Magnetic separation-electrical separation process for complex refractory iron ores
Through the magnetic separation-electric separation process and the magnetic-electricity-flotation combined process, the difference in magnetic and electrical properties of iron ore is used to solve the problem of poor flotation effect of complex and difficult-to-separate iron ore, and achieve high efficiency and environmental protection. Iron ore recovery and process simplification.
Patent Information
- Application Number
- PCT/CN2023/123768
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-10-10
- Publication Date
- 2024-10-24
AI Technical Summary
Existing technology is difficult to effectively process complex and difficult-to-separate iron ores, especially those with fine particle size and easy-to-sludge minerals, resulting in poor flotation results. In addition, traditional processes have problems such as high energy consumption, carbon emissions, and environmental pollution.
It adopts the magnetic separation-electric separation process of complex difficult-to-separate iron ore, and uses the 'staged dry grinding, magnetic separation-electric separation' fully dry separation process and the 'magnetic-electricity-flotation' combined separation process to make use of the ore's The differences in magnetic and electrical properties separate magnetite, hematite, siderite, limonite, chlorite and other minerals to achieve the recovery of high-grade iron concentrate.
It achieves efficient separation of complex and difficult-to-separate iron ore, avoids poor indexes in the flotation process, pollutes the environment and wet tailings discharge, shortens the process flow, saves environmental protection costs, and can process iron ore with high ferrous carbonate content. .
Smart Images

Figure CN2023123768_24102024_PF_FP_ABST
Abstract
Description
A complex and difficult-to-separate iron ore magnetic separation-electric separation process Technical Field
[0001] The present invention relates to the technical field of mineral processing, and in particular to a magnetic separation-electric separation process for complex and difficult-to-separate iron ore. Background Art
[0002] With the continuous exploitation of iron ore resources worldwide, ore quality has declined annually, showing a pattern of decreasing grade, increasing composition complexity, and finer particle size distribution. Currently, numerous complex and refractory iron ore belts exist worldwide, characterized by poor quality, fine quality, and complex composition. These include the Liaoning and Shanxi regions of China, the Appalachian Geosyncline Iron Belt of North America, the Lorraine-Germany Salkangit Belt, the Kachkanal Iron Belt of Russia, and the Carrara region of Australia. The iron ore in these producing areas is low-grade and complex, primarily composed of magnetite or hematite, but also containing various iron-bearing minerals such as siderite, limonite, and chlorite, as well as gangue such as quartz and calcite. These minerals often coexist, requiring grinding to a very fine particle size for complete separation.
[0003] Among the above-mentioned minerals, siderite (FeCO3), limonite and chlorite are all weakly magnetic minerals with low hardness and easy to be muddied (Mohs hardness <4.0). In the traditional wet "grinding-magnetic separation-flotation" process, they cannot be separated by strong magnetic separation and enter the flotation operation, resulting in a large amount of fine mud and calcium and magnesium ions in the ore pulp, reducing the selectivity of the reagent, seriously worsening the flotation process, and making it difficult for the flotation process to obtain better separation indicators.
[0004] Taking the iron ore produced in Anshan, China as an example, its FeCO3 content continues to rise, reaching over 10% in some mining areas. However, the current mineral processing plant's combined process of "stage grinding, coarse and fine grading, gravity separation-magnetic separation-anion reverse flotation" is difficult to handle such high-carbonate iron ore. The flotation index has seriously declined, and even the phenomenon of indistinguishable fines and tails has occurred. The mining site has to blend the iron ore from each mining area to reduce the ferrous carbonate content in the selected material to below 3%.
[0005] For example, the patent document with publication number CN106944248A discloses a "Method for Separating Mixed Iron Ore Containing High Carbonate." This method involves grinding the raw ore, performing weak magnetic separation and strong magnetic separation, to obtain weak magnetic separation iron concentrate and strong magnetic separation iron concentrate. The strong magnetic separation iron concentrate is then screened through a fine screen to obtain qualified undersize iron concentrate. The oversize product is then subjected to a pre-grading-regrinding-strong magnetic separation process to obtain a strong magnetic separation coarse concentrate. The strong magnetic separation coarse concentrate is then subjected to direct flotation to obtain a direct flotation iron concentrate. The patent document with publication number CN104014416B discloses a "Method for Separating Iron Ore Containing Carbonate." This method involves crushing the carbonate-containing iron ore, performing staged ball milling, and performing strong-weak magnetic separation to obtain a magnetic separation mixed concentrate. This is then classified to obtain coarse and fine products, and finally reverse flotation to obtain a coarse and fine concentrate, respectively. Both of the above methods combine flotation with magnetic separation or gravity separation to process mixed iron ore. However, these methods cannot achieve good flotation performance when the iron ore contains high levels of weakly magnetic minerals that easily form mud, such as siderite, limonite, and chlorite. Publication No. CN113680534A discloses a "Method for Asynchronous Coarse and Fine Flotation of Carbonate-Containing Iron Ores Using a Collector for Fine-Grained Iron Minerals." This method classifies the mixed magnetic concentrate obtained by high-intensity and low-intensity magnetic separation to produce coarse and fine products. The coarse fraction is then subjected to reverse flotation using different collectors, and the fine fraction is subjected to forward flotation to obtain separate flotation concentrates. This method can achieve better performance than conventional magnetic separation-flotation processes, but it involves complex steps and a longer process, requiring a greater amount and type of flotation reagents. Furthermore, the siderite content treated by this method is less than 6%, and no other complex components, such as chlorite and limonite, were observed in the examples. For example, the "A beneficiation method for high-carbonate refractory iron ore" disclosed in publication number CN113877851A, and the "A low-temperature hydrogen reduction magnetic roasting process for refractory iron ore" disclosed in publication number CN108950179A, both use the magnetic roasting method to convert weakly magnetic siderite into strongly magnetic hematite, and then perform magnetic separation and recovery to prevent it from entering the flotation operation and affecting the indicators. Although the above methods can effectively process iron ore with a high iron carbonate content, they have problems such as high energy consumption and carbon emissions. At the same time, they cannot process refractory iron ore containing other complex components such as chlorite.
[0006] Therefore, it is urgent to develop new separation process flows for complex and difficult-to-separate iron ore to achieve its green and efficient utilization.
[0007] Summary of the Invention
[0008] In order to solve the problems of complex and difficult-to-select iron ores with fine embedded particle size, containing easily muddy minerals, and poor flotation effect, the present invention provides a magnetic separation-electric separation process for complex and difficult-to-select iron ores. The process utilizes the magnetic difference of the ore to separately select magnetite through weak magnetic separation; and utilizes the differences in electrical properties such as dielectric constant, conductivity, and rectification of the ore to separate siderite, limonite, chlorite and other minerals that are easily muddy but have poor conductivity from hematite in weakly magnetic minerals, thereby obtaining high-grade iron concentrate.
[0009] To achieve the above objectives, the present invention adopts the following technical solutions:
[0010] A magnetic separation-electric separation process for complex and difficult-to-separate iron ore adopts a "staged dry grinding, magnetic separation-electric separation" fully dry separation process. Specifically, the complex mixed iron ore is crushed and roller-milled to obtain a magnetic separation feed product, the magnetic separation feed product is subjected to dry weak magnetic separation I, and the concentrate is subjected to grinding operation dry grinding a, wind classification operation, and multi-stage dry weak magnetic separation operation to obtain magnetite concentrate; the dry weak magnetic separation I tailings are fed into a coarse-grained dry strong magnetic operation dry strong magnetic operation I, and the obtained coarse-grained strong magnetic concentrate is further subjected to grinding operation dry grinding b, wind classification, and dry strong magnetic operation, and the concentrate enters a multi-stage electric separation operation to obtain hematite concentrate; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
[0011] The specific steps include:
[0012] 1) The complex mixed ore crushing product is fed into the high pressure roller grinding mill as the raw ore, and a closed circuit grinding system is formed with the screening operation to obtain the magnetic separation feed product.
[0013] 2) The magnetic separation feed product of step 1) is fed into the coarse-grained dry weak magnetic separation operation dry weak magnetic I, wherein the concentrate enters the next grinding operation dry grinding a; the tailings are fed into the coarse-grained dry strong magnetic operation dry strong magnetic I, the coarse-grained strong magnetic tailings are discarded, and the obtained coarse-grained strong magnetic concentrate enters the next grinding operation dry grinding b.
[0014] Dry weak magnetic I tailings contain iron-containing weak magnetic minerals, including hematite, siderite, limonite and chlorite.
[0015] 3) Dry grinding and pneumatic classification form a closed-circuit grinding system, producing a fine product with a particle size of -200 mesh, accounting for more than 60%, with the specific fineness depending on the degree of ore dissociation. This is followed by several stages of dry weak magnetic separation to produce a high-grade magnetite concentrate with a TFe ≥ 66.5%. The middlings from each stage of dry weak magnetic separation are returned to the previous stage, and the tailings are combined and discarded.
[0016] Dry grinding methods include dry ball milling, dry autogenous grinding, and dry stirred milling; the number of dry weak magnetic separation stages and magnetic field strength should be determined according to the actual ore properties and concentrate grade requirements. Generally, wind-powered dry magnetic separators are used, with 3 to 5 stages of process.
[0017] 4) Dry grinding (B) is combined with wind classification to form a closed-circuit grinding system, producing a fine product with a particle size of -200 mesh, accounting for more than 60%. The specific fineness depends on the degree of ore dissociation. This is followed by several stages of dry high-intensity magnetic separation, during which the concentrate enters the electrostatic separation process and the tailings are discarded.
[0018] Dry grinding methods include dry ball milling, dry autogenous grinding, and dry stirred milling; the number of dry high-intensity magnetic separation operation stages, magnetic field strength, etc. should be determined according to the actual ore properties and concentrate grade requirements. Generally, a dry vibrating high-gradient magnetic separator is used, with 1 to 3 stages of operation.
[0019] 5) The dry strong magnetic concentrate in step 4) is subjected to several stages of electrostatic separation to obtain a high-grade hematite concentrate with TFe ≥ 65%; the middlings from each stage of electrostatic separation and the tailings from the next stage of electrostatic separation are returned to the feed ore in sequence.
[0020] The total content of siderite, limonite and chlorite in the hematite concentrate is less than 1% by weight.
[0021] The number of electrostatic separation operation sections, voltage (electric field) intensity, etc. should be determined according to the actual ore properties and concentrate grade requirements. Generally, a high-voltage electrostatic separator is used, with 2 to 4 process sections.
[0022] 6) Combine the tailings from dry weak magnetic separation operations, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0023] A magnetic separation-electric separation process for complex and difficult-to-separate iron ore adopts a "magnetic-electric-flotation" combined separation process. Specifically, the complex mixed iron ore is crushed and roller-milled and then subjected to grinding and screening to obtain a graded overflow product. The overflow product is fed into a weak magnetic pre-separation operation, and the resulting concentrate is fed into a weak magnetic concentration operation to obtain a magnetite concentrate; the tailings of the weak magnetic pre-separation operation are fed into a strong magnetic separation operation, and the resulting strong magnetic concentration concentrate is dried and fed into an electric separation operation, and the electric separation operation concentrate is subjected to reverse flotation and scavenging operations to obtain a magnetic-hematite mixed concentrate; the tailings of the weak magnetic concentration operation and the concentrate of the electric separation operation are combined and fed into reverse flotation and scavenging operations; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
[0024] The specific steps include:
[0025] 1) The product from the crushing roller mill of the complex mixed iron ore is fed into the grinding and screening process as the raw ore, producing a fine-grained overflow product with a particle size of -200 mesh, accounting for more than 60%. The specific fineness depends on the degree of ore dissociation. Grinding and screening operations can include high-pressure roller grinding, ball milling, stirred milling, or a combination of multiple grinding methods.
[0026] 2) The overflow product is fed into the weak magnetic pre-selection process, the resulting concentrate enters the multi-stage weak magnetic concentration process, and the tailings enter the high-intensity magnetic separation process.
[0027] The weak magnetic pre-selection equipment is a wet drum magnetic separator, and the magnetic field strength should be determined according to the specific properties of the material and the concentrate grade requirements.
[0028] The weak magnetic concentration equipment selects one or more combinations of wet drum magnetic separators, elutriators, and magnetic vibration machines. The magnetic field strength during separation should be determined according to the specific properties of the material and the concentrate grade requirements; the number of sections for weak magnetic concentration operations can be determined according to the actual ore properties, and is generally set to 3 to 5 sections.
[0029] 3) The concentrated ore obtained from the high-intensity magnetic separation operation is dried and then fed into the electric separation operation, and the tailings are discarded.
[0030] For high-intensity magnetic separation, a high-gradient magnetic separator (such as the SLon series) should be selected. Parameters such as magnetic field strength should be determined according to the specific properties of the material and the concentrate grade requirements. The number of sections for high-intensity magnetic separation can be determined according to the actual ore properties, and is generally set to 1 to 2 sections.
[0031] For electrostatic separation, a high-voltage drum-type electrostatic separator is selected. Parameters such as voltage (electric field) intensity should be determined according to the specific properties of the material and the concentrate grade requirements. The number of electrostatic separation sections can be determined according to the actual ore properties, and is generally set to 1 to 3 sections.
[0032] 4) The concentrate from the electrostatic separation operation is fed to the reverse flotation operation. The tailings are discarded or subjected to magnetic roasting or other treatments, and the middlings are returned to the electrostatic separation operation for further separation. The total content of siderite, limonite, and chlorite in the electrostatic separation concentrate is less than 3% by weight.
[0033] 5) After multiple weak magnetic separation operations, the ore is demagnetized by a demagnetizer between each weak magnetic separation to obtain a magnetite concentrate with a grade of not less than 66%. The tailings of the multiple weak magnetic separation operations are combined and fed into the reverse flotation operation.
[0034] 6) The tailings of the multi-stage weak magnetic concentration operation are combined with the concentrate of the electrostatic separation operation, and then subjected to reverse flotation operation to obtain a mixed maghemitic concentrate, the iron grade of which is not less than 67.5%.
[0035] The tailings from the multi-stage weak magnetic separation operation and the concentrate from the electrostatic separation operation are combined and mixed before being concentrated to control the feed concentration of reverse flotation at 40% to 45%.
[0036] The recovery rate of reverse flotation operation shall not be less than 80%.
[0037] 7) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0038] The reagent system for reverse flotation, such as the type and dosage of collectors, depressants and activators, should be determined according to the specific properties of the material and the concentrate grade requirements; the number of reverse flotation operation sections can be determined according to the actual ore properties, generally one coarse, one fine and three sweeping.
[0039] In the iron phase composition of the complex mixed iron ore, FeCO3 is ≥3% by weight.
[0040] Compared with the existing technology, the beneficial effects of the present invention are:
[0041] 1) The present invention discloses a magnetic separation-electric separation process for complex and difficult-to-separate iron ore. The process first separates magnetite through weak magnetic separation by utilizing the magnetic difference of the ores. Then, the differences in the electrical properties of the ores, such as dielectric constant, conductivity, and rectification, are utilized to separate the hematite from the siderite, limonite, chlorite, and other minerals that are easily sludged but have poor conductivity, thereby ultimately obtaining a high-grade iron concentrate.
[0042] 2) The fully dry separation process of "staged dry grinding, magnetic separation-electrostatic separation" in the present invention is to separate the strongly magnetic magnetite in the mixed iron ore through weak magnetic separation; then, through several electrostatic separation operations, the siderite, limonite, chlorite and other minerals that are easy to mud but have poor conductivity in the weakly magnetic minerals are separated to recover high-grade iron concentrate. The entire process does not include a flotation process, which is a fully dry separation process. The overall problem of poor flotation operation indicators, the impact on the ball-forming performance of iron concentrate, and environmental pollution is eliminated. At the same time, the fully dry operation shortens the process flow, avoids the wet discharge of tailings, relieves the pressure on the tailings pond, and saves environmental protection costs.
[0043] 3) The "magnetic-electric-flotation" combined separation process of the present invention uses "magnetic-electric-flotation" combined separation to separate the strongly magnetic magnetite in the mixed iron ore through weak magnetic separation; then, through electrostatic separation, easily sludged but poorly conductive siderite, such as limonite, and chlorite, are pre-separated and discarded from the weakly magnetic minerals. Before the electrostatic separation, the ore is subjected to strong magnetic separation and drying. This combined separation process retains the traditional flotation process equipment and process, but reduces the content of easily sludged minerals in the iron ore fed to the flotation, thereby improving the flotation performance.
[0044] 4) Compared with the existing process, the method used in the present invention can process more mineral types in the ore, especially iron ore with a ferrous carbonate content greater than 10%, and can still be effectively processed, thereby realizing the efficient development and utilization of complex and difficult-to-select mixed iron ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] FIG1 is a flow chart of the "stage dry grinding, magnetic separation-electric separation" full dry separation process of the present invention (Example 1).
[0046] FIG2 is a flow chart of the “magnetic-electric-levitation” combined separation process of the present invention (Example 5). DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only for illustration and are not intended to limit the present invention.
[0048] Example 1:
[0049] As shown in FIG1 , the complex and difficult-to-separate iron ore selected in this embodiment is taken from Anshan, Liaoning, China, with a total iron grade of 24.06%, of which magnetite contains 20.66%, hematite contains 10.15%, siderite (FeCO 3 ) contains 4.15%, chlorite contains 3.12%, and the gangue is mainly quartz and a small amount of mica. The process of the present invention is used for separation, which specifically includes the following steps:
[0050] 1) The complex mixed ore is crushed into fine products of 0-12 mm as raw ore and fed into a high-pressure roller grinding machine. Together with the screening operation, a closed-circuit grinding system is formed to obtain an undersize product with a particle size of P80 = 2.55 mm;
[0051] 2) The undersize product is fed into the coarse dry weak magnetic separation process I, where the concentrate enters the dry grinding process A; together with the wind classifier, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0052] 3) The product from the wind classification in step 2) is fed into three stages of dry weak magnetic separation (dry weak magnetic separation II, III, and IV), and demagnetized in a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 66.9%;
[0053] 4) The dry weak magnetic I tailings are fed into the dry strong magnetic I, the coarse strong magnetic tailings are discarded, and the coarse strong magnetic concentrate is fed into the dry grinding B; together with the wind classification operation, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%, followed by a dry strong magnetic operation (dry strong magnetic II). The resulting concentrate is fed into the electrostatic separation operation, and the tailings are discarded;
[0054] 5) The concentrate of dry strong magnetic II is subjected to two-stage electrostatic separation operations to obtain a hematite concentrate with a grade of 67.5%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0055] 6) Combine the tailings of dry weak magnetic sections II, III, and IV, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0056] Example 2:
[0057] The complex and difficult-to-separate iron ore selected in this implementation case was taken from Anshan, Liaoning Province, with a total iron grade of 33.52%, of which magnetite contained 17.65%, hematite contained 25.11%, siderite (FeCO3) contained 6.55%, and chlorite contained 2.36%. The gangue was mainly quartz and a small amount of feldspar. The process of the present invention was used for separation, which specifically includes the following steps:
[0058] 1) The complex mixed ore is crushed into fine products of 0-12 mm as raw ore and fed into a high-pressure roller grinding machine. Together with the screening operation, a closed-circuit grinding system is formed to obtain an undersize product with a particle size of P80 = 2.55 mm;
[0059] 2) The undersize product is fed into the coarse dry weak magnetic separation process I, where the concentrate enters the dry grinding process A; together with the wind classifier, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh accounting for 85%;
[0060] 3) The product from the wind classification in step 2) is fed into four stages of dry weak magnetic separation (dry weak magnetic separation II, III, IV, and V), and demagnetized in a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.8%;
[0061] 4) The dry weak magnetic I tailings are fed into the dry strong magnetic I, the coarse strong magnetic tailings are discarded, and the coarse strong magnetic concentrate is fed into the dry grinding B; together with the wind classification operation, a closed-circuit grinding system is formed to obtain a fine-grained product with a particle size of -200 mesh, accounting for 85%. The product then enters two stages of dry strong magnetic operations (dry strong magnetic II and III), and the resulting concentrate enters the electrostatic separation operation, and the tailings are discarded;
[0062] 5) The dry strong magnetic III concentrate is subjected to three-stage electrostatic separation to obtain a hematite concentrate with a grade of 67.7%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0063] 6) Combine the tailings of dry weak magnetic sections II, III, IV, and V, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0064] Example 3:
[0065] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 34.48%, of which magnetite contained 35.78%, hematite contained 8.63%, siderite (FeCO3) contained 5.25%, and chlorite contained 3.74%. The gangue was mainly quartz, containing a small amount of dolomite and calcite. The process flow of the present invention was used for separation.
[0066] 1) The finely crushed product, which has been crushed to 0-12 mm, is fed into a high-pressure roller mill as the raw ore, and a closed-circuit grinding system is formed with a dry vibrating screen to obtain an undersize product with a particle size of P80 = 2.70 mm;
[0067] 2) The high pressure roller mill product is fed into the dry weak magnetic I, and the concentrate of the dry weak magnetic I is fed into the dry mill a, which forms a closed circuit grinding system with the wind classifier to obtain a fine particle product with a particle size of -200 mesh accounting for 85%;
[0068] 3) The product from the wind classification in step 2) is fed into five stages of dry weak magnetic separation (dry weak magnetic II, III, IV, V, and VI), and demagnetized in a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.7%;
[0069] 4) The tailings of dry weak magnetic I are fed into dry strong magnetic I, the coarse strong magnetic tailings are discarded, and the concentrate of dry strong magnetic I is fed into dry grinding B, which forms a closed-circuit grinding system with a wind classifier to obtain a fine-grained product with a particle size of -200 mesh, accounting for 85%; then it enters dry strong magnetic II, and the resulting concentrate enters the electric separation operation, and the tailings are discarded;
[0070] 5) The dry strong magnetic II concentrate is fed into a three-stage electrostatic separation operation to obtain a hematite concentrate with a grade of 66.5%; the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1%.
[0071] 6) The tailings of dry weak magnetic sections II, III, IV, V, and VI, dry strong magnetic tailings, and electrostatic separation tailings are combined into comprehensive tailings with a grade of 11.8%.
[0072] Example 4:
[0073] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 37.09%, of which magnetite contained 11.25%, hematite contained 36.88%, siderite (FeCO3) contained 6.50%, and chlorite contained 4.05%. The gangue was mainly quartz, containing a small amount of dolomite and calcite. The process flow of the present invention was used for separation.
[0074] 1) The finely crushed product, which has been crushed to 0-12 mm, is fed into a high-pressure roller mill as the raw ore, and a closed-circuit grinding system is formed with a dry vibrating screen to obtain an undersize product with a particle size of P80 = 2.75 mm;
[0075] 2) The high pressure roller mill product is fed into the dry weak magnetic I, and the concentrate of the dry weak magnetic I is fed into the dry mill a, which forms a closed circuit grinding system with the wind classifier to obtain a fine particle product with a particle size of -200 mesh accounting for 85%;
[0076] 3) The product from the wind classification in step 2) is fed into three stages of dry weak magnetic separation (dry weak magnetic separation II, III, and IV), and demagnetized in a demagnetizer between each stage of weak magnetic separation to obtain a magnetite concentrate with a grade of 67.5%;
[0077] 4) The tailings of dry weak magnetic I are fed into dry strong magnetic I, the coarse strong magnetic tailings are discarded, and the dry strong magnetic I concentrate is fed into dry grinding B, which forms a closed-circuit grinding system with a wind classifier to obtain a fine-grained product with a particle size of -200 mesh, accounting for 85%; then it enters the three-stage dry strong magnetic operation (dry strong magnetic II, III, IV), the resulting concentrate enters the electric separation operation, and the tailings are discarded;
[0078] 5) The dry high-strength magnetic concentrate is fed into a three-stage electrostatic separation process to obtain a hematite concentrate with a grade of 66.8%; the total content of siderite, limonite, and chlorite in the hematite concentrate is less than 1%.
[0079] 6) Combine the tailings of dry weak magnetic sections II, III, and IV, dry strong magnetic tailings, and electrostatic separation tailings into comprehensive tailings.
[0080] In Examples 1-4 of the present invention, the processes from grinding, classification to magnetic separation and electrostatic separation are all fully dry processes, which do not consume water and do not produce wet tailings. Compared with the prior art, the process of the present invention can remove siderite, limonite, chlorite and other weakly magnetic minerals that are easily muddied in difficult-to-select mixed iron ore through the electrostatic separation process, and obtain higher-grade iron concentrate under dry conditions, which is impossible with the prior art. In addition, the processes of Examples 1-4 do not involve flotation operations, which can save slurry heating energy consumption and greenhouse gas emissions, and at the same time do not produce chemical pollution, which can eliminate the influence of chemicals on the subsequent iron concentrate pelletizing process.
[0081] Example 5:
[0082] As shown in FIG2 , the complex and difficult-to-separate iron ore selected in this embodiment was taken from Anshan, Liaoning, China, with a total iron grade of 30.05%. Calculated by mass percentage, the ore contains 15.90% magnetite, 16.87% hematite, 13.95% siderite (FeCO 3 ), and 2.13% chlorite. The gangue is mainly quartz and a small amount of feldspar, and the process of the present invention is used for separation.
[0083] 1) The high pressure roller mill product with a particle size of ≤3 mm is fed into a ball mill and formed into a closed circuit grinding system with a cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0084] 2) The overflow product is fed into the weak magnetic pre-selection process, and the resulting concentrate is subjected to three stages of weak magnetic concentration. Between each stage of weak magnetic separation, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.45%.
[0085] 3) The tailings from the weak magnetic pre-selection operation are fed into a strong magnetic separation operation, and the tailings from the strong magnetic separation operation are discarded; the strong magnetic separation concentrate is dried and fed into an electrostatic separation operation, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain an electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0086] 4) The weak magnetic concentrate tailings and electrostatic concentrate are combined and fed into reverse flotation operation (one coarse, one fine and three sweeps) to obtain a mixed magma concentrate with an iron grade of 67.85% and a recovery rate of 82.55%.
[0087] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0088] Example 6:
[0089] The complex and difficult-to-select iron ore used in this implementation case was taken from Anshan, Liaoning, China, with a total iron grade of 25.69%. Calculated by mass percentage, it contains 21.55% magnetite, 9.90% hematite, 6.55% siderite (FeCO3), and 1.66% chlorite. The gangue minerals are mainly quartz, and the process flow of the present invention is used for separation.
[0090] 1) The high pressure roller mill product with a particle size of ≤3 mm is fed into a ball mill and formed into a closed circuit grinding system with a cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0091] 2) The overflow product is fed into a weak magnetic pre-selection process, and the resulting concentrate is subjected to three stages of weak magnetic concentration. Between each stage of weak magnetic separation, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.8%.
[0092] 3) The weak magnetic pre-selection tailings are fed to a high-intensity magnetic separation process, where the tailings are discarded. The high-intensity magnetic separation concentrate is dried and fed to an electrostatic separation process, where the tailings, primarily composed of siderite, limonite, chlorite, and gangue such as quartz, are discarded, yielding an electrostatic separation concentrate with a total siderite, limonite, and chlorite content of less than 3%. The middlings are then returned for reselection, and the electrostatic separation concentrate enters a reverse flotation process. 4) The weak magnetic separation tailings and electrostatic separation concentrate are combined and fed to a reverse flotation process (one coarse, one fine, and three sweeps), yielding a mixed magnetic and hematite concentrate with an iron grade of 67.66% and a recovery rate of 83.75%.
[0093] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0094] Example 7:
[0095] The complex and difficult-to-select iron ore used in this implementation case was taken from Yuanjia Village, Shanxi Province, China, with a total iron grade of 32.07%. Calculated by mass percentage, it contains 12.66% magnetite, 26.83% hematite, 8.55% siderite (FeCO3), and 5.33% chlorite. The gangue minerals are mainly quartz and a small amount of mica. The process of the present invention is used for separation.
[0096] 1) The high pressure roller mill product with a particle size of ≤3 mm is fed into a ball mill and formed into a closed circuit grinding system with a cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0097] 2) The overflow product is fed into the weak magnetic pre-selection process, and the resulting concentrate is subjected to four stages of weak magnetic concentration. Between each stage of weak magnetic separation, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 66.5%.
[0098] 3) The weak magnetic pre-selection tailings are fed into two-stage strong magnetic separation operations, and the strong magnetic separation tailings are discarded; the strong magnetic separation concentrate is dried and fed into two-stage electrostatic separation operations, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0099] 4) The weak magnetic concentrate tailings and electrostatic concentrate are combined and fed into reverse flotation operation (one coarse, one fine and three sweeps) to obtain a magnetic and red mixed concentrate with an iron grade of 67.88% and a recovery rate of 82.65%.
[0100] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0101] Example 8:
[0102] The ore samples used in this implementation case were mixed and prepared from multiple regions. After testing, the total iron grade was 37.63%, of which, calculated by mass percentage, magnetite contained 20.74%, hematite contained 21.93%, siderite (FeCO3) contained 15.05%, and chlorite contained 4.87%. The gangue minerals were mainly quartz, and the process flow of the present invention was used for separation.
[0103] 1) The high pressure roller mill product with a particle size of ≤3 mm is fed into a ball mill and formed into a closed circuit grinding system with a cyclone to obtain a product with an overflow particle size of 85% to 95% of -200 mesh.
[0104] 2) The overflow product is fed into the weak magnetic pre-selection process, and the resulting concentrate is subjected to four stages of weak magnetic concentration. Between each stage of weak magnetic separation, it is demagnetized by a demagnetizer to obtain a magnetite concentrate with a grade of 67.75%.
[0105] 3) The weak magnetic pre-selection tailings are fed into two-stage strong magnetic separation operations, and the strong magnetic separation tailings are discarded; the strong magnetic separation concentrate is dried and fed into three-stage electrostatic separation operations, and the tailings whose main components are siderite, limonite, chlorite and quartz and other gangue are discarded to obtain electrostatic separation concentrate with a total content of siderite, limonite and chlorite less than 3%; the middlings are returned for re-selection in turn, and the electrostatic separation concentrate enters the reverse flotation operation.
[0106] 4) The weak magnetic concentrate tailings and electrostatic concentrate are combined and fed into reverse flotation operation (one coarse, one fine and three sweeps) to obtain a magnetic and red mixed concentrate with an iron grade of 67.68% and a recovery rate of 82.75%.
[0107] 5) Combine the strong magnetic separation tailings, electrostatic separation tailings and reverse flotation sweeping tailings into comprehensive tailings.
[0108] In view of the fact that the existing "magnetic separation-anion reverse flotation" process is limited to purifying iron ore with a content of easily muddy minerals such as iron carbonate below 3%, but is difficult to process high-carbonate and high-chlorite iron ore, Examples 5-8 of the present invention combine the electrostatic separation process with magnetic separation and flotation, and add an electrostatic separation process after the strong magnetic separation operation. This effectively removes siderite, limonite, chlorite and other easily muddy weak magnetic minerals in the mixed iron ore before the mixed iron ore enters the flotation process, reduces their impact on the flotation process, improves the iron ore separation index, and realizes the efficient development and utilization of complex and difficult-to-separate mixed iron ore.
Claims
1. A complex and difficult iron ore magnetic separation-electric separation process, It is characterized in that The complex mixed iron ore is crushed and roller-milled to obtain a magnetic separation feed product, and the magnetic separation feed product is subjected to dry weak magnetic separation I. The concentrate is subjected to grinding operation dry grinding a, wind classification operation, and multi-stage dry weak magnetic separation operation to obtain magnetite concentrate; the dry weak magnetic separation I tailings are fed into dry strong magnetic operation dry strong magnetic I, and the obtained strong magnetic concentrate is further subjected to grinding operation dry grinding b, wind classification, dry strong magnetic operation, and the concentrate enters multi-stage electric separation operation to obtain hematite concentrate; the complex mixed iron ore contains magnetite, hematite, siderite, limonite, and chlorite.
2. A complex and difficult iron ore magnetic separation-electric separation process according to claim 1, It is characterized in that The specific steps include: 1) The complex mixed ore is crushed and fed into the roller mill, and a closed-circuit grinding system is formed with the screening operation to obtain the magnetic separation feed product; 2) The magnetic separation feed product of step 1) is fed into the dry weak magnetic separation operation dry weak magnetic I, wherein the concentrate enters the next grinding operation dry grinding a; the tailings are fed into the dry strong magnetic operation dry strong magnetic I, the dry strong magnetic I tailings are discarded, and the obtained strong magnetic concentrate enters the next grinding operation dry grinding b; 3) Dry grinding a and wind classification operations form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, followed by several stages of dry weak magnetic separation operations to obtain magnetite concentrate with TFe ≥ 66.5%; The intermediate ore from each stage of dry weak magnetic separation is returned to the previous stage in turn, and the tailings are merged and discarded; 4) Dry grinding b and wind classification operation form a closed-circuit grinding system to obtain fine-grained products with a particle size of -200 mesh accounting for more than 60%, followed by several stages of dry strong magnetic operation, in which the concentrate enters the electric separation operation and the tailings are discarded; 5) The dry strong magnetic concentrate of step 4) is subjected to several stages of electrostatic separation to obtain hematite concentrate with TFe≥65%; the middlings of each stage of electrostatic separation and the tailings of the next stage of electrostatic separation are returned to the feed ore in sequence.
3. The complex and difficult iron ore magnetic separation-electric separation process according to claim 2, It is characterized in that In the above step 2), the dry weak magnetic I tailings contain iron-containing weak magnetic minerals, including hematite, siderite, limonite and chlorite.
4. The complex and difficult iron ore magnetic separation-electric separation process according to claim 2, It is characterized in that In the above step 5), the total content of siderite, limonite and chlorite in the hematite concentrate is less than 1% by weight.
5. A complex and difficult iron ore magnetic separation-electric separation process, It is characterized in that The complex mixed iron ore is crushed and roller-milled, and then subjected to grinding and screening to obtain a graded overflow product, the overflow product is fed into a weak magnetic pre-selection operation, the obtained concentrate is fed into a weak magnetic concentration operation to obtain a magnetite concentrate; the tailings of the weak magnetic pre-selection operation are fed into a strong magnetic separation operation, the obtained strong magnetic separation concentrate is fed into an electrostatic separation operation after drying, the electrostatic separation concentrate is subjected to a reverse flotation operation to obtain a magnetic hematite mixed concentrate; the tailings of the weak magnetic concentration operation and the concentrate of the electrostatic separation operation are combined and fed into a reverse flotation operation; the complex mixed iron ore contains magnetite, hematite, siderite, limonite and chlorite.
6. A complex and difficult iron ore magnetic separation-electric separation process according to claim 5, It is characterized in that The specific steps include: 1) The product of the complex mixed iron ore after crushing and roller milling is fed into the grinding and screening operation as the raw ore to obtain the graded overflow product; 2) The overflow product is fed into the weak magnetic pre-selection process, the resulting concentrate enters the multi-stage weak magnetic concentration process, and the tailings enter the strong magnetic separation process; 3) The concentrated ore obtained from the high-intensity magnetic separation operation is dried and then fed to the electric separation operation, and the tailings are discarded; 4) The concentrate obtained from the electrostatic separation operation is fed into the reverse flotation operation, and the middlings are returned to the electrostatic separation operation for further separation; 5) After multiple weak magnetic concentration operations, a magnetite concentrate with a grade of not less than 66% is obtained, and the multiple weak magnetic concentration operations are combined with tailings to feed reverse flotation operations; 6) The tailings of the multi-stage weak magnetic concentration operation are combined with the concentrate of the electrostatic separation operation, and then subjected to reverse flotation operation to obtain a mixed maghemitic concentrate, the iron grade of which is not less than 67.5%.
7. A complex and difficult iron ore magnetic separation-electric separation process according to claim 6, It is characterized in that The above step 1) is to feed the particle product of the complex mixed iron ore after crushing and roller grinding into the grinding and screening operation as the raw ore to obtain the classified overflow product with a fineness of ≤0.075mm accounting for more than 60%.
8. A complex and difficult iron ore magnetic separation-electric separation process according to claim 6, It is characterized in that In the above step 4), the total content of siderite, limonite and chlorite in the electrolytic concentrate is less than 3% by weight.
9. A complex and difficult iron ore magnetic separation-electric separation process according to claim 6, It is characterized in that In the above step 6), the tailings from the multi-stage weak magnetic separation operation and the concentrate from the electrostatic separation operation are combined and mixed and then concentrated, so that the reverse flotation feed concentration is controlled at 40% to 45%. The recovery rate of the reverse flotation operation in step 6) is not less than 80%.
10. A complex and difficult iron ore magnetic separation-electric separation process according to any one of claims 1 to 9, It is characterized in that In the iron phase composition of the complex mixed iron ore, FeCO 3 ≥3%.
Citation Information
Patent Citations
Method for ore dressing preconcentration of vanadium-titanium magnetite
CN108855583A
Method for recovering iron and titanium from vanadium-titanium magnetite tailings
CN109332001A
Concentrating separating dressing technology of raw sand
CN109772575A
Process method for recovering ilmenite from beach placer
CN114505172A
Complex refractory iron ore stage dry grinding and magnetic separation-electric separation full-dry separation process
CN116474931A
Cited By
Hematite hydrogen-based ore phase conversion-magnetic separation-reverse flotation combined process
CN119793682A
Multistage magnetic separation closed cycle process for magnetite
CN121892288A