Dust-free insulation material and method for producing same
A dust-free insulation material made from silica and alumina, coated with a specific sol-based solution, addresses the challenge of dust generation in high-temperature applications, offering a stable and cost-effective solution for hydrogen production processes.
Patent Information
- Application Number
- PCT/KR2024/095227
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-17
AI Technical Summary
The need for dust-free insulation materials that can be applied inside combustion chambers without generating dust, which is essential for reducing environmental pollution and manufacturing costs in hydrogen production processes, where high-temperature insulation is required but traditional insulation materials are expensive and generate dust.
A dust-free insulation material composed of silica and alumina, coated with a solution containing 51.4 to 62.9% silica sol and 12.9 to 15.7% alumina sol, with water as the solvent, which is applied through an impregnation, drying, firing, and polishing process to create a stable, high-temperature-resistant insulation that prevents dust generation.
The solution provides a cost-effective, environmentally friendly insulation material with improved mechanical strength and durability, capable of withstanding high temperatures without generating dust, thus suitable for use inside combustion chambers in hydrogen production processes.
Smart Images

Figure KR2024095227_17102024_PF_FP_ABST
Abstract
Description
Dust-free insulation material and method for manufacturing the same
[0001] The present invention relates to a dust-free insulating material, and more specifically, to a dust-free insulating material that does not generate dust and can be applied inside a combustion chamber, and a method for manufacturing the same.
[0002]
[0003] Recently, countries and companies are making significant efforts to address environmental pollution and global warming. Fossil fuels, while currently the most widely used energy source, are significantly contributing to environmental pollution and global warming. Therefore, significant efforts are being made to secure alternative energy sources. In particular, technologies related to the catalytic reforming of various gases to produce hydrogen, a promising alternative energy source, are attracting attention. Representative examples include reactions that convert fossil fuels such as methane, methanol, gasoline, and natural gas into hydrogen, including steam reforming, partial oxidation, and autothermal reforming.
[0004] These reforming reactions require the use of catalysts, and catalytic reactions produce reactants through endothermic or exothermic reactions depending on fuel conditions.
[0005] In the case of an endothermic reaction, a method is applied in which a catalytic reactor is installed inside a combustion chamber and a heat source is supplied to the catalytic reactor using a burner installed inside the combustion chamber.
[0006] In the case of an exothermic reaction, a heat source is required at the beginning of the catalytic reaction inside the reactor, and thereafter, temperature control is possible due to the exothermic reaction, and heat according to the reaction temperature is transferred to the outside of the catalytic reactor.
[0007] Accordingly, the temperature of the combustion chamber rises high, and insulation is applied to the combustion chamber to prevent the temperature inside the combustion chamber from being transferred to the outside of the combustion chamber and to maintain the temperature of the combustion chamber at a constant level.
[0008] For example, insulation can be installed outside the combustion chamber, but this has the disadvantage that the combustion chamber, which is directly exposed to heat, must be made of expensive metal materials that can withstand high temperatures.
[0009] Furthermore, installing insulation inside the combustion chamber allows for the replacement of expensive metals in combustion chambers not directly exposed to heat, allowing for the construction of combustion chambers using less expensive metals. However, to prevent dust from being mixed with the exhaust gas generated by the combustion chamber, insulation must be non-dust-generating. Therefore, to improve reactor manufacturing costs, the development of non-dust-generating and non-dust-free insulation materials is urgently needed.
[0010]
[0011] The present invention aims to solve the above problems by providing an insulating material that does not generate dust and a method for manufacturing the same.
[0012]
[0013] The present invention provides a dust-free insulating material coating solution for manufacturing a dust-free insulating material, which is coated on an insulating material including silica and alumina, and comprises 51.4 to 62.9 wt% of silica sol; 12.9 to 15.7 wt% of alumina sol; and the remainder being a solvent, wherein the solvent is water, thereby preventing environmental and safety problems during the manufacturing of a dust-free insulating material and preventing an increase in drying and firing time required to completely remove organic solvents and organic substances.
[0014] In addition, the present invention provides a method for manufacturing a dust-free insulating material, comprising: an insulating material preparation step of preparing an insulating material containing silica and alumina; an insulating material coating step of manufacturing a coated insulating material including an impregnation step of impregnating the insulating material with a dust-free insulating material coating solution and a drying step of drying the insulating material after completion of the impregnation step; a firing step of heating and firing the coated insulating material; a first polishing step of polishing the surface of the coated insulating material with a first polishing paper; and a second polishing step of polishing the surface of the coated insulating material after completion of the first polishing step with a second polishing paper.
[0015]
[0016] According to one embodiment of the present invention, it is possible to manufacture an insulating material that is stable at high temperatures and does not generate dust, and can be applied inside a combustion chamber.
[0017]
[0018] Figure 1 is a schematic diagram of a method for manufacturing a dust-free insulating material according to one embodiment of the present invention.
[0019] Figure 2 shows a dust generation test of Example 1 and uncoated insulation according to one embodiment of the present invention.
[0020] Figure 3 shows a dust generation test of Example 1 and Comparative Examples 1 to 3 according to one embodiment of the present invention.
[0021]
[0022] Hereinafter, embodiments of the present invention are described in detail. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments are provided solely to ensure complete disclosure of the present invention and to more fully inform those skilled in the art of the present invention.
[0023]
[0024] The present invention provides a dust-free insulating material, a dust-free insulating coating solution for coating the insulating material so that dust is not generated on the surface of the insulating material, and a method for manufacturing the dust-free insulating material to which the insulating material is applied using the dust-free insulating coating solution. Accordingly, the dust-free insulating material is provided by using the dust-free insulating coating solution and the manufacturing method to prevent dust from being generated from the insulating material due to its low density and low mechanical strength. Accordingly, the dust-free insulating material can be applied to the inside of a combustion chamber.
[0025] It is preferable that the above-mentioned insulating material be one that has a large surface area, low thermal conductivity, is physically / chemically stable, is made of safe materials, is easy to process, and has a low unit price. For example, it is preferable that the above-mentioned insulating material be one that uses silica with excellent thermal stability and alumina with excellent strength, and an insulating material formed of Al2O3: 46-85%, SiO2: 25-54%, and a density of 350 ± 35 kg / ㎥ can be applied, but is not limited thereto.
[0026]
[0027] Hereinafter, a dust-free insulating material coating solution for manufacturing the dust-free insulating material of the present invention will be described in detail.
[0028] The dust-free insulating coating solution according to the present invention comprises silica sol, alumina sol, and a solvent.
[0029] The above dust-free insulating material coating liquid can improve the mechanical strength and durability of the outer surface of the insulating material by densifying some of the surface pores of the insulating material.
[0030] The above dust-free insulating material coating solution may contain 51.4 to 62.9 wt% of silica sol, 12.9 to 15.7 wt% of alumina sol, and the remainder of a solvent. Accordingly, since the insulating material and the dust-free insulating material coating solution, which are mainly composed of Al2O3 and SiO2, have the same components, the dust-free insulating material coating solution can be well coated on the surface of the insulating material.
[0031] For example, the silica sol may be a dispersion in which SiO2 particles are dispersed at a content of 27 to 33 wt%, and a silica sol in which the size of the SiO2 particles is 8 to 25 nm may be applied.
[0032] In addition, the alumina sol may be a dispersion in which Al2O3 particles are dispersed in a content of 5 to 20 wt%, and an alumina sol having an Al2O3 particle size of 15 to 170 nm may be applied.
[0033] Additionally, the solvent may be water. For example, distilled water and DI-water may be used, but are not limited thereto.
[0034] Accordingly, by applying hydrophilic substances such as silica sol and alumina sol, it is possible to manufacture a dust-free insulating coating solution even in an environment that does not use an organic solvent, and environmental and safety problems that may arise when using an organic solvent can be prevented, and the increase in drying and firing time required to completely remove the organic solvent can be prevented.
[0035] In addition, by applying silica sol and alumina sol at the same time to the dust-free insulation coating liquid, a double coating effect of two substances can be achieved with a single coating, thereby ensuring ease of production and economic feasibility.
[0036] In the above dust-free insulating coating liquid, if the silica sol ratio is low and the alumina sol ratio is high, dust may be generated on the insulating material, and the insulating effect may deteriorate. For example, if the silica sol is contained in the dust-free insulating coating liquid in an amount of less than 51.4 wt% and the alumina sol exceeds 15.7 wt%, when the silica sol is coated on the surface of the insulating material, the ability to densify a portion of the surface pores of the insulating material may be reduced, which may adversely affect the mechanical strength and durability of the outer side of the coated insulating material, and the dust-prevention ability may be reduced. In addition, if the alumina sol ratio is increased, the insulating effect may be reduced.
[0037] In addition, in the dust-free insulating coating solution, if the silica sol ratio and the alumina sol ratio are low and the solvent ratio is high, the strength of the coated insulating material may decrease. For example, if the dust-free insulating coating solution contains less than 51.4 wt% of silica sol and less than 12.9 wt% of alumina sol, the silica sol and the alumina sol may not sufficiently coat the surface of the insulating material, which may adversely affect the mechanical strength and durability of the outer side of the coated insulating material, and the dust-prevention ability may decrease.
[0038]
[0039] Figure 1 is a schematic diagram of a method for manufacturing a dust-free insulating material according to one embodiment of the present invention.
[0040] Referring to Fig. 1, the method for manufacturing a dust-free insulation material includes an insulation material preparation step (S1), an insulation material coating step (S2), a firing step (S3), a first polishing step (S4), and a second polishing step (S5).
[0041]
[0042] The insulation preparation step (S1) is a step for preparing an insulation material containing silica and alumina. For example, this is a step for preparing an insulation material to be used in the insulation coating step (S2).
[0043] The insulation preparation step (S1) may include a step of processing the insulation into various shapes before processing is completed. At this time, the insulation can be processed so that it can be installed inside a combustion chamber.
[0044] The insulation preparation step (S1) may include a foreign substance removal step for removing foreign substances attached to the surface of the insulation. For example, dust generated during the processing of the insulation or foreign substances attached during the handling of the insulation may be removed using various methods such as a brush or blower. Accordingly, when coating the insulation with the dust-free insulation coating solution, the formation of uneven coating areas or uncoated areas due to foreign substances attached to the surface of the insulation can be prevented, and dust generation due to foreign substances can be prevented.
[0045]
[0046] The insulation coating step (S2) is a step for manufacturing a coated insulation material coated with the above dust-free insulation coating liquid, and may include an impregnation step and a drying step.
[0047] The impregnation step of the insulation coating step (S2) is a step of impregnating the insulation with the dust-free insulation coating liquid.
[0048] In the above impregnation step, it is preferable that the dust-free insulating coating solution and the insulating material be prepared in a volume ratio of 1.2 to 1.5:1, and the insulating material be impregnated with the dust-free insulating coating solution. For example, if the dust-free insulating coating solution ratio is less than 1.2, the insulating material surface may be coated in an amount less than necessary. In addition, if the dust-free insulating coating solution ratio exceeds 1.5, waste of the dust-free insulating coating solution may occur.
[0049]
[0050] The drying step of the insulation coating step (S2) is a step of drying the insulation material after the impregnation step is completed. For example, hot air drying, infrared drying, and combinations thereof may be applied, but are not limited thereto.
[0051] In addition, it is preferable to dry the insulating material so that the insulating material does not overlap each other, so that the insulating material can be dried evenly. Accordingly, during the drying step, SiO2 and Al2O3, which were mixed with the solvent on the insulating material, adhere to the surface and surface pores of the insulating material to form a coating layer, and the solvent can be removed.
[0052] The above drying step is preferably performed at a drying temperature of 180 to 220°C for 0.5 to 1.5 hours. For example, if the drying temperature is lower than 180°C, insufficient heat is applied, resulting in a prolonged drying time and a decrease in process efficiency and cost-effectiveness. Furthermore, if the drying temperature exceeds 220°C, heat exceeding the amount sufficient to form a coating layer on the surface of the insulation material by the dust-free insulation coating solution may be applied, resulting in unnecessary energy consumption and a decrease in process efficiency.
[0053] In addition, if the drying time is less than 0.5 hours, a coating layer by the dust-free insulating coating solution may not be stably formed on the surface of the insulating material, and if it exceeds 1.5 hours, a decrease in process efficiency due to unnecessary energy use may occur after the coating layer by the dust-free insulating coating solution is sufficiently formed on the surface of the insulating material.
[0054] The impregnation step and the drying step of the insulation coating step (S2) can be repeated at least once. For example, the impregnation step and the drying step of the insulation coating step (S2) can be repeated at least once until the coating amount calculated by calculating the density difference based on the weight difference between the coated insulation material that has completed the insulation coating step (S2) and the insulation material before entering the insulation coating step (S2) becomes 150 to 300 kg / ㎥ (0.15 to 0.30 g / ㎤). At this time, since the dust-free insulation coating liquid penetrates and coats the pores of the insulation material in the insulation coating step (S2), the change in volume can be ignored when calculating the density. Accordingly, the coated insulation material can be effectively produced through the insulation coating step (S2).
[0055]
[0056] The firing step (S3) is a step of heating and firing the above-mentioned coating insulation.
[0057] The firing step (S3) is a step of heating and firing the coated insulation material that has completed the insulation coating step (S2). For example, the firing step (S3) can be applied using various heating methods such as hot air heating, infrared heating, and combinations thereof, but is not limited thereto. At this time, the heating conditions are preferably such that the temperature inside the combustion chamber is increased by a heating rate of 5 to 10°C to a target temperature of +50°C, for example, 800 to 1,200°C, and then maintained for 6 to 12 hours.
[0058] The firing step (S3) can form a coating layer on the surface of the coated insulation, from which all solvents and organic substances have been removed, while raising the temperature to the target temperature. Furthermore, this step involves pre-shrinking the coated insulation, which includes pores, to prevent the dust-free insulation produced through a subsequent process from shrinking when applied to the combustion chamber.
[0059] For example, if the target temperature of the firing step (S3) is less than 800°C, the temperature of the combustion chamber to which the dust-free insulation material manufactured from the coated insulation material is applied may be lower. Accordingly, when the dust-free insulation material is used in the combustion chamber, additional shrinkage may occur, thereby reducing the insulation efficiency of the combustion chamber.
[0060] Additionally, if the target temperature of the firing step (S3) exceeds 1200°C, the temperature is significantly higher than the reaction temperature of the combustion chamber to which the dust-free insulation material manufactured from the coated insulation material is applied. Accordingly, a decrease in process efficiency may occur due to unnecessary energy consumption.
[0061] In addition, if the heating rate is less than 5℃, it may take too long to reach the target temperature, which may result in a decrease in process efficiency, and if the heating rate exceeds 10℃, deformation of the coating insulation may occur due to rapid temperature increase.
[0062] If the firing stage (S3) is operated for less than 6 hours after reaching the target temperature, firing may not be completed, and if it exceeds 12 hours, a decrease in process efficiency may occur due to unnecessary energy and time consumption after firing is completed.
[0063]
[0064] The first polishing step (S4) is a step of polishing the surface of the above-mentioned coated insulation material with a first polishing paper.
[0065] The first polishing step (S4) can remove surface irregularities and dust by polishing the coated insulation material surface at a speed of 300 to 500 rpm for 5 to 10 seconds per surface using a polishing machine to which a first polishing paper of #800 to #1000 is applied. At this time, the first polishing paper may be applied to a polishing paper applied with aluminum oxide, zirconium silicate, ceramic particles, etc., but is not limited thereto, and the polishing machine may be applied to a circular or square polishing machine type, but is not limited thereto.
[0066] For example, when using a first abrasive paper with a grit of less than #800, the coated surface may be excessively abraded, reducing the dust-prevention effect. Furthermore, when using a first abrasive paper with a grit of more than #1000, the effect of abrading the micro-roughness of the surface may be reduced, preventing the polishing from being completed within the working time and taking excessive time.
[0067] The first polishing step (S4) may include a step of removing dust or foreign substances attached to the surface of the coated insulation material after polishing the surface of the coated insulation material using various methods such as a brush or blower.
[0068]
[0069] The second polishing step (S5) is a step of manufacturing a dust-free insulating material by polishing the surface of the coated insulating material that has completed the first polishing step with a second polishing paper.
[0070] The second polishing step (S5) can remove surface irregularities and dust by polishing the coated insulation material surface at a speed of 300 to 500 rpm for 5 to 10 seconds per surface using a polishing machine with #3000 second polishing paper applied. At this time, the second polishing paper may be, but is not limited to, a sponge polishing paper type, and the polishing machine may be, but is not limited to, a circular or square polishing machine type.
[0071] In the second polishing step (S5), if a second polishing paper of less than #3000 is used, the surface may be excessively abraded, which may reduce the dust generation prevention effect. Furthermore, if a second polishing paper of more than #3000 is used, the effect of polishing the micro-roughness of the surface may be reduced, so polishing may not be completed within the working time and may take excessive time.
[0072] The second polishing step (S5) may include a step of removing dust or foreign substances attached to the coated insulation material during handling after polishing the surface of the coated insulation material using various methods such as a brush or blower.
[0073]
[0074] Hereinafter, the present invention will be described in more detail through examples, comparative examples, and experimental examples. However, the following examples are intended only to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.
[0075]
[0076] Examples 1-3
[0077]
[0078] Insulation: Al2O3 46~85%, SiO2 25~54%, density 350±10% kg / ㎥, insulation used.
[0079] Silica sol: Mix and use silica sol SS-30SG (Schemtech), SS-30A (Schemtech) and SS-30 (Schemtech) with SiO2 particle content of 29-31 wt% and SiO2 particle size of 10-20 nm.
[0080] Alumina sol: Use alumina sol (Alintec) with Al2O3 particle content of 5 to 20 wt% and Al2O3 particle size of 20 to 150 nm.
[0081] Water: distilled water
[0082] Insulation coating stage conditions: Dust-free insulation coating solution: insulation = 1.5:1 volume ratio, impregnation temperature 20℃, impregnation was performed until no bubbles were generated in the insulation, then drying was performed at a drying temperature of 200℃ for 1 hour, and the coating amount was 200 kg / ㎥ (0.20 g / ㎤).
[0083] Firing stage conditions: Firing at 1000℃ for 6 hours.
[0084] First polishing stage conditions: #1000 first polishing paper (a polishing paper with aluminum oxide, nitride, and ceramic particles) was applied to a polishing machine (circular polishing machine) at a speed of 300 rpm for 10 seconds per surface of the coated insulation.
[0085] Second polishing stage conditions: Using a polishing machine (circular polishing machine) with #3000 second polishing paper (sponge polishing paper type), polishing was performed for 10 seconds per surface of the coated insulation at a speed of 300 rpm.
[0086]
[0087] Using the above-mentioned insulating material, the above-mentioned silica sol, the above-mentioned alumina sol, and the above-mentioned water, 10 dust-free insulating materials were manufactured using a work method that satisfies the above-mentioned insulating material coating step conditions, the above-mentioned firing step conditions, the above-mentioned first polishing step conditions, and the above-mentioned second polishing step conditions, based on the content of the dust-free insulating material coating solution described in Table 1.
[0088] At this time, the coating liquid content in Table 1 below allowed a 1% measurement error, and was randomly selected from 10 dust-free insulators corresponding to Example 1, randomly selected from 10 dust-free insulators corresponding to Example 2, and randomly selected from 10 dust-free insulators corresponding to Example 3, and used for the test.
[0089]
[0090] Content of dust-free insulation coating solution Silica sol (g) Alumina sol (g) Water (g) Example 1 100 2550 Example 2 110 22.54 2.5 Example 3 90 27.55 7.5
[0091]
[0092] Comparative examples 1-3
[0093]
[0094] Insulation: Al2O3 46~85%, SiO2 25~54%, density 350±10% kg / ㎥, insulation used.
[0095] Silica sol: Mix and use silica sol SS-30SG (Schemtech), SS-30A (Schemtech) and SS-30 (Schemtech) with SiO2 particle content of 29-31 wt% and SiO2 particle size of 10-20 nm.
[0096] Alumina sol: Use alumina sol (Alintec) with Al2O3 particle content of 5 to 20 wt% and Al2O3 particle size of 20 to 150 nm.
[0097] Water: distilled water
[0098] Insulation coating stage conditions: Dust-free insulation coating solution: insulation = 1.5:1 volume ratio, impregnation temperature 20℃, impregnation was performed until no bubbles were generated in the insulation, then drying was performed at a drying temperature of 200℃ for 1 hour, and the coating amount was 200 kg / ㎥ (0.20 g / ㎤).
[0099] Firing stage conditions: Firing at 1000℃ for 6 hours.
[0100] First polishing stage conditions: #1000, a polishing machine (circular polishing machine) with first polishing paper (polishing paper with aluminum oxide, nitrous oxide, and ceramic particles) was used to polish the coated insulation for 10 seconds per surface at a speed of 300 rpm.
[0101] Second polishing stage conditions: #3000, using a polishing machine (circular polishing machine) with a second polishing paper (sponge polishing paper type) applied, polished at a speed of 300 rpm for 10 seconds per surface of the coated insulation.
[0102]
[0103] Using the above-mentioned insulating material, the above-mentioned silica sol, the above-mentioned alumina sol, and the above-mentioned water, 10 dust-free insulating materials were manufactured each by a work method that satisfies the above-mentioned insulating material impregnation step conditions, the above-mentioned firing step conditions, the above-mentioned first polishing step conditions, and the above-mentioned second polishing step conditions based on the content of the dust-free insulating material coating liquid described in Table 2.
[0104] At this time, the coating liquid content in Table 2 below allowed a 1% measurement error, and was randomly selected from 10 dust-free insulators corresponding to Comparative Example 1, randomly selected from 10 dust-free insulators corresponding to Comparative Example 2, and randomly selected from 10 dust-free insulators corresponding to Comparative Example 3, and used for the test.
[0105]
[0106] Content of dust-free insulation coating solution Silica sol (g) Alumina sol (g) Water (g) Comparative example 1 100 5550 Comparative example 2 100 4550 Comparative example 3 100 3550
[0107]
[0108] Experimental Example 1
[0109] Temperature: 23 ± 1℃, Humidity: 31 ± 1 %RH environment
[0110] The thermal conductivity (W / mK) according to temperature of the uncoated insulation material before coating with the dust-free insulation coating solution and the dust-free insulation material according to Examples 1 to 3 was evaluated based on the test method KS L 1604, and the evaluation results are shown in Table 3.
[0111]
[0112] Classification Uncoated Insulation Example 1 Example 2 Example 3 25℃ 0.47 0.38 0.37 0.49 600℃ 0.66 0.56 0.59 0.64 800℃ 0.71 0.97 0.86 1.01 1,000℃ 1.12 1.14 1.10 1.18
[0113] Referring to Table 3, it can be confirmed that there is no significant difference in thermal conductivity of Examples 1 to 3 of the present invention compared to uncoated insulation before coating with a dust-free insulation coating solution.
[0114] Accordingly, even if a dust-free insulating material is manufactured by coating the insulating material with the dust-free insulating material coating solution according to the present invention, an insulating effect can be secured, and the material can be applied inside the combustion chamber of a reactor.
[0115]
[0116] Experimental Example 2
[0117] Device Name: PARTICLE COUNTER
[0118] Production company: PMS
[0119] Format: LASAIRⅡ-110
[0120] Using standard equipment.
[0121] Temperature: 23.2 ± 0.1℃, Humidity: 48 ± 3 %RH In an environment, the number of particles was measured 20 times at a point 2 mm away from the surface of Example 1, and the number of particles was measured 20 times at a point 100 mm away, and the average measurement results are shown in Table 4.
[0122]
[0123] ClassificationExample 1Example 2Example 320 times average measurement (units)20 times average measurement (units)20 times average measurement (units)Particle size2mm point100mm point2mm point100mm point2mm point100mm point0.1㎛3.353.903.643.853.293.640.2㎛1.001.651.021.790.961.620.3㎛0.100.200.120.230.090.180.5㎛0.000.000.000.000.000.001.0㎛0.000.000.000.000.000.005.0㎛0.000.000.000.000.000.00
[0124] Referring to Table 4, it can be confirmed that the dust-free insulation materials according to Examples 1 to 3 generated an average of less than 10 particles smaller than 0.5 μm, and no particles larger than 0.5 μm were generated. Accordingly, it can be confirmed that when an insulation material is manufactured using the dust-free insulation coating composition according to the present invention, dust generation can be suppressed.
[0125]
[0126] Experimental Example 3
[0127] Before coating the dust-free insulation coating solution on a black adhesive board (applied on A4 paper printed with black ink using a general commercial stick-type adhesive), the insulation material and the dust-free insulation material according to Example 1 were placed on the adhesive board and left on for 1 minute so that they could adhere to the adhesive board by their own weight.
[0128] Afterwards, the insulation and the dust-free insulation were removed from the adhesive plate to check whether dust was attached to the adhesive plate, and this is shown in Fig. 2.
[0129] Referring to Fig. 2, it can be seen that the uncoated insulation material before coating with the dust-free insulation coating liquid has dust attached to the adhesive plate, and the black surface of the adhesive plate is stained white.
[0130] On the other hand, in Example 1, it can be seen that dust does not stick to the adhesive plate, and the adhesive plate is confirmed to be black.
[0131] Accordingly, it can be confirmed that when a dust-free insulating material is manufactured by coating the insulating material with the dust-free insulating material coating solution according to the present invention, dust generation can be suppressed.
[0132]
[0133] Experimental Example 4
[0134] The dust-free insulation material according to Example 1 and the insulation materials produced in Comparative Examples 1 to 3 were placed on a black adhesive board (applied on A4 paper printed with black ink using a general commercial stick-type adhesive) and left on the adhesive board for 1 minute so that they would adhere to the adhesive board by their own weight. Thereafter, the insulation material and the dust-free insulation material were removed from the adhesive board to check whether dust was attached to the adhesive board, which is shown in Fig. 3.
[0135] Referring to Figure 3, in Comparative Examples 1 to 3, it can be confirmed that dust adheres to the adhesive plate, and the black surface of the adhesive plate is stained white.
[0136] On the other hand, in Example 1, it can be seen that dust does not stick to the adhesive plate, and the adhesive plate is confirmed to be black.
[0137] Accordingly, it can be confirmed that when an insulating material is manufactured using a dust-free insulating material coating composition according to the present invention, dust generation can be suppressed.
[0138]
[0139] As described above, the specific description of the present invention has been made by way of embodiments with reference to the attached drawings, but the above-described embodiments have only been described as preferred examples of the present invention, and therefore, the present invention should not be understood as being limited to the above-described embodiments, and the scope of the rights of the present invention should be understood by the claims described below and their equivalent concepts.
Claims
1. Coated with insulation containing silica and alumina, Silica sol 51.4-62.9 wt%; 12.9 to 15.7 wt% of alumina sol; and Including solvent as a residual amount; The above solvent is applied with water, which can prevent environmental and safety issues when manufacturing dust-free insulation, and can prevent an increase in drying and firing time required to completely remove organic solvents and organic substances. Dust-free insulation coating liquid for manufacturing dust-free insulation.
2. In claim 1, The above silica sol is a dispersion in which SiO2 particles are dispersed at a content of 27 to 33 wt%, and the size of the SiO2 particles is 8 to 25 nm. Dust-free insulation coating liquid.
3. In claim 1, The above alumina sol is a dispersion in which Al2O3 particles are dispersed in a content of 5 to 20 wt%, and the Al2O3 particle size is 15 to 170 nm. Dust-free insulation coating liquid.
4. Insulation preparation step for preparing insulation containing silica and alumina; An insulation coating step of manufacturing a coated insulation material coated with the dust-free insulation coating solution by coating the above insulation material with a dust-free insulation coating solution; A firing step of heating and firing the above-mentioned coating insulation; A first polishing step of polishing the surface of the coated insulation material that has completed the above firing step using a first polishing paper; and A second polishing step of polishing the surface of the coated insulation material that has completed the first polishing step using a second polishing paper; Method for manufacturing dust-free insulation material.
5. In claim 4, The above insulation coating step is: An impregnation step of impregnating the above insulation material with a coating liquid; and A drying step for drying the above insulation material after the impregnation step is completed; The above impregnation step and the above drying step are included at least once. Method for manufacturing dust-free insulation material.
Citation Information
Patent Citations
Energy-saving particle-free heat insulating material and manufacturing method thereof
KR101448141B1
Particle-free heat insulating furnace and construction method thereof
KR101662019B1
Particle-free heat insulating material manufacturing method
KR101810787B1
Method of providing non-face-to-face English education contents using 360 degree digital XR images
KR102359253B1
Particle free heat insulating material and manufacturing method thereof
KR102562885B1