Plated steel material
The plated steel material with a Zn-Al-Mg alloy layer and oriented (002) plane of the η-Zn phase addresses the lack of corrosion resistance in acidic environments, offering superior acidic environment corrosion resistance and sacrificial protection.
Patent Information
- Application Number
- PCT/JP2024/014682
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Existing plated steel materials lack effective corrosion resistance in acidic environments, such as those exposed to acid rain, where the corrosion resistance in prior art has not been adequately addressed.
A plated steel material with a Zn-Al-Mg alloy layer is developed, where the chemical composition includes specific ranges of Al, Mg, and other elements, and the (002) plane of the η-Zn phase is oriented parallel to the surface, enhancing corrosion resistance through a controlled plating process that forms a ternary eutectic structure.
The solution provides excellent corrosion resistance in acidic environments, both planar and sacrificial, by ensuring the Zn-Al-Mg alloy layer's durability and protection against corrosion, even in challenging acidic conditions.
Smart Images

Figure JP2024014682_17102024_PF_FP_ABST
Abstract
Description
Plated steel
[0001] This application claims priority from Japanese Patent Application No. 2023-064064, filed on April 11, 2023, the contents of which are incorporated herein by reference.
[0002] Steel materials having a Zn-plated layer containing Al and Mg formed on the surface thereof (Zn-Al-Mg-plated steel materials) have excellent corrosion resistance, and therefore are widely used as materials for structural members that require corrosion resistance, such as building materials.
[0003] For example, Patent Document 1 describes a plated steel sheet comprising a steel sheet and a plating layer formed on the surface of the steel sheet, the plating layer containing, in average, 0 to 90 mass % Al, 0 to 10 mass % Mg, with the remainder containing Zn and impurities, a patterned portion and a non-patterned portion arranged to have a predetermined shape, the patterned portion and the non-patterned portion each including one or two of a first region and a second region, the absolute value of the difference between the area ratio of the first region in the patterned portion and the area ratio of the first region in the non-patterned portion being 30% or more, the first region being a region having an orientation ratio of 3.5 or more, and the second region being a region having an orientation ratio of less than 3.5.
[0004] Patent Document 2 describes a Zn-Al-Mg-plated steel sheet that includes a steel sheet and a plating layer containing 4 mass % or more and 22 mass % or less of Al, 1 mass % or more and 5 mass % or less of Mg, with the balance being Zn and unavoidable impurities, in which a diffraction intensity ratio I(200) / I(111), which is the ratio of the X-ray diffraction intensity I(200) of the (200) plane of the Al phase to the X-ray diffraction intensity I(111) of the (111) plane of the Al phase, in a cross section of the plating layer parallel to the surface of the plating layer, is 0.8 or more.
[0005] Plated steel products are exposed to a variety of environments, and in areas where volcanic gases are generated or industrial areas, SOx gas in the atmosphere dissolves in rainwater and turns into acid rain, which can affect the corrosion resistance of plated steel products. However, in the prior art, little research has been done on improving corrosion resistance in acidic environments.
[0006] Patent Document 1 discloses that the diffraction peak intensity I of the (0002) plane of the Zn phase 0002 and the diffraction peak intensity of the (10-11) plane I 10-11 When a region where the intensity ratio to the non-patterned portion is 3.5 or more is defined as a first region and a region where the intensity ratio is less than 3.5 is defined as a second region, it is possible to intentionally make characters, designs, etc. appear on the surface of the plating layer by making the difference between the area ratio of the first region in the patterned portion and the area ratio of the first region in the non-patterned portion 30% or more, but corrosion resistance in acidic environments is not considered.
[0007] In Patent Document 2, the orientation of the Al phase in the plating layer is controlled to give the plating layer a fine-grained, smooth, pear-skin appearance with many shiny portions, but corrosion resistance in an acidic environment is not considered.
[0008] Japanese Patent Application Publication No. 2021-85086 International Publication No. 2011 / 001662
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plated steel material that is excellent in sacrificial corrosion resistance and corrosion resistance in an acidic environment.
[0010] In order to solve the above problems, the present invention employs the following configuration: [1] A steel material and a plating layer on the steel material, wherein the chemical composition of the plating layer contains, in mass %, Al: 6.0 to 30.0%, Mg: 3.0 to 15.0%, Fe: 0.01 to 15.00%, Si: 0 to 2.0%, and Ca: 0 to 2.00%; Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1.00%, Z r: 0-1.00%, Ni: 0-1.000%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0-1.000%, C A plated steel material containing one or more elements selected from the group consisting of e: 0-1.000%, B: 0-0.500%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.50%, V: 0-0.500%, and W: 0-0.50%, with the total amount of these elements being 0-5.0%, and the balance being Zn and impurities, wherein the diffraction intensity obtained from X-ray diffraction measurement of the plated layer satisfies the following formula (1): 0.5≦I(002) Zn / {I(100) Zn +I(101) Zn}≦25.0 (1) where I(002) in formula (1) Zn is the diffraction intensity of (002) of the η-Zn phase, and I(100) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase. [2] The plated steel material according to [1], wherein the Al and Mg contents of the plated layer are Al: 10.0 to 25.0% and Mg: 4.5 to 15.0%, respectively. [3] The plated steel material according to [1] or [2], wherein the Al and Mg contents of the plated layer are Al: 15.0 to 22.0% and Mg: 5.5 to 15.0%, respectively. [4] The plated steel material according to any one of [1] to [3], wherein the diffraction intensity obtained from the results of X-ray diffraction measurement of the plated layer satisfies the following formula (2): 1.5≦I(002) Zn / {I(100) Zn +I(101)Zn}≦25.0 ... (2) [5] The [α / MgZn 2 [6] The plated steel material according to any one of [1] to [4], wherein the area ratio of the [α / MgZn eutectic structure] contained in the surface structure when the plated layer is viewed from above is 5 to 70%. 2 [7] The plated steel material according to any one of [1] to [5], wherein the area ratio of the eutectic structure of the plated layer is 10 to 70%. [8] The plated steel material according to any one of [1] to [5], wherein the area ratio of the eutectic structure of the plated layer is 10 to 70%. [9] The plated steel material according to any one of [1] to [5], wherein the area ratio of the eutectic structure of the plated layer is 10 to 70%.
[10] The plated steel material according to any one of [1] to [5], wherein the area ratio of the eutectic structure of the plated layer is 10 to 70%. 2 [8] The plated steel material according to any one of [1] to [7], in which a Sn phase is detected. [9] The plated steel material according to any one of [1] to [7], containing one or two of La and Ce in a total amount of 0.005 to 0.500%.
[0011] According to the present invention, a plated steel material having excellent corrosion resistance in an acidic environment can be provided.
[0012] 1 is a cross-sectional schematic view of a plated steel material according to an embodiment of the present invention.
[0013] To improve the corrosion resistance of plated steel in acidic environments, it is necessary to form a plating layer on the surface of the steel that has excellent corrosion resistance in acidic environments such as acid rain. To improve the corrosion resistance of the plating layer in acidic environments, it is necessary that the elements that make up the plating layer are less likely to dissolve even in acidic environments.
[0014] Therefore, the inventors of the present invention have conducted extensive research to improve the corrosion resistance in acidic environments of Zn coating layers containing Al and Mg. The η-Zn phase contained in the coating layer has a hexagonal crystal structure, which includes various crystal orientation planes. The corrosion resistance of these crystal orientation planes is not uniform across all orientation planes. For example, the (002) plane of the η-Zn phase is a dense crystal orientation plane with a relatively high Zn atomic density, making Zn itself relatively difficult to dissolve and therefore considered to have relatively high corrosion resistance. On the other hand, the (100) plane of the η-Zn phase is a crystal orientation plane with a lower Zn atomic density than the (002) plane, making Zn itself relatively easy to dissolve. However, although the corrosion resistance of Zn itself is low, the corrosion products generated by the corrosion of Zn protect the base steel from corrosion, and therefore the sacrificial corrosion protection of the base steel is considered to be high. Therefore, it was thought that the corrosion resistance in an acidic environment of a Zn plating layer containing Al and Mg could be improved by orienting the (002) plane of the η-Zn phase parallel to the surface of the plating layer.
[0015] Therefore, the inventors attempted to orient the (002) plane of the η-Zn phase contained in the coating layer parallel to the surface of the coating layer. When a Zn coating layer containing Al and Mg is solidified from a molten state, the α phase first crystallizes, followed by the MgZn phase. 2 The α-phase and η-Zn phase crystallize, and further, the α-phase and MgZn 2 A ternary eutectic structure containing the η-Zn phase and the η-Zn phase is formed. The ternary eutectic temperature, which is a guideline for the onset of formation of the ternary eutectic structure, can generally be predicted based on the chemical composition of the coating layer. However, it has been found that when the eutectic reaction is caused to occur at a temperature lower than the predicted ternary eutectic temperature, the (002) plane of the η-Zn phase in the ternary eutectic structure is oriented parallel to the surface of the coating layer. Specifically, it has been found that by adjusting the immersion temperature when the steel material is immersed in the coating bath and the cooling conditions after the steel material is withdrawn from the coating bath, the eutectic reaction can be caused to occur at a temperature lower than the predicted ternary eutectic temperature, and the (002) plane of the η-Zn phase can be oriented parallel to the surface of the coating layer.
[0016] Hereinafter, a plated steel material according to an embodiment of the present invention will be described. The plated steel material according to this embodiment comprises a steel material and a plating layer disposed on the surface of the steel material, and the chemical composition of the plating layer contains, in mass %, Al: 6.0 to 30.0%, Mg: 3.0 to 15.0%, Fe: 0.01 to 15.00%, Si: 0 to 2.0%, Ca: 0 to 2.00%, Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0 to 1.00%, Zr: 0 to 1.00%, Ni: 0 to 1.000%, Mn: 0 to 1.00%, Mo: 0 to 1.00%, Ag: 0 to 1.000%, and the like. The plated steel material contains one or more elements selected from the group consisting of: 0.00%, Li: 0-1.00%, La: 0-1.000%, Ce: 0-1.000%, B: 0-0.500%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.50%, V: 0-0.500%, and W: 0-0.50%, with the total of these elements being 0-5.0%, the balance being Zn and impurities, and the diffraction intensity obtained from X-ray diffraction measurement of the plated layer satisfies the following formula (1):
[0017] 0.5≦I(002) Zn / {I(100) Zn +I(101) Zn}≦25.0 ... (1)
[0018] However, I(002) in formula (1) Zn is the diffraction intensity of (002) of the η-Zn phase, and I(100) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase.
[0019] In the following description, the "%" used to indicate the content of each element in the chemical composition means "mass %." The content of an element in the chemical composition may be expressed as element concentration (e.g., Zn concentration, Mg concentration, etc.). "Corrosion resistance in acidic environments" refers to the property of a plating layer (specifically, a Zn-Al-Mg alloy layer) that is resistant to corrosion in an acidic environment. "Plane corrosion resistance" refers to the property of the plating layer (specifically, a Zn-Al-Mg alloy layer) itself that is resistant to corrosion. "Sacrificial corrosion protection" refers to the property of inhibiting corrosion of exposed steel material (e.g., cut end surfaces of plated steel material, cracked areas in the plating layer during processing, and areas where the steel material is exposed due to peeling of the plating layer). Furthermore, "plated layer" refers to a plating film produced by a so-called hot-dip plating process.
[0020] As shown in Fig. 1, the plated steel material 1 according to this embodiment has a steel material 11. There are no particular limitations on the shape of the steel material 11, and an example of the steel material 11 is a steel plate. The steel material 11 may also be a formed, bare steel material such as a steel pipe, a civil engineering and construction material (such as a fence, a corrugated pipe, a drainage ditch cover, a sand-flying prevention plate, a bolt, a wire mesh, a guardrail, a water cut-off wall, etc.), a home appliance component (such as a housing for an outdoor unit of an air conditioner), or an automobile part (such as an undercarriage component). The forming process may be any of various plastic processing techniques, such as pressing, roll forming, and bending.
[0021] The material of the steel material 11 is not particularly limited. The steel material 11 can be various steel materials such as general steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The steel material 11 may also be a hot-rolled steel sheet, hot-rolled steel strip, cold-rolled steel sheet, or cold-rolled steel strip described in JIS G 3302:2010. There are also no particular limitations on the method for manufacturing the steel sheet (hot rolling method, pickling method, cold rolling method, etc.) and the specific manufacturing conditions thereof.
[0022] Furthermore, the steel material 11 serving as the plating base sheet may be a pre-plated steel material in which the surface of the steel material 11 is pre-plated. An example of the pre-plated steel material is a Ni pre-plated steel material having a Ni plating on the steel material 11. The pre-plated steel material can be obtained, for example, by electrolytic treatment or displacement plating. Electrolytic treatment is performed by immersing the base steel material in a sulfate bath or chloride bath containing metal ions of various pre-plating components. Displacement plating is performed by immersing the base steel material in an aqueous solution containing metal ions of various pre-plating components and having the pH adjusted with sulfuric acid, thereby causing displacement deposition of the metal.
[0023] The plated steel material 1 according to this embodiment has a plating layer 12 on a steel material 11. The plating layer 12 of the plated steel material 1 according to this embodiment is mainly composed of a Zn-Al-Mg alloy layer due to its chemical composition, which will be described later. Furthermore, the plating layer 12 of the plated steel material 1 according to this embodiment may include an Fe-Al-based interfacial alloy layer between the steel material 11 and the Zn-Al-Mg alloy layer. That is, the plating layer 12 may have a single-layer structure of a Zn-Al-Mg alloy layer, or a multilayer structure including a Zn-Al-Mg alloy layer and an Fe-Al-based interfacial alloy layer. Furthermore, the Fe-Al-based interfacial alloy layer may contain Ni.
[0024] The chemical composition of the plating layer according to this embodiment is composed of Zn and other alloying elements. The chemical composition of the plating layer will be described in detail below. Note that elements with a lower limit of 0% concentration are not essential for solving the problems of the plated steel material according to this embodiment, but are optional elements that are allowed to be included in the plating layer for the purpose of improving characteristics, etc.
[0025] <Al: 6.0 to 30.0%> Al forms an α-phase solid solution with Zn, contributing to improvements in flat corrosion resistance, acidic environment corrosion resistance, and sacrificial corrosion protection. Therefore, the Al concentration is set to 6.0% or more. The Al concentration may be set to 10.0% or more, 12.0% or more, or 15.0% or more. On the other hand, if Al is excessive, the Mg concentration and Zn concentration decrease relatively, resulting in deterioration of sacrificial corrosion protection. Therefore, the Al concentration is set to 30.0% or less. The Al concentration may be set to 28.0% or less, 25.0% or less, 22.0% or less, or 20.0% or less.
[0026] <Mg: 3.0 to 15.0%> Mg is an essential element for ensuring flat surface corrosion resistance, acidic environment corrosion resistance, and sacrificial corrosion protection. Therefore, the Mg concentration is set to 3.0% or more. The Mg concentration may be set to 4.5% or more, 5.5% or more, or 6.0% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering resistance, may deteriorate, and flat surface corrosion resistance may also deteriorate. Therefore, the Mg concentration is set to 15.0% or less. The Mg concentration may also be set to 12.0% or less, 10.0% or less, or 8.0% or less.
[0027] <Fe: 0.01% to 15.00%> The plating layer may contain 0.01% or more of Fe. It has been confirmed that an Fe concentration of 15.00% or less does not adversely affect the performance of the plating layer. The Fe concentration may be, for example, 0.05% or more, 0.10% or more, 0.50% or more, or 1.00% or more. The Fe concentration may be, for example, 10.00% or less, 5.00% or less, 2.00% or less, or 1.00% or less. Because Fe may be mixed in from the steel material, the Fe concentration may be 0.05% or more.
[0028] <Si: 0% to 2.0%> The Si concentration may be 0%. On the other hand, Si contributes to improving flat surface corrosion resistance and acidic environment corrosion resistance. Therefore, the Si concentration may be 0.05% or more, 0.1% or more, 0.2% or more, or 0.5% or more. On the other hand, if the Si concentration is excessive, flat surface corrosion resistance, acidic environment corrosion resistance, and sacrificial corrosion protection will deteriorate. Therefore, the Si concentration is set to 2.0% or less. The Si concentration may also be 1.5% or less, 1.0% or less, or 0.5% or less.
[0029] <Ca: 0% to 2.00%> The Ca concentration may be 0%. On the other hand, Ca is an element that can adjust the amount of Mg elution that is optimal for imparting flat surface corrosion resistance and acidic environment corrosion resistance. Therefore, the Ca concentration may be 0.05% or more, 0.10% or more, or 0.50% or more. On the other hand, if the Ca concentration is excessive, flat surface corrosion resistance and workability will deteriorate. Therefore, the Ca concentration is set to 2.00% or less. The Ca concentration may also be set to 1.00% or less, 0.50% or less, or 0.10% or less.
[0030] Furthermore, the plating layer according to this embodiment contains Sb: 0 to 0.50%, Pb: 0 to 0.50%, Cu: 0 to 1.00%, Sn: 0 to 1.00%, Ti: 0 to 1.00%, Cr: 0 to 1.00%, Nb: 0 to 1.00%, Zr: 0 to 1.00%, Ni: 0 to 1.000%, Mn: 0 to 1.00%, Mo: 0 to 1.00%, Ag: 0 to 1.00%, Li: 0 to The steel sheet may contain one or more elements selected from the group consisting of 1.00%, La: 0-1.000%, Ce: 0-1.000%, B: 0-0.500%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.50%, V: 0-0.500%, and W: 0-0.50%. The total of these elements is 0-5.0%. If the total exceeds 5.0%, the flat corrosion resistance, red rust resistance, and base steel corrosion resistance may be reduced. Furthermore, since these elements are optional addition elements, the total amount may be 0%.
[0031] <Sb, Pb: 0 to 0.50% each> The concentrations of Sb and Pb may be 0%. On the other hand, Sb and Pb contribute to improving sacrificial corrosion protection. Therefore, the concentrations of Sb and Pb may be 0.05% or more, 0.10% or more, or 0.15% or more. On the other hand, excessive concentrations of Sb and Pb deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of Sb and Pb are set to 0.50% or less. The concentrations of Sb and Pb may also be 0.40% or less, 0.30% or less, or 0.25% or less.
[0032] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li: 0 to 1.00% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0%. On the other hand, these elements contribute to improving sacrificial corrosion protection. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0.05% or more, 0.08% or more, or 0.10% or more. On the other hand, excessive concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li deteriorate flat surface corrosion resistance. Therefore, the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li are each set to 1.00% or less. The concentration of each of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may be 0.80% or less, 0.70% or less, or 0.60% or less.
[0033] <Ni: 0 to 1.000%> The Ni concentration may be 0%. However, these elements contribute to improving sacrificial corrosion protection. Therefore, the Ni concentration may be 0.050% or more, 0.080% or more, or 0.100% or more. However, if the Ni concentration is excessive, the corrosion resistance of flat surfaces will deteriorate. Therefore, the Ni concentration is set to 1.000% or less. The Ni concentration may also be 0.800% or less, 0.700% or less, or 0.600% or less.
[0034] <Sn: 0 to 1.00%> The Sn concentration may be 0%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the sacrificial corrosion protection of the plating layer. Therefore, the Sn concentration may be 0.01% or more, 0.05% or more, or 0.10% or more. However, if the Sn concentration is excessive, planar corrosion resistance will deteriorate. Therefore, the Sn concentration is set to 1.00% or less. The Sn concentration may also be 0.50% or less, 0.30% or less, or 0.20% or less.
[0035] <La, Ce: 0 to 1.000% each> The concentrations of La and Ce may each be 0%. On the other hand, La and Ce contribute to improving sacrificial corrosion protection. Therefore, the concentrations of La and Ce may each be 0.100% or more, 0.150% or more, or 0.200% or more. On the other hand, excessive concentrations of La and Ce deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of La and Ce are each set to 1.000% or less. The concentrations of La and Ce may each be set to 0.500% or less. Furthermore, the total of one or both of La and Ce may be set to 0.010 to 0.500%.
[0036] <B: 0 to 0.500%> The concentration of B may be 0%. On the other hand, B contributes to improving sacrificial corrosion protection. Therefore, the concentration of B may be 0.100% or more, 0.150% or more, or 0.200% or more. On the other hand, if the concentration of B is excessive, the corrosion resistance of flat surfaces deteriorates. Therefore, the concentration of B is set to 0.500% or less. The concentration of B may also be set to 0.400% or less, or 0.300% or less.
[0037] <Y, P, and Sr: 0 to 0.50% each> The concentrations of Y, P, and Sr may each be 0%. On the other hand, Y, P, and Sr contribute to improving sacrificial corrosion protection. Therefore, the concentrations of Y, P, and Sr may each be 0.10% or more, 0.15% or more, or 0.20% or more. On the other hand, excessive concentrations of Y, P, and Sr deteriorate flat surface corrosion resistance. Therefore, the concentrations of Y, P, and Sr each are set to 0.50% or less. The concentrations of Y, P, and Sr each may be set to 0.40% or less, or 0.30% or less.
[0038] <Co, Bi, V: 0 to 0.500% each> The concentrations of Co, Bi, and V may each be 0%. On the other hand, Co, Bi, and V contribute to improving sacrificial corrosion protection. Therefore, the concentrations of Co, Bi, and V may each be 0.100% or more, 0.150% or more, or 0.200% or more. On the other hand, excessive concentrations of Co, Bi, and V deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of Co, Bi, and V are each set to 0.500% or less. The concentrations of Co, Bi, and V may each be set to 0.400% or less, or 0.300% or less.
[0039] <In, W: 0 to 0.50% each> The concentrations of In and W may each be 0%. On the other hand, In and W contribute to improving sacrificial corrosion protection. Therefore, the concentrations of In and W may each be 0.10% or more, 0.15% or more, or 0.20% or more. On the other hand, excessive concentrations of In and W deteriorate the corrosion resistance of flat surfaces. Therefore, the concentrations of In and W are each set to 0.50% or less. The concentrations of In and W may each be set to 0.40% or less, or 0.30% or less.
[0040] <Balance: Zn and Impurities> The balance of the components of the plating layer according to this embodiment is Zn and impurities. Zn is an element that provides the plating layer with flat corrosion resistance, acidic environment corrosion resistance, and sacrificial corrosion protection. In this embodiment, "impurities" refers to elements that are mixed in from the manufacturing environment, etc., and elements that are tolerated to the extent that they do not adversely affect the properties of the plated steel material according to this embodiment. For example, trace amounts of elements other than Fe may be mixed into the plating layer as impurities due to mutual atomic diffusion between the base steel material and the plating bath.
[0041] The chemical composition of the plating layer is measured by the following method. For example, a plated steel material is cut into a size of 30 mm x 30 mm to obtain a measurement sample. Next, the plating layer of the measurement sample is stripped and dissolved using a 10% aqueous hydrochloric acid solution containing 0.06 mass% of an inhibitor (Ivit 710K, manufactured by Asahi Chemical Industry Co., Ltd.) that suppresses corrosion of steel materials, to obtain an acid solution. The obtained acid solution is then subjected to ICP analysis. This allows the chemical composition of the plating layer to be obtained. Note that when cutting the plated steel material, it is preferable to avoid the edges and welds of the plated steel material. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. For example, 10% by volume of HCl is used. Note that the chemical composition is measured three times using the above method, and the average of the measurements is used as the chemical composition of the plating layer.
[0042] Next, the metal structure of the plating layer will be described.
[0043] The plating layer contains α-phase and MgZn 2 The α phase contains a fine Al phase and a fine Zn phase. 2 The phase is partially lamellar binary eutectic structure (α phase / MgZn 2eutectic structure of α phase / MgZn 2 However, when the α phase and MgZn eutectic structure are contained, the corrosion resistance of the flat surface of the coating layer is further improved. 2 The excessive precipitation of the phase causes the formation of the α phase / MgZn 2 When a large amount of the eutectic structure of α-Zn is contained, the proportion of the η-Zn phase becomes relatively small, and the red rust resistance and corrosion resistance of the base steel deteriorate. 2 The area ratio of the eutectic structure of [α phase / MgZn] is preferably in the range of 70% or less, more preferably in the range of 5 to 70%, and may be in the range of 10 to 70%. 2 The eutectic structure of the alloy may be 0% or more than 0%.
[0044] In addition, the plating layer of this embodiment contains α-phase and MgZn 2 In addition to the α-Zn phase, the η-Zn phase is also present. The η-Zn phase is at least partially composed of the α-phase and MgZn 2 The η-Zn phase forms a ternary eutectic structure together with the η-Zn phase. The η-Zn phase may be contained in the plating layer as a massive η-Zn phase.
[0045] In addition, when the plating layer contains 0.05 to 0.5% Sn, the plating layer contains Mg 2 The Sn phase is definitely included. 2 The Sn phase may be contained even when the Sn content is 0.05% or less. 2 Since the Sn phase is present in a small amount, its presence can be confirmed by X-ray diffraction measurement. 2 The inclusion of the Sn phase further improves the sacrificial corrosion resistance of the plated steel material.
[0046] X-ray diffraction measurement was performed using Kα rays from a Cu tube, and if a peak was detected at 23.4±0.3°, it was determined that the Mg2Sn phase was present. Using an X-ray diffractometer (Rigaku Corporation, model number RINT-TTR III), X-ray output was 50 kV, 300 mA, copper target, goniometer TTR (horizontal goniometer), Kβ filter slit width 0.05 mm, longitudinal limiting slit width 2 mm, receiving slit width 8 mm, receiving slit 2 open, and measurement conditions were a scan speed of 5° / min, a step width of 0.01°, and a scan axis 2θ (5 to 90°).
[0047] The plating layer may contain other phases as the balance, such as an Al—Ca—Si phase.
[0048] Next, the crystal orientation of the η-Zn phase will be described. In the plating layer of this embodiment, the X-ray diffraction intensity obtained from the X-ray diffraction measurement of the plating layer must satisfy the relationship of the following formula (1). When the following formula (1) is satisfied, the (002) plane of the η-Zn phase is oriented parallel to the surface of the plating layer, improving corrosion resistance in an acidic environment. It is more preferable that the following formula (2) is satisfied. I(002) Zn / {I(100) Zn +I(101) Zn If the I(002)} is less than 0.5, the orientation of the (002) plane of the η-Zn phase is insufficient, resulting in insufficient corrosion resistance in an acidic environment. Zn / {I(100) Zn +I(101) Zn If the value of} exceeds 25.0, the sacrificial corrosion protection may be reduced.
[0049] 0.5≦I(002) Zn / {I(100) Zn +I(101) Zn}≦25.0 ... (1)
[0050] 1.5≦I(002) Zn / {I(100) Zn +I(101) Zn}≦25.0 ... (2)
[0051] However, I(002) in formula (1) and formula (2)Zn is the diffraction intensity of (002) of the η-Zn phase, and I(100) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase.
[0052] [α phase / MgZn 2 The method for measuring the area ratio of the eutectic structure of MgZn is as follows. First, the surface of the plating layer is adjusted to be flat by mechanical polishing. Next, the surface of the plating layer is chemically polished by colloidal polishing until the surface is polished to a mirror finish. The polished surface of the plating layer is observed with an SEM. Specifically, an element distribution image is taken using an SEM-EDS at a magnification of 5000 times (area of 200 μm vertical and 200 μm horizontal). In this element distribution image, a phase in which Mg and Zn coexist is identified as MgZn 2 The phase containing Al and Zn is identified as the α phase. Most of the α phase shows a dendritic morphology. The α phase and MgZn 2 phase and [α phase / MgZn 2 After identifying the eutectic structure of the α phase / MgZn 2 The area ratio of the eutectic structure is calculated by binarization using image analysis software.
[0053] I(002) in formula (1) and formula (2) Zn / {I(100) Zn +I(101) ZnThe measurement method for the {} is as follows. First, the surface of the plating layer is mechanically polished, and if necessary, chemically polished to make the surface of the plating layer into a mirror-finished state. Then, for example, an X-ray diffraction apparatus (manufactured by Rigaku Corporation (Model No. RINT-TTR) X-ray diffraction measurements were performed using a TTR (horizontal goniometer) with an X-ray output of 50 kV, 300 mA, a copper target, a Kβ filter slit width of 0.05 mm, a longitudinal limiting slit width of 2 mm, a receiving slit width of 8 mm, and a receiving slit 2 open. Measurement conditions included a scan speed of 5 deg. / min, a step width of 0.01 deg., and a scan axis 2θ (5 to 90°). The diffraction intensity of the (100) plane of the η-Zn phase (maximum intensity in the range of 38.993 ± 0.2°), the diffraction intensity of the (002) plane (maximum intensity in the range of 36.297 ± 0.2°), and the diffraction intensity of the (101) plane (maximum intensity in the range of 43.232 ± 0.2°) were measured. The diffraction intensities were calculated by subtracting the background intensity. From the obtained diffraction intensities, the I(002) Zn / {I(100) Zn +I(101) Zn} is sought.
[0054] In addition, Mg 2 Whether or not the Sn phase is contained can be determined by examining the Mg 2 The determination is made based on whether or not a diffraction peak specific to Sn appears.
[0055] The coating weight of the plating layer per side is, for example, 20 to 300 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 300 g / m or more, the flat corrosion resistance, acidic environment corrosion resistance, and sacrificial corrosion resistance of the plated steel material can be further improved. 2 By setting the following, the workability of the plated steel material can be further improved.
[0056] Next, a method for producing the plated steel material according to this embodiment will be described, but the method for producing the plated steel material according to this embodiment is not particularly limited. For example, the plated steel material according to this embodiment can be obtained according to the production conditions described below.
[0057] In the method for producing a plated steel material according to this embodiment, a steel material is annealed in a reducing atmosphere, and after the temperature of the annealed steel material is reduced to (coating bath temperature - 20)°C or less, the steel material is immersed in a hot-dip coating bath and then pulled out of the hot-dip coating bath, thereby forming a coating layer on the surface of the steel material. Next, the steel material is immersed in a hot-dip coating bath at a flux of 5000 (L / min / m) until the temperature of the coating layer is raised from the bath temperature to 320°C. 2 ) or less, while blowing cooling gas at an average cooling rate of 15 ° C / sec or more, and then, in the range of 320 to 260 ° C, 2 ) or higher, the material is cooled at an average cooling rate of 5°C / sec or less while blowing cooling gas onto the material.
[0058] Annealing of the steel material to be plated is carried out in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. By this annealing, oxides present on the surface of the steel material are removed as much as possible.
[0059] Next, the steel immediately after annealing is cooled by a cooling gas such as nitrogen until the temperature of the steel reaches (the plating bath temperature - 20) ° C. or less, and then immersed in a hot dip plating bath. By lowering the temperature of the steel by 20 ° C. or more than the plating bath temperature, the surface roughness of the Fe-Al-based interfacial alloy layer (surface roughness on the Zn-Al-Mg alloy layer side) formed at the interface between the steel and the plating layer is reduced.
[0060] The chemical composition of the plating bath may be adjusted as needed to obtain the above-described chemical composition of the plating layer. The temperature of the plating bath is not particularly limited, and any temperature at which hot-dip plating can be performed may be appropriately selected. For example, the plating bath temperature may be set to a value approximately 20°C or more higher than the melting point of the plating bath.
[0061] Next, the steel material is pulled up from the hot-dip galvanizing bath. The coating weight of the coating layer can be controlled by controlling the pulling speed of the steel material. If necessary, the coating weight of the coating layer may be controlled by wiping the steel material to which the coating layer is attached. The coating weight of the coating layer is not particularly limited and can be, for example, within the above-mentioned range.
[0062] Next, the coating layer is cooled. The coating layer is first cooled from the bath temperature to 320°C at an average cooling rate of 15°C / sec or more. The average cooling rate from the bath temperature to 320°C may be 30°C / sec or less. The cooling is performed, for example, by spraying a cooling gas, and the cooling gas flux is set to 5000 (L / min / m 2 ) or less to minimize vibration of steel materials. 2 When cooling is performed by spraying cooling gas, a plurality of nozzles for spraying the cooling gas may be arranged along the transport path of the steel material, and the cooling gas may be sprayed from the nozzles.
[0063] In the bath temperature range from 320°C, α phase and MgZn 2 The phase is crystallized, and further the α phase and MgZn 2 The eutectic reaction proceeds to form the α phase and MgZn 2 Binary eutectic structure with phase (α phase / MgZn 2 In this case, by cooling the steel material at a rate of 15°C / sec or more in the range from the bath temperature to 320°C while suppressing the flux of the cooling gas to suppress vibration of the steel material, the crystallization of the ternary eutectic structure originating from the surface of the coating layer becomes less likely to proceed.
[0064] Next, the range of 320 to 260°C was set at a flux of 25,000 (L / min / m 2 ) or more, while spraying cooling gas at an average cooling rate of 5°C / sec or less. In this case, multiple spray nozzles for the cooling gas are also arranged along the steel material transport path. The flow rate is set to 25,000 (L / min / m 2 ) or more, the cooling gas is blown onto the plating layer to vibrate it. The cooling gas flux in the range of 320 to 260°C is 80,000 (L / min / m 2 ) or less. This initiates the crystallization of the ternary eutectic structure, which has been suppressed until now, and at this time, the (002) plane of the η-Zn phase contained in the ternary eutectic structure is oriented so as to be parallel to the surface of the plating layer.
[0065] In the cooling range from the bath temperature to 320°C and the cooling range from 320°C to 260°C, the cooling gas to be sprayed is not particularly limited, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or air, or a mixed gas of these.
[0066] When controlling the flux of cooling gas, the shape of the gas nozzle from which the cooling gas is ejected is, for example, in the range of 1 to 50 mm in diameter. The angle between the tip of the gas nozzle and the steel plate is, for example, in the range of 70 to 110°, more preferably 90° (right angle). The distance between the tip of the gas nozzle and the steel plate is in the range of 30 to 1000 mm. Note that the shape, angle, and distance of the gas nozzle are merely examples and are not limited to the above ranges.
[0067] The cooling conditions below 260°C are not particularly limited, and either air cooling or natural cooling may be used.
[0068] By cooling the plating layer so as to satisfy the above-mentioned conditions, a plating layer that satisfies the above formula (1) is formed. The reason for this is presumed to be as follows.
[0069] In the above manufacturing method, by lowering the temperature of the steel material when immersed in the coating bath by 20°C or more below the coating bath temperature, the surface roughness of the Fe-Al-based interface alloy layer is reduced and the number of nucleation sites for the ternary eutectic structure is reduced. The temperature difference between the temperature of the steel material when immersed in the coating bath and the coating bath temperature is 40°C or less. If the temperature difference between the temperature of the steel material when immersed in the coating bath and the coating bath temperature exceeds 40°C, poor coating appearance occurs. Then, when the steel material immersed in the coating bath is pulled up, the steel material is rapidly cooled in the range from the bath temperature to 320°C while suppressing vibration of the steel material, thereby forming an α-phase and MgZn in the coating layer. 2 While the crystallization of the ternary eutectic structure is suppressed, the temperature at which the eutectic reaction begins is set lower than the eutectic start temperature predicted from the plating composition. Next, by cooling in the range of 320°C to 260°C under the above conditions, the crystallization of the ternary eutectic structure begins, but because the crystallization begins at a temperature lower than the eutectic start temperature predicted from the plating composition, it is believed that the (002) plane of the η-Zn phase contained in the ternary eutectic structure becomes oriented parallel to the surface of the plating layer, thereby satisfying the above formula (1).
[0070] Examples of the present invention will be described below. However, the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0071] The plated base sheet was a hot-rolled steel sheet having a thickness of 1.6 mm. The plated base sheet was annealed. The annealing conditions were: N 2 -4% H 2 The conditions were a soaking temperature of 800°C and a soaking time of 2 minutes in a nitrogen atmosphere. 2 The steel sheets were cooled with gas to adjust the temperature at the time of immersion in the plating bath to (plating bath temperature - 20) ° C. or less, and then immersed in various hot dip plating baths, and then pulled up at a pulling speed of 20 to 200 mm / sec. 2 The coating weight was controlled by wiping gas. After the steel material was pulled out of the coating bath, it was cooled under the conditions shown in Table 2.
[0072] When cooling in the bath temperature range of up to 320°C and 320 to 260°C, the cooling gas was N 2 The cooling gas was used, and the gas flux was controlled as shown in the table. The gas nozzle from which the cooling gas was ejected had a diameter of 6 mm, the angle between the tip of the gas nozzle and the steel sheet was a right angle, and the distance between the tip of the gas nozzle and the steel sheet was 35 mm. In this manner, plated steel products No. 1 to 50 were produced.
[0073] The chemical composition of the plating layer was as shown in Table 1. The metallographic structure of the plating layer was evaluated, and the results are shown in Table 3. Furthermore, the acidic environment corrosion resistance and sacrificial corrosion protection of the plated steel material were evaluated, and the results are shown in Table 3.
[0074] The chemical composition of the plating layer was measured by immersing a sample cut into a size of 30 mm × 30 mm in a 10% HCl aqueous solution containing an inhibitor to pickle and remove the plating layer, and then performing ICP analysis of the elements eluted into the aqueous solution.
[0075] [α phase / MgZn 2The area ratio of the eutectic structure of MgZn was evaluated as follows. First, the surface of the plating layer was polished to a mirror finish by mechanical polishing and colloidal polishing. Next, the plating layer surface was observed at a magnification of 5000 times (area of 200 μm long and 200 μm wide) using a field emission scanning electron microscope (FE-SEM) equipped with an energy dispersive elemental analyzer (EDS), and an element distribution image was taken using the EDS. In the element distribution image, a phase in which Mg and Zn coexist was designated as MgZn 2 The phase containing Al and Zn is identified as the α phase, and the phase containing Al and Zn is identified as the α phase. 2 The eutectic structure of α phase / MgZn was identified. 2 The area ratio of the eutectic structure was calculated by binarization using image analysis software.
[0076] I(002) in formula (1) Zn / {I(100) Zn +I(101) Zn The measurement method for {} was as follows. First, the surface of the plating layer was polished to a mirror finish in the same manner as above. Next, X-ray diffraction measurement was performed using an X-ray diffractometer (Rigaku Corporation, model number RINT-TTR III) with an X-ray output of 50 kV, 300 mA, a copper target, a goniometer TTR (horizontal goniometer), a Kβ filter slit width of 0.05 mm, a longitudinal limiting slit width of 2 mm, a receiving slit width of 8 mm, and a receiving slit 2 open, under the measurement conditions of a scan speed of 5 deg. / min, a step width of 0.01 deg, and a scan axis 2θ (5 to 90°). Then, the diffraction intensity of the (100) plane of the η-Zn phase (maximum intensity in the range of 38.993±0.2°), the diffraction intensity of the (002) plane (maximum intensity in the range of 36.297±0.2°), and the diffraction intensity of the (101) plane (maximum intensity in the range of 43.232±0.2°) were measured. The diffraction intensity was the intensity excluding the background intensity. From the obtained diffraction intensities, the I(002) Zn / {I(100) Zn +I(101) Zn} was sought.
[0077] Mg in the plating layer 2Whether or not the Sn phase is contained can be determined by examining the Mg 2 The determination was made based on whether or not a diffraction peak specific to Sn appeared.
[0078] The corrosion resistance in an acidic environment was evaluated as follows. Test specimens were prepared by cutting the plated steel material into pieces measuring 150 mm x 50 mm. The end faces of the test specimens were protected with polyester tape manufactured by Nitto Denko Corporation to prevent exposure, and the area of the flat portion to be used for corrosion evaluation was then measured.
[0079] The test specimens, whose end faces were protected with tape, were then subjected to the artificial acid rain cycle test specified in JIS H8502:1999. The artificial acid rain cycle test consisted of one cycle of spraying the acid test solution (spraying time: 2 hours, temperature: 35°C, pH: 3.5), drying (drying time: 4 hours, temperature: 60°C, humidity: 20-30% RH), and wetting (wetting time: 2 hours, temperature: 50°C, humidity: 95% RH), and this cycle was repeated. The acid test solution used was 5% NaCl to which HNO3·H2SO4 was added, and the pH was adjusted to 3.5 with NaOH.
[0080] After the artificial acid rain cycle test, the tape protecting the end faces of the test pieces was peeled off, and the test pieces were immersed in a 30% chromic acid (VI) solution at 25°C for 10 minutes to remove corrosion products that had formed on the sample surface. The weight of the test pieces after immersion in the chromic acid (VI) solution was measured, and the difference from the weight before the test was calculated. This was then divided by the area of the evaluation surface to convert it into corrosion weight loss and evaluate corrosion resistance. The evaluation criteria were as follows: "AAAA", "AAA", "AA", and "A" were considered pass. "AAAA", "AAA", "AA", and "A" were considered pass.
[0081] AAAA: Corrosion weight loss of 20 g / m after 60 cycles 2 AAA: Corrosion weight loss of 20 g / m after 60 cycles 2 Super 40g / m 2 AA: Corrosion weight loss of 40 g / m after 60 cycles 2 Super 60g / m 2 A: Corrosion weight loss after 60 cycles is 60 g / m 2 Super 100g / m 2B: Corrosion weight loss after 60 cycles is 100 g / m 2 super
[0082] Sacrificial corrosion protection (simulated edge corrosion resistance) was evaluated as follows. Plated steel was cut into 100 mm x 100 mm pieces to prepare test specimens. The plating layer in a 25 mm diameter area centered on the intersection of the diagonal lines of the test specimen was removed by milling to expose the steel sheet (base steel). The exposed 25 mm diameter area of the base steel was subjected to a neutral salt spray test as specified in JIS Z2371:2015, and evaluation was based on the occurrence of red rust in the exposed area of the base steel. The evaluation criteria for sacrificial corrosion protection are as follows: "AAA", "AA", and "A" were considered to be acceptable.
[0083] AAA: Red rust area ratio 5% or less after 2200 hours AA: Red rust area ratio over 5% and 10% or less after 1800 hours A: Red rust area ratio over 10% and 15% or less after 1000 hours B: Red rust area ratio over 15% after 1000 hours
[0084] In Nos. 1 to 32, 42 to 45, 47, 48, and 50 (Examples) according to the present invention, the chemical composition and metal structure of the plating layer were appropriately controlled, and both the acidic environment corrosion resistance and sacrificial corrosion resistance were excellent.
[0085] Comparative Example No. 33 had an insufficient amount of Al in the plating layer, and therefore, No. 33 had insufficient corrosion resistance in an acidic environment.
[0086] Comparative Example No. 34 had an excessive amount of Al in the coating layer. As a result, in No. 34, excessive α-phase dendrites were formed, and these dendrites functioned as nucleation sites for the η-Zn phase, making it impossible to ensure the orientation of the η-Zn phase, resulting in insufficient corrosion resistance in both acidic environments and sacrificial corrosion protection.
[0087] Comparative Example No. 35 had an insufficient amount of Mg in the plating layer, which meant that the orientation of the η-Zn phase could not be ensured, resulting in insufficient corrosion resistance in an acidic environment and insufficient sacrificial corrosion protection.
[0088] In the comparative example No. 36, the amount of Mg in the plating layer was excessive. 2 The phase became excessive, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0089] In Comparative Example No. 37, the cooling gas flux was excessive during cooling in the range of bath temperature to 320° C. Therefore, in No. 37, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0090] In Comparative Example No. 38, the cooling gas flux was insufficient during cooling in the range of 320° C. to 260° C. As a result, in No. 38, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0091] In Comparative Example No. 39, the cooling rate was low in the cooling bath temperature range of 320° C. As a result, the orientation of the η-Zn phase could not be ensured in No. 39, and the corrosion resistance in an acidic environment was insufficient.
[0092] In Comparative Example No. 40, the cooling rate was excessive in the range of 320° C. to 260° C. Therefore, in No. 40, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0093] In Comparative Example No. 41, the temperature of the steel sheet when immersed in the coating bath was above (bath temperature - 20) ° C. Therefore, in No. 41, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0094] In Comparative Example No. 46, the cooling rate was excessive in the range of 320° C. to 260° C. Therefore, in No. 46, the orientation of the η-Zn phase could not be ensured, and the corrosion resistance in an acidic environment was insufficient.
[0095] In Comparative Example No. 49, the difference between the entry temperature of the plate and the bath temperature was over 40° C., which resulted in poor plating appearance.
[0096]
[0097]
[0098]
[0099] The plated steel material of the present disclosure has excellent sacrificial corrosion resistance and corrosion resistance in acidic environments, and therefore has high industrial applicability.
[0100] 1...plated steel material, 11...steel material, 12...plated layer
Claims
1. A steel material and a plating layer on the steel material, the plating layer having a chemical composition, in mass%, containing Al: 6.0-30.0%, Mg: 3.0-15.0%, Fe: 0.01-15.00%, Si: 0-2.0%, and Ca: 0-2.00%, Sb: 0-0.50%, Pb: 0-0.50%, Cu: 0-1.00%, Sn: 0-1.00%, Ti: 0-1.00%, Cr: 0-1.00%, Nb: 0-1.00%, Z r: 0-1.00%, Ni: 0-1.000%, Mn: 0-1.00%, Mo: 0-1.00%, Ag: 0-1.00%, Li: 0-1.00%, La: 0-1.000%, C A plated steel material containing one or more elements selected from the group consisting of e: 0-1.000%, B: 0-0.500%, Y: 0-0.50%, P: 0-0.50%, Sr: 0-0.50%, Co: 0-0.500%, Bi: 0-0.500%, In: 0-0.50%, V: 0-0.500%, and W: 0-0.50%, with the total of these elements being 0-5.0%, and the balance being Zn and impurities, wherein the diffraction intensity obtained from an X-ray diffraction measurement of the plated layer satisfies the following formula (1): 0.5≦I(002) Zn / {I(100) Zn +I(101) Zn }≦25.0 (1) where I(002) in formula (1) Zn is the diffraction intensity of (002) of the η-Zn phase, and I(100) Zn is the diffraction intensity of (100) of the η-Zn phase, and I(101) Zn is the diffraction intensity of (101) of the η-Zn phase.
2. The plated steel material according to claim 1, wherein the Al and Mg content of the plated layer is, respectively, Al: 10.0 to 25.0% and Mg: 4.5 to 15.0%.
3. A plated steel material according to claim 1 or 2, wherein the Al and Mg content of the plated layer is, respectively, Al: 15.0 to 22.0% and Mg: 5.5 to 15.0%.
4. The plated steel material according to any one of claims 1 to 3, wherein the diffraction intensity obtained from the X-ray diffraction measurement of the plated layer satisfies the following formula (2): 1.5≦I(002) Zn / {I(100) Zn +I(101) Zn }≦25.0 ... (2) 5. The surface structure of the plating layer when viewed in plan is [α / MgZn 2 The plated steel material according to any one of claims 1 to 4, wherein an area ratio of the eutectic structure is 5 to 70%.
6. The surface structure of the plating layer when viewed in plan is [α / MgZn 2 The plated steel material according to any one of claims 1 to 5, wherein an area ratio of the eutectic structure is 10 to 70%.
7. The Sn content of the plating layer is, by mass%, Sn: 0.05 to 0.50%, and the X-ray diffraction measurement of the plating layer shows that Mg 2 The plated steel material according to claim 1 , wherein a Sn phase is detected.
8. The plated steel material according to any one of claims 1 to 7, containing one or both of La and Ce in a total amount of 0.005 to 0.500%.
Citation Information
Patent Citations
Hot-dip metal coated steel sheet
JP2021085086A
Noble metal recovery method
JP2023064064A
Zn-Al-Mg HOT-DIP COATED STEEL SHEET AND PROCESS FOR PRODUCTION THEREOF
WO2011001662A1
Method for manufacturing aluminum-zinc alloy plated steel sheet
JP2001164350A
Hot dip zn-al-mg-si plated steel excellent in surface property and its production method
JP2001355053A