Matte decorative sheet and manufacturing method thereof

The three-step photocuring process for the matte decor sheet forms a micro-folding structure on the hard coating layer, overcoming the challenges of conventional methods by achieving a uniform, low-gloss, and stain-resistant finish without matting agents, ensuring minimal angle-dependent brightness and gloss variations.

WO2024214897A1PCT designated stage expired Publication Date: 2024-10-17TORAY ADVANCED MATERIALS KOREA INC

Patent Information

Application Number
PCT/KR2023/017734
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-11-07
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional methods for manufacturing matte decorative sheets for furniture face challenges in achieving a low-gloss, uniform appearance and stain resistance due to the use of matting agents, which result in surface roughness and contamination issues, as well as significant differences in brightness and gloss when viewed from different angles.

Method used

A matte decor sheet is created using a three-step photocuring process that forms a micro-folding structure on a hard coating layer without matting agents, comprising a color sheet layer, skin layers, and a hard coating layer made from specific polyethylene terephthalate and acrylate oligomers, with a photoinitiator, and applied using various coating methods and UV curing wavelengths to achieve a smooth, matte finish.

Benefits of technology

The solution results in a matte finish with minimal color and gloss differences across angles, enhanced stain resistance, and a soft texture, addressing the issues of surface roughness and contamination resistance associated with traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023017734_17102024_PF_FP_ABST
    Figure KR2023017734_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A matte decorative sheet according to one embodiment of the present invention comprises a colored sheet layer, a first skin layer positioned on one surface of the colored sheet layer, a second skin layer positioned on the other surface of the colored sheet layer, and a hard coating layer positioned on the first skin layer, and exhibits small difference or change in color or gloss, caused by changes in angle, and a matte or low-gloss decorative sheet is implemented, without using a quencher, through a micro-folding structure so as to solve a contamination resistance problem caused by use of a quencher, and thus has an anti-fingerprint effect and can implement a soft texture.
Need to check novelty before this filing date? Find Prior Art

Description

Matte decorative sheet and manufacturing method thereof

[0001] The present invention relates to a matte decorative sheet for furniture and a method for manufacturing the same, and more specifically, to a matte decorative sheet and a method for manufacturing the same, which enables low gloss compared to conventional general UV curing products by applying a three-step photocuring process, thereby significantly reducing color change and gloss change depending on the angle.

[0002] Traditionally, decorative sheets have been widely used to decorate and protect the surfaces of products such as home appliances, electronic products, architecture, furniture, and automobiles. These decorative sheets are classified into glossy and matte sheets depending on the shape of the surface. Generally, to implement a matte surface in decorative sheets, a phenomenon of light scattering on the surface must occur after the coating composition is cured, so a method of including particles or additives that can increase surface roughness in the material composition is used. In particular, matting agents have been mainly used in the past to implement a low gloss or matte finish. However, the large particle size of matting agents results in a high surface roughness, giving the surface a rough feel, and the porous nature of matting agents reduces the stain resistance of the decorative sheets.

[0003] In addition, for furniture decorative sheets, which are one type of decorative sheets, the conventional furniture decorative sheet process has been using a method of curing a solvent-free or solvent-type hard coating liquid using UV or heat curing. However, it is difficult to secure the appearance by directly coating the hard coating liquid on the decorative sheet fabric. To solve this difficulty in securing the appearance, a method of coating using a transfer method using a pre-manufactured decorative sheet or decorative film is being used. However, the transfer method coating can only implement a limited gloss, so there are restrictions on its use.

[0004] In addition, it is difficult to achieve low matte finish using the conventional matte decorative sheet manufacturing method for furniture, and there is a problem that brightness (L value) and glossiness differ significantly depending on the angle (viewing angle).

[0005] The present invention has been devised to solve the above problems and to meet the needs of the prior art, and the problem to be solved by the present invention is to solve the appearance problem and the contamination resistance problem due to the use of a matting agent in the prior matte decorative sheet manufacturing method for furniture, and at the same time provide a matte decorative sheet and a manufacturing method thereof with a small difference in brightness and gloss depending on the angle.

[0006] The above and other objects and advantages of the present invention will become apparent from the following description of preferred embodiments.

[0007] The above object is achieved by a matte decorative sheet including a color sheet layer, a first skin layer located on one side of the color sheet layer, a second skin layer located on the other side of the color sheet layer, and a hard coating layer located on the first skin layer.

[0008] Preferably, the matte decorative sheet may have a difference in L* value of less than 60 within a range of -15° to +110° from the black standard of the Lab color coordinates.

[0009] Preferably, the matte decorative sheet may have a gloss difference of less than 15 within a range of 20° to 85°.

[0010] Preferably, the hard coating layer may have an arithmetic mean roughness (Ra) of 0.5 to 15 µm, a 10-point average roughness (Rz) of 5 to 10 µm, and a maximum roughness (Rt) of 6 to 15 µm.

[0011] Preferably, the color sheet layer may comprise amorphous polyethylene terephthalate (PET-A).

[0012] Preferably, the first skin layer and the second skin layer may comprise glycol modified polyethylene terephthalate (PET-G).

[0013] Preferably, the first skin layer or the second skin layer may include 10 to 25 parts by weight of glycol-modified polyethylene terephthalate per 100 parts by weight of amorphous polyethylene terephthalate included in the color sheet layer.

[0014] Preferably, the hard coating composition forming the hard coating layer includes a monofunctional acrylate monomer, a difunctional acrylate monomer, a trifunctional urethane acrylate oligomer, and a hexafunctional urethane acrylate oligomer, and may further include a trifunctional acrylate monomer.

[0015] Preferably, the hard coating composition forming the hard coating layer may include 10 to 40 parts by weight of a monofunctional acrylate monomer, 10 to 40 parts by weight of a difunctional acrylate monomer, 10 to 40 parts by weight of a trifunctional urethane acrylate oligomer, and 10 to 40 parts by weight of a hexafunctional urethane acrylate oligomer, based on 100 parts by weight of the total.

[0016] Preferably, the hard coating layer may further include a photoinitiator.

[0017] Preferably, the thickness of the hard coating layer may be 5 to 20 μm, the thickness of the first skin layer and the second skin layer may be 15 to 60 μm, and the thickness of the color sheet layer may be 150 to 600 μm.

[0018] Preferably, the hard coating layer may have a micro-folding structure.

[0019] Preferably, the adhesion between the first skin layer and the hard coating layer may be 5B to 4B as measured according to method B of ASTM D3359.

[0020] In addition, the above object is achieved by a method for manufacturing a matte decorative sheet, which comprises a skin layer forming step of forming a first skin layer on an upper surface of a color sheet layer and a second skin layer on a lower surface, a coating step of applying a hard coating composition to the surface of the first skin layer, a first curing step of pre-gelling by curing the applied hard coating composition in a wavelength range of 400 to 450 nm, a second curing step of curing the first-cured hard coating composition in a wavelength range of 150 to 180 nm, and a third curing step of curing the second-cured hard coating composition in a wavelength range of 300 to 400 nm to form a hard coating layer.

[0021] Preferably, in the coating step, the hard coating composition may be coated by any one method selected from gravure, micro gravure, slot die, lip die, and comma coater.

[0022] Preferably, the first curing step may be performed with a gallium lamp or an LED lamp.

[0023] Preferably, the secondary curing step may be performed using an excimer lamp under nitrogen purging conditions.

[0024] Preferably, the third curing step may be performed using any one selected from a UV lamp, a mercury lamp, and a metal halide lamp.

[0025] According to the matte decorative sheet and the method for manufacturing the same according to the present invention, the color and gloss difference or change according to the angle change is very small, and a matte or low-gloss decorative sheet is implemented through a micro-folding structure without using a matting agent, thereby solving the appearance problem and contamination resistance problem due to the use of a matting agent, and not only has an anti-fingerprint effect, but also has a technical effect such as being able to implement a soft texture.

[0026] However, the effects of the present invention are not limited to the effects mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the description below.

[0027] Figure 1 is a configuration diagram of a matte decorative sheet according to one embodiment of the present invention.

[0028] Figure 2 is a configuration diagram of a matte decorative sheet according to another embodiment of the present invention.

[0029] Figure 3 is a flow chart showing a method for manufacturing a matte decorative sheet according to one embodiment of the present invention.

[0030] Figure 4 is a graph showing the change in L* value by angle of the matte decorative sheet according to Examples 1, 5, 7, and 9 of the present invention and Comparative Examples 1 to 3.

[0031] Hereinafter, with reference to the attached drawings, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement the present invention. The present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0032] In order to clearly explain the present invention in the drawings, parts that are not related to the description are omitted, and the same reference numerals are added to the same or similar components throughout the specification. In addition, the thickness is shown in the drawings to clearly express various layers and regions. In addition, when it is mentioned in this specification that an element is disposed "on" or "over" another element, the element may be disposed directly on the other element, or there may be elements interposed between the elements. On the other hand, when it is mentioned that an element is disposed "directly on" or "directly above" another element, there may not be interposed elements.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In the event of a conflict, the present specification, including its definitions, will govern. Furthermore, although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein.

[0034] In this specification, the terms "~-based resin", "~-based polymer", or / and "~-based copolymer" are broad concepts encompassing all of "~ resin", "~ polymer", "~ copolymer", or / and "derivatives of ~ resin, polymer, or copolymer." In addition, in this specification, the term "polymer or copolymer crosslinked with these resins" means "polymer or copolymer crosslinked with the aforementioned resin."

[0035] In this specification, “compound” is a broad concept that includes “monatomic molecules,” “oligomers,” and “polymer compounds including homopolymers and copolymers.”

[0036] The term "including" in this specification means that other components may be included rather than excluding other components unless specifically stated to the contrary.

[0037] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.

[0038] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one" or "one or more" preceding elements herein may supplement the entire list of elements and do not imply that they supplement individual elements described above.

[0039] Unless otherwise stated herein, all percentages, parts, ratios, etc. are by weight. Additionally, whenever an amount, concentration, or other value or parameter is given as a range, a preferred range, or a list of upper preferred values ​​and lower preferred values, this should be understood to specifically disclose all ranges formed from any pair of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether ranges are separately disclosed.

[0040] When a range of numerical values ​​is mentioned in this specification, unless otherwise stated, the range is intended to include the endpoints and all integers and fractions within the range. The scope of the present invention is not intended to be limited to the specific values ​​mentioned when defining the range. Each element in this specification is a concept that includes both the singular and plural.

[0041] Figure 1 is a configuration diagram of a matte decorative sheet according to one embodiment of the present invention.

[0042] Referring to FIG. 1, a matte decorative sheet according to one embodiment of the present invention includes a color sheet layer (110), a first skin layer (120) positioned on one surface of the color sheet layer (100), a second skin layer (130) positioned on the other surface of the color sheet layer (110), and a hard coating layer (140) positioned on the first skin layer (120).

[0043] In one embodiment, the color sheet layer (110) is located at the center of the matte decorative sheet and preferably includes amorphous polyethylene terephthalate (PET-A). By forming the color sheet layer (110) with polyethylene terephthalate (PET-A), the crystallinity can be lowered through the amorphous polymer structure, and excellent thermal stability and transparency can be achieved, thereby improving flexibility and formability of the decorative sheet.

[0044] Additionally, the color sheet layer (110) may further include a color master batch to impart color.

[0045] In one embodiment, the first skin layer (120) and the second skin layer (130) are positioned on each of both sides of the color sheet layer (110), and preferably include glycol-modified polyethylene terephthalate (PET-G). The glycol-modified polyethylene terephthalate (PET-G) resin included in the glycol-modified polyethylene terephthalate (PET-G) is an amorphous resin copolymerized with terephthalic acid (TPA), ethylene glycol (EG), and cyclohexanedimethanol (CHDM). Such glycol-modified polyethylene terephthalate (PET-G) has excellent processability, moldability, and printability, is not deformed due to shrinkage, has excellent impact resistance, and does not generate chlorine gas when incinerated or in a fire, so it has the characteristics of being free of harmful substances such as environmental hormones, and is therefore suitable as a material included in the matte decorative sheet according to the present invention.

[0046] In addition, it is preferable that the first skin layer (120) or the second skin layer (130) include 10 to 25 parts by weight of glycol-modified polyethylene terephthalate with respect to 100 parts by weight of amorphous polyethylene terephthalate included in the color sheet layer (110).

[0047] In one embodiment, the hard coating layer (140) is formed by applying a hard coating composition on the first skin layer (120).

[0048] In addition, the hard coating composition forming the hard coating layer (140) preferably includes a monofunctional acrylate monomer, a difunctional acrylate monomer, a trifunctional urethane acrylate oligomer, and a hexafunctional urethane acrylate oligomer, and may further include a trifunctional acrylate monomer. In addition, the hard coating composition may further include a photoinitiator or other additives.

[0049] The monofunctional acrylate monomer (or monofunctional acrylate monomer) included in the hard coating composition controls the viscosity of the hard coating composition and improves the adhesion between the substrate and the hard coating layer (140). One or more types of acrylic monomers having a single functional group known in the art, such as 2-hydroxyethyl acrylate (2-HEA), 4-hydroxybutyl acrylate (4-HBA), 2-hydroxypropyl acrylate (2-HPA), 2-hydroxyethyl methacrylate (2-HEMA), and hydroxypropyl methacrylate (HPMA), may be used, but it is preferable to use 2-hydroxypropyl acrylate (2-HPA) alone, which has excellent adhesion.

[0050] In addition, it is preferable that the hard coating composition contain 10 to 40 parts by weight of a monofunctional acrylate monomer per 100 parts by weight of the total composition. If the content of the monofunctional acrylate monomer is less than 10 parts by weight, there is a concern that it may be difficult to control the viscosity of the hard coating composition or that the adhesion between the first skin layer (120) and the hard coating layer (140) may be insufficient, and if it exceeds 40 parts by weight, the content of the bifunctional or higher acrylate monomer may decrease, resulting in a decrease in reactivity.

[0051] The difunctional acrylate monomer included in the hard coating composition may be at least one monomer selected from the group consisting of 1,6-hexanediol diacrylate (HDDA), hydroxypivalic neopentylglycol diacrylate (HPNDA), dipropylene glycol diacrylate (DPGDA), and tripropylene glycol diacrylate (TPGDA). The acrylic monomer (or difunctional acrylic monomer) having two functional groups is used to control the viscosity of the coating composition and increase the reactivity, and at least one of common acrylic monomers having two functional groups known in the art, such as 1,6-hexanediol diacrylate (HDDA), hydroxypivalic neopentylglycol diacrylate (HPNDA), dipropylene glycol diacrylate (DPGDA), and tripropylene glycol diacrylate (TPGDA), may be used.

[0052] In addition, it is preferable that the hard coating composition contains 10 to 40 parts by weight of a difunctional acrylate monomer per 100 parts by weight of the total composition. If the content of the difunctional acrylate monomer is less than 10 parts by weight, there is a concern that viscosity control of the coating composition may become difficult or reactivity may become weakened, and if it exceeds 40 parts by weight, viscosity control of the coating composition may likewise become difficult and reactivity may become excessively high.

[0053] Meanwhile, the acrylic monomer described so far refers to not only acrylate but also methacrylate or derivatives in which a substituent has been introduced into acrylate or methacrylate.

[0054] The oligomer component included in the hard coating composition is a urethane acrylate oligomer, and preferably includes a trifunctional urethane acrylate oligomer and a hexafunctional urethane acrylate oligomer. In the matte decorative sheet according to one embodiment of the present invention, the hard coating composition can form a micro-folding structure such as a wave pattern upon excimer irradiation by mixing a trifunctional urethane acrylate oligomer and a hexafunctional urethane acrylate oligomer, and by adding an oxysilane compound as a surface energy control agent without using any particles and controlling the surface energy of the hard coating composition to be as close to that of the substrate as possible, a matte surface with completely removed glossy points can be implemented.

[0055] In addition, the trifunctional urethane acrylate oligomer is preferably a trifunctional urethane acrylate oligomer having three acrylates and having a weight average molecular weight of 800 to 5,000. It is preferable that such a trifunctional urethane acrylate oligomer include at least one selected from the aliphatic acrylate oligomer series. As an example, commercial products such as PU320, PU330, and PU340 can be used as such a trifunctional urethane acrylate oligomer.

[0056] It is preferable that the hard coating composition contain 10 to 40 parts by weight of a trifunctional urethane acrylate oligomer for a total of 100 parts by weight. If the content of the trifunctional urethane acrylate oligomer is less than 10 parts by weight, the area of ​​the flat portion increases compared to the microfolding pattern, which causes the gloss to become excessively high. If the content exceeds 40 parts by weight, the scratch resistance becomes deteriorated.

[0057] In addition, the hexafunctional urethane acrylate oligomer is preferably a hexafunctional urethane acrylate oligomer having six acrylates and having a weight average molecular weight of 800 to 5,000. Since such a hexafunctional urethane acrylate oligomer has excellent reactivity, it can increase the hardness of the hard coating layer (140), and also has a relatively large molecular weight, so that the mechanical properties such as durability and pencil hardness after the hard coating layer is formed are excellent. The hexafunctional urethane acrylate oligomer is preferably a weight average molecular weight of 800 to 5,000, but if the weight average molecular weight is less than 800, there is a problem that the hard coating layer is damaged, and conversely, if the weight average molecular weight exceeds 5,000, there is a problem that the hardness of the hard coating layer is weakened. Such a hexafunctional urethane acrylate oligomer preferably includes at least one selected from the aliphatic acrylate oligomer series. As an example, commercial products such as PU500, PU610, and PU620 can be used as hexafunctional urethane acrylate oligomers.

[0058] It is preferable that the hard coating composition contain 10 to 40 parts by weight of a hexafunctional urethane acrylate oligomer for a total of 100 parts by weight. If the content of the hexafunctional urethane acrylate is less than 10 parts by weight, the hard coating layer (140) may be damaged, and if it exceeds 40 parts by weight, the hardness of the hard coating layer (140) is reduced.

[0059] Additionally, a photoinitiator may be added to the hard coating composition. At this time, the photoinitiator plays a role in enabling curing of the hard coating layer (140), and it is preferable to further include 1 to 3 parts by weight per 100 parts by weight of the hard coating composition described above.

[0060] Additionally, the hard coating composition may further include an oxysilane-containing compound as an additional additive. More specifically, the hard coating composition may include an oxysilane-containing compound according to Chemical Formula 1 as an additional additive.

[0061] (Chemical formula 1)

[0062] [Correction pursuant to Rule 91, November 20, 2023]

[0063] In chemical formula 1, R1 and R2 are at least one of cross-linking groups including alkenes, alkynes, acrylates, carboxylic acids, alcohols, isocyanates, aldehydes, amines, urethane acrylates, and polyester acrylates, and n is an integer of 1 or greater.

[0064] The oxysilane-containing compound according to Chemical Formula 1 can be a multifunctional silicone-modified urethane acrylate oligomer, and commercially available products include SIU2400 (Miwon) and PN8941 (Polynetron).

[0065] According to one embodiment of the present invention, a matte decorative sheet achieves matte characteristics by performing a three-step curing process on the hard coating composition described above to form a micro-folding structure. More specifically, the hard coating layer (140) can achieve matte characteristics through a first curing step of applying the hard coating composition described above and then curing it in a wavelength range of 400 to 450 nm to pre-gel, a second curing step of curing it in a wavelength range of 150 to 180 nm, and a third curing step of curing it in a wavelength range of 300 to 400 nm. Through the hard coating layer (140) forming process as described above, a micro-folding structure is formed on the surface of the hard coating layer (140), thereby suppressing the occurrence of glossy points and creating a matte surface that can be commercialized.

[0066] The detailed configuration for forming such a hard coating layer is described in detail again in the manufacturing method of the matte decorative sheet described later.

[0067] It is preferable that the hard coating layer (140) as described above has an arithmetic mean roughness (Ra) of 0.5 to 15 µm, a 10-point average roughness (Rz) of 5 to 10 µm, and a maximum roughness (Rt) of 6 to 15 µm. In this case, if the arithmetic mean roughness (Ra) of the hard coating layer (140) is less than 0.5 µm, the 10-point average roughness (Rz) is less than 5 µm, or the maximum roughness (Rt) is less than 6 µm, there is a problem of increased glossiness, and if the arithmetic mean roughness (Ra) of the hard coating layer (140) exceeds 15 µm, the 10-point average roughness (Rz) exceeds 10 µm, or the maximum roughness (Rt) exceeds 15 µm, the surface becomes excessively rough, making it difficult to use as a decorative sheet.

[0068] In the present invention, the thickness of the hard coating layer (140) is preferably 5 to 20 μm, the thickness of the first skin layer (120) and the second skin layer (130) is preferably 15 to 60 μm, and the thickness of the color sheet layer (110) is preferably 150 to 600 μm.

[0069] According to one embodiment of the present invention, the matte decorative sheet preferably has a difference in L* value of less than 60 within a range of -15° to +110° based on the black color of the Lab color coordinates measured on the surface of the hard coating layer (140). If the difference in L* value is 60 or more, there is a problem in that the brightness differs significantly depending on the angle at which the decorative sheet is viewed.

[0070] In addition, it is preferable that the matte decorative sheet according to one embodiment of the present invention has a gloss difference of less than 15 within a range of 20 to 85°. If the gloss difference is 15 or more, there is a problem that the gloss difference is severe depending on the angle at which the decorative sheet is viewed.

[0071] Additionally, it is preferable that the adhesion between the first skin layer (120) and the hard coating layer (140) measured according to method B of ASTM D3359 is 5B to 4B.

[0072] Figure 2 is a configuration diagram of a matte decorative sheet according to another embodiment of the present invention.

[0073] Referring to FIG. 2, a matte decorative sheet according to another embodiment of the present invention includes a color sheet layer (110), a first skin layer (120) and a second skin layer (130) formed on both sides of the color sheet layer (110), a hard coating layer (140) formed on the first skin layer (120), and further includes a protective layer (150) formed on the hard coating layer (140).

[0074] The color sheet layer (110), the first skin layer (120), the second skin layer (130), and the hard coating layer (140) have the same configuration as in the above-described Fig. 1, and redundant descriptions are omitted.

[0075] The protective layer (150) formed on the hard coating layer (140) is configured to supplement the mechanical strength, scratch resistance, contamination resistance, chemical resistance, and heat resistance of the hard coating layer (140), and can be freely used as a film used for decorative sheets, flooring materials, and decorative materials, as long as it does not impair the properties and purpose of the present invention.

[0076] Figure 3 is a flow chart showing a method for manufacturing a matte decorative sheet according to one embodiment of the present invention.

[0077] Referring to FIG. 3, a method for manufacturing a matte decorative sheet according to an embodiment of the present invention includes a skin layer forming step (S301) of forming a first skin layer on an upper surface of a color sheet layer and a second skin layer on a lower surface, a coating step (S302) of applying a hard coating composition to the surface of the first skin layer, a first curing step (S303) of curing the applied hard coating composition in a wavelength range of 400 to 450 nm to pre-gel, a second curing step (S304) of curing the first-cured hard coating composition in a wavelength range of 150 to 180 nm, and a third curing step (S305) of curing the second-cured hard coating composition in a wavelength range of 300 to 400 nm to form a hard coating layer.

[0078] First, in the skin layer formation step (S301), the detailed configuration of the color sheet layer, the first skin layer, and the second skin layer follows the configuration of the detailed description for Fig. 1.

[0079] Next, in the coating step (S302), the hard coating composition described in Fig. 1 is applied to the surface of the first skin layer. At this time, the application method is not particularly limited, and application methods such as gravure, micro gravure, slot die, lip die, and comma coater can be used.

[0080] Next, in the first curing step (S303), curing is performed in a wavelength range of 400 to 450 nm using a gallium lamp or an LED lamp, thereby pregelling (partially curing) the hard coating composition applied to the surface of the color sheet layer. In this way, by first performing the first curing step (S303), which is a preliminary curing step, before the second curing step (S304), and then performing the second curing step (S304), the occurrence of a micro-folding structure on the surface of the hard coating layer can be significantly increased.

[0081] Next, in the secondary curing step (S304), curing is performed in a wavelength range of 150 to 180 nm using an excimer lamp under nitrogen purging conditions (nitrogen gas conditions). Through this secondary curing step (S304), a micro-folding structure is formed on the surface during the hard coating composition's curing process. Through the formation of this micro-folding structure, the surface roughness of the hard coating layer can be controlled without using a separate matting agent, thereby implementing a matte characteristic.

[0082] Next, in the third curing step (S305), curing is performed in a wavelength range of 300 to 400 nm using any one selected from a UV lamp, a mercury lamp, and a metal halide lamp to form a hard coating layer. At this time, the third curing step (S305) is preferably performed under oxygen gas or air conditions.

[0083] In this way, in the present invention, by forming a hard coating layer through the three-step curing process described above for the hard coating composition, a micro-folding structure is formed on the surface of the hard coating layer, thereby minimizing changes in brightness (L* value) and gloss depending on the angle.

[0084] Hereinafter, the composition and resulting effects of the present invention will be described in more detail through examples and comparative examples. However, these examples are intended to more specifically illustrate the present invention, and the scope of the present invention is not limited to these examples.

[0085] [Example]

[0086] [Example 1]

[0087] 1. Formation of coating layer

[0088] A 400 ㎛ thick skin layer was formed by melt-extruding glycol-modified polyethylene terephthalate (PET-G) on both sides of a 400 ㎛ thick sheet formed of amorphous polyethylene terephthalate (PET-A).

[0089] 2. Preparation of hard coating composition

[0090] Based on 100 parts by weight of a hard coating composition, 40 parts by weight of a trifunctional urethane acrylate oligomer (PU320, Miwon) and 10 parts by weight of a hexafunctional urethane acrylate oligomer (PU620, Miwon) are mixed, and then 21 parts by weight of a monofunctional acrylate monomer (M150, Miwon), 7 parts by weight of a monofunctional acrylate monomer (2-hydroxypropyl acrylate, 2-HPA, Miwon), 15 parts by weight of a difunctional acrylate monomer (M220, Miwon), and 7 parts by weight of a trifunctional acrylate monomer (M370, Miwon) are added to lower the viscosity, thereby manufacturing a hard coating composition. Next, based on 100 parts by weight of the hard coating composition, 1.0 parts by weight of a photoinitiator (DR-1173, Miwon), 0.5 parts by weight of a photoinitiator (TPO, Miwon), and 3 parts by weight of an oxysilane-containing compound having the structure of chemical formula 1 (SIU2400, Miwon) were added and stirred to prepare a hard coating composition.

[0091] 3. Manufacturing of decorative sheets

[0092] After applying the hard coating composition manufactured above to the surface of one skin layer, it was first cured using a gallium lamp with a wavelength of 450 nm, and then second cured by exposing to 172 nm excimer under nitrogen purging conditions at 150 mJ / cm2, and then exposed to Ag UV with a wavelength of 330 nm at 172 mJ / cm2 in an air state to form a hard coating layer having a micro-folding structure, thereby manufacturing a matte decorative sheet.

[0093] [Examples 2 and 9]

[0094] A matte decorative sheet was manufactured in the same manner as in Example 1, except that the composition and content of the hard coating composition were changed as shown in Table 1.

[0095] [Comparative example]

[0096] [Comparative Examples 1 to 3]

[0097] A matte decorative sheet was manufactured in the same manner as in Example 1, except that the composition and content of the hard coating composition were changed as shown in Table 2.

[0098] Product NameExample 1Example 2Example 3Example 4Example 5Example 6Example 7Example 8Example 93Sensitive / OligomerPU320404040404040PU3304025106Sensitive / OligomerPU62010101010101010102540Monofunctional / MonomerM1502121212-HPA777M13040 25101010102Sensitive / MonomerM2201515151025404040403Sensitive / MonomerM370777PhotoinitiatorDR-11731.00.500.50.50.51.01.01.0TPO0.50.50.50.50.50.50.50.50.50.50.5AdditiveSIU2400333333333

[0099] Product name Comparative example 1 Comparative example 2 Comparative example 3 Functional / oligomer PU3204125 PU33096 Functional / oligomer PU62094110 Monofunctional / monomer M13041442 Functional / monomer M2004661 M2209 Photoinitiator DR-11730.50.50.5 TPO0.50.50.5 Additive SIU2400333

[0100] The physical properties of the matte decorative sheets according to Examples 1 to 9 and Comparative Examples 1 to 3 were measured through the following experimental examples, and the results are shown in Tables 3 and 4 below.

[0101] [Experimental Example]

[0102] (1) Gloss measurement

[0103] The 20° gloss (gloss 20° condition), 60° gloss (gloss 60° condition), and 85° gloss (gloss 85° condition) of the decorative sheet were measured using a gloss meter according to ASTM D2457.

[0104] (2) Color difference measurement

[0105] According to ASTM E1164 standard, brightness (L*) was measured in the range of -15° to +110° from black standard using a D65 light source and CM-2500d (Minolta). As an example, Fig. 4 is a graph showing the change in L* value according to angle of matte decorative sheets according to Examples 1, 5, 7, and 9 according to the present invention and Comparative Examples 1 to 3.

[0106] (3) Surface roughness measurement

[0107] Each matte decorative sheet was analyzed using a 3D surface roughness measuring device (SE3500K31, KOSAKA) under the conditions of a 5 μm tip radius, 30 mg stylus pressure, 0.5 mm measuring length, and 0.25 mm CUTOFF value, and the arithmetic mean roughness (Ra), 10-point average roughness (Rz), and maximum roughness (Rt) were measured.

[0108] (4) Measurement of contamination resistance

[0109] Iodine, red wine, mustard, and coffee were dropped onto a matte decorative sheet, respectively, and measured according to the evaluation criteria of DIN 68861:2011, par. 1.

[0110] Experimental examplesExample 1Example 2Example 3Example 4Example 5Example 6Example 7Example 8 9 Glossiness 20° 0.10.10.11.5 0.20.10.10.20.460° 0.91.00.93.50.90.71.52.33.485° 5.84.83.51.42.72.75.47.78.5L*-15° 51.30 50.51 51.20 47.57 42.24 46.55 56.82 59.50 61.28+110° 14.32 14.91 14.84 18.84 17.22 15.04 10.87 6.46 6.23 Surface roughness Ra 1.31.31.84.22.62.51.41.21 .0Rz8.07.69.79.69.99.68.37.76.5Rt8.98.711.314.115.012.29.58.57.1Stain-resistantIodine2.011.931.990.930.891.441.281.080.83Red wine0.500.530.130.320.240.240.180.140.21Mustard1.080.700.691.330.930.590.360.190.29Coffee0.280.090.411.110.070.140.190.150.19

[0111] Experimental Preliminary Comparative Example 1 Comparative Example 2 Comparative Example 3 Glossiness 20° 1.8 1.8 1.8 60° 6.1 6.4 6.0 85° 30.8 38.1 42.1 L* -15° 72.0 977.0 073.8 8+110° 5.0 014.3 99.1 5 Surface Roughness Ra 0.4 0.3 0.2 Rz 3.3 1.7 1.1 Rt 3.7 2.1 1.9 Stain Resistance Iodine 0.8 3 0.9 6 0.8 8 Red Wine 0.2 1 0.2 4 0.1 2 Mustard 0.2 9 0.4 0.1 7 Coffee 0.1 9 0.2 9 0.2 0

[0112] As can be seen in Tables 3 and 4, the matte decorative sheets according to Examples 1 to 9 of the present invention achieve a difference in L* value of less than 60 within a range of -15° to +110° with respect to the black color of the Lab color coordinates, and a difference in gloss of less than 15 within a range of 20° to 85°, thereby confirming that the occurrence of a difference in gloss and brightness depending on the angle at which the decorative sheet is observed is very small, and confirming that it has strong stain resistance.

[0113] On the other hand, Comparative Examples 1, 2, and 3 have a problem in that the difference in L* value is 60 or more within the range of -15° to +110° based on the black color of the Lab color coordinates, and the difference in gloss is 15 or more within the range of 20 to 85°, so that the difference in gloss is severe depending on the angle at which the decorative sheet is viewed.

[0114] This difference is more clearly revealed through a graph showing the change in L* value by angle of the matte decorative sheet according to the embodiment and comparative example according to the present invention as shown in FIG. 4. For example, as shown in FIG. 4, while Examples 1, 5, 7, and 9 have relatively small differences in L* by angle in the range of -15° to +110°, Comparative Examples 1 to 3 have relatively large differences in L* by angle, resulting in a problem of a significant difference in brightness depending on the angle at which the decorative sheet is viewed.

[0115] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. Color sheet layer; A first skin layer located on one side of the above color sheet layer; A second skin layer located on the other side of the above color sheet layer; and A hard coating layer positioned on the first skin layer; Matte decorative sheet, including:

2. In paragraph 1, The above matte decorative sheet is a matte decorative sheet with a difference in L* value of less than 60 within the range of -15° to +110° based on the black color of the Lab color coordinates.

3. In paragraph 1, The above matte decorative sheet is a matte decorative sheet having a gloss difference of less than 15 within a range of 20° to 85°.

4. In paragraph 1, The above hard coating layer is a matte decorative sheet having an arithmetic mean roughness (Ra) of 0.5 to 15 ㎛, a 10-point average roughness (Rz) of 5 to 10 ㎛, and a maximum roughness (Rt) of 6 to 15 ㎛.

5. In paragraph 1, The above color sheet layer is a matte decorative sheet containing amorphous polyethylene terephthalate (PET-A).

6. In paragraph 1, A matte decorative sheet, wherein the first skin layer and the second skin layer comprise glycol-modified polyethylene terephthalate (PET-G).

7. In paragraph 1, A matte decorative sheet, wherein the first skin layer or the second skin layer comprises 10 to 25 parts by weight of glycol-modified polyethylene terephthalate relative to 100 parts by weight of amorphous polyethylene terephthalate included in the color sheet layer.

8. In paragraph 1, A matte decorative sheet, wherein the hard coating composition forming the hard coating layer comprises a monofunctional acrylate monomer, a difunctional acrylate monomer, a trifunctional urethane acrylate oligomer, and a hexafunctional urethane acrylate oligomer.

9. In paragraph 8, A matte decorative sheet, wherein the hard coating composition forming the hard coating layer comprises 10 to 40 parts by weight of a monofunctional acrylate monomer, 10 to 40 parts by weight of a difunctional acrylate monomer, 10 to 40 parts by weight of a trifunctional urethane acrylate oligomer, and 10 to 40 parts by weight of a hexafunctional urethane acrylate oligomer, based on a total of 100 parts by weight.

10. In paragraph 8, A matte decorative sheet, wherein the hard coating composition forming the hard coating layer further comprises a trifunctional acrylate monomer.

11. In paragraph 8, A matte decorative sheet wherein the hard coating layer further comprises a photoinitiator.

12. In paragraph 1, The thickness of the above hard coating layer is 5 to 20㎛, The thickness of the first skin layer and the second skin layer is 15 to 60 μm, A matte decorative sheet having a thickness of the color sheet layer of 150 to 600 μm.

13. In paragraph 1, The above hard coating layer is a matte decorative sheet having a micro-folding structure.

14. In paragraph 1, A matte decorative sheet having an adhesion between the first skin layer and the hard coating layer of 5B to 4B as measured according to method B of ASTM D3359.

15. Skin layer forming step of forming a first skin layer on the upper surface of the color sheet layer and forming a second skin layer on the lower surface; A coating step of applying a hard coating composition to the surface of the first skin layer; A first curing step of pre-gelling by curing the applied hard coating composition in a wavelength range of 400 to 450 nm; A secondary curing step of curing the first cured hard coating composition in a wavelength range of 150 to 180 nm; and A third curing step of curing the second-cured hard coating composition in a wavelength range of 300 to 400 nm to form a hard coating layer; A method for manufacturing a matte decorative sheet, comprising:

16. In paragraph 15, A method for manufacturing a matte decorative sheet, wherein in the above coating step, the hard coating composition is coated by any one method selected from gravure, micro gravure, slot die, lip die, and comma coater.

17. In paragraph 15, A method for manufacturing a matte decorative sheet, wherein the first curing step is performed using a gallium lamp or LED lamp.

18. In paragraph 15, A method for manufacturing a matte decorative sheet, wherein the above-mentioned second curing step is performed using an excimer lamp under nitrogen purging conditions.

19. In paragraph 15, A method for manufacturing a matte decorative sheet, wherein the above-mentioned third curing step is performed using any one selected from a UV lamp, a mercury lamp, and a metal halide lamp.

Citation Information

Patent Citations

  • Coating, ultra-matte finish material and preparation process of ultra-matte finish material

    CN115785796A

  • Matt coating composition, matt coating sheet and the manufacturing method of the same

    KR1020160038937A

  • Device, method and computer program for deriving response based on learning model

    KR1020210093618A

  • Resin composition, decoration sheet using same and method of manufacturing thereof

    KR102125939B1

  • Monochromatic ultraviolet hardening matte paint composition, matte sheets and method for manufacturing matte decosheet using the same

    KR102357693B1

Cited By

  • Semi-cured hardened film as well as preparation method and application thereof

    CN122071034A