Shape memory polymer comprising 8-arm structured compound and use thereof

The 8-arm structural compound with shape memory properties addresses the issue of abnormal blood flow and strength limitations in current polymers, enhancing vascular graft support and expanding its industrial applications by controlling shape restoration temperature and improving strength, effectively preventing vascular stenosis and improving graft patency.

WO2024205140A1PCT designated stage expired Publication Date: 2024-10-03TMD LAB CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003609
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current shape memory polymers used in medical applications, such as coronary artery bypass grafts, face challenges due to differences in physical properties between arteries and veins, leading to abnormal blood flow and vascular stenosis, and lack the necessary strength for industrial applications.

Method used

A novel 8-arm structural compound with shape memory properties is developed, allowing for controlled shape restoration temperature and improved strength through crosslinking, which can be used as both a medical material and industrial material, specifically designed to support vascular grafts during coronary artery bypass surgery.

Benefits of technology

The 8-arm compound effectively prevents vascular stenosis by controlling abnormal blood flow and enhancing the strength of vascular grafts, improving the patency rate of vein grafts and expanding its use beyond medical applications to various industrial materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003609_03102024_PF_FP_ABST
    Figure KR2024003609_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a shape memory polymer comprising an 8-arm structured compound and use thereof. The 8-arm structured compound according to the present invention can be prepared as a temperature-based shape memory polymer that exhibits shape memory properties by crosslinking, and has a shape restoration temperature that is adjustable through monomer control, and thus not only can be developed into various industrial materials, but can also be developed into biocompatible medical materials.
Need to check novelty before this filing date? Find Prior Art

Description

Shape memory polymer comprising 8-ARM structural compound and use thereof

[0001] The present invention relates to a shape memory polymer comprising an 8-arm structured compound and a use thereof, and more particularly, to a shape memory polymer comprising an 8-arm structured compound which exhibits shape memory properties by crosslinking and allows shape restoration temperature control through monomer control, and a use thereof.

[0002] Coronary artery disease (CAD) is a cardiovascular disease caused by vascular narrowing due to arteriosclerosis. It encompasses angina, myocardial infarction, and ischemic heart disease. Treatment strategies for CAD include lifestyle modifications, medications, and interventional procedures such as stents and balloon angioplasty. For severe cases of CAD, characterized by three or more vascular stenosis, surgical treatment called coronary artery bypass grafting (CABG) is necessary.

[0003] Coronary artery bypass grafting (CABG) is a surgical procedure that reroutes blood flow to the heart muscle by connecting a narrowed artery to a new blood vessel. This requires a vascular graft to facilitate the bypass. The left internal mammary artery (LMA) is typically used, but because it can only be used as a single bypass, the saphenous vein is harvested from the patient's leg and grafted.

[0004] However, the patency rate of grafted vessels using the venous graft is significantly lower than that of grafted arteries. This is due to the difference in physical properties between arteries and veins, which causes abnormal blood flow at the vascular junction, leading to endothelial dysfunction and vascular stenosis. Therefore, a device is needed to suppress the occurrence of abnormal blood flow, the fundamental cause of vascular stenosis, and prevent arterialization and stenosis of the vein.

[0005] Korean Patent Registration Nos. 10-1906472 and 10-2208921, and Korean Publication No. 10-2021-0158356 disclose shape memory polymers, their manufacturing methods, and their use as medical materials. However, in order to use them as various industrial materials, it was necessary to further improve their strength. Accordingly, the inventors of the present invention have made efforts to develop a compound having improved strength characteristics that can be used not only as a medical material but also as a variety of industrial materials, taking note of the problems of the prior art, and as a result, when synthesizing a compound with an 8-arm structure as in the present invention, shape memory temperature control is possible along with shape memory characteristics by crosslinking, and strength characteristics can be improved compared to existing compounds, and when a shape memory polymer with improved strength is used as a medical material, it is possible to manufacture a vascular outer wall support that can prevent vascular stenosis by controlling abnormal blood flow when blood flow moves from a vein graft to an artery by wrapping it outside the blood vessel during coronary artery bypass surgery, thereby completing the present invention.

[0006] The purpose of the present invention is to provide a novel compound having an 8-arm structure, a method for preparing the same, and a use thereof.

[0007] To achieve the above purpose, the present invention provides a compound represented by the following chemical formula (1):

[0008] Chemical formula (1)

[0009]

[0010] In the above chemical formula (1),

[0011] x and y are integers from 1 to 20, independently of each other,

[0012] m and n represent the mole % of repeating units,

[0013] m+n is 100, and m is between 70 and 99.

[0014] In the present invention, the compound may be characterized by having shape memory properties through crosslinking.

[0015] In the present invention, the compound may be characterized in that it has an average shape restoration ability of 90% or more at a temperature of 25 to 58°C after crosslinking.

[0016] The present invention also provides a method for preparing the compound, comprising a step of reacting tripentaerythritol, a lactone monomer, and glycidyl methacrylate.

[0017] In the present invention, the reaction may be characterized as being a ring-opening polymerization reaction.

[0018] In the present invention, the reaction may be characterized by reacting in the presence of a catalyst selected from the group consisting of 1,5,7-triazabicyclo(4.4.0)dec-5-ene, tin(II)(2-ethylhexanoate), trimethylopropane tris(3-mercaptopropionate), and zinc succinate.

[0019] In the present invention, it may be characterized by reacting at 80 to 160°C.

[0020] The present invention also provides a shape memory polymer in which the compound is crosslinked.

[0021] The present invention also provides a method for producing a shape memory polymer, further comprising a step of inducing a crosslinking reaction in the compound produced by the above production method.

[0022] In the present invention, the crosslinking reaction may be characterized as being a photocrosslinking or thermal crosslinking reaction.

[0023] The present invention also provides a medical material comprising the compound.

[0024] In the present invention, the medical material may be characterized as being a support for a vascular graft or a ligator for a vascular graft.

[0025] In the present invention, the support of the vascular graft may be characterized as being a support of the vascular graft that is provided to surround and ligate the coronary vein during coronary artery bypass grafting.

[0026] In the present invention, the support of the vascular graft may be characterized in that the diameter thereof becomes wider as it goes outward from the anastomosis site of the artery and vein.

[0027] In the present invention, the support of the vascular graft may be characterized in that the angle of the tangent line of the anastomosis between the artery and vein is 15° to 60°.

[0028] The present invention also provides an industrial material comprising the compound.

[0029] The 8-arm structural compound according to the present invention can be manufactured into a temperature-dependent shape memory polymer exhibiting shape memory properties by crosslinking, and the shape recovery temperature can be controlled by controlling the monomer, so that the strength properties are improved, enabling development into various industrial materials. In addition, it has the advantage of enabling development into a medical material due to its biocompatibility.

[0030]

[0031] Figure 1 illustrates a synthetic mechanism of a compound having an 8-arm structure according to some embodiments of the present invention.

[0032] Figure 2 is a structural analysis of a compound having an 8-arm type structure according to some embodiments of the present invention. 1This is the H-NMR result.

[0033] FIG. 3 is a DSC measurement graph confirming the melting temperature (a) and crystallization temperature (b) of a compound having an 8-arm structure before crosslinking into a shape memory polymer according to some embodiments of the present invention.

[0034] FIG. 4 is a DSC measurement graph confirming the melting temperature (a) and crystallization temperature (b) after crosslinking of a compound having an 8-arm structure into a shape memory polymer according to some embodiments of the present invention.

[0035] FIG. 5 is a result of confirming the mechanical properties of a compound having an 8-arm structure according to one embodiment of the present invention after crosslinking with a shape memory polymer.

[0036] FIG. 6 is a result of confirming the shape memory characteristics after crosslinking of a compound having an 8-arm structure according to one embodiment of the present invention into a shape memory polymer.

[0037] Figure 7a shows a designed single unit pattern of a vascular graft scaffold for coronary artery bypass grafting, and Figure 7b shows a designed overall device design of a vascular graft scaffold for coronary artery bypass grafting.

[0038] Figure 8 is a computer modeling result showing the effect of improving blood flow according to the presence or absence of a vascular graft support for coronary artery bypass grafting.

[0039] Figures 9a-9e are computer modeling results showing the abnormal blood flow control effect according to the shape and length of a vascular graft scaffold for coronary artery bypass grafting.

[0040] Figure 10 shows the results of computer modeling analysis according to the anastomotic angle of a vascular graft support for coronary artery bypass grafting.

[0041]

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In general, the nomenclature used herein and the experimental methods described below are well known and commonly used in the art.

[0043]

[0044] In the present invention, a "shape memory polymer (SMP)" means a polymer that has the property of returning to its original shape when an object is made to have a certain shape under specific conditions and the shape is subsequently changed by an external impact, when the object is made to have the same initial conditions (temperature, light, pH, humidity, etc.).

[0045] In the present invention, it should be understood that terms such as “include” or “have” are intended to specify the presence of a feature, number, step, operation, component, part or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts or combinations thereof.

[0046]

[0047] In the present invention, when a lactone monomer (e.g., epsilon-caprolactone (ε-CL)) and glycidyl methacrylate (GMA) are reacted with an initiator (e.g., tripentaerythritol), a novel polycaprolactone-based compound can be synthesized, and it was confirmed that excellent shape memory properties are imparted when a network is formed between the polymer chains of the compound through crosslinking, and that shape recovery temperature control is also possible when the monomer is controlled.

[0048] Accordingly, the present invention relates, in one aspect, to a compound represented by the following chemical formula (1):

[0049] Chemical formula (1)

[0050]

[0051] In the above chemical formula (1),

[0052] x and y are integers from 1 to 20, independently of each other,

[0053] m and n represent the mole % of repeating units,

[0054] m+n is 100, and m is between 70 and 99.

[0055] The shape restoration temperature, etc. of the compound of the present invention can be controlled depending on the amount of ε-caprolactone monomer and glycidyl methacrylate monomer constituting the compound.

[0056] More specifically, in the above chemical formula (1), x and y are each independently an integer from 1 to 20, which can be adjusted by the carbon number of the initiator in the step of synthesizing the compound of chemical formula (1).

[0057] For example, when epsilon caprolactone (ε-CL) is used, x can be 3, and when dipentaerythritol is used, y can be 1. In addition, the number of x can be controlled by using monomers such as α-acetolactone, β-propiolactone, γ-butyrolactone, and δ-valerolactone instead of epsilon caprolactone (ε-CL), and the number of y can be controlled by using an initiator such as 8-arm PEG instead of dipentaerythritol.

[0058] In addition, in the chemical formula (1), m and n represent the molar % of repeating units, m+n is 100, and x can be 70 to 99, or 88 to 96, or 92 to 96, or 94 to 96.

[0059] Here, mole% refers to the ratio of repeating units of m and n, and specifically, may refer to mole fraction. For example, in PCL-co-PGMA, it may refer to the mole fraction of repeating units of PCL and PGMA.

[0060] In the present invention, the compound may be characterized by having shape memory properties through crosslinking.

[0061] In the present invention, the compound is crosslinked at a temperature of 25 to 58°C after crosslinking, or at any range of 25 to 58°C, or at any temperature of 25 to 58°C, for example, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, about 30°C, about 31°C, about 32°C, about 33°C, about 34°C, about 35°C, about 36°C, about 37°C, about 38°C, about 39°C, about 40°C, about 41°C, about 42°C, about 43°C, about 44°C, about 45°C, about 46°C, about 47°C, about 48°C, about 49°C, about 50°C, about 51°C, about 52°C, about 53°C, about 54°C, about 55°C, about 56°C, about It may be characterized by an average shape recovery ability of 90% or more, for example, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, or about 100% at 57°C or about 58°C, but is not limited thereto.

[0062]

[0063] In the present invention, the shape restoration ability (%) can be calculated by the following equation (1).

[0064] ----- Formula (1)

[0065]

[0066] The compound of the present invention can be prepared by reacting an α-acetolactone, β-propiolactone, γ-butyrolactone, δ-valerolactone or εcaprolactone monomer with an acrylic monomer containing a glycidyl group (e.g., glycidyl methacrylate) and an initiator.

[0067] For example, the compound of the present invention can be prepared by ring-opening polymerization of tripentaerythritol, caprolactone, and glycidyl methacrylate.

[0068] In this case, the reactivity can be improved by adding a catalyst or by adding a polymerization inhibitor together with or simultaneously with the initiator during the initial reaction when the polymerization conversion is almost zero, thereby inhibiting the reaction between temperature-sensitive glycidyl methacrylate groups.

[0069]

[0070] Accordingly, the present invention relates to a method for preparing the compound, comprising a step of reacting tripentaerythritol, a lactone monomer (e.g., caprolactone) and glycidyl methacrylate from another aspect.

[0071] In the present invention, the reaction may be characterized as being a ring-opening polymerization reaction.

[0072] In the present invention, the reaction may be characterized by reacting in the presence of a catalyst selected from the group consisting of 1,5,7-triazabicyclo(4.4.0)dec-5-ene, tin(II)(2-ethylhexanoate), trimethylopropane tris(3-mercaptopropionate), and zinc succinate, but is not limited thereto.

[0073] In particular, it is preferable to use 1,5,7-Triazabicyclo(4.4.0)dec-5-ene as a catalyst, which can shorten the synthesis time of the compound, as a substance for inducing simultaneous ring-opening polymerization of two monomers (CL, GMA).

[0074] In the present invention, a polymerization inhibitor can be added during the initial reaction, i.e., before adding glycidyl methacrylate, to inhibit the reaction between methacrylate groups.

[0075] In addition, the polymerization inhibitor plays a role in suppressing the exothermic reaction that occurs locally in the latter half of polymerization and eliminating unreacted residual radicals to terminate the reaction.

[0076] In this way, when the initiator and polymerization inhibitor are reacted with the lactone monomers caprolactone and glycidyl methacrylate at about 110°C for about 6 hours, the ring structure in the monomers is opened, and an 8-arm polycaprolactone-polyglycidyl methacrylate (8-arm PCL-PGMA) polymer is synthesized.

[0077] In the present invention, the initiator may be characterized as being tripentaerythritol, and specifically, the present invention may be characterized as being characterized in that an 8-arm polycaprolactone-polyglycidyl methacrylate (8-arm PCL-PGMA) polymer is synthesized by the initial addition of the initiator.

[0078] In the present invention, the polymerization inhibitor may be at least one selected from the group consisting of hydroquinone, hydroquinone monomethyl ether, p-benzoquinone, and phenothiazine, but is not limited thereto. Preferably, the polymerization inhibitor may be hydroquinone.

[0079] In the present invention, the manufacturing method may be characterized by reacting tripentaerythritol, caprolactone, and glycidyl methacrylate at 80 to 160°C, preferably 100 to 130°C, for example, at about 110°C.

[0080] In this case, if the synthesis of the compound of the present invention proceeds at a temperature below 100°C, the catalytic reaction may not proceed, and if the synthesis of the compound of the present invention proceeds at a temperature exceeding 130°C, a problem may occur in which methacrylate reacts and hardens during the reaction.

[0081]

[0082] In a preferred embodiment, the polymerization mechanism of the compound of the present invention can be expressed as follows.

[0083]

[0084] [Reaction Formula 1]

[0085]

[0086]

[0087] In the present invention, the crosslinking reaction may be characterized as being a photocrosslinking or thermal crosslinking reaction, but is not limited thereto.

[0088] The compound of the present invention may have a structure of a polymer in which an ε-caprolactone monomer and an acrylic monomer containing a glycidyl group are polymerized. For example, the compound may have a structure of a polymer [PCL-co-PGMA] in which an ε-caprolactone monomer (CL; caprolactone) and a glycidyl methacrylate (GMA) monomer are polymerized.

[0089] In the compound of the present invention, the arrangement order of the ε-caprolactone monomer and the glycidyl methacrylate monomer is not particularly limited, and may be arranged alternately, randomly, or in blocks.

[0090] Additionally, a hydroxyl group or the like may be bonded to the terminal of the copolymer. A copolymer having a hydroxyl group bonded to the terminal can be produced by polymerization using an initiator having a hydroxyl group bonded to the terminal.

[0091] Meanwhile, the glycidyl group included in the glycidyl methacrylate monomer may be a crosslinkable functional group, and may be a photocrosslinkable functional group or a thermally crosslinkable functional group. In addition, the copolymer may have shape memory properties due to crosslinking.

[0092] In another aspect, the present invention relates to a shape memory polymer in which the compound is crosslinked.

[0093] In another aspect, the present invention relates to a method for producing a shape memory polymer, further comprising a step of inducing a cross-linking reaction in the compound.

[0094] In the present invention, the crosslinking agent for the crosslinking reaction may be at least one selected from the group consisting of potassium persulfate, ammonium persulfate, benzoyl peroxide, diauryl peroxide, dicumyl peroxide, hydrogen peroxide, azobisisobutuyronitrile, Irgacure, Darocure, LAP (lithium phenyl-2,4,6-trim ethylbenzoylphosphinate), TPO (diphenyl(2,4,6-trimethylbenzoyl)phosphine), and TPO-L (ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate).

[0095] For example, the crosslinking agent that initiates the crosslinking reaction may be, but is not limited to, a peroxide crosslinking agent (benzoyl peroxide, dicumyl peroxide, etc.), Irgacure2959, Irgacure784, Irgacure819, Darocur1173, or Darocur4265.

[0096]

[0097] Meanwhile, the compound of the present invention is a thermosensitive compound that has biocompatibility and can control shape restoration temperature by controlling monomers, so it can be used as a medical material, and its strength characteristics are improved by the multi-structure, so its range of use can be expanded to various industrial materials.

[0098] Therefore, the present invention, from another aspect, relates to a medical material comprising the compound.

[0099] In the present invention, the medical material may be manufactured using a shape memory polymer crosslinked with the compound.

[0100] In the present invention, the medical material may be characterized as being a support for a vascular graft or a ligator for a vascular graft.

[0101] In the present invention, the support of the vascular graft may be characterized as being a support of the vascular graft that is provided to surround and ligate the coronary vein during coronary artery bypass grafting.

[0102] In the present invention, the support of the vascular graft may be characterized in that the diameter thereof becomes wider as it goes outward from the anastomosis site of the artery and vein.

[0103] In the present invention, the support of the vascular graft may have a diameter of about 1 mm to about 4 mm at the anastomosis site of the artery and vein, and a diameter of about 5 mm to about 10 mm at the outermost side from the anastomosis site, but is not limited thereto.

[0104] In one embodiment, the scaffold of the vascular graft may have a diameter of about 2.5 mm to about 3.5 mm at the anastomotic site between the artery and vein, and a diameter of about 5 mm to about 7 mm at the outermost end from the anastomotic site.

[0105] In the present invention, the support of the vascular graft may be about 8 cm to 20 cm, preferably about 10 cm to 15 cm. By manufacturing the support of the vascular graft to be about 8 cm or more, preferably about 10 cm or more, there is an advantage in that the area having low shear stress is minimized; however, if the support of the vascular graft becomes excessively long, it is unsuitable for vascular grafting.

[0106] In the present invention, the support of the vascular graft may be characterized in that the angle of the tangent line of the anastomosis between the artery and vein is 15° to 60°.

[0107] Considering the vibration shear coefficient and time-averaged shear stress, the angle of the tangent line between the anastomotic portion of the artery and vein of the support of the vascular graft is preferably 15° or more, but there is a problem that the maximum wall shear stress increases rapidly when it exceeds 60°.

[0108] In one embodiment, the scaffold of the vascular graft may have an angle of 15° to 45° between the tangent lines of the anastomotic portions of the artery and vein.

[0109] Preferably, the support of the vascular graft may have an angle of about 15° to about 40° between the tangent lines of the anastomotic portion of the artery and vein.

[0110] In another aspect, the present invention relates to an industrial material comprising the compound.

[0111] In the present invention, the industrial material may be manufactured using a shape memory polymer crosslinked with the compound.

[0112] In another aspect, the present invention relates to the use of the compound for manufacturing medical devices or industrial products.

[0113] In another aspect, the present invention relates to a medical treatment or surgical method, comprising a step of inserting or implanting a medical device including the medical material into an individual in need thereof.

[0114] In one aspect, the medical device may be for endovascular implantation.

[0115]

[0116] [Example]

[0117] Hereinafter, the present invention will be described in more detail through examples. These examples are intended solely to illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples.

[0118]

[0119] Example: Synthesis of 8armx%PCL-y%PGMA

[0120] By varying the ratio of PCL and PGMA, 8-armx%PCL-y%PGMA was synthesized as shown in Table 1.

[0121]

[0122]

[0123]

[0124] Tripentaerythritol (initiator, Sigma Aldrich) and hydroquinone (HQ, inhibitor, Sigma Aldrich) were placed in a three-necked flask, vacuum-dried, and nitrogen purged at a rate of 50 cc / min. Purified epsilon-caprolactone (CL, monomer, AVENTION) was added and stirred at 110°C for 10 minutes. After that, glycidyl methacrylate (GMA, monomer, Sigma Aldrich) was added and stirred for 10 minutes, and then triazabicyclodecene (TBD, catalyst, TCI) dissolved in acetonitrile (ACN, Sigma Aldrich) was injected. After that, the reaction was carried out at 110°C for 6 hours. The final compound was dissolved in chloroform (Daejung chemicals & metals CO., LTD.), precipitated in cold ethyl ether (Daejung chemicals & metals CO., LTD.), filtered, and vacuum dried.

[0125]

[0126] Comparative Example 1: (4-arm 94% PCL - 0.6% PGMA)

[0127] Comparative Example 1 was polymerized with the composition shown in Table 2.

[0128]

[0129]

[0130]

[0131] Pentaerythritol (initiator, Sigma Aldrich) and hydroquinone (HQ, inhibitor, Sigma Aldrich) were placed in a three-necked flask, vacuum-dried for 10 minutes, and then purged with nitrogen at a rate of 50 cc / min. Purified epsilon-caprolactone (ε-CL, monomer, AVENTION) was additionally added and stirred at 110°C for 10 minutes. After adding glycidyl methacrylate (GMA, monomer, Sigma Aldrich) and stirring for 10 minutes, 1,5,7-Triazabicyclo(4.4.0)dec-5-ene (TBD, catalyst, TCI) dissolved in acetonitrile (ACN, Sigma Aldrich) was injected and reacted at 110°C for 6 hours. The final compound was dissolved in chloroform (Daejung chemicals & metals CO., LTD.), precipitated in ethyl ether (Daejung chemicals & metals CO., LTD.) at 4°C, filtered, and vacuum dried.

[0132]

[0133]

[0134] Comparative Example 2: Synthesis of 6arm 94%PCL-06%PGMA

[0135] Comparative Example 2 was polymerized with the composition shown in Table 3.

[0136]

[0137]

[0138]

[0139] Dipentaerythritol (initiator, Sigma Aldrich) and hydroquinone (HQ, inhibitor, Sigma Aldrich) were placed in a three-necked flask, vacuum-dried, and nitrogen purged at a rate of 50 cc / min. Purified epsilon-caprolactone (CL, monomer, AVENTION) was added and stirred at 110°C for 10 minutes. After that, glycidyl methacrylate (GMA, monomer, Sigma Aldrich) was added and stirred for 10 minutes, and then triazabicyclodecene (TBD, catalyst, TCI) dissolved in acetonitrile (ACN, Sigma Aldrich) was injected. After that, the reaction was carried out at 110°C for 6 hours. The final compound was dissolved in chloroform (Daejung chemicals & metals CO., LTD.), precipitated in cold ethyl ether (Daejung chemicals & metals CO., LTD.), filtered, and vacuum dried.

[0140]

[0141] Experimental Example 1: Compound Crosslinking

[0142]

[0143] 100 w / v% of the polymer synthesized in N-methyl-2-pyrrolidone (NMP, Sigma Aldrich) and 1 w / v% of Irgacure 2959 (photoinitiator, Sigma Aldrich) were dissolved. The dissolved polymer solution was applied to a certain mold and crosslinked using a UV lamp (300-400 nm / 200 s) to obtain a film-type sample.

[0144]

[0145] Experimental Example 2: Structural Analysis (1H-NMR)

[0146]

[0147] In structural analysis 1 Measurements were made using H-NMR (AVANCE III Bruker Biospin, USA). For sample preparation, the manufactured example polymer was dissolved in deuterium-substituted chloroform (chloroform-D, Sigma Aldrich) at a concentration of 10 mg / ml.

[0148] As a result of confirming the molecular structure and the ratio of PCL and PGMA by NMR (Nuclear Magnetic Resonance), as shown in Fig. 2, in the case of PCL, peaks appeared at δ= 4.10 [m, -OCH2, (E)], 2.41 [m, -CH2, (A)], 1.74 [m, -CH2, (B and D)], 1.45 [m, -CH2, (C)], and in the case of PGMA, peaks appeared at δ= 6.13 [s, =CH2, (G2)], 5.58 [s, =CH2, (G1)], 1.97 [s, ​​-CH3, (F)], confirming that 8-arm PCL-PGMA was synthesized.

[0149]

[0150] In addition, the area values ​​of PCL and PGMA were substituted into equation (2) to confirm the ratio of PCL and PGMA.

[0151]

[0152] ----- Formula (2)

[0153]

[0154] Experimental Example 3: Molecular Weight Analysis (GPC)

[0155]

[0156] In order to confirm the molecular weight according to the ratio of PCL and PGMA before crosslinking, GPC (1260 Infinity Ⅱ) was used to measure. The sample was filtered with a syringe filter at a concentration of 5 mg / mL with the synthesized polymer and tetrahydrofuran (THF, JTBaker). THF was used as the eluent. The flow rate was 1 mL / min, and the column temperature was 40°C, and the measurement was performed according to the manufacturer's method. PS (polystyrene, Agilent) was used as the standard curve.

[0157] As a result of GPC analysis, as shown in Table 4, it was confirmed that there was no significant difference in molecular weight depending on the PCL ratio of Examples 1, 2, and 3, and it was also confirmed that there was no significant difference when compared with Comparative Examples 1 and 2.

[0158]

[0159]

[0160] * PDI: polydispersity index

[0161]

[0162] Experimental Example 4: Thermal Characterization (DSC)

[0163]

[0164] The thermal properties of the samples were investigated according to the ratio of PCL and PGMA before and after crosslinking. Thermal properties were analyzed using DSC (DSC214, NETZSCH). Measurement conditions were heating-cooling-heating mode, and measurements were made in the temperature range of -80℃ to 150℃, and the heating and cooling rates were set to 10℃ / min.

[0165]

[0166] The thermal properties before crosslinking are represented by the melting temperature in Fig. 3a and the crystallization temperature in Fig. 3b. The 8-arm PCL-PGMA polymer before crosslinking exhibits two melting temperature peaks, which is because PGMA is randomly positioned between PCL, hindering crystallinity.

[0167]

[0168] Meanwhile, as shown in Table 5, when comparing Examples 1, 2, and 3, the melting temperature (T m ) and crystallization temperature (T c ) and crystallinity were confirmed to increase.

[0169]

[0170]

[0171]

[0172] In addition, when comparing Examples 1 to 3, it can be confirmed that when the content of PGMA in the polymer increases, the melting temperature and crystallinity decrease. This is because PGMA is randomly located in PCL, reducing the crystallinity of PCL.

[0173] When Comparative Examples 1 and 2 and Example 2 were compared, it was confirmed that there was no significant difference in melting temperature and crystallinity when the same amount of PGMA was included.

[0174]

[0175] The thermal properties after crosslinking are represented by the melting temperature in Fig. 4a and the crystallization temperature in Fig. 4b. Comparing the melting temperatures before and after crosslinking, two peaks appear before crosslinking, but after crosslinking, a network is formed, resulting in a single peak. Furthermore, because crosslinking forms a network structure, crystallinity decreases, lowering the melting temperature.

[0176]

[0177] Meanwhile, as shown in Table 6, when comparing Examples 1, 2, and 3 similarly to before crosslinking, it was confirmed that as the PCL content increased, the melting temperature value, crystallization temperature, and crystallinity increased.

[0178]

[0179]

[0180]

[0181] In Example 1, when the temperature is increased, the crystallization temperature (T cc ) appears because as the PGMA content increases, the crystallinity decreases and crystals are not formed during cooling. When Comparative Examples 1 and 2 and Example 2 were compared, it was confirmed that there was no significant difference in melting temperature and crystallinity when the same content of PGMA was included, as in Fig. 3.

[0182]

[0183] Experimental Example 5: Mechanical Characterization (UTM)

[0184]

[0185] 5-1. Tensile strength

[0186] To confirm the mechanical properties after crosslinking of comparative examples and examples, tensile strength was measured. Tensile strength was measured using UTM (34SC-1, INSTRON). Samples were UV crosslinked in the form of films and manufactured with the sizes of W 5 mm XL 5 mm XT 0.4 mm. The measurement conditions were room temperature, initial length 10 mm, and tensile speed 10 mm / min.

[0187]

[0188] In the case of Example 1, 8-arm 92%PCL-08%PGMA, the PGMA content was high, so it was over-cured during crosslinking and could not be measured. When Comparative Examples 1 and 2 were compared with Example 2, the tensile strain (ε) value did not differ significantly, but in Example 2, Young's modulus (E) increased by about 44% and about 20%, and the tensile stress (σ) increased by about 72% and about 54%, respectively, compared to Comparative Examples 1 and 2 (Table 7). This is expected to be the result of an increase in the number of arms, which increases the number of crosslinking points and strengthens the chain entanglement. In addition, the tensile strength increases as the PCL ratio increases, because Example 3 has higher crystallinity than Example 2.

[0189]

[0190]

[0191]

[0192] 5-2. Compressive strength

[0193]

[0194] To confirm the mechanical properties after crosslinking of comparative examples and examples, compressive strength was measured. Tensile strength was measured using UTM (34SC-1, INSTRON). Samples were UV crosslinked and manufactured into sizes of W 10 mm XL 10 mm XT 2.5 mm. Measurement conditions were compression at a speed of 1 mm / min at room temperature.

[0195] In the case of Example 1, 8-arm 92%PCL-08%PGMA, the content of PGMA was high, so it was over-cured during crosslinking and could not be measured. When the Example was compared with Comparative Examples 1 and 2, it was confirmed that the compressive Young's modulus increased as the number of arms structurally increased, and when Examples 2 and 3 were compared, it was confirmed that the compressive Young's modulus relatively decreased as the PCL content increased. (Table 8). This is believed to be because as the number of arms increases, the crosslinking points increase and the chain entanglement becomes stronger, thereby increasing the strength.

[0196]

[0197]

[0198]

[0199] Experimental Example 6: Analysis of Shape Memory Characteristics

[0200]

[0201] The shape memory properties of Example 2 were confirmed after cross-linking. To deform the chains by inducing movement, Example 2 was stretched or folded at 55°C and then fixed at 0°C. Afterwards, heat of 43°C, close to the melting temperature, was applied to confirm whether it returned to its original shape.

[0202] As a result, as shown in Fig. 6, it was confirmed that the polymer according to the present invention has shape memory properties.

[0203]

[0204] Experimental Example 7: Analysis of a Coronary Artery Bypass Graft Device Using Computer Modeling

[0205]

[0206] Computer modeling was performed to determine the hemodynamic effects of a model of a vascular graft scaffold for coronary artery bypass grafting. The modeling analyzed blood flow changes with and without the device, with and without the device, with different device shapes and lengths, and with different anastomotic angles.

[0207] ANSYS Fluent 20.0 software was used for the simulation, which enables blood flow simulation through the finite volume method (FVM), which discretizes the continuous physical space through a grid to convert the Navier-Stokes Partial Differential Equation (Navier-Stokes PDE), the governing equation of the flow, into the Finite Differential Equation (FDE), an algebraic equation.

[0208] The K-ωSST turbulence model was used as a turbulence model, and the Carreau-Yasuda model (Equation (3)) was used to apply the non-Newtonian model of blood.

[0209]

[0210] ----- Equation (3)

[0211]

[0212]

[0213]

[0214] The properties of arteries and veins were input by applying the Mooney-Rivlin 2 parameter model, assuming that they were hyperelastic materials (Equation (4)).

[0215]

[0216] ----- Formula (4)

[0217]

[0218]

[0219]

[0220] The analysis of the modeling set the wall shear stress (WSS), time average wall shear stress (TAWSS), and oscillatory shear index (OSI) as hemodynamic descriptors indicating the presence or absence of abnormal blood flow. The areas where WSS > 50 Pa, TAWSS < 1 Pa, and OSI > 0.1 were assumed to be areas where abnormal blood flow occurred and compared in each model. The hemodynamic descriptors used in the modeling are shown in Table 11.

[0221]

[0222]

[0223]

[0224] In the present invention, the vascular graft scaffold for coronary artery bypass grafting is manufactured in a structure that surrounds the vein portion to be grafted, and in the case of the strut spacing, which is the interval between each pattern, the spacing was narrowed to 1.8 mm in the third pattern after the anastomosis portion, and was arranged at an interval of 2.4 mm thereafter. In addition, a diffuser model was used that is designed so that the diameter of the blood vessel can gradually narrow from 6 mm to 3 mm as it enters the artery portion from the vein, and the length of the device was adjusted from 3 cm to 10 cm.

[0225] In coronary artery bypass grafting, arterial blood flows through the vein graft, and at this time, the arterial pressure causes the vein to expand. When the pulsatile environment according to the cardiac contraction and relaxation of the coronary artery was applied through modeling and then blood flow modeling was performed, the Low TAWSS area, maximum OSI, and maximum WSS values, which indicate abnormal blood flow, all improved, confirming that the rapid expansion of the vein is controlled when the coronary artery bypass grafting device is inserted (Fig. 8).

[0226]

[0227] The optimal shape and length of a vascular graft scaffold for coronary artery bypass grafting were identified through computer modeling. By applying a diffuser model with a gradually narrowing width from 6 mm to 3 mm, abnormal blood flow was dramatically reduced compared to a cylindrical model. Furthermore, when the device was manufactured to a length greater than 10 cm, the area with low shear stress was minimized (Figs. 9a-9e).

[0228] Subsequently, computer modeling was performed to determine the optimal anastomosis angle between the artery and vein. The maximum wall shear stress increased rapidly to 133.92 Pa at an angle of 60°, and there was no significant difference in the maximum shear stress below 30°. The oscillatory shear coefficient results showed the lowest values ​​at angles of 15° and 30°, but a tendency for the time-averaged shear stress to increase at an anastomosis angle of 15° was confirmed. Therefore, it was confirmed that a 30° anastomosis angle induces the best blood flow (Fig. 10).

[0229]

[0230] While specific aspects of the present invention have been described in detail above, it will be apparent to those skilled in the art that these specific descriptions merely represent preferred embodiments and are not intended to limit the scope of the present invention. Therefore, the substantial scope of the present invention is defined by the appended claims and their equivalents.

[0231]

[0232] National Research and Development Project that supported this invention

[0233] [Project ID] 1711138303

[0234] [Assignment Number] RS-2020-KD0000152

[0235] [Ministry Name] Multi-Ministry (Ministry of Science and ICT, Ministry of Trade, Industry and Energy, Ministry of Health and Welfare, Ministry of Food and Drug Safety)

[0236] [Name of Project Management (Specialist) Institution] (Foundation) Inter-Ministry Full-cycle Medical Device Research and Development Project Group

[0237] [Research Project Name] Inter-Ministry Full-cycle Medical Device Research and Development Project (R&D) (Ministry of Science and ICT, Ministry of Health and Welfare, Ministry of Trade, Industry and Energy)

[0238] [Research Project Title] Development of a Temperature-Sensitive Medical Device for Vascular Anastomosis Assistance to Improve the Success Rate of Surgical Transplantation

[0239] [Contribution rate] 1 / 1

[0240] [Name of the project performing organization] TMD Lab Co., Ltd.

[0241] Research Period: September 1, 2020 - December 31, 2023

Claims

1. A compound represented by the following chemical formula (1): Chemical formula (1) In the above chemical formula (1), x and y are integers from 1 to 20, independently of each other, m and n represent the mole % of repeating units, m+n is 100, and m is between 70 and 99.

2. In paragraph 1, The above compound is characterized by having shape memory properties through cross-linking.

3. In paragraph 1, The compound is characterized in that the average shape recovery ability is 90% or more at a temperature of 25 to 58°C after crosslinking.

4. A method for producing a compound of claim 1, comprising a step of reacting tripentaerythritol, a lactone monomer, and glycidyl methacrylate.

5. A manufacturing method, characterized in that in the fourth paragraph, the reaction is a ring-opening polymerization reaction.

6. In paragraph 4, the reaction is A manufacturing method characterized by reacting in the presence of a catalyst selected from the group consisting of 1,5,7-triazabicyclo(4.4.0)dec-5-ene, tin(II)(2-ethylhexanoate), trimethylopropane tris(3-mercaptopropionate), and zinc succinate.

7. A manufacturing method characterized in that the reaction is carried out at 80 to 160°C in the fourth paragraph.

8. A shape memory polymer cross-linked with the compound of paragraph 1.

9. A method for producing a shape memory polymer, further comprising a step of inducing a cross-linking reaction in the compound of claim 1 produced by the method of any one of claims 4 to 7.

10. In paragraph 9, A manufacturing method, characterized in that the above cross-linking reaction is a photocross-linking or thermal cross-linking reaction.

11. A medical material comprising a compound according to any one of claims 1 to 3.

12. In paragraph 11, The above medical material is a medical material characterized in that it is a support for a vascular graft or a ligator for a vascular graft.

13. In paragraph 12, A medical material characterized in that the support of the above vascular graft is a support of a vascular graft that is provided to surround and ligate the coronary vein during coronary artery bypass grafting.

14. In paragraph 13, A medical material characterized in that the support of the above vascular graft has a diameter that increases as it goes outward from the anastomosis site of the artery and vein.

15. In paragraph 14, A medical material characterized in that the support of the above vascular graft has an angle of 15° to 60° between the tangent lines of the anastomotic portion of the artery and vein.

16. An industrial material comprising a compound according to any one of paragraphs 1 to 3.

Citation Information

Patent Citations

  • Dendritic polymer with enhanced extension and interior functionality

    JP2013231034A

  • Artificial blood scaffold and the method for manufacturing the same

    KR1020150053528A

  • A Substrate for blood vessel anastomosis including shape memory polymers

    KR102355542B1

  • Method for intra prediction and apparatus thereof

    KR102442270B1

  • Shape memory polymers comprising 8-arm structure compound and use thereof

    KR102610524B1