Electrolyte and lithium battery comprising same

The electrolyte, composed of lithium salts with varying dissociation degrees and a fluorine-containing solvent, addresses dendrite issues and internal resistance in lithium metal thin film batteries, enhancing their energy density and lifespan for improved performance in applications like electric vehicles.

WO2024205203A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003790
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-03
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal thin film batteries suffer from dendrite formation and limited energy density and lifespan due to high internal resistance, which hinders their performance in applications like electric vehicles.

Method used

An electrolyte comprising a first lithium salt with high dissociation and a second lithium salt with low dissociation, combined with a fluorine-containing linear ester solvent, reduces internal resistance and forms a protective layer preventing dendrite growth, thereby enhancing the lifespan and energy density of lithium batteries.

Benefits of technology

The proposed electrolyte solution significantly improves lithium battery lifespan and energy density by reducing internal resistance and preventing dendrite formation, making lithium metal thin film batteries more suitable for high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003790_03102024_PF_FP_ABST
    Figure KR2024003790_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an electrolyte and a lithium secondary battery comprising same, the electrolyte comprising: a first lithium salt including a lithium ion and a first negative ion; a second lithium salt including a lithium ion and a second negative ion; and a solvent including a fluorine-containing linear ester, wherein the degree of dissociation of the first lithium salt with respect to the fluorine-containing linear ester is greater than the degree of dissociation of the second lithium salt with respect to the fluorine-containing linear ester.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte and lithium battery containing the same

[0001] An electrolyte and a lithium battery containing the same are presented.

[0002] Lithium batteries are high-performance batteries with the highest energy density among currently commercialized batteries and can be used in various fields, such as electric vehicles.

[0003] Lithium metal thin films can be used as anodes in lithium batteries. These films are typically manufactured by rolling lithium into a plate shape. However, in lithium secondary batteries using these films as anodes, dendrites form and grow on the films, resulting in unsatisfactory energy density and long-life characteristics. This leaves significant room for improvement.

[0004] One aspect is to provide an electrolyte that reduces the internal resistance of lithium batteries and improves their life characteristics.

[0005] Another aspect is to provide a lithium battery comprising the electrolyte described above.

[0006] According to one aspect

[0007] A first lithium salt comprising a lithium ion and a first anion;

[0008] A second lithium salt comprising a lithium ion and a second anion; and

[0009] A solvent comprising a fluorine-containing linear ester;

[0010] An electrolyte is provided in which the degree of dissociation of the first lithium salt for the fluorine-containing linear ester is greater than the degree of dissociation of the second lithium salt for the fluorine-containing linear ester.

[0011] Depending on other aspects

[0012] positive electrode; negative electrode; and

[0013] It is placed between the positive electrode and the negative electrode,

[0014] A lithium battery including the above electrolyte is provided.

[0015] According to one embodiment, the electrolyte has excellent lithium ion conductivity by including a specific solvent, so that the internal resistance of a lithium battery including the electrolyte can be reduced.

[0016] In addition, the electrolyte simultaneously includes a first lithium salt and a second lithium salt, thereby forming a protective layer that prevents lithium dendrite formation on the negative electrode, so that the life characteristics of a lithium battery including the electrolyte can be improved.

[0017] Figure 1 schematically illustrates the structure of a lithium battery according to an embodiment.

[0018] Figure 2 schematically illustrates the structure of a lithium battery according to an embodiment.

[0019] Figure 3 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0020] Figure 4 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0021] Figure 5 is a schematic diagram of a lithium battery according to an exemplary embodiment.

[0022] Hereinafter, an electrolyte according to an embodiment and a lithium battery containing the same will be examined in more detail. These examples are provided solely as examples to more specifically illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present specification, including its definitions, shall prevail.

[0024] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein. The singular expression "singular" includes plural expression unless the context clearly indicates otherwise.

[0025] In this specification, the terms "include" or "have" are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials or combinations thereof.

[0026] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.

[0027] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one," "one or more," or "one or more" preceding elements herein may supplement the entire list of elements and do not mean that they supplement individual elements described above.

[0028] In this specification, the term "non-anode battery" means a battery in which i) there is no lithium-removable negative active material, or ii) no negative active material layer is used during battery assembly. Here, "thickness of the negative electrode" means the total thickness of the negative electrode current collector and the negative active material layer.

[0029] In order to clearly represent various layers and regions in the drawings, the thicknesses are enlarged or reduced. The same drawing reference numerals are used for similar parts throughout the specification. When a layer, film, region, plate, etc. is referred to as being "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. The terms first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only to distinguish one component from another.

[0030] The electrolyte comprises a first lithium salt comprising lithium ions and a first anion; a second lithium salt comprising lithium ions and a second anion; and a solvent comprising a fluorine-containing linear ester; wherein the degree of dissociation of the first lithium salt with respect to the fluorine-containing linear ester may be greater than the degree of dissociation of the second lithium salt with respect to the fluorine-containing linear ester.

[0031] For example, the greater the absolute value of the interaction energy (Interaction Energy, |IE|) between the lithium ion and the anion contained in the lithium salt, the lower the degree of dissociation, and the smaller the absolute value of the interaction energy (Interaction Energy, |IE|) between the lithium ion and the anion, the higher the degree of dissociation.

[0032] For example, the larger the absolute value of the interaction energy, the greater the binding energy between the lithium ion and the anion, and thus a relatively large amount of energy is required to separate the lithium salt into lithium ions and anions, which may decrease the degree of dissociation of the lithium ions in the solvent. Conversely, the smaller the absolute value of the interaction energy, the smaller the binding energy between the lithium ion and the anion, which may increase the degree of dissociation of the lithium ion in the solvent, as a relatively small amount of energy is required to separate the lithium salt into lithium ions and anions.

[0033] For example, the absolute value of the interaction energy (|IE|) can be obtained using the DFT method of the Gaussian program with structural optimization at the M062X / 6-311+G** level.

[0034] For example, the electrolyte of the present invention includes a first lithium salt and a second lithium salt, and when the electrolyte is applied to a lithium battery, a protective layer may be formed between the electrolyte and the negative electrode by the first lithium salt and the second lithium salt during charge and discharge, and the life characteristics of the lithium battery may be improved by the protective layer. However, the internal resistance of the lithium battery may increase by the protective layer. In this case, since the electrolyte includes a solvent including a fluorine-containing linear ester, the conductivity of lithium ions in the electrolyte is improved, thereby reducing the internal resistance of the lithium battery while easily implementing excellent life characteristics.

[0035] In addition, since the electrolyte simultaneously includes a first lithium salt having a high degree of dissociation with respect to a fluorine-containing linear ester and a second lithium salt having a low degree of dissociation, the conductivity of lithium ions in the electrolyte can be improved by including the first lithium salt having a high degree of dissociation, and a protective layer in a lithium battery can be formed more easily by including the second lithium salt having a low degree of dissociation.

[0036] According to one embodiment, the fluorine-containing linear ester may be represented by the following chemical formula 1.

[0037] <Chemical Formula 1>

[0038]

[0039] In the above chemical formula 1,

[0040] R1 and R2 are independently an alkyl group having 1 to 10 carbon atoms, which is unsubstituted or substituted with -F, -Cl, -Br or -I; an aryl group having 6 to 20 carbon atoms, which is unsubstituted or substituted with -F, -Cl, -Br or -I; or a heteroaryl group having 2 to 20 carbon atoms, which is unsubstituted or substituted with -F, -Cl, -Br or -I, wherein at least one of R1 and R2 may be substituted with one or more fluorine (F).

[0041] According to one embodiment, in the above formula 1, R1 may be substituted with one or more fluorine (F). According to another embodiment, in the above formula 1, R2 may be substituted with one or more fluorine (F). According to another embodiment, in the above formula 1, both R1 and R2 may be substituted with one or more fluorine (F).

[0042] According to one embodiment, in the above formula 1, R1 may be substituted with one fluorine (F). According to another embodiment, in the above formula 1, R2 may be substituted with one fluorine (F). According to another embodiment, in the above formula 1, both R1 and R2 may be substituted with one fluorine (F).

[0043] According to one embodiment, in the above chemical formula 1, R1 and R2 may be independently an alkyl group having 1 to 10 carbon atoms, which is unsubstituted or substituted with -F. According to one embodiment, in the above chemical formula 1, R2 may be an alkyl group having 1 to 10 carbon atoms, which is unsubstituted or substituted with -F. According to one embodiment, in the above chemical formula 1, both R1 and R2 may be an alkyl group having 1 to 10 carbon atoms, which is unsubstituted or substituted with -F.

[0044] According to one embodiment, the fluorine-containing linear ester may be represented by the following chemical formula 1-1.

[0045] <Chemical Formula 1-1>

[0046]

[0047] In the above chemical formula 1-1,

[0048] L1 is an alkylene group having 1 to 10 carbon atoms, and R3 is an alkyl group having 1 to 10 carbon atoms.

[0049] According to one embodiment, in the chemical formula 1-1, L1 may be a methylene group, an ethylene group, or a propylene group. According to one embodiment, in the chemical formula 1-1, R3 may be a methyl group, an ethyl group, a propyl group, a butyl group, or a pentyl group.

[0050] According to one embodiment, the content of the fluorine-containing linear ester may be 10 wt% or more based on the total weight of the solvent. For example, the content of the fluorine-containing linear ester may be 20 wt% or more, 30 wt% or more, or 40 wt% based on the total weight of the solvent. For example, the content of the fluorine-containing linear ester may be 10 to 90 wt%, 20 to 90 wt%, 30 to 90 wt%, 40 to 90 wt%, 10 to 80 wt%, 10 to 70 wt%, or 40 to 70 wt% based on the total weight of the solvent.

[0051] According to one embodiment, the fluorine-containing linear ester can satisfy the following condition 1 and the following condition 2.

[0052] Condition 1

[0053] | E Li-s | > 1.8 eV

[0054] Among the above conditions 1,

[0055] |E Li-s | is the absolute value of the interaction energy between the fluorine-containing linear ester and lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level,

[0056] Condition 2

[0057] | E PF6-s | < 0.1 eV

[0058] |E PF6-s | is measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, and the fluorine-containing linear ester and PF6 - It is the absolute value of the interaction energy between them.

[0059] For example, the above fluorine-containing linear ester has a large interaction energy with lithium ions and anions (e.g., PF6) -- ) may be small. For example, if a fluorine-containing linear ester has excellent interaction with lithium ions but relatively poor interaction with anions, the lithium ion conductivity of an electrolyte containing the fluorine-containing linear ester may be excellent.

[0060] According to one embodiment, in the above condition 1, the absolute value of the interaction energy between the fluorine-containing linear ester and the lithium ion may be greater than 1.82 eV, greater than 1.84 eV, or greater than 1.86 eV.

[0061] According to one embodiment, among the above conditions 2, the fluorine-containing linear PF6 - The absolute value of the interaction energy between them may be less than 0.1 eV, less than 0.08 eV, less than 0.06 eV, or less than 0.04 eV.

[0062] According to one embodiment, the solvent may further comprise an asymmetric cyclic carbonate.

[0063] According to one embodiment, the asymmetric cyclic carbonate may be represented by the following chemical formula 2.

[0064] <Chemical Formula 2>

[0065]

[0066] In the above chemical formula 2,

[0067] R 21 Inland R 24 are independently hydrogen, deuterium (-D), -F, -Cl, -Br or -I; an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I; an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I; or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I, wherein R 21 and R 22 The combination of R 23 and R 24 It is different from the combination of .

[0068] According to one implementation example, R 21 Inland R 24 are independently hydrogen or an alkyl group having 1 to 10 carbon atoms, and R21 and R 22 The combination of R 23 and R 24 The combination may be different.

[0069] According to one implementation example, R 21 Inland R 24 are independently hydrogen, methyl, ethyl, propyl, butyl, pentyl or hexyl groups, and R 21 and R 22 The combination of R 23 and R 24 The combination may be different.

[0070] According to one embodiment, the content of the asymmetric cyclic carbonate may be 20 wt% or less based on the total weight of the solvent. For example, the content of the asymmetric cyclic carbonate may be 18 wt% or less, 15 wt% or less, 12 wt% or less, 10 wt% or less, 1 to 20 wt%, 1 to 18 wt%, 1 to 15 wt%, 1 to 12 wt%, 1 to 10 wt%, 2 to 20 wt%, 2 to 18 wt%, 2 to 15 wt%, 2 to 12 wt%, 2 to 10 wt%, 4 to 20 wt%, 4 to 18 wt%, 4 to 15 wt%, 4 to 12 wt%, or 4 to 10 wt% based on the total weight of the solvent.

[0071] According to one embodiment, the solvent may further include one or more selected from an ester solvent, a glyme solvent, a dioxolane solvent, an ether solvent, a fluorinated ether solvent, a sulfone solvent, a ketone solvent, a nitrile solvent, and a carbonate compound.

[0072] The above-mentioned glyme solvents are, for example, ethylene glycol dimethyl ether (1,2-dimethoxyethane), ethylene glycol diethyl ether (1,2-diethoxyethane), propylene glycol dimethyl ether, propylene glycol diethyl ether, butylene glycol dimethyl ether, butylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, dibutylene glycol dimethyl ether, tributylene glycol dimethyl ether, tetrabutylene glycol dimethyl ether, dibutylene glycol diethyl ether, tributylene glycol diethyl ether and tetrabutylene glycol. It may contain one or more selected from diethyl ether.

[0073] The above ester solvent may include, for example, one or more selected from methyl propionate, ethyl propionate, ethyl butyrate, methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, gamma butyrolactone, decanolide, gamma valerolactone, mevalonolactone, and caprolactone.

[0074] The above ether solvent may include, for example, one or more selected from dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran.

[0075] The above ketone solvent may include cyclohexanone, and the above nitrile solvent may include at least one selected from acetonitrile (AN), succinonitrile (SN), and adiponitrile.

[0076] The above fluorinated ether solvent may include, for example, at least one selected from 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, and 2,2,3,3,4,4,5,5-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether.

[0077] The above dioxolane solvent may include, for example, at least one selected from 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, and 2-ethyl-2-methyl-1,3-dioxolane.

[0078] The above sulfone solvent may include, for example, one or more selected from dimethylsulfone, diethylsulfone, and ethylmethylsulfone.

[0079] The above carbonate solvent may include, for example, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, and the like.

[0080] According to one embodiment, the solvent may include at least one selected from a glyme solvent, a dioxolane solvent, a fluorinated ether solvent, a sulfone solvent, and a carbonate solvent.

[0081] According to one embodiment, the solvent may further comprise a fluorinated ether compound. According to one embodiment, the content of the fluorinated ether compound may be 50% by volume or less, for example, 0.1 to 50% by volume, for example, 1 to 30% by volume, based on the total amount of the solvent.

[0082] For example, fluorinated ether compounds have a high flash point of about 80°C or higher, which means they have excellent flame retardancy. Using them as solvents for liquid electrolytes allows for the production of lithium batteries with improved high-temperature stability. Furthermore, the fluorinated ether solvents have a structure in which fluorine-substituted functional groups are bonded around a -CH2-O- moiety and have low polarity. Therefore, these fluorinated ether solvents have excellent miscibility with high-solubility ether solvents capable of solvating lithium ions, such as DME.

[0083] The above fluorine-substituted ether solvent may be a compound represented by the following chemical formula 3.

[0084] [Chemical Formula 3]

[0085] R-CH2-OC n F 2n H

[0086] In the above chemical formula 3, R is C m+1 H m F 2m or C m F 2m+1 , n is an integer from 2 to 5, and m is an integer from 1 to 5.

[0087] The fluorine-substituted ether solvent represented by the above chemical formula 3 may be, for example, at least one selected from the group consisting of HCF2CF2CH2OCF2CF2H, HCF2CF2CH2OCF2CF2CF2H, HCF2CF2OCH2CF3, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2CH2OCF2CF2H, HCF2CF2OCF2CF2CF2H, HCF2CF2OCH2CH2OCF2CF2CF2H, and HCF2CF2OCH2CH2CH2OCF2CF2CF2H.

[0088] The fluorine-substituted ether solvent represented by the above chemical formula 3 may be, for example, 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, or 2,2,3,3,4,4,5,5-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether.

[0089] According to another embodiment, the electrolyte may further include at least one selected from gamma-butyrolactone, succinonitrile, adiponitrile, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, dioxane, sulfolane, dichloroethane, chlorobenzene, and nitrobenzene, in addition to the organic solvent described above.

[0090] According to one embodiment, the electrolyte may include a first lithium salt and a second lithium salt. For example, the degree of dissociation of the first lithium salt with respect to the fluorine-containing linear ester may be greater than the degree of dissociation of the second lithium salt with respect to the fluorine-containing linear ester.

[0091] According to one embodiment, the first lithium salt and the second lithium salt may satisfy the following equation 1.

[0092] <Formula 1>

[0093] |E Li-A1 | < |E Li-A2 |

[0094] In equation 1,

[0095] |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level,

[0096] |E Li-A2| is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

[0097] For example, when the first lithium salt and the second lithium salt satisfy the above formula 1, the condition that the degree of dissociation of the first lithium salt is greater than the degree of dissociation of the second lithium salt can be more easily satisfied.

[0098] For example, the above |E Li-A1 | may be proportional to the binding energy value between the lithium ion and the first anion. In this case, the above |E Li-A1 The smaller |E is, the lower the binding energy between the lithium ion and the first anion is, so that the first lithium salt can more easily dissociate into the lithium ion and the first anion in the solvent. For example, the above |E Li-A2 | may be proportional to the binding energy value between the lithium ion and the second anion. In this case, the above |E Li-A2 | The larger the value, the greater the binding energy between the lithium ion and the second anion, and the second lithium salt may not easily dissociate into the lithium ion and the second anion in the solvent. Accordingly, the degree of dissociation of the first lithium salt may be greater than that of the second lithium salt.

[0099] For example, when the first lithium salt and the second lithium salt satisfy the above formula 1, the first lithium salt having a large degree of dissociation improves the lithium ion conductivity of the electrolyte including it, and the second lithium salt having a small degree of dissociation forms a protective layer on the negative electrode, so that the life characteristics of the lithium battery including the electrolyte can be improved.

[0100] According to one embodiment, the first lithium salt and the second lithium salt may satisfy the following equation 2.

[0101] <Formula 2>

[0102] |ELi-A1 - E Li-A2 | > 0.3 eV

[0103] In equation 2,

[0104] |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, and |E Li-A2 | is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

[0105] For example, the above |E Li-A1 | and the above |E Li-A2 |If the difference satisfies the above equation 2, the lithium ion conductivity improvement effect of the first lithium salt and the protective layer formation effect of the second lithium salt can be further improved.

[0106] According to one implementation example, |E in the above formula 2 Li-A1 - E Li-A2 | The value can be greater than 0.4 eV, greater than 0.5 eV, greater than 0.6 eV, greater than 0.7 eV, greater than 0.8 eV, from 0.2 eV to 2 eV, from 0.2 eV to 1.8 eV, from 0.2 eV to 1.6 eV, from 0.2 eV to 1.4 eV, from 0.2 eV to 1.2 eV, from 0.4 eV to 2 eV, from 0.6 eV to 2 eV, from 0.8 eV to 2 eV, or from 0.2 eV to 1.2 eV.

[0107] According to one embodiment, the first lithium salt may satisfy the following equation 3, and the second lithium salt may satisfy the following equation 4.

[0108] <Formula 3>

[0109] |E Li-A1| ≤ 5.55 eV

[0110] In equation 3,

[0111] |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

[0112] <Formula 4>

[0113] |E Li-A2 | > 5.55 eV

[0114] In equation 4,

[0115] |E Li-A2 | is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

[0116] For example, when the first lithium salt satisfies the above formula 3, the degree of dissociation of the first lithium salt can be further improved, and the lithium ion conductivity of the electrolyte including the first lithium salt can be further improved.

[0117] According to one implementation example, |E in the above formula 3 Li-A1 |The value can be 5.5 eV or less, 5.4 eV or less, 5.3 eV or less, 5.2 eV or less, 5.1 eV or less, or 5 eV or less.

[0118] For example, when the second lithium salt satisfies the above formula 4, a protective layer can be formed more easily on the negative electrode included in the lithium battery described later from the second lithium salt.

[0119] According to one implementation example, |E in the above formula 4 Li-A2The value of | can be greater than 5.5 eV, greater than 5.6 eV, greater than 5.7 eV, or greater than 5.8 eV. For example, |E in Equation 4 above Li-A2 The value of | can be greater than 5.5 eV and less than or equal to 6.5 eV, greater than 5.5 eV and less than or equal to 6.4 eV, greater than 5.5 eV and less than or equal to 6.3 eV, greater than 5.5 eV and less than or equal to 6.2 eV, greater than 5.5 eV and less than or equal to 6.1 eV, greater than 5.5 eV and less than or equal to 6.0 eV, or greater than 5.5 eV and less than or equal to 5.9 eV.

[0120] According to one embodiment, the first lithium salt and the second lithium salt can form a protective layer on the negative electrode when applied to a lithium battery.

[0121] According to one embodiment, the first lithium salt may include LiDFOP (lithium difluoro(bisoxalato)phosphate), LiBOB (lithium bis(oxalato)borate), LiFMDFB (lithium fluoromalonato(difluoro)borate), LiTDI (lithium 2-trifluoromethyl-4,5-dicyanoimidazole), LiBSO4F2, LiPF6, LiDFOB (lithium difluoro(oxalato)borate), or any combination thereof. For example, the first lithium salt may include LiDFOP (lithium difluoro(bisoxalato)phosphate), LiBOB (lithium bis(oxalato)borate), LiFMDFB (lithium fluoromalonato(difluoro)borate), LiTDI (lithium 2-trifluoromethyl-4,5-dicyanoimidazole), LiBSO4F2, or any combination thereof. According to one embodiment, the first lithium salt may include LiDFOP (Lithium difluoro(bisoxalato)phosphate), LiBOB (Lithium bis(oxalato)borate), LiFMDFB (Lithium fluoromalonato(difluoro)borate), LiTDI (Lithium 2-trifluoromethyl-4,5-dicyanoimidazole), or any combination thereof.

[0122] In one embodiment, the second lithium salt may include LiPOF4, LiPO2F2, LiBF4, LiCF3SO3, LiTFSI (Lithium bis(trifluoromethanesulfonyl)imide), LiFSI (Lithium bis(fluorosulfonyl)imide), LiDCTA (Lithium 4,5-dicyano-1,2,3-triazolate), LiDFOB (Lithium difluoro(oxalato)borate), or any combination thereof. For example, the second lithium salt may include LiPOF4, LiPO2F2, LiBF4, LiCF3SO3, LiTFSI (Lithium bis(trifluoromethanesulfonyl)imide), LiFSI (Lithium bis(fluorosulfonyl)imide), LiDCTA (Lithium 4,5-dicyano-1,2,3-triazolate), or any combination thereof.

[0123] According to one embodiment, the electrolyte may further include a lithium salt other than the lithium salt described above.

[0124] For example, the lithium salt may be any lithium salt commonly used in the art for manufacturing electrolytes.

[0125] According to one embodiment, the lithium salt is LiSCN, LiN(CN)2, Li(CF3SO2)3C, Li(FSO2)2N(LiFSI), LiC4F9SO3, LiN(SO2CF2CF3)2, LiPF3(C2F5)3, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiPF6, LiPF5(CF3), LiPF5(C2F5), LiPF5(C3F7), LiPF4(CF3)2, LiPF4(CF3)(C2F5), LiPF3(CF3)3, LiPF3(CF2CF3)3, LiPF4(C2O4)2, LiBF4, LiBF3(C2F5), lithium tetrafluoro(oxalate) phosphate, lithium difluoro(bisoxalato) phosphate lithium bis(oxalato)borate (LiBOB), lithium oxalyldifluoroborate (LIODFB), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2), LiN(SO2C2F5)2, LiCF3SO3, LiAsF6, LiSbF6, LiClO4, or mixtures thereof.

[0126] According to one embodiment, the sum of the concentrations of the first lithium salt and the second lithium salt in the electrolyte is 0.1 to 10.0 M, for example, 0.1 to 5.0 M, 0.1 to 4.0 M, 1 to 10.0 M, 1 to 5.0 M, 1 to 4.0 M, 2 to 10.0 M, 2 to 5.0 M, or 2 to 4.0 M. When the concentration of the lithium salt is within the above range, further improved lithium secondary battery characteristics can be obtained.

[0127] According to one embodiment, the electrolyte may further include at least one selected from an ionic liquid and a polymer ionic liquid.

[0128] For example, the ionic liquid may be used without limitation as long as it is an ionic substance that is in a molten state at room temperature (25°C) and contains cations and anions.

[0129] The cation of the ionic liquid may include imidazolium, ammonium, pyrrolidinium, or piperidinium, and the anion of the ionic liquid may include bis(fluorosulfonyl)imide, bis(fluorosufonyl)amide, fluoroborate, or fluorophosphate.

[0130] The cation of the ionic liquid may include an alkylammonium such as triethylammonium, an imidazolium such as ethylmethylimidazolium or butylmethylimidazolium, a pyrrolidinium such as 1-methyl-1-propylpyrrolidinium, or a methylpropylpiperidinium.

[0131] The anion of the ionic liquid may include bis(trifluoromethylsulfonyl)imide (TFSI), bis(pentafluoroethylsufonyl)amide (BETI), tetrafluoroborate (BF4), or hexafluorophosphate (PF6).

[0132] For example, the ionic liquids include [emim]Cl / AlCl3 (emim = ethyl methyl imidazolium), [bmpyr]NTf2 (bppyr = butyl methyl pyridinium), [bpy]Br / AlCl3 (bpy = 4, 4'-bipyridine), [choline]Cl / CrCl3·6H2O, [Hpy(CH2)3pyH][NTf2]2(NTf = trifluoromethanesulfonimide), [emim]OTf / [hmim]I(hmim = hexyl methyl imidazolium), [choline]Cl / HOCH2CH2OH, [Et2MeN(CH2CH2OMe)]BF4(Et = ethyl, Me = methyl, Pr = propyl, Bu = butyl, Ph = phenyl, Oct = octyl, Hex = hexyl), [Bu3PCH2CH2C8F 17 ]OTf (OTf = trifluoromethane sulfonate), [bmim]PF6 (bmim = butyl methyl imidazolium), [bmim]BF4, [omim]PF6 (omim = octyl methyl imidazolium), [Oct3PC 18 H 37]I, [NC(CH2)3mim]NTf2(mim = methyl imidazolium), [Pr4N][B(CN)4], [bmim]NTf2, [bmim]Cl, [bmim][Me(OCH2CH2)2OSO3], [PhCH2mim]OTf, [Me3NCH(Me)CH(OH)Ph] NTf2, [pmim][(HO)2PO2] (pmim = propyl methyl imidazolium), [b(6-Me)quin]NTf2(bquin = butyl quinoline, [bmim][Cu2Cl3], [C 18 H 37 OCH2mim]BF4(mim = methyl imidazolium) 14 H 29 mim]Br(mim = methyl imidazolium), [Me2N(C 12 H 25 )2]NO3, [emim]BF4, [mm(3-NO2)im][dinitrotriazolate], [MeN(CH2CH2OH)3], [MeOSO3], [Hex3PC 14 H 29 ]NTf2, [emim][EtOSO3], [choline][ibuprofenate], [emim]NTf2, [emim][(EtO)2PO2], [emim]Cl / CrCl2, [Hex3PC 14 H 29 ]N(CN)2, or any combination of these may be included.

[0133] The above polymeric ionic liquid may include an ionic compound in the form of a polymer composed of an organic cation containing an imidazolium group and an organic or inorganic anion.

[0134] For example, the organic cation of the polymeric ionic liquid may include poly(1-vinyl-3-alkylimidazolium), poly(1-allyl-3-alkylimidazolium), poly(1-(meth)acryloyloxy-3-alkylimidazolium). The organic anion of the polymeric ionic liquid may include CH3COO. - , CF3COO - , CH3SO3 - , CF3SO3 - , (CF3SO2)2N - , (CF3SO2)3C - , (CF3CF2SO2)2N - , C4F9SO3 - , C3F7COO - , (CF3SO2)(CF3CO)N - may include.

[0135] For example, the polymeric ionic liquid may comprise poly(1-vinyl-3-alkylimidazolium), poly(1-allyl-3-alkylimidazolium), poly(1-(meth)acryloyloxy-3-alkylimidazolium), or any combination thereof.

[0136] According to one embodiment, the viscosity of the electrolyte may be 5 cP or less at 25°C. For example, when the electrolyte satisfies the viscosity range described above, ions within the electrolyte may move freely and have excellent ionic conductivity. For example, the ionic conductivity of the electrolyte may be 1.0 mS / cm to 5.0 mS / cm at 25°C.

[0137] According to one embodiment, the electrolyte may be in a liquid, gel, or semi-solid form. When the electrolyte is in a liquid, gel, or semi-solid form, the disadvantages of conventional lithium metal batteries can be overcome because at least one selected from lithium metal and lithium alloys can be freely expanded during charging and discharging, compared to when the electrolyte is in a completely solid form.

[0138]

[0139] [Lithium battery (100)]

[0140] Referring to FIGS. 1 and 2, a lithium battery according to an embodiment will be described in detail.

[0141] For example, referring to FIG. 1, the lithium battery may be a lithium non-anode metal battery (100). For example, referring to FIG. 2, the lithium battery may be a lithium metal battery (200).

[0142] A lithium battery according to one embodiment may include a positive electrode; a negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode, and the electrolyte may include the electrolyte described above.

[0143] According to one embodiment, the electrolyte may have a liquid or gel form.

[0144] A lithium battery according to an embodiment may include, as shown in FIG. 1, a negative electrode current collector (110) that does not have a plate-shaped lithium metal thin film; an electrolyte (120) disposed on the negative electrode current collector (110); and a positive electrode (150) disposed on the electrolyte (120). In this case, the negative electrode may include only the negative electrode current collector (110) that does not have a lithium metal thin film, and the positive electrode (250) may include a positive electrode current collector (140) and a positive electrode active material layer (130) disposed on the positive electrode current collector (140).

[0145] According to one embodiment, a lithium battery (200) may further include a metal layer (225) disposed between a negative electrode current collector (210) and an electrolyte (220), as shown in FIG. 2. In this case, the negative electrode may include a negative electrode current collector (210); and a metal layer (225) disposed between the negative electrode current collector (210) and the electrolyte (220). For example, the lithium battery (200) may include a negative electrode current collector (110), a metal layer (225) disposed on the negative electrode current collector (110), an electrolyte (120) disposed on the metal layer (225); and a positive electrode (150) disposed on the electrolyte (120). For example, the metal layer (225) may include lithium metal or a lithium alloy. For example, the metal layer (225) may dissociate into lithium ions and metal cations during a discharge process, so that the thickness of the metal layer (225) may be reduced. Conversely, the metal layer (225) may have lithium ions precipitated during the charging process, which may increase the thickness of the metal layer (225).

[0146] According to one embodiment, a lithium battery including the electrolyte described above may further include a protective layer (not shown) disposed between the negative electrode and the electrolyte during a charge / discharge process. For example, the protective layer (not shown) may be formed between the negative electrode and the electrolyte through the interaction of the first lithium salt, the second lithium salt, and the solvent described above.

[0147] Referring to FIG. 1, the protective layer (not shown) can be formed between the negative electrode collector (110) and the electrolyte (120).

[0148] Referring to FIG. 2, the protective layer (not shown) may be formed on the negative electrode current collector (110) and the electrolyte (120). For example, the protective layer (not shown) may be formed between the metal layer (225) and the electrolyte (120).

[0149]

[0150] [Cathode current collector (110, 210)]

[0151] For example, the material constituting the negative electrode current collector (110, 210) can be any material that does not react with lithium, that is, any material that does not form an alloy or compound with lithium and has conductivity. The metal substrate is, for example, a metal or an alloy. The metal substrate can be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The electrode current collector (200) can have a shape selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these shapes, and any shape used in the relevant technical field can be used.

[0152] For example, the negative electrode current collector (110, 210) may have a reduced thickness compared to the negative electrode current collector included in a conventional negative electrode. Therefore, the negative electrode according to the present disclosure is distinguished from the conventional electrode including a thick film current collector, for example, by including a thin film current collector. Since the electrode according to one embodiment employs a thin film current collector having a reduced thickness, the thickness of the negative electrode active material layer in the negative electrode including the thin film current collector is relatively increased. As a result, the energy density of a lithium metal battery employing such an electrode is increased. The thickness of the negative electrode current collector (110, 210) may be, for example, less than 15 um, 14.5 um or less, or 14 um or less. The thickness of the negative electrode current collector (110, 210) may be, for example, 0.1 um to less than 15 um, 1 um to 14.5 um, 2 um to 14 um, 3 um to 14 um, 5 um to 14 um, or 10 um to 14 um.

[0153] The material constituting the negative electrode collector (110, 210) may be any material that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The negative electrode collector (110, 210) is, for example, a metal or an alloy. The negative electrode collector (210) may be made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0154] The negative electrode current collector (110, 210) may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field is possible.

[0155] The negative electrode current collector (110, 210) may include, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. The negative electrode current collector (110, 210) includes a substrate, and the substrate may have a structure including, for example, a base film and a metal substrate layer disposed on one or both sides of the base film. An intermediate layer may additionally be disposed on the metal substrate layer.

[0156] For example, the base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can melt when a short circuit occurs, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal substrate layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal substrate layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by controlling the thickness of the metal substrate layer. The metal substrate layer may be plated or deposited on the base film. When the thickness of the metal substrate layer is reduced, the limit current and / or maximum current of the negative electrode current collector (110, 210) decreases, thereby improving the stability of the lithium metal battery in the event of a short circuit. A lead tab may be added on the metal substrate layer for connection to the outside. The lead tab may be welded to the metal substrate layer or the metal substrate layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal substrate layer may be melted, so that the metal substrate layer may be electrically connected to the lead tab. In order to make the welding of the metal substrate layer and the lead tab more solid, a metal chip may be added between the metal substrate layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal substrate layer. The metal chip may be, for example, a metal foil, a metal mesh, etc.The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After arranging the metal piece on the metal substrate layer, the lead tab may be welded to the metal piece / metal substrate layer laminate or the metal piece / metal substrate layer / base film laminate by welding the metal piece with the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal substrate layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the negative electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. To improve the adhesion between the base film and the metal substrate layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal substrate layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal substrate layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the negative electrode. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode collector (110, 210) can reduce the weight of the electrode and consequently improve the energy density.

[0157] According to one embodiment, the metal layer (225) including the plate-shaped lithium metal thin film may be free on the negative electrode current collector (110) before performing charge / discharge. For example, in the case of a non-anode lithium metal battery in which the plate-shaped lithium metal thin film is free on the negative electrode current collector (110) before performing charge / discharge, dendrite formation can be prevented, thereby further improving the life characteristics.

[0158] According to another embodiment, a metal layer (225) including a plate-shaped lithium metal thin film may be disposed on the negative electrode current collector (210) before performing charge and discharge. For example, in the process of disposing an electrolyte on the metal layer (225) disposed on the negative electrode current collector (210), the metal cations included in the electrolyte may react with the metal layer (225), so that the metal cations may be precipitated as metal. The precipitated metal cations may be dissociated into metal cations during discharge.

[0159] According to one embodiment, the negative electrode current collector (210) may further include a protective layer (not shown) derived from the first lithium salt and the second lithium salt. For example, the negative electrode current collector (210) may further include a protective layer (not shown) derived from the first lithium salt and the second lithium salt.

[0160] According to one embodiment, the negative electrode may further include an interlayer disposed between the negative electrode current collector (210) and the metal layer (225).

[0161] According to one embodiment, the interlayer may be directly disposed on, for example, one or both surfaces of the negative electrode collector (210). Accordingly, no other layer may be disposed between the negative electrode collector (210) and the interlayer. By directly disposing the interlayer on one or both surfaces of the negative electrode collector (210), the bonding force between the negative electrode collector (210) and the metal layer (225) may be further enhanced.

[0162] The thickness of the intermediate layer (not shown) is, for example, 30% or less of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. By having the above intermediate layer (not shown) with a thickness in this range, the bonding force between the negative electrode current collector (210) and the metal layer (225) can be further improved, and an increase in interface resistance can be suppressed.

[0163] For example, the intermediate layer may include a binder. By including the binder in the intermediate layer, the bonding strength between the negative electrode current collector (210) and the metal layer (225) may be further enhanced. The binder included in the intermediate layer (not shown) may be, for example, a conductive binder or a non-conductive binder.

[0164] The conductive binder may be, for example, an ion-conducting binder and / or an electron-conducting binder. A binder having both ion-conducting and electron-conducting properties may be classified as either an ion-conducting binder or an electron-conducting binder.

[0165] The ion-conducting binder is, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, and polyacetylene. The ion-conducting binder may include a polar functional group. Examples of the ion-conducting binder including a polar functional group include Nafion, Aquibion, etc. (Aquivion), Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi+), etc.Electronically conductive binders include, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc. The intermediate layer may be a conductive layer comprising, for example, a conductive polymer.

[0166] The binder included in the intermediate layer may be, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer may be, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be disposed on the negative electrode current collector (210) in a dry or wet manner, for example. The intermediate layer may be, for example, a binding layer including a binder.

[0167] The intermediate layer may additionally include, for example, a carbon-based conductive material. By including the carbon-based conductive material, the intermediate layer may be, for example, a conductive layer. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.

[0168] The intermediate layer may be disposed on the negative electrode current collector (210) in a dry manner, for example, by deposition such as CVD or PVD. The intermediate layer may be disposed on the negative electrode current collector (210) in a wet manner, for example, by spin coating, dip coating, or the like. The intermediate layer may be disposed on the negative electrode current collector (210) by, for example, depositing a carbon-based conductive material on the negative electrode current collector (210) by deposition. The dry-coated intermediate layer may be made of a carbon-based conductive material and may not include a binder. Alternatively, the intermediate layer may be disposed on the negative electrode current collector by, for example, coating a composition including a carbon-based conductive material, a binder, and a solvent on the surface of the negative electrode current collector and drying it. The intermediate layer may have a single-layer structure or a multi-layer structure including a plurality of layers.

[0169] [Cathode: Metal layer]

[0170] Referring to FIG. 2, the lithium battery (200) may further include a metal layer (225) disposed between the negative electrode current collector (210) and the electrolyte (220). For example, the metal layer (225) may include lithium metal or a lithium alloy.

[0171] For example, the lithium metal or the lithium alloy may be generated when lithium ions included in the electrolyte (120) are deposited on the negative electrode current collector (110) as the lithium battery (200) is charged. For example, the metal layer (225) may include a lithium alloy and a lithium metal. For example, the lithium alloy included in the metal layer (225) may weaken the reactivity of the lithium metal, thereby effectively preventing a side reaction between the metal layer (225) and the electrolyte (120). In addition, the metal layer (225) has excellent electrical conductivity, so that the internal resistance of the lithium battery (200) including the metal layer (225) may be reduced. Accordingly, the lithium battery (200) including the metal layer (225) may have improved not only life characteristics but also charge and discharge efficiency.

[0172] According to one embodiment, the metal layer (225) may include, for example, lithium foil, lithium powder, plated lithium, a carbon-based material, or a combination thereof. For example, the metal layer (225) may include lithium foil. For example, the metal layer (225) may be introduced by coating a slurry including lithium powder and a binder onto the negative electrode current collector (210). For example, the binder may be a fluorine-based binder such as polyvinylidene fluoride (PVDF).

[0173] According to one embodiment, the metal layer (225) may not include a carbon-based negative electrode active material. Accordingly, the metal layer (225) may be formed of a metal-based negative electrode active material.

[0174] For example, the thickness of the metal layer (225) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted according to the required shape, capacity, etc. of the lithium battery. If the thickness of the metal layer (225) increases excessively, the structural stability of the lithium battery may deteriorate and side reactions may increase. If the thickness of the metal layer (225) is excessively small, the energy density of the lithium metal battery may decrease.

[0175] According to one embodiment, the thickness of the lithium foil may be, for example, 1 μm to 50 μm, 1 μm to 30 μm, or 10 μm to 30 μm, or 10 μm to 80 μm. By having the lithium foil have a thickness in this range, the life characteristics of the lithium battery can be further improved.

[0176] According to one embodiment, the particle size of the lithium powder may be, for example, 0.1 μm to 3 μm, 0.1 μm to 2 μm, or 0.1 μm to 2 μm. When the lithium powder has a thickness within this range, the life characteristics of the lithium battery can be further improved.

[0177]

[0178] [Electrolyte (120)]

[0179] For example, the electrolyte (120) may include a first lithium salt as described above; a second lithium salt; and a solvent including a fluorine-containing linear ester.

[0180] According to another embodiment, the electrolyte (120) may further include a nonwoven fabric. The nonwoven fabric may serve to support at least one selected from lithium metal and lithium alloys precipitated during the charging process. For example, the nonwoven fabric may be omitted. For example, if the negative electrode current collector is of the mesh type, the nonwoven fabric may not be used.

[0181] The above nonwoven fabric may have a porosity of 10 to 90%, for example, 10 to 80%, for example, 10 to 50 vol%, for example, 25 to 50 vol%, and an average pore size of 0.1 to 10 µm, for example, 0.01 to 8 µm, for example, 0.1 to 1.0 µm. The average pore size represents the diameter when the pore shape is spherical, and represents the major axis length when the pore shape is non-spherical.

[0182] According to one embodiment, the nonwoven fabric may include one or more nonwoven fabrics selected from cellulose, polyester (e.g., polyethylene terephthalate (PET), polyetherimide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, nylon, and polyparaphenylenebenzobisoxazole.

[0183]

[0184] [anode]

[0185] As shown in FIGS. 1 and 2, a positive electrode active material layer (130, 230) is disposed on a positive electrode current collector (140, 240) to form a positive electrode (150, 250). More specifically, a positive electrode active material layer (130, 230) may be disposed on an electrolyte (120, 220), and a positive electrode current collector (140, 240) may be disposed on the positive electrode active material layer (130, 230).

[0186] [Anode: Anode current collector]

[0187] Referring to FIGS. 1 and 2, the positive electrode (150, 250) includes a positive electrode current collector (140, 240). For example, the positive electrode (150, 250) can be prepared by forming the positive electrode active material layer (130, 230) on the positive electrode current collector (140, 240).

[0188] For example, the positive electrode current collector (140, 240) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0189] According to one embodiment, the positive electrode collector (140, 240) may include aluminum (Al).

[0190]

[0191] [Anode: Anode active material layer]

[0192] The above positive electrode active material layer (130, 230) may include a positive electrode active material, a conductive material, and a binder.

[0193] For example, the cathode active material may be at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Li a A 1-b B 1 b D 12 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B 1 b O 2-c D 1 c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B 1 b O 4-c D 1 c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni1-b-c Mn b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f)J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:

[0194] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, Ga, Si, W, Mo, Cu, Zn, Ti, boron (B), rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, Cl, Br or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0195] For example, the positive electrode active material may include a lithium transition metal oxide containing nickel and another transition metal. In the lithium transition metal oxide containing nickel and another transition metal, the content of nickel may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, for example, 90 mol% or more, based on the total mole number of transition metals.

[0196] For example, the lithium transition metal oxide may be a compound represented by the following chemical formula 3:

[0197] <Chemical Formula 3>

[0198] Li a Ni x Co y M z O 2-b A b

[0199] In chemical formula 3, 1.0≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상이고,

[0200] A is F, S, Cl, Br or a combination thereof.

[0201] For example, in chemical formula 3, 0.7≤x<1, 0 <y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, 0<z≤0.15; 또는 0.85≤x<0.95, 0<y≤0.1, 0<z≤0.1일 수 있다.

[0202] For example, the lithium transition metal oxide may be at least one of the compounds represented by the following chemical formulae 3-1 and 3-2:

[0203] <Chemical Formula 3-1>

[0204] LiNi x Co y Mn z O2

[0205] In Chemical Formula 3-1, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이고,

[0206] <Chemical Formula 3-2>

[0207] LiNi x Co y Al z O2

[0208] In Chemical Formula 3-2, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.8≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.82≤x≤0.95, 0<y≤0.15, 0<z≤0.15이다. 예를 들어, 0.85≤x≤0.95, 0<y≤0.1, 0<z≤0.1이다.

[0209] For example, lithium transition metal oxide is LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.2 O2 or LiNi 0.88 Co 0.1 Al 0.02 It could be O2.

[0210] For example, the above-mentioned positive electrode active material may be used as one having a coating layer on the surface of the lithium transition metal oxide, or may be used by mixing the lithium transition metal oxide and a lithium transition metal oxide having a coating layer.

[0211] For example, the coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element.

[0212] For example, the compound forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the lithium transition metal oxide with the coating elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0213] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.

[0214] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.

[0215]

[0216] [Separator]

[0217] A lithium battery according to an embodiment may further include a separator (not shown).

[0218] Specific examples of the above separator include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0219] According to one embodiment, the battery case including the lithium battery may be cylindrical, square, thin-film, etc. For example, the lithium battery may be a large-scale thin-film battery. The lithium battery may be a lithium ion battery.

[0220] According to an embodiment, the lithium battery (100, 200) may be, for example, a lithium-air battery, a lithium-sulfur battery, etc.

[0221] According to one embodiment, the lithium battery (100, 200) can be used in electric vehicles (EVs) due to its excellent lifespan and high-rate characteristics. For example, it can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring large amounts of power storage. For example, it can be used in electric bicycles, power tools, etc.

[0222] When stacking multiple lithium batteries (100, 200) according to an embodiment, a gel-type electrolyte may be placed between the positive electrode and the liquid-impermeable ion-conductive composite membrane. The gel-type electrolyte may include, for example, a PVDF-HFP copolymer, a lithium salt, and a solvent.

[0223] Referring to FIG. 3, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.

[0224] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.

[0225] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), the aforementioned negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.

[0226] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 3 to 5, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.

[0227] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0228] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.

[0229]

[0230] Hereinafter, the following examples will be used to explain in more detail, but the present invention is not limited to the following examples.

[0231] Evaluation Example 1: Calculation of the interaction energy between lithium salt and solvent

[0232] For the solvents listed in Table 1 below, the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level was used to determine the solvent and lithium ion and solvent and PF6. - - The interaction energy between them was calculated and listed in Table 1 below. In Table 1 below, |E PF6-s | is a solvent and PF6 - is the absolute value of the interaction energy, |E Li-s | is the absolute value of the interaction energy between the yomae and the lithium ion.

[0233] Target substance name|E Li-s |(eV)|E PF6-s |(eV)FECFluoroethylene carbonate1.650.43DMCDimethyl carbonate1.70.16ECEthylene carbonate1.860.36MFAMethyl fluoroacetate1.890.03PCPropylene carbonate1.920.38DECDiethyl carbonate1.920.12VECVinyl ethylene carbonate1.930.38

[0234] In addition, the interaction energy between lithium ions and anions contained in the lithium salt was calculated using the DFT method of the Gaussian program, which was structure optimized at the M062X / 6-311+G** level for the lithium salts described in Table 2 below, and is described in Table 1 below. In Table 2 below, |E Li-A | is the absolute value of the interaction energy between lithium ions and anions in a lithium salt.

[0235] Target substance name | ELi-A |(eV)LiDFOPLithium difluoro(bisoxalato)phosphate4.87LiBOBLithium bis(oxalato)borate5LiFMDFBLithium fluoromalonato(difluoro)borate5.12LiTDILithium 2-trifluoromethyl-4,5-dicyanoimidazole5.41LiBSO4F2Lithium difluoro(sulfato)borate5.49LiPF6Lithium hexafluorophosphate5.5LiDFOBLithium difluoro(oxalato)borate5.54LiDCTALithium 4,5-dicyano-1,2,3-triazolate5.6LiFSILithium bis(fluorosulfonyl)imide5.65LiTFSILithium bis(trifluoromethanesulfonyl)imide5.74LiCF3SO3Lithium triflate5.8LiBF4Lithium tetrafluoroborate5.86LiPO2F2Lithium Difluorophosphate6.08LiPOF4-6.21

[0236]

[0237] (Electrolyte production)

[0238] Manufacturing Example 1

[0239] The electrolyte was prepared by dissolving 0.6 M LiBF4 and 0.6 M LiDFOB in a liquid mixed solvent containing FEC:DMC:MFA in a weight ratio of 32:60:8.

[0240] Manufacturing Examples 2 to 6 and Comparative Manufacturing Examples 1 to 3

[0241] An electrolyte was prepared in the same manner as Example 1, except that the types of the first lithium salt, the second lithium salt, and the solvent were changed as shown in Table 3 below.

[0242] Evaluation Example 2: Ionic Conductivity

[0243] The ionic conductivity of the electrolytes according to Manufacturing Examples 1 to 6 and Comparative Manufacturing Examples 1 to 3 was evaluated at 20°C using a Mettler Toledo conductivity measuring device.

[0244] The results of the ionic conductivity measurements are shown in Table 3 below.

[0245] First lithium salt Second lithium salt Solvent ion conductivity (mS / cm) Preparation example 10.6M LiDFOB 0.6M LiBF4FEC / DMC / MFA (32wt / 60wt / 8wt) 10.1 Preparation example 20.6M LiDFOB 0.6M LiBF4FEC / DEC / MFA (32wt / 8wt / 60wt) 6.8 Preparation example 30.6M LiDFOB 0.6M LiBF4FEC / PC / MFA (32wt / 8wt / 60wt) 7.4 Preparation example 40.6M LiDFOB 0.6M LiBF4FEC / DMC / MFA (15wt / 25wt / 60wt) 9.3 Preparation example 50.6M LiDFOB 0.6M LiBF4FEC / DMC / MFA(15wt / 60wt / 25wt)10.4 Manufacturing example 60.6M LiDFOB0.6M LiBF4FEC / DMC / MFA(32wt / 8wt / 60wt)7.6 Comparative manufacturing example 10.6M LiDFOB0.6M LiBF4FEC / DMC(41wt / 59wt)4.1 Comparative manufacturing example 20.6M LiDFOB0.6M LiBF4FEC / DEC(41wt / 59wt)2.8 Comparative manufacturing example 31.2M LiPF6-FEC / DEC(41wt / 59wt)6.4

[0246] Referring to Table 2 above, the degree of dissociation of the first lithium salt (LiDFOB) having a low interaction energy between the lithium ions and anions contained in the lithium salt was greater than that of the second lithium salt (LiBF4) having a high interaction energy between the lithium ions and anions contained in the lithium salt.

[0247] In addition, referring to Table 3 above, it was confirmed that the ionic conductivity was improved when the first lithium salt (LiDFOB) with a large degree of dissociation and the second lithium salt (LiBF4) with a small degree of dissociation were dissolved in a solvent containing a linear fluorine-containing ester (MFA).

[0248] Example 1

[0249] (Manufacturing of positive electrode)

[0250] LiNi as a cathode active material x Co y Al 1-x-y A slurry was prepared by mixing a mixture of O2, carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVdF) in a weight ratio of 97:1.5:1.5 with N-methylpyrrolidone (NMP) in an agate mortar.

[0251] The slurry was applied at 23 mg / cm on a 10 μm thick aluminum collector. 2 By loading, bar coating, drying at room temperature, drying again under vacuum at 120℃, rolling and punching, a positive electrode plate having a thickness of 65㎛ and an electrode density of 3.7g / cc was manufactured.

[0252] (Cathode manufacturing)

[0253] A copper (Cu) current collector with a thickness of 10 ㎛ was used.

[0254] (Manufacturing of lithium batteries)

[0255] A lithium battery was manufactured using the positive and negative electrodes manufactured above, a PE separator, and an electrolyte according to Manufacturing Example 1, through an appropriate pouch or can sealing process. A certain level of pressure or higher may be applied to the lithium battery.

[0256]

[0257] Examples 2 to 6 and Comparative Examples 1 to 3

[0258] A lithium battery was manufactured in the same manner as in Example 1, except that the electrolyte according to Manufacturing Examples 2 to 6 and Comparative Manufacturing Examples 1 to 3 was used instead of the electrolyte according to Manufacturing Example 1.

[0259]

[0260] Evaluation Example 3: Charge / Discharge Characteristics

[0261] Lithium batteries manufactured according to Examples 1 to 5 and Comparative Examples 1 to 6 were charged at a constant current of 0.1 C at 45°C until the voltage reached 4.30 V (vs. Li), and then cut-off was made at a current of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, discharge was performed at a constant current of 0.1 C (Mars stage, 1 st Cycle). This process was repeated once to complete the Mars process.

[0262] The lithium battery that had gone through the above-described Martian step was charged to 4.3 V compared to the lithium standard reduction potential at a current of 0.2 C at 45°C, cut off at a current of 0.05 C while maintaining 4.3 V in constant voltage charging mode, and then discharged at a constant current of 0.5 C. The above-described charge and discharge process was repeated a total of 50 times.

[0263] In all the above charge / discharge cycles, a 10-minute pause was allowed after each charge / discharge cycle. Here, 50 th The capacity retention rate in a cycle is defined by the following equation.

[0264] [ceremony]

[0265] Capacity retention rate (%) = [ x 100]

[0266] 50 th The capacity retention rate during the cycle is shown in Table 4 below.

[0267]

[0268] Evaluation Example 4: 0.5C discharge capacity compared to the Mars process discharge capacity

[0269] In order to compare the cell resistance of the lithium batteries according to Examples 1 to 6 and Comparative Examples 1 to 3, the values ​​of the 0.5C discharge capacity and the 0.1C ignition process discharge capacity were compared at 45°C.

[0270] The 0.5C / 0.1C discharge capacity ratio results are shown in Table 4 below.

[0271] Electrolyte capacity retention rate @50 th Cycle discharge capacity ratio (0.5C / 0.1C, %) Example 1 Manufacturing example 186.0893.4 Example 2 Manufacturing example 288.9495.4 Example 3 Manufacturing example 387.8395.6 Example 4 Manufacturing example 488.7396.0 Example 5 Manufacturing example 593.9796.0 Example 6 Manufacturing example 689.5695.7 Comparative example 1 Comparative manufacturing example 185.3393.2 Comparative example 2 Comparative manufacturing example 283.5192.7 Comparative example 3 Comparative manufacturing example 376.9893.4

[0272]

[0273] Referring to Table 4 above, Examples 1 to 6 including the electrolyte according to Manufacturing Examples 1 to 5 had improved rate characteristics and thus excellent life characteristics compared to Comparative Examples 1 to 3.

[0274]

[0275] While the above has been described with reference to drawings and examples, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent implementations are possible. Accordingly, the scope of protection of the present invention should be defined by the appended claims.

[0276]

[0277] <Explanation of symbols>

[0278] 100, 200: Lithium battery

[0279] 110, 210: cathode assembly 120, 220: electrolyte

[0280] 130, 230: Cathode active material layer 140, 240: Cathode current collector

[0281] 150, 250: anode 225: metal layer

Claims

1. A first lithium salt comprising a lithium ion and a first anion; A second lithium salt comprising a lithium ion and a second anion; and A solvent comprising a fluorine-containing linear ester; An electrolyte wherein the degree of dissociation of the first lithium salt for the fluorine-containing linear ester is greater than the degree of dissociation of the second lithium salt for the fluorine-containing linear ester.

2. In paragraph 1, The above fluorine-containing linear ester is an electrolyte represented by the following chemical formula 1: <Chemical Formula 1> In the above chemical formula 1, R1 and R2 are independently an alkyl group having 1 to 10 carbon atoms, substituted or unsubstituted with -F, -Cl, -Br or -I; an aryl group having 6 to 20 carbon atoms, substituted or unsubstituted with -F, -Cl, -Br or -I; or a heteroaryl group having 2 to 20 carbon atoms, substituted or unsubstituted with -F, -Cl, -Br or -I, At least one of the above R1 and R2 is substituted with one or more fluorine (F).

3. In paragraph 2, In the above chemical formula 1, An electrolyte wherein R1 and R2 are independently an alkyl group having 1 to 10 carbon atoms, which is unsubstituted or substituted with -F.

4. In paragraph 1, The above fluorine-containing linear ester is an electrolyte represented by the following chemical formula 1-1: <Chemical Formula 1-1> In the above chemical formula 1-1, L1 is an alkylene group having 1 to 10 carbon atoms, R3 is an alkyl group having 1 to 10 carbon atoms.

5. In paragraph 1, An electrolyte wherein the content of the fluorine-containing linear ester is 10 wt% or more based on the total weight of the solvent.

6. In paragraph 1, The above fluorine-containing linear ester is an electrolyte that satisfies the following conditions 1 and 2: Condition 1 | E Li-s | > 1.8 eV Among the above conditions 1, |E Li-s | is the absolute value of the interaction energy between the fluorine-containing linear ester and lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, Condition 2 | E PF6-s | < 0.1 eV |E PF6-s | is measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, and the fluorine-containing linear ester and PF6 - It is the absolute value of the interaction energy between them.

7. In paragraph 1, An electrolyte wherein the solvent further comprises an asymmetric cyclic carbonate, a linear carbonate or a combination thereof.

8. In paragraph 7, The above asymmetric cyclic carbonate is an electrolyte represented by the following chemical formula 2: <Chemical Formula 2> In the above chemical formula 2, R 21 Inland R 24 are independently hydrogen, deuterium (-D), -F, -Cl, -Br or -I; an alkyl group having 1 to 10 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I; an aryl group having 6 to 20 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I; or a heteroaryl group having 2 to 20 carbon atoms substituted or unsubstituted with -F, -Cl, -Br or -I, R 21 and R 22 The combination of R 23 and R 24 It is different from the combination of .

9. In paragraph 8, In the above chemical formula 2, R 21 Inland R 24 An electrolyte in which each independently represents hydrogen or an alkyl group having 1 to 10 carbon atoms.

10. In paragraph 7, An electrolyte wherein the content of the asymmetric cyclic carbonate is 20 wt% or less based on the total weight of the solvent.

11. In paragraph 1, The first lithium salt and the second lithium salt are electrolytes that satisfy the following equation 1: <Formula 1> |And Li-A1 | < |E Li-A2 | In equation 1, |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, |E Li-A2 | is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

12. In paragraph 1, The first lithium salt and the second lithium salt are electrolytes that satisfy the following equation 2: <Formula 2> |E Li-A1 - E Li-A2 | > 0.3 eV In equation 2, |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level, |E Li-A2 | is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

13. In paragraph 1, The above first lithium salt satisfies the following equation 3, The second lithium salt is an electrolyte that satisfies the following equation 4: <Formula 3> |E Li-A1 | ≤ 5.55 eV In equation 3, |E Li-A1 | is the absolute value of the interaction energy between the first anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level. <Formula 4> |E Li-A2 | > 5.55 eV In equation 4, |E Li-A2 | is the absolute value of the interaction energy between the second anion and the lithium ion, measured using the DFT method of the Gaussian program with structure optimization at the M062X / 6-311+G** level.

14. In paragraph 1, An electrolyte wherein the first lithium salt comprises LiDFOP (lithium difluoro(bisoxalato)phosphate), LiBOB (lithium bis(oxalato)borate), LiFMDFB (lithium fluoromalonato(difluoro)borate), LiTDI (lithium 2-trifluoromethyl-4,5-dicyanoimidazole), LiBSO4F2, LiPF6, LiDFOB (lithium difluoro(oxalate)borate), or any combination thereof.

15. In paragraph 1, An electrolyte wherein the second lithium salt comprises LiPOF4, LiPO2F2, LiBF4, LiCF3SO3, LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiFSI (lithium bis(fluorosulfonyl)imide), LiDCTA (lithium 4,5-dicyano-1,2,3-triazolate), or any combination thereof.

16. Anode; cathode; and A lithium battery, comprising an electrolyte according to claims 1 to 15, disposed between the positive electrode and the negative electrode.

17. In paragraph 16, A lithium battery wherein the electrolyte is in a liquid or gel form.

18. In paragraph 16, The above positive electrode includes a positive electrode current collector; and a positive electrode active material layer, A lithium battery, wherein the negative electrode comprises only a negative electrode current collector.

19. In paragraph 16, The above positive electrode includes a positive electrode current collector; and a positive electrode active material layer, The negative electrode includes a negative current collector; and a metal layer disposed between the negative current collector and the electrolyte, A lithium battery, wherein the metal layer comprises lithium metal or a lithium alloy.

20. In paragraph 16, It is placed between the cathode and the electrolyte, A lithium battery further comprising a protective layer derived from the first lithium salt or the second lithium salt.

Citation Information

Patent Citations

  • Low-temperature lithium ion electrolyte and lithium ion battery prepared from same

    CN110943251A

  • Organic electrolyte for lithium secondary battery and lithium secondary battery comprising same

    EP1498979B1

  • Nonaqueous electrolyte and lithium secondary battery containing the same

    KR1020150048499A

  • Cloud computing system for academy maganament

    KR1020240130917A

  • Electrolytes and separators for lithium metal batteries

    US20220140394A1