Multilayer film, vapor-deposited multilayer film, multilayer structure, packaging material, recovery composition, method for recovering multilayer structure, and method for manufacturing multilayer film

A polyolefin-based multilayer film composition with a high melt flow rate and specific ion content addresses die buildup and gas barrier issues, ensuring efficient production and recyclability while maintaining high gas barrier properties.

WO2024214755A1PCT designated stage expired Publication Date: 2024-10-17KURARAY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014607
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The production of multilayer films with gas barrier resin layers as the outermost layer often results in die buildup during manufacturing, leading to quality issues and insufficient gas barrier properties, especially when an inorganic vapor-deposited layer is laminated on the surface.

Method used

A multilayer film composition featuring a polyolefin-based resin with a high melt flow rate and specific ion content, combined with a gas barrier resin like EVOH or PA, which reduces die buildup and enhances recyclability by improving the affinity with metal surfaces and maintaining high gas barrier properties.

Benefits of technology

The solution effectively suppresses die buildup during production, maintains excellent gas barrier properties, and facilitates recyclability, ensuring the quality and efficiency of the multilayer film production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a multilayer film in which die build-up during manufacturing is suppressed and which has excellent gas barrier properties and recycling properties. This multilayer film has a layer (X) as an outermost layer and at least one layer different from the layer (X), wherein: the layer (X) is composed of only a resin composition (A) that contains at least one gas barrier resin (a) selected from the group consisting of PA and vinyl alcohol-based resins and a polyolefin (b) having an MFR of at least 3.0 g / 10 min at 190ºC under a load of 2.160 kg, as measured in accordance with JIS K7210-1 (2014); and the resin composition (A) contains 0.1-20 parts by mass of the polyolefin (b) with respect to 100 parts by mass of the gas barrier resin (a).
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer film, vapor-deposited multilayer film, multilayer structure, packaging material, recovered composition, recovery method for multilayer structure, and method for producing multilayer film

[0001] The present invention relates to a multilayer film, a vapor-deposited multilayer film, a multilayer structure, and a packaging material, a recovery composition, and a recovery method using the same.

[0002] Packaging materials for long-term storage of foods and other foods often require gas barrier properties, including oxygen barrier properties. The use of packaging materials with high gas barrier properties can prevent oxidative deterioration of foods and other foods due to oxygen intrusion and the proliferation of microorganisms. Metal foils or metal vapor-deposited layers such as aluminum, and inorganic oxide vapor-deposited layers such as silicon oxide and aluminum oxide are widely used as layers for improving gas barrier properties. Meanwhile, resin layers with gas barrier properties, such as vinyl alcohol polymers and polyvinylidene chloride, are also widely used. Vinyl alcohol polymers exhibit gas barrier properties by crystallizing and densifying due to hydrogen bonding between hydroxyl groups in the molecules. Among these, ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as "EVOH") are suitable for melt molding due to their excellent thermal stability. Therefore, with the development of coextrusion technology, multilayer films with an EVOH layer as an intermediate layer have become widely used as gas barrier packaging materials (Patent Document 1).

[0003] Furthermore, in recent years, driven by environmental and waste issues, there has been a growing global demand for post-consumer recycling (hereinafter sometimes simply referred to as "recycling"), which involves recovering and recycling packaging materials consumed in the market. Recycling typically involves shredding recovered packaging materials, separating and cleaning them as necessary, and then melt-mixing them using an extruder. The pellets obtained in this manner are then used to manufacture various molded products. In this regard, packaging materials are required to be composed of as single a material as possible (mono-materialization), which allows for the production of high-purity, high-quality recycled resins. To this end, there has been an increasing demand for barrier films primarily made of polyolefins, which are widely used as packaging materials. To achieve extremely high gas barrier properties, a vapor-deposited multilayer film has also been proposed (Patent Document 2), in which an inorganic vapor-deposited layer is laminated on the surface of an EVOH layer of a polyolefin-based multilayer film, the outermost layer of which is EVOH.

[0004] International Publication No. 2020 / 071513 International Publication No. 2021 / 261560

[0005] When a multilayer film having a gas barrier resin layer as the outermost layer is produced by melt molding, the gas barrier resin with high metal affinity is likely to remain inside the die, causing viscosity changes and degradation. Furthermore, the gas barrier resin is likely to expand in volume at the die exit and come into contact with the die exit. Therefore, when a multilayer film having a gas barrier resin layer as the outermost layer is produced by melt molding, deposits (die buildup) may form at the die exit, adversely affecting the quality of the resulting multilayer film. Furthermore, if die buildup occurs, cleaning to remove this die buildup may be necessary. Furthermore, when an inorganic vapor deposition layer is laminated on the surface of the gas barrier resin layer of such a multilayer film, the gas barrier property may be insufficient.

[0006] In view of these circumstances, a first object of the present invention is to provide a multilayer film that suppresses die buildup during production and has excellent gas barrier properties and recyclability, and a method for producing the same. A second object of the present invention is to provide, using the multilayer film, a vapor-deposited multilayer film that has excellent gas barrier properties and recyclability, a multilayer structure, and a packaging material containing the multilayer structure. A third object of the present invention is to provide a recovered composition containing recovered material from the multilayer structure, and a method for recovering the same.

[0007] The present inventors have intensively investigated combinations of various resin compositions and laminate structures and have found that, when producing a multilayer film in which a gas barrier resin layer is the outermost layer, die buildup during production can be suppressed and a multilayer film with excellent gas barrier properties and recyclability can be obtained by using a gas barrier resin composition containing a specific polyolefin. They have also found that the use of this multilayer film can produce vapor-deposited multilayer films and multilayer structures with excellent gas barrier properties and recyclability, and have thus completed the present invention. That is, the object is to provide a multilayer film having a layer (X) as an outermost layer and at least one layer different from the layer (X), wherein the layer (X) is a layer made only of a resin composition (A) containing at least one gas barrier resin (a) selected from the group consisting of polyamide (hereinafter sometimes abbreviated as "PA") and vinyl alcohol-based resins, and a polyolefin (b) having a melt flow rate of 3.0 g / 10 min or more at 190°C under a load of 2.160 kg, as measured in accordance with JIS K7210-1 (2014), and wherein the resin composition (A) contains 0.1 parts by mass or more and 20 parts by mass or less of the polyolefin (b) per 100 parts by mass of the gas barrier resin (a); [2] The multilayer film of [1], wherein the gas barrier resin (a) is at least one selected from the group consisting of nylon 6 / 66 and EVOH; [3] The multilayer film of [1], wherein the gas barrier resin (a) is EVOH having an ethylene unit content of 20 to 50 mol% and a saponification degree of 90 mol% or more; [4] The multilayer film of any of [1] to [3], wherein the polyolefin (b) has a melt flow rate of 10 g / 10 min or more at 190°C under a load of 2.160 kg, measured in accordance with JIS K7210-1 (2014); [5] The multilayer film of any of [1] to [4], wherein the polyolefin (b) is an ethylene-vinyl acetate copolymer (hereinafter sometimes abbreviated as "EVA") having an ethylene unit content of 75 to 98 mol% or more or a saponified product thereof; [6] The multilayer film of [5], wherein the polyolefin (b) is a saponified EVA having a saponification degree of 30 mol% or more; [7] The multilayer film of any of [1] to [6], wherein the number average molecular weight (Mn) of the polyolefin (b) is 3,000 to 25,000;[8] The multilayer film of any one of [1] to [7], wherein the resin composition (A) contains 40 ppm to 500 ppm of alkali metal ions (c); [9] The multilayer film of any one of [1] to [8], wherein the resin composition (A) contains 20 ppm to 2000 ppm of at least one polyvalent metal ion (d) selected from the group consisting of magnesium ions, calcium ions, and zinc ions;

[10] The multilayer film of any one of [1] to [9], wherein the layer (X) is a layer obtained by melt-molding pellets consisting of only the resin composition (A);

[11] The multilayer film of any of [1] to

[10] , which has a layer (Y) and a layer (Z) as layers different from the layer (X), wherein the layer (Y) contains an adhesive resin (B) having a melting point of less than 170°C as a main component, and the layer (Z) contains a polyolefin resin (C) having a melting point of less than 170°C as a main component, and the layer (X), the layer (Y), and the layer (Z) are laminated in this order;

[12] The multilayer film of

[11] , wherein the adhesive resin (B) is acid-modified polyethylene or acid-modified polypropylene;

[13] The multilayer film of

[11] , wherein the polyolefin resin (C) is polyethylene or polypropylene;

[14] The multilayer film of any of [1] to

[13] , wherein the weight loss W of the resin composition (A) when maintained at 200°C for 30 minutes in a nitrogen atmosphere is 0.01 to 0.3% in thermogravimetry (TG);

[15] Any of the multilayer films of [1] to

[14] , which does not have a layer containing as a main component a resin having a melting point of 200°C or higher and a metal layer having an average thickness of 1 μm or higher;

[16] Any of the multilayer films of [1] to

[15] , in which the average thickness of layer (X) is 0.2 μm or higher and lower than 20 μm, and the ratio of the average thickness of layer (X) to the average thickness of the multilayer film is less than 25%;

[17] Any of the multilayer films of [1] to

[16] , in which the multilayer film is not stretched;

[18] Any of the multilayer films of [1] to

[16] , in which the multilayer film is stretched uniaxially by 3 times or higher and lower than 12 times;

[19] Any of the multilayer films of [1] to

[16] , in which the multilayer film is stretched biaxially by 3 times or higher and lower than 12 times;

[20] Any of the multilayer films of [1] to

[19] , in which the ratio of the total average thickness of layers containing as a main component a polyethylene-based resin or a polypropylene-based resin is 75% or higher;

[21] A vapor-deposited multilayer film comprising the multilayer film of any one of [1] to

[20] and an inorganic vapor-deposited layer (I) laminated on the exposed surface of the layer (X) in the multilayer film;

[22] The vapor-deposited multilayer film of

[21] , wherein the inorganic vapor-deposited layer (I) is a metal vapor-deposited layer containing aluminum as the main component or an inorganic oxide vapor-deposited layer containing alumina or silica as the main component;

[23] The vapor-deposited multilayer film of

[21] , wherein the oxygen transmission rate measured in accordance with JIS K7126-2 (2006) under conditions of 20°C and 65% RH is 60 cc / (m); 2

[24] A multilayer structure obtained by laminating a multilayer film or a vapor-deposited multilayer film according to any one of [1] to

[23] and at least one resin layer (R) containing a thermoplastic resin (D) as a main component;

[25] The multilayer structure according to

[24] , wherein the thermoplastic resin (D) is polyethylene or polypropylene;

[26] A packaging material having the multilayer structure according to

[24] or

[25] ;

[27] A recovered composition comprising a recovered product of the multilayer structure according to

[24] or

[25] ;

[28] A method for recovering a multilayer structure, comprising a step of crushing the multilayer structure according to

[24] or

[25] and then melt-molding the crushed multilayer structure;

[29] A method for producing a multilayer film according to any one of [1] to

[20] , comprising a step of melt-kneading a gas barrier resin (a) and a polyolefin (b) to obtain resin composition (A) pellets, and a step of melt-molding the resin composition (A) pellets to form a layer (X); This is achieved by providing

[0008] According to the present invention, a multilayer film can be provided that exhibits excellent gas barrier properties and recyclability while suppressing die buildup during production. Furthermore, by using this multilayer film, a vapor-deposited multilayer film, a multilayer structure, and a packaging material using the same can be provided that exhibit excellent gas barrier properties and recyclability. Furthermore, because the multilayer structure has good recyclability, a recovered composition containing recovered material from the multilayer structure and a recovery method therefor can be provided. Here, "recyclability" in this specification means that when the recovered material from the multilayer structure or packaging material of the present invention is melt-kneaded to produce a recovered composition, gelation of the resin is suppressed, allowing for the efficient production of a recovered composition with excellent appearance, and this can be evaluated by the recovery test described in the Examples. Furthermore, "die buildup" in this specification refers to polymer deposits that occur on the gas barrier layer side of the die outlet.

[0009] Hereinafter, embodiments of the present invention will be described. Note that in the following description, specific materials (compounds, etc.) that exhibit specific functions may be exemplified, but the present invention is not limited to embodiments using such materials. Furthermore, the exemplified materials may be used alone or in combination, unless otherwise specified.

[0010] The multilayer film of the present invention has a layer (X) as an outermost layer and at least one layer different from layer (X), wherein layer (X) is a layer made solely of a resin composition (A) containing at least one gas barrier resin (a) selected from the group consisting of PA and vinyl alcohol-based resins, and a polyolefin (b) having a melt flow rate of 3.0 g / 10 min or more at 190°C under a load of 2.160 kg, as measured in accordance with JIS K7210-1 (2014), and wherein the resin composition (A) contains 0.1 to 20 parts by mass of polyolefin (b) per 100 parts by mass of the gas barrier resin (a).

[0011] At least one gas barrier resin (a) selected from the group consisting of PA and vinyl alcohol-based resins has excellent gas barrier properties, and the multilayer film of the present invention having layer (X) as the outermost layer can achieve high gas barrier properties. Furthermore, since the gas barrier resin (a) of the outermost layer has high affinity with the inorganic vapor-deposited layer (I) described below, the vapor-deposited film of the present invention tends to exhibit high gas barrier properties stably. On the other hand, the gas barrier resin (a) has a problem in that die buildup is likely to occur during the production of the multilayer film, possibly due to its high affinity with the metal surface of an extruder or the like. Therefore, it has been difficult to simultaneously produce a multilayer film having gas barrier resin (a) in the outermost layer and stable production with suppressed die buildup. Therefore, the present inventors conducted extensive research and found that by using a resin composition (A) containing a polyolefin (b) having a melt flow rate of 3.0 g / 10 min or more according to JIS K7210-1 (2014) (190°C, 2.160 kg load), the slipperiness between the metal surface of an extruder or the like and the molten resin during the production of a multilayer film is improved, resulting in the suppression of die buildup during production. Generally, die buildup occurs when the pressure of the molten resin received within the die is released at the die exit, causing volume expansion and adhesion of the molten resin to the die lip surface, and is not due to thermal degradation due to retention within the extruder, etc. The higher the stress received by the resin within the die, the more likely it is that volume expansion at the die exit will occur. In the present invention, since layer (X), which is the outermost layer, contains polyolefin (b), the frictional force between the gas barrier resin (a) having polar groups and the inner metal wall surface of the die is reduced, and the stress received by the gas barrier resin (a) is reduced, which is thought to result in suppression of volume expansion of the molten gas barrier resin (a) and the effect of reducing die build-up.

[0012] In this specification, "Layer (X), Layer (Y), and Layer (Z) are laminated adjacently in this order" means that adjacent layers are directly laminated. Specifically, it means that Layer (X), Layer (Y), and Layer (Z) are laminated in this order, with Layer (X) and Layer (Y) directly laminated, and Layer (Y) and Layer (Z) directly laminated. "Major component" refers to a component present in an amount of more than 50% by mass. Unless otherwise specified, the "average thickness" of each layer refers to the average thickness measured at any five locations. "ppm" refers to the mass content (ppm by mass). "Polyethylene" refers to ethylene homopolymers, copolymers of 80 mol% or more ethylene and 20 mol% or less α-olefin monomers, and copolymers of 90 mol% or more ethylene and less than 10 mol% non-olefin monomers whose functional groups contain atoms other than carbon, oxygen, and hydrogen atoms. "Polypropylene" refers to a propylene homopolymer, a copolymer of 80 mol% or more propylene and 20 mol% or less α-olefin monomer, and a copolymer of 90 mol% or more propylene and less than 10 mol% non-olefin monomer whose functional groups contain no atoms other than carbon, oxygen, and hydrogen atoms. "Acid-modified polyethylene" refers to a polymer obtained by modifying polyethylene with acid. Acid-modified polyethylene may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into polyethylene. "Acid-modified polypropylene" refers to a polymer obtained by modifying polypropylene with acid. Acid-modified polypropylene may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into polypropylene. "Polyethylene-based resin" refers to polyethylene and modified polyethylene (such as acid-modified polyethylene). Modified polyethylene refers to a polymer obtained by modifying polyethylene. "Polypropylene-based resin" refers to polypropylene and modified polypropylene (such as acid-modified polypropylene). Modified polypropylene refers to a polymer obtained by modifying polypropylene. Furthermore, the term "surface (or surface layer)" in a multilayer film or a multilayer structure does not refer to the front or back, but refers to the exposed surface. In other words, a multilayer film or a multilayer structure has two surfaces.Similarly, multilayer films and multilayer structures have two outermost layers. In this specification, "consisting essentially of" means that optional components may be included to the extent that they do not affect the effects of the present invention, and "consisting only of" means that optional components other than impurities that are inevitably included are excluded. In this specification, a numerical range described using "to" means that the numerical values ​​before and after "to" are included as the lower and upper limits.

[0013] <Layer (X)> The multilayer film of the present invention has, as its outermost layer, a layer (X) consisting solely of a resin composition (A) containing at least one gas barrier resin (a) selected from the group consisting of PA and vinyl alcohol-based resins, and a polyolefin (b) having a melt flow rate of 3.0 g / 10 min or more according to JIS K7210-1 (2014; 190°C, 2.160 kg load). The resin composition (A) contains 0.1 to 20 parts by mass of the polyolefin (b) per 100 parts by mass of the gas barrier resin (a).

[0014] <Gas Barrier Resin (a)> The gas barrier resin (a) is at least one selected from the group consisting of PA and vinyl alcohol-based resins. The presence of the gas barrier resin (a) improves the gas barrier properties of the multilayer film. Furthermore, since the gas barrier resin (a) has a high affinity with the inorganic vapor deposition layer (I) described below, the multilayer film of the present invention, which has as its outermost layer a layer (X) consisting solely of a resin composition (A) containing the gas barrier resin (a), can easily provide the inorganic vapor deposition layer (I) on the layer (X), and the vapor-deposited multilayer film having the inorganic vapor deposition layer (I) tends to stably exhibit good gas barrier properties.

[0015] Examples of PA include polycaproamide (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecaneamide (nylon 11), polylauryllactam (nylon 12), polyethylenediamineadipamide (nylon 26), polytetramethyleneadipamide (nylon 46), polyhexamethyleneadipamide (nylon 66), polyhexamethylenesebacamide (nylon 610), and polyhexamethylenedodecaamide (nylon 612). , polyoctamethylene adipamide (nylon 86), polydecamethylene adipamide (nylon 106), caprolactam / lauryllactam copolymer (nylon 6 / 12), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylenediammonium adipate copolymer (nylon 6 / 66), lauryllactam / hexamethylenediammonium adipate copolymer (nylon 12 / 66), ethylenediammonium adipate / hexamethylenediammonium adipate ammonium adipate copolymer (nylon 26 / 66), caprolactam / hexamethylenediammonium adipate / hexamethylenediammonium sebacate copolymer (nylon 6 / 66 / 610), ethylenediammonium adipate / hexamethylenediammonium adipate / hexamethylenediammonium sebacate copolymer (nylon 26 / 66 / 610), polyhexamethylene isophthalamide (nylon 6I), polyhexamethylene terephthalamide (nylon 6T), hexamethylene Examples of such PAs include ethylene isophthalamide / hexamethylene terephthalamide copolymer (nylon 6I / 6T), 11-aminoundecanamide / hexamethylene terephthalamide copolymer, polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyhexamethylene cyclohexylamide, polynonamethylene cyclohexylamide, and those PAs modified with aromatic amines such as methylenebenzylamine and metaxylylenediamine. Further examples include metaxylylenediammonium adipate.Among these, nylon 6 / 66 or nylon 6 is preferred as the PA because it is excellent in all of economy, melt moldability, and mechanical properties, and nylon 6 / 66 is more preferred as the PA from the viewpoint of recyclability of the multilayer film.

[0016] The vinyl alcohol-based resin may be a polymer in which the content (mol %) of vinyl alcohol units relative to all monomer units exceeds 50 mol %. Examples of vinyl alcohol-based resins include polyvinyl alcohol (hereinafter sometimes abbreviated as "PVA") and ethylene-vinyl alcohol copolymer (EVOH). From the viewpoint of melt moldability, the vinyl alcohol-based resin is preferably EVOH. In particular, from the viewpoint of achieving particularly balanced improvements in gas barrier properties, melt moldability, and recyclability, EVOH having an ethylene unit content of 20 to 50 mol % and a saponification degree of 90 mol % or more is more preferred.

[0017] PVA is a polymer obtained by saponifying polyvinyl ester, which is usually obtained by polymerizing vinyl ester.

[0018] The viscosity average degree of polymerization of the PVA is preferably 400 or more and 2000 or less. The lower limit of the viscosity average degree of polymerization is more preferably 500, and even more preferably 700. When the viscosity average degree of polymerization is equal to or more than the lower limit, the adhesiveness and thermal stability of the PVA are improved. The upper limit of the viscosity average degree of polymerization is more preferably 1500, and even more preferably 1000. When the viscosity average degree of polymerization is equal to or less than the upper limit, the melt moldability of the PVA is improved.

[0019] The viscosity-average degree of polymerization of PVA is measured in accordance with JIS K6726 (1994). Specifically, the intrinsic viscosity [η] (liters / g) of PVA is measured in water at 30°C, and the viscosity-average degree of polymerization P is calculated using the intrinsic viscosity [η] value according to the following formula. When the saponification degree of PVA is less than 99.5 mol%, the PVA is saponified to a saponification degree of 99.5 mol% or more, and then the intrinsic viscosity [η] is measured. P = ([η] x 10 4 / 8.29) (1/0.62)

[0020] The saponification degree of the PVA is preferably 70 mol% or more, more preferably 75 mol%, and even more preferably 85 mol% or more. The saponification degree of the PVA refers to the ratio of the number of vinyl alcohol units to the total number of vinyl alcohol units and vinyl ester units in the PVA. When the saponification degree is 70 mol% or more, the water solubility of the PVA is excellent, and the peelability in the separation step of the multilayer structure is improved. The saponification degree of the PVA is preferably 95 mol% or less, more preferably 93 mol% or less, and even more preferably 90 mol% or less. When the saponification degree is 95 mol% or less, the melt moldability of the PVA is excellent. The saponification degree of the PVA is measured in accordance with JIS K6726 (1994).

[0021] The total content of vinyl alcohol units and vinyl ester units in all monomer units constituting the PVA is preferably 95 mol% or more. When the total content is 95 mol% or more, the solubility of the PVA in water is further improved, and as a result, the separability of the multilayer structure is further improved. The total content of vinyl alcohol units and vinyl ester units is more preferably 97 mol% or more, even more preferably 98 mol% or more, and particularly preferably 99 mol% or more.

[0022] The PVA may contain a monomer unit other than the vinyl alcohol unit and the vinyl ester unit, provided that the effect of the present invention is not impaired. Examples of such a monomer include α-olefins such as ethylene units, propylene, n-butene, and isobutylene; acrylic acid and its salts; acrylic acid esters; methacrylic acid and its salts; methacrylic acid esters; acrylamide; acrylamide derivatives such as N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid and its salts, acrylamidopropyldimethylamine and its salts or quaternary salts thereof, and N-methylolacrylamide and its derivatives; methacrylamide; N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropanesulfonic acid and its salts, methacrylamidepropyldimethylamine and its salts or quaternary salts thereof, and N-methylolacrylamide. Examples of suitable PVA monomers include methacrylamide derivatives such as methylol methacrylamide and its derivatives; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether; nitriles such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride and vinyl fluoride; vinylidene halides such as vinylidene chloride and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; unsaturated dicarboxylic acids and their salts or esters such as maleic acid, itaconic acid, and fumaric acid; vinyl silyl compounds such as vinyltrimethoxysilane; and isopropenyl acetate. The content of these monomers varies depending on the purpose and application, but is preferably 10 mol% or less, more preferably less than 5 mol%, even more preferably less than 1 mol%, particularly preferably less than 0.5 mol%, and may even be 0 mol%. One type of PVA may be used alone, or two or more types may be used.

[0023] EVOH is a polymer obtained by saponifying an ethylene-vinyl ester copolymer, which is usually obtained by polymerizing ethylene and a vinyl ester.

[0024] The ethylene unit content of EVOH is preferably 20 to 50 mol%. An ethylene unit content of 20 mol% or more improves the melt moldability of EVOH and pulverized products of multilayer films and multilayer structures containing EVOH. The ethylene unit content is preferably 23 mol% or more, more preferably 26 mol% or more, and may be 29 mol% or more, 32 mol% or more, 35 mol% or more, or 38 mol% or more. On the other hand, an ethylene unit content of 50 mol% or less improves the gas barrier properties of the multilayer film of the present invention. The ethylene unit content is preferably 46 mol% or less, more preferably 42 mol% or less, and may be 38 mol% or less, 34 mol% or less, or 30 mol% or less. The ethylene unit content is the content (mol%) of ethylene units relative to all monomer units constituting EVOH.

[0025] The saponification degree of EVOH is preferably 90 mol% or more. The saponification degree of EVOH means the ratio of the number of vinyl alcohol units to the total number of vinyl alcohol units and vinyl ester units in EVOH. When the saponification degree is 90 mol% or more, the gas barrier property of the multilayer film of the present invention is improved. The saponification degree is preferably 95 mol% or more, more preferably 99 mol% or more, and even more preferably 99.9 mol% or more. The upper limit of the saponification degree of EVOH may be 100 mol%. The ethylene unit content and saponification degree of EVOH are 1 It is determined by H-NMR measurement.

[0026] The EVOH may be a mixture of two or more types of EVOH having different ethylene unit contents. In this case, the difference in ethylene unit content between the EVOHs having the most different ethylene unit contents is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less, and may be 3 mol% or more. Similarly, the EVOH may be a mixture of two or more types of EVOH having different saponification degrees. In this case, the difference in saponification degree between the EVOHs having the most different ethylene unit contents is preferably 7 mol% or less, more preferably 5 mol% or less, and may be 0.5 mol% or more. When it is desired to achieve both thermoformability and gas barrier properties at a higher level, it is preferable to use a mixture of EVOH (less than 34 mol%) having an ethylene unit content of 24 mol% or more and less than 34 mol% and a degree of saponification of 99 mol% or more and EVOH (34 mol% or more) having an ethylene unit content of 34 mol% or more and less than 50 mol% and a degree of saponification of 99 mol% or more, in a blending mass ratio (less than 34 mol% / 34 mol% or more) of 60 / 40 to 90 / 10.

[0027] The EVOH may have a melting point of 150°C or higher but lower than 190°C, or may have a melting point lower than 150°C. The melting point of EVOH lower than 150°C may improve the appearance and interlayer adhesion of a multilayer film having layer (X) as the outermost layer. This is thought to be because the melting point of EVOH lower than 150°C improves the fluidity of polymer chains, thereby effectively alleviating stress even at relatively low temperatures during secondary processing such as melt molding and stretching, and maintaining adhesive reaction activity with adjacent layers. From the viewpoint of more pronounced effects of the present invention, the melting point of EVOH is preferably lower than 140°C, more preferably lower than 130°C, and may be lower than 125°C or lower than 120°C. On the other hand, from the viewpoint of processability during secondary processing such as melt molding and stretching, and heat resistance as a packaging material, the melting point of EVOH is preferably higher than 80°C, more preferably higher than 90°C, and even more preferably higher than 100°C. The melting point of EVOH can be controlled by one or a combination of the following methods, but in the present invention, the following method (3) is a preferred example: (1) Changing the ethylene unit content (increasing the ethylene unit content decreases the melting point). (2) Changing the degree of saponification (decreasing the degree of saponification decreases the melting point). (3) Introducing a modifying group containing a primary hydroxyl group (introducing a modifying group containing a primary hydroxyl group decreases the melting point).

[0028] The primary hydroxyl group-containing modifying group used in (3) above is preferably a primary hydroxyl group-containing modifying group represented by the following general formula (I). The degree of melting point reduction per introduction rate of the modifying group varies depending on the structure of the primary hydroxyl group-containing modifying group introduced. However, the introduction of 1 mol % of the primary hydroxyl group-containing modifying group represented by the following general formula (I) generally reduces the melting point by approximately 6 to 9°C. Controlling the melting point in this manner can lower the melting point while relatively maintaining gas barrier properties and thermal stability. Furthermore, deterioration in interlayer adhesion with the layer (Y) and inorganic vapor deposition layer (I), described below, is also suppressed, resulting in a multilayer film with particularly excellent quality and performance. This is thought to be due to the fact that the melting point can be lowered while maintaining the hydroxyl group content, and the primary hydroxyl group has high adhesive reactivity with the layer (Y) and inorganic vapor deposition layer (I), described below. The content of the modifying group containing a primary hydroxyl group in EVOH may be adjusted as appropriate, taking into consideration the balance between the melting point and various physical properties, but a content of 2 mol% or more and less than 20 mol% often results in a good balance of physical properties. The lower limit of the content of the modifying group containing a primary hydroxyl group in EVOH is more preferably 3 mol%. On the other hand, the upper limit of the content of the modifying group containing a primary hydroxyl group in EVOH is more preferably 10 mol%, and even more preferably 8 mol%. The modifying group containing a primary hydroxyl group can be introduced by copolymerization or polymer reaction. The "content of the modifying group containing a primary hydroxyl group in EVOH" may be the content (mol%) of monomer units containing a primary hydroxyl group relative to all monomer units constituting EVOH.

[0029] [wherein X is a hydrogen atom, a methyl group, or R 2 represents a group represented by —OH. 1 and R 2 each independently represents a single bond, an alkylene group having 1 to 9 carbon atoms, or an alkyleneoxy group having 1 to 9 carbon atoms, and the alkylene group and the alkyleneoxy group may contain a hydroxyl group, an alkoxy group, or a halogen atom.]

[0030] In general formula (I), X is preferably a hydrogen atom or R 2 R is a group represented by —OH, and more preferably a hydrogen atom. 1is preferably a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkyleneoxy group having 1 to 5 carbon atoms, and more preferably a methylmethyleneoxy group (—O—C(CH 3 )H)-). R 1 When is an alkyleneoxy group, the oxygen atom of the alkyleneoxy group is usually bonded to a carbon atom of the main chain.

[0031] EVOH may contain other monomer units other than ethylene units, vinyl ester units, vinyl alcohol units, and the modifying group containing a primary hydroxyl group, as long as the effects of the present disclosure are not impaired. The content of other monomer units is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably substantially none. Examples of such other monomers include alkenes such as propylene, butylene, pentene, and hexene; 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, and the like. 1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, 5,6-diacyloxy-1-hexene, 1,3-diacetoxy-2-methyl- Examples of suitable vinyl silane compounds include alkenes having an ester group such as ethylenepropane or saponified products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, or the like, or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, and methallylsulfonic acid, or their salts; vinyl silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and γ-methacryloxypropylmethoxysilane; alkyl vinyl ethers, vinyl ketone, N-vinylpyrrolidone, vinyl chloride, and vinylidene chloride.

[0032] The EVOH may be post-modified by a method such as urethanization, acetalization, cyanoethylation, or oxyalkylenation.

[0033] The MFR (190°C, under a load of 2.160 kg) of EVOH measured in accordance with JIS K7210-1 (2014) is preferably 0.2 to 20 g / 10 min. The MFR of EVOH is more preferably 0.5 g / 10 min or more, and even more preferably 0.8 g / 10 min or more. On the other hand, the MFR of EVOH is more preferably 15 g / 10 min or less, even more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, and particularly preferably 3 g / 10 min or less. When the MFR of EVOH is within the above range, the melt moldability of EVOH and pulverized products of multilayer films and multilayer structures containing EVOH is improved.

[0034] The proportion of EVOH in the gas barrier resin (a) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable that the gas barrier resin (a) is EVOH.

[0035] The gas barrier resin (a) may be used alone or in combination of two or more kinds.

[0036] The gas barrier resin (a) is preferably the main component of the layer (X). When the gas barrier resin (a) is the main component of the layer (X), the gas barrier properties of the multilayer film are further improved. The lower limit of the content of the gas barrier resin (a) in the layer (X) is preferably 70% by mass, more preferably 80% by mass, even more preferably 90% by mass, even more preferably 95% by mass, and particularly preferably 97% by mass. The upper limit of the content of the gas barrier resin (a) in the layer (X) is preferably 99.8% by mass, more preferably 99.5% by mass, and even more preferably 99.0% by mass.

[0037] <Polyolefin (b)> The resin composition (A) of the present invention contains a polyolefin (b) having a melt flow rate (MFR) of 3.0 g / 10 min or more according to JIS K7210-1 (2014; 190°C, 2.160 kg load). If the MFR is less than 3.0 g / 10 min, die buildup cannot be sufficiently suppressed during the production of a multilayer film. The MFR of the polyolefin (b) is preferably 5 g / 10 min or more, more preferably 10 g / 10 min or more, even more preferably 50 g / 10 min or more, particularly preferably 100 g / 10 min or more, and may be 130 g / 10 min or more, 170 g / 10 min or more, or 180 g / 10 min or more. For convenience of measurement, the accuracy of the MFR decreases when it exceeds 1000 g / 10 min, and therefore, in this specification, when the MFR exceeds 1000 g / 10 min, the melt viscosity is defined by a different measurement method (BL type viscometer). When the MFR of polyolefin (b) is 1000 g / 10 min or less, the MFR of polyolefin (b) may be 1000 g / 10 min or less, 500 g / 10 min or less, or 300 g / 10 min or less.

[0038] When the MFR of the polyolefin (b) exceeds 1000 g / 10 min, the melt viscosity of the polyolefin (b) measured at 140°C with a BL type viscometer is preferably 300 to 10000 mPa s, more preferably 1500 to 8000 mPa s, and even more preferably 3000 to 6000 mPa s.

[0039] The polyolefin (b) may be a polymer having an olefin unit content (mol%) of more than 50 mol% relative to the total monomer units. The lower limit of the olefin unit content relative to the total monomer units in the polyolefin (b) is preferably 60 mol%, more preferably 70 mol%, even more preferably 75 mol%, even more preferably 80 mol%, and may be 85 mol%, 90 mol%, or 92 mol%. The upper limit of the olefin unit content relative to the total monomer units in the polyolefin (b) may be 100 mol%, or may be 99 mol%, 98 mol%, 97 mol%, or 96 mol%.

[0040] Examples of the polyolefin (b) include polyethylene, polypropylene, poly(1-butene), poly(4-methyl-1-pentene), a copolymer of a polyolefin and maleic anhydride, EVA or a saponified product thereof, an ethylene-acrylic acid ester copolymer, or a modified polyolefin obtained by graft-modifying any of these with an unsaturated carboxylic acid or a derivative thereof. Among these, from the viewpoint of exhibiting the effect of suppressing die build-up, at least one selected from the group consisting of polyethylene, polypropylene, EVA, and a saponified EVA is preferred, at least one selected from the group consisting of polyethylene, EVA, and a saponified EVA is more preferred, at least one selected from the group consisting of polyethylene and a saponified EVA is even more preferred, and a saponified EVA is particularly preferred from the viewpoint of recyclability.

[0041] When the polyolefin (b) is EVA or a saponified product thereof, the ethylene unit content is preferably 75 mol% or more and 98 mol% or less from the viewpoint of exhibiting the effect of suppressing die buildup. When the ethylene unit content is within the above range, the occurrence of die buildup during the production of a multilayer film tends to be further suppressed. The ethylene unit content of EVA or a saponified product thereof is more preferably 85 mol% or more and 96 mol% or less. The ethylene unit content of EVA or a saponified product thereof is 1 It is determined by H-NMR measurement.

[0042] When the polyolefin (b) is a saponified EVA, the saponification degree is preferably 30 mol% or more, more preferably 50 mol% or more, even more preferably 70 mol% or more, and particularly preferably 85 mol% or more, from the viewpoint of suppressing die buildup. On the other hand, the saponification degree is preferably 99 mol% or less. The saponification degree of the saponified EVA is 1 It is determined by H-NMR measurement.

[0043] From the viewpoint of suppressing die buildup, the number average molecular weight (hereinafter sometimes abbreviated as Mn) of the polyolefin (b) is preferably 3,000 to 25,000. The Mn of the polyolefin (b) is more preferably 5,000 to 22,500, and even more preferably 10,000 to 20,000. The Mn of the polyolefin (b) can be determined by GPC measurement.

[0044] When the polyolefin (b) is polyethylene, the MFR of the polyolefin (b) is preferably greater than 1,000 g / 10 min. That is, when the polyolefin (b) is polyethylene, the melt viscosity of the polyolefin (b) measured at 140°C with a BL-type viscometer is preferably 300 to 10,000 mPa s, more preferably 1,500 to 8,000 mPa s, and even more preferably 3,000 to 6,000 mPa s. When the polyolefin (b) is a saponified EVA, the MFR of the polyolefin (b) is more preferably 10 g / 10 min or more, even more preferably 50 g / 10 min or more, particularly preferably 100 g / 10 min or more, and may be 150 g / 10 min or more. When the polyolefin (b) is a saponified EVA, the MFR of the polyolefin (b) is preferably 500 g / 10 min or less, more preferably 400 g / 10 min or less, even more preferably 300 g / 10 min or less, and particularly preferably 250 g / 10 min or less.

[0045] The resin composition (A) contains 0.1 parts by mass or more and 20 parts by mass or less of polyolefin (b) per 100 parts by mass of the gas barrier resin (a). The content of the polyolefin (b) is preferably 12 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, and may be 4 parts by mass or less or 3 parts by mass or less. When the content of the polyolefin (b) is equal to or less than the upper limit, gas barrier properties and recyclability tend to be improved. Furthermore, the content of the polyolefin (b) is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more. When the content of the polyolefin (b) is equal to or more than the lower limit, die buildup tends to be further suppressed.

[0046] <Alkali Metal Ions (c)> The resin composition (A) preferably contains 40 to 500 ppm of alkali metal ions (c). When the resin composition (A) contains alkali metal ions (c) in the above range, the interlayer adhesion with the layer (Y), which will be described later, tends to be significantly improved. When the alkali metal ions (c) are 40 ppm or more, the recyclability tends to be improved. On the other hand, when the content of alkali metal ions (b) is 500 ppm or less, the recyclability and the hue of the recovered composition tend to be improved. The lower limit of the content of alkali metal ions (c) is more preferably 80 ppm, and even more preferably 120 ppm. The upper limit of the content of alkali metal ions (c) is more preferably 400 ppm, and even more preferably 300 ppm. Furthermore, by controlling the content ratio of the alkali metal ions (c) to the carboxylic acid, which will be described later, the melt moldability and color resistance of the resulting resin composition can be further improved.

[0047] Examples of the alkali metal ion (c) include ions of lithium, sodium, potassium, rubidium, cesium, etc., but sodium or potassium ions are preferred from the viewpoint of industrial availability. These ions may be used alone or in combination of two or more.

[0048] Examples of alkali metal compounds that provide the alkali metal ions (c) include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, hydroxides, and metal complexes of alkali metals such as lithium, sodium, and potassium. Among these, aliphatic carboxylates and phosphates are more preferred because of their ease of availability and handling. Preferred aliphatic carboxylates are acetates, caprylates, and stearates.

[0049] <Polyvalent Metal Ion (d)> The resin composition (A) preferably contains 20 ppm to 2000 ppm of at least one polyvalent metal ion (d) selected from the group consisting of magnesium ions, calcium ions, and zinc ions. When the polyvalent metal ion (d) is contained in an amount of 20 ppm or more, thickening, gelation, and adhesion of the resin to the screw are suppressed, and the occurrence of die build-up during the production of a multilayer film tends to be further suppressed. The lower limit of the polyvalent metal ion (d) is more preferably 40 ppm, even more preferably 100 ppm, and particularly preferably 150 ppm. On the other hand, when the content of the polyvalent metal ion (d) is 2000 ppm or less, excessive decomposition and coloration during melt molding of the resin composition (A) tend to be suppressed, and the interlayer adhesion between the layer (X) and the layer (Y) can be maintained. The upper limit of the polyvalent metal ion (d) is more preferably 1500 ppm, even more preferably 1000 ppm, particularly preferably 500 ppm, and may be 300 ppm. The resin composition (A) preferably contains magnesium ions or calcium ions as the polyvalent metal ions (d), and more preferably contains calcium ions from the viewpoint of easily maintaining the quality of the resin composition (A) and from the viewpoint of coloring of the recovered composition. Furthermore, by controlling the content ratio of the polyvalent metal ions (d) to the carboxylic acid described below, the melt moldability and coloring resistance of the obtained resin composition (A) can be further improved.

[0050] Examples of polyvalent metal compounds that provide the polyvalent metal ions (d) include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, hydroxides, and metal complexes of magnesium, calcium, and zinc. Among these, aliphatic carboxylates and hydroxides are more preferred because of their ease of availability and handling. Preferred aliphatic carboxylates are acetates, caprylates, and stearates.

[0051] <Higher Aliphatic Carboxylic Acid (e)> The resin composition (A) preferably contains 100 to 25,000 ppm of a higher aliphatic carboxylic acid (e) having 8 to 30 carbon atoms. The higher aliphatic carboxylic acid (e) may be contained in part or in whole in the form of a salt, or as a salt with an alkali metal ion (c) or a polyvalent metal ion (d). The higher aliphatic carboxylic acid (e) is preferably caprylic acid or stearic acid. The multilayer film of the present invention has a layer (X) made of the resin composition (A) as the outermost layer. It is believed that the higher aliphatic carboxylic acid (e) acts as a lubricant for the die metal surface in the die, thereby suppressing poor appearance due to uneven thickness of the multilayer film and the occurrence of gels and bumps due to retained resin. For this reason, the resin composition (A) preferably contains 100 ppm or more of the higher aliphatic carboxylic acid (e). On the other hand, if the content of the higher aliphatic carboxylic acid (e) is 25,000 ppm or less, thickening of the resin composition (A) during melt molding tends to be suppressed and interlayer adhesion with the layer (Y) described below tends to be maintained. From these viewpoints, the content of the higher aliphatic carboxylic acid (e) is more preferably 200 to 20,000 ppm, and even more preferably 300 to 15,000 ppm.

[0052] The resin composition (A) may contain other components in addition to the gas barrier resin (a), polyolefin (b), alkali metal ions (c), polyvalent metal ions (d), and higher aliphatic carboxylic acids (e), as long as the effects of the present invention are not impaired. Examples of other components include alkaline earth metal ions and transition metal ions other than the polyvalent metal ions (d), carboxylic acids (monocarboxylic acids, polycarboxylic acids) other than the higher aliphatic carboxylic acids (e), thermoplastic resins other than the gas barrier resin (a) and polyolefin (b), phosphoric acid compounds, boron compounds, antioxidants (hindered phenol compounds, etc.), plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorizers, UV absorbers, antistatic agents, lubricants, colorants, fillers, desiccants, bulking agents, pigments, dyes, processing aids, flame retardants, antifogging agents, surfactants, crosslinking agents, fiber reinforcements, etc. From the viewpoint of suppressing coloration during melt molding of a pulverized multilayer film or multilayer structure containing the resin composition (A), it is preferable to contain a carboxylic acid and / or a phosphoric acid compound. Furthermore, by including a boron compound, the melt viscosity of the resin composition (A) and the pulverized product of the multilayer film or multilayer structure containing the resin composition (A) can be controlled.

[0053] <Carboxylic Acid> The resin composition (A) preferably contains a carboxylic acid other than the higher aliphatic carboxylic acid (e). The lower limit of the carboxylic acid content is preferably 50 ppm, more preferably 100 ppm. On the other hand, the upper limit of the carboxylic acid content is preferably 400 ppm, more preferably 350 ppm. When the carboxylic acid content is 50 ppm or more, the coloring resistance tends to be improved. On the other hand, when the carboxylic acid content is 400 ppm or less, the interlayer adhesion tends to be maintained and the generation of odor tends to be suppressed.

[0054] The pKa of the carboxylic acid is preferably 3.5 to 5.5. When the pKa of the carboxylic acid is within this range, the pH buffering ability of the resulting resin composition (A) is enhanced, further improving the melt moldability and further improving the coloration caused by acidic or basic substances.

[0055] The carboxylic acid may be a monocarboxylic acid. These may be used alone or in combination of two or more. A monocarboxylic acid is a compound having one carboxyl group in the molecule. Monocarboxylic acids having a pKa in the range of 3.5 to 5.5 are not particularly limited, and examples thereof include formic acid (pKa = 3.77), acetic acid (pKa = 4.76), propionic acid (pKa = 4.85), and acrylic acid (pKa = 4.25). These carboxylic acids may further have a substituent such as a hydroxyl group, an amino group, or a halogen atom. Among these, acetic acid is preferred because of its high safety and ease of availability and handling.

[0056] The carboxylic acid may be a polycarboxylic acid. When the carboxylic acid is a polycarboxylic acid, the discoloration resistance of the resin composition (A) at high temperatures and the discoloration resistance of the melt-molded product of the crushed material of the resulting multilayer structure may be further improved. It is also preferable that the polycarboxylic acid compound has three or more carboxyl groups. In this case, discoloration resistance may be more effectively improved. The polycarboxylic acid is a compound having two or more carboxyl groups in the molecule. In this case, it is preferable that the pKa of at least one carboxyl group is in the range of 3.5 to 5.5, and examples thereof include oxalic acid (pKa2=4.27), succinic acid (pKa1=4.20), fumaric acid (pKa2=4.44), malic acid (pKa2=5.13), glutaric acid (pKa1=4.30, pKa2=5.40), adipic acid (pKa1=4.43, pKa2=5.50), and the like. 2=5.41), pimelic acid (pKa1=4.71), phthalic acid (pKa2=5.41), isophthalic acid (pKa2=4.46), terephthalic acid (pKa1=3.51, pKa2=4.82), citric acid (pKa2=4.75), tartaric acid (pKa2=4.40), glutamic acid (pKa2=4.07), aspartic acid (pKa=3.90), etc.

[0057] <Phosphate Compound> The resin composition (A) may further contain a phosphate compound. The lower limit of the content of the phosphate compound is preferably 5 ppm in terms of phosphate radicals. On the other hand, the upper limit of the content of the phosphate compound is preferably 100 ppm in terms of phosphate radicals. By containing the phosphate compound in this range, coloration of the resulting resin composition (A) and the resulting melt-molded product of the pulverized multilayer film or multilayer structure may be suppressed, and thermal stability may be improved.

[0058] As the phosphate compound, various acids such as phosphoric acid and phosphorous acid and their salts can be used. The phosphate may be any of primary phosphate, secondary phosphate, and tertiary phosphate. The cation species of the phosphate is not particularly limited, but the cation species is preferably an alkali metal or alkaline earth metal. Among them, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are preferred as the phosphate compound.

[0059] <Boron Compound> The resin composition (A) may further contain a boron compound. When a boron compound is contained, the lower limit of the content in the resin composition (A) is preferably 50 ppm, more preferably 100 ppm, in terms of elemental boron. On the other hand, the upper limit of the content of the boron compound in the resin composition (A) is preferably 400 ppm, more preferably 200 ppm, in terms of elemental boron. By containing the boron compound within this range, the thermal stability of the resin composition (A) and the pulverized product of the resulting multilayer film or multilayer structure during melt molding may be improved, and the occurrence of gels and lumps may be suppressed. In addition, the drawdown resistance and neck-in resistance during film formation may be improved, and the mechanical properties of the resulting molded product may be improved. These effects are presumed to be due to the occurrence of a chelate interaction between the gas barrier resin (a) such as EVOH and the boron compound.

[0060] Examples of boron compounds include boric acid, boric acid esters, borate salts, and boron hydrides. 3 BO 3boric acid such as tetraboric acid, metaboric acid, and the like; boric acid esters such as trimethyl borate and triethyl borate; alkali metal salts or alkaline earth metal salts of the above boric acid; and boric acid salts such as borax. Of these, orthoboric acid is preferred.

[0061] <Hindered phenol compound> The resin composition (A) may further contain a hindered phenol compound as an antioxidant. When a hindered phenol compound is contained, the content of the hindered phenol compound in the resin composition (A) is preferably 1,000 to 10,000 ppm. When the content is 1,000 ppm or more, coloration, thickening, and gelation of the resin can be suppressed when the pulverized product of the multilayer film or multilayer structure is melt-molded. The content of the hindered phenol compound is more preferably 2,000 ppm or more. On the other hand, when the content of the hindered phenol compound is 10,000 ppm or less, coloration and bleed-out resulting from the hindered phenol compound can be suppressed. The content of the hindered phenol compound is more preferably 8,000 ppm or less.

[0062] The hindered phenol compound has at least one hindered phenol group. A hindered phenol group is a group in which a bulky substituent is bonded to at least one carbon atom adjacent to the carbon atom to which the hydroxyl group of a phenol is bonded. The bulky substituent is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably a t-butyl group.

[0063] The hindered phenol compound is preferably in a solid state at around room temperature. From the viewpoint of suppressing bleed-out of the compound, the melting point or softening temperature of the hindered phenol compound is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. From the same viewpoint, the molecular weight of the hindered phenol compound is preferably 200 or higher, more preferably 400 or higher, and even more preferably 600 or higher. Meanwhile, the molecular weight is usually 2000 or lower. Furthermore, from the viewpoint of facilitating mixing with the gas barrier resin (a) such as EVOH, the melting point or softening temperature of the hindered phenol compound is preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower.

[0064] The hindered phenol compound preferably has an ester bond or an amide bond. Examples of the hindered phenol compound having an ester bond include esters of aliphatic carboxylic acids having a hindered phenol group and aliphatic alcohols, and examples of the hindered phenol compound having an amide bond include amides of aliphatic carboxylic acids having a hindered phenol group and aliphatic amines. Among these, it is preferable that the hindered phenol compound has an amide bond.

[0065] Specific structures of hindered phenol compounds having an ester bond or an amide bond include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from BASF as Irganox 1010, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate commercially available from Irganox 1076, 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from Irganox 1035, and 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from Irganox 1135. Examples of such an acid include octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoate, which is commercially available; ethylene bis(oxyethylene)(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoate), which is commercially available as Irganox 245; 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], which is commercially available as Irganox 259; and N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide], which is commercially available as Irganox 1098. Among these, N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide] commercially available as Irganox 1098 and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available as Irganox 1010 are preferred, with the former being more preferred.

[0066] The resin composition (A) may further contain a thermoplastic resin other than the gas barrier resin (a) and the polyolefin (b). Examples of thermoplastic resins other than the gas barrier resin (a) and the polyolefin (b) include polyolefins having an MFR of less than 3.0 g / 10 min at 190 ° C and a load of 2.160 kg as measured in accordance with JIS K7210-1 (2014), various polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyacrylonitrile, polyurethane, polycarbonate, polyacetal, and polyacrylate. The content of the thermoplastic resin in the resin composition (A) is typically less than 40% by mass, preferably less than 30% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass. It may be less than 5% by mass or even less than 1% by mass, and it is particularly preferred that the resin composition is substantially free of the thermoplastic resin.

[0067] The total mass ratio of the gas barrier resin (a) and polyolefin (b) in the resin constituting the resin composition (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, from the viewpoint of suppressing die build-up. The resin constituting the resin composition (A) may essentially consist of only the gas barrier resin (a) and polyolefin (b), or the resin constituting the resin composition (A) may consist of only the gas barrier resin (a) and polyolefin (b). Furthermore, from the viewpoint of suppressing die build-up, the total mass ratio of the gas barrier resin (a) and polyolefin (b) in the resin composition (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 98% by mass or more, or may be 99% by mass or more.

[0068] In thermogravimetry (TG), the resin composition (A) preferably exhibits a weight loss W of 0.01 to 0.3% when maintained at 200°C in a nitrogen atmosphere for 30 minutes. This reflects the low-molecular-weight components present in the resin composition (A) and the thermal decomposition characteristics of the gas barrier resin (a) and polyolefin (b). By having layer (X) comprise a resin composition (A) that satisfies the specific TG conditions, a multilayer film with excellent appearance characteristics can be stably produced over an extended period of time. From the viewpoint of stably producing a multilayer film with even better appearance characteristics, the weight loss W when maintained at 200°C in a nitrogen atmosphere for 30 minutes is preferably 0.02 to 0.15%, more preferably 0.03 to 0.10%, and even more preferably 0.04 to 0.08%. W can be controlled by the ethylene unit content and degree of saponification when the gas barrier resin (a) is EVOH, the types and contents of the polyolefin (b), alkali metal ions (c), polyvalent metal ions (d), higher aliphatic carboxylic acids (e) and other components contained in the resin composition (A), and the production conditions (particularly the thermal history such as temperature and time) when producing the resin composition (A). For example, when producing the resin composition (A) by melt-kneading, the weight loss W tends to be small by performing the melt-kneading while removing gas components using a vent device or the like.

[0069] The method for producing the resin composition (A) is not particularly limited, but it can be produced by melt-kneading the gas barrier resin (a) and polyolefin (b), and, if necessary, other components such as alkali metal ions (c), polyvalent metal ions (d), and higher aliphatic carboxylic acids (e). Each component may be blended as a solid, such as a powder, or as a melt. They may also be blended as solutes in a solution or dispersoids in a dispersion. An aqueous solution and an aqueous dispersion are preferred as the solution and dispersion, respectively. For melt-kneading, known mixing or kneading devices such as a kneader-ruder, extruder, mixing roll, or Banbury mixer can be used. The temperature range during melt-kneading can be adjusted appropriately depending on the gas barrier resin (a) used and the melting points of each component, and is typically 150 to 250°C. Alternatively, the resin composition may be produced by adding some components to the gas barrier resin (a) in advance, and then melt-kneading additional components as described above. An example of a method for preliminarily adding some components to the gas barrier resin (a) is to immerse the gas barrier resin (a) in the form of pellets or powder in a solution in which the added components are dissolved. An aqueous solution is preferred as the solution. From the viewpoint of suppressing die buildup, it is particularly preferred to melt-knead the gas barrier resin (a) and the polyolefin (b) to obtain pellets of the resin composition (A). Furthermore, it is preferred that the layer (X) be a layer obtained by melt-molding pellets consisting of only the resin composition (A).

[0070] <Layer (Y)> The multilayer film of the present invention has at least one layer different from layer (X). It is preferable to have layer (Y) containing, as a main component, an adhesive resin (B) having a melting point of less than 170°C. By including layer (Y) in the multilayer film of the present invention, a multilayer film with excellent appearance and interlayer adhesion tends to be obtained. Furthermore, by including layer (Y), compatibility between layer (X) and layer (Z) described below is improved during recycling, which tends to improve recyclability. Examples of adhesive resin (B) include acid-modified polyolefin resins obtained by graft polymerizing an unsaturated carboxylic acid such as maleic anhydride or a derivative thereof onto a polyolefin resin. The melting point of adhesive resin (B) mainly depends on the polyolefin resin before acid modification. Regarding the polyolefin resin, the description of the unmodified polyolefin resin (C) described below is applicable. However, adhesive resin (B) is preferably acid-modified polyethylene or acid-modified polypropylene. The acid-modified polyolefin resin may be a carboxylic acid-modified polyolefin resin. The acid-modified polyethylene may be a carboxylic acid-modified polyethylene, and the acid-modified polypropylene may be a carboxylic acid-modified polypropylene.

[0071] The proportion of the acid-modified polyolefin resin in the adhesive resin (B) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Y) may be substantially composed of the acid-modified polyolefin resin alone, or may be composed of the acid-modified polyolefin resin alone. The proportion of the adhesive resin (B) in the layer (Y) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Y) may be substantially composed of the adhesive resin (B) alone, or may be composed of the adhesive resin (B) alone.

[0072] <Layer (Z)> The multilayer film of the present invention preferably has a layer (Z) containing, as a main component, a polyolefin resin (C) having a melting point of less than 170° C. The polyolefin resin (C) is not particularly limited as long as it is a polyolefin having a melting point of less than 170° C. Examples of the polyolefin resin (C) include polyethylene-based resins such as linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, and high-density polyethylene; polypropylene-based resins such as homopolypropylene, random polypropylene, and block polypropylene; vinyl ester resins; ethylene-propylene copolymers; propylene-α-olefin copolymers (α-olefins having 4 to 20 carbon atoms); olefin homopolymers or copolymers thereof such as polybutene and polypentene; and chlorinated polyethylene.

[0073] The lower limit of the content of olefin units relative to all monomer units in the polyolefin resin (C) is preferably 60 mol%, more preferably 70 mol%, even more preferably 80 mol%, even more preferably 90 mol%, and may be 95 mol%, 98 mol%, 99 mol%, or 99.9 mol%. The upper limit of the content of olefin units relative to all monomer units in the polyolefin resin (C) may be 100 mol%. The polyolefin resin (C) may be modified, such as by acid modification, or may be unmodified, but is preferably unmodified.

[0074] From the viewpoint of improving the recyclability of a multilayer structure containing polyolefin resin (C), the polyolefin resin (C) preferably contains a polyethylene-based resin or a polypropylene-based resin as a main component, more preferably polyethylene or polypropylene, and even more preferably polyethylene. Polyethylene-based resins and polypropylene-based resins are widely used in packaging materials regardless of whether they have gas barrier properties, and therefore recycling infrastructures for them have been widely established in various countries. When polyolefin resin (C) contains polyethylene as a main component, the polyethylene is preferably at least one selected from linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, and high-density polyethylene, and more preferably at least one selected from linear low-density polyethylene and low-density polyethylene, or a mixture of at least one selected from linear low-density polyethylene and low-density polyethylene with high-density polyethylene.

[0075] From the viewpoint of making the effects of the present invention more pronounced, the melting point of the polyolefin resin (C) is preferably less than 160°C, more preferably less than 150°C, and may be less than 140°C or less than 130°C. On the other hand, from the viewpoint of processability during secondary processing such as melt molding and stretching, and from the viewpoint of heat resistance as a packaging material, the melting point of the polyolefin resin (C) is preferably 80°C or higher, more preferably 90°C or higher. Furthermore, from the viewpoint of improving melt moldability, the melt flow rate (MFR) (190°C, under a load of 2.160 kg) of the polyolefin resin (C) measured in accordance with the method described in JIS K7210-1 (2014) is preferably 0.1 to 30 g / 10 min, more preferably 0.3 to 25 g / 10 min, and even more preferably 0.5 to 20 g / 10 min.

[0076] When the polyolefin resin (C) contains a polyethylene resin or a polypropylene resin as a main component, the content of the polyethylene resin or the polypropylene resin in the polyolefin resin (C) is more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 95% by mass or more, and the polyolefin resin (C) may be essentially composed of a polyethylene resin or a polypropylene resin alone, or the polyolefin resin (C) may be composed of a polyethylene resin or a polypropylene resin alone. Furthermore, the proportion of the polyolefin resin (C) in the layer (Z) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Z) may be essentially composed of a polyolefin resin (C) alone, or the layer (Z) may be composed of a polyolefin resin (C) alone.

[0077] Layer (Y) and layer (Z) contain adhesive resin (B) and polyolefin resin (C) as main components, respectively, but these layers may also contain other components such as antioxidants, plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorizers, UV absorbers, antistatic agents, lubricants, colorants, fillers, desiccants, bulking agents, pigments, dyes, processing aids, flame retardants, and antifogging agents, as long as the effects of the present invention are not impaired. However, the total amount of these components is less than 50% by mass of each layer, preferably less than 40% by mass, more preferably less than 30% by mass, even more preferably less than 20% by mass, and particularly preferably less than 10% by mass, and may be less than 5% by mass, less than 3% by mass, or less than 1% by mass.

[0078] <Multilayer Film> The multilayer film of the present invention has a layer (X) as the outermost layer and at least one layer different from layer (X). The layer different from layer (X) is not particularly limited, but is preferably at least one type selected from the group consisting of layer (Y) and layer (Z). The multilayer film more preferably has a configuration comprising layer (X), layer (Y), and layer (Z), with layer (X), layer (Y), and layer (Z) laminated adjacently in this order. The multilayer film may have a plurality of layers (X), layer (Y), and layer (Z). When there are a plurality of layers (X), it is sufficient that there is at least one layer (X) located as the outermost layer. In other words, when there are a plurality of layers (X), there may be a layer (X) that is not located as the outermost layer.

[0079] The multilayer film of the present invention may have layers other than the layer (X), the layer (Y), and the layer (Z). However, as one embodiment of the present invention, the multilayer film of the present invention may not have layers other than the layer (X), the layer (Y), and the layer (Z).

[0080] The layer structure of the multilayer film of the present invention may be X / Y / Z, X / Y / Z / Y / X, X / Y / Z / Y / X / Y / Z, X / Y / Z / Y / X / Y / Z, X / Y / Z / Y / X / Y / Z / Y / X / Y / Z / Y / X, etc., where X represents layer (X), Y represents layer (Y), and Z represents layer (Z), and " / " indicates that the layers are directly laminated.

[0081] From the viewpoints of gas barrier properties, recyclability, and economy, the average thickness of layer (X) in the multilayer film is preferably 0.2 μm or more and less than 20 μm. It is also preferable that the ratio of the average thickness of layer (X) to the average thickness of the multilayer film is less than 25%. The average thickness of layer (X) is more preferably 0.4 μm or more and less than 16 μm, and even more preferably 0.6 μm or more and less than 12 μm. The ratio of the average thickness of layer (X) to the average thickness of the multilayer film is more preferably less than 20%, and even more preferably less than 15%. The ratio of the average thickness of layer (X) to the average thickness of the multilayer film may be 1% or more. When multiple layers (X) are present, the average thickness of layer (X) is the sum of the average thicknesses of the layers (X). The average thickness of the multilayer film is equal to the sum of the average thicknesses of each layer of the multilayer film.

[0082] From the viewpoints of interlayer adhesion, recyclability, and economy, the average thickness of layer (Y) in the multilayer film is preferably 0.2 μm or more and less than 20 μm. It is also preferable that the ratio of the average thickness of layer (Y) to the average thickness of the multilayer film is less than 25%. The average thickness of layer (Y) is more preferably 0.4 μm or more and less than 16 μm, and even more preferably 0.6 μm or more and less than 12 μm. The ratio of the average thickness of layer (Y) to the average thickness of the multilayer film is more preferably less than 20%, and even more preferably less than 15%. The ratio of the average thickness of layer (Y) to the average thickness of the multilayer film may be 1% or more. When a plurality of layers (Y) are present, the average thickness of layer (Y) is the sum of the average thicknesses of the layers (Y).

[0083] From the viewpoint of recyclability, the average thickness of the layer (Z) in the multilayer film is preferably 1 μm or more and less than 200 μm. It is also preferable that the ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film is more than 55%. The average thickness of the layer (Z) is more preferably 5 μm or more, even more preferably 10 μm or more, and may be 20 μm or more. The average thickness of the layer (Z) is more preferably 100 μm or less, and may be 50 μm or less. The ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film is more preferably more than 60%, even more preferably more than 70%. The ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film may be 98% or less. When a plurality of layers (Z) are present, the average thickness of the layer (Z) is the sum of the average thicknesses of the layers (Y).

[0084] The average thickness of the multilayer film is preferably 10 μm or more and less than 200 μm, more preferably 10 μm or more and less than 150 μm. In the case of a stretched multilayer film described below, the average thickness of the stretched multilayer film is preferably 10 μm or more and less than 50 μm, more preferably 10 μm or more and less than 40 μm.

[0085] The multilayer film may be an unstretched multilayer film, or may be a stretched multilayer film stretched uniaxially or biaxially (at least uniaxially). An unstretched multilayer film refers to a multilayer film that has not been stretched, but slight orientation during film formation (e.g., orientation as if stretched 1.01 times) is considered to be unstretched. Furthermore, a uniaxially stretched multilayer film that has been stretched only uniaxially is considered to be uniaxially stretched, ignoring slight orientation in other axial directions during film formation (e.g., orientation as if stretched 1.01 times). Unstretched multilayer films have excellent impact resistance and can be suitably used as heat-sealable films. On the other hand, uniaxial or biaxial stretching can improve the mechanical properties and gas barrier properties of the resulting multilayer film. From the viewpoint of economy and ease of tearing the multilayer film (making it easy to open the packaging material when used as a packaging material), the multilayer film is preferably a uniaxially stretched multilayer film. From the viewpoint of obtaining a film with little anisotropy in mechanical properties and a strong film, the multilayer film is preferably a biaxially stretched multilayer film. From the viewpoint of thickness uniformity and mechanical strength of the resulting multilayer film, the multilayer film is preferably stretched at least 3 times but less than 12 times in one axial direction. In the case of a uniaxially stretched multilayer film, it is preferably stretched 3 times or more but less than 12 times in one axial direction, and more preferably stretched 4 times or more but less than 10 times. Furthermore, in the case of a uniaxially stretched multilayer film, the stretching axis is preferably in the machine direction (MD) or a direction perpendicular to the machine direction, i.e., the width direction (TD), and more preferably in the machine direction (MD). In the case of a biaxially stretched multilayer film, it is preferably stretched 3 times or more but less than 12 times in each of the two axial directions, and more preferably stretched 4 times or more but less than 10 times.

[0086] The lower limit of the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film of the present invention (the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin to the average thickness of the multilayer film) is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. Increasing the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film can improve recyclability. The upper limit of the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film is preferably 99.5%, more preferably 99%, and may even be 98%. The "total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin" refers to the combined average thickness of layers primarily composed of polyethylene-based resin and layers primarily composed of polypropylene-based resin. Examples of layers primarily composed of polyethylene-based resin or polypropylene-based resin include layer (Y) when the adhesive resin (B) is, for example, acid-modified polyethylene or acid-modified polypropylene, and layer (Z) when the polyolefin resin (C) is polyethylene or polypropylene. It is preferable that the adhesive resin (B) and the polyolefin resin (C) are the same type of resin. For example, when the adhesive resin (B) is acid-modified polyethylene, it is preferable that the polyolefin resin (C) is polyethylene, and when the adhesive resin (B) is acid-modified polypropylene, it is preferable that the polyolefin resin (C) is polypropylene.

[0087] For example, the lower limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as a main component in the multilayer film of the present invention is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. The upper limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as a main component in the multilayer film is preferably 99.5%, more preferably 99%, or even 98%. Furthermore, the lower limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as a main component in the multilayer film of the present invention is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. The upper limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as a main component in the multilayer film is preferably 99.5%, more preferably 99%, or even 98%.

[0088] The multilayer film of the present invention preferably does not have a layer containing as its main component a resin having a melting point of 200°C or higher, or a metal layer having an average thickness of 1 μm or higher. Furthermore, it is preferable that none of the layers (X), (Y), and (Z) contain as its main component a resin having a melting point of 200°C or higher. The absence of a layer containing as its main component a resin having a melting point of 200°C or higher, or a metal layer having an average thickness of 1 μm or higher, can prevent the multilayer film or pulverized multilayer structure from being mixed with other components in a non-uniform manner when the pulverized multilayer film or multilayer structure is melt-molded. Here, the metal layer refers to a layer having continuous and discontinuous surfaces made of metal, such as aluminum foil.

[0089] <Method for Producing a Multilayer Film> The method for producing a multilayer film (film formation method) is not particularly limited. Generally, a conventional coextrusion method can be used, in which each resin is extruded through a separate die or a common die and laminated. Either a circular die or a T-die can be used as the die. The method for uniaxial or biaxial stretching is also not particularly limited. The film can be produced by stretching in the machine direction and / or the direction perpendicular to the machine direction, i.e., the width direction, using a conventional stretching method such as roll-type uniaxial stretching, tenter-type uniaxial stretching, tubular-type simultaneous biaxial stretching, tenter-type sequential biaxial stretching, or tenter-type simultaneous biaxial stretching. Furthermore, tenter-type sequential biaxial stretching may use a tenter for both axes, or may be a combination of roll-type stretching and tenter-type stretching. The effects of the present invention are particularly pronounced in the case of a multilayer film produced by tenter-type sequential biaxial stretching, which is a combination of roll-type stretching and tenter-type stretching. From the viewpoint of processability, the temperature during stretching is usually 40 to 170° C., and more preferably 50 to 160° C. If necessary, after stretching, it is preferable to carry out a heat treatment at a temperature equal to or higher than the glass transition point and lower than the melting point, thereby increasing the crystallinity and fixing the orientation of the molecular chains, which is called heat setting.

[0090] From the viewpoint of suppressing die build-up, the method for producing a multilayer film preferably includes a step of melt-kneading a gas barrier resin (a) and a polyolefin (b) to obtain pellets of a resin composition (A), and a step of melt-molding the pellets of the resin composition (A) to form the layer (X). The specific method for obtaining pellets of the resin composition (A) is as described above.

[0091] <Vapor-deposited multilayer film> The vapor-deposited multilayer film of the present invention comprises the multilayer film of the present invention and an inorganic vapor-deposited layer (I) laminated on the exposed surface of layer (X) of the multilayer film. That is, the multilayer film of the present invention may be used by laminating the inorganic vapor-deposited layer (I) on the surface of layer (X). The inorganic vapor-deposited layer (I) is preferably laminated on the exposed surface of layer (X) of the multilayer film directly or via another layer such as an adhesive layer, and is preferably laminated directly on the exposed surface of layer (X). The inorganic vapor-deposited layer (I) is made of an inorganic substance such as a metal or inorganic oxide and has gas barrier properties against oxygen and water vapor. Layer (X) has a higher affinity with metals and inorganic oxides than ordinary thermoplastic resins, allowing the formation of a dense, defect-free inorganic vapor-deposited layer (I). The resulting vapor-deposited multilayer film has good interlayer adhesion between layer (X) and inorganic vapor-deposited layer (I). Furthermore, because layer (X) has gas barrier properties, deterioration of gas barrier properties can be suppressed even when defects occur in the inorganic vapor-deposited layer (I) due to bending or the like. The inorganic vapor-deposited layer (I) generally has an average thickness of less than 500 nm. When the average thickness is less than 500 nm, the viscosity of the vapor-deposited multilayer film or multilayer structure containing the inorganic vapor-deposited layer (I) is stable during melt molding, and the occurrence of gels or lumps can be suppressed.

[0092] The inorganic vapor deposition layer (I) is preferably either a metal vapor deposition layer containing aluminum as a main component or an inorganic oxide vapor deposition layer containing alumina or silica as a main component. A metal vapor deposition layer is preferred when light-shielding properties are to be imparted, but an inorganic oxide vapor deposition layer is preferred from the viewpoints of visibility of the contents as a packaging material, microwave suitability, and suppression of gels and lumps when pulverized materials are melt-molded. Furthermore, an inorganic oxide vapor deposition layer is preferred from the viewpoint of suppressing coloration during recycling of the multilayer structure of the present invention.

[0093] The aluminum atom content in the metal vapor-deposited layer is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. The average thickness of the metal vapor-deposited layer is preferably 120 nm or less, more preferably 100 nm or less, and even more preferably 90 nm or less. The average thickness of the metal vapor-deposited layer is preferably 25 nm or more, more preferably 35 nm or more, and even more preferably 45 nm or more. The average thickness of the metal vapor-deposited layer is the average value of thicknesses at any 10 points on the cross section of the metal vapor-deposited layer measured using an electron microscope. When the vapor-deposited multilayer film of the present invention has a metal vapor-deposited layer, the light transmittance at a wavelength of 600 nm can be 10% or less, and the film has excellent light-blocking properties.

[0094] In a metal vapor deposition layer containing aluminum as a main component, oxidation may occur irreversibly, and aluminum oxide may be partially contained. In a metal vapor deposition layer containing aluminum as a main component (inorganic vapor deposition layer (I)), the molar ratio of the oxygen atom content to the aluminum atom content (O mol / Al mol) is preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less.

[0095] Examples of inorganic oxide vapor-deposited layers include vapor-deposited films of inorganic oxides such as oxides of silicon, aluminum, magnesium, calcium, potassium, tin, sodium, boron, titanium, lead, zirconium, and yttrium, preferably alumina or silica. The average thickness of the inorganic oxide vapor-deposited layer is preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less. The average thickness of the inorganic oxide vapor-deposited layer is preferably 10 nm or more, more preferably 15 nm or more, and even more preferably 20 nm or more. The average thickness of the inorganic oxide vapor-deposited layer is the average value of thicknesses at any 10 points on the cross section of the inorganic oxide vapor-deposited layer measured using an electron microscope. When the vapor-deposited multilayer film of the present invention has an inorganic oxide vapor-deposited layer, it can have a light transmittance of 80% or more at a wavelength of 600 nm, providing excellent visibility of the contents when used as a packaging material. To further improve visibility, a light transmittance of 90% or more at a wavelength of 600 nm is more preferred. Light transmittance can be increased, for example, by suppressing thickness unevenness in the multilayer film used in the production of the multilayer film. The vapor-deposited multilayer film preferably has a light transmittance of 80% or more, more preferably 90% or more, at a wavelength of 600 nm.

[0096] The inorganic vapor deposition layer (I) can be formed by a known physical vapor deposition method or chemical vapor deposition method. Specific examples include vacuum deposition, sputtering, ion plating, ion beam mixing, plasma CVD, laser CVD, MO-CVD, and thermal CVD. Physical vapor deposition is preferred, with vacuum vapor deposition being particularly preferred. The upper limit of the surface temperature of layer (X) during the formation of inorganic vapor deposition layer (I) is preferably 60°C, more preferably 55°C, and even more preferably 50°C. The lower limit of the surface temperature of layer (X) during the formation of inorganic vapor deposition layer (I) is not particularly limited, but is preferably 0°C, more preferably 10°C, and even more preferably 20°C. Prior to film formation, the exposed surface of layer (X) may be plasma-treated. This plasma treatment can be performed by a known method, with atmospheric pressure plasma treatment being preferred. In atmospheric pressure plasma treatment, nitrogen, helium, neon, argon, krypton, xenon, radon, or the like is used as a discharge gas. Among these, nitrogen, helium, and argon are preferably used, and nitrogen is particularly preferred because it can reduce costs. A known protective layer or the like may be provided on the inorganic vapor deposition layer (I) to improve flex resistance.

[0097] The multilayer film or vapor-deposited multilayer film of the present invention has an oxygen transmission rate (under conditions of 20°C and 65% RH) of 60 cc / (m) as measured in accordance with JIS K7126-2 (isobaric method; 2006). 2 ·day·atm), and 2 ·day·atm), and more preferably less than 3 cc / (m 2 ·day·atm), and more preferably less than 0.5 cc / (m 2 A multilayer film or a vapor-deposited multilayer film having an oxygen transmission rate within the above range has excellent gas barrier properties.

[0098] <Multilayer structure, recovered composition, method for recovering multilayer structure, and packaging material> The multilayer film or vapor-deposited multilayer film of the present invention can itself be used as a packaging material having gas barrier properties, but by laminating at least one resin layer (R) containing a thermoplastic resin (D) as a main component to form a multilayer structure, it is possible to impart various functions as a packaging material, such as designability and heat-sealability. In other words, the multilayer structure of the present invention is formed by laminating the multilayer film or vapor-deposited multilayer film of the present invention with at least one resin layer (R) containing a thermoplastic resin (D) as a main component.

[0099] The thermoplastic resin (D) is not particularly limited, and examples thereof include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, vinyl ester resin, ethylene-propylene copolymer, polypropylene, propylene-α-olefin copolymer (α-olefin having 4 to 20 carbon atoms), polybutene, polypentene, and other olefin homopolymers or copolymers thereof, PA such as nylon 6 and nylon 6,6, polyester such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polystyrene, polyvinyl chloride, polyvinylidene chloride, acrylic resin, polycarbonate, chlorinated polyethylene, chlorinated polypropylene, etc. Among these, polyolefins are preferred from the viewpoints of excellent moisture resistance, mechanical properties, economical efficiency, heat sealability, etc., and PA and polyesters are preferred from the viewpoints of excellent mechanical properties, heat resistance, etc. In order to obtain a multilayer structure having particularly excellent recyclability, the thermoplastic resin (D) is preferably the same type as the polyolefin resin (C), i.e., a polyolefin resin having a melting point of less than 170°C, more preferably a polyethylene-based resin or a polypropylene-based resin as the main component, even more preferably polyethylene or polypropylene, and particularly preferably polyethylene. Therefore, in order to obtain a multilayer structure having excellent recyclability, the polyolefin resin (C) and the thermoplastic resin (D) preferably contain a polyethylene-based resin or a polypropylene-based resin as the main component, more preferably polyethylene or polypropylene, and even more preferably polyethylene. Such a resin layer (R) may be unstretched, or may be uniaxially or biaxially stretched or rolled. From the viewpoint of improving mechanical strength, a biaxially stretched layer is preferred, and from the viewpoint of improving heat sealability, a non-stretched layer is preferred.

[0100] The method for producing the resin layer (R) is not particularly limited, but it is generally produced by melt extrusion using an extruder. Either a circular die or a T-die can be used as the die. The method for uniaxial or biaxial stretching is also not particularly limited, and the film can be produced by stretching the film in the machine direction and / or the direction perpendicular to the machine direction, i.e., the width direction, using a conventionally known stretching method such as roll-type uniaxial stretching, tubular-type simultaneous biaxial stretching, tenter-type sequential biaxial stretching, or tenter-type simultaneous biaxial stretching. From the viewpoint of the thickness uniformity and mechanical strength of the resulting layer, the area ratio is preferably 8 to 60 times. The area ratio is more preferably 55 times or less, and even more preferably 50 times or less. Furthermore, the area ratio is more preferably 9 times or more. If the area ratio is less than 8 times, stretching unevenness may remain, and if it exceeds 60 times, the layer may be more likely to break during stretching.

[0101] The average thickness of the resin layer (R) is preferably 10 to 200 μm from the viewpoint of industrial productivity. Specifically, the average thickness is more preferably 10 to 150 μm in the case of an unstretched layer, and more preferably 10 to 50 μm in the case of a biaxially stretched layer.

[0102] The average thickness of the multilayer structure of the present invention is preferably 300 μm or less. With an average thickness within this range, the multilayer structure of the present invention is lightweight and flexible, making it suitable for use in flexible packaging. Furthermore, the amount of resin used in the multilayer structure is small, thereby reducing the environmental impact.

[0103] The average thickness of each layer in the multilayer structure of the present invention may be adjusted appropriately depending on the application, but from the viewpoints of suppressing discoloration during melt molding of the pulverized material, improving thermal stability during melt molding, and suppressing the occurrence of lumps, it is preferable that at least one of the layer (Z) and the resin layer (R) contains a polyethylene resin or a polypropylene resin as a main component. The ratio of the total average thickness of the layers containing a polyethylene resin or a polypropylene resin as a main component to the average thickness of the multilayer structure is preferably 80% or more, more preferably 85% or more. On the other hand, from the viewpoint of improving gas barrier properties, this ratio is preferably 99.7% or less, more preferably 99.5% or less, and may be 99.3% or less.

[0104] For example, the lower limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as the main component in the multilayer structure of the present invention is preferably 80%, more preferably 85%. The upper limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as the main component in the multilayer structure is preferably 99.7%, more preferably 99.5%, or even 99.3%. Furthermore, the lower limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as the main component in the multilayer structure of the present invention is preferably 80%, more preferably 85%. The upper limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as the main component in the multilayer structure is preferably 99.7%, more preferably 99.5%, or even 99.3%.

[0105] The method for laminating the resin layer (R) on the multilayer film or vapor-deposited multilayer film of the present invention is not particularly limited, and examples include extrusion lamination, coextrusion lamination, dry lamination, etc. An adhesive layer may be provided when laminating the resin layer (R) on the multilayer film or vapor-deposited multilayer film. Furthermore, each layer constituting the multilayer structure of the present invention may be laminated via an adhesive layer, if necessary. However, it is preferable that no adhesive layer is present between layer (X) and layer (Y) of the multilayer film or vapor-deposited multilayer film, or between layer (Y) and layer (Z). The adhesive layer can be formed by applying and drying a known adhesive. The adhesive is preferably a two-component reactive polyurethane adhesive in which a polyisocyanate component and a polyol component are mixed and reacted. The average thickness of the adhesive layer is not particularly limited, but is preferably 1 to 5 μm, more preferably 2 to 4 μm.

[0106] The multilayer structure of the present invention is not particularly limited, and from the viewpoint of obtaining a multilayer structure with excellent recyclability, for example, the following layer configurations are preferred. In the following layer configurations, layer (X) is represented as X, layer (Y) as Y, layer (Z) as Z, inorganic vapor deposition layer (I) as I, and layer (R) as R, where " / " means directly laminated, and " / / " means laminated via an adhesive layer or directly laminated, with laminated via an adhesive layer being preferred. (1) Z / Y / X / I / / R (2) R / / Z / Y / X / I / / R In the above layer configurations, layer (X), layer (Y), and layer (Z) are preferably stretched at least uniaxially, and more preferably biaxially. Layer (Z) and layer (R) are preferably polyethylene-based resins or polypropylene-based resins, and layer (Y) is preferably maleic anhydride-modified polyethylene or maleic anhydride-modified polypropylene. Furthermore, when recycling the packaging material of the present invention, the pulverized material obtained by pulverizing the packaging material can be recovered as a composition mainly composed of a polyethylene-based resin or a polypropylene-based resin, so that the outermost layers of the multilayer structure of the present invention preferably have layers containing a polyethylene-based resin or a polypropylene-based resin as a main component. That is, when resin layers (R) are arranged in both outermost layers, it is preferable that the resin layer (R) be a layer mainly composed of a polyethylene-based resin or a polypropylene-based resin, and when layer (Z) and resin layer (R) are arranged in both outermost layers, it is preferable that layer (Z) and resin layer (R) be layers mainly composed of a polyethylene-based resin or a polypropylene-based resin. It is preferable that one of the outermost layers is an unstretched layer, and the other is a layer stretched at least uniaxially, which may be preferred from the viewpoint of obtaining a multilayer structure that combines heat-sealability and mechanical properties.

[0107] The multilayer structure of the present invention may have layers other than those described above, provided that the effects of the present invention are not impaired. An example of such layers is a recovery layer. It is particularly preferable to reuse a recovered composition containing recovered materials from the multilayer structure of the present invention, as described below, as part or all of the recovery layer. Another example of such layers is a printed layer. The printed layer may be included at any position in the multilayer structure of the present invention. Examples of the printed layer include a film obtained by applying a solution containing a pigment or dye, and optionally a binder resin, followed by drying. Examples of methods for applying the printed layer include gravure printing and various other application methods using a wire bar, spin coater, die coater, etc. The average thickness of the ink layer is not particularly limited, but is preferably 0.5 to 10 μm, more preferably 1 to 4 μm.

[0108] It is preferable to reuse scraps (ends and defective products) recovered during the production of the multilayer structure of the present invention. A method for recovering a multilayer structure of the present invention, which comprises a step of crushing the multilayer structure of the present invention and then melt-molding the crushed multilayer structure, and a recovered composition containing the recovered multilayer structure of the present invention are also preferred embodiments of the present invention.

[0109] When recovering the multilayer structure of the present invention, the recovered multilayer structure of the present invention is first pulverized. The pulverized recovered material may be melt-molded directly to obtain a recovered composition, or may be melt-molded together with other components as needed to obtain a recovered composition. A preferred component to be added to the recovered material is a polyolefin resin, and a polyethylene-based resin or a polypropylene-based resin is more preferred. The polyolefin resin used is the same type as the polyolefin resin (C) described above for use in the multilayer film of the present invention. The pulverized recovered material may be directly used to produce a molded product such as a multilayer structure, or the pulverized recovered material may be melt-molded to obtain pellets of the recovered composition, and the pellets may then be used to produce a molded product.

[0110] In the recovered composition, the mass ratio of the resin composition (A) to the polyolefin resin [resin composition (A) / polyolefin resin] is preferably 0.01 / 99.99 to 20 / 80. When the mass ratio is 0.01 / 99.99 or more, the proportion of recovered material used increases. On the other hand, when the mass ratio is 20 / 80 or less, the melt-moldability and mechanical properties of the recovered composition are improved. From the viewpoint of improving the melt-moldability and mechanical properties of the resulting recovered composition, the mass ratio is more preferably 15 / 85 or less, even more preferably 10 / 90 or less, and may even be 5 / 95 or less.

[0111] The multilayer structure of the present invention has gas barrier properties and recyclability, and therefore can be suitably used as a material for various types of packaging, such as food packaging, pharmaceutical packaging, industrial chemical packaging, and agricultural chemical packaging. In particular, packaging materials having the multilayer structure of the present invention can be suitably used as packaging materials with excellent recyclability. The multilayer film and vapor-deposited multilayer film of the present invention can also be suitably used as packaging materials.

[0112] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples in any way.

[0113] [Materials Used] Gas barrier resin (a) EVOH (a-1): EVOH (ethylene (Et) unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 180 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.) EVOH (a-1A): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain alkali metal ions or polyvalent metal ions.) EVOH (a-1B): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 150 ppm of sodium acetate calculated as sodium ions, 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain polyvalent metal ions.) EVOH (a-1C): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 250 ppm of sodium acetate calculated as sodium ions, 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain polyvalent metal ions.) EVOH (a-1D): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 550 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.EVOH (a-2): EVOH (ethylene unit content 27 mol%, saponification degree 99.99 mol%, MFR (210°C, 2.160 kg load) 4.0 g / 10 min, melting point 191°C, volatile content 0.8%, contains 180 ppm of sodium acetate as sodium ions, 30 ppm of phosphate ions as phosphate radicals, and 150 ppm of boric acid as boron element, but does not contain polyvalent metal ions. EVOH (a-3): EVOH (ethylene unit content 44 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 5.7 g / 10 min, melting point 165°C, volatile content 0.8%, contains 180 ppm of sodium acetate as sodium ions, and 30 ppm of phosphate ions as phosphate radicals, but does not contain polyvalent metal ions.) EVOH (a-2 / 3): A mixture (dry blend) of EVOH (a-2) and EVOH (a-3) in a mass ratio of 75 / 25. EVOH (a-4): EVOH (ethylene unit content 48 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.160 kg load) 6.4 g / 10 min, melting point 157°C, volatile content 0.8%, contains 180 ppm of sodium acetate in terms of sodium ions, and 50 ppm of phosphate ions in terms of phosphate radicals, but does not contain polyvalent metal ions.) EVOH (a-5): EVOH produced by the following production method (ethylene unit content 44 mol%, saponification degree 99.99 mol%, epoxypropane modification degree 4.6 mol%, MFR (190°C, 2.160 kg load) 5.6 g / 10 min, volatile content 0.8%, melting point 119°C, sodium acetate 220 ppm calculated as sodium ions, phosphate ions 30 ppm calculated as phosphate radicals). Note that the epoxypropane modification degree refers to the content of monomer units modified with epoxypropane relative to all monomer units. (Production Method of EVOH (a-5)) 28 parts by mass of zinc acetylacetonate monohydrate was mixed with 957 parts by mass of 1,2-dimethoxyethane to obtain a mixed solution. 15 parts by mass of trifluoromethanesulfonic acid was added to the obtained mixed solution with stirring to obtain a catalyst solution.Next, EVOH having an ethylene unit content of 44 mol% and a degree of saponification of 99.99 mol% or more (but containing no alkali metal ions and 30 ppm of phosphate ions) was charged into a TEM-35BS extruder (37 mmφ, L / D = 52.5) ​​manufactured by Toshiba Machine Co., Ltd., and operated under the following conditions: barrel C1 was water-cooled, barrels C2 to C3 were cooled to 200°C, barrels C4 to C15 were cooled to 240°C, and a screw rotation speed of 250 rpm. Epoxypropane (1.5 kg / hr) and the catalyst solution were added through pressure inlet 1 of C8. Next, an aqueous sodium acetate solution was added through pressure inlet 2 of C13. The discharged strand was cooled and solidified in a cooling tank, cut, and then dried to obtain EVOH (a-5). In this step, the amount of catalyst solution added was adjusted so that the melting point of the resulting EVOH (a-5) would be 119°C. The amount of sodium acetate solution added was adjusted appropriately so that the content of sodium ions in EVOH (a-5) was as described above. PA (a-6): Nylon 6 / 66 ("Ultramid (trademark) C40LN" manufactured by BASF).

[0114] Polyolefins (b) Polyolefin (b-1): EVA saponification product ("Mersen (trademark) H-6822X" manufactured by Tosoh Corporation, ethylene unit content 94 mol%, degree of saponification 92 mol%, MFR (190°C, 2.160 kg load) 190 g / 10 min, number average molecular weight (Mn) 16,800) Polyolefin (b-2): EVA saponification product ("Mersen (trademark) H-6051K" manufactured by Tosoh Corporation, ethylene unit content 89 mol%, degree of saponification 97 mol%, MFR (190°C, 2.160 kg load) 6.2 g / 10 min, number average molecular weight (Mn) 24,300) Polyolefin (b-3): EVA ("Ultrathene (trademark) 680" manufactured by Tosoh Corporation, ethylene unit content 93 mol%, MFR (190°C, 2.160 kg load) 150 g / 10 min, number average molecular weight (Mn) unknown) Polyolefin (b-4): Polyethylene ("Sunwax (trademark) 161-P" manufactured by Sanyo Chemical Industries, Ltd., MFR (190°C, 2.160 kg load) more than 1000 g / 10 min, melt viscosity (BL type viscometer, 140°C) 4200 mPa s, number average molecular weight (Mn) 5000) Polyolefin (b-5): Partially saponified EVA (ethylene unit content 93 mol%, degree of saponification 50 mol%, MFR (190°C, 2.160 kg load) 120 g / 10 min, number average molecular weight (Mn) unknown) obtained by saponifying EVA ("Ultrathene (trademark) 680" manufactured by Tosoh Corporation, ethylene unit content 93 mol%, MFR (190°C, 2.160 kg load) 150 g / 10 min) by a known method. Polyolefin (b-6): EVA ("Ultrathene (trademark) 636" manufactured by Tosoh Corporation, ethylene unit content 89 mol%, MFR (190°C, 2.16 kg load) 2.5 g / 10 min, number average molecular weight (Mn) unknown). The MFRs of the gas barrier resin (a) and polyolefin (b) were measured in accordance with JIS K7210-1 (2014).

[0115] Example 1 (1) Preparation of Resin Composition (A) Containing Gas Barrier Resin (a) for Layer (X) 100 parts by mass of EVOH (a-1) pellets, 2 parts by mass of polyolefin (b-1) pellets, and calcium stearate were dry-blended so that the calcium ion content in the resulting resin composition was 250 ppm, and then melt-kneaded to obtain resin composition (A) pellets for Layer (X). The extruder used for melt-kneading was a twin-screw extruder with a D (mm) of 25 and a co-rotating, fully intermeshing screw with an L / D ratio of 30. A mixing zone consisting of a feed-type kneading disc, a neutral-type kneading disc, and a return-type kneading disc in succession was located midway through the screw, and a vacuum vent was located downstream of the zone. The resin temperature was maintained at 230°C.

[0116] (2) Thermogravimetry (TG) of Resin Composition (A) Pellets Thermogravimetry (TG) was performed on the obtained resin composition (A) pellets under conditions of holding at 200°C for 30 minutes in a nitrogen atmosphere to measure the weight loss (W). The results are shown in Table 1.

[0117] (3) Resin composition containing adhesive resin (B) for layer (Y) A maleic anhydride-modified polyethylene "ADMER (trademark) NF518" manufactured by Mitsui Chemicals, Inc. (MFR (190°C, 2.160 kg load) 3.1 g / 10 min, melting point 121°C, density 0.91 g / cm 3 The resin composition pellets for the layer (Y) were prepared by subjecting the adhesive resin (B) to the polymerization of 1.0 mg KOH / g (1.8 mg KOH / g, acid value 1.8 mg KOH / g). In this specification, a substance consisting essentially of only one component is also referred to as a composition.

[0118] (4) Resin composition containing polyolefin resin (C) for layer (Z) Low-density polyethylene "INNATE (trademark) TF80" (MFR (190°C, 2.160 kg load) 1.6 g / 10 min, melting point 124°C, density 0.926 g / cm) manufactured by DOW 3 ) was used as polyolefin resin (C) as resin composition pellets for layer (Z).

[0119] (5) Preparation of Multilayer Films Using the resin composition pellets obtained in (1), (3), and (4) above, multilayer films having an average thickness and layer structure of (X) / (Y) / (Z) = 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32 were prepared using coextrusion film-forming equipment. Each extruder was a single-screw extruder with a D (mm) of 30, and a full-flight screw with an L / D of 28 and a compression ratio of 3.0. A 350 mm wide feedblock lamination type T-die was used as the die. The temperature conditions used are shown below. The ratio of the total average thickness of the layers primarily composed of polyethylene-based resin in the multilayer film (PO-based thickness ratio) was 90%. Extrusion temperature of resin composition (A): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Extrusion temperature of resin composition containing adhesive resin (B): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Extrusion temperature of resin composition containing polyolefin resin (C): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Die temperature: 240°C Chill roll temperature: 50°C

[0120] (6) Die Build-Up Evaluation The multilayer film (5) was produced continuously for 6 hours, and after 6 hours, die build-up that occurred near the T-die lip on the layer (X) side was visually evaluated and judged according to the following criteria. A rating of E was determined to indicate poor die build-up properties (die build-up not being suppressed). The results are shown in Table 2. Judgment: Criteria A: No die build-up was observed across the entire width even after 6 hours of operation. B: A slight amount of die build-up was observed after 6 hours of operation. C: Die build-up was observed after 4 hours of operation, and then an increase in die build-up was observed. D: Die build-up was observed after 2 hours of operation, and then an increase in die build-up was observed. E: Die build-up was observed after 1 hour of operation, and then an increase in die build-up was observed.

[0121] (7) Oxygen Transmission Rate of Multilayer Film The oxygen transmission rate of the multilayer film obtained in (5) above was measured in accordance with the method described in JIS K7126-2 (isobaric method; 2006) with the layer (Z) as the oxygen supply side. Specifically, the oxygen transmission rate (unit: cc / (m)) was measured using an oxygen transmission rate measuring device ("MOCON OX-TRAN2 / 21" manufactured by Modern Control Co., Ltd.) under the conditions of a temperature of 20°C, a humidity of 65% RH on the oxygen supply side, a humidity of 65% RH on the carrier gas side, an oxygen pressure of 1 atmosphere, and a carrier gas pressure of 1 atmosphere. 2 The gas barrier properties were evaluated based on the following criteria: Nitrogen gas containing 2% by volume of hydrogen gas was used as the carrier gas. When the evaluation was E, it was determined that the gas barrier properties were poor. The results are shown in Table 2. Evaluation: Criteria A: 1 cc / (m 2 ・day・atm) B: 1cc / (m 2 ・day・atm) or more, 3cc / (m 2 ・day・atm) C: 3cc / (m 2 ・day・atm) or more, 10cc / (m 2 · day · atm) less than D: 10cc / (m 2 ・day・atm) or more, 60cc / (m 2 ・day・atm) Less than E: 60cc / (m 2 ・day・atm) or more

[0122] (8) Preparation of multilayer structure A two-component reactive polyurethane adhesive (24 parts by mass of "Takelac (trademark) A-520" manufactured by Mitsui Chemicals, Inc. and 4 parts by mass of "Takenate (trademark) A-50") was mixed with 37 parts by mass of ethyl acetate to prepare an adhesive solution. Next, the adhesive solution was applied to the corona-treated surface of a resin layer (R) (an LLDPE film having an average thickness of 50 μm ("Unilux (trademark) LS-760C" manufactured by Idemitsu Unitech Co., Ltd.)) so that the average thickness after drying was 2 μm using a wire bar, dried at 100 ° C. for 5 minutes, and laminated with the multilayer film obtained in (5) to prepare a multilayer structure having an average thickness and layer structure of (R) / adhesive / (X) / (Y) / (Z) = 50 μm / 2 μm / 4 μm / 4 μm / 32 μm. The adhesion temperature (heat roll temperature) during lamination was 80°C, and then aging was carried out at 40°C for 3 days.

[0123] (9) Coloring evaluation and recyclability evaluation of the multilayer structure The pulverized product obtained by pulverizing the multilayer structure obtained in (8) into a size of 4 mm square or less and low-density polyethylene (LDPE) "Novatec (trademark) LD LJ400" manufactured by Nippon Polyethylene Co., Ltd. (MFR (190 °C, 2.160 kg load) 1.5 g / 10 min, melting point 111 °C, density 0.921 g / cm 3 ) were dry-blended at a mass ratio (recovered material / low-density polyethylene) of 50 / 50, and a single-layer film (recovered material) with an average thickness of 100 μm was obtained by performing single-layer film formation under the following extrusion conditions. Also, as a control, a single-layer film with an average thickness of 100 μm (hereinafter sometimes simply referred to as "control") was obtained using only the low-density polyethylene. The extruder was a single-screw extruder with D (mm) = 20, and a full-flight screw with L / D = 20 and a compression ratio of 3.5 was used. As the die, a 300 mm-wide T-die was used. The average thickness of the single-layer film was adjusted by appropriately changing the screw rotation speed and the take-up roll speed. The temperature conditions at this time are shown below. Extrusion temperature: supply section / compression section / measurement section / adapter = 175 / 220 / 220 / 220 °C Die temperature: 220 °C Cooling roll temperature: 80 °C Regarding the coloring situation and defects of the obtained single-layer film (recovered material), a visual comparison with the control was made, and the judgment was made according to the following criteria. In addition, when the evaluation of defects was E, it was judged that the recyclability was insufficient. The results are shown in Table 2. Judgment of coloring: Criteria A: Compared with the control, the degree of hue change was small. B: Compared with the control, slight coloring was observed. C: Compared with the control, medium coloring was observed. D: Compared with the control, significant coloring was observed. E: Compared with the control, significant coloring was observed, and unevenness was also observed. Judgment of defects (recyclability): Criteria A: Compared with the control, the amount of lumps hardly changed. B: Compared with the control, the amount of small lumps was slightly more. C: Compared with the control, the amount of small lumps was large. D: Compared with the control, the amount of large lumps was large. E: Compared with the control, the amount of large lumps was very large.

[0124] Examples 2 to 23, 35, and 36, and Comparative Examples 3 and 4: Resin composition pellets, multilayer films, and multilayer structures were prepared and evaluated in the same manner as in Example 1, except that the type of gas barrier resin (a), the type and content of polyolefin (b), the content of alkali metal ions (c), and the type and content of polyvalent metal ions (d) were as shown in Tables 1 and 3. The contents of alkali metal ions (c) and polyvalent metal ions (d) in Tables 1 and 3 are based on the total mass of the resin composition (A). The results are shown in Tables 1 to 4. In Examples 12 and 13, magnesium stearate was used instead of calcium stearate, and in Examples 16 and 17, zinc stearate was used instead of calcium stearate. In Examples 18 and 23, calcium stearate was not added during melt-kneading to prepare the gas barrier resin (a)-containing resin composition (A) for layer (X) (1) in Example 1.

[0125] Example 24 Gas barrier resin-containing resin composition pellets were prepared in the same manner as in Example 1, except that no polyolefin (b-1) was added. Thereafter, 100 parts by mass of the obtained resin composition and 2 parts by mass of polyolefin (b-1) pellets were dry-blended to prepare a dry blend, which was used as the resin composition for layer (X). A multilayer film and a multilayer structure were prepared and evaluated in the same manner as in Example 1. The results are shown in Tables 3 and 4.

[0126] Example 25 Resin composition pellets and a multilayer film were prepared in the same manner as in Example 1, except that an open vent was used instead of a vacuum vent when preparing resin composition (A) pellets for layer (X), and various measurements and evaluations were carried out. The results are shown in Tables 3 and 4.

[0127] Example 26 Resin composition pellets and a multilayer film were prepared in the same manner as in Example 1, except that a vacuum vent was not used when preparing the resin composition (A) pellets for layer (X), and various measurements and evaluations were carried out. The results are shown in Tables 3 and 4.

[0128] Example 27 An alumina (AlOx) vapor-deposited layer (inorganic vapor-deposited layer (I)) having an average thickness of 30 nm was laminated by a known vacuum vapor deposition method on the surface of layer (X) of the multilayer film obtained in (5) above to prepare a vapor-deposited multilayer film. Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 1, except that the vapor-deposited multilayer film was used instead of the vapor-deposited multilayer film to prepare the multilayer structure. The results are shown in Tables 3 and 4. The oxygen transmission rate was measured for the vapor-deposited multilayer film.

[0129] Example 28: Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 27, except that the alumina vapor-deposited layer was replaced with a silica (SiOx) vapor-deposited layer. The results are shown in Tables 3 and 4.

[0130] Example 29: Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 27, except that the alumina vapor-deposited layer was replaced with an aluminum (Al) vapor-deposited layer having an average thickness of 50 nm. The results are shown in Tables 3 and 4.

[0131] Example 30 Resin composition pellets, a multilayer film, and a multilayer structure were prepared in the same manner as in Example 1, except that the average thickness of each layer of the multilayer film was changed as shown in Table 4, and various measurements and evaluations were carried out. The results are shown in Tables 3 and 4.

[0132] Example 31 Using each of the resin composition pellets obtained in (1), (3), and (4), a coextruded film having an average thickness and layer structure of (X) / (Y) / (Z) = 20 μm / 20 μm / 160 μm = EVOH20 / Tie20 / PE160 was produced, and this was stretched 5 times in the longitudinal direction (MD direction) to produce a multilayer film having an average thickness and layer structure of 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32. Except for using this multilayer film, resin composition pellets, multilayer films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Tables 3 and 4.

[0133] Example 32 Gas barrier resin-containing resin composition pellets were prepared in the same manner as in Example 1, except that EVOH (a-5) was used instead of EVOH (a-1). The resulting resin composition pellets and the resin composition pellets obtained in (3) and (4) above were used to prepare a co-extruded film having an average thickness and layer structure of (X) / (Y) / (Z) = 128 μm / 128 μm / 1024 μm = EVOH128 / Tie128 / PE1024. This film was stretched 4 times in the longitudinal direction (MD) and then 8 times in the transverse direction (TD) to prepare a multilayer film having an average thickness and layer structure of 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32. Except for using this multilayer film, resin composition pellets, multilayer films, and multilayer structures were prepared and evaluated in the same manner as in Example 1. The results are shown in Tables 3 and 4.

[0134] Example 33 As the adhesive resin (B), a maleic anhydride-modified polypropylene "ADMER (trademark) QF551" (MFR (230°C, 2.160 kg load) 5.7 g / 10 min, melting point 144°C, density 0.89 g / cm) manufactured by Mitsui Chemicals, Inc. was used. 3 ) was used as polyolefin resin (C), and polypropylene "Novatec (trademark) PP EA7AD" (MFR (230°C, 2.160 kg load) 1.4 g / 10 min, melting point 161°C, density 0.90 g / cm) manufactured by Japan Polypropylene Corporation was used. 3 ) was used as the resin layer (R), a polypropylene film having an average thickness of 50 μm was used, and the temperature conditions during the production of the multilayer film were changed as follows. Resin composition pellets, a multilayer film, and a multilayer structure were produced and evaluated in the same manner as in Example 1. The results are shown in Tables 3 and 4. Extrusion temperature of resin composition (A): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 230°C Extrusion temperature of resin composition containing adhesive resin (B): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Extrusion temperature of resin composition containing polyolefin resin (C): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Die temperature: 240°C Chill roll temperature: 50°C

[0135] Comparative Example 1 Multilayer films and multilayer structures were produced and evaluated in the same manner as in Example 1, except that a layer (Z) (single layer film) having an average thickness of 40 μm was used instead of the multilayer film. The layer (Z) having an average thickness of 40 μm was produced by extruding only a polyolefin resin (C)-containing resin composition (low-density polyethylene "INNATE (trademark) TF80" manufactured by DOW) without simultaneously extruding the resin composition (A) and adhesive resin (B) when producing the multilayer film in Example 1, and adjusting the average thickness. The results are shown in Tables 3 and 4.

[0136] Comparative Example 2 Except for not adding polyolefin (b-1), resin composition pellets, a multilayer film, and a multilayer structure were prepared in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Tables 3 and 4.

[0137] Example 34: 100 parts by mass of PA (a-6) pellets and 2 parts by mass of polyolefin (b-1) pellets were dry blended and then melt-kneaded to obtain resin composition (A) pellets for layer (X). The extruder used for melt-kneading was a twin-screw extruder with D (mm) = 25 and a co-rotating, fully intermeshing screw with L / D = 30. A multilayer film and a multilayer structure were produced in the same manner as in Example 1, except that the resin composition (A) pellets obtained in this example were used as the resin composition (A) pellets, and various performances were evaluated. The results are shown in Tables 3 and 4.

[0138] Comparative Example 5 A resin composition, a multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 34, except that polyolefin (b-1) was not used. The results are shown in Tables 3 and 4.

[0139]

[0140]

[0141]

[0142]

Claims

1. A multilayer film having a layer (X) as an outermost layer and at least one layer different from layer (X), wherein layer (X) is a layer made only of a resin composition (A) containing at least one gas barrier resin (a) selected from the group consisting of polyamide and vinyl alcohol-based resins, and a polyolefin (b) having a melt flow rate of 3.0 g / 10 min or more at 190°C under a load of 2.160 kg, as measured in accordance with JIS K7210-1 (2014), at least one of which is a polyolefin, and wherein the resin composition (A) contains 0.1 to 20 parts by mass of polyolefin (b) per 100 parts by mass of the gas barrier resin (a).

2. The multi-layer film according to claim 1, wherein the gas barrier resin (a) is at least one selected from the group consisting of nylon 6 / 66 and an ethylene-vinyl alcohol copolymer.

3. The multi-layer film according to claim 1, wherein the gas barrier resin (a) is an ethylene-vinyl alcohol copolymer having an ethylene unit content of 20 to 50 mol % and a degree of saponification of 90 mol % or more.

4. The multilayer film according to any one of claims 1 to 3, wherein the polyolefin (b) has a melt flow rate of 10 g / 10 min or more at 190°C under a load of 2.160 kg, as measured in accordance with JIS K7210-1 (2014).

5. The multi-layer film according to any one of claims 1 to 4, wherein the polyolefin (b) is an ethylene-vinyl acetate copolymer having an ethylene unit content of 75 to 98 mol % or a saponified product thereof.

6. The multi-layer film according to claim 5, wherein the polyolefin (b) is a saponified ethylene-vinyl acetate copolymer having a degree of saponification of 30 mol % or more.

7. The multilayer film according to any one of claims 1 to 6, wherein the polyolefin (b) has a number average molecular weight (Mn) of 3,000 to 25,000.

8. The multilayer film according to any one of claims 1 to 7, wherein the resin composition (A) contains 40 ppm or more and 500 ppm or less of alkali metal ions (c).

9. A multilayer film according to any one of claims 1 to 8, wherein the resin composition (A) contains 20 ppm or more and 2,000 ppm or less of at least one polyvalent metal ion (d) selected from the group consisting of magnesium ions, calcium ions, and zinc ions.

10. The multilayer film according to any one of claims 1 to 9, wherein the layer (X) is a layer formed by melt molding pellets consisting of only the resin composition (A).

11. The multilayer film according to any one of claims 1 to 10, comprising a layer (Y) and a layer (Z) as layers different from the layer (X), the layer (Y) comprising as a main component an adhesive resin (B) having a melting point of less than 170°C, the layer (Z) comprising as a main component a polyolefin resin (C) having a melting point of less than 170°C, and the layer (X), layer (Y) and layer (Z) being laminated in this order.

12. The multilayer film according to claim 11, wherein the adhesive resin (B) is an acid-modified polyethylene or an acid-modified polypropylene.

13. The multilayer film according to claim 11, wherein the polyolefin resin (C) is polyethylene or polypropylene.

14. The multilayer film according to any one of claims 1 to 13, wherein in thermogravimetry (TG) of resin composition (A), the weight loss W when held at 200°C for 30 minutes in a nitrogen atmosphere is 0.01 to 0.3%.

15. The multilayer film according to any one of claims 1 to 14, which does not have a layer containing, as a main component, a resin having a melting point of 200°C or higher, and does not have a metal layer having an average thickness of 1 µm or more.

16. The multilayer film according to any one of claims 1 to 15, wherein the average thickness of layer (X) is 0.2 µm or more and less than 20 µm, and the ratio of the average thickness of layer (X) to the average thickness of the multilayer film is less than 25%.

17. The multilayer film of any one of claims 1 to 16, wherein the multilayer film is not oriented.

18. The multilayer film according to any one of claims 1 to 16, wherein the multilayer film is stretched uniaxially only by a factor of 3 or more and less than 12.

19. The multilayer film according to any one of claims 1 to 16, wherein the multilayer film is stretched in each of two axial directions by a factor of 3 or more and less than 12.

20. A multilayer film according to any one of claims 1 to 19, in which the ratio of the total average thickness of layers containing a polyethylene resin or a polypropylene resin as a main component is 75% or more.

21. A vapor-deposited multilayer film comprising: the multilayer film according to any one of claims 1 to 20; and an inorganic vapor-deposited layer (I) laminated on the exposed surface side of the layer (X) in the multilayer film.

22. The vapor-deposited multilayer film according to claim 21, wherein the inorganic vapor-deposited layer (I) is a vapor-deposited metal layer mainly composed of aluminum or a vapor-deposited inorganic oxide layer mainly composed of alumina or silica.

23. The oxygen transmission rate measured in accordance with JIS K7126-2 (2006) under conditions of 20°C and 65% RH is 60 cc / (m 2 The multilayer film or vapor-deposited multilayer film according to any one of claims 1 to 22, wherein the viscosity is less than 1 / day atm.

24. A multilayer structure comprising the multilayer film or vapor-deposited multilayer film according to any one of claims 1 to 23 laminated with at least one resin layer (R) containing a thermoplastic resin (D) as a main component.

25. The multilayer structure of claim 24, wherein the thermoplastic resin (D) is polyethylene or polypropylene.

26. A packaging material comprising the multi-layer structure of claim 24 or 25.

27. A recovery composition comprising a recovered multi-layer structure according to claim 24 or 25.

28. A method for recovering a multi-layer structure, comprising the steps of crushing the multi-layer structure according to claim 24 or 25 and then melt-molding the crushed multi-layer structure.

29. A method for producing a multilayer film according to any one of claims 1 to 20, comprising the steps of melt-kneading a gas barrier resin (a) and a polyolefin (b) to obtain pellets of a resin composition (A), and melt-molding the pellets of the resin composition (A) to form a layer (X).

Citation Information

Patent Citations

  • Resin composition and laminate

    JP1989279949A

  • Stretched multilayer film

    WO2010061970A1

  • Multi-layer film, and multi-layer structure in which same is used

    WO2021261560A1