Surfacing process for outer wall of pipe

By applying multiple layers of columnar crystal welding layers to the outer wall of the pressure pipeline and using CNC equipment to control the welding process, the problem of insufficient creep resistance of the pressure pipeline is solved, achieving higher creep resistance and extending service life.

WO2024212623A1PCT designated stage expired Publication Date: 2024-10-17CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/070242
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-01-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The existing pressure pipelines have insufficient creep resistance under high temperature, high pressure and corrosive media, resulting in a short service life of the equipment, and the existing metal creep damage theory has not been effectively applied to the strengthening of pressure furnace pipelines.

Method used

Using the outer wall surfacing process, multiple layers of columnar crystal welding layers are applied to the outer wall of the pipe, and CNC equipment is used to achieve smooth rotation and translation. The inclination angle between the welding wire and the pipe surface is 60° to 80° to form a uniform columnar crystal distribution and improve creep. Resistance.

Benefits of technology

It significantly improves the creep resistance and service life of the pipeline, extends the economic benefits of the equipment, and ensures stable operation in high temperature and high pressure environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024070242_17102024_PF_FP_ABST
    Figure CN2024070242_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A surfacing process for the outer wall of a pipe, comprising: (1) performing rust removal, dehumidification, oil removal and decontamination, and nondestructive testing on a welding area on the outer wall of a pipe, and selecting the model and specification of a welding wire and a protective gas in the welding process according to an actual working environment and a single-layer surfacing thickness; (2) using an outer wall surfacing mode, after the pipe is preheated, controlling the pipe to continuously rotate and move in the axial direction so as to be welded while the position of a welding gun remains unchanged, and regulating and controlling the pipe to rotate and translate at a flat and stable speed in the welding process, the inclination angle between the welding wire and the surface of the pipe is 60°-80°; (3) when multi-layer surfacing needs to be performed, performing post-heat treatment on the surfacing surface after each layer of surfacing other than the last layer of surfacing, and then performing grinding; and (4) after surfacing is completed, performing heat treatment, performing nondestructive testing, and if the product meets the standards, finishing the surfacing process. The surfacing process effectively improves the creep resistance of the pipe.
Need to check novelty before this filing date? Find Prior Art

Description

A pipeline outer wall surfacing process Technical Field

[0001] The invention belongs to the technical field of surfacing welding, and in particular relates to a pipeline outer wall surfacing welding process. Background Art

[0002] In the fields of petrochemicals, nuclear power, metallurgy, and so on, there are a large number of pressure piping equipment that serve under conditions such as high temperature, high pressure, corrosive media, or cyclic loads. In recent years, my country's thermal power and chemical industries have developed rapidly, with production capacity and related production technologies greatly improved. Correspondingly, various types of pressure-bearing equipment have also developed towards large-scale and high-parameter with the advancement of industrial technology. Among them, pressure piping is a key component of various pressure-bearing equipment. It is not only the transportation channel for raw materials and products, but also the place where some reactions occur. Its importance is self-evident. With the development of equipment and processes, pressure furnace pipes need to be continuously improved and upgraded as the operating temperature increases. At the same time, due to the complexity of its working environment, high requirements are placed on the selection of pipeline materials. The pipeline itself needs to have good mechanical properties to ensure the safe and efficient operation of the equipment.

[0003] Currently, the use of microstructure to determine a material's creep resistance has been widely used in the materials field. One such theory, the crystal boundary load-bearing theory, which uses the microscopic grain arrangement pattern perpendicular to the material's stress direction as a reference, can effectively correlate metal creep damage with microstructure. By analyzing the microstructure of the same weld creep specimen under three different stress directions, two different causes of creep damage can be identified. The first is that the grain boundaries perpendicular to the stress direction have a high number of three-grain intersections, which easily lead to stress concentration and the initiation of creep voids. As the damage further evolves, wedge-shaped cracks will form at the grain boundaries / subgrain boundaries parallel to the stress direction, further reducing the specimen's bearing area. There are obvious subgrain boundaries within the crystal perpendicular to the stress direction, where creep voids will also form, resulting in localized creep voids (see Figure 1(a)). The second case involves a longer grain boundary perpendicular to the direction of stress. Consequently, there are fewer three-grain intersections. Although the applied load is the same as in the second case, the stress acting locally on the grain boundary is relatively small, resulting in creep cavities that primarily grow due to diffusion (see Figure 1(b)). Figure 1(c) shows the fracture life of the same material under two different microscopic stress conditions. Compared to the first microstructure, the material with the second microstructure and stress distribution has a longer actual life. Technical issues

[0004] While this theory has been used to explain creep damage in metallic materials, it has not been practically applied to enhancing the creep resistance of pressure furnace pipes. Therefore, the present invention utilizes this theory as a foundation to design a cladding process to improve the creep resistance of pressure furnace pipes. Technical Solutions

[0005] The purpose of the present invention is to provide a pipeline outer wall surfacing process to effectively solve the problem of low creep resistance of pressure furnace pipes.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0007] A pipeline outer wall surfacing process comprises the following steps:

[0008] S1. Derust, dehumidify, degrease and perform non-destructive testing on the welding area of ​​the outer wall of the pipeline, and select the type and specification of welding wire and the shielding gas during welding according to the actual working environment and the thickness of the single layer of cladding;

[0009] S2. Using external wall cladding, after preheating the pipeline, the welding is performed by keeping the welding gun in a fixed position while the pipeline is continuously rotated and moved axially. During the welding process, the pipeline is controlled by a numerical control device to rotate and translate smoothly and at a steady speed. The welding equipment is fixed in a fixed position for cladding. The specific rotation speed of the pipeline is determined by the appropriate welding speed for cladding. The inclination angle between the welding wire and the pipeline surface is 60° to 80° to achieve control of the internal structure of the cladding layer of the pipeline.

[0010] S3. When multi-layer cladding is required, except for the last layer, the cladding surface must be post-heat treated after each layer and then polished to remove slag and spatter;

[0011] S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.

[0012] Furthermore, in step S2, the welding direction is from one end of the pipe to the other end along a spiral trajectory.

[0013] Furthermore, when there are requirements for the thickness of the pipeline, multi-layer surfacing should be used to meet the thickness requirements.

[0014] Furthermore, the inclination angle between the welding wire and the pipe surface in step S2 is determined according to the surfacing material and the welding environment.

[0015] Furthermore, the microscopic crystals of the surfacing layer of the pipe are columnar crystals, the direction of the columnar crystals is the same as the direction of the welding wire, and the arrangement of the columnar crystals is uniformly distributed in the surfacing layer. Beneficial effects

[0016] The beneficial technical effects of the present invention are:

[0017] The surfacing process provided by the present invention enables the columnar crystals of the pipeline surfacing layer to be distributed evenly along the wall thickness, thereby making the stress conditions of the pipeline more reasonable when subjected to circumferential and axial loads, improving the creep resistance of the pipeline, and thereby extending the service life of the pipeline and significantly improving the economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0019] FIG1 is a schematic diagram showing the effect of heterogeneous structure on creep damage;

[0020] FIG2 is a metallographic image of a VDF cracking furnace pipe sample before surfacing;

[0021] Figure 3 shows the columnar crystal arrangement pattern of the VDF cracking furnace pipe before cladding;

[0022] Figure 4 shows the stress conditions of microscopic columnar crystals in the VDF cracking furnace pipe before surfacing under axial and hoop stresses;

[0023] Figure 5 shows the microscopic stress conditions of the ideal arrangement of columnar crystals under axial and hoop stress;

[0024] FIG6 is a schematic diagram of a specific embodiment of the present invention;

[0025] Figure 7 is the metallographic image of the VDF cracking furnace pipe sample after surfacing and the corresponding microscopic crystal arrangement. Modes for Carrying Out the Invention

[0026] This study uses the theory of crystal interface load bearing to explore the microscopic crystal arrangement of pipelines without additional processing. The mechanical performance defects caused by this microscopic crystal arrangement are summarized, and the ideal crystal arrangement is derived based on the specific stress conditions under actual pipeline operating conditions. Aiming to achieve the optimal microscopic crystal arrangement, the optimal process solution is determined to be external wall cladding. The control method for this microscopic crystal arrangement and the process implementation process are also determined.

[0027] Below, the VDF cracking furnace tube is taken as a representative of the pressure furnace tube, the microstructure of the VDF cracking furnace tube is analyzed and its optimal microstructure form is obtained.

[0028] Figure 2 shows metallographic images of VDF cracking furnace pipe specimens before cladding. Figure 2(a) shows a metallographic image of the circumferential cross-section of the pipe in zone A, Figure 2(b) shows a metallographic image of the longitudinal cross-section of the pipe in zone B, Figure 2(c) shows an enlarged image of the outer layer of the pipe in zone C, and Figure 2(d) shows an enlarged image of the inner wall of the pipe in zone D.

[0029] Figure 3 shows the arrangement of columnar crystals in a VDF cracking furnace pipe before cladding. Figure 3(a) shows the crystal arrangement of section A, Figure 3(b) shows the crystal arrangement of section B, and Figure 3(c) shows the columnar crystal arrangement.

[0030] The VDF cracking furnace tubes are made of pure N6 nickel. As shown in Figure 2, samples were taken from the VDF cracking furnace tubes and the microstructure of each cross-section was analyzed to determine the internal crystal arrangement. As shown in Figure 3, the microscopic columnar crystals in the VDF cracking furnace tubes are distributed along the tube's axial direction.

[0031] The stress state of microscopic columnar crystals in VDF cracking furnace pipelines under different stresses was analyzed, focusing on the stress state of microscopic grain boundaries under the conditions of circumferential force and axial force, which are relatively large loads in actual working conditions. Figure 4 (a) shows the stress state of microscopic columnar crystals under axial stress. As shown in Figure 4 (a), in the vertical direction of the stress under axial force, the VDF cracking furnace pipeline has many columnar crystal three-crystal intersections. As the main stress sites, the crystal intersections are prone to stress concentration, which is very likely to cause damage and the initiation of creep cavities. As the damage further evolves, wedge cracks will appear at the grain boundaries / subgrain boundaries parallel to the stress direction. Figure 4 (b) shows the stress conditions of microscopic columnar crystals under hoop stress. As shown in Figure 4 (b), the grain boundaries of the VDF cracking furnace pipe are longer in the vertical stress direction under the hoop force, and the three-crystal intersection points are relatively few. Part of the stress is shared to a certain extent at the grain boundaries. Therefore, under the same external load, the local stress is small, and the long grain boundaries will limit the expansion of creep holes at the grain boundaries. However, due to the presence of more non-columnar crystals in its microstructure, the length of the grain boundaries in the vertical stress direction is not uniform, and local stress concentration is still prone to occur, so there is room for improvement.

[0032] By analyzing the actual stress conditions of VDF cracking furnace pipelines, it can be concluded that the optimal microstructure for pressure pipelines is a microstructure composed entirely of columnar crystals distributed along the wall thickness, as shown in Figure 5. This microstructure maintains the stress state of the pipeline material's grain boundaries uniformly distributed along the long grain boundaries under high hoop stress and axial stress, making the stress distribution more uniform and reducing stress concentration. This optimal microstructure is also applicable to the creep resistance analysis of pipelines in various current fields.

[0033] After studying and analyzing the wire welding process, the applicant has determined that the microstructural pattern produced during wire overlay welding is that each weld creates a columnar microstructure aligned with the wire's direction, and that this microstructure is composed entirely of columnar crystals. For pressure pipes with relatively small inner diameters, using external overlay welding can reinforce the existing pipe while ensuring that the material flow through the original pipe wall is not affected by the overlay thickness. Furthermore, controlling the microstructural pattern of external overlay welding is significantly easier than with internal overlay welding.

[0034] Therefore, the microstructure morphology composed entirely of columnar crystals distributed along the wall thickness direction is set as the goal of the pipeline processing technology. Based on the microstructure laws generated during the wire cladding process, the applicant has developed a pipeline outer wall cladding process that is different from the traditional pipeline inner wall cladding process, thereby achieving a microstructure arrangement with better mechanical properties.

[0035] The present invention provides a pipeline outer wall surfacing process, comprising the following steps:

[0036] S1. Derust, dehumidify, degrease and perform non-destructive testing on the welding area of ​​the outer wall of the pipeline, and select the type and specification of the welding wire and the shielding gas during the welding process according to the actual working environment and the thickness of the single layer of cladding.

[0037] S2. Using external wall cladding, after preheating the pipe, as shown in Figure 6, the welding process is performed by continuously rotating and moving the pipe axially while maintaining the welding torch in a fixed position. Welding proceeds in a spiral trajectory from one end of the pipe toward the other. During welding, CNC equipment controls the pipe's steady rotation and translation, while the welding equipment performs the cladding at a fixed position. The specific rotation speed of the pipe is determined by the appropriate welding speed for the cladding process.

[0038] During the welding process, the angle between the welding wire and the surface of the welded pipe needs to ensure both the microstructure arrangement and the specific implementation process. During the welding process tested in the laboratory, if the optimal microscopic columnar crystal arrangement is considered alone and the angle between the welding wire and the welded pipe surface is unilaterally set to 80° to 90°, the welding wire metal will not fully solidify during the welding process and will flow and drip during the rotation of the pipe, resulting in poor final welding quality; and if the angle between the welding wire and the welded pipe surface is too low, its microscopic columnar crystal arrangement will not meet the requirements of mechanical property strengthening. Therefore, the applicant has determined through a large number of experiments that the inclination angle between the welding wire and the pipe surface should be selected between 60° and 80° based on the cladding material and the welding environment, so as to achieve the regulation of the internal structure of the cladding layer of the pipe.

[0039] S3. When there are requirements for the thickness of the pipeline, multiple layers of cladding should be used to meet the thickness requirements. When multiple layers of cladding are required, except for the last layer, the cladding surface must be post-heat treated after each layer of cladding and then polished to remove slag and spatter.

[0040] S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.

[0041] The pipe outer wall surfacing process provided by the present invention will be further described below with reference to the accompanying drawings, taking the VDF cracking furnace pipe as an example. Example

[0042] The VDF cracking furnace pipeline is constructed from pure N6 nickel, with dimensions of 108 x 4 mm before welding. Prior to welding, the weld area on the pipeline's exterior was rigorously cleaned of rust, moisture, and oil by grinding and cleaning. 100% MT magnetic particle testing was also performed, achieving Class I compliance according to JB / T 4730.4-2011.

[0043] The welding material used in the welding process is flux-cored wire, model TFW-625 (ENiCrMo-3), specification Φ1.2mm; the surfacing thickness is 4.5mm, and the effective thickness is 4mm; the shielding gas used is industrial-grade purity CO2.

[0044] The first layer of hardfacing was performed on the weld zone of the pipeline's outer wall, with the corresponding specification parameters shown in Table 1. Low heat input and narrow weld beads were used during the welding process, with strictly controlled heat input. During welding, the furnace tube was controlled by CNC equipment for steady rotation and translation. The welding equipment was positioned for hardfacing, maintaining a 65° inclination angle between the welding wire and the pipeline surface. After the first layer of hardfacing was completed, the weld surface underwent a post-heat treatment at (100-350)°C for 2 hours. This was to ensure slow cooling of the pipeline after welding and to remove some hydrogen. Because CO2 gas shielded welding produces a certain amount of spatter, which can deteriorate the weld surface after welding, post-heat treatment was followed by grinding to remove slag and spatter. If equipment issues cause localized weld overlap, resulting in unevenness greater than 1mm between the two joints, this should be corrected through grinding, which has no impact on the overall weld surface.

[0045] Table 1 Process parameters for the first layer of CO2 gas shielded flux-cored wire cladding

[0046]

[0047] Table 2 Process parameters for the second layer of CO2 gas shielded flux-cored wire cladding

[0048]

[0049] Table 2 shows the corresponding standard parameters for the second layer of cladding. During the second layer, the weld heat input and interpass temperature must be strictly controlled to ≤200°C. If the temperature is too high, welding is stopped and allowed to cool naturally before resuming welding. To control the thickness of the cladding layer, the welding wire is tilted at a 75° angle to the pipe surface.

[0050] Nondestructive testing (NDT) was performed on the welded cladding pipes after welding. Penetrant testing of the weld surface was performed, and the results met the requirements of JB / T 4730.5-2011, achieving Class I. Ultrasonic testing of the interface between the weld cladding and the pipe base material was also performed, achieving Class I compliance, according to JB / T 4730.3-2011. The cladding of the VDF cracking furnace pipes was found to be free of defects and fully qualified.

[0051] Figure 7 shows the metallographic images and corresponding microscopic crystal arrangement of the VDF cracking furnace pipe sample after surfacing welding. Figure 7 (a) shows the metallographic image and crystal arrangement of section A, Figure 7 (b) shows the metallographic image and crystal arrangement of section B, Figure 7 (c) shows the metallographic image of section C (the outer surfacing surface of the pipe), Figure 7 (d) shows the metallographic image of section D (the inner wall surface of the pipe), Figure 7 (e) shows the arrangement of columnar crystals in the pipe after surfacing welding, Figure 7 (f) shows the stress of columnar crystals in the surfacing layer under axial stress after surfacing welding, and Figure 7 (g) shows the stress of columnar crystals in the surfacing layer under hoop stress after surfacing welding.

[0052] As shown in Figure 7, the VDF cracking furnace tube after surfacing welding in Example 1 was cut and sampled, and a metallographic specimen was prepared and observed under an optical microscope. It was concluded that the columnar crystal distribution of the surfacing layer of the VDF cracking furnace pipe obtained by the surfacing welding process provided by the present invention has an obvious regularity of uniform distribution along the wall thickness, and the stress conditions of the VDF cracking furnace pipe after surfacing welding under circumferential and axial loads are more reasonable, and the mechanical properties are more excellent.

[0053] Under the same specifications and operating conditions, the actual service life of an N6 pipe in a VDF cracking furnace without the pipe outer wall cladding process provided by the present invention is approximately 2 to 3 years. Mechanical performance tests have shown that the service life of the N6 pipe in a VDF cracking furnace treated with the pipe outer wall cladding process provided by the present invention is extended to approximately 10 years. Therefore, the pipe outer wall cladding process provided by the present invention significantly improves the mechanical performance and economic benefits of a VDF cracking furnace.

[0054] The present invention mainly controls the arrangement of microscopic crystals in the pipeline cladding layer by the process implementation process itself, and has no special requirements for the selection of cladding materials. Therefore, this cladding process is also applicable to other types of furnace pipes, and cladding materials are selected based on their materials for processing.

[0055] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the scope of protection of the present invention.

Claims

1. A pipeline outer wall cladding process, It is characterized in that The following steps are involved: S1. Derust, dehumidify, degrease and perform non-destructive testing on the welding area of ​​the outer wall of the pipeline, and select the model and specification of the welding wire and the protective gas during welding according to the actual working environment and the thickness of the single-layer cladding; S2. Adopt the form of outer wall cladding. After the pipeline is preheated, the welding is performed by keeping the welding gun in the same position and manipulating the pipeline to rotate continuously and move axially. During the welding process, the pipeline is regulated to rotate and translate at a steady speed. The welding equipment is cladding at a fixed position. The specific rotation speed of the pipeline is determined according to the appropriate welding speed for cladding. The inclination angle between the welding wire and the pipeline surface is 60° to 80°, so as to realize the regulation of the internal structure of the cladding layer of the pipeline; S3. When multiple layers of cladding are required, except for the last layer, the cladding surface needs to be post-heat treated after each layer of cladding and then polished to remove slag and spatter; S4. After the surfacing is completed, heat treatment is carried out and non-destructive testing is passed, and the surfacing process is completed.

2. The pipeline outer wall cladding process according to claim 1, It is characterized in that In step S2, the welding direction is from one end of the pipe to the other end along a spiral trajectory.

3. The pipeline outer wall cladding process according to claim 2, It is characterized in that When there are requirements for the thickness of the pipeline, multi-layer cladding should be used to meet the thickness requirements.

4. The pipeline outer wall cladding process according to claim 1, It is characterized in that The inclination angle between the welding wire and the pipeline surface in step S2 is determined according to the surfacing material and the welding environment.

5. The pipeline outer wall surfacing process according to claim 3 or 4, It is characterized in that The microscopic crystals of the surfacing layer of the pipeline are columnar crystals, the direction of the columnar crystals is the same as the direction of the welding wire, and the arrangement of the columnar crystals is uniformly distributed in the surfacing layer.

Citation Information

Patent Citations

  • Surfacing welding method for abraded large roll shaft

    CN105382378A

  • Main circuit of nuclear main pump test bench and inner wall surfacing welding and circumferential weld butt welding method of main circuit

    CN111151845A

  • Stress-reducing welding method for repairing metal pipeline on site

    CN112846460A

  • Pipeline outer wall surfacing welding process

    CN116652456A

  • Build-up repair welding method for austenite alloy pipe

    JP1989192495A