Ultra-thin heat insulation gasket, and preparation method therefor and use thereof

By developing ultra-thin thermal insulation gaskets with a fiber/aerogel composite layer structure, the problem of fire spread caused by spontaneous combustion and thermal runaway of lithium-ion batteries in new energy vehicles is solved, providing high-temperature insulation and mechanical strength to meet the fire protection of battery packs. Thermal insulation and insulation requirements.

WO2024216625A1PCT designated stage expired Publication Date: 2024-10-24ZHONGKE RUNZI (CHONGQING) AEROGEL RES INST CO LTD

Patent Information

Application Number
PCT/CN2023/089761
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The spontaneous combustion problem of lithium-ion batteries in new energy vehicles has not been completely solved, especially in the case of thermal runaway, causing fire to spread and causing serious safety threats and damage. Existing flame-retardant and thermal insulation materials cannot meet the requirements of thinness, high strength, vibration reduction, Temperature resistance, low thermal conductivity and waterproof and moisture-proof requirements.

Method used

Develop an ultra-thin thermal insulation gasket with a fiber/aerogel composite layer structure, including basalt fiber and polyimide, that has high tensile strength and stiffness and maintains excellent thermal insulation and insulation under high temperature conditions performance, suitable for fireproof and heat insulation design of battery packs.

Benefits of technology

This thermal insulation gasket provides excellent thermal insulation performance at high temperatures, as well as excellent mechanical strength and impact resistance. It can effectively block thermal runaway, delay the spread of fire, and meet the thermal insulation and insulation requirements of new energy vehicle battery packs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089761_24102024_PF_FP_ABST
    Figure CN2023089761_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are an ultra-thin heat insulation gasket, and a preparation method therefor and the use thereof. The heat insulation gasket is prepared according to the present invention. The heat insulation gasket of the present invention has excellent heat insulation performance at a high temperature, for example, at 500°C or above, and can also maintain the insulation performance at the high temperature, and also has excellent mechanical strength and impact resistance. The heat insulation gasket of the present invention, which is applied to a battery pack of a new energy vehicle, can meet both flame-retardant and heat-insulation requirements and an electrical insulation requirement, and also meets requirements in terms of mechanical strength and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Ultra-thin thermal insulation gasket and its preparation method and application Technical Field

[0001] The present invention belongs to the technical field of thermal insulation materials, and in particular relates to an ultra-thin thermal insulation gasket, a preparation method thereof, and an application thereof in a power battery. Background Art

[0002] With the introduction of carbon neutrality goals, new energy vehicles (NEVs) have experienced rapid growth due to their carbon neutrality. Furthermore, technological advancements have led to an increasing number of consumers choosing to purchase NEVs. While batteries are a key component of NEVs, safety concerns associated with these vehicles have also gradually become apparent. Batteries, particularly lithium-ion batteries, are prone to spontaneous combustion. These combustion hazards pose a serious threat to life and property, hindering the further development and adoption of NEVs. To address the issue of spontaneous combustion, major automakers and battery manufacturers have conducted extensive research. While some progress has been made, the issue, particularly of lithium-ion batteries, remains largely unresolved. Statistical analysis of lithium-ion battery spontaneous combustion cases reveals that in most cases, spontaneous combustion occurs when a small, abnormally performing lithium-ion battery cell undergoes spontaneous combustion or thermal runaway, triggering combustion of surrounding, healthy battery cells, which in turn triggers a wider range of battery combustion.

[0003] At present, the intrinsic safety of batteries cannot be fully guaranteed. Therefore, when it is impossible to solve the problem of natural or thermal runaway of batteries, we can also start with passive safety and design fireproof and heat-insulating batteries for cells, battery packs and battery packs to prevent the burning battery cells or battery packs from igniting adjacent batteries, and block the spread of thermal runaway from the runaway cells to the surrounding areas, so as to reduce the damage to the battery pack and the incidental destructive effects. Designing the battery pack with fireproof and heat-insulating design can also buy more escape time for the passengers and delay the spread of fire.

[0004] When designing fireproof and heat-insulating battery cells, battery packs, and battery packs, using flame-retardant insulation sheets between them is a very effective technical approach. However, the use of new energy vehicles has put forward new requirements for flame-retardant and heat-insulating materials, such as lightness, high strength, vibration reduction, temperature resistance, low thermal conductivity, non-toxic gas generation, waterproof, moisture-proof, shockproof, and electrical insulation. Therefore, it is urgent to develop an aerogel heat-insulating and flame-retardant mat and its production method that are suitable for the use of new energy vehicles.

[0005] Summary of the Invention

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A thermal insulation gasket, wherein the insulation performance of the thermal insulation gasket meets at least one of the following conditions:

[0008] A1) Breakdown voltage: not less than 10KV / mm;

[0009] A2) Volume resistivity: greater than or equal to 1×10 13 Ω / cm.

[0010] A thermal insulation gasket, wherein the strength of the thermal insulation gasket meets at least one of the following conditions:

[0011] B1) The tensile strength parameter is not less than 2MPa;

[0012] B2) When the thickness is not greater than 3mm, the stiffness shall not be less than 85g / cm.

[0013] A thermal insulation gasket having the following properties:

[0014] The insulation performance meets at least one of the following conditions:

[0015] A1) Breakdown voltage: not less than 10KV / mm;

[0016] A2) Volume resistivity: greater than or equal to 1×10 13 Ω / cm;

[0017] and, the strength satisfies at least one of the following conditions:

[0018] B1) The tensile strength parameter is not less than 2MPa;

[0019] B2) When the thickness is not greater than 3mm, the stiffness shall not be less than 85g / cm.

[0020] According to the present invention, the thickness of the thermal insulation gasket is no more than 3 mm.

[0021] According to the present invention, the thermal insulation gasket contains at least one fiber / aerogel composite layer; the fiber / aerogel composite layer includes a substrate, aerogel and polyimide, the substrate is fiber, and the substrate is filled with aerogel; the fiber includes basalt fiber.

[0022] According to the present invention, the thermal insulation gasket at least comprises:

[0023] An intermediate layer, which is a polymer sheet and / or a metal foil and is used for structural support and / or bonding;

[0024] The first outer layer is located on one side surface of the middle layer. When used in a battery pack, the first outer layer faces the battery pack. The first outer layer is the fiber / aerogel composite layer.

[0025] The present invention also provides a method for preparing a thermal insulation gasket, the method comprising:

[0026] 1) Preparing silica sol: mixing a silicon source, water, and an alcohol solvent to prepare silica sol;

[0027] 2) preparing a gel: introducing a fiber preform into the silica sol of step 1) to obtain a gel;

[0028] 3) Solvent replacement: using a replacement solvent to replace the liquid in the gel to obtain an intermediate;

[0029] 4) Drying: The intermediate of step 3) is subjected to supercritical drying to obtain a fiber / aerogel composite layer, namely the thermal insulation gasket.

[0030] According to the present invention, the preparation method further comprises the following steps:

[0031] 5) Providing a structural reinforcement layer: Providing an adhesive layer and / or an outer film layer on the surface of the fiber / aerogel composite layer in step 4) to obtain a thermal insulation gasket including the adhesive layer and / or the outer film layer.

[0032] According to the present invention, the preparation method further comprises the following steps:

[0033] 6) Combining the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) with the intermediate layer to obtain a thermal insulation gasket with a composite structure.

[0034] According to the present invention, the preparation method further comprises the following steps:

[0035] 7) The other side surface of the intermediate layer in step 6) is combined with the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) to obtain a thermal insulation gasket with a sandwich structure.

[0036] The present invention also provides the use of the thermal insulation gasket as a thermal insulation material and / or insulating material in a battery. Beneficial effects

[0037] The present invention provides a thermal insulation gasket, which has excellent thermal insulation performance under high temperature conditions (for example, above 500°C). Furthermore, the thermal insulation gasket can also maintain insulation performance under high temperature conditions. Furthermore, the thickness of the thermal insulation gasket is extremely low, and it is completely suitable for use as an insulation material in batteries, especially power batteries.

[0038] In addition, the present invention also provides a thermal insulation gasket, which has excellent mechanical properties in an ultra-thin state, such as excellent mechanical strength and stiffness, and is completely suitable for use as a thermal insulation material in batteries, especially power batteries.

[0039] Furthermore, the present invention provides a thermal insulation gasket, which has both thermal insulation performance and strength, and has extremely low thickness. Applying the thermal insulation gasket of the present invention to the battery pack of new energy vehicles can meet the flame retardant thermal insulation requirements, the electrical insulation requirements, and the mechanical strength and impact resistance requirements.

[0040] The heat-insulating gasket of the present invention can be easily inserted between battery pack components during the battery pack assembly process, and the assembly process is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] FIG1 is a schematic diagram of the structure of a three-layer thermal insulation gasket of the present invention.

[0042] FIG2 is a schematic diagram of a three-layer thermal insulation gasket of the present invention, wherein the first outer layer and the second outer layer are made of different materials.

[0043] FIG3 is a schematic diagram of a thermal insulation gasket including an adhesive layer according to the present invention.

[0044] FIG4 is a schematic diagram of a three-layer thermal insulation gasket containing an adhesive layer according to the present invention.

[0045] FIG5 is a schematic diagram of a thermal insulation gasket and a battery according to the present invention.

[0046] FIG6 is a schematic diagram of a thermal insulation gasket and multiple battery cells according to the present invention.

[0047] FIG7 is a schematic diagram of a battery pack containing a thermal insulation gasket according to the present invention.

[0048] FIG8 is a schematic diagram of a battery separator and a hexagonal battery cell according to the present invention.

[0049] FIG9 is a schematic diagram showing the state change of the polyimide in the fiber of the present invention after heat shrinkage.

[0050] Figure numerals: thermal insulation gasket-100, first outer layer-110, second outer layer-120, middle layer-130, outer film layer-140, fiber / aerogel composite layer-150, fiber-151, polyimide-152, silicon micropowder-153, adhesive layer-160, battery pack-200, battery cell-210, electrode-220, battery casing-230. DETAILED DESCRIPTION

[0051] [Thermal insulation gasket]

[0052] As mentioned above, the present invention provides a thermal insulation gasket, the insulation performance of which satisfies at least one of the following conditions:

[0053] A1) Breakdown voltage: not less than 10KV / mm;

[0054] A2) Volume resistivity: greater than or equal to 1×10 13 Ω / cm.

[0055] The breakdown voltage and volume resistivity in the present invention are tested at 500°C.

[0056] According to an embodiment of the present invention, the volume resistivity is greater than or equal to 1×10 17 Ω / cm.

[0057] The present invention also provides a thermal insulation gasket, the strength of which satisfies at least one of the following conditions:

[0058] B1) The tensile strength parameter is not less than 2MPa;

[0059] B2) When the thickness is not greater than 3mm, the stiffness shall not be less than 85g / cm.

[0060] According to an embodiment of the present invention, the tensile strength parameter is, for example, not less than 10 MPa; or, for example, not less than 30 MPa; further, for example, not less than 50 MPa; further, for example, not less than 100 MPa; further, for example, not less than 200 MPa; further, for example, not less than 500 MPa; illustratively, it can be 10 MPa, 20 MPa, 30 MPa, 50 MPa, 100 MPa, 150 MPa, 200 MPa, 300 MPa, 400 MPa, 500 MPa, 600 MPa, 700 MPa, 800 MPa or 900 MPa.

[0061] According to an embodiment of the present invention, when the thickness is no greater than 2 mm, for example no greater than 1 mm, the stiffness is no less than 85 g / cm.

[0062] The present invention also provides a thermal insulation gasket, the insulation performance and strength of the thermal insulation gasket have the value ranges as described above.

[0063] According to an embodiment of the present invention, the thickness of the thermal insulation gasket is not greater than 3 mm, for example not greater than 2 mm, and also for example not greater than 1 mm, and illustratively can be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 1 mm or 2 mm.

[0064] According to an embodiment of the present invention, the thermal insulation gasket contains at least one fiber / aerogel composite layer; the fiber / aerogel composite layer includes a substrate and aerogel, the substrate is fiber, and the substrate is filled with aerogel; the fiber includes basalt fiber.

[0065] Research has found that the thermal insulation gaskets produced using basalt fiber as a substrate in the present invention have a higher hardness than those made with glass fiber and other fibers. Furthermore, compared to aerogels using other fiber types, the thermal insulation gaskets produced by the present invention have less fuzz and are smoother and cleaner.

[0066] According to an embodiment of the present invention, the aerogel can be selected from aerogels or modified aerogels known in the art, and preferably an aerogel with good high temperature resistance, such as the rare earth-doped silica aerogel prepared in Chinese patent document CN113651334A.

[0067] According to an embodiment of the present invention, the fiber / aerogel composite layer further comprises polyimide.

[0068] Preferably, the polyimide is disposed in the aerogel and / or the fiber. Specifically, the polyimide exists in the aerogel and / or the fiber in a cross-linked form.

[0069] According to an embodiment of the present invention, the aerogel content in the thermal insulation gasket is at least 1wt%, preferably 1wt% to 30wt%, more preferably 13wt% to 18wt%, for example 10wt%, 15wt%, 20wt%, or 25wt%.

[0070] According to an embodiment of the present invention, the aerogel is filled in the interior and / or surface of the substrate.

[0071] According to the embodiment of the present invention, the diameter and length of the fiber are not specifically limited, as long as the composite layer can be obtained. For example, the diameter of the fiber is 10 μm to 20 μm; the length of the fiber is 6 mm to 25 mm.

[0072] According to an embodiment of the present invention, the surface density (gram weight) of the thermal insulation gasket is 100-200 g / m 2 , for example, 150 to 200 g / m 2 , for example 160g / m 2 , 170g / m 2 , 180g / m 2 , 190g / m 2 .

[0073] According to an embodiment of the present invention, the fibers may further include glass fibers and / or other fibers.

[0074] Preferably, the other fibers are selected from at least one of aluminum silicate fibers, alumina fibers, mullite fibers, and SiO2 ceramic nanofibers.

[0075] According to a preferred embodiment of the present invention, the fibers include basalt fibers and glass fibers. Further, the mass ratio of the basalt fibers to the glass fibers is (6-8):(4-2), for example, 7:3.

[0076] According to an embodiment of the present invention, the substrate is preferably a fiber felt or a fiber cloth, for example, a fiber woven cloth.

[0077] According to a preferred embodiment of the present invention, the substrate is a fiber woven fabric obtained by weaving a mixture of basalt fiber and glass fiber and / or other fibers in a certain proportion, preferably by weaving a mixture of basalt fiber and glass fiber in a certain proportion. In the present invention, the fiber woven fabric obtained by weaving a mixture of basalt fiber and glass fiber in a certain proportion as the substrate increases both the hardness and thermal insulation properties of the fiber woven fabric.

[0078] Preferably, when mixed and spun, the mass ratio of the basalt fiber to the glass fiber and / or other fibers is (6-8):(4-2), for example, 7:3.

[0079] According to an embodiment of the present invention, the thermal insulation gasket further comprises an intermediate layer, and the intermediate layer is provided on any one surface of the fiber / aerogel composite layer.

[0080] According to an embodiment of the present invention, the intermediate layer is a polymer sheet and / or a metal foil, which is used for structural support and / or bonding.

[0081] According to an embodiment of the present invention, the polymer sheet may be a polyethylene (PE) sheet or a polyimide (PI) sheet.

[0082] According to an embodiment of the present invention, the metal foil may be aluminum foil or copper foil.

[0083] According to an embodiment of the present invention, the thermal insulation gasket comprises at least:

[0084] middle layer;

[0085] a first outer layer, the first outer layer being located on one side surface of the middle layer, and when used in a battery pack, the first outer layer faces the battery pack;

[0086] The first outer layer is a fiber / aerogel composite layer, wherein the base material of the fiber / aerogel composite layer contains basalt fibers.

[0087] According to an embodiment of the present invention, the thermal insulation gasket further includes a second outer layer, which is located on the other side surface of the middle layer. When used in a battery pack, the second outer layer faces away from the battery pack.

[0088] According to an embodiment of the present invention, the second outer layer and the first outer layer may be the same or different. Preferably, the second outer layer is a fiber / aerogel composite layer, and the second outer layer may or may not contain basalt fibers.

[0089] Exemplarily, the thermal insulation gasket has a sandwich structure, which includes a first outer layer, a middle layer and a second outer layer in sequence; the first outer layer and the second outer layer are the same, and are both selected from a fiber / aerogel composite layer containing only basalt fibers in the base material.

[0090] Exemplarily, the thermal insulation gasket has a sandwich structure, including a first outer layer, a middle layer and a second outer layer in sequence; the first outer layer and the second outer layer are the same, and are both selected from a fiber / aerogel composite layer containing basalt fiber and glass fiber in the base material.

[0091] Exemplarily, the thermal insulation gasket has a sandwich structure, which includes a first outer layer, a middle layer and a second outer layer in sequence; the first outer layer is a fiber / aerogel composite layer containing basalt fiber in the base material; the second outer layer is a fiber / aerogel composite layer containing only glass fiber in the base material.

[0092] Exemplarily, the thermal insulation gasket has a sandwich structure, which includes a first outer layer, a middle layer and a second outer layer in sequence; the first outer layer is a fiber / aerogel composite layer whose base material contains basalt fiber and glass; the second outer layer is a fiber / aerogel composite layer whose base material contains only glass fiber.

[0093] According to an embodiment of the present invention, the thickness of the first outer layer is 0.1-1.5 mm, for example, 0.5 mm or 1 mm.

[0094] According to an embodiment of the present invention, the thickness of the intermediate layer is 0.1-0.5 mm, for example, 0.2 mm, 0.3 mm, or 0.4 mm.

[0095] According to an embodiment of the present invention, the thickness of the second outer layer is 0.1-1.5 mm, for example, 0.5 mm or 1 mm.

[0096] The study found that using solid hot melt glue or adhesive to combine the first outer layer and the middle layer, or the middle layer and the second outer layer, the hardness increased significantly after treatment, and no additional spraying of glue was required after treatment.

[0097] According to a preferred embodiment of the present invention, the amount of solid hot melt glue or adhesive used in the thermal insulation gasket is 10g / m 2 ~20g / m2 , preferably 15g / m 2 ~20g / m 2 , for example 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 .

[0098] According to a preferred embodiment of the present invention, the surface of the fiber / aerogel composite layer further includes a structural reinforcement layer (eg, an adhesive layer and / or an outer film layer), that is, the structural reinforcement layer is at least located on at least one surface of the fiber / aerogel composite layer.

[0099] According to an embodiment of the present invention, if the thermal insulation gasket includes an intermediate layer, the structural reinforcement layer may be located between the fiber / aerogel composite layer and the intermediate layer, or located on a surface of the fiber / aerogel composite layer away from the intermediate layer.

[0100] According to an embodiment of the present invention, the outer film layer may be a heat shrinkable film.

[0101] Preferably, the heat shrinkable film may be at least one of a polyethylene (PE) heat shrinkable film, a polyvinyl chloride (PVC) heat shrinkable film, a multi-layer co-extruded polyolefin heat shrinkable film (POF), and a polyimide (PI) heat shrinkable film, preferably a PI heat shrinkable film.

[0102] According to an embodiment of the present invention, when the surface of the fiber / aerogel composite layer includes an adhesive layer, the outer film layer is located on the surface of the adhesive layer.

[0103] According to an embodiment of the present invention, the adhesive layer is obtained by the following surface treatment method: an adhesive is coated on the surface of the fiber / aerogel composite layer to obtain the adhesive layer.

[0104] According to an embodiment of the present invention, after the adhesive layer is provided, the surface density of the thermal insulation gasket can be further increased by up to 50 g / m 2 , for example, the surface density can be increased by 10g / m 2 , 30g / m 2 or 50g / m 2 .

[0105] According to an embodiment of the present invention, the adhesive is selected from rubber-based adhesives, resin-based adhesives, polysulfide-based adhesives, acrylic-based adhesives, oil-based adhesives, polyurethane-based adhesives, white latex, and acrylate adhesives.

[0106] According to the embodiment of the present invention, before the adhesive is applied, a pre-treatment is required, which specifically includes:

[0107] Method 1: The fiber / aerogel composite layer is subjected to a hydrophobic-to-hydrophilic treatment: a) spraying a hydrophilic modifier on the surface of the fiber / aerogel composite layer; or b) baking the fiber / aerogel composite layer at a temperature above 200° C. (e.g., 250° C., 300° C., etc.);

[0108] Or, method 2: the adhesive is modified with organosilicon before coating.

[0109] The study found that when applying the adhesive, the adhesive is not easy to adhere to the surface of the fiber / aerogel composite layer due to the hydrophobicity of the aerogel. After the above pretreatment, the adhesive can be more evenly coated on the surface of the fiber / aerogel composite layer.

[0110] According to an embodiment of the present invention, in method one, the hydrophilic modifier is an aqueous solution of a surfactant and a low surface tension solvent or a low surface tension solvent or an aqueous solution of low surface tension; the surfactant is one or more of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants; the anionic surfactant is one or more of fatty alcohol phosphate salts, fatty alcohol polyoxyethylene ether phosphate salts, alkyl sulfates, fatty alcohol polyoxyethylene ether sulfates, glycerol fatty acid ester sulfates, sulfated ricinoleates, cycloalkane sulfates, fatty amide alkyl sulfates, alkylbenzene sulfonates, alkyl sulfonates, fatty acid methyl ester ethoxylate sulfonates, fatty acid methyl ester sulfonates, and fatty alcohol polyoxyethylene ether carboxylates; the cationic surfactant is an aliphatic ammonium salt; the amphoteric surfactant is one or more of alkyl amino acids, carboxylic acid betaines, sulfobetaines, phosphate betaines, and alkyl hydroxyl amine oxides; the nonionic surfactant is an aliphatic polyester, One or more of alkylphenol polyoxyethylene ether, high-carbon fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, fatty acid methyl ester ethoxylate, polypropylene glycol ethylene oxide adduct, sorbitan ester, sucrose fatty acid ester, and alkyl ester amide; the low surface tension solvent is a mixture of one or more of acetone, n-hexane, n-pentane, n-heptane, ethanol, isopropanol, tert-butanol, propylene glycol, and glycerol.

[0111] According to an embodiment of the present invention, in method 1, the organosilicon is selected from, for example, silane coupling agent ethyl orthosilicate, vinyl silane, aminosilane, methacryloxysilane, isobutyl triethoxysilane, propyl trimethoxysilane, triethoxysilane, and specifically KH-550 and KH-560.

[0112] According to an embodiment of the present invention, in method 2, the adhesive is preferably an acrylic adhesive, which has strong adhesion to polar organic materials and good alkali resistance.

[0113] According to an embodiment of the present invention, in the surface treatment method, the adhesive is applied by at least one method selected from spraying, dipping, and roller coating, preferably dipping.

[0114] In the present invention, the amount of adhesive is not specifically limited. The amount of adhesive is determined according to the hardness required by the thermal insulation gasket, and after the adhesive layer is provided, the surface density of the thermal insulation gasket increases to 30g / m 2 For example, the amount of the adhesive used is not more than 15 g / m2 per square meter of the fiber / aerogel composite layer. 2 .

[0115] [Method for preparing thermal insulation gasket]

[0116] The present invention also provides a method for preparing the above-mentioned thermal insulation gasket, the method comprising:

[0117] 1) Preparing silica sol: mixing a silicon source, water, and an alcohol solvent to prepare silica sol;

[0118] 2) preparing a gel: introducing a fiber preform into the silica sol of step 1) to obtain a gel;

[0119] 3) Solvent replacement: using a replacement solvent to replace the liquid in the gel to obtain an intermediate;

[0120] 4) Drying: The intermediate of step 3) is subjected to supercritical drying to obtain a fiber / aerogel composite layer, namely the thermal insulation gasket.

[0121] According to an embodiment of the present invention, the preparation method further comprises the following steps:

[0122] 5) Providing a structural reinforcement layer: optionally providing a structural reinforcement layer (eg, including an adhesive layer and / or an outer film layer) on the surface of the fiber / aerogel composite layer in step 4) to obtain a fiber / aerogel composite layer including a structural reinforcement layer, i.e., the thermal insulation gasket.

[0123] According to an embodiment of the present invention, step 1) specifically includes: adding a silicon source, an alcohol solvent and water into a container in proportion, mixing, adding a hydrolysis catalyst, mixing again, and standing to obtain a silica sol.

[0124] According to an embodiment of the present invention, in step 1), the molar ratio of the silicon source, alcohol solvent and water is 1:(7-20):3; specifically, the silicon source, alcohol solvent and water are sequentially added to the container in a molar ratio of 1:8-15:3.

[0125] According to an embodiment of the present invention, in step 1), the silicon source is selected from at least one of sodium silicate, ethyl orthosilicate, methyl orthosilicate, tetrapropoxysilane, tetrabutoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane.

[0126] According to an embodiment of the present invention, in step 1), the alcohol solvent is methanol, ethanol or a combination thereof.

[0127] According to an embodiment of the present invention, polyimide powder may optionally be added to the silica sol in step 1). Preferably, the polyimide powder has a particle size range of 500-1200 mesh, for example, 600 mesh, 700 mesh, 800 mesh, 900 mesh, 1000 mesh, 1100 mesh, or 1200 mesh. Preferably, the amount of polyimide powder added is 0.5%-5% of the mass of the silica sol.

[0128] According to an embodiment of the present invention, in step 1), the time for the first mixing is 10 min to 15 min.

[0129] According to an embodiment of the present invention, in step 1), a hydrolysis catalyst may be added to the silica sol to accelerate the hydrolysis of the silicon source and obtain the silica sol more quickly.

[0130] Preferably, the hydrolysis catalyst is selected from hydrochloric acid, oxalic acid, nitric acid, sulfuric acid, phosphoric acid or a combination thereof.

[0131] Preferably, the hydrolysis catalyst is added in the form of a solution, the mass fraction of the hydrolysis catalyst solution is 0.05-0.1 wt%, and the molar ratio of the silicon source to the hydrolysis catalyst can be 1:(10-4).

[0132] According to an embodiment of the present invention, silicon micropowder may be added to the silica sol in step 1). Preferably, the silicon micropowder has a particle size range of 600-1500 mesh. Preferably, the silicon micropowder is amorphous silicon micropowder. Preferably, the amount of silicon micropowder added is 1%-15% of the molar ratio of the silicon source.

[0133] According to an embodiment of the present invention, a sunscreen may be added to the silica sol in step 1). Preferably, the sunscreen comprises at least one of titanium dioxide, carbon black, SiC, potassium hexatitanate, and ZrO2. Furthermore, the titanium dioxide may be anatase titanium dioxide, fluorine-doped titanium dioxide nanoparticles, or nitrogen-doped titanium dioxide nanoparticles. The addition of the titanium dioxide of the present invention can enhance the sunscreen effect of infrared radiation.

[0134] According to an embodiment of the present invention, in step 2), the fiber preform has a thickness of no greater than 3 mm, such as no greater than 2 mm, and such as no greater than 1 mm, illustratively 0.1 mm, 0.2 mm, 0.5 mm, 1 mm or 2 mm.

[0135] According to an embodiment of the present invention, the fiber preform is selected from basalt fiber preform, glass fiber preform, aluminum silicate fiber preform, alumina fiber preform, mullite fiber preform, and SiO2 ceramic nanofiber preform. Preferably, the fiber preform is a woven fiber preform.

[0136] According to an embodiment of the present invention, the fibers of the fiber preform may optionally contain polyimide powder particles, and the polyimide powder particles have the meaning as described above.

[0137] According to an embodiment of the present invention, in step 2), the method of introducing the fiber preform is specifically as follows:

[0138] After adding a gel catalyst to the silica sol in step 1), pouring it into a fiber preform and allowing it to stand to obtain a gel; or,

[0139] After adding a gel catalyst to the silica sol in step 1), reinforcing fibers and a fiber dispersant are added, and the mixture is allowed to stand to obtain a gel.

[0140] According to an embodiment of the present invention, in step 2), the replacement solvent is selected from methanol, ethanol or a combination thereof.

[0141] According to an embodiment of the present invention, in step 3), the replacement solvent is selected from methanol, ethanol or a combination thereof.

[0142] According to an embodiment of the present invention, in step 4), the conditions for supercritical drying include: A1) after heating and pressurizing to the critical point of the replacement solvent (for example, ethanol), at a constant temperature, slowly releasing the fluid inside the reactor until the internal and external pressures are balanced; A2) when the pressure exceeds 8MPa, slowly release the pressure, and after releasing the pressure to normal pressure, introduce N2 to purge the reactor, and after cooling to room temperature, obtain the fiber / aerogel composite layer. Preferably, in step A1), N2 can be used to pre-fill the reactor before heating, and the pressure of the pre-filled N2 is 1-4MPa. The temperature is raised to above 240°C, and the heating rate is 0.5-2°C / min. Preferably, in step A2), the pressure relief can be carried out by methods known in the art, such as by a cooling device.

[0143] Specifically, the supercritical drying conditions may be: using a replacement solvent (for example, ethanol) as the supercritical drying medium, pre-filling N2 to a pressure in the kettle of 2 MPa, raising the temperature in the kettle to 270°C at a heating rate of 1°C / min, keeping warm for 2 to 4 hours until the pressure in the kettle is 8 to 10 MPa, then slowly releasing the pressure in the kettle to normal pressure, passing N2 into the kettle for purge, and cooling to room temperature to obtain the fiber / aerogel composite layer.

[0144] According to an embodiment of the present invention, in step 5), the outer film layer may be disposed on at least one surface of the fiber / aerogel composite layer or on the surface of the adhesive layer.

[0145] Specifically, the definition of the outer membrane layer is the same as described above.

[0146] In some embodiments, no adhesive layer is provided on the surface of the fiber / aerogel composite layer, and the outer film layer is provided on at least one surface of the fiber / aerogel composite layer.

[0147] In some embodiments, adhesive layers are provided on both surfaces of the fiber / aerogel composite layer, and the outer film layer is provided on the surface of at least one of the adhesive layers.

[0148] In some embodiments, an adhesive layer is provided on one surface of the fiber / aerogel composite layer, and the outer film layer is provided on the surface of the fiber / aerogel composite layer and / or the surface of the adhesive layer.

[0149] Exemplarily, the outer film layer is bonded to one side surface of the fiber / aerogel composite layer to obtain the thermal insulation gasket.

[0150] Exemplarily, the thermal insulation gasket is obtained by bonding the same or different fiber / aerogel composite layers to both side surfaces of the outer film layer.

[0151] According to an embodiment of the present invention, in step 5), the outer film layer is a heat shrinkable film. Furthermore, after the heat shrinkable film is covered on the adhesive layer, it is heated to shrink the heat shrinkable film and adhere to the adhesive layer.

[0152] According to an embodiment of the present invention, in step 5), the method of providing the adhesive layer includes: attaching an adhesive solution to the surface of the fiber / aerogel composite layer by spraying and / or dipping to obtain the adhesive layer.

[0153] Preferably, the spraying comprises spraying the adhesive solution onto the surface of the fiber / aerogel composite layer using a spray gun, with the spray gun port being 20 cm to 50 cm from the first outer layer and / or the second outer layer, and the spray gun being at an angle of 80 to 100° to the first outer layer and / or the second outer layer to ensure uniform spraying. The spray gun flow rate is 10 L to 35 L / h.

[0154] Preferably, the dipping means: dipping the fiber / aerogel composite layer into an adhesive solution for 10-30 seconds and then taking it out.

[0155] Furthermore, after spraying and / or dipping, the coating may be dried naturally or in an oven. Preferably, the drying temperature may be 50°C-90°C.

[0156] According to an embodiment of the present invention, in step 5), the adhesive is selected from rubber-based adhesives, resin-based adhesives, polysulfide-based adhesives, acrylic-based adhesives, oil-based adhesives, polyurethane-based adhesives, white latex, and acrylate adhesives.

[0157] According to an embodiment of the present invention, the adhesive solution includes the following components: 20-40 parts by mass of adhesive, 1-5 parts of gelling agent, 1-3 parts of modifier, 1-5 parts of dispersant, and 37-67 parts of solvent.

[0158] Preferably, the preparation method of the adhesive comprises: adding the components of the adhesive solution in parts by mass into a container, mixing well, heating to 40° C.-60° C., and continuously stirring vigorously for 60-80 minutes; and cooling to room temperature to obtain an adhesive solution.

[0159] Preferably, the adhesive is selected from ethyl cyanoacrylate, epoxy resin adhesive, amino resin adhesive, phenolic resin adhesive, liquid polysulfide rubber, acrylic adhesive, polyurethane adhesive, and polyvinyl acetate.

[0160] Preferably, the gelling aid includes any one of polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene oxide.

[0161] Preferably, the dispersant includes any one of sodium hexametaphosphate, potassium pyrophosphate, and polyacrylamide.

[0162] Preferably, the modifier includes any one of citric acid, potassium citrate, lactic acid, tartaric acid, and potassium tartrate.

[0163] Preferably, the solvent includes at least one of water, methanol, ethanol, and acetone, or a mixed solvent of two or more.

[0164] Preferably, water is optionally added to the adhesive solution, and the water is deionized water. The present invention does not impose any specific limitation on the amount of water in the adhesive solution.

[0165] Preferably, the adhesive solution comprises: 20-30 parts of modified starch, 1-3 parts of polyvinyl alcohol, 1-3 parts of sodium hexametaphosphate or polyacrylamide, 1-2 parts of citric acid, 3-8 parts of magnesium hydroxide, and 50-60 parts of deionized water.

[0166] According to an embodiment of the present invention, when providing the adhesive layer, a pre-treatment is required before spraying and / or dipping, specifically including:

[0167] Method 1: The fiber / aerogel composite layer is subjected to a hydrophobic-to-hydrophilic treatment: a) spraying a hydrophilic modifier on the surface of the fiber / aerogel composite layer; or b) baking the fiber / aerogel composite layer at a temperature above 200° C. (e.g., 250° C., 300° C., etc.);

[0168] Or, in method 2, the adhesive is modified with organic silicon before attachment.

[0169] The study found that when attaching the adhesive, the adhesive is not easy to adhere to the surface of the fiber / aerogel composite layer due to the hydrophobicity of the aerogel. After the above pretreatment, the adhesive can be more evenly attached to the surface of the fiber / aerogel composite layer.

[0170] According to an embodiment of the present invention, after the adhesive layer is provided, the surface density of the thermal insulation gasket can be further increased by up to 50 g / m 2 , for example, the surface density can be increased by 10g / m 2 , 30g / m 2 or 50g / m 2 .

[0171] According to an embodiment of the present invention, the preparation method further comprises the following steps:

[0172] 6) Combining the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) with the intermediate layer to obtain the thermal insulation gasket with a composite structure of the present invention.

[0173] According to an embodiment of the present invention, the preparation method further comprises the following steps:

[0174] 7) The other side surface of the intermediate layer in step 6) is combined with the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) to obtain the thermal insulation gasket with a sandwich structure of the present invention.

[0175] According to an embodiment of the present invention, the intermediate layer has the above-mentioned definition.

[0176] According to an embodiment of the present invention, the bonding can be performed by methods known in the art, such as pressing (specifically, pressing at room temperature or hot pressing, etc.).

[0177] [Thermal insulation gasket and its application]

[0178] The present invention also provides a thermal insulation gasket obtained by the above preparation method.

[0179] According to an embodiment of the present invention, the thermal insulation gasket has the meaning as described above.

[0180] The present invention also provides the use of the thermal insulation gasket as a thermal insulation material and / or insulating material in a battery.

[0181] According to an embodiment of the present invention, the battery is a battery for a power vehicle.

[0182] The technical solutions of the present invention will be described in further detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are encompassed within the scope of protection that the present invention is intended to protect.

[0183] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0184] Example 1

[0185] Preparation of a thermal insulation gasket, which is a single layer of glue-free basalt fiber aerogel with a thickness of 1 mm, specifically includes the following steps:

[0186] (1) 20.8 g of TEOS, 55.2 g of anhydrous ethanol, and 5.4 g of H2O were added to a three-necked flask and mechanically stirred for 15 min. 3.65 g of a 0.05 wt% hydrochloric acid ethanol dilution was added dropwise. After stirring for 120 min, the mixture was sealed and allowed to stand at room temperature for 24 h to obtain a SiO2 sol with a molar ratio of n(TEOS):n(C2H5OH):n(H2O)=1:12:3.

[0187] (2) Add ammonia ethanol dilution solution to the SiO2 sol obtained in step (1) and stir evenly. Then, place 1 mm thick basalt fiber felt into the sol and let it stand until the sol is transformed into gel.

[0188] (3) Using ethanol to perform solvent replacement on the gel in step (2) to replace water and other impurities in the gel.

[0189] (4) The gel was sealed and aged for 24 hours before being supercritically dried. Ethanol was used as the supercritical drying medium and nitrogen was pre-filled to a pressure of 2 MPa in the autoclave. The temperature in the autoclave was raised to 270°C at a heating rate of 1°C / min and kept at that temperature for 2 hours until the pressure in the autoclave reached 10 MPa. The water cooling device was turned on and the pressure in the autoclave was slowly released to atmospheric pressure. N2 was then introduced into the autoclave to purge the autoclave. After cooling to room temperature, a thermal insulation gasket was obtained.

[0190] Example 2

[0191] Preparation of a thermal insulation gasket, which is a single layer of glue-free basalt fiber aerogel with a thickness of 2 mm, specifically includes the following steps:

[0192] (1) 20.8 g of TEOS, 55.2 g of anhydrous ethanol, and 5.4 g of H2O were added to a three-necked flask and mechanically stirred for 15 min. 3.65 g of a 0.05 wt% hydrochloric acid ethanol dilution was added dropwise. After stirring for 120 min, the mixture was sealed and allowed to stand at room temperature for 24 h to obtain a SiO2 sol with a molar ratio of n(TEOS):n(C2H5OH):n(H2O)=1:12:3.

[0193] (2) Add ammonia ethanol dilution solution dropwise to the SiO2 sol obtained in step (1), stir evenly, place 2mm thick basalt fiber felt into the SiO2 sol, and let it stand until the sol is transformed into gel.

[0194] (3) Using ethanol to perform solvent replacement on the gel in step (2) to replace water and other impurities in the gel.

[0195] (4) The gel was sealed and aged for 24 hours before being supercritically dried. Ethanol was used as the supercritical drying medium and nitrogen was pre-filled to a pressure of 2 MPa in the autoclave. The temperature in the autoclave was raised to 270°C at a heating rate of 1°C / min and kept at that temperature for 2 hours until the pressure in the autoclave reached 10 MPa. The water cooling device was turned on and the pressure in the autoclave was slowly released to atmospheric pressure. N2 was then introduced into the autoclave to purge the autoclave. After cooling to room temperature, a thermal insulation gasket was obtained.

[0196] Example 3

[0197] Preparation of a thermal insulation gasket, which is a single layer of adhesive-free polyimide-modified basalt fiber aerogel with a thickness of 2 mm, specifically includes the following steps:

[0198] (1) 20.8 g of TEOS, 55.2 g of anhydrous ethanol, 5.4 g of H2O, and 1.9 g of polyimide powder were added to a three-necked flask and mechanically stirred for 15 min. 3.65 g of a 0.05 wt% hydrochloric acid ethanol dilution was added dropwise. After stirring for 120 min, the mixture was sealed and allowed to stand at room temperature for 24 h to obtain a SiO2 sol with a molar ratio of n(TEOS):n(C2H5OH):n(H2O)=1:12:3.

[0199] (2) Add ammonia ethanol dilution solution dropwise to the SiO2 sol obtained in step (1), stir evenly, place 2 mm thick basalt fiber felt into the sol, and let it stand until the sol is converted into gel.

[0200] (3) Using ethanol to perform solvent replacement on the gel in step (2) to replace water and other impurities in the gel.

[0201] (4) The gel was sealed and aged for 24 hours before being supercritically dried. Ethanol was used as the supercritical drying medium and nitrogen was pre-filled to a pressure of 2 MPa in the autoclave. The temperature in the autoclave was raised to 270°C at a heating rate of 1°C / min and kept at that temperature for 2 hours until the pressure in the autoclave reached 10 MPa. The water cooling device was turned on and the pressure in the autoclave was slowly released to atmospheric pressure. N2 was then introduced into the autoclave to purge the autoclave. After cooling to room temperature, a thermal insulation gasket was obtained.

[0202] Example 4

[0203] A thermal insulation gasket is prepared. The thermal insulation gasket is a single layer of basalt fiber aerogel with a thickness of 2 mm. The preparation method includes the following steps:

[0204] Step 1, preparation of basalt fiber aerogel:

[0205] (1) 20.8 g of TEOS, 55.2 g of anhydrous ethanol, and 5.4 g of H2O were added to a three-necked flask and mechanically stirred for 15 min. 3.65 g of a 0.05 wt% hydrochloric acid ethanol dilution was added dropwise. After stirring for 120 min, the mixture was sealed and allowed to stand at room temperature for 24 h to obtain a SiO2 sol with a molar ratio of n(TEOS):n(C2H5OH):n(H2O)=1:12:3.

[0206] (2) Add ammonia ethanol dilution solution dropwise to the material obtained in step (1), stir evenly, place 2 mm thick basalt fiber felt into the sol, and let it stand until the sol is transformed into gel.

[0207] (3) Using ethanol to perform solvent replacement on the gel in step (2) to replace water and other impurities in the gel.

[0208] (4) The gel was sealed and aged for 24 hours before being supercritically dried. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle reached 2 MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10 MPa. The water cooling device was turned on and the pressure in the kettle was slowly released to atmospheric pressure. N2 was then introduced into the kettle to purge the kettle. After cooling to room temperature, basalt fiber aerogel was obtained.

[0209] Step 2: Set the adhesive layer:

[0210] 1) Hydrophilic modification: The surface of the basalt fiber aerogel was pretreated with ethanol by spraying.

[0211] 2) Glue spraying: Use a spray gun to attach the adhesive solution to the surface of the basalt fiber aerogel treated in step 1) to obtain a thermal insulation gasket; the specific conditions are: the distance between the spray gun port and the thermal insulation gasket is 30 cm, the spray gun and the surface of the thermal insulation gasket are at a 90° angle to ensure uniform spraying, and the spray gun flow rate is 15 L / h.

[0212] The adhesive solution in step 2) specifically comprises: 20 parts of rubber-type adhesive, 1 part of polyvinyl alcohol, 1 part of citric acid, 1 part of sodium hexametaphosphate, and 40 parts of water.

[0213] Example 5

[0214] A three-layer thermal insulation gasket with a thickness of 2 mm was prepared. The thermal insulation gasket sequentially comprised: a first outer layer of glue-coated basalt fiber aerogel, a middle layer of aluminum foil, and a second outer layer of basalt fiber aerogel. The specific steps included:

[0215] Step 1: Preparation of glue-coated basalt fiber aerogels of different thicknesses:

[0216] (1) 20.8 g of TEOS, 55.2 g of anhydrous ethanol, and 5.4 g of H2O were added to a three-necked flask and mechanically stirred for 15 min. 3.65 g of a 0.05 wt% hydrochloric acid ethanol dilution was added dropwise. After stirring for 120 min, the flask was sealed and allowed to stand at room temperature for 24 h to obtain a SiO2 sol with a molar ratio of n(TEOS):n(C2H5OH):n(H2O)=1:12:3.

[0217] (2) Ammonia ethanol dilution was added dropwise to the material obtained in step (1), and after stirring evenly, basalt fiber felts were placed in the sol, with the thickness of the fiber felts being 1.5 mm and 0.3 mm respectively, and the sol was allowed to stand until it turned into a gel.

[0218] (3) Using ethanol to perform solvent replacement on the gel in step (2) to replace water and other impurities in the gel.

[0219] (4) The gel was sealed and aged for 24 hours before being supercritically dried. Ethanol was used as the supercritical drying medium and N2 was pre-filled until the pressure in the kettle reached 2 MPa. The temperature in the kettle was raised to 270°C at a heating rate of 1°C / min and kept warm for 2 hours until the pressure in the kettle reached 10 MPa. The water cooling device was turned on and the pressure in the kettle was slowly released to atmospheric pressure. N2 was then introduced into the kettle to purge the kettle. After cooling to room temperature, basalt fiber aerogels with thicknesses of 1.5 mm and 0.3 mm were obtained, respectively.

[0220] Step 2: Set the adhesive layer:

[0221] 1) Hydrophilic modification: The surface of the basalt fiber aerogel with a thickness of 1.5 mm was pretreated with ethanol by spraying.

[0222] 2) Glue spraying: Use a spray gun to attach the adhesive solution to the surface of the basalt fiber aerogel treated in step 1) to obtain the first outer layer; the specific conditions are: the distance between the spray gun port and the thermal insulation gasket is 30 cm, the spray gun and the surface of the thermal insulation gasket are at an angle of 90° to ensure uniform spraying, the spray gun flow rate is 15 L / h, as long as the weight of the first outer layer obtained after spraying can be controlled within 30 g / m 2 Below (can be 10g / m 2 , 50g / m 2 ).

[0223] Among them, the adhesive solution: 20 parts of rubber-type adhesive, 1 part of polyvinyl alcohol, 1 part of citric acid, 1 part of sodium hexametaphosphate, and 40 parts of water.

[0224] Step 3: Assemble three layers of thermal insulation gaskets:

[0225] The 0.3 mm thick basalt fiber aerogel obtained in step 1 was used as the second outer layer, and the first outer layer obtained in step 2 was bonded to both sides of the middle layer (0.2 mm aluminum foil) to obtain a thermal insulation gasket.

[0226] Example 6

[0227] A three-layer thermal insulation gasket with a thickness of 2 mm was prepared. The thermal insulation gasket sequentially comprised: a first outer layer of glue-coated basalt fiber aerogel, a middle layer of aluminum foil, and a second outer layer of glass fiber aerogel. The preparation method was similar to that of Example 5, except that:

[0228] In step 1, (2) an ammonia-ethanol dilution solution is dripped into the material obtained in step (1), and after stirring evenly, a 1.5 mm thick basalt fiber felt and a 0.3 mm thick glass fiber felt are respectively placed into the sol, and the mixture is allowed to stand to convert the sol into a gel; the rest is the same as in Example 5, and a basalt fiber aerogel with a thickness of 1.5 mm and a glass fiber aerogel with a thickness of 0.3 mm are obtained.

[0229] In step 3, the second outer layer is replaced with the glass fiber aerogel with a thickness of 0.3 mm in step 1 of this embodiment, and the rest is the same as in embodiment 5 to obtain a thermal insulation gasket.

[0230] Example 7

[0231] A three-layer thermal insulation gasket with a thickness of 2 mm was prepared. The thermal insulation gasket sequentially comprised: a first outer layer of polyimide-modified basalt fiber aerogel, a middle layer of polyethylene sheet, and a second outer layer of polyimide-modified basalt fiber aerogel. The specific method is as follows:

[0232] Step 1: Referring to the preparation method of Example 3, a polyimide-modified basalt fiber aerogel is prepared, except that: (2) an ammonia-ethanol dilution solution is dripped into the material obtained in step (1), and after stirring evenly, a 1.5 mm thick basalt fiber felt and a 0.3 mm thick basalt fiber felt are respectively placed in the sol, and the sol is allowed to stand to convert into a gel; the rest is the same as Example 5, and polyimide-modified basalt fiber aerogels with thicknesses of 1.5 mm and 0.3 mm are obtained, respectively.

[0233] Step 2: Set the adhesive layer:

[0234] 1) Hydrophilic modification: The surface of the polyimide-modified basalt fiber aerogel with a thickness of 1.5 mm was pretreated with ethanol by spraying.

[0235] 2) Glue spraying: Use a spray gun to attach the adhesive solution to the surface of the basalt fiber aerogel treated in step 1) to obtain the first outer layer; the specific conditions are: the distance between the spray gun port and the thermal insulation gasket is 30 cm, and the spray gun is at a 90° angle to the surface of the thermal insulation gasket to ensure uniform spraying. The spray gun flow rate is 15L / h. As long as the weight of the first outer layer obtained after spraying can be controlled within 30g / m 2 Below (can be 10g / m 2 , 50g / m 2 ).

[0236] Among them, the adhesive solution: 20 parts of rubber-type adhesive, 1 part of polyvinyl alcohol, 1 part of citric acid, 1 part of sodium hexametaphosphate, and 40 parts of water.

[0237] Step 3: Assemble three layers of thermal insulation gaskets:

[0238] The polyimide-modified basalt fiber aerogel with a thickness of 0.3 mm obtained in step 1 was used as the second outer layer, and the first outer layer obtained in step 2 was bonded to the two sides of the middle layer (0.2 mm polyethylene sheet) to obtain a thermal insulation gasket.

[0239] Example 8

[0240] A two-layer thermal insulation gasket with a thickness of 2 mm was prepared. The thermal insulation gasket sequentially comprised: a first outer layer of glue-coated basalt fiber aerogel and an intermediate layer of aluminum foil. The preparation method of this embodiment was basically the same as that of embodiment 4, except that:

[0241] In step 1, (2) ammonia ethanol dilution was dripped into the material obtained in step (1), and after stirring evenly, 1.8 mm thick basalt fiber felt was placed into the sol, and the sol was allowed to stand to convert into gel; the rest was the same as in Example 4, and a basalt fiber aerogel with a thickness of 1.8 mm was obtained.

[0242] Step 2: Set the adhesive layer:

[0243] 1) Hydrophilic modification: The surface of the basalt fiber aerogel with a thickness of 1.8 mm was pretreated with ethanol by spraying.

[0244] 2) Glue spraying: Use a spray gun to attach the adhesive solution to the surface of the basalt fiber aerogel treated in step 1) to obtain the first outer layer; the specific conditions are: the distance between the spray gun port and the thermal insulation gasket is 30 cm, and the spray gun is at a 90° angle to the surface of the thermal insulation gasket to ensure uniform spraying. The spray gun flow rate is 15L / h. As long as the weight of the first outer layer obtained after spraying can be controlled within 30g / m 2 Below (can be 10g / m 2 , 50g / m 2 ).

[0245] Among them, the adhesive solution: 20 parts of rubber-type adhesive, 1 part of polyvinyl alcohol, 1 part of citric acid, 1 part of sodium hexametaphosphate, and 40 parts of water.

[0246] Step 3: Assemble the double-layer thermal insulation gasket:

[0247] The first outer layer obtained in step 2 is bonded to one side of the middle layer (0.2 mm aluminum foil) to obtain a thermal insulation gasket.

[0248] Comparative Example 1

[0249] Prepare a thermal insulation gasket, which is a single layer of adhesive-free glass fiber aerogel with a thickness of 2 mm. The preparation method is basically the same as that of Example 2, except that:

[0250] The 2 mm thick basalt fiber felt in step (2) was replaced with a 2 mm thick glass fiber felt, and the rest was the same as in Example 1, to obtain a 2 mm thick basalt fiber aerogel, which is a thermal insulation gasket.

[0251] Test Example 1

[0252] The thermal insulation gaskets prepared in the above examples and comparative examples were tested for breakdown strength and volume resistivity under high temperature conditions. The specific testing methods are as follows:

[0253] Breakdown strength: Place the thermal insulation gasket in a 300°C environment for 10 minutes, then maintain the temperature at 300°C for a breakdown strength test. The breakdown strength test standard can refer to GB / T 8411.2-2008 and is recorded in Table 1A and Table 1B.

[0254] Volume resistivity: After placing the thermal insulation gasket in a 300°C environment for 10 minutes, maintain the temperature at 300°C, measure the volume resistivity for 1 minute, and take the average value of this 1 minute, and record it in Table 1A and Table 1B.

[0255] Table 1A Parameters of thermal insulation gasket

[0256] Table 1B Parameters of thermal insulation gasket

[0257] The above describes exemplary embodiments of the present invention. However, the scope of protection of this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc. made by those skilled in the art within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A thermal insulation gasket, the insulation performance of which satisfies at least one of the following conditions: A1) Breakdown voltage: not less than 10KV / mm; A2) Volume resistivity: greater than or equal to 1×10 13 Ω / cm.

2. A thermal insulation gasket, the strength of which satisfies at least one of the following conditions: B1) The tensile strength parameter is not less than 2MPa; B2) When the thickness is not more than 3mm, the stiffness shall not be less than 85g / cm.

3. A thermal insulation gasket, characterized in that: The thermal insulation gasket has the following properties: The insulation performance meets at least one of the following conditions: A1) Breakdown voltage: not less than 10KV / mm; A2) Volume resistivity: greater than or equal to 1×10 13 Ω / cm; and, the strength satisfies at least one of the following conditions: B1) The tensile strength parameter is not less than 2MPa; B2) When the thickness is not more than 3mm, the stiffness shall not be less than 85g / cm.

4. The thermal insulation gasket according to any one of claims 1 to 3, characterized in that: The thickness of the thermal insulation gasket is not greater than 3 mm.

5. The thermal insulation gasket according to any one of claims 1 to 3, characterized in that: The thermal insulation gasket contains at least one fiber / aerogel composite layer; the fiber / aerogel composite layer comprises a substrate, aerogel and polyimide, the substrate is fiber, and the substrate is filled with aerogel; the fiber comprises basalt fiber.

6. The thermal insulation gasket according to claim 5, characterized in that: The fibers also include glass fibers and / or other fibers.

7. The thermal insulation gasket according to claim 5, characterized in that: The substrate is fiber felt or fiber cloth.

8. The thermal insulation gasket according to claim 5, characterized in that: The thermal insulation gasket also includes an intermediate layer, and the intermediate layer is arranged on any surface of the fiber / aerogel composite layer.

9. The thermal insulation gasket according to claim 8, characterized in that: The thermal insulation gasket at least comprises: An intermediate layer, which is a polymer sheet and / or a metal foil, and is used for structural support and / or bonding; A first outer layer, the first outer layer is located on one side surface of the middle layer, and when used in a battery pack, the first outer layer faces the battery pack; The first outer layer is the fiber / aerogel composite layer.

10. The thermal insulation gasket according to claim 9, characterized in that: The thermal insulation gasket further includes a second outer layer, which is located on the other side surface of the middle layer. When used in a battery pack, the second outer layer faces away from the battery pack.

11. The method for preparing the thermal insulation gasket according to any one of claims 1 to 10, characterized in that: The preparation method comprises: 1) Preparing silica sol: mixing a silicon source, water and an alcohol solvent to prepare silica sol; 2) preparing gel: introducing the fiber preform into the silica sol in step 1) to obtain a gel; 3) Solvent replacement: using a replacement solvent to replace the liquid in the gel to obtain an intermediate; 4) Drying: The intermediate of step 3) is subjected to supercritical drying to obtain a fiber / aerogel composite layer, namely the thermal insulation gasket.

12. The preparation method according to claim 11, characterized in that: In step 1), the molar ratio of silicon source, alcohol solvent and water is 1:(7-20):3; And / or, in step 1), the silicon source is selected from at least one of sodium silicate, ethyl orthosilicate, methyl orthosilicate, tetrapropoxysilane, tetrabutoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane; And / or, in step 1), the alcohol solvent is methanol, ethanol or a combination thereof; And / or, polyimide powder particles are optionally added or not added to the silica sol in step 1); if added, the amount of the polyimide powder particles added is 0.5% to 5% of the mass of the silica sol.

13. The preparation method according to claim 11, characterized in that: In step 2), the thickness of the fiber preform is not more than 3 mm; And / or, the fiber preform is selected from basalt fiber preform, glass fiber preform, aluminum silicate fiber preform, alumina fiber preform, mullite fiber preform, SiO2 ceramic nanofiber preform.

14. The preparation method according to claim 11, characterized in that: In step 3), the replacement solvent is selected from methanol, ethanol or a combination thereof.

15. The preparation method according to claim 11, characterized in that: The preparation method further comprises the following steps: 5) Arranging a structural reinforcement layer: Arranging an adhesive layer and / or an outer film layer on the surface of the fiber / aerogel composite layer in step 4) to obtain a thermal insulation gasket including an adhesive layer and / or an outer film layer; In step 5), the outer film layer is disposed on at least one surface of the fiber / aerogel composite layer or on a surface of the adhesive layer.

16. The preparation method according to claim 15, characterized in that , the preparation method further comprises the following steps: 6) Combining the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) with the intermediate layer to obtain a thermal insulation gasket with a composite structure.

17. The preparation method according to claim 15 or 16, characterized in that: The preparation method further comprises the following steps: 7) The other side surface of the middle layer in step 6) is combined with the fiber / aerogel composite layer obtained in step 4) or the fiber / aerogel composite layer including the structural reinforcement layer obtained in step 5) to obtain a thermal insulation gasket with a sandwich structure.

18. Use of the thermal insulation gasket according to any one of claims 1 to 10 as a thermal insulation material and / or insulating material in a battery.

Citation Information

Patent Citations

  • Preparation method of modified silicon oxide aerogel heat insulation sheet

    CN112079618A

  • Heat-insulating and high-temperature-resistant aerogel gradient composite material and preparation method thereof

    CN112830760A

  • Wave-transmitting, efficient and heat-insulating aerogel composite material and preparation method thereof

    CN112851292A

  • Composite heat insulation pad and manufacturing process thereof

    CN113860850A

  • Ultrathin glass fiber paper composite aerogel and preparation method thereof

    CN115852739A

Cited By

  • Packaging film for battery heat insulation sheet as well as preparation method and application of packaging film

    CN118893880A

  • Preparation method of heat insulation tile composite aerogel material

    CN120647411A