Three-dimensional artificial tubular tissue, preparation method therefor, and use thereof
By dividing different cell planting areas on the scaffold and controlling the thickness ratio, a dense and loose layer structure is formed, which solves the problem of cavities between cell layers in three-dimensional artificial tubular tissue, achieves cavity-free tissue construction, and reduces the risk of aneurysms. , and is suitable for tubular tissues with a variety of structures and functions.
Patent Information
- Application Number
- PCT/CN2023/104699
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-06-30
- Publication Date
- 2024-10-24
AI Technical Summary
Existing technology is difficult to eliminate the cavities between cell layers in three-dimensional artificial tubular tissues, leading to bleeding and arterial dissection, increasing the risk of aneurysms, and it is difficult to construct multi-layered cellular structures smaller than 6 mm in diameter.
By dividing different cell planting areas on the scaffold, controlling the thickness ratio to form dense and loose layer structures, ensuring uniform growth of cells in the three-dimensional topology, eliminating interlayer cavities, and using multi-layer film-laying needle carding or electrospinning and other processes to prepare scaffolds to ensure adhesion and growth between cell layers.
It achieves a cavity-free three-dimensional artificial tubular tissue, avoids bleeding and arterial dissection, reduces the risk of aneurysm, and can construct various three-dimensional tubular tissues with different structures and functions.
Smart Images

Figure CN2023104699_24102024_PF_FP_ABST
Abstract
Description
Three-dimensional artificial tubular tissue and its preparation method and application Technical Field
[0001] The present invention belongs to the technical field of tissue engineering, and in particular relates to a three-dimensional artificial tubular tissue and a preparation method and application thereof. Background Art
[0002] Tissue engineering is an interdisciplinary field that studies the structure, function, and growth mechanisms of biological tissues through the application of materials engineering and life sciences, with the goal of developing biological substitutes that can repair, maintain, or improve the function of damaged tissues. Tissue engineering holds great promise in biomedicine, with its primary goal being the repair and regeneration of damaged tissues. Consequently, the key to this discipline lies in how to cultivate highly biomimetic cell-based scaffold structures in vitro and ensure their successful reconstruction of artificial tissues and organs with superior structure and function upon transplantation into the body.
[0003] Biological systems with tubular structures are widespread in the human body, primarily including the vascular system, digestive system, respiratory system, nervous system, and reproductive system. Common tubular tissues include the trachea, blood vessels, lymphatic vessels, esophagus, nerve ducts, urethra, intestines, and reproductive tract. These hollow organs and tissues drive various bodily functions and perform their respective functions. Therefore, three-dimensional artificial tubular tissues also have a variety of structures and functions. When constructing various types of biomimetic tubular tissues using tissue engineering, it is necessary to consider the structural and functional differences among these various tubular tissues.
[0004] To better develop biomimetic tubular implants with realistic structures and functions, we first need to gain a comprehensive understanding of the structures of various human tubular tissues and organs. The following sections focus on the vascular system, digestive system, respiratory system, and nervous system.
[0005] The primary function of the vascular system is to transport blood throughout the body at a relatively high rate, generating significant fluid shear stress on the vessel walls. Blood vessels are primarily composed of three membrane layers: the endothelium, the media, and the adventitia, with a hollow core. The endothelium is relatively permeable, allowing biochemical factors to be transported through the vessel wall and even cells in certain disease states. The tunica media, composed of a dense, circumferential layer of smooth muscle cells (VSMCs) and elastin, primarily functions to withstand the dilation and impact forces of blood flow. The adventitia, composed primarily of collagen and fibroblasts, is a loose connective tissue that wraps around and supports the vessels, while also imparting tensile strength. Collagen in the vessels imparts strength, while elastin provides elasticity. Blood vessels range in size from capillaries and microvessels, with diameters of only a few micrometers, to veins and arteries, with diameters up to 30 mm. Small capillaries, such as those that constitute the blood-brain barrier, consist of a single cell, which wraps around itself to form an internal lumen. Therefore, the different tubular diameters and structural differences of blood vessels make the construction of tissue-engineered blood vessels more complicated. Currently, mainly large-caliber artificial vascular tissues have been prepared, while small-caliber artificial vascular tissues still need to be further conquered.
[0006] The digestive system primarily consists of the gastrointestinal tract. Each part of the GI tract is composed of four layers: the mucosa, submucosa, muscularis propria, and serosa, starting with the luminal lining. The mucosa contains enterocytes, which perform absorptive, secretory, and protective functions. The intestinal epithelium is a tight barrier system that separates the contents of the luminal cavity from the surrounding tissues. The intestinal epithelium has a complex 3D structure with luminal protrusions (called villi) and invaginations (called crypts). This 3D structure maximizes internal surface area, facilitating nutrient absorption. The submucosa houses a network of immune cells, nerves, and lymphocytes. This layer is surrounded by the muscularis propria, which, through its muscle cells, provides a peristaltic pump, performing the critical function of intestinal motility. The outermost layer is the serosa (or adventitia), which forms a barrier around the GI tract. The intestine also possesses a complex network of nerves, known as the enteric nervous system, consisting of two parallel nerve plexuses: the submucosal plexus and the myenteric plexus. Therefore, the complex structure of the GI tract further complicates the design of artificial digestive tract tissue.
[0007] The respiratory system comprises the upper and lower respiratory tracts. The trachea, which serves as the foundation for swallowing, speaking, and breathing, lies beneath the upper respiratory tract (nasal cavity, throat, and pharynx) and is part of the lower respiratory tract (trachea, bronchi, bronchioles, and alveoli). The trachea is primarily composed of four layers: the mucosa, submucosa, hyaline cartilage, and adventitia. The mucosa, composed of pseudostratified epithelium, lines the lumen and contains a variety of cell types. The submucosa is a connective tissue layer containing submucosal glands that facilitate mucus secretion. The cartilaginous layer consists of horseshoe-shaped rings of hyaline cartilage, connected by fibroelastic tissue, which is closed by a membranous structure composed of longitudinally oriented smooth muscle. Finally, the adventitia is composed of connective tissue. Both the cartilage and adventitia contribute to the unique structural and mechanical properties of the trachea. The adventitia also contains numerous other cell types, such as fibroblasts, adipocytes, nerves, and connections to the vascular system, which are essential for meeting blood, nutritional, and metabolic needs. Unlike in vitro models of the vascular system and intestine, the trachea is susceptible to a range of airway disorders caused by infection, stenosis, collapse, or cancer. To date, tracheal tissue engineering has mainly focused on implantable scaffolds for tracheal replacement.
[0008] The nervous system is vital to the human body, responsible for regulating physiological functions and the internal environment. It is divided into the central nervous system and the peripheral nervous system. The central nervous system primarily provides instructions for comprehensive human behavior, while the peripheral nervous system primarily guides perception and movement. Damage to the nervous system can lead to loss of sensory abilities such as vision, hearing, and smell, as well as motor abilities such as chewing, walking, and grasping, as well as impaired consciousness such as dementia, dizziness, and amnesia, significantly impacting human health. The primary component of the nervous system is neural tissue, which is composed of neurons and glial cells. Unlike ordinary cells in the body, neurons vary in length, ranging from a few microns to one meter. This phenomenon is attributed to two specialized protrusions within neurons: axons and dendrites. Glia make up a large proportion of neural tissue, and their cell bodies also have irregular protrusions. Their primary functions include supporting neurons, insulating signals, providing nutrition, and protecting them. The entire nerve exhibits a three-layer structure, with a flat cross-section. Therefore, to achieve a high degree of biomimetic properties in tissue-engineered neural scaffolds, it is crucial to mimic the structural composition of neural tissue.
[0009] Although humans have long understood various living systems and tissues, culturing cells in vitro and attempting to construct artificial tissues and organs has been a long and arduous journey. The concept of in vitro cell culture was first established in 1885, when Willhelm Roux isolated cells from chicken embryos. Initially, traditional cell culture methods were based on two-dimensional surfaces and underwent a long period of development. However, it was discovered that this monolayer cell culture method, due to the altered in vitro environment, gradually lost its original properties during cell proliferation, which was inconsistent with the in vivo environment. Cells grown in three-dimensional tissues showed significant differences from monolayer cells and suspended cells.
[0010] Numerous studies have shown that the environment and behavior of cells in real three-dimensional tissues are more complex than those in two-dimensional tissues. Compared to two-dimensional cultures, cells cultured in three dimensions exhibit a high degree of complexity in many aspects, including morphology, biochemistry, protein expression, and gene expression. The in vitro three-dimensional culture environment is more conducive to maintaining and performing cell functions than a two-dimensional one. Growing cells in a three-dimensional environment more closely resembles in vivo growth patterns, making it more conducive to forming structures similar to in vivo tissues and thus performing their functions. Consequently, three-dimensional cell culture technology emerged, and has undergone decades of development to date.
[0011] Three-dimensional cell culture (TDCC) refers to the in vitro co-culturing of different types of cells with different material carriers with three-dimensional structures, allowing cells to grow and migrate within the three-dimensional structure of the carrier, simulating the in vivo cell growth environment to the greatest extent possible, and making the cells closer to the in vivo growth pattern. In the first half of the 20th century, scholar Holtfreder and his colleagues creatively established an in vitro three-dimensional cell culture method, laying the foundation for subsequent three-dimensional culture technology. By the 1950s, scholar Moscona and his colleagues were the first to use three-dimensional culture methods to study the proliferation, differentiation and aggregation of cancer cells. In recent decades, three-dimensional culture technology has been widely studied and developed, and has been widely used in the field of tumor research.
[0012] The construction of artificial tissue generally involves three key elements: seed cells, scaffold materials, and the in vitro construction of these cells and materials. However, due to the complex physiological structure and diverse types of real human tubular tissue, each of which performs distinct functions, a combination of these factors is required to create an approximate model of the desired tissue, posing a significant challenge to the development of artificial tubular tissue.
[0013] First, the source and type of cells must be considered. Any tubular system requires a source of epithelial cells, but the exact behavior of these cells depends on the different tissues involved. Epithelial cells are usually co-cultured with cells that produce extracellular matrix (ECM) such as fibroblasts or smooth muscle cells, but even the type of matrix-producing cells can vary depending on the application. For example, the trachea requires the use of chondrocytes or mesenchymal stem cells that differentiate along the chondrogenic pathway. On the other hand, different tissues also require different supporting cells. For example, the native intestinal epithelium contains goblet cells that secrete mucus, and the native blood vessels and intestines both have a layer of muscle tissue, so appropriate muscle cells need to be obtained.
[0014] Secondly, scaffold design is equally challenging. First, a structure must be created to support cell growth before the desired tissue can be created, without compromising overall functionality after synthesis. These challenges are particularly prominent in the design of tubular systems. Tubular scaffolds must not only provide the necessary three-dimensional support for cell nutrient acquisition, growth, proliferation, and differentiation and metabolism, but also provide cells with appropriate chemical, morphological, and topological information to guide the formation of the desired functional tissue. Furthermore, they must provide a favorable physiological microenvironment for the secretion of the extracellular matrix and the ultimate formation of the corresponding tissue or organ. Therefore, tubular scaffolds must possess an appropriate pore size and porosity to facilitate the delivery of nutrients and metabolites and the incorporation of seed cells. They must also possess sufficient mechanical strength to ensure that the newly formed tissue maintains its proper morphology during regeneration, resisting external forces and causing no mechanical damage to the surrounding preexisting tissue. Furthermore, the scaffold material itself should be widely available, biocompatible, and not prone to adverse reactions such as coagulation, inflammation, and immune rejection. It should also be sterilizable, have good plasticity, and a suitable degradation rate to accommodate the growth and proliferation rates of different tissues and cells, thereby providing sufficient space for tissue regeneration. This undoubtedly brings many difficulties to the development of tissue engineering scaffolds.
[0015] Third, the combination of cells and scaffold materials is also extremely difficult. The main reasons are: the presence of air in the scaffold, the presence of interfacial forces and surface tension in the scaffold, the hydrophilic and hydrophobic properties of the scaffold material, and the complex shape of the scaffold. These structures lead to uneven distribution of implanted cells on the scaffold, uncontrollable implantation positions, and low implantation efficiency. On the other hand, the complex structure of tubular tissue makes it more difficult for cells to grow on the scaffold. For example, the formation and continued integrity of the epithelial or endothelial barrier ensures the selective permeation of nutrients and metabolic byproducts while preventing the entry of harmful or pathogenic compounds. Without successful barrier formation and description of its characteristics, the function of these models and even cell survival will be limited.
[0016] With the continuous development of tissue engineering research, it has been discovered that although tubular tissues have diverse functions, they also have unified structural characteristics. Within the lumen of these tubular tissues lies a group of cells called epithelial cells (endothelial cells in the vascular system), which form a barrier. Their function is to separate the internal contents of the lumen from the surrounding tissues and organs, while allowing selective permeation and transport through the epithelial cells. Based on this, when producing tubular scaffolds suitable for different tissue engineering applications, it is first necessary to create a complete tubular opening and form a semipermeable epithelium or endothelium.
[0017] The primary requirement for tubular scaffolds is the ability to form adjacent epithelial or endothelial linings. The most effective approach is to uniformly seed cells on a two-dimensional (2D) non-porous surface or in an injectable medium (such as a hydrogel). However, tubular scaffolds are usually three-dimensional, not two-dimensional, so uniform seeding of cells on a 3D surface is essential. Some researchers seed cells on planar membranes and then curl these membranes into tubes; others use dynamic methods, relying on cells to uniformly adhere to the surrounding walls through rotation or pressure. However, the porous structure of the scaffold makes the formation of adjacent epithelium more difficult. Other studies use a layered approach to fill ECM-producing cells or deposited cells back into the pores to assist in the formation of epithelial cells; many implantation-driven studies also rely on cell infiltration in vivo, but these methods all have certain limitations.
[0018] After more than 20 years of development, the preparation of tissue engineering scaffolds has made great progress. Based on the characteristics of tubular tissue structure, people have developed various methods to produce tubular scaffolds, including fiber bonding, solvent casting / particulate leaching, phase separation, in situ polymerization, emulsion freeze drying, gas foaming, rapid prototyping, self-assembly and electrospinning.
[0019] The above preparation methods have been widely developed and used in the preparation of various three-dimensional tissues. However, these methods still have many problems that cannot be solved.
[0020] For example, the blood vessels cultured with large-pore, non-woven tubular degradable scaffolds cannot control the precise spatial distribution of the three types of cells, making it impossible to achieve a more bionic three-layer structure and to construct small-caliber blood vessels with a diameter of less than 6 mm and a multi-layer cell structure.
[0021] For example, traditional 3D cell seeding methods simply involve immersing a three-dimensional topological scaffold in a cell suspension of a certain concentration and subjecting it to dynamic stimulation, including rotation and oscillation. This seeding method is unable to effectively cultivate and differentiate specific cells in a specific topological structure, resulting in the inability to achieve properties similar to those of real tissue.
[0022] For example, the cell 3D printer developed based on 3D printing and microscopy technology combines the overlapping spraying of polymer matrices and cells in a solution to achieve the purpose of printing 3D structures. However, in order to ensure the smoothness of the printer nozzle, the scaffold material used in the cell 3D printer is mostly hydrogel, which makes it difficult for the printed scaffold to form tissue with a certain mechanical strength. On the other hand, due to the limitations of hydrogel materials, it cannot achieve the biomimetic preparation of biological structures such as capillaries or villi. In addition, this method cannot achieve high-throughput tissue printing.
[0023] Existing methods for cell seeding also suffer from low seeding rates and uneven cell distribution within the scaffold. While various approaches have been attempted to improve the efficiency and uniformity of cell seeding, such as perfusion seeding and seeding in stirred flask reactors, these technologies have limited practical application and are not widely used in the field of tissue engineering.
[0024] For example, in the biomimetic design of multilayered structures of natural blood vessels, significant challenges remain in achieving structural orientation within the scaffold, forming an intraluminal endothelial layer, and colonizing cells within the scaffold. Further research is needed to improve the long-term patency and compliance of tissue-engineered vascular scaffolds; develop biomaterials with excellent bioactivity to reduce thrombosis and infection; find the optimal balance between mechanical strength, degradation rate, and tissue formation rate of scaffold materials; and address the limited availability of seed cells and the long time required to construct autologous blood vessels in vitro.
[0025] In order to overcome the above-mentioned defects, researchers have carried out a lot of work and developed a series of advanced methods for constructing three-dimensional tubular tissues, and achieved the following results.
[0026] Patent document CN 102884172 B provides a system for aseptically isolating, collecting cells, and implanting them onto scaffolds or tissue grafts. This system can isolate and collect cells from a target and implant these cells onto a biocompatible three-dimensional scaffold or tissue graft. These scaffolds or grafts can be cultivated and / or implanted into a target within a system for culture, transportation, storage, and testing, for example as a tissue graft (e.g., a vascular graft), to regenerate and / or repair tissue in vivo, in vitro, or ex vivo. However, this system is extremely complex and is not suitable for the collection, culture, and implantation of all cells, resulting in significant limitations in the field of tissue engineering.
[0027] Patent document CN 106085847 B provides a scaffold-based cell seeding platform and method based on 3D printing technology, comprising a three-dimensional motion platform, a control system, a scaffold, an image acquisition system, an image processing system, a host computer, and a dual-nozzle system. However, the scaffold material used in this cell seeding platform is still primarily hydrogel, which suffers from uncontrollable fine structure and weak mechanical properties.
[0028] Patent document CN 108653815 B discloses a three-dimensional curled structure, which uses a method of first performing two-dimensional cell patterning and then self-curling to construct an artificial blood vessel. However, this structure cannot complete the three-dimensional planting and construction of cells well. When the scaffold is a dense structure, the planted cells find it difficult to penetrate the dense scaffold, resulting in the single layer thickness of the tubular tissue finally formed not reaching the required thickness; when the scaffold material is a loose structure, the cells will form unnecessary excessive migration between layers in the early stage, resulting in a mixture of multiple cells, resulting in the inability to accurately control the distribution and proliferation of cells in the three-dimensional scaffold material. More importantly, the different cell layers obtained using this patented method have relatively obvious cavities between layers, and the same cell tissue has the defect of not being able to fuse well after curling.
[0029] Analysis of existing manufacturing processes reveals that when producing tubular stents, the gaps between endothelial cells are often large. This increases the chances of vascular smooth muscle cells or growth factors entering the subendothelial space, leading to intimal hyperplasia. These artificial tubular tissue manufacturing processes fail to eliminate the cavities between cell layers, resulting in a higher risk of bleeding and arterial dissection. Blood can enter the vessel wall through the intima, causing stenosis and occlusion of the lumen, and potentially leading to the development of aneurysms.
[0030] According to relevant literature (DOI: https: / / doi.org / 10.7461 / jcen.2020.22.3.127, Clinical analysis of young adult patients with ruptured intracranial aneurysms: a single-center study of 113 consecutive patients, J Cerebrovasc Endovasc Neurosurg. 2020; 22(3): 127-133. Published online September 21, 2020), a study on intracranial aneurysms in young people (<=40 years old) showed that the average size of aneurysms was in the range of 6.6±3.7mm. However, in young people, aneurysms smaller than 5mm can cause symptoms. The study pointed out that young people have a higher risk of rupture of small aneurysms than middle-aged and elderly people, of which 94.2% of aneurysm ruptures occurred in aneurysms smaller than 10mm, and 47.6% of these ruptures occurred in aneurysms smaller than 5mm. What is more noteworthy is that the time point of aneurysm rupture in young patients is also earlier than that in middle-aged and elderly patients. When the aneurysm is initially formed, the thickness of the blood vessel wall that constitutes the cavity has not yet reached the mechanical strength to support itself. At this time, if it is often exposed to high pressure and high-intensity living environment, it is very easy to cause the aneurysm to rupture. Not only the size of the aneurysm, but also its shape has a great influence on the probability of rupture. It is pointed out in the literature that aneurysms with long or other irregular shapes are more likely to rupture. At the same time, smoking is a major cause of aneurysms. At present, the popularity of e-cigarettes has caused the overall age structure of the smoking group to sink, and aneurysms have also become earlier.
[0031] However, since the current stent preparation process cannot solve the problem of cavities between cell layers, once arterial dissection occurs and causes an aneurysm, surgical treatment is the only option. The commonly used methods are cranial aneurysm clipping or intravascular interventional therapy, which seriously limits the application of tissue engineering and causes secondary pain to patients.
[0032] Therefore, how to improve the preparation process of existing tubular tissue engineering scaffolds and solve the problems of cavities between cell layers, bleeding and arterial dissection, as well as the risk of causing aneurysms, has become a technical problem that needs to be solved urgently.
[0033] Summary of the Invention
[0034] The present invention aims to address the aforementioned technical issues, thereby providing a three-dimensional artificial tubular tissue, its preparation method, and its application. The present invention aims to address the problem that existing preparation methods fail to eliminate cavities or gaps between cell layers, making the resulting tissue engineering scaffolds susceptible to in vivo bleeding, arterial dissection, and aneurysms.
[0035] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0036] One of the objects of the present invention is to provide a method for preparing a three-dimensional artificial tubular tissue, which comprises the following steps:
[0037] A method for preparing a three-dimensional artificial tubular tissue comprises the following steps:
[0038] (1) Preparing a rollable stent;
[0039] (2) Planting cells on the scaffold;
[0040] (3) curling the product obtained in step (2) into a three-dimensional tubular structure and culturing the structure in vitro to obtain the three-dimensional artificial tubular tissue;
[0041] The method for preparing the rollable stent includes any one of the following:
[0042] Method 1: A rollable scaffold is divided into two distinct cell seeding regions from the start to the end of the coiling. The widths of the two distinct cell seeding regions are controlled along the coiling direction of the scaffold so that each cell seeding region forms at least one complete tubular layer after coiling, and the outer tubular layer after coiling can wrap around the inner tubular layer. The thickness ratio of the scaffold in the two distinct cell seeding regions is controlled from thin to thick to range from 1:2 to 80.
[0043] Method 2: A rollable scaffold is divided into three different cell seeding areas from the starting end to the end of the roll. The widths of the three different cell seeding areas are controlled along the roll direction of the scaffold so that each of the different cell seeding areas forms at least one complete tubular layer after roll-up, and the tubular layer located on the outer layer after roll-up can sequentially wrap the tubular layer located on the inner layer; the outermost layer after roll-up wraps the middle layer, and the middle layer wraps the innermost layer. The thickness ratio of the scaffold in the three different cell seeding areas is controlled from thin to thick to be 1:2 to 80:2 to 3000.
[0044] Method three: The curlable scaffold is divided into four different cell seeding areas from the curling start end to the curling end, and the widths of the four different cell seeding areas are controlled along the curling direction of the scaffold so that each of the different cell seeding areas forms at least one complete tubular layer after curling, and the tubular layer located on the outer layer after curling can sequentially wrap the tubular layer located on the inner layer; the outermost layer after curling wraps the second outermost layer, the second outermost layer wraps the middle layer, and the middle layer wraps the innermost layer, and the thickness ratio of the scaffold in the four different cell seeding areas is controlled from thin to thick to be 1:2~80:2~700:2~3000.
[0045] It should be noted that the multiple different cell-seeding areas mentioned in the present invention each form at least one complete tubular layer after curling, which respectively refer to the following situations: two different cell-seeding areas each form an outer and an inner tubular layer after curling, and the outer layer wraps the inner layer; three different cell-seeding areas each form an outer, middle and inner tubular layer after curling, and the outer layer wraps the middle layer, and the middle layer wraps the inner layer; four different cell-seeding areas each form an outer, sub-outer, middle and inner tubular layer after curling, and the outer layer; the outer layer wraps the sub-outer layer, the sub-outer layer wraps the middle layer, and the middle layer wraps the inner layer.
[0046] In addition, the fact that each layer in the present invention forms at least one complete tubular layer means that after curling, it is not limited to forming only one tubular layer. For example, the inner layer can also form a tubular layer of 1.5, 2, or 2.5 turns, and then the outer layer wraps the inner layer. In this case, the outer layer can also form a tubular layer with more than one turn, such as the outer layer also forming a tubular layer of 1.5 or 3 turns. The above situation is also applicable to three-layer and four-layer structures, as long as the tubular layer formed in the cell-seeding area of the outer layer after curling can sequentially wrap the adjacent inner layer.
[0047] The method for preparing the three-dimensional artificial tubular tissue provided by the present invention is to design a three-dimensional topological structure during the scaffold preparation process. By controlling different scaffold thickness ratios, the two-dimensional cell patterning can be directly replaced with three-dimensional cell patterning, so that the implanted cells can directly achieve three-dimensional growth in the three-dimensional topological structure. Therefore, in the subsequent coiling process, each week of coiling of the scaffold can provide sufficient tissue thickness for the current cell tissue, so that there will be no cavities between the same tissues, and the cells can better adhere and grow. By well controlling the thickness ratio of each different cell planting area during the three-dimensional topological structure design process, the method of the present invention solves the problems of existing methods that cannot eliminate cavities between cell layers, are prone to bleeding and cause arterial dissection, and have the risk of causing aneurysms.
[0048] The design of the three-dimensional topological structure of the present invention can be prepared by different processes such as multi-layer membrane laying needle piercing and combing, or electrospinning and melt blowing. As long as the corresponding thickness ratio is controlled in accordance with the method of the present invention to form a specific three-dimensional topological structure, the three-dimensional growth of cells can be well guaranteed, thereby eliminating the cavity between the cell layers, solving the problem that artificial tubular tissue is prone to bleeding and causing arterial dissection, and will not cause aneurysms.
[0049] The three-dimensional tissue structures formed by curling in the present invention are available in two-, three-, and four-layer configurations with varying porosity, pore size, and fiber diameter. Two-layer structures are suitable for neural tissue, three-layer structures are suitable for vascular tissue, urethra tissue, and vas deferens, and four-layer structures are suitable for intestinal tissue, esophageal tissue, tracheal tissue, and fallopian tubes. This invention is highly suitable for producing a variety of three-dimensional tubular tissue structures with varying structures and functions.
[0050] The present invention contributes to the existing art by providing a three-dimensional artificial tubular tissue with no cavities between layers. This artificial tubular tissue eliminates the risk of bleeding, arterial dissection, or aneurysms during implantation. Existing three-dimensional artificial tubular tissues, on the other hand, often have cavities between layers, which can easily lead to bleeding, arterial dissection, and aneurysms.
[0051] Furthermore, the scaffold of the present invention includes a dense scaffold and a loose scaffold, and the porosity and pore size of the loose scaffold are both larger than those of the dense scaffold. The present invention designs a scaffold with a three-dimensional topological structure to be composed of a dense scaffold and a loose scaffold, and finds that the scaffold structure can well prevent the migration of cells between different layers, and provide sufficient growth space for cells, so that cells can fully grow on the scaffold. By designing the above structure of the scaffold, it is found that the seeded cells can easily invade the loose layer scaffold and be evenly distributed in the scaffold gaps. The advantage is that the cells not only stay on the surface of the scaffold, but can make the formed tissue have the same thickness as this loose scaffold; secondly, the seeded cells cannot penetrate the dense layer scaffold, so that the cells in the overlapping part of the scaffold will not migrate between layers before the dense layer degrades during the curling process. In this way, the thickness of the tissue formed after cell culture can be fully guaranteed, so that the cultured tissue has a controllable thickness and can have a multi-layer tissue composed of cells with different functions.
[0052] For example, when constructing three-dimensional artificial blood vessels, the result of culturing cells on such a scaffold is that the cell suspension can quickly penetrate into the loose layer, while the cells will not fall through the gaps to the bottom of the seeding vessel during the cell seeding process. The endothelial cells in the suspension can quickly aggregate into cell clusters. The clustered cells can grow in accordance with the flat dense layer and will not migrate to the smooth muscle layer. The endothelial tissue formed can be smoother, and the decellularized product is more conducive to the differentiation of autologous vascular cells into endothelial cells after implantation.
[0053] Furthermore, the thickness of the loose scaffold of the present invention is 20-5000 μm, the porosity is more than 90%, the pore size is 20-1000 μm, and the fiber diameter is 0.05-30 μm; the thickness of the dense scaffold is 1-200 μm, the porosity is 59-90%, the pore size is 0.05-500 μm, and the fiber diameter is 0.05-30 μm.
[0054] Furthermore, the preparation process of the loose scaffold and the dense scaffold includes any one or more of casting, microinjection molding, blowing, extrusion, calendering, blown film extrusion, rotational molding, dip coating, 2D printing, hot stamping, meltblowing, water spinning, needle spinning, electrospinning, melt spinning, meltblowing, thermal bonding, chemical bonding, spunlace or needle punching non-woven processes.
[0055] Furthermore, the materials used for the loose scaffold and the dense scaffold include at least one of PGA, PLA, PCL, PLC, PPDO, PHBV, HA, PU, PET, PP, PE, PA, PMMA, PTFE, PES, PEEK, PS, PP, PMMA, PC, PGA-TMC, PGA-CL, chitosan or collagen, or their copolymer materials.
[0056] On the basis of the above, firstly, the present invention provides an artificial tubular tissue consisting of a double-layer structure.
[0057] Specifically, the three-dimensional artificial tubular tissue with a double-layer structure provided by the present invention is neural tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into two different cell planting areas, and controlling the scaffold thickness ratio of the two different areas from thin to thick to be 1:20 to 50 from the starting end to the end of the curling.
[0058] Furthermore, the scaffold of the nerve tissue also includes a double-layer nerve bundle structure, in which the bundled nerves are wrapped by two layers of epithelial tissue, and the thickness ratio of the bundled nerve scaffold is controlled from thin to thick to 1:12 to 24 from the beginning of curling to the end of curling.
[0059] Furthermore, in the area of the nerve stent at the starting end of curling, there are axially distributed prismatic bubbles, with a distribution density of 10-15 per millimeter and a length of 5-20 mm. Each prismatic bubble is independent of each other and is separated from each other by a dense layer of 1-8 microns.
[0060] Peripheral nerve trauma caused by car accidents, accidents, and natural disasters prevents the patient's sensory signals from being transmitted to the brain and spinal cord, and motor commands from the brain cannot be smoothly transmitted to the target organs. Patients who lose the ability to coordinate movements and perceptions of the nervous system will lose the ability to take care of themselves in daily life, causing great trouble to their lives. Currently, there are two mainstream treatment options: one is to use autologous nerve transplantation, and the other is to use allogeneic decellularized nerve transplantation. The former requires a second surgery and requires nerves from other parts of the patient. The latter requires organ or body donation to extract peripheral nerves, so it cannot be mass-produced and is difficult to standardize. Using the technology mentioned in the present invention, an artificial nerve tissue scaffold is constructed, and by seeding the scaffold with neurons, glial cells, and Schwann cells expanded from a cell bank, and using electrical stimulation to guide the nerve axons to extend along the tubular scaffold, the tissue-engineered artificial peripheral nerve produced can be well used for the repair of peripheral nerve trauma after decellularization. The artificial nerve tissue constructed by the method of the present invention does not have cavities between the layers, so there will be no problems such as bleeding and arterial dissection, and there is no risk of causing aneurysms.
[0061] In addition, the three-dimensional artificial tubular tissue with a double-layer structure provided by the present invention also includes medium-caliber arterial vascular tissue, and the preparation method of the stent includes: dividing the stent into two different cell planting areas, and controlling the stent thickness ratio of the two different areas from thin to thick to 1:3 to 75 from the starting end to the end of the curling.
[0062] Secondly, the present invention also provides an artificial tubular tissue composed of a three-layer structure. The artificial tubular tissue with a three-layer structure includes the following categories:
[0063] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention includes medium-caliber arterial vascular tissue, and the preparation method of the stent includes: dividing the stent into three different cell planting areas, and controlling the stent thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:3~58:3~60.
[0064] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention also includes small-caliber arterial vascular tissue, and the preparation method of the stent includes: dividing the stent into three different cell planting areas, and controlling the stent thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:2 to 25:3 to 48.
[0065] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention also includes medium-caliber venous vascular tissue, and the preparation method of the stent includes: dividing the stent into three different cell planting areas, and controlling the stent thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:2 to 38:3 to 70.
[0066] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention includes small-caliber venous vascular tissue, and the preparation method of the stent includes: dividing the stent into three different cell planting areas, and controlling the stent thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:5~50:7~66.
[0067] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention also includes female urethral tissue, and the preparation method of the scaffold includes: dividing the scaffold into three different cell planting areas, and controlling the scaffold thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:5~27:8~60.
[0068] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention also includes male urethral tissue, and the preparation method of the scaffold includes: dividing the scaffold into three different cell planting areas, and controlling the scaffold thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:4~28:10~66.
[0069] Specifically, the three-layered three-dimensional artificial tubular tissue provided by the present invention also includes vas deferens tissue, and the preparation method of the scaffold includes: dividing the scaffold into three different cell planting areas, and controlling the scaffold thickness ratio of the three different areas from thin to thick from the starting end to the end of the curling to be 1:4~700:16~1000.
[0070] In addition, the present invention provides a three-dimensional artificial tubular tissue with a four-layer structure. The artificial tubular tissue with a four-layer structure includes the following categories:
[0071] Specifically, the four-layer three-dimensional artificial tubular tissue provided by the present invention includes intestinal tissue, and the preparation method of the scaffold includes: dividing the scaffold into four different cell planting areas, and controlling the scaffold thickness ratio of the four different areas from thin to thick from the starting end to the end of the curling to be 1:2~4:2~30:3~35.
[0072] Specifically, the intestinal tissue provided by the present invention includes the small intestine, and a protrusion with an axial height of 4-7 mm and a width of 2-3 mm is further provided in the curling starting end region of the small intestine stent.
[0073] Furthermore, the protrusions include villi and crypts, wherein the radial length of the villi is 1200-1600 μm and the axial width is 300-600 μm; the diameter of the crypt neck is 2-10 μm and the inner diameter is 40-50 μm.
[0074] Specifically, the intestinal tissue provided by the present invention also includes the large intestine, and crypts are provided in the stent area of the large intestine stent located at the starting end of curling. The distribution density of the crypts in the inner layer is 100 per square millimeter, the radial depth of the crypts is 1500-2200 μm, and the diameter is 400-500 μm.
[0075] Specifically, the four-layer three-dimensional artificial tubular tissue provided by the present invention includes esophageal tissue, and the preparation method of the scaffold includes: dividing the scaffold into four different cell planting areas, and controlling the scaffold thickness ratio of the four different areas from thin to thick from the starting end to the end of the curling to be 1:2~100:5~600:20~1000.
[0076] Specifically, the four-layer three-dimensional artificial tubular tissue provided by the present invention includes tracheal tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into four different cell planting areas, and controlling the scaffold thickness ratio of the four different areas from thin to thick from the starting end to the end of the curling to be 1:4~9:15~38:25~56.
[0077] Furthermore, the third cell planting region of the tracheal tissue scaffold from the curling start end also includes a portion made of a polymer material or chondrocytes with a mechanical strength higher than 5-10 MPa.
[0078] Furthermore, the region with high mechanical strength is annular and has at least one opening.
[0079] Specifically, the three-dimensional artificial tubular tissue provided by the present invention includes fallopian tube tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into four different cell planting areas, and controlling the scaffold thickness ratio of the four different areas from thin to thick to be 1:2~150:3~300:20~1000 from the starting end of the curling to the end of the curling.
[0080] Furthermore, a villus structure is provided in the cell implantation region of the fallopian tube tissue scaffold near the curling starting end. The villus structure is a protrusion with an axial height of 10-11 μm and a diameter of 0.2-0.3 μm.
[0081] A second object of the present invention is to provide a three-dimensional artificial tubular tissue prepared by any of the above methods.
[0082] Specifically, the three-dimensional artificial tubular tissue includes artificial nerves, artificial arteries, artificial veins, artificial small intestine, artificial large intestine, artificial esophagus, artificial trachea, artificial urethra, artificial fallopian tubes and artificial vas deferens.
[0083] Furthermore, the artificial arterial blood vessels include medium-caliber arterial blood vessels and small-caliber arterial blood vessels.
[0084] Furthermore, the artificial veins include medium-caliber veins and small-caliber veins.
[0085] Furthermore, the artificial urethra includes a male urethra and a female urethra.
[0086] A third object of the present invention is to provide an application of a three-dimensional artificial tubular tissue prepared by any of the above methods, wherein the three-dimensional artificial tubular tissue is used as a replacement for damaged tissue or as an implant in the body.
[0087] The beneficial effects of the present invention are as follows:
[0088] (1) The present invention provides a method for preparing a three-dimensional artificial tubular tissue. The method effectively realizes the design of the three-dimensional topological structure of the scaffold by controlling the thickness ratio between different cell planting areas on the scaffold, promotes the three-dimensional growth of cells, and ensures that during the curling process of the scaffold, each curled scaffold can provide sufficient tissue thickness for the current cell tissue, so that there will be no cavity between the cell layers of the same tissue, and the cells can better adhere and grow on the same scaffold; at the same time, the present invention can prevent the migration of cells between different layers by setting a loose layer and a dense layer scaffold.
[0089] (2) The method for preparing tubular tissue provided by the present invention effectively solves the problems of the existing methods that the cavity between the cell layers cannot be eliminated, bleeding is prone to occur and arterial dissection occurs, and there is a risk of causing aneurysms. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] FIG1 is a schematic diagram of the method for preparing an artificial blood vessel in Example 1;
[0091] Figure 2 is a diagram representing the tissue structure of an artificial blood vessel; (A) The artificial blood vessel prepared by the method of Example 1 of this patent was stained with Masson trichrome after decellularization. The blue part is the extracellular matrix mainly composed of collagen, and the red arrow is the endothelial layer; (B) The human autologous blood vessel was stained with Masson trichrome after decellularization. The blue part is the extracellular matrix mainly composed of collagen; (C) The artificial blood vessel prepared by three-layer curling reported by Cheng Shiyu and his team in 2017 was stained with Masson trichrome. The blue part is the extracellular matrix mainly composed of collagen, and the red arrow indicates the cavity formed by the blood vessel prepared by multi-layer curling; (D) The multilayered artificial blood vessel reported by L'heureux and his team was stained using Masson's trichrome staining. Blue represents the collagen-based extracellular matrix, dark red represents the cell nuclei, and the red arrow indicates the cavity formed by the multilayered coiling method. (E) The multilayered artificial blood vessel Lifeline™ reported by Marissa Peck and her team in 2011. Brown represents CD31 immunostaining, blue represents contrast staining of the cell nuclei, black arrows represent endothelial cells, and the red arrow indicates the cavity formed by the multilayered coiling method. EM: Endothelial membrane; IM: Internal membrane; M: Media; A: Adverta.
[0092] FIG3 is a physical picture of an artificial blood vessel prepared using the method of the present invention;
[0093] FIG4 is an axial tensile test of the artificial blood vessel prepared by the method of the present invention;
[0094] FIG5 is a radial ductility test of the artificial blood vessel prepared by the method of the present invention;
[0095] FIG6 shows the Young's modulus test results of the artificial blood vessel prepared by the method of the present invention, the internal mammary artery, and the artificial blood vessel made of synthetic materials; FIG7 shows the bursting pressure test results of the artificial blood vessels prepared by different methods;
[0096] FIG8 shows the suture strength test results of artificial blood vessels prepared by different methods;
[0097] FIG9 shows the compliance test results of artificial blood vessels prepared by different methods;
[0098] FIG10 shows the elongation at break test results of artificial blood vessels prepared by different methods;
[0099] FIG11 shows the long-term patency test results of artificial blood vessels prepared by different methods;
[0100] FIG12 is a cross-sectional photograph of artificial blood vessels prepared by different methods before the start of mechanical stimulation culture.
[0101] FIG13 is a cross-sectional view of the middle inner wall of each artificial blood vessel after two months of mechanical stimulation but before decellularization.
[0102] FIG14 is a diagram showing the evolution of the cavity ratio in three stages, from the initial stage of culture of each artificial blood vessel to the completion of the decellularization process of the blood vessel.
[0103] FIG15 is a diagram showing the evolution of the cavity ratio of the artificial blood vessels prepared in the examples of the present invention and the comparative example in three stages, from the initial stage of culture to the completion of the decellularization treatment of the blood vessels.
[0104] FIG16 shows angiographic images of each artificial blood vessel taken three months after implantation.
[0105] FIG17 is an angiographic image of the artificial blood vessel prepared by the method of Example 2-7 of the present invention three months after implantation.
[0106] FIG18 is an angiographic image of the artificial blood vessel prepared by the method of Comparative Examples 1-9 of the present invention at the third month after implantation.
[0107] FIG19 is a comparison result of the tissue cell density of the scaffold of the present invention using a dense layer and a loose layer structure and using only a loose layer structure.
[0108] FIG20 shows the cell distribution density statistics of each layer of tissue after section staining of the dense layer and loose layer structure used in the scaffold and the loose layer structure used only in the scaffold after culturing for 2 weeks, 4 weeks and 6 weeks.
[0109] FIG21 is a diagram showing the intestinal crypt and villus structures designed in the artificial intestine of the present invention.
[0110] FIG22 is a diagram showing the structure of the prismatic vesicle designed in the artificial nerve of the present invention.
[0111] 23-30 show the results of cavities in artificial blood vessel tissues described in prior arts 1 to 7. DETAILED DESCRIPTION
[0112] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in detail below with reference to the following embodiments. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not intended to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still fall within the scope of protection of the present invention.
[0113] Example 1
[0114] The method for preparing a 3 mm caliber artificial blood vessel comprises the following steps:
[0115] (1) Preparation of scaffolds;
[0116] (2) Seeding cells on the scaffold;
[0117] (3) Curling into a three-dimensional tubular structure and culturing in vitro.
[0118] The cell scaffold used in this 3mm caliber artificial blood vessel product has three cell planting areas: endothelial cell planting area, smooth muscle cell planting area and fibroblast planting area. The three areas can be connected by inserting fibers into each other through needle piercing, or by using degradable sutures, or by using electrospinning / melt spinning overlap spinning, or ultrasonic welding. The inner radius of the blood vessel is 1.5mm and the length is 12cm. The thickness of the three cell planting areas on the cell scaffold is controlled to be 100μm, 400μm and 500μm from thin to thick, that is, the scaffold thickness ratio is 1:4:5 from thin to thick.
[0119] The scaffold in the endothelial cell planting area has a double-layer structure, consisting of a dense layer and a loose layer structure. The material of the dense layer scaffold preferably uses a smaller fiber diameter of 8μm, a smaller void diameter of 3μm, a thinner scaffold thickness of 5μm, and a width of 12.6mm. A flat and uniform scaffold is preferred, and the scaffold material can be degraded within 4-6 weeks. This dense layer can be prepared by weaving, meltblowing or electrospinning. The material of the loose layer scaffold preferably has a fiber diameter of 5μm, a larger void diameter of 30μm, and a scaffold thickness of 95μm. The above-mentioned dense layer and loose layer structures are bonded by biological glue or the like. The result of culturing cells on this type of cell scaffold is that the cell suspension can quickly penetrate into the loose layer, while the cells will not fall through the gaps to the bottom of the seeding vessel during the cell seeding process. The endothelial cells in the suspension can quickly aggregate into cell clusters. The clustered cells can grow in contact with the flat dense layer and will not migrate to the smooth muscle layer. The formed endothelial tissue can be smoother, and the decellularized product is more conducive to the differentiation of autologous vascular cells into endothelial cells after implantation.
[0120] The smooth muscle cell-seeding area also has a bilayer structure, with the dense and loose layers differing from the endothelial cell area in parameters, characteristics, and functions. The dense layer preferably has a smaller fiber diameter of 5μm, a void diameter of 3μm, a scaffold thickness of 10μm, and a width of 13mm. The preferred scaffold material can degrade within 2-5 weeks. This dense layer can be prepared by methods such as weaving, meltblowing, or electrospinning. The loose layer preferably has a fiber diameter of 2μm, a larger void diameter of 10μm, and a scaffold thickness of 390μm. The scaffold is preferably flat and uniform, and degrades within 2-5 weeks. The two layers are bonded together by a bioglue or other method. Culturing cells on this cell scaffold results in rapid infiltration of the smooth muscle cell suspension into the loose layer, where the smooth muscle cells in the suspension rapidly aggregate into cell clusters, forming smooth muscle tissue. These cells secrete varying amounts of elastin and collagen under varying axial mechanical stimulation, facilitating the differentiation of autologous vascular cells into smooth muscle cells after implantation.
[0121] The scaffold in the fibroblast seeding area is composed of a single-layer loose scaffold, preferably with a minimum fiber diameter of 2μm, a maximum void diameter of 12μm, a maximum scaffold thickness of 500μm, and a width of 26mm. The scaffold is preferably flat and uniform, and made of a scaffold material that degrades within 2-5 weeks. As a result of culturing cells on this cell scaffold, the fibroblast suspension can quickly penetrate into the loose layer, and the fibroblasts in the suspension can quickly aggregate into cell clusters, forming fibroblast tissue, which secretes varying amounts of elastin, fibronectin, and collagen, exchanging substances and providing nutrients to the vascular tissue during the culture process.
[0122] The materials used for the dense layer and loose layer scaffolds mentioned above may include at least one of PGA, PLA, PCL, PLC, PPDO, PHBV, HA, PU, PET, PP, PE, PA, PMMA, PTFE, PES, PEEK, PS, PP, PMMA, PC, PGA-TMC, PGA-CL, chitosan or collagen, or copolymer materials thereof.
[0123] The specific scaffold preparation methods are listed as follows: PGA-CL, PLGA or PLC is combed into a loose structure through a melt-blowing process, the same or different materials are dissolved in an organic solvent using an electrospinning process, and the materials are sprayed on the loose structure through an electric field to form a scaffold structure that combines dense and loose structures. The electric field used is controlled at 10-30kV, the nozzle diameter is between 0.1-0.8mm, the polymer extrusion speed is controlled at 0.1 to 20ml / min, the dissolved polymer concentration is between 5-50%, and the distance between the nozzle and the collector is controlled at 2-30cm. Collectors including rollers and flat plates can be used. PLA or PHB can also be used as an adhesive, applying 3g / cm between the loose layer and the dense layer. 2 Then overlap and let it stand for 20 minutes to 8 hours to wait for it to be bonded and fixed. Similarly, thinner stents can also be fused with thicker stents in this way. Or use ultrasonic welding to heat the polymer material in situ by ultrasonic wave at the overlap of thinner stent and thicker stent, every 1-10cm 2 Set a welding point, and weld each time for 0.1ms to 1s to combine the two layers of structure. Alternatively, the two layers of brackets to be combined can be woven by high-pressure water spunlace. The water spunlace nozzle pressure is controlled at 70-180Pa, the nozzle is generally between 0.15 and 0.3mm, the water flow is controlled at 0.2 to 2 liters / minute, and the water spunlace density is set at 2-10 / cm 2 .
[0124] After the stent is prepared, glue is dispensed into the target area every 10mm. 2 200 μl of cells were seeded. The cell-seeded scaffold was tightly crimped along a clean 1.5 mm radius stainless steel rod. After crimping, the overlapping layers of the tubular scaffold were sutured and fixed at both ends using surgical sutures, and then removed from the metal rod.
[0125] The coiled tubular tissue is cultured in a 37°C culture medium under continuous periodic mechanical pulse stimulation for eight weeks, with the medium replaced every 72 hours. Once the scaffold material has completely degraded, the tissue undergoes decellularization and is immersed in a preservation solution containing sodium heparin and modified proteins such as endothelial growth factor for more than 24 hours before it can be used for clinical treatment or long-term storage.
[0126] The small-caliber artificial blood vessel prepared using the above method has a smooth endothelial layer and has radial and axial extensibility that matches that of autologous blood vessels. It has strong compliance and will not easily cause lumen closure under twisting or bending.
[0127] FIG1 is a schematic diagram of the division of different cell seeding areas on the scaffold in the above preparation method, seeding cells in different areas, and curling into blood vessels from the curling starting end to the curling ending end after the cell seeding is completed.
[0128] Example 2
[0129] Referring to the method of Example 1, the difference is that the thickness of the three cell seeding areas on the cell scaffold is controlled to be 100 μm, 500 μm and 700 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:5:7.
[0130] Example 3
[0131] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 100 μm, 1000 μm and 4000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:10:40.
[0132] Example 4
[0133] Referring to the method of Example 1, the difference is that the thickness of the three cell seeding areas on the cell scaffold is controlled to be 100 μm, 200 μm and 300 μm from thin to thick, that is, the scaffold thickness ratio is 1:2:3 from thin to thick.
[0134] Example 5
[0135] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 100 μm, 200 μm and 210 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:2:2.1.
[0136] Example 6
[0137] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 100 μm, 2500 μm and 4800 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:25:48.
[0138] Example 7
[0139] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 800 μm and 5000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:80:500.
[0140] Example 8
[0141] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 500 μm and 660 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:50:66.
[0142] Comparative Example 1
[0143] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 100 μm, 180 μm and 500 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:1.8:5.
[0144] Comparative Example 2
[0145] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 1 μm, 40 μm and 3200 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:40:3200.
[0146] Comparative Example 3
[0147] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 100 μm, 150 μm and 2000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:1.5:20.
[0148] Comparative Example 4
[0149] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 12 μm and 3000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:1.2:300.
[0150] Comparative Example 5
[0151] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 180 μm and 3100 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:1.8:310.
[0152] Comparative Example 6
[0153] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 820 μm and 3000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:82:300.
[0154] Comparative Example 7
[0155] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 850 μm and 2500 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:85:250.
[0156] Comparative Example 8
[0157] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 1000 μm and 4000 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:100:400.
[0158] Comparative Example 9
[0159] Referring to the method of Example 1, the difference is that the scaffold thicknesses of the three cell seeding areas on the cell scaffold are controlled to be 10 μm, 18 μm and 4800 μm from thin to thick, that is, the scaffold thickness ratio from thin to thick is 1:1.8:480.
[0160] Comparative Example 10
[0161] Prior art 1: An artificial blood vessel was prepared according to the method described in the reference (Stankus JJ, Soletti L, Fujimoto K, et al. Fabrication of cell microintegrated blood vessel constructs through electrohydrodynamic atomization [J]. Biomaterials, 2007, 28(17): 2738-2746.). The artificial blood vessel slices described in the reference have cavities (as shown in FIG23 ). According to the cavity ratio calculation method described in the subsequent patent, the cavity ratio of the blood vessel was 15% three months after implantation in an animal.
[0162] Comparative Example 11
[0163] Prior art 2: An artificial blood vessel was prepared by referring to the method in the literature (Zheng W, Wang Z, Song L, et al. Endothelialization and patency of RGD-functionalized vascular grafts in a rabbit carotid artery model [J]. Biomaterials, 2012, 33 (10): 2880-2891.). The artificial blood vessel slices described in the literature had cavities (as shown in FIG24 ), and the cavity rate of the blood vessel was 12% three months after implantation in the animal body.
[0164] Comparative Example 12
[0165] Prior art three: An artificial blood vessel was prepared according to the method described in the literature (Teebken OE, Haverich A. Tissue engineering of small diameter vascular grafts [J]. European journal of vascular and endovascular surgery, 2002, 23(6): 475-485.). The artificial blood vessel slices described in the literature had cavities (as shown in FIG25 ). The cavity rate of the blood vessel was 10% three months after implantation in an animal.
[0166] Comparative Example 13
[0167] Prior Art 4: An artificial blood vessel was prepared according to the method described in the literature (Kim MJ, Kim JH, Yi G, et al. In vitro and in vivo application of PLGA nanofiber for artificial blood vessel [J]. Macromolecular Research, 2008, 16: 345-352). The artificial blood vessel slices described in the literature contained cavities (as shown in FIG26 ). The cavity rate of the blood vessel was 14% three months after implantation in an animal.
[0168] Comparative Example 14
[0169] Prior art 5: An artificial blood vessel was prepared according to the method in the literature (Wang W, Hu J, He C, et al. Heparinized PLLA / PLCL nanofibrous scaffold for potential engineering of small-diameter blood vessel: Tunable elasticity and anticoagulation property [J]. Journal of Biomedical Materials Research Part A, 2015, 103(5): 1784-1797.). The artificial blood vessel slices described in the literature had cavities (as shown in FIG27 ). The cavity rate of the blood vessel was 13% three months after implantation in animals.
[0170] Comparative Example 15
[0171] Prior art six: An artificial blood vessel was prepared according to the method of the literature (L'Heureux N, Dusserre N, Konig G, et al. Human tissue-engineered blood vessels for adult arterial revascularization [J]. Nature medicine, 2006, 12(3): 361-365.). The artificial blood vessel slices described in the literature had cavities (as shown in Figures 28 and 29). The cavity rate of the blood vessel was 10% three months after implantation in animals.
[0172] Comparative Example 16
[0173] Prior art seven: An artificial blood vessel was prepared by referring to the method in the literature (Talacua H, Smits AIPM, Muylaert DEP, et al. In situ tissue engineering of functional small-diameter blood vessels by host circulating cells only [J]. Tissue Engineering Part A, 2015, 21 (19-20): 2583-2594.). The artificial blood vessel slices recorded in the literature had cavities (as shown in Figure 30), and the cavity rate of the blood vessel was 9% three months after implantation in animals.
[0174] Experimental Example 1
[0175] Taking the preparation of an artificial blood vessel with a small diameter of 3 mm as an example, after decellularization, a cross section of the blood vessel was taken and the tissue structure was characterized using Masson's trichrome staining.
[0176] From Figure 2, it can be clearly observed that the prepared artificial blood vessel has a structure composed of three types of cells. Among them, the inner epidermis secreted by endothelial cells is denser than the endothelial layer and the middle layer made by smooth muscle cells, and is only the thickness of a single cell. Smooth muscle cells form two structures, the endothelial layer and the middle layer. The extracellular matrix of the endothelial layer is distributed in a circumferential direction, and the extracellular matrix of the middle layer is distributed axially. The outer layer is composed of the extracellular matrix of fibroblasts and is the loosest compared to the other three layers. These characteristics are highly consistent with human autologous blood vessels. The artificial blood vessel prepared by the present invention has a dense endothelial layer similar to the original body.
[0177] Experimental Example 2
[0178] The key to the mechanical indicators of artificial blood vessels lies in whether their mechanical properties can match those of human autologous blood vessels, while having better toughness and being able to maintain operation for a longer period of time. For example, the small-caliber arterial blood vessels mentioned in the present invention have nonlinear elastic constants that can cause the blood vessels to have greater stress when the blood flow suddenly increases and the inner diameter of the blood vessels increases, preventing them from further expanding; at the same time, under normal pulsation, the blood vessels can freely shrink and expand, reducing the pressure in the blood vessels. An artificial blood vessel made of a single material will not be able to match the autologous blood vessels at the graft site due to its linear elastic curve, accelerating intimal hyperplasia and thrombosis.
[0179] In this experiment, the following mechanical properties tests were performed on 6 cm long tissue-engineered artificial blood vessels (3 mm inner diameter, N=6), synthetic blood vessels (3 mm inner diameter, PU, N=5), and decellularized human mammary arteries (~2.8 mm, N=7).
[0180] (1) Ring / length tensile test:
[0181] This experiment uses a uniaxial tensile device to pull a vascular tissue along its cross section until it breaks, and then records and estimates its maximum tensile strength and elongation at break.
[0182] First, a 5 mm long section of blood vessel was cut and placed on two parallel hooks made of 1.2 mm diameter stainless steel wire. The hooks were then pulled apart at a speed of 35 mm / min until the tissue was disconnected. The data were sampled using a LabView data acquisition system.
[0183] In addition, a 20 mm long blood vessel was cut and the two ends were fixed on two 60 mm long stainless steel wire clamps. The hooks were then pulled apart at a speed of 45 mm / min until the tissue was disconnected, and samples were collected using a LabView data acquisition system.
[0184] (2) Suture strength test:
[0185] For suture strength testing, a vascular segment approximately 15 mm in length was cannulated onto a vertical metal support shaft connected to an electronic scale. A simple, brief suture with a 2-mm interval between stitches was performed using a BV-1 needle and 5-0 suture. The suture was pulled out at a constant speed of 120 mm / min until it broke. Data was collected using a LabView data acquisition system.
[0186] (3) Burst pressure test:
[0187] A blood vessel of approximately 5 cm in length was cannulated at both ends and pressurized with phosphate-buffered saline (PBS) at a rate of 80 to 100 mmHg / s until the tissue burst. Samples were collected using a LabView data acquisition system and an electronic pressure gauge.
[0188] (IV) Compliance test:
[0189] Compliance testing involves measuring the ratio of the difference in internal diameter between the vessel at rest and under pressure to the pressure difference. A 5-cm vessel segment is tensioned to 0.460 Newtons and pressurized with phosphate-buffered saline (PBS) to 50 and 300 mmHg. High-definition images are then captured for external diameter measurement. Prior to testing, cross-sections from the same vessel are fixed in formalin to allow for histological analysis of the resting geometry.
[0190] The experimental results are shown in Figures 3 to 11.
[0191] Figure 3 shows an artificial blood vessel prepared using the method of Example 1 of the present invention. The artificial blood vessel was found to be soft, smooth, and exhibited uniform tissue growth. Figure 4 shows the artificial blood vessel stretched at both ends using forceps, showing that it could be stretched to approximately twice its original length, demonstrating that the artificial blood vessel prepared using the patented method has excellent axial stretchability. Figure 5 shows the artificial blood vessel stretched to approximately 1.5 times its original diameter using forceps, demonstrating that the artificial blood vessel prepared using the patented method has excellent radial extensibility.
[0192] From the mechanical property comparison of FIG6-FIG11, it can be seen that the mechanical properties of the artificial blood vessel prepared by the present invention are highly similar to those of the autologous blood vessel.
[0193] Further research has revealed that tissue-engineered artificial blood vessels produced using this patented method have no cavities in their endothelial layer. However, existing multi-layer blood vessels produced using other coiling methods, such as stacking multiple coils within the same region, can create multiple cavities of varying sizes within that region. These cavities significantly reduce the mechanical strength of the circumferential direction and hinder post-implantation vessel repair, significantly increasing the risk of post-operative endothelial hyperplasia, smooth muscle cell migration, and aneurysm formation.
[0194] Furthermore, the artificial blood vessels prepared using this patented method match the Young's modulus and compliance of the upstream and downstream autologous blood vessels after implantation, far outperforming existing synthetic blood vessels. Furthermore, the blood vessels prepared using this patented method exhibit superior long-term patency, are less prone to kinking during implantation, and exhibit hemodynamically compatible sutures, further reducing the risk of endothelial hyperplasia and improving long-term patency (see Experimental Example 3 for details).
[0195] Experimental Example 3
[0196] Testing of the cavity ratio of tissue-engineered artificial blood vessels
[0197] According to the literature (DOI: https: / / doi.org / 10.7461 / jcen.2020.22.3.127, Clinical analysis of young adult patients with ruptured intracranial aneurysms: a single-center study of 113 consecutive patients, J Cerebrovasc Endovasc Neurosurg. 2020; 22(3): 127-133. Published online September 21, 2020), the average size of intracranial aneurysms in young people (<=40 years old) is in the range of 6.6±3.7mm. However, in young people, aneurysms smaller than 5mm can cause symptoms. The study pointed out that young people have a higher risk of rupture of small aneurysms than middle-aged and elderly people. Among them, 94.2% of aneurysm ruptures occurred in aneurysms smaller than 10mm, and among these, 47.6% of ruptures occurred in aneurysms smaller than 5mm.
[0198] When an aneurysm is initially formed, the vessel wall thickness that forms the cavity is not yet strong enough to support the aneurysm. Frequent exposure to high pressure and high-intensity living environments at this time can easily lead to aneurysm rupture. The risk of rupture is significantly influenced not only by the size of the aneurysm but also by its shape. The literature indicates that elongated or other irregularly shaped aneurysms are more prone to rupture.
[0199] The above results indicate that if cavities exist within the artificial blood vessel's walls, particularly gaps near the inner wall, the endothelial cell layer, after decellularization, can easily rupture under the impact of blood, causing blood to flow into the smooth muscle layer and form an aneurysm. Therefore, cavities within finished artificial blood vessels should be minimized or eliminated. Cavities and gaps of any shape and size pose a hidden danger to patients. The inventors, using healthy blood vessels as a benchmark, analyzed 300 stained sections of human radial arteries and found a cavitation rate of 2±0.6%. Therefore, this experiment established that the cavitation rate of artificial blood vessels must be at least less than 2%.
[0200] The aneurysm mechanism described above also applies to other artificial tubular tissues, such as the intestine or urethra. The presence of cavities between the layers of the tubular wall can also cause digestive fluids, gas, or urine to flow into the middle layer, forming a cystic aneurysm. Under pressure, this can also lead to rupture, threatening the patient's life. Therefore, the walls of artificial tubular tissues should be free of any cavities or gaps of any kind.
[0201] For example, when a cavity exists within a vascular implant, it can lead to various vascular lesions, ultimately causing necrosis and blockage. The most common lesion is a hemangioma. When the vessel wall surrounding the cavity ruptures, blood flows into the cavity, tearing the wall and causing the cavity to expand, forming a false lumen. The expanded false lumen prevents blood from flowing in the correct direction, resulting in reverse flow and vascular blockage.
[0202] On the other hand, when autologous cells attempt to repair the cavity, they may also cause thrombosis. Once blood penetrates the vessel wall and flows into the cavity, platelets and cholesterol accumulate there to form a thrombus. The formation of thrombi further reduces the mechanical strength and flexibility of the blood vessels, making them more susceptible to rupture. Continued accumulation of thrombi further narrows the vessel lumen, hindering normal blood flow, resulting in decreased flow rate and even blockage. When thrombi fall off, the free blood clots in the vessel can also cause blockage of downstream vessels.
[0203] At the same time, the cavity reduces the strength of the blood vessel itself, lowering its burst pressure and making it more likely to cause endothelial rupture. Smooth muscle cells in the middle layer of the blood vessel migrate to the inner wall of the blood vessel, causing endothelial hyperplasia, which in turn narrows the blood vessel and causes blockage.
[0204] In addition to the aforementioned lesions, cavities are more susceptible to the accumulation of infection sources and inflammation, which in turn leads to connective tissue proliferation, which can also cause vascular stenosis and blockage. In summary, cavities within blood vessels can lead to a variety of vascular lesions, including hemangiomas, thrombosis, endothelial rupture, and endothelial hyperplasia, ultimately leading to vascular blockage. These lesions are also the primary cause of early vascular blockage requiring intervention.
[0205] Under this premise, the inventors of this patent studied all previously prepared artificial tubular tissues and counted the number and size of cavities. The preparation methods of artificial blood vessel samples were based on the following methods: (a) constructing a multilayer tubular blood vessel by using a traditional multilayer curling and stacking method (A completely biological tissue-engineered human blood vessel, 1998, NICOLA SL'HEUREUX et al.); (b) constructing a three-layer tubular blood vessel by using a self-curling method (CN108653815B, National Center for Nanoscience and Technology); and (c) preparing a tissue-engineered artificial blood vessel using the method of this patent.
[0206] Compared with the artificial blood vessels prepared by the above-mentioned methods (a) and (b), the artificial blood vessels prepared by the method (c) of this patent can control the interlayer thickness, thereby minimizing the formation of cavities while ensuring the mechanical properties and physiological structure of the blood vessels. This ensures that the prepared blood vessels will not develop the above-mentioned lesions due to cavities, greatly increasing the patency of the vascular implant and achieving good results in three months of animal experiments.
[0207] (1) The experimental method is as follows:
[0208] According to the method in Example 1, 4 mm inner diameter, 12 cm long blood vessels were prepared, with 30 samples of each type. Sampling was performed in four stages. In the first stage, five blood vessels were removed after cell seeding and coiling, and before mechanical stimulation culture began, for cross-sectional imaging. In the second and third stages, ten blood vessels were collected, respectively, after eight weeks of culture, before and after decellularization. In the fourth stage, 5 cm of each blood vessel was implanted into New Zealand rabbits for radial artery replacement, and their patency was observed three months after surgery.
[0209] In the first stage, because the connection between the inner layers of the tube wall has not yet been established, the slicing process is prone to cause peeling of the layers, and the cavity at this time is visible to the naked eye, so only the cross-section is used to evaluate the cavity in the blood vessel wall. During the evaluation, samples are taken from each blood vessel at both ends (3 cm) and the middle (6 cm) to observe the uniformity of the fusion between its layers. After processing, the blood vessels in the second, third and fourth stages are sent to professional institutions for slicing and staining. Each blood vessel is sampled from both ends (3 cm) and the middle (6 cm) to observe the uniformity of the fusion between its layers. The specific slicing and staining process refers to the public conventional method and will not be explained in detail here. However, in order to reduce the impact of slicing on the structure of the blood vessel wall, the following treatments are performed on the blood vessels when preparing the samples:
[0210] 1) Take two blood vessels with a total length of 12 cm and soak them in a culture dish filled with PBS buffer to clean the remaining culture medium in the blood vessels;
[0211] 2) Select the middle portion of the 12 cm blood vessel and cut it 3 cm and 9 cm from the left or right end respectively using medical scissors;
[0212] 3) Use a disposable scalpel to trim irregularities on the blood vessel cross section. Insert the knife from the outer edge of the cross section and perform rotary excision on the irregular area. During excision, always keep the blade in contact with the vessel wall and the backing plate to avoid radial compression of the vessel.
[0213] 4) The two treated blood vessels were named a and b; blood vessel a was decellularized, and blood vessel b served as a blank control group;
[0214] 5) Place blood vessels a and b into separate centrifuge tubes filled with paraformaldehyde fixative, allowing the paraformaldehyde solution to submerge the blood vessels, and then send them for examination.
[0215] Since blood vessels prepared using different preparation methods have different inner diameters, in order to more objectively quantify and compare the interlaminar cavities of different blood vessels, the following formula is used to define the cavitation rate:
[0216] Cavity ratio % = (cavity area / tube inner area) × 100%.
[0217] The cavity area is the sum of all spaces larger than the cell diameter in the photograph or slice.
[0218] (2) Experimental results: The experimental results are shown in Figures 12-15.
[0219] Figure 12 shows cross-sectional photographs of artificial blood vessels before mechanical stimulation culture, including: (a) an artificial blood vessel prepared using the traditional multi-layer curling and stacking method; (b) an artificial blood vessel prepared using the self-curling method; and (c) an artificial blood vessel prepared using the patented method. As can be seen from Figure 12, the artificial blood vessels prepared using the traditional multi-layer curling and stacking method exhibit numerous cavities between layers before mechanical stimulation culture. This is because, despite being fixed with biological glue, the multiple layers of material will inevitably collapse due to gravity, leading to cavities. Artificial blood vessels prepared using the self-curling method achieve a certain improvement in cavitation ratio before culture due to the material's own tension, but the consistent thickness prevents them from achieving a thickness ratio compatible with autologous blood vessels after curling. However, blood vessels prepared using the patented method naturally develop an appropriate thickness ratio after forming, and cavities are not enlarged due to collapse. Layers can be bonded together in the early stages of culture, promoting fusion and formation of the vessel wall.
[0220] Figure 13 shows cross-sectional images of the mid-section of a blood vessel after two months of mechanical stimulation and before decellularization. The images include: (a) an artificial vessel produced using the traditional multi-layer coiling method; (b) an artificial vessel produced using the self-coiling method; (c) an artificial vessel produced using the patented method; and (d) a section of a rat artery, with the arrows marking the larger cavities. As can be seen from the images, the cavities in the vessels produced using the traditional multi-layer coiling method are smaller and more numerous, with a higher concentration located close to the endothelium, significantly reducing endothelial strength. These cavities lack a fixed shape but generally extend radially outwards over a large distance. In the vessels produced using the self-coiling method, the cavities appear at the interface between the layers, are mostly narrow and elongated, and their distance from the endothelium is determined by the coiling material. The inner wall of the vessels produced using the patented method is smooth, compact, and free of obvious cavities. The inner wall is uniformly covered with a layer of endothelial cells. The outermost layer of fibroblasts and smooth muscle cells exhibits a distinct density, more similar to that of a normal blood vessel. Furthermore, the biodegradable polymer used as the scaffold has been completely absorbed.
[0221] Figure 14 shows the evolution of the cavity rate in three stages, from the initial stage of vascular culture to the completion of decellularization of the blood vessels. As can be seen from Figure 14, the traditional multi-layer curling superposition method and the self-curling method have a cavity rate of nearly 40% in the first stage. After mechanical stimulation and culture, the degradable scaffold further shrinks and the tissue layers begin to fuse, resulting in a reduction in the cavity. In the third stage after the cell elution treatment, cells that have not fully formed tissue are peeled off to form new cavities, so the cavity rate increases. In contrast, the cavity rate of the blood vessels prepared using this patented method always remains at a low level, and the cavity rate does not rise again after decellularization, indicating that dense tissue has been formed inside the blood vessel wall.
[0222] The artificial blood vessels prepared in the embodiments of the present invention and the comparative examples were cultured, and their cavity rates were statistically analyzed in three stages. The results are shown in Table 1, and a cavity rate evolution diagram was drawn. Figure 15 shows the cavity rate evolution of different artificial blood vessel samples prepared in the embodiments and comparative examples in three stages from the initial stage of blood vessel culture to the completion of the decellularization of the blood vessels. As can be seen from Figure 15, in the initial stage of blood vessel culture, the cavity rate of the artificial blood vessels obtained by the method of the embodiments of the present invention is relatively low, while the cavity rate of the artificial blood vessels obtained by the comparative example method is relatively high. After the second stage of mechanical stimulation culture, the scaffold degraded and the contracted tissue layers began to fuse, resulting in a decrease in the cavity rate. In the third stage after the cell elution treatment, the cells of the comparative example that had not fully formed tissue were peeled off to form new cavities, so the cavity rate increased; in contrast, the cavity rate of the artificial blood vessels prepared by the method provided in the embodiments of this patent always remained at a low level, and the cavity rate did not rise again after the decellularization treatment, indicating that dense tissue has been formed inside the blood vessel wall.
[0223] Table 1
[0224] To further compare the impact of the void ratio of the artificial blood vessels prepared in the first stage on the subsequent culture stage, the inventors used an artificial blood vessel prepared by the self-curling method as an example. By applying a degradable biofusion agent mainly composed of biogelatin, PEG, or fibrin to each layer before curling, the void ratio of the artificial blood vessels in the first stage was tested to be 3%. Then, experiments in the second and third stages were carried out. The results showed that the void ratio still increased after the culture. After adopting the above treatment method, the void ratio in the second stage was 2%, but after the third stage, the void ratio rebounded to more than 6%. This shows that even if the existing preparation process achieves a good initial void ratio, it is still easy to produce a large number of cavities during the subsequent culture process.
[0225] Figure 16 compares angiographic images of the prepared blood vessels three months after implantation into animals, including: (a) an artificial blood vessel made using the traditional multi-layer curling and stacking method; (b) an artificial blood vessel made using the self-curling method; and (c) an artificial blood vessel made using the patented method. The black areas indicated by arrows indicate areas with reverse flow. It is clear from the figures that the blood vessels prepared using the traditional multi-layer curling and stacking method are completely blocked and even have reverse flow, which is highly likely to be an aneurysm. The blood flow rate in the blood vessels prepared using the self-curling method is significantly slowed, and thrombosis may have occurred within the blood vessels. Only the blood vessels prepared using the patented method maintain a flow rate consistent with that at the time of initial implantation, demonstrating that the artificial blood vessels prepared using the patented method have no cavities and will not experience thrombosis or aneurysms.
[0226] In this experiment, artificial blood vessels prepared according to Examples 2-7 of the present invention were implanted in animals and angiographic observations were performed three months later. The resulting angiographic images are shown in Figure 17 , where images A to F correspond to the artificial blood vessels prepared according to Examples 2-7, respectively. As can be seen in Figure 17 , blood flow in the artificial blood vessels prepared according to the methods provided in the above examples of the present invention remained unobstructed, with no evidence of thrombosis or aneurysms.
[0227] Three months after implantation of the artificial blood vessels prepared in Comparative Examples 1-9 of the present invention into animals, angiographic observations were performed. The resulting angiographic images are shown in Figure 18 , where A and B correspond to the artificial blood vessel samples prepared by the methods of Comparative Examples 1-9, respectively. As can be seen from Figure 18 , the artificial blood vessels prepared by the methods provided in the comparative examples all exhibited blood flow obstruction three months after implantation into the animals, indicating a high probability of developing thrombosis or aneurysm.
[0228] Experimental Example 4
[0229] The loose layer and dense layer scaffold structure used in this patent method is compared with the scaffold using only the loose layer, as follows:
[0230] (1) Ten loose scaffolds and ten loose-dense composite scaffolds were taken and fluorescent transfected cells (50,000 cells / cm) were planted at fixed locations and quantitatively. 2 ), cultured for 2 days, and every 12 hours, the cell distribution density and number on the scaffold were counted using a confocal microscope. The results are shown in Figure 19. The solid line represents the use of loose and dense composite scaffolds, and the dotted line represents the use of only loose structure scaffolds. The y-axis represents the cell distribution density, and the unit is (10,000 cells / cm 2 ), with the x-axis representing time. As shown in Figure 19, the cell differentiation rate of scaffolds using only the loose layer is lower than that of cells using the loose-dense composite scaffold. Furthermore, the cell distribution of the composite scaffold is narrower than that of cells on the same scaffold, making it more suitable for process standardization in mass production.
[0231] (II) 12 loose tubular scaffolds and 12 loose dense composite scaffolds were taken after seeding cells. Four scaffolds were sacrificed at each stage after two weeks, four weeks, and six weeks of culture. The distribution of cells in each layer of tissue was counted after section staining. As shown in Figure 20, the dotted line is the loose scaffold, the solid line is the composite scaffold, the black line is the fibroblast layer, the dark gray line is the smooth muscle cell layer, and the light gray line is the endothelial cell layer. As can be seen from Figure 20, the distribution boundaries between the layers of the tubular tissue using the composite scaffold are more obvious, without too much overlap. A small amount of cells migrated after the dense scaffold layer degraded after about four weeks. At the same time, the tubular tissue made by using a single loose structure scaffold has unclear cell distribution boundaries, and more cells migrate, making it difficult for the same type of cells to combine and grow into a cluster to form tissue. As can be seen from the figure, the cell density of the single scaffold after six weeks of culture is not obvious compared to the fourth week. In addition, smooth muscle cells entering the endothelial layer may increase the probability of endothelial hyperplasia after implantation, burying hidden dangers for patients.
[0232] Example 9
[0233] This example provides a method for preparing a venoarterial fistula for artificial dialysis. The method differs from Example 1 only in that the vessel caliber is increased from 3 cm to 6 cm, and therefore the width of each region is appropriately increased to accommodate this inner diameter. The scaffold material for this venoarterial fistula can be PCL, PLGA, PLC, or PLA. The cells seeded on the scaffold include human endothelial cells, smooth muscle cells, and fibroblasts. The preparation method is the same as in Example 1, with the thickness ratio of the three cell-seeding regions on the scaffold being controlled to be 1:30:500, from thin to thick.
[0234] Example 10
[0235] A method for preparing a venoarterial fistula for artificial dialysis is described with reference to Example 9, except that the thickness ratios of the three cell layer seeding areas on the stent are controlled to be 1:2:4 from thin to thick.
[0236] Example 11
[0237] This example provides a method for preparing a venoarterial fistula for artificial dialysis. This method differs from Example 1 in that the vessel diameter is increased from 3 cm to 6 cm, and the vessel comprises only two layers: a smooth muscle layer and a fibroblast layer. Therefore, the width of each region is appropriately increased to accommodate this inner diameter. The scaffold material for this venoarterial fistula for artificial dialysis can be PGLA, PLC, or PLA. The cells seeded on the scaffold are human endothelial cells and smooth muscle cells. The preparation method is the same as in Example 1, with the thickness ratio of the two cell-seeding regions on the scaffold being controlled to be 1:20, from thin to thick.
[0238] Example 12
[0239] A method for preparing a venoarterial fistula for artificial dialysis is described with reference to Example 11, except that the thickness ratio of the two cell layer seeding areas on the stent is controlled from thin to thick to be 1:2.
[0240] Example 13
[0241] A method for preparing a venoarterial fistula for artificial dialysis is described with reference to Example 11, except that the thickness ratio of the two cell layer seeding areas on the stent is controlled from thin to thick to be 1:80.
[0242] Example 14
[0243] A method for preparing a venoarterial fistula for artificial dialysis is described with reference to Example 11, except that the thickness ratio of the two cell layer seeding areas on the stent is controlled from thin to thick to be 1:40.
[0244] Example 15
[0245] This embodiment provides a method for preparing an artificial intestinal organ, which differs from the preparation method of Example 1 in that the scaffold of the intestinal lining stem cell area is prepared by a hydrogel containing arginine-glycine-aspartic acid. Intestinal stem cells are embedded in the hydrogel, and the stem cells and hydrogel are mixed together by suspension culture so that they are evenly distributed in the gel. 405nm light irradiation is used to degrade and soften the hydrogel matrix, thereby controlling the spatiotemporal specificity of the gel. The growth and differentiation of stem cells in the gel can be controlled by controlling the position and time of light irradiation. The thickness ratio of the artificial intestinal scaffold is controlled from thin to thick to be 1:2:10:35. By microscopy, each gel is patterned into an in vivo crypt size of 20μm×300μm and placed in a differentiation medium. The stem cells in the gel are cultured. Differentiation and crypt villus patterning are induced in the differentiation medium (EGF, Noggin and R-spondin), so that the stem cells differentiate into different cell types in the gel and form a crypt villus structure. The scaffold material for this artificial intestinal tissue can be made of PPDO, PHBV, HA, or PLC. The cells planted on the scaffold are intestinal stem cells and smooth muscle cells. The scaffold preparation method includes the method in Example 1, and the following method can also be used: the pattern of intestinal crypts and villi is etched onto a wafer using lithography. This technique first uses lithography to etch the pattern onto the wafer using photoresist and a photolithography machine, and then transfers the pattern to a PDMS mold. Next, the mold is placed upside down on the hydrogel layer, and the three-dimensional structure of the villi and crypts is transferred to the scaffold through extrusion and temperature curing. This technique can accurately replicate the morphology of intestinal villi and crypts on the scaffold surface, thereby simulating the microstructure of the intestine. The intestinal tissue is also designed with a microtopological structure composed of intestinal villi and intestinal crypts. The villi have a radial length of 1200 to 1600 μm, an axial width of 300 to 600 μm, a crypt neck diameter of 2 to 10 μm, and an intraluminal diameter of approximately 40 to 50 μm (structure shown in Figure 21).
[0246] Example 16
[0247] A method for preparing an artificial intestinal organ is described with reference to Example 15, except that the thickness ratio of the artificial intestinal scaffold is controlled from thin to thick to be 1:2:500:2000.
[0248] Example 17
[0249] A method for preparing an artificial intestinal organ is described with reference to Example 15, except that the thickness ratio of the artificial intestinal scaffold is controlled from thin to thick to be 1:50:300:1000.
[0250] Example 18
[0251] A method for preparing an artificial intestinal organ is described with reference to Example 15, except that the thickness ratio of the artificial intestinal scaffold is controlled from thin to thick to be 1:80:700:3000.
[0252] Example 19
[0253] This embodiment provides a method for preparing an artificial nerve, and the only difference between the preparation method and Example 1 is that the artificial nerve and the artificial nerve scaffold thickness ratio from thin to thick are 1:50. In the loose scaffold area of the nerve at the starting end of curling, there are prismatic bubbles distributed along the axial direction. The distribution density of the prismatic bubbles in the inner layer is 10-15 per millimeter, and the length is 5-20 mm. Each prismatic bubble is independent of each other and is separated from each other by a dense layer of 1-8 microns. The material used for the artificial nerve scaffold can be HA, PLGA, PDO or PLC. The cells planted in different cell planting areas on the scaffold are nerve cells, glial cells and Schwann cells respectively. The scaffold preparation method can be: using micro-printing transfer technology, first make a crystal element with a prismatic protrusion structure, then transfer this three-dimensional structure to the hydrogel scaffold, and then curl along the short side direction of the prismatic structure so that its long side is parallel to the axis of the tubular tissue. Low-temperature hot stamping can also be used to shrink the area between the prismatic protrusions. The hot stamping mold used has a pattern staggered with the prismatic protrusions. Temperatures of 30 to 180 degrees Celsius, pressures of 20 to 100 kPa, and a hot stamping time of 10 to 120 minutes are used. Furthermore, axially distributed prismatic bubbles are placed in the loose scaffold region at the beginning of the nerve curl. These bubbles are distributed in the inner layer at a density of 10-15 per millimeter and are 5-20 mm long. Each prismatic bubble is independent of the others and separated by a dense layer of 1-8 microns (see structure in Figure 22).
[0254] Example 20
[0255] This embodiment provides a method for preparing an artificial trachea. The artificial trachea product has a diameter of 1.2-2.0 cm, a length of 5-10 cm, a wall thickness of approximately 1.5 mm, and exhibits longitudinal extensibility and transverse rigidity. The trachea has a four-layer structure: an endothelial cell layer, a smooth muscle cell layer, a chondrocyte layer, and a fibroblast layer. The thickness ratio of each layer, from thin to thick, is 1:9:38:56.
[0256] The difference between its preparation method and Example 1 is that the chondrocyte layer uses a composite structure, which is formed in a dense loose layer with a thickness of 0.7 mm, giving a polymer corrugated support structure with higher mechanical strength. The polymer material is preferably poly-ε-caprolactone (PCL), which is 3D printed by fused deposition molding or electrospinning to form a trapezoidal column with a narrow upper and wide lower part. The upper base of the trapezoidal column is 0.9 mm, and the side is at an angle of 35°±1.5° to the vertical. The length accounts for 80% of the dense loose layer, and is arranged at intervals of 3 mm in the center, and is docked by ultrasonic welding. Chondrocytes are cultured in a high cell density conformation and supplemented with transforming growth factor β (TGF-β). Under long-term mechanical stimulation, cartilage structure is generated, and type II collagen (COL2) and aggrecan (ACAN), as well as cartilage ECM, are secreted. After curling, the cartilage ring is formed into a C-shaped cartilage ring scaffold, which allows for longitudinal stretching and bending. The inner region is compressed, while the outer region is subjected to tension. The tensile equilibrium modulus ranges from 1 to 20 MPa to accommodate diaphragm contraction, lung expansion, and neck movement. Simultaneously, the C-shaped ring structure enables the migration of smooth muscle cells and fibroblasts into the interstitial region, possessing radial and axial extensibility that matches that of the native trachea, and allows for the growth and infiltration of autologous microvascular tissue.
[0257] Example 21
[0258] This embodiment provides a method for preparing an artificial digestive tract, with reference to Example 1. The artificial digestive tract in this embodiment is described in detail below:
[0259] 1. Small intestine
[0260] The artificial small intestine has an inner diameter of 15mm to 30mm and consists of four layers: inner, basal, middle, and outer. The wall thickness t and inner diameter d are related by a ratio of t to d / 7. The artificial small intestine scaffold is prepared by dividing the scaffold into four distinct cell seeding regions. From the beginning to the end of the coil, the scaffold thickness ratio of the four regions is controlled to be 1:2:25:35.
[0261] The small intestine has a relatively complex inner layer topology to facilitate the differentiation and metabolism of intestinal stem cells after seeding. This topology can be specifically classified as microscopic topology and macroscopic topology. The microscopic topology is composed of intestinal villi and intestinal crypts. The radial length of the villi is 1200 to 1600 μm, the axial width is 300 to 600 μm, the diameter of the crypt neck is 2 to 10 μm, and the intraluminal diameter is approximately 40 to 50 μm. The macroscopic structure is composed of axial folds similar to the Kerklin folds in the natural structure, which are used to slow down the movement of food in the intestine. The structure is an axial protrusion with a height of 4 to 7 mm and a width of 2 to 3 mm. These two topological structures can be prepared by different methods.
[0262] 2. Large Intestine
[0263] The artificial large intestine has an inner diameter of 40 to 50 mm. The tissue has a four-layer structure: inner, basal, middle, and outer layers. The wall thickness t and inner diameter d have a relationship of approximately t equal to d / 15 to d / 7. The artificial large intestine scaffold is prepared by dividing the scaffold into four distinct cell-seeding regions, maintaining a scaffold thickness ratio of 1:4:30:35 from the beginning to the end of the coil.
[0264] The large intestine also possesses a complex inner topology, primarily composed of intestinal crypts. Crypts are distributed at a density of approximately 100 per square millimeter. Their radial depth ranges from 1500 to 2200 μm, and their diameters range from 400 to 500 μm. This topology can be achieved through various methods.
[0265] Example 22
[0266] This embodiment provides a method for preparing an artificial esophagus, with reference to Example 1. The artificial esophagus in this embodiment is described in detail below:
[0267] The artificial esophagus has an inner diameter of 18 to 22 mm. The tissue has a four-layer structure: inner, basal, middle, and outer layers. The relationship between the wall thickness (t) and the inner diameter (d) is approximately equal to d / 4. The artificial esophagus stent is prepared by dividing the stent into four distinct cell seeding regions, maintaining a thickness ratio of 1:2:5:20 from the beginning to the end of the coil.
[0268] The inner wall of the artificial esophagus does not have a special topological structure and has a smooth surface, which is conducive to the differentiation of autologous vascular stem cells into vascular endothelial cells.
[0269] Example 23
[0270] This embodiment provides a method for preparing an artificial trachea, with reference to Example 1. The artificial trachea in this embodiment is described in detail below:
[0271] The diameter of this artificial trachea is 10-23mm. It has a four-layer structure: inner, basal, middle, and outer layers. The wall thickness (t) and inner diameter (d) are related by a ratio of approximately t / d / 6. The tracheal wall thickness is approximately 3000μm. The artificial tracheal stent is prepared by dividing the stent into four distinct cell seeding regions, maintaining a thickness ratio of 1:9:15:26 from the beginning to the end of the coil.
[0272] Notably, the middle layer of this artificial trachea consists of two sections: one-quarter of the circumference is a loose polymer scaffold, while the other three-quarters is made of a mechanically strong polymer material. This polymer material is characterized by its ability to withstand axial stresses of 5 to 10 MPa without breaking. This section simulates the hyaline cartilage of the autologous trachea. Under prolonged mechanical stimulation, the seeded chondrocytes secrete type II collagen and chondroitin sulfate, promoting the differentiation of autologous stem cells into chondrocytes after implantation.
[0273] The inner wall of this artificial trachea has no unique topological structure; its surface is smooth, facilitating the differentiation of autologous stem cells into tracheal mucosal cells. However, within the layered structure, high-intensity regions are distributed axially in a ring-like pattern, with a spacing of 3-9 mm and a ring width of approximately 7-9 mm.
[0274] Example 24
[0275] The preparation of an artificial male urethra comprises the following steps:
[0276] (1) Preparation of scaffolds;
[0277] (2) Seeding cells on the scaffold;
[0278] (3) curling into a three-dimensional tubular structure and culturing in vitro;
[0279] The scaffold material and preparation process are in accordance with the method mentioned in Example 1.
[0280] The artificial male urethra has a diameter of 5-7 mm. It has a three-layer structure: inner, middle, and outer. The wall thickness (t) and diameter (d) are related by a ratio of approximately t = d / 1.2. The urethra wall thickness is approximately 2-2.6 mm. The artificial male urethra stent is prepared by dividing the stent into three distinct cell seeding regions, maintaining a thickness ratio of 1:4:10 between the coiling start and coiling end.
[0281] It is noteworthy that the middle layer of the artificial trachea is made of a loose and elastic polymer material. The inner wall of the artificial male urethra does not have a special topological structure and its surface is smooth.
[0282] Example 25
[0283] The preparation of an artificial female urethra comprises the following steps:
[0284] (1) Preparation of scaffolds;
[0285] (2) Seeding cells on the scaffold;
[0286] (3) curling into a three-dimensional tubular structure and culturing in vitro;
[0287] The scaffold material and preparation process are in accordance with the method mentioned in Example 1.
[0288] The artificial female urethra has an inner diameter of 5-7 mm. It has a three-layer structure: inner, middle, and outer. The wall thickness (t) and inner diameter (d) are related by a ratio of approximately t = d / 1.5. The urethra wall thickness is approximately 2-2.6 μm. The female urethra stent is prepared by dividing the stent into three distinct cell-seeding regions, maintaining a thickness ratio of 1:27:60 from the beginning to the end of the coil.
[0289] The inner wall of the artificial female urethra does not have any special topological structure and has a smooth surface.
[0290] Example 26
[0291] The preparation of an artificial fallopian tube includes the following steps:
[0292] (1) Preparation of scaffolds;
[0293] (2) Seeding cells on the scaffold;
[0294] (3) curling into a three-dimensional tubular structure and culturing in vitro;
[0295] The scaffold material and preparation process are in accordance with the method mentioned in Example 1.
[0296] The diameter of this artificial fallopian tube is 5 to 12 mm. The tissue has a four-layer structure: inner layer, basal layer, middle layer, and outer layer. The relationship between the tube wall thickness t and the inner diameter d is approximately equal to d / 6. The artificial fallopian tube scaffold is prepared by dividing the scaffold into four distinct cell seeding areas. From the beginning to the end of the coil, the scaffold thickness ratio of the four different areas is controlled to be 1:2:3:20.
[0297] The fallopian tube has a complex inner topology, which facilitates the differentiation of stem cells into mucosal cells after seeding. Within the cell seeding area near the beginning of the curling of the fallopian tube tissue scaffold, a villous structure is present. These protrusions are 10 to 11 μm in height and 0.2-0.3 μm in diameter along the axial direction.
[0298] Example 27
[0299] The preparation of artificial insemination tube includes the following steps:
[0300] (1) Preparation of scaffolds;
[0301] (2) Seeding cells on the scaffold;
[0302] (3) curling into a three-dimensional tubular structure and culturing in vitro;
[0303] The scaffold material and preparation process are in accordance with the method mentioned in Example 1.
[0304] This artificial vas deferens has a diameter of 5 to 7 mm. The tissue has a three-layer structure: inner, middle, and outer. The wall thickness t and inner diameter d have a relationship of approximately t = d / 6. The artificial vas deferens scaffold is prepared by dividing the scaffold into three distinct cell seeding regions, maintaining a scaffold thickness ratio of 1:4:16 from the beginning to the end of the coil.
[0305] The vas deferens has a relatively complex inner topological structure, which facilitates the differentiation of stem cells into mucosal cells after seeding. The inner wall of the artificial vas deferens does not have a special topological structure and its surface is smooth.
[0306] Experimental Example 28
[0307] The preparation of artificial neural tissue includes the following steps:
[0308] (1) Preparation of scaffolds;
[0309] (2) Seeding cells on the scaffold;
[0310] (3) curling into a three-dimensional tubular structure and culturing in vitro;
[0311] The scaffold material and preparation process are in accordance with the method mentioned in Example 1.
[0312] The artificial nerve tissue has a two-layer structure, an inner layer and an outer layer. The preparation method of the artificial nerve tissue scaffold is as follows: the scaffold is divided into two different cell planting areas, and the scaffold thickness ratio of the two different areas is controlled to be 1:20 from the curling start end to the curling end end.
[0313] The artificial nerve tissue can be composed of several double-layer nerves bundled into a bundle, and the bundled artificial nerve is wrapped by two layers of outer skin tissue. The thickness ratio of the scaffold in two different areas from the beginning of curling to the end of curling is controlled to be 1:12.
[0314] This artificial nerve has a relatively complex topological structure. In the loose scaffold area at the starting end of the nerve curling, there are axially distributed prismatic bubbles. The distribution density of the prismatic bubbles in the inner layer is 10-15 per millimeter, and the length is 5-20 mm. Each prismatic bubble is independent of each other and is separated from each other by a dense layer of 1-8 microns.
[0315] Example 29
[0316] Three-dimensional patterning of cell seeding in vascular tissue
[0317] (1) The preparation of this type of tubular vascular tissue is usually felt-type, with a large porosity and a certain elasticity of the pores. After the needle is inserted, it has the ability to rebound and repair the pores. At the same time, because it needs to be fixed horizontally on the cell planting instrument during operation, its structure has a certain rigidity. When preparing this type of felt-type scaffold, the existing felt cloth made of highly biocompatible degradable or non-degradable materials is first used to form a tubular scaffold by curling it and the fibers at its seams are cross-fused by needle piercing. The thickness of the scaffold can be controlled by the number of curled layers, and its thickness ranges from 100μm to 500μm;
[0318] (2) The two ends of the stent tube are butt-jointed with sleeves made of highly biocompatible non-degradable elastic material, and the seams are tightly sutured with surgical sutures. The outermost ends are butt-jointed with the male end of a set of Luer quick connectors, which are fixed to this section of connectors with sutures. This section of the stent can then be butt-jointed and fixed to the cell implantation device using a quick connector;
[0319] (3) When starting the culture, ensure that there is sufficient excess liquid in all necessary feed bottles, and that the cell suspension and PBS are kept at 37 degrees Celsius, which is suitable for their growth activity. The needle should be placed in the cleaning tank and soaked in 75% alcohol at all times before use.
[0320] (4) Endothelial cell implantation. Before implantation, turn on the stirring device in the endothelial cell suspension vessel. This step is to make the cells evenly suspended in the liquid to avoid uneven distribution of cells squeezed out by the needle when implanting the cells. First, empty the alcohol in the cleaning tank and use 100-150mL of PBS in the liquid control feeding bottle 4 to use an air pump to directly infuse the cleaning pipeline into the needle. It should be noted that the pipeline needs to be cleaned and sterilized or replaced regularly. The cleaning here is to drain and clean the alcohol at the needle to avoid residual alcohol killing the implanted cells. Then use the solenoid valve to close the feeding bottle 4 and open the feeding bottle 1, and transfer the endothelial cells to the needle through the air pump until the liquid discharged from the needle changes from colorless to the rose red of the culture medium. At this time, maintain the air pump pressure at 0.5 to 1kPa slightly higher than the standard atmospheric pressure, so that the liquid in the catheter is maintained in a state that is not affected by external forces and will not be squeezed out. At this point, the preparation work is completed;
[0321] (5) By controlling the screw 1 and the lead screw 1, the needle is moved to a position 2-3 mm away from the leftmost end of the tubular stent. The needle is then inserted into the inner wall area of the stent to plant endothelial cells. The position of the inner wall is determined by the thickness of the tube wall and the thickness occupied by the required cells. For example, there is a blood vessel with an inner diameter of 6 mm and a thickness of 500 μm. As endothelial cells, they need to cling to a layer of inner wall. The inner wall is defined here as 450 μm away from the outermost side. The needle will be inserted into the tube wall to a depth of 450 μm through the distance sensor and the lead screw 2 and the piezoelectric material will extrude 1-5 μm of endothelial cells here. The needle is then lifted. The hydrophobic needle can ensure that the planted cell suspension droplet is left at the planting position. The needle moves 300-500 μm to the right and starts the same operation until the needle is 2 mm away from the rightmost end of the tubular stent. After this row of cells is planted, the tubular stent is rotated 2 degrees by the servo motor 1 and the next round of endothelial cell planting begins;
[0322] (6) When the inner wall of the entire stent has been planted with endothelial cells (the stent has been rotated one circle), the needle is moved to the cleaning tank for ultrapure water rinsing and cleaning. The electromagnetic pinch valve 1 is closed and the electromagnetic pinch valve 4 is opened to use the PBS in the feeding bottle 4 to clean the pipeline. The stirring of the endothelial cells in the feeding bottle 1 is stopped, and the stirring of the smooth muscle cells in the feeding bottle 2 is started. Close the electromagnetic pinch valve 4 and open the electromagnetic pinch valve 2. Use the air pump to flow the smooth muscle cell suspension to the needle until the color of the outflowing liquid changes from colorless to the rose red of the cell culture fluid. At this time, the air pump pressure is maintained at 0.5 to 1 kPa slightly higher than the standard atmospheric pressure, so that the liquid in the catheter is maintained in a state where it is not affected by external forces and will not be squeezed out;
[0323] (7) The needle moves to the area 5mm away from the suture of the left barrel through screw 1 and screw 1, and starts to drip 15-20μL of cell liquid downward from 1mm above the barrel using an air pump, then moves 1mm to the right and drips the cell liquid again until the needle is 2-3mm to the right of the barrel. The purpose of this step is to allow smooth muscle cells to penetrate the suture of the barrel and the stent, so that the vascular cells after the initial culture form a dense cell colony at the seam to ensure that the stent will not leak or break due to stent dissolution in the later stage of culture. Similarly, the barrel on the right side needs to complete the same operation. Smooth muscle cells are mainly distributed in the middle layer of the blood vessels to provide good mechanical properties. Therefore, the needle is inserted into the stent wall at 300μm under the guidance of screw 2 and screw 2, and the smooth muscle cell suspension is injected into the stent through the air pump. The interval between each injection is 500-1000μm. After the stent is rotated one circle, the next cell type is implanted;
[0324] (8) Following the same cell solution replacement steps, the needle injects the fibroblast suspension at a depth of 100 μm from the outermost side of the scaffold wall, injecting 10-15 μl of fibroblasts using the same method as above, until the entire scaffold surface is covered with fibroblasts. Cell implantation is now complete, and the needle is returned to the cleaning tank for cleaning and storage. Prepare for the next cell implantation.
[0325] (9) It is worth noting that two methods of discharging liquid for cell seeding are mentioned in this embodiment. When a small volume of liquid is required (μL level), a piezoelectric material is used to drive the liquid. When a larger volume of liquid (10-100μL) is required, the air pump is directly controlled to control the liquid.
[0326] (10) The implanted tissue will be removed from the female connector on the device and enter the next step of cultivation.
[0327] Example 30
[0328] Three-dimensional patterning of intestinal tissue cells
[0329] (1) This embodiment differs from the 3D cell seeding of blood vessels described in Example 10 in that the intestinal endothelial surface requires a preferred topological structure, such as villi and concavities, and the inner diameter of the intestine is larger than that of blood vessels (greater than 10 mm). Given these two characteristics, the method of first seeding cells in a planar manner and then forming a 3D structure is preferred.
[0330] (2) Specific differences from Example 10 are the different cell types used and the different distribution order. The specific distribution order is intestinal endothelial cells, fibroblasts, and smooth muscle cells. For example, a 12 cm long intestinal tract with an inner diameter of 10 mm and a wall thickness of 500 μm requires a 140 mm long planar scaffold with 32 mm of intestinal endothelial cells, 33 mm of fibroblasts, and the remainder of the scaffold being smooth muscle cells.
[0331] (3) Another specific difference is that the topological structure described above needs to be constructed using a gel-type material (such as hydrogel). The specific construction method is as follows: a PDMS mold with the same size as the area required for the hydrogel is placed on a flat support. Using the above example, the size is 32mmx100mm, 5mm high and 4mm thick. The cell implantation machine first injects the hydrogel into this mold. Then the conveyor belt transports the support with the mold and the hydrogel to the three-dimensional structure patterning area. This area has a PDMS stamp made by photolithography silicon wafer molding. Under the action of the lead screw and the lead screw, the stamp will descend and press out the villi and concave structures described above on the hydrogel, while the hydrogel is heated to complete the curing. After the curing is completed, the mechanical claws around the stamp will peel the PDMS mold from the support and discard it together with the stamp. The support is then transported back to the cell implantation area to complete the cell implantation similar to that in Example 11, and the tissue curling similar to that in Example 11. At this point, the artificial intestine completes the cell implantation and can enter the next culture stage.
[0332] (4) A major advantage of using this curling method is that fibroblasts can easily migrate to other cell layers and interfere with intestinal endothelial cells, thereby affecting the function of intestinal tissue. By curling the degradable scaffold, the scaffold itself can act as a physical barrier in the early stage of culture, thereby ensuring that the intestinal function after the culture is completed is not affected.
[0333] Example 31
[0334] Three-dimensional patterning of cell seeding for artificial muscle tissue
[0335] (1) In order to generate dense muscle cells to simulate the texture of meat, this embodiment performs three-dimensional planarization of the planar scaffold into rounded edges and then curls it, so that the gaps between the edges form a tubular cavity to achieve the exchange of substances inside and outside the cells during culture.
[0336] (2) The process of this specific embodiment is similar to that described in Example 11, which involves adding a mold to the membrane-type scaffold, perfusing the hydrogel, three-dimensionally patterning the hydrogel, and then seeding the cells. The difference is that after the cells are seeded, they will undergo tight three-dimensional curling. The difference from Example 11 is that there is only one inner cavity in the middle that is negligible compared to the tissue. At the same time, only one type of bovine skeletal muscle cell is used in this embodiment. For example, if a muscle tissue with a thickness of 1.5 cm and a length of 10 cm is to be formed, a planar scaffold with a length and width of 36 cm × 11 cm is required. A PDMS mold with an inner length of 35 cm, a width of 10 cm, a height of 5 mm, and a wall thickness of 5 mm is used on this planar scaffold. Subsequently, a different PDMS stamp is used. The specific difference is that, unlike the stamp that simulates the inner wall of the intestine, this stamp can form rounded ridge-like protrusions with a height of 500 μm and a spacing of 300 μm. After completing the cell seeding inside the hydrogel scaffold, the entire planar scaffold will be transported to the curling device and curled as described in Example 10 but with an inner diameter of 0.5 mm. The final tissue is shown in the figure. The tissue that has completed curling can enter the next step of culture.
[0337] (3) The advantage of using this curling method to construct three-dimensional muscle tissue is that capillary channels for material exchange can be formed around the muscle tissue, thereby improving the overall survival rate of dense muscle tissue during culture.
[0338] Example 32
[0339] Cell implantation and three-dimensional patterning of skin tissue
[0340] The specific method is similar to that of Example 1. As a planar tissue, the skin itself does not need to be curled. Its three-dimensional structure is specifically reflected in the different cells used in each layer of the structure. Therefore, compared to patterning cells in different areas of the skin scaffold, this example will drip different cells at different depths in the same area to achieve the purpose of three-dimensional patterning. For example, a skin with a length, width, and width of 10cm×10cm and a thickness of 500μm requires an 11cm×11cm membrane scaffold with a thickness of 200μm. The hydrogel is then perfused into the 10cm×10cm area using the hydrogel formation method described in Example 13. The difference is that only a 300μm thick hydrogel layer is formed, and no three-dimensional patterning is required. After the hydrogel layer is formed, different cells are seeded at different depths: fibroblasts at a depth of 250μm, dermal cells at a depth of 150μm, and epidermal cells at a depth of 100μm. Another difference is that compared to suturing elastic non-degradable materials at both ends of the scaffold, the skin tissue scaffold here is sewed with elastic non-degradable materials on all sides, and smooth muscle cells are used to reinforce the sutures. After the cell scaffold is planted, it will begin its next step of culture.
[0341] In the above embodiments, as long as the stent thickness ratio design is within the scope of protection of the present invention, the cavity between the layers can be eliminated well, so that the cavity rate of the artificial tissue material is less than 2% three months after implantation. However, the stent thickness ratio design that is not within the scope of protection of the present invention cannot eliminate the cavity between the layers well. Even if the initial cavity rate is lower than 5%, the cavity rate in the subsequent third stage will rise back to 8-15%. The inventors will not list them one by one here.
Claims
1. A method for preparing a three-dimensional artificial tubular tissue, characterized in that: The following steps are involved: (1) Preparing a rollable stent; (2) Planting cells on the scaffold; (3) curling the product obtained in step (2) into a three-dimensional tubular structure and culturing it in vitro to obtain the three-dimensional artificial tubular tissue; Wherein, the preparation method of the rollable stent includes any one of the following: Method 1: The rollable stent is divided into two different cell planting areas from the start end to the end end of the roll, and the widths of the two different cell planting areas are controlled along the roll direction of the stent so that each of the different cell planting areas can form at least one complete tubular layer after roll-up, and the tubular layer located at the outer layer after roll-up can wrap the tubular layer at the inner layer; and the thickness ratio of the stent in the two different cell planting areas is controlled from thin to thick to be 1:2 to 80; Method 2: The rollable scaffold is divided into three different cell planting areas from the start end to the end end of the roll, and the widths of the three different cell planting areas are controlled along the roll direction of the scaffold so that each of the different cell planting areas can form at least one complete tubular layer after roll-up, and the tubular layer located in the outer layer after roll-up can sequentially wrap the tubular layer located in the inner layer; and the thickness ratio of the scaffold in the three different cell planting areas is controlled from thin to thick to be 1:2 to 80:2 to 3000; Method three: The curlable scaffold is divided into four different cell planting areas from the curling start end to the curling end, and the widths of the four different cell planting areas are controlled along the curling direction of the scaffold so that each of the different cell planting areas can form at least one complete tubular layer after curling, and the tubular layer located in the outer layer after curling can wrap the tubular layer located in the inner layer in sequence; and the thickness ratio of the scaffold in the four different cell planting areas is controlled from thin to thick to be 1:2~80:2~700:2~3000.
2. The preparation method according to claim 1, characterized in that: The scaffold includes a dense scaffold and a loose scaffold, the porosity and pore size of the loose scaffold are greater than those of the dense scaffold; preferably, the thickness of the loose scaffold is 20-5000 μm, the porosity is more than 90%, the pore size is 20-1000 μm, and the fiber diameter is 0.05-30 μm; the thickness of the dense scaffold is 1-200 μm, the porosity is 59-90%, the pore size is 0.05-500 μm, and the fiber diameter is 0.05-30 μm; further preferably, the preparation process of the loose scaffold and the dense scaffold includes casting, micro injection molding, blowing, extrusion, calendaring, blown film extrusion, Any one or more of the non-woven processes of rotational molding, dip coating, 2D printing, hot stamping, melt blowing, water spinning, needle spinning, electrospinning, melt spinning, melt blowing spinning, thermal bonding, chemical bonding, spunlace or needle punching; More preferably, the materials used for the loose scaffold and the dense scaffold include at least one of PGA, PLA, PCL, PLC, PPDO, PHBV, HA, PU, PET, PP, PE, PA, PMMA, PTFE, PES, PEEK, PS, PP, PMMA, PC, PGA-TMC, PGA-CL, chitosan or collagen, or their copolymer materials.
3. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes nerve tissue, and the preparation method of the scaffold thereof includes: dividing the curlable scaffold into two different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the two different cell planting areas from thin to thick to be 1:20-50; preferably, the scaffold of the nerve tissue also includes a double-layer nerve bundle structure, the bundled nerves are wrapped by two layers of epithelial tissue, and the thickness ratio of the bundled nerves is controlled to be 1:12-24 from the curling start end to the curling end; further preferably, axially distributed prismatic bubbles are also provided in the area of the nerve scaffold located at the curling start end, the distribution density of the prismatic bubbles is 10-15 per millimeter, the length is 5-20 millimeters, each prismatic bubble is independent of each other, and is separated from each other by a dense layer of 1-8 microns.
4. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes medium-caliber arterial vascular tissue, and the preparation method of the stent includes: dividing the curlable stent into two different cell planting areas from the curling start end to the curling end, and controlling the stent thickness ratio of the two different cell planting areas from thin to thick to be 1:3-75; or dividing the curlable stent into three different cell planting areas from the curling start end to the curling end, and controlling the stent thickness ratio of the three different cell planting areas from thin to thick to be 1:3-58:3-60; Alternatively, preferably, the three-dimensional artificial tubular tissue comprises small-caliber arterial vascular tissue, and the preparation method of the stent comprises: In summary: the rollable scaffold is divided into three different cell planting areas from the start end to the end end of the roll, and the scaffold thickness ratio of the three different cell planting areas is controlled to be 1:2-25:3-48 from thin to thick; Alternatively, preferably, the three-dimensional artificial tubular tissue includes medium-caliber venous vascular tissue, and the preparation method of the stent thereof includes: dividing the curlable stent into three different cell planting areas from the curling start end to the curling end, and controlling the stent thickness ratio of the three different cell planting areas from thin to thick to be 1:2-38:3-70; Alternatively, preferably, the three-dimensional artificial tubular tissue includes small-caliber venous vascular tissue, and the preparation method of the stent includes: dividing the curlable stent into three different cell planting areas from the curling start end to the curling end, and controlling the stent thickness ratio of the three different cell planting areas from thin to thick to be 1:5~50:7~66.
5. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes female urethral tissue, and the preparation method of the scaffold includes: dividing the scaffold into three different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the three different cell planting areas from thin to thick to be 1:5-27:8-60; Alternatively, preferably, the three-dimensional artificial tubular tissue includes male urethral tissue, and the preparation method of the scaffold thereof includes: dividing the curlable scaffold into three different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the three different cell planting areas from thin to thick to be 1:4 to 28:10 to 66.
6. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes vas deferens tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into three different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the three different cell planting areas from thin to thick to be 1:4-700:16-1000; Alternatively, preferably, the three-dimensional artificial tubular tissue includes fallopian tube tissue, and the preparation method of the scaffold thereof includes: dividing the curlable scaffold into four different cell planting areas from the curling starting end to the curling ending end, and controlling the scaffold thickness ratio of the four different cell planting areas to be 1:2 to 150:3 to 300:20 to 1000 from thin to thick; further preferably, a villus structure is also provided in the cell planting area near the curling starting end of the fallopian tube tissue scaffold, and the villus structure is a protrusion with an axial height of 10-11 μm and a diameter of 0.2-0.3 μm.
7. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes intestinal tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into four different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the four different cell planting areas from thin to thick to be 1:2-4:2-30:3-35; Preferably, the intestinal tissue includes the small intestine, and a protrusion with an axial height of 4-7 mm and a width of 2-3 mm is further provided in the area of the small intestine stent located at the curling starting end; further preferably, the protrusion includes villi and crypts, wherein the radial length of the villi is 1200-1600 μm and the axial width is 300-600 μm; the diameter of the crypt neck is 2-10 μm, and the inner diameter of the cavity is 40-50 μm; Preferably, the intestinal tissue includes the large intestine, and crypts are provided in the stent region of the large intestine stent at the curling start end, the crypts have a distribution density of 100 per square millimeter in the inner layer, a radial depth of 1500-2200 μm, and a diameter of 400-500 μm.
8. The preparation method according to claim 1 or 2, characterized in that: The three-dimensional artificial tubular tissue includes esophageal tissue, and the preparation method of the scaffold thereof includes: dividing the scaffold into four different cell planting areas from the curling start end to the curling end, and controlling the scaffold thickness ratio of the four different cell planting areas from thin to thick to be 1:2-100:5-600:20-1000; Preferably, the three-dimensional artificial tubular tissue includes tracheal tissue, and the preparation method of the scaffold thereof includes: dividing the curlable scaffold into four different cell planting areas from the curling starting end to the curling ending end, and controlling the scaffold thickness ratio of the four different cell planting areas to be 1:4-9:15-38:25-56 from thin to thick; further preferably, the tracheal tissue scaffold further includes a part made of a polymer material or chondrocytes with a mechanical strength higher than 5-10 MPa in the third cell planting area from the curling starting end; further preferably, the area with high mechanical strength is annular and has at least one opening.
9. A three-dimensional artificial tubular tissue, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8; preferably, the three-dimensional artificial tubular tissue includes artificial nerves, artificial arteries, artificial veins, artificial small intestine, artificial large intestine, artificial esophagus, artificial trachea, artificial urethra, artificial fallopian tube and artificial vas deferens; further preferably, the artificial arteries include medium-caliber arteries and small-caliber arteries; further preferably, the artificial veins include medium-caliber veins and small-caliber veins; further preferably, the artificial urethra includes male urethra and female urethra.
10. The use of the three-dimensional artificial tubular tissue prepared by the method according to any one of claims 1 to 8 or the three-dimensional artificial tubular tissue according to claim 9, characterized in that: The three-dimensional artificial tubular tissue is used as a replacement for damaged tissue or as an implant in the body.
Citation Information
Patent Citations
System for seeding cells onto three-dimensional scaffolds
CN102884172B
A cell seeding platform and method in a stent based on 3D printing technology
CN106085847B
Three-dimensional roll-shaped structures with self-adjusting structural functions, their preparation methods and applications
CN108653815B
Three-dimensional coiled structure with function of automatically adjusting structure, as well as preparation method and applications of three-dimensional coiled structure
CN108653815A
Systems and methods for the generation of gastrointestinal tissue in anastomotic or physiological locations
JP2019503819A
Cited By
Self-assembly ventricle-like structure, system and method based on stress-induced curly membrane