Lithium battery
The lithium battery design with a 30 GPa modulus protective layer and nitrile-based additives addresses stability and conductivity issues, enhancing performance by improving initial capacity and lifespan through improved electrode stability and reduced internal resistance.
Patent Information
- Application Number
- PCT/KR2024/003734
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-01
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium batteries with protective films thicker than 10㎛ face reduced current density and stability issues due to challenges in forming a stable SEI during initial electrodeposition, particularly when using hybrid binders like polyimide and polyvinyl alcohol.
A lithium battery design incorporating a protective layer with a modulus of 30 GPa or more, featuring a nitrile-based additive in the electrolyte to enhance ionic conductivity and flame retardancy, and a hybrid binder for improved electrode stability and volume suppression.
The solution improves initial capacity, lifespan, and electrode stability while suppressing volume changes and internal resistance, leading to enhanced charge and discharge efficiency and lifespan characteristics.
Smart Images

Figure KR2024003734_03102024_PF_FP_ABST
Abstract
Description
lithium batteries
[0001] It relates to a lithium battery including an electrolyte and a protective layer containing an additive.
[0002] In a lithium battery employing a cathode containing lithium metal or a non-cathode containing no cathode active material, a protective film is applied to prevent dendrite formation and ensure uniform ion flux when dendrites are formed.
[0003] Protective films can be polymeric, inorganic, or organic / inorganic composite. Most protective films require a thickness of at least 10 μm to ensure sufficient ionic conductivity. However, thicker protective films lead to lower current densities in lithium batteries employing them.
[0004] To solve these problems, a hybrid binder of polyimide and polyvinyl alcohol was applied to the protective film, but it was not easy to form a stable SEI during the initial deposition.
[0005] Therefore, in a lithium battery employing a cathode including lithium metal or a cathode without a cathode active material, a protective film capable of suppressing volume change of the electrode and a binder forming the protective film are required, which provides high initial efficiency and life characteristics, and improved electrode stability.
[0006] One aspect is to provide a lithium battery having improved initial capacity, life characteristics and electrode stability, and including an electrolyte including a protective film capable of suppressing volume change of the electrode and an additive that improves ionic conductivity and flame retardancy.
[0007] According to one implementation example,
[0008] A cathode; an anode; and an electrolyte disposed between the cathode and the anode;
[0009] The above negative electrode includes a negative current collector, and a protective layer disposed between the negative current collector and the electrolyte,
[0010] The above electrolyte comprises a nitrile-based additive containing two or more nitrile groups,
[0011] A lithium battery is provided, wherein the modulus of the protective layer is 30 Gpa or more.
[0012] According to one aspect, the electrolyte may include a nitrile-based additive containing two or more nitrile groups, thereby improving ionic conductivity and flame retardancy. In addition, since a protective layer having a modulus of 30 GPa or more is disposed between the negative electrode current collector and the electrolyte, side reactions between the nitrile-based additive and the negative electrode current collector may be suppressed. Accordingly, decomposition of the nitrile-based additive occurring during the charge / discharge process of a lithium battery may be suppressed, and the internal resistance, charge / discharge efficiency, life characteristics, and electrode stability of a lithium battery including the electrolyte and the protective layer may be improved.
[0013] Additionally, the lithium battery can suppress volume change by including a protective layer having a modulus of 30 GPa or higher.
[0014] Figure 1 is a cross-sectional view of a lithium battery according to an exemplary embodiment.
[0015] Figure 2 is a cross-sectional view of a lithium battery according to another exemplary embodiment.
[0016] Figure 3 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0017] Figure 4 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0018] Figure 5 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0019] Hereinafter, a lithium battery comprising a protective layer and an electrolyte simultaneously according to exemplary embodiments is described in more detail.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present specification, including its definitions, shall prevail.
[0021] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein. The singular expression "singular" includes plural expression unless the context clearly indicates otherwise.
[0022] In this specification, the terms "include" or "have" are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials or combinations thereof.
[0023] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.
[0024] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one," "one or more," or "one or more" preceding elements herein may supplement the entire list of elements and do not mean that they supplement individual elements described above.
[0025] In order to clearly represent various layers and regions in the drawings, the thicknesses are enlarged or reduced. The same drawing reference numerals are used for similar parts throughout the specification. When a layer, film, region, plate, etc. is referred to as being "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. The terms first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only to distinguish one component from another.
[0026] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0027] In this disclosure, “alloy” means a mixture of two or more metals.
[0028] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0029] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0030] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.
[0031] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0032] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0033] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0034] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0035] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0036] As used herein, "cross-link" means a bond that connects one polymer chain to another polymer chain. As used herein, a cross-link is a covalent bond. As used herein, a "linker" or "cross-linker" means a functional group that connects one polymer chain to another polymer chain. As used herein, a "cross-linked polymer" means a polymer in which one polymer chain and another polymer chain are connected by one or more linkers. Furthermore, a cross-linked polymer is a product of a cross-linking reaction of one or more polymers.
[0037] As used herein, “fluorine-substituted” means that any hydrogen contained in the polymer is replaced with fluorine or an alkyl group having 1 to 5 carbon atoms substituted with fluorine.
[0038] [Lithium battery]
[0039] Fig. 1 is a cross-sectional view of a lithium battery according to an exemplary embodiment. Fig. 2 is a cross-sectional view of a lithium battery according to another exemplary embodiment.
[0040] Referring to FIGS. 1 and 2, a lithium battery (100) includes a negative electrode (110); a positive electrode (150); and an electrolyte (120) disposed between the negative electrode (110) and the positive electrode (150), wherein the negative electrode (110) includes a negative electrode current collector (112), and a protective layer (114) disposed between the negative electrode current collector (112) and the electrolyte (120), wherein the electrolyte (120) includes a nitrile-based additive containing two or more nitrile groups, and the modulus of the protective layer (114) is 30 Gpa or more. For example, when the electrolyte (120) includes a nitrile-based additive containing two or more nitrile groups, the ionic conductivity and flame retardancy of the electrolyte (120) can be improved. However, the nitrile-based additive may be decomposed through a side reaction with the negative electrode current collector (112) during the charge / discharge process of the lithium battery (100), but the lithium battery (100) can prevent the side reaction between the negative electrode current collector (112) and the nitrile-based additive by the protective layer (114) having a modulus of 30 GPa or more, which is disposed between the electrolyte (120) and the negative electrode current collector (112). Accordingly, the lithium battery including the electrolyte (120) and the protective layer (114) can have improved internal resistance, capacity, and lifespan characteristics.
[0041] In addition, the protective layer (114) has a modulus of 30 Gpa or more, so it can suppress volume changes in the lithium battery.
[0042] For example, the above modulus is an indentation modulus and can be measured using a microindenter (DUH-211, Shimadzu). For example, the above modulus can be calculated from the force applied to the tip from the protective film according to the distance the microindenter tip moves into the protective film.
[0043]
[0044] [Electrolyte (120)]
[0045] According to one embodiment, the electrolyte (120) may include a nitrile-based additive containing two or more nitrile groups. Since the electrolyte (120) includes the nitrile-based additive containing two or more nitrile groups, ionic conductivity and flame retardancy may be improved. Accordingly, a lithium battery (100) including the electrolyte (120) may have improved charge / discharge efficiency and lifespan characteristics.
[0046] According to one embodiment, the nitrile-based additive may be represented by the following chemical formula 1.
[0047] <Chemical Formula 1>
[0048]
[0049] In the above chemical formula 1, L1 is an alkylene group having 1 to 10 carbon atoms.
[0050] According to one embodiment, L1 in the above chemical formula 1 may be a methylene group, ethylene group, propylene group, or butylene group substituted or unsubstituted with an alkyl group having 1 to 5 carbon atoms. For example, L1 in the above chemical formula 1 may be an ethylene group.
[0051] According to one embodiment, the nitrile-based additive may include succinonitrile, acetonitrile, butyronitrile, and the like.
[0052] According to one embodiment, the content of the nitrile-based additive may be 0.1 to 5 wt% with respect to the total weight of the electrolyte (120).
[0053] The electrolyte (120) may be, for example, a liquid electrolyte or a gel electrolyte.
[0054] The electrolyte (120) is, for example, an organic electrolyte. The organic electrolyte is manufactured by dissolving a lithium salt in an organic solvent, for example.
[0055] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0056] According to one embodiment, the organic solvent in the electrolyte (120) may not include fluoroethylene carbonate (FEC).
[0057] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.
[0058] Gel electrolytes are, for example, gel polymer electrolytes. Gel polymer electrolytes are electrolytes that contain, for example, a liquid electrolyte and a polymer, or an organic solvent and a polymer having ion-conducting functional groups.
[0059] Among the gel electrolytes, the liquid electrolyte may be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid, and an organic solvent.
[0060] Among the gel electrolytes, the polymers include, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), Polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi) +) or a combination thereof, but is not limited thereto, and any polymer electrolyte used in the relevant technical field is possible.
[0061] Among the gel electrolytes, the organic solvent may be selected from organic solvents used in liquid electrolytes. The lithium salt may be any one that can be used as a lithium salt in the relevant technical field. The lithium salt may be, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.
[0062] Ionic liquids are salts that are liquid at room temperature or molten at room temperature and are composed only of ions and have a melting point below room temperature.
[0063] Among the gel electrolytes, the ionic liquid may include, for example, one or more cations selected from among a) ammonium-based, pyrrolidinium-based, pyridinium-based, pyrimidinium-based, imidazolium-based, piperidinium-based, pyrazolium-based, oxazolium-based, pyridazinium-based, phosphonium-based, sulfonium-based, triazolium-based, and mixtures thereof, and b) one or more anions selected from among BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, BF4-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-.
[0064] For example, a gel polymer electrolyte can be formed by impregnating a polymer with an electrolyte solution within a lithium battery. The gel electrolyte can further include inorganic particles.
[0065] According to one embodiment, the electrolyte (120) may further include a solid electrolyte.
[0066] The above solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.
[0067] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La yTiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.
[0068] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0혎<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n (0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0069] A polymer solid electrolyte is an electrolyte that includes, for example, a mixture of a lithium salt and a polymer, or a polymer having an ion-conducting functional group. A polymer solid electrolyte is, for example, a polymer electrolyte that does not include a liquid electrolyte. The polymer included in the polymer solid electrolyte may be selected from among the polymers used in gel electrolytes. The lithium salt may be selected from among the lithium salts used in gel electrolytes.
[0070]
[0071] [cathode]
[0072] Referring to FIG. 1, the negative electrode (110) may include a negative electrode current collector (112) and a protective layer (114) disposed between the negative electrode current collector (112) and the electrolyte (120). Referring to FIG. 2, the negative electrode (110) may further include a lithium metal layer (225) disposed between the negative electrode current collector (112) and the protective layer (120). For example, referring to FIG. 1, the lithium battery (100) may be a non-anode lithium metal battery. For example, referring to FIG. 2, the lithium battery (100) may be a lithium metal battery.
[0073]
[0074] [Cathode: Protective layer]
[0075] Referring to FIGS. 1 and 2, the negative electrode (110) includes a negative electrode current collector (112); and a protective layer (114) disposed between the negative electrode current collector (112) and the electrolyte (120). The modulus of the protective layer (114) may be 30 Gpa or more.
[0076] According to one embodiment, the modulus of the protective layer (114) may be 30 to 100 Gpa, 30 to 80 Gpa, 30 to 60 Gpa, 30 to 45 Gpa, 32 to 100 Gpa, 34 to 100 Gpa, or 34 to 45 Gpa. The modulus may be an indentation modulus.
[0077] According to one embodiment, the thickness of the protective layer (114) may be 2 μm or less. The thickness of the protective layer (114) may be, for example, 0.1 μm to 2 μm, 0.1 μm to 2 μm, 0.1 μm to 1.5 μm, 0.1 μm to 1.2 μm, 0.1 μm to 1.2 μm, or 0.2 to 1 μm. When the protective layer (114) has a thickness in this range, the decomposition of the electrolyte can be effectively suppressed and the imbalance of local current density can be effectively prevented, thereby effectively preventing the generation and / or growth of lithium dendrites. Accordingly, the life characteristics of a lithium battery including the protective layer (114) can be further improved. If the thickness of the protective layer (114) increases excessively, the energy density of the lithium metal battery may be reduced.
[0078] According to one embodiment, the recovery rate of the protective layer (114) may be 60% or more. For example, the recovery rate of the protective layer (114) may be 65% or more. For example, the recovery rate of the protective layer (114) may be 67% or more. For example, the recovery rate of the protective layer (114) may be 70% or more.
[0079] For example, the recovery rate may mean the ratio of the distance the tip moves back toward the surface of the protective layer (114) from the point at which the tip moves the maximum distance inside the protective layer (114) to the point at which the force applied to the tip becomes zero, relative to the maximum distance the tip moves inside the protective layer (114).
[0080] According to one implementation example, the hardness (indentation hardness) of the protective layer (114) is 1400 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (114) is 1500 N / mm 2 It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1550 N / mm 2It may be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1600 N / mm 2 It can be ideal. For example, the hardness (indentation hardness) of the protective layer (24) is 1500 N / mm 2 Up to 2000 N / mm 2 It can be. For example, the hardness (indentation hardness) of the protective layer (24) is 1550 N / mm 2 It could be strange.
[0081] According to one embodiment, the swelling ratio of the protective layer (114) may be less than 10%. For example, the swelling ratio of the protective layer (114) can be calculated by impregnating the protective layer (114) with an electrolyte for 24 hours and calculating the mass change rate before and after impregnation. After impregnation, the electrolyte on the surface is removed and the weight is measured within 5 minutes. For example, the swelling ratio (%) of the protective layer (114) can be calculated as a percentage of the value obtained by subtracting the mass before impregnation (g) from the mass after impregnation (g) and then dividing the result by the mass after impregnation (g).
[0082] According to one embodiment, the swelling ratio of the protective layer (114) may be less than 8%, less than 7%, less than 5%, less than 4%, or less than 3%.
[0083] According to one embodiment, the extension of the protective layer (114) may be 0.8 mm or less. For example, the extension of the protective layer (114) may be measured from the distance that the tip of the microindenter moves into the protective film until a certain force is applied to the tip. According to one embodiment, the extension of the protective layer (114) may be 0.5 mm or less or 0.4 mm or less.
[0084] According to one embodiment, the ionic conductivity of the protective layer (114) at room temperature (25°C) may be 0.1 mS / cm or more, and the ionic conductivity of the protective layer at high temperature (45°C) may be 0.2 mS / cm or more. For example, the ionic conductivity of the protective layer (114) at room temperature (25°C) may be 0.1 mS / cm to 1 mS / cm, 0.15 mS / cm to 1 mS / cm, or 0.2 mS / cm to 1 mS / cm. For example, the ionic conductivity of the protective layer (114) at high temperature (45°C) may be 0.2 mS / cm to 1.2 mS / cm, 0.22 mS / cm to 1.2 mS / cm, 0.24 mS / cm to 1.2 mS / cm, or 0.2 mS / cm to 1 mS / cm.
[0085] According to one embodiment, the protective layer (114) may include a polymer binder.
[0086] For example, the binder includes a third polymer which is a crosslinking reaction product of at least one first polymer selected from among polyamic acid and polyimide substituted with fluorine and a water-soluble second polymer having a second functional group, wherein the first polymer and the second polymer are crosslinked by forming an ester bond through a reaction between the first functional group and the second functional group. The third polymer is a crosslinked polymer of the first polymer and the second polymer. Since the binder includes the third binder which is a crosslinked polymer in which the first polymer containing fluorine and the second polymer are crosslinked by an ester bond, a lithium battery employing an anode having a protective film including the binder can simultaneously provide excellent anode stability derived from a polyimide containing fluorine, suppression of volume expansion of the anode, and improved initial charge / discharge efficiency and cycle life characteristics due to fluorine.
[0087] In the above binder, the first functional group and the second functional group included in the first polymer and the second polymer may be independently one or more selected from a carboxyl group, a hydroxyl group, an amide group, and an aldehyde group, but are not necessarily limited thereto, and any functional group that can react with the first functional group and the second functional group to form a cross-linking bond including an ester bond is possible. For example, the first functional group may be a carboxyl group (-COOH), and the second functional group may be a hydroxyl group (-OH). The carboxyl group and the hydroxyl group may react to form an ester cross-linking bond. In the first polymer, the first functional group may not be connected to a trivalent aromatic group included in polyamic acid and polyimide, but may be connected to a divalent aromatic group as a side chain.
[0088] The first polymer among the above binders may include an alkali metal. The alkali metal may be sodium, lithium, or the like. The first polymer may be substituted or doped with an alkali metal. For example, in polyamic acid, the hydrogen of a carboxyl group connected to a trivalent aromatic group included in the polyamic acid may be substituted with an alkali metal ion. For example, in polyimide, an alkali metal ion may be doped and coordinated to an amide group. The initial charge / discharge efficiency may be improved by the first polymer including an alkali metal in advance (pre-lithiation).
[0089] The content of the alkali metal included in the first polymer may be 0.2 to 1.0 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.2 to 0.8 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.3 to 0.7 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.4 to 0.6 in terms of an equivalent ratio to the carboxyl group or the amide group. For example, the content of the alkali metal included in the first polymer may be 0.45 to 0.55 in terms of an equivalent ratio to the carboxyl group or the amide group. In the above alkali metal content range, further improved binder properties may be provided.
[0090] If the lithium content of the polyamic acid, i.e., the degree of substitution of lithium ions, is lower than 0.2 in terms of the equivalent ratio to the carboxylic acid, the prelithiation rate is low, so the effect of suppressing irreversible occurrence in the first cycle is not significant. In addition, if the lithium content of the polyamic acid, i.e., the degree of substitution of lithium ions, is higher than 1.0 in terms of the equivalent ratio to the carboxylic acid, the imidization rate is significantly reduced, which may lower the life characteristics. The lithium content, i.e., the degree of substitution of lithium ions, in the above range can be obtained by adding the content of LiOH used to lithiate the polyamic acid in the range of 0.2 to 1.0 in terms of the equivalent ratio to the carboxylic acid of the polyamic acid.
[0091] For example, the polyimide may be represented by the following chemical formula 2 or chemical formula 3:
[0092] <Chemical Formula 2>
[0093]
[0094] <Chemical Formula 3>
[0095]
[0096] Among the above chemical formulas 2 and 3,
[0097] M is an alkali metal,
[0098] Ar1, Ar2, Ar4 and Ar5 are each independently a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O,
[0099] Ar3 and Ar6 are each independently a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; An aromatic ring group selected from among, wherein the aromatic ring group is one aromatic ring, a fused ring of two or more aromatic rings, or a ring of two or more aromatic rings connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-, X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 and Y2 are each independently an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction in a repeating unit, 0 <n<1, 0<m<1, n+m=1이다.
[0100] For example, the polyimide may be represented by the following chemical formula 4 or chemical formula 5:
[0101] <Chemical Formula 4>
[0102]
[0103] <Chemical Formula 5>
[0104]
[0105] Among the above chemical formulas 4 and 5,
[0106] M is lithium or sodium,
[0107] R1 to R 20are independently a halogen; -COOH; -OH; -CO-NH2; -COH; a C1 to C10 alkyl group substituted or unsubstituted with a halogen; a C6 to C20 aryl group substituted or unsubstituted with a halogen; or a C2 to C20 heteroaryl group substituted or unsubstituted with a halogen; wherein at least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, and R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.
[0108] For example, the polyamic acid may be represented by the following chemical formula 8 or chemical formula 9:
[0109] <Chemical Formula 8>
[0110]
[0111] <Chemical Formula 9>
[0112]
[0113] Among the above chemical formulas 8 and 9,
[0114] M is an alkali metal,
[0115] Ar1, Ar2, Ar4 and Ar5 are each independently a trivalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; or a trivalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with a halogen or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with a halogen; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-O,
[0116] Ar3 and Ar6 are each independently a divalent arylene group having 6 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; or a divalent heteroarylene group having 4 to 24 carbon atoms, substituted or unsubstituted with fluorine or an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine; An aromatic ring group selected from among, wherein the aromatic ring group is a ring in which one aromatic ring, two or more aromatic rings are fused, or two or more aromatic rings are connected by a single bond, -O-, -S-, -C(=O)-, -S(=O)2-, -Si(Ra)(Rb)- (Ra and Rb are each independently an alkyl group having 1 to 10 carbon atoms), an alkylene group having 1 to 10 carbon atoms substituted or unsubstituted with a halogen, or -C(=O)-NH-.
[0117] X1 is -COOH, -OH, -CO-NH2, or -COH, Y1 is an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.
[0118] For example, the polyamic acid may be represented by the following chemical formula 10 or chemical formula 11:
[0119] <Chemical Formula 10>
[0120]
[0121] <Chemical Formula 11>
[0122]
[0123] Among the above chemical formulas 10 and 11,
[0124] M is lithium or sodium,
[0125] R1 to R 20 are independently hydrogen; halogen; -COOH; -OH; -CO-NH2; -COH; a C1 to C10 alkyl group substituted or unsubstituted with a halogen; a C6 to C20 aryl group substituted or unsubstituted with a halogen; or a C2 to C20 heteroaryl group substituted or unsubstituted with a halogen; wherein at least one of R5 to R8 is -COOH, -OH, -CO-NH2, or -COH, and R 13 Inland R 20 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, Y1 to Y3 are each independently a single bond or an alkylene group having 1 to 10 carbon atoms substituted with fluorine; n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.
[0126] For example, in the binder, the polyimide may be represented by the following chemical formula 6 or chemical formula 7, and the polyamic acid may be represented by the following chemical formula 12 or chemical formula 13:
[0127] <Chemical Formula 6>
[0128]
[0129] <Chemical Formula 7>
[0130]
[0131] <Chemical Formula 12>
[0132]
[0133] <Chemical Formula 13>
[0134]
[0135] Among the above chemical formulas 6, 7, 12 and 13,
[0136] R 51 Inland R 58 are independently an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with fluorine (F), R 51 Inland R 58 At least one of which is an alkyl group having 1 to 10 carbon atoms substituted with fluorine, and n and m are each a mole fraction within the repeating unit, 0 <n<1, 0<m<1, n+m=1이다.
[0137] For example, in the first polymer represented by the above chemical formulas 2 to 13, the mole fractions of repeating units including a crosslinking group and repeating units not including a crosslinking group are each 0. <m<0.5, 0.5<n<1 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 2 내지 13으로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.1<m<0.4, 0.6<n<0.9 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 2 내지 13으로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.15<m<0.35, 0.65<n<0.85 및 m+n=1일 수 있다. 예를 들어, 상기 화학식 2 내지 13으로 표시되는 제1 고분자에서 가교기를 포함하는 반복단위와 가교기를 포함하지 않는 반복단위의 몰분율이 각각 0.2<m<0.3, 0.7<n<0.8 및 m+n=1일 수 있다. 상기 몰분율 범위에서 바인더가 더욱 향상된 물성을 제공할 수 있다.
[0138] For example, the first polymer represented by the chemical formulae 2 to 13 may be a random copolymer. For example, the first polymer represented by the chemical formulae 2 to 13 may be a block copolymer.
[0139] The weight average molecular weight of the first polymer may be 10,000 to 1,200,000 Daltons. For example, the weight average molecular weight of the first polymer in the binder may be 10,000 to 1,100,000 Daltons. For example, the weight average molecular weight of the first polymer in the binder may be 10,000 to 1,000,000 Daltons. For example, the weight average molecular weight of the first polymer may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 500,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 400,000 Daltons. For example, the weight average molecular weight of the first polymer may be 100,000 to 300,000 Dalton. The properties of the binder may be further improved within the weight average molecular weight range of the first polymer.
[0140] In the binder, the second polymer may be a polymerization reaction product of one or more monomers selected from a vinyl monomer, an acetate monomer, an alcohol monomer, an acrylic monomer, a methacrylic monomer, an acrylamide monomer, and a methacrylamide monomer, or a hydrolyzate thereof.
[0141] For example, the second polymer may be vinyl acetate, vinyl alcohol, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxyethylene glycol (meth)acrylate, 2-hydroxypropylene glycol (meth)acrylate, acrylic acid, methacrylic acid, 2-(meth)acryloyloxy acetic acid, 3-(meth)acryloyloxy propyl acid, 4-(meth)acryloyloxy butyric acid, itaconic acid, maleic acid, 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl It may be a polymerization reaction product of one or more monomers selected from (meth)acrylate, 4-isocyanatobutyl (meth)acrylate, (meth)acrylamide, ethylenedi(meth)acrylate, diethyleneglycol(meth)acrylate, triethyleneglycoldi(meth)acrylate, trimethylenepropanetri(meth)acrylate, trimethylenepropanetriacrylate, 1,3-butanediol(meth)acrylate, 1,6-hexanedioldi(meth)acrylate, allyl acrylate, and N-vinyl caprolactam, or a hydrolyzate thereof.
[0142] In particular, the second polymer may be polyvinyl alcohol (PVA). For example, polyvinyl alcohol may be a hydrolyzate obtained by hydrolyzing polyvinyl acetate with an alkali.
[0143] The degree of saponification of the polyvinyl alcohol may be 60 to 99%. For example, the degree of saponification of the polyvinyl alcohol may be 70 to 95%. For example, the degree of saponification of the polyvinyl alcohol may be 75 to 90%. For example, the degree of saponification of the polyvinyl alcohol may be 80 to 90%. For example, the degree of saponification of the polyvinyl alcohol may be 85 to 90%. In the above saponification range, the binder can provide further improved physical properties.
[0144] The weight average molecular weight of the polyvinyl alcohol may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 400,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 300,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 10,000 to 200,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 50,000 to 150,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 70,000 to 100,000 Daltons. For example, the weight average molecular weight of the polyvinyl alcohol may be 80,000 to 100,000 Daltons. The physical properties of the binder may be further improved within the weight average molecular weight range of the polyvinyl alcohol.
[0145] The weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 1:99 to 50:50. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 45:55. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 40:60. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 5:95 to 35:65. For example, the weight ratio of the first polymer to the second polymer included in the third polymer in the binder may be 10:90 to 30:70. The physical properties of the binder may be further improved within the above range of the weight ratio of the first polymer to the second polymer.
[0146] The crosslinking reaction in the binder may be performed at a temperature of 100°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 100°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 120°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 140°C or higher. For example, the crosslinking reaction may be performed by heat-treating a composition comprising the first polymer and the second polymer at a temperature of 160°C or higher. The crosslinking reaction may proceed within the above temperature range to produce a crosslinked polymer.
[0147] In addition, by performing the crosslinking reaction in the binder at a temperature of 100°C or higher, the polyamic acid can be cured into polyimide. For example, the imidization rate of the polyamic acid can be 60% or higher. For example, the imidization rate of the polyamic acid can be 70% or higher. For example, the imidization rate of the polyamic acid can be 80% or higher. For example, the imidization rate of the polyamic acid can be 90% or higher. The imidization rate of the polyamic acid 1 It can be obtained using H-NMR. The mechanical properties of the binder can be further improved by curing the polyamic acid in the binder into polyimide.
[0148] In one embodiment, the acid equivalent of the polyamic acid may be less than 300 g / eq. For example, the acid equivalent of the polyamic acid may be in the range of 50 g / eq to 250 g / eq. When the acid equivalent of the polyamic acid is lowered to less than 300 g / eq, the amount of carboxyl groups and / or carboxylates per unit mass may increase. When the amount of carboxyl groups and / or carboxylates per unit mass increases, for example, when a silicon-based negative electrode active material is used as the negative electrode material, the interaction between the negative electrode active material having a hydroxyl group on the surface and the binder may increase, thereby improving the bonding strength with the negative electrode active material. When the acid equivalent is 300 g / eq or more, the initial efficiency and life characteristics of the lithium battery may decrease.
[0149] The third polymer, which is a cross-linked polymer in the binder, may have a three-dimensional network structure in which a plurality of first polymer chains and a plurality of second polymer chains are cross-linked with each other by a linker or a cross-linker. Since the third polymer has a network structure, volume change during charge and discharge of an electrode including the binder can be suppressed.
[0150] The weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,500,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,200,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,100,000 Daltons. For example, the weight average molecular weight of the third polymer in the binder may be from 10,000 to 1,000,000 Daltons. For example, the weight average molecular weight of the third polymer may be from 10,000 to 500,000 Daltons. For example, the weight average molecular weight of the third polymer may be from 100,000 to 500,000 Daltons. For example, the weight average molecular weight of the third polymer may be 100,000 to 400,000 Daltons. For example, the weight average molecular weight of the third polymer may be 100,000 to 300,000 Daltons. The physical properties of the binder may be further improved within the weight average molecular weight range of the third polymer.
[0151] For example, the third polymer in the binder may be represented by one or more of the following chemical formulae 14 to 17:
[0152] <Chemical Formula 14>
[0153]
[0154] <Chemical Formula 15>
[0155]
[0156] <Chemical Formula 16>
[0157]
[0158] <Chemical Formula 17>
[0159]
[0160] In the above equations, n and m are the mole fractions within the repeating unit, respectively, and 0 <n<1, 0<m<1, n+m=1이며, p는 중합도로서 250 내지 12500다.
[0161] For example, the binder included in the protective layer (114) may additionally include a water-soluble fourth polymer selected from among cellulose hydroxyethyl ether, dextran, carboxymethylcellulose (CMC), alginate, cellulose nanofiber, xanthan gum, and guar gum. By additionally including the fourth polymer in the binder, the physical properties of the binder can be variously controlled.
[0162] The above binder can be used, for example, in an electrochemical cell. The above binder can be used, for example, in a protective film included in an electrochemical cell. The type of electrochemical cell is not particularly limited as long as it is a device that can store energy through an electrochemical reaction, and includes both primary and secondary batteries. The electrochemical cell can be, for example, an alkali metal battery such as a lithium battery or a sodium battery, an alkaline earth metal battery such as a magnesium battery, a metal-air battery, a supercapacitor, a fuel cell, etc.
[0163] According to one embodiment, the protective layer (114) can be manufactured by curing a composition for forming a protective film, which will be described later.
[0164] The composition for forming the protective film may include the first polymer described above and the second polymer described above. The protective layer (114) may be formed, for example, by applying the composition for forming the protective film on a negative electrode current collector (112) and then curing it at a temperature of 100°C or higher.
[0165] The protective layer (114) can be formed, for example, by applying the composition for forming a protective film on the negative electrode current collector (112) and then heat-treating at a temperature of 100° C. or higher for 1 to 10 hours. The protective layer (114) can be formed, for example, by applying the composition for forming a protective film on the negative electrode current collector (112) and then heat-treating at a temperature of 160° C. or higher for 1 to 10 hours.
[0166] According to one embodiment, the protective layer (114) may further include a conductive material.
[0167] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used.
[0168] According to one embodiment, the protective layer (114) may further include a lithium salt.
[0169] The above lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiTFSi, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof.
[0170]
[0171] [Cathode: Negative current collector]
[0172] For example, the material constituting the negative electrode current collector (112) can be any material that does not react with lithium, that is, any material that does not form an alloy or compound with lithium and has conductivity. The metal substrate is, for example, a metal or an alloy. The metal substrate can be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The electrode current collector (200) can have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field can be used.
[0173] For example, the negative electrode current collector (112) may have a reduced thickness compared to the negative electrode current collector included in a conventional negative electrode. Therefore, the negative electrode according to the present disclosure is distinguished from a conventional electrode including a thick film current collector, for example, by including a thin film current collector. Since the electrode according to one embodiment employs a thin film current collector having a reduced thickness, the thickness of the negative electrode active material layer in the negative electrode including the thin film current collector is relatively increased. As a result, the energy density of a lithium metal battery employing such an electrode is increased. The thickness of the negative electrode current collector (112) may be, for example, less than 15 μm, 14.5 μm or less, or 14 μm or less. The thickness of the negative electrode current collector (112) may be, for example, 0.1 μm to less than 15 μm, 1 μm to 14.5 μm, 2 μm to 14 μm, 3 μm to 14 μm, 5 μm to 14 μm, or 10 μm to 14 μm.
[0174] The material constituting the negative electrode current collector (112) may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The negative electrode current collector (112) is, for example, a metal or an alloy. The negative electrode current collector (112) may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0175] The negative electrode collector (112) may have a form selected from among, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field is possible.
[0176] The negative electrode current collector (112) may include, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. The negative electrode current collector (112) includes a substrate, and the substrate may have a structure including, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. An intermediate layer may additionally be disposed on the metal substrate layer.
[0177] For example, the base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can melt when a short circuit occurs, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal substrate layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal substrate layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by controlling the thickness of the metal substrate layer. The metal substrate layer may be plated or deposited on the base film. When the thickness of the metal substrate layer is reduced, the limit current and / or maximum current of the negative electrode current collector (110, 210) decreases, thereby improving the stability of the lithium metal battery in the event of a short circuit. A lead tab may be added on the metal substrate layer for connection to the outside. The lead tab may be welded to the metal substrate layer or the metal substrate layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal substrate layer may be melted, so that the metal substrate layer may be electrically connected to the lead tab. In order to make the welding of the metal substrate layer and the lead tab more solid, a metal chip may be added between the metal substrate layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal substrate layer. The metal chip may be, for example, a metal foil, a metal mesh, etc.The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After arranging the metal piece on the metal substrate layer, the lead tab may be welded to the metal piece / metal substrate layer laminate or the metal piece / metal substrate layer / base film laminate by welding the metal piece with the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal substrate layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the negative electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal substrate layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal substrate layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal substrate layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the negative electrode. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode collector (112) can reduce the weight of the electrode and consequently improve the energy density.
[0178] Referring to Fig. 1, the negative electrode current collector (112) may be free of a negative electrode active material layer before performing charge / discharge. For example, the negative electrode current collector (112) may be free of a lithium metal layer before performing charge / discharge. For example, in the case of a non-anode lithium metal battery in which the negative electrode active material layer or lithium metal layer is free on the negative electrode current collector (112) before performing charge / discharge, dendrite formation can be prevented, thereby further improving the life characteristics.
[0179] Referring to FIG. 2, a lithium metal layer (116) including a plate-shaped lithium metal thin film may be placed on the negative electrode current collector (112) before performing charge / discharge. For example, the lithium metal layer (116) may be placed between the negative electrode current collector (112) and the protective layer (114).
[0180] According to one embodiment, the negative electrode may further include an interlayer disposed between the negative electrode current collector (112) and the lithium metal layer (116).
[0181] According to one embodiment, the interlayer (not shown) may be directly disposed on, for example, one or both surfaces of the negative electrode collector (112). Accordingly, no other layer may be disposed between the negative electrode collector (112) and the interlayer (not shown). By directly disposing the interlayer on one or both surfaces of the negative electrode collector (112), the bonding force between the negative electrode collector (112) and the lithium metal layer (116) may be further enhanced.
[0182] The thickness of the intermediate layer (not shown) is, for example, 30% or less of the thickness of the negative electrode current collector (112). The thickness of the intermediate layer (not shown) is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the negative electrode current collector (112). The thickness of the intermediate layer (not shown) is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. By having the above intermediate layer (not shown) with a thickness in this range, the bonding force between the negative electrode current collector (112) and the metal layer (116) can be further improved, and an increase in interface resistance can be suppressed.
[0183] For example, the intermediate layer (not shown) may include a binder. By including the binder in the intermediate layer, the bonding strength between the negative electrode current collector (112) and the lithium metal layer (116) may be further enhanced. The binder included in the intermediate layer (not shown) may be, for example, a conductive binder or a non-conductive binder.
[0184] The conductive binder may be, for example, an ion-conducting binder and / or an electron-conducting binder. A binder having both ion-conducting and electron-conducting properties may be classified as either an ion-conducting binder or an electron-conducting binder.
[0185] The ion-conducting binder is, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, and polyacetylene. The ion-conducting binder may include a polar functional group. Examples of the ion-conducting binder including a polar functional group include Nafion, Aquibion, etc. (Aquivion), Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi+), etc.Electronically conductive binders include, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc. The intermediate layer may be a conductive layer comprising, for example, a conductive polymer.
[0186] The binder included in the intermediate layer may be, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer may be, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be disposed on the negative electrode current collector (210) in a dry or wet manner, for example. The intermediate layer may be, for example, a binding layer including a binder.
[0187] The intermediate layer may additionally include, for example, a carbon-based conductive material. By including the carbon-based conductive material, the intermediate layer may be, for example, a conductive layer. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.
[0188] The intermediate layer may be disposed on the negative electrode current collector (210) in a dry manner, for example, by deposition such as CVD or PVD. The intermediate layer may be disposed on the negative electrode current collector (210) in a wet manner, for example, by spin coating, dip coating, or the like. The intermediate layer may be disposed on the negative electrode current collector (210) by, for example, depositing a carbon-based conductive material on the negative electrode current collector (210) by deposition. The dry-coated intermediate layer may be made of a carbon-based conductive material and may not include a binder. Alternatively, the intermediate layer may be disposed on the negative electrode current collector by, for example, coating a composition including a carbon-based conductive material, a binder, and a solvent on the surface of the negative electrode current collector and drying it. The intermediate layer may have a single-layer structure or a multi-layer structure including a plurality of layers.
[0189]
[0190] [Cathode: Lithium metal layer]
[0191] Referring to FIG. 2, the lithium battery (100) may further include a lithium metal layer (116) disposed between the negative electrode current collector (112) and the electrolyte (120). For example, the lithium metal layer (116) may include lithium metal or a lithium alloy. For example, the lithium metal layer (116) may be a negative electrode active material layer. For example, the lithium metal layer (116) may be a lithium electrodeposition layer.
[0192] For example, the lithium metal layer (116) may be generated when lithium ions included in the electrolyte (120) are electrodeposited on the negative electrode current collector (112) as the lithium battery (100) is charged. For example, the lithium metal layer (116) may include a lithium alloy and a lithium metal. For example, the lithium alloy included in the lithium metal layer (116) may weaken the reactivity of the lithium metal, thereby effectively preventing a side reaction between the lithium metal layer (116) and the polymer electrolyte (120). In addition, the lithium metal layer (116) has excellent electrical conductivity, so that the internal resistance of the lithium battery (100) including the lithium metal layer (116) may be reduced. Accordingly, the lithium battery (100) including the lithium metal layer (116) may have improved lifespan characteristics as well as charge / discharge efficiency. According to one embodiment, the lithium metal layer (116) may include only the electrodeposited lithium metal or lithium alloy. In this case, the lithium metal layer (116) may be a lithium electrodeposition layer.
[0193] According to one embodiment, the lithium metal layer (116) may include, for example, lithium foil, lithium powder, plated lithium, a carbon-based material, or a combination thereof. For example, the lithium metal layer (116) may include lithium foil. In this case, the lithium metal layer (116) may be a negative electrode active material layer. For example, the lithium metal layer (116) may be introduced by coating a slurry including lithium powder and a binder, etc., onto the negative electrode current collector (112). For example, the binder may be a fluorine-based binder such as polyvinylidene fluoride (PVDF).
[0194] According to one embodiment, the lithium metal layer (116) may not include a carbon-based negative electrode active material. Accordingly, the lithium metal layer (116) may be formed of a metal-based negative electrode active material.
[0195] For example, the thickness of the lithium metal layer (116) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted according to the shape, capacity, etc. of the required lithium battery. If the thickness of the lithium metal layer (116) increases excessively, the structural stability of the lithium battery may deteriorate and side reactions may increase. If the thickness of the lithium metal layer (116) is excessively small, the energy density of the lithium metal battery may decrease.
[0196] According to one embodiment, the thickness of the lithium foil included in the lithium metal layer (116) may be, for example, 1 μm to 50 μm, 1 μm to 30 μm, or 10 μm to 30 μm, or 10 μm to 80 μm. When the lithium foil has a thickness in this range, the life characteristics of the lithium battery can be further improved.
[0197] According to one embodiment, the particle size of the lithium powder included in the lithium metal layer (116) may be, for example, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.1 μm to 2 μm. When the lithium powder has a thickness within this range, the life characteristics of the lithium battery can be further improved.
[0198]
[0199] [Cathode: Electrodeposition induction layer]
[0200] The negative electrode (110) may include an electrodeposition inducing layer (not shown) disposed between the negative electrode current collector (112) and the protective layer (114). Since the negative electrode (110) includes the electrodeposition inducing layer, lithium metal can be uniformly deposited between the negative electrode current collector (112) and the protective layer (114), thereby more effectively suppressing the generation and / or growth of lithium dendrites.
[0201] The electrodeposition inducing layer (not shown) may include, for example, a lithium-compatible metal. The electrodeposition inducing layer (not shown) may include, for example, a lithium-compatible metal and a carbon material.
[0202] The lithium-compatible metal is a material that can be lithiated and delithiated. The electrodeposition-inducing layer (not shown) can be formed by introducing the lithium-compatible metal onto the negative electrode current collector (112) through nanoparticle casting. Thereafter, a protective layer (114) can be introduced onto the electrodeposition-inducing layer (not shown). For example, when the electrodeposition-inducing layer (not shown) is introduced between the negative electrode current collector (112) and the protective layer (114) through nanoparticle casting, lithium ions can penetrate the protective layer (114), and lithium metal can be formed between the protective layer (114) and the electrodeposition-inducing layer (not shown).
[0203] The lithium-affinity metal included in the electrodeposition-inducing layer (not shown) may be nanoparticles of the lithium-affinity metal. The average particle diameter of the lithium-affinity metal may be, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the lithium-affinity metal has an average particle diameter in this range, reversible plating and / or dissolution of lithium may be facilitated during charge and discharge. The average particle diameter of the lithium-affinity metal is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.
[0204] The lithium-affinity metal may include, for example, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The lithium-affinity metal may include, for example, silver (Ag).
[0205] The carbon material can uniformly coat the lithium-affinity metal on the negative electrode current collector (112). The carbon material can uniformly coat the lithium-affinity metal on the negative electrode current collector (112) by uniformly applying the lithium-affinity metal on the negative electrode current collector (112). The uniformly coated first particles can uniformly precipitate lithium metal between the negative electrode current collector (112) and the protective layer (114), thereby preventing the formation of lithium dendrites.
[0206] The carbon material may include, for example, amorphous carbon, crystalline carbon, or any combination thereof. The carbon material may include, for example, amorphous carbon.
[0207] The amorphous carbon may include, for example, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or any combination thereof. The amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphitic carbon.
[0208] The electrodeposition-inducing layer (not shown) may include, for example, a lithium-affinity metal and / or a carbon material, and uniformly apply the lithium-affinity metal onto the negative electrode current collector (112) through the carbon material, and the lithium-affinity metal may uniformly deposit lithium metal between the electrodeposition-inducing layer (not shown) and the protective layer (114). Accordingly, the formation of lithium dendrites may be suppressed, and the life characteristics of a lithium battery (110) including the negative electrode (110) may be improved.
[0209] The mixing ratio of the lithium-affinity metal and the carbon material included in the electrodeposition induction layer (not shown) may be, for example, 10:1 to 1:10, 10:1 to 1:1, 10:1 to 2:1, 5:1 to 1:1, or 5:1 to 2:1 in weight ratio.
[0210] The electrodeposition induction layer (not shown) may further include a binder. The binder included in the electrodeposition induction layer (not shown) may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the art may be used. The binder may be composed of a single binder or multiple different binders. When the electrodeposition induction layer (not shown) does not include a binder, the electrodeposition induction layer (not shown) can be easily separated from the protective layer (114) or the negative electrode current collector (112). The content of the binder included in the electrodeposition induction layer (not shown) may be, for example, 5 wt% or less, 0.1 to 5 wt%, 0.1 to 3 wt%, or 0.1 to 1 wt% based on the total weight of the electrodeposition induction layer.
[0211] The thickness of the electrodeposition induction layer (not shown) may be, for example, 0.1 μm to 5 μm, 0.1 μm to 3 μm, or 0.5 μm to 5 μm, 0.5 μm to 3 μm, or 0.5 μm to 2 μm.
[0212]
[0213] [anode]
[0214] Referring to FIGS. 1 and 2, a lithium battery (100) may include a positive electrode current collector (140) and a positive electrode active material layer (130) disposed on the positive electrode current collector (140). More specifically, the positive electrode active material layer 130) may be disposed between an electrolyte (1200) and the positive electrode current collector (140).
[0215]
[0216] [Anode: Anode current collector]
[0217] Referring to FIGS. 1 and 2, the positive electrode (150) includes a positive electrode current collector (140). For example, the positive electrode (150) can be prepared by forming the positive electrode active material layer (130) on the positive electrode current collector (140) to form a positive electrode (150, 250).
[0218] For example, the positive electrode current collector (140) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0219] According to one embodiment, the positive electrode collector (140) may include aluminum (Al).
[0220] For example, the positive electrode current collector (140) may include a base film and a metal substrate layer disposed on one or both sides of the base film, similar to the negative electrode current collector (110, 220) described above.
[0221]
[0222] [Anode: Anode active material layer]
[0223] The above positive electrode active material layer (130) may include a positive electrode active material, a conductive material, and a binder.
[0224] For example, the cathode active material may be at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Lia A 1-b B 1 b D 1 2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B 1 b O 2-c D 1 c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B 1 b O 4-c D 1 c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c D α(In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G bO4 (in the above formula, 0.90 a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:
[0225] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, Ga, Si, W, Mo, Cu, Zn, Ti, boron (B), rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, Cl, Br or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0226] For example, the positive electrode active material may include a lithium transition metal oxide containing nickel and another transition metal. In the lithium transition metal oxide containing nickel and another transition metal, the content of nickel may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, for example, 90 mol% or more, based on the total mole number of transition metals.
[0227] For example, the lithium transition metal oxide may be a compound represented by the following chemical formula 18:
[0228] <Chemical Formula 18>
[0229] Lia Ni x Co y M z O 2-b A b
[0230] In chemical formula 18, 1.0≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상이고,
[0231] A is F, S, Cl, Br or a combination thereof.
[0232] For example, in chemical formula 18, 0.7≤x<1, 0 <y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, 0<z≤0.15; 또는 0.85≤x<0.95, 0<y≤0.1, 0<z≤0.1일 수 있다.
[0233] For example, the lithium transition metal oxide may be at least one of the compounds represented by the following chemical formulae 18-1 and 18-2:
[0234] <Chemical Formula 18-1>
[0235] LiNi x Co y Mn z O2
[0236] In Chemical Formula 18-1, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이고,
[0237] <Chemical Formula 18-2>
[0238] LiNi x Co y Al z O2
[0239] In Chemical Formula 18-2, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.8≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.82≤x≤0.95, 0<y≤0.15, 0<z≤0.15이다. 예를 들어, 0.85≤x≤0.95, 0<y≤0.1, 0<z≤0.1이다.
[0240] For example, lithium transition metal oxide is LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.2 O2 or LiNi 0.88 Co 0.1 Al 0.02 It could be O2.
[0241] For example, the above-mentioned positive electrode active material may be used as one having a coating layer on the surface of the lithium transition metal oxide, or may be used by mixing the lithium transition metal oxide and a lithium transition metal oxide having a coating layer.
[0242] For example, the coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element.
[0243] For example, the compound forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the lithium transition metal oxide with the coating elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0244] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.
[0245] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.
[0246] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0247] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0248] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0249] (Separator)
[0250] Next, a separator to be inserted between the positive and negative electrodes is prepared.
[0251] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.
[0252] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.
[0253] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.
[0254] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0255]
[0256] (lithium battery)
[0257] Referring to FIG. 3, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0258] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0259] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.
[0260] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 3 to 5, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0261] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0262] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0263] Lithium batteries may be, but are not limited to, lithium primary batteries, lithium secondary batteries, lithium-sulfur batteries, lithium-air batteries, etc., and any lithium battery used in the relevant technical field may be used.
[0264] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0265]
[0266] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0267] (Manufacture of cross-linked polymers)
[0268] Manufacturing Example 1: PI-F
[0269] After filling a three-necked round-bottom flask with nitrogen, 9.9790 g (0.0498 mol) of 2,2'-Bis(trifluoromethyl)benzidine (TFMB) and 2.5275 g (0.0166 mol) of 1,3-diaminobenzoic acid (DABA) were added, and 153 g of N-methylpyrrolidone (NMP) was added and completely dissolved using a mechanical stirrer. Subsequently, 14.4935 g (0.0664 mol) of 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA) was added, and the mixture was stirred at room temperature for 24 hours to produce a fluorine-substituted polyamic acid represented by the following chemical formula 17 (6FDA / TFMB / DABA, acid equivalent 210 g / eq, weight average molecular weight Mw = approximately 1,000,000). The fluorine-substituted polyamic acid is a random copolymer. The molar ratio of 6FDA:TFMB:DABA was 4:3:1. In chemical formula 19, the molar ratio of m:n was 1:3.
[0270] <Chemical Formula 19>
[0271]
[0272] Comparative manufacturing example 1: PVA
[0273] The polyvinyl alcohol used in Example 1 was used as is.
[0274] Comparative manufacturing example 2: PVDF
[0275] Poly(vinylidene fluoride) was compared.
[0276] Comparative Manufacturing Example 3: SBR / CMC
[0277] A 1:1 weight ratio mixture of styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) was prepared.
[0278]
[0279] (Manufacturing of lithium batteries)
[0280] Example 1: Cu substrate / PI-F:PVA=20:80 protective layer (1 μm) / electrolyte excluding FEC including SN
[0281] (Cathode manufacturing)
[0282] The fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1 was added to N,N-dimethylacetamide (DMAc, 99%, Sigma-Aldrich) and stirred overnight at 60°C to prepare a first composition.
[0283] Polyvinyl alcohol (weight average molecular weight, Mw=78,000, degree of saponification 88%, Polysciences, 15132) was added to N,N-dimethylacetamide (DMAc, 99%, Sigma-Aldrich) and stirred overnight at 60°C to prepare a second composition.
[0284] The first composition and the second composition were mixed so that the fluorine-substituted polyamic acid and the polyvinyl alcohol had a weight ratio of 20:80 to prepare a third composition.
[0285] A crosslinked polymer was prepared by performing a crosslinking reaction through heat treatment at 180°C for 2 hours in a vacuum oven. A crosslinked polymer of fluorine-substituted polyimide and polyvinyl alcohol was prepared by reacting the carboxyl group of the fluorine-substituted polyamic acid with the hydroxyl group of polyvinyl alcohol to form an ester linker. The crosslinked polymer has a three-dimensional network structure in which the polyimide and polyvinyl alcohol are crosslinked at multiple points.
[0286] After coating the third composition on a copper (Cu) current collector having a thickness of 20 ㎛ using a doctor blade, a protective layer was introduced by removing the solvent at 140°C for 6 hours.
[0287] A negative electrode having a negative electrode collector / protective layer structure was manufactured. The thickness of the protective layer was 1 μm.
[0288] (Manufacturing of coin cells)
[0289] A coin cell was manufactured by using a lithium foil with a thickness of 20 μm as a counter electrode, placing a polypropylene separator (Celgard 3510) between the counter electrode and the cathode, and injecting an electrolyte.
[0290] An electrolyte containing 0.2 wt% of succinonitrile dissolved in a LiDFOB:LiBF40.6 / 0.6M in DMC / DEC (1 / 2 v / v) solution was used.
[0291]
[0292] Example 2: Cu substrate / PI-F:PVA=20:80+LiTFSi protective layer (1 μm) / electrolyte excluding FEC including SN
[0293]
[0294] A coin cell was manufactured in the same manner as in Example 1, except that 5 g of LiTFSi was additionally added to 10 g of the third composition to include LiTFSi (lithium bis(trifluoromethanesulfonyl)imide) as a lithium salt in the protective layer.
[0295]
[0296] Example 3: Cu substrate / PI-F:PVA=20:80 protective layer (1 μm) / electrolyte containing FEC including SN
[0297]
[0298] Coin cells were manufactured in the same manner as in Example 1, except that DMC in the electrolyte was replaced with FEC solvent.
[0299]
[0300] Example 4: Cu substrate / PI-F:PVA=20:80 protective layer (1.5 μm) / electrolyte excluding FEC including SN
[0301]
[0302] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 1.5 μm.
[0303]
[0304] Example 5: Cu substrate / PI-F:PVA=20:80 protective layer (2.1 μm) / electrolyte excluding FEC including SN
[0305]
[0306] Coin cells were manufactured in the same manner as in Example 1, except that the thickness of the protective layer was 2.1 μm.
[0307]
[0308] Comparative Example 1: Cu substrate / PVA protective layer (1 μm) / electrolyte excluding FEC including SN
[0309]
[0310] A coin cell was manufactured in the same manner as in Example 1, except that polyvinyl alcohol manufactured in Comparative Manufacturing Example 2 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.
[0311]
[0312] Comparative Example 2: Cu base / PVDF protective layer (1 μm) / electrolyte excluding FEC including SN
[0313]
[0314] A coin cell was manufactured in the same manner as Example 1, except that PVDF prepared in Comparative Manufacturing Example 2 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.
[0315] Comparative Example 3: Cu substrate / SBR-CMC protective layer (1 μm) / electrolyte excluding FEC including SN
[0316]
[0317] A coin cell was manufactured in the same manner as in Example 1, except that SBR-CMC manufactured in Comparative Manufacturing Example 3 was used instead of the fluorine-substituted polyamic acid represented by the chemical formula 17 manufactured in Manufacturing Example 1.
[0318]
[0319] Comparative Example 4: Cu substrate / without protective film / electrolyte excluding FEC with SN
[0320]
[0321] Coin cells were manufactured in the same manner as in Example 1, except that the cathode did not include a protective film.
[0322]
[0323] Evaluation Example 1: Evaluation of the physical properties of the protective film
[0324] Using the protective films manufactured in Examples 1 to 2, 4 to 5 and Comparative Examples 1 to 3, a 5×5 cm sized film was formed on a glass substrate. 2 After manufacturing a polymer film with a thickness of 50 ㎛, the mechanical properties of the polymer were evaluated as follows.
[0325] The extension, recovery, modulus, and hardness of the protective films manufactured in Examples 1 to 2, 4 to 5, and Comparative Examples 1 to 3 were measured using a microindenter (DUH-211, Shimadzu). The force applied to the polymer film samples was 10 mN.
[0326] The measurement results are shown in Table 1 below. Extension is the distance that the tip of the microindenter moves into the protective film until a certain force is applied to the tip, and recovery is the ratio of the distance that the tip moves back toward the surface of the protective film from the point where the tip moves the maximum into the protective film to the point where the force applied to the tip becomes zero, to the distance that the tip has moved into the protective film. Modulus is the indentation modulus, and hardness is the indentation hardness, and they are calculated from the force applied to the tip from the protective film according to the distance that the microindenter tip has moved.
[0327] Extension [mm] Recovery [%] Modulus [GPa] Hardness [N / mm 2 ]Example 10.3968.638.11578Example 20.3871.040.31771Example 40.3770.141.21784Example 50.3870.742.51806Comparative Example 10.3366.529.51695Comparative Example 20.8761.76.3336Comparative Example 31.2353.94.2169
[0328] As shown in Table 1 above, the protective films of Examples 1 to 2 and 4 to 5 had an increased modulus, i.e., elastic coefficient, compared to the protective films of Comparative Examples 1 to 3, thereby suppressing expansion of the negative electrode.
[0329]
[0330] Evaluation Example 2: Measurement of ionic conductivity of the protective film at room temperature (25°C) and high temperature (45°C).
[0331] A symmetry cell was prepared by placing an indium (In) electrode having a thickness of 50 μm on each side of the protective film manufactured in Examples 1 to 2, 4 to 5 and Comparative Examples 1 to 3. The preparation of the symmetry cell was carried out in a Glover box under an Ar atmosphere.
[0332] The impedance of the pellets was measured using a two-probe method using an impedance analyzer (Material Mates 7260 impedance analyzer) for specimens with indium electrodes placed on both sides. The frequency range was 0.1 Hz to 1 MHz, and the amplitude voltage was 10 mV. Measurements were performed at room temperature (25°C) and high temperature (45°C) in an Ar atmosphere. The resistance value was obtained from the arc of the Nyquist plot for the impedance measurement results, and the ionic conductivity was calculated by considering the area and thickness of the specimen.
[0333] The results of ionic conductivity measurements are shown in Table 2 below.
[0334]
[0335] Evaluation Example 3: Evaluation of the expansion rate of the protective film
[0336] The protective films manufactured in Examples 1 to 2, 4 to 5 and Comparative Examples 1 to 2 were impregnated in LE for 24 hours. The expansion ratio of the protective film was calculated according to the following equation.
[0337] Expansion ratio (%) = ((mass of protective film after impregnation) - (mass of protective film before impregnation))*100 / mass of protective film after impregnation
[0338] The measurement results are shown in Table 2 below.
[0339] Room temperature ionic conductivity (mS / cm)High temperature ionic conductivity (mS / cm)Expansion ratio (%)Example 10.180.250Example 20.760.92.2Example 40.750.832.3Example 50.780.871.9Comparative example 10.070.0819.4Comparative example 20.050.0511.8Comparative example 30.040.0452.6
[0340]
[0341] As shown in Table 2 above, the protective films of Examples 1 to 2 and 4 to 5 had superior ionic conductivity and reduced expansion ratio compared to the protective films of Comparative Examples 1 to 2.
[0342] Evaluation Example 4: Charge / Discharge Characteristics Evaluation
[0343] The lithium batteries (coin cells) manufactured in Examples 1 to 5 and Comparative Examples 1 to 4 were charged at a constant current rate of 0.1 C at 25°C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After charging, the lithium batteries were allowed to rest for 10 minutes, and then discharged at a constant current rate of 0.1 C until the voltage reached 1.5 V (vs. Li) (1 st cycle).
[0344] Then, the coin cell was charged at a constant current rate of 0.2C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After the coin cell was rested for 10 minutes after charging, it was discharged at a constant current rate of 0.2C until the voltage reached 1.5 V (vs. Li) (2 nd cycle)(1st-2nd cycle is the Mars phase).
[0345] The coin cell that had undergone the above-mentioned Mars step was charged at a constant current rate of 1.0 C at 25°C until the voltage reached 0.01 V (vs. Li), and then charged at a constant voltage rate until the current reached 0.01 C while maintaining 0.01 V. After the coin cell was rested for 10 minutes after completion of charging, the discharge cycle was repeated 50 times at a constant current rate of 1.0 C until the voltage reached 1.5 V (vs. Li). Some of the results of the charge-discharge experiment are shown in Table 3 below.
[0346] The capacity retention rate was calculated from the following mathematical equation 1. In the electrode thickness expansion rate, the electrode is the cathode.
[0347] <Mathematical Formula 1>
[0348] Capacity retention rate [%] = [53 rd Discharge capacity of cycle / 3 rd Discharge capacity of cycle] × 100
[0349] Protective film electrolyte capacity retention rate [%] Type Thickness (㎛) SNFEC Example 1 PI-F: PVA1 Included Not Included 89.1 Example 2 PI-F: PVA+LiTFSi0.5 Included Not Included 93.2 Example 3 PI-F: PVA1 Included Not Included 94.3 Example 4 PI-F: PVA1.5 Included Not Included 87.9 Example 5 PI-F: PVA2.1 Included Not Included 86.7 Comparative Example 1 PVA1 Included Not Included 71.3 Comparative Example 2 PVDF1 Included Not Included 55.5 Comparative Example 3 SBR / CMC1 Included Not Included 37.1 Comparative Example 4 Protective film Not Included - Included Not Included 83.5
[0350]
[0351] As shown in Table 3, the lithium batteries of Examples 1 to 5 showed improved battery efficiency and capacity retention even after several charge / discharge cycles, as compared to the lithium batteries of Comparative Examples 1 to 4, in which succinonitrile remained in the electrolyte without being decomposed, thereby reducing the electrode thickness expansion rate.
Claims
1. A cathode; an anode; and an electrolyte disposed between the cathode and the anode; The above cathode is negative current collector, and A protective layer disposed between the negative electrode collector and the electrolyte, The above electrolyte comprises a nitrile-based additive containing two or more nitrile groups, A lithium battery having a modulus of the protective layer of 30 Gpa or more.
2. In paragraph 1, The above nitrile-based additive is represented by the following chemical formula 1, a lithium battery: <Chemical Formula 1> In the above chemical formula 1, L1 is an alkylene group having 1 to 10 carbon atoms.
3. In paragraph 1, A lithium battery, wherein the nitrile-based additive comprises succinonitrile, acetonitrile, and butyronitrile.
4. In paragraph 1, A lithium battery, wherein the content of the nitrile-based additive is 0.1 to 5 wt% based on the total weight of the electrolyte.
5. In paragraph 1, A lithium battery, wherein the electrolyte further comprises an organic solvent.
6. In paragraph 5, A lithium battery comprising the organic solvent selected from the group consisting of propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether or a mixture thereof.
7. In paragraph 6, The above organic solvent is a lithium battery free of fluoroethylene carbonate (FEC).
8. In paragraph 1, The above electrolyte further contains a lithium salt, The above lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 A lithium battery comprising SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof.
9. In paragraph 1, A lithium battery wherein the electrolyte is in a liquid or gel form.
10. In paragraph 1, A lithium battery, wherein the thickness of the protective layer is 2㎛ or less.
11. In paragraph 1, A lithium battery, wherein the swelling ratio of the protective layer is less than 10%.
12. In paragraph 1, The ionic conductivity of the above protective layer at room temperature (25℃) is 0.1 mS / cm or more, A lithium battery having a high temperature (45°C) ionic conductivity of the above protective layer of 0.2 mS / cm or more.
13. In paragraph 1, A lithium battery, wherein the protective layer comprises a polymer binder.
14. In paragraph 13, The polymer binder comprises a third polymer which is a crosslinking reaction product of at least one first polymer selected from among polyamic acid and polyimide substituted with a first functional group and a water-soluble second polymer having a second functional group, A lithium battery in which the first polymer and the second polymer are crosslinked by forming an ester bond through a reaction between the first functional group and the second functional group.
15. In paragraph 14, A lithium battery, wherein the first functional group and the second functional group are independently any one selected from the group consisting of a carboxyl group, an amide group, an aldehyde group, and a hydroxyl group.
16. In paragraph 14, A lithium battery, wherein the first polymer comprises an alkali metal.
17. In paragraph 14, A lithium battery, wherein the second polymer is polyvinyl alcohol.
18. In paragraph 14, A lithium battery, wherein the weight ratio of the first polymer and the second polymer is 1:99 to 50:
50.
19. In paragraph 1, A lithium battery, wherein the protective layer further comprises a lithium salt.
20. In paragraph 1, The above negative electrode collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
Citation Information
Patent Citations
Negative electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
KR1020100120238A
Negative electrode for lithium metal battery and lithium metal battery including the same
KR1020170001069A
Memory controller and operating method thereof
KR1020200114149A
Air compressor device
KR1020220158619A
KR20200016620A