Basic glass, microcrystalline glass and preparation method therefor, glass product and terminal device

Through the heat treatment crystallization and chemical ion strengthening treatment of the basic glass of the yttrium aluminum silicon system, the problems of high cost and insufficient performance of lithium aluminum silicon glass-ceramics are solved, and high-strength, high-transparency and low-cost glass-ceramics are prepared, which are suitable for on mobile terminal devices.

WO2024217113A1PCT designated stage expired Publication Date: 2024-10-24HUAWEI TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/074757
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-01-30
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing lithium aluminum silicon-ceramic glass has high lithium oxide content, high cost, low elastic modulus, easy breakage and low surface hardness, and is not resistant to scratches and impacts from sharp objects.

Method used

Using the basic glass of the yttrium aluminum silicon system, through heat treatment crystallization and chemical ion strengthening treatment, a crystallized glass with high mechanical properties and optical properties is prepared. The specific composition includes yttrium trioxide, alumina, zirconium oxide, lithium oxide, Sodium oxide and phosphorus pentoxide form glass-ceramics with specific crystal forms and sizes by adjusting the component ratio and heat treatment process.

Benefits of technology

The realization of high strength, high transparency and low-cost crystallized glass is suitable for mobile terminal equipment, improving the scratch resistance and impact resistance of the glass, while reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024074757_24102024_PF_FP_ABST
    Figure CN2024074757_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the embodiments of the present application is basic glass. The basic glass comprises the following components in percentages by mol: Y2O3: 4-15%; Al2O3: 3-30%; SiO2: 40-75%; ZrO2: 0.5-4%; Li2O: 3-12%; Na2O: 1.5-9%; P2O5: 0.1-2%; and ZnO: 1-8%. The basic glass can be subjected to heat treatment devitrification and / or a chemical ion strengthening treatment. Further provided in the embodiments of the present application are microcrystalline glass and a preparation method therefor, a glass product and a terminal device. The basic glass of an yttrium-aluminum-silicon system provided in the present application can be subjected to heat treatment microcrystallization to obtain microcrystalline glass, and the microcrystalline glass can be further subjected to a chemical strengthening treatment, such that the obtained microcrystalline glass has relatively high mechanical performance and optical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Basic glass, glass-ceramics, preparation methods thereof, glass products and terminal equipment

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to a Chinese patent application filed with the Patent Office of China on April 19, 2023, with application number 202310446898.4 and application name “Basic glass, microcrystalline glass and its preparation method, glass products and terminal equipment”, all contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of glass technology, and in particular to a basic glass, a microcrystalline glass and a preparation method thereof, a glass product and a terminal device using the glass product. Background Art

[0004] With the development of communication and electronic technologies, lightweight, thin, large-size, and high-performance mobile terminals have become the mainstream development trend. Therefore, the use of transparent micro-ceramic glass with more outstanding performance has become a necessity for the development of the mobile terminal industry.

[0005] Currently, research on lithium-aluminum-silicon glass-ceramics is relatively mature. While these glass-ceramics exhibit excellent optical properties, they are relatively expensive due to their high lithium oxide content. Furthermore, these glass-ceramics have a low elastic modulus and surface hardness. This low elastic modulus makes the glass susceptible to breakage during drop tests (i.e., after being subjected to a certain mechanical impact). This low surface hardness makes it less scratch-resistant and more susceptible to scratches. Furthermore, the glass is prone to cracking when impacted by sharp objects.

[0006] Summary of the Invention

[0007] In view of this, in order to solve at least one of the above defects, an embodiment of the present application provides a base glass of yttrium aluminum silicon system, which can be subjected to heat treatment crystallization and / or chemical ion strengthening treatment, and the microcrystalline glass made from this base glass has both high mechanical properties and optical properties.

[0008] In addition, the embodiments of the present application also provide microcrystalline glass made from the basic glass, a method for preparing the microcrystalline glass, a glass product, and a terminal device using the glass product.

[0009] In a first aspect, an embodiment of the present application provides a base glass, which comprises the following components, calculated by mole percentage: yttrium oxide (Y2O3): 4% to 15%;

[0010] Aluminum oxide (Al2O3): 3% to 30%;

[0011] Silicon dioxide (SiO2): 40% to 75%;

[0012] Zirconium dioxide (ZrO2): 0.5% to 4%;

[0013] Lithium oxide (Li2O): 3% to 12%;

[0014] Sodium oxide (Na2O): 1.5% to 9%;

[0015] Phosphorus pentoxide (P2O5): 0.1% to 2%;

[0016] Zinc oxide (ZnO) 1% to 8%,

[0017] The base glass may be subjected to heat treatment for crystallization and / or chemical ion strengthening treatment.

[0018] By limiting the specific components that make up the yttrium aluminum silicate base glass and the content of each component, a new type of yttrium aluminum silicate base glass can be prepared. The batch material composed of this base glass can be melted at a lower temperature. After optimizing the heat treatment process, the base glass can precipitate a crystalline phase with a specific crystal form and size to form microcrystalline glass. Moreover, the obtained microcrystalline glass can also be strengthened by chemical ion exchange. This forms a microcrystalline yttrium aluminum silicate system with high mechanical properties, high transparency, low cost, and large-scale production. It is understandable that the base glass itself can be directly subjected to chemical ion strengthening treatment to obtain strengthened glass to meet different usage requirements.

[0019] In combination with the first aspect, in some possible embodiments, at least one of the following ratio relationships exists between the components of the base glass:

[0020] The ratio of the molar percentage of Al2O3 to the molar percentage of Y2O3 is 0.2 to 7.5;

[0021] The sum of the molar percentage of Y2O3 and the molar percentage of Al2O3 is 7% to 45%;

[0022] The ratio of the molar percentage of Y2O3 to the molar percentage of Li2O is 0.33 to 8; and

[0023] The ratio of the molar percentage of Li2O to the molar percentage of Na2O is 0.33 to 8.

[0024] By limiting at least one of the above component ratios, transparent yttrium aluminum silicate glass can be prepared to avoid phase separation or devitrification of the glass. Then, through controllable crystallization, the expected crystal phase type can be formed, the crystal size and distribution can be regulated, and a better ion exchange effect can be obtained, thereby obtaining microcrystalline glass with high strength, high transparency and low cost.

[0025] In combination with the first aspect, in some possible embodiments, the base glass further includes 0-2% titanium dioxide (TiO2) calculated as a molar percentage.

[0026] Titanium dioxide can be introduced as a nucleating agent and compounded with ZrO2 and P2O5 to form a composite nucleating agent. Titanium dioxide can increase the nucleation rate of microcrystalline glass, but if the amount introduced is too large, it will cause the microcrystalline glass to be colored. Therefore, the addition amount of titanium dioxide is controlled within the range of 0-2%.

[0027] Furthermore, the total molar percentage of ZrO2, TiO2 and P2O5 is 2% to 6%.

[0028] By controlling the total amount of the composite nucleating agent, transparent yttrium aluminum silicate glass can be prepared, making crystallization controllable, thereby forming the expected crystal phase type and regulating the crystal size and distribution.

[0029] Furthermore, the ratio of the molar percentage of Y2O3 to the total molar percentage of ZrO2+TiO2+P2O5 is 0.5-25.

[0030] By controlling the ratio of Y2O3 to the total amount of the composite nucleating agent, the precipitation of the yttrium-containing crystal phase can be made more controllable, thereby forming the expected main crystal phase type and regulating the crystal size and distribution.

[0031] In combination with the first aspect, in some possible embodiments, the base glass further includes the following components, calculated by mole percentage:

[0032] Magnesium oxide (MgO): 0% to 2%;

[0033] Cerium oxide (CeO2): 0.1% to 0.5%;

[0034] Antimony trioxide (Sb2O3): 0.1%~0.5%.

[0035] The introduction of MgO is beneficial to improve the melting and forming of glass, but when the amount is too large, the glass is prone to phase separation and is not conducive to ion exchange. CeO2 and Sb2O3 are introduced as composite clarifiers.

[0036] The second aspect of the embodiment of the present application provides a glass-ceramic, which is obtained by crystallizing the base glass described in the first aspect of the embodiment of the present application through heat treatment, and the main crystalline phase of the glass-ceramic includes Y y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5y And one or more composite crystal phases of ZrO2. Further, the main crystal phase of the microcrystalline glass includes Y y Zr x O 1.5y+2x and Zr x Y y O 2x+1.5y One or two composite crystal phases.

[0037] The above-mentioned primary crystalline phases help improve the hardness, elastic modulus, and fracture toughness of the glass-ceramics, thereby enhancing the glass-ceramics' scratch and impact resistance. Specifically, the glass-ceramics have a Young's modulus greater than or equal to 90 GPa; a microhardness greater than or equal to 700 Hv at 0.2 kgf; and a transmittance greater than or equal to 88% at 550 nm in the visible light region.

[0038] It can be understood that the crystal phase of the microcrystalline glass may include other crystal phases in addition to the above main crystal phases, such as a composite crystal phase of one or more of ZnAl2O4, spodumene and quartz solid solution.

[0039] In combination with the second aspect, in some possible embodiments, the crystallinity of the main crystalline phase is greater than or equal to 5% and less than or equal to 90%, and the average crystal size of the main crystalline phase is less than or equal to 100 nm.

[0040] The crystallinity of the main crystalline phase affects the hardness, elastic modulus, fracture toughness, and transmittance of the microcrystalline glass. The greater the crystallinity, the greater the hardness, elastic modulus, and fracture toughness of the microcrystalline glass, but the transmittance will decrease, making it difficult to apply to mobile terminals. The smaller the crystallinity, the higher the transmittance of the microcrystalline glass, but the hardness, elastic modulus, and fracture toughness are too small, making it difficult to apply to mobile terminals. Therefore, in the embodiment of the present application, during the heat treatment process, the crystallinity of the main crystalline phase is controlled to be greater than or equal to 5% and less than or equal to 90%.

[0041] The average crystal size and uniformity of distribution of the primary crystalline phase affect the mechanical and optical properties of the resulting glass-ceramics. A too large average crystal size results in poor optical properties, such as low transmittance. A too small average crystal size reduces mechanical properties, such as poor strength and impact resistance. Therefore, in the embodiments of the present application, during the heat treatment process, the average crystal size of the primary crystalline phase is controlled to be less than or equal to 100 nm.

[0042] In combination with the second aspect, in some possible embodiments, the glass-ceramics may be subjected to chemical ion strengthening treatment.

[0043] By optimizing the formula of the above basic glass and optimizing the heat treatment process, the obtained microcrystalline glass can be chemically strengthened to further increase the strength of the microcrystalline glass while ensuring that the optical properties are not lost.

[0044] Specifically, after chemical ion strengthening treatment, the glass-ceramics have an ion exchange stress layer depth (DOC) greater than or equal to 90 μm; a surface compressive stress (Cs50) greater than or equal to 100 MPa; a surface compressive stress value (Cs) greater than or equal to 260 MPa; and an average tensile stress greater than or equal to 60 MPa. The chemically ion-strengthened glass-ceramics have a microhardness greater than or equal to 780 Hv at 0.2 kgf. For a 0.7 mm thick sample of the chemically ion-strengthened glass-ceramics, the four-point bending strength is greater than or equal to 600 MPa at an impact energy greater than or equal to 0.2 J.

[0045] In combination with the second aspect, in some possible embodiments, the glass transition temperature of the glass-ceramics is greater than or equal to 560°C.

[0046] The glass-ceramics obtained after heat treatment and crystallization of the aforementioned base glass has a higher glass transition temperature, and the glass network structure is relatively compact, which can improve the strength of the glass-ceramics and reduce the damage to the glass network structure during the chemical strengthening process.

[0047] A third aspect of the present invention provides a method for preparing glass-ceramics, the method comprising:

[0048] Melting, forming, and annealing batch materials corresponding to the chemical composition of the base glass to obtain the base glass, wherein the base glass comprises the following components, calculated in molar percentage: yttrium oxide (Y2O3): 4% to 15%; aluminum oxide (Al2O3): 3% to 30%; silicon dioxide (SiO2): 40% to 75%; zirconium dioxide (ZrO2): 0.5% to 4%; lithium oxide (Li2O): 3% to 12%; sodium oxide (Na2O): 1.5% to 9%; phosphorus pentoxide (P2O5): 0.1% to 2%; and zinc oxide (ZnO): 1% to 8%; and

[0049] The base glass is subjected to heat treatment and crystallization to obtain the microcrystalline glass.

[0050] By adjusting the basic glass formula, the obtained yttrium aluminum silicon basic glass can be heat treated and crystallized to obtain the main crystal phase including Y y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5y , and at least one of the crystal phase types of ZrO2, and the crystallinity and crystal size are controllable, so that microcrystalline glass with high mechanical properties and optical properties can be prepared.

[0051] In combination with the third aspect, in some possible embodiments, the heat treatment includes a first step heat treatment and a second step heat treatment performed sequentially, wherein the heat treatment temperature of the first step heat treatment is 600-720°C, and the heat treatment time is 0.5-40h; the heat treatment temperature of the second step heat treatment is 730-850°C, and the heat treatment time is 0.5-8h.

[0052] By optimizing the heat treatment process and combining it with the regulation of the aforementioned components, the crystallinity and crystal size of the main crystalline phase in the microcrystalline glass can be better controlled, making both the crystallinity and the crystal size as small as possible. The specific crystallinity can be 5% to 90%, and the average crystal size is less than or equal to 100nm. This ensures that the microcrystalline glass has high strength while reducing the refractive index of the microcrystalline glass to improve the transmittance of the microcrystalline glass.

[0053] In conjunction with the third aspect, in some possible embodiments, after the step of obtaining the glass-ceramics, the preparation method further includes:

[0054] The glass-ceramics is subjected to chemical ion strengthening treatment.

[0055] The obtained glass-ceramics can be subjected to chemical strengthening treatment, thereby further improving the mechanical properties of the glass-ceramics.

[0056] In conjunction with the third aspect, in some possible embodiments, the chemical ion strengthening treatment includes at least one ion exchange, and the ion exchange is performed in a metal molten salt, and the metal molten salt contains at least one of sodium ions and potassium ions. Specifically, the chemical ion strengthening treatment includes a first ion exchange and a second ion exchange, wherein:

[0057] The metal molten salt of the first ion exchange comprises sodium nitrate, potassium nitrate and lithium nitrate, the exchange temperature is 430° C. to 530° C., and the exchange time is 4 h to 12 h;

[0058] The metal molten salt for the second ion exchange comprises sodium nitrate, potassium nitrate and lithium nitrate, the exchange temperature is 400° C. to 500° C., and the exchange time is 0.5 h to 5 h.

[0059] By controlling the chemical strengthening process, the depth of ion exchange can be increased, resulting in a stress layer depth (DOC) greater than or equal to 90 μm; a surface compressive stress (Cs50) greater than or equal to 100 MPa; a surface compressive stress value (Cs) greater than or equal to 260 MPa; and an average tensile stress greater than or equal to 60 MPa. The strengthened glass-ceramics exhibit a microhardness greater than or equal to 780 Hv at 0.2 kgf. A 0.7 mm thick sample of the strengthened glass-ceramics exhibits a four-point bending strength greater than or equal to 600 MPa at an impact energy greater than or equal to 0.2 J.

[0060] In conjunction with the third aspect, in some possible embodiments, the melting temperature of the batch material corresponding to the basic glass chemical composition is 1500°C to 1650°C.

[0061] The melting temperature of the batch materials corresponding to the basic glass chemical composition is relatively low, and they can be prepared by conventional melting methods. For example, they can be melted by high-temperature melting equipment such as silicon-molybdenum furnaces, electric melting furnaces, and flame kilns. No special process is required for preparation, and large-scale production can be achieved.

[0062] In conjunction with the third aspect, in some possible embodiments, at least one of the following ratio relationships exists between the components of the base glass:

[0063] The ratio of the molar percentage of Al2O3 to the molar percentage of Y2O3 is 0.2 to 7.5;

[0064] The sum of the molar percentage of Y2O3 and the molar percentage of Al2O3 is 7% to 45%;

[0065] The ratio of the molar percentage of Y2O3 to the molar percentage of Li2O is 0.33 to 8; and

[0066] The ratio of the molar percentage of Li2O to the molar percentage of Na2O is 0.33 to 8.

[0067] In combination with the third aspect, in some possible embodiments, the base glass further includes 0-2% titanium dioxide (TiO2) calculated as a molar percentage.

[0068] Furthermore, the total molar percentage of ZrO2, TiO2 and P2O5 is 2% to 6%.

[0069] Furthermore, the ratio of the molar percentage of Y2O3 to the molar percentage of ZrO2+TiO2+P2O5 is 0.5-25.

[0070] A fourth aspect of the present application provides a glass product, wherein the glass product is made from the base glass described in the first aspect of the present application, or from the glass-ceramic described in the second aspect of the present application, or from glass-ceramic prepared by the method for preparing glass-ceramic described in the third aspect of the present application. Specifically, the glass product is a glass cover plate.

[0071] The microcrystalline glass made from the basic glass of the aforementioned yttrium aluminum silicon system has both high optical and mechanical properties. The glass product can be used as, but not limited to, a protective material in various mobile terminals or electronic products, such as a glass cover for various mobile terminals or electronic products.

[0072] A fifth aspect of the present application provides a terminal device comprising the glass product described in the fourth aspect of the present application. Specifically, the glass product may be a glass cover plate for the terminal device. It will be appreciated that, in addition to terminal devices, the glass product may also be used for other products requiring surface protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] FIG1 is a schematic structural diagram of a terminal device provided in an embodiment of the present application.

[0074] FIG2 is a schematic diagram of the preparation process of glass-ceramics provided in one embodiment of the present application.

[0075] FIG3 is a crystal diffraction pattern of the glass-ceramics prepared in Examples 1 to 4 and Comparative Example 1 of the present application.

[0076] FIG4A is a “stress-depth” curve of the glass-ceramics prepared in Example 1 of the present application after ion exchange.

[0077] FIG4B is a diagram showing the Na ion concentration distribution of the glass-ceramics prepared in Example 1 of the present application after ion exchange.

[0078] 5A to 5D are crystal morphology diagrams of Examples 1 to 4 of the present application, respectively.

[0079] Description of main component symbols

[0080] Device 100

[0081] Housing 10

[0082] Glass cover 20 DETAILED DESCRIPTION

[0083] The present invention will be described below in conjunction with the accompanying drawings in the embodiments of the present invention. The data ranges involved in this application should include upper and lower limits, as well as any range between the upper and lower limits unless otherwise specified. In addition, when quantity, concentration or other numerical values ​​or parameters are given in the form of a range, one or more preferred ranges, or a preferred upper limit and a preferred lower limit, this should be understood as clearly disclosing all ranges formed by any combination of any range upper limit or preferred value and any range lower limit or preferred value. It should also be understood that the various features disclosed in the specification and the accompanying drawings can be used in any combination.

[0084] In this application, unless otherwise specified, the content of each glass component is expressed as mole percentage of oxide.

[0085] In this application, "base glass" refers to glass that has not yet formed crystals and has not been strengthened. In this application, "glass-ceramics" refers to glass containing a crystalline phase obtained by heat-treating base glass, or by heat-treating and strengthening it. In this application, the compositions of base glass and corresponding glass-ceramics are essentially equivalent.

[0086] Current lithium-aluminum-silicon glass-ceramics systems suffer from the following issues: high lithium oxide content, resulting in high costs; low elastic modulus, making the glass susceptible to breakage after certain mechanical impacts; and low surface hardness, making it less scratch-resistant and prone to cracking when impacted by sharp objects. However, these issues are inherent to the characteristics of the lithium-aluminum-silicon glass-ceramics system, leaving limited room for improvement.

[0087] In view of this, the inventors of the present application have prepared a new type of yttrium aluminum silicate glass, and prepared the corresponding yttrium aluminum silicate microcrystalline glass through a heat treatment process. Yttrium oxide is added to the aluminum silicate glass, and the yttrium ions can fill the glass gaps very well, change the density of the glass, and achieve a high elastic modulus and high Vickers hardness of the glass, thereby improving the drop resistance of the glass. However, when the added yttrium oxide content is too high, the melting point of yttrium oxide is as high as 2410°C, which will cause the melting of the glass to be difficult. Special processes such as plasma are required, which makes it difficult to produce on a large scale. In addition, when the yttrium oxide content is too high, it will also lead to a higher refractive index of the glass, which seriously reduces the transmittance of the glass, especially the microcrystalline glass obtained after heat treatment has a very low transmittance and poor optical properties, making it difficult to apply to the field of terminal cover plates. When the yttrium oxide content is too low, the glass network structure is relatively loose and the crystal content is also low, resulting in poor mechanical properties of the microcrystalline glass.

[0088] To this end, the inventors of this application have conducted repeated experiments and studies to optimize the selection of specific components constituting the yttrium aluminum silicate glass system, the content of each component, and the content ratio between the specific components, thereby preparing a new type of base glass of the yttrium aluminum silicate system, the batch material composed of which can be melted at a lower temperature; and after optimizing the heat treatment process, the base glass can precipitate a crystalline phase with a specific crystal form and size to form microcrystalline glass; moreover, the obtained microcrystalline glass can also be subjected to chemical ion exchange strengthening treatment, thereby forming a microcrystalline glass of the yttrium aluminum silicate system with high strength, high transparency, low cost, and the ability to be produced on a large scale.

[0089] The base glass provided in the embodiments of the present application mainly comprises the following components, calculated in molar percentage: yttrium oxide (Y2O3): 4% to 15%; aluminum oxide (Al2O3): 3% to 30%; silicon dioxide (SiO2): 40% to 75%; zirconium dioxide (ZrO2): 0.5% to 4%; lithium oxide (Li2O): 3% to 12%; sodium oxide (Na2O): 1.5% to 9%; phosphorus pentoxide (P2O5): 0.1% to 2%; and zinc oxide (ZnO) 1% to 8%.

[0090] After the base glass is formed, crystallization can be performed by heat treatment to prepare glass-ceramics, wherein the main crystalline phase of the glass-ceramics includes Y y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5y , ZrO2, and further, the main crystalline phase of the microcrystalline glass may include Y y Zr x O 1.5y+2x and Zr x Y y O 2x+1.5y The above main crystalline phases help to improve the hardness, elastic modulus and fracture toughness of the glass-ceramics, thereby improving the scratch resistance and impact resistance of the glass-ceramics. It is understandable that in addition to the above main crystalline phases, the glass-ceramics also contains other crystalline phases with relatively small contents, specifically including one or more composite crystalline phases of ZnAl2O4, spodumene and quartz solid solution.

[0091] Among them, the crystallinity of the main crystalline phase affects the hardness, elastic modulus, fracture toughness and transmittance of the microcrystalline glass. The greater the crystallinity, the greater the hardness, elastic modulus and fracture toughness of the microcrystalline glass will be, but the transmittance will decrease, making it difficult to apply to mobile terminals. The smaller the crystallinity, although the transmittance of the microcrystalline glass will increase, the hardness, elastic modulus and fracture toughness are too small, making it difficult to apply to mobile terminals. Therefore, in the embodiment of the present application, during the heat treatment process, the crystallinity of the main crystalline phase is controlled to be greater than or equal to 5%, and less than or equal to 90%. If the crystallinity is too low, the mechanical properties of the glass will be poor, such as Young's modulus, Vickers hardness, etc. If the crystallinity is too high, it will easily lead to the formation of impurities and reduce the transmittance of the glass. In some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 8%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 10%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 12%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 15%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 17%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 20%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 25%; in some embodiments, the crystallinity of the main crystalline phase is greater than or equal to 30%. By controlling the crystallinity of the main crystalline phase within the above range, the obtained microcrystalline glass can have excellent optical properties while improving mechanical properties such as hardness, elastic modulus and fracture toughness.

[0092] Among them, the average crystal size of the main crystalline phase and the uniformity of its distribution will affect the mechanical and optical properties of the obtained microcrystalline glass. If the average crystal size is too large, the optical properties will be poor, such as low transmittance. If the average crystal size is too small, the mechanical properties will be reduced, such as poor strength and impact resistance. Therefore, in the embodiments of the present application, during the heat treatment process, the average crystal size of the main crystalline phase is controlled to be less than or equal to 100 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 95 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 90 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 85 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 80 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 75 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 70 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 65 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 60 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 55 nm; in some embodiments, the average crystal size of the main crystalline phase is less than or equal to 50 nm. By controlling the average crystal size of the main crystalline phase within the above range and controlling the uniform distribution of the main crystalline phase, the obtained microcrystalline glass can have excellent optical properties while improving mechanical properties such as hardness, elastic modulus and fracture toughness.

[0093] Among them, Y2O3 is an essential component in the base glass, which can fill the gaps in the glass well and effectively improve the stacking degree of the base glass network structure. In addition, Y2O3 as a raw material can form Y2O3 after heat treatment. y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5yA crystalline phase containing at least one of ZrO2 as the main component can improve the hardness, elastic modulus, and fracture toughness of the glass-ceramics, thereby improving the scratch resistance and impact resistance of the glass-ceramics. However, an excessively high yttrium oxide content will increase the refractive index and reduce the transmittance of the glass-ceramics, making it difficult to use in mobile terminals. Therefore, the yttrium oxide content needs to be controlled within a certain range to balance the optical and mechanical properties of the glass-ceramics. Through extensive experimental research, the composition range of Y2O3 was determined: the lower limit is 5%. If it is too low, below 5%, the glass crystallization ability is weak and the expected glass-ceramics cannot be prepared. The lower limit can be further 6%, the lower limit can be further 7%, and the lower limit can be further 7.5%. The upper limit of Y2O3 can be 15%. If it is too high, above 15%, due to the high melting point of Y2O3, the components of the base glass are difficult to melt, and the resulting glass-ceramics have a high refractive index and low transmittance. The upper limit can be further 14%, the upper limit can be further 12.5%, the upper limit can be further 11%, and the upper limit can be further 10%. It is understood that in the embodiments of the present application, the content of Y2O3 can be within the range between any upper limit and any lower limit above. For example, in the embodiments of the present application, the content of Y2O3 can be 5% to 15%, further 6% to 14%, further 6% to 12.5%, further 7% to 11%, and further 7.5% to 10%. For example, the content of Y2O3 can be 5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, or a value between any two of the above values. By controlling the Y2O3 content within the above range, microcrystalline glass with excellent mechanical and optical properties can be obtained. In particular, when the Y2O3 content is within the range of 7.5% to 10%, the optical and mechanical properties of the obtained microcrystalline glass are significantly improved.

[0094] Al2O3 is an essential component in this base glass. When there is sufficient free oxygen, it can participate in the construction of the glass network structure, which is beneficial to improving the glass strength and chemical stability. The appropriate amount of Al2O3 is conducive to the ion exchange of microcrystalline glass. However, if the Al2O3 content is too low, the glass network structure will be loose, and the glass strength and chemical stability will be low. If the Al2O3 content is too high, the glass network structure will be too dense, making the precipitation and growth of crystals difficult, thus affecting the formation of microcrystalline glass. Therefore, in the embodiments of the present application, the lower limit of the Al2O3 content is set at 3%, the lower limit can be further 5%, the lower limit can be further 8%, and the lower limit can be further 10%; the upper limit of the Al2O3 content can be 20%, the upper limit can be further 18%, the upper limit can be further 15%, and the upper limit can be further 14%. It is understood that in the embodiments of the present application, the Al2O3 content can be within the range between any of the above upper and lower limits. For example, in the embodiments of the present application, the Al2O3 content can be 5% to 20%, further 5% to 18%, further 8% to 15%, and further 8% to 14%. Exemplarily, the content of Al2O3 can be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or a value between any two of the above values. By controlling the content within the above range, it is beneficial to improve the strength and chemical stability of the glass, while providing more sufficient space for crystallization and crystal growth, and helping to control the precipitation of target crystals during heat treatment. In particular, when the content of Al2O3 is between 8% and 15%, a more stable network structure can be formed, and more sufficient space can be provided for crystallization and crystal growth.

[0095] SiO2 is an essential component in the base glass, mainly used to form the network structure of the glass and improve the chemical and thermal stability of the glass. If the SiO2 content is below 40%, the glass forming properties deteriorate, the chemical stability deteriorates, phase separation is easy, and even glass cannot be formed. Therefore, the lower limit of the SiO2 content can be above 40%, and further above 45%. However, when the SiO2 content is too high, the melting and crystallization control of the microcrystalline glass will become difficult. Therefore, the upper limit of the SiO2 content can be limited to below 75%, and further below 65%. It can be understood that in the embodiments of the present application, the SiO2 content can be within the range between any of the above upper and lower limits. For example, in the embodiments of the present application, the SiO2 content can be 40% to 75%, and further can be 45% to 65%. For example, the SiO2 content can be 45%, 50%, 55%, 60%, 65%, 70%, 75%, or a value between any two of the above values. By controlling the SiO2 content within the above range, the chemical stability and thermal stability of the base glass can be improved, the difficulty of crystallization during heat treatment can be reduced, and the controllability of crystallization can be improved.

[0096] ZrO2 is an essential component in this base glass. Its main functions are: first, it acts as a nucleating agent, ensuring uniform crystallization of the glass, effectively controlling crystal precipitation and size, and preventing oversized crystals from affecting optical properties; second, it improves the chemical stability of the base glass or glass-ceramics even when the lithium content is relatively high. During experimental research, the inventors discovered that ZrO2 can also effectively reduce the risk of devitrification of the base glass during the forming process. To achieve the aforementioned glass-ceramics effect, the lower limit of the ZrO2 content can be 0.5%, further 1.5%, and even further 2.5%. However, if the ZrO2 content is too high, it will increase the melting temperature of the glass, making the melting process more difficult. Therefore, the upper limit of the ZrO2 content can be 4%, and further 3.5%. It is understood that in the embodiments of this application, the ZrO2 content can range between any of the above upper and lower limits. For example, in the embodiments of this application, the ZrO2 content can range from 0.5% to 4%, further 1.5% to 3.5%, and further 2% to 3.5%. For example, the content of ZrO2 can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or a value between any two of the above values.

[0097] Li2O is an essential component in the base glass. It can reduce the viscosity of the base glass to facilitate melting. It is also the main component in the ion exchange process. It is a component that replaces sodium ions and potassium ions and can increase the depth of chemical ion strengthening compressive stress. However, if its content is less than 3%, on the one hand, it is not conducive to the glass melting effect, and on the other hand, it is difficult to obtain a deeper ion exchange depth. Therefore, the lower limit of the Li2O content is 3%, and further 6%. If too much Li2O is contained, the chemical stability of the glass will deteriorate, and it will be difficult to control during crystallization, resulting in phase separation or changes in the main crystal phase type. Therefore, the upper limit of the Li2O content is 12%, further 11%, and further 10.5%. It can be understood that in the embodiments of the present application, the content of Li2O can be in the range between any of the above upper and lower limits. For example, in the embodiments of the present application, the content of Li2O can be 3% to 12%, further 6% to 11%, and further 6% to 10.5%. Illustratively, the content of Li2O can be 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12% or a value between any two of the above values.

[0098] Na2O is an essential component in this base glass, which is significantly different from the low Na2O content in general microcrystalline glass. As the outer body of the glass network, Na2O mainly plays the role of breaking the network and providing free oxygen, and has a strong effect of inhibiting crystal precipitation. Generally, the Na2O content of microcrystalline glass is low, which is beneficial to crystallization. However, in the embodiment of the present application, if the Na2O content is too low, during ion exchange, the exchange content of Na ions and K ions in the microcrystalline glass is insufficient, and the surface compressive stress value is low, which affects the strength. Therefore, in the embodiment of the present application, the Na2O content cannot be too low, and the lower limit can be 1.5%, and further 2%. If the glass contains too much Na2O, on the one hand, it will increase the glass expansion coefficient, poor thermal stability, make annealing difficult, and easily cause the risk of bursting. On the other hand, it will also inhibit the precipitation of crystals, reduce the crystal content, and thus reduce the strength of the microcrystalline glass. Therefore, in the embodiment of the present application, the upper limit of the Na2O content can be 9%, and further 6%. It is understood that in the embodiments of the present application, the content of Na2O can be within the range between any upper limit and any lower limit above. For example, in the embodiments of the present application, the content of Na2O can be 1.5% to 9%, and further can be 2% to 6%. For example, the content of Na2O can be 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, or a value between any two of the above values.

[0099] P2O5 is an essential component in the base glass. Its introduction can increase the amount of zirconium oxide introduced and make the glass network loose due to the effect of π bonds. Therefore, a small amount of P2O5 can lower the melting temperature of the glass and improve the ion exchange efficiency. However, too high a P2O5 content can cause phase separation of the glass, affect the optical properties, and even cause devitrification. Therefore, the P2O5 content is 0.1% to 2%, and further 0.3-1%. Exemplary, the P2O5 content can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or a value between any two of the above values.

[0100] ZnO is an essential component in the base glass. Its introduction helps improve the melting, nucleation and crystallization properties of the glass. However, when the amount introduced is too large, the glass is prone to phase separation. Therefore, the ZnO content in the embodiment of the present application is 1% to 8%, and further 3% to 5%. Exemplarily, the ZnO content can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8% or a value between any two of the above values.

[0101] MgO is an optional component in the base glass. Its introduction is beneficial to improving the melting and forming of the glass. However, when the amount introduced is too large, the glass is prone to phase separation and is not conducive to ion exchange. Therefore, the content of MgO in the embodiment of the present application is 0% to 2%, and further 0.5% to 1.5%. Exemplarily, the content of MgO can be 0, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or a value between any two of the above values.

[0102] TiO2 is an optional component of the base glass. It is introduced as a nucleating agent to increase the nucleation rate of the microcrystalline glass. However, when the amount of TiO2 introduced is too large, it will cause the microcrystalline glass to be colored. Therefore, the content of TiO2 in the embodiment of the present application is 0% to 2%, and further 0.5% to 1.5%. Exemplarily, the content of TiO2 can be 0, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or a value between any two of the above values.

[0103] CeO2 and Sb2O3 are introduced as composite fining agents. Therefore, in the embodiments of the present application, the contents of CeO2 and Sb2O3 can be 0.1% to 0.5%, and further 0.2% to 0.3%. For example, the contents of CeO2 and Sb2O3 can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, or any value between the above two values.

[0104] In addition, in order to prepare transparent yttrium aluminum silicate glass, avoid phase separation or devitrification of the glass, and then form the desired crystal phase type through controlled crystallization, regulate the crystal size and distribution, and obtain a better ion exchange effect, thereby obtaining a microcrystalline glass with high strength, high transparency and low cost. The embodiment of the present application also defines at least one of the following component ratio relationships (1) to (6):

[0105] (1) The ratio of the molar percentage of Al2O3 to the molar percentage of Y2O3 can be 0.2 to 7.5, further 0.7 to 3. Exemplarily, the ratio can be 0.2, 0.5, 0.7, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5 or a value between any two of the above values.

[0106] (2) The sum of the molar percentage of Y2O3 and the molar percentage of Al2O3 can be 7% to 45%, further 10% to 40%. Exemplarily, the sum of the molar ratios can be 7%, 10%, 15%, 18%, 20%, 25%, 30%, 35%, 40%, 45% or a value between any two of the above values.

[0107] (3) The ratio of the mole percentage of Y2O3 to the mole percentage of Li2O can be 0.33 to 8, further 0.33 to 5. Exemplarily, the ratio can be 0.33, 0.35, 0.38, 0.4, 0.45, 0.5, 0.55, 0.6, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8 or a value between any two of the above values.

[0108] (4) The ratio of the molar percentage of Li2O to the molar percentage of Na2O can be 0.33 to 8, further 1 to 5. Exemplarily, the ratio can be 0.33, 0.38, 0.4, 0.45, 0.5, 0.55, 0.6, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8 or a value between any two of the above values.

[0109] (5) When TiO2 is added to the formula, the total molar percentage of ZrO2, TiO2 and P2O5 as composite nucleating agents can be 2% to 6%, further 2% to 5%. Exemplarily, the total molar percentage of the composite nucleating agent can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7% or a value between any two of the above values.

[0110] (6) When TiO2 is added to the formulation, the ratio of the molar percentage of Y2O3 to the total molar percentage of ZrO2+TiO2+P2O5 can be 0.5-25, further 1.5-14. Exemplarily, the ratio can be 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25 or a value between any two of the above values.

[0111] Specifically, the Young's modulus of the microcrystalline glass obtained after the base glass of the yttrium aluminum silicon system is heat-treated and crystallized can reach more than 100Gpa. The microcrystalline glass that has not been chemically strengthened can reach a microhardness of more than 700Hv under the action of 0.2Kgf, and further can reach more than 750Hv. The microcrystalline glass can be further chemically strengthened. After chemical strengthening, the depth of the stress layer DOC of the ion exchange is ≥90μm (0.6t), and further more than 110μm. The microcrystalline glass after strengthening can reach a microhardness of more than 780Hv under the action of 0.2Kgf, and further more than 820Hv. And the transmittance of the microcrystalline glass can reach more than 88% (550nm), and further more than 90%; the haze is ≤0.5%, and further ≤0.2%. The microcrystalline glass that has been strengthened, a 0.7mm thick sample, under the condition of impact energy greater than or equal to 0.2J, has a four-point bending strength greater than or equal to 600MPa. The glass transition temperature of the glass-ceramics is greater than or equal to 560°C.

[0112] Therefore, glass-ceramics made from this YAS-based glass system offer both high optical and mechanical properties and can be used, but not limited to, as protective materials in various mobile terminals or electronic products, such as glass cover plates. Mobile terminal products include, but are not limited to, mobile phones, tablets, desktop computers, laptops, smart screens, monitors, speakers, glasses, watches, headphones, in-car products, and other electronic terminal devices related to mobile office, smart home, sports and health, audio and video entertainment, and smart travel. It is understood that in addition to terminal devices, these glass products can also be used in other products requiring surface protection.

[0113] In some embodiments, referring to FIG. 1 , the terminal device 100 may be a mobile phone. The terminal device 10 includes a middle frame 10 and a glass cover 20 connected to the middle frame 10 .

[0114] It is understandable that, in addition to terminal equipment, the glass product can also be used for other products that require surface protection.

[0115] It is also understandable that, depending on different application scenarios, the base glass can also be directly subjected to chemical strengthening treatment to obtain strengthened glass.

[0116] Based on the same inventive concept, referring to FIG. 2 , the present embodiment further provides a method for preparing the aforementioned glass-ceramics, comprising:

[0117] In step S1, a batch material corresponding to the chemical composition of the basic glass is melted, formed, and annealed to obtain the basic glass. The components of the basic glass are described above and will not be described in detail here.

[0118] Specifically, the chemical raw materials or mineral raw materials corresponding to the various components of the basic glass can be melted using high-temperature melting equipment such as a silicon-molybdenum furnace, an electric melting furnace, and a flame kiln, and stirred using a platinum stirring paddle. Subsequently, they are formed using conventional processes such as casting, rolling, float glass, and down-drawing, and after heat preservation and annealing treatment, yttrium aluminum silicon system glass is obtained.

[0119] The melting temperature of the basic glass formula in the embodiment of the present application is relatively low, roughly in the range of 1500°C to 1650°C, and can be prepared by conventional melting methods without the need for special processes, thereby enabling large-scale production.

[0120] After annealing, the glass is cut on six sides to obtain glass of appropriate size. Then, a wire cutting machine, a CNC engraving machine, and a flat grinding and polishing machine are used to perform fine cutting, flat grinding, and edge sweeping to obtain basic glass of a certain size. The thickness of the basic glass can be between 0.1mm and 1.5mm.

[0121] Step S2: heat-treating and crystallizing the obtained basic glass to obtain microcrystalline glass.

[0122] Since nucleation and growth occur simultaneously in the one-step heat treatment, there are situations where crystal agglomeration, unstable generated crystals, and co-growth of polycrystalline phases occur. During the growth process, small crystals become smaller and large crystals become larger, resulting in coarse and uneven crystal size, and the subsequent decorrelation and ion exchange effects are not ideal.

[0123] Therefore, the embodiment of the present application adopts a two-step heat treatment, specifically:

[0124] The first step of heat treatment is to heat treat the base glass at a nucleation temperature of 600 to 720°C for 0.5 to 40 hours to slowly and fully form crystal nuclei - a nucleation process.

[0125] In some embodiments, the nucleation temperature can further be 650-720°C. Exemplarily, the nucleation temperature can be 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C or a value between any two of the above values.

[0126] In some embodiments, the nucleation time can further be 5 to 30 h, 10 to 20 h. Exemplarily, the nucleation time can be 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 22 h, 25 h, 28 h, 30 h, 35 h, 40 h or a value between any two of the above values.

[0127] The second step is heat treatment, which involves heat treating the nucleated glass plate at a crystallization temperature of 730-850°C for 0.5-8 hours to precipitate crystals and allow the crystals to grow further - a crystallization process, thereby obtaining microcrystalline glass with relatively uniform crystal size, no obvious edges and corners, and an average crystal size of 5-100nm.

[0128] In some embodiments, the crystallization temperature can further be 750-780°C. Exemplarily, the nucleation temperature can be 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C or a value between any two of the above values.

[0129] In some embodiments, the crystallization time can further be 0.5-6 h, 1-4 h. Exemplarily, the nucleation time can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h, 8 h or a value between any two of the above values.

[0130] During the heat treatment process, when the nucleation temperature is too high or the crystallization temperature is too low, it is difficult to form crystals of a specific size and uniform size distribution; when the nucleation temperature is too low or the crystallization temperature is too high, the temperature of the base glass during normal crystallization is too high, and the crystal size tends to grow too large, reducing the transmittance. Therefore, within the above crystallization temperature and nucleation temperature range, it is beneficial to control the size and distribution of the crystals. In addition, a longer heat treatment time in the nucleation process can make the nucleation more complete and improve the uniformity of the crystal distribution. A shorter heat treatment time in the crystallization stage can control the size of the crystals from growing too large. Therefore, through the above heat treatment process, microcrystalline glass with both high mechanical and optical properties can be obtained.

[0131] By optimizing the heat treatment process and combining it with the regulation of the aforementioned components, the crystallinity and crystal size of the main crystalline phase in the microcrystalline glass can be better controlled, making both the crystallinity and the crystal size as small as possible. The specific crystallinity can be 5%-90%, and the average crystal size is less than or equal to 100nm. This ensures that the microcrystalline glass has high strength while reducing the refractive index of the microcrystalline glass to improve the transmittance of the microcrystalline glass.

[0132] Step S3: chemically strengthening the glass-ceramics.

[0133] The chemical strengthening treatment includes at least one ion exchange, and the ion exchange is carried out in a metal molten salt, wherein the metal molten salt may contain at least one of metal salts such as sodium ions, potassium ions and lithium ions.

[0134] Specifically, in the embodiments of the present application, the chemical strengthening treatment includes secondary ion exchange.

[0135] The metal molten salt for the first ion exchange includes sodium nitrate, potassium nitrate, lithium nitrate, etc., the exchange temperature is 430° C. to 530° C., and the exchange time is 4 hours to 12 hours.

[0136] In some embodiments, the exchange temperature may further be 450° C.-500° C., further 450° C.-480° C. Exemplarily, the exchange temperature may be 430° C., 440° C., 450° C., 460° C., 470° C., 480° C., 490° C., 500° C., 510° C., 520° C., 530° C., or a value between any two of the above values.

[0137] In some embodiments, the exchange time can further be 5 hours to 10 hours. Exemplarily, the exchange time can be 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours or a value between any two of the above values.

[0138] The metal molten salt for the second ion exchange includes sodium nitrate, potassium nitrate, lithium nitrate, etc., and the exchange time is 400-500° C. and the exchange time is 0.5h-5h.

[0139] In some embodiments, the exchange temperature may further be 430° C.-480° C., further 450° C.-480° C. Exemplarily, the exchange temperature may be 400° C., 410° C., 420° C., 430° C., 440° C., 450° C., 460° C., 470° C., 480° C., 490° C., 500° C., or a value between any two of the above values.

[0140] In some embodiments, the exchange time can further be 1 hour to 4 hours. Exemplarily, the exchange time can be 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours or a value between any two of the above values.

[0141] During the strengthening process, the primary ion exchange increases the depth of the glass's strengthening stress, while the secondary ion exchange increases surface stress. By controlling the strengthening process, optimal stress levels can be achieved, improving the glass's impact and drop resistance.

[0142] The following is a further explanation of the embodiments of the present application through specific examples. In different embodiments, the composition of the base glass and the preparation and strengthening process conditions of the microcrystalline glass are different. The specific base glass material and process conditions are shown in Table 1, and the corresponding characteristic parameters are shown in Table 2.

[0143] Table 1

[0144] Table 2

[0145] Note: The chemical strengthening conditions in Examples 1 to 4 above all involved a two-step strengthening process. The first step involved a NaNO₃ (95%) + KNO₃ (5%) salt bath at 490°C for 8 hours; the second step involved a KNO₃ (100%) salt bath at 450°C for 1 hour. The thickness of the glass-ceramics was 0.65 mm.

[0146] The above performance test method is:

[0147] Elastic modulus: Refer to GB / T 7962.6-2010 and measure with elastic modulus meter.

[0148] Microhardness: Refer to GB / T 37900-2019 and measure with Vickers hardness tester.

[0149] Visible light transmittance: Refer to GB / T 2410-2008 and measured by spectrophotometer.

[0150] Haze: Refer to GB / T2410-2008, using Konica Minolta CM3600A colorimeter.

[0151] Cs50 after ion exchange: measured using Orihara SLP series instruments.

[0152] Ion exchange depth: measured using an Orihara SLP series instrument.

[0153] Surface compressive stress value: measured using Orihara SLP series instrument.

[0154] Average tensile stress Ct-Av: measured using Orihara SLP series instruments.

[0155] Drop ball impact: Use a steel ball with a diameter of ¢20mm and a weight of 32.65g to perform an impact test on the glass in the form of free fall. Record the drop ball height h corresponding to the glass breaking and convert it into the corresponding impact energy using the energy calculation formula: J=Mgh. Where M is the mass of the steel ball and g=9.8m / s 2 , h is the failure height of the glass.

[0156] In addition, as shown in FIG3, the diffraction patterns of the crystals in the glass-ceramics prepared in Examples 1-4 and Comparative Example 1 are shown. It can be seen from the figure that the main crystalline phase in the glass-ceramics of Examples 2-3 is Y4Zr3O 12 Crystal phase, the main crystal phase in the glass-ceramics of Example 1 is Y4Zr3O 12 The main crystal phase in the glass-ceramics of Example 4 is Zr 0.72 Y 0.28 O 1.862 , Li(AlSi2O6) and Y2Si2O7 three crystal phases. The main crystal phase in the glass-ceramics of comparative example 1 is Zr 0.9 Y 0.1 O 1.95 、Y2Si2O7、Y4Zr3O 12 This indicates that when the composition design is not appropriate, crystals such as Li(AlSi2O6) and Y2Si2O7 are likely to precipitate in the glass-ceramics, resulting in a decrease in transmittance and an increase in haze.

[0157] As shown in FIG4A and FIG4B, the concentration distribution diagram of Na ions in the glass-ceramics of Example 1 after ion exchange is shown in FIG4A. As can be seen from FIG4A, after chemical strengthening, Na + Ions are concentrated in the surface layer of the glass. As the depth increases, Na +As shown in Figure 4B, after chemical strengthening, the ion exchange depth can reach 136 μm, and the compressive stress value is high, while the tensile stress is appropriate.

[0158] As shown in Figures 5A to 5D, they are morphologies of crystals in the microcrystalline glass of Examples 1-4, respectively. It can be seen from the figures that the crystals in the microcrystalline glass of Examples 1-4 are evenly distributed and have uniform crystal sizes. The formed crystals are nanocrystals with a size of less than 100 nm, which can help improve the transmittance of the microcrystalline glass.

[0159] It should be noted that the above are only specific embodiments of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present application should be included in the scope of protection of the present application; the embodiments of the present application and the features of the embodiments can be combined with each other unless there is a conflict. Therefore, the scope of protection of the present application shall be based on the scope of protection of the claims.

Claims

1. A basic glass, It is characterized in that The base glass comprises the following components in terms of molar percentage: yttrium trioxide (Y 2 O 3 ): 4% to 15%; Aluminum oxide (Al 2 O 3 ): 3% to 30%; Silicon dioxide (SiO 2 ): 40% to 75%; Zirconium dioxide (ZrO 2 ): 0.5% to 4%; Lithium oxide (Li 2 O): 3% to 12%; Sodium oxide (Na 2 O): 1.5% to 9%; Phosphorus pentoxide (P 2 O 5 ): 0.1% to 2%; Zinc oxide (ZnO) 1% to 8%, The base glass may be subjected to heat treatment for crystallization and / or chemical ion strengthening treatment.

2. The base glass according to claim 1, It is characterized in that There is at least one of the following ratio relationships between the components of the base glass: Al 2 O 3 The molar percentage of Y 2 O 3 The molar percentage ratio is 0.2 to 7.5; Y 2 O 3 The molar percentage of Al 2 O 3 The sum of the molar percentages is 7% to 45%; Y 2 O 3 The molar percentage of Li 2 The molar percentage ratio of O is 0.33 to 8; and Li 2 The molar percentage of O and Na 2 The molar percentage ratio of O is 0.33-8.

3. The base glass according to claim 1 or 2, It is characterized in that The base glass also includes 0-2% titanium dioxide (TiO 2 ).

4. The base glass according to claim 3, It is characterized in that ZrO 2 、TiO 2 and P 2 O 5 The total molar percentage is 2% to 6%.

5. The base glass according to claim 3 or 4, It is characterized in that Y 2 O 3 The molar percentage of ZrO 2 +TiO 2 +P 2 O 5 The total mole percentage ratio is 0.5-25.

6. The base glass according to any one of claims 1 to 5, It is characterized in that The base glass further comprises the following components in terms of molar percentage: magnesium oxide (MgO): 0% to 2%; cerium oxide (CeO 2 ): 0.1% to 0.5%; Antimony trioxide (Sb 2 O 3 ):0.1%~0.5%.

7. A glass-ceramic, It is characterized in that The microcrystalline glass is obtained by crystallizing the base glass according to any one of claims 1 to 6 through heat treatment, and the main crystalline phase of the microcrystalline glass includes Y y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5y and ZrO 2 One or more composite crystalline phases.

8. The glass-ceramic according to claim 7, It is characterized in that The main crystalline phase of the microcrystalline glass includes Y y Zr x O 1.5y+2x and Zr x Y y O 2x+1.5y One or two composite crystal phases.

9. The glass-ceramic according to claim 7 or 8, It is characterized in that The crystal phase of the microcrystalline glass also includes ZnAl 2 O 4 , spodumene and one or more composite crystal phases of quartz solid solution.

10. The glass-ceramic according to any one of claims 7 to 9, It is characterized in that The crystallinity of the main crystalline phase is 5% to 90%, and the average crystal size of the main crystalline phase is less than or equal to 100 nm.

11. The glass-ceramic according to any one of claims 7 to 10, It is characterized in that The Young's modulus of the glass-ceramics is greater than or equal to 90 GPa; The microhardness of the microcrystalline glass under the action of 0.2Kgf is greater than or equal to 700Hv.

12. The glass-ceramic according to any one of claims 7 to 11, It is characterized in that The transmittance of the microcrystalline glass at 550 nm in the visible light region is greater than or equal to 88%.

13. The glass-ceramic according to any one of claims 7 to 12, It is characterized in that The glass-ceramics may be subjected to chemical ion strengthening treatment.

14. The glass-ceramic according to claim 13, It is characterized in that After the microcrystalline glass is subjected to the chemical ion strengthening treatment, the ion exchange stress layer depth DOC is greater than or equal to 90 μm; The surface compressive stress Cs50 is greater than or equal to 100MPa; The surface compressive stress value Cs is greater than or equal to 260MPa; The average tensile stress is greater than or equal to 60Mpa; The microcrystalline glass subjected to the chemical ion strengthening treatment has a microhardness greater than or equal to 780 Hv under the action of 0.2 Kgf.

15. The glass-ceramic according to claim 13 or 14, It is characterized in that The microcrystalline glass that has been subjected to the chemical ion strengthening treatment has a 0.7 mm thick sample, under an impact energy condition of greater than or equal to 0.2 J, a four-point bending strength greater than or equal to 600 MPa.

16. The glass-ceramic according to any one of claims 7 to 15, It is characterized in that The glass transition temperature of the microcrystalline glass is greater than or equal to 560°C.

17. A method for preparing glass-ceramics, It is characterized in that include: The batch materials corresponding to the chemical composition of the basic glass are melted, formed, and annealed to obtain the basic glass, wherein the basic glass comprises the following components in terms of molar percentage: Yttrium trioxide (Y 2 O 3 ): 4% to 15%; Aluminum oxide (Al 2 O 3 ): 3% to 30%; Silicon dioxide (SiO2): 40% to 75%; Zirconium dioxide (ZrO 2 ): 0.5%~4%; Lithium oxide (Li 2 O): 3% to 12%; Sodium oxide (Na 2 O): 1.5% to 9%; Phosphorus pentoxide (P 2 O 5 ): 0.1%~2%; Zinc oxide (ZnO) 1% to 8%; and The base glass is subjected to heat treatment and crystallization to obtain the microcrystalline glass.

18. The method for preparing glass-ceramics according to claim 17, It is characterized in that The heat treatment comprises a first heat treatment and a second heat treatment performed sequentially, wherein: The heat treatment temperature of the first step heat treatment is 600-720°C, and the heat treatment time is 0.5-40h; The heat treatment temperature of the second step heat treatment is 730-850° C., and the heat treatment time is 0.5-8 hours.

19. The method for preparing glass-ceramics according to claim 17 or 18, It is characterized in that After the step of obtaining the glass-ceramics, the preparation method further comprises: The glass-ceramics is subjected to chemical ion strengthening treatment.

20. The method for preparing glass-ceramics according to claim 19, It is characterized in that The chemical ion strengthening treatment includes at least one ion exchange, wherein the ion exchange is performed in a metal molten salt containing at least one of sodium ions, potassium ions and lithium ions.

21. The method for preparing glass-ceramics according to claim 20, It is characterized in that The chemical ion strengthening treatment includes a first ion exchange and a second ion exchange, wherein: The metal molten salt of the first ion exchange comprises sodium nitrate, potassium nitrate and lithium nitrate, the exchange temperature is 430° C. to 530° C., and the exchange time is 4 h to 12 h; The metal molten salt for the second ion exchange comprises sodium nitrate, potassium nitrate and lithium nitrate, the exchange temperature is 400° C. to 500° C., and the exchange time is 0.5 h to 5 h.

22. The method for preparing glass-ceramics according to any one of claims 17 to 21, It is characterized in that The melting temperature of the batch material corresponding to the basic glass chemical composition is 1500°C to 1650°C.

23. The method for preparing glass-ceramics according to any one of claims 17 to 22, It is characterized in that The main crystalline phase of the microcrystalline glass includes Y y Zr x O 1.5y+2x 、Zr x Y y O 2x+1.5y and ZrO 2 One or more composite crystalline phases.

24. The method for preparing glass-ceramics according to claim 23, It is characterized in that The main crystalline phase of the microcrystalline glass comprises Y y Zr x O 1.5y+2x and Zr x Y y O 2x+1.5y One or two composite crystal phases.

25. The method for preparing glass-ceramics according to any one of claims 17 to 24, It is characterized in that There is at least one of the following ratio relationships between the components of the base glass: Al 2 O 3 The molar percentage of Y 2 O 3 The molar percentage ratio is 0.2 to 7.5; Y 2 O 3 The molar percentage of Al 2 O 3 The sum of the molar percentages is 7% to 45%; Y 2 O 3 The molar percentage of Li 2 The molar percentage ratio of O is 0.33 to 8; and Li 2 The molar percentage of O and Na 2 The molar percentage ratio of O is 0.33-8.

26. The method for preparing glass-ceramics according to any one of claims 17 to 25, It is characterized in that The base glass also includes 0-2% titanium dioxide (TiO 2 ).

27. The method for preparing glass-ceramics according to claim 26, It is characterized in that ZrO 2 、TiO 2 and P 2 O 5 The total molar percentage is 2% to 6%.

28. The method for preparing glass-ceramics according to claim 26 or 27, It is characterized in that Y 2 O 3 The molar percentage of ZrO 2 +TiO 2 +P 2 O 5 The molar percentage ratio is 0.5-25.

29. A glass product, It is characterized in that The glass product is made of the base glass as described in any one of claims 1 to 7, or is made of the microcrystalline glass as described in any one of claims 8 to 16, or is made of microcrystalline glass prepared by the method for preparing microcrystalline glass as described in any one of claims 17 to 28.

30. The glass article according to claim 29, It is characterized in that The glass product is a glass cover plate.

31. A terminal device, It is characterized in that Comprising the glass product according to claim 29 or 30.

Citation Information

Patent Citations

  • Low-temperature crystallized glass ceramic capable of achieving ion exchange

    CN110104954A

  • Rare earth doped tempered glass ceramic and preparation method and application thereof

    CN111087175A

  • Glass ceramics and glass ceramic articles having spinel crystalline phases

    CN111908793A

  • Chemically strengthened glass and microcrystalline glass, and methods for producing same

    CN114728838A