Polymer electrolyte and lithium battery comprising same

The use of a crosslinked polymer electrolyte with specific repeating units in lithium batteries addresses the reactivity and dendrite issues, enhancing stability and capacity retention by improving ionic conductivity and reducing unreacted monomer content, leading to improved lithium battery performance.

WO2024205197A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD

Patent Information

Application Number
PCT/KR2024/003783
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-03
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal batteries with liquid electrolytes face issues of high reactivity and dendrite formation, leading to reduced lifespan and stability due to the high reactivity of lithium with the electrolyte and potential for dendrite growth on the negative electrode.

Method used

A polymer electrolyte with a crosslinked structure, incorporating a repeating unit derived from a crosslinkable monomer with multiple double bond functional groups and an ionic monomer with an ionic functional group, providing improved high-temperature stability and ionic conductivity, which reduces unreacted monomer content and prevents dendrite formation.

Benefits of technology

The polymer electrolyte enhances the capacity retention rate and lifespan characteristics of lithium batteries by improving ionic conductivity and stability, preventing side reactions and dendrite formation, thus improving both room temperature and high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003783_03102024_PF_FP_ABST
    Figure KR2024003783_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A polymer electrolyte comprising a cross-linked polymer containing: repeating unit (A) derived from a cross-linkable monomer containing two or more double bond functional groups including an ester bond; and repeating unit (B) derived from an ionic monomer containing one double bond functional group and an ionic functional group.
Need to check novelty before this filing date? Find Prior Art

Description

Polymer electrolyte and lithium battery containing the same

[0001] A polymer electrolyte, a method for manufacturing the same, and a lithium metal battery including the same are presented.

[0002] Lithium secondary batteries are high-performance secondary batteries with the highest energy density among the currently commercialized secondary batteries and can be used in various fields such as electric vehicles.

[0003] Lithium metal films are used as anodes in lithium metal batteries. When these films are used as anodes, the high reactivity of lithium leads to a high reactivity with the liquid electrolyte during charge and discharge. Furthermore, dendrites can form on the lithium anode film, reducing the lifespan and stability of lithium metal batteries employing the film. Therefore, improvements are needed.

[0004] One aspect is to provide an ion-conducting polymer electrolyte with improved high temperature stability.

[0005] Another aspect is to provide a lithium battery comprising the polymer electrolyte described above.

[0006] According to one aspect

[0007] A repeating unit (A) derived from a crosslinkable monomer containing two or more double bond functional groups including an ester bond; and

[0008] A polymer electrolyte is provided, comprising a crosslinked structure comprising a crosslinked polymer comprising repeating units (B) derived from an ionic monomer comprising an ionic functional group and one double bond functional group.

[0009] According to another aspect, a lithium battery is provided, which includes a positive electrode; a negative electrode; and the above-described polymer electrolyte interposed between the positive electrode and the negative electrode.

[0010] The polymer electrolyte according to one embodiment has a low content of unreacted monomers, resulting in excellent ionic conductivity and high-temperature stability. Using this polymer electrolyte, a lithium battery with improved capacity retention and capacity characteristics can be manufactured.

[0011] Figure 1 schematically illustrates the structure of a cross-linked polymer constituting a polymer electrolyte according to an embodiment.

[0012] Figure 2 shows a cross-sectional view of a lithium battery according to an embodiment.

[0013] Figure 3 shows a cross-sectional view of a lithium battery according to an embodiment.

[0014] Figure 4 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0015] Figure 5 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0016] Figure 6 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0017] Hereinafter, a polymer electrolyte and a lithium battery containing the polymer electrolyte according to an exemplary embodiment will be examined in more detail. These examples are provided solely as illustrative examples to more specifically illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present specification, including its definitions, shall prevail.

[0019] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein. The singular expression "singular" includes plural expression unless the context clearly indicates otherwise.

[0020] In this specification, the terms "include" or "have" are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials or combinations thereof.

[0021] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.

[0022] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one," "one or more," or "one or more" preceding elements herein may supplement the entire list of elements and do not mean that they supplement individual elements described above.

[0023] In order to clearly represent various layers and regions in the drawings, the thicknesses are enlarged or reduced. The same drawing reference numerals are used for similar parts throughout the specification. When a layer, film, region, plate, etc. is referred to as being "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. The terms first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only to distinguish one component from another.

[0024] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.

[0025] In this disclosure, “alloy” means a mixture of two or more metals.

[0026] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.

[0027] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.

[0028] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.

[0029] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.

[0030] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.

[0031] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.

[0032] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.

[0033] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during the discharge process.

[0034] With reference to the attached drawings, exemplary polymer electrolytes and lithium batteries including the same will be described in more detail below.

[0035]

[0036] [Polymer electrolyte]

[0037] The polymer electrolyte comprises a crosslinked polymer comprising repeating units (A) derived from a crosslinkable monomer comprising two or more double bond functional groups including an ester bond; and repeating units (B) derived from an ionic monomer comprising an ionic functional group and one double bond functional group.

[0038] For example, when the crosslinked polymer comprises repeating units (A) derived from a crosslinkable monomer containing two or more double bond functional groups including an ester bond; and repeating units (B) derived from an ionic monomer containing an ionic functional group and one double bond functional group, not only can ionic conductivity be improved by including the ionic monomer, but also stability at room temperature and high temperature can be improved. Accordingly, a lithium battery comprising the polymer electrolyte can have improved capacity characteristics and capacity retention characteristics.

[0039] For example, when the crosslinked polymer includes a repeating unit (A) derived from a crosslinkable monomer having two or more double bond functional groups including an ester bond, high temperature stability can be improved. For example, since the crosslinked polymer includes a double bond functional group including an ester bond rather than an ether bond, the reactivity of the crosslinkable monomer increases, so that the content of unreacted monomer remaining after the crosslinking reaction during the preparation of the crosslinked polymer can be reduced. Accordingly, side reactions due to unreacted monomers are prevented, so that the high temperature stability of the crosslinked polymer is further improved, and a lithium battery including the polymer electrolyte can have further improved high temperature capacity characteristics and high temperature life characteristics.

[0040] For example, when the crosslinked polymer includes a repeating unit (B) derived from an ionic monomer having an ionic functional group and one double bond functional group, the ionic conductivity of the polymer electrolyte is improved, and lithium ions are uniformly deposited on an anode to be described later, thereby effectively preventing the formation of lithium dendrite. For example, since the ionic monomer includes one double bond functional group, a crosslinking reaction between ionic monomers is prevented, and the ionic monomers can be dispersed and arranged at the terminals of the main chain and side chains of the crosslinked polymer in the form of end-capping during the crosslinking reaction. Accordingly, charge unevenness due to aggregation of ionic monomers is prevented, and the repeating unit (B) derived from a uniformly matched ionic monomer uniformly improves the ionic conductivity of the polymer electrolyte, so that lithium ions can be uniformly deposited on an anode to be described later. Accordingly, the capacity characteristics and life characteristics of a lithium battery including the polymer electrolyte can be further improved.

[0041] Figure 1 schematically illustrates the structure of a cross-linked polymer constituting a polymer electrolyte according to an embodiment.

[0042] Referring to Fig. 1, the crosslinked polymer (1) may include a main chain (M) and a plurality of side chains (S) extending from the main chain (M). For example, the plurality of side chains (S) may include a side chain (S1) extending from the main chain (M) and a side chain (S2) extending from the side chain (S1) extending from the main chain (M).

[0043] Referring to Fig. 1, the main chain (M) and the plurality of side chains (S) may include a terminal portion (E) at which a crosslinking reaction or polymerization reaction is completed. For example, a repeating unit (B) derived from an ionic monomer may be disposed at one or more terminal portions (E) among the terminal portions (E) included in the main chain (S) and the plurality of side chains (M). For example, the crosslinking reaction or polymerization reaction is performed at a double bond functional group, and since the ionic monomer includes one double bond functional group, when the ionic monomer is crosslinked or polymerized in the crosslinked polymer, it no longer includes a site at which a crosslinking reaction or polymerization reaction is performed, and therefore, the repeating unit (B) derived from the ionic monomer may be disposed at one or more terminal portions (E) among the terminal portions (E) included in the main chain (S) and the plurality of side chains (M). For example, when a repeating unit (B) derived from the ionic monomer is arranged at one or more terminal portions (E) among the terminal portions (E) included in the main chain (S) and the plurality of side chains (M), the ionic monomer is uniformly distributed throughout the crosslinked polymer (1) rather than being aggregated, thereby uniformly improving the ionic conductivity of the polymer electrolyte including the crosslinked polymer (1). Accordingly, the life characteristics and capacity characteristics of a lithium battery including the polymer electrolyte can be improved.

[0044] According to one embodiment, the double bond functional group among the crosslinking monomers may include an acrylate group.

[0045] According to one embodiment, the double bond functional group among the crosslinkable monomers may be represented by the following chemical formula 1.

[0046] <Chemical Formula 1>

[0047]

[0048] In chemical formula 1,

[0049] R1 is any one selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, and a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, and * is a bonding site with an adjacent atom.

[0050] According to one embodiment, R1 in the above chemical formula 1 may be hydrogen or an alkyl group having 1 to 20 carbon atoms.

[0051] According to one embodiment, R1 in the above chemical formula 1 may be hydrogen, a methyl group, an ethyl group, a propyl group, or a butyl group.

[0052] According to one embodiment, the crosslinking monomer may include three or more double bond functional groups including an ester bond. For example, when the crosslinking monomer includes three or more double bond functional groups including an ester bond, the reactivity of the crosslinking monomer is further enhanced, so that the content of unreacted monomer can be more easily reduced. Accordingly, when the crosslinking monomer includes three or more double bond functional groups including an ester bond, the high temperature stability of a polymer electrolyte including a crosslinked polymer including a repeating unit derived from the crosslinking monomer can be further improved. In addition, when the crosslinkable monomer includes three or more double bond functional groups including an ester bond, as the number of double bond functional groups including an ester bond increases, even if the proportion of repeating units (A) derived from the crosslinkable monomer in the crosslinked polymer decreases, the content of unreacted monomers can be reduced more easily, and as the proportion of repeating units (A) derived from the crosslinkable monomer decreases, the proportion of repeating units (B) derived from the ionic monomer can relatively increase. Accordingly, the ionic conductivity of the crosslinked polymer is further improved, and a lithium battery including a polymer electrolyte including a crosslinked polymer with improved ionic conductivity can have further improved capacity characteristics.

[0053] According to one embodiment, the double bond functional group in the crosslinking monomer may not include an ether group (-O-). For example, the double bond functional group in the crosslinking monomer may include an ester group (-C(=O)-O-) and may not include an ether group (-O-). For example, when the double bond functional group in the crosslinking monomer includes an ether group (-O-) instead of an ester group (-C(=O)-O-), the content of unreacted monomer in the crosslinking polymer may increase, resulting in a decrease in high-temperature stability.

[0054] According to one embodiment, the crosslinking monomer is trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate, ethoxylated glycerin triacrylate, glycerol propoxylate triacrylate, ethoxylated dipentaerythritol hexaacrylate, Or it may contain dipentaerythritol hexaacrylate.

[0055] According to one embodiment, the double bond functional group in the ionic monomer may include an allyl group, an acrylic group, a vinyl group, or any combination thereof. For example, the ionic monomer may include an acrylic group, a vinyl group, or any combination thereof.

[0056] According to one embodiment, the ionic functional group included in the ionic monomer may include a cationic functional group, an anionic functional group, or a combination thereof. For example, if the ionic monomer includes a cationic functional group, the ionic monomer may be a cationic monomer. For example, if the ionic monomer includes an anionic functional group, the ionic monomer may be an anionic monomer. For example, if the ionic monomer includes both a cationic functional group and an anionic functional group, the ionic monomer may be a zwitterionic monomer.

[0057] In one embodiment, the cationic functional group may include pyrrolidium, piperidinium, ammonium, imidazolium, phosphonium, or any combination thereof. For example, the cationic functional group may include pyrrolidium, piperidinium, ammonium, imidazolium, or any combination thereof.

[0058] According to one embodiment, the anionic functional group is trifluoromethanesulfonyl imide (TFSI), bis(fluorosulfonyl) imide (FSI), acetate, bromide (Br). - ), chloride (Cl - ), iodide (I - ), dicyanamide, hexafluorophosphate, tetrafluoroborate, hydrogen sulfate, or any combination thereof. For example, the anionic functional group may include trifluoromethanesulfonyl imide (TFSI), bis(fluorosulfonyl) imide (FSI), or a combination thereof.

[0059] According to one embodiment, the ionic monomer may include a cationic monomer or a zwitterionic monomer. For example, when the ionic monomer includes a cationic monomer, the cationic monomer may include a cationic functional group and a double bond functional group. For example, when the ionic monomer includes a zwitterionic monomer, the zwitterionic monomer may include an anionic functional group, a cationic functional group, and a double bond functional group.

[0060] In one embodiment, the ionic monomer may comprise a cationic monomer and an anion. In this case, the cationic monomer may comprise a cationic functional group and a double bond functional group. The anion may comprise the anionic functional group. For example, the anion may be the anionic functional group.

[0061] According to one embodiment, the ionic monomer may include a cationic monomer such as a pyrrolidium-allyl monomer, a pyrrolidium-acrylate monomer, an ammonium-aryl monomer, an ammonium-acrylate monomer, or any combination thereof. In this case, the ionic monomer may include an anionic monomer such as trifluoromethanesulfonyl imide (TFSI), bis(fluorosulfonyl) imide (FSI), acetate, or bromide (Br). - ), chloride (Cl - ), iodide (I - ), dicyanamide, hexafluorophosphate, tetrafluoroborate, hydrogen sulfate, or any combination thereof.

[0062] For example, a pyrrolidium-allyl monomer may contain allyl and pyrrolidium in one monomer. For example, a pyrrolidium-acrylate monomer may contain acrylate and pyrrolidium in one monomer. For example, an ammonium-allyl monomer may contain allyl and ammonium in one monomer. For example, an ammonium-acrylate monomer may contain acrylate and ammonium in one monomer.

[0063] According to one embodiment, the ionic monomer may include 1-allyl-1-methylpyrrolidium, dimethyl[2-(methacryloyloxy)ethyl]propylaminium, or a combination thereof as a cationic monomer. For example, the cationic monomer may be dimethyl[2-(methacryloyloxy)ethyl]propylaminium. In this case, the ionic monomer may include trifluoromethanesulfonyl imide (TFSI) or bis(fluorosulfonyl) imide (FSI) as an anion.

[0064] According to one embodiment, the molar ratio of the repeating unit (A) derived from the crosslinkable monomer contained in the crosslinked polymer to the repeating unit (B) derived from the ionic monomer may be 5:5 to 9:1. For example, the molar ratio of the repeating unit (A) derived from the crosslinkable monomer contained in the crosslinked polymer to the repeating unit (B) derived from the ionic monomer may be 5:5 to 8:2, 5:5 to 7:3, or more than 5:5 and less than or equal to 7:3. For example, when the molar ratio of the repeating unit (A) derived from the crosslinkable monomer contained in the crosslinked polymer to the repeating unit (B) derived from the ionic monomer is satisfied, the molar number of the repeating unit (A) derived from the crosslinkable monomer may be greater than or equal to the molar number of the repeating unit (B) derived from the ionic monomer. For example, when the molar number of repeating units (A) derived from a crosslinkable monomer is greater than or equal to the molar number of repeating units (B) derived from an ionic monomer, the content of unreacted monomer is reduced, so that the polymer electrolyte including the crosslinked polymer can have improved high-temperature stability. According to one embodiment, the molar number of repeating units (A) derived from a crosslinkable monomer can be greater than the molar number of repeating units (B) derived from an ionic monomer.

[0065] The polymer electrolyte may further include one or more selected from an organic solvent, an ionic liquid, a polymer ionic liquid, and an inorganic particle.

[0066] According to one embodiment, the polymer electrolyte further comprises a lithium salt. Here, the content of the lithium salt is 20 to 100 parts by weight based on 100 parts by weight of the copolymer. For example, when the polymer electrolyte comprises a lithium salt, the polymer electrolyte may be a polymer solid electrolyte comprising a lithium salt.

[0067] The polymer solid electrolyte may, for example, comprise a mixture of a lithium salt and the cross-linked polymer described above. The polymer solid electrolyte may, for example, be a polymer electrolyte that does not comprise a liquid electrolyte.

[0068] According to one embodiment, the polymer solid electrolyte may include a polymer in addition to the cross-linked polymer described above. For example, the polymers include polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA), poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, Polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi) +) or a combination thereof, but is not limited thereto, and any polymer electrolyte used in the relevant technical field is possible.

[0069] For example, the lithium salt can be any one that can be used as a lithium salt in the relevant technical field. The lithium salt can be, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.

[0070] According to one embodiment, the polymer electrolyte may further comprise a liquid electrolyte. For example, the polymer electrolyte may be a gel polymer electrolyte comprising the cross-linked polymer described above and a liquid electrolyte. For example, the liquid electrolyte may be disposed within a cross-linked network formed by the cross-linked polymer.

[0071] According to one embodiment, the liquid electrolyte may include an organic solvent or an ionic liquid. For example, the liquid electrolyte may further include a lithium salt. For example, the liquid electrolyte may be an ionic liquid, an organic solvent, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid, and an organic solvent.

[0072] According to one embodiment, the organic solvent may be any organic solvent used in the art. The organic solvent may include, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0073] For example, the ionic liquid refers to a salt or a molten salt in a liquid state at room temperature that has a melting point below room temperature and is composed only of ions. The ionic liquid may comprise at least one selected from compounds comprising, for example, a) at least one cation selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) at least one anion selected from BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, BF4-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-.

[0074] For example, the polymer solid electrolyte may be impregnated into an electrolyte solution within a lithium battery to form a gel polymer electrolyte. The gel polymer electrolyte may further include inorganic particles.

[0075] According to one embodiment, the polymer electrolyte may further include a solid electrolyte.

[0076] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.

[0077] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12(M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.

[0078] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5(An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n (0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.

[0079] According to one embodiment, the polymer electrolyte is useful as a polymer electrolyte of a lithium battery. For example, the lithium battery may be a lithium metal battery or a non-anode lithium metal battery.

[0080] For example, the lithium battery may include a lithium-air battery, a lithium-ion battery, a lithium polymer battery, a lithium sulfur battery, etc., all of which use lithium electrodes.

[0081] The polymer electrolyte according to one embodiment can be used as a protective film for a lithium electrode or as an electrolyte. The polymer electrolyte has excellent interfacial properties and a high lithium transfer constant, and thus can have excellent lithium ion transfer capability.

[0082]

[0083] [Method for producing polymer electrolyte]

[0084] A method for manufacturing a polymer electrolyte according to an embodiment of the present invention will be described.

[0085] A crosslinking monomer having two or more double bond functional groups including an ester bond and an ionic monomer having an ionic functional group and one double bond functional group are mixed, a polymerization initiator is added thereto to obtain a polymer electrolyte composition, and a polymerization reaction of the composition is performed. The mixing ratio of the crosslinking monomer having two or more double bond functional groups including an ester bond and the ionic monomer having an ionic functional group and one double bond functional group is controlled so as to correspond to the mixing ratio of the repeating unit (A) and the repeating unit (B) in the desired crosslinked polymer.

[0086] According to one embodiment, the molar ratio of the crosslinking monomer including two or more double bond functional groups including an ester bond included in the composition and the ionic functional group and one double bond functional group may be 5:5 to 9:1, 5:5 to 8:1, 5:5 to 7:3, or more than 5:5 and less than or equal to 7:3.

[0087] For a description of a crosslinking monomer comprising two or more double bond functional groups including an ester bond and an ionic monomer comprising an ionic functional group and one double bond functional group, refer to the above description.

[0088] The polymerization reaction can be carried out by applying heat or irradiating light, such as UV light. Here, heat or light can be applied within a range that does not negatively affect the lithium metal electrode. For example, the polymerization reaction can be carried out by applying heat.

[0089] The above polymerization reaction may be a copolymerization reaction, a crosslinking reaction or a grafting reaction.

[0090] When heat is applied or light such as UV is irradiated to carry out a polymerization reaction, the heat or light may be applied within a range that does not negatively affect the lithium metal electrode.

[0091] According to another embodiment, it is also possible to carry out a polymerization reaction of the polymers by irradiating light at room temperature (25°C). A photopolymerization initiator is used during the crosslinking reaction by irradiating light. The photopolymerization initiator may be any compound that can form radicals by light such as ultraviolet rays, without limitation on its composition. As the photopolymerization initiator, for example, one or more selected from the group consisting of 2-hydroxy2-methyl-1-phenyl-propan-1-one (HMPP), benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone may be used. The above acylphosphine may be, for example, 2,4,6-trimethyl-benzoyl-trimethyl phosphine oxide.

[0092] As the above thermal polymerization initiator, one or more selected from the group of initiators consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid can be used. Specifically, examples of persulfate-based initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8), and examples of azo-based initiators include 2, 2-azobis-(2-amidinopropane) dihydrochloride, 2, 2-azobis-(N, N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitril, 2, Examples include 2-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride and 4,4-azobis-(4-cyanovaleric acid).

[0093] A lithium salt is added to the above polymer electrolyte composition.

[0094] A liquid electrolyte is added to the above polymer electrolyte composition.

[0095] For a description of the above lithium salt and the above liquid electrolyte, refer to the above-described description.

[0096]

[0097] [Lithium battery]

[0098] A lithium battery according to one embodiment includes a positive electrode; a negative electrode; and the above-described solid electrolyte disposed between the positive electrode and the negative electrode. By including the above-described solid electrolyte, the lithium battery can simultaneously provide improved capacity and excellent room temperature and high temperature lifespan characteristics.

[0099] Lithium batteries may be, but are not limited to, lithium primary batteries, lithium secondary batteries, lithium-sulfur batteries, lithium-air batteries, etc., and any lithium battery used in the relevant technical field may be used.

[0100] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.

[0101] Referring to FIGS. 2 and 3, a lithium battery according to an embodiment will be described in detail.

[0102] For example, referring to FIG. 2, the lithium battery may be a non-anode lithium metal battery (100). For example, referring to FIG. 3, the lithium battery may be a lithium metal battery (200).

[0103] A lithium battery according to one embodiment may include a positive electrode; a negative electrode; and a polymer electrolyte disposed between the positive electrode and the negative electrode, and the polymer electrolyte described above.

[0104] According to one embodiment, the polymer electrolyte may have a solid, liquid or gel form.

[0105] A lithium battery (100) according to an embodiment may include, as shown in FIG. 2, a negative electrode current collector (110); a polymer electrolyte (120) disposed on the negative electrode current collector (110); and a positive electrode (150) disposed on the polymer electrolyte (120). In this case, the negative electrode may include a negative electrode current collector (110) free of a negative electrode active material layer, and the positive electrode (250) may include a positive electrode current collector (140) and a positive electrode active material layer (130) disposed on the positive electrode current collector (140).

[0106] According to one embodiment, a lithium battery (200) may further include a lithium metal layer (225) disposed between a negative electrode current collector (210) and an electrolyte (220), as shown in FIG. 3. In this case, the negative electrode may include a negative electrode current collector (210); and a lithium metal layer (225) disposed between the negative electrode current collector (210) and the electrolyte (220). For example, the lithium battery (200) may include a negative electrode current collector (110), a lithium metal layer (225) disposed on the negative electrode current collector (110), a polymer electrolyte (120) disposed on the lithium metal layer (225); and a positive electrode (150) disposed on the polymer electrolyte (120). For example, the lithium metal layer (225) may include lithium metal or a lithium alloy. For example, the metal layer (225) may be dissociated into lithium ions and metal cations during the discharge process, so that the thickness of the lithium metal layer (225) may decrease. Conversely, the lithium metal layer (225) may be electrodeposited with lithium ions during the charge process, so that the thickness of the lithium metal layer (225) may increase.

[0107] According to one embodiment, a lithium battery (100, 200) including the above-described polymer electrolyte may further include a protective layer (not shown) disposed between the negative electrode and the polymer electrolyte during a charge / discharge process.

[0108] Referring to FIG. 1, the protective layer (not shown) can be formed between the negative electrode collector (110) and the polymer electrolyte (120).

[0109] Referring to FIG. 2, the protective layer (not shown) may be formed between the negative electrode current collector (110) and the polymer electrolyte (120). For example, the protective layer (not shown) may be formed between the lithium metal layer (225) and the polymer electrolyte (120).

[0110]

[0111] [Cathode current collector (110, 210)]

[0112] For example, the material constituting the negative electrode current collector (110, 210) can be any material that does not react with lithium, that is, any material that does not form an alloy or compound with lithium and has conductivity. The metal substrate is, for example, a metal or an alloy. The metal substrate can be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The electrode current collector (200) can have a shape selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these shapes, and any shape used in the relevant technical field can be used.

[0113] For example, the negative electrode current collector (110, 210) may have a reduced thickness compared to the negative electrode current collector included in a conventional negative electrode. Therefore, the negative electrode according to the present disclosure is distinguished from the conventional electrode including a thick film current collector, for example, by including a thin film current collector. Since the electrode according to one embodiment employs a thin film current collector having a reduced thickness, the thickness of the negative electrode active material layer in the negative electrode including the thin film current collector is relatively increased. As a result, the energy density of a lithium metal battery employing such an electrode is increased. The thickness of the negative electrode current collector (110, 210) may be, for example, less than 15 um, 14.5 um or less, or 14 um or less. The thickness of the negative electrode current collector (110, 210) may be, for example, less than 0.1 um to 15 um, 1 um to 14.5 um, 2 um to 14 um, 3 um to 14 um, 5 um to 14 um, or 10 um to 14 um.

[0114] The material constituting the negative electrode collector (110, 210) may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The negative electrode collector (110, 210) is, for example, a metal or an alloy. The negative electrode collector (210) may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0115] The negative electrode current collector (110, 210) may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field is possible.

[0116] The negative electrode current collector (110, 210) may include, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. The negative electrode current collector (110, 210) includes a substrate, and the substrate may have a structure including, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. An intermediate layer may additionally be disposed on the metal substrate layer.

[0117] For example, the base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can melt when a short circuit occurs, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal substrate layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal substrate layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by controlling the thickness of the metal substrate layer. The metal substrate layer may be plated or deposited on the base film. When the thickness of the metal substrate layer is reduced, the limit current and / or maximum current of the negative electrode current collector (110, 210) decreases, thereby improving the stability of the lithium metal battery in the event of a short circuit. A lead tab may be added on the metal substrate layer for connection to the outside. The lead tab may be welded to the metal substrate layer or the metal substrate layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal substrate layer may be melted, so that the metal substrate layer may be electrically connected to the lead tab. In order to make the welding of the metal substrate layer and the lead tab more solid, a metal chip may be added between the metal substrate layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal substrate layer. The metal chip may be, for example, a metal foil, a metal mesh, etc.The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After arranging the metal piece on the metal substrate layer, the lead tab may be welded to the metal piece / metal substrate layer laminate or the metal piece / metal substrate layer / base film laminate by welding the metal piece with the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal substrate layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the negative electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal substrate layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal substrate layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal substrate layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the negative electrode. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode collector (110, 210) can reduce the weight of the electrode and consequently improve the energy density.

[0118] According to one embodiment, the negative electrode current collector (110, 220) may be free of a negative electrode active material layer before performing charge / discharge. For example, the negative electrode current collector (110, 220) may be free of a lithium metal layer (225) before performing charge / discharge. For example, in the case of a non-anode lithium metal battery in which the negative electrode active material layer or the lithium metal layer (225) is free on the negative electrode current collector (110, 220) before performing charge / discharge, dendrite formation can be prevented, thereby further improving the life characteristics.

[0119] According to another embodiment, a lithium metal layer (225) including a plate-shaped lithium metal thin film may be disposed on the negative electrode current collector (210) before performing charge and discharge. For example, in the process of disposing a polymer electrolyte on the lithium metal layer (225) disposed on the negative electrode current collector (210), the metal cations included in the polymer electrolyte may react with the lithium metal layer (225), so that the metal cations may be precipitated as metal. The precipitated metal cations may be dissociated into metal cations during discharge.

[0120] According to one embodiment, the negative electrode may further include an interlayer disposed between the negative electrode current collector (210) and the lithium metal layer (225).

[0121] According to one embodiment, the interlayer may be directly disposed on, for example, one or both surfaces of the negative electrode collector (210). Accordingly, no other layer may be disposed between the negative electrode collector (210) and the interlayer. By directly disposing the interlayer on one or both surfaces of the negative electrode collector (210), the bonding force between the negative electrode collector (210) and the lithium metal layer (225) may be further enhanced.

[0122] The thickness of the intermediate layer (not shown) is, for example, 30% or less of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. By having the above intermediate layer (not shown) with a thickness in this range, the bonding force between the negative electrode current collector (210) and the metal layer (225) can be further improved, and an increase in interface resistance can be suppressed.

[0123] For example, the intermediate layer may include a binder. By including the binder in the intermediate layer, the bonding strength between the negative electrode current collector (210) and the lithium metal layer (225) may be further enhanced. The binder included in the intermediate layer (not shown) may be, for example, a conductive binder or a non-conductive binder.

[0124] The conductive binder may be, for example, an ion-conducting binder and / or an electron-conducting binder. A binder having both ion-conducting and electron-conducting properties may be classified as either an ion-conducting binder or an electron-conducting binder.

[0125] The ion-conducting binder is, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, and polyacetylene. The ion-conducting binder may include a polar functional group. Examples of the ion-conducting binder including a polar functional group include Nafion, Aquibion, etc. (Aquivion), Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi+), etc.Electronically conductive binders include, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc. The intermediate layer may be a conductive layer comprising, for example, a conductive polymer.

[0126] The binder included in the intermediate layer may be, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer may be, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be disposed on the negative electrode current collector (210) in a dry or wet manner, for example. The intermediate layer may be, for example, a binding layer including a binder.

[0127] The intermediate layer may additionally include, for example, a carbon-based conductive material. By including the carbon-based conductive material, the intermediate layer may be, for example, a conductive layer. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.

[0128] The intermediate layer may be disposed on the negative electrode current collector (210) in a dry manner, for example, by deposition such as CVD or PVD. The intermediate layer may be disposed on the negative electrode current collector (210) in a wet manner, for example, by spin coating, dip coating, or the like. The intermediate layer may be disposed on the negative electrode current collector (210) by, for example, depositing a carbon-based conductive material on the negative electrode current collector (210) by deposition. The dry-coated intermediate layer may be made of a carbon-based conductive material and may not include a binder. Alternatively, the intermediate layer may be disposed on the negative electrode current collector by, for example, coating a composition including a carbon-based conductive material, a binder, and a solvent on the surface of the negative electrode current collector and drying it. The intermediate layer may have a single-layer structure or a multi-layer structure including a plurality of layers.

[0129] [Cathode: Lithium metal layer]

[0130] Referring to FIG. 2, the lithium battery (200) may further include a metal layer (225) disposed between the negative electrode current collector (210) and the electrolyte (220). For example, the lithium metal layer (225) may include lithium metal or a lithium alloy. For example, the lithium metal layer (225) may be a negative electrode active material layer. For example, the lithium metal layer (225) may be a lithium electrodeposition layer.

[0131] For example, the lithium metal layer (225) may be generated when lithium ions included in the polymer electrolyte (120) are deposited on the negative electrode current collector (110) as the lithium battery (200) is charged. For example, the lithium metal layer (225) may include a lithium alloy and a lithium metal. For example, the lithium alloy included in the lithium metal layer (225) may weaken the reactivity of the lithium metal, thereby effectively preventing a side reaction between the lithium metal layer (225) and the polymer electrolyte (120). In addition, the lithium metal layer (225) has excellent electrical conductivity, so that the internal resistance of the lithium battery (200) including the lithium metal layer (225) may be reduced. Accordingly, the lithium battery (200) including the lithium metal layer (225) may have improved not only life characteristics but also charge and discharge efficiency.

[0132] According to one embodiment, the lithium metal layer (225) may include, for example, lithium foil, lithium powder, plated lithium, a carbon-based material, or a combination thereof. For example, the lithium metal layer (225) may include lithium foil. In this case, the lithium metal layer (225) may be a negative electrode active material layer. For example, the lithium metal layer (225) may be introduced by coating a slurry including lithium powder and a binder, etc., onto the negative electrode current collector (210). For example, the binder may be a fluorine-based binder such as polyvinylidene fluoride (PVDF).

[0133] According to one embodiment, the lithium metal layer (225) may include only a deposited lithium metal or lithium alloy. In this case, the lithium metal layer (225) may be a lithium deposition layer.

[0134] According to one embodiment, the lithium metal layer (225) may not include a carbon-based negative electrode active material. Accordingly, the lithium metal layer (225) may be formed of a metal-based negative electrode active material.

[0135] For example, the thickness of the lithium metal layer (225) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted according to the shape, capacity, etc. of the required lithium battery. If the thickness of the lithium metal layer (225) increases excessively, the structural stability of the lithium battery may deteriorate and side reactions may increase. If the thickness of the lithium metal layer (225) is excessively small, the energy density of the lithium metal battery may decrease.

[0136] According to one embodiment, the thickness of the lithium foil included in the lithium metal layer (225) may be, for example, 1 μm to 50 μm, 1 μm to 30 μm, or 10 μm to 30 μm, or 10 μm to 80 μm. When the lithium foil has a thickness in this range, the life characteristics of the lithium battery can be further improved.

[0137] According to one embodiment, the particle size of the lithium powder included in the lithium metal layer (225) may be, for example, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.1 μm to 2 μm. When the lithium powder has a thickness within this range, the life characteristics of the lithium battery can be further improved.

[0138]

[0139] [Polymer electrolyte (120)]

[0140] For example, the polymer electrolyte (120) may include a crosslinked polymer as described above. The polymer electrolyte (120) may include a crosslinked network formed by the crosslinked polymer.

[0141] According to another embodiment, the polymer electrolyte (120) may further include a nonwoven fabric. The nonwoven fabric may serve to support at least one selected from lithium metal and lithium alloys precipitated during the charging process. For example, the nonwoven fabric may be omitted. For example, if the negative electrode current collector is of the mesh type, the nonwoven fabric may not be used.

[0142] The above nonwoven fabric may have a porosity of 10 to 90%, for example, 10 to 80%, for example, 10 to 50 vol%, for example, 25 to 50 vol%, and an average pore size of 0.1 to 10 µm, for example, 0.01 to 8 µm, for example, 0.1 to 1.0 µm. The average pore size represents the diameter when the pore shape is spherical, and represents the major axis length when the pore shape is non-spherical.

[0143] According to one embodiment, the nonwoven fabric may include one or more nonwoven fabrics selected from cellulose, polyester (e.g., polyethylene terephthalate (PET), polyetherimide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, nylon, and polyparaphenylenebenzobisoxazole.

[0144]

[0145] [anode]

[0146] As shown in FIGS. 2 and 3, a positive electrode active material layer (130, 230) is disposed on a positive electrode current collector (140, 240) to form a positive electrode (150, 250). More specifically, a positive electrode active material layer (130, 230) may be disposed on a polymer electrolyte (120, 220), and a positive electrode current collector (140, 240) may be disposed on the positive electrode active material layer (130, 230).

[0147]

[0148] [Anode: Anode current collector]

[0149] Referring to FIGS. 2 and 3, the positive electrode (150, 250) includes a positive electrode current collector (140, 240). For example, the positive electrode (150, 250) can be prepared by forming the positive electrode active material layer (130, 230) on the positive electrode current collector (140, 240).

[0150] For example, the positive electrode current collector (140, 240) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0151] According to one embodiment, the positive electrode collector (140, 240) may include aluminum (Al).

[0152] For example, the positive electrode current collector (140, 240) may include a base film and a metal substrate layer disposed on one or both sides of the base film, similar to the negative electrode current collector (110, 220) described above.

[0153]

[0154] [Anode: Anode active material layer]

[0155] The above positive electrode active material layer (130, 230) may include a positive electrode active material, a conductive material, and a binder.

[0156] For example, the cathode active material may be at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Li a A 1-b B 1 b D 1 2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B 1 b O 2-c D 1 c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B 1 b O 4-c D 1 c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Lia Ni 1-b-c Mn b B 1 c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG bO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:

[0157] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, Ga, Si, W, Mo, Cu, Zn, Ti, boron (B), rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, Cl, Br or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0158] For example, the positive electrode active material may include a lithium transition metal oxide containing nickel and another transition metal. In the lithium transition metal oxide containing nickel and another transition metal, the content of nickel may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, for example, 90 mol% or more, based on the total mole number of transition metals.

[0159] For example, the lithium transition metal oxide may be a compound represented by the following chemical formula 3:

[0160] <Chemical Formula 3>

[0161] Li a Ni x Co y M z O 2-b A b

[0162] In chemical formula 3, 1.0≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상이고,

[0163] A is F, S, Cl, Br or a combination thereof.

[0164] For example, in chemical formula 3, 0.7≤x<1, 0 <y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, 0<z≤0.15; 또는 0.85≤x<0.95, 0<y≤0.1, 0<z≤0.1일 수 있다.

[0165] For example, the lithium transition metal oxide may be at least one of the compounds represented by the following chemical formulae 3-1 and 3-2:

[0166] <Chemical Formula 3-1>

[0167] LiNi x Co y Mn z O2

[0168] In Chemical Formula 3-1, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이고,

[0169] <Chemical Formula 3-2>

[0170] LiNi x Co y Al z O2

[0171] In Chemical Formula 3-2, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.8≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.82≤x≤0.95, 0<y≤0.15, 0<z≤0.15이다. 예를 들어, 0.85≤x≤0.95, 0<y≤0.1, 0<z≤0.1이다.

[0172] For example, lithium transition metal oxide is LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.2 O2 or LiNi 0.88 Co 0.1 Al 0.02 It could be O2.

[0173] For example, the above-mentioned positive electrode active material may be used as one having a coating layer on the surface of the lithium transition metal oxide, or may be used by mixing the lithium transition metal oxide and a lithium transition metal oxide having a coating layer.

[0174] For example, the coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element.

[0175] For example, the compound forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the lithium transition metal oxide with the coating elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0176] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.

[0177] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.

[0178]

[0179] [Separator]

[0180] A lithium battery according to an embodiment may further include a separator (not shown).

[0181] Specific examples of the above separator include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0182] According to one embodiment, the battery case including the lithium battery may be cylindrical, square, thin-film, etc. For example, the lithium battery may be a large-scale thin-film battery. The lithium battery may be a lithium ion battery.

[0183] According to an embodiment, the lithium battery (100, 200) may be, for example, a lithium-air battery, a lithium-sulfur battery, etc.

[0184] According to one embodiment, the lithium battery (100, 200) can be used in electric vehicles (EVs) due to its excellent lifespan and high-rate characteristics. For example, it can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring large amounts of power storage. For example, it can be used in electric bicycles, power tools, etc.

[0185] When stacking multiple lithium batteries (100, 200) according to an embodiment, a gel-type electrolyte may be placed between the positive electrode and the liquid-impermeable ion-conductive composite membrane. The gel-type electrolyte may include, for example, a VDF-HFP copolymer, a lithium salt, and a solvent.

[0186] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). A polymer electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0187] For example, a polymer electrolyte including a positive electrode (3), a negative electrode (2), and a separator (4) is wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). A liquid electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing a lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0188] Referring to FIG. 5, a lithium battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. The above-described polymer electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1).

[0189] For example, after a polymer electrolyte including a separator (4) is placed between a positive electrode (3) and a negative electrode (2), the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. A liquid electrolyte may be injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.

[0190] Referring to FIG. 6, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The above-described polymer electrolyte including the separator (4) is disposed between the positive electrode (3) and the negative electrode (2), thereby forming a battery structure. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) serving as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. A liquid electrolyte is injected into the battery case (5) and sealed, thereby completing the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin-film shape, etc.

[0191] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 4 to 6, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A polymer electrolyte is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with a liquid electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, a polymer electrolyte including the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, a liquid electrolyte is injected into the pouch and sealed to complete the lithium battery.

[0192] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0193] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0194]

[0195] Below, we will look at the definitions of substituents used in chemical formulas.

[0196] The term alkyl, as used in chemical formulas, refers to a fully saturated branched or unbranched (or straight-chain or linear) hydrocarbon.

[0197] Non-limiting examples of the above alkyl include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, n-pentyl, isopentyl, neopentyl, iso-amyl, n-hexyl, 3-methylhexyl, 2,2-dimethylpentyl, 2,3-dimethylpentyl, n-heptyl, and the like.

[0198] At least one hydrogen atom of the above alkyl is selected from the group consisting of a halogen atom, a C1-C20 alkyl group substituted with a halogen atom (e.g., CCF3, CHCF2, CH2F, CCl3, etc.), a C1-C20 alkoxy, a C2-C20 alkoxyalkyl, a hydroxy group, a nitro group, a cyano group, an amino group, an amidino group, a hydrazine, a hydrazone, a carboxyl group or a salt thereof, a sulfonyl group, a sulfamoyl group, a sulfonic acid group or a salt thereof, a phosphoric acid or a salt thereof, or a C1-C20 alkyl group, a C2-C20 alkenyl group, a C2-C20 alkynyl group, a C1-C20 heteroalkyl group, a C6-C20 aryl group, a C6-C20 arylalkyl group, a C6-C20 heteroaryl group, a C7-C20 heteroarylalkyl group, It may be substituted with a C6-C20 heteroaryloxy group, a C6-C20 heteroaryloxyalkyl group, or a C6-C20 heteroarylalkyl group.

[0199] The term halogen atoms includes fluorine, bromine, chlorine, iodine, etc.

[0200] The term C1-C20 alkyl group substituted with a halogen atom refers to a C1-C20 alkyl group substituted with one or more halo groups, including, but not limited to, polyhaloalkyl containing monohaloalkyl, dihaloalkyl or perhaloalkyl.

[0201] Monohaloalkyl refers to an alkyl group having one iodine, bromine, chlorine or fluorine, and dihaloalkyl and polyhaloalkyl refer to an alkyl group having two or more identical or different halo atoms.

[0202] The term aryl group used in chemical formulas, used alone or in combination, refers to an aromatic hydrocarbon containing one or more rings.

[0203] The term aryl also includes groups in which an aromatic ring is fused to one or more cycloalkyl rings.

[0204] Non-limiting examples of the above aryl include phenyl, naphthyl, tetrahydronaphthyl, etc.

[0205] Additionally, one or more hydrogen atoms in the above aryl group can be substituted with a substituent similar to that in the case of the above-described alkyl group.

[0206] One or more hydrogen atoms in the above carbon rings can be substituted with a substituent similar to that in the case of the alkyl group described above.

[0207]

[0208] The following examples and comparative examples are provided for further details. However, the examples are provided for illustrative purposes only and are not intended to be limiting.

[0209] Manufacturing Example 1: Manufacturing of polymer electrolyte

[0210] Trimethylolpropane trimethacrylate (TMPTMA), represented by compound 1-1 below, as a crosslinking monomer, and dimethyl[2-(methacryloyloxy)ethyl] propylaminium-bis(fluorosulfonyl) imide, represented by compound 2-1 below, as an ionic monomer, were mixed with a liquid electrolyte. The liquid electrolyte was prepared by dissolving 1.15 M LiPF6 in a mixed solution of EC / EMC / DEC (3:5:2). The weight ratio of the liquid electrolyte to the weight of trimethylolpropane trimethacrylate (TMPTMA) represented by Compound 1-1 below and dimethyl[2-(methacryloyloxy)ethyl] propylaminium-bis(fluorosulfonyl) imide represented by Compound 2-1 below was 95:5. In addition, the mixing ratio of trimethylolpropane trimethacrylate (TMPTMA) represented by Compound 1-1 below and dimethyl[2-(methacryloyloxy)ethyl] propylaminium-bis(fluorosulfonyl) imide represented by Compound 2-1 below was about 7:3 molar ratio.

[0211] A polymer electrolyte composition was obtained by adding tert-butyl peroxypivalate as a thermal polymerization initiator to the above mixture. The content of the thermal polymerization initiator was 5 parts by weight based on 100 parts by weight of the total weight of trimethylolpropane trimethacrylate (TMPTMA) represented by the following compound 1-1 and dimethyl[2-(methacryloyloxy)ethyl] propylaminium-bis(fluorosulfonyl) imide represented by the following compound 2-1.

[0212] The above polymer electrolyte composition was injected into a polyolefin separator having a thickness of 30 μm, and thermally polymerized at 70°C for 2 hours to produce a polymer electrolyte having a thickness of 30 μm.

[0213]

[0214] Manufacturing Examples 2 to 5 and Comparative Manufacturing Examples 1 to 3

[0215] A polymer electrolyte was prepared in the same manner as in Manufacturing Example 1, except that the types and molar ratios of crosslinking monomers and ionic monomers were changed as shown in Table 1 below.

[0216] Crosslinking monomerIonic monomerMixing molar ratioPreparation example 1 Compound 1-1 Compound 2-17:3Preparation example 2 Compound 1-1 Compound 2-27:3Preparation example 3 Compound 1-2 Compound 2-17:3Preparation example 4 Compound 1-3 Compound 2-17:3Preparation example 5 Compound 1-1 Compound 2-13:7Comparative Preparation example 1 Compound 1-1--Comparative Preparation example 2 Compound A Compound 2-17:3Comparative Preparation example 3 Compound 1-1 Compound B 7:3

[0217]

[0218]

[0219]

[0220]

[0221]

[0222] Evaluation Example 1: Ionic Conductivity

[0223] The ionic conductivity of the polymer electrolytes manufactured according to Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 3 was evaluated at 25°C and 45°C, respectively.

[0224] The ionic conductivity of the polymer electrolyte is measured using the AC impedance method. More specifically, the ionic conductivity is evaluated by applying a voltage bias of 10 mV to the polymer electrolyte in the frequency range of 0.1 Hz to 1 MHz, scanning the temperature, and measuring the resistance, and the results are shown in Table 2 below.

[0225] Classification Room temperature (25℃) ionic conductivity High temperature (45℃) ionic conductivity Manufacturing example 10.29 0.92 Manufacturing example 20.29 0.95 Manufacturing example 30.28 0.87 Manufacturing example 40.27 0.71 Manufacturing example 50.25 0.53 Comparative manufacturing example 10.25 0.53 Comparative manufacturing example 20.26 0.56 Comparative manufacturing example 30.23 0.55

[0226] Referring to this, the polymer electrolytes of Manufacturing Examples 1 to 5 exhibited improved room temperature and high temperature ionic conductivity compared to those of Comparative Manufacturing Examples 1 to 3.

[0227]

[0228] Example 1: Manufacturing of lithium battery (pouch cell)

[0229] LiNi 0.6 Co 0.2 Al 0.2 O2, a conductive agent (Super-P; Timcal Ltd.), a binder (PVdF; Solvay), and N-methylpyrrolidone were mixed to obtain a cathode composition. LiNi in the cathode composition 0.6 Co 0.2 Al 0.2 The mixing weight ratio of O2, the challenge agent, and the polymer electrolyte was 95:3:2.

[0230] The above positive electrode composition was coated on top of aluminum foil (thickness: about 10 μm), dried at 50°C, and the dried resultant was dried in a vacuum at about 120°C to manufacture a positive electrode.

[0231] A separator (PE; 20 ㎛) was placed between the positive electrode obtained through the above process and a copper (Cu) current collector with a thickness of 10 ㎛, an electrolyte was injected, and then thermally cured to manufacture a lithium metal battery (pouch cell).

[0232] Examples 2 to 5 and Comparative Examples 1 to 3: Manufacturing of lithium batteries (pouch cells)

[0233] A polymer electrolyte was prepared in the same manner as in Manufacturing Example 1, except that the type of polymer electrolyte used was changed as shown in Table 3 below.

[0234]

[0235] Evaluation Example 2: Charge / Discharge Characteristics

[0236] Lithium batteries (pouch cells) manufactured according to Examples 1 to 5 and Comparative Examples 1 to 3 were charged at a constant current of 0.1 C at 45°C until the voltage reached 4.30 V (vs. Li), and then cut-off was achieved at a current of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, discharge was performed at a constant current of 0.1 C until the voltage reached 3.6 V (vs. Li) (formation stage, 1st cycle). This charge-discharge process was repeated twice more to complete the formation process.

[0237] The lithium battery that had gone through the above-described Mars step was charged at a constant current of 0.2 C until the voltage reached 4.3 V (vs. Li), and then cut-off was achieved at a current rate of 0.05 C while maintaining 4.3 V in constant voltage mode. After charging, constant current discharge was performed at 0.5 C until the cut-off voltage of 3.6 V was reached. The above-described charge and discharge process was repeated a total of 200 times.

[0238] In all of the above charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Here, the capacity retention rate at the 200th cycle is defined by the following equation.

[0239] [ceremony]

[0240] Capacity retention rate (%) = [ x 100]

[0241] 200 for each of room temperature (25℃) and high temperature (45℃) th The capacity retention rate and discharge capacity during the cycle are shown in Table 3 below.

[0242] Classification Polymer electrolyte Room temperature (25℃) High temperature (45℃) Capacity (mAh) Capacity retention rate (%) Capacity (mAh) Capacity retention rate (%) Example 1 Manufacturing example 1 15.276 17.278 Example 2 Manufacturing example 2 13.970 15.571 Example 3 Manufacturing example 3 13.668 14.265 Example 4 Manufacturing example 4 14.372 15.672 Example 5 Manufacturing example 5 12.164 13.361 Comparative example 1 Comparative manufacturing example 112.06 113.261 Comparative example 2 Comparative manufacturing example 2 10.65 3 10.649 Comparative example 3 Comparative manufacturing example 3 10.95 7 12.759

[0243] Referring to Table 3, Examples 1 to 5, which each include a polymer electrolyte according to Manufacturing Examples 1 to 5, had superior room temperature and high temperature capacity characteristics and capacity retention characteristics compared to Comparative Examples 1 to 2, which each include a polymer electrolyte according to Comparative Manufacturing Examples 1 to 3.

[0244] While the above has been described with reference to drawings and examples, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent implementations are possible. Accordingly, the scope of protection of the present invention should be defined by the appended claims.

[0245] [Explanation of symbols]

[0246] 100, 200: Lithium battery

[0247] 110, 210: cathode assembly 120, 220: electrolyte

[0248] 130, 230: Cathode active material layer 140, 240: Cathode current collector

[0249] 150, 250: anode 225: metal layer

[0250] M: main chain S: side chain

[0251] E: distal end

Claims

1. A repeating unit (A) derived from a crosslinkable monomer containing two or more double bond functional groups including an ester bond; and A polymer electrolyte comprising a crosslinked polymer comprising a repeating unit (B) derived from an ionic monomer comprising an ionic functional group and one double bond functional group.

2. In paragraph 1, The above cross-linked polymer comprises a main chain and a plurality of side chains extending from the main chain, A polymer electrolyte in which a repeating unit (B) derived from an ionic monomer is arranged at one or more terminal portions among the terminal portions included in the main chain and the plurality of side chains.

3. In paragraph 1, A polymer electrolyte wherein the double bond functional group among the above crosslinking monomers includes an acrylate group.

4. In paragraph 1, Among the above crosslinking monomers, the double bond functional group is represented by the following chemical formula 1, a polymer electrolyte: <Chemical Formula 1> In chemical formula 1, R1 is any one selected from the group consisting of hydrogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, and a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, * is a bonding site with a neighboring atom.

5. In paragraph 1, A polymer electrolyte wherein the crosslinking monomer comprises three or more double bond functional groups including an ester bond.

6. In paragraph 1, A polymer electrolyte in which the double bond functional group among the above crosslinking monomers does not include an ether group (-O-).

7. In paragraph 1, A polymer electrolyte wherein the double bond functional group among the above ionic monomers comprises an allyl group, an acrylic group, a vinyl group, or any combination thereof.

8. In paragraph 1, A polymer electrolyte, wherein the ionic functional group contained in the above ionic monomer includes a cationic functional group, an anionic functional group, or a combination thereof.

9. In paragraph 8, A polymer electrolyte wherein the cationic functional group comprises pyrrolidium, piperidinium, ammonium, imidazolium, phosphonium or any combination thereof.

10. In paragraph 8, The above anionic functional groups include trifluoromethanesulfonyl imide (TFSI), bis(fluorosulfonyl) imide (FSI), acetate, and bromide (Br). - ), chloride (Cl-), iodide (I-), dicyanamide, hexafluorophosphate, tetrafluoroborate, hydrogen sulfate, or any combination thereof.

11. In paragraph 1, A polymer electrolyte wherein the ionic monomer comprises a cationic monomer or a zwitterionic monomer.

12. In paragraph 1, A polymer electrolyte in which the molar ratio of repeating units (A) derived from a crosslinkable monomer contained in the above crosslinked polymer to repeating units (B) derived from an ionic monomer is 5:5 to 9:

1.

13. In paragraph 1, The polymer electrolyte further comprises a lithium salt.

14. In paragraph 13, The above lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 A polymer electrolyte comprising SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.

15. In paragraph 1, The above polymer electrolyte further comprises a liquid electrolyte, The above liquid electrolyte is a polymer electrolyte containing an organic solvent or an ionic liquid.

16. In paragraph 15, The organic solvent comprises propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether or a mixture thereof. The above ionic liquid contains cations and anions, The above cation includes at least one selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof. A polymer electrolyte comprising at least one anion selected from among BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, BF4-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-.

17. Anode; cathode; and A lithium battery comprising a polymer electrolyte according to any one of claims 1 to 16 interposed between the positive electrode and the negative electrode.

18. In paragraph 17, The above negative electrode includes a negative electrode collector, The above negative electrode is a lithium battery in which a negative electrode active material layer is absent (free).

19. In paragraph 18, The above negative electrode collector comprises a base film and a metal substrate layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, An all-solid-state secondary battery, wherein the metal substrate layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

20. In paragraph 18, A lithium battery further comprising a lithium metal layer disposed between the negative electrode current collector and the polymer electrolyte.

Citation Information

Patent Citations

  • Polymer solid electrolyte

    JP2004281147A

  • Polymer solid electrolyte and lithium secondary battery comprising the same

    KR1020180116145A

  • Functional coffee mix composition for diet

    KR1020210115352A

Cited By

  • polymer composition for electrolyte and / or positive electrode of a rechargeable battery

    FR3174161A1

  • Polymer composition for electrolyte and / or positive electrode of a rechargeable battery

    WO2026215444A1