyanate having more than two functional groups.
[0064] For example, a first aromatic diisocyanate compound containing two or more arylene groups has a much faster reactivity than an aromatic isocyanate compound containing one arylene group, and thus, when reacted with a polyol at a typical reaction temperature, it can play a role in shortening the pot life of the composition. Non-limiting examples of the first aromatic isocyanate containing two or more arylene groups that can be used include at least one selected from the group consisting of 4,4-methylenediphenyl diisocyanate (4,4-MDI), 2,4-methylenediphenyl diisocyanate (2,4-MDI), and carbodiimide-modified 4,4-diphenylmethane diisocyanate.
[0065] In addition, the second aromatic isocyanate compound containing one arylene group has a large difference in reactivity between the two terminals, so that when reacted with polyol at a normal temperature, the isocyanate group at the terminal with high reactivity reacts, and the terminal with low reactivity remains free (does not participate in the reaction) and reacts with the hydroxyl group of the curing agent, thereby maintaining the pot life of the composition containing it constant. In addition, it can play a role in improving the mechanical properties by reinforcing the rigidity of the cured product. Such second aromatic isocyanates include toluene diisocyanate, 1,4-Phenylene diisocyanate (PPDI), 1,5-naphthalene diisocyanate, xylene diisocyanate, or mixtures thereof.
[0066] In addition, a third polyfunctional aromatic isocyanate exceeding two functions can form a dense network structure by the polyfunctional groups. At this time, the number of functional groups (NCO) contained in the third polyfunctional aromatic isocyanate is not particularly limited as long as it exceeds 2. For example, it is more than 2 and 5 or less, and specifically, it can be 2.1 to 4.5, and more specifically, 2.3 to 4.0.
[0067] In the present invention, considering a long working life, a short complete curing time, excellent mechanical properties and thermal conductivity, it is preferable to control at least three kinds of aromatic isocyanates at a specific mixing ratio.
[0068] For example, the mixing ratio of the first aromatic diisocyanate, the second aromatic diisocyanate, and the third polyfunctional aromatic isocyanate may be 1:1.1 to 2.0:0.1 to 0.9 by weight, and specifically, may be 1:1.3 to 1.8:0.4 to 0.8 by weight. In other words, the mixing ratio of the first aromatic diisocyanate, the second aromatic diisocyanate, and the third polyfunctional aromatic isocyanate may be 7 to 17:15 to 25:5 to 10 by weight.
[0069] The content of the at least three kinds of isocyanates is not particularly limited, and may be, for example, 34 to 44 parts by weight based on the total weight of the curing agent part (e.g., 100 parts by weight), and specifically, 38 to 42 parts by weight.
[0070] It is preferable that the curing agent according to the present invention be adjusted to have an appropriate isocyanate content (NCO content) considering a long working life and a short complete curing time. For example, the NCO content of the curing agent may be 14 to 16 wt%, and specifically 14 to 15 wt%.
[0071] A urethane prepolymer is formed by reacting at least three kinds of aromatic isocyanate compounds included in the curing agent with a second polyol. This urethane prepolymer may have an unreacted isocyanate group (NCO) content of 13 to 18 wt%, and specifically 14 to 16 wt%. In addition, the weight average molecular weight may be 4,000 to 8,000 g / mol, and more specifically 6,000 to 7,000 g / mol.
[0072] In addition, the viscosity (at 25°C) of the curing agent, for example, the urethane-based prepolymer, may be approximately 1000 to 1500 cP, and more specifically, 1050 to 1450 cP.
[0073] Weapon Filler
[0074] The urethane-based heat-dissipating adhesive composition according to the present invention may include a conventional inorganic filler known in the art, specifically a thermally conductive inorganic filler, to ensure heat dissipation properties. This inorganic filler enhances the mechanical properties of the heat-dissipating adhesive and improves thermal conductivity.
[0075] The above inorganic filler is not particularly limited as long as it is a typical filler used in a heat-dissipating adhesive composition. For example, it may be at least one selected from gold, silver, copper, nickel, iron, silica, alumina (Al2O3), aluminum nitride (AlN), boron nitride (BN), graphene, carbon, silver-coated copper powder (Ag coated Cu), silver-coated nickel powder (Ag coated Ni), silver-coated iron powder (Ag coated Fe), and silver-coated glass powder (Ag coated glass).
[0076] The average particle diameter of such inorganic fillers may range from 0.5 μm to 100 μm, specifically from 1.0 to 80 μm, and more specifically from 1.0 to 70 μm.
[0077] The content of the above-mentioned inorganic filler is not particularly limited, and for example, it may be included in an amount of 75 to 95 parts by weight, specifically 85 to 92 parts by weight, based on 100 parts by weight of the heat-dissipating adhesive composition.
[0078] Additives
[0079] The urethane heat-resistant adhesive composition of the present invention may optionally further include at least one additive commonly used in the relevant field, within a range that does not impair the inherent properties of the composition.
[0080] Non-limiting examples of usable additives include antioxidants, plasticizers, flow regulators, leveling agents, coupling agents, surfactants, pigments, dispersants, lubricants, flame retardants, antifoaming agents, colorants, diluents, chain extenders, adhesion improvers, curing retardants, surface conditioners, softeners, thickeners, defoamers, weather-resistant additives, desiccants, appearance regulators, coupling agents, moisture absorbers, coupling agents, colorants, or mixtures of two or more thereof. In addition, the content of the additives may be appropriately added within a content range known in the art, and for example, may be 0.1 to 10 parts by weight based on the total weight of the urethane-based heat-resistant adhesive composition.
[0081] The urethane heat-resistant adhesive composition of the present invention can be manufactured according to a conventional method known in the art, and for example, can be manufactured by forming a main part containing the first polyol and a chain extender as described above, a curing agent part containing the second polyol and at least three kinds of aromatic isocyanates, and, if necessary, one or more kinds of additives as described above, and then mixing them at a specific ratio.
[0082] Here, the mixing ratio between the subject part and the hardener part is not particularly limited, and may be, for example, a weight ratio of 1.0:1.1 to 1.5, and specifically, a weight ratio of 1.0:1.1 to 1.3.
[0083] The urethane-based heat-resistant adhesive composition of the present invention, described above, exhibits a longer working life and a shorter complete curing time compared to compositions for the same purpose, thereby improving process stability and handling. Furthermore, it can secure high thermal conductivity and excellent mechanical properties.
[0084] For example, the urethane-based heat-resistant adhesive composition may have a working time of 50 minutes or more until the initial viscosity formed by mixing the main component and the hardener component becomes twice that of the original viscosity, specifically 50 to 65 minutes, and more specifically 52 to 65 minutes.
[0085] For another specific example, the urethane-based heat-resistant adhesive composition is 2250 cm after the main body and the hardener are mixed. -1 The complete cure time at which the IR peak of the region disappears may be within 24 hours, and specifically may be between 21 and 24 hours.
[0086] For example, a polyurethane heat-resistant adhesive composition for the same purpose, which has a complete curing time of about 24 hours or less, generally exhibits a pot life of about 30 minutes. In contrast, the polyurethane heat-resistant adhesive composition of the present invention exhibits a comparable complete curing time of less than 24 hours, while exhibiting a pot life of about 60 minutes. Thus, the polyurethane heat-resistant adhesive composition of the present invention selectively increases only the pot life by about two times or more, and thus, the relationship between the existing proportional pot life and the complete curing time can be freely adjusted and / or changed, thereby significantly improving process workability and mass productivity.
[0087] As another specific example, the urethane-based heat-dissipating adhesive composition may have a viscosity of approximately 1000 to 1500 cP, and more specifically, 1050 to 1450 cP.
[0088] The urethane-based heat-dissipating adhesive composition and its cured product according to the present invention can be usefully applied to heat-emitting displays, various portable devices, and electric vehicle batteries. They can also be applied without limitation to various other technical fields.
[0089]
[0090] Hereinafter, the present invention will be described in detail through examples, but the following examples and experimental examples are merely illustrative of one form of the present invention, and the scope of the present invention is not limited to the following examples and experimental examples.
[0091]
[0092] [Reference example]
[0093] The specific specifications of the components used in the following examples and comparative examples are as shown in Table 1 below.
[0094] Composition Composition Detailed Specifications Subject Polyol A Primary Polyol SK PEURO Product Name Y-3328 Chain Extender B Chain Extender Tripropylene Glycol CAS# 24800-44-0 Curing Agent Secondary Polyol SK PEURO Product Name Y-3328 Isocyanate D-1 Primary Aromatic Isocyanate Kumho Mitsui Chemicals Product Name PICAS# 101-68-8 D-2 Second Aromatic Isocyanate 2,4-Toluene Diisocyanate (TDI) CAS# 584-84-9 D-3 Third Aromatic Isocyanate Kumho Mitsui Chemicals Product Name M2002.7 Functional (NCO) D-4 Primary Aliphatic Isocyanate hexamethylene diisocyanate (HDI) CAS# 822-06-0 D-5 Second Aliphatic Isocyanate isophorone diisocyanate(IPDI) CAS# 4098-71-9
[0095]
[0096] [Experimental Example 1]
[0097] An experiment was conducted to determine the appropriate hydroxyl value (OH value) of the main component and the appropriate NCO content of the hardener by composing the main component and the hardener according to the mixing ratio in Table 2 below.
[0098] Specifically, the curing agent portion in Table 2 below is a prepolymer commonly used in the polyurethane industry, and was manufactured by placing all raw materials constituting the curing agent portion into a reactor and stirring at 80°C for 2.5 hours at a speed of 150 rpm. In addition, the main portion was manufactured by stirring all raw materials constituting the main portion at 800 rpm for approximately 10 minutes.
[0099] Here, the OH value of the main component refers to a calculated value derived by calculating the OH value of the polyol and the OH value of the chain extender as a ratio. In addition, the NCO content of the hardener component refers to a calculated value derived by calculating the NCO content of each raw material as a ratio.
[0100] And the viscosity of each of the main component and the hardener is the value measured using Anton Parr's Rheometer at room temperature (e.g., 25℃). In addition, the physical properties such as viscosity, pot life, and complete curing time below are the values measured using Anton Parr's Rheometer immediately after putting the main component and the hardener into a container in equal masses and stirring them for 1 minute at 800 rpm using a paste mixer.
[0101] Composition of composition (by weight) #1 Nos. 1234567891011 Subject A66-7653-6362-7272-8281-9166-7666-7666-7666-7653-6362-7272-82 B24-3437-4728-3818-289-1924-3424-3424-3424-3424-3437-4728-3818-28 Total 100100100100100100100100100100100100100OH value (mg KOH / g)190-200265-275213-223155-165103-113190-200190-200190-200190-200265-275213-223155-165Viscosity(cP)123672591311881998138314641581175046810611816Curing agentC48-5848-5848-5848-5848-5832-4243-535 5-6566-7632-4243-5355-65D-135-4535-4535-4535-4535-4551-6140-5028-3817-2751-6140-5028-38D-35 -105-105-105-105-105-105-105-105-105-105-105-10Total100100100100100100100100100100100100NCO Content (wt%) 14-1614-1614-1614-1614-1619-2115-1711-137-919-2115-1711-13 Viscosity (cP) 130176396112502103145615411664184249311171912 Composition Properties Pot Life (min) 23.011.011.026.027.013.016.020.026.011.016.029.0 Complete Cure Time (hrs) 21.017.017.025.026.018.019.024.025.017.018.024.0
[0102] As shown in Table 2 above, when the hydroxyl value (OH value) of the main part is 190 to 200 and the NCO content of the hardener is 14 to 16, it was confirmed that the pot life of the urethane-based heat-dissipating adhesive composition formed by mixing them was approximately 23 minutes and the complete curing time was 21 hours. In addition to the pot life and complete curing time, one of the important physical properties is viscosity. If the viscosity is too low, the inorganic filler will quickly settle when mixed, preventing it from exhibiting proper physical properties, and if it is too high, uniform mixing with the inorganic filler will not occur. Accordingly, in the present invention, the range of the appropriate viscosity that allows for proper mixing without causing the inorganic filler to settle too quickly was determined to be approximately 1,000 cP to 1,500 cP.
[0103]
[0104] [Experimental Example 2]
[0105] The urethane-based heat-dissipating adhesive compositions of Example 1 and Comparative Examples 1 to 9 were prepared by respectively configuring the main component and the curing agent component according to the mixing ratios in Table 3 below. In Table 3 below, the unit of amount of each composition used is parts by weight.
[0106] Specifically, as shown in #1 of Table 2 above, the composition of Example 1 was formed by setting the appropriate hydroxyl value (OH value) of the main part to 190 to 200 and the appropriate NCO content of the hardener part to 14 to 16 wt%. In addition, urethane-based heat-dissipating adhesive compositions of Comparative Examples 1 to 9 were formed in the same manner as in Example 1 except that the mixing ratio was changed as shown in Table 3 below. Thereafter, the working time and complete curing time for each composition were confirmed.
[0107] Here, the working time means the time until the initial viscosity is doubled after mixing the main part and the hardener part, and the complete curing time means the time until the isocyanate functional group is measured at 2250 cm when mixing the main part and the hardener part and measuring the IR. -1The peak in the region completely disappears, or 1730 cm, which means carbonyl group. -1 It refers to the time at which the peak of the area no longer expands compared to the initial point.
[0108] Composition of composition (weight part) Example 1 Comparative example 1 2 3 4 5 6 7 8 9 Subject part A 66-7666-7666-7666-7666-7666-7666-7666-7666-7666-7666-76B 24-3424-3424-3424-3424-3424-3424-3424-3424-3424-3424-3424-3424-34 Total 100 100 100 100 100 100 100 100 OH value (mg) KOH / g)190-200190-200190-200190-200190-200190-200190-200190-200190-200190-200190-200Viscosity(cP)1258125012441236118811471121117911641156Curing agentC56-6652-6260-7048-5852-6257-6762-7249-5950-6051-61D-17-1721-310. 1-3.035-4521-316-160.1-1.024-3413-232-12D-215-255-1525-35-------D-35-105-101-55-105-105-101-55- 105-105-10D-4----5-1515-2525-35---D-5-------5-1515-2525-35Total100100100100100100100100100100NCO Content (wt%) 14-16 14-16 14-16 16 14-16 16 14-16 16 14-16 16 14-16 16 16 16 16 16 16 16 16 13 2 4 13 16 13 0 9 13 0 11 2 5 0 12 0 7 11 8 0 12 4 11 2 2 5 12 17 Composition Properties Pot Life (min) 6 2.0 4 3.0 7 5.0 2 3 39.0 3 8.0 4 5.0 4 0.0 4 4.0 5 1.0 Complete Cure Time (hrs) 22.0 2 2.0 2 6.0 2 1 2 3.0 2 3.0 2 3.0 2 3.0 2 4.0 2 4.0 2 5.0
[0109] As shown in Table 3 above, Example 2, which included three types of aromatic isocyanates and was composed by adjusting their mixing ratios within a predetermined range, exhibited a pot life of 62 minutes and a complete curing time of 22 hours. Accordingly, it was confirmed that the composition has a long pot life and a short complete curing time, which are the characteristics sought by the present invention.
Claims
1. A main component comprising a first polyol and a chain extender; and A curing agent comprising a second polyol and at least three kinds of aromatic isocyanates; Includes, A urethane-based heat-resistant adhesive composition having a working time of 50 minutes or more until the initial viscosity formed by mixing the above-mentioned main component and the above-mentioned hardener component becomes twice that of the original viscosity.
2. In paragraph 1, After the above-mentioned subject and the above-mentioned hardener are mixed, 2250 cm -1 A urethane-based heat-dissipating adhesive composition having a complete curing time of less than 24 hours at which the IR peak of the region disappears.
3. In paragraph 1, The above composition, The running time is 50 to 65 minutes, A urethane-based heat-insulating adhesive composition having a complete curing time of 21 to 24 hours.
4. In paragraph 1, The above at least three kinds of aromatic isocyanates, A first aromatic diisocyanate comprising at least two arylene groups; A second aromatic diisocyanate containing one arylene group; and Polyfunctional tertiary aromatic isocyanates exceeding two functions A urethane-based heat-dissipating adhesive composition comprising:
5. In paragraph 4, A urethane-based heat-dissipating adhesive composition, wherein the mixing ratio of the first aromatic diisocyanate, the second aromatic diisocyanate, and the third aromatic isocyanate is 1:1.1 to 2.0:0.1 to 0.9 by weight.
6. In paragraph 1, The above hardening agent part is, 56 to 66 parts by weight of a second polyol; and A urethane-based heat-resistant adhesive composition comprising 34 to 44 parts by weight of at least three kinds of aromatic isocyanates.
7. In paragraph 1, The above hardening agent part is, NCO content of 14 to 16 wt%; and A urethane-based heat-resistant adhesive composition having a viscosity of 1100 to 1500 cP (at 25°C).
8. In paragraph 1, The above subject matter is, 66 to 76 parts by weight of the first polyol; and A urethane-based heat-resistant adhesive composition comprising 24 to 34 parts by weight of a chain extender.
9. In paragraph 1, The above subject matter is, OH value of 190 to 200 mg KOH / g; and A urethane-based heat-resistant adhesive composition having a viscosity of 1100 to 1400 cP (at 25°C).
10. In paragraph 1, A urethane-based heat-dissipating adhesive composition having a mixing ratio between the above-mentioned main body and the hardener body of 1.0:1.1 to 1.
5.
11. In paragraph 1, A urethane-based heat-dissipating adhesive composition further comprising at least one selected from the group consisting of a thermally conductive inorganic filler, a dispersant, a plasticizer, a pigment, and an antioxidant.
Citation Information
Patent Citations
Curable urethane composition
JP2022108266A
Curable urethane composition, and cured product thereof
JP2022134107A
Polyurethane resin for hot melt adhesive and two-component polyurethane hot melt adhesive comprising the same, and method for forming polyurethane resin for hot melt adhesive
KR101874301B1
Resin Composition
KR102112790B1
Polyol component and use thereof for producing rigid polyurethane foams