Molybdenum oxide sintered body, sputtering target, and oxide thin film

By adding specific metal oxide dopants to molybdenum oxide, the sinterability and density of sputtering targets are improved, addressing the challenges of low-density targets and foreign matter generation, resulting in high-quality oxide thin films for LCD and OLED applications.

WO2024214900A1PCT designated stage expired Publication Date: 2024-10-17LT METAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/019523
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-11-30
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Molybdenum oxide-based sintered bodies are difficult to sinter and result in low-density targets, leading to poor sputtering performance and foreign matter generation, which affects the quality and reliability of oxide thin films in LCD and OLED devices.

Method used

Incorporating specific metal oxide dopants like niobium, alkaline earth metals, and zirconium in predetermined ratios into molybdenum oxide to enhance sinterability and density, allowing for pressure-free sintering and optimizing particle size for improved thin film homogeneity.

Benefits of technology

The approach results in high-density sputtering targets and oxide thin films with enhanced chemical and heat resistance, reducing foreign matter and compositional non-uniformity, suitable for use in TFT structures of LCD and OLED devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023019523_17102024_PF_FP_ABST
    Figure KR2023019523_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: an oxide sintered body comprising a molybdenum oxide as the main component; a sputtering target comprising the sintered body; and an oxide thin film formed therefrom. According to the present invention, by adding a specific metal oxide in an amount in a predetermined range to sinter-resistant molybdenum oxide and niobium oxide, it is possible to simultaneously achieve improved sinterability, high-density characteristics, and thin film uniformity, which is achieved through particle growth control, even when performing non-pressurized sintering.
Need to check novelty before this filing date? Find Prior Art

Description

Molybdenum oxide sintered body, sputtering target and oxide thin film

[0001] The present invention relates to an oxide sintered body containing molybdenum as a main component, a sputtering target including the sintered body, and an oxide thin film formed therefrom. More specifically, the present invention relates to a molybdenum oxide-based sintered body, a sputtering target, and an oxide thin film formed therefrom, in which sinterability and density characteristics are simultaneously improved by adding a specific metal oxide dopant in a predetermined content range when manufacturing a sputtering target used in a TFT structure of LCDs and OLEDs.

[0002]

[0003] Low-reflectivity conductive thin films are commonly used in flat panel displays (FPDs), touch screen panels, solar cells, light emitting diodes (LEDs), and organic light emitting diodes (OLEDs).

[0004] Indium oxide-tin oxide (In2O3-SnO2) ("ITO") is a representative material for this purpose, and ITO compositions are used to form conductive thin films with high visible light transmittance and electrical conductivity. While these ITO compositions exhibit excellent low-reflectivity performance, they are not cost-effective, and research into materials that can completely or partially replace indium oxide is ongoing.

[0005] However, the area of ​​interest in these studies is the low reflectivity of the thin film formed through the target material, and it is necessary to consider the chemical resistance and heat resistance characteristics that can increase the reliability of the thin film for long-term use.

[0006] Meanwhile, molybdenum oxide is a difficult-to-sinter material. Using molybdenum oxide ceramic materials with such low sintering densities makes it difficult to fabricate high-density (e.g., greater than 90%) targets. Furthermore, sputtering using these targets inevitably leads to the generation of foreign matter, such as back deposits and nodules, which deteriorate the properties of the thin film.

[0007] [Prior Art Literature]

[0008] [Patent Document]

[0009] (Patent Document 1) Republic of Korea Publication No. 10-2020-0069314

[0010]

[0011] The present invention has been made to solve the above-mentioned problems, and the technical task of the present invention is to provide a novel molybdenum oxide-based sintered body, which can improve sinterability and secure high density even when sintered under no pressure by adding a specific metal oxide dopant in a predetermined content range to the main raw material, difficult-to-sinter molybdenum oxide, a sputtering target including the sintered body, and an oxide thin film formed therefrom.

[0012] Other objects and advantages of the present invention can be more clearly explained by the detailed description of the invention and the claims below.

[0013]

[0014] In order to achieve the above-mentioned technical task, the present invention provides an oxide sintered body containing molybdenum (M1); niobium (M2); at least one alkaline earth metal (M3); and zirconium (M4), and including molybdenum (M1) as a main component in an amount of 60 atomic% or more based on 100 atomic% of the total of the metal components, wherein the zirconium (M4) is included in an amount of 0.1 to 7 atomic% based on 100 atomic% of the total of the metal components.

[0015] In one embodiment of the present invention, at least one alkaline earth metal (M3) and the zirconium (M4) in the oxide sintered body may be included in an atomic ratio of 1:0.03 to 0.54.

[0016] In one embodiment of the present invention, the average grain size (D50) in the oxide sintered body may be 80% or less compared to the average grain size (D50) in the oxide sintered body that does not contain zirconium.

[0017] In one embodiment of the present invention, the oxide sintered body may include a MgZrNb2O8 crystal phase.

[0018] In one embodiment of the present invention, the oxide sintered body may be a molded body manufactured by mixing molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and zirconium (M4) oxide, and then pressurelessly sintering the molded body under atmospheric pressure.

[0019] In one embodiment of the present invention, the molybdenum oxide (M1) includes at least one of MoO2 and MoO3, and may be included in an amount of 60 to 70 wt% based on the total weight of the oxide sintered body.

[0020] In one embodiment of the present invention, the molybdenum oxide (M1) and the niobium oxide (M2) are included in an amount of 85.0 wt% or more and less than 100 wt% based on 100 wt% of the oxide sintered body, and the content ratio of the molybdenum oxide (M1) and the niobium oxide (M2) may be a weight ratio of 50:50 to 90:10.

[0021] In one embodiment of the present invention, the metal oxide (M3) may include at least one selected from the group consisting of CaCO3 and MgO.

[0022] In one embodiment of the present invention, the metal oxide (M3) may be included in an amount of more than 0 wt% and less than 10 wt% based on 100 wt% of the oxide sintered body.

[0023] In one embodiment of the present invention, the oxide sintered body may further include one or more metals (M5) selected from the group consisting of Mo, Ti, Cr, W, and Cu.

[0024] In one embodiment of the present invention, the metal (M5) may be included in an amount of 3 to 50 wt% based on the total weight of the sintered body.

[0025] In one embodiment of the present invention, the average grain size (D50) of the non-pressurized sintered oxide sintered body is 5 to 30 ㎛, the difference in surface roughness (Ra) of the oxide sintered body before and after sputtering is 1.0 ㎛ or less, and the resistivity is 1×10 -2 Ωcm or less, and the relative density may be 80% or more.

[0026] The present invention also provides a sputtering target including the above-described oxide sintered body.

[0027] In addition, the present invention provides an oxide thin film formed from the aforementioned sputtering target.

[0028]

[0029] According to one embodiment of the present invention, by adding a metal oxide dopant that assists sintering properties and a metal oxide dopant that controls grain growth to a difficult-to-sinter molybdenum oxide in a predetermined content range, the sinterability of a molybdenum oxide sintered body can be improved even under no pressure, and grain size optimization and high density can be secured.

[0030] Accordingly, the molybdenum oxide-based sintered body and sputtering target according to the present invention can be usefully applied to forming electrodes or wiring used in TFT structures of LCDs and OLEDs.

[0031] The effects according to the present invention are not limited to those exemplified above, and more diverse effects are included in this specification.

[0032]

[0033] Figure 1 is a photograph showing the microstructure and average grain size of the oxide sintered bodies manufactured in Examples 1 to 4 in which zirconium oxide (M4) was added.

[0034] Figure 2 is a photograph showing the microstructure and average grain size of oxide sintered bodies manufactured in Comparative Examples 1 to 4 without adding zirconium oxide (M4).

[0035] Figure 3 is a graph showing the average particle diameter of the oxide sintered bodies sintered without pressure in Examples 1 to 4 and Comparative Examples 1 to 4.

[0036] Figure 4 is a photograph of the target appearance after sputtering using the oxide sintered body target of Example 3 and Comparative Example 1.

[0037] Figure 5 is a graph showing the change in relative density according to the sintering temperature of the oxide sintered bodies manufactured in Examples 1 to 4 and Comparative Examples 1 to 4.

[0038] Figure 6 is a graph showing the change in shrinkage ratio according to the sintering temperature of the oxide sintered bodies manufactured in Examples 1 to 4 and Comparative Examples 1 to 4.

[0039] Figure 7 is a graph showing the change in mass loss rate according to the sintering temperature of the oxide sintered bodies manufactured in Examples 1 to 4 and Comparative Examples 1 to 4.

[0040] Figure 8 is an XRD graph of the oxide sintered bodies manufactured in Example 3, Comparative Example 1, and Comparative Example 3.

[0041]

[0042] All terms (including technical and scientific terms) used in this specification may be used with meanings commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Furthermore, terms defined in commonly used dictionaries should not be interpreted ideally or excessively unless explicitly and specifically defined otherwise.

[0043] Furthermore, throughout the specification, when a part is said to "include" a component, unless otherwise specifically stated, this does not exclude other components but rather means that other components may be included. Furthermore, throughout the specification, the terms "above" or "on" include not only cases where the target part is located above or below it, but also cases where there is another part in between, and do not necessarily mean that the target part is located above it in the direction of gravity. In addition, terms such as "first" and "second" in the specification do not indicate any arbitrary order or importance, but are used to distinguish between components.

[0044] MoO2-Nb2O5 materials, conventionally used as n-type semiconductor thin films, are typically manufactured via pressure sintering. However, pressure sintering is not suitable for mass production due to the increased manufacturing process costs associated with equipment costs. Furthermore, the high-pressure manufacturing process limits the ability to increase the size of the sintered body.

[0045] In order to solve the above-mentioned problems, when MoO2-Nb2O5 materials are sintered without pressure, there is a limit to the increase in sintered density, so it is difficult to apply, and also, when the sintering temperature is increased, the amount of melting and volatilization increases, which actually causes the density to decrease. In other words, heat is required as a driving force during sintering, and while higher heat is generally advantageous in securing sinterability (densification), in the case of some raw materials, problems such as volatilization occur, which actually lowers the density.

[0046] Meanwhile, the inventors of the present invention, in Korean Patent Application No. 10-2022-0132119, have discovered that by using a small amount of an alkaline earth metal oxide dopant (M3) that assists sinterability in a difficult-to-sinter material having a basic composition of molybdenum oxide and niobium oxide, they can simultaneously secure the effects of improving sinterability and securing high density even when sintering without pressure under atmospheric conditions. While the addition of the alkaline earth metal oxide (M3) dopant ensures bonding between particles within the oxide sintered body, this also causes the particle size within the sintered body to increase. When the particle size increases in this way, the particles are formed unevenly during the sputtering process, which results in a deterioration in the quality and reliability of the final oxide thin film.

[0047] Accordingly, the present invention provides a molybdenum oxide-based sintered body and a sputtering target using the same, which are composed primarily of molybdenum oxide (M1) and niobium oxide (M2), and which are mixed with an alkaline earth metal oxide dopant (M3) that assists sinterability and zirconium oxide (M4) that optimizes particle size to improve the homogeneity of a thin film formed by sputtering, and by controlling the composition thereof, thereby obtaining a high-density target due to improved sinterability, and which can improve compositional unevenness and foreign matter generation that may occur during a sputtering process by controlling particle growth due to the addition of zirconium oxide (M4).

[0048]

[0049] High-density targets for oxide sintering and sputtering

[0050] An example of the present invention is a metal oxide sintered body for manufacturing a sputtering target having molybdenum as a main component, and more specifically, a molybdenum-based oxide sintered body used in a TFT structure of an LCD and / or OLED, and a high-density sputtering target including the same.

[0051] For example, the oxide sintered body contains molybdenum (M1); niobium (M2); at least one alkaline earth metal (M3); and zirconium (M4), and includes molybdenum (Mo) as a main component in an amount of 60 atomic% or more based on 100 atomic% of the total of the metal components, wherein the zirconium (M4) is included in a predetermined atomic ratio (e.g., 0.1 to 7 atomic%) based on 100 atomic% of the total of the metal components included in the sintered body.

[0052] 0.001 ≤ M4 / (M1+M2+M3+M4) ≤ 0.07

[0053] Here, the total of 100 atomic% of the metal components means that the sum of each metal component included in the sintered body, for example, M1+M2+M3+M4, is 100, and the atomic ratio may mean that the sum of M1+M2+M3+M4 of a specific atom is 1. If necessary, the above-mentioned atomic% and atomic ratio may further include M5 and / or inevitable impurities, in which case the above-mentioned values ​​may be partially changed.

[0054] As described above, when at least one type of alkaline earth metal (M3) and a zirconium (M4) dopant are mixed, the coarsening of the particle size in the sintered body due to the addition of the alkaline earth metal (M3) dopant can be resolved, and the particle size can be optimized to ensure the homogeneity of the thin film formed by sputtering. In addition, the sinterability of the molybdenum oxide sintered body having difficulty in sintering due to the combined use of molybdenum (M1); niobium (M2); and at least one type of alkaline earth metal (M3) can be improved, and high-density characteristics can be secured.

[0055] Below, each component is described in detail.

[0056] The oxide sintered body according to the present invention comprises molybdenum (M1) and niobium (M2) as basic compositions, and at least one alkaline earth metal (M3) that assists sintering characteristics and zirconium (M4) that controls grain growth, respectively, as additional dopant components.

[0057] For example, molybdenum (M1) and niobium (M2) included in the oxide sintered body can each satisfy the following atomic ratios.

[0058] (i) 0.85 ≤ (M1+M2) / (M1+M2+M3+M4) < 1.0; (ii) 0.5 ≤ M1 / (M1+M2) ≤ 0.9; (iii) 0.1 ≤ M2 / (M1+M2) ≤ 0.5, and more specifically, (i) 0.90 ≤ (M1+M2) / (M1+M2+M3+M4) ≤ 0.995; (ii) 0.6 ≤ M1 / (M1+M2) ≤ 0.8; (iii) 0.2 ≤ M2 / (M1+M2) ≤ 0.4.

[0059] For another specific example, the alkaline earth metal (M3) included in the oxide sintered body may be included in an amount of more than 0 atomic% and less than or equal to 15 atomic%, specifically 3.0 to 10 atomic%, and more specifically 5.5 to 7.5 atomic%, based on 100 atomic% of the total of metal components included in the oxide sintered body. Here, at least one alkaline earth metal (M3) functions as a sintering aid, and may specifically include Ca, Mg, or both. In this case, when Ca and Mg are mixed, the atomic ratio of Ca and Ma in the oxide sintered body can be adjusted to 1:4 to 6, specifically 1:4.5 to 5.5, and more specifically 1:5.

[0060] As another specific example, zirconium (M4) included in the oxide sintered body is included in an amount of 0.1 to 7 atomic% or less, specifically 0.5 to 5.0 atomic%, and more specifically 1 to 3 atomic% based on 100 atomic% of the total of metal components included in the oxide sintered body.

[0061] For another specific example, at least one alkaline earth metal (M3) and zirconium (M4) included in the oxide sintered body may be included in an atomic ratio of 1:0.03 to 0.54, and more specifically, an atomic ratio of 1:0.06 to 0.27. When the above-described atomic ratio is satisfied, sintering characteristics and high-density characteristics according to the use of the alkaline earth metal (M3) dopant can be secured, and a grain growth control effect according to the use of the zirconium (M4) dopant can be promoted.

[0062] As another specific example, niobium (M2) and zirconium (M4) included in the oxide sintered body may be included in an atomic ratio of 1:0.01 to 1.0, specifically, in an atomic ratio of 1:0.05 to 0.5, and more specifically, in an atomic ratio of 1:0.05 to 0.2.

[0063] For another specific example, the oxide sintered body may further include at least one metal (M5) selected from the group consisting of Mo, Ti, Cr, W, and Cu. Preferably, Mo may be further included. At this time, the content of the metal (M5) is not particularly limited and may be appropriately adjusted within a range that constitutes 100 atomic% of the total of the metal components included in the oxide sintered body. For example, the metal (M5) may be included in an amount of 1 to 50 atomic%, specifically 3 to 50 atomic%, based on 100 atomic% of the total of the metal components included in the oxide sintered body.

[0064] The oxide sintered body according to the present invention, which is composed of the above-described composition, not only has a finer average grain size (D50) compared to a conventional sintered body that does not contain zirconium (M4), but also has a smaller difference in surface roughness before and after sputtering of the sintered body target, so that it can have uniform surface characteristics and excellent thin film characteristics.

[0065] For example, the average grain size (D50) in the oxide sintered body may be 80% or less, specifically 60% or less, and more specifically 40 to 50%, of the average grain size (D50) in the oxide sintered body that does not contain zirconium (M4). For example, the average grain size (D50) of the oxide sintered body according to the present invention may be 5 to 30 μm, specifically 10 to 20 μm. In comparison, the average grain size (D50) of the oxide sintered body that does not contain zirconium (M4) may be 20 to 50 μm.

[0066] For another specific example, the difference in surface roughness (Ra) of the oxide sintered target before and after sputtering may be 1.0 ㎛ or less, and more specifically, 0.7 ㎛ or less. At this time, the target used for sputtering is 4 inches in size, and the process is performed using a DC power supply, and the process is performed under the conditions of Working pressure 0.61 Pa and Power density 2.5 W / ㎠. In addition, the target is consumed up to a total cumulative 8 kWh, which is based on when 40 wt% of the total target weight is consumed.

[0067] In addition, the oxide sintered body of the present invention having the aforementioned composition includes at least one crystal phase, and is distinguished from a conventional sintered body in that at least one crystal phase component essentially includes zirconium (M4).

[0068] For another specific example, the oxide sintered body is a MoO2 phase in which Nb2O5 is partially dissolved, for example, Mo 1-x Nb xIt includes O2 (wherein, x is 0 to 0.25, specifically 0.15 to 0.25) as a main crystal phase, and may include MgNb2O6, CaMo6O9, and / or MgZrNb2O8 as a secondary crystal phase. In addition, the area ratio (area ratio) of the MgZrNb2O8 crystal phase containing zirconium (M4) is not particularly limited, and may be included in an amount of, for example, 1% or more, more specifically, 3 to 10%, relative to the entire crystal phase of the sintered body.

[0069] Meanwhile, the oxide sintered body according to the present invention may include stoichiometric molybdenum oxides such as MoO2 and MoO3 based on the final product, but may also include substoichiometric molybdenum oxides, such as Mo4O 11 , Mo 17 O 47 , Mo5O 14 , Mo8O 23 , Mo9O 26 , and Mo 18 O 52 At least one or more of the above are substantially absent. Here, "substantially absent" means that an unavoidable content of 2.0 wt% or less, specifically 1.0 wt% or less, and more specifically 0.5 wt% or less may be present relative to 100 wt% of the oxide sintered body.

[0070] The oxide sintered body according to the present invention may be manufactured by mixing oxides containing each metal component (M1, M2, M3, M4), for example, molybdenum (M1) oxide; niobium (M2) oxide; alkaline earth metal (M3) containing metal oxide; and zirconium (M4) oxide according to a target composition, and then pressurelessly sintering the formed body under atmospheric pressure.

[0071] Conventionally, heat or pressure is required as a driving force when sintering an oxide sintered body. Generally, the higher the heat and pressure, the more secure the sinterability of the sintered body and the more advantageous it is for densification. However, in the case of some materials, problems such as melting and volatilization occur, which lowers the density. In the present invention, by adding an additional element (dopant), even when sintered without pressure, it is possible to secure a density (densification) of the sintered body that can be used as a sputtering target, and also to improve the homogeneity of the thin film formed by sputtering by optimizing the particle size.

[0072] Here, molybdenum oxide is the main component that constitutes the sintered body.

[0073] Molybdenum (M1) oxide is a component that has oxygen bonded to molybdenum, such as MoO2, MoO3, and MoO4. In the present invention, MoO is used as molybdenum (M1) oxide. 2, MoO3, or MoO2 and A mixture of MoO3 can be used. In this case, when using a mixture of MoO2 and MoO3 as molybdenum oxide, the mixing ratio between them is not particularly limited and can be appropriately adjusted within the typical content range known in the art. Meanwhile, since MoO3 has a melting point of approximately 800°C, it volatilizes at high temperatures of 1,000°C or higher. Accordingly, in the present invention, which performs pressureless sintering at high temperatures of 1,000°C or higher, it is preferable to use MoO2 as the molybdenum (M1) oxide.

[0074] Additionally, one of the additive components included in the oxide sintered body according to the present invention is niobium (M2) oxide.

[0075] This niobium (M2) oxide is an oxide dopant that improves chemical resistance and heat resistance properties, and the chemical resistance and heat resistance properties of molybdenum oxide can be improved by adding the metal oxide. The niobium oxide is not particularly limited as long as it is a component in which oxygen is bonded to niobium, and may be Nb2O5, for example. In the following description, the niobium oxide component is symbolized as M2.

[0076] Another of the additive components included in the oxide sintered body according to the present invention is a metal oxide containing at least one alkaline earth metal (M3).

[0077] For example, the metal oxide (M3) may include at least one of Ba, Ca, Mg, and Sr, and specifically, may include a metal oxide (M3) including at least one of Ca and Mg.

[0078] The metal oxide containing an alkaline earth metal (M3) acts as a dopant that assists the sintering of difficult-to-sinter molybdenum oxide and exhibits a density-increasing effect. By adding such a metal oxide (M3), the chemical resistance and heat resistance properties of the molybdenum oxide can be improved. The metal oxide containing an alkaline earth metal (M3) is not particularly limited as long as it is a component in which oxygen is bonded to at least one element (A) among Ca and Mg, and may include, for example, one or more selected from the group consisting of CaCO3 and MgO.

[0079] One of the additive components included in the oxide sintered body according to the present invention is zirconium (M4) oxide.

[0080] When the density of the conventional oxide sintered body is low (relative density ≥ 90%), foreign substances such as back deposits and nodules are generated in the thin film during sputtering, and the higher the density, the more advantageous it is for the sputtering process. Meanwhile, during sputtering, pull-out of each particle on the target surface occurs. At this time, the space where the particles fall out becomes empty, and the smaller the particle, the smaller the space where the particles fall out, so the curvature of the sputtered target surface is reduced. Accordingly, under the same density, the smaller the particle size constituting the oxide sintered body, the more uniform the particle deposition is possible during the sputtering process, and the effect of improving the compositional unevenness and foreign substance generation that may occur during the sputtering process can be secured.

[0081] The zirconium (M4) oxide used in the present invention controls the growth of particles constituting the oxide sintered body, thereby improving compositional inhomogeneity and foreign matter generation that may occur during the sputtering process. The zirconium (M4) oxide is not particularly limited as long as it is a component in the form of zirconium combined with oxygen, and may be, for example, ZrO2. In the following description, the zirconium oxide component is symbolized as M4.

[0082] The metal oxide sintered body comprising the above-mentioned molybdenum (M1) oxide, niobium (M2) oxide, at least one alkaline earth metal (M3)-containing metal oxide, zirconium (M4) oxide, and optionally a metal (M5) may comprise 85 wt% or more and less than 100 wt% of molybdenum (M1) oxide and niobium (M2) oxide, more than 0 wt% and less than 10 wt% of alkaline earth metal (M3)-based metal oxide, and 0.1 to 10 wt% of zirconium (M4) oxide, based on 100 wt% of the sintered body. More specifically, the metal oxide sintered body may comprise 85.0 to 99.5 wt% of molybdenum (M1) oxide and niobium (M2) oxide; 0.5 to 5.0 wt% of alkaline earth metal (M3)-based metal oxide; And it may have a composition consisting of 0.5 to 5.0 wt% of zirconium (M4) oxide.

[0083] Here, the content ratio of molybdenum oxide (M1) and niobium oxide (M2) is 50:50 to 90:10 by weight, specifically 70:30 to 90:10 by weight, and more specifically 75:25 to 90:10 by weight. In the present invention, when the ratio of molybdenum oxide is 60 wt% or more, specifically 60 to 70 wt%, of the entire metal oxide sintered body, it can have low-reflection characteristics when deposited as a thin film.

[0084] If necessary, the oxide sintered body according to the present invention may further include one or more metals (M5) selected from the group consisting of Mo, Ti, Cr, W, and Cu.

[0085] This metal (M5) is a metal dopant that assists the sintering of molybdenum oxide and exhibits a density-increasing effect. By adding the metal, the chemical resistance and heat resistance properties of molybdenum oxide can be improved. In addition, due to the high electrical conductivity of the metal, the sheet resistance of the unit film can be reduced, thereby expanding the range of use. Mo is preferred. In the following description, at least one component among Mo, Ti, Cr, W, and Cu is symbolized and represented as M5.

[0086] The metal (M5) may be included in an amount of 1.0 to 30.0 wt% based on 100 wt% of the oxide sintered body. Specifically, the content of the metal (M5) may be in the range of 3.0 to 25.0 wt%, and more specifically, 5.0 to 20.0 wt%.

[0087] The oxide sintered body according to the present invention, which is configured as described above, may have a relative density of 80% or more, and specifically 90% or more, even when sintered without pressure under atmospheric pressure. In this case, the upper limit thereof is not particularly limited. In addition, the resistivity of the oxide sintered body may be 1×10 -2 Ωcm or less, and its lower limit is not specifically limited.

[0088] And the size (D50) of the crystal grains included in the oxide sintered body is not particularly limited, and may be, for example, 1 to 30 ㎛, specifically 3 to 30 ㎛, and more specifically 5 to 30 ㎛.

[0089] In addition, when a metal oxide sintered body having the above-mentioned composition is used as a target material to form a thin film, the formed thin film has low reflection characteristics and, at the same time, heat resistance and chemical resistance are improved through optimization of the ratio and composition of molybdenum oxide. In addition, since density improvement is realized by adding a small amount of a specific dopant (M3), pressure sintering does not need to be used, and a Mo-Nb-O sputtering target, which is a difficult-to-sinter material, can be manufactured. In addition, by adding zirconium (M4) oxide, grain growth within the sintered body can be controlled within a predetermined range, thereby ensuring homogeneity and high quality of the thin film.

[0090]

[0091] <Method for manufacturing oxide sintered body and sputtering target>

[0092] Hereinafter, a method for manufacturing an oxide sintered body and a sputtering target according to one embodiment of the present invention will be described. However, the present invention is not limited to the manufacturing method described below, and each process step may be modified or selectively combined and performed as needed.

[0093] The present invention relates to the manufacture of a sputtering target, wherein raw metal or ceramic powder is heat-treated to form a single mass. For example, when manufacturing the oxide sintered body and sputtering target, the raw metal or ceramic powder is made of MoO2 and / or MoO3, Nb2O5 as a base material, and additional elements are added and mixed to form the final sputtering target.

[0094] One example of the above manufacturing method may comprise the steps of: (i) preparing and mixing raw material powders containing molybdenum (M1) oxide; niobium (M2) oxide; metal oxide containing at least one alkaline earth metal (M3); and zirconium (M4) oxide according to a target composition ('step S10'); (ii) manufacturing a molded body using the mixed raw material powders ('step S20'); and (iii) performing a pressureless heat treatment on the molded body under atmospheric pressure in an inert atmosphere at 1,200 to 1,600°C for 1 to 20 hours to manufacture a sintered body ('step S30').

[0095] Hereinafter, the above manufacturing method is explained in detail by each process step.

[0096] (i) Preparation of raw powder ('Step S10')

[0097] In the above step S10, it is a step of preparing raw material powders including molybdenum (M1) oxide, niobium (M2) oxide, metal oxides containing at least one alkaline earth metal (M3), and zirconium (M4) oxide. Specifically, molybdenum (M1) oxide, niobium (M2) oxide, at least one alkaline earth metal (M3)-based metal oxide selected from the group consisting of CaCO3 and MgO, zirconium (M4) oxide powder, and metal (M5) powder such as Mo as needed are weighed according to the target composition, and each powder is placed into a mixer, ground, and mixed to prepare a mixture.

[0098] When mixing the above-mentioned raw material powders, conventional additives known in the art, such as binders, dispersants, and antifoaming agents, may be additionally included as needed. At this time, the amount of additives used may be appropriately adjusted within a conventional range known in the art, and for example, 0.01 to 10 wt% may be used relative to the total weight of powders in the slurry (e.g., 100 wt%).

[0099] The mixing and grinding of raw material powders is not particularly limited and can be performed using a conventional ball mill, attraction mill, bead mill, etc. known in the art. For example, the mixed raw material powders can be mixed and ground using a wet bead mill using zirconia balls, and then the powder can be spheroidized (spray dryer) and then sieved to obtain the final powder.

[0100] Add pure water, antifoaming agent, plasticizer, binder, etc. in an amount approximately twice that of the raw material powder, and mix thoroughly using a mixer for approximately 2 hours.

[0101] Afterwards, 0.8 pi zirconia beads (about 2 kg) are placed in a 1 L sized vessel made of zirconia, and the raw materials mixed with pure water are added and crushed sufficiently. At this time, the bead mill speed is not particularly limited, and may be, for example, about 2000 to 4000 rpm, specifically 2500 to 3500 rpm, and more specifically about 3000±200 rpm, and the raw materials are added at a speed of 4 to 6 liters per minute, specifically 4.5 to 6.5 liters, and more specifically about 5 liters.

[0102] After sufficient crushing, a spherical powder is produced using a spray dryer. Afterwards, the good powder and scrap powder are separated using a 90 to 110 mesh screen, specifically a 100 mesh screen, as needed.

[0103] (ii) Manufacturing of molded body ('Step S20')

[0104] The above S0 step is a step of manufacturing a molded body using prepared raw material powder. More specifically, a molded body of a predetermined specification is manufactured through a process of putting raw material powder into a molding machine and molding it.

[0105] To increase the density of the molded body, the molding process may be performed at least once, or more specifically, twice. For example, the first molding process may involve feeding raw material powder into a single-screw molding machine to produce the primary molded body, while the second molding process may utilize a hydrostatic press (CIP) machine.

[0106] The conditions in the above first molding process are not particularly limited and can be appropriately adjusted within the general conditions known in the art. For example, a first molded body is manufactured using a 50Φ ultra-hard mold according to the weight of a given powder. At this time, the pressure during the first molding can be carried out at the minimum pressure required to form a shape, and specifically, it can be carried out at a level where it is maintained at about 10 Mpa for about 1 minute. Thereafter, the second molding process can be carried out using isostatic pressing (CIP) under conditions of about 200 Mpa with a holding time of several hours. At this time, since the second isostatic pressing is carried out together with an organic solvent including water, it can be carried out while being placed in an acrylic sealant (e.g., an envelope).

[0107] (iii) Manufacturing of sintered body ('S30 stage')

[0108] In the above step S30, the manufactured molded body is sintered under predetermined conditions to manufacture a sintered body.

[0109] At this time, the sintering conditions are not particularly limited and can be appropriately adjusted within the range of common conditions known in the art. For example, pressureless sintering can be performed at 1,200 to 1,600°C for 1 to 20 hours, and specifically, for 1 to 4 hours. The sintering can be performed in an oxygen atmosphere or under inert conditions.

[0110] As a specific example of the above S30 step, the prepared molded body is placed in an alumina crucible of a certain specification and sintered. In this experiment, in order to confirm the difference in properties between the molded body before heat treatment and the pressureless sintered body after heat treatment, the weight, diameter, height, etc. of the molded body and the sintered body were measured and each physical property was compared (see Table 1-2 and Figures 4 to 6 below).

[0111] The pressureless sintered body manufactured through this process may have a relative density of 80% or more, specifically 85% or more, and more specifically 90% or more. In this case, the upper limit is not particularly limited.

[0112] (iv) Sputtering target manufacturing

[0113] Next, the sintered body is removed and processed. For example, after removing the sintered body, the surface of the target can be polished by processing the upper and lower parts of the target by at least 1 mm.

[0114] Afterwards, a commercial sputtering target is manufactured through diffusion bonding and final processing commonly known in the industry.

[0115] Specifically, the oxide sintered body obtained in step S30 is bonded to a backing plate. Indium may be used as an adhesive, and a bonding rate of 95% or higher is preferably achieved. Subsequently, machining is performed using machining equipment to reach the final target thickness, and the backing plate surface is subjected to bead and / or arc spray treatment to obtain the final sputtering target.

[0116] A metal oxide target can be manufactured through the aforementioned process. The target density of the manufactured target is preferably at least 90%, and more specifically, at least 95%.

[0117]

[0118] <Oxide thin film>

[0119] Another example of the present invention is a metal oxide thin film deposited using the aforementioned molybdenum oxide target. This metal oxide thin film can be formed by performing sputtering using the aforementioned sintered body as a target material.

[0120] The above oxide film may have slight differences in composition depending on the deposition atmosphere, but since it is manufactured by sputtering the above-mentioned oxide target, its composition is substantially the same as that of the target. Accordingly, it has a density characteristic of 80% or more relative density and a density of 1×10 -2 An oxide film having excellent resistivity characteristics of Ωcm or less can be formed. In addition, by adding specific metal oxides and metals to the main raw material, molybdenum oxide, within a predetermined range, chemical resistance and heat resistance characteristics can be improved through optimization of the molybdenum oxide ratio and composition.

[0121] The metal oxide thin film according to the present invention can be formed (deposited) using a conventional sputtering method known in the art. One example of the above manufacturing method includes the step of mounting the aforementioned molybdenum oxide pressureless sintered body sputtering target, and then depositing the thin film at room temperature in an oxygen and / or argon atmosphere in a vacuum chamber. In this case, the sputtering can be performed using a DC sputter.

[0122] The substrate and sputtering device used can be any of those known in the art without limitation. Specifically, the film can be formed by supplying oxygen or oxygen and high-purity argon gas at a rate of 80 to 110 sccm (standard cubic centimeters per minute) in a vacuum chamber, and specifically, by supplying at a rate of 95 to 105 sccm, the film can be deposited at room temperature (RT) without applying temperature to the substrate on which the film is to be formed. In addition, the power density of the DC sputter is 1.0 to 2.0 W / cm. 2The thickness of the metal oxide thin film may be 300 to 500 Å, but is not particularly limited thereto.

[0123] The oxide thin film obtained as described above can be used in various ways in the manufacture of semiconductor devices, and for example, can be applied for forming wiring or electrodes in the manufacture of semiconductors. In particular, the metal oxide thin film can be used as at least one of a gate layer, a source layer, and a drain layer of a thin film transistor (TFT). When the thin film of the present invention is used as a barrier layer of the source and drain electrodes included in a thin film transistor, the contact resistance can be reduced, and the physical properties of the thin film transistor can be improved by having excellent transparency and a low refractive index.

[0124] The molybdenum oxide-based sputtering target according to the present invention described above and the oxide thin film formed therefrom have high density and excellent resistivity characteristics even under no pressure, and thus can suppress the connection resistance with the TFT structure of LCDs and OLEDs or the electron injection layer of an organic electroluminescent device to a low level. Accordingly, the oxide thin film described above can be applied without limitation to various display devices such as liquid crystal displays or organic electroluminescent display devices; information transmission devices such as flat panel displays such as LCDs, PDPs, OLEDs, and LEDs; surface light source lighting device touch panels such as OLEDs and LEDs; mobile phones, tablets, and / or information transmission devices using the same.

[0125] Hereinafter, the present invention will be described in detail through examples. However, the following examples are only illustrative of the present invention, and the present invention is not limited to the following examples.

[0126]

[0127] [Example 1-4] Preparation of MoO2-Nb2O5 and ZrO2-added sintered bodies

[0128] A molded body was manufactured by mixing molybdenum (M1) oxide, niobium (M2) oxide, alkaline earth metal (M3) oxide, zirconium (M4) oxide, and optionally metal (M5) in a ratio as shown in Table 1 below.

[0129] When manufacturing a molded body, most samples were manufactured with a diameter of 50Φ. Afterwards, the oxide sintered bodies of Examples 1 to 4 were manufactured by heat-treating at approximately 1400 to 1500°C for 2 hours in a nitrogen atmosphere using heat treatment equipment.

[0130] M1M2M3M4M5Total(wt%)MoO2Nb2O5CaCO3MgOZrO2MoExample 164.525.01.02.00.57.0100Example 264.025.01.02.01.07.0100Example 363.025.01.02.02.07.0100Example 470.025.01.02.02.0-100Comparative Example 175.025.0----100Comparative Example 268.025.0---7.0100Comparative Example 365.025.01.02.0-7.0100Comparative Example 472.025.01.02.0--100

[0131]

[0132] [Comparative Example 1-4] Manufacturing of MoO2-Nb2O5 and α-added sintered body

[0133] Except for changing the composition to be injected as shown in Table 1 above, a 50Φ molded body was manufactured in the same manner as in the above example. Thereafter, a heat treatment was performed at 1400 to 1500°C for 2 hours in a nitrogen atmosphere using a heat treatment facility to manufacture sintered bodies of Comparative Examples 1 to 4.

[0134]

[0135] [Experimental Example 1] Evaluation of the properties of the molded body

[0136] The physical properties of each molded body manufactured in Examples 1 to 4 and Comparative Examples 1 to 4 were evaluated as follows.

[0137] Specifically, the diameter (D) and height (T) of each molded body were measured using a vernier caliper, and the weight (Mass) was weighed using a scale. In addition, the relative density was converted into a volume % by converting the input amount of each weight into a level compared to the theoretical density, and the results are shown in Table 2 below. The density of the measured sample was calculated as weight / volume, and when multiple identical samples were produced, it was expressed as an average value.

[0138] For reference, in Table 2 below, each sample was not sintered and had a low relative density, and after sintering (heat treatment), the relative density of each sintered body was at the level of 96%.

[0139] Dopant diameter (D) height (T) weight (g) relative density (%) theoretical density (g / cm 3 ) Example 1 M3+M4+M5 46.3 29.16 58.0 26 1.5 6.118 Example 2 M3+M4+M5 46.229.10 58.13 6 2.36 115 Example 3 M3+M4+M5 46.28 9.0 9 58.0 7 6 2.26 106 Example 4 M3+M4 46.27 9.28 58.0 16 2.45 958 Comparative Example 1-46.3 29.12 58.12 6 2.06 098 Comparative Example 2 M5 46.119.0 5 58.15 6 1.66 249 Comparative Example 3 M3+M5 46.24 8.9 58.19 6 3.36 122 Comparative Example 4M346.319.1158.2163.55.976

[0140]

[0141] [Experimental Example 2] Evaluation of structural changes and average particle size of sintered bodies

[0142] The structural changes and average particle size of the sintered bodies heat-treated at 1,437℃ were evaluated.

[0143] Specifically, the sintered bodies of Examples 1 to 4 manufactured under non-pressurized conditions and the Comparative Examples 1 to 3 manufactured under the same conditions were used as samples. These two types of samples were cut into 10X10X10 mm sizes using a metal blade, and then polished for several minutes using a polishing machine from SiC paper #100 to #2000, and then finally prepared using a 1㎛ paste slurry and ultrafine cloth. Afterwards, the samples were immersed in hydrogen peroxide water at about 200℃ for 1 minute and heat-treated so that the surface of the tissue could be exposed.

[0144] In addition, the average particle size of the sintered body was measured using FE-SEM (Hitachi, S-4800) at the same magnification of 1,000 for each sample, and 5 lines were randomly drawn on the measured photograph, and the linear intercept method according to the following mathematical formula 1 was used to calculate the average particle size for about 100 particles, and the results are shown in Figures 1 to 3.

[0145] [Mathematical Formula 1]

[0146] D = 1.56 × C / MN

[0147] In the above formula,

[0148] D = mean particle diameter, C = total length of the line, M = magnification, N = number of particles on the line.

[0149] As a result of the experiment, in the case of Comparative Example 1, which is composed of molybdenum oxide and niobium oxide, the average particle diameter of the sintered body was approximately 11.8 ㎛. In addition, in the case of Comparative Example 3, which includes molybdenum oxide and niobium oxide as the basic composition but also includes alkaline earth metal oxide, the average particle diameter was 27.2 ㎛, indicating that the average particle diameter of the sintered body was somewhat larger due to the alkaline earth metal dopant.

[0150] In comparison, it was confirmed that Examples 1 to 4, which included molybdenum oxide and niobium oxide as basic compositions but also included alkaline earth metal oxide and zirconium oxide, had an average particle size that was significantly smaller than that of Comparative Example 3 (see Figures 1 to 3 below).

[0151]

[0152] [Experimental Example 3] Evaluation of target appearance after sputtering of sintered body

[0153] After sputtering was performed using the sintered body targets of Example 3 and Comparative Example 3, the appearance of the targets was evaluated, and the results are shown in Table 3 and Figure 4 below.

[0154] In general, when the surface roughness (Ra) of the sputtering target is high, problems such as foreign matter contamination and non-uniformity of the thin film composition occur.

[0155] As a result of the experiment, the sintered target of Comparative Example 3, which does not contain zirconium, had a surface roughness of 0.59 ㎛ before sputtering and a surface roughness of 4.9 ㎛ after sputtering. In comparison, the sintered target of Example 3 had a surface roughness of 0.53 ㎛ and a surface roughness of 0.82 ㎛ after sputtering.

[0156] Through the above-described results, it was confirmed that the oxide sintered body of the present invention controls the particle growth within the sintered body by the alkaline earth metal (M3) dopant to a predetermined range or less by adding the zirconium (M4) dopant, thereby achieving the effect of homogenizing the composition and improving the film quality.

[0157] Surface roughness of target before sputtering (㎛) Surface roughness of target after sputtering (㎛) Example 30.5 30.82 Comparative example 30.5 9 4.9

[0158]

[0159] [Experimental Example 4] Evaluation of density and shrinkage of sintered body

[0160] After heat treatment was performed on each sample manufactured in Examples 1 to 4 and Comparative Examples 1 to 3, the changes in the physical properties of each sintered body were measured.

[0161] (1) Density evaluation after heat treatment

[0162] The physical properties of the sintered body after heat treatment were measured in the same manner as in Experimental Example 1 described above. As an example, the results of the relative density calculated by measuring the diameter, height, and weight of the heat-treated sintered body are shown in Figure 4 below.

[0163] Experimental results showed that in Examples 1 to 4, the relative density significantly increased as the sintering temperature increased from 1400°C to 1500°C (see Fig. 5). In contrast, in Comparative Examples 1 and 2, the relative density of the molded body was lower or similar depending on the sintering temperature, and Comparative Example 3 had a density similar to that of the Examples.

[0164] (2) Evaluation of shrinkage rate before and after heat treatment

[0165] The diameter and height of the pre-heat-treated molded body and the post-heat-treated sintered body were measured, respectively, and the shrinkage ratio was calculated. The calculated shrinkage ratio results are shown in Figure 6 below.

[0166] As a result of the experiment, in the case of Comparative Examples 1 to 3, the rate of change in shrinkage rate due to heat treatment was not large. In contrast, in the case of Examples 1 to 4, it was found that the rate of change in shrinkage rate of the sintered body due to heat treatment was relatively high (see Fig. 6). Such a high shrinkage rate before and after heat treatment means that a large number of pores existing in the molded body were removed by heat treatment, and as a result, it was found that the density and density characteristics of the sintered body were significantly improved by heat treatment.

[0167]

[0168] [Experimental Example 5] Evaluation of sintered body density and mass reduction rate

[0169] After heat treatment was performed on each of the molded body samples manufactured in Examples 1 to 4 and Comparative Examples 1 to 4, the mass change of each sintered body was measured.

[0170] When measuring the mass change, the weight before sintering is measured, and the weight at the time of taking out is measured, and the mass loss value is converted into a percentage, and the results are shown in Figure 7 below.

[0171] As a result of the experiment, it was found that the rate of decrease in mass change of the sintered body due to heat treatment in Examples 1 to 4 was relatively greater than in Comparative Examples 1 to 4 (see Fig. 7).

[0172]

[0173] [Experimental Example 6] Evaluation of Sintered Body Resistivity

[0174] The resistivity characteristics of each sintered body sample manufactured in Examples 1 to 4 and Comparative Examples 1 to 4 were evaluated.

[0175] Specifically, the resistivity of the sintered body samples of Examples 1 to 4 and Comparative Examples 1 to 4 was measured using the Loresta-GX MCP-T700 product (Mitsubishi Chemical Co., Ltd.), and the results are shown in Table 4 below.

[0176] Resistivity characteristics according to sintering temperature (10^10 -3 Ωcm)1400℃1425℃1437℃1450℃1500℃Example 1--2.46--Example 2-1.952.252.69-Example 3-1.892.342.55-Example 44.25-3.89-3.42Comparative Example 1Not measurable-30.3-24.3Comparative Example 2Not measurable-21.5-13.2Comparative Example 32.099-2.63-3.02Comparative Example 43.28-2.34-3.62

[0177] As shown in Table 4 above, it was confirmed that the sintered bodies of Examples 1 to 4 containing a predetermined metal oxide as an additive had superior resistivity characteristics compared to the sintered bodies of Comparative Examples 1 to 4 not containing a specific dopant additive.

[0178]

[0179] [Experimental Example 7] XRD Evaluation of Sintered Body

[0180] XRD analysis was performed to confirm the crystal phase of the oxide sintered body according to Example 3, Comparative Example 1, and Comparative Example 3, and the results are shown in Figure 8 below.

[0181] Unlike Comparative Examples 1 and 3 that do not contain zirconium, it can be confirmed that the oxide sintered body of Example 3 additionally forms a MgZrNb2O8 phase, which is judged to have reduced the movement between particles within the sintered body and thus reduced the average grain size (see Fig. 8).

Claims

1. Containing molybdenum (M1); niobium (M2); at least one alkaline earth metal (M3); and zirconium (M4), An oxide sintered body containing molybdenum (M1) as a main component in an amount of 60 atomic% or more based on a total of 100 atomic% of the metal components in question, The above zirconium (M4) is an oxide sintered body containing 0.1 to 7 atomic% based on 100 atomic% of the total of the metal components.

2. In paragraph 1, An oxide sintered body comprising at least one alkaline earth metal (M3) and zirconium (M4) in an atomic ratio of 1:0.03 to 0.

54.

3. In paragraph 1, An oxide sintered body, wherein the average grain size (D50) in the oxide sintered body is 80% or less of the average grain size (D50) in the oxide sintered body that does not contain zirconium.

4. In paragraph 1, Molybdenum (M1) and niobium (M2) included in the above oxide sintered body are oxide sintered bodies satisfying the following atomic ratios: (i) 0.85 ≤ (M1+M2) / (M1+M2+M3+M4) < 1.0 (ii) 0.5 ≤ M1 / (M1+M2) ≤ 0.9 (iii) 0.1 ≤ M2 / (M1+M2) ≤0.5 5. In paragraph 1, An oxide sintered body in which the niobium (M2) and the zirconium (M4) are included in an atomic ratio of 1:0.01 to 1.

0.

6. In paragraph 1, An oxide sintered body, wherein at least one alkaline earth metal (M3) comprises at least one element selected from Ca and Mg.

7. In paragraph 1, An oxide sintered body, wherein the oxide sintered body further comprises at least one metal (M5) selected from the group consisting of Mo, Ti, Cr, W, and Cu.

8. In paragraph 1, The above oxide sintered body is an oxide sintered body including a MgZrNb2O8 crystal phase.

9. In paragraph 1, The above oxide sintered body is, An oxide sintered body, which is manufactured by mixing molybdenum (M1) oxide; niobium (M2) oxide; at least one alkaline earth metal (M3) oxide; and zirconium (M4) oxide to form a molded body and then sintering the molded body under atmospheric pressure without applying pressure.

10. In paragraph 9, The above molybdenum oxide (M1) includes at least one of MoO2 and MoO3, An oxide sintered body, which comprises 60 to 70 wt% of the total weight of the oxide sintered body.

11. In paragraph 9, The above molybdenum oxide (M1) and the above niobium oxide (M2) are included in an amount of 85.0 wt% or more and less than 100 wt% based on 100 wt% of the oxide sintered body, An oxide sintered body in which the content ratio of the above molybdenum oxide (M1) and the above niobium oxide (M2) is 50:50 to 90:10 by weight.

12. In paragraph 9, The above alkaline earth metal oxide (M3) is an oxide sintered body comprising at least one selected from the group consisting of CaCO3 and MgO.

13. In paragraph 9, An oxide sintered body, wherein the metal oxide (M3) is contained in an amount of more than 0 wt% and less than 10 wt% based on 100 wt% of the oxide sintered body.

14. In paragraph 9, An oxide sintered body, wherein the oxide sintered body further comprises at least one metal (M5) selected from the group consisting of Mo, Ti, Cr, W, and Cu.

15. In paragraph 14, An oxide sintered body, wherein the metal (M5) is included in an amount of 3 to 50 wt% based on the total weight of the sintered body.

16. In paragraph 9, The average grain size (D50) of the above non-pressurized sintered oxide sintered body is 5 to 30 ㎛, The difference in surface roughness (Ra) of the oxide sintered body before and after sputtering is less than 1.0 ㎛, Resistivity is 1×10 -2 Ωcm or less, Oxide sintered body with a relative density of 80% or more.

17. A sputtering target comprising an oxide sintered body according to any one of claims 1 to 16.

18. An oxide thin film formed from the sputtering target of Article 17. 19.(i) A step of preparing and mixing raw material powders containing molybdenum oxide (M1); niobium oxide (M2); metal oxide containing at least one alkaline earth metal (M3); and zirconium oxide (M4) according to a target composition; (ii) a step of manufacturing a molded body using mixed raw material powder; and (iii) a step of manufacturing a sintered body by subjecting the molded body to a non-pressurized heat treatment under atmospheric pressure in an inert atmosphere at 1,200 to 1,600°C for 1 to 20 hours; A method for manufacturing an oxide sintered body of claim 1, comprising:

Citation Information

Patent Citations

  • Free-cutting ceramics and method of producing the same

    JP2002104869A

  • Target materials for depositing molybdenum oxide layers

    JP2020536174A

  • Thin-film solar array having molybdenum-containing rear electrode layer

    KR1020100097194A

  • Method of making a heating element of molybdenum silicide type

    US20050184058A1

  • KR20230041149A