Modified negative electrode sheet, and preparation method therefor and use thereof
By using a stacked structure of needle coke primary particles and petroleum coke secondary particles in the negative electrode sheet of the lithium-ion battery, the problem of lithium precipitation during high-rate fast charging of lithium ions is solved, and the fast charging performance and performance of the battery core are improved. safety performance, and improved energy density and cycle performance.
Patent Information
- Application Number
- PCT/CN2023/092990
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-05-09
- Publication Date
- 2024-10-17
AI Technical Summary
The existing negative electrode plates of lithium-ion batteries cannot effectively transmit lithium ions during high-rate fast charging, resulting in the accumulation of lithium ions and lithium precipitation on the upper layer of the electrode plates, affecting the service life and safety performance of the battery cells.
A modified negative electrode sheet is used, including a first negative active material layer and a second negative active material layer on the surface of the current collector. The first layer uses needle coke primary particles, and the second layer uses petroleum coke secondary particles. The coating method and material ratio increase lithium ion diffusion and compaction density to prevent lithium precipitation.
It effectively improves the fast charging performance and safety performance of the battery, extends the service life of the battery, and takes into account high energy density. The 4C fast charging cycle can reach more than 2350 times, the capacity retention rate is more than 85.6%, and the energy density of 0.33C can reach 280Wh/Kg and above.
Smart Images

Figure PCTCN2023092990-FTAPPB-I100001
Abstract
Description
A modified negative electrode sheet and its preparation method and application Technical Field
[0001] The embodiments of the present application relate to the technical field of lithium-ion batteries, for example, a modified negative electrode plate and its preparation method and application. Background Art
[0002] With the promotion of new energy vehicles, lithium-ion batteries have become a hot topic for researchers. The popularity of new energy vehicles depends largely on their range and fast charging performance, so lithium-ion batteries must have characteristics such as fast charging and high specific energy.
[0003] Anode materials are carriers of lithium ions and electrons during the battery's charge and discharge processes, storing and releasing energy. Anode materials account for approximately 5-15% of battery costs and are a key raw material for lithium-ion batteries. Currently, graphite is the most widely commercialized and mature anode material. Energy storage lithium-ion batteries require anode materials with long-term, stable cycling performance to ensure the continued, stable operation of the energy storage system over extended periods of use.
[0004] CN112086645A discloses a negative electrode plate for a lithium battery, comprising a substrate and a negative electrode coating coated on the substrate, wherein the negative electrode coating is formed by condensing a negative electrode slurry, wherein the negative electrode slurry comprises an active material, a binder and a conductive agent, and the conductive agent comprises carbon nanotubes and carbon nanohorns.
[0005] CN106848190A discloses a negative electrode plate, comprising a primer, a midcoat and a topcoat sequentially coated on the surface of a current collector, wherein the primer, midcoat and topcoat are coated with a slurry comprising a negative electrode active material, a conductive agent, a thickener and a binder; the binder in the primer and midcoat is a water-based slurry binder, and the binder content in the midcoat is less than the binder content in the primer, and the binder in the topcoat is a solvent-based slurry binder.
[0006] Related technologies typically apply the negative electrode slurry evenly to the current collector. This coating method prevents lithium ions from effectively transferring from the upper electrode layer to the lower electrode layer during high-rate fast charging. Lithium ions accumulate in the upper electrode layer, eventually leading to lithium plating. This severely impacts the battery cell's lifespan and safety.
[0007] Summary of the Invention
[0008] The present invention provides a modified negative electrode sheet, a preparation method, and applications thereof. The modified negative electrode sheet can effectively improve the fast-charging performance of a battery cell, prevent lithium plating during high-rate charging, and extend the battery cell's service life and safety. Furthermore, the negative electrode sheet can meet the high energy density requirements of the battery cell.
[0009] In a first aspect, an embodiment of the present application provides a modified negative electrode plate, which includes a current collector and a first negative electrode active material layer and a second negative electrode active material layer stacked in sequence on the surface of the current collector, wherein the negative electrode active material of the first negative electrode active material layer is needle coke primary particles, and the negative electrode active material of the second negative electrode active material layer is petroleum coke secondary particles.
[0010] In the modified negative electrode sheet described in this application, the negative electrode active material of the second active material layer is secondary petroleum coke particles. The low OI value of these secondary particles facilitates the diffusion of lithium ions into the inner layer, preventing lithium plating during high-rate charge and discharge, and improving the fast-charging and safety performance of the battery cell. The negative electrode active material of the first active material layer is primary needle coke particles. The presence of these primary particles in the inner layer can increase the negative electrode compaction density, thereby increasing the energy density of the battery cell. Furthermore, the coating of the primary particles on the inner layer makes the internal structure of the electrode sheet more stable, which can improve the cycling performance of the battery cell.
[0011] In one embodiment, the petroleum coke secondary particles are prepared by the following method:
[0012] The petroleum coke particles, resin and dispersant are mixed, stirred and heated to obtain petroleum coke secondary particles.
[0013] In one embodiment, the resin includes phenolic resin.
[0014] In one embodiment, the dispersant includes anhydrous ethanol.
[0015] In one embodiment, the mass ratio of the petroleum coke particles to the resin is 100:(5-10), for example, 100:5, 100:6, 100:7, 100:8, 100:9 or 100:10.
[0016] In one embodiment, during the stirring and heating process, the heating method is: the time from room temperature to 300°C is 0.5 to 2 hours, then the time from 300°C to 500°C is 0.5 to 1.5 hours, and finally the time from 500°C to 600 to 700°C is 1 to 3 hours, and the temperature is kept warm for 3 to 5 hours.
[0017] In one embodiment, the OI value of the needle coke primary particles is 8-12, for example, 8, 9, 10, 11 or 12.
[0018] In one embodiment, the OI value of the petroleum coke secondary particles is 4-7, for example, 4, 5, 6 or 7.
[0019] In one embodiment, the median particle size D50 of the needle coke primary particles is 8 to 20 μm, for example, 8 μm, 10 μm, 12 μm, 15 μm, or 20 μm.
[0020] In one embodiment, the median particle size D50 of the petroleum coke secondary particles is 3 to 8 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm.
[0021] In the modified negative electrode sheet described in the present application, the particle size of the active material coated on the outer layer of the negative electrode slurry is small, which is conducive to the diffusion of lithium ions to the inner layer, and can prevent lithium ion plating during high-rate charging and discharging, thereby improving the fast charging performance and safety performance of the battery cell.
[0022] In one embodiment, the thickness of the first negative electrode active material layer is 110-120 μm, for example, 110 μm, 112 μm, 115 μm, 118 μm, or 120 μm.
[0023] In one embodiment, the thickness of the second negative electrode active material layer is 75-80 μm, for example, 75 μm, 76 μm, 77 μm, 78 μm, 79 μm or 80 μm.
[0024] In one embodiment, the first negative electrode active material layer and the second negative electrode active material layer further include a conductive agent and a binder.
[0025] In one embodiment, the conductive agent includes any one of conductive carbon black, carbon nanotubes, or acetylene black, or a combination of at least two thereof.
[0026] In one embodiment, the binder includes polyvinylidene fluoride.
[0027] In one embodiment, the mass ratio of the needle coke primary particles, the conductive agent, and the binder in the first negative electrode active material layer is (96-97):(0.5-1):(2-3), for example: 96.5:0.9:2.6, 96.2:0.8:3, 96.5:0.8:2.7, or 97:0.5:2.5.
[0028] In one embodiment, the mass ratio of the petroleum coke secondary particles, the conductive agent and the binder in the second negative electrode active material layer is (95-97):(1-1.5):(2.5-3), for example: 96:1.2:2.8, 95.5:1.5:3, 96.5:1:2.5 or 96.5:1:2.5, etc.
[0029] In a second aspect, an embodiment of the present application provides a method for preparing the modified negative electrode sheet as described in the first aspect, the preparation method comprising the following steps:
[0030] (1) mixing needle coke primary particles, a conductive agent, CMC, a binder, and a solvent to obtain a first negative electrode slurry, and mixing petroleum coke secondary particles, a conductive agent, CMC, a binder, and a solvent to obtain a second negative electrode slurry;
[0031] (2) The first negative electrode slurry is coated on one side or both sides of the current collector, and after drying, the second negative electrode slurry is coated on the surface of the first negative electrode slurry, and after drying, cold pressing is performed to obtain the modified negative electrode sheet.
[0032] In a third aspect, an embodiment of the present application provides a lithium-ion battery, wherein the lithium-ion battery includes the modified negative electrode sheet as described in the first aspect.
[0033] Compared with the related art, the embodiments of the present application have the following beneficial effects:
[0034] (1) In the modified negative electrode plates described in the embodiments of the present application, the negative electrode slurry active material coated on the outer layer is petroleum coke secondary particles. The secondary particles have a low OI value, which is conducive to the diffusion of lithium ions to the inner layer, and can prevent lithium ion deposition during high-rate charge and discharge, thereby improving the fast charging performance and safety performance of the battery cell. The negative electrode slurry active material coated on the inner layer is needle coke primary particles. The primary particles in the inner layer can increase the negative electrode compaction density, thereby increasing the energy density of the battery cell; at the same time, the primary particles are coated on the inner layer. This coating method makes the internal structure of the plate more stable, which can improve the cycle performance of the battery cell.
[0035] (2) The battery cell made of the negative electrode sheet described in the embodiment of the present application can have a 4C fast charging cycle of more than 2350 times, a capacity retention rate of more than 85.6%, and a 0.33C energy density of more than 280Wh / Kg. DETAILED DESCRIPTION
[0036] The petroleum coke secondary particles used in the examples and comparative examples of the present application were prepared by the following method:
[0037] Petroleum coke green coke powder was mixed with 8% binder pitch by mass and thoroughly mixed in a VC mixer for 1 hour at a frequency of 50 Hz. The mixture was pelletized in a homemade converter under a 0.1 L / min nitrogen atmosphere at a frequency of 20 Hz. The temperature was increased at a rate of 3°C / min to 650°C and held at that temperature for 2 hours. The pelletized mixture was then placed in a graphitization furnace and graphitized at 2800°C to produce secondary petroleum coke pellets.
[0038] Example 1
[0039] This embodiment provides a modified negative electrode sheet, and the preparation method of the modified negative electrode sheet is as follows:
[0040] (1) Primary particles of needle coke with a median particle size D50 of 15 μm and an OI value of 10, conductive carbon black, CMC, and SBR were mixed with a solvent in a mass ratio of 96.5:0.9:1.1:1.5 to obtain a first negative electrode slurry. Secondary particles of petroleum coke with a median particle size D50 of 5 μm and an OI value of 5, conductive carbon black, CMC, and SBR were mixed with a solvent in a mass ratio of 96:1.2:1.3:1.5 to obtain a second negative electrode slurry.
[0041] (2) The first negative electrode slurry is coated on one side or both sides of the current collector, and after drying, the second negative electrode slurry is coated on the surface of the first negative electrode slurry, and after drying, cold pressing is performed to obtain the modified negative electrode plate, wherein the thickness of the first active material layer in the negative electrode plate is 116 μm, and the thickness of the second active material layer is 77 μm.
[0042] Example 2
[0043] This embodiment provides a modified negative electrode sheet, and the preparation method of the modified negative electrode sheet is as follows:
[0044] (1) Primary particles of needle coke with a median particle size D50 of 15 μm and an OI value of 10, conductive carbon black, CMC, and SBR were mixed with a solvent in a mass ratio of 96.5:0.9:1.1:1.5 to obtain a first negative electrode slurry, and secondary particles of petroleum coke with a median particle size D50 of 5 μm and an OI value of 5, conductive carbon black, CMC, and SBR were mixed with a solvent in a mass ratio of 96:1.2:1.3:1.5 to obtain a second negative electrode slurry;
[0045] (2) The first negative electrode slurry is coated on one side or both sides of the current collector, and after drying, the second negative electrode slurry is coated on the surface of the first negative electrode slurry, and after drying, cold pressing is performed to obtain the modified negative electrode plate, wherein the thickness of the first active material layer in the negative electrode plate is 135 μm, and the thickness of the second active material layer is 58 μm.
[0046] Example 3
[0047] The only difference between this embodiment and embodiment 1 is that the median particle size D50 of the needle coke primary particles is 5 μm, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0048] Example 4
[0049] The only difference between this embodiment and embodiment 1 is that the median particle size D50 of the needle coke primary particles is 25 μm, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0050] Example 5
[0051] The only difference between this embodiment and embodiment 1 is that the median particle size D50 of the petroleum coke secondary particles is 2 μm, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0052] Example 6
[0053] The only difference between this embodiment and embodiment 1 is that the median particle size D50 of the petroleum coke secondary particles is 10 μm, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0054] Comparative Example 1
[0055] The only difference between this comparative example and Example 1 is that both the first active material layer and the second active material layer use needle coke primary particles as the negative electrode material, and the other conditions and parameters are exactly the same as those in Example 1.
[0056] Comparative Example 2
[0057] The only difference between this comparative example and Example 1 is that both the first active material layer and the second active material layer use secondary petroleum coke particles as the negative electrode material, and the other conditions and parameters are exactly the same as those in Example 1.
[0058] Comparative Example 3
[0059] The only difference between this comparative example and Example 1 is that the first active material layer uses petroleum coke secondary particles as the active material, and the second active material layer uses needle coke primary particles as the negative electrode material. Other conditions and parameters are exactly the same as those in Example 1.
[0060] Performance testing:
[0061] The negative electrode sheets prepared in the embodiment and the comparative example were taken, and the batteries were subjected to a 4C fast charge cycle test, and the battery capacity retention rate was recorded. The test results are shown in Table 1:
[0062] Table 1
[0063] As can be seen from Table 1, it can be obtained from Examples 1-2 that the battery cell made of the negative electrode sheet described in the present application can have a 4C fast charging cycle of more than 2350 times, a capacity retention rate of more than 85.6%, and a 0.33C energy density of more than 280Wh / Kg. Increasing the thickness of the first active material layer will increase the energy density of the battery cell, but will affect the fast charging performance of the battery cell.
[0064] By comparing Example 1 with Examples 3-4, it can be seen that in the modified negative electrode sheet described in the present application, the particle size of the needle coke primary particles will affect its performance. When the median particle size D50 of the needle coke primary particles is controlled at 8 to 20 μm, the performance of the modified negative electrode sheet is better. If the particle size of the needle coke primary particles is too large, the energy density of the battery cell will increase, but the fast charging cycle performance of the battery cell will decrease. If the particle size of the needle coke primary particles is too small, the fast charging performance of the battery cell will increase, but the energy density of the battery cell will decrease.
[0065] By comparing Example 1 with Examples 5-6, it can be seen that in the modified negative electrode sheet described in the present application, the particle size of the petroleum coke secondary particles will affect its performance. When the median particle size D50 of the petroleum coke secondary particles is controlled at 3 to 8 μm, the performance of the modified negative electrode sheet is better. If the particle size of the petroleum coke secondary particles is too large, the energy density of the battery cell will increase, but the fast charging cycle performance of the battery cell will decrease. If the particle size of the petroleum coke secondary particles is too small, the fast charging performance of the battery cell will increase, but the energy density of the battery cell will decrease.
[0066] A comparison of Example 1 and Comparative Examples 1-3 shows that in the modified negative electrode sheets described in this application, the active material coating the outer layer of the negative electrode slurry is secondary petroleum coke particles. These secondary particles have a low OI value, which facilitates the diffusion of lithium ions into the inner layer, preventing lithium ion deposition during high-rate charge and discharge, thereby improving the fast-charging performance and safety of the battery cell. The active material coating the inner layer of the negative electrode slurry is primary needle coke particles. The presence of these primary particles in the inner layer can increase the negative electrode compaction density, thereby increasing the energy density of the battery cell. Furthermore, this coating method stabilizes the internal structure of the sheet and improves the cycling performance of the battery cell.
Claims
1. A modified negative electrode sheet, wherein: The modified negative electrode sheet includes a current collector and a first negative electrode active material layer and a second negative electrode active material layer sequentially stacked on the surface of the current collector, the negative electrode active material of the first negative electrode active material layer is needle coke primary particles, and the negative electrode active material of the second negative electrode active material layer is petroleum coke secondary particles.
2. The modified negative electrode sheet according to claim 1, wherein: The petroleum coke secondary particles are prepared by the following method: The petroleum coke particles, resin and dispersant are mixed, stirred and heated to obtain petroleum coke secondary particles.
3. The modified negative electrode sheet according to claim 2, wherein: The resin includes a phenolic resin.
4. The modified negative electrode sheet according to claim 2 or 3, wherein: The dispersant includes anhydrous ethanol.
5. The modified negative electrode sheet according to any one of claims 2 to 4, wherein: The mass ratio of the petroleum coke particles to the resin is 100:(5-10).
6. The modified negative electrode sheet according to any one of claims 2 to 5, wherein: During the stirring and heating process, the heating method is: the time from room temperature to 300°C is 0.5-2h, then the time from 300°C to 500°C is 0.5-1.5h, and finally the time from 500°C to 600-700°C is 1-3h, and the temperature is kept for 3-5h.
7. The modified negative electrode sheet according to any one of claims 1 to 6, wherein: The OI value of the needle coke primary particles is 8 to 12; Preferably, the OI value of the petroleum coke secondary particles is 4-7.
8. The modified negative electrode sheet according to any one of claims 1 to 7, wherein: The median particle size D50 of the needle coke primary particles is 8 to 20 μm; Preferably, the median particle size D50 of the petroleum coke secondary particles is 3 to 8 μm.
9. The modified negative electrode sheet according to any one of claims 1 to 8, wherein: The thickness of the first negative electrode active material layer is 110 to 120 μm; Preferably, the second negative electrode active material layer has a thickness of 75-80 μm.
10. The modified negative electrode sheet according to any one of claims 1 to 9, wherein: The first negative electrode active material layer and the second negative electrode active material layer further include a conductive agent and a binder; Preferably, the conductive agent comprises any one of conductive carbon black, carbon nanotubes or acetylene black, or a combination of at least two thereof; Preferably, the binder comprises polyvinylidene fluoride.
11. The modified negative electrode sheet according to any one of claims 1 to 10, wherein: The mass ratio of the needle coke primary particles, the conductive agent and the binder in the first negative electrode active material layer is (96-97):(0.5-1):(2-3); Preferably, the mass ratio of the petroleum coke secondary particles, the conductive agent and the binder in the second negative electrode active material layer is (95-97):(1-1.5):(2.5-3).
12. A method for preparing the modified negative electrode sheet according to any one of claims 1 to 11, comprising the following steps: (1) mixing needle coke primary particles, a conductive agent, CMC, a binder and a solvent to obtain a first negative electrode slurry, and mixing petroleum coke secondary particles, a conductive agent, CMC, a binder and a solvent to obtain a second negative electrode slurry; (2) The first negative electrode slurry is coated on one side or both sides of the current collector, and after drying, the second negative electrode slurry is coated on the surface of the first negative electrode slurry, and after drying, cold pressing is performed to obtain the modified negative electrode sheet.
13. A lithium ion battery, characterized in that: The lithium-ion battery comprises the modified negative electrode sheet as described in any one of claims 1 to 11.
Citation Information
Patent Citations
Preparation method of negative electrode material of lithium ion battery and prepared negative electrode material
CN105523544A
Artificial graphite negative electrode material, preparation method thereof and application of artificial graphite negative electrode material in lithium ion battery
CN111620331A
Quick-charging type negative pole piece as well as preparation method and application thereof
CN115472778A
Negative pole piece and preparation method thereof, secondary battery, battery module, battery pack and device
CN115917780A