Positive electrode active material composition, positive electrode sheet, battery, and electric device
By using a combination of positive electrode active materials with different crystal forms to control particle size distribution, the compaction density and efficiency of the battery are improved, solving the problems of high energy density and long life of the battery, and realizing a low-cost, high-performance battery design.
Patent Information
- Application Number
- PCT/CN2023/089002
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Existing technologies make it difficult to achieve high energy density and long lifespan for batteries while maintaining low cost.
By using a combination of first and second positive electrode active materials with different crystal forms, and by controlling their particle size distribution curves, the positive electrode can be tightly packed, thereby improving the compaction density and efficiency of the positive electrode sheet.
This achieves high energy density and long lifespan for batteries while maintaining low production costs.
Smart Images

Figure CN2023089002_24102024_PF_FP_ABST
Abstract
Description
Positive electrode active material composition, positive electrode sheet, battery and electrical device Technical Field
[0001] The present application relates to a positive electrode active material composition, a positive electrode plate, a battery and an electrical device. Background Art
[0002] In recent years, batteries have been widely used in energy storage systems such as hydropower, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As battery applications continue to expand, the demand for battery energy density and service life is increasing.
[0003] Summary of the Invention
[0004] The present application provides a positive electrode active material composition, a positive electrode plate, a battery and an electrical device, which can enable the battery to have high energy density, low cost and good service life.
[0005] In a first aspect, the present application provides a positive electrode active material composition, comprising a first positive electrode active material and a second positive electrode active material having a crystal form different from that of the first positive electrode active material, wherein the first positive electrode active material comprises phosphate, and the particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50.
[0006] By making the positive electrode active material composition include a first positive electrode active material and a second positive electrode active material with different crystal forms, and making the particle size distribution curve of the positive electrode active material composition satisfy 0<|Dv1-Dv2| / Dv1≤50, the first positive electrode active material and the second positive electrode active material can be tightly stacked, thereby improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and further enabling the battery using the positive electrode active material composition to have a higher energy density and a longer service life.
[0007] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm.
[0008] In any embodiment, the volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.
[0009] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:
[0010] 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or,
[0011] 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or,
[0012] 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.
[0013] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thus enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.
[0014] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:
[0015] 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or,
[0016] 2.0 μm≤Dv1≤12.5 μm, optionally, 3.0 μm≤Dv1≤12.3 μm; and / or,
[0017] 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.
[0018] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thus enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.
[0019] In any embodiment, the morphology of the first cathode active material includes one or more of single crystal and polycrystalline, and the morphology of the second cathode active material includes one or more of single crystal and polycrystalline.
[0020] In any embodiment, the volume distribution particle size Dv50 of the single-crystal first positive electrode active material is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm.
[0021] In any embodiment, the volume distribution particle size Dv10 of the single-crystal first positive electrode active material is 0.05 μm to 1.5 μm, and optionally 0.1 μm to 1.0 μm.
[0022] In any embodiment, the volume distribution particle size Dv50 of the polycrystalline first positive electrode active material is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm.
[0023] In any embodiment, the volume distribution particle size Dv10 of the polycrystalline first positive electrode active material is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm.
[0024] In any embodiment, the volume distribution particle size Dv50 of the single-crystal second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm.
[0025] In any embodiment, the volume distribution particle size Dv10 of the single-crystal second positive electrode active material is 0.3 μm to 8 μm, and optionally 1.0 μm to 3.5 μm.
[0026] In any embodiment, the volume distribution particle size Dv50 of the polycrystalline second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 15.5 μm.
[0027] In any embodiment, the volume distribution particle size Dv10 of the polycrystalline second positive electrode active material is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.
[0028] When the volume distribution particle size of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density, reduce side reactions, lower interface impedance, and extend the battery life.
[0029] In any embodiment, based on the total weight of the positive electrode active material composition, the weight content of the first positive electrode active material is recorded as w a The weight content of the second positive electrode active material is recorded as w b , then w a is selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%; and / or, w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.
[0030] When the content of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density and / or a longer service life.
[0031] In any embodiment, the powder compaction density P1 of the first positive electrode active material at 30000N is 1.89 g / cm 3 Above, 1.95g / cm2 is optional 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 the following.
[0032] In any embodiment, the powder compaction density P2 of the second positive electrode active material at 30000N is greater than or equal to 2.90 g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3g / cm 3 .
[0033] When the powder compaction density of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density.
[0034] In any embodiment, the BET specific surface area of the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be less than or equal to 1.5m 2 / g, 0.28m can be selected 2 / g to 1.5m 2 / g. This can reduce side reactions and improve the cycle performance of the battery.
[0035] In any embodiment, the first positive electrode active material includes a compound represented by formula (I), Li a A x Mn 1-y B y P 1-z C z O 4-n D n (I)
[0036] A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB and Group VIII; C includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; n is selected from the range of 0 to 0.5.
[0037] By doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping element at the Mn position, obtaining improved cycle performance and / or high-temperature stability, and the gram capacity and compaction density of the material are also improved.
[0038] In any embodiment, A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and can optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W.
[0039] In any embodiment, B includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can optionally include one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge.
[0040] In any embodiment, C includes one or more elements selected from B (boron), S, Si, and N.
[0041] In any embodiment, D includes one or more elements selected from S, F, Cl, and Br.
[0042] In any embodiment, A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, and may optionally include any one element selected from Mg and Nb.
[0043] In any embodiment, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may further optionally include at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and may further optionally include at least two elements selected from Fe, Ti, V, Co and Mg, and may further optionally include Fe and one or more elements selected from Ti, V, Co and Mg.
[0044] In any embodiment, C includes any one element selected from B (boron), S, Si, and N, and may be S.
[0045] In any embodiment, D includes any one element selected from S, F, Cl and Br, and may be F.
[0046] By selecting the Li-position doping element within the above range, the lattice change rate during the delithiation process can be further reduced, thereby further improving the rate performance of the battery. By selecting the Mn-position doping element within the above range, the electronic conductivity can be further improved and the lattice change rate can be further reduced, thereby improving the rate performance and gram capacity of the battery. By selecting the P-position doping element within the above range, the rate performance of the battery can be further improved. By selecting the O-position doping element within the above range, the side reactions at the interface can be further reduced, thereby improving the high-temperature performance of the battery.
[0047] In any embodiment, a is selected from the range of 0.9 to 1.1, optionally from the range of 0.97 to 1.01.
[0048] In any embodiment, x is selected from the range of 0.001 to 0.005.
[0049] In any embodiment, y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5.
[0050] In any embodiment, z is selected from the range of 0.001 to 0.5, alternatively selected from the range of 0.001 to 0.1, more alternatively selected from the range of 0.001 to 0.005.
[0051] In any embodiment, n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.
[0052] By selecting the value of y within the above range, the gram capacity and rate performance of the first positive electrode active material can be further improved. By selecting the value of x within the above range, the kinetic performance of the first positive electrode active material can be further improved. By selecting the value of z within the above range, the rate performance of the battery can be further improved. By selecting the value of n within the above range, the high-temperature performance of the battery can be further improved.
[0053] In any embodiment, x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.5, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0.
[0054] By doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, especially doping a specific element in a specific amount at the Mn position and P position of LiMnPO4 or at the Li position, Mn position, P position and O position of LiMnPO4, the rate performance can be improved, the dissolution of Mn and the doping element at the Mn position can be reduced, the cycle performance and / or high temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.
[0055] In any embodiment, y:z is selected from the range of 0.002 to 999, optionally from the range of 0.025 to 999 or from the range of 0.002 to 500, and more optionally from the range of 0.2 to 600. In this way, defects of the first positive electrode active material can be reduced, and the integrity of the framework structure of the first positive electrode active material can be improved, thereby effectively improving the structural stability of the first positive electrode active material and further improving the cycle stability of the battery.
[0056] In any embodiment, z:n is selected from the range of 0.002 to 500, optionally from the range of 0.2 to 100, and more optionally from the range of 0.2 to 50. In this way, defects of the first positive electrode active material can be further reduced, the integrity of the framework structure of the first positive electrode active material can be further improved, the structural stability of the first positive electrode active material can be effectively improved, and the cycle stability of the battery can be improved.
[0057] In any embodiment, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.1.
[0058] By doping specific elements in specific amounts at the Li, Mn, P, and O positions of the compound LiMnPO4 simultaneously, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping elements at the Mn position, thereby obtaining improved cycle performance and / or high-temperature stability, and the gram capacity and compaction density of the first positive electrode active material can also be improved.
[0059] In any embodiment, B includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can optionally include one or more elements selected from Zn, Fe, Ti, V, Ni, Co and Mg; C includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.
[0060] By doping specific elements at specific amounts at both the Mn and P sites of the LiMnPO4 compound, rate performance can be improved, the dissolution of Mn and the doping element at the Mn site can be reduced, the cycle performance and / or high-temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.
[0061] In any embodiment, (1-y):y is in the range of 0.1-999, optionally in the range of 0.1-10 or in the range of 0.67-999, more optionally in the range of 1 to 10, further optionally in the range of 1 to 4, and further optionally in the range of 1.5 to 3. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.
[0062] In any embodiment, a:x is in the range of 1 to 1200, optionally in the range of 9 to 1100, and more optionally in the range of 190 to 998. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.
[0063] In any embodiment, z:(1-z) is 1:9 to 1:999, and can be optionally 1:499 to 1:249. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.
[0064] In any embodiment, the first positive electrode active material includes a core and a shell covering the core, the core includes the compound represented by formula (I); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
[0065] By arranging a coating layer with ionic conductivity and / or electronic conductivity on the surface of the inner core, a first positive electrode active material with a core-shell structure is provided. Applying the first positive electrode active material to a battery can improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0066] In any embodiment, the one or more coating layers each independently include one or more selected from the group consisting of pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer.
[0067] In any embodiment, the shell comprises a coating layer; optionally, the coating layer comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.
[0068] The above materials can be used to obtain a coating layer with ionic conductivity and / or electronic conductivity, thereby improving the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0069] In any embodiment, the shell includes a first coating layer coating the core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer; more optionally, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide, and boride, and the second coating layer includes one or more selected from carbon and doped carbon. Using a first coating layer and a second coating layer of a specific material can further improve rate performance and further reduce the dissolution of Mn and Mn-site doping elements, thereby improving the battery's cycling performance and / or high-temperature stability.
[0070] In any embodiment, the shell includes a first coating layer coating the core, a second coating layer coating the first coating layer, and a third coating layer coating the second coating layer; optionally, the first coating layer, the second coating layer, and the third coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer; more optionally, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphate, oxide, and boride, and the third coating layer includes one or more selected from carbon and doped carbon. The use of a first coating layer of a specific material, a second coating layer of a specific material, and a third coating layer of a specific material further improves rate performance, further reduces the dissolution of Mn and Mn-site doping elements, thereby improving the cycle performance and / or high-temperature stability of the battery, and further increases the gram capacity and compaction density of the first positive electrode active material.
[0071] In any embodiment, the pyrophosphate is M b (P2O7) c ; and / or, the phosphate is X m (PO4) q and / or, the doping element in the doped carbon includes one or more elements selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or, the oxide is M' d O e ; and / or, the boride is Z v B w ; and / or, the polymer includes one or more elements selected from polysaccharides and their derivatives, polysiloxanes; M, X and Z each independently include one or more elements selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB, Group VIIB and Group VIII; b is selected from the range of 1 to 4; c is selected from the range of 1 to 6; m is selected from the range of 1 to 2; q is selected from the range of 1 to 4; M′ includes one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides and Sb; d is greater than 0 and less than or equal to 2; e is greater than 0 and less than or equal to 5; v is selected from the range of 1 to 7; w is selected from the range of 1 to 2.
[0072] By using the above materials as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, the gram capacity and compaction density of the first positive electrode active material can be further increased, and the battery's rate performance, high-temperature cycle performance and high-temperature storage performance can be further improved.
[0073] In any embodiment, M, X, and Z each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn, and Al.
[0074] In any embodiment, the doping element in the doped carbon includes one or more elements selected from nitrogen, phosphorus, sulfur, boron and fluorine.
[0075] In any embodiment, M′ includes one or more elements selected from Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La and Ce, and can optionally include one or more elements selected from Mg, Al, Si, Zn, Zr and Sn.
[0076] In any embodiment, the polysiloxane is selected from one or more of linear polysiloxanes and cyclic polysiloxanes.
[0077] In any embodiment, the polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.
[0078] By using the above-mentioned specific material as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, and the high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.
[0079] In any embodiment, the first positive electrode active material includes a core and a shell covering the core, wherein the core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and C includes one or more elements selected from B (boron), S, Si and N; the shell includes a first coating layer coating the core and a second coating layer coating the first coating layer, the first coating layer includes pyrophosphate MP2O7 and phosphate XPO4, M and X each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the second coating layer contains carbon.
[0080] In any embodiment, the first positive electrode active material includes a core and a shell covering the core, wherein the core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, C includes one or more elements selected from B (boron), S, Si and N; the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer and a third coating layer covering the second coating layer, the first coating layer includes pyrophosphate Li f QP2O7 and / or Q g (P2O7) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, the pyrophosphate Li f QP2O7 and / or Q g (P2O7) h wherein Q independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the second coating layer comprises crystalline phosphate XPO4, and X comprises one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; and the third coating layer comprises carbon.
[0081] By doping lithium manganese phosphate with specific elements and coating its surface, the dissolution of Mn during the lithium insertion and extraction process can be effectively reduced, while promoting the migration of lithium ions, thereby improving the battery's rate performance, cycle performance and high-temperature performance.
[0082] In any embodiment, the one or more coating layers in the shell that are furthest from the core each independently comprise one or more selected from polysiloxanes, polysaccharides, and polysaccharide derivatives. This improves coating uniformity and effectively blocks interfacial side reactions caused by high voltage, thereby enhancing the high-temperature cycling and storage performance of the first positive electrode active material. Furthermore, the coating layer has good ionic conductivity, contributing to an increase in the specific capacity of the first positive electrode active material while reducing heat generation in the battery.
[0083] In any embodiment, the polysiloxane comprises a structural unit represented by formula (i),
[0084] R1 and R2 are independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic and C2-C20 halogenated heteroaromatic; optionally, R1 and R2 are independently selected from H, amino, phosphate, polyether segment, C1-C8 alkyl, C1-C8 halogenated alkyl, C1-C8 heteroalkyl, C1-C8 halogenated heteroalkyl, C2-C8 alkenyl and C2-C8 halogenated alkenyl.
[0085] In any embodiment, the polysiloxane further comprises an end-capping group, wherein the end-capping group comprises one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.
[0086] In any embodiment, the polysiloxane comprises a polysiloxane selected from polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side chain aminopropyl polysiloxane. , aminopropyl-terminated polydimethylsiloxane, side chain phosphate grafted polydimethylsiloxane, side chain polyether grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, and one or more of cyclic polydimethylsiloxane.
[0087] In any embodiment, the number average molecular weight of the polysiloxane, the polysaccharide and the polysaccharide derivative is independently below 300,000, optionally 10,000 to 200,000, more optionally 20,000 to 120,000, further optionally 400 to 80,000.
[0088] In any embodiment, the mass percentage of the polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.
[0089] In any embodiment, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH and its salts, -R-OH, -SO3H and its salts, -R-OH, -R-SO3H and its salts, sulfate, alkoxy, R represents an alkylene group, optionally representing a C1 to C5 alkylene group; optionally, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO3H, -SO3Li, -SO3Na, -SO3K, -CH2-SO3H, -CH2-SO3Li, -CH2-SO3Na, -CH2-SO3K, methoxy, ethoxy.
[0090] In any embodiment, the polysaccharide comprises one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum and fenugreek gum.
[0091] In any embodiment, the weight percentage of the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivative is independently 20% to 85%, optionally 30% to 78%.
[0092] In any embodiment, the lattice mismatch between the core material and the shell material is less than 10%, thereby ensuring good contact between the core and the shell (or coating layer) to prevent the shell (or coating layer) from falling off.
[0093] In any embodiment, based on the total weight of the first positive electrode active material, the manganese content is in the range of 10 weight %-35 weight %, optionally in the range of 13.3 weight %-33.2 weight %, more optionally in the range of 15 weight %-30 weight %, and further optionally in the range of 17 weight %-20 weight %; and / or, the phosphorus content is in the range of 12 weight %-25 weight %, optionally in the range of 15 weight %-20 weight %, and more optionally in the range of 16.8 weight %-19.5 weight %; and / or, the weight ratio of manganese to phosphorus is in the range of 0.71-1.85, optionally in the range of 0.90-1.25, and more optionally in the range of 0.95-1.20.
[0094] Limiting the manganese content within the above range can further improve the stability and density of the first positive electrode active material, thereby improving the battery's cycling, storage, and compaction properties; and can maintain a higher voltage platform, thereby improving the battery's energy density.
[0095] Limiting the phosphorus content within the above range can effectively reduce the influence of small polaron conductivity on the conductivity of the first positive electrode active material, and can further improve the stability of the lattice structure, thereby enhancing the overall stability of the first positive electrode active material.
[0096] Limiting the weight ratio of manganese to phosphorus within the above range can further reduce manganese dissolution, improve the stability and gram capacity of the first positive electrode active material, and improve the cycle performance and storage performance of the battery; it can also reduce impurities, enable the first positive electrode active material to maintain a higher discharge voltage platform, and enable the battery to have a high energy density.
[0097] In any embodiment, the surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; optionally, the surface of the first positive electrode active material is coated with carbon, thereby improving the conductivity of the first positive electrode active material.
[0098] In any embodiment, the doping element in the doped carbon includes one or more elements selected from nitrogen, phosphorus, sulfur, boron and fluorine.
[0099] In any embodiment, the coating amount of the shell is 0.1 wt% to 6 wt%, based on the weight of the core.
[0100] In any embodiment, the coating amount of the first coating layer is greater than 0 and less than or equal to 7 weight%, optionally greater than 0 and less than or equal to 6 weight%, more optionally greater than 0 and less than or equal to 5.5 weight% or 4-5.6 weight%, further optionally greater than 0 and less than or equal to 2 weight%, based on the weight of the core; and / or, the coating amount of the second coating layer is greater than 0 and less than or equal to 6 weight%, optionally greater than 0 and less than or equal to 5.5 weight%, more optionally 2-4 weight% or 3-5 weight%, based on the weight of the core; and / or, the coating amount of the third coating layer is greater than 0 and less than or equal to 6 weight%, optionally greater than 0 and less than or equal to 5.5 weight%, more optionally greater than 0 and less than or equal to 2 weight%, based on the weight of the core.
[0101] In any embodiment, the shell further includes a fourth coating layer coating the third coating layer and a fifth coating layer coating the fourth coating layer; the coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 wt % to 10 wt %, optionally 0.05 wt % to 10 wt %, more optionally 0.1 wt % to 5 wt %, and further 0.1 wt % to 2 wt %, based on the weight of the core.
[0102] The coating amount of each coating layer is preferably within the above range, so that the core can be fully coated and the kinetic performance of the battery can be further improved without sacrificing the gram capacity of the first positive electrode active material.
[0103] In any embodiment, the shell is located on 40% to 90% of the surface of the core, and optionally 60% to 80% of the surface, thereby fully covering the core and improving the dynamic performance of the battery.
[0104] In any embodiment, the shell has a thickness of 1-15 nm.
[0105] In any embodiment, the thickness of the first cladding layer is 1-10nm, optionally 2-10nm; and / or the thickness of the second cladding layer is 2-25nm, optionally 2-15nm, more optionally 3-15nm; and / or the thickness of the third cladding layer is 2-25nm, optionally 5-25nm.
[0106] In any embodiment, the one or more coating layers independently include one or more selected from pyrophosphate, phosphate and oxide, and one or more selected from the pyrophosphate, phosphate and oxide is crystalline; optionally, the crystallinity of the pyrophosphate, the phosphate and the oxide is independently 10% to 100%, and more optionally 50% to 100%.
[0107] Pyrophosphate and phosphate with a certain degree of crystallinity are not only conducive to giving full play to the pyrophosphate coating layer's ability to reduce manganese dissolution and the phosphate coating layer's excellent lithium ion conductivity and the function of reducing interface side reactions, but also enable the pyrophosphate coating layer and the phosphate coating layer to better lattice match, thereby achieving a close bond between the coating layers.
[0108] In any embodiment, the weight ratio of the pyrophosphate to the phosphate and the weight ratio of the pyrophosphate to the oxide in the shell are each independently 1:3 to 3:1, and can be optionally 1:3 to 1:1. Thus, by having the pyrophosphate to the phosphate or the pyrophosphate to the oxide in a suitable weight ratio range, manganese dissolution can be effectively reduced, the surface impurity lithium content can be effectively reduced, and interfacial side reactions can be reduced, thereby improving the high-temperature storage performance and high-temperature cycling performance of the battery.
[0109] In any embodiment, the one or more coating layers each independently comprise carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon. Optionally, the molar ratio of the SP2 carbon to the SP3 carbon in the carbon is any value in the range of 0.07-13, more preferably any value in the range of 0.1-10, and further preferably any value in the range of 2.0-3.0. By selecting the carbon morphology in the carbon coating layer, the overall electrical performance of the battery can be improved.
[0110] In any embodiment, the one or more coating layers independently include doped carbon, and the weight content of the doping element in the doped carbon is less than 30%; alternatively, the weight content of the doping element in the doped carbon is less than 20%. The doping element within the above content range can not only fully improve the conductivity of the pure carbon layer, but also effectively avoid excessive surface activity caused by excessive doping of the doping element, thereby effectively controlling interfacial side reactions caused by excessive doping of the coating layer.
[0111] In any embodiment, the one or more coating layers independently include doped carbon, in which the doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or, the doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%; optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.
[0112] Since nitrogen atoms and sulfur atoms are closer in atomic radius to carbon atoms and are less likely to destroy the carbon skeleton, when the doping amount of nitrogen atoms and sulfur atoms is within the above relatively wide range, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transport and lithium ion desolvation capabilities can be promoted.
[0113] Since the atomic radius of phosphorus atoms, boron atoms and / or fluorine atoms is different from that of carbon atoms, excessive doping can easily destroy the carbon skeleton. Therefore, when the doping amount of phosphorus atoms, boron atoms and / or fluorine atoms is within the above-mentioned relatively small range, it can not only fully exert the conductivity of the doped carbon layer, but also promote lithium ion transmission and lithium ion desolvation capabilities.
[0114] In any embodiment, the one or more coating layers independently include pyrophosphate, the interplanar spacing of the pyrophosphate is in the range of 0.293-0.470nm, optionally 0.297-0.462nm or 0.293-0.326nm, more optionally 0.300-0.310nm, and the angle range of the crystal direction (111) is 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, and further optionally 29.00°-30.00°.
[0115] In any embodiment, the one or more coating layers independently include phosphate, the interplanar spacing of the phosphate is in the range of 0.244-0.425nm, optionally 0.345-0.358nm, and the angle of the crystal direction (111) is in the range of 20.00°-37.00°, optionally 24.25°-26.45°.
[0116] In this way, the impurity phase in the coating layer can be effectively reduced, thereby improving the material's specific capacity, cycle performance and rate performance.
[0117] In any embodiment, the first coating layer or the second coating layer comprises phosphate.
[0118] In any embodiment, the lattice change rate of the first positive electrode active material before and after complete lithium deintercalation is 50% or less, optionally 9.8% or less, more optionally 8.1% or less, further optionally 7.5% or less, further optionally 6% or less, further optionally 4% or less, further optionally 3.8% or less, and further optionally 2.0-3.8%. By reducing the lattice change rate, lithium ion transport can be facilitated, that is, the mobility of lithium ions in the first positive electrode active material is stronger, which is beneficial to improving the rate performance of the battery.
[0119] In any embodiment, the Li / Mn antisite defect concentration of the first positive electrode active material is 5.3% or less, optionally 5.1% or less, more optionally 4% or less, further optionally 2.2% or less, further optionally 2% or less, further optionally 1.5%-2.2% or 0.5% or less. By reducing the Li / Mn antisite defect concentration, the specific capacity and rate performance of the first positive electrode active material are improved.
[0120] In any embodiment, the surface oxygen valence state of the first positive electrode active material is -1.55 or less, optionally -1.82 or less, more optionally -1.88 or less, further optionally -1.90 or less, or -1.98 to -1.88, further optionally -1.98 to -1.89, and further optionally -1.98 to -1.90. By reducing the surface oxygen valence state, it is possible to reduce interfacial side reactions between the first positive electrode active material and the electrolyte, thereby improving the cycle performance and high-temperature stability of the battery.
[0121] In any embodiment, the positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045,w a represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition, y is the molar amount of element B in 1 mol of the compound represented by formula (I), V B is the voltage platform of the B element in the compound represented by formula (I), with the unit being V (volts). When the positive electrode active material composition further satisfies the above conditions, it is beneficial for the positive electrode sheet to achieve both high compaction density and high compaction density efficiency, and for the battery to achieve both high energy density and long service life.
[0122] In any embodiment, the second positive electrode active material comprises a layered oxide. By properly combining the first and second positive electrode active materials, the actual packing density of the positive electrode active material composition can be increased, as can the compaction density and compaction density efficiency of the positive electrode sheet. This can further enable batteries employing the positive electrode active material composition to have higher energy density and longer service life.
[0123] In any embodiment, the second positive electrode active material includes a compound represented by formula (II), Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 , (II)
[0124] A 1 including one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1including Mn and / or Al; C 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group VIA, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, and Group VIII; D 1 Includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.
[0125] In any embodiment, A 1 It includes one or more elements selected from Na, K, Mg, Rb, Zn, and Zr.
[0126] In any embodiment, C 1 It includes one or more elements selected from Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and can optionally include one or more elements selected from Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, B.
[0127] In any embodiment, D 1 The invention comprises one or more elements selected from N, S, F, Cl and Br, and may optionally comprise S and / or F.
[0128] In any embodiment, a1 is selected from the range of 0.9 to 1.1.
[0129] In any embodiment, b1 is selected from the range of 0 to 0.1.
[0130] In any embodiment, c1 is selected from the range of 0.314 to 0.990, and optionally selected from the range of 0.500 to 0.990.
[0131] In any embodiment, d1 is selected from the range of 0 to 0.320, and optionally selected from the range of 0 to 0.150.
[0132] In any embodiment, e1 is selected from the range of 0.001 to 0.450, and optionally selected from the range of 0.005 to 0.4.
[0133] In any embodiment, f1 is selected from the range of 0.001 to 0.1, and optionally selected from the range of 0.001 to 0.05.
[0134] In any embodiment, g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.05.
[0135] In any embodiment, the second positive electrode active material includes a core and a shell covering the core, the core includes the compound represented by formula (II); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
[0136] In any embodiment, in the shell of the second positive electrode active material, the one or more coating layers each independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.
[0137] In any embodiment, the shell of the second positive electrode active material includes a coating layer; optionally, the coating layer includes one or more selected from phosphate, pyrophosphate, and oxide.
[0138] In any embodiment, the shell of the second positive electrode active material includes a first coating layer coating the inner core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphates, pyrophosphates, and oxides; more optionally, the first coating layer includes one or more selected from phosphates and oxides, and the second coating layer includes one or more selected from pyrophosphates and oxides.
[0139] In any embodiment, the coating amount of the shell of the second positive electrode active material is 0.005 wt % to 1 wt %, optionally 0.01 wt % to 0.5 wt %, based on the weight of the core; and / or the thickness of the shell is 2 nm to 200 nm, optionally 5 nm to 50 nm.
[0140] The second aspect of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material, and the positive electrode active material comprising the positive electrode active material composition of the first aspect of the present application.
[0141] In any embodiment, the content of the positive electrode active material composition in the positive electrode film layer is 90 wt % to 99.5 wt %, more preferably 95 wt % to 99.5 wt %, based on the total weight of the positive electrode film layer.
[0142] In any embodiment, the positive electrode film layer further includes a third positive electrode active material, and the third positive electrode active material includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel-type lithium manganate material, and their respective modified compounds, and the modification methods include doping and / or surface coating modification.
[0143] In any embodiment, the third positive electrode active material includes a compound represented by formula (III), Li 1+p1 A 2 q1 B 2 r1 O s1 , (III)
[0144] 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 includes one or more elements selected from Co, Ni, Mn, and Al; B 2 includes one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.
[0145] In any embodiment, the third positive electrode active material includes a core and a shell coating the core, and the core includes the compound represented by formula (III); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity. <00005, (IV)
[0149] A 3 including one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB, and Group VIB; 3 including one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 including one or more elements selected from Group IIIA, Group IVA, Group VA, and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.5.
[0150] In any embodiment, A 3 Includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and can optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W.
[0151] In any embodiment, B 3 Includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can optionally include one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge.
[0152] In any embodiment, C 3 The present invention includes one or more elements selected from B (boron), S, Si and N.
[0153] In any embodiment, D 3 It includes one or more elements selected from S, F, Cl and Br.
[0154] In any embodiment, a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01.
[0155] In any embodiment, x2 is selected from the range of 0.001 to 0.005.
[0156] In any embodiment, y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5.
[0157] In any embodiment, z2 is selected from the range of 0.001 to 0.5, alternatively selected from the range of 0.001 to 0.1, more alternatively selected from the range of 0.001 to 0.005.
[0158] In any embodiment, n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.
[0159] In any embodiment, the third positive electrode active material includes a core and a shell covering the core, the core including the compound represented by formula (IV); and the shell is the same as the shell covering the compound represented by formula (I).
[0160] In any embodiment, the third positive electrode active material includes a compound represented by formula (V), LiMn t1 A 4 2-t1 O4, (V)
[0161] t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.
[0162] In any embodiment, the third positive electrode active material includes a core and a shell covering the core, the core includes the compound represented by formula (V); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
[0163] In any embodiment, the one or more coating layers in the shell coating the compound represented by formula (V) independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.
[0164] In any embodiment, the coating amount of the shell coating the compound represented by formula (V) is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core; and / or the thickness of the shell coating the compound represented by formula (V) is 2 nm to 200 nm, optionally 5 nm to 50 nm.
[0165] In any embodiment, the positive electrode film layer includes a positive electrode binder and / or a positive electrode conductor.
[0166] In any embodiment, the positive electrode binder includes vinylidene fluoride homopolymer and / or copolymer. More optionally, the comonomer includes one or more of tetrafluoroethylene, hexafluoropropylene, and propylene.
[0167] In any embodiment, the positive electrode binder has a weight average molecular weight of 300,000 to 2,000,000.
[0168] In any embodiment, the positive electrode film layer further includes functional additives, and the functional additives include one or more of a dispersant, a plasticizer, a pore former, a water removal additive, an acid removal additive, and a lithium supplement.
[0169] In any embodiment, the positive electrode plate further includes a functional coating, which is located between the positive electrode collector and the positive electrode film layer and / or on the surface of the positive electrode film layer facing away from the positive electrode collector, and the functional coating includes one or more of conductive carbon, a water removal additive, an acid removal additive, and a lithium supplement.
[0170] A third aspect of the present application provides a battery, comprising the positive electrode active material composition of the first aspect of the present application or the positive electrode plate of the second aspect of the present application.
[0171] In any embodiment, the battery includes an electrolyte, and the electrolyte includes one or more of a liquid electrolyte, an all-solid electrolyte, and a gel electrolyte.
[0172] In any embodiment, the liquid electrolyte includes a lithium salt, a non-aqueous solvent for dissolving the lithium salt, and optional additives; optionally, the lithium salt includes one or more selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2, LiBF2C2O4, and LiPO2F2.
[0173] In any embodiment, the concentration of the lithium salt is 0.5-1.5 mol / L.
[0174] In any embodiment, the non-aqueous solvent includes one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, cyclopentane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.
[0175] In any embodiment, the additive includes one or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, optionally including vinylene carbonate, 1,2,3-tris(2-cyanoethoxy)propane, 1-aza-12-crown 4-ether, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate. .
[0176] In any embodiment, the battery includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, the negative electrode film layer includes a negative electrode active material, and the negative electrode active material includes one or more of a carbon-based material, a silicon-based material, a tin-based material and lithium titanate; optionally, the negative electrode active material includes a carbon-based material, or a combination of a carbon-based material and a silicon-based material.
[0177] In any embodiment, the porosity of the negative electrode film layer is 20% to 50%.
[0178] In any embodiment, the negative electrode active material includes a carbon-based material, and the carbon-based material includes graphite, or a combination of graphite and hard carbon.
[0179] In any embodiment, the negative electrode active material includes a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of the silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.
[0180] In any embodiment, the negative electrode plate further includes a functional coating, which is located between the negative electrode collector and the negative electrode film layer and / or on the surface of the negative electrode film layer facing away from the negative electrode collector; optionally, the functional coating includes carbon.
[0181] In any embodiment, the negative electrode film layer further includes a lithium replenishing material. Optionally, the lithium replenishing material includes one or more of lithium foil, lithium ribbon, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent includes one or more of Li-aromatic hydrocarbons, complexes of Li-aromatic hydrocarbons and ether solvents, and more optionally includes one or more of lithium naphthalene and lithium biphenyl-dimethyl ether.
[0182] In any embodiment, the negative electrode plate includes a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer respectively arranged on two surfaces of the negative electrode current collector. Optionally, the thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:5.
[0183] In any embodiment, the battery includes a negative electrode sheet, and the negative electrode sheet does not include a negative electrode active material capable of inserting and extracting lithium ions.
[0184] In any embodiment, the negative electrode plate includes a lithium plate or a lithium alloy plate.
[0185] In any embodiment, the negative electrode sheet includes a mesh or foam three-dimensional skeleton layer.
[0186] In any embodiment, the battery includes a separator comprising a porous substrate.
[0187] In any embodiment, the isolation membrane further comprises a coating located on at least one surface of the porous substrate. Optionally, the coating comprises one or more of inorganic heat-resistant particles and organic heat-resistant particles.
[0188] In any embodiment, the isolation membrane has a porosity of 10%-40%.
[0189] A fourth aspect of the present application provides an electrical device comprising the battery of the third aspect of the present application.
[0190] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0191] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0192] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0193] FIG2 is an exploded schematic diagram of an embodiment of a battery cell of the present application.
[0194] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0195] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0196] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .
[0197] FIG6 is a schematic diagram of an embodiment of an electric device including the battery of the present application as a power source.
[0198] FIG. 7 is a particle size distribution curve of the positive electrode active material composition of Example 11. FIG.
[0199] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 battery cell, 51 housing, 52 electrode assembly, 53 cover plate. DETAILED DESCRIPTION
[0200] Below, with appropriate reference to the accompanying drawings, the embodiments of the positive electrode active material composition, positive electrode sheet, battery, and electrical device of the present application are described in detail. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0201] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0202] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0203] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0204] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0205] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0206] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0207] Unless otherwise specified, in this application, the terms "first", "second", "third", "fourth", "fifth", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.
[0208] In this application, the terms "plurality" and "multiple" refer to two or more.
[0209] Throughout this specification, substituents of compounds are disclosed in groups or ranges. It is expressly intended that such descriptions include each individual subcombination of the members of these groups and ranges. For example, it is expressly intended that the term "C1-C6 alkyl" individually discloses C1, C2, C3, C4, C5, C6, C1-C6, C1-C5, C1-C4, C1-C3, C1-C2, C2-C6, C2-C5, C2-C4, C2-C3, C3-C6, C3-C5, C3-C4, C4-C6, C4-C5, and C5-C6 alkyl.
[0210] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0211] Unless otherwise stated, the values of the various parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise stated, the test temperature of each parameter is 25°C.
[0212] Unless otherwise specified, all ratio parameters mentioned in this application are compared in the same units. For example, the ratio of the volume distribution particle sizes of A and B is 1:1, and the units of the volume distribution particle sizes of A and B are the same.
[0213] In this application, the term "compaction density efficiency" refers to the ratio of the compaction density of the membrane layer to the theoretical compaction density of the active material powder.
[0214] In the present application, the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material can be tested for element content using inductively coupled plasma emission spectroscopy (ICP).
[0215] The battery mentioned in the embodiments of this application refers to a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application may include a battery cell, a battery module or a battery pack.
[0216] A battery cell is the smallest unit of a battery, independently capable of charging and discharging. A battery cell can be cylindrical, flat, rectangular, or in other shapes, though this is not a limitation in the present invention. Figure 1 shows a battery cell 5 with a rectangular structure as an example.
[0217] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed series via a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed in the housing. In some embodiments, the housing may serve as part of the vehicle's chassis structure. For example, a portion of the housing may form at least a portion of the vehicle's floor, or a portion of the housing may form at least a portion of the vehicle's crossbeam or longitudinal beam.
[0218] In some embodiments, the battery may be an energy storage device, including an energy storage container, an energy storage cabinet, and the like.
[0219] The battery cells mentioned in the embodiments of the present application include lithium-ion primary battery cells, lithium-ion secondary battery cells, lithium metal battery cells, negative electrode-free lithium metal battery cells, etc., which are not limited in the embodiments of the present application.
[0220] A battery cell generally includes an electrode assembly. The electrode assembly generally includes a positive electrode sheet, a negative electrode sheet, and a separator located between the positive and negative electrode sheets. The electrode assembly can be a wound structure or a laminated structure, which is not limited in the present embodiment.
[0221] The battery cell may also include an outer packaging that can be used to encapsulate the electrode assembly and electrolyte. The outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0222] In some embodiments, as shown in Figure 2, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening, thereby sealing the receiving cavity. The electrode assembly 52 is enclosed in the receiving cavity. The number of electrode assemblies 52 contained in a battery cell 5 can be one or more, and can be adjusted according to needs.
[0223] In some embodiments, battery cells can be assembled into a battery module. The number of battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 is a schematic diagram of a battery module 4 as an example. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged in sequence along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.
[0224] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0225] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0226] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The housing comprises an upper housing 2 and a lower housing 3. The upper housing 2 covers the lower housing 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the housing.
[0227] The positive electrode sheet contains the positive electrode active material. As an important component of the battery, the performance of the positive electrode active material is a major factor that affects the battery's energy density and service life. Currently, no positive electrode active material has been developed that can simultaneously meet the requirements of low cost, high capacity, and low side reactions.
[0228] In view of this, the inventors have proposed a positive electrode active material composition, which can enable a battery to have high energy density, low cost and good service life.
[0229] The positive electrode active material composition provided in the embodiments of the present application includes a first positive electrode active material and a second positive electrode active material having a different crystal form from the first positive electrode active material, wherein the first positive electrode active material includes a phosphate. The different crystal forms of the first and second positive electrode active materials refer to the first and second positive electrode active materials having different crystal systems.
[0230] The particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50. "||" represents an absolute value.
[0231] The first positive electrode active material includes phosphate, which is usually an olivine structure and generally has a low production cost. However, the compaction density of the first positive electrode active material is relatively low, making it difficult to meet the requirements of high energy density batteries. Combining it with another positive electrode active material with a high compaction density can increase the compaction density of the positive electrode sheet. However, simply mixing the two positive electrode active materials generally does not improve the compaction density and compaction density efficiency of the positive electrode sheet, making it difficult to fully utilize the battery capacity and also affecting the battery life.
[0232] The inventors have found that by making the positive electrode active material composition include a first positive electrode active material and a second positive electrode active material with different crystal forms, and making the particle size distribution curve of the positive electrode active material composition satisfy 0<|Dv1-Dv2| / Dv1≤50, the first positive electrode active material and the second positive electrode active material can be tightly stacked, thereby improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and further enabling the battery using the positive electrode active material composition to have a higher energy density and a longer service life.
[0233] The particle size distribution curve of the positive electrode active material composition can be adjusted by adjusting one or more parameters such as the volume distribution particle size, volume particle size distribution width, and mass content of each of the first positive electrode active material and the second positive electrode active material.
[0234] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm.
[0235] In some embodiments, the volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.
[0236] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:
[0237] 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or,
[0238] 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or,
[0239] 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.
[0240] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thus enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.
[0241] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:
[0242] 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or,
[0243] 2.0 μm≤Dv1≤12.5 μm, optionally, 3.0 μm≤Dv1≤12.3 μm; and / or,
[0244] 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.
[0245] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thus enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.
[0246] In some embodiments, the morphology of the first cathode active material includes one or more of single crystal and polycrystalline, and the morphology of the second cathode active material includes one or more of single crystal and polycrystalline.
[0247] The term "single crystal" also includes quasi-single crystals (also known as single-crystal-like particles), which generally refer to particles formed by the aggregation of a small number of primary particles. Polycrystalline particles refer to secondary particles formed by the aggregation of multiple primary particles.
[0248] In some embodiments, the volume distribution particle size Dv50 of the single-crystal first positive electrode active material is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm.
[0249] In some embodiments, the volume distribution particle size Dv10 of the single-crystal first positive electrode active material is 0.05 μm to 1.5 μm, and optionally 0.1 μm to 1.0 μm.
[0250] In some embodiments, the volume distribution particle size Dv50 of the polycrystalline first positive electrode active material is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm.
[0251] In some embodiments, the volume distribution particle size Dv10 of the polycrystalline first positive electrode active material is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm.
[0252] In some embodiments, the volume distribution particle size Dv50 of the single-crystal second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm.
[0253] In some embodiments, the volume distribution particle size Dv10 of the single-crystal second positive electrode active material is 0.3 μm to 8 μm, and optionally 1.0 μm to 3.5 μm.
[0254] In some embodiments, the volume distribution particle size Dv50 of the polycrystalline second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 15.5 μm.
[0255] In some embodiments, the volume distribution particle size Dv10 of the polycrystalline second positive electrode active material is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.
[0256] When the volume distribution particle size of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density, reduce side reactions, lower interface impedance, and extend the battery life.
[0257] In some embodiments, the first cathode active material comprises a single crystal morphology, for example, the single crystals may account for greater than 80% or greater than 90%. Polycrystalline first cathode active materials with a higher specific surface area may increase hygroscopicity and process time during production, thereby increasing battery production costs.
[0258] In some embodiments, the second cathode active material comprises a polycrystalline morphology, for example, the polycrystalline morphology may account for more than 80% or more than 90%. The polycrystalline second cathode active material can have a larger particle size and a higher powder compaction density, thereby helping to improve the energy density of the battery.
[0259] In some embodiments, the weight content of the first positive electrode active material is expressed as w based on the total weight of the positive electrode active material composition. a , then w a Selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%.
[0260] In some embodiments, the weight content of the second positive electrode active material is expressed as w based on the total weight of the positive electrode active material composition. b , then w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.
[0261] When the content of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density and / or a longer service life.
[0262] In some embodiments, the powder compaction density P1 of the first positive electrode active material at 30000N is 1.89 g / cm 3 Above, 1.95g / cm2 is optional 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 the following.
[0263] In some embodiments, the powder compaction density P2 of the second positive electrode active material at 30000N is greater than or equal to 2.90 g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3g / cm 3 .
[0264] When the powder compaction density of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density.
[0265] In some embodiments, the BET specific surface area of the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be less than or equal to 1.5m 2 / g, 0.28m can be selected 2 / g to 1.5m 2 / g. This can reduce side reactions and improve the cycle performance of the battery.
[0266] The specific surface area of a material is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using the nitrogen adsorption specific surface area analysis method in accordance with GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The testing instrument can be a Tri-Star 3020 Specific Surface Area Pore Size Analyzer from Micromeritics, Inc., USA.
[0267] The powder compaction density of the material (eg, the first positive electrode active material, the second positive electrode active material, etc.) can be measured according to GB / T 24533-2009.
[0268] The volume distribution particle sizes Dv10 and Dv50 of materials (e.g., the first positive electrode active material, the second positive electrode active material, etc.) have well-known meanings in the art and represent the particle sizes corresponding to 10% and 50% of the cumulative volume distribution percentage of the material, respectively. They can be measured using instruments and methods known in the art. For example, they can be measured using a laser particle size analyzer with reference to GB / T 19077-2016. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK. Deionized water can be used as the solvent for the test, and the material can be ultrasonically treated for 5 minutes before testing.
[0269] The particle size distribution curve of the positive electrode active material composition can be measured with reference to GB / T 19077-2016 using a laser particle size analyzer. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK. Deionized water can be used as the solvent for testing, and the material can be ultrasonically treated for 5 minutes before testing.
[0270] In some embodiments, the first cathode active material includes a compound represented by formula (I), Li a A x Mn 1-y B y P 1-z C z O 4-n D n (I)
[0271] A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB and Group VIII; C includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; n is selected from the range of 0 to 0.5.
[0272] Unless otherwise specified, in the above chemical formula, when A is two or more elements, the above-mentioned numerical range for x is not only a limit on the stoichiometric number of each element serving as A, but also a limit on the sum of the stoichiometric numbers of each element serving as A. For example, when A is two or more elements A1, A2, ..., An, the stoichiometric numbers x1, x2, ..., xn of A1, A2, ..., An must each fall within the numerical range for x specified in this application, and the sum of x1, x2, ..., xn must also fall within this numerical range.
[0273] Similarly, for other symbols mentioned in the embodiments of this application (such as B, C, D, M, M', X, Z, P, Q, A 1 、B 1 、C 1 、D 1 、A 2 、B 2 、A 3 、A 4 When two or more elements are present, the numerical range of the stoichiometric number thereof in the present application also has the above meaning.
[0274] The first positive electrode active material is obtained by doping elements in the compound LiMnPO4, wherein A, B, C and D are elements doped at the Li, Mn, P and O positions of the compound LiMnPO4, respectively. Without wishing to be bound by theory, it is now believed that the performance improvement of lithium manganese phosphate is related to reducing the lattice change rate of lithium manganese phosphate during lithium insertion and extraction and reducing surface activity. Reducing the lattice change rate can reduce the lattice constant difference between the two phases at the grain boundary, reduce the interfacial stress, and enhance the Li +The transport capacity at the interface improves the rate performance of the first positive electrode active material. However, high surface activity can easily lead to serious side reactions at the interface, exacerbating gas production, electrolyte consumption and interface damage, thereby affecting the cycle performance of the battery. The lattice change rate can be reduced by doping with Li and / or Mn. Mn doping can also effectively reduce surface activity, thereby reducing Mn dissolution and side reactions at the interface between the first positive electrode active material and the electrolyte. P-site doping makes the change rate of the Mn-O bond length faster, reduces the migration barrier of the small polaron of the material, and is beneficial to improve the electronic conductivity. O-site doping has a good effect on reducing side reactions at the interface. P-site and / or O-site doping also affects the Mn dissolution and kinetic properties of antisite defects. Therefore, doping reduces the concentration of antisite defects in the material, improves the kinetic properties and specific capacity of the material, and can also change the morphology of the particles, thereby improving the compaction density. The inventors unexpectedly discovered that by doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping element at the Mn position, obtaining improved cycle performance and / or high-temperature stability, and the gram capacity and compaction density of the material are also improved.
[0275] In some embodiments, A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo, and W, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; and / or
[0276] B comprises one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and may optionally comprise one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge; and / or
[0277] C includes one or more elements selected from B (boron), S, Si and N; and / or,
[0278] D includes one or more elements selected from S, F, Cl and Br.
[0279] In some embodiments, A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, and may optionally include any one element selected from Mg and Nb; and / or
[0280] B comprises one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may optionally comprise at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may further optionally comprise at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and may further optionally comprise at least two elements selected from Fe, Ti, V, Co and Mg, and may further optionally comprise Fe and one or more elements selected from Ti, V, Co and Mg; and / or
[0281] C includes any one element selected from B (boron), S, Si and N, and may be S; and / or,
[0282] D includes any one element selected from S, F, Cl and Br, and may be F.
[0283] By selecting the Li-position doping element within the above range, the lattice change rate during the delithiation process can be further reduced, thereby further improving the rate performance of the battery. By selecting the Mn-position doping element within the above range, the electronic conductivity can be further improved and the lattice change rate can be further reduced, thereby improving the rate performance and gram capacity of the battery. By selecting the P-position doping element within the above range, the rate performance of the battery can be further improved. By selecting the O-position doping element within the above range, the side reactions at the interface can be further reduced, thereby improving the high-temperature performance of the battery.
[0284] In some embodiments, a is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or,
[0285] x is selected from the range of 0.001 to 0.005; and / or,
[0286] y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or,
[0287] z is selected from the range of 0.001 to 0.5, alternatively selected from the range of 0.001 to 0.1, more alternatively selected from the range of 0.001 to 0.005; and / or,
[0288] n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.
[0289] By selecting the value of y within the above range, the gram capacity and rate performance of the first positive electrode active material can be further improved. By selecting the value of x within the above range, the kinetic performance of the first positive electrode active material can be further improved. By selecting the value of z within the above range, the rate performance of the battery can be further improved. By selecting the value of n within the above range, the high-temperature performance of the battery can be further improved.
[0290] In some embodiments, x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is 0, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0.
[0291] Thus, by doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, especially doping a specific element in a specific amount at the Mn position and P position of LiMnPO4 or at the Li position, Mn position, P position and O position of LiMnPO4, the rate performance can be improved, the dissolution of Mn and the doping element at the Mn position can be reduced, the cycle performance and / or high temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.
[0292] In some embodiments, y:z is selected from the range of 0.002 to 999, optionally from the range of 0.025 to 999 or from the range of 0.002 to 500, and more optionally from the range of 0.2 to 600, such as 0.2, 0.25, 1, 2, 3, 4, 5, 6, 8, 10, 12, 13, 15, 17, 20, 70, 80, 84, 67, 91, 100, 134, 150, 182, 200, 250, 300, 320, 350, 400, 420, 450, 500, 600, 999, or a range consisting of any two of the above values. Thus, the defects of the first positive electrode active material can be reduced, the integrity of the framework structure of the first positive electrode active material can be improved, thereby effectively improving the structural stability of the first positive electrode active material, and further improving the cycle stability of the battery.
[0293] In some embodiments, z:n is selected from the range of 0.002 to 500, optionally from the range of 0.2 to 100, and more optionally from the range of 0.2 to 50, such as 0.2, 0.8, 1, 1.25, 4, 5, 50, or a range consisting of any two of the foregoing values. This can further reduce defects in the first positive electrode active material, further improve the integrity of the framework structure of the first positive electrode active material, effectively enhance the structural stability of the first positive electrode active material, and improve the cycling stability of the battery.
[0294] In some embodiments, (1-y):y is in the range of 0.1-999, optionally in the range of 0.1-10 or in the range of 0.67-999, more optionally in the range of 1 to 10, further optionally in the range of 1 to 4, and further optionally in the range of 1.5 to 3; and / or, a:x is in the range of 1 to 1200, optionally in the range of 9 to 1100, and more optionally in the range of 190-998.
[0295] Here, y represents the sum of the stoichiometric numbers of the doping elements at the Mn site. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.
[0296] In some embodiments, z:(1-z) is 1:9 to 1:999, and can be 1:499 to 1:249. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.
[0297] In some embodiments, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.1.
[0298] By doping specific elements in specific amounts at the Li, Mn, P, and O positions of the compound LiMnPO4 simultaneously, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping elements at the Mn position, thereby obtaining improved cycle performance and / or high-temperature stability, and the gram capacity and compaction density of the first positive electrode active material can also be improved.
[0299] In some embodiments, B includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include one or more elements selected from Zn, Fe, Ti, V, Ni, Co and Mg; C includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.
[0300] By doping specific elements at specific amounts at both the Mn and P sites of the LiMnPO4 compound, rate performance can be improved, the dissolution of Mn and the doping element at the Mn site can be reduced, the cycle performance and / or high-temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.
[0301] In some embodiments, the first positive electrode active material includes a core and a shell coating the core, wherein the core includes a compound represented by formula (I) above. The shell includes one or more coating layers. Each coating layer has ionic conductivity and / or electronic conductivity. In practice, each coating layer may be fully or partially coated.
[0302] By arranging a coating layer with ionic conductivity and / or electronic conductivity on the surface of the inner core, a first positive electrode active material with a core-shell structure is provided. Applying the first positive electrode active material to a battery can improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0303] In some embodiments, the one or more coating layers each independently comprise one or more selected from the group consisting of pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer.
[0304] In some embodiments, the shell comprises a coating; optionally, the coating comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer.
[0305] The above materials can be used to obtain a coating layer with ionic conductivity and / or electronic conductivity, thereby improving the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0306] In some embodiments, the shell includes a first coating layer coating the core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.
[0307] Using the above materials as the materials for the coating layer and providing two coating layers can further improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0308] In some embodiments, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide, and boride, and the second coating layer includes one or more selected from carbon and doped carbon.
[0309] The use of a first coating layer of a specific material and a second coating layer of a specific material can further improve rate performance and further reduce the dissolution of Mn and Mn-doping elements, thereby improving the cycle performance and / or high-temperature stability of the battery.
[0310] In some embodiments, the shell includes a first coating layer encapsulating the core, a second coating layer encapsulating the first coating layer, and a third coating layer encapsulating the second coating layer. Optionally, the first coating layer, the second coating layer, and the third coating layer each independently comprise one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer. The "polymer" can be either an oligomer or a polymer, and this is not limited in the present embodiment.
[0311] Using the above materials as the coating layer material and providing three coating layers can further reduce the dissolution of Mn and Mn-doping elements, and further improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.
[0312] In some embodiments, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphates, oxides, and borides, and the third coating layer includes one or more selected from carbon and doped carbon.
[0313] The use of a first coating layer of a specific material, a second coating layer of a specific material, and a third coating layer of a specific material further improves the rate performance, further reduces the dissolution of Mn and Mn-doping elements, thereby improving the cycle performance and / or high-temperature stability of the battery, and further increases the gram capacity and compaction density of the first positive electrode active material.
[0314] In some embodiments, the pyrophosphate is b (P2O7) c and / or,
[0315] Phosphate is X m (PO4) q and / or,
[0316] The doping element in the doped carbon includes one or more elements selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or,
[0317] Oxide is M'd O e and / or,
[0318] Boride is Z v B w and / or,
[0319] The polymer includes one or more selected from polysaccharides and their derivatives, and polysiloxanes;
[0320] M, X, and Z each independently comprise one or more elements selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB, Group VIIB, and Group VIII;
[0321] b is selected from the range of 1 to 4, c is selected from the range of 1 to 6; m is selected from the range of 1 to 2, q is selected from the range of 1 to 4;
[0322] M′ comprises one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides, and Sb;
[0323] d is greater than 0 and less than or equal to 2, e is greater than 0 and less than or equal to 5;
[0324] v is selected from the range of 1 to 7, and w is selected from the range of 1 to 2.
[0325] By using the above materials as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, the gram capacity and compaction density of the first positive electrode active material can be further increased, and the battery's rate performance, high-temperature cycle performance and high-temperature storage performance can be further improved.
[0326] In some embodiments, M, X, and Z each independently comprise one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn, and Al; and / or,
[0327] The doping element in the doped carbon includes one or more elements selected from nitrogen, phosphorus, sulfur, boron and fluorine; and / or,
[0328] M′ comprises one or more elements selected from the group consisting of Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La, and Ce, and may optionally comprise one or more elements selected from the group consisting of Mg, Al, Si, Zn, Zr, and Sn; and / or
[0329] The polysiloxane is selected from one or more of linear polysiloxanes and cyclic polysiloxanes; and / or,
[0330] The polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.
[0331] By using the above-mentioned specific material as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, and the high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.
[0332] In some embodiments, the first positive active material includes a core and a shell covering the core.
[0333] The core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and C includes one or more elements selected from B (boron), S, Si and N.
[0334] The shell includes a first coating layer coating the core and a second coating layer coating the first coating layer, the first coating layer includes pyrophosphate MP2O7 and phosphate XPO4, M and X each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the second coating layer contains carbon.
[0335] The first positive electrode active material can have a core-shell structure with two coating layers. The element B doped at the manganese position of the lithium manganese phosphate helps reduce the rate of lattice change during lithium insertion and extraction, improving the structural stability of the first positive electrode active material, significantly reducing manganese dissolution, and lowering oxygen activity on the particle surface. The element C doped at the phosphorus position helps modify the ease of change in the Mn-O bond length, thereby lowering the lithium ion migration barrier, promoting lithium ion migration, and improving the battery's rate performance. The first coating layer of the first positive electrode active material includes pyrophosphate and phosphate. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1 eV), it can effectively reduce transition metal dissolution. Phosphate has excellent lithium ion conductivity and can reduce the surface impurity lithium content. Furthermore, the second coating layer, which contains carbon, effectively improves the conductivity and desolvation ability of the LiMnPO4. Furthermore, the "barrier" effect of the second coating layer further reduces the migration of manganese ions into the electrolyte and reduces electrolyte corrosion of the second active material. Therefore, by doping lithium manganese phosphate with specific elements and surface coating, the dissolution of Mn during the lithium insertion and extraction process can be effectively reduced, while promoting the migration of lithium ions, thereby improving the battery's rate performance, cycle performance and high-temperature performance.
[0336] In some embodiments, the first positive active material includes a core and a shell covering the core.
[0337] The core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and C includes one or more elements selected from B (boron), S, Si and N.
[0338] The shell includes a first covering layer covering the inner core, a second covering layer covering the first covering layer, and a third covering layer covering the second covering layer.
[0339] The first coating layer includes Li pyrophosphate f QP2O7 and / or Q g (P2O7) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, pyrophosphate Li f QP2O7 and / or Q g (P2O7) h Each Q in the above-mentioned ions independently comprises one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al.
[0340] The second coating layer includes crystalline phosphate XP04, where X includes one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al.
[0341] The third coating layer includes carbon.
[0342] The first positive electrode active material is a core-shell structure, in which the manganese site and phosphorus site of the inner core are doped with elements B and C respectively, which can not only effectively reduce the dissolution of manganese, thereby reducing the manganese ions migrating to the negative electrode, reducing the electrolyte consumed due to the decomposition of the SEI film, and improving the cycle performance of the battery, but also promote the adjustment of the Mn-O bond, reduce the lithium ion migration barrier, promote lithium ion migration, and improve the battery's rate performance; by coating the inner core with a first coating layer including pyrophosphate, the migration resistance of manganese can be further increased, its dissolution can be reduced, and the surface impurity lithium content and the contact between the inner core and the electrolyte can be reduced, thereby reducing interfacial side reactions, reducing gas production, and improving the high-temperature storage performance and cycle performance of the battery; by further coating with a phosphate coating layer having excellent lithium ion conductivity, the interfacial side reactions on the surface of the first positive electrode active material can be effectively reduced, thereby improving the high-temperature cycle and storage performance of the battery; by further coating with a carbon layer as a third coating layer, the battery's kinetic performance can be further improved. In addition, in the core, the element B doped at the manganese position also helps to reduce the lattice change rate of lithium manganese phosphate during the lithium insertion and extraction process of the material, improves the structural stability of the first positive electrode active material, greatly reduces the dissolution of manganese and reduces the oxygen activity on the surface of the particles; the element C doped at the phosphorus position also helps to change the difficulty of the Mn-O bond length change, thereby improving the electronic conductivity and reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the battery's rate performance.
[0343] Furthermore, maintaining electrical neutrality throughout the core system minimizes defects and impurities in the first cathode active material. If the first cathode active material contains an excess transition metal (e.g., manganese), due to the inherently stable structure of the material system, the excess transition metal is likely to precipitate as a single element or form impurities within the crystal lattice. Maintaining electrical neutrality minimizes these impurities. Furthermore, maintaining electrical neutrality can, in some cases, create lithium vacancies within the material, thereby enhancing the kinetic performance of the first cathode active material.
[0344] In some embodiments, the one or more coating layers in the shell that are farthest from the core each independently comprise one or more selected from polysiloxanes, polysaccharides, and polysaccharide derivatives.
[0345] As a result, the uniformity of the coating can be improved, and the interfacial side reactions caused by high voltage can be effectively blocked, thereby improving the high-temperature cycle performance and high-temperature storage performance of the first positive electrode active material; and the coating layer has good ionic conductivity, which helps to improve the gram capacity of the first positive electrode active material while reducing the heat generation of the battery.
[0346] In some embodiments, the polysiloxane comprises a structural unit represented by the following formula (i):
[0347] R1 and R2 are independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic, and C2-C20 halogenated heteroaromatic;
[0348] Optionally, R1 and R2 are independently selected from H, amino, phosphate, polyether segment, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl and C2-C8 haloalkenyl.
[0349] In some embodiments, the polysiloxane further comprises an end-capping group, which includes one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.
[0350] In some embodiments, the polysiloxane comprises a polysiloxane selected from polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side chain aminopropyl polysiloxane, One or more of aminopropyl-terminated polydimethylsiloxane, side chain phosphate-grafted polydimethylsiloxane, side chain polyether-grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentasiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, and cyclic polydimethylsiloxane.
[0351] In some embodiments, the number average molecular weight of polysiloxane, polysaccharide, and polysaccharide derivative is independently less than 300,000, optionally 10,000 to 200,000, more optionally 20,000 to 120,000, and further optionally 400 to 80,000.
[0352] The number average molecular weight of polysiloxane, polysaccharide and polysaccharide derivatives can be measured by methods known in the art, such as gel permeation chromatography (GPC), using a PL-GPC 220 high temperature gel permeation chromatograph.
[0353] In some embodiments, the mass percentage of polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.
[0354] The "mass percentage of polar functional groups in the polysiloxane" refers to the mass proportion of polar functional groups in R1, R2, and end-capping groups in the polysiloxane. Polar functional groups include one or more of -COOH, -OH, -SH, -CN, -SCN, amino groups (including -NH2 and -NH-), phosphate groups, carboxylate groups (-COO-), amide groups (-CONH-), aldehyde groups (-CHO), sulfonyl groups (-S(=O)2-), polyether segments, halogen groups, alkoxy groups, and epoxy groups. When the aforementioned polar functional groups are directly attached to silicon atoms, α represents the mass fraction of these polar functional groups in the polysiloxane. When the aforementioned polar functional groups are not directly attached to silicon atoms, α represents the sum of the mass fractions of the polar functional groups and the divalent to tetravalent methyl groups (e.g., -CH2, -CH-, -C-, etc.) directly attached to them in the polysiloxane. Here, "divalent to tetravalent methyl groups" refers to the carbon atoms directly attached to the polar functional groups and located between the polar functional groups and the silicon atoms, as well as other non-polar functional groups attached to the carbon atoms. For example, in polymethyltrifluoropropylsiloxane, α refers to the mass percentage of -CF3, excluding the ethylene group; in polymethylchloropropylsiloxane, α refers to the mass percentage of -CH2Cl, excluding the ethylene group; in hydroxypropyl-terminated polydimethylsiloxane, α refers to the mass percentage of -CH2OH. The mass percentage of the polar functional groups in the polysiloxane can be determined by methods known in the art, such as titration (eg, acid-base titration, redox titration, precipitation titration), infrared spectroscopy, and nuclear magnetic resonance spectroscopy.
[0355] In some embodiments, the substituents attached to the sugar units in the polysaccharides and polysaccharide derivatives independently include one or more of the group consisting of the following functional groups: -OH, -COOH and its salts, -R-OH, -SO3H and its salts, -R-OH, -R-SO3H and its salts, sulfate, alkoxy, R represents an alkylene group, optionally representing a C1 to C5 alkylene group.
[0356] Optionally, the substituents attached to the sugar units in the polysaccharide and polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO3H, -SO3Li, -SO3Na, -SO3K, -CH2-SO3H, -CH2-SO3Li, -CH2-SO3Na, -CH2-SO3K, methoxy, ethoxy.
[0357] The term "substituents attached to the sugar unit" includes all groups attached to the sugar unit backbone.
[0358] In some embodiments, the polysaccharide comprises one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum, and fenugreek gum.
[0359] In some embodiments, the weight percentage of substituents attached to the sugar units in the polysaccharide and polysaccharide derivatives is independently 20% to 85%, and optionally 30% to 78%. The weight percentage of substituents attached to the sugar units in the polysaccharide and polysaccharide derivatives can be determined by methods known in the art, such as titration (e.g., acid-base titration, redox titration, precipitation titration), infrared spectroscopy, and nuclear magnetic resonance spectroscopy.
[0360] In some embodiments, the lattice mismatch between the core material and the shell material is less than 10%, thereby enabling good contact between the core and the shell (or coating) to prevent the shell (or coating) from falling off.
[0361] In some embodiments, based on the weight of the positive electrode active material,
[0362] The manganese content is in the range of 10 wt% to 35 wt%, optionally in the range of 13.3 wt% to 33.2 wt%, more optionally in the range of 15 wt% to 30 wt%, further optionally in the range of 17 wt% to 20 wt%; and / or,
[0363] The phosphorus content is in the range of 12 wt% to 25 wt%, optionally in the range of 15 wt% to 20 wt%, and more optionally in the range of 16.8 wt% to 19.5 wt%; and / or,
[0364] The weight ratio of manganese element to phosphorus element ranges from 0.71 to 1.85, optionally from 0.90 to 1.25, and more preferably from 0.95 to 1.20.
[0365] In the case where manganese is contained only in the core of the first positive active material, the content of manganese may correspond to that of the core.
[0366] Limiting the manganese content within the above range can further improve the stability and density of the first positive electrode active material, thereby improving the battery's cycling, storage, and compaction properties; and can maintain a higher voltage platform, thereby improving the battery's energy density.
[0367] Limiting the phosphorus content within the above range can effectively reduce the influence of small polaron conductivity on the conductivity of the first positive electrode active material, and can further improve the stability of the lattice structure, thereby enhancing the overall stability of the first positive electrode active material.
[0368] Limiting the weight ratio of manganese to phosphorus within the above range can further reduce manganese dissolution, improve the stability and gram capacity of the first positive electrode active material, and improve the cycle performance and storage performance of the battery; it can also reduce impurities, enable the first positive electrode active material to maintain a higher discharge voltage platform, and enable the battery to have a high energy density.
[0369] Manganese and phosphorus can be measured using conventional techniques in the art. Specifically, the following method is used to determine the manganese and phosphorus contents: the material is dissolved in dilute hydrochloric acid (concentration 10-30%), the content of each element in the solution is measured using ICP, and then the manganese content is measured and converted to obtain its weight percentage.
[0370] In some embodiments, the surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; alternatively, the surface of the first positive electrode active material is coated with carbon, thereby improving the conductivity of the first positive electrode active material.
[0371] In some embodiments, the doping element in the doped carbon layer includes one or more elements selected from nitrogen, phosphorus, sulfur, boron, and fluorine, so as to facilitate control of the properties of the doped carbon layer.
[0372] In some embodiments, the coating amount of the shell (which is only one coating layer) is 0.1 wt % to 6 wt % based on the weight of the core. The coating amount of the coating layer is preferably within the above range, which can fully coat the core and further improve the kinetic performance of the battery without sacrificing the gram capacity of the first positive electrode active material.
[0373] In some embodiments, the coating amount of the first coating layer is greater than 0 and less than or equal to 7 weight %, optionally greater than 0 and less than or equal to 6 weight %, more optionally greater than 0 and less than or equal to 5.5 weight % or 4-5.6 weight %, further optionally greater than 0 and less than or equal to 2 weight %, based on the weight of the kernel; and / or,
[0374] The coating amount of the second coating layer is greater than 0 and less than or equal to 6 weight%, optionally greater than 0 and less than or equal to 5.5 weight%, more optionally 2-4 weight% or 3-5 weight%, based on the weight of the kernel; and / or,
[0375] The coating amount of the third coating layer is greater than 0 and less than or equal to 6 wt %, optionally greater than 0 and less than or equal to 5.5 wt %, and more optionally greater than 0 and less than or equal to 2 wt %, based on the weight of the core.
[0376] In some embodiments, the shell further includes a fourth cladding layer covering the third cladding layer and a fifth cladding layer covering the fourth cladding layer.
[0377] The coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 to 10 wt %, optionally 0.05 to 10 wt %, more optionally 0.1 to 5 wt %, further 0.1 to 2 wt %, based on the weight of the core.
[0378] The coating amount of each coating layer is preferably within the above range, so that the core can be fully coated and the kinetic performance of the battery can be further improved without sacrificing the gram capacity of the first positive electrode active material.
[0379] In some embodiments, the shell is located on 40% to 90% of the surface of the core, and optionally 60% to 80% of the surface, thereby fully covering the core and improving the dynamic performance of the battery.
[0380] In some embodiments, the shell (which is just one coating layer) has a thickness of 1-15 nm.
[0381] In some embodiments, the thickness of the first coating layer is 1-10 nm, optionally 2-10 nm; and / or,
[0382] The thickness of the second coating layer is 2-25 nm, optionally 2-15 nm, more optionally 3-15 nm; and / or,
[0383] The thickness of the third cladding layer is 2-25 nm, and can be optionally 5-25 nm.
[0384] In some embodiments, the thickness of the first cladding layer can be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, or about 10 nm, or any range thereof.
[0385] In some embodiments, the thickness of the second coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, or within any range of any of the above values.
[0386] In some embodiments, the thickness of the third coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, about 16 nm, about 17 nm, about 18 nm, about 19 nm, about 20 nm, about 21 nm, about 22 nm, about 23 nm, about 24 nm or about 25 nm, or within any range of any of the above values.
[0387] The first coating layer has a thickness within the above range, which can further reduce the adverse effects on the kinetic properties of the first positive electrode active material.
[0388] The second coating layer has the above-mentioned thickness range, so that the surface structure of the second coating layer is stable and the side reaction with the electrolyte is small, thereby effectively reducing the interface side reaction and improving the high temperature performance of the battery.
[0389] The third coating layer has the above-mentioned thickness range, which can enhance the electrical conductivity of the first positive electrode active material and improve the compaction density of the positive electrode sheet prepared using the first positive electrode active material.
[0390] The thickness test of the coating layer is mainly carried out by FIB. The specific method may include the following steps: randomly selecting a single particle from the first positive electrode active material powder to be tested, cutting a thin slice with a thickness of about 100nm from the middle position or near the middle position of the selected particle, and then performing TEM testing on the thin slice to measure the thickness of the coating layer, measuring 3-5 positions, and taking the average value.
[0391] In some embodiments, the one or more coating layers each independently include one or more selected from pyrophosphate, phosphate, and oxide, and the one or more selected from pyrophosphate, phosphate, and oxide are crystalline.
[0392] Optionally, the crystallinity of the pyrophosphate, phosphate, and oxide are each independently from 10% to 100%, more preferably from 50% to 100%.
[0393] Herein, crystalline means a crystallinity of 50% or more, i.e., 50%-100%. That is, when the crystalline pyrophosphate and crystalline phosphate of the present application appear, it means a crystallinity of 50% to 100%.
[0394] Pyrophosphate and phosphate with a certain degree of crystallinity are not only conducive to giving full play to the pyrophosphate coating layer's ability to reduce manganese dissolution and the phosphate coating layer's excellent lithium ion conductivity and the function of reducing interface side reactions, but also enable the pyrophosphate coating layer and the phosphate coating layer to better lattice match, thereby achieving a close bond between the coating layers.
[0395] It should be noted that the crystallinity can be adjusted, for example, by adjusting the process conditions of the sintering process, such as sintering temperature, sintering time, etc. The crystallinity can be measured by methods known in the art, such as X-ray diffraction, density method, infrared spectroscopy, differential scanning calorimetry, and nuclear magnetic resonance absorption method. A specific method for testing the crystallinity of the first positive electrode active material by X-ray diffraction method may include the following steps:
[0396] Take a certain amount of the first positive electrode active material powder and measure the total scattering intensity by X-ray. It is the sum of the scattering intensities of all the matter in space and is only related to the intensity of the primary rays, the chemical structure of the first positive electrode active material powder, and the total number of electrons participating in the diffraction, that is, the mass, but has nothing to do with the order state of the sample. Then, separate the crystalline scattering and the non-crystalline scattering from the diffraction pattern. The crystallinity is the ratio of the scattering of the crystalline part to the total scattering intensity.
[0397] In some embodiments, in the shell, the weight ratio of the pyrophosphate to the phosphate, and the weight ratio of the pyrophosphate to the oxide, are each independently 1:3 to 3:1, and may be 1:3 to 1:1. Thus, by having the pyrophosphate to the phosphate or the pyrophosphate to the oxide in a suitable weight ratio range, manganese dissolution can be effectively reduced, the surface lithium content can be effectively reduced, and interfacial side reactions can be reduced, thereby improving the high-temperature storage performance and high-temperature cycling performance of the battery.
[0398] In some embodiments, one or more coating layers independently include carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon. Optionally, the molar ratio of SP2 carbon to SP3 carbon in the carbon is any value in the range of 0.07-13, more preferably any value in the range of 0.1-10, and further preferably any value in the range of 2.0-3.0.
[0399] In some embodiments, the molar ratio of sp2 carbon to sp3 carbon can be about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10, or any range thereof.
[0400] In this application, "about" a numerical value represents a range, which means a range of ±10% of the numerical value.
[0401] By selecting the carbon morphology in the carbon coating, the overall electrical performance of the battery can be improved. Specifically, by using a mixture of SP2 carbon and SP3 carbon and limiting the ratio of SP2 carbon to SP3 carbon to a certain range, the following situations can be avoided: if the carbon in the coating is all amorphous SP3, the conductivity is poor; if it is all graphitized SP2, although the conductivity is good, there are few lithium ion pathways, which is not conducive to lithium intercalation and deintercalation. In addition, limiting the molar ratio of SP2 carbon to SP3 carbon to the above range can achieve good conductivity and promote the transport of lithium ions, which is beneficial to the realization of battery functions and its cycle performance.
[0402] The mixing ratio of the SP2 and SP3 carbon forms can be controlled by sintering conditions, such as temperature and time. The molar ratio of SP2 to SP3 carbon can be determined by Raman spectroscopy. The Raman spectrum is separated to obtain the peak intensity of the SP3 carbon form (Id / Ig), where Id represents the peak intensity of the SP3 carbon form and Ig represents the peak intensity of the SP2 carbon form. This allows the molar ratio of the two to be determined.
[0403] In some embodiments, one or more coating layers independently include doped carbon, and the weight content of the doping element in the doped carbon is less than 30%; alternatively, the weight content of the doping element in the doped carbon is less than 20%. The doping element within the above content range can not only fully improve the conductivity of the pure carbon layer, but also effectively avoid excessive surface activity caused by excessive doping of the doping element, thereby effectively controlling interfacial side reactions caused by excessive doping of the coating layer.
[0404] In some embodiments, one or more coating layers each independently include doped carbon, wherein the doped carbon
[0405] The doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or,
[0406] The doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%;
[0407] Optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.
[0408] Since nitrogen atoms and sulfur atoms are closer in atomic radius to carbon atoms and are less likely to destroy the carbon skeleton, when the doping amount of nitrogen atoms and sulfur atoms is within the above relatively wide range, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transport and lithium ion desolvation capabilities can be promoted.
[0409] Since the atomic radius of phosphorus atoms, boron atoms and / or fluorine atoms is different from that of carbon atoms, excessive doping can easily destroy the carbon skeleton. Therefore, when the doping amount of phosphorus atoms, boron atoms and / or fluorine atoms is within the above-mentioned relatively small range, it can not only fully exert the conductivity of the doped carbon layer, but also promote lithium ion transmission and lithium ion desolvation capabilities.
[0410] In some embodiments, the one or more coating layers independently comprise pyrophosphate, the interplanar spacing of the pyrophosphate is in the range of 0.293-0.470 nm, optionally 0.297-0.462 nm or 0.293-0.326 nm, more optionally 0.300-0.310 nm, and the angle of the crystal direction (111) is in the range of 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, further optionally 29.00°-30.00°; and / or,
[0411] The one or more coating layers independently include phosphate, the interplanar spacing of the phosphate is in the range of 0.244-0.425 nm, optionally 0.345-0.358 nm, and the angle of the crystal orientation (111) is in the range of 20.00°-37.00°, optionally 24.25°-26.45°;
[0412] Optionally, the first coating layer or the second coating layer comprises phosphate.
[0413] The first and second coating layers of the first positive electrode active material are both crystalline, with their interplanar spacing and angles falling within the aforementioned ranges. This effectively reduces impurity phases in the coating layers, thereby improving the material's specific capacity, cycle performance, and rate capability.
[0414] In some embodiments, the lattice change rate of the first positive electrode active material before and after complete deintercalation of lithium is less than 50%, optionally less than 9.8%, more optionally less than 8.1%, further optionally less than 7.5%, further optionally less than 6%, further optionally less than 4%, further optionally less than 3.8%, and further optionally less than 2.0-3.8%.
[0415] By reducing the lattice change rate, Li ion transport can be facilitated, that is, the mobility of Li ions in the first positive electrode active material is enhanced, which is beneficial to improving the rate performance of the battery. The lattice change rate can be measured by methods known in the art, such as X-ray diffraction (XRD).
[0416] In some embodiments, the Li / Mn antisite defect concentration of the first positive electrode active material is less than 5.3%, optionally less than 5.1%, more optionally less than 4%, further optionally less than 2.2%, further optionally less than 2%, further optionally less than 1.5%-2.2% or less than 0.5%.
[0417] The so-called Li / Mn antisite defect refers to the Li + With Mn 2+ The positions of Li / Mn are interchanged. The Li / Mn antisite defect concentration refers to the concentration of Li / Mn in the first positive electrode active material. 2+ Li exchange occurs + Occupy + The percentage of total antisite defect Mn 2+ Will hinder Li + The transport of Li / Mn antisite defects can improve the specific capacity and rate performance of the first positive electrode active material by reducing the concentration of Li / Mn antisite defects. The concentration of Li / Mn antisite defects can be measured by methods known in the art, such as XRD.
[0418] In some embodiments, the surface oxygen valence state of the first positive electrode active material is below -1.55, optionally below -1.82, more optionally below -1.88, further optionally below -1.90 or -1.98 to -1.88, further optionally -1.98 to -1.89, further optionally -1.98 to -1.90.
[0419] By reducing the surface oxygen valence state, the interfacial side reactions between the first cathode active material and the electrolyte can be reduced, thereby improving the cycle performance and high temperature stability of the battery. The surface oxygen valence state can be measured by methods known in the art, such as electron energy loss spectroscopy (EELS).
[0420] In some embodiments, the positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045.
[0421] w a It represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition.
[0422] y is the molar amount of element B in 1 mol of the compound represented by formula (I), and y can be used to detect the element content by inductively coupled plasma emission spectroscopy (ICP).
[0423] V Bis the voltage platform of element B in the compound represented by formula (I), with the unit being V (volt). B The test can be performed as follows: at 25°C, let the battery stand for 10 minutes, and discharge it at 0.33C to the lower cut-off voltage; after standing for 10 minutes, charge the battery at a constant current of 0.33C to the upper cut-off voltage, and continue to charge at constant voltage until the current is ≤0.05C; after standing for 10 minutes, discharge the battery at 0.33C to the lower cut-off voltage, and obtain the discharge capacity of the battery, which is recorded as C0; after standing for 10 minutes, charge the battery at a constant current of 0.04C0 to the upper cut-off voltage, and continue to charge at constant voltage until the current is ≤0.05C0; after standing for 10 minutes, discharge the battery at 0.04C0 to the lower cut-off voltage, and obtain the discharge capacity of the battery, which is recorded as C1. The discharge differential capacity dQ / dV curve is made according to the discharge curve, and the peak less than 3.4V on the dQ / dV curve is the peak of element B, and the voltage corresponding to the peak is V B .
[0424] The battery is a battery including a positive electrode active material composition.
[0425] When the positive electrode active material composition further meets the above conditions, it is beneficial for the positive electrode sheet to have both high compaction density and high compaction density efficiency, and it is beneficial for the battery to have both high energy density and long service life.
[0426] In some embodiments, the second positive active material includes a layered oxide.
[0427] The second positive electrode active material has a high compaction density, but this is costly, often results in numerous side reactions during battery use, and has relatively poor crystal structure stability. By properly combining the first and second positive electrode active materials, the actual bulk density of the positive electrode active material composition can be increased, as can the compaction density and compaction density efficiency of the positive electrode sheet. This, in turn, can result in batteries using this positive electrode active material composition having higher energy density and a longer service life.
[0428] In some embodiments, the second positive electrode active material includes a compound represented by formula (II), Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 , (II)
[0429] A 1including one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1 including Mn and / or Al; C 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group VIA, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, and Group VIII; D 1 Includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.
[0430] In some embodiments, A 1 including one or more elements selected from Na, K, Mg, Rb, Zn, and Zr; and / or,
[0431] C 1 including one or more elements selected from the group consisting of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and optionally including one or more elements selected from the group consisting of Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, and B; and / or,
[0432] D 1 comprising one or more elements selected from N, S, F, Cl and Br, optionally including S and / or F; and / or,
[0433] a1 is selected from the range of 0.9 to 1.1; and / or,
[0434] b1 is selected from the range of 0 to 0.1; and / or,
[0435] c1 is selected from the range of 0.314 to 0.990, and may be selected from the range of 0.500 to 0.990; and / or,
[0436] d1 is selected from the range of 0 to 0.320, and optionally from the range of 0 to 0.150; and / or,
[0437] e1 is selected from the range of 0.001 to 0.450, and can be optionally selected from the range of 0.005 to 0.4; and / or,
[0438] f1 is selected from the range of 0.001 to 0.1, and may be selected from the range of 0.001 to 0.05; and / or,
[0439] g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.05.
[0440] In some embodiments, the second positive electrode active material includes a core and a shell covering the core, wherein the core includes a compound represented by formula (II); the shell includes one or more coating layers; and each coating layer has ionic conductivity and / or electronic conductivity.
[0441] In some embodiments, the one or more coating layers independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.
[0442] In some embodiments, one or more coating layers each independently include one or more elements selected from Al, Zr, Mg, Ba, Cd, Zn, Ti, Co, W, Y, Si, Sn, B, P, S, and C.
[0443] In some embodiments, the fast ion conductor includes Li 3x3 La 2 / 3-x3 M 2 a3 TiN 2 z3 O3、Li 2+2x4 Zn 1-x4 GeO4、LiM 3 2(PO4)3, one or more, M 2 Including one or more elements selected from Ba, Sr, N 2 including one or more elements selected from Al, Zr, M 3 It is one or more elements selected from Zr, Ti, Ge, and Hf, 0.04≤x3≤0.167, 0≤a3≤1, 0≤z3≤1, and -0.3≤x4≤0.8.
[0444] In some embodiments, the shell of the second positive electrode active material includes a coating layer; optionally, the coating layer includes one or more selected from phosphate, pyrophosphate, and oxide.
[0445] In some embodiments, the shell of the second positive active material includes a first coating layer coating the inner core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphate, pyrophosphate, and oxide.
[0446] Optionally, the first coating layer comprises one or more selected from phosphates and oxides, and the second coating layer comprises one or more selected from pyrophosphates and oxides. Optionally, the oxide in the first coating layer is an oxide of one or more elements selected from Al, Zr, Mg, Ti, Co, Y, Ba, and Cd. Optionally, the oxide in the second coating layer is an oxide of one or more elements selected from B, Sn, S, and P.
[0447] In some embodiments, the coating amount of the shell of the second positive active material is 0.005 wt % to 1 wt %, optionally 0.01 wt % to 0.5 wt %, based on the weight of the core.
[0448] In some embodiments, the shell of the second positive active material has a thickness of 2 nm to 200 nm, optionally 5 nm to 50 nm.
[0449] The first positive electrode active material and the second positive electrode active material can be prepared by a sintering method. The shells of the first positive electrode active material and the second positive electrode active material can be prepared by a liquid phase coating method.
[0450] [Positive electrode]
[0451] The positive electrode sheet provided in the embodiments of the present application includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. The positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes the aforementioned positive electrode active material composition. The positive electrode current collector has two surfaces that oppose each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0452] In some embodiments, the content of the positive electrode active material composition in the positive electrode film layer is 50-99.5 wt %, optionally 90-99.5 wt %, or 95-99.5 wt %, based on the total weight of the positive electrode film layer.
[0453] In some embodiments, the positive electrode film layer also includes a third positive electrode active material, which includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel-type lithium manganese oxide material, and their respective modified compounds, and the modification method includes doping and / or surface coating modification.
[0454] In some embodiments, the third positive electrode active material includes a compound represented by formula (III), Li 1+p1 A 2 q1 B 2 r1 O s1 , (III)
[0455] 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 comprises one or more elements selected from Co, Ni, Mn, and Al; B 2 comprises one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.
[0456] In some embodiments, the third positive electrode active material comprises one or more selected from 1.11 Li 0.22 Ni 0.58 Mn 0.02 Ti 1.2 O2, Li 0.6 Mn 0.2 Ni 1.16 O2, Li 0.22 Ni 0.6 Mn 1.16 O2, Li 0.13 Ni 0.06 Co 0.59 Mn 1.1 O2 and Li 0.2 Ni 0.2 Co 0.48 Mn
[0457] O2.
[0458] In some embodiments, the third positive electrode active material comprises a core and a shell coating the core, the core comprises a compound represented by formula (III); the shell comprises one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
[0459] Phosphates, pyrophosphates, and solid electrolytes can improve the ionic transport properties of the third positive electrode active material.
[0460] The conductive polymer can form a uniform film with high electronic conductivity, improving the charge transfer at the interface between the positive electrode and the electrolyte. At the same time, the conductive polymer can adapt to the volume change of the material, thereby reducing crack formation.
[0461] The material capable of reversibly intercalating and deintercalating lithium ions can include some different types of positive electrode active materials.
[0462] In some embodiments, the coating amount of the shell coating the compound represented by formula (III) is 0.1 wt% to 5 wt%, optionally 0.5 wt% to 2 wt%, based on the weight of the core.
[0463] In some embodiments, the thickness of the shell encapsulating the compound of formula (III) is 2 nm to 200 nm, optionally 5 nm to 50 nm.
[0464] In some embodiments, the third positive electrode active material includes a compound represented by formula (IV), Li a2 A 3 x2 B 3 y2 P 1-z2 C 3 z2 O 4-n2 D 3 n2 , (IV)
[0465] A 3 including one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB, and Group VIB; 3 including one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 including one or more elements selected from Group IIIA, Group IVA, Group VA, and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.5.
[0466] In some embodiments, A 3 including one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and optionally including one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; and / or,
[0467] B 3 including one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally including one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge; and / or,
[0468] C 3 including one or more elements selected from B (boron), S, Si and N; and / or,
[0469] D 3 comprising one or more elements selected from S, F, Cl and Br; and / or,
[0470] a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or,
[0471] x2 is selected from the range of 0.001 to 0.005; and / or,
[0472] y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or,
[0473] z2 is selected from the range of 0.001 to 0.5, alternatively selected from the range of 0.001 to 0.1, more alternatively selected from the range of 0.001 to 0.005; and / or,
[0474] n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.
[0475] In some embodiments, the third positive electrode active material includes a core and a shell covering the core, wherein the core includes a compound represented by formula (IV); the shell is the same as the shell covering the compound represented by formula (I), and will not be repeated here.
[0476] In some embodiments, the third positive electrode active material includes a compound represented by formula (V), LiMn t1 A 4 2-t1 O4, (V)
[0477] t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.
[0478] In some embodiments, the third positive electrode active material includes a core and a shell covering the core, wherein the core includes a compound represented by formula (V); the shell includes one or more coating layers; and each coating layer has ionic conductivity and / or electronic conductivity.
[0479] In some embodiments, the one or more coating layers independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly intercalating and deintercalating lithium ions.
[0480] Phosphate, pyrophosphate, and solid electrolyte can improve the ion transport performance of the third positive electrode active material.
[0481] Conductive polymers can form uniform films with high electronic conductivity, improving charge transfer at the cathode-electrolyte interface. They can also accommodate volume changes in materials, thereby reducing crack formation.
[0482] Materials capable of reversibly intercalating and deintercalating lithium ions may include several different types of positive electrode active materials.
[0483] In some embodiments, the coating amount of the shell coating the compound represented by formula (V) is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core.
[0484] In some embodiments, the thickness of the shell encapsulating the compound represented by formula (V) is 2 nm to 200 nm, optionally 5 nm to 50 nm.
[0485] The third positive active material can be prepared by a sintering method, and the shell can be prepared by a liquid phase coating method.
[0486] In some embodiments, the positive electrode film layer may include a positive electrode binder.
[0487] In some embodiments, the positive electrode binder may include a vinylidene fluoride homopolymer and / or copolymer. Optionally, the comonomer may include one or more of tetrafluoroethylene, hexafluoropropylene, and propylene. Optionally, the weight proportion of the comonomer is ≤1%. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer.
[0488] In some embodiments, the positive electrode binder may include one or more of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.
[0489] In some embodiments, the positive electrode binder may have a weight average molecular weight of 300,000 to 2,000,000.
[0490] In some embodiments, the positive electrode film layer may include a positive electrode conductive agent. As an example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, which are not limited in the present embodiment.
[0491] In some embodiments, the positive electrode film layer may further include functional additives, which may include one or more of a dispersant, a plasticizer, a pore former, a water scavenger, an acid scavenger, and a lithium supplementer.
[0492] The dispersant may comprise an abc-type block copolymer, wherein the a block comprises polyvinyl pyrrolidone, the b block comprises polyacrylic acid, and the c block comprises one or more of a polytetrahydrofuran chain, a polyethylene oxide chain, a polyethylene glycol chain, a polypropylene glycol chain, and a polyoxypropylene triol chain. Optionally, the ratio of the average degree of polymerization of the a block to the b block is greater than 10:1. Optionally, the ratio of the average degree of polymerization of the a block to the c block is (0.1-10):1. Optionally, the weight-average molecular weight of the dispersant is 2,000 to 100,000.
[0493] The plasticizer may include one or more of a strong solvent type (PP-SS) plasticizer, a low temperature resistant type (PP-LT) plasticizer, a low volatility type (PP-LV) plasticizer, a low diffusion type (SP-LD) plasticizer, a heat stable type (SP-Stab) plasticizer, and a flame retardant type (SP-FR) plasticizer.
[0494] Strong solvent type (PP-SS) plasticizers can provide strong plasticizing properties, and may include, for example, phthalates, non-phthalates (such as benzoates, tricresyl phosphate, etc.).
[0495] Low-temperature resistant (PP-LT) plasticizers can also provide good low-temperature resistance and may include, for example, aliphatic dibasic acid esters.
[0496] Low volatility (PP-LV) plasticizers also have lower volatility and may include, for example, trimellitates and polyesters.
[0497] Low-diffusivity (SP-LD) plasticizers also have lower diffusivity and, for example, may include polyesters.
[0498] Thermally stable (SP-Stab) plasticizers also have a thermal stabilization function and may include, for example, epoxy compounds.
[0499] Flame retardant (SP-FR) plasticizers also have flame retardant functions and may include, for example, phosphate esters and halogenated hydrocarbons.
[0500] The lithium supplement agent may include one or more of lithium-rich oxides (such as Li2NiO2, Li5FeO4, etc.), nanocomposites and binary lithium compounds. Optionally, the number of Li atoms in the molecular formula of the lithium supplement agent is ≥1.5.
[0501] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0502] The positive electrode sheet does not exclude other additional functional layers in addition to the positive electrode film layer. For example, in some embodiments, the positive electrode sheet may further include a functional coating, which may be located between the positive electrode current collector and the positive electrode film layer and / or located on the surface of the positive electrode film layer facing away from the positive electrode current collector. As an example, the functional coating may include one or more of conductive carbon, a water removal additive, an acid removal additive, and a lithium supplement, which is not limited in this embodiment of the present application. In some embodiments, the thickness of the functional coating may be 0.1 μm-10 μm.
[0503] The positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material composition, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0504] [Negative electrode]
[0505] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0506] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0507] In some embodiments, the thickness of the negative electrode current collector may be 3 μm to 20 μm.
[0508] In some embodiments, the negative electrode active material may include one or more of a carbon-based material, a silicon-based material, a tin-based material, and lithium titanate. The carbon-based material may include one or more of graphite (e.g., artificial graphite, natural graphite, etc.), soft carbon, and hard carbon. The silicon-based material may include one or more of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxides, and tin alloys.
[0509] In some embodiments, the negative electrode active material may include a carbon-based material, or a combination of a carbon-based material and a silicon-based material.
[0510] In some embodiments, the negative electrode active material may include a carbon-based material, and the carbon-based material may include graphite, or a combination of graphite and hard carbon. Optionally, the graphite may have a porous structure. Optionally, the graphite may have a specific capacity greater than or equal to 340 mAh / g.
[0511] In some embodiments, the negative electrode active material may include a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.
[0512] In some embodiments, the negative electrode film layer may include a negative electrode binder. As an example, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS), but the present invention is not limited thereto.
[0513] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, which are not limited in the present embodiment.
[0514] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC)).
[0515] In some embodiments, the porosity of the negative electrode film layer is 20% to 50%.
[0516] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. In some embodiments, the negative electrode plate may further include a functional coating. The functional coating may be located between the negative electrode current collector and the negative electrode film layer and / or on the surface of the negative electrode film layer facing away from the negative electrode current collector. Optionally, the functional coating may include carbon.
[0517] In some embodiments, the negative electrode film layer may further include a lithium replenishing material. Optionally, the lithium replenishing material includes one or more of lithium foil, lithium ribbon, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent may include one or more of lithium-aromatic hydrocarbons, complexes of lithium-aromatic hydrocarbons and ether solvents, and may optionally include one or more of lithium naphthalene and lithium biphenyl-dimethyl ether (DME).
[0518] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer, respectively, disposed on two surfaces of the negative electrode current collector. The first negative electrode film layer and the second negative electrode film layer may have the same or different compositions; and the first negative electrode film layer and the second negative electrode film layer may have the same or different thicknesses.
[0519] In some embodiments, the thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:5.
[0520] The negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0521] In some embodiments, the negative electrode plate may not include a negative electrode active material capable of intercalating and deintercalating lithium ions. For example, the negative electrode plate may include a lithium plate or a lithium alloy plate; or, the negative electrode plate may include a three-dimensional skeleton layer in a network or foam form; or, the negative electrode plate may include a negative electrode current collector and a lithium-containing layer disposed on at least one surface of the negative electrode current collector.
[0522] [Electrolytes]
[0523] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application does not specifically limit the type of electrolyte, and it can be selected according to the needs. For example, the electrolyte may include one or more of liquid electrolyte (also known as electrolyte), all-solid electrolyte, gel electrolyte, etc.
[0524] In some embodiments, the electrolyte is liquid and includes a lithium salt, a non-aqueous solvent for dissolving the lithium salt, and optional additives.
[0525] In some embodiments, the lithium salt may include one or more selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2, LiBF2C2O4, and LiPO2F2.
[0526] In some embodiments, the concentration of the lithium salt may be 0.5-1.5 mol / L.
[0527] In some embodiments, the non-aqueous solvent may include one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, sulfolane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.
[0528] In some embodiments, the additives may include one or more of negative electrode film-forming additives, positive electrode film-forming additives, additives for improving battery overcharge performance, additives for improving battery high temperature performance, additives for improving battery low temperature power performance, water removal additives, acid removal additives, and additives capable of complexing transition metal ions. As an example, the additives may include
[0529] One or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, optionally Including one or more of vinylene carbonate (VC), 1,2,3-tris(2-cyanoethoxy)propane (TCP), 1-aza-12-crown 4-ether (A12C4), N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate.
[0530] In some embodiments, the content of the additive may be less than or equal to 10% based on the total weight of the electrolyte.
[0531] [Isolation film]
[0532] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0533] In some embodiments, the separator includes a porous substrate. The porous substrate may be made of at least one of fiberglass, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, polyester, and polyimide. The porous substrate may be a single-layer film or a multi-layer composite film, without particular limitation. When the porous substrate is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0534] In some embodiments, the isolation membrane may further include a coating layer located on at least one surface of the porous substrate. Optionally, the coating layer includes one or more of inorganic heat-resistant particles and organic heat-resistant particles.
[0535] In some embodiments, the isolation membrane has a porosity of 10% to 40%.
[0536] In some embodiments, the isolation film may have a thickness of 3 μm to 20 μm.
[0537] The present application also provides an electrical device, which includes at least one of the battery cells, battery modules, or battery packs provided in the present application. The battery cells, battery modules, or battery packs can be used as power sources for the electrical device, or as energy storage units for the electrical device. The electrical device may include, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.
[0538] As an electrical device, a battery cell, battery module or battery pack can be selected according to its usage requirements.
[0539] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module can be used.
[0540] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0541] Example
[0542] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0543] The batteries of Examples 1-26 and Comparative Example 3 were prepared according to the following method.
[0544] Preparation of positive electrode
[0545] The first positive electrode active material and the second positive electrode active material shown in Table 1 and Table 2, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were thoroughly stirred and mixed in an appropriate amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.
[0546] Preparation of negative electrode sheet
[0547] The negative electrode active material graphite, binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water at a mass ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained.
[0548] Preparation of electrolyte
[0549] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0550] Preparation of isolation membrane
[0551] A porous polyethylene film was used as the separator.
[0552] Battery preparation
[0553] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in sequence to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a battery is obtained.
[0554] Comparative Example 1
[0555] The preparation method of the battery is the same as that of Example 1, except for the preparation of the positive electrode sheet.
[0556] The second positive electrode active material shown in Table 1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were thoroughly stirred and mixed in an appropriate amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.
[0557] Comparative Example 2
[0558] The preparation method of the battery is the same as that of Example 1, except for the preparation of the positive electrode sheet.
[0559] The first positive electrode active material shown in Table 1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were thoroughly stirred and mixed in an appropriate amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.
[0560] In Table 1 and Table 2, NCM523 refers to LiNi 0.5 Co 0.2 Mn 0.3 O2, LMFP refers to carbon-coated LiMn 0.7 Fe 0.3 PO4.
[0561] The NCM523 and LMFP of each embodiment and comparative example can be commercially purchased, and then a variety of commercially available materials are screened by selecting a suitable sieve and then mixed in a predetermined proportion to obtain the obtained materials; or, the commercially available materials are first ball-milled to a suitable size, and then screened by selecting a suitable sieve, and then mixed in a predetermined proportion to obtain the obtained materials; or, a sintering method is adopted and the sintering process parameters (such as sintering temperature, sintering time, sintering atmosphere, etc.) and grinding parameters (such as grinding speed, grinding time, etc.) are adjusted, and a suitable sieve is selected for screening to obtain the obtained materials; or, a variety of materials of different sizes prepared by the sintering method are mixed in a predetermined proportion to obtain the obtained materials.
[0562] w a w represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition. b It represents the weight content of the second positive electrode active material based on the total weight of the positive electrode active material composition.
[0563] P1 is the powder compaction density of the first positive electrode active material at 30,000 N. P2 is the powder compaction density of the second positive electrode active material at 30,000 N.
[0564] PD represents the compacted density of the positive electrode film.
[0565] Compaction density efficiency of positive electrode sheet = PD / [(P1×W a )+(P2×W b )]. (P1×W a )+(P2×W b ) represents the theoretical compacted density of the positive electrode active material composition.
[0566] y is the molar amount of Fe element in LMFP, i.e. 0.3.
[0567] V B is the voltage platform of the Fe element in LMFP, in V (volts).
[0568] In the particle size distribution curve of the positive electrode active material composition, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2.
[0569] Figure 7 is the particle size distribution curve of the positive electrode active material composition of Example 11. As shown in Figure 7, in the particle size distribution curve of the positive electrode active material composition, the peak on the left is the second peak (i.e., the volume distribution peak with the second largest peak intensity), and the peak on the right is the first peak (i.e., the volume distribution peak with the largest peak intensity).
[0570] The above parameters can be measured according to the test methods given above.
[0571] In Table 1, the first positive electrode active material is primarily single crystal, accounting for more than 90% of the total. The second positive electrode active material of Examples 1-11 is primarily polycrystalline, accounting for more than 90% of the total. The second positive electrode active material of Examples 12-16 is primarily single crystal, accounting for more than 90% of the total.
[0572] In Table 2, the first positive electrode active material is primarily polycrystalline, accounting for more than 90% by volume. The second positive electrode active materials of Examples 17-21 are primarily single crystal, accounting for more than 90% by volume. The second positive electrode active materials of Examples 22-26 are primarily polycrystalline, accounting for more than 90% by volume.
[0573] Test section
[0574] At 25°C, charge the battery at a constant current of 1C to 4.3V. Continue charging at a constant voltage until the current reaches 0.05C. At this point, the battery is fully charged. Record the charge capacity at this point, which is the first cycle charge capacity. After the battery rests for 5 minutes, discharge it at a constant current of 1C to 2.8V. This constitutes one cycle of charge and discharge. Record the discharge capacity at this point, which is the first cycle discharge capacity. Repeat the battery's cyclic charge and discharge test as described above, recording the discharge capacity after each cycle until the battery's discharge capacity decays to 80% of the first cycle discharge capacity. The number of cycles at this point is used to characterize the battery's cycling performance. The higher the number of cycles, the longer the battery's service life.
[0575] It can be seen from the test results in Tables 1 and 2 that when the particle size distribution curve of the positive electrode active material composition satisfies 0<|Dv1-Dv2| / Dv1≤50, the positive electrode sheet using the positive electrode active material composition can have both high compaction density and high compaction density efficiency, thereby enabling the secondary battery to have a high energy density and a long service life.
[0576] The preparation methods of the batteries of Examples 27-31 are similar to those of Example 4, except that the types of the first positive electrode active materials are different. See Table 3 for details.
[0577] The first positive electrode active material of Examples 27-31 is obtained by sintering and adjusting the sintering process parameters (such as sintering temperature, sintering time, sintering atmosphere, etc.), grinding parameters (such as grinding speed, grinding time, etc.), and selecting a suitable screen for screening; or, by mixing a plurality of materials of different particle sizes prepared by the sintering method according to a predetermined proportion.
[0578] It can be seen from the test results in Table 3 that by doping specific elements at the Mn position of LiMnPO4 and at the Li position, P position and / or O position, it is optional to dope specific elements at the Mn position and P position of LiMnPO4, and more optionally at the Li position, Mn position, P position and O position of LiMnPO4, the compaction density of the positive electrode sheet can be further improved, the energy density of the battery can be improved, and the cycle performance of the battery can be improved.
[0579] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical concept and exerting the same effects are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A positive electrode active material composition, wherein: The positive electrode active material composition includes a first positive electrode active material and a second positive electrode active material having a crystal form different from that of the first positive electrode active material, the first positive electrode active material includes phosphate, and the particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50.
2. The positive electrode active material composition according to claim 1, wherein The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm; and / or, The volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.
3. The positive electrode active material composition according to claim 1 or 2, wherein: The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies: 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or, 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or, 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.
4. The positive electrode active material composition according to claim 1 or 2, wherein: The volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies: 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or, 2.0 μm ≤ Dv1 ≤ 12.5 μm, optionally, 3.0 μm ≤ Dv1 ≤ 12.3 μm; and / or, 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.
5. The positive electrode active material composition according to any one of claims 1 to 4, wherein: The morphology of the first positive electrode active material includes one or more of single crystal and polycrystalline, and the morphology of the second positive electrode active material includes one or more of single crystal and polycrystalline; Optionally, the volume distribution particle size Dv50 of the first positive electrode active material with a single crystal morphology is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the first positive electrode active material with a single crystal morphology is 0.05 μm to 1.5 μm, and optionally 0.1 μm to 1.0 μm; and / or, Optionally, the volume distribution particle size Dv50 of the first positive electrode active material with polycrystalline morphology is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the first positive electrode active material with polycrystalline morphology is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm; and / or, Optionally, the volume distribution particle size Dv50 of the second positive electrode active material with single crystal morphology is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the second positive electrode active material with a single crystal morphology is 0.3 μm to 8 μm, and optionally 1.0 μm to 3.5 μm; and / or, Optionally, the volume distribution particle size Dv50 of the second positive electrode active material with polycrystalline morphology is 2.5 μm to 16.5 μm, which can be Selected as 3.0μm to 15.5μm; Optionally, the volume distribution particle size Dv10 of the second positive electrode active material with a polycrystalline morphology is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.
6. The positive electrode active material composition according to any one of claims 1 to 5, wherein: Based on the total weight of the positive electrode active material composition, the weight content of the first positive electrode active material is recorded as w a The weight content of the second positive electrode active material is recorded as w b ,but w a Selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%; and / or, w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.
7. The positive electrode active material composition according to any one of claims 1 to 6, wherein: The powder compaction density P1 of the first positive electrode active material at 30000N is 1.89 g / cm 3 Above, optional 1.95g / cm 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2 g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 The following; and / or, The powder compaction density P2 of the second positive electrode active material at 30000N is greater than or equal to 2.90g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3 g / cm 3 and / or, The BET specific surface area of the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be selected to be less than or equal to 1.5m 2 / g, 0.28m 2 / g to 1.5m 2 / g.
8. The positive electrode active material composition according to any one of claims 1 to 7, wherein:The first positive electrode active material includes a compound represented by formula (I), Li a A x Mn 1-y B y P 1-z C z O 4-n D n (I) A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB and Group VIII; C includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; n is selected from the range of 0 to 0.
5.
9. The positive electrode active material composition according to claim 8, wherein A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, B includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or, C includes one or more elements selected from B (boron), S, Si and N; and / or, D includes one or more elements selected from S, F, Cl and Br.
10. The positive electrode active material composition according to claim 8 or 9, wherein: A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include any one element selected from Mg and Nb; and / or, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may include at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and may include at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and may include at least two elements selected from Fe, Ti, V, Co and Mg, and may include Fe and one or more elements selected from Ti, V, Co and Mg; and / or C includes any one element selected from B (boron), S, Si and N, and may be S; and / or, D includes any one element selected from S, F, Cl and Br, and may be F.
11. The positive electrode active material composition according to any one of claims 8 to 10, wherein: a is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or, x is selected from the range of 0.001 to 0.005; and / or, y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or, z is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or, n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.
005.
12. The positive electrode active material composition according to any one of claims 8 to 11, wherein: x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.
1.
13. The positive electrode active material composition according to any one of claims 8 to 12, wherein: y:z is selected from the range of 0.002 to 999, and may be selected from the range of 0.025 to 999 or the range of 0.002 to 500, and may be further selected from the range of 0.2 to 600.
14. The positive electrode active material composition according to any one of claims 8 to 13, wherein: z:n is selected from the range of 0.002 to 500, can be selected from the range of 0.2 to 100, and can be further selected from the range of 0.2 to 50.
15. The positive electrode active material composition according to any one of claims 8 to 14, wherein: A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.
1.
16. The positive electrode active material composition according to any one of claims 8 to 14, wherein: B includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be optionally selected from one or more elements selected from Zn, Fe, Ti, V, Ni, Co and Mg; C includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.
17. The positive electrode active material composition according to any one of claims 8 to 16, wherein: (1-y): y is in the range of 0.1-999, optionally in the range of 0.1-10 or in the range of 0.67-999, more optionally in the range of 1 to 10, further optionally in the range of 1 to 4, and further optionally in the range of 1.5 to 3; and / or, a:x is in the range of 1 to 1200, and can be optionally in the range of 9 to 1100, and can be more optionally in the range of 190-998.
18. The positive electrode active material composition according to any one of claims 8 to 17, wherein: z:(1-z) is 1:9 to 1:999, and can be optionally 1:499 to 1:
249.
19. The positive electrode active material composition according to any one of claims 8 to 18, wherein: The first positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (I); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
20. The positive electrode active material composition according to claim 19, wherein: The one or more coating layers each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.
21. The positive electrode active material composition according to claim 19 or 20, wherein: The shell includes a coating; Optionally, the coating layer comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.
22. The positive electrode active material composition according to claim 19 or 20, wherein: The shell includes a first coating layer covering the core and a second coating layer covering the first coating layer; Optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer; More optionally, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide and boride, and the second coating layer includes one or more selected from carbon and doped carbon.
23. The positive electrode active material composition according to claim 19 or 20, wherein: The shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; Optionally, the first coating layer, the second coating layer and the third coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer; More optionally, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphates, oxides and borides, and the third coating layer includes one or more selected from carbon and doped carbon.
24. The positive electrode active material composition according to any one of claims 20 to 23, wherein: The pyrophosphate is M b (P2O7) c and / or, The phosphate is X m (PO4) q and / or, The doping element in the doped carbon includes one or more elements selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or, The oxide is M' d O e and / or, The boride is Z v B w and / or, The polymer includes one or more selected from polysaccharides and their derivatives, and polysiloxanes; M, X and Z each independently include a group selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB One or more elements from Group A, Group VIIB and Group VIII; b is selected from the range of 1 to 4; c is selected from the range of 1 to 6; m is selected from the range of 1 to 2; q is selected from the range of 1 to 4; M′ comprises one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides and Sb; d is greater than 0 and less than or equal to 2; e is greater than 0 and less than or equal to 5; v is selected from the range of 1 to 7; w is selected from the range of 1 to 2.
25. The positive electrode active material composition according to claim 24, wherein: M, X and Z each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn and Al; and / or, The doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine; and / or, M′ comprises one or more elements selected from Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La and Ce, and may optionally comprise one or more elements selected from Mg, Al, Si, Zn, Zr and Sn; and / or The polysiloxane is selected from one or more of linear polysiloxane and cyclic polysiloxane; and / or, The polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.
26. The positive electrode active material composition according to any one of claims 19 to 20, 22, 24 to 25, wherein: The first positive electrode active material includes a core and a shell covering the core, The core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and C includes one or more elements selected from B (boron), S, Si and N; The shell includes a first coating layer coating the inner core and a second coating layer coating the first coating layer, wherein the first coating layer includes pyrophosphate MP2O7 and phosphate XPO4, and M and X each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; and the second coating layer contains carbon.
27. The positive electrode active material composition according to any one of claims 19 to 20, 23 to 25, wherein: The first positive electrode active material includes a core and a shell covering the core, The core includes Li a Mn 1-y B y P 1-z C z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and C includes one or more elements selected from B (boron), S, Si and N; The shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer. The first coating layer includes pyrophosphate Li f QP2O7 and / or Q g (P2O7) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, the pyrophosphate Li f QP2O7 and / or Q g (P2O7) h wherein Q independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; The second coating layer comprises crystalline phosphate XPO4, wherein X comprises one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; The third coating layer includes carbon.
28. The positive electrode active material composition according to any one of claims 19 to 25, wherein: The one or more coating layers in the shell that are farthest from the core each independently include one or more selected from polysiloxane, polysaccharide and polysaccharide derivatives.
29. The positive electrode active material composition according to any one of claims 19 to 25 and 28, wherein: The polysiloxane comprises a structural unit represented by formula (i), R1 and R2 are independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic and C2-C20 halogenated heteroaromatic; Optionally, R1 and R2 are independently selected from H, amino, phosphate, polyether segment, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl and C2-C8 haloalkenyl.
30. The positive electrode active material composition according to any one of claims 19 to 25, 28 to 29, wherein: The polysiloxane further comprises an end-capping group, which comprises one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.
31. The positive electrode active material composition according to any one of claims 19 to 25, 28 to 30, wherein: The polysiloxane comprises polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side-chain aminopropyl polysiloxane, aminopropyl One or more of end-capped polydimethylsiloxane, side chain phosphate grafted polydimethylsiloxane, side chain polyether grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, and cyclic polydimethylsiloxane.
32. The positive electrode active material composition according to any one of claims 19 to 25 and 28 to 31, wherein: The number average molecular weight of the polysiloxane, the polysaccharide and the polysaccharide derivative is independently below 300,000, and may be 10,000 to 200,000, more preferably 20,000 to 120,000, and further preferably 400 to 80,000.
33. The positive electrode active material composition according to any one of claims 19 to 25 and 28 to 32, wherein: The mass percentage of the polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.
34. The positive electrode active material composition according to any one of claims 19 to 25 and 28 to 33, wherein: The substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH and salts thereof, -R-OH, -SO3H and salts thereof, -R-OH, -R-SO3H and salts thereof, sulfate, alkoxy, R represents an alkylene group, optionally a C1 to C5 alkylene group; Optionally, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO3H, -SO3Li, -SO3Na, -SO3K, -CH2-SO3H, -CH2-SO3Li, -CH2-SO3Na, -CH2-SO3K, methoxy, ethoxy.
35. According to any one of claims 19 to 25, 28 to 34, the positive electrode active material composition, the polysaccharide comprises one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum and fenugreek gum.
36. The positive electrode active material composition according to any one of claims 19 to 25 and 28 to 35, wherein: The mass percentage of the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives is independently 20% to 85%, and optionally 30% to 78%.
37. The positive electrode active material composition according to any one of claims 19 to 36, wherein: The lattice mismatch between the material of the core and the material of the shell is less than 10%.
38. The positive electrode active material composition according to any one of claims 8 to 37, wherein: Based on the total weight of the first positive electrode active material, The manganese content is in the range of 10 wt% to 35 wt%, optionally in the range of 13.3 wt% to 33.2 wt%, more optionally in the range of 15 wt% to 30 wt%, further optionally in the range of 17 wt% to 20 wt%; and / or, The phosphorus content is in the range of 12 wt% to 25 wt%, optionally in the range of 15 wt% to 20 wt%, and more optionally in the range of 16.8 wt% to 19.5 wt%; and / or, The weight ratio of manganese element to phosphorus element ranges from 0.71 to 1.85, and can be selected from 0.90 to 1.25, and more preferably from 0.95 to 1.
20.
39. The positive electrode active material composition according to any one of claims 1 to 18, wherein: The surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; optionally, the surface of the first positive electrode active material is coated with carbon.
40. The positive electrode active material composition according to claim 39, wherein The doping elements in the doped carbon include one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine.
41. The positive electrode active material composition according to any one of claims 19 to 21, 24 to 25, 28 to 40, wherein: The coating amount of the shell is 0.1 wt % to 6 wt % based on the weight of the core.
42. The positive electrode active material composition according to any one of claims 19 to 20, 22 to 38, wherein: The coating amount of the first coating layer is greater than 0 and less than or equal to 7% by weight, and can be greater than 0 and less than or equal to 6% by weight, and can be greater than 0 and less than or equal to 5.5% by weight or 4-5.6% by weight, and can be further greater than 0 and less than or equal to 2% by weight, based on the weight of the core; and / or, The coating amount of the second coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally 2-4% by weight or 3-5% by weight, based on the weight of the core; and / or, The coating amount of the third coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally greater than 0 and less than or equal to 2% by weight, based on the weight of the core.
43. The positive electrode active material composition according to any one of claims 19 to 20, 23 to 25, 27 to 38, and 42, wherein: The shell further includes a fourth coating layer covering the third coating layer and a fifth coating layer covering the fourth coating layer; The coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 wt % to 10 wt %, optionally 0.05 wt % to 10 wt %, more optionally 0.1 wt % to 5 wt %, further 0.1 wt % to 2 wt %, based on the weight of the core.
44. The positive electrode active material composition according to any one of claims 19 to 43, wherein: The shell is located on 40% to 90% of the surface of the inner core, optionally 60% to 80% of the surface.
45. The positive electrode active material composition according to any one of claims 19 to 21, 24 to 25, 28 to 41, 44, wherein: The shell has a thickness of 1-15 nm.
46. The positive electrode active material composition according to any one of claims 19 to 20, 22 to 38, 42 to 45, wherein: The thickness of the first coating layer is 1-10 nm, and can be 2-10 nm; and / or, The thickness of the second coating layer is 2-25 nm, optionally 2-15 nm, more optionally 3-15 nm; and / or, The thickness of the third coating layer is 2-25 nm, and can be optionally 5-25 nm.
47. The positive electrode active material composition according to any one of claims 19 to 46, wherein: The one or more coating layers each independently include one or more selected from pyrophosphate, phosphate and oxide, and the one or more selected from the pyrophosphate, phosphate and oxide are crystalline; Optionally, the crystallinity of the pyrophosphate, the phosphate and the oxide is each independently 10% to 100%, more preferably 50% to 100%.
48. The positive electrode active material composition according to any one of claims 19 to 47, wherein: In the shell, the weight ratio of pyrophosphate to phosphate and the weight ratio of pyrophosphate to oxide are each independently 1:3 to 3:1, and optionally 1:3 to 1:
1.
49. The positive electrode active material composition according to any one of claims 19 to 48, wherein The one or more coating layers each independently include carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon; Optionally, in the carbon, the molar ratio of the SP2 carbon to the SP3 carbon is any value in the range of 0.07-13, more preferably any value in the range of 0.1-10, and further preferably any value in the range of 2.0-3.
0.
50. The positive electrode active material composition according to any one of claims 19 to 49, wherein: The one or more coating layers each independently include doped carbon, and the mass content of the doping element in the doped carbon is less than 30%; optionally, the mass content of the doping element in the doped carbon is less than 20%.
51. The positive electrode active material composition according to any one of claims 19 to 50, wherein: The one or more coating layers each independently include doped carbon, in which: The doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or, The doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%; Optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.
52. The positive electrode active material composition according to any one of claims 19 to 51, wherein: The one or more coating layers independently include pyrophosphate, the interplanar spacing of the pyrophosphate is in the range of 0.293-0.470nm, optionally 0.297-0.462nm or 0.293-0.326nm, more optionally 0.300-0.310nm, and the angle of the crystal direction (111) is in the range of 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, and further optionally 29.00°-30.00°; and / or, The one or more coating layers independently include phosphate, the interplanar spacing of the phosphate is in the range of 0.244-0.425 nm, optionally 0.345-0.358 nm, and the angle of the crystal direction (111) is in the range of 20.00°-37.00°, optionally 24.25°-26.45°; Optionally, the first coating layer or the second coating layer comprises phosphate.
53. The positive electrode active material composition according to any one of claims 1 to 52, wherein: The lattice change rate of the first positive electrode active material before and after complete lithium deintercalation is 50% or less, optionally 9.8% or less, more optionally 8.1% or less, further optionally 7.5% or less, further optionally 6% or less, further optionally 4% or less, further optionally 3.8% or less, further optionally 2.0-3.8%; and / or, The Li / Mn antisite defect concentration of the first positive electrode active material is 5.3% or less, optionally 5.1% or less, more optionally 4% or less, further optionally 2.2% or less, further optionally 2% or less, further optionally 1.5%-2.2% or 0.5% or less; and / or, The surface oxygen valence state of the first positive electrode active material is -1.55 or less, optionally -1.82 or less, more optionally -1.88 or less, further optionally -1.90 or less or -1.98 to -1.88, further optionally -1.98 to -1.89, further optionally -1.98 to -1.
90.
54. The positive electrode active material composition according to any one of claims 5, 8 to 53, wherein: The positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045, w a represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition, y is the molar amount of the B element in 1 mole of the compound represented by formula (I), V B is the voltage platform of the B element in the compound represented by formula (I), with the unit being V (volt).
55. The positive electrode active material composition according to any one of claims 1 to 54, wherein: The second positive electrode active material includes a layered oxide.
56. The positive electrode active material composition according to claim 55, wherein The second positive electrode active material includes a compound represented by formula (II), Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 , (II) A 1 Includes one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1 including Mn and / or Al; C 1 Including selected from IA group, IIA group, IIIA group, IVA group, VA group, VIA group, IIB group, One or more elements from Group IIIB, Group IVB, Group VB, Group VIB and Group VIII; D 1 It includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.
57. The positive electrode active material composition according to claim 56, wherein A 1 including one or more elements selected from the group consisting of Na, K, Mg, Rb, Zn, and Zr; and / or, C 1 including one or more elements selected from the group consisting of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and optionally including one or more elements selected from the group consisting of Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, B; and / or, D 1 comprising one or more elements selected from N, S, F, Cl and Br, and optionally comprising S and / or F; and / or, a1 is selected from the range of 0.9 to 1.1; and / or, b1 is selected from the range of 0 to 0.1; and / or, c1 is selected from the range of 0.314 to 0.990, and may be selected from the range of 0.500 to 0.990; and / or, d1 is selected from the range of 0 to 0.320, and may be selected from the range of 0 to 0.150; and / or, e1 is selected from the range of 0.001 to 0.450, and may be selected from the range of 0.005 to 0.4; and / or, f1 is selected from the range of 0.001 to 0.1, and may be selected from the range of 0.001 to 0.05; and / or, g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.
05.
58. The positive electrode active material composition according to claim 56 or 57, wherein The second positive electrode active material includes a core and a shell covering the core, The core comprises the compound represented by formula (II); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
59. The positive electrode active material composition according to claim 58, wherein The one or more coating layers each independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.
60. The positive electrode active material composition according to claim 58 or 59, wherein The shell includes a coating; Optionally, the coating layer includes one or more selected from phosphates, pyrophosphates, and oxides.
61. The positive electrode active material composition according to claim 58 or 59, wherein: The shell includes a first coating layer covering the core and a second coating layer covering the first coating layer; Optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphates, pyrophosphates, and oxides; More optionally, the first coating layer includes one or more selected from phosphates and oxides, and the second coating layer includes one or more selected from pyrophosphates and oxides.
62. The positive electrode active material composition according to any one of claims 58 to 61, wherein The coating amount of the shell is 0.005 wt % to 1 wt %, and optionally 0.01 wt % to 0.5 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.
63. A positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material, the positive electrode active material comprising the positive electrode active material composition according to any one of claims 1 to 62, optionally, the content of the positive electrode active material composition in the positive electrode film layer is 90 weight % to 99.5 weight %, more optionally 95 weight % to 99.5 weight %, based on the total weight of the positive electrode film layer.
64. The positive electrode sheet according to claim 63, wherein: The positive electrode film layer also includes a third positive electrode active material, which includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel lithium manganese oxide material, and their respective modified compounds, and the modification method includes doping and / or surface coating modification.
65. The positive electrode sheet according to claim 64, wherein: The third positive electrode active material includes a compound represented by formula (III), Li 1+p1 A 2 q1 B 2 r1 O s1 , (III) 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 comprises one or more elements selected from Co, Ni, Mn, and Al; B 2 comprises one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.
66. The positive electrode sheet according to claim 65, wherein: The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (III); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
67. The positive electrode sheet according to claim 66, wherein: The one or more coating layers independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.
68. The positive electrode sheet according to claim 66 or 67, wherein: The coating amount of the shell is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.
69. The positive electrode sheet according to claim 64, wherein: The third positive electrode active material includes a compound represented by formula (IV), Li a2 A 3 x2 B 3 y2 P 1-z2 C 3 z2 O 4-n2 D 3 n2 , (IV) A 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 Includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.
5.
70. The positive electrode sheet according to claim 69, wherein: A 3 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, B 3 The invention comprises one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may be selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, One or more elements selected from Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or, C 3 comprising one or more elements selected from B (boron), S, Si and N; and / or, D 3 comprising one or more elements selected from S, F, Cl and Br; and / or, a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or, x2 is selected from the range of 0.001 to 0.005; and / or, y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or, z2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or, n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.
005.
71. The positive electrode sheet according to claim 69 or 70, wherein: The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (IV); The shell is a shell according to any one of claims 19 to 52.
72. The positive electrode sheet according to claim 64, wherein: The third positive electrode active material includes a compound represented by formula (V), LiMn t1 A 4 2-t1 O4, (V) t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.
73. The positive electrode sheet according to claim 72, wherein: The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (V); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.
74. The positive electrode sheet according to claim 73, wherein: The one or more coating layers independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.
75. The positive electrode sheet according to claim 73 or 74, wherein: The coating amount of the shell is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.
76. The positive electrode sheet according to claim 75, wherein: The positive electrode film layer includes a positive electrode binder and / or a positive electrode conductor; Optionally, the positive electrode binder includes a vinylidene fluoride homopolymer and / or copolymer, and more optionally, the comonomer includes one or more of tetrafluoroethylene, hexafluoropropylene, and propylene; and / or, Optionally, the weight average molecular weight of the positive electrode binder is 300,000 to 2,000,000.
77. The positive electrode sheet according to claim 75 or 76, wherein: The positive electrode film layer further includes functional additives, wherein the functional additives include one or more of a dispersant, a plasticizer, a pore former, a water removal additive, an acid removal additive, and a lithium supplement; and / or, The positive electrode plate also includes a functional coating, which is located between the positive electrode current collector and the positive electrode film layer. The functional coating is located between and / or on the surface of the positive electrode film layer away from the positive electrode current collector, and the functional coating includes one or more of conductive carbon, a water removal additive, an acid removal additive, and a lithium supplement.
78. A battery comprising the positive electrode active material composition according to any one of claims 1 to 62 or the positive electrode sheet according to any one of claims 63 to 77.
79. The battery of claim 78, wherein The battery includes an electrolyte, and the electrolyte includes one or more of a liquid electrolyte, an all-solid electrolyte, and a gel electrolyte.
80. The battery of claim 79, wherein The liquid electrolyte comprises a lithium salt, a non-aqueous solvent for dissolving the lithium salt, and an optional additive; Optionally, the lithium salt includes one or more selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2, LiBF2C2O4, LiPO2F2; and / or, Optionally, the concentration of the lithium salt is 0.5-1.5 mol / L; and / or, Optionally, the non-aqueous solvent includes one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, cyclopentane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, tetrahydrofuran; and / or, Optionally, the additive includes one or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, and optionally includes vinylene carbonate, 1,2,3-tris(2-cyanoethoxy)propane, 1-aza-12-crown 4-ether, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate.
81. A battery according to any one of claims 78 to 80, wherein The battery comprises a negative electrode plate, the negative electrode plate comprises a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer comprises a negative electrode active material, and the negative electrode active material comprises one or more of a carbon-based material, a silicon-based material, a tin-based material and lithium titanate; Optionally, the negative electrode active material includes a carbon-based material, or a combination of a carbon-based material and a silicon-based material; Optionally, the porosity of the negative electrode film layer is 20% to 50%.
82. The battery of claim 81, wherein The negative electrode active material includes a carbon-based material, and the carbon-based material includes graphite, or a combination of graphite and hard carbon; or The negative electrode active material includes a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of the silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.
83. The battery according to claim 81 or 82, wherein The negative electrode plate further comprises a functional coating, wherein the functional coating is located between the negative electrode current collector and the negative electrode film layer and / or located on a surface of the negative electrode film layer away from the negative electrode current collector; optionally, the functional coating comprises carbon; and / or, The negative electrode film layer also includes a lithium replenishing material. Optionally, the lithium replenishing material includes one or more of lithium foil, lithium strip, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent includes one or more of Li-aromatic hydrocarbons, complexes of Li-aromatic hydrocarbons and ether solvents, and may further include one or more of naphthalene lithium and biphenyl lithium-dimethyl ether.
84. A battery according to any one of claims 81 to 83, wherein The negative electrode plate includes a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer respectively arranged on two surfaces of the negative electrode current collector. Optionally, the thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:
5.
85. A battery according to any one of claims 78 to 80, wherein The battery comprises a negative electrode plate, and the negative electrode plate does not comprise a negative electrode active material capable of inserting and removing lithium ions; Optionally, the negative electrode plate comprises a lithium plate or a lithium alloy plate; or, The negative electrode plate includes a mesh or foam three-dimensional skeleton layer.
86. A battery according to any one of claims 78 to 85, wherein The battery includes a separator including a porous substrate.
87. The battery of claim 86, wherein The isolation membrane further comprises a coating located on at least one surface of the porous substrate. Optionally, the coating comprises one or more of inorganic heat-resistant particles and organic heat-resistant particles.
88. The battery of claim 86 or 87, wherein The porosity of the isolation film is 10%-40%.
89. An electrical device comprising the battery according to any one of claims 78 to 88.
Citation Information
Patent Citations
Lithium ion battery anode material and lithium ion battery and anode containing the material
CN101207197A
Mixed positive material of lithium-ion power battery
CN103618084A
Positive electrode active material, positive electrode plate, lithium ion soft package battery cell, lithium ion battery pack and application of lithium ion battery pack
CN112952050A
Composite positive electrode material as well as preparation method and application thereof
CN115241449A
Composite compound with mixed crystalline structure
US20090220860A1
Cited By
Secondary battery and electric device
CN120432492A
Lithium-ion secondary battery and electrical device