Secondary battery and electric device
By designing the negative active material layer and protective film on the negative electrode sheet of the secondary battery, and combining the hydrogen fluoride and fluorine-containing lithium salt in the organic electrolyte, the problem of poor fast charging performance of the secondary battery under high energy density is solved and achieved Balance of high energy density and long cycle life.
Patent Information
- Application Number
- PCT/CN2023/140127
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-12-20
- Publication Date
- 2024-10-24
AI Technical Summary
Under the premise of high energy density, secondary batteries have poor fast charging performance, resulting in shortened cycle life and extended charging time.
By designing the negative active material layer on the negative electrode sheet, combining the protective film and appropriate particle size distribution, and combining the hydrogen fluoride and fluorine-containing lithium salt in the organic electrolyte, the thickness and porosity of the negative active material layer are optimized to form a non-dissolvable Protective film to improve fast charging performance and cycle life.
It achieves improved fast charging performance and cycle life on the basis of high energy density, ensures excellent battery dynamic performance, and takes into account high-rate charge and discharge capabilities and long cycle life.
Smart Images

Figure CN2023140127_24102024_PF_FP_ABST
Abstract
Description
Secondary battery and electrical device
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 19, 2023, with application number 202310458235.4 and application name “A Secondary Battery and Electrical Device”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The embodiments of the present application relate to, but are not limited to, the field of battery technology, and specifically to a secondary battery and an electrical device. Background Art
[0003] Secondary batteries, especially lithium-ion batteries, have brought great convenience to people's daily lives. Lithium-ion batteries occupy a large market share in mobile terminal products and new energy vehicles with excellent electrochemical properties such as high energy density, high voltage and low self-discharge. Lithium-ion batteries mostly use graphite as the negative electrode. This is because graphite has a high theoretical capacity. However, when the lithium-ion negative electrode is charged at a high rate, metallic lithium is easily precipitated on the negative electrode surface, which causes the battery's reversible capacity to decrease and the cycle life to shorten. At the same time, it causes a large internal polarization voltage of the battery, reduces the fast charging capability, and prolongs the charging time. Technical issues
[0004] The present application provides a secondary battery and an electrical device to solve the problem of poor fast charging performance of the battery under the premise of high energy density. Technical Solutions
[0005] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0006] In a first aspect, the present application provides a secondary battery comprising a negative electrode sheet and a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on a surface of the positive electrode current collector, wherein the positive electrode active material layer comprises lithium nickel cobalt manganese oxide;
[0007] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector; the negative electrode active material layer includes a negative electrode active substance, and the surface of the negative electrode active material layer has a protective film. The negative electrode plate meets the following requirements:
[0008] 0.05≤Dv50 / A≤0.25, 300≤A / B≤5000, and 5≤Dv50≤25; wherein Dv50 is the particle size corresponding to when the cumulative volume percentage of the negative electrode active material reaches 50%, and the unit is μm, A is the thickness of the negative electrode active material layer, and the unit is μm, and B is the average thickness of the protective film, and the unit is μm.
[0009] Optionally, the negative electrode plate satisfies: 600≤A / B≤2000.
[0010] Optionally, the secondary battery includes an organic electrolyte, and the organic electrolyte includes an organic solvent, hydrogen fluoride and a fluorine-containing lithium salt;
[0011] The secondary battery satisfies: 0.75≤1000B / C≤3; wherein B is the thickness of the protective film, in μm, and C is the concentration of hydrogen fluoride in the organic electrolyte, in ppm.
[0012] Optionally, 90≤A≤180.
[0013] Optionally, 0.015≤B≤0.3.
[0014] Optionally, 5≤C≤500.
[0015] Optionally, the fluorine-containing lithium salt includes LiPF6, and at least one of LiPO2F2, LiFSI and LiTFSI.
[0016] Optionally, the porosity of the negative electrode active material layer is from 20% to 50%.
[0017] Optionally, the compaction density of the negative electrode active material layer is from 1.3 g / cm 3 to 1.7g / cm 3 .
[0018] Optionally, the negative electrode active material includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, soft carbon, carbon fiber and modified graphite.
[0019] Optionally, the lithium nickel cobalt manganese oxide includes Li a Ni x Co y Mn z M b O2; wherein, 0.9<a<1.1, 0.6≤x<1, 0<y<0.3, 0<z<0.4, 0≤b<0.15, M includes a combination of one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and y:z is 1:(1~3).
[0020] Optionally, the organic solvent includes any one or more of cyclic esters, linear esters, linear ethers and acetonitrile.
[0021] Optionally, the cyclic ester includes at least one of γ-butyrolactone and cyclic carbonate.
[0022] Optionally, the linear ester includes at least one of acetate and linear carbonate.
[0023] Optionally, the linear ether includes at least one of dimethoxyethane, dimethoxymethane, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl trifluoromethyl ether, bis(1,1,2,2-tetrafluoroethyl) ether, 2,2,3,3-tetrafluoropropyl trifluoromethyl ether, 2,2,2-trifluoroethyl ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, 1,1,2,2-tetrafluoroethyl ethyl ether and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether.
[0024] In a second aspect, the present application further provides an electrical device, comprising the secondary battery as described above, wherein the secondary battery serves as a power supply for the electrical device. Beneficial effects
[0025] Compared to the prior art, the secondary battery provided by the present application includes a negative electrode plate, which includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector; the negative electrode active material layer includes a negative electrode active material, and the surface of the negative electrode active material layer has a protective film. The negative electrode plate satisfies the following conditions: 0.05≤Dv50 / A≤0.25, 300≤A / B≤5000, and 5≤Dv50≤25; wherein Dv50 is the particle size corresponding to when the cumulative volume percentage of the negative electrode active material reaches 50%, in μm, A is the thickness of the negative electrode active material layer, in μm, and B is the average thickness of the protective film, in μm. The negative electrode active material in the negative electrode active material layer of the secondary battery of the present application has the ability to charge quickly, and has good compatibility with organic electrolytes, and can form a non-dissolving protective film on the surface of the negative electrode active material layer. The secondary battery of the present application can improve high-rate charge and discharge capabilities, while greatly improving cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is a transmission electron microscope image of a protective film formed by a negative electrode active material in a negative electrode active material layer of a negative electrode sheet according to Example 1 of the present application.
[0027] Implementation Methods of the Application
[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. The described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative efforts are within the scope of protection of this application.
[0029] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the components and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application.
[0030] In order to improve the problem that existing secondary batteries are difficult to achieve fast charging performance while obtaining high energy density, the present application provides a solution to develop a high-capacity and high-safety battery that has both energy density and fast charging performance. It has excellent dynamic performance and can simultaneously take into account the characteristics of long cycle life and high energy density, solving the problem of poor fast charging performance of batteries under the premise of high energy density.
[0031] The embodiments of the present application provide a secondary battery and an electrical device. These are described in detail below. It should be noted that the order in which the following embodiments are described does not limit the order of the embodiments.
[0032] The present invention provides a secondary battery comprising a negative electrode sheet and a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises lithium nickel cobalt manganese oxide;
[0033] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector; the negative electrode active material layer includes a negative electrode active substance, and the surface of the negative electrode active material layer has a protective film. The negative electrode plate satisfies: 0.05≤Dv50 / A≤0.25, 300≤A / B≤5000, and 5≤Dv50≤25; wherein Dv50 is the particle size corresponding to when the cumulative volume percentage of the negative electrode active substance reaches 50%, in μm; A is the thickness of the negative electrode active material layer, in μm; B is the thickness of the protective film, in μm.
[0034] In the embodiments of the present application, the thickness of the negative electrode active material layer refers to the sum of the thicknesses of the negative electrode active material layer coated on the current collector. If both surfaces of the current collector are coated with negative electrode active material layers, the thickness of the negative electrode active material layer is the sum of the thicknesses of the negative electrode active material layers on the two surfaces. In a battery system, the particle size of the negative electrode active material will have a direct impact on the accumulation of the particles, and the morphology of the particles, the accumulation conditions between the particles, etc. will directly affect the lithium ion deintercalation process, affect the ion migration rate, and thus affect the battery performance. In addition, the thickness of the negative electrode active material layer is also an important factor affecting the battery capacity and rate characteristics. In addition, during the first charge and discharge process of the battery, a passivation layer, i.e., a protective film, will be formed at the solid-liquid interface between the negative electrode active material layer and the electrolyte. This protective film can prevent the electrolyte from directly contacting the negative electrode active material, reduce the decomposition of the electrolyte, and also prevent lithium ions from being co-embedded with solvent molecules, avoid causing the expansion of the graphite negative electrode, and ensure the capacity of the battery. Based on the above factors, the present application controls the particle size distribution of the negative electrode active material and the thickness of the negative electrode active material layer, thereby affecting the formation of the protective film and the thickness of the protective film, so that the battery takes into account the influence of the particle size distribution of the negative electrode active material, the thickness of the negative electrode active material layer, and the thickness of the protective film on the battery performance, so that the secondary battery can achieve high energy density while taking into account the fast charging performance of the battery. When the above three conditions of the secondary battery are satisfied: 0.05≤Dv50 / A≤0.25, 300≤A / B≤5000, and 5≤Dv50≤25, the secondary battery can obtain excellent fast charging performance and high energy density, where Dv50 is the particle size corresponding to the cumulative volume percentage of the negative electrode active material reaching 50%, in μm; A is the thickness of the negative electrode active material layer, in μm; B is the thickness of the protective film, in μm.
[0035] In some embodiments, lithium nickel cobalt manganese oxide includes Li a Ni x Co y Mn z M b O2; wherein, 0.9<a<1.1, 0.6≤x<1, 0<y<0.3, 0<z<0.4, 0≤b<0.15, M includes a combination of one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and y:z is 1:(1-3). The secondary battery uses a high-nickel ternary positive electrode active material with a nickel content greater than or equal to 60%, and the ratio of cobalt and manganese in the material is limited to 1:(1-3), which can further improve the battery capacity. M is selected from a combination of one or more of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, which can improve the mechanical properties of lithium nickel cobalt manganese oxide, which is beneficial to improving the stability of the material and increasing the battery cycle performance.
[0036] In some embodiments, the value of Dv50 / A is any value selected from 0.05, 0.08, 0.10, 0.15, 0.20, 0.22, and 0.25, or a range consisting of any two values.
[0037] In some embodiments, the value of A / B is any value of 300, 400, 500, 600, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500 and 5000, or a range consisting of any two values. The value of A / B can be selected from 600 to 2000.
[0038] A battery's rate performance and energy density are related to the particle size of the negative electrode active material. A reasonable particle size allows for a more optimal diffusion path for active ions within the particles, facilitating high-rate charging. Furthermore, a reasonable particle size allows for a thinner active material layer while maintaining the same energy density, facilitating the diffusion of active ions, reducing polarization and lithium plating, and improving cycling performance. In some embodiments, when the particle size Dv50 of the negative electrode active material satisfies the following conditions: 5 ≤ Dv50 ≤ 25, both high-rate charging and cycling performance can be achieved.
[0039] In some embodiments, Dv50 ranges from 7 μm to 18 μm.
[0040] In some embodiments, the value of Dv50 (in μm) is any value among 5, 7, 8, 10, 15, 18, 20 and 25, or a range of any two values.
[0041] In some embodiments, the secondary battery includes an organic electrolyte comprising an organic solvent, hydrogen fluoride, and a fluorine-containing lithium salt;
[0042] The secondary battery satisfies: 0.75≤1000B / C≤3; wherein B is the thickness of the protective film, in μm, and C is the concentration of hydrogen fluoride in the organic electrolyte, in ppm.
[0043] The hydrogen fluoride (HF) in the non-aqueous organic electrolyte will form a protective film rich in inorganic salt components such as LiF during the first charging process. This film is more resistant to high temperature and high pressure and is not easily dissolved in organic solvents. It effectively improves the battery's initial discharge capacity, cycle life and high and low temperature performance, and solves the problem of stripping of the negative electrode active material during the battery charging process. 1000B / C can effectively balance the battery's charging rate and cycle life in the range of 0.75 to 3.
[0044] In some embodiments, the value of 1000B / C is any value among 0.75, 1, 2 and 3, or a range consisting of any two values.
[0045] In some embodiments, 90≤A≤180. The thickness of the negative electrode active layer of the present application is within this range, which can balance the high energy density and high rate charge and discharge performance of the battery.
[0046] In some embodiments, the value of A (in μm) is any value selected from 90, 100, 110, 120, 130, 140, 150, 160, 170, and 180, or a range consisting of any two values.
[0047] In some embodiments, 0.015≤B≤0.3, which minimizes the irreversible capacity consumed by the battery and achieves the purpose of improving the reversible capacity and energy density of the battery.
[0048] In some embodiments, the value of B (in μm) is any value selected from 0.015, 0.01, 0.02, 0.05, 0.1, 0.15, 0.20, 0.25, and 0.30, or a range consisting of any two values.
[0049] The hydrogen fluoride contained in the organic electrolyte of the secondary battery of the present application enables the secondary battery to form a protective film that is more resistant to high temperature and high pressure and not easily dissolved. The lithium ion embedding speed is fast and it is not easy to deposit on the surface of the particles. The hydrogen fluoride (HF) in the organic electrolyte will form a protective film rich in inorganic salt components such as LiF during the first charging process. This film is more resistant to high temperature and high pressure, and is not easily dissolved in organic solvents. It effectively improves the initial discharge capacity, cycle life and high and low temperature performance of the battery, and solves the problem of negative electrode materials such as graphite peeling during the charging process of the battery; if the content of hydrogen fluoride is too high, it will deteriorate the cycle performance and increase the internal resistance, and a small amount of hydrogen fluoride can promote the formation of a better interface protective film for the lithium ion path, further improving the charging speed. If the content is too low, this effect cannot be achieved. The hydrogen fluoride of the present application comes from the impurity hydrogen fluoride in the fluorine-containing lithium salt and the trace decomposition of the fluorine-containing lithium salt. In some embodiments, 5≤C≤500.
[0050] In some embodiments, the value of C (in ppm) is any value selected from 5, 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, and 500, or a range consisting of any two values.
[0051] In some embodiments of the present application, the fluorine-containing lithium salt includes LiPF6 (lithium hexafluorophosphate), and at least one of LiPO2F2 (lithium difluorophosphate), LiFSI (lithium bis(difluorosulfonyl)imide), and LiTFSI (lithium bis(trifluoromethanesulfonyl)imide). The electrolyte in the battery system has a significant impact on the formation of the negative electrode protective film. In the electrolyte of the same solvent, different types and concentrations of electrolyte salts have different reactivity with the solvent, resulting in differences in the composition and thickness of the formed protective film. Therefore, by adjusting the type or concentration of the electrolyte salt in the electrolyte, a protective film with better performance can be obtained, and the thickness of the protective film can also be adjusted.
[0052] In some embodiments, the fluorine-containing lithium salt accounts for 5 wt % to 25 wt % of the organic electrolyte.
[0053] In some embodiments, LiPF6 accounts for from 60% to 99% of the total weight of the fluorine-containing lithium salt.
[0054] In some embodiments, the mass percentage (wt %) of the fluorine-containing lithium salt in the organic electrolyte is any value selected from 5, 8, 10, 15, 18, 20, and 25, or a range consisting of any two values.
[0055] The microstructure of the battery electrode has an important influence on the performance of lithium-ion batteries. Studies have shown that the transport of lithium ions includes the transport process in the electrolyte in the electrode gap, which is related to the porosity, pore structure, and electrode / electrolyte wettability of the battery electrode. The liquid phase conduction of ions inside the pores of the negative porous electrode has a very important influence on the improvement of the battery's fast charging capability, and the liquid phase conduction of ions inside the pores of the negative porous electrode is closely related to the pore structure morphology of the negative electrode. Controlling the porosity of the negative active material layer can affect the internal pore structure of the negative active material layer, thereby affecting the liquid phase conduction of ions and the electronic contact between the negative active material particles. In some embodiments, the porosity of the negative electrode active material layer is 20%-50%. Within this range, the negative electrode sheet has a better ability to retain the electrolyte, and can also ensure good electrolyte wettability between the negative electrode active material particles, and the interfacial charge transfer impedance between the negative electrode active material and the electrolyte is also lower. Within this range, the protective film is more tightly attached to the negative electrode active material layer, and lithium ions are transmitted back and forth between the protective film and the negative electrode active material layer more smoothly, thereby improving the battery's fast charging capability and cycle life.
[0056] In some embodiments, the porosity (unit: %) of the negative electrode active material layer is any value selected from 20, 25, 30, 35, 40, 45, and 50, or a range consisting of any two values.
[0057] Low compaction density is beneficial to changing the porosity distribution of the electrode itself, improving the electrolyte's infiltration ability, and improving the battery filling efficiency and battery consistency. A higher compaction density helps reduce the material's contact internal resistance and helps the material's performance. However, as the electrolyte has difficulty in infiltrating into the interior of the electrode, it is impossible to ensure the movement path of ions, making it difficult to achieve smooth ion movement, which will cause a decrease in battery performance and life characteristics. In some embodiments, the compaction density of the negative electrode active material layer is 1.3-1.7 g / cm 3 Within this range, the negative porous electrode can maintain a reasonable pore structure while avoiding the negative electrode active material and the electrolyte from producing more side reactions that affect the improvement of battery performance.
[0058] In some embodiments, the compaction density of the negative electrode active material layer (unit: g / cm 3 ) is any value among 1.3, 1.4, 1.5, 1.6 and 1.7, or a range consisting of any two values.
[0059] In some embodiments, the negative electrode active material includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, soft carbon, carbon fiber, and modified graphite.
[0060] In some embodiments, the organic solvent includes one or more of cyclic esters, linear esters, linear ethers, and acetonitrile.
[0061] In some embodiments, the cyclic ester includes at least one of gamma-butyrolactone and a cyclic carbonate.
[0062] In some embodiments, the linear ester comprises at least one of an acetate or a linear carbonate.
[0063] In some embodiments, the linear ether includes at least one of dimethoxyethane, dimethoxymethane, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl trifluoromethyl ether, bis(1,1,2,2-tetrafluoroethyl) ether, 2,2,3,3-tetrafluoropropyl trifluoromethyl ether, 2,2,2-trifluoroethyl ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, 1,1,2,2-tetrafluoroethyl ethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether.
[0064] In some embodiments, the cyclic carbonate includes at least one of ethylene carbonate and propylene carbonate.
[0065] In some embodiments, the acetate includes at least one of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, and ethyl propionate.
[0066] In some embodiments, the linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0067] In some embodiments, the negative active material layer further includes a conductive agent and a binder.
[0068] In some embodiments, the mass percentage of the active material in the negative electrode active material layer is 93%-98%.
[0069] In some embodiments, the secondary battery further includes: a positive electrode plate and a separator.
[0070] In some embodiments, the positive electrode sheet includes a positive electrode current collector, a positive electrode active material coated on the positive electrode current collector, a binder, and a conductive agent. The type and content of the conductive agent and binder are not specifically limited and can be selected according to actual needs. In some embodiments, the conductive agent may include conductive carbon black, carbon nanotubes, graphene, etc., and the binder may include polyvinylidene fluoride.
[0071] In some embodiments, the preparation of the positive electrode sheet includes: dispersing the above-mentioned positive electrode active material, conductive agent, and binder in N-methylpyrrolidone (NMP) in a certain proportion, coating the resulting slurry on aluminum foil, drying, and then cold pressing and slitting to obtain the positive electrode sheet.
[0072] In some embodiments, the type of the diaphragm is not particularly limited and can be selected according to actual needs. The diaphragm can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride film, a spandex film, an aramid film, or a multi-layer composite film modified by a coating.
[0073] In some embodiments, the preparation of secondary batteries includes: assembling positive electrode sheets, negative electrode sheets, separators and other battery components, and obtaining secondary batteries through processes such as shaping, baking, packaging, liquid injection, formation, and capacity separation. Battery types include soft packs, cylinders, aluminum shells, etc.
[0074] This application provides an electrical device that includes the aforementioned secondary battery, which serves as a power source for the device. The device can be used for, but is not limited to, backup power supplies, motors, electric vehicles, electric motorcycles, power-assisted bicycles, bicycles, power tools, and large household batteries.
[0075] The present invention has been tested many times, and some of the test results are now cited as reference to further describe the invention in detail, and the following is a detailed description of the invention in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0076] Example 1
[0077] A secondary battery is provided, the preparation steps of which include:
[0078] (1) Preparation of positive electrode sheet:
[0079] The positive electrode active material NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive agent carbon black, and binder PVDF are mixed in a mass ratio of 96:2:2, solvent NMP is added, and the mixture is stirred under the action of a vacuum mixer to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then rolled and cut into pieces to obtain a positive electrode sheet.
[0080] (2) Preparation of negative electrode sheet:
[0081] The negative electrode active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber and the additive sodium carboxymethyl cellulose are mixed in a mass ratio of 96.5:1.5:1.5:0.5, deionized water is added as a solvent, and the mixture is stirred under the action of a vacuum mixer to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried at room temperature, and then transferred to an oven for further drying, and then rolled and cut to obtain a negative electrode sheet. The Dv50 of the negative electrode active material is 10 μm, and the double-sided thickness of the negative electrode active material layer is 100 μm.
[0082] (3) Preparation of electrolyte:
[0083] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then a fluorine-containing lithium salt (LiPF6 and LiFSI in a mass ratio of 2:1, i.e., the mass proportion of LiPF6 in the fluorine-containing lithium salt is 66%) is dissolved in a mixed organic solvent and mixed evenly to prepare an electrolyte, wherein the fluorine-containing lithium salt accounts for 15% of the total mass of the electrolyte;
[0084] (4) Preparation of lithium-ion batteries:
[0085] The positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, using Celgard 2300 separator. They are then wound into a battery cell and placed in a soft-pack shell. After top and side sealing, liquid injection, formation, and sorting, a lithium-ion battery is obtained. The parameters of the lithium-ion battery are detailed in Table 1.
[0086] Examples 2 to 4: The preparation method is the same as that of Example 1, except that the type of positive electrode material and the Dv50 of the negative electrode active material are adjusted; the HF content and the thickness of the protective film are adjusted by adjusting the mass concentration of the fluorine-containing lithium salt; and the porosity and compaction density of the negative electrode active material layer are adjusted by adjusting the rolling pressure of the negative electrode sheet. The specific parameters of Examples 2 to 4 are detailed in Table 1.
[0087] Examples 5-6: The type of positive electrode material and the Dv50 of the negative electrode active material were adjusted, and the mass concentration of the fluorine-containing lithium salt was adjusted to adjust the HF content and the thickness of the protective film. The specific parameters of Examples 5-6 are detailed in Table 1.
[0088] Examples 7-8: The preparation method is the same as that of Example 1, except that the thickness of the negative electrode active material layer is adjusted by adjusting the coating amount of the negative electrode active material layer and controlling the rolling pressure of the negative electrode sheet. The specific parameters of Examples 7-8 are detailed in Table 1.
[0089] Examples 9-10: The preparation method is the same as that of Example 1, except that the compaction density is adjusted by adjusting the rolling pressure of the negative electrode sheet. The specific parameters of Examples 9-10 are detailed in Table 1.
[0090] Examples 11-12: The preparation method is the same as that of Example 1, except that the thickness of the negative electrode active material layer is adjusted by adjusting the coating amount of the negative electrode active material layer and controlling the rolling pressure of the negative electrode sheet. The specific parameters of Examples 11-12 are detailed in Table 1.
[0091] Examples 13-14: The preparation method is the same as that of Example 1, except that the porosity of the negative electrode active material layer is adjusted by adjusting the rolling pressure of the negative electrode sheet. The specific parameters of Examples 13-14 are detailed in Table 1.
[0092] Examples 15-16: The compaction density of the negative electrode active material layer was adjusted by adjusting the rolling pressure of the negative electrode sheet. The specific parameters of Examples 15-16 are shown in Table 1.
[0093] Example 17: A lithium-ion battery is provided, and the preparation method is the same as that of Example 1, except that during the preparation of the electrolyte, the fluorine-containing lithium salt is adjusted to LiPF6 and LiPO2F2, and the mass ratio of LiPF6 and LiPO2F2 in the fluorine-containing lithium salt is 99:1 (that is, the mass ratio of LiPF6 in the fluorine-containing lithium salt is 99%).
[0094] Example 18: A lithium-ion battery is provided, and the preparation method is the same as that of Example 1, except that during the preparation of the electrolyte, the fluorine-containing lithium salt is adjusted to LiPF6 and LiTFSI, and the mass ratio of LiPF6 and LiTFSI in the fluorine-containing lithium salt is 85:15 (that is, the mass ratio of LiPF6 in the fluorine-containing lithium salt is 85%).
[0095] Example 19: A lithium-ion battery is provided, and the preparation method is the same as that of Example 1, except that in the electrolyte preparation process, the fluorine-containing lithium salt is only LiPF6.
[0096] Comparative Examples 1-2: The preparation method is the same as Example 1, except that the Dv50 of the negative electrode active material, the mass concentration of the fluorine-containing lithium salt, and the HF content and the thickness of the protective film are adjusted. The specific parameters of Comparative Examples 1 and 2 are detailed in Table 1.
[0097] Test Example 1
[0098] In this test example, the secondary batteries in Examples 1 to 19 and Comparative Examples 1 to 2 of the present application were subjected to performance tests. The battery performance parameters were measured according to the following methods. The results are shown in Table 2:
[0099] (1) Rate performance test:
[0100] The lithium-ion battery is left at rest for 30 minutes at 25°C, discharged at a constant current of 1C, then charged at a constant current and constant voltage of 1C, left at rest for 5 minutes, and discharged at a constant current of 1C. At this time, the discharge capacity is the actual capacity C0 of the battery at 1C. The battery is charged at a constant current and constant voltage of 1C, left at rest for 5 minutes, and discharged at a constant current of 2C. The discharge capacity C1 is the 2C discharge capacity. 2C rate capacity retention rate = (2C discharge capacity / 1C discharge capacity) × 100% = C1 / C0 × 100%.
[0101] (2) Dynamic performance test:
[0102] The lithium-ion battery is left at 25°C for 30 minutes. It is then fully charged at xC and fully discharged at 1C, repeated 10 times. The battery is then fully charged at xC. The negative electrode is then disassembled and the surface of the negative electrode observed for lithium deposition. If no lithium is deposited on the negative electrode surface, the charge rate xC is increased by 0.1C and the test is repeated until lithium deposition occurs on the negative electrode surface. The test is then stopped. The maximum charge rate of the battery is calculated by subtracting 0.1C from the charge rate xC at this point.
[0103] (3) Cyclic performance test:
[0104] The lithium-ion battery was placed at 25°C for 30 minutes, discharged at 1C constant current, allowed to stand for 10 minutes, charged at 1C constant current and constant voltage, allowed to stand for 10 minutes, and subjected to a full charge and discharge cycle test. The capacity retention rate after 1000 cycles was recorded.
[0105] (4) Battery capacity test:
[0106] After the lithium-ion battery has been allowed to stand at 25°C for 30 minutes, the following steps are performed: ① 0.33C constant current discharge, ② standing for 30 minutes, ③ 0.33C constant current and constant voltage charging with a cut-off current of 0.05C, ④ standing for 30 minutes, ⑤ 0.33C constant current discharge, ② to ⑤ are repeated three times, and the average of the three tests is the battery capacity.
[0107] Table 1
[0108] Table 2
[0109] As can be seen from Table 1, the embodiments of the present application achieve the following technical effects: it can improve the rate charging capability, and has excellent charge and discharge performance such as fast charging speed, long battery cycle life, and high battery safety.
[0110] By comparing Comparative Examples 1 to 2 with Examples 1 to 19, it can be found that in Comparative Examples 1 to 2, when the average thickness of the protective film formed by the active material particles in the negative electrode active material layer and the hydrogen fluoride content in the electrolyte fail to meet the range of this application, the battery cycle or lithium plating ability deteriorates, and it is impossible to simultaneously take into account long cycle life, high energy density and fast charging capability.
[0111] The above is a detailed introduction to a secondary battery and electrical equipment provided by the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, based on the ideas of the present application, there may be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A secondary battery, It is characterized in that It comprises a negative electrode sheet and a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active substance, and the positive electrode active substance comprises lithium nickel cobalt manganese oxide; The negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector; the negative electrode active material layer comprises a negative electrode active substance, and the surface of the negative electrode active material layer has a protective film, and the negative electrode plate satisfies: 0.05≤Dv50 / A≤0.25, 300≤A / B≤5000, and 5≤Dv50≤25; Wherein, Dv50 is the particle size corresponding to when the cumulative volume percentage of the negative electrode active material reaches 50%, in μm; A is the thickness of the negative electrode active material layer, in μm; B is the thickness of the protective film, in μm.
2. The secondary battery according to claim 1, It is characterized in that The negative electrode plate satisfies: 600≤A / B≤2000.
3. The secondary battery according to claim 1, It is characterized in that The organic electrolyte comprises an organic solvent, hydrogen fluoride and a fluorine-containing lithium salt; The secondary battery satisfies: 0.75≤1000B / C≤3; wherein B is the thickness of the protective film, in μm, and C is the concentration of hydrogen fluoride in the organic electrolyte, in ppm.
4. The secondary battery according to claim 3, It is characterized in that 90≤A≤180。 5. The secondary battery according to claim 3, It is characterized in that 0.015≤B≤0.3。 6. The secondary battery according to claim 3, It is characterized in that 5≤C≤500。 7. The secondary battery according to claim 3, It is characterized in that The fluorine-containing lithium salt includes LiPF 6 、LiPO 2 F 2 , LiFSI and LiTFSI.
8. The secondary battery according to claim 1, It is characterized in that The porosity of the negative electrode active material layer is from 20% to 50%.
9. The secondary battery according to claim 1, It is characterized in that The compaction density of the negative electrode active material layer is from 1.3 g / cm 3 To 1.7g / cm 3 .
10. The secondary battery according to claim 1, It is characterized in that The negative electrode active material includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, hard carbon, soft carbon, carbon fiber and modified graphite.
11. The secondary battery according to any one of claims 1 to 10, It is characterized in that The lithium nickel cobalt manganese oxide includes Li a Ni x Co y Mn z M b O 2 ; Among them, 0.9<a<1.1, 0.6≤x<1, 0<y<0.3, 0<z<0.4, 0≤b<0.15, M includes one or more combinations of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and y:z is 1:(1~3).
12. The secondary battery according to claim 3, It is characterized in that The organic solvent includes any one or more of cyclic esters, linear esters, linear ethers and acetonitrile.
13. The secondary battery according to claim 3, It is characterized in that The mass percentage of the fluorine-containing lithium salt in the organic electrolyte is from 5wt% to 25wt%.
14. The secondary battery according to claim 1, It is characterized in that The Dv50 ranges from 7 μm to 18 μm.
15. An electrical device, It is characterized in that It comprises the secondary battery as claimed in any one of claims 1 to 14, wherein the secondary battery is used as a power supply for the electrical device.
Citation Information
Patent Citations
Secondary battery and electric equipment
CN116314610A
Electrolyte and electrochemical device using same
CN111261939A
Lithium ion battery
CN113644317A
Secondary battery and electric device
CN115832201A
Lithium ion secondary battery
US20210242498A1
Cited By
Method for nondestructive analysis of overall wettability of battery
CN119556161A
Rechargeable battery and electric apparatus
WO2026118580A1