Organic compound containing benzoxazolyl or benzothiazolyl and light-emitting device
By using organic compounds containing benzoxazole or benzothiazole groups as covering layers in OLED devices, combined with organic compounds of triazine and naphthalene structural units, the problem of brightness and color differences in top-emission OLED devices at different angles is solved. , improving light extraction efficiency and service life, achieving lower operating voltage and higher BI luminous efficiency.
Patent Information
- Application Number
- PCT/CN2023/103805
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-06-29
- Publication Date
- 2024-10-24
AI Technical Summary
Existing top-emitting OLED devices have large differences in brightness and color at different viewing angles, which affects product performance. The evaporation temperature of the covering layer material is high and the light extraction efficiency is low, resulting in poor device quality and low yield.
Using organic compounds containing benzoxazole or benzothiazole groups as the covering layer, combined with organic compounds of triazine and naphthalene structural units, the light extraction efficiency is improved and the angle dependence is improved, the operating voltage is reduced and the service life is improved.
It improves light extraction efficiency, improves angle dependence, reduces operating voltage, improves BI luminous efficiency and service life, and is better than traditional OLED devices.
Smart Images

Figure CN2023103805_24102024_PF_FP_ABST
Abstract
Description
An organic compound containing benzoxazolyl or benzothiazolyl and a light-emitting device Technical Field
[0001] The present invention relates to the technical field of preparation of organic photoelectric materials, and in particular to an organic compound containing a benzoxazolyl group or a benzothiazolyl group and a light-emitting device. Background Art
[0002] Organic light-emitting diodes (OLEDs), also known as organic electroluminescent devices, are a technology that uses organic materials to emit light through carrier injection and recombination under the influence of an electric field. They convert electrical energy into light through the organic light-emitting material. OLEDs are essentially thin-film stacked devices. Theoretically, when both the anode and cathode are transparent electrodes, light emitted by the light-emitting layer can propagate from the anode to the outside of the device, as well as from the cathode. Therefore, based on the light transmission path, devices can be categorized as bottom-emitting or top-emitting. In bottom-emitting devices, light propagates from the anode through the substrate to the outside of the device, while in top-emitting devices, light propagates from the cathode to the outside of the device. Top-emitting devices emit light toward the cathode, bypassing the substrate, resulting in clearer, more detailed images and higher color vividness. However, in top-emitting organic electroluminescent devices, brightness and color can vary significantly at different viewing angles, seriously impacting product performance.
[0003] In recent years, to improve light extraction efficiency and mitigate color shift, OLED device performance has been enhanced by placing a high-refractive-index "capping layer" on the outer surface of a low-refractive-index semitransparent electrode. However, current capping layer materials can present issues such as excessively high evaporation temperatures, low light extraction efficiency, and limited improvement in device luminous efficiency. This leads to high manufacturing process requirements, significant variability in device quality, and low yield rates. This requires careful coordination with other materials to improve yield rates.
[0004] To continuously improve the performance of OLED devices, not only innovations in OLED device structure and manufacturing processes are needed, but also continuous research and innovation in OLED optoelectronic functional materials are needed to create higher-performance OLED functional materials and rationally combine them with existing materials to improve the luminous efficiency and service life of the devices. Therefore, finding suitable OLED optoelectronic functional materials for OLED devices to solve the above problems is a long-standing need in the field.
[0005] Summary of the Invention
[0006] In response to the problems existing in the prior art, the present application provides an organic compound containing a benzoxazolyl group or a benzothiazolyl group and a light-emitting device. The compound of the present invention is particularly suitable for use in light-related devices or components. In particular, the compound of the present invention can be used as a covering layer in the device or component to improve light extraction efficiency and improve angle dependence. In addition, using the compound of the present invention as a covering layer and preparing a device or component together with a transport layer of an organic compound containing triazine and naphthalene structural units can enable the device or component to exhibit a lower operating voltage, higher BI luminous efficiency and longer service life.
[0007] The present invention provides an organic compound containing a benzoxazolyl group or a benzothiazolyl group, wherein the organic compound has a structure as shown in Formula I:
[0008] In formula I, X2 is O or S;
[0009] L1, L2, L3 are each independently selected from a single bond, a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group; Ar1, Ar2
[0010] Each independently selects a substitutable, condensable polycyclic aromatic group; at least one structural formula of Ar1 and Ar2 is selected from the structure shown in Formula II:
[0011] In formula II, X1 is O or S, Independently selected from non-existent, substituted C6-C30 aryl, and substituted C5-C30 heteroaryl;
[0012] R1-R5 are each independently selected from hydrogen, a substitutable C6-C30 aryl group, and a substitutable C5-C30 heteroaryl group.
[0013] Preferably, the specific structural formula of the organic compound is any one of the following structures:
[0014] The present invention also provides a use of the above-mentioned organic compound containing a benzoxazolyl group or a benzothiazolyl group in an organic electroluminescent device.
[0015] The present invention also provides an organic electroluminescent device, comprising: a substrate layer; a first electrode, the first electrode being on the substrate; an organic light-emitting functional layer, the organic light-emitting functional layer being on the first electrode; a second electrode, the second electrode being on the organic light-emitting functional layer; and a covering layer, the covering layer being on the second electrode.
[0016] The organic light-emitting functional layer includes a light-emitting layer and an electron transport layer, wherein the light-emitting layer includes at least one layer of an organic light-emitting material layer; the electron transport layer includes an organic compound containing triazine and naphthalene structural units; and the covering layer contains at least one organic compound containing a benzoxazolyl group or a benzothiazolyl group as described above.
[0017] Preferably, the organic compound containing triazine and naphthalene structural units has a structure as shown in Formula III:
[0018] wherein L4 is selected from a single bond, a substitutable C6-C30 aryl group, or a substitutable C5-C30 heteroaryl group; Ar3-Ar5 are each independently selected from a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group, or a cyano group;
[0019] Y1-Y3 can be selected from C atoms or N atoms;
[0020] R6-R 13 It can be selected from hydrogen, a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group; when it contains a substituent, the substituent is selected from deuterium, a cyano group, a C6-C24 aryl group or a C2-C24 heteroaryl group.
[0021] Furthermore, the organic compound containing triazine and naphthalene structural units is selected from any one or a combination of at least two of the following materials:
[0022] Preferably, the device comprises one or more combinations of blue, green or red organic light-emitting material layers; different organic light-emitting material layers are stacked in a transverse or longitudinal manner.
[0023] Preferably, in the device, the refractive index of the organic compound containing benzoxazolyl or benzothiazolyl at a wavelength of 450nm is greater than or equal to 2.10, the refractive index at a wavelength of 528nm is greater than or equal to 1.95, and the refractive index at a wavelength of 620nm is greater than or equal to 1.85; the refractive index of the organic compound containing triazine and naphthalene structural units at a wavelength of 450nm is less than or equal to 1.90, the refractive index at a wavelength of 528nm is less than or equal to 1.85; and the refractive index at a wavelength of 620nm is less than or equal to 1.82.
[0024] The organic electroluminescent device of the present invention can be used in OLED lighting and display devices. Specifically, it can be used in the commercial field, such as display screens of products and equipment such as POS machines and ATM machines, copiers, vending machines, game consoles, gas stations, time clocks, access control systems, and electronic scales; in the communications field, such as display screens of products such as mobile phones, various video intercom systems (videophones), mobile network terminals, and ebooks; in the computer field, such as display screens of home and / or commercial computers (PCs / workstations, etc.), PDAs, and laptops; in consumer electronic products, such as display screens of decorative items (soft screens) and lamps, various audio equipment, MP3s, calculators, digital cameras, head-mounted displays, digital video cameras, portable DVDs, portable televisions, electronic clocks, handheld game consoles, and various household appliances (OLED TVs); and in the transportation field, such as display screens of various indicator signs such as GPS, car audio, car phones, and aircraft instruments and equipment.
[0025] Preferably, the organic electroluminescent device prepared by the present invention is used in smart phones, tablet computers, smart wearable devices, televisions, VR, micro-display fields, and car central control screens or car taillights.
[0026] The present invention also provides a display or lighting device, which comprises one or more of the organic electroluminescent devices described above.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The compound represented by the general formula (I) provided by the present invention has excellent properties and is particularly suitable for use in light-related devices or components. The compound of the present invention can be used as a covering layer in the device or component to improve light extraction efficiency and improve angle dependence. In addition, using the compound of the present invention as a covering layer and preparing a device or component together with a transport layer of an organic compound containing triazine and naphthalene structural units can enable the device or component to exhibit a lower operating voltage, higher BI luminous efficiency and longer service life, which is better than existing commonly used OLED devices. It has good industrial prospects. DETAILED DESCRIPTION
[0029] The following is a clear and complete description of the technical solutions of the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making any creative efforts shall fall within the scope of protection of the present invention.
[0030] The aryl group described in the present invention refers to a general term for a monovalent group remaining after removing a hydrogen atom from the aromatic carbon nucleus of an aromatic hydrocarbon molecule. It can be a monocyclic aryl group or a condensed ring aryl group. Examples may include phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl or pyrenyl, but are not limited thereto.
[0031] The heteroaryl group described in the present invention refers to a general term for groups in which one or more aromatic carbon atoms in an aromatic group are replaced by heteroatoms, wherein the heteroatoms include but are not limited to oxygen, sulfur or nitrogen atoms. The heteroaryl group can be a monocyclic heteroaryl group or a condensed-ring heteroaryl group. Examples may include pyridyl, pyrrolyl, pyridyl, thienyl, furyl, indolyl, quinolyl, isoquinolyl, benzothienyl, benzofuranyl, dibenzofuranyl, dibenzothienyl, carbazolyl, etc., but are not limited thereto.
[0032] Throughout this specification, unless explicitly stated to the contrary, references to "comprising" any component will be understood to implicitly include, but not exclude, any other elements. Furthermore, it should be understood that throughout this specification, when an element such as a layer, film, region, or substrate is referred to as being "on" or "over" another element, it can be "directly on" the other element, or intervening elements may be present. Furthermore, "on" or "above" refers to being above the target portion, not necessarily above in terms of gravity.
[0033] In this article, "n@450nm" refers to the refractive index of the material relative to vacuum for blue light with a wavelength of 450nm; "n@528nm" refers to the refractive index of the material relative to vacuum for green light with a wavelength of 528nm; "n@620nm" refers to the refractive index of the material relative to vacuum for red light with a wavelength of 620nm.
[0034] One object of the present invention is to provide an organic electroluminescent device, which includes: a substrate layer; a first electrode, which is on the substrate; an organic light-emitting functional layer, which is on the first electrode; a second electrode, which is on the organic light-emitting functional layer; and a covering layer, which is on the second electrode; the organic light-emitting functional layer includes a light-emitting layer and an electron transport layer, and the light-emitting layer includes at least one layer of organic light-emitting material; the electron transport layer includes an organic compound containing triazine and naphthalene structural units; the covering layer contains at least one organic compound containing benzoxazolyl or benzothiazolyl as described above.
[0035] In one embodiment of the present invention, the electron transport layer in the organic electroluminescent (OLED) device comprises one or more of the compounds represented by the above general formula (III), or consists of one or more compounds of the above general formula (III); the covering layer comprises one or more of the compounds represented by the above general formula (1), or consists of one or more compounds of the above general formula (1).
[0036] In a preferred embodiment of the present invention, an OLED is provided, which includes a substrate, an anode, a cathode, an organic light-emitting functional layer and a covering layer, wherein the organic light-emitting functional layer may include a light-emitting layer, a hole transport layer, a hole injection layer, an electron transport layer, an electron injection layer, etc., or may only include a light-emitting layer and one or more other layers; wherein the electron transport layer comprises one or more of the compounds represented by the above general formula (III), or is composed of one or more compounds of the above general formula (III); the covering layer comprises one or more of the compounds represented by the above general formula (1), or is composed of one or more compounds of the above general formula (1). Optionally, there is a protective layer and / or an encapsulation layer on top of the covering layer. The substrate of the present invention can be any substrate used in a typical organic light-emitting device. It can be a glass or transparent plastic substrate, or a substrate of an opaque material such as silicon or stainless steel, or a flexible PI film. Different substrates have different mechanical strength, thermal stability, transparency, surface smoothness, and water resistance, and the usage direction is different depending on the nature of the substrate.
[0037] As materials for the hole injection layer, the hole transport layer, and the electron injection layer, any material can be selected from known materials used in OLED devices.
[0038] As a guest material capable of producing blue fluorescence, blue phosphorescence, green fluorescence, green phosphorescence and blue-green fluorescence, it is not only required to have extremely high fluorescence quantum luminescence efficiency, but also to have an appropriate energy level that can effectively absorb the excitation energy of the host material to emit light. Such materials are not particularly limited.
[0039] The light-emitting layer included in the OLED device of the present invention can use not only fluorescent materials but also phosphorescent materials. The phosphorescent dopant material is not particularly limited as long as it has phosphorescent luminescence function. In addition to the fluorescent or phosphorescent host-guest materials used in the light-emitting layer described above, the light-emitting layer material can also use non-host-guest doped system materials, host-guest materials with thermally activated delayed fluorescence (TADF) function, and combinations of TADF functional materials and the above-mentioned fluorescent or phosphorescent materials.
[0040] The present invention will be described in detail below with reference to specific examples. Synthesis Examples All raw materials and solvents were commercially available unless otherwise specified, and the solvents were used directly without further treatment.
[0041] Example 1: Preparation of A-006
[0042] (1) P1 (6mmoL), P2 (8mmoL), Pd (dppf) Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture, which was then placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then the solution was slowly extracted three times with saturated MgSO4 aqueous solution and ethyl acetate. The organic layer was then subjected to rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product A-006-1. The structure of the target product A-006-1 was determined by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z)(M+): theoretical value 259.10, measured value 259.30.
[0043] (2) A-006-1 (10 mmol), P3 (25 mmol), sodium tert-butoxide (10 mmol), and 200 ml of toluene were added to the reaction flask. After nitrogen replacement, pd2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2 mmol), heated to 100-120°C, refluxed for 6 hours, and then stopped the reaction. Cooled to 30-40°C, added 200mL of water, and separated. After washing twice with water, the toluene was concentrated and 100mL of n-heptane was added and slurried. The target product A-006 was obtained. The structure of the target product A-006 was analyzed by liquid chromatography-mass spectrometry and ESI-MS (m / z) (M+): the theoretical value was 645.21, and the measured value was 645.70.
[0044] Example 2: Preparation of A-009
[0045] (1) P4 (6mmoL), P5 (8mmoL), Pd (dppf) Cl2 (5×10 -210 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and KCO (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product A-009-1. The structure of the target product A-009-1 was determined by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z)(M+): theoretical value 259.10, measured value 259.30.
[0046] (2) A-009-1 (10 mmol), P3 (25 mmol), sodium tert-butoxide (10 mmol), and 200 mL of toluene were added to the reaction flask. After nitrogen replacement, pd2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2 mmol), heated to 100-120°C, refluxed for 6 hours, and stopped the reaction. Cooled to 30-40°C, added 200mL of water, and separated. After washing with water twice, the toluene was concentrated and 100ml of n-heptane was added and slurried. The target product A-009 was obtained. The structure of the target product A-009 was analyzed by liquid chromatography-mass spectrometry and ESI-MS (m / z) (M+): the theoretical value was 645.21, and the measured value was 645.70.
[0047] Example 3: Preparation of A-017
[0048] (1) P6 (6mmoL), P5 (8mmoL), Pd (dppf) Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added (9 mmol) and KCO (9 mmol) to a 50 mL flask. The mixture was refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product A-017-1. The structure of the target product A-017-1 was determined by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z) (M+): theoretical value 275.08, measured value 275.37.
[0049] (2) A-017-1 (10 mmol), P3 (25 mmol), sodium tert-butoxide (10 mmol), and 200 ml of toluene were added to the reaction flask. After nitrogen replacement, PD2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2mmol), heated to 100-120 ° C, refluxed for 6 hours, and stopped the reaction. Cooled to 30-40 ° C, added 200 mL of water, and separated. After washing with water twice, the toluene was concentrated and 100 mL of n-heptane was added and slurried. The target product A-017 was obtained. The structure of the target product A-017 was analyzed by liquid chromatography-mass spectrometry to obtain LC-MS (m / z) (M +): the theoretical value was 661.18, and the test value was 661.77.
[0050] Example 4: Preparation of A-019
[0051] (1) P6 (8mmoL), P7 (6mmoL), Pd (dppf) Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product A-019-1. The structure of the target product A-019-1 was tested by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z) (M+): theoretical value was 276.07, and the measured value was 276.36.
[0052] (2) A-019-1 (10 mmol), P3 (25 mmol), sodium tert-butoxide (10 mmol), and 200 ml of toluene were added to the reaction flask. After nitrogen replacement, pd2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2 mmol), heated to 100-120°C, refluxed for 6 hours, and stopped the reaction. Cooled to 30-40°C, added 200ml of water, and separated. After washing twice with water, the toluene was concentrated and 100ml of n-heptane was added for slurrying. The target product A-019 was obtained. The structure of the target product A-019 was analyzed by liquid chromatography-mass spectrometry and ESI-MS (m / z) (M+): the theoretical value was 662.18, and the measured value was 662.76.
[0053] Example 5: Preparation of A-032
[0054] (1) P8 (10 mmol), P3 (25 mmol), sodium tert-butoxide (10 mmol), and 200 mL of toluene were added to the reaction flask. After nitrogen replacement, PD2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2mmol), heated to 100-120 ° C, refluxed for 6 hours, and stopped the reaction. Cooled to 30-40 ° C, added 200 mL of water, and separated. After washing with water twice, the toluene was concentrated and 100 mL of n-heptane was added and slurried. The target product A-032 was obtained. The structure of the target product A-032 was analyzed by liquid chromatography-mass spectrometry and ESI-MS (m / z) (M +): the theoretical value was 619.19, and the measured value was 619.67.
[0055] Example 6: Preparation of A-057
[0056] (1) P9 (10 mmol), P10 (25 mmol), sodium tert-butoxide (10 mmol), and 200 ml of toluene were added to the reaction flask. After nitrogen replacement, PD2(dba)3 (5×10 -2 mmoL), Sphos(5×10 -2 mmol), heated to 100-120 ° C, refluxed for 6 hours, and stopped the reaction. Cooled to 30-40 ° C, added 200 mL of water, and separated. After washing with water twice, the toluene was concentrated and 100 mL of n-heptane was added and slurried. The target product A-057 was obtained. The structure of the target product A-057 was analyzed by liquid chromatography-mass spectrometry and ESI-MS (m / z) (M +): the theoretical value was 642.19, and the measured value was 642.70.
[0057] Example 7: Preparation of B-012
[0058] (1) N1 (8mmoL), N2 (6mmoL), Pd(dppf)Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product B-012-1. The structure of the target product B-012-1 was tested by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z) (M+): theoretical value was 545.17, and the measured value was 546.06.
[0059] (2) Add B-012-1 (10 mmol), P10 (25 mmol), Pd(dppf)Cl2 (5×10 -210 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and KCO (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the target product B-012. The structure of the target product B-12 was analyzed by liquid chromatography-mass spectrometry (ESI-MS) (m / z) (M+): the theoretical value was 664.26, and the measured value was 664.79.
[0060] Example 8: Preparation of B-018
[0061] (1) N1 (6mmoL), N2 (8mmoL), Pd(dppf)Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product B-018-1. The structure of the target product B-018-1 was tested by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z) (M+): the theoretical value was 545.17, and the measured value was 546.06.
[0062] (2) Add B-018-1 (10 mmol), N4 (25 mmol), Pd(dppf)Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to rotary evaporation to remove the solvent. Column chromatography was performed to obtain the target product B-018. The structure of the target product B-018 was analyzed by liquid chromatography-mass spectrometry (ESI-MS) (m / z) (M+): the theoretical value was 612.23, and the measured value was 612.72.
[0063] Example 9: Preparation of B-048
[0064] (1) N1 (6mmoL), N5 (8mmoL), Pd (dppf) Cl2 (5×10 -210 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product B-048-1. The structure of the target product B-048-1 was tested by liquid chromatography-mass spectrometry (LC-MS) (m / z) (M+): theoretical value 545.17, measured value 546.06.
[0065] (2) Add B-048-1 (10 mmol), N6 (25 mmol), Pd(dppf)Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to rotary evaporation to remove the solvent, and column chromatography was performed to obtain the target product B-048. The structure of the target product B-048 was analyzed by liquid chromatography-mass spectrometry (ESI-MS) (m / z) (M+): the theoretical value was 688.26, and the measured value was 688.82.
[0066] Example 10: Preparation of B-072
[0067] (1) N1 (8mmoL), N7 (6mmoL), Pd (dppf) Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and KCO (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product B-072-1. The structure of the target product B-072-1 was tested by liquid chromatography-mass spectrometry (LC-MS) (m / z) (M+): theoretical value was 545.17, and the measured value was 546.06.
[0068] (2) Add B-072-1 (10 mmol), N6 (25 mmol), Pd(dppf)Cl2 (5×10 -210 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and KCO (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to rotary evaporation to remove the solvent, and column chromatography was performed to obtain the target product B-072. The structure of the target product B-072 was analyzed by liquid chromatography-mass spectrometry (ESI-MS) (m / z) (M+): theoretical value was 688.26, and the measured value was 688.82.
[0069] Example 11: Preparation of B-090
[0070] (1) N1 (8mmoL), N8 (6mmoL), Pd (dppf) Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. Column chromatography was performed to obtain the crude product B-090-1. The structure of the target product B-090-1 was determined by liquid chromatography-mass spectrometry analysis (LC-MS) (m / z)(M+): theoretical value 545.17, measured value 546.06.
[0071] (2) B-090-1 (8mmoL), N4 (6mmoL), Pd(dppf)Cl2 (5×10 -2 10 mL of a 4:1 dioxane:water solution was added to the mixture (9 mmol) and K2CO3 (9 mmol). The mixture was placed in a 50 mL flask and refluxed for 24 hours. The mixture was cooled to room temperature, and then saturated MgSO4 aqueous solution and ethyl acetate were slowly added to the solution for extraction three times. The organic layer was then subjected to a rotary evaporation to remove the solvent. The target product, B-090, was obtained by column chromatography. The structure of the target product B-090 was analyzed by liquid chromatography-mass spectrometry (LC-MS) (m / z)(M+): the theoretical value was 612.23, and the measured value was 612.72.
[0072] Performance Test 1: Material Refractive Index Characterization
[0073] The refractive index of compounds A-006, A-009, A-017, A-019, A-032, and A-057 at wavelengths of 460 nm, 528 nm, and 620 nm was measured using an ellipsometer. The test results are shown in Table 1 below:
[0074] Table 1. Refractive index of compounds at different wavelengths
[0075] As can be seen from Table 1, the compounds A-006, A-009, A-017, A-019, A-032, and A-057 prepared by the present invention have a higher refractive index than the comparative compound 1, and can effectively improve the light extraction efficiency of the three light colors RGB (450nm / 528nm / 620nm).
[0076] The following are several examples of the application of the organic compounds of the present invention in OLED devices to further illustrate the beneficial effects of the compounds of the present invention. The materials used in the examples were purchased commercially or synthesized in-house:
[0077] Device embodiment - structure and manufacturing method of application example 1:
[0078] First, an alkali-free glass substrate was cleaned with isopropyl alcohol in an ultrasonic cleaner for 15 minutes, followed by a 30-minute UV ozone cleaning in air. The treated substrate was vacuum-deposited with 100nm of ITO / Ag / ITO as the anode. A hole injection layer (HATCN, 50nm), a hole transport layer (NPB, 30nm), a blue light-emitting layer (host ADN and doped BD (weight ratio 97:3, 30nm), an electron transport layer (compound B-012:Liq = 1:1, 30nm), and an electron injection layer (LiF, 0.5nm) were then sequentially deposited on the anode. Mg and Ag (weight ratio 10:1, 15nm) were co-deposited to form a semi-transparent cathode. Compound A-006 (65nm) was then deposited as a capping layer. Finally, the light-emitting device was encapsulated using epoxy resin adhesive under a nitrogen atmosphere, as in Example 1. The molecular structures of the relevant materials are shown below:
[0079] Device Example - Application Example 2-30:
[0080] The device structure and manufacturing method are similar to those of Application Example 1, except that the electron transport layer and cover layer materials of the OLED device are prepared using the compounds listed in Table 2 (Application Example 2-30).
[0081] Device Examples - Comparative Examples 1-4:
[0082] The device structure and manufacturing method are similar to those of Application Example 1, except that the electron transport layer and cover layer materials of the OLED device are prepared using the compounds listed in Table 2 to prepare Comparative Examples 1-4.
[0083] The structures of comparative compound 1 and comparative compound 2 are as follows:
[0084] Table 2.
[0085] Performance evaluation of OLED devices:
[0086] The current of the OLED device at different voltages was measured using a Keithley 2365A digital nanovoltmeter, and the current density of the OLED device at different voltages was obtained by dividing the current by the luminous area. The brightness and radiant energy flux density of the OLED device at different voltages were measured using a Konicaminolta CS-2000 spectroradiometer. Based on the current density and brightness of the OLED device at different voltages, the luminance at the same current density (10 mA / cm 2 ) operating voltage Volt and current efficiency (cd / A). BI = E / CIEy refers to the Blue Index of blue light, a parameter that measures the luminous efficiency of blue light. E refers to the current efficiency, and CIEy refers to the vertical coordinate color point obtained by substituting the device's half-width at half-peak wavelength into the CIE1930 software. The test data is shown in Table 3.
[0087] Table 3
[0088] As can be seen from the test data in Table 3, Application Examples 1 to 30 have lower operating voltage, higher BI luminous efficiency, and longer service life compared to Comparative Examples 1 to 4. The performance improvement of each application example is based on the electron transport material of the present invention having better electron migration. Furthermore, the organic cover layer material is simultaneously prepared into an electronic device with a higher refractive index, effectively improving the light extraction efficiency of the three light colors RGB (corresponding to 450nm / 528nm / 620nm). At the same time, the organic cover layer material has a relatively small effect on the operating voltage and service life of the device.
[0089] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An organic compound containing a benzoxazolyl group or a benzothiazolyl group, characterized in that: The organic compound has a structure as shown in Formula I: In formula I, X2 is O or S; L1, L2, L3 are each independently selected from a single bond, a substitutable C6-C30 aryl group, or a substitutable C5-C30 heteroaryl group; Ar1 and Ar2 are each independently selected from a substitutable, condensable polycyclic aromatic group; at least one of Ar1 and Ar2 is selected from the structure shown in Formula II: In formula II, X1 is O or S, Independently selected from non-existent, substitutable C6-C30 aryl, substitutable C5-C30 heteroaryl; R1-R5 are each independently selected from hydrogen, a substitutable C6-C30 aryl group, and a substitutable C5-C30 heteroaryl group.
2. The organic compound according to claim 1, characterized in that The specific structural formula of the organic compound is any one of the following structures:
3. Use of the organic compound according to any one of claims 1 to 2 in the field of preparation of organic electroluminescent devices.
4. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises: a substrate layer; a first electrode, which is on the substrate; an organic light-emitting functional layer, which is on the first electrode; a second electrode, which is on the organic light-emitting functional layer; and a covering layer, which is on the second electrode; the organic light-emitting functional layer comprises a light-emitting layer and an electron transport layer, and the light-emitting layer comprises at least one layer of an organic light-emitting material layer; the electron transport layer comprises an organic compound containing triazine and naphthalene structural units; and the covering layer comprises at least one organic compound containing a benzoxazolyl group or a benzothiazolyl group as claimed in any one of claims 1 to 2.
5. The organic electroluminescent device according to claim 4, characterized in that: The organic compound containing triazine and naphthalene structural units has a structure as shown in Formula III: Wherein, L4 is selected from a single bond, a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group; Ar3-Ar5 are each independently selected from a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group, and a cyano group; Y1-Y3 can be selected from C atoms or N atoms; R6-R 13 It may be selected from hydrogen, a substitutable C6-C30 aryl group, a substitutable C5-C30 heteroaryl group; when containing a substituent, the substituent may be selected from deuterium, a cyano group, a C6-C24 aryl group or a C2-C24 heteroaryl group.
6. The organic electroluminescent device according to claim 4, characterized in that: The organic compound containing triazine and naphthalene structural units is selected from any one or a combination of at least two of the following materials:
7. The organic electroluminescent device according to claim 4, characterized in that: The organic light-emitting material layer of the organic electroluminescent device includes one or more combinations of blue, green or red; different organic light-emitting material layers can be stacked and combined horizontally or vertically.
8. The organic electroluminescent device according to claim 4, characterized in that: The refractive index of the organic compound containing benzoxazolyl or benzothiazolyl in the organic electroluminescent device at a wavelength of 450nm is greater than or equal to 2.10, the refractive index at a wavelength of 528nm is greater than or equal to 1.95, and the refractive index at a wavelength of 620nm is greater than or equal to 1.85; the refractive index of the organic compound containing triazine and naphthalene structural units at a wavelength of 450nm is less than or equal to 1.90, the refractive index at a wavelength of 528nm is less than or equal to 1.85; and the refractive index at a wavelength of 620nm is less than or equal to 1.
82.
9. Use of the organic electroluminescent device according to any one of claims 4 to 8 in a display or lighting device.
10. A display or lighting device, characterized in that: The device comprises the organic electroluminescent device according to any one of claims 4 to 8.
Citation Information
Patent Citations
Organic compound based on heteroaryl amine structure and application thereof to OLED (Organic Light Emitting Diode)
CN109761967A
Triarylamine compound and organic electroluminescent device thereof
CN111808042A
A brand-new organic compound for coating layer and organic light-emitting element comprising organic compound for coating layer are provided
CN112538060A
Organic compound containing triazine structure and organic electroluminescent device
CN114621216A
Compound for organic electric element, organic electric element using the compound, and electronic device including the organic electric element
CN115943749A
Cited By
Organic light-emitting device
CN119403356A