Highly stretchable, self-healable, transparent and solid-state poly(ionic liquid) filler for high-performance dielectric elastomer actuators

The development of a high dielectric constant, stretchable, and self-healable solid-state PIL filler addresses the challenges of actuation strain and filler leakage in DEAs, improving actuation performance and durability by enhancing adhesion and preventing leakage.

WO2024205492A1PCT designated stage expired Publication Date: 2024-10-03NANYANG TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/SG2024/050169
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Dielectric elastomer actuators (DEAs) face challenges in achieving high actuation strain while maintaining low Young's modulus and preventing filler leakage due to the use of soft liquid fillers, which often result in dielectric breakdown.

Method used

A soft and stretchable solid-state poly(ionic liquid) (PIL) filler with a high dielectric constant is developed by regulating the amount of acetonitrile in the precursor solution, enhancing adhesion with the elastomer matrix and enabling self-healability, thus preventing filler leakage and improving actuation performance.

Benefits of technology

The PIL filler increases area strain in planar DEAs and bending angle and blocking force in unimorph DEAs, while maintaining a low Young's modulus and preventing filler leakage, thereby enhancing the overall actuation performance and durability of DEAs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SG2024050169_03102024_PF_FP_ABST
    Figure SG2024050169_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed herein is a poly (io n ic liquid) (PIL) film, comprising from 40 to 60 wt% of a crosslinked polymer of formula I and from 40-60 wt% of 1 -hexyl-3-vinylimidazolium BF4 in monomeric form, wherein the PIL film has the following properties: a glass transition temperature of from -100 to -25 °C; a stretchability of from 150 to 500% of its original dimension; and a Young's modulus of from 0.05 to 0.3 MPa. Also disclosed herein are a composite elastomeric material suitable for use in a dielectric elastomer actuator (DEA), and a DEA device.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] HIGHLY STRETCHABLE, SELF-HEALABLE, TRANSPARENT AND SOLID-STATE POLY(IONIC LIQUID) FILLER FOR HIGH-PERFORMANCE DIELECTRIC ELASTOMER ACTUATORS

[0002] Field of Invention

[0003] The current invention relates to a poly(ionic liquid) (PIL) film, a dielectric elastomer actuator (DEA) device using said film and method of manufacturing these materials.

[0004] Background

[0005] The listing or discussion of a prior-published document in this specification should not necessarily be taken as an acknowledgement that the document is part of the state of the art or is common general knowledge.

[0006] Soft actuators enable multi-responsiveness, gentle manipulation, and dexterous mobility, thereby showing huge potential in applications such as soft robotics, human-machine interactions, and wearables. Among various soft actuators, dielectric elastomer actuators (DEAs) are promising, as they possess high actuation strains, quick response, large energy densities, and low weight. In a typical device, DEAs are comprised of a soft dielectric elastomer sandwiched between two compliant electrodes. Actuation is realized when an electric field is applied due to the generation of a Maxwell pressure that compresses the elastomer. To generate a larger Maxwell pressure, various methods like the introduction of fillers with high dielectric constant, and chemical modification of elastomer backbone have been introduced. While incorporating solid conductive or ceramic fillers (such as graphene, carbon nanotube, BaTiOs, TiC>2, etc.) can readily enhance the dielectric constant of the materials, the Young’s modulus of the composite is increased concurrently, constraining the actuation strain. In contrast, soft liquid fillers such as liquid metal and ionic liquid can effectively solve this problem, simultaneously realizing materials with high dielectric constant and low Young’s modulus. However, soft liquid fillers possess a tendency of filler leakage due to their fluidic nature, especially under high deformations, which leads to a higher likelihood of dielectric breakdown. Therefore, an ideal filler should exhibit high dielectric constants, low Young’s modulus, and be in a solid state.

[0007] To combine the high static dielectric constant of ionic liquids and the desirable mechanical features of polymers, ionic liquid can be polymerized to form a poly(ionic liquid) (PIL) and be used as a filler for DEAs. This is an unprecedented concept for DEAs, even though PILs have been actively studied for other applications, their use in DEA as filler materials have not been explored. As DEAs need to withstand high actuation strain repeatedly, it is critical to ensure that PILs are stretchable. To endow PILs with stretchability, different synthetic strategies have been deployed, such as grafting PIL on stretchable matrix like PDMS, copolymerization with acrylamide (AAm), acrylic acid, n-butyl acrylate, etc. for a stretchable network, and using hyperbranched crosslinker. Despite this, the addition of other components compromises the low Young’s modulus and high dielectric constant of PILs. Besides, excessive IL used to dissolve hyperbranched crosslinker could cause a weak interface between PIL and elastomer matrix, which induces defects under a high strain.

[0008] Therefore, there exists a need for new soft and stretchable solid-state PIL fillers with high dielectric constant for enhanced actuation performance of DEAs.

[0009] Summary of Invention

[0010] It has been surprisingly found that a soft and stretchable solid-state PIL filler with high dielectric constant can be prepared by regulating the amount of acetonitrile in the precursor solution containing optimized monomer, crosslinker and photoinitiator. This PIL filler can enhance the dielectric constant while reducing the Young’s modulus of elastomer, enhancing actuation performance of DEAs. Notably, the excellent adhesion of PIL filler realizes a strong interface with elastomer matrix (e g. 3M VHB tapes) for durable actuation without filler leakage, while the fast self-healability of PIL filler endows DEAs with recoverability. Thereby, when introducing PIL fillers, planar DEAs show greatly increased area strain at the same electrical field, and bending DEAs achieve increased bending angle and blocking force.

[0011] Aspects and embodiments of the invention are provided in the following numbered clauses.

[0012] 1. A poly(ionic liquid) (PIL) film, comprising: from 40 to 60 wt% of a crosslinked polymer of formula I having the repeating unit:

[0013] where: x represents monomeric repeating unit; y represents a crosslinking repeating unit; z represents a repeating unit for ethylene glycol, where the total Mn of the repeating unit y is from 500 to 1 ,000 Daltons ; and from 40 to 60 wt% of 1-hexyl-3-vinylimidazolium BF4 in monomeric form, wherein the PIL film has the following properties: a glass transition temperature of from -100 to -25 °C; a stretchability of from 150 to 500% of its original dimension; and a Young’s modulus of from 0.05 to 0.3 MPa.

[0014] 2. The PIL film according to Clause 1 , wherein the PIL film has an adhesion of from 8 to 25 N, such as from 10 to 15 N, such as about 11 N in a probe tack test.

[0015] 3. The PIL film according to Clause 1 or Clause 2, wherein the crosslinked polymer of formula I and the 1-hexyl-3-vinylimidazolium BF4 monomer are present in approximately equal amounts.

[0016] 4. The PIL film according to any one of the preceding clauses, wherein the PIL film has one or more of the following properties: (a) a glass transition temperature of from -75 to -40 °C, such as about -52.1 °C;

[0017] (b) a stretchability of from 200 to 400%, such as about 300%, of its original dimension;

[0018] (c) a Young’s modulus of from 0.07 to 0.2 MPa, such as about 0.11 MPa; and

[0019] (d) an ability to self-heal following damage within 1 minute of the damage occurring.

[0020] 5. The PIL film according to any one of the preceding clauses, wherein the PIL film exhibits a self-healing efficiency of from 60 to 80%, such as about 70%.

[0021] 6. The PIL film according to any one of the preceding clauses, wherein the total Mn of the repeating unit y is about 700 Daltons.

[0022] 7. A composite elastomeric material suitable for use in a dielectric elastomer actuator (DEA), the composite elastomeric material comprising: a poly(ionic liquid) (PIL) film layer as described in any one of Clauses 1 to 6; and two dielectric elastomer layers, wherein the PIL film layer is sandwiched between and encapsulated by the two dielectric elastomer layers.

[0023] 8. The composite elastomeric material according to Clause 7, wherein the elastomeric material has an effective dielectric constant of from 10 to 40 at 1 kHz, such as from 14 to 20 at 1 kHz, such as about 16.4 at 1 kHz.

[0024] 9. The composite elastomeric material according to Clause 7 or Clause 8, wherein the thickness of each of the two dielectric elastomer layers is from several to 500 pm, such as about 300 pm.

[0025] 10. The composite elastomeric material according to any one of Clauses 7 to 9, wherein the two dielectric elastomer layers are formed from one or more of an acrylic foam adhesive material and a polydimethylsiloxane (PDMS) material.

[0026] 11. A dielectric elastomer actuator (DEA) device, comprising: a composite elastomeric material as described in any one of Clauses 7 to 10, having a first surface and a second surface; a first electrode and a second electrode attached to the first and second surfaces, respectively, of the composite elastomeric material; and at least one substrate layer attached to at least one of the first and second surfaces of the composite elastomeric material and / or at least one of the first and second electrodes. 12. The DEA device according to Clause 11 , wherein the DEA device is a bending DEA device wherein: the first and second electrodes are in the form of a first electrode layer and a second electrode layer, which substantially cover the first and second surfaces; and the at least one substrate layer is a passive layer attached to one of the first or second electrode layers.

[0027] 13. The DEA device according to Clause 12, wherein the passive layer is a polymeric tape or an electroluminescence layer with an elastic modulus that is greater than that of the composite elastomeric material.

[0028] 14. The DEA device according to Clause 13, wherein the electroluminescence layer comprises a PDMS polymeric matrix and ZnS:Cu particles homogeneously distributed throughout the PDMS polymeric matrix, optionally wherein the electroluminescence layer has a first surface attached to the first electrode layer or the second electrode layer and a second surface attached to a third electrode layer.

[0029] 15. The DEA device according to any one of Clauses 12 to 14, wherein the electrode layers are formed from a transparent and compliant electrode material, optionally wherein the electrode layers are formed from silver nanowires.

[0030] 16. The DEA device according to Clause 11 , wherein the DEA device is a planar DEA device, wherein: the at least one substrate layer is in the form of a first frame and a second frame, the first frame being attached to the first surface and the second frame being attached to the second surface, respectively, of the composite elastomeric material; the dielectric elastomer layers of the composite elastomeric material are in a biaxially 0 to 300% by 0 to 300% stretched conformation, such as a biaxially 200% by 200% stretched conformation and the first and second electrodes partly cover the first and second surfaces, respectively, of the composite elastomeric material.

[0031] 17. The DEA device according to Clause 16, wherein the first and second frames each have an aperture that corresponds at least to the size of the first and second electrodes. 18. The DEA device according to Clause 16 or Clause 17, wherein the first and second electrodes are formed from carbon grease.

[0032] Drawings

[0033] Fig. 1 depicts (a) molecular structure of raw materials of PILs. (b) Fourier Transform Infrared (FTIR) spectra of raw materials of PILs. (c) FTIR spectra of 1-hexyl-3-vinylimidazolium BF4 (HVIM BF4), different PILs and acetonitrile, (d) Molecular structure of PIL filler.

[0034] Fig. 2 depicts (a) schematic diagram of PILs preparation with different solvent amount in precursors, (b) FTIR spectra of PILs and their monomer HVIM BF4. (c) Swelling ratio of PILs equilibrated in the acetonitrile with respect to different PILs (error bar: standard deviations). PIL-150 is absent due to its dissolution, (d) Frequency-dependent storage modulus (G1) and loss modulus (G”) of PILs. PIL-0 is too rigid to be measured by the same probe of rheometer.

[0035] Fig. 3 depicts (a, b, c) differential scanning calorimetry (DSC) thermograms of different PILs. (d) Thermogravimetric analysis (TGA) of different PILs.

[0036] Fig. 4 depicts mechanical and adhesive properties of different PILs and self-healing of PIL- 100. (a) Tensile stress-strain curves of PIL-0, PIL-50, PIL-100 at a loading rate of 100 mm / min. Inset is the clearly visible stress-strain curve of PIL-100. (b) Young’s modulus and strain at break of PIL-0, PIL-50, PIL-100 (error bars: standard deviations), (c) Adhesion forcedisplacement curves of PIL-50, PIL-100 measured by a probe tack test. Upper inset with red frame shows no connection between PIL-50 and the probe after the departure. Lower inset with blue frame demonstrates residue of PIL-100 remains between the surface of the probe and PIL-100 after the departure, (d) Cyclic stress-strain curves of PIL-100 to 100% strain for 10 continuous cycles, (e) Cyclic stress-strain curves and its subsequent recovery cycle after resting for 2 min of PIL-100. (f) Healing efficiency of PIL-100 for 5 cycles, (g) The cut, heal, stretch state of PIL-100 to illustrate the self-healability.

[0037] Fig. 5 depicts (a) frequency-dependent storage modulus (G’) and loss modulus (G”) of PIL- 75, PIL-100 and PIL-125. PIL-125 is more liquid-like than PIL-100 while PIL-75 is more solidlike. (b) Tensile stress-strain curves of PIL-75 at a loading rate of 100 mm / min.

[0038] Fig. 6 depicts a schematic representation of a typical tack adhesion measurement apparatus during (a) contact and (b) separation steps. Fig. 7 depicts cyclic stress-strain curves of PIL-100 to various strains of 25%, 50%, 75% and 100%.

[0039] Fig. 8 depicts stress-strain curves of PIL-100 for 5 cycles of self-healing.

[0040] Fig. 9 depicts the mechanical and dielectric properties of C-VHB, where PIL filler is PIL with optimal solvent amount in the precursor, namely PIL-100. (a) Adhesion force between VHB and PIL-100 measured by a shear test, with a schematic representation, (b) Digital photograph of PIL-100 being pulled up while adhering to the surface of VHB, showing a cohesive failure, (c) Tensile stress-strain curves of VHB and C-VHB at a loading rate of 100 mm / min. (d) Cyclic stress-strain curves of VHB and C-VHB to 100% strain at 100 mm / min for 10 continuous cycles, (e, f) Dielectric constant and dielectric loss of VHB and C-VHB at different frequencies measured by dielectric spectroscopy.

[0041] Fig. 10 depicts (a) photograph of C-VHB at 200% strain showing a great contact between VHB and PIL filler, (b) Photograph of C-VHB at 400% strain showing delamination.

[0042] Fig. 11 depicts (a) schematic of the fabrication of C-PDMS. (b) Dielectric constant of PDMS and C-PDMS. (c) Cyclic actuation of bending DEAs with PDMS at 14.3 V / pm and with C- PDMS at 5.8 V / pm and 100 Hz.

[0043] Fig. 12 depicts (a) schematic representation of bending DEAs in the off and on state, (b) Schematic representation of the measurement of bending angle, (c) Dependence of bending angle on time of voltage applied (12 V / pm for VHB, 12.6 V / pm for C-VHB), which shows equilibrium state after 3 seconds.

[0044] Fig. 13 depicts the performance of DEAs with C-VHB. (a) Schematic of the configuration of a planar DEA with area strain, (b) Dielectric constant of DEAs with different filler loading of PIL precursor over the frequency range of 40 Hz to 10 kHz. (c) Actuated area of DEAs with different filler loading of PIL precursor. Insets are the photographs of electrode areas of DEAs with 200 pL PIL precursor at 0 (Off state) and 17 V / pm (On state), respectively, (d) Schematic of the configuration of an unimorph bending DEA. (e) Bending angles of DEAs with VHB and C-VHB. Inset is the overlapping digital photograph of DEA with C-VHB at 0 V / pm (Off state) and 12.6 V / pm (On state), (f) Bending angles of DEAs with C-VHB and recovered C-VHB.

[0045] Fig. 14 depicts a schematic representation of DEA with area strain. Fig. 15 depicts dielectric loss of C-VHB with different loadings of PIL precursor at different frequencies measured by dielectric spectroscopy.

[0046] Fig. 16 depicts (a) actuated area of DEA with VHB. (b) Weibull distribution of dielectric breakdown strength of VHB and C-VHB.

[0047] Fig. 17 depicts the blocking forces of DEAs with VHB and C-VHB.

[0048] Fig. 18 depicts the original, cut, contact state of C-VHB to illustrate the recoverability.

[0049] Fig. 19 depicts (a) adhesion forces between PIL-100 and VHB or PDMS, measured by shear tests, (b) Digital photograph of PIL-100 being pulled up showing no cohesive failure.

[0050] Fig. 20 depicts the performance of a light emissive bending DEA. (a) Schematic of the configuration of the integrated bending DEA and alternating-current electroluminescent (ACEL) layer, where the DEA consists of C-VHB and the ACEL layer consists of PDMS+ZnS:Cu. (b) Young’s modulus difference of VHB, PDMS, PDMS and PDMS+ZnS:Cu. Error bar: standard deviations, (c) Ultraviolet-visible (UV-Vis) spectrum of VHB, PIL and C- VHB. Inset is the digital photograph of C-VHB above flowers. Scale bar: 1 cm. (d) The emission spectrum of the light emissive bending DEA from top and bottom view, respectively. Top view refers to the C-VHB side and bottom view refers to the EL layer side, (e) Digital photographs of light emissive bending DEA showing simultaneous actuation and light emission. The actuation is controlled by voltage on and off.

[0051] Fig. 21 depicts the bending angles of the integrated bending DEA and ACEL, where ACEL functions as a passive layer.

[0052] Fig. 22 depicts the emission spectrum of the light emissive bending DEA at initial state and after 1000 cycles of bending.

[0053] Description

[0054] It has been surprisingly found that by simply regulating the solvent amount during the polymerization of precursors, the mechanical properties of PILs can be tuned over a wide range. The PILs disclosed herein can display a high stretchability (e.g. -300%), low Young’s modulus (e.g. 0.11 MPa), strong adhesion ability, fast self-healing (within 1 min), recoverability, and a high transparency of -99%, thereby becoming an outstanding candidate as a filler for dielectric elastomer actuators (DEAs). By introducing the PIL filler to a suitable dielectric elastomer (e.g. a VHB elastomer), the dielectric constant can be increased from 4.7 to 16.4 at 1 kHz and the Young’s modulus decreased to 0.21 MPa. For planar DEAs, a composite material using the PILs disclosed herein can show an area strain of 137% at an electric field of 17 V / pm, surpassing most DEAs with fillers at similar electric fields. Also, a unimorph DEA using a composite material incorporating a PIL of the current invention demonstrated a bending angle of 38.6° at 12.6 V / pm, which is over twice that of the pristine dielectric elastomer chosen for the example (VHB). Meanwhile, the blocking force of the bending DEA increased from ~0.2 mN to 1.45 mN at 12.6 V / pm with the addition of PIL filler. Importantly, the excellent adhesion and fast self-healability of a PIL disclosed herein (e g. PIL-100) prevent DEAs from filler leakage problems and enables the recovery of actuation performance after damage. Finally, a bending DEA integrated with an ACEL layer is also disclosed herein and demonstrates simultaneous dynamic motion and light emission, which is attractive for interactive displays, camouflage wearable electronics, soft robotics, and human-machine interfaces.

[0055] In a first aspect of the invention, there is provided a poly(ionic liquid) (PIL) film, comprising: from 40 to 60 wt% of a crosslinked polymer of formula I having the repeating unit: where: x represents monomeric repeating unit; y represents a crosslinking repeating unit; z represents a repeating unit for ethylene glycol, where the total Mn of the repeating unit y is from 500 to 1 ,000 Daltons ; and from 40 to 60 wt% of 1-hexyl-3-vinylimidazolium BF4 in monomeric form, wherein the PI L film has the following properties: a glass transition temperature of from -100 to -25 °C; a stretchability of from 150 to 500% of its original dimension; and a Young’s modulus of from 0.05 to 0.3 MPa.

[0056] In embodiments herein, the word “comprising” may be interpreted as requiring the features mentioned, but not limiting the presence of other features. Alternatively, the word “comprising” may also relate to the situation where only the components / features listed are intended to be present (e.g. the word “comprising” may be replaced by the phrases “consists of” or “consists essentially of”). It is explicitly contemplated that both the broader and narrower interpretations can be applied to all aspects and embodiments of the present invention. In other words, the word “comprising” and synonyms thereof may be replaced by the phrase “consisting of’ or the phrase “consists essentially of’ or synonyms thereof and vice versa.

[0057] The phrase, “consists essentially of’ and its pseudonyms may be interpreted herein to refer to a material where minor impurities may be present. For example, the material may be greater than or equal to 90% pure, such as greater than 95% pure, such as greater than 97% pure, such as greater than 99% pure, such as greater than 99.9% pure, such as greater than 99.99% pure, such as greater than 99.999% pure, such as 100% pure.

[0058] The PI L films disclosed herein may have any suitable adhesiveness. For example, the PI L film may have an adhesion of from 8 to 25 N, such as from 10 to 15 N, such as about 11 N in a probe tack test. Details of the probe tack test may be found in the examples section below.

[0059] As will be appreciated, the relative amounts of the crosslinked polymer of formula I and the 1- hexyl-3-vinylimidazolium BF4 monomer are chosen to add up to 100%. Thus, if there is 60% of the crosslinked polymer of formula I, then there will be 40% of the 1-hexyl-3- vinylimidazolium BF4 monomer, etc. In certain embodiments, the crosslinked polymer of formula I and the 1-hexyl-3-vinylimidazolium BF4 monomer may be present in approximately equal amounts (i.e. about 50% ±1% for each component, such as ±0.5% for each component, such as ±0.1% for each component. The PI L films of the current invention may have particularly good properties. For example, the PIL films of the current invention may have one or more of the following properties:

[0060] (a) a glass transition temperature of from -75 to -40 °C, such as about -52.1 °C;

[0061] (b) a stretchability of from 200 to 400%, such as about 300%, of its original dimension;

[0062] (c) a Young’s modulus of from 0.07 to 0.2 MPa, such as about 0.11 MPa; and

[0063] (d) an ability to self-heal following damage within 1 minute of the damage occurring.

[0064] As noted above, the PIL films of the current invention may display a self-healing ability, and in particular a fast self-healing ability, where they are able to self-heal within 1 minute of taking damage. In addition, the PIL films disclosed herein exhibit a self-healing efficiency of from 60 to 80%, such as about 70%.

[0065] As noted above, the PIL films include a crosslinked polymer of formula I where the repeating unit y may have a Mn that is from 500 to 1 ,000 Daltons. In particular embodiments of the invention, the total Mn of the repeating unit y may be about 700 Daltons.

[0066] In a second aspect of the invention, there is provided a composite elastomeric material suitable for use in a dielectric elastomer actuator (DEA), the composite elastomeric material comprising: a poly(ionic liquid) (PIL) film layer as described hereinbefore; and two dielectric elastomer layers, wherein the PIL film layer is sandwiched between and encapsulated by the two dielectric elastomer layers.

[0067] The composite elastomeric material may have any suitable effective dielectric constant. For example, a suitable effective dielectric constant may be from 10 to 40 at 1 kHz, such as from 14 to 20 at 1 kHz, such as about 16.4 at 1 kHz.

[0068] The thickness of each of the two dielectric elastomer layers may be any suitable thickness. For example, the thickness of each of the two dielectric elastomer layers may be from several pm to 500 pm, such as from 100 pm to 400 pm, such as about 300 pm.

[0069] The two dielectric elastomer layers may be formed from any suitable dielectric material that has an adhesive quality. For example, the two dielectric elastomer layers may be formed from one or more of an acrylic foam adhesive material and a polydimethylsiloxane (PDMS) material. In a third aspect of the invention, there is provided a dielectric elastomer actuator (DEA) device, comprising: a composite elastomeric material as described hereinbefore, having a first surface and a second surface; a first electrode and a second electrode attached to the first and second surfaces, respectively, of the composite elastomeric material; and at least one substrate layer attached to at least one of the first and second surfaces of the composite elastomeric material and / or at least one of the first and second electrodes.

[0070] In embodiments of the invention, the DEA device may be a bending DEA device wherein: the first and second electrodes are in the form of a first electrode layer and a second electrode layer, which substantially cover the first and second surfaces; and the at least one substrate layer is a passive layer attached to one of the first or second electrode layers.

[0071] Such DEA devices may be suitable for use as a bending actuator. In particular, there may be a single substrate layer that is attached to the first or second surface of the composite elastomeric material and / or to the first or second electrode.

[0072] In embodiments of the invention, the passive layer may be a polymeric tape or an electroluminescence layer with an elastic modulus that is greater than that of the composite elastomeric material. In embodiments of the invention where an electroluminescence layer is present, the electroluminescence layer may comprise a PDMS polymeric matrix and ZnS:Cu particles homogeneously distributed throughout the PDMS polymeric matrix. In particular embodiments, the electroluminescence layer may have a first surface attached to the first electrode layer or the second electrode layer and a second surface attached to a third electrode layer.

[0073] The electrode layers may be formed from any suitable transparent and compliant electrode material. For example, the electrode layers may be formed from silver nanowires.

[0074] In certain embodiments of the invention, the DEA device may be a planar DEA device, wherein: the at least one substrate layer is in the form of a first frame and a second frame, the first frame being attached to the first surface and the second frame being attached to the second surface, respectively, of the composite elastomeric material; the dielectric elastomer layers of the composite elastomeric material are in a biaxially 0 to 300% by 0 to 300% stretched conformation, such as a biaxially 200% by 200% stretched conformation; and the first and second electrodes partly cover the first and second surfaces, respectively, of the composite elastomeric material. In such embodiments, the first and second frames may each have an aperture that corresponds at least to the size of the first and second electrodes. Any suitable material may be used as the electrodes. For example, the electrodes may be formed from carbon grease.

[0075] As will be appreciated, the present disclosure provides the following advantages and improvement over existing materials: a. solid state or immobilized; b. high stretchability; c. low Young’s modulus; d. high static dielectric constant; e. strong adhesion; and f. fast self-healing.

[0076] Further aspects and embodiments of the invention are summarised in the below numbered clauses.

[0077] 1. Preparation of PIL a. The monomer 1-Hexyl-3-vinylimidazolium BF4 (HVIM BF4) was synthesized by two steps. Firstly, 1-bromohexane (52.8 g, 0.320 mol) was added dropwise into 1-vinylimidazole (30.0 g, 0.319 mol) over a period of 2 hours and stirred at 35 °C for 3 days. The resulting viscous liquid was washed with ether three times and dried in vacuo to yield a pale-yellow liquid. Secondly, HVIM Br obtained in the first step was mixed with NaBF4 (42.0 g, 0.382 mol) in water and stirred at 35 °C for 2 days. Afterwards, ethyl acetate was used to extract the product which are then dried in vacuo to get pure HVIM BF4. b. The PIL precursor was prepared by mixing the monomer HVIM BF4 (1000 mg), the crosslinker poly(ethylene glycol) diacrylate (PEGDA, Mn700, 20 mg) and the photo initiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TPO, 5 mg) were mixed together. Then, the mixture was mixed with acetonitrile of the same weight with monomer, namely 100 wt.%, though the acetonitrile may also be used in an amount of from 75 to 125 wt.%. The obtained solution was sonicated for 15 minutes as PIL precursor. c. To obtain PIL with fixed shape, the precursor was drop casted into frames or molds and polymerized by ultraviolet light (395 nm) for 1 min, and then heated at 80 °C in an oven for 1 h to remove the acetonitrile.

[0078] 2. Fabrication of planar DEAs a. For DEA fabrication with PIL filler, 200 pL of PIL precursor was drop-casted on the center of a layer of prestretched 3M VHB 4905 tape (biaxially 200% by 200%) with a diameter of 3 cm and thickness of 55 pm, and then cured and heated to obtain a solid-state PIL membrane directly on VHB. After cooling down to the room temperature, another layer of prestretched 3M VHB 4905 tape (biaxially 200% by 200%) was attached or sticked on the top of the PIL membrane to seal it between the two layers of VHB tapes and the composite elastomer C-VHB with the thickness of -300 pm was obtained. As a control, the blank DEA is using a layer of prestretched 3M VHB 4905 tape (biaxially 200% by 200%) with the same thickness of -55 pm and mounting it on the circular frame (inner diameter: 3 cm). b. Compliant carbon grease electrodes were coated onto the top and bottom of the composite elastomer (and similarly on the control blank DEA) with a circular overlapping region with a diameter of 1 cm and two connecting lines to silver tapes were applied to electrically connect to a high voltage power source. c. The obtained DEA could show an area strain under the high voltage. The area covered by the overlapping electrodes was recorded by a video camera and then calculated by the software Image J. The voltage applied on the device increased by 500 V until the breakdown voltage of DEAs. Area strains (AA) were calculated using the equation: AA = (Ar - Ao) / Ao x 100%, where Af is the area under different voltages and Ao is the initial area of the overlapping region.

[0079] 3. Fabrication of bending DEAs a. For bending DEAs, VHB is not prestretched and no frame is needed. To lower the thickness of composite elastomer for bending DEAs, 3M VHB F9473PC tape with a thickness of 260 pm was applied. The composite elastomer of bending DEA was formed following the same steps of planar DEAs. A piece of 3M VHB F9473PC tape (3 x 1 .2 cm2) with a central rectangular hole (3 x 1 cm2) was sticked on an intact layer of 3M VHB F9473PC tape (3 x 1.2 cm2). Then, 150 pL of PIL precursor was dropped in the hole and then cured and heated to form PIL filler. Another layer of 3M VHB F9473PC tape (3 * 1.2 cm2) was sticked to seal the PIL filler between the two layers of VHB tapes. The thickness of corresponding C-VHB is -0.8 mm. b. Silver nanowire (AgNW) electrodes were spray coated on the top and bottom of the composite elastomer with a rectangular overlapping region (2 * 1 cm2) and the top of two narrow silver tapes to strengthen the connection with them. A 3M Scotch Magic Tape was cut to fully cover the bottom of the elastomer and used as the passive layer. The silver tapes were connected to a high voltage power source to enable the deformation of the composite elastomer. The state of bending DEAs was recorded by a video camera. The angles between the initial state and deformed state were calculated by the software Image J. The voltage applied on the device increased by 1 kV.

[0080] Further aspects and embodiments of the invention will now be discussed by reference to the following non-limiting examples.

[0081] Examples

[0082] Materials

[0083] 1-vinylimizadole (>98%), and 1-bromohexane (>98%) were purchased from TCI Chemicals. Polyethylene glycol) diacrylate (PEGDA700, Mn700), diphenyl(2,4,6- trimethylbenzoyl)phosphine oxide (TPO, 97%), sodium tetrafluoroborate (NaBF4) were purchased from Sigma-Aldrich. Carbon grease was procured from Nanjing Xilite Adhesive Co. Ltd. Commercial silver nanowire (AgNW) was purchased from Xfnano Technology with diameters of 50 nm and length of 100 ~ 200 mm. The AgNW solution in isopropyl alcohol (I PA) was diluted to a concentration of 0.5 mg / mL before use.

[0084] 1H NMR spectrum was obtained from Bruker Avance DPX-400 (400 MHz) Fourier- transform NMR spectrometer at 298 K and calibrated against tetramethylsilane, Si(CH3)4.

[0085] Fourier Transform Infrared (FTIR) spectroscopy

[0086] All FTIR spectra were collected in the wavenumber range of 4000-600 erm1by a PerkinElmer FTIR Frontier spectrometer with attenuated total reflection (ATR) accessory, which average over 16 scans at a resolution of 1 erm1.

[0087] TGA

[0088] TGA was done through ramping from room temperature to 700 °C at 10 °C mim1to determine the thermal stability of PILs. DSC

[0089] DSC was applied to determine the Tgof different PILs by cooling / heating at 10 °C min1.

[0090] General procedure for mechanical test

[0091] All the samples for mechanical tests were cut into rectangular shape with a length of ~20 mm, a width of ~10 mm. The thickness of independent PIL-100, VHB 4905, C-VHB is ~0.7, 0.5, -1.25 mm, respectively. The stress-strain curves were obtained with MTS criterion model 42 (MTS Systems Corporation, Eden Prairie, MN, USA) static mechanical tester at a strain rate of 100 mm / min. Three independent samples for each PIL were measured to calculate the standard deviation. Young’s modulus was obtained from the slopes of tensile curves from 0% to 5% strain.

[0092] Example 1. Preparation of PILs

[0093] In the present disclosure, we report a soft and stretchable solid-state PIL filler with high dielectric constant for enhanced actuation performance of DEAs. PILs were prepared by photopolymerization of 1-hexyl-3-vinylimidazolium BF4(HVIM BF4) with varied acetonitrile amounts in the precursor solution, leading to different cross-link densities and a wide range of mechanical properties.

[0094] Preparation of monomers of PIL

[0095] The monomer 1-Hexyl-3-vinylimidazolium BF4(HVIM BF4) was synthesized by two steps. Firstly, 1-bromohexane (52.8 g, 0.320 mol) was added dropwise into 1-vinylimidazole (30.0 g, 0.319 mol) over a period of 2 hours and stirred at 35 °C for 3 days. The resulting viscous liquid was washed with ether three times and dried in vacuo to yield a pale-yellow liquid. Secondly, HVIM Br obtained in the first step was mixed with NaBF4(42.0 g, 0.382 mol) in water and stirred at 35 °C for 2 days. Afterwards, ethyl acetate was used to extract the product which are then dried in vacuo to get pure HVIM BF4.

[0096] 1H NMR (400 MHz, DMSO-cfe, 298K, 6): 9.42 (s, 1 H); 8.16 (t, 1 H); 7.90 (t, 1 H); 7.26 (q, 1 H); 5.93 (dd, 1 H); 5.42 (dd, 1 H); 4.18 (t, 2 H); 1.82 (quintet, 2 H); 1.27 (m, 6 H); 0.86 (t, 3 H).

[0097] Preparation of PILs

[0098] The monomer HVIM BF4(1000 mg), 2 wt.% of the crosslinker poly(ethylene glycol) diacrylate (PEGDA700, Mn700, 20 mg) and 0.5 wt.% of the photo initiator diphenyl(2,4,6- trimethylbenzoyl)phosphine oxide (TPO, 5 mg) were mixed together. Then, the mixture was mixed with different amount of the solvent (acetonitrile) such as 0, 50, 100, 150 wt.%, respectively. The structure and FTIR spectra of raw materials are shown in Fig. 1. The obtained four solutions were sonicated for 15 minutes by a Digital Ultrasonic Cleaner (DIGITAL PRO). The sufficiently sonicated solutions are the precursors of PI L with four different amounts of solvent. To obtain PI L with fixed shape, the precursors were dropped into frames or molds respectively and polymerized by ultraviolet light (395 nm) for 1 min, and then heated at 80 °C in an oven for 1 h to remove the acetonitrile solvent. The PIL were named as PIL-X as X refers to the weight percentage of the solvent to monomer in the precursors.

[0099] Example 2. Characterization of stretchable PIL

[0100] Rheology

[0101] The rheology of different PILs was measured by a MCR 702e (Anton Paar) rheometer using a plain-plate geometry (PP-10) in an oscillation mode at angular frequencies from 0.1 to 100 rad / s.

[0102] Probe tack test

[0103] A probe with a diameter of 12 mm was held by an upper gripper which was controlled by MTS criterion model 42 (MTS Systems Corporation, Eden Prairie, MN, USA) static mechanical tester. PILs were cured on the steel plates and fixed on the bottom plate below the probe. By moving the upper gripper, a good contact between probe and PILs was first established by pressing the probe onto PILs with a constant contact force of 5 N for 1 min. Subsequently, the probe was pulled up with a constant separation speed of 0.01 mm / s. The force required for separation of the probe from the surface of PILs was recorded as a function of distance by the mechanical tester. The integral areas under the force-distance curves demonstrate the adhesion energy.

[0104] Swelling test

[0105] For swelling tests, different PILs with an area of 1 x 1 cm2were placed in petri dishes respectively. Then they were immersed in acetonitrile and equilibrated at room temperature for 2 days. Swelling ratio Q is defined as the difference between the initial weight of dry PIL (Mo) and the weight at swelling equilibrium (Ms) divided by the initial weight the ratio of the weight to that in the as-prepared state, Q = (Ms-Mo) / Mo. Three independent samples were measured to calculate the standard deviation.

[0106] Results and discussion PILs were prepared by the photopolymerization of the monomer in the precursor solution, followed by the removal of the acetonitrile solvent, as described in Example 1. The complete evaporation of acetonitrile was verified by FTIR (Fig. 1c), in which the peak at 2254 cm-1associated with C=N bond disappeared in all the PILs. For all precursors, the amount of monomer HVIM BF4 and crosslinker were kept constant, while the weight percentage of the solvent was varied. The as-prepared PIL is denoted as PIL-X, where X refers to the relative weight percentage of the solvent to monomer in the precursor solution. By regulating the amount of solvent added, the concentration of the monomer was readily tuned to achieve different degrees of polymerization and cross-link density within PILs. When more solvent was added into the monomer precursor, the lowered monomer concentration reduces the probability of monomers / oligomers reacting with each other, leading to a looser polymer network (Fig. 2a). In contrast, a high-concentration monomer in the precursor (with less solvent) could readily react, forming a denser polymer network. The extent of the reaction can be reflected by the amount of unreacted monomer, which is related to the peak intensity at 1654 cm-1associated with the C=C bond in FTIR spectrum (Fig. 2b). The weight percentage of the unreacted monomer in PIL-100 was 40-60 wt.%. As the weight percentage of solvent decreases, the peak intensity at 1654 cm-1decreases correspondingly after solvent evaporation, indicative of a higher degree of polymerization. The higher extent polymerization leads to a tighter network in PIL, which restricts the chain motion and reduces the swelling ratio. As shown in Fig. 2c, as the solvent amount increases from 0 to 100 wt.%, the swelling ratio increases from 3.41 to 9.11 due to a loosely packed network within PIL that allows chain motion. For PIL-150, the polymer spontaneously dissolves in the solvent, indicating minimal cross-link density.

[0107] Rheological measurements of PILs showed that with reduced solvent, the corresponding modulus of PIL increased considerably (Fig. 2d). For PIL-150, the value of storage modulus (G’) was lower than that of loss modulus (G”), which reflects its liquid behavior. When the solvent amount decreases to 100 wt.%, PIL-100 shows an elastic-viscous crossover at around 60 rad / s at room temperature, exhibiting a solid-like elasticity at low frequency and liquid-like viscosity at high frequency. Meanwhile, PIL-50 is solid-like as the value of G’ is higher than that of G” in the measured frequency range. When there is no solvent in the precursor, PIL-0 is essentially a rigid solid polymer which is no longer suitable for rheological measurement. The difference in cross-link density of PILs leads to totally different values of glass transition temperature (Tg), which can be assessed by using DSC. With the increase of solvent amount in the precursors, the obtained PILs exhibited a reduced Tgvalue of 174.8, 78.3, -52.1 °C for PIL-0, PIL-50, and PIL-100, respectively (Figs. 3a-c). PIL-0 and PIL-50 have a Tgvalue that is higher than room temperature, which suggests that they are in a glassy state, which explains their stiffness and inflexibility. In contrast, PIL-100 displayed flexible motion of polymer chains as it has a Tgmuch lower than room temperature. At high temperatures, all PILs show high thermal stability, with thermal decomposition occurring at around 380 °C (Fig. 3d).

[0108] By varying the solvent amount in the precursors, the strength and stretchability of PILs can be regulated over a wide range. Based on stress-strain curves (Fig. 4a), PIL-0, PIL-50, and PIL- 100 achieved a stretchability of 14%, 148%, and 300%, respectively. PIL-0 is too rigid and non-stretchable to be a filler. PIL-75 and PIL-125 were supplemented in Fig. 5 to show a clearer trend of mechanical properties change. PIL-75 breaks at a strain of 245% but PIL-125 is not so free-standing as PIL-100. The increased stretchability with solvent concentration was attributed to the reduced cross-link density that allowed polymer chains to slide across each other easily. From the slope of the curves from 0 to 5% strain, the Young’s modulus of PIL-0, PIL-50, PIL-100 is derived to be 125.9±13.8, 15.3±5.3, and 0.11±0.03 MPa, respectively (Fig. 4b). The softness of PIL-100 was contributed by not only its low cross-link density but also the monomer remnants within PILs that could act as a plasticizer to decrease the Young’s modulus further. Therefore, a soft and stretchable solid-state PIL filler with high dielectric constant can be prepared by regulating the acetonitrile amount in the precursor solution containing optimized monomer, crosslinker and photoinitiator.

[0109] The adhesion property of PIL with different solvent amount in precursors was quantified by probe tack tests (Fig. 6). As shown in Fig. 6, there is a typical tack adhesion measurement apparatus 600 that includes a probe 601, an adhesive 602, and a substrate 603. In Fig. 6a, there is a contact force 604. In Fig. 6b, there is a separation force 605. As shown in Fig. 4c, the adhesion energy of PIL-100 was almost 12 times greater than that of PIL-50, illustrating the strong adhesion capability of PIL-100. The inset in Fig. 4c shows that PIL-100 detached adhesively from the probe surface, illustrating the strong adhesion of PIL. Thus, it was clearly observed that PIL-100 detached adhesively from the probe surface, whereas PIL-50 directly departed from the probe without any remaining connection. The good adhesion took advantage of the ideal viscoelasticity of PIL-100, whose G’ was less than 105Pa, meeting the Dahlquist criterion, and sufficient G” for dissipating energy via viscous contributions. On the contrary, PIL-50 was deprived of segmental mobility for adhesive bond formation with the probe, causing the low adhesion energy. Benefiting from the good adhesion property and similar modulus, PIL-100 was envisioned to form a good interface with the elastomer matrix, reducing the tendency of delamination during DEA deformation. All the properties of different PILs are listed in Table 1 for comparison.

[0110] Table 1. Properties of PILs with different solvent amount in precursors. Sample Liquid / solid Swelling TgStrain at Young’s Adhesion ratio (°C) break (%) modulus (MPa) property

[0111] PIL-0 Solid 3.41±0.47 174.8 14.0±8.8 125.9±13.8 Not adhesive

[0112] PIL-50 Solid 6.61±0.59 78.3 163.2±53.4 15.3±5.3 Slightly adhesive

[0113] PIL-100 Solid 9.11±1.41 -52.1 276.4±21.3 0.11±0.03 Strongly adhesive

[0114] PIL-150 Liquid N.A. -55.5 N.A. N.A. N.A.

[0115] Based on the discussion above, PIL-100 delivers the best features and therefore, it is further studied to assess its viability as a DEA filler. Cyclic tensile test was conducted at various strains from 25% to 100%, as shown in Fig. 7. Similar to many viscoelastic materials, this hysteresis loss further validates the rubbery feature of PIL-100. When stretched repeatedly at 100 % strains for ten cycles, it was found that the first hysteresis loop is larger than the subsequent loops (Fig. 4d). After the first cycle, a stable hysteresis loop was formed. Besides, the tensile strength remained the same for all the cycles. PIL-100 could undergo reversible deformation thanks to the ideal viscoelastic nature of the material. As shown in Fig. 4e, the initial stretching curve shows great superimposition of the curve after relaxation for merely 2 min, indicative of outstanding recoverability. Furthermore, the self-healing performance of PIL- 100 was explored. As shown in Fig. 4g, the free-standing PIL-100 was first cut in the middle by a scalpel, and then, the two separate parts were brought into contact and healed for a minute. It was found that the healed PIL could be stretched to almost four times of its initial length. Fig. 4f shows the healing efficiency of PIL-100 for five cycles of self-healing, which was calculated from the ratio of tensile strength of each cycle to the original material. As shown in the stress-strain curves in Fig. 8, the strain at break of each cycle is similar to that of original PIL, while the tensile strength decreases after healing. As a result, the healing efficiency is around 70%, which is associated with the irreversible breaking of chemical bonds and reversible breaking and recombination of ionic interactions. Besides, this healing ability can be attributed to the low Tg(-52.1 °C) of PIL-100, which enables sufficient chain mobility for the cationic polymer at the interface to spontaneously reform ionic interactions with the anions at the other interface. Overall, the stable cyclic performance, adhesion properties, and self- healing ability of PIL-100 build the basis of a promising filler for durable and safe DEAs.

[0116] Example 3. PIL filler for VHB To form a composite elastomer (C-VHB), PIL-100 was incorporated by curing the PIL filler in the central region of one 3M VHB 4905 tape which was eventually sealed by another layer of 3M VHB 4905 tape. As both VHB and PIL-100 are adhesive, the adhesion strength between them was evaluated via a lap-shear test. Different from the typical methods of blending of fillers, the optimized PIL filler was encapsulated by two layers of VHB elastomer to form a composite, to reduce the possibility of electrical stress propagation.

[0117] Shear test

[0118] The shear test was conducted by MTS criterion model 42 (MTS Systems Corporation, Eden Prairie, MN, USA) static mechanical tester according to ASTM D1002. VHB 4905 (or PDMS) and PIL-100 were fixed on two stainless steel plates respectively. Then, the two materials were overlapped to make a contact. The length and width of the overlapping region were 12.7 and 21 mm, respectively. The gripper holding the steel with PIL-100 was pulling up with a speed of 1.3 mm / min while the VHB was fixed by the bottom gripper.

[0119] Capacitance and dielectric loss measurements

[0120] The capacitance and dielectric loss were measured simultaneously by a dielectric spectroscopy (Agilent 4294A). The dielectric constant of VHB and C-VHB was calculated by the equation sr= where C, d, £0and A are capacitance, thickness of the elastomer, vacuum dielectric constant and the area of electrodes, respectively. The thickness is controlled as the same of 250 pm, and the electrode area is the same as well. The dielectric breakdown strength of VHB and C-VHB was measured based on ASTM D3755-20. Samples were immersed in silicone oil to avoid the existence of oxygen and both sides of the samples were contacted with disk copper electrodes which connect to a high voltage power source. Ten samples of each type of elastomers were tested for Weibull analysis. The relationship between -(—) / * cumulative failure probability and breakdown field is described as P(E) = 1 - eEt , where Eb and / 3 are dielectric breakdown field and Weibull modulus, respectively.

[0121] Results and discussion

[0122] Fig. 9a demonstrates a shear bond force of around 4 N. After the detachment, it was found that residual PIL-100 remained intact on the surface of VHB, indicative of a cohesive failure of PIL-100 (Fig. 9b). This implies that the adhesion bonding at the interface between VHB and PIL-100 is stronger than the internal structural strength of PIL-100, ensuring a strong connection between VHB and PIL-100. Tensile tests were conducted to examine the change in stretchability and Young’s modulus of C-VHB, compared with pristine VHB. When compared with pristine VHB, C-VHB breaks earlier and possesses a lower Young’s modulus. As depicted in Fig. 9c, VHB breaks at a strain of 782%, whereas the C-VHB breaks slightly in advance at 622%. The abrupt change in stress at around 300% strain of C-VHB originates from the fracture of PIL filler inside VHB which is in line with the maximum stretchability of PIL filler at around 300%. Before the rupture of PIL filler, the bonding interaction between VHB and PIL is robust as no delamination was observed in Fig. 10a. When C-VHB was stretched beyond the maximum stretchability of the PIL filler, more cracks were formed within the PIL (Fig. 10b), subsequently leading to premature mechanical failure of C-VHB. Despite the reduced stretchability, the Young’s modulus of C- VHB was 0.21 MPa, slightly lower than 0.25 MPa of VHB, due to the introduction of a softer PIL filler. Taking VHB as a control, cyclic tensile test at 100% strain for ten cycles was conducted to assess the influence of PIL filler on the composite elastomer. A large hysteresis loss was observed for the first cycle, and gradually reduced to a stable state after five cycles (Fig. 9d). This strain softening behavior can be associated to the dissociation of non-covalent bonds within VHB and C-VHB. The hysteresis loss of C-VHB is 37.09%, which is slightly higher than pristine VHB (33.28%), as PIL is also a viscoelastic material with a similar hysteresis loss of 34.30%.

[0123] As Maxwell pressure P is in direct proportion to the dielectric constant (er), eris another significant parameter for the performance of DEAs. PIL-100 was encapsulated between 2 layers of prestretched 3M VHB 4905 to fabricate a C-VHB with thickness of 260 pm, to compare with a pure VHB of the same thickness. As shown in Fig. 9e, the effective erincreased from 4.7 to 16.4 at 1 kHz with the introduction of PIL filler, due to the additional ionic polarization effect. The dielectric loss of C-VHB in Fig. 9f is 0.24 at 1 kHz, somewhat higher than that of VHB, which is typical for the elastomer with high-dielectric-constant fillers.

[0124] Example 4. Actuation performance

[0125] Two modes of DEAs were fabricated to evaluate the actuation performance of DEAs using C- VHB and VHB. Capacitance and dielectric loss measurements were carried out by following the protocol in Example 3.

[0126] Fabrication of planar DEAs

[0127] The blank DEA was fabricated using a layer of prestretched 3M VHB 4905 (biaxially 200% by 200%) with a diameter of 3 cm and thickness of 55 pm, and mounting it on a circular frame (inner diameter: 3 cm). For the DEA with PIL filler, a fixed volume such as 100, 200, 300, 400 pL of the precursor of PI L- 100 was dropped on the center of a layer of prestretched 3M VHB 4905 (biaxially 200% by 200%), and then cured and heated to obtain a solid-state PIL membrane. After cooling down to the room temperature, another layer of prestretched 3M VHB 4905 (biaxially 200% by 200%) was sticked on the top of the PIL membrane to seal it between the two layers of VHB tapes and the composite elastomer C-VHB was obtained. Carbon grease electrodes were coated onto the top and bottom of the composite elastomer (and similarly on the control blank DEA) with a circular overlapping region with a diameter of 1 cm and two connecting lines to silver tapes were applied to electrically connect to a Unicorn UHP-75 high voltage power source. The obtained DEA could show an area strain under the high voltage. The area covered by the overlapping electrodes was recorded by a video camera and then calculated by the software Image J. The voltage applied on the device increased by 500 V until the breakdown voltage of DEAs. Area strains (AA) were calculated by the equation: AA = (Af - Ao) / Ao * 100%, where Af is the area under different voltages and Ao is the initial area of the overlapping region.

[0128] Fabrication of bending DEAs

[0129] Similarly, the composite elastomer of bending DEA was formed following the same steps as the protocol for fabrication of planar DEAs above, but the VHB was not prestretched. Therefore, no frame was needed. To lower down the thickness of bending DEAs with C-VHB, 3M VHB F9473PC with a thickness of 260 pm was applied here. A piece of 3M VHB F9473PC tape (3 x 1 .2 cm2) with a central rectangular hole (3 x 1 cm2) was sticked on an intact layer of 3M VHB F9473PC tape (3 x 1.2 cm2). Then, 150 pL of PIL precursor was dropped in the hole and then cured and heated to form PIL filler. Another layer of 3M VHB F9473PC tape (3 x 1.2 cm2) was sticked to seal the PIL filler between the two layers of VHB tapes. The thickness of the corresponding C-VHB was ~0.8 mm.

[0130] DEAs with composite PDMS (C-PDMS) was constructed by similar steps (Fig. 11a). PDMS base and curing agent were mixed with a weight ratio of 10:1 , stirred for 5 min and then degassed for 0.5 h. After degassing, the mixture was blade coated on a glass slide and cured at 80 °C for 2 h, forming a PDMS layer with a thickness of 300 pm. A piece of 3M VHB 4905 tape with a central rectangular hole of 2 x 1 cm2was sticked on the PDMS layer. The precursor of PIL- 100 of 100 pL was dropped in the hole and then cured and heated. The VHB tape was removed and the uncured mixture of PDMS was blade coated on the PIL- 100 and bottom PDMS layer to encapsulate PIL-100 inside. This was heated at 80 °C until the top PDMS was fully cured, thereby C-PDMS was formed. The thickness of C-PDMS was 0.86 mm. The silver nanowire (AgNW) electrodes were spray coated on the top and bottom of the composite elastomer with a rectangular overlapping region (2 x 1 cm2) and the top of two narrow silver tapes to strengthen the connection with them. A 3M Scotch Magic Tape was cut to fully cover the bottom of the elastomer and used as the passive layer. The silver tapes were connected to the Unicorn UHP-75 high voltage power source to enable the deformation of the composite elastomer. The state of bending DEAs was recorded by a video camera. The angles between the initial state and deformed state were calculated by the software Image J (Fig. 12b). The voltage applied on the device increased by 1 kV.

[0131] Specific energy density Emasscalculations

[0132] For bending DEAs, specific energy density Emass is calculated by the following equation: where Ft, a, m are blocking force, bending displacement and mass of DEAs, respectively. Here, m for DEA with VHB and C-VHB (including electrodes and passive layers) are 0.1678 and 0.2782 g, respectively. Equation 2 can be used to transfer bending angles Q to bending displacements or with known length / of DEAs. a = — z \x

[0133] 180 (v2J)

[0134] Here / for DEAs with VHB and C-VHB is the same, namely 23 mm.

[0135] Electromechanical conversion efficiency (o) is the ratio of mechanical work output to electrical energy input, which can be calculated by: where C and V are capacitance and voltage, respectively.

[0136] Results and discussion

[0137] The first mode is a planar DEA in which VHB 4905 is prestretched biaxially at 200% by 200%, with the area strain being recorded (Fig. 13a). As shown in Fig. 13a, there is a planar DEA with area strain 1300. The planar DEA with area strain 1300 includes frames 1301 , electrodes 1302, and dielectric elastomer 1303. Upon voltage application, charges accumulate on electrodes and attract each other. The electrostatic force between the electrodes then compresses the soft elastomer and achieves an in-plane area expansion (Fig. 14). A range of PIL-100 precursor volume from 100 to 400 pL was added into VHB to determine the optimal PIL filler for improved actuation. The thickness of the corresponding C-VHB was 253, 293, 334, and 375 pm, respectively. As shown in Fig. 13b, the effective £rat 1 kHz increased with more volume of PIL due to greater contributions from ionic polarization with higher loading. However, the dielectric loss increases as well (Fig. 15). Among the DEAs, the device with 200 pL PIL precursor showed a maximum actuated area that is as high as 137% at 17 V / pm (5 kV), far larger than that of DEA without PIL filler (area strain of only 5.4% at the same electric field) as shown in Fig. 16a. While DEA with higher PIL filler loading enables higher dielectric constant, lower Young’s modulus, and better actuation performance, the increasing dielectric loss causes a reduction in electrical breakdown field strength from 20 to 15 V / pm, constraining the maximum actuation strain. The dielectric breakdown strength of VHB and C-VHB was measured through Weibull analysis, in which C-VHB showed an earlier breakdown than VHB (Fig. 16b). Nonetheless, the actuation performance achieved by C-VHB surpasses most DEAs with fillers at a similar electric field (Table 2).

[0138] Table 2. Comparison of dielectric constant and actuation performance of this work against other DEAs with fillers.

[0139]

[0140] The second mode is a unimorph DEA 1310, which consists of a soft dielectric elastomer 1311 , compliant silver nanowire (AgNW) electrodes 1312, and a relatively rigid passive layer 1313 (Fig. 13d). During voltage application, the area expansion of the elastomer is constrained by the rigid passive layer, leading to bending motion towards the passive layer (Fig. 12a). The change in angle between the voltage off state and the voltage on state at equilibrium would be recorded as the bending angle (Fig. 12b). As shown in Fig. 12c, the bending angle of DEA at 12.6 V / pm reached the equilibrium for 3 seconds after turning on the voltage. Thus, the states of DEAs for analysis were taken after 3 seconds. Fig. 13e illustrates that the DEA with C-VHB has a bending angle of 38.6° at an electric field of 12.6 V / pm, which is over twice the value of the DEA with solely VHB. Moreover, the blocking forces of both the DEAs with C-VHB and VHB were investigated. It was found that DEA with C-VHB reached a blocking force of 1.45 mN at an electric field of 12.6 V / pm, 60-fold higher than that of DEA with VHB (0.2 mN) under the same condition (Fig. 17). Similar to planar DEAs, these enhanced bending angles were attributed to the ability of PIL in raising the dielectric constant and maintaining a low Young’s modulus.

[0141] Based on the displacement and blocking force results, DEA with C-VHB showed higher specific energy density of 40.39 J / g than 3.33 J / g of DEA with VHB at the same electric field of 12.6 V / pm. Besides, the electromechanical conversion efficiency of DEA with C-VHB is 0.57% at 12.6 V / pm, over twice the value of DEA with VHB (0.26%). In consideration of the self-healability of PIL-100 and the adhesion of VHB, the recoverability of DEA with C-VHB was investigated. As shown in Fig. 18, the C-VHB was first cut in the middle and then the two separated parts were brought into contact. After that, AgNW electrodes were spray coated on both sides of the recovered C-VHB and the passive layer was adhered. The actuation performance of DEA with recovered C-VHB was directly checked after the device fabrication, which showed similar bending angles compared to DEA with pristine C-VHB (Fig. 13f). This result illustrates the great recoverability of C-VHB, allowing these devices to achieve longer lifetimes. Further, without wishing to be bound by theory, the great recoverability of C-VHB benefits from the self-healability of PIL and the adhesion of VHB, allowing DEAs to achieve longer lifetimes.

[0142] PIL fillers can also work in silicone elastomer like PDMS to achieve fast response. Due to the low surface energy of PDMS, the adhesion between PIL and PDMS is not so strong as PIL and VHB (Fig. 19). With the addition of PIL filler, the dielectric constant of composite PDMS (C-PDMS) increased from 2.9 to 6.5 at 1 kHz (Fig. 11b). Benefiting from the low viscous loss of PDMS, bending DEAs with C-PDMS can achieve stable cyclic displacement of 20 pm at 5.8 V / pm and 100 Hz, which can be realized by bending DEAs with pristine PDMS at a higher electric field of 14.3 V / pm (Fig. 11c).

[0143] Example 5. Bending DEAs integrated with ACEL

[0144] Light emissive actuators that realize simultaneous graphic displays and dynamic motion are of great interest due to its potential applicability in AR and VR for metaverse, camouflage wearable electronics, smart soft robotics, human-machine interfaces, and biological systems. Herein, a bending DEA integrated with ACEL is fabricated to showcase this possibility. Capacitance and dielectric loss measurements were carried out by following the protocol in Example 3.

[0145] Fabrication of DEA integrated with ACEL

[0146] The fabrication of bending DEA was carried out by following the steps described in the protocol for the fabrication of bending DEAs in Example 4. The difference is that the passive layer here is an EL layer composed of PDMS mixed with ZnS:Cu particles. To form the EL layer, PDMS base and curing agent were mixed with a weight ratio of 10:1 and stirred for 5 min. Then ZnS:Cu particles were added into the PDMS liquid mixture with a weight ratio of 1 :2. The mixture of liquid and powder was stirred for 10 min and degassed for 0.5 h. After degassing, the mixture was blade coated on a glass slide and cured at 80 °C for 2 h, forming a PDMS+ZnS:Cu film with a thickness of ~125 pm. This EL layer was peeled off from the glass slide and sticked to the bottom of DEA. Another layer of AgNW electrode was spray coated on the bottom of the EL layer with a silver tape extended for connection with a withstanding voltage tester (Kikusui TOS5051). A thin PDMS layer was spin coated on the bottom to protect the AgNW electrode.

[0147] Transparency

[0148] The transparency of PI L- 100, VHB and C-VHB (composite VHB consists of VHB and PIL filler) was determined by absorption spectra using a Perkin Elmer Lambda 950 spectrophotometer in transmittance mode.

[0149] Emission spectroscopy

[0150] Emission from the light emissive bending DEA was collected by an optical fiber connected to an Acton SP-2300 monochromator. Emission spectra from the light emissive bending DEA were measured by a Princeton Pixis 100B spectroscopy CCD detector on the monochromator.

[0151] Results and discussion The integrated structure is shown in Fig. 20a, the C-VHB and the ACEL layer are stacked together, sharing a common electrode between them. The C-VHB elastomer was applied to realize better actuation performance than pure VHB. The ACEL layer was composed of PDMS and ZnS:Cu particles (PDMS+ZnS:Cu), which served as both the light emissive layer and the passive layer. The ability of PDMS+ZnS:Cu to be a passive layer was examined by a mechanical test. As shown in Fig. 20b, the Young’s modulus of VHB, PDMS, PDMS+ZnS:Cu is 279.9±12.9, 1239.3±231.1 and 1930.6±44.1 kPa, respectively. With the addition of rigid ZnS:Cu particles, PDMS+ZnS:Cu becomes much more rigid, broadening the gap on the mechanical properties with VHB. Therefore, the rigid PDMS+ZnS:Cu layer could realize the bending motion of DEA, with noticeable bending angles shown in Fig. 21. Furthermore, the DEA has excellent transparency based on the highly transparent components such as VHB (-91%) and PIL (~99%), which would not block the light emission from the ACEL layer (Fig. 20c). As a result, minimal EL intensity change was observed at 506 nm, when viewed from the DEA layer or the EL layer at an applied AC bias of 650 V, 50 Hz (Fig. 20d). The simultaneous actuation and light emission of the integrated device is shown in Fig. 20e. The bending DEA displayed a bending angle of 9.5° at an electric field of 6.3 V / pm, with a continuous teal light emission under a constant AC bias (650 V, 50 Hz). Furthermore, the EL intensity kept stable after 1000 cycles of actuation, illustrating the durability of the integrated device (Fig. 22).

[0152] By simply regulating the solvent amount during the polymerization of precursors, the mechanical properties of PILs can be tuned over a wide range. Among them, PIL-100 displays a high stretchability of -300%, low Young’s modulus of 0.11 MPa, strong adhesion ability, fast self-healing (with 1 min), recoverability, and a high transparency of -99%, thereby becoming an outstanding candidate as a filler for DEAs. By introducing the PIL filler to the VHB elastomer, the dielectric constant increased from 4.7 to 16.4 at 1 kHz and the Young’s modulus decreased to 0.21 MPa, thereby enhancing the actuation performance for planar and unimorph DEAs. For planar DEAs, C-VHB showed an area strain of 137% at an electric field of 17 V / pm, surpassing most DEAs with fillers at similar electric fields. Also, unimorph DEA with C-VHB demonstrated a bending angle of 38.6° at 12.6 V / pm, which is over twice that of pristine VHB. Meanwhile, the blocking force of the bending DEA increased from -0.2 mN to 1 .45 mN at 12.6 V / pm with the addition of PIL filler. Notably, the optimized PIL exhibited excellent adhesion, fast self-healability and recoverability, which was ascribed to the ionic interaction between cations on the polymer chains and mobile anions. Importantly, the excellent adhesion and fast self-healability of PIL-100 prevent DEAs from filler leakage problems because a strong interface between the elastomer matrix (VHB) and PIL filler is formed, and enables durable actuation and the recovery of actuation performance after damage. Finally, a bending DEA integrated with ACEL layer demonstrates simultaneous dynamic motion and light emission, which is attractive for interactive displays, camouflage wearable electronics, soft robotics, and human-machine interfaces. Therefore, when PIL fillers are introduced, planar DEAs show greatly increased area strain at the same electrical field, and bending DEAs achieve increased bending angle and blocking force. Overall, this work paves the way for synthesizing soft solid- state filler with a large dielectric constant for high-performance DEAs.

Claims

Claims1. A poly(ionic liquid) (PI L) film, comprising: from 40 to 60 wt% of a crosslinked polymer of formula I having the repeating unit:where: x represents monomeric repeating unit; y represents a crosslinking repeating unit; z represents a repeating unit for ethylene glycol, where the total Mn of the repeating unit y is from 500 to 1 ,000 Daltons ; and from 40 to 60 wt% of 1-hexyl-3-vinylimidazolium BF4 in monomeric form, wherein the PI L film has the following properties: a glass transition temperature of from -100 to -25 °C; a stretchability of from 150 to 500% of its original dimension; and a Young’s modulus of from 0.05 to 0.3 MPa.

2. The PIL film according to Claim 1 , wherein the PIL film has an adhesion of from 8 to 25 N, such as from 10 to 15 N, such as about 11 N in a probe tack test.

3. The PIL film according to Claim 1 or Claim 2, wherein the crosslinked polymer of formula I and the 1-hexyl-3-vinylimidazolium BF4 monomer are present in approximately equal amounts.

4. The PIL film according to any one of the preceding claims, wherein the PIL film has one or more of the following properties:(a) a glass transition temperature of from -75 to -40 °C, such as about -52.1 °C;(b) a stretchability of from 200 to 400%, such as about 300%, of its original dimension;(c) a Young’s modulus of from 0.07 to 0.2 MPa, such as about 0.11 MPa; and(d) an ability to self-heal following damage within 1 minute of the damage occurring.

5. The PIL film according to any one of the preceding claims, wherein the PIL film exhibits a self-healing efficiency of from 60 to 80%, such as about 70%.

6. The PIL film according to any one of the preceding claims, wherein the total Mn of the repeating unit y is about 700 Daltons.

7. A composite elastomeric material suitable for use in a dielectric elastomer actuator (DEA), the composite elastomeric material comprising: a poly(ionic liquid) (PIL) film layer as described in any one of Claims 1 to 6; and two dielectric elastomer layers, wherein the PIL film layer is sandwiched between and encapsulated by the two dielectric elastomer layers.

8. The composite elastomeric material according to Claim 7, wherein the elastomeric material has an effective dielectric constant of from 10 to 40 at 1 kHz, such as from 14 to 20 at 1 kHz, such as about 16.4 at 1 kHz.

9. The composite elastomeric material according to Claim 7 or Claim 8, wherein the thickness of each of the two dielectric elastomer layers is from several to 500 pm, such as about 300 pm.

10. The composite elastomeric material according to any one of Claims 7 to 9, wherein the two dielectric elastomer layers are formed from one or more of an acrylic foam adhesive material and a polydimethylsiloxane (PDMS) material.

11. A dielectric elastomer actuator (DEA) device, comprising:a composite elastomeric material as described in any one of Claims 7 to 10, having a first surface and a second surface; a first electrode and a second electrode attached to the first and second surfaces, respectively, of the composite elastomeric material; and at least one substrate layer attached to at least one of the first and second surfaces of the composite elastomeric material and / or at least one of the first and second electrodes.

12. The DEA device according to Claim 11 , wherein the DEA device is a bending DEA device wherein: the first and second electrodes are in the form of a first electrode layer and a second electrode layer, which substantially cover the first and second surfaces; and the at least one substrate layer is a passive layer attached to one of the first or second electrode layers.

13. The DEA device according to Claim 12, wherein the passive layer is a polymeric tape or an electroluminescence layer with an elastic modulus that is greater than that of the composite elastomeric material.

14. The DEA device according to Claim 13, wherein the electroluminescence layer comprises a PDMS polymeric matrix and ZnS:Cu particles homogeneously distributed throughout the PDMS polymeric matrix, optionally wherein the electroluminescence layer has a first surface attached to the first electrode layer or the second electrode layer and a second surface attached to a third electrode layer.

15. The DEA device according to any one of Claims 12 to 14, wherein the electrode layers are formed from a transparent and compliant electrode material, optionally wherein the electrode layers are formed from silver nanowires.

16. The DEA device according to Claim 11 , wherein the DEA device is a planar DEA device, wherein: the at least one substrate layer is in the form of a first frame and a second frame, the first frame being attached to the first surface and the second frame being attached to the second surface, respectively, of the composite elastomeric material; the dielectric elastomer layers of the composite elastomeric material are in a biaxially 0 to 300% by 0 to 300% stretched conformation, such as a biaxially 200% by 200% stretched conformation andthe first and second electrodes partly cover the first and second surfaces, respectively, of the composite elastomeric material.

17. The DEA device according to Claim 16, wherein the first and second frames each have an aperture that corresponds at least to the size of the first and second electrodes.

18. The DEA device according to Claim 16 or Claim 17, wherein the first and second electrodes are formed from carbon grease.

Citation Information

Patent Citations

  • Intrinsic conductive elastomer, preparation method thereof and flexible device

    CN113214431A

  • Actuator element using polymer ion gel and method for manufacturing the same