Positive active material and application thereof

By introducing specific peaks I and peak II, lithium-cobalt molar ratio and particle size distribution, as well as lithium, oxygen, and selenium coating layers into the lithium-ion battery cathode active material, the problem of structural collapse of the cathode active material under high pressure conditions is solved. Significantly improve the capacity and cycle performance of lithium-ion batteries.

WO2024217207A1PCT designated stage expired Publication Date: 2024-10-24ZHUHAI COSMX BATTERY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082354
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-03-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode active materials are prone to crystal structure collapse under high-pressure conditions, resulting in rapid capacity fading and reduced cycle performance, making it difficult to meet high capacity requirements.

Method used

Develop a new cathode active material with specific peaks I and peaks II in its The surface of some particles is covered with lithium, oxygen and selenium elements, forming excellent specific capacity and pressure resistance.

Benefits of technology

The material maintains structural stability under high voltage conditions of 4.5V and above, improves the deintercalation efficiency of lithium ions, significantly improves the capacity and cycle performance of lithium-ion batteries, and the first charge and discharge efficiency reaches 97% to 103%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082354_24102024_PF_FP_ABST
    Figure CN2024082354_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A positive active material and an application thereof. A peak I and a peak II, either of which have 2θ ranging from 17.8° to 19.5°, are present in an X-ray diffraction pattern of the positive active material. The positive active material is special for improving the capacity, energy density and cycling performance of a battery.
Need to check novelty before this filing date? Find Prior Art

Description

A positive electrode active material and its application

[0001] This application claims priority to two Chinese patent applications filed with the China Patent Office on April 18, 2023, with application number 202310420121.0 and application name “A positive electrode active material and its application”, and two Chinese patent applications filed with the China Patent Office on April 18, 2023, with application number 202310420146.0 and application name “A positive electrode active material and its application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to a pole piece material, in particular to a positive electrode active material and its application, belonging to the technical field of secondary batteries. Background Art

[0003] With the development and progress of lithium-ion battery technology, higher and higher requirements are placed on its capacity. In the composition of lithium-ion batteries, the capacity of the positive electrode active material plays a vital role in the capacity of lithium-ion batteries.

[0004] To increase the capacity of lithium-ion batteries, the most common method currently is to increase their charge and discharge voltage. However, as the voltage increases, the crystal structure of the positive electrode active material collapses, leading to a series of problems such as rapid capacity decay and a significant decrease in cycle performance.

[0005] Therefore, developing a lithium-ion battery positive electrode active material with high specific capacity is a technical problem to be solved urgently in this field.

[0006] Summary of the Invention

[0007] The present application provides a positive electrode active material, which has a special composition and excellent specific capacity, and its pressure resistance also meets current needs, thereby helping to improve the capacity and cycle performance of the battery.

[0008] The present application provides a positive electrode sheet, which includes the above-mentioned positive electrode active material, thereby helping to improve the capacity and cycle performance of the battery.

[0009] The present application also provides a lithium-ion battery, which includes the above-mentioned positive electrode sheet, so that the lithium-ion battery has excellent performance in terms of capacity and cycle performance.

[0010] The present application provides a positive electrode active material, wherein the X-ray diffraction pattern of the positive electrode active material comprises a peak I and a peak II with 2θ ranging from 17.8° to 19.5°.

[0011] The positive electrode active material as described above, wherein the difference in 2θ between peak II and peak I is 0.92° to 1.12°;

[0012] The lithium-cobalt molar ratio of the positive electrode active material is 0.73-0.99.

[0013] The positive electrode active material as described above, wherein the molar ratio of lithium to cobalt of the positive electrode active material is 0.85 to 0.95.

[0014] The positive electrode active material as described above, wherein D50 of the positive electrode active material is 12 to 18 μm.

[0015] The positive electrode active material as described above, wherein the positive electrode active material comprises first particles and second particles, the D50 of the first particles is 3 to 8 μm, and the D50 of the second particles is 13 to 20 μm.

[0016] The positive electrode active material as described above, wherein, 5%≤m1 / (m1+m2)≤35% Formula A

[0017] m1 is the mass of the first particle, and m2 is the mass of the second particle.

[0018] The positive electrode active material as described above, wherein 15%≤m1 / (m1+m2)≤30% Formula B.

[0019] The positive electrode active material as described above, wherein at least a portion of the outer surface of the positive electrode active material is covered by the coating layer.

[0020] The positive electrode active material as described above, wherein the coating layer includes at least one of lithium, oxygen and selenium.

[0021] The positive electrode active material as described above, wherein the X-ray diffraction pattern of the positive electrode active material further comprises a peak III with 2θ at 17.8° to 19.5°.

[0022] The positive electrode active material as described above, wherein it comprises a first lithium metal oxide represented by Formula 1 and / or Formula 2, a second lithium metal oxide represented by Formula 3, and a third lithium metal oxide represented by Formula 4;

[0023] The first lithium metal oxide is a cubic crystal of Cmca space group and has a 002a peak with a 2θ of 17.8° to 18.2° in an X-ray diffraction pattern;

[0024] The second lithium metal oxide is a cubic R3-m space group and has a 003 peak with a 2θ of 18.7° to 19.2° in an X-ray diffraction pattern;

[0025] The third lithium metal oxide has a space group of P63mc and has a 002b peak with 2θ of 18.4° to 18.65° in the X-ray diffraction pattern; Li

[0028] , x4 ,

[0029] , b3 ,

[0032] , 1-a3-b3 ,

[0027] , 1-y3 ,

[0030] ,

[0031] , y4 , , , 1-y1 , , m-x4-y5 , , , a3 , y3 , y5 , x3 , Na y1 Co 1-a1-b1 M1 b1 M2 a1 O2 Formula 1 Li n2-y2-b2 Na y2 Co<0​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​​The positive electrode active material as described above, wherein the molar ratio of lithium to cobalt of the positive electrode active material is 0.87 to 0.95.

[0033] The positive electrode active material as described above, wherein the ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide is 5 to 25%;

[0034] The total mass of the lithium metal oxide is the total mass of the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide.

[0035] The positive electrode active material as described above, wherein the ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide is 14-20%.

[0036] The positive electrode active material as described above, wherein the first lithium metal oxide comprises particles A and / or particles B, the D50 of particles A is 13 to 20 μm, and the D50 of particles B is 3 to 8 μm;

[0037] The second lithium metal oxide includes particles C and / or particles D, the D50 of particles C is 3 to 8 μm, and the D50 of particles D is 13 to 20 μm;

[0038] The third lithium metal oxide includes particles E and / or particles F, wherein the D50 of the particles E is 3 to 8 μm, and the D50 of the particles F is 13 to 20 μm;

[0039] The positive electrode active material includes at least one of particles A, particles D, and particles F, and includes at least one of particles B, particles C, and particles E.

[0040] The positive electrode active material as described above, wherein 5%≤(m B +m C +m E ) / (m A +m B +m C +m D +m E +m F )≤35% Formula C

[0041] m A 、m B 、m C 、m D 、m E 、m F are the masses of particle A, particle B, particle C, particle D, particle E, and particle F respectively, and m B 、m C 、m E At least one of them is greater than 0.

[0042] The positive electrode active material as described above, wherein 15%≤(m B +m C +m E ) / (m A +m B +m C +m D +m E +m F )≤30% Formula D.

[0043] The positive electrode active material as described above, wherein the volume particle size distribution curve of the positive electrode active material is a bimodal distribution curve.

[0044] The present application also provides a positive electrode sheet, which includes any of the positive electrode active materials described above.

[0045] The present application also provides a battery, which includes any of the above-mentioned positive electrode materials and / or positive electrode sheets.

[0046] The battery as described above, wherein the negative electrode sheet of the battery comprises lithium metal.

[0047] The positive electrode active material of the present application has excellent specific capacity and pressure resistance. Therefore, the lithium-ion battery made from this positive electrode active material not only has excellent capacity, but also does not suffer structural collapse due to poor pressure resistance even under high-voltage conditions of 4.5V and above. This good structural stability can ensure the intercalation and deintercalation of more lithium ions, thereby improving the capacity and cycle performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] FIG1A is a SEM image of the first lithium metal oxide particle 1-1 of the present application;

[0049] FIG2A is a particle size distribution diagram of Example 6A of the present application;

[0050] FIG3A is a SEM image of Example 6A of the present application;

[0051] FIG4A is an XRD pattern of the positive electrode active material of Example 3A of the present application;

[0052] FIG5A is an XRD pattern of the positive electrode active material of Example 15A of the present application;

[0053] FIG6A is a charge and discharge curve of a button cell assembled with the positive electrode active material of Example 1A of the present application.

[0054] FIG1B is an XRD pattern of the first lithium metal oxide B-1 of the present application;

[0055] FIG2B is an XRD pattern of the second lithium metal oxide C-1 of the present application;

[0056] FIG3B is an XRD pattern of the third lithium metal oxide E-1 of the present application;

[0057] FIG4B is a particle size distribution diagram of Example 11B of the present application;

[0058] FIG5B is an XRD pattern of Example 1B of the present application;

[0059] FIG6B is an XRD pattern of Example 3B of the present application;

[0060] FIG7 is an XRD pattern of Example 9B of the present application;

[0061] FIG8 is a charge and discharge curve of a button cell assembled with the positive electrode active material of Example 3B of the present application. DETAILED DESCRIPTION

[0062] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0063] In a first aspect, the present application provides a positive electrode active material, wherein an X-ray diffraction pattern of the positive electrode active material comprises a peak I and a peak II with 2θ ranging from 17.8° to 19.5°.

[0064] X-ray diffraction analysis of the positive electrode active material of the present application shows that the positive electrode active material has two peaks I and II with different 2θ values ​​in the range of 2θ of 17.8° to 19.5°.

[0065] Positive electrode active materials exhibiting Peaks I and II exhibit excellent specific capacity and pressure resistance. Therefore, lithium-ion batteries fabricated from these positive electrode active materials exhibit not only excellent capacity but also, even under high-voltage conditions of 4.5V and above, exhibit no structural collapse due to poor pressure resistance. This excellent structural stability ensures the intercalation and deintercalation of more lithium ions, thereby enhancing the capacity and cycle performance of lithium-ion batteries.

[0066] In one embodiment, the difference in 2θ between Peak II and Peak I is 0.92° to 1.12°; the lithium-cobalt molar ratio of the positive electrode active material is 0.73 to 0.99. The 2θ of Peak II is greater than the 2θ of Peak I, and the difference between the two is 0.92° to 1.12°.

[0067] The above-mentioned lithium-cobalt molar ratio refers to the molar ratio of lithium and cobalt in the positive electrode active material without any charge and discharge treatment;

[0068] Alternatively, the molar ratio of lithium to cobalt in the positive electrode active material of a battery that has only undergone a formation treatment and has not undergone a discharge treatment (not reaching 0% SOC). Specifically, when a battery that has only undergone a formation treatment (without limiting the charging mechanism of the formation treatment) and has not undergone a discharge is discharged at a rate of 0.1C to 3.0V (the final cutoff voltage is in the range of 3.0 to 3.6V), at a potential of 0% SOC, the current lithium-cobalt molar ratio of the positive electrode active material in the positive electrode sheet of the battery is the lithium-cobalt molar ratio of this application;

[0069] Alternatively, the molar ratio of lithium to cobalt in the positive electrode active material after the positive electrode active material is used in a battery and has undergone a formation treatment and a discharge treatment (the discharge treatment refers to a discharge treatment after a maximum of 10 cycles). Specifically, after the formed battery has undergone no more than 10 charge and discharge cycles and is discharged to 3.0V at a 0.1C rate (with a final cutoff voltage in the range of 3.0 to 3.6V), at a potential of 0% SOC, the current lithium-to-cobalt molar ratio of the positive electrode active material in the positive electrode sheet of the battery is the lithium-to-cobalt molar ratio of this application.

[0070] The present application does not limit the method for detecting the lithium-cobalt molar ratio. For example, the positive electrode active material can be detected by an inductively coupled plasma spectrometer (ICP). Alternatively, when detecting the positive electrode active material in the positive electrode sheet, the discharged battery is disassembled and the positive electrode sheet is taken out. The positive electrode sheet is soaked in dimethyl carbonate (DMC) for 1-3 hours or rinsed with DMC, and then naturally dried in a drying room. It is then placed in a muffle furnace and calcined at 300-600° C. for 2-5 hours. After that, the active layer falls off the current collector, and the powder to be detected is obtained after being sieved with 200 mesh. The metal elements in the powder to be detected are then detected by ICP to calculate the lithium-cobalt molar ratio.

[0071] According to the positive electrode active material provided by the present application, it can improve the energy density and cycle performance of lithium-ion batteries, especially under high-voltage conditions. Based on this phenomenon, the inventor analyzed the reasons for the optimization of lithium-ion battery performance and believed that it may be: the positive electrode active material has two diffraction peaks, Peak I and Peak II, and belongs to a layered structure compound. In this application, the angle of diffraction Peak I is lower than that of diffraction Peak II, and the angle difference between the two is within the appropriate range of 0.92° to 1.12°. Therefore, under the premise of ensuring the stability of the positive electrode active material structure, it has a larger interlayer spacing than commercial lithium cobalt oxide, which makes it easier to achieve lithium ion deintercalation. Specifically, during the charge and discharge process, it exhibits better electronic conductivity than existing commercial lithium cobalt oxide at high voltage, which is more conducive to the deintercalation of lithium ions, thereby showing higher capacity and better cycle performance. In addition to improved pressure resistance and specific capacity, the positive electrode active material also has an initial charge and discharge efficiency of 97% to 145%. Specifically, the button battery assembled with lithium metal was charged and discharged at a rate of 0.1C for the first time, with a charge cut-off voltage of 4.5-4.6V and a discharge cut-off voltage of 3.0V. The first charge and discharge efficiency was calculated by the ratio of the first charge capacity (C0) (mAh / g) to the first discharge capacity (D0) (mAh / g).

[0072] This application does not limit the chemical composition of the positive electrode active material.

[0073] For example, it includes at least lithium, sodium and cobalt. More specifically, its chemical formula may be Formula I, or its chemical formula may be Formula II. n1-y1 Na y1 Co 1-a1-b1 M1 b1 M2 a1 O2·DLi x3 Me 1-y3 M y3 O2 Formula I ELi n2-y2-b2 Na y2 Co 1-a2 M1 b2 M2 a2 O2·GLi x3 Me 1-y3 M y3 O2 Formula II

[0074] In Formula I, 0.6 ≤ n1 ≤ 0.8, 0 < y1 ≤ 0.05, 0 ≤ a1 ≤ 0.1, 0 < b1 ≤ 0.1, 0 < b1 / (1 - a1 - b1) < 0.1, 0.95 ≤ x3 ≤ 1.03, 0 ≤ y3 ≤ 0.1, 0 < a3 ≤ 0.2, 0 < b3 ≤ 0.1, M1 is selected from at least one of Te, W, Al, B, P, and K, M2 is a doping element different from M1, M is one or more of Al, Mg, Ti, Zr, Co, Ni, Mn, Y, La, Sr, W, Sc, Z is one or more of Y, La, Mg, Ti, Zr, Ni, Mn, Ce, A > 0, D > 0.

[0075] In Formula II, 0.6 ≤ n2 ≤ 0.8, 0 < y2 ≤ 0.05, 0 ≤ a2 ≤ 0.1, 0 < b2 ≤ 0.02, 0.95 ≤ x3 ≤ 1.03, 0 ≤ y3 ≤ 0.1, 0 < a3 ≤ 0.2, 0 < b3 ≤ 0.1, M1 is selected from at least one of Te, W, Al, B, P, and K, M2 is a doping element different from M1, M is one or more of Al, Mg, Ti, Zr, Co, Ni, Mn, Y, La, Sr, W, Sc, Z is one or more of Y, La, Mg, Ti, Zr, Ni, Mn, Ce, E > 0, G > 0.

[0076] Furthermore, the positive electrode active material of the present application has a lithium-cobalt molar ratio of 0.85 to 0.95. This lithium-cobalt molar ratio helps to further improve the specific capacity of the positive electrode active material and the lithium-ion deintercalation efficiency, thereby significantly improving the capacity and cycle performance of the lithium-ion battery. And the first charge-discharge efficiency of the positive electrode active material with this lithium-cobalt molar ratio is 97% to 103%.

[0077] In addition, when the D50 (particle size when the cumulative volume reaches 50% of the total volume of all positive electrode active materials) of the positive electrode active material of the present application is 12 to 18 μm, it also helps to promote the improvement of the energy density of the lithium-ion battery. The inventor speculates that this may be because the positive electrode active material with this particle size has excellent performance in fluidity and is more likely to form a tightly packed state, thereby improving the energy density of the lithium-ion battery through the tap density of the positive electrode active material.

[0078] Furthermore, the volume particle size distribution curve of the positive electrode active material of the present application is a bimodal distribution curve. The curve characteristics of this bimodal distribution help to achieve the limitation that the D50 of this positive electrode active material is 12 to 18 μm.

[0079] Specifically, after testing the positive electrode active material using a laser particle size analyzer, its volume particle size distribution curve showed a distinct double peak. Even if the positive electrode active material is present in the positive electrode active layer of the positive electrode sheet, the positive electrode sheet can be removed by disassembling the positive electrode active layer, soaking it in dimethyl carbonate (DMC) for 3 hours, air-drying it in a drying room, and then calcining it in a muffle furnace at 300°C for 3 hours. The positive electrode powder can then be separated from the current collector, sieved through a 200-mesh sieve, and subjected to ultrasonication for 2 minutes before testing using a laser particle size analyzer.

[0080] This application does not limit the specific implementation method for achieving the above-mentioned bimodal distribution curve characteristics. For example, limiting the particle size composition of the positive electrode active material can help achieve the bimodal distribution curve characteristics. In one specific embodiment, the positive electrode active material includes first particles and second particles, wherein the first particles have a D50 of 3 to 8 μm and the second particles have a D50 of 13 to 20 μm.

[0081] Furthermore, when the first particle and the second particle meet the requirements of formula A, and further, when the first particle and the second particle meet the requirements of formula B, the positive electrode active material can not only achieve the characteristics of a double-peak curve, but also has excellent performance in terms of compaction density, which is conducive to further improving the energy density and cycle performance of the lithium-ion battery. 5% ≤ m1 / (m1+m2) ≤ 35% Formula A 15% ≤ m1 / (m1+m2) ≤ 30% Formula B

[0082] In formula A and formula B, m1 is the mass of the first particle, and m2 is the mass of the second particle.

[0083] Furthermore, at least a portion of the outer surface of the positive electrode active material is covered by a coating layer. In one embodiment, the coating layer comprises at least one of lithium, oxygen, and selenium. For example, the coating layer is one of a lithium-containing coating layer, an oxide coating layer, and a selenium layer. More specifically, the lithium-containing coating layer is, for example, a LATP coating layer; the oxide coating layer is a metal oxide or non-metal oxide coating layer, such as magnesium oxide or aluminum oxide.

[0084] The present application does not limit the preparation method of the positive electrode active material. In one possible implementation, the positive electrode active material is prepared by a method including the following steps:

[0085] The positive electrode active material is obtained by sintering and / or coating the first lithium metal oxide represented by Formula 1-1 and / or Formula 1-2 and the second lithium metal oxide represented by Formula 1-3; n1-y1 Na y1 Co 1-a1-b1 M1 b1 M2 a1O2 Formula 1-1 Li n2-y2-b2 Na y2 Co 1-a2 M1 b2 M2 a2 O2 Formula 1-2

[0086] In Formula 1-1, 0.6 ≤ n1 ≤ 0.8, 0 < y1 ≤ 0.05, 0 ≤ a1 ≤ 0.1, 0 < b1 ≤ 0.1, 0 < b1 / (1 - a1 - b1) < 0.1; in Formula 1-2, 0.6 ≤ n2 ≤ 0.8, 0 < y2 ≤ 0.05, 0 ≤ a2 ≤ 0.1, 0 < b2 ≤ 0.02; in Formulas 1 and 2, M1 is selected from at least one of Te, W, Al, B, P, and K; M2 is a doping element different from M1;

[0087] Li x3 Me 1-y3 M y3 O2, where Me = Co 1-a3-b3 Al a3 Z b3 Formula 1-3

[0088] In Formula 1-3, M is one or more of Al, Mg, Ti, Zr, Co, Ni, Mn, Y, La, Sr, W, Sc; Z is one or more of Y, La, Mg, Ti, Zr, Ni, Mn, Ce; 0.95 ≤ x3 ≤ 1.03, 0 ≤ y3 ≤ 0.1, 0 < a3 ≤ 0.2, 0 < b3 ≤ 0.1.

[0089] The above first lithium metal oxide has a chemical composition of Formula 1-1 and / or Formula 1-2, that is, the first lithium metal oxide may only include the compound shown in Formula 1-1, may only include the compound shown in Formula 1-2, or may include both the compounds shown in Formula 1-1 and Formula 1-2. In addition, based on the compositions of Formula 1-1 and Formula 1-2, Formula 1-1 and Formula 1-2 may also represent the same compound. Further, in Formula 1-1, M1 is selected from one of Al, W, and / or Te, B, and / or P; in Formula 1-2, M1 is K.

[0090] The above second lithium metal oxide has a chemical composition shown in Formula 1-3.

[0091] It should be noted that this application does not limit the specific quantity of the compounds that satisfy Formulas 1-1, 1-2, and 1-3 above. For example, the first lithium metal oxide that satisfies Formula 1-1 may be one or more compounds with different chemical compositions. Again, for example, the second lithium metal oxide that satisfies Formula 1-3 may be one or more compounds with different chemical compositions.

[0092] The sintering process includes mixing the first lithium metal oxide and the second lithium metal oxide, and then sintering the mixture at a temperature ranging from 150° C. to 350° C. for 5 to 60 minutes to obtain the positive electrode active material of the present application. The present application does not limit the specific equipment for the sintering process; for example, a muffle furnace can be used.

[0093] The coating treatment includes mixing a first lithium metal oxide and a second lithium metal oxide to form a mixture, and then using a coating layer raw material to form a lithium-containing coating layer or an oxide coating layer on the surface of the positive electrode active material by atomic layer vapor deposition (ALD). The lithium-containing coating layer refers to a coating layer including lithium elements, such as an LATP coating layer; the oxide coating layer is a metal oxide or non-metallic oxide coating layer, such as magnesium oxide, aluminum oxide, etc. The thickness of the coating layer is no more than 100nm, preferably no more than 20nm, for example, 2nm, 5nm, 7nm, 10nm, 13nm, 15nm, 18nm, or 20nm.

[0094] More specifically, in one embodiment, when the coating layer is a lithium-containing coating layer, the first lithium metal oxide and the second lithium metal oxide are placed in a reaction chamber of an ALD reaction device, the reaction temperature is controlled, and the lithium source and other coating layer raw materials are introduced into the reaction chamber using an inert gas as a carrier gas, and atomic layer vapor deposition is achieved in an interval pulse manner to form a lithium-containing coating layer.

[0095] Furthermore, the lithium source is an organic lithium compound, such as lithium tert-butoxide, lithium bis(trimethylsilyl)amide, etc.; other coating layer materials refer to materials other than the lithium source for forming a lithium-containing coating layer. For example, when the coating layer is LATP, the other coating layer materials refer to compounds containing aluminum, phosphorus, and titanium, respectively, such as titanium tetrachloride, trimethylphosphine and other organic phosphorus compounds and trimethylaluminum and other organic aluminum compounds.

[0096] In another embodiment, when the coating layer is an oxide, the first lithium metal oxide and the second lithium metal oxide are placed in the reaction chamber of the ALD reaction equipment, the reaction temperature is controlled, and the coating layer raw material is introduced into the reaction chamber using an inert gas as a carrier gas, and atomic layer vapor deposition is achieved in an interval pulse manner to form an oxide coating layer.

[0097] Furthermore, when the oxide coating layer is aluminum oxide, the coating layer raw material is trimethylaluminum; when the oxide coating layer is magnesium oxide, the coating layer raw material is bismuth magnesium, etc.; as long as it can form an oxide coating layer, it can be used as the coating layer raw material of this application, and no examples are listed one by one in this application.

[0098] In the above-mentioned ALD coating treatment, the reaction temperature is 120°C to 350°C, for example, it can be 150°C, 170°C, 180°C, 220°C, 250°C, 270°C, 300°C, 330°C, and 350°C; the number of interval pulses is 20 to 220 times, for example, it can be 30 times, 50 times, 70 times, 90 times, 100 times, 120 times, 140 times, 150 times, 150 times, and 200 times; the inert gas includes argon or nitrogen; the flow rate of the carrier gas is 20-100 mL / min, for example, it can be 20 mL / min, 40 mL / min, 50 mL / min, 80 mL / min, and 100 mL / min.

[0099] Alternatively, the coating process includes mixing the first lithium metal oxide and the second lithium metal oxide, and then sintering the mixture at high temperature using a coating layer raw material to form a positive electrode active material having a selenium coating layer. The thickness of the coating layer is no greater than 100 nm, preferably no greater than 20 nm, and can be, for example, 2 nm, 5 nm, 7 nm, 10 nm, 13 nm, 15 nm, 18 nm, or 20 nm.

[0100] More specifically, the first lithium metal oxide, the second lithium metal oxide and a certain stoichiometric ratio of Se are mixed evenly using a corresponding mixing device, and then placed in a corresponding sintering device (such as a muffle furnace) for sintering to obtain a positive electrode active material with a selenium element coating layer.

[0101] In the above-mentioned coating treatment of the selenium single layer, the mass proportion of Se in the positive electrode active material is not higher than 0.5%; the sintering treatment temperature is 200-350°C, preferably 250-350°C; the sintering treatment time is 5-60 minutes, preferably 25-50 minutes.

[0102] When a positive electrode active material having first particles and second particles is prepared according to the above method, this can be achieved by controlling the D50 of the first lithium metal oxide and the second lithium metal oxide. For example, the first lithium metal oxide and / or the second lithium metal oxide can both include particles with a D50 of 3 to 8 μm and 13 to 20 μm, or one of the first lithium metal oxide and the second lithium metal oxide can include particles with a D50 of 3 to 8 μm and the other can include particles with a D50 of 13 to 20 μm, thereby making the positive electrode active material have the aforementioned first particles and second particles. And the definitions of the above formulas A and B can be achieved by controlling the mass of the above-mentioned various particles of the first lithium metal oxide and / or the second lithium metal oxide. That is, the composition and mass of the above-mentioned various particles of the first lithium metal oxide and / or the second lithium metal oxide are used to define the particle composition of the positive electrode active material and the mass ratio between the particles.

[0103] In a specific embodiment, the ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide can be 5-90%, thereby achieving the above-mentioned lithium-cobalt molar ratio, thereby significantly improving the capacity, first efficiency, and cycle performance of the lithium-ion battery. The total mass of the lithium metal oxide is the total mass of the first lithium metal oxide and the second lithium metal oxide.

[0104] In the positive electrode active material of the present application, the first and second lithium metal oxides may have a single crystal or polycrystalline morphology, with the specific morphology being related to the selection and ratio of the doping elements. Specifically, when polycrystalline, the first and second lithium metal oxides are spherical or quasi-spherical particles; when single crystal, the first and second lithium metal oxides may have whisker-like, flake-like, or other irregular shapes.

[0105] The present application does not limit the preparation method of the first lithium metal oxide. In one embodiment, a cobalt source, a sodium source, an M1 source, and an M2 source are mixed in a target ratio and then calcined (700-900°C for 8-50 hours) to obtain an oxide containing sodium, cobalt, M1, and M2. This oxide is then mixed with a lithium source and heat-treated (at 80-300°C for no more than 10 hours) to obtain the first lithium metal oxide.

[0106] The present application does not limit the specific selection of cobalt source, sodium source, M1 source and M2 source. For example, the cobalt source is selected from one or more of cobalt hydroxide, cobalt trioxide, doped cobalt trioxide, cobaltous oxide, cobalt oxyhydroxide, cobalt nitrate, cobalt sulfate, etc.; the sodium source is selected from one or more of sodium carbonate, sodium nitrate, sodium hydroxide, sodium bicarbonate, sodium sulfate, etc.; the M1 source can be an oxide of M1. When M1 is W, the M1 source is, for example, tungstic acid and / or sodium tungstate; when M1 is Te, the M1 source is, for example, telluric acid and / or sodium tellurate; when M1 is Al, the M1 source is, for example, aluminum sulfate. , aluminum nitrate, aluminum hydroxide, etc.; when M1 is B, the M1 source is, for example, boric acid and / or sodium borate, etc.; when M1 is P, the M1 source is, for example, phosphoric acid and / or sodium phosphate, etc.; when M1 is K, the M1 source is, for example, one or more of potassium carbonate, potassium nitrate, potassium hydroxide, potassium bicarbonate, potassium sulfate, etc.; the M2 source can be, for example, an oxide of M2, such as one or more of basic magnesium carbonate, magnesium hydroxide, zirconium oxide, yttrium oxide, lanthanum oxide, lanthanum fluoride, nickel oxide, niobium oxide, etc.

[0107] The present application does not limit the preparation method of the second lithium metal oxide. The second lithium metal oxide is a currently commercialized lithium cobalt oxide material.

[0108] It should be noted that, in one embodiment, when preparing the first lithium metal oxide and the second lithium metal oxide, the particle size of the metal source raw material can be limited to finally obtain the first lithium metal oxide and the second lithium metal oxide having a particle size that meets the expected D50.

[0109] In another embodiment, the X-ray diffraction pattern of the positive electrode active material further has a peak III with 2θ ranging from 17.8° to 19.5°.

[0110] Specifically, the positive electrode active material includes a first lithium metal oxide represented by Formula 1 and / or Formula 2, a second lithium metal oxide represented by Formula 3, and a third lithium metal oxide represented by Formula 4;

[0111] The first lithium metal oxide has a Cmca space group of the cubic crystal system and has a 002a peak with 2θ ranging from 17.8° to 18.2° in the X-ray diffraction pattern;

[0112] The second lithium metal oxide has a R3-m space group of the cubic crystal system and has a 003 peak with 2θ ranging from 18.7° to 19.2° in the X-ray diffraction pattern;

[0113] The third lithium metal oxide has a P63mc space group and has a 002b peak with 2θ ranging from 18.4° to 18.65° in the X-ray diffraction pattern; Li n1-y1 Na y1 Co 1-a1-b1 M1 b1 M2 a1 O2 Formula 1 Li n2-y2-b2 Na y2 Co 1-a2 M1 b2 M2 a2 O2 Formula 2

[0114] In Formula 1, 0.6 ≤ n1 ≤ 0.8, 0 < y1 ≤ 0.05, 0 ≤ a1 ≤ 0.1, 0 < b1 ≤ 0.1, 0 < b1 / (1 - a1 - b1) < 0.1; in Formula 2, 0.6 ≤ n2 ≤ 0.8, 0 < y2 ≤ 0.05, 0 ≤ a2 ≤ 0.1, 0 < b2 ≤ 0.02; in Formula 1 and Formula 2, M1 is selected from at least one of Te, W, Al, B, P, and K; M2 is a doping element different from M1;

[0115] Li x3 Me 1-y3 M y3 O2, where Me = Co 1-a3-b3 Al a3 Z b3 Formula 3

[0116] In formula 3, M is one or more of Al, Mg, Ti, Zr, Co, Ni, Mn, Y, La, Sr, W, and Sc; Z is one or more of Y, La, Mg, Ti, Zr, Ni, Mn, and Ce; 0.95≤x3≤1.03, 0≤y3≤0.1, 0 <a3≤0.2,0<b3≤0.1; Li m-x4-y5 Na x4 Co 1-y1 M3 y4 M4 y5 O2, Equation 4

[0117] In formula 4, 0.95≤m≤1.03, 0<x4≤0.05, 0≤y4, y5≤0.15, M3 and M4 are each independently selected from one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, and K;

[0118] The D50 of the positive electrode active material is 12 to 18 μm.

[0119] Specifically, the 002a peak is a diffraction peak of the 002 crystal plane of the first lithium metal oxide, the 003 peak is a diffraction peak of the 003 crystal plane of the second lithium metal oxide, and the 002b peak is a diffraction peak of the 002 crystal plane of the third lithium metal oxide. The 002a peak, the 003 peak, and the 002b peak can be understood as one of Peak I, Peak II, and Peak III, respectively.

[0120] In addition to having a cubic Cmca space group and a 002a peak, the first lithium metal oxide in the positive electrode active material of the present application has a chemical composition of Formula 1 and / or Formula 2, that is, the first lithium metal oxide may include only the compound shown in Formula 1, or only the compound shown in Formula 2, or may include both the compounds shown in Formula 1 and Formula 2. In addition, based on the composition of Formula 1 and Formula 2, Formula 1 and Formula 2 may represent the same compound. Further, in Formula 1, M1 is selected from one of Al, W and / or Te, B and / or P; in Formula 2, M1 is K.

[0121] In addition to having a cubic R3-m space group and the aforementioned 003 peak, the second lithium metal oxide in the positive electrode active material of the present application has a chemical composition as shown in Formula 3.

[0122] In addition to having the P63mc space group and the aforementioned 002b peak, the third lithium metal oxide in the positive electrode active material of the present application has a chemical composition of Formula 4.

[0123] It should be noted that the positive electrode active material of the present application needs to include the above-mentioned first lithium metal oxide, second lithium metal oxide and third lithium metal oxide at the same time. In addition, the lithium metal oxide satisfying any chemical formula can be one or more compounds with different compositions. For example, the first lithium metal oxide satisfying Formula 1 can be one or more compounds with different chemical compositions. For example, the third lithium metal oxide satisfying Formula 4 can be one or more compounds with different chemical compositions.

[0124] The positive electrode active material of the present application includes a first lithium metal compound, a second lithium metal compound and a third lithium metal compound. The special matching of the three lithium metal compounds significantly improves the specific capacity and pressure resistance of the positive electrode active material. According to the positive electrode active material provided by the present application, it can improve the capacity and cycle performance of lithium-ion batteries, especially under high-voltage conditions. Based on this phenomenon, the inventor analyzed the reasons for the optimization of lithium-ion battery performance and believed that it may be: the positive electrode active material including the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide of the above-mentioned crystal structure and chemical composition has a more complete layered crystal phase structure with a suitable interlayer spacing. Therefore, on the one hand, it realizes the smooth deintercalation of a large number of lithium ions, and on the other hand, it effectively suppresses the structural collapse that may occur under high pressure, so that the lithium-ion battery ultimately exhibits excellent capacity and cycle performance.

[0125] Furthermore, the D50 (particle size at which the cumulative volume reaches 50% of the total volume of the total positive electrode active material) of the present application's positive electrode active material of 12 to 18 μm also contributes to the improvement of lithium-ion battery capacity. The inventors speculate that this may be due to the excellent fluidity of positive electrode active materials of this particle size, which makes it easier to form a densely packed state, thereby improving the energy density and cycle performance of lithium-ion batteries through the compaction density of the positive electrode active material.

[0126] In addition to improved voltage resistance and specific capacity, the cathode active material also exhibits high initial charge and discharge efficiency. Specifically, a button cell assembled with lithium metal was subjected to an initial 0.1C charge and discharge rate, with a charge cutoff voltage of 4.5-4.6V and a discharge cutoff voltage of 3.0V. The initial charge and discharge efficiency was calculated by the ratio of the initial charge gram capacity (C0) (mAh / g) to the initial discharge gram capacity (D0) (mAh / g).

[0127] When XRD analysis is performed on the positive electrode active material of the present application that meets the above-mentioned requirements, the diffraction data of the positive electrode active material satisfies the following conditions: the intensity of the 003 peak / the intensity of the 002a peak > 1.5, and the 2θ of the 002b peak - the 2θ of the 002a peak > the 2θ of the 003 peak - the 2θ of the 002b peak. The 2θ of the 002a peak is 17.8° to 18.2°, the 2θ of the 002b peak is 18.4° to 18.65°, and the 2θ of the 003 peak is 18.7° to 19.2°.

[0128] The present application does not limit the preparation method of the positive electrode active material, as long as it includes the step of mixing the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide.

[0129] Furthermore, the cathode active material of the present application has a lithium-cobalt molar ratio of 0.87 to 0.95. This lithium-cobalt molar ratio helps further enhance the specific capacity of the cathode active material and the efficiency of lithium ion insertion and extraction, thereby significantly improving the capacity and cycle performance of lithium-ion batteries. The cathode active material with this lithium-cobalt molar ratio has an initial charge and discharge efficiency of 97% to 103%.

[0130] It should be noted that the lithium-cobalt ratio is the lithium-cobalt ratio of the positive electrode material powder;

[0131] Alternatively, the above-mentioned lithium-cobalt molar ratio is the molar ratio of lithium and cobalt in the positive electrode active material of a battery that has only undergone a formation treatment and has not undergone a discharge treatment (not reaching 0% SOC). Specifically, when a battery that has only undergone a formation treatment (without limiting the charging mechanism of the formation treatment) and has not undergone a discharge is discharged at a rate of 0.1C to 3.0V (the final cutoff voltage is in the range of 3.0 to 3.6V), at a potential of 0% SOC, the current lithium-cobalt molar ratio of the positive electrode active material in the positive electrode sheet of the battery is the lithium-cobalt molar ratio described in this application, and the lithium-cobalt molar ratio is 0.87 to 0.95;

[0132] Alternatively, the lithium-cobalt molar ratio is the molar ratio of lithium to cobalt in the positive electrode active material after the positive electrode active material is used in a battery and undergoes a formation treatment and a discharge treatment (the discharge treatment refers to a discharge treatment after a maximum of 10 cycles). Specifically, after the formed battery has undergone no more than 10 charge and discharge cycles and is discharged to 3.0V at a 0.1C rate (the final cutoff voltage is in the range of 3.0 to 3.6V), at a 0% SOC potential, the current lithium-cobalt molar ratio of the positive electrode active material in the positive electrode sheet is the lithium-cobalt molar ratio of this application, and the lithium-cobalt molar ratio is 0.87 to 0.95.

[0133] This application does not limit the detection method of the lithium-cobalt molar ratio. For example, an inductively coupled plasma spectrometer (ICP) test can be used. For example, when detecting the lithium-cobalt molar ratio of the positive electrode active material in a battery that meets the above requirements, the discharged battery is disassembled and the positive electrode sheet is taken out. The positive electrode sheet is soaked in dimethyl carbonate (DMC) for 1-3 hours or rinsed with DMC, and then naturally dried in a drying room. After being calcined in a muffle furnace at 300-600°C for 2-5 hours, the active layer falls off the current collector, and the powder to be tested is obtained after being sieved with 200 mesh. The metal elements in the powder to be tested are then detected by ICP to calculate the lithium-cobalt molar ratio.

[0134] In one specific embodiment, the ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxides is 5-25%, which can achieve the above-mentioned lithium-cobalt molar ratio and thus significantly improve the capacity, first efficiency, and cycle performance of the lithium-ion battery. The total mass of the lithium metal oxides is the total mass of the first lithium metal oxide, the second lithium metal oxide, and the third lithium metal oxide.

[0135] Furthermore, when the ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide is 14-20%, it is beneficial to further reduce the lithium consumption during the charge and discharge process of the lithium-ion battery, thereby further optimizing the cycle performance.

[0136] It should be noted that the first lithium metal oxide, the second lithium metal oxide, and the third lithium metal oxide are mixed in a certain mass ratio to obtain a positive electrode active material. At this time, when the positive electrode active material is tested according to the aforementioned inductively coupled plasma spectrometer (ICP), the obtained value is the initial lithium-cobalt molar ratio of the positive electrode active material (i.e., the lithium-cobalt molar ratio of the positive electrode active material before formation and discharge treatment). Generally, when the initial lithium-cobalt molar ratio is 0.91 to 0.99, and further, when the initial lithium-cobalt molar ratio is 0.935 to 0.98, it is helpful to achieve the aforementioned lithium-cobalt molar ratio of 0.85 to 0.95.

[0137] In the present application, the lithium-cobalt molar ratio is lower than the initial lithium-cobalt molar ratio. The reason for the lithium-cobalt molar ratio being lower than the initial lithium-cobalt molar ratio is that, during charge-discharge applications, the three lithium metal oxides having the aforementioned crystal structures lose some lithium ions as they pass through the negative electrode due to film formation, thereby reducing the molar amount of lithium ions compared to before charge-discharge applications.

[0138] In a specific embodiment, the volume particle size distribution curve of the positive electrode active material of the present application is a bimodal distribution curve. The bimodal distribution curve feature helps to achieve the limitation of D50 of the positive electrode active material to be 12 to 18 μm.

[0139] Specifically, after testing the positive electrode active material using a laser particle size analyzer, its volume particle size distribution curve showed a distinct double peak. Even if the positive electrode active material is present in the positive electrode active layer of the positive electrode sheet, the positive electrode sheet can be removed by disassembling the positive electrode active layer, soaking it in dimethyl carbonate (DMC) for 3 hours, air-drying it in a drying room, and then calcining it in a muffle furnace at 300°C for 3 hours. The positive electrode powder can then be separated from the current collector, sieved through a 200-mesh sieve, and subjected to ultrasonication for 2 minutes before testing using a laser particle size analyzer.

[0140] This application does not limit the specific implementation method for achieving the above-mentioned bimodal distribution curve characteristics. For example, limiting the particle size composition of the positive electrode active material can help achieve this bimodal distribution curve characteristics. In this application, the D50 of the above-mentioned positive electrode active material is controlled by limiting the particle size of each of the first lithium metal oxide, the second lithium metal oxide, and the third lithium metal oxide.

[0141] In a specific embodiment, the first lithium metal oxide includes particles A and / or particles B, the D50 of particles A is 13 to 20 μm, and the D50 of particles B is 3 to 8 μm; the second lithium metal oxide includes particles C and / or particles D, the D50 of particles C is 3 to 8 μm, and the D50 of particles D is 13 to 20 μm; the third lithium metal oxide includes particles E and / or particles F, the D50 of particles E is 3 to 8 μm, and the D50 of particles F is 13 to 20 μm; wherein the positive electrode active material includes at least one of particles A, particles D and particles F, and includes at least one of particles B, particles C and particles E.

[0142] The above “and / or” means that the lithium metal oxide may include only one type of particles, or may include both types of particles. For example, the third lithium metal oxide may include particles E, or particles F, or both particles E and F.

[0143] In detail, when the first lithium metal oxide includes a compound with only one chemical composition, the first lithium metal oxide may include particles A and / or particles B; when the first lithium metal oxide includes two or more compounds with different chemical compositions, the two or more compounds each independently include particles A and / or particles B.

[0144] Similarly, when the second lithium metal oxide includes a compound with only one chemical composition, the second lithium metal oxide may include particles C and / or particles D; when the second lithium metal oxide includes two or more compounds with different chemical compositions, the two or more compounds each independently include particles C and / or particles D.

[0145] When the third lithium metal oxide includes a compound with only one chemical composition, the third lithium metal oxide may include particles E and / or particles F; when the third lithium metal oxide includes two or more compounds with different chemical compositions, the two or more compounds each independently include particles E and / or particles F.

[0146] It should be noted that the positive electrode active material including the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide, each having a different D50, includes at least one of particles A, D and F, and at least at least one of particles B, C and E.

[0147] In the present application, by limiting the particle size of the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide, it is helpful to achieve the bimodal distribution curve characteristics of the positive electrode active material, and further achieve the limitation of D50 to 12 to 18 μm.

[0148] Furthermore, when the mass m of particles A, B, C, D, E, and F is A 、m B 、m C 、m D 、m E 、m F When formula C is satisfied, further, when the mass m of particles A, B, C, D, E, and F is A 、m B 、m C 、m D 、m E 、m F When formula D is satisfied, the positive electrode active material can not only realize the characteristics of the double-peak curve, but also has excellent performance in terms of compaction density, which is conducive to further improving the energy density of lithium-ion batteries. 5%≤(m B +m C +m E ) / (m A +m B +m C +m D +m E +m F )≤35% Formula C 15%≤(m B +m C +m E ) / (m A +m B +m C +m D +m E +m F )≤30% Formula D

[0149] In formula C, the ratio of the total mass of the small D50 particles (particles B, particles C and particles E) of each of the three lithium metal oxides to the total mass of particles A, particles B, particles C, particles D, particles E, and particles F of the three lithium metal oxides is 5% to 35%; in formula D, the ratio of the total mass of the small D50 particles (particles B, particles C and particles E) of each of the three lithium metal oxides to the total mass of particles A, particles B, particles C, particles D, particles E, and particles F of the three lithium metal oxides is 15% to 30%.

[0150] It can be understood that in order to satisfy Formula C and Formula D, the total mass of particles B, particles C, and particles E is greater than 0, and the mass of at least one of particles A, particles D, and particles F is greater than 0.

[0151] Furthermore, at least one of the first, second, and third lithium metal oxides has a core-shell structure. The core-shell structure referred to herein refers to a structure in which one of the first, second, and third lithium metal oxides serves as a core, and at least a portion of the surface of the core is covered by a coating layer. When at least a portion of the surface of any one of the first, second, and third lithium metal oxides is covered by a coating layer, the battery performance is further improved. By providing the coating layer, the positive electrode active material has a core-shell structure comprising a lithium metal oxide core and a coating layer covering the core. The coating layer helps reduce or inhibit side reactions between the lithium metal oxide and the electrolyte. Even when the battery operates under high voltage, a stable interface can still be formed between the lithium metal oxide and the electrolyte, improving the battery's cycle performance by preventing the excessive dissolution of metal ions from the positive electrode active ions and avoiding electrolyte starvation. Furthermore, the inhibition or reduction of side reactions can also reduce gas production within the battery, thereby ensuring battery safety. It should be noted that when at least one of the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide is a core-shell structure, the above-mentioned limitations on the mass of various lithium metal oxides in Formula C and Formula D refer to limitations on the entire core-shell structure.

[0152] The present application does not limit the choice of coating layer material, as long as it can inhibit side reactions and allow normal lithium ion migration. In order to further improve lithium ion conductivity, the coating layer can be made of carbon-containing compounds, fast ion conductors and other materials.

[0153] In the positive electrode active material of the present application, the first and third lithium metal oxides may have a single crystal or polycrystalline morphology, with the specific morphology being related to the selection and ratio of the doping elements. Specifically, when polycrystalline, they are spherical or quasi-spherical particles; when single crystal, they may be whisker-like, flake-like, or any other irregular shape.

[0154] The present application does not limit the preparation method of the positive electrode active material, and it is only necessary to mix the first lithium metal oxide, the second lithium metal oxide, and the third lithium metal oxide.

[0155] The present application does not limit the preparation method of the above-mentioned first lithium metal oxide. In a specific embodiment, the first lithium metal oxide of the present application can be prepared by mixing a sodium metal oxide represented by Formula 1a or 2a with a lithium compound and performing an ion exchange treatment. Na x1 Co 1-a1-b1 M1 b1 M2 a1 [[ID=1V2]]O2 Formula 1a Na x2 Co 1-a2 M1 b2 M2 a1 O2 Formula 2a

[0156] In Formula 1a, 0.68 < x1 < 0.74, 0 < b1 < 0.1, 0 ≤ a < 0.10, 0 < b1 / (1 - a1) < 0.05; in Formula 2a, 0.68 < x2 < 0.74, 0 < b2 < 0.02, 0 ≤ a2 < 0.1.

[0157] The above ion exchange treatment is a heat treatment process, specifically referring to heat-treating the mixture of the sodium metal oxide and the lithium compound at 80°C to 300°C for no more than 10 hours. After the ion exchange treatment, the ion-exchanged system is washed and dried to finally obtain lithium metal oxides 1 and 2. Among them, the drying temperature is 80 to 180°C, and the time is at least 10 hours. There is no limitation on the equipment for ion exchange treatment and the drying equipment. For example, the equipment for ion exchange treatment can be a closed container equipment with a closed function and stirring ability, or a baking or sintering furnace with a heating function, such as a wet coating reaction equipment, a coprecipitation reaction equipment, a muffle furnace, a box furnace, a tray dryer, etc.; the drying equipment can be a blast oven, a vacuum drying oven, a rotary kiln, a tray dryer, an oven, etc.

[0158] The above lithium compound can be a commonly used lithium source compound in the art, such as at least one of lithium carbonate, lithium chloride, lithium bromide, lithium iodide, lithium nitrate, lithium hydroxide, and lithium fluoride.

[0159] Furthermore, when a positive electrode active material with a coating layer covering the lithium metal oxide needs to be prepared, in the ion exchange treatment, in addition to the raw materials of the sodium metal oxide and the lithium compound, a coating layer raw material needs to be added.

[0160] For the sodium metal compound represented by Formula 1a or Formula 2a, exemplarily, it can be prepared by a method including the following process:

[0161] The cobalt source, the sodium source, the M1 source, and the M2 source are mixed in a target ratio and then calcined to obtain a sodium metal compound represented by Formula 1a or Formula 2a.

[0162] Specifically, the calcination temperature is 700-900°C for 8-50 hours, and the calcination can be carried out in an oxygen or air atmosphere. The calcination equipment can be, for example, a muffle furnace, a tunnel furnace, a roller kiln, a tubular furnace, or other high-temperature sintering equipment.

[0163] Mixing of the above-mentioned sources can be performed using high-speed mixers, sand mills, ball mills, plowshare mixers, inclined mixers, etc. It should be noted that if a sand mill or ball mill is used and a solvent (water, ethanol, or other solvent medium) is added during the ball or sand milling process, the mixed system must be dried after the mixing process. Generally, the mixing time should not exceed 4 hours.

[0164] This application does not limit the specific selection of cobalt source, sodium source, M1 source and M2 source. For example, the cobalt source is selected from one or more of cobalt hydroxide, cobalt trioxide, doped cobalt trioxide, cobaltous oxide, cobalt oxyhydroxide, cobalt nitrate, cobalt sulfate, etc.; the sodium source is selected from one or more of sodium carbonate, sodium nitrate, sodium hydroxide, sodium bicarbonate, sodium sulfate, etc.; the M1 source can be an oxide of M1. When M1 is W, the M1 source is, for example, tungstic acid and / or sodium tungstate; when M1 is Te, the M1 source is, for example, telluric acid and / or sodium tellurate; when M1 is Al, the M1 source is, for example, aluminum sulfate. , aluminum nitrate, aluminum hydroxide, etc.; when M1 is B, the M1 source is, for example, boric acid and / or sodium borate, etc.; when M1 is P, the M1 source is, for example, phosphoric acid and / or sodium phosphate, etc.; when M1 is K, the M1 source is, for example, one or more of potassium carbonate, potassium nitrate, potassium hydroxide, potassium bicarbonate, potassium sulfate, etc.; the M2 source can be, for example, one or more of M2 oxides, such as basic magnesium carbonate, magnesium hydroxide, zirconium oxide, yttrium oxide, lanthanum oxide, lanthanum fluoride, nickel oxide, niobium oxide, etc.

[0165] The present application does not limit the preparation method of the second lithium metal oxide. The second lithium metal oxide is a currently commercialized lithium cobalt oxide material.

[0166] The present application does not limit the preparation method of the third lithium metal oxide. Its preparation method is similar to that of the first lithium metal oxide. The difference is that the ion exchange treatment in the third metal oxide is a heat treatment process, specifically referring to mixing sodium metal oxide and lithium compound and then performing a heat treatment at 80°C to 300°C for no more than 10 hours, which can be carried out in a solution system. After the ion exchange treatment, the ion-exchanged system is washed and dried to finally obtain the third lithium metal oxide. The drying temperature is 80 to 180°C and the time is at least 10 hours.

[0167] It should be noted that, in one embodiment, when preparing the first lithium metal oxide and the third lithium metal oxide, the particle size of the metal source raw material can be limited to finally obtain the first lithium metal oxide and the third lithium metal oxide having a particle size that meets the expected D50.

[0168] A second aspect of the present application provides a positive electrode sheet, which includes the positive electrode active material described in the first aspect.

[0169] Based on the characteristics of the positive electrode active material of the first aspect, the positive electrode sheet of the present application helps to improve the cycle performance and capacity of the lithium-ion battery.

[0170] The present application does not limit the specific structure of the positive electrode sheet. For example, the positive electrode sheet of the present application includes a positive electrode current collector and a positive electrode active layer provided on at least one surface of the positive electrode current collector, and the positive electrode active layer includes the aforementioned positive electrode active material. It can be understood that in addition to the positive electrode active material, the positive electrode active layer also includes a conductive agent and a binder. Exemplarily, the positive electrode active layer includes 70-99wt% of the positive electrode active material, 0.5-15wt% of the conductive agent, and 0.5-15wt% of the binder in terms of mass percentage. Further, it includes 80-98wt% of the positive electrode active material, 1-10wt% of the conductive agent, and 1-10wt% of the binder.

[0171] The conductive agent and the binder are not particularly limited and may be conventionally selected in the art. For example, the conductive agent may be selected from at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, single-walled carbon nanotubes, multi-arm carbon nanotubes, and carbon fibers; and the binder may be selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyacrylate lithium (PAALi).

[0172] Furthermore, to enhance safety, a safety layer can be placed between the positive electrode active layer and the current collector. The safety layer is typically made of a non-conductive safety material, such as an iron-containing compound (e.g., lithium iron phosphate, lithium phosphate), or an aluminum-containing compound (e.g., ceramic alumina). The safety layer also includes a binder, and the ratio of binder to safety material can be determined based on specific needs.

[0173] In some embodiments of the present application, the compaction density of the positive electrode active layer is greater than or equal to 3.5 g / cm 3 When the battery is heated, the cycle performance and capacity of the battery can be further improved.

[0174] A third aspect of the present application provides a lithium-ion battery, which includes the positive electrode sheet according to the second aspect, and thus has outstanding performance in terms of cycle performance and capacity.

[0175] The present application does not limit the specific structure of the lithium-ion battery, for example, it can be a square shell or a cylindrical battery, etc. In addition to the positive electrode sheet, the lithium-ion battery of the present application also includes a negative electrode sheet, a separator and an electrolyte.

[0176] For example, the electrolyte is a conventional electrolyte known in the art comprising a lithium salt and a solvent, wherein the solvent comprises ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), or fluoroethylene carbonate (FEC). Furthermore, the electrolyte may further comprise an additive represented by formula T, wherein the additive has a mass percentage in the electrolyte of 0.1 to 10%.

[0177] Exemplarily, the negative electrode sheet includes a stacked negative electrode current collector and a negative electrode active layer disposed on one or both sides of the negative electrode current collector. In a specific embodiment, the negative electrode active layer comprises, by weight percentage, 70-99 wt% of a negative electrode active material, 0.5-15 wt% of a conductive agent, and 0.5-15 wt% of a binder. Furthermore, the negative electrode active layer comprises 80-98 wt% of a negative electrode active material, 1-10 wt% of a conductive agent, and 1-10 wt% of a binder. The negative electrode active material is selected from one or more of artificial graphite, natural graphite, hard carbon, mesophase carbon microbeads, lithium titanate, silicon carbon, and silicon monoxide.

[0178] In addition, the negative electrode sheet can also be a lithium metal negative electrode containing lithium metal, thereby facilitating the provision of more lithium sources for the battery. Specifically, when the cobalt molar ratio is 0.73 to 0.935, a negative electrode containing lithium metal is preferred.

[0179] For example, the diaphragm is a material with polypropylene as the base material, or a rubber-coated diaphragm with ceramic coated on one side or both sides.

[0180] The lithium-ion battery of the present application is suitable for high-voltage systems. Specifically, it has excellent energy density and cycle performance at voltages ≥ 4.50 V. Therefore, the lithium-ion battery of the present application, which has good cycle stability and high gram capacity at voltages such as 4.50 V, can meet the demand for lightweight and thin high-end digital products.

[0181] The technical solution of the present application will be further explained below with reference to specific embodiments.

[0182] The preparation method of the first lithium metal oxide particles 1-1 used in the following examples and comparative examples is as follows:

[0183] 1) Weigh 1.536 kg of sodium carbonate powder, 1.599 kg of sodium hydroxide powder, 0.185 kg of boric acid powder, 0.195 kg of phosphoric acid powder, and 7.625 kg of cobalt tetroxide powder, and place them in a high-speed mixing device. Set the mixing program to mix at 300 rpm for 3 minutes, then at 500 rpm for 5 minutes, and then at 1000 rpm for 10 minutes. After taking out the mixture, confirm that there are no small white spots in the mixture, and consider the mixture to be uniform;

[0184] 2) Take about 3 kg of the mixed material and evenly load it into a ceramic crucible in batches. Use a pit muffle furnace with equipment model VBF-1200X for high-temperature sintering. The sintering temperature rise curve is 5 ° C / min. When the temperature is raised to 890 ° C, the constant temperature sintering is carried out for 15 hours. After sintering, the sample is taken out after naturally cooling to room temperature to obtain the sintered cobalt and sodium compound Na 0.69 Co 0.95 B 0.03 P 0.02 O2;

[0185] 3) Weigh 0.162 kg of lithium chloride and 2.114 kg of lithium nitrate particles, add the two lithium compounds into the mixing container, weigh 1 kg of the cobalt and sodium compound Na synthesized in step 2) 0.69 Co 0.95 B 0.03 P 0.02 O2 was poured into a mixing container and initially mixed, and then placed in a muffle furnace for ion exchange at 280°C for 0.5h to obtain a crude product;

[0186] 4) The crude product was filtered and washed with deionized water three times, and then dried in a forced air drying oven at 100° C. for 8 h to obtain the first lithium metal oxide particle 1-1, whose corresponding chemical formula is Li 0.70 Na 0.009 Co 0.95 B 0.03 P 0.02 O2.

[0187] FIG1A is a SEM image of the first lithium metal oxide particle 1-1 of the present application. As can be seen from FIG1A , the particle size of the particle 1-1 is 13 to 20 μm. The actual particle size D50 of the sample tested is 16.8 μm.

[0188] The preparation methods of the first lithium metal oxide particles 1-2 and 1-3 used in the following examples and comparative examples are as follows:

[0189] The preparation method is basically the same as that of particle 1-1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1A and Table 2A.

[0190] The preparation method of the first lithium metal oxide particles 2-1 used in the following examples and comparative examples is as follows:

[0191] 1) Weigh 1.536 kg of sodium carbonate powder, 1.599 kg of sodium hydroxide powder, 0.020 kg of potassium carbonate powder, 0.100 kg of magnesium oxide powder, and 28.773 kg of cobalt nitrate hexahydrate powder, place them in a high-speed mixing device, set the mixing program, mix at 300 rpm for 3 minutes, then at 500 rpm for 5 minutes, and then at 1000 rpm for 10 minutes, then remove the mixture and confirm that there are no small white spots in the mixture, which is considered to be uniform;

[0192] 2) Take about 3 kg of the mixed material and evenly load it into a ceramic crucible in batches. Use a pit-type muffle furnace with an equipment model of VBF-1200X for high-temperature sintering. The sintering temperature rise curve is 5 ° C / min. When the temperature is raised to 800 ° C, the constant temperature sintering is carried out for 15 hours. After sintering, the sample is taken out after naturally cooling to room temperature to obtain the sintered cobalt and sodium compound Na 0.69 K 0.003 Co 0.975 Mg 0.025 O2;

[0193] 3) Weigh 0.643 kg of lithium hydroxide monohydrate and 1.057 kg of lithium nitrate particles, add the two lithium compounds into a mixing container, and weigh 1 kg of the cobalt and sodium compound Na synthesized in step 2). 0.69 K 0.003 Co 0.975 Mg 0.025 O2 was poured into a mixing container and initially mixed, and then placed in a muffle furnace for ion exchange at 280°C for 0.5h to obtain a crude product;

[0194] 4) The crude product was filtered and washed with deionized water three times, and then dried in a forced air drying oven at 100°C for 8 hours to obtain particles 2-1, whose corresponding chemical formula is Li 0.698 Na 0.015 K 0.003 Co 0.975 Mg 0.025 O2.

[0195] The preparation methods of the first lithium metal oxide particles 2-2 and 2-3 used in the following examples and comparative examples are as follows:

[0196] The preparation method is basically the same as that of particle 2-1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1A and Table 2A.

[0197] Table 1A

[0198] Table 2A

[0199] The second lithium metal oxide particles 3-1 used in the following examples and comparative examples (particles 3-1 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (5.8 μm, with the shell material being TiO2) is as follows:

[0200] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.4:1.2:0.2, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control flow rate does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization twice and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0201] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0202] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.4:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1010°C for 12 hours, and then the sintered product was crushed to obtain D 50 Al, Y, and Mg co-doped lithium cobalt oxide (Li) with uniform particle size of 5.8 μm 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2;

[0203] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.2:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles 3-1 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.982 Al 0.012 Mg 0.002 Y 0.002 Ti 0.002 O2, its particle size D 50 It is 5.8μm (the shell thickness is at the nanometer level).

[0204] The second lithium metal oxide particles 3-2 used in the following examples and comparative examples (particles 3-2 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.003 Co 0.983 Al 0.013 Mg 0.003 Ti 0.001 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (with a diameter of 4.7 μm and a shell material of La2O3) is as follows:

[0205] 1) Dissolve CoSO4, Al2(SO4)3, and Mg(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Mg=98.3:1.3:0.3, and the Co in the mixed salt solution is 2+The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control flow rate does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization twice and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Mg;

[0206] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Mg in step 1) uniformly, placing it in a muffle furnace at 750° C. for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0207] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, titanium dioxide was weighed at a molar ratio of Co:Ti=98.3:0.1, and the Al and Mg co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1010°C for 12 hours, and then the sintered product was crushed to obtain D 50 Al, Mg, and Ti co-doped lithium cobalt oxide (Li) with uniform particle size of 4.7 μm 1.003 Co 0.983 Al 0.013 Mg 0.003 Ti 0.001 O2;

[0208] 4) Lanthanum trioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:La=98.1:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles 3-2 having a core-shell structure, the chemical formula of which is Li 1.003 Co 0.981 Al 0.013 Mg 0.003 Ti 0.001 La 0.002 O2, its particle size D 50 It is 4.7 μm (the shell thickness is at the nanometer level).

[0209] The second lithium metal oxide particles 4-1 used in the following examples and comparative examples (particles 4-1 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (17.1 μm, with the shell material being TiO2) is as follows:

[0210] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.4:1.2:0.2, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control speed does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization 5 times and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0211] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0212] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.4:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1070°C for 12 hours, and then the sintered product was crushed to obtain D 50 17.1μm particles with uniform distribution of Al, Y, and Mg co-doped lithium cobalt oxide Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2;

[0213] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.2:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles 4-1 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.982 Al 0.012 Mg 0.002 Y 0.002 Ti 0.002 O2, its particle size D 50 It is 17.1 μm (the shell thickness is at the nanometer level).

[0214] The second lithium metal oxide particles 4-2 used in the following examples and comparative examples (particles 4-2 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.983 Al 0.012 Mg 0.002 Y 0.003 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (17.7 μm, with the shell material being TiO2) is as follows:

[0215] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.3:1.2:0.3, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control speed does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization 5 times and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0216] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0217] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.3:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1070°C for 12 hours, and then the sintered product was crushed to obtain D 50 17.7μm particles with uniform distribution of Al, Y, and Mg co-doped lithium cobalt oxide Li 1.0025 Co 0.9833 Al 0.012 Mg 0.002 Y 0.003 O2;

[0218] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.1:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles 4-2 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.981 Al 0.012 Mg 0.002 Y 0.003 Ti 0.002 O2, its particle size D 50 It is 17.7 μm (the shell thickness is at the nanometer level).

[0219] Example 1A

[0220] The positive electrode active material of this embodiment was prepared according to the following method:

[0221] 8g of lithium metal oxide 2-1, 10g of lithium metal oxide 1-1, 10g of lithium metal oxide 3-1, and 72g of lithium metal oxide 4-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and considered uniform. The mixed materials were then removed and sintered in a muffle furnace at 200°C for 30 minutes. The D50 (μm) values ​​were measured, and the corresponding results are shown in Table 5A below.

[0222] Examples 2A-16A

[0223] The preparation method of the positive electrode active material of each embodiment is basically the same as that of Example 1A, except that: the selected particles and proportions, the detailed proportions and contents of which are shown in Table 3A below, and their D50 are tested, and the corresponding results are shown in Table 5A below and Figure 2A. In Figure 2A, a bimodal phenomenon can be clearly observed in the particle size distribution diagram of Example 6A, where the first peak appears at 4 to 5 μm and the second peak appears at around 16 to 18 μm. Figure 3A is an SEM image of Example 6A of the present application. It can be seen from Figure 3A that the positive electrode active material includes large particles and small particles, and its D50 is actually tested to be 15.98 μm.

[0224] Example 17A

[0225] The raw materials with the particle size and proportions shown in Table 3A were selected and mixed according to the method of Example 1A. The mixed material was removed and placed in the reaction chamber of an ALD reactor. The reaction temperature was controlled at 290°C. The lithium source, lithium tert-butoxide, and other precursor materials (trimethylaluminum, titanium tetrachloride, and trimethylphosphine) were introduced into the reaction chamber using inert nitrogen as a carrier gas (flow rate of 50 ml / min). Atomic layer vapor deposition (ALVD) was performed on the surface of the material at intervals of 150 pulses, thereby forming a positive electrode active material with a LATP coating layer having a thickness of approximately 10 to 12 nm. The D50 (D50) of the material was measured, and the corresponding results are shown in Table 5A below.

[0226] Example 18A

[0227] The raw materials with the particle size and proportions shown in Table 3A were selected and mixed according to the method of Example 1A. The mixed materials were removed and placed in the reaction chamber of an ALD reactor. The reaction temperature was controlled at 220°C. The precursor materials trimethylaluminum and deionized water were introduced into the reaction chamber using inert nitrogen as a carrier gas (flow rate of 50 ml / min). Atomic layer vapor deposition was performed on the surface of the material at intervals of 150 pulses, thereby forming a positive electrode active material with an Al2O3 coating layer having a thickness of 10 to 12 nm. The D50 value was measured, and the corresponding results are shown in Table 5A below.

[0228] Example 19A

[0229] 8g of lithium metal oxide 2-1, 10g of lithium metal oxide 1-1, 10g of lithium metal oxide 3-1, and 72g of lithium metal oxide 4-1, along with 0.15g of selenium powder (20 nm diameter), were weighed and placed in a high-speed mixing device. The mixing program was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and deemed uniform. The mixture was then placed in a VBF-1200X muffle furnace and sintered at 300°C for 15 minutes to obtain the corresponding positive electrode active material. The D50 value of the material was measured, and the corresponding results are shown in Table 5A below.

[0230] Example 20A

[0231] 18g of lithium metal oxide 2-1 and 82g of lithium metal oxide 3-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and deemed uniform. The mixed materials were then sintered in a muffle furnace at 200°C for 30 minutes. The D50 values ​​were measured, and the corresponding results are shown in Table 5A below.

[0232] Example 21A

[0233] 18g of lithium metal oxide 1-1 and 82g of lithium metal oxide 4-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and deemed uniform. The mixed materials were then sintered in a muffle furnace at 200°C for 30 minutes. The D50 values ​​were measured, and the corresponding results are shown in Table 5A below.

[0234] Example 22A

[0235] 2g of lithium metal oxide 2-1, 16g of lithium metal oxide 1-1, and 82g of lithium metal oxide 4-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and considered uniform. The mixed materials were then sintered in a muffle furnace at 200°C for 30 minutes. The D50 values ​​were measured, and the corresponding results are shown in Table 5A below.

[0236] Example 23A

[0237] 8g of lithium metal oxide 2-1, 10g of lithium metal oxide 1-1, 40g of lithium metal oxide 3-1, and 42g of lithium metal oxide 4-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and considered uniform. The mixed materials were then removed and sintered in a muffle furnace at 200°C for 30 minutes. The D50 values ​​were measured, and the corresponding results are shown in Table 5A below.

[0238] Table 3A

[0239] Comparative Example 1A

[0240] The method for preparing the positive electrode active material of Comparative Example 1A comprises the following steps:

[0241] 20 g of lithium metal oxide 3-1 and 80 g of lithium metal oxide 4-1 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and confirmed to be uniform. The mixed material was then removed and baked in a vacuum oven at 100°C for 24 hours to obtain the positive electrode active material of Comparative Example 1A. The D50 value of the material was tested, and the corresponding results are shown in Table 5A below.

[0242] Comparative Example 2A

[0243] The method for preparing the positive electrode active material of Comparative Example 2A comprises the following steps:

[0244] 20 g of lithium metal oxide 3-2 and 80 g of lithium metal oxide 4-2 were weighed and placed in a high-speed mixing device. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and confirmed to be uniform. The mixed material was then removed and baked in a vacuum oven at 100°C for 24 hours to obtain the positive electrode active material of Comparative Example 2A. The D50 value of the material was tested, and the corresponding results are shown in Table 5A below.

[0245] The preparation method of the first lithium metal oxide particles A-1 used in the following examples and comparative examples is as follows:

[0246] 1) Weigh 1.536 kg of sodium carbonate powder, 1.599 kg of sodium hydroxide powder, 0.185 kg of boric acid powder, 0.195 kg of phosphoric acid powder, and 7.625 kg of cobalt tetroxide powder, and place them in a high-speed mixing device. Set the mixing program to mix at 300 rpm for 3 minutes, then at 500 rpm for 5 minutes, and then at 1000 rpm for 10 minutes. After taking out the mixture, confirm that there are no small white spots in the mixture, and consider the mixture to be uniform;

[0247] 2) Take about 3 kg of the mixed material and evenly load it into a ceramic crucible in batches. Use a pit muffle furnace with equipment model VBF-1200X for high-temperature sintering. The sintering temperature rise curve is 5 ° C / min. When the temperature is raised to 890 ° C, the constant temperature sintering is carried out for 15 hours. After sintering, the sample is taken out after naturally cooling to room temperature to obtain the sintered cobalt and sodium compound Na 0.69 Co 0.95 B 0.03 P 0.02 O2;

[0248] 3) Weigh 0.162 kg of lithium chloride and 2.114 kg of lithium nitrate particles, add the two lithium compounds into the mixing container, weigh 1 kg of the cobalt and sodium compound Na synthesized in step 2) 0.69 Co 0.95 B 0.03 P 0.02 O2 was poured into a mixing container and initially mixed, and then placed in a muffle furnace for ion exchange at 280°C for 0.5h to obtain a crude product;

[0249] 4) The crude product was filtered and washed with deionized water three times, and then dried in a forced air drying oven at 100° C. for 8 h to obtain the first lithium metal oxide particle A-1, which corresponds to the chemical formula Li 0.70 Na 0.009 Co 0.95 B 0.03 P 0.02 O2.

[0250] The preparation method of the first lithium metal oxide particles A-2 used in the following examples and comparative examples is as follows:

[0251] The preparation method of particles A-2 is basically the same as that of particles A-1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1B and Table 2B.

[0252] The preparation method of the first lithium metal oxide particles B-1 used in the following examples and comparative examples is as follows:

[0253] 1) Weigh 1.536 kg of sodium carbonate powder, 1.599 kg of sodium hydroxide powder, 0.020 kg of potassium carbonate powder, 0.100 kg of magnesium oxide powder, and 28.773 kg of cobalt nitrate hexahydrate powder, place them in a high-speed mixing device, set the mixing program, mix at 300 rpm for 3 minutes, then at 500 rpm for 5 minutes, and then at 1000 rpm for 10 minutes, then remove the mixture and confirm that there are no small white spots in the mixture, which is considered to be uniform;

[0254] 2) Take about 3 kg of the mixed material and evenly load it into a ceramic crucible in batches. Use a pit-type muffle furnace with an equipment model of VBF-1200X for high-temperature sintering. The sintering temperature rise curve is 5 ° C / min. When the temperature is raised to 800 ° C, the constant temperature sintering is carried out for 15 hours. After sintering, the sample is taken out after naturally cooling to room temperature to obtain the sintered cobalt and sodium compound Na 0.69 K 0.003 Co 0.975 Mg 0.025 O2;

[0255] 3) Weigh 0.643 kg of lithium hydroxide monohydrate and 1.057 kg of lithium nitrate particles, add the two lithium compounds into a mixing container, and weigh 1 kg of the cobalt and sodium compound Na synthesized in step 2). 0.69 K 0.003 Co 0.975 Mg 0.025 O2 was poured into a mixing container and initially mixed, and then placed in a muffle furnace for ion exchange at 280°C for 0.5h to obtain a crude product;

[0256] 4) The crude product was filtered and washed with deionized water three times, and then dried in a forced air drying oven at 100°C for 8 hours to obtain particles B-1, whose corresponding chemical formula is Li 0.698 Na 0.015 K 0.003 Co 0.975 Mg 0.025 O2.

[0257] FIG1B is an XRD pattern of the first lithium metal oxide B-1 of the present application.

[0258] The preparation method of the first lithium metal oxide particles B-2 used in the following examples and comparative examples is as follows:

[0259] The preparation method of particles B-2 is basically the same as that of particles B-1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1B and Table 2B.

[0260] The second lithium metal oxide particles C-1 used in the following examples and comparative examples (particles C-1 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (5.8 μm, with the shell material being TiO2) is as follows:

[0261] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.4:1.2:0.2, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control flow rate does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization twice and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0262] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0263] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.4:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1010°C for 12 hours, and then the sintered product was crushed to obtain D 50 Al, Y, and Mg co-doped lithium cobalt oxide (Li) with uniform particle size of 5.8 μm 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2;

[0264] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.2:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles C-1 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.982 Al 0.012 Mg 0.002 Y 0.002 Ti 0.002 O2, its particle size D 50 The shell thickness is 5.8 μm (the shell thickness is at the nanometer level). FIG2B is an XRD pattern of the second lithium metal oxide C-1 of the present application.

[0265] The second lithium metal oxide particles C-2 used in the following examples and comparative examples (particles C-2 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.003 Co 0.983 Al 0.013 Mg 0.003 Ti 0.001 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (with a diameter of 4.7 μm and a shell material of La2O3) is as follows:

[0266] 1) Dissolve CoSO4, Al2(SO4)3, and Mg(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Mg=98.3:1.3:0.3, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control flow rate does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization twice and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Mg;

[0267] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Mg in step 1) uniformly, placing it in a muffle furnace at 750° C. for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0268] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, titanium dioxide was weighed at a molar ratio of Co:Ti=98.3:0.1, and the Al and Mg co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1010°C for 12 hours, and then the sintered product was crushed to obtain D 50 Al, Mg, and Ti co-doped lithium cobalt oxide (Li) with uniform particle size of 4.7 μm 1.003 Co 0.983 Al 0.013 Mg 0.003 Ti 0.001 O2;

[0269] 4) Lanthanum trioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:La=98.1:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles C-2 having a core-shell structure, the chemical formula of which is Li 1.003 Co 0.981 Al 0.013 Mg 0.003 Ti 0.001 La 0.002 O2, its particle size D 50 It is 4.7 μm (the shell thickness is at the nanometer level).

[0270] The second lithium metal oxide particles D-1 used in the following examples and comparative examples (particles D-1 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (17.1 μm, with the shell material being TiO2) is as follows:

[0271] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.4:1.2:0.2, and the Co in the mixed salt solution is 2+The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control speed does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization 5 times and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0272] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0273] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.4:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1070°C for 12 hours, and then the sintered product was crushed to obtain D 50 17.1μm particles with uniform distribution of Al, Y, and Mg co-doped lithium cobalt oxide Li 1.0025 Co 0.984 Al 0.012 Mg 0.002 Y 0.002 O2;

[0274] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.2:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles D-1 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.982 Al 0.012 Mg 0.002 Y 0.002 Ti 0.002 O2, its particle size D 50 It is 17.1 μm (the shell thickness is at the nanometer level).

[0275] The second lithium metal oxide particles D-2 used in the following examples and comparative examples (particles D-2 have a core-shell structure, including a core material and a shell material, wherein the chemical composition of the core material is Li 1.0025 Co 0.983 Al 0.012 Mg 0.002 Y 0.003 O2, nuclear material D 50 The preparation method of the nanostructured carbon nanotube (17.7 μm, with the shell material being TiO2) is as follows:

[0276] 1) Dissolve CoSO4, Al2(SO4)3, and Y(NO3)2 in deionized water to prepare a mixed salt solution with a molar ratio of Co:Al:Y=98.3:1.2:0.3, and the Co in the mixed salt solution is 2+ The concentration is 1.25 mol / L; concentrated ammonia water and distilled water are selected in a volume ratio of 1:10 to prepare a complexing agent solution; 1.2 mol / L sodium carbonate solution is selected as a precipitant solution; the precipitant solution of 1 / 3 of its solvent is injected into the reactor, and under strong stirring and inert gas protection, the mixed salt solution, complexing agent solution and precipitant solution are continuously injected into the reactor at the same time by a parallel flow control method to react, the parallel flow control speed does not exceed 200 L / h, and stirring is performed at the same time, the stirring speed does not exceed 300 rpm, and the pH value of the reaction system is controlled to 7-9, and the temperature of the reactor is controlled to 40-70°C during the reaction process; the liquid phase ion concentration of the doping elements Al and Co in the reaction system is monitored in real time during the reaction process; the continuous reaction is repeated for crystallization 5 times and then centrifuged to obtain a co-doped precursor cobalt salt MeCO3 doped with Al and Y;

[0277] 2) stirring and mixing the cobalt salt MeCO3 precursor of the co-doped Al and Y in step 1) uniformly, placing it in a muffle furnace at 750°C for 8 hours, and then crushing the sintered product to obtain an Al and Y co-doped Co3O4 precursor with uniform particle distribution;

[0278] 3) Lithium carbonate was weighed at a molar ratio of Li:Co=103:100, magnesium oxide was weighed at a molar ratio of Co:Mg=98.3:0.2, and the Al and Y co-doped Co3O4 precursor of step 2) was stirred and mixed uniformly, placed in a muffle furnace at 1070°C for 12 hours, and then the sintered product was crushed to obtain D 50 17.7μm particles with uniform distribution of Al, Y, and Mg co-doped lithium cobalt oxide Li 1.0025 Co 0.9833 Al 0.012 Mg 0.002 Y 0.003 O2;

[0279] 4) Titanium dioxide and the lithium cobalt oxide prepared in step 3) were weighed and mixed uniformly in a molar ratio of Co:Ti=98.1:0.2, and the mixture was placed in a muffle furnace at 930°C for 12 hours. The sintered product was then pulverized to obtain particles D-2 having a core-shell structure, the chemical formula of which is Li 1.0025 Co 0.981 Al 0.012 Mg 0.002 Y 0.003 Ti 0.002 O2, its particle size D 50 It is 17.7 μm (the shell thickness is at the nanometer level).

[0280] The preparation method of the third lithium metal oxide particles E-1 used in the following examples and comparative examples is as follows:

[0281] 1) Weigh 1.536 kg of sodium carbonate powder, 1.599 kg of sodium hydroxide powder, 0.024 kg of potassium carbonate powder, 0.080 kg of magnesium oxide powder, and 28.522 kg of cobalt nitrate hexahydrate powder, place them in a high-speed mixing device, mix them at 300 rpm for 3 minutes, then at 500 rpm for 5 minutes, and then at 1000 rpm for 10 minutes, then take out the mixture and confirm that there are no white spots of sodium carbonate in the mixture, which means the mixture is uniform;

[0282] 2) 3 kg of the mixture was placed in a ceramic crucible and sintered at high temperature using a pit-type muffle furnace with a model of VBF-1200X. The sintering temperature was increased by 5 ° C / min. When the temperature was increased to 750 ° C, the mixture was sintered at a constant temperature for 10 h. After the mixture was naturally cooled to room temperature, the sample was taken out to obtain the sintered compound containing cobalt and sodium elements Na 0.69 K 0.0035 Co 0.98 Mg 0.02 O2;

[0283] 3) Add 20L of deionized water, 1.049kg of lithium hydroxide monohydrate and 1.059kg of lithium chloride to the reaction vessel, stir for 5 minutes at a water temperature of 78°C and a rotation speed of 20rpm, and then add 1kg of the cobalt and sodium compound Na obtained in step 2. 0.69 K 0.0035 Co 0.98 Mg 0.02 O2, maintain 78℃, rotation speed 20rpm, and continue the reaction for 18h;

[0284] 4) After the reaction, the reaction product was taken out, filtered and washed with deionized water three times, and then dried in a forced air drying oven at 90°C for 8 hours to obtain particles E-1, whose corresponding chemical formula is Li 0.98 Na0.03 K 0.0035 Co 0.98 Mg 0.02 FIG3B is an XRD pattern of the third lithium metal oxide E-1 of the present application.

[0285] The preparation method of the third lithium metal oxide particles E-2 used in the following examples and comparative examples is as follows:

[0286] The preparation method of the third lithium metal oxide particle E-2 is basically the same as the preparation method of the particle E-1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1B and Table 2B.

[0287] The preparation method of the third lithium metal oxide particles F-1 used in the following examples and comparative examples is as follows:

[0288] The preparation method of particles F-1 is basically the same as that of particles E-1, except that in step 1) different metal sources and different metal source masses are selected, and in step 2) 3 kg of the mixture is put into a ceramic crucible and sintered at high temperature using a pit muffle furnace with equipment model VBF-1200X. The sintering heating curve is 5°C / min, and the temperature is raised to 910°C for constant temperature sintering for 10 hours. After sintering, the sample is taken out after naturally cooling to room temperature to obtain particles F-1.

[0289] The preparation method of the third lithium metal oxide particles F-2 used in the following examples and comparative examples is basically the same as the preparation method of lithium metal oxide F1, except that different metal sources and different metal source masses are selected in step 1). The specific differences are shown in Table 1B and Table 2B.

[0290] Table 1B

[0291] Table 2B

[0292] Example 1B

[0293] The positive electrode active material of this embodiment was prepared according to the following method:

[0294] 17g of Particle B-1, 3g of Particle C-1, 70g of Particle D-1, and 10g of Particle F-1 were weighed and placed in a high-speed mixer. The mixing process was set to 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and considered uniform. The mixed materials were then removed and baked in a vacuum oven at 100°C for 24 hours to obtain the positive electrode active material of Example 1B. D50 was measured, and the results are shown in Table 5B below.

[0295] Examples 2B-15B

[0296] The preparation methods for the positive electrode active materials in each example were essentially the same as those in Example 1B, differing in the types and proportions of lithium metal oxides used. The detailed proportions are shown in Table 3B below. D50 values ​​were measured, with the results shown in Figure 4B and Table 5B. In Figure 4B , the particle size distribution of Example 11B clearly shows a bimodal phenomenon, with the first peak occurring at 4-5 μm and the second peak at approximately 16-18 μm.

[0297] Comparative Example 1B

[0298] The preparation method for the positive electrode active material of Comparative Example 1B was essentially the same as that of Example 1B, except that 20 g of particles B-2 and 80 g of particles D-2 were weighed and placed in a high-speed mixing apparatus. The mixing program was set to mix at 300 rpm for 1 minute, 500 rpm for 2 minutes, and 1000 rpm for 10 minutes. The mixture was then removed and considered uniform. The mixed materials were then removed and baked in a vacuum oven at 100°C for 24 hours to obtain the positive electrode active material of Comparative Example 1B. The D50 values ​​were measured, and the results are shown in Table 5B below.

[0299] Comparative Examples 2B-14B

[0300] The preparation methods for the positive electrode active materials of Comparative Examples 2B-14B were essentially the same as those of Example 1B, with the difference being the composition. The detailed composition is shown in Table 3B below. The D50 values ​​were tested, and the results are shown in Table 5B.

[0301] Table 3B

[0302] Test Example 1

[0303] XRD analysis was performed on the positive electrode active materials in Examples 1A to 23A, Examples 1 to 15B, Comparative Examples 1A to 2A, and Comparative Examples 1 to 14B. The relevant data are shown in Figures 4A, 5A, Table 4A, 5B, 6B, 7, and Table 4B. In Table 4A, 2θ 峰Irepresents the 2θ of peak I, 2θ 峰II Indicates the 2θ of Peak II. 002a represents the intensity of the 002a peak, I 003 Indicates the intensity of the 003 peak, I 003 / 002a Indicates the intensity of the 003 peak / the intensity of the 002a peak, 2θ 002a represents the 2θ of the 002a peak, 2θ 002b represents the 2θ of the 002b peak, 2θ 003 represents the 2θ of the 003 peak.

[0304] Test Example 2

[0305] The positive electrode active materials of Examples 1A to 23A, Examples 1 to 15B, Comparative Examples 1A to 2A, and Comparative Examples 1 to 14B were each fabricated into a positive electrode sheet, which was then assembled with a negative electrode sheet, an electrolyte, and a separator according to the following method to produce a button cell. The method includes:

[0306] Each lithium metal oxide was mixed with conductive carbon black (SP) and PVDF in a weight ratio of 80%:10%:10% to form a positive electrode slurry. This slurry was then coated onto an aluminum foil current collector and roll-pressed to produce a positive electrode sheet. The positive electrode sheet was then punched into a small disc with a diameter of 12 mm using a mold. After drying and weighing, the positive electrode was assembled into a button cell in a glove box under Ar gas, using a 2025 button cell shell, a lithium metal disc as the negative electrode, and a conventional high-voltage lithium cobalt oxide electrolyte.

[0307] After each button cell was left to stand for 4 hours under normal conditions, the first charge and discharge capacity test was carried out. The test conditions were: 0.1C charging to 4.55V, constant voltage charging to 0.025C and then cut off, after standing for 3 minutes, 0.1C discharge to 3.0V. The first charge capacity C0 (mAh / g) and the first discharge capacity D0 (mAh / g) at 4.4-4.55V were recorded respectively. The first efficiency was calculated. The results are shown in Tables 5A and 5B. Figure 6A is the charge and discharge curve of the button cell assembled with the positive active material of Example 1A of the present application. Figure 8 is the charge and discharge curve of the button cell assembled with the positive active material of Example 3B of the present application.

[0308] Test Example 3

[0309] The positive electrode active materials of Examples 1A to 23A, Examples 1 to 15B, Comparative Examples 1A to 2A, and Comparative Examples 1 to 14B are made into positive electrode sheets, which are then assembled with negative electrode sheets, electrolytes, and separators according to the following method to produce lithium-ion batteries. The method includes:

[0310] 1) The positive electrode active materials in the examples and comparative examples were mixed with conductive carbon black and PVDF in a weight ratio of 96%:2%:2% respectively, and a positive electrode slurry was obtained by dispersion. The slurry was coated on an aluminum foil current collector, and the positive electrode compaction density was 4.12 g / cm 3 Roll pressing is performed to prepare a positive electrode sheet;

[0311] 2-1) Artificial graphite, styrene diene rubber (SBR), sodium carboxymethyl cellulose, and conductive carbon black were mixed in a weight ratio of 94%:3%:2%:1%, and the mixture was dispersed in water and mixed using a double planetary mixer to obtain a negative electrode slurry. This slurry was coated onto a copper current collector, followed by roll pressing and drying to obtain negative electrode sheets according to Examples 1A to 13A, Examples 17A to 23A, Examples 1 to 15B, Comparative Examples 1A to 2A, and Comparative Examples 1 to 14B.

[0312] 2-2) Artificial graphite, styrene diene rubber (SBR), sodium carboxymethyl cellulose, and conductive carbon black were mixed in a weight ratio of 94%:3%:2%:1%. The mixture was dispersed in water and mixed using a double planetary mixer to obtain a negative electrode slurry. This slurry was coated onto a copper current collector, followed by roller pressing and drying.

[0313] Subsequently, the surface density of the negative electrode active layer was 0.0728 mg / cm by rolling. 2 The negative electrode sheet of Example 14A was obtained by rolling the negative electrode active layer to a surface density of 0.1139 mg / cm 2 The negative electrode sheet of Example 15A was obtained by rolling the negative electrode active layer to a surface density of 0.1301 mg / cm 2 lithium foil to obtain the negative electrode sheet of Example 16A;

[0314] 3) Assemble the positive electrode sheet, negative electrode sheet and separator into a lithium-ion battery and inject non-aqueous electrolyte.

[0315] Among them, the electrolyte is a conventional electrolyte known in the art, which is mixed in a mass ratio of ethylene carbonate (abbreviated as EC): diethyl carbonate (abbreviated as DEC): propylene carbonate (abbreviated as PC) = 2:5:3, and then 5% of the total mass of the electrolyte is added with fluoroethylene carbonate (abbreviated as FEC), 13% of the total mass of the electrolyte is added with lithium hexafluorophosphate (abbreviated as LiPF6), and the additive shown in formula T, and the content of the additive accounts for 2% of the total content of the electrolyte.

[0316] The capacity retention rate of each lithium-ion battery obtained was tested. The specific test method was as follows: at 25°C, the battery was charged at a constant current of 1C to 4.50V, then charged at a constant voltage of 0.05C to 4.50V, and then discharged at a discharge rate of 1C to 3.0V. This charge and discharge cycle was repeated 500 times. The discharge capacity at the first cycle and the discharge capacity at the 500th cycle were measured. The capacity retention rate Q2 after 500 cycles was calculated according to the following formula. The results are shown in Tables 5A and 5B.

[0317] Capacity retention rate Q2 = (discharge capacity at the 500th cycle) / (discharge capacity at the first cycle) * 100%

[0318] Test Example 4

[0319] The uncycled (formed) lithium-ion battery in Test Example 3 was discharged to 3.0 V at a current of 1 / 10 of the rated capacity, and its voltage was tested to find that its voltage was 3.0-3.6 V. The lithium-ion battery was then disassembled, the positive electrode sheet was removed, and it was soaked in dimethyl carbonate (DMC) for 3 h. After natural drying in a drying room, it was placed in a muffle furnace and calcined at 300° C. for 3 h. After sieving through 200 mesh, a sample powder was obtained. The content of Li and Co elements in the examples and comparative examples was tested using ICP to obtain the lithium-cobalt molar ratio. The results are shown in n1 in Table 5A and n in Table 5B.

[0320] The same method was used to detect the content of Li and Co in the positive electrode active materials of the various examples and comparative examples to obtain the initial lithium-cobalt molar ratio. The results are shown in n2 in Table 5A and n in Table 5B. 初 .

[0321] Table 4A

[0322] Table 5A

[0323] Table 4B

[0324] Table 5B

[0325] According to Table 5A and Table 5B, it can be seen that the positive electrode active material of the present application is beneficial to improving the discharge capacity and cycle performance of lithium-ion batteries.

[0326] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A positive electrode active material, wherein: The X-ray diffraction pattern of the positive electrode active material has peaks I and II with 2θ in the range of 17.8° to 19.5°.

2. The positive electrode active material according to claim 1, wherein The difference in 2θ between peak II and peak I is 0.92° to 1.12°; The lithium-cobalt molar ratio of the positive electrode active material is 0.73 to 0.

99.

3. The positive electrode active material according to claim 1 or 2, wherein The lithium-cobalt molar ratio of the positive electrode active material is 0.85 to 0.

95.

4. The positive electrode active material according to any one of claims 1 to 3, wherein: The D50 of the positive electrode active material is 12 to 18 μm.

5. The positive electrode active material according to any one of claims 1 to 4, wherein The positive electrode active material includes first particles and second particles, the D50 of the first particles is 3 to 8 μm, and the D50 of the second particles is 13 to 20 μm.

6. The positive electrode active material according to claim 5, wherein 5% ≤ m1 / (m1 + m2) ≤ 35% Formula A m1 is the mass of the first particles, and m2 is the mass of the second particles.

7. The positive electrode active material according to claim 5 or 6, wherein 15% ≤ m1 / (m1 + m2) ≤ 30% Formula B.

8. The positive electrode active material according to any one of claims 1 to 7, wherein At least a part of the outer surface of the positive electrode active material is covered by a coating layer.

9. The positive electrode active material according to claim 8, wherein The coating layer includes at least one of lithium element, oxygen element, and selenium element.

10. The positive electrode active material according to claim 1, wherein The X-ray diffraction pattern of the positive electrode active material also has peak III with 2θ in the range of 17.8° to 19.5°.

11. The positive electrode active material according to claim 10, wherein It includes a first lithium metal oxide represented by Formula 1 and / or Formula 2, a second lithium metal oxide represented by Formula 3, and a third lithium metal oxide represented by Formula 4; The first lithium metal oxide has a Cmca space group of cubic crystal system and has a 002a peak with 2θ of 17.8° to 18.2° in the X-ray diffraction pattern; The second lithium metal oxide has an R3-m space group of cubic crystal system and has a 003 peak with 2θ of 18.7° to 19.2° in the X-ray diffraction pattern; The third lithium metal oxide has a P63mc space group and has a 002b peak with 2θ of 18.4° to 18.65° in the X-ray diffraction pattern; Li n1-y1 Na y1 Co 1-a1-b1 M1 b1 M2 a1 O2 Formula 1 Li n2-y2-b2 Na y2 Co 1-a2 M1 b2 M2 a2 O2 Formula 2 In Formula 1, 0.6 ≤ n1 ≤ 0.8, 0 < y1 ≤ 0.05, 0 ≤ a1 ≤ 0.1, 0 < b1 ≤ 0.1, 0 < b1 / (1 - a1 - b1) < 0.1; in Formula 2, 0.6 ≤ n2 ≤ 0.8, 0 < y2 ≤ 0.05, 0 ≤ a2 ≤ 0.1, 0 < b2 ≤ 0.02; in Formula 1 and Formula 2, M1 is selected from at least one of Te, W, Al, B, P, and K; M2 is a doping element different from M1; Li x3 Me 1-y3 M y3 O2, Where Me = Co 1-a3-b3 Al a3 Z b3 Formula 3 In Formula 3, M is one or more of Al, Mg, Ti, Zr, Co, Ni, Mn, Y, La, Sr, W, Sc, Z is one or more of Y, La, Mg, Ti, Zr, Ni, Mn, Ce; 0.95 ≤ x3 ≤ 1.03, 0 ≤ y3 ≤ 0.1, 0 < a3 ≤ 0.2, 0 < b3 ≤ 0.1; Li m-x4-y5 Na x4 Co 1-y1 M3 y4 M4 y5 O2, formula 4 In Formula 4, 0.95 ≤ m ≤ 1.03, 0 < x4 ≤ 0.05, 0 ≤ y4, y5 ≤ 0.15, M3 and M4 are each independently selected from one or more of Al, Mg, Ti, Zr, Ni, Mn, Y, La, Sr, W, Sc, Ce, P, Nb, V, Ta, Te, B, K; The D50 of the positive electrode active material is 12 to 18 μm.

12. The positive electrode active material according to claim 11, wherein The lithium-cobalt molar ratio of the positive electrode active material is 0.87 to 0.

95.

13. The positive electrode active material according to claim 11 or 12, whereinThe ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide is 5 to 25%; The total mass of the lithium metal oxide is the total mass of the first lithium metal oxide, the second lithium metal oxide and the third lithium metal oxide.

14. The positive electrode active material according to claim 13, wherein The ratio of the mass of the first lithium metal oxide to the total mass of the lithium metal oxide is 14-20%.

15. The positive electrode active material according to any one of claims 11 to 14, wherein: The first lithium metal oxide includes particles A and / or particles B, the D50 of particles A is 13 to 20 μm, and the D50 of particles B is 3 to 8 μm; The second lithium metal oxide includes particles C and / or particles D, the D50 of particles C is 3 to 8 μm, and the D50 of particles D is 13 to 20 μm; The third lithium metal oxide includes particles E and / or particles F, the D50 of particles E is 3 to 8 μm, and the D50 of particles F is 13 to 20 μm; The positive electrode active material includes at least one of particles A, particles D and particles F, and includes at least one of particles B, particles C and particles E.

16. The positive electrode active material according to claim 15, wherein 5% ≤ (m B + m C + m E ) / (m A + m B + m C + m D + m E + m F ) ≤ 35% Equation C m A 、m B 、m C 、m D 、m E 、m F are the masses of particle A, particle B, particle C, particle D, particle E, and particle F respectively, and m B 、m C 、m E At least one of is greater than 0.

17. The positive electrode active material according to claim 16, wherein 15% ≤ (m B + m C + m E ) / (m A + m B + m C + m D + m E + m F ) ≤ 30% Formula D 18. The positive electrode active material according to any one of claims 1 to 17, wherein: The volume particle size distribution curve of the positive electrode active material is a bimodal distribution curve.

19. A positive electrode sheet, wherein: The positive electrode sheet comprises the positive electrode active material according to any one of claims 1 to 18.

20. A battery, wherein: The battery comprises the positive electrode material according to any one of claims 1 to 18 and / or the positive electrode sheet according to claim 19.

21. The battery according to claim 20, wherein The negative electrode sheet of the battery includes lithium metal.

Citation Information

Patent Citations

  • Positive electrode active material and application thereof

    CN118825257A

  • Positive electrode active material and application thereof

    CN118825258A

  • Battery, positive electrode active material, positive electrode, method for manufacturing positive electrode active material

    CN103779542A

  • Positive-electrode active material powder, positive electrode containing positive-electrode active material powder, and secondary battery

    CN105940533A

  • Positive electrode active material, electrochemical device, and electronic device

    CN114497525A