Rectangular wire and production method for same

The extrusion molding method for forming fluorine-containing copolymer coatings on rectangular wires addresses productivity and smoothness issues, ensuring adherence and preventing peeling during deformation, thus enhancing the manufacturing process and performance of rectangular wires.

WO2024214814A1PCT designated stage expired Publication Date: 2024-10-17AGC INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014830
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing methods for manufacturing rectangular wires with insulating coatings face challenges such as low productivity, poor surface smoothness, and poor followability of the coating during bending deformation, leading to peeling issues when using powder coating methods.

Method used

A method involving extrusion molding to form a fluorine-containing copolymer-based insulating coating directly on a rectangular conductor, with specific properties including a melt flow rate, thickness uniformity, and the presence of hydroxyl groups, ensuring the coating adheres well and does not peel during bending tests.

Benefits of technology

The solution results in a rectangular wire with high productivity, excellent surface smoothness, and improved followability of the insulating coating during bending deformation, preventing peeling and maintaining insulation integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention pertains to a rectangular wire comprising a rectangular conductor and an insulating coating film that is formed via extrusion molding and that directly covers the rectangular conductor along the entirety of peripheral direction, wherein: the melt flow rate of the insulating coating at a temperature of 372°C is 13-300 g / 10 minutes; the average thickness of the insulating coating film is 10-1000 µm; the unbiased standard deviation of the thickness of the insulating coating film in the axial direction of the rectangular wire is less than 0.06 mm; the insulating coating contains a fluorine-containing copolymer that has units based on tetrafluoroethylene and units based on perfluoroalkyl vinyl ether; and in a winding test performed on the rectangular wire in accordance with "5.1.2 Rectangular Wire of JIS 3216-3: 2011", the insulating coating film does not peel from the rectangular conductor.
Need to check novelty before this filing date? Find Prior Art

Description

Rectangular wire and its manufacturing method The present invention relates to a rectangular wire and a manufacturing method thereof. This application claims priority based on Japanese Patent Application No. 2023-064887, filed on April 12, 2023, the contents of which are incorporated herein by reference. There is a demand for smaller and lighter vehicle equipment and the like used in automobiles, railways, aircraft, and the like. Therefore, there is a demand for thinner coatings of insulating covering materials for insulated electric wires of electrical equipment used in the vehicle equipment. Furthermore, with the trend toward higher output and higher voltage of electrical equipment, the insulating covering materials are required to have not only excellent insulation properties but also strong adhesion to conductors. By using rectangular conductors for electric wires, the space factor is higher when coiled compared to round wires. As a result, it is possible to save space for the entire coil, which contributes to the miniaturization of electrical equipment. However, with rectangular conductors, it is more difficult to form a uniform insulating coating compared to round wires, and there is a problem that insulation cannot be maintained sufficiently. Patent Document 1 discloses a method for manufacturing a rectangular wire, in which a powder having an average particle diameter of 0.02 μm or more and 150 μm or less, which contains a melt-formable fluororesin having a melting point of 100° C. or more and 325° C. or less and which has at least one functional group selected from the group consisting of a carbonyl group-containing group, a hydroxyl group, an epoxy group, and an isocyanate group, is applied to the rectangular conductor, thereby forming an insulating coating layer having a thickness of 10 to 150 μm on the outer periphery of the rectangular conductor. JP 2017-204410 A However, the manufacturing method described in Patent Document 1 requires a powder preparation step and a firing step after the powder coating, which results in low productivity. In addition, the surface smoothness of the coating of the insulating coating material is low because the powder is coated. Furthermore, the coating of the insulating coating material has low conformity to the rectangular conductor, which results in wrinkles in the coating of the insulating coating material and peeling off from the rectangular conductor when the rectangular wire is bent. The present invention aims to provide a rectangular wire which is highly productive and has excellent surface smoothness of the insulating coating material and excellent conformity of the insulating coating material to the rectangular conductor during bending deformation, and a method for producing the same. The present invention has the following aspects. [1] A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and an insulating coating film formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the insulating coating has a melt flow rate of 13 to 300 g / 10 min at 372°C, the insulating coating film has an average thickness of 10 to 1000 μm, and the unbiased standard deviation of the thickness of the insulating coating film in the axial direction of the rectangular wire is less than 0.06 mm, the insulating coating material contains a fluorine-containing copolymer having a unit based on tetrafluoroethylene and a unit based on perfluoroalkyl vinyl ether, and the insulating coating film does not peel off from the rectangular conductor in a winding test in accordance with "JIS3216-3:2011 5.1.2 Flat wire". [2] The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 The rectangular wire according to [1] above. [3] The fluorine-containing copolymer is —CH 2 The -CH 2 The content of OH groups is 1×10 6 The rectangular wire according to [1] or [2], wherein the number of the first and second wires is more than 30. [4] The flexural modulus FM of a test piece having a thickness of 4 mm when the fluorocopolymer is molded into the test piece B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The rectangular wire according to any one of [1] to [3], wherein the linear modulus is 1.2 or more. [5] The rectangular wire according to any one of [1] to [4], wherein the insulating coating material has a partial discharge inception voltage of 800 Vrms or more. [6] A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, the method comprising: melting a fluorine-containing copolymer using an extruder equipped with a die; and extruding the molten fluorine-containing copolymer from the die around the rectangular conductor to coat the rectangular conductor with the molten fluorine-containing copolymer to form the insulating coating material; the insulating coating material has a melt flow rate of 13 to 300 g / 10 min at 372° C., an average thickness of the coating of the insulating coating material is 10 to 1000 μm, and an unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm; the fluorine-containing copolymer has units based on tetrafluoroethylene and units based on perfluoroalkyl vinyl ether; and the rectangular wire is formed in accordance with 5.1.2 of JIS3216-3:2011. A manufacturing method of a rectangular wire in which the coating of the insulating coating material does not peel off from the rectangular conductor in a winding test conforming to the "Rectangular Wire" standard. [7] The method for producing a rectangular wire according to [6], wherein the drawdown ratio DDR calculated by the following formula 1 is 0.5 or more and less than 10.0. DDR = (D A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of ​​the die (mm 2 ) and C A is the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 ). [8] The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 The method for producing a rectangular wire according to [6] or [7] above. [9] The fluorine-containing copolymer is —CH 2 The -CH 2 The content of OH groups is 1×10 6The method for manufacturing a rectangular wire according to any one of [6] to [8], wherein the number of the rectangular wires is more than 30 per one.

[10] The flexural modulus FM of a test piece having a thickness of 4 mm when the fluorocopolymer is molded into the test piece B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The method for producing a rectangular wire according to any one of [6] to [9], wherein is 1.2 or more.

[11] The method for manufacturing a rectangular wire according to any one of [6] to

[10] , wherein the insulating coating material has a partial discharge inception voltage of 800 Vrms or more. [1A] A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the melt flow rate of the insulating coating material at 372°C is 13 to 300 g / 10 min, 15 to 200 g / 10 min, 18 to 150 g / 10 min, or 20 to 60 g / 10 min, the average thickness of the coating of the insulating coating material is 10 to 1000 μm, 20 to 500 μm, or 50 to 200 μm, and the rectangular wire A rectangular wire, wherein the unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the wire is less than 0.06 mm, 0.03 mm or less, 0.01 mm or less, 0.001 mm or more but less than 0.06 mm, 0.001 to 0.03 mm, or 0.001 to 0.01 mm, the insulating coating material contains a fluorine-containing copolymer having a unit based on tetrafluoroethylene and a unit based on perfluoroalkyl vinyl ether, and the coating of the insulating coating material does not peel off from the rectangular conductor in a winding test in accordance with "JIS3216-3:2011, 5.1.2, Flat wire." [2A] The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 More than 3.0 mm 2 Above 2.6 to 15 mm 2 , or 3.0 to 15 mm 2 The rectangular wire according to [1A], [3A] The fluorine-containing copolymer is —CH 2 The -CH 2The content of OH groups is 1×10 6 The flat wire according to [1A] or [2A], wherein the number of the flat wires is more than 30, 100 or more, 150 or more, more than 30 to 5000, 100 to 2000, or 150 to 1000 per square inch. [4A] The flexural modulus FM of the test piece having a thickness of 4 mm when the fluorocopolymer is molded into the test piece B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The flat wire according to any one of [1A] to [3A], wherein is 1.2 or more, 1.5 or more, 1.9 or more, 1.2 to 10, 1.5 to 5, or 1.9 to 3. [5A] The rectangular wire according to any one of [1A] to [4A], wherein the insulating coating material has a partial discharge inception voltage of 800 Vrms or more, 1000 Vrms or more, 1100 Vrms or more, 800 to 3000 Vrms, 1000 to 2500 Vrms, or 1100 to 2000 Vrms. [6A] A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, the method comprising: melting a fluorine-containing copolymer using an extruder equipped with a die; and extruding the molten fluorine-containing copolymer from the die around the rectangular conductor to coat the rectangular conductor with the molten fluorine-containing copolymer to form the insulating coating material; and the insulating coating has an average thickness of 10 to 1000 μm, 20 to 500 μm, or 50 to 200 μm; the unbiased standard deviation of the thickness of the insulating coating in the axial direction of the rectangular wire is less than 0.06 mm, 0.03 mm or less, 0.01 mm or less, 0.001 mm or more but less than 0.06 mm, 0.001 to 0.03 mm, or 0.001 to 0.01 mm; the fluorine-containing copolymer has units based on tetrafluoroethylene and units based on perfluoroalkyl vinyl ether; and the rectangular wire is not subjected to a winding test in accordance with "JIS 3216-3: 2011, 5.1.2, rectangular wire", in which the coating of the insulating coating does not peel off from the rectangular conductor. [7A] The method for producing a rectangular wire according to [6A], wherein the drawdown ratio DDR calculated by the following formula 1 is 0.1 or more and less than 10.0, 0.5 or more and less than 10.0, 0.5 to 5, or 0.8 to 1.5. DDR = (D A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of ​​the die (mm 2 ) and C A is the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 ). [8A] The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 More than 3.0 mm2 Above 2.6 to 15 mm 2 , or 3.0 to 15 mm 2 The method for producing a rectangular wire according to [6A] or [7A], [9A] The fluorine-containing copolymer is —CH 2 The -CH 2 The content of OH groups is 1×10 6 The method for producing a rectangular wire according to any one of [6A] to [8A], wherein the number of the rectangular wires is more than 30, 100 or more, 150 or more, more than 30 to 5000, 100 to 2000, or 150 to 1000 per square inch. [10A] The flexural modulus FM of the test piece when the fluorocopolymer is molded into a test piece having a thickness of 4 mm. B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The method for producing a rectangular wire according to any one of [6A] to [9A], wherein is 1.2 or more, 1.5 or more, 1.9 or more, 1.2 to 10, 1.5 to 5, or 1.9 to 3. [11A] The method for producing a rectangular wire according to any one of [6A] to [10A], wherein the partial discharge inception voltage of the insulating coating material is 800 Vrms or more, 1000 Vrms or more, 1100 Vrms or more, 800 to 3000 Vrms, 1000 to 2500 Vrms, or 1100 to 2000 Vrms. According to the present invention, it is possible to provide a rectangular wire which is highly productive and has excellent surface smoothness of the insulating coating material and excellent conformity of the insulating coating material to the rectangular conductor during bending deformation, as well as a manufacturing method thereof. The melt flow rate is the melt mass flow rate defined in JIS K 7210-1:2014 (corresponding international standard ISO 1133-1:2011). Hereinafter, the melt flow rate is also referred to as MFR. The measurement conditions for MFR are a temperature of 372°C and a load of 49N. The average thickness of the insulating coating is determined by taking a 5 m length of rectangular wire, measuring the thickness of the insulating coating on the long side of a rectangular cross section perpendicular to the axial direction every 100 mm, and taking the arithmetic average. The unbiased standard deviation of the thickness of the insulating coating material in the axial direction of a rectangular wire is determined by taking a 5 m length of rectangular wire, measuring the thickness of the insulating coating material on the long sides of the rectangular cross section perpendicular to the axial direction every 100 mm, and using the measured values. The shear stress of the insulating coating material is a value measured using a known formula (for example, JIS K 7199:1999) according to the die provided in the device used for extrusion molding. In this specification, it is a value measured using a capillary die. Specifically, it is a value measured by the method described in paragraphs

[0073] to

[0075] and

[0079] to

[0081] of JP2015-086364A. -CH in fluorine-containing copolymer 2 The content of OH groups can be determined by infrared spectroscopy. Specifically, it can be determined by the method described in the Examples. The melting point of the fluorocopolymer can be determined as the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The flexural modulus and partial discharge inception voltage can be determined by the method described in the Examples. The unit of a polymer means a portion (polymerization unit) derived from a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by processing the polymer. In this specification, a unit based on a monomer is also referred to as a monomer unit. <Rectangular wire> The wire comprises a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and an insulating coating formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor. In a winding test conforming to "JIS3216-3:2011 5.1.2 Rectangular Wire", the insulating coating does not peel off from the rectangular conductor. If the insulating coating does not peel off from the rectangular conductor in the winding test, the surface smoothness of the insulating coating and the ability of the insulating coating to follow the rectangular conductor during bending deformation are improved. <Rectangular conductor> The rectangular conductor is a core wire of a rectangular wire, and is a conductor whose cross section perpendicular to the axial direction is rectangular. The material of the rectangular conductor may be any known material for the core of an electric wire, such as copper, tin, silver, gold, aluminum, alloys thereof, etc. Among these, copper is preferred from the viewpoint of ease of forming the rectangular conductor. The thickness of the rectangular conductor is, for example, 0.5 mm to 3.0 mm. The width of the rectangular conductor is, for example, 1.0 mm to 5.0 mm. The thickness of a rectangular conductor is the short side of its rectangular cross section perpendicular to the axial direction. The width of a rectangular conductor is the long side of its rectangular cross section perpendicular to the axial direction. The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 More than 3.0 mm is preferable. 2 The upper limit of the cross-sectional area of ​​the rectangular conductor is not particularly limited, but is, for example, 15 mm 2 The cross-sectional area of ​​the rectangular conductor is 2.6 to 15 mm 2 is preferable, and 3.0 to 15 mm 2 is more preferred. The cross-sectional area of ​​a rectangular conductor is the area of ​​the cross section perpendicular to the axial direction. If the insulating coating film has poor conformity to the rectangular conductor during bending deformation, the larger the cross-sectional area of ​​the rectangular conductor, the more likely it is that the insulating coating film will wrinkle or peel off from the rectangular conductor during bending deformation of the rectangular wire. The rectangular wire of this embodiment has excellent conformity of the insulating coating film to the rectangular conductor during bending deformation, so the larger the cross-sectional area of ​​the rectangular conductor, the more useful it is. <Insulating coating film> The average thickness of the coating of the insulating coating material is 10 to 1000 μm, preferably 20 to 500 μm, and more preferably 50 to 200 μm. When the average thickness of the coating is equal to or greater than the lower limit, the coating has excellent tracking resistance. When the average thickness of the coating is equal to or less than the upper limit, the overall thickness of the rectangular wire can be made thin, and when the wire is coiled, the overall coil space can be saved, which contributes to the miniaturization of electrical equipment. The unbiased standard deviation of the thickness of the insulating coating material in the axial direction of the rectangular wire (hereinafter, simply referred to as "thickness variation") is less than 0.06 mm, preferably 0.03 mm or less, and more preferably 0.01 mm or less. When the thickness variation of the coating is less than (or equal to) the upper limit, the crack resistance and tracking resistance during bending deformation are excellent. The smaller the variation in thickness of the coating, the more preferable, and it may be 0. From the viewpoints of ease of manufacture and yield, the variation in thickness of the coating is preferably 0.001 mm or more. The lower limit and the upper limit can be appropriately combined. Examples of the combinations include 0.001 mm or more and less than 0.06 mm, 0.001 to 0.03 mm, and 0.001 to 0.01 mm, when the thickness variation of the coating is not 0. In order to keep the thickness variation to less than 0.06 mm, it is preferable to form the insulating coating film by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor. Other methods, such as powder coating, are not preferable because they tend to cause large thickness variations. In particular, when forming the insulating coating film by powder coating using fluorine-containing resin, the viscosity adjustment during melting is difficult, and therefore the thickness variation is likely to be large, compared to non-fluorine resins such as acrylic resin, epoxy resin, epoxy-acrylic resin, polyurethane resin, polyester resin, polyimide resin, polyamideimide resin, and polyesterimide resin. The MFR of the insulating coating material at 372° C. is from 13 to 300 g / 10 min, preferably from 15 to 200 g / 10 min, more preferably from 18 to 150 g / 10 min, and even more preferably from 20 to 60 g / 10 min. When the MFR of the insulating coating material at 372°C is equal to or higher than the lower limit, the surface smoothness of the coating of the insulating coating material and the ability of the coating of the insulating coating material to conform to the rectangular conductor during bending deformation are improved.When the MFR of the insulating coating material at 372°C is equal to or lower than the upper limit, the strength of the coating of the insulating coating material is increased. The shear stress of the insulating coating material is preferably 0.1 to 400 kPa, more preferably 1 to 300 kPa, and even more preferably 5 to 200 kPa. When the shear stress of the insulating coating material is equal to or greater than the lower limit, the thickness uniformity of the coating of the insulating coating material is improved. When the shear stress of the insulating coating material is equal to or less than the upper limit, the adhesion to the conductor is improved. The partial discharge inception voltage of the insulating coating material is preferably 800 Vrms or more, more preferably 1000 Vrms or more, and even more preferably 1100 Vrms or more. The upper limit of the partial discharge inception voltage of the insulating coating material is not particularly limited, and may be, for example, 3000 Vrms or less, 2500 Vrms or less, or 2000 Vrms or less. The partial discharge inception voltage of the insulating coating material is preferably 800 to 3000 Vrms, more preferably 1000 to 2500 Vrms, and even more preferably 1100 to 2000 Vrms. If there is a minute gap-like defect in the insulating coating material, an electric field concentrates at that part, causing a weak discharge. This discharge is called partial discharge. If the partial discharge inception voltage is equal to or higher than the lower limit, it means that there are few defects. If the partial discharge inception voltage of the insulating coating material is equal to or higher than the lower limit, the adhesiveness of the insulating coating material to the rectangular conductor is improved. As a result, the ability of the insulating coating material to conform to the rectangular conductor during bending deformation is improved. The insulating coating material contains a fluorine-containing copolymer having units based on tetrafluoroethylene (hereinafter also referred to as "TFE") and units based on perfluoroalkyl vinyl ether (hereinafter also referred to as "PAVE"). The insulating coating material may further contain components other than the fluorine-containing copolymer, so long as the properties of the insulating coating material are not significantly impaired. The content of the fluorine-containing copolymer relative to the total mass of the insulating coating material is preferably 50 mass % or more, more preferably 70 mass % or more, and may be 100 mass %. (Fluorine-containing copolymer) The fluorine-containing copolymer has TFE units and PAVE units. The fluorine-containing copolymer may be a fluorine-containing copolymer consisting of only TFE units and PAVE units, or may be a fluorine-containing copolymer having TFE units, PAVE units and other units. As an example of PAVE, CF 2 =CFOR f1 (However, R f1 is a perfluoroalkyl group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms. Specific examples of PAVE include CF 2 = CFOCF 2 CF 3 , C.F. 2 = CFOCF 2 CF 2 CF 3 (hereinafter, also referred to as "PPVE"), CF 2 = CFOCF 2 CF 2 CF 2 CF 3 , C.F. 2 = CFO (CF 2 ) 6 Examples include F. The PAVE is preferably PPVE. Examples of other units include units u1 based on a fluorine-containing monomer other than the TFE unit and the PAVE unit, and units u2 based on a monomer having a functional group (excluding monomers having fluorine). As the fluorine-containing monomer of the unit u1, a fluorine-containing compound having one polymerizable carbon-carbon double bond is preferable. For example, a fluoroolefin (e.g., vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoropropylene (hereinafter also referred to as "HFP"), chlorotrifluoroethylene, hexafluoroisobutylene, etc., except for TFE), CF 2 =CFOR f2 SO 2 X 1 (However, R f2 is a perfluoroalkylene group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms, 1 is a halogen atom or a hydroxyl group.), CF 2 =CFOR f3 CO 2 X 2 (However, R f3is a perfluoroalkylene group having 1 to 10 carbon atoms which may contain an oxygen atom between the carbon atoms, 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; CF 2 = CF (CF 2 ) p OCF = CF 2 (wherein p is 1 or 2), fluoroalkylethylene (hereinafter also referred to as "FAE"), fluorine-containing monomers having a ring structure (for example, perfluoro(2,2-dimethyl-1,3-dioxole), 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, perfluoro(2-methylene-4-methyl-1,3-dioxolane), etc.). The fluorine-containing monomers may be used alone or in combination of two or more kinds. As the fluorine-containing monomer of the unit u1, at least one selected from the group consisting of HFP and FAE is preferable in terms of excellent moldability of the fluorine-containing copolymer, and HFP is more preferable in terms of excellent electrical properties (dielectric constant, dielectric tangent) and heat resistance. As the FAE, for example, CH 2 = C.X. 3 (CF 2 ) q X 4 (However, X 3 is a hydrogen atom or a fluorine atom, q is an integer of 2 to 10, and X 4 is a hydrogen atom or a fluorine atom. Specific examples of FAE include CH 2 = CF (CF 2 ) 2 F, C.H. 2 = CF (CF 2 ) 3 F, C.H. 2 = CF (CF 2 ) 4 F, C.H. 2 = CF (CF 2 ) 5 F, C.H. 2 = CF (CF 2 ) 6 F, C.H. 2 = CF (CF 2 ) 2 H, C.H.2 = CF (CF 2 ) 3 H, C.H. 2 = CF (CF 2 ) 4 H, C.H. 2 = CF (CF 2 ) 5 H, C.H. 2 = CF (CF 2 ) 6 H, C.H. 2 =CH(CF 2 ) 2 F, C.H. 2 =CH(CF 2 ) 3 F, C.H. 2 =CH(CF 2 ) 4 F, C.H. 2 =CH(CF 2 ) 5 F, C.H. 2 =CH(CF 2 ) 6 F, C.H. 2 =CH(CF 2 ) 2 H, C.H. 2 =CH(CF 2 ) 3 H, C.H. 2 =CH(CF 2 ) 4 H, C.H. 2 =CH(CF 2 ) 5 H, C.H. 2 =CH(CF 2 ) 6 Examples include H. As FAE, CH 2 =CH(CF 2 ) q1 X 4 (wherein q1 is 2 to 6, preferably 2 to 4), and CH 2 =CH(CF 2 ) 2 F, C.H. 2 =CH(CF 2 ) 3 F, C.H. 2 =CH(CF 2 ) 4 F, C.H. 2 = CF (CF 2) 3 H, C.H. 2 = CF (CF 2 ) 4 H is more preferred, CH 2 =CH(CF 2 ) 4 F, C.H. 2 =CH(CF 2 ) 2 F is particularly preferred. Examples of monomers having a functional group of unit u2 include monomers having a carboxy group (e.g., maleic acid, itaconic acid, citraconic acid, undecylenic acid, etc.); monomers having an acid anhydride group (e.g., itaconic anhydride (hereinafter also referred to as "IAH"), citraconic anhydride (hereinafter also referred to as "CAH"), 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"), maleic anhydride, etc.), monomers having a hydroxyl group and an epoxy group (e.g., hydroxybutyl vinyl ether, glycidyl vinyl ether, etc.). The monomers having a functional group may be used alone or in combination of two or more kinds. As the monomer having a functional group of unit u2, a monomer having an acid anhydride group is preferred, and one or more selected from the group consisting of IAH, CAH and NAH are preferred, IAH or NAH are more preferred, and NAH is even more preferred. By using one or more selected from the group consisting of IAH, CAH and NAH, a fluorine-containing copolymer having an acid anhydride group can be easily produced without using a special polymerization method (see JP-A-11-193312) which is required when maleic anhydride is used. The preferred contents and ratios of each unit in the fluorine-containing copolymer are as follows. The content of TFE units relative to the total amount of constituent units of the fluorine-containing copolymer is preferably from 90.0 to 99.9 mol %, more preferably from 95.0 to 99.5 mol %, and even more preferably from 96 to 99.0 mol %. When the fluorine-containing copolymer contains at least one of the units u1 and the units u2, the content of the TFE units relative to the total amount of the constituent units of the fluorine-containing copolymer is preferably from 79 to 99.85 mol%, more preferably from 89.5 to 99.4 mol%, and even more preferably from 90.5 to 98.9 mol%. The content of PAVE units relative to the total amount of constituent units of the fluorine-containing copolymer is preferably from 0.1 to 10.0 mol %, more preferably from 0.5 to 5.0 mol %, and even more preferably from 1.0 to 4.0 mol %. When the fluorine-containing copolymer contains at least one of the units u1 and the units u2, the content of the PAVE units relative to the total amount of the constituent units of the fluorine-containing copolymer is preferably from 0.1 to 10.0 mol%, more preferably from 0.5 to 5.0 mol%, and even more preferably from 1.0 to 4.0 mol%. The total content of TFE units and PAVE units based on the total amount of constituent units of the fluorine-containing copolymer is preferably from 80 to 100 mol %, more preferably from 85 to 100 mol %, and even more preferably from 90 to 100 mol %. In the fluorine-containing copolymer, the molar ratio of PAVE units / TFE units is preferably from 0.1 / 99.9 to 10.0 / 90.0, more preferably from 0.5 / 99.5 to 5.0 / 95.0, and even more preferably from 1.0 / 99.0 to 4.0 / 96.0. When the fluorine-containing copolymer contains units u1, the content of units u1 relative to the total amount of constituent units of the fluorine-containing copolymer is preferably from 0.5 to 15 mol %, more preferably from 1 to 10 mol %. When the fluorine-containing copolymer contains the unit u2, the content of the unit u2 relative to the total amount of the constituent units of the fluorine-containing copolymer is preferably from 0.05 to 1 mol %, more preferably from 0.1 to 0.5 mol %. When the content and ratio of each unit are within the above range, the surface smoothness of the coating of the insulating coating material in the obtained rectangular wire and the ability of the coating of the insulating coating material to conform to the rectangular conductor during bending deformation are improved. The proportion of each unit can be calculated by melt NMR analysis, fluorine content analysis, infrared absorption spectrum analysis, etc. of the fluorocopolymer. The fluorine-containing copolymer may contain units based on a dicarboxylic acid (itaconic acid, citraconic acid, 5-norbornene-2,3-dicarboxylic acid, maleic acid, etc.) corresponding to the acid anhydride group-containing cyclic hydrocarbon monomer as a result of hydrolysis of a part of the acid anhydride group in the unit u2. When the unit based on the dicarboxylic acid is contained, the unit is referred to as unit u2. Preferred specific examples of the fluorine-containing copolymer include a TFE / PAVE copolymer and a TFE / PAVE / NAH copolymer. The MFR of the fluorine-containing copolymer at 372° C. is preferably from 13 to 300 g / 10 min, more preferably from 15 to 200 g / 10 min, further preferably from 18 to 150 g / 10 min, particularly preferably from 18 to 80 g / 10 min. The fluorine-containing copolymer is -CH 2 It is preferable that the alkyl group has an OH group. 2 The content of OH groups is 1×10 6 Preferably, the number is more than 30, more preferably 100 or more, and even more preferably 150 or more. 2 The upper limit of the content of OH groups is not particularly limited, but may be, for example, 5,000 or less, 2,000 or less, or 1,000 or less. 2 The content of OH groups is 1×10 6 The number of particles is preferably more than 30 and not more than 5,000, more preferably 100 to 2,000, and even more preferably 150 to 1,000. Fluorine-containing copolymer -CH 2 When the content of OH groups is equal to or more than the lower limit, -CH 2 The OH groups bond with atoms on the surface of the rectangular conductor, increasing the adhesion of the insulating coating material to the rectangular conductor, which in turn increases the ability of the insulating coating material to conform to the rectangular conductor during bending deformation. Fluorine-containing copolymer -CH 2 The OH group is, for example, a -CH group derived from a chain transfer agent or a polymerization initiator used in producing the fluorine-containing copolymer. 2 For example, alcohol is used as a chain transfer agent, or -CH 2 When a peroxide having an OH group is used, the main chain terminal of the copolymer is provided with -CH 2 An OH group is introduced. Also, -CH 2 By polymerizing a monomer having an OH group, -CH 2 An OH group is introduced into the side chain terminal of the fluorine-containing copolymer. In addition, -CH 2By fluorinating a fluorine-containing copolymer having an OH group, -CH 2 The amount of OH groups can be reduced. In addition, the amount of -CH 2 The amount of OH groups can be controlled. The melting point of the fluorine-containing copolymer is preferably from 260 to 350°C, more preferably from 280 to 340°C, and even more preferably from 290 to 330°C. The flexural modulus FM of a test piece having a thickness of 4 mm when the fluorocopolymer is molded B (MPa) vs. the flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A (MPa) A / FM B is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 1.9 or more. A / FM B The upper limit of is not particularly limited, but may be, for example, 10 or less, 5 or less, or 3 or less. A / FM B is preferably from 1.2 to 10, more preferably from 1.5 to 5, and even more preferably from 1.9 to 3. F.M. A / FM B When the insulating coating material has a thickness of 100 mm or more, the insulating coating material can adhere to the rectangular conductor more closely, and the insulating coating material can conform to the rectangular conductor more closely during bending deformation. F.M. B is preferably 200 to 900 MPa, more preferably 300 to 800 MPa, and further preferably 400 to 700 MPa. F.M. A is preferably 710 to 3000 MPa, more preferably 750 to 2500 MPa, and even more preferably 900 to 2000 MPa. The fluorine-containing copolymer may be one produced by a known production method, or a commercially available one. Examples of known production methods include those described in WO 2015 / 182702, WO 2016 / 006644, and WO 2016 / 017801. <Other Ingredients> Examples of other components include fluorine-containing polymers other than the fluorine-containing copolymer having TFE units and PAVE units, fluorine-free polymers, fillers, pigments, and other additives. Specific examples of the filler include resins and inorganic fillers. Examples of the resin include fibrous resins such as aramid fibers and liquid crystal polyester fibers, and examples of powdered resins include powdered resins such as polytetrafluoroethylene. Examples of the inorganic filler include fibrous fillers such as glass fibers, carbon fibers, boron fibers, and stainless steel microfibers; and powdered fillers such as talc, mica, graphite, molybdenum disulfide, calcium carbonate, silica, silica alumina, alumina, and titanium dioxide. Other examples include hydrotalcites and metal oxides, such as zinc oxide, magnesium oxide, titanium oxide, lead oxide, and copper oxide. Metal powders can also be used, such as powders of stainless steel, iron-based materials, titanium, copper, and nickel. The fillers may be used alone or in combination of two or more. Examples of the pigment include color pigments such as organic pigments and inorganic pigments. Specific examples include carbon black (black pigment), iron oxide (red pigment), aluminum cobalt oxide (blue pigment), copper phthalocyanine (blue pigment, green pigment), perylene (red pigment), and bismuth vanadate (yellow pigment). The other components may be used alone or in combination of two or more. <Method of manufacturing rectangular wire> The rectangular wire can be manufactured by melting a fluorocopolymer using an extruder equipped with a die, and extruding the molten fluorocopolymer from the die around a rectangular conductor to coat the rectangular conductor with the molten fluorocopolymer, thereby forming the insulating coating material. In addition to the fluorocopolymer, the other components may be added to the extruder. Examples of the extruder include a twin-screw extruder and a single-screw extruder, with the twin-screw extruder being preferred. The open face of the die is rectangular in shape. The cylinder temperature and die temperature of the extruder are set according to the type of fluorocopolymer. The cylinder temperature of the extruder is preferably 50 to 450°C, more preferably 80 to 440°C, and even more preferably 90 to 430°C. The die temperature is preferably 100 to 420°C, more preferably 120 to 400°C, and even more preferably 150 to 380°C. When the cylinder temperature and die temperature of the extruder are equal to or higher than the lower limit, the compatibility of the materials by kneading is improved. When the cylinder temperature and die temperature of the extruder are equal to or lower than the upper limit, deterioration of the fluorocopolymer due to heat is easily suppressed. The residence time in the extruder is preferably from 10 seconds to 30 minutes. The screw rotation speed of the extruder is preferably 0.5 to 100 rpm. It is preferable to preheat the rectangular conductor. The temperature of the preheated rectangular conductor is preferably 50 to 400° C., more preferably 80 to 250° C. The preheating method is not particularly limited, but examples include light heating, hot air heating, radiation heating, gas burner heating, and induction heating. (Drawdown ratio) In the manufacturing method of the rectangular wire of this embodiment, the drawdown ratio (hereinafter also referred to as "DDR") calculated by the following formula 1 is preferably 0.1 or more and less than 10.0, more preferably 0.5 or more and less than 10.0, even more preferably 0.5 to 5, and particularly preferably 0.8 to 1.5. When the DDR is equal to or greater than the lower limit, a rectangular wire having excellent surface smoothness of the insulating coating film is easily obtained.When the DDR is less than (or equal to) the upper limit, a rectangular wire having excellent surface smoothness of the insulating coating film and excellent conformity of the insulating coating film to the rectangular conductor during bending deformation is easily obtained. DDR = (D A -C A ) / (F A -C A ) Formula 1 In the above formula 1, D A is the opening area of ​​the die (mm 2 ) and C A is the cross-sectional area (mm 2) and F A is the cross-sectional area (mm 2 ). D A can be calculated from the following formula 2. D A =D L xD S Formula 2 In the above formula 2, D L is the inner dimension (mm) of the long side of the rectangular opening of the die, and D S is the inner dimension (mm) of the short side of the rectangular opening surface of the die. C A can be calculated from the following formula 3. C A = C L ×C S Formula 3 In the above formula 3, C L is the long side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular conductor, and C S is the short side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular conductor. F A can be calculated from the following formula 4. F A = F L ×F S Formula 4 In the above formula 4, F L is the long side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular wire, and F S is the short side (mm) of the rectangular cross section perpendicular to the axial direction of the rectangular wire. In this embodiment, it is preferable to adopt a so-called pressure molding method in which the insulating coating material is formed under pressure. By adopting the pressure molding method, the DDR is more likely to be less than the upper limit value (or less) than the conventional tube molding method, and as a result, it is easier to obtain a rectangular wire having excellent surface smoothness of the insulating coating material film and excellent conformity of the insulating coating material film to the rectangular conductor during bending deformation. (Application) The rectangular wire of the present invention can be suitably used for, for example, insulating amplifiers, insulating transformers, automobile alternators, hybrid cars, electric ships, electric aircraft, electric vertical take-off and landing aircraft motors, etc. It can also be used as various electric wires (wrapping electric wires, electric wires for automobiles, electric wires for robots) and coil windings (magnet wires). The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, Examples 1 and 3 are examples, and Examples 2, 4, 5 and 6 are comparative examples. <Evaluation method> (MFR of Fluorine-Containing Copolymer and Insulating Coating Material) The fluorocopolymer pellets or insulating coating material were preheated for 5 minutes, and then the MFR at 49 N was measured in accordance with JIS K 7210-1: 2014. The measurement was carried out at 372°C. In Table 1, this is represented as MFR. (shear stress of insulating coating material) Measurement was performed in accordance with JIS K 7199:1999. Specifically, the measurement was performed by the method described in paragraphs

[0073] to

[0075] and

[0079] to

[0081] of JP 2015-086364 A (using a capillary die). The insulating coating was separated from the rectangular conductor of the rectangular wire to prepare a measurement sample. The shear rate was 122 sec -1 The measurement temperature was 350°C. (Flexural Modulus of Fluorine-Containing Copolymer) The fluorocopolymer pellets were pre-dried for 3 hours under heating at 200° C. Then, the resin composition was injection molded using an injection molding machine (ROBOSHOT α-50, manufactured by Fanuc Corporation) under conditions of cylinder temperature: 380° C. and mold temperature: 170° C. to obtain an injection molded article having a thickness of 4 mm. The test piece was heated in an air atmosphere at 275° C. for 96 hours to obtain a post-heating injection molded article. The injection molded article and the heated injection molded article were cut into a length of 80 mm and a width of 10 mm to obtain test pieces and heated test pieces, respectively. The test pieces and heated test pieces were subjected to bending modulus measurement using TENSILON (manufactured by A&D Co., Ltd., RTF-1350) in accordance with JIS K7171 (corresponding international standard ISO 527-1:2012) with a load cell rating of 10 kN, a support distance of 64 mm, and a speed of 2 mm / min. In Table 1, the bending modulus of the test pieces is shown as FM B After heating, the flexural modulus of the test piece was measured as F A It is written as follows. (Fluorine-containing copolymer -CH 2 OH group amount) The pellets of the fluorocopolymer were molded by cold pressing to prepare a film having a thickness of 0.25 to 0.30 mm. This film was scanned 40 times by a Fourier transform infrared spectrometer (FT-IR (Spectrum One, manufactured by PerkinElmer)) and analyzed to obtain an infrared absorption spectrum 1. 2 The same procedure was carried out for pellets of a fluorine-containing copolymer having no OH group (however, the thickness of the film was the same), and infrared absorption spectrum 2 was obtained. Infrared absorption spectrum 2 was subtracted from infrared absorption spectrum 1 to obtain a difference spectrum. -1 From the peak (absorbance) of 6 -CH for each 2 The OH group content was calculated. -1 The peak is -CH 2 C, a model compound with an OH group 7 H 15 CH 2 This is a peak confirmed for -OH. 2 The molar absorption coefficient of the OH group is 104 (absorbance / cm / mol). 2 The amount of OH groups is -CH 2 The denominator of the unit [unit] is 1×10, which is the number of carbon atoms in the main chain of the fluorine-containing copolymer. 6 However, the numbers are omitted in Table 1. N=I×A×t Formula 5 In the above formula 5, I is absorbance, A is a correction coefficient, and -CH 2 2236 for OH groups, and t is the thickness of the film (mm). (Partial discharge inception voltage of insulating coating material) The insulating coating film was cut out from the rectangular conductor of the rectangular wire and press molded (350°C, preheating for 5 minutes, pressurization for 2 minutes) to obtain a measurement sample of 130 mm x 130 mm x 0.12 mm thick. Using the obtained measurement sample, the partial discharge inception voltage of the insulating coating material was measured under the following measurement conditions (low frequency method). The voltage when a discharge charge of 10 pC was detected was obtained as the partial discharge inception voltage. The measurement was performed on five measurement samples, and the average of these was taken as the partial discharge inception voltage. In Table 1, the partial discharge inception voltage is represented as PDIV. [Measurement conditions] Measuring device: Partial Discharge Detector A-006, manufactured by Fujikura Dia Cable Co., Ltd. Electrodes: Electrodes conforming to JIS C 2110-1 are used. Test voltage: Set to a maximum of 20 kVrms (50 Hz), and reduced after detecting a discharge charge of 100 pC. Voltage rise / fall speed: 100V / sec. Other conditions: in the atmosphere, temperature: 18 degrees, relative humidity: 30%. (Average thickness and thickness variation of the coating) A 5 m length of rectangular wire was taken, and the thickness of the insulating coating material on the long side of the rectangular cross section perpendicular to the axial direction was measured every 100 mm (only on the side in contact with the upper inner surface of the die during molding). The arithmetic mean of the measured values ​​(mm) was taken as the average thickness. The unbiased standard deviation of the measured values ​​(mm) was taken as the thickness variation. (Wrapping test) The rectangular wire was evaluated by a winding test in accordance with "JIS 3216-3: 2011, 5.1.2, rectangular wire." The cross section of the rectangular wire was visually inspected and evaluated according to the following criteria. In Table 1, this is referred to as the winding test. A: The insulating coating film did not peel off from the rectangular conductor. B: The insulating coating film peeled off from the rectangular conductor. (Following ability) The rectangular wire was bent edgewise and flatwise at an angle of 90±10°. The surface of the insulating coating film at the bent portion and the cross section of the rectangular wire were then visually observed, and the conformability was evaluated according to the following criteria. A: When the wire was bent, no wrinkles were formed on the surface of the film of the insulating coating material, and no peeling of the film of the insulating coating material from the rectangular conductor occurred. B: When the wire was bent, wrinkles were generated on the surface of the film of the insulating coating material, or the film of the insulating coating material peeled off from the rectangular conductor. (Surface smoothness) The surface roughness (Ra) of the rectangular wire was measured using a digital microscope (HRX-1, manufactured by Hirox Co., Ltd.) at a magnification of 80 and a measurement length of 4 mm. A: Surface roughness is 45 μm or less B: Surface roughness exceeds 45 μm (Materials used) Fluorine-containing copolymer 1: A fluorine-containing copolymer having a molar ratio of TFE units:PPVE units=98.0:2.0 (melting point: 310° C.) Fluorine-containing copolymer 2: A fluorine-containing copolymer having a molar ratio of TFE units:PPVE units:NAH units=97.9:2.0:0.1 (melting point: 300° C., specific gravity: 2.13) Fluorine-containing copolymer 3: A fluorine-containing copolymer having a molar ratio of TFE units:PPVE units=98.0:2.0 (melting point: 312° C.) In addition, the fluorine-containing copolymer 3 has a main chain carbon number of 1×10 6 -CH for each 2 This is a fluorine-containing copolymer having zero OH group content. (Example 1) A rectangular wire was produced by wire extrusion molding under the following conditions using the fluorocopolymer 1. The DDR was set to 1. In the wire extrusion molding, a so-called pressure molding method was adopted in which the insulating coating material is formed under pressure. Die temperature: 400°C. Cylinder temperature: 280-380°C. Flat conductor: Flat copper wire, thickness 1.5 mm x width 2.3 mm. Preheating temperature of rectangular conductor: 180°C. Coating thickness (set value): 0.18 mm. (Example 2) A rectangular wire was produced in the same manner as in Example 1, except that the DDR was set to 15. However, in the electric wire extrusion molding, a so-called tube molding method was adopted in which the insulating coating material was formed substantially under normal pressure. (Example 3) A rectangular wire was produced by wire extrusion molding under the following conditions using fluorocopolymer 2. The DDR was set to 1. In the wire extrusion molding, a so-called pressure molding method was adopted in which the insulating coating material is formed under pressure. Die temperature: 390°C. Cylinder temperature: 280-390°C. Flat conductor: Flat copper wire, thickness 1.5 mm x width 2.3 mm. Preheating temperature of rectangular conductor: 180°C. Coating thickness (set value): 0.18 mm. (Example 4) A rectangular wire was produced in the same manner as in Example 3, except that the DDR was set to 15. However, in the electric wire extrusion molding, a so-called tube molding method was adopted in which the insulating coating material was formed substantially under normal pressure. (Example 5) A rectangular wire was produced by wire extrusion molding under the following conditions using the fluorocopolymer 3. The DDR was set to 1. In the wire extrusion molding, a so-called pressure molding method was adopted in which the insulating coating material is formed under pressure. Die temperature: 380°C. Cylinder temperature: 280-380°C. Flat conductor: Flat copper wire, thickness 1.5 mm x width 2.3 mm. Preheating temperature of rectangular conductor: 180°C. Coating thickness (set value): 0.18 mm. (Example 6) A rectangular wire was produced in the same manner as in Example 5, except that the DDR was set to 15. However, in the electric wire extrusion molding, a so-called tube molding method was adopted in which the insulating coating material was formed substantially under normal pressure. The insulating coating material and rectangular wire of each example were subjected to the above-mentioned evaluations. The results are shown in Table 1. Examples 1 and 3 were excellent in surface smoothness of the coating of the insulating coating material and in conformity of the coating of the insulating coating material to the rectangular conductor during bending deformation. On the other hand, in Examples 2, 4, and 6 in which the DDR was 15, the surface smoothness of the coating of the insulating coating material and the ability of the coating of the insulating coating material to conform to the rectangular conductor during bending deformation were poor. In Example 5, in which the MFR of the insulating coating material at 372°C was less than 13 g / 10 min, even when the DDR was 1, the surface smoothness of the insulating coating film and the ability of the insulating coating film to conform to the rectangular conductor during bending deformation were poor.

Claims

1. A rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and an insulating coating film formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, wherein the insulating coating has a melt flow rate of 13 to 300 g / 10 min at 372°C, the insulating coating film has an average thickness of 10 to 1000 μm, and the unbiased standard deviation of the thickness of the insulating coating film in the axial direction of the rectangular wire is less than 0.06 mm, the insulating coating material contains a fluorine-containing copolymer having units based on tetrafluoroethylene and units based on perfluoroalkyl vinyl ether, and the insulating coating film does not peel off from the rectangular conductor in a winding test in accordance with "JIS 3216-3: 2011, 5.1.2, Flat Wire." 2. The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 The rectangular wire according to claim 1 .

3. The fluorine-containing copolymer is —CH 2 It has an OH group, and the -CH 2 The content of OH groups is 1×10 6 The rectangular wire according to claim 1 or 2, wherein the number of the first and second wires is more than 30.

4. The flexural modulus FM of the test piece when the fluorocopolymer is molded into a test piece having a thickness of 4 mm B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The rectangular wire according to claim 1 or 2, wherein the linear modulus is 1.2 or more.

5. The rectangular wire according to claim 1 or 2, wherein the partial discharge inception voltage of the insulating coating material is 800 Vrms or more.

6. A method for producing a rectangular wire comprising a rectangular conductor having a rectangular cross section perpendicular to the axial direction, and a coating of an insulating coating material formed by extrusion molding that directly covers the entire circumferential direction of the rectangular conductor, the method comprising: melting a fluorine-containing copolymer using an extruder equipped with a die, and extruding the molten fluorine-containing copolymer from the die around the rectangular conductor to coat the rectangular conductor with the molten fluorine-containing copolymer to form the insulating coating material; the insulating coating material has a melt flow rate of 13 to 300 g / 10 min at 372°C, an average thickness of the coating of the insulating coating material is 10 to 1000 μm, and an unbiased standard deviation of the thickness of the coating of the insulating coating material in the axial direction of the rectangular wire is less than 0.06 mm; the fluorine-containing copolymer has units based on tetrafluoroethylene and units based on perfluoroalkyl vinyl ether; and the rectangular wire is formed in accordance with JIS 3216-3:2011 5.1.

2. A manufacturing method of a rectangular wire in which the coating of the insulating coating material does not peel off from the rectangular conductor in a winding test conforming to the "Rectangular Wire" standard.

7. The method for producing a rectangular wire according to claim 6, wherein the drawdown ratio DDR calculated by the following formula 1 is 0.5 or more and less than 10.

0. A -C A ) / (F A -C A In the above formula 1, D A is the opening area of ​​the die (mm 2 ) and C A is the cross-sectional area (mm 2 ) and F A is the cross-sectional area (mm 2 ).

8. The cross-sectional area of ​​the rectangular conductor is 2.6 mm 2 The method for producing a rectangular wire according to claim 6 or 7, wherein 9. The fluorine-containing copolymer is —CH 2 It has an OH group, and the -CH 2 The content of OH groups is 1×10 6 The method for producing a rectangular wire according to claim 6 or 7, wherein the number of the wires is more than 30.

10. The flexural modulus (FM) of the test piece having a thickness of 4 mm when the fluorocopolymer is molded B The flexural modulus FM of the test piece after heating the test piece at 275° C. for 96 hours A The ratio of FM A / FM B The method for producing a rectangular wire according to claim 6 or 7, wherein the ratio of the linear modulus to the linear modulus is 1.2 or more.

11. The method for manufacturing a rectangular wire according to claim 6 or 7, wherein the partial discharge inception voltage of the insulating coating material is 800 Vrms or more.

Citation Information

Patent Citations

  • Fluororesin and coated electric wire

    WO2005052015A1

  • Insulated wire and method for producing same

    WO2016031675A1

  • Magnet wire and coil

    WO2020218205A1