Secondary battery and electronic device

By controlling the thickness ratio of the active material layer and the insulating layer and using inorganic particles, the problem of penetration and mixing at the junction of the active material layer and the insulating layer in the battery is solved, and the dimensional accuracy and safety of the battery are improved.

WO2024217032A1PCT designated stage expired Publication Date: 2024-10-24XIAMEN AMPACE TECH LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/140135
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-12-20
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

In existing batteries, the active material layer and the insulating layer may infiltrate and mix with each other during the drying process, resulting in blurred boundaries, affecting the size of the pole pieces, and thus causing the risk of low battery capacity.

Method used

By controlling the thickness ratio of the active material layer and the insulating layer to 0.5 to 0.7, ensure that the thickness of the active material layer is 200 to 400 μm, and use inorganic particles and active materials during the coating process to reduce the size impact of the interaction zone.

Benefits of technology

It effectively reduces the size of the interaction area, reduces the impact on the size of the pole piece, improves the storage thickness expansion rate and safety of the battery, and avoids burrs and broken belt problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023140135_24102024_PF_FP_ABST
    Figure CN2023140135_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A secondary battery and an electronic device. The secondary battery comprises a positive electrode sheet. The positive electrode sheet comprises a current collector, a tab protruding from the current collector, and at least one surface insulating layer provided on the current collector. The insulating layer is arranged along the side edge of the current collector close to the tab, and is adjacent to an active material layer. The ratio of the thickness of the insulating layer to the thickness of the active material layer is 0.5-0.7, and the thickness of the active material layer is 200-400 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary batteries and electronic devices Technical Field

[0001] The present application relates to the field of energy storage devices, and in particular to a secondary battery and an electronic device including the secondary battery. Background Art

[0002] The edges of battery pole pieces are typically protected by an insulating layer to prevent burrs. The active material layer and insulating layer are typically applied simultaneously to the current collector surface of the pole piece. However, during the drying process, the active material layer and insulating layer may interpenetrate and blend at the boundary, blurring the boundary between the active material layer and insulating layer after drying. This can lead to inaccurate judgment of the active material layer's position, affect the pole piece's dimensions, and potentially lead to the risk of low battery capacity.

[0003] Summary of the Invention

[0004] One object of the present application is to provide a secondary battery and an electronic device, which can improve the problem that the size of the electrode is affected by the interaction area at the junction of the active material layer and the insulating layer.

[0005] In a first aspect, the present application provides a secondary battery comprising a positive electrode sheet. The positive electrode sheet comprises a current collector, a tab protruding from the current collector, and at least one surface insulating layer disposed on the current collector. The insulating layer is disposed along the side of the current collector proximal to the tab and adjacent to the active material layer. The ratio of the thickness of the insulating layer to the thickness of the active material layer is 0.5 to 0.7, and the thickness of the active material layer is 200 to 400 μm.

[0006] In the secondary battery provided in the present application, the thickness of the active material layer is controlled to be 200 to 400 μm, and the ratio of the thickness of the insulating layer to the thickness of the active material layer is controlled to be 0.5 to 0.7. This can reduce the size of the interaction zone located at the junction of the active material layer and the insulating layer formed by the infiltration and mixing of the active slurry and the insulating slurry during the coating process, and improve the influence of the interaction zone on the size of the electrode.

[0007] According to some embodiments of the present application, the ratio of the thickness of the insulating layer to the thickness of the active material layer is 0.6 to 0.7, which is more conducive to reducing the size of the interaction area.

[0008] According to some embodiments of the present application, the thickness of the active material layer is further controlled to be between 200 and 370 μm, further reducing the size of the interaction region. Furthermore, the thickness of the active material layer is controlled to be between 200 and 280 μm, further reducing the size of the interaction region.

[0009] According to some embodiments of the present application, the coating weight of the active material layer is 427-740 mg / 1540.25 mm 2 , which helps to reduce the size of the interaction area.

[0010] According to some embodiments of the present application, the coating weight of the active material layer is 427-640 mg / 1540.25 mm 2 .

[0011] According to some embodiments of the present application, the compaction density of the active material layer is 2.6 to 3 g / cc, which is beneficial for reducing the size of the interaction zone.

[0012] According to some embodiments of the present application, the insulating layer includes inorganic particles, and the inorganic particles include one or more of aluminum oxide, boehmite, zirconium oxide, boron oxide, or hexagonal boron nitride.

[0013] According to some embodiments of the present application, the active material layer includes an active material, and the active material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium iron phosphate, or lithium manganese iron phosphate.

[0014] According to some embodiments of the present application, the active material is composed of lithium manganese oxide and lithium iron phosphate, and the mass ratio of lithium manganese oxide to lithium iron phosphate is 3.5 to 12, so that the width of the interaction zone of the secondary battery is appropriate and the thickness expansion rate of the secondary battery after storage is appropriate.

[0015] According to some embodiments of the present application, the active material is composed of lithium manganese oxide and lithium iron phosphate, and the mass ratio of lithium manganese oxide to lithium iron phosphate is 4 to 10, which can further reduce the thickness expansion rate of the secondary battery after storage.

[0016] A second aspect of the present application provides an electronic device comprising a secondary battery according to any one of the above embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0018] FIG1 is a partial plan view of a positive electrode plate provided in one embodiment of the present application.

[0019] FIG2 is a schematic cross-sectional view of the positive electrode sheet shown in FIG1 along line II-II.

[0020] Main Component Symbols Description Positive electrode sheet 10 Current collector 11 Tab 12 Active material layer 13 Insulating layer 14 First surface 11a Second surface 11b DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present application are described clearly and in detail below. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present application. The terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.

[0022] Below, embodiments of the present application will be described in detail. However, the present application may be embodied in many different forms and should not be construed as limited to the exemplary embodiments illustrated herein. Rather, these exemplary embodiments are provided to make the present application thorough and detailed for those skilled in the art.

[0023] In addition, for the sake of brevity and clarity, the size or thickness of various components, layers may be exaggerated in the accompanying drawings. Throughout the text, the same numerical value refers to the same element. As used herein, the terms "and / or" and "and / or" include any and all combinations of one or more related enumerated items. In addition, it should be understood that when element A is referred to as "connecting" element B, element A may be directly connected to element B, or there may be an intermediate element C and element A and element B may be indirectly connected to each other.

[0024] Further, when describing embodiments of the present application, the use of “may” refers to “one or more embodiments of the present application.”

[0025] The technical terms used herein are for the purpose of describing specific embodiments and are not intended to limit this application. As used herein, the singular is intended to include the plural, unless the context clearly indicates otherwise. It should be further understood that the term "comprising", when used in this specification, refers to the presence of the described features, values, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, values, steps, operations, elements, components and / or combinations thereof.

[0026] Spatial related terms, such as "on" etc., can be used herein for convenient description, to describe the relationship between an element or feature and another element (multiple elements) or feature (multiple features) as illustrated in the figure. It should be understood that, in addition to the directions described in the figure, spatial related terms are intended to include different directions of equipment or devices in use or operation. For example, if the equipment in the figure is turned over, the elements described as "above" or "on" other elements or features will be oriented "below" or "below" other elements or features. Therefore, the exemplary term "on" can include the direction above and below. It should be understood that although the terms first, second, third, etc. can be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are used to distinguish an element, component, region, layer or part from another element, component, region, layer or part. Therefore, the first element, component, region, layer or part discussed below can be referred to as the second element, component, region, layer or part, without departing from the teachings of the exemplary embodiments.

[0027] In the prior art, as demand for high-energy-density batteries increases, it is often necessary to coat the electrode with a heavy active material layer to increase battery capacity. This heavy coating weight results in a thicker active material layer. The applicant discovered that when coating a thicker active material layer, the boundary between the active material layer and the insulating layer becomes blurred, causing the two layers to interpenetrate and blend at the boundary, forming an interaction zone that affects the size of the electrode.

[0028] Based on the above problems discovered by the applicant, the applicant has improved the thickness of the active material layer and the insulating layer of the electrode to reduce the size of the interaction zone, thereby reducing the impact of the interaction zone on the size of the electrode. The following is a further description of the embodiments of the present application.

[0029] An embodiment of the present application provides a secondary battery, including a housing and a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte accommodated in the housing, wherein a separator is provided between the positive electrode sheet and the negative electrode sheet.

[0030] Referring to Figures 1 and 2 , the positive electrode sheet 10 includes a current collector 11, a tab 12, an active material layer 13, and an insulating layer 14. The current collector 11 includes a first surface 11a and a second surface 11b disposed opposite each other. The tab 12 protrudes from the side of the current collector 11 and is connected to the first surface 11a and the second surface 11b. The active material layer 13 is disposed on the first surface 11a and separated from the tab 12. In other embodiments, the active material layer 13 may be disposed on both the first surface 11a and the second surface 11b to increase energy density. The insulating layer 14 is disposed on the first surface 11a along the side of the current collector 11 near the tab 12 and is adjacent to the active material layer 13. In a direction perpendicular to the first surface 11a (the thickness direction of the positive electrode sheet 10), the thickness of the active material layer 13 is 200 to 400 μm, and the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is 0.5 to 0.7.

[0031] The current collector 11 may be any positive electrode current collector known in the art, such as copper foil, copper alloy foil, or composite current collector, etc. The tab 12 and the current collector 11 are integrally formed, for example, by cutting a copper foil to form the current collector 11 and the tab 12 .

[0032] Insulating layer 14 includes inorganic particles and a binder. The inorganic particles include one or more of aluminum oxide, boehmite, zirconium oxide, boron oxide, or hexagonal boron nitride. The binder includes one or more of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, or sodium carboxymethyl cellulose.

[0033] The active material layer 13 includes an active material, a conductive agent, and a binder. The active material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium iron phosphate, or lithium manganese iron phosphate. The conductive agent can use any conductive agent known in the art, for example, the conductive agent includes one or more of doxeljen black, Super-P, acetylene black, graphene, carbon nanotubes, carbon fibers, etc. The binder can use any binder known in the art, for example, the binder includes one or more of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, and sodium carboxymethyl cellulose.

[0034] The active material layer 13 and the insulating layer 14 are prepared by a simultaneous coating process. In some embodiments, the preparation method of a secondary battery includes the following steps: dissolving the active material, conductive agent, and binder in a solvent to form an active slurry with a solid content greater than or equal to 65%, wherein the active material accounts for greater than or equal to 95.5%; dissolving inorganic particles and a binder in a solvent to form an insulating slurry with a solid content of 30-50%, wherein the inorganic particles account for greater than or equal to 80%; simultaneously coating the active slurry and the insulating slurry on the surface of the current collector 11; drying the active slurry coating and the insulating slurry coating to form the active material layer 13 and the insulating layer 14 to prepare the positive electrode sheet 10; and stacking or winding the positive electrode sheet 10, the separator, and the negative electrode sheet to produce a secondary battery. The solvent may include, but is not limited to, one or more of N-methylpyrrolidone, anhydrous ethanol, and acetone.

[0035] In the present application, the thickness of the active material layer 13 is controlled to be 200 to 400 μm, and the ratio of the thickness of the insulating layer 14 to the thickness of the active material layer 13 is controlled to be 0.5 to 0.7. This can reduce the size of the interaction zone at the junction of the active material layer 13 and the insulating layer 14 formed by the infiltration and mixing of the active slurry and the insulating slurry during the coating process, and improve the influence of the interaction zone on the size of the electrode.

[0036] When the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is less than 0.5, the difference in thickness between the insulating layer 14 and the active material layer 13 is too large. During the drying process, due to the fluidity of the active slurry and the surface tension of the active slurry, the active slurry and the insulating slurry easily mix at the boundary to form an interaction zone. The size of the interaction zone is too large, affecting the size of the positive electrode sheet 10. In addition, when the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is less than 0.5, the thickness H of the insulating layer 14 may be too small. When the height of the burrs formed by cutting is greater than the thickness H of the insulating layer 14, the burrs may pierce the insulating layer 14, easily causing a short circuit within the positive and negative electrodes, leading to safety issues.

[0037] When the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is greater than 0.7, the thickness H of the insulating layer 14 is close to the thickness T of the active material layer 13, so that the insulating layer 14 may be compressed during the cold pressing process of the secondary battery 100. Since the inorganic particles are incompressible, the part of the current collector 11 corresponding to the insulating layer 14 may be damaged by the pressure, thereby causing the problem of cold pressing fracture. In addition, when the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is greater than 0.7, due to the large difference in solid content between the insulating slurry and the active slurry, by increasing the coating weight (up to 740mg / 1540.25mm 2) When the thickness of the insulating layer 14 is increased, the insulating layer is not completely dried during the coating process and will adhere to the rubber roller, causing scratches and broken tape on the electrode.

[0038] In some embodiments, the ratio of the thickness H of the insulating layer 14 to the thickness T of the active material layer 13 is 0.6-0.7, which is more conducive to reducing the size of the interaction region.

[0039] In some embodiments, the thickness of the active material layer is further controlled to be 200-370 μm, which is more conducive to reducing the size of the interaction area.

[0040] In some embodiments, the thickness of the active material layer 13 is adjusted by controlling the coating weight of the active material layer 13 and the compaction density of the active material layer 13. In some embodiments, the coating weight of the active material layer 13 is 427-740 mg / 1540.25 mm 2 The compacted density of the active material layer 13 is 2.6 to 3 g / cc. In this way, the active material layer 13 can be controlled to have a suitable thickness, which is conducive to reducing the size of the interaction zone. Preferably, the coating weight of the active material layer 13 is 427 to 640 mg / 1540.25 mm 2 In some embodiments, the thickness of the insulating layer 14 is adjusted by controlling the solid content of the insulating paste and the coating weight of the insulating layer 14 .

[0041] In some embodiments, the active material of the active material layer 13 is composed of lithium manganese oxide and lithium iron phosphate, and the mass ratio of lithium manganese oxide to lithium iron phosphate is 3.5 to 12. When the content of lithium manganese oxide is higher, more gas is generated in the secondary battery. By controlling the mass ratio of lithium manganese oxide and lithium iron phosphate to 3.5 to 12, the width of the interaction zone and the thickness expansion rate of the secondary battery after storage can be made more appropriate. In some embodiments, the active material is composed of lithium manganese oxide and lithium iron phosphate, and the mass ratio of lithium manganese oxide to lithium iron phosphate is 4 to 10, which can further reduce the thickness expansion rate of the secondary battery after storage. In some embodiments, the active material of the active material layer 13 is composed of lithium manganese oxide and lithium iron phosphate, and the mass ratio of lithium manganese oxide to lithium iron phosphate is preferably 3.5 to 9, and more preferably 3.5 to 7.65.

[0042] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material disposed on the surface of the negative electrode current collector. The negative electrode current collector may use any negative electrode current collector known in the art, such as copper foil, copper alloy foil or composite current collector. The negative electrode active material may use any negative electrode active material known in the art, for example, it may include at least one of graphite, hard carbon, soft carbon, silicon, silicon carbon or silicon oxide. The negative electrode active material may also include a conductive agent and a binder. The conductive agent may include at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fiber or graphene, and the binder may include at least one of styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) or sodium carboxymethyl cellulose (CMC-Na).

[0043] The separator can be any separator known in the art. For example, the separator can be a film made of one or more materials selected from polyethylene, polypropylene, non-woven fabric, and polyfiber.

[0044] The electrolyte can be any electrolyte known in the art. For example, the electrolyte can be selected from an electronically insulating and ionically conductive solution containing one or more organic carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, or ethyl methyl carbonate as a solvent, and one or more lithium salts selected from the group consisting of TiPF6, TiBF4, TiBOB, TiAsF6, Ti(CF3SO2)2N, TiCF3SO3, and TiCTO4 as a solute.

[0045] The housing may be any housing known in the art. For example, the housing may be a packaging bag encapsulated with an encapsulating film, such as an aluminum-plastic film or a steel-plastic film; or the housing may be a metal housing, such as a steel shell or an aluminum shell.

[0046] One embodiment of the present application further provides an electronic device comprising the secondary battery of the present application. The electronic device can be any electrical device that uses an electrochemical device, for example, a mobile phone, a portable device, a laptop computer, a battery-powered vehicle, an electric vehicle, a ship, a spacecraft, an electric toy, or an electric tool.

[0047] Some specific embodiments and comparative examples are listed below to better illustrate the present application.

[0048] Example 1

[0049] 9.64% lithium iron phosphate, 86.76% lithium manganese oxide (the mass ratio of lithium manganese oxide to lithium iron phosphate is 9), 0.6% conductive carbon slurry, 1.2% conductive carbon black and 1.8% polyvinylidene fluoride are dispersed in nitrogen methyl pyrrolidone to obtain an active slurry with a solid content of 67%. 88% boehmite and 12% polyvinylidene fluoride are dispersed in nitrogen methyl pyrrolidone to obtain an insulating slurry with a solid content of 35%. The active slurry and the insulating slurry are coated on aluminum foil to form an active coating and an insulating coating. The active coating and the insulating coating are adjacent, and the thickness of the active coating is equal to the thickness of the insulating coating. The active coating and the insulating coating are dried to obtain an active material layer and an insulating layer. Then, after cold pressing, die cutting and striping, the positive electrode sheet shown in Figure 1 is obtained. Among them, the coating weight of the active material layer is 427mg / 1540.25mm 2 The compaction density of the active material layer is 3 g / cc, the thickness T of the active material layer is 200 μm, the thickness H of the insulating layer is 130 μm, and H / T is 0.65.

[0050] Graphite, polyvinylidene fluoride and conductive carbon black are mixed and coated on copper foil, and then cold pressed, die-cut and striped to obtain the negative electrode sheet.

[0051] The positive electrode sheet, polyethylene separator, and negative electrode sheet are stacked in sequence with the separator placed between the positive and negative electrode sheets, and then wound to obtain an electrode assembly; the electrode assembly is placed in an aluminum-plastic film, and after liquid injection and formation, a lithium-ion battery is obtained.

[0052] Example 2-11

[0053] The same as Example 1 except for at least one of the coating weight of the active material layer, the thickness T of the active material layer, the compaction density of the active material layer, the thickness H of the insulating layer, and H / T, wherein T is 200-400 μm and H / T is 0.5-0.7.

[0054] Examples 12-17

[0055] Except for the content of lithium manganate, the content of lithium iron phosphate, and the thickness H of the insulating layer, the rest of Example 3 is the same.

[0056] Example 18

[0057] Except for the lithium iron phosphate, the coating weight of the active material layer, and the compaction density of the active material layer, the rest of the embodiment is the same as that of Example 3.

[0058] Comparative Examples 1-5

[0059] Comparative Examples 1-5 are the same as Example 1 except for the coating weight of the active material layer, the thickness T of the active material layer, the compaction density of the active material layer, and the thickness H of the insulating layer.

[0060] Observe and measure the sizes of the interaction zones in Examples 1-18 and Comparative Examples 1-5:

[0061] Take the positive electrode sheet, cut the positive electrode sheet horizontally with a slitting knife, and analyze the cross section using a high-power microscope (SEM). You can see a white insulating layer, a black active material layer, and a gray interactive area between the white insulating layer and the black active material layer in the width direction of the positive electrode sheet.

[0062] Use the "point-line mode" to measure the distance from the highest point of the white insulating layer to the current collector. Repeat the above steps three times, and the average value is the insulating layer thickness H. Measure the distance from the surface of the white active material layer to the current collector at three points along the width of the electrode, 25 to 35 mm laterally from the edge of the black active material layer. The average value is the active material layer thickness T.

[0063] Along the width direction of the electrode, the intersection point of the white insulating layer and the gray interaction area is used as the starting point, and the intersection point of the black active material layer and the gray interaction area is used as the end point. The distance between the two parallel lines is measured using the "parallel line mode", which is the width of the interaction area. The above steps are repeated three times and the average value is the measured width of the interaction area.

[0064] Observe the frequency of positive electrode breakage during the cold pressing process.

[0065] When the width of the interaction zone is less than or equal to 0.5 mm, and the belt break frequency is greater than or equal to 20,000 m / time, it is judged to be within the acceptable range of the product and process, and the effect is "OK"; otherwise, the effect is judged to be "NG".

[0066] The high temperature storage performance of the lithium ion batteries of Examples 1-18 and Comparative Examples 1-5 was tested:

[0067] Place the lithium-ion battery in a 25°C constant temperature box and let it stand for 5 minutes to allow the lithium-ion battery to reach a constant temperature. Charge it to 4.2V at a constant current of 0.5C, charge it at a constant voltage to a current of 0.05C, let it stand for 30 minutes, then discharge it to 2.8V at a constant current of 0.2C and let it stand for 5 minutes. Use a micrometer to test and record the thickness of the lithium-ion battery as the initial thickness. Transfer the test lithium-ion battery to a 60°C constant temperature box for storage for 60 days, then take it out and place it in a 25°C constant temperature box. Let it stand for 5 minutes to allow the lithium-ion battery to reach a constant temperature. Test the thickness of the lithium-ion battery as the thickness after storage.

[0068] Thickness expansion ratio = (thickness after storage - initial thickness) / initial thickness × 100%.

[0069] The data and measurement results of Examples 1-18 and Comparative Examples 1-5 are shown in Table 1.

[0070] Table 1

[0071] Comparison of Examples 1-12 and Comparative Examples 1-5 shows that when the thickness T of the active material layer is 200-400 μm and the ratio H / T of the thickness H of the insulating layer to the thickness T of the active material layer is 0.5-0.7, the width of the interaction zone is 0.13-0.4 mm, and the tape break frequency is 20,000-26,000 m / time, indicating acceptable results. When H / T is 0.6-0.7, the width of the interaction zone is 0.13-0.23 mm, which is even smaller.

[0072] It can be seen from Examples 3, 12-17 that when the thickness of the active material layer and the thickness of the insulating layer are within an appropriate range, the mass ratio of lithium manganese oxide and lithium iron phosphate has a greater impact on the high-temperature storage performance; when the mass ratio of lithium manganese oxide and lithium iron phosphate is smaller, the thickness expansion rate after storage is smaller; when the mass ratio of lithium manganese oxide and lithium iron phosphate is larger, the thickness expansion rate after storage is larger; in addition, it can be seen from Example 18 that when the positive electrode active material is only lithium iron phosphate, the width of the interaction zone will become larger. When the positive electrode active material only contains lithium iron phosphate, the active layer dries relatively quickly and the insulating layer dries slowly. Under the action of capillary stress, the insulating layer flows toward the active layer; and the surface tension of the lithium iron phosphate slurry is high. During the drying process, the edge of the positive electrode active material layer shrinks, causing the insulating layer slurry to further flow toward the positive electrode active material layer and penetrate into the positive electrode active material layer, thus forming a wider interaction zone.

[0073] The above disclosure is only a preferred embodiment of the present application and certainly cannot be used to limit the present application. Therefore, equivalent changes made based on the present application are still within the scope covered by the present application.

Claims

1. A secondary battery, comprising a positive electrode sheet, wherein: The positive electrode sheet comprises: current collector; A tab protruding from the current collector; An active material layer, disposed on at least one surface of the current collector; An insulating layer is arranged along the side of the current collector close to the electrode ear and adjacent to the active material layer, wherein the ratio of the thickness of the insulating layer to the thickness of the active material layer is 0.5-0.7, and the thickness of the active material layer is 200-400 μm.

2. The secondary battery according to claim 1, wherein The ratio of the thickness of the insulating layer to the thickness of the active material layer is 0.6 to 0.

7.

3. The secondary battery according to claim 1, wherein The thickness of the active material layer is 200 to 370 μm.

4. The secondary battery according to claim 1, wherein The thickness of the active material layer is 200 to 280 μm.

5. The secondary battery according to claim 1, wherein The coating weight of the active material layer is 427-740 mg / 1540.25 mm 2 .

6. The secondary battery according to claim 5, wherein: The coating weight of the active material layer is 427-640 mg / 1540.25 mm 2 .

7. The secondary battery according to claim 1, wherein The compaction density of the active material layer is 2.6 to 3 g / cc.

8. The secondary battery according to claim 1, wherein The insulating layer includes inorganic particles, and the inorganic particles include one or more of aluminum oxide, boehmite, zirconium oxide, boron oxide, or hexagonal boron nitride.

9. The secondary battery according to claim 1, wherein The active material layer includes an active material, and the active material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium iron phosphate, or lithium manganese iron phosphate.

10. The secondary battery according to claim 9, wherein The active material consists of the lithium manganese oxide and the lithium iron phosphate, and the mass ratio of the lithium manganese oxide to the lithium iron phosphate is 3.5-12.

11. The secondary battery according to claim 9, wherein The active material consists of the lithium manganese oxide and the lithium iron phosphate, and the mass ratio of the lithium manganese oxide to the lithium iron phosphate is 3.5-9.

12. The secondary battery according to claim 9, wherein The active material consists of the lithium manganese oxide and the lithium iron phosphate, and the mass ratio of the lithium manganese oxide to the lithium iron phosphate is 3.5 to 7.

65.

13. The secondary battery according to claim 9, wherein The active material consists of the lithium manganese oxide and the lithium iron phosphate, and the mass ratio of the lithium manganese oxide to the lithium iron phosphate is 4-10.

14. An electronic device, wherein: The invention comprises the secondary battery according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Power battery with anode made of hybrid material of lithium manganate and lithium iron phosphate

    CN101794902A

  • Electrode plate and manufacturing method thereof, battery using electrode plate and manufacturing method thereof, and die head

    CN111129506A

  • Battery and electric equipment

    CN115764179A

  • Columnar battery and electric device comprising same

    CN115911256A

  • Secondary battery and electronic device

    CN116230855A