Substrate etching method and device
By using a pulse signal-controlled gas supply method in wet etching, the problem of etching unevenness in the deep structure of the substrate is solved, the etching uniformity and material transfer efficiency are improved, and the reliability of the semiconductor device is enhanced.
Patent Information
- Application Number
- PCT/CN2024/082820
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-24
AI Technical Summary
During the wet etching process, the etching unevenness in the deep structure of the substrate results in different concentrations of etching products and reactants at the top and bottom of the deep structure, forming a concentration gradient, which affects the reliability of semiconductor devices.
A gas supply method based on pulse signal control is adopted to generate bubbles in the etching solution and adjust the gas supply period and intermittent period to ensure that key components in the deep structure reach a diffusion balance and improve etching uniformity. The specific method includes that the interval time between adjacent bubbles generated during the gas supply period is less than the time required for key components in the deep structure to reach diffusion equilibrium after the previous bubble is disturbed, and continuously or intermittently supplies gas to the etching solution during the gas supply period, Multiple bubbles are generated to enhance perturbation efficiency.
By rationally controlling the gas supply mode, the etching uniformity in deep structures can be improved, the material transfer efficiency can be enhanced, the accumulation of etching products at the bottom of deep structures can be reduced, the risks of stickback and over-etching can be reduced, and the reliability of semiconductor devices can be improved.
Smart Images

Figure CN2024082820_24102024_PF_FP_ABST
Abstract
Description
Substrate etching method and device Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a substrate etching method and device. Background Art
[0002] Wet etching involves immersing a substrate in an etching solution, which chemically etches the thin film to be removed. Gas is often introduced into the etching solution to create bubbles, improving the etching effect. Currently, the industry is focusing on optimizing the flow rate and distribution of supplied gas to achieve optimal etching rates and uniformity. Improving etching uniformity generally focuses on improving both within-substrate etching uniformity and between-substrate etching uniformity.
[0003] However, when wet etching thin films in deep structures on a substrate, for example, silicon nitride films in deep structures such as narrow gaps, narrow trenches, and / or high-aspect-ratio through-holes formed on the substrate, etching uniformity in the deep structures also becomes a significant factor affecting the reliability of semiconductor devices. Compared to the top of the deep structure, the macroscopic flow and mass transfer efficiency at the bottom of the deep structure decreases, resulting in different concentrations of etching products and etching reactants at the top and bottom of the deep structure, forming a concentration gradient. Furthermore, the greater the aspect ratio of the deep structure, the greater the concentration gradient in the deep structure, which increases the etching differences between different locations in the deep structure, thereby affecting the etching uniformity in the deep structure.
[0004] Therefore, it is necessary to improve wet etching to control the etching uniformity in deep structures.
[0005] Summary of the Invention
[0006] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a substrate etching method and apparatus for solving the problem of uneven etching in deep structures of a substrate in the prior art.
[0007] To achieve the above-mentioned and other related purposes, the present invention provides a substrate etching method, comprising:
[0008] Immersing the substrate in a treatment tank containing an etching solution, wet-etching the substrate with the etching solution, and forming a deep structure on the surface of the substrate;
[0009] Gas is supplied to the etching solution based on a pulse signal to generate bubbles in the etching solution. One pulse time of the pulse signal includes a gas supply period and an intermittent period. The intermittent period depends on the diffusion time required for key components in the deep structure to reach diffusion equilibrium after the gas supply period ends.
[0010] Optionally, the interval time T between adjacent bubbles generated during the gas supply period is gLess than the diffusion time T required for the key components in the deep structure to reach diffusion equilibrium after the previous bubble disturbance in the adjacent bubble d1 .
[0011] Optionally, the gas supply period continuously supplies gas to the etching solution.
[0012] Optionally, the gas supply period intermittently supplies gas to the etching solution based on N sub-pulse signals, each sub-pulse signal generates a bubble, and N is a natural number and N≤10.
[0013] On the other hand, the present invention also provides a substrate etching device, comprising:
[0014] a processing tank for containing an etching solution;
[0015] A holding mechanism, used for holding a substrate and immersing the substrate in an etching solution, wherein a deep structure is formed on a surface of the substrate;
[0016] a gas supply portion, configured to supply gas into the etching solution to generate bubbles to disturb the etching solution; and
[0017] The controller is configured to control the gas supply part to provide gas to the etching solution based on a pulse signal, wherein a pulse time of the pulse signal includes a gas supply period and an intermittent period, and the intermittent period depends on the diffusion time required for the key components in the deep structure to reach diffusion equilibrium after the end of the gas supply period.
[0018] As described above, the present invention provides a substrate etching method and apparatus, which have the following beneficial effects:
[0019] 1) During the wet etching process, gas is supplied to the etching solution in a pulsed manner. One pulse consists of a gas supply period and an intermittent period. The intermittent period is determined based on the diffusion time required for key components in the deep structure to reach diffusion equilibrium after the gas supply period. The disturbance interval of the trench between adjacent gas supply periods is reasonably controlled to regulate the diffusion degree in the trench, thereby improving the etching uniformity in the trench.
[0020] 2) By making the interval between adjacent bubbles generated during the gas supply period shorter than the diffusion time required for key components in the deep structure to reach diffusion equilibrium after the previous bubble disturbance, the disturbance intensity during the gas supply period is enhanced by superposition of multiple bubble disturbances, thereby expanding the range of the convection area in the deep structure and improving the material transfer efficiency in the deep structure;
[0021] 3) A single-bubble pulse mode is used to intermittently supply gas to the etching solution using N sub-pulse signals during the gas supply period. This mode can not only effectively control the generation time of a single bubble, thereby precisely controlling the interval time between adjacent bubbles; it can also use a larger gas flow rate to obtain bubbles with a higher gas velocity, thereby further enhancing the bubble disturbance capability.
[0022] Summary of the Figures
[0023] The features and properties of the present invention are further described by the following examples and accompanying drawings.
[0024] FIG1 is a schematic diagram of a wet etching device.
[0025] FIG2 is a schematic diagram showing a partial structure of a 3D NAND flash memory device having stacked layers and trenches penetrating the stacked layers;
[0026] FIG3 is a schematic diagram showing the change of SiO2 etching rate with the silicon concentration in the reaction system;
[0027] FIG4 is a schematic diagram showing SiO2 back-adhesion and silicon oxide film over-etching in the trench;
[0028] FIG5 is a schematic diagram showing how the subsequent bubble inhibits the diffusion of key components in the groove after the previous bubble disturbs it;
[0029] FIG6 shows a timing diagram of a pulse signal in the first embodiment of the present application;
[0030] FIG7 is a schematic diagram showing the principle of the superposition effect of adjacent bubbles;
[0031] FIG8 shows a timing diagram of a pulse signal in the second embodiment of the present application; and
[0032] FIG9 is a timing diagram showing a pulse signal in another embodiment of the present application.
[0033] Preferred embodiments of the present invention
[0034] The following describes the embodiments of the present invention through specific examples. Those skilled in the art will readily understand the other advantages and benefits of the present invention from the disclosure herein. The present invention may also be implemented or applied through various other specific embodiments, and the details in this specification may be modified or altered based on different viewpoints and applications without departing from the spirit of the present invention.
[0035] Please refer to Figures 1 to 9. It should be noted that the figures provided in this embodiment are merely schematic illustrations of the basic concept of the present invention. Although the figures only show components relevant to the present invention and are not drawn according to the number, shape, and size of components in actual implementation, the shape, number, and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complex.
[0036] The substrate etching method of the present application is suitable for etching a substrate with a deep structure in a wet etching device that performs batch processing. FIG1 shows an exemplary wet etching device (i.e., a substrate etching device) for implementing the substrate etching method of the present application. As shown in FIG1 , the wet etching device 10 includes a processing tank 11 for accommodating an etching solution; a holding mechanism 12 for holding a substrate w and immersing the substrate w in the etching solution; a liquid supply part 13 for supplying an etching solution to the processing tank; a gas supply part 14 for supplying gas to the etching solution to generate bubbles to disturb the etching solution; and a controller 15. The liquid supply part 13 includes a liquid supply line 131 and a liquid nozzle 132. The liquid nozzle 132 is arranged in the processing tank 11 and is located below the substrate W. A liquid regulating valve 133 is arranged on the liquid line 131. The gas supply unit 14 includes a gas supply line 141 and a gas nozzle 142. The gas nozzle 142 is disposed in the processing tank 11 and below the substrate w. A gas regulating valve 143 is disposed on the gas supply line 141. The controller 15 controls the flow rate of gas supplied from the gas supply line 141 to the gas nozzle 142 by controlling the operation of the gas regulating valve 143, and controls the flow rate of liquid supplied from the liquid supply line 131 to the liquid nozzle 132 by controlling the operation of the liquid regulating valve 132.
[0037] In response to the current problem of uneven etching in deep structures of substrates, the present application proposes a substrate etching method, including immersing a substrate w in a processing tank 11 containing an etching solution, and wet etching the substrate w with the etching solution; and during the wet etching process, providing gas to the etching solution based on a pulse signal to generate bubbles in the etching solution. In the present application, with reference to Figure 1, the controller 15 controls the action of the gas regulating valve 143 based on the pulse signal to provide pulse gas to the gas nozzle 142. Among them, a pulse time of the pulse signal includes a gas supply period and an intermittent period, wherein the intermittent period depends on the diffusion time required for the diffusion of the key components in the groove to reach equilibrium after the end of the gas supply period. The specific settings of the pulse signal will be explained later and will not be repeated here. In addition, it should be noted that the key components refer to the main components in the reaction system that affect the etching uniformity, including etching reactants and / or etching products.
[0038] The following will take the wet etching of selectively removing the silicon nitride film in the stack layer using a phosphoric acid solution in the manufacture of 3D NAND flash memory devices as an example to explain in detail the uneven etching phenomenon in the grooves and the causes thereof, so as to better understand the substrate etching method proposed in this application.
[0039] FIG2 exemplifies a partial structure of a 3D NAND flash memory device. As shown in FIG2 , the structure includes a stacked layer 100 formed on a substrate w and a trench 103 extending through the stacked layer 100. The stacked layer 100 is formed from alternatingly deposited silicon nitride films 101 and silicon oxide films 102. In this example, the trench 103 in the stacked layer 100 is a deep structure formed on the substrate w. During the manufacturing process of the 3D NAND flash memory device, the silicon nitride film 101 in the stacked layer 100 needs to be removed. Typically, the substrate is wet-etched with a phosphoric acid solution (etching solution) to selectively remove the silicon nitride film 101 in the stacked layer 100.
[0040] Silicon nitride (Si3N4) can undergo a chemical reaction in phosphoric acid solution as shown in formula (1): Si3N4+H3PD4+H2O→NH4H2PO4+Si(OH)4---------(1)
[0041] Silicon oxide (SiO2) can undergo a chemical reaction in phosphoric acid solution as shown in formula (2):
[0042] The above formula (2) is a reversible reaction. The reaction direction of formula (2) can be controlled by adjusting the silicon concentration (such as Si(OH)4 concentration) in the reaction system. Figure 3 shows a schematic diagram of the change of the SiO2 etching rate with the silicon concentration in the reaction system. As shown in Figure 3, when the silicon concentration is the equilibrium concentration, the reversible reaction of formula (2) reaches equilibrium and the SiO2 etching rate is zero; when the silicon concentration is lower than the equilibrium concentration, the reversible reaction of formula (2) proceeds to the right, the SiO2 etching rate is greater than zero, SiO2 hydrolyzes to form Si(OH)4, and the SiO2 etching reaction occurs; when the silicon concentration is higher than the equilibrium concentration, the reversible reaction of formula (2) proceeds to the left, the SiO2 etching rate is less than zero, Si(OH)4 self-polymerizes to form SiO2, and the SiO2 deposition reaction occurs. In addition, since the silicon concentration has little effect on the Si3N4 etching rate, the etching selectivity of phosphoric acid to silicon nitride and silicon oxide can be controlled by adjusting the silicon concentration in the phosphoric acid solution. Generally, the silicon concentration in the phosphoric acid solution is slightly lower than the equilibrium concentration. Taking a 160° C. phosphoric acid solution as an etching solution as an example, the equilibrium concentration of silicon is 80 ppm. At this time, the process range of the silicon concentration of the phosphoric acid solution is set to about 40 ppm to 70 ppm.
[0043] It can be seen from the above formula (1) that when the silicon nitride film 101 in the trench 103 is etched, an etching product Si(OH)4 is generated. The diffusion efficiency of the etching product Si(OH)4 will affect the silicon concentration distribution in the trench 103. When the silicon concentration in a local area of the trench 103 exceeds the equilibrium concentration, a SiO2 deposition reaction will occur in the local area (in conjunction with reference to chemical formula (2) and Figure 3). The generated SiO2 deposits will adhere to the silicon oxide film 102 and cause SiO2 to stick back. When the silicon concentration in a local area of the trench 103 is lower than the equilibrium concentration, a SiO2 etching reaction will occur in the local area (in conjunction with reference to chemical formula (2) and Figure 3). When the etching amount of the silicon oxide film 102 exceeds the process requirements, the silicon oxide film 102 will be over-etched. The above-mentioned SiO2 sticking back and over-etching of the silicon oxide film 102 are both manifestations of uneven etching in the trench 103, which will affect the performance and reliability of the product and are undesirable. Relatively speaking, the silicon concentration at the top of trench 103 is low, making overetching of silicon oxide film 102 more likely. The silicon concentration at the bottom of trench 103 is high, making SiO2 sticking back more likely. Figure 4, A, shows SiO2 sticking back at the bottom of trench 103, while Figure 4, B, shows overetching of silicon oxide film 102 at the top of trench 103, where silicon nitride film 101 is partially etched.
[0044] The storage capacity of a 3D NAND flash memory device is generally quantified by the number of stacked layers 100. Currently, the stacked layers 100 of 3D NAND flash memory devices include 64, 96, 128, or even more layers. The greater the number of stacked layers 100, the greater the aspect ratio of the trench 103, making material transport in the trench 103 increasingly difficult. This causes Si(OH)4, an etching product of the silicon nitride film 101, to accumulate in the trench 103, especially at the bottom of the trench 103, increasing the risk of SiO2 sticking back in the trench 103. Therefore, as the aspect ratio of the trench 103 increases, the challenge of uniform etching in the trench 103 becomes increasingly greater.
[0045] At present, the common means to improve the etching uniformity in the groove 103 is to continuously supply gas to the phosphoric acid solution to generate continuous bubbles, increase the liquid flow rate on the surface of the substrate w, so as to promote the mass transfer efficiency in the groove 103, and continuously increase the flow rate of the supplied gas as the aspect ratio of the groove 103 increases, in order to obtain better etching uniformity.
[0046] In fact, for trenches 103 with low aspect ratios, bubbles generated by a lower gas flow rate can effectively improve the mass transfer efficiency in the trenches 103. However, for trenches 103 with high aspect ratios, for example, when the aspect ratio of the trenches 103 exceeds 40:1, the bubbles generated by the lower gas flow rate have a weaker effect on promoting the mass transfer efficiency in the trenches 103, especially at the bottom of the trenches 103. The etching product Si(OH)4 accumulates at the bottom of the trenches 103 due to the low mass transfer efficiency, making the risk of SiO2 sticking back at the bottom of the trenches 103 increasingly high. In this case, to overcome the SiO2 sticking back problem at the bottom of the trenches 103, it is indeed possible to increase the gas flow rate to generate bubbles at a faster rate and in greater numbers, thereby enhancing the promoting effect on the mass transfer efficiency in the trenches 103 and reducing the risk of SiO2 sticking back at the bottom of the trenches 103. However, it should be noted that while increasing the gas flow rate can help reduce the silicon concentration at the bottom of the trench 103 and improve SiO2 sticking back at the bottom of the trench 103, a higher gas flow rate can also cause the silicon concentration near the top of the trench 103 to drop too quickly, increasing the risk of over-etching the silicon oxide film 102 at the top of the trench 103. Therefore, in the continuous gas supply mode, as the aspect ratio of the trench 103 continues to increase, simply increasing the gas flow rate cannot effectively solve the problem of uneven etching in the trench 103.
[0047] In addition, in practice, the applicant has also found that the bubble interval time is also an important factor affecting the diffusion of substances in the groove 103. Specifically, if the interval time between adjacent bubbles is less than the time required for the etching product Si(OH)4 in the groove 103 to reach diffusion equilibrium after the disturbance of the previous bubble, the outward diffusion of the etching product Si(OH)4 in the groove 103 may be suppressed.
[0048] For ease of understanding, the above findings are briefly described below with reference to Figure 5. Figure 5 shows positions 1 and 2, as the bubble ascends along the Z-direction. Position 1 approximately represents the location where the bubble approaches groove 103, while position 2 approximately represents the location where the bubble leaves groove 103. Both positions 1 and 2 are within the range where the bubble disturbs groove 103. It should be noted that Figure 5 simplifies the flow field in groove 103 and does not represent the actual flow field in groove 103.
[0049] Figure 5(a) shows the effect of bubble G1 on the flow field in groove 103 when it passes through position 1. Figure 5(b) shows the effect of bubble G1 on the flow field in groove 103 when it passes through position 2. In Figure 5(a), as bubble G1 passes through position 1, it approaches groove 103 and squeezes the etching solution outside groove 103 into the interior of groove 103, causing the flow field in groove 103 to flow from the outside of groove 103 to the inside of groove 103, which facilitates the diffusion of fresh phosphoric acid solution into groove 103. In Figure 5(b), when bubble G1 passes through position 2, bubble G1 leaves groove 103. The inward squeezing effect exerted by bubble G1 on the liquid in groove 103 begins to disappear, and the pressure of the liquid in groove 103 is released, causing the flow field in groove 103 to tend to flow from the inside of groove 103 to the outside of groove 103. The old phosphoric acid solution in groove 103 diffuses outward, which facilitates the diffusion of the etching product Si(OH)4 in groove 103 outward. Therefore, the disturbance of groove 103 by the bubble includes two stages: squeezing the liquid inward and releasing the liquid outward.
[0050] FIG5( c ) shows the effect of bubble G1 passing through position 2 and the subsequent bubble G2 passing through position 1 on the flow field in groove 103. In FIG5( c ), when bubble G1 is at position 2, an outward flow field is generated in groove 103 that is conducive to the diffusion of etching product Si(OH)4 to the outside of groove 103 (as indicated by the solid arrow in FIG5( c )). It takes some time for the etching product Si(OH)4 in groove 103 to reach diffusion equilibrium. If, at this time, the subsequent bubble G2 is already at a position where an inward flow field is generated in groove 103 that is conducive to the diffusion of fresh phosphoric acid solution to the inside of groove 103 (as indicated by the dotted arrow in FIG5( c )), for example, if bubble G2 is at position 1 at this time, then in the area near the opening of groove 103, the inward flow field will hinder the outward flow field, or even force the outward flow field to reverse direction, which will inhibit the diffusion of etching product Si(OH)4 in groove 103 to the outside of groove 103. If the outward diffusion of the etching product Si(OH)4 in the trench 103 is always suppressed, the etching product Si(OH)4 will accumulate in the trench 103, causing the SiO2 sticking back problem. Therefore, the interval between adjacent bubbles should be properly controlled to allow the etching product Si(OH)4 in the trench 103 time to fully diffuse, which is beneficial to improving the replacement efficiency of the etching product Si(OH)4, improving the silicon concentration distribution in the trench 103, and further improving the etching uniformity in the trench 103.
[0051] In view of the above analysis, in the substrate etching method proposed in this application, when the substrate is immersed in an etching solution for wet etching, gas is supplied to the etching solution based on a pulse signal. One pulse of the pulse signal includes a gas supply period and an intermittent period. The intermittent period is determined based on the diffusion time required for the key components in the groove 103 to reach equilibrium after the end of the gas supply period. This allows the disturbance interval of the groove 103 between adjacent gas supply periods to be reasonably controlled, and the diffusion degree in the groove 103 is regulated, thereby improving the etching uniformity in the groove 103. It should be noted that the pulse signal can be applied to the entire process time of the substrate etching, or it can be applied to only a portion of the process time of the substrate etching.
[0052] The following describes a specific embodiment of the substrate etching method proposed in this application using the wet etching method for selectively removing the silicon nitride film 101 in the stack layer 100 using phosphoric acid as an example. The key component that affects etching uniformity is the etching product Si(OH)4.
[0053] (Implementation Method 1)
[0054] FIG6 shows a timing diagram of a pulse signal in the first embodiment of the present application. As shown in FIG6 , a pulse time T of a pulse signal includes a gas supply period t1 and an intermittent period t2. In some embodiments, the gas supply period t1 can be set to 10ms to 1s; the intermittent period t2 can be set to 10ms to 1s. The intermittent period t2 depends on the diffusion time T required to reach diffusion equilibrium in the groove 103 after the gas supply period t1 ends. d2 Preferably, the value of the intermittent period t2 is equal to the diffusion time T d2 Directly proportional, recorded as t2=k*T d2 , where k>0 and is the set value, T d2 is the experimental measurement value or the calculated simulation value, that is, T d2 It can be obtained through experiments or computational simulations.
[0055] During the wet etching of the silicon nitride film 101 in the stack layer 100, k can be set to be no less than 0.5, for example, in the range of 0.5 to 2, or even 0.6 to 1, so that the etching product Si(OH)4 in the trench 103 has sufficient time to diffuse outward between two adjacent gas supply periods t1. This not only allows the disturbance formed in the previous gas supply period t1 to enhance the diffusion of substances in the trench 103, but also prevents the disturbance formed in the next gas supply period t1 from inhibiting the diffusion of substances in the trench 103, thereby ensuring sufficient diffusion of substances in the trench 103, improving the diffusion efficiency in the trench 103, and reducing the silicon concentration gradient in the trench 103. Reducing the silicon concentration gradient not only reduces the silicon concentration in the trench 103, especially at the bottom of the trench 103, thereby suppressing SiO2 sticking back at the bottom of the trench 103, but also increases the silicon concentration at the top of the trench 103, thereby improving over-etching of the silicon oxide film 102 at the top of the trench 103.
[0056] It should be noted that the above-mentioned k value for wet etching of the silicon nitride film 101 in the stack layer 100 is only an example. The setting range of the k value can be reasonably adjusted according to the wet etching object and the actual process conditions. For example, in some wet etching, k may also be set to less than 0.5.
[0057] During gas supply period t1, gas is supplied to the etching solution at a first gas volume, and during intermittent period t2, gas is supplied to the etching solution at a second gas volume. The first gas volume is greater than the second gas volume and is used to generate bubbles in the etching solution, causing disturbances in localized areas of the substrate surface, such as the surface of groove 103, thereby enhancing material transfer in groove 103. The second gas volume can be set to zero or greater than zero, primarily to prevent the etching solution from flowing back into the gas nozzle. The minimum gas flow rate to prevent the etching solution from flowing back into the gas nozzle is defined as the critical gas flow rate, and the second gas volume can be set to be no less than the critical gas flow rate.
[0058] The number of bubbles generated by the gas supplied during the gas supply period t1 in the etching solution is N, where N is a natural number and N≤10. For example, the number of bubbles generated during the gas supply period t1 is 1, 2, 3, or more than 3. All bubbles generated during the gas supply period t1 are recorded as a bubble group, and the interval time T between adjacent bubbles in the bubble group is g It depends on the diffusion time T required for the previous bubble in the adjacent bubble to reach the diffusion equilibrium in the groove 103 after the previous bubble disturbs it. d1 In order to enhance the overall disturbance effect of the bubble group, the interval time between adjacent bubbles is T g It should be less than the diffusion time T required for the previous bubble in the adjacent bubble to reach the diffusion equilibrium in the groove 103 after the previous bubble disturbs it. d1 , that is, T g <T d1 . Preferably, T g =k1*T d1, k1∈(0,0.5). In this way, before the release effect of the previous bubble, which is beneficial to the outward diffusion of the etching products in the groove 103, ends, the squeezing effect of the next bubble, which is detrimental to the outward diffusion of the etching products in the groove 103, begins. As a result, the disturbance effects of adjacent bubbles in the bubble group on the liquid in the groove 103 are superimposed, enhancing the disturbance ability of the etching solution during the gas supply period t1, effectively improving the mass transfer efficiency in the groove 103, and facilitating shortening the etching process time.
[0059] The principle of the superposition of adjacent bubbles is explained below with reference to FIG7. As shown in FIG7(a), when the bubble G1 is at position 1, the bubble G1 squeezes the fresh etching solution outside the groove 103 to flow into the groove 103, and the depth of the disturbance to the liquid in the groove 103 is h1; as shown in FIG7(b), when the bubble G1 moves to position 2, the squeezing force generated by the bubble G1 on the inside of the groove 103 is in a state of being about to be released or not completely released, and the liquid inside the groove 103 tends to flow outward (as shown by the solid arrow in FIG7(b)), that is, the etching products inside the groove 103, such as Si(OH)4, are in the stage of outward diffusion. However, the etching product Si It takes a certain amount of time for (OH)4 to reach diffusion equilibrium. Assuming that the interval between bubbles G1 and G2 is less than the diffusion time required for the etching product Si(OH)4 in the groove 103 to reach diffusion equilibrium after the disturbance by bubble G1, before the etching product Si(OH)4 reaches diffusion equilibrium after the disturbance by bubble G1, bubble G2 has moved to a position where another fresh etching solution outside the groove 103 is squeezed to flow into the groove 103 (as shown by the dotted arrow in Figure 7(b)), for example, position 1. Then, bubble G2 will push the depth of the liquid disturbance in the groove 103 forward to become h2.
[0060] In other words, during the gas supply period t1, it is desirable to reduce the spacing between adjacent bubbles and to superimpose the squeezing effect of multiple bubbles that forces fresh etching solution from the outside of the trench 103 into the interior of the trench 103. This increases the depth of liquid disturbance in the trench 103 as much as possible, thereby increasing the concentration of etching reactants such as H3PO4 in the trench 103, increasing the etching rate of the silicon nitride film 101, and promoting material transfer deep in the trench 103, especially at the bottom of the trench 103, by enhancing the internal disturbance in the trench 103. Ideally, forced convection is formed from the top to the bottom of the trench 103. During the intermittent period t2, it is desirable to have adequate time for the etching products (such as Si(OH)4) inside the trench 103 to diffuse outward.
[0061] 6 , in the first embodiment, the etching solution is continuously supplied with gas during the gas supply period t1 . When the gas is continuously supplied during the gas supply period t1 , the first gas volume is preferably 0.5 L / min to 2 L / min.
[0062] (Implementation Method 2)
[0063] Referring to FIG. 8 , this embodiment provides a substrate etching method. Compared to the first embodiment, the second embodiment differs in that gas supply period t1 intermittently supplies gas to the etching solution based on N sub-pulse signals, each sub-pulse signal corresponding to the generation of one bubble, where N is a natural number and N ≤ 10.
[0064] FIG8 shows a timing diagram of a pulse signal in the second embodiment of the present application. As shown in FIG8 , a pulse time T of a pulse signal includes a gas supply period t1 and a pause period t2. In FIG8 , each gas supply period t1 includes three sub-pulse signals, and each sub-pulse signal has a pulse time t1 and a pause period t2. a The single bubble pulse can effectively control the generation time of a single bubble, thereby precisely controlling the interval between adjacent bubbles. In this example, the pulse time t a It can be approximately considered as the time interval T between adjacent bubbles g The pulse time of the sub-pulse signal can be set to, for example, 10 ms to 100 ms.
[0065] Single-bubble pulses can also utilize a larger gas flow rate to generate higher-speed bubbles, achieving a better disturbance effect on the etching solution through high-speed bubbles. In one example, the gas flow rate supplied to the etching solution by the sub-pulse signal is set to no less than 2 L / min, for example, 2 L / min to 30 L / min, preferably 5 L / min to 20 L / min. Specifically, the gas flow rate supplied to the etching solution by the sub-pulse signal can be set to 2.5 L / min, 3 L / min, 10 L / min, 15 L / min, etc.
[0066] It should be noted that compared with the upper limit of the gas flow rate that can be adopted in the continuous gas supply mode in Implementation Method One, the upper limit of the gas flow rate that can be adopted in the single bubble pulse mode during the gas supply period in Implementation Method Two is larger. This is because when the continuous gas supply mode is adopted during the gas supply period, when the gas flow rate exceeds a certain range, for example, the gas flow rate is 5L / min, the supplied gas may form a gas column in the etching solution that is not conducive to etching.
[0067] It should be noted that the substrate etching method proposed in this application can not only be used to remove the silicon nitride film 101 in the stack layer 100 of the 3D NAND device, but can also be used to remove thin films in deep structures such as logic devices, interconnect structures, fin field effect transistors (FinFETs), 3D semiconductor structures, etc., which have narrow gaps, narrow trenches, and high aspect ratio channels.
[0068] In addition, in the substrate etching method proposed in the present application, the pulse signal can be periodic or non-periodic. Specifically, the duty cycle, frequency, and amplitude of the pulse signal can be fixed or adjusted according to the actual process, wherein the duty cycle refers to the proportion of the gas supply period in a pulse time, and the amplitude corresponds to the gas flow rate supplied. For example, the pulse signals shown in Figures 6 and 8 are periodic, that is, the duty cycle, frequency, amplitude, etc. of each pulse in the pulse signal are the same. For another example, the pulse signal shown in Figure 9 is non-periodic, and the duty cycle of the pulse signal gradually decreases, that is, the proportion of the gas supply period t1 in a pulse time T gradually decreases. It is understandable that when supplying gas to the etching solution with a non-periodic pulse signal, the duty cycle, frequency, amplitude, etc. of the pulse signal can be adjusted to control the number of bubbles generated in different gas supply periods. In addition, Figure 9 is only a specific example of a non-periodic pulse signal. In actual applications, the non-periodic setting of the pulse signal can be reasonably set according to specific process conditions.
[0069] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical principles disclosed herein are intended to be covered by the claims of the present invention.
Claims
1. A substrate etching method, characterized in that: include: Immersing the substrate in a treatment tank containing an etching solution, wet-etching the substrate with the etching solution, and forming a deep structure on the surface of the substrate; Gas is provided to the etching solution based on a pulse signal to generate bubbles in the etching solution. One pulse time of the pulse signal includes a gas supply period and an intermittent period. The intermittent period depends on the diffusion time required for key components in the deep structure to reach diffusion equilibrium after the gas supply period ends.
2. The substrate etching method according to claim 1, characterized in that: The intermittent period is 10ms to 1s.
3. The substrate etching method according to claim 1, characterized in that: The intermittent period is recorded as t2, and the diffusion time required for the key components in the deep structure to reach diffusion equilibrium after the gas supply period ends is recorded as T d2 , t2 is proportional to T d2 , recorded as t2 = k*T d2 , where k>0.
4. The substrate etching method according to claim 3, characterized in that: The k is not less than 0.
5.
5. The substrate etching method according to claim 4, characterized in that: The value range of k is 0.5-2.
6. The substrate etching method according to claim 1, characterized in that: During the gas supply period, gas is supplied to the etching solution in a first gas volume, and during the intermittent period, gas is supplied to the etching solution in a second gas volume, wherein the second gas volume is smaller than the first gas volume.
7. The substrate etching method according to claim 6, characterized in that: The second gas volume is zero.
8. The substrate etching method according to claim 6, characterized in that: The processing tank is provided with a gas nozzle for providing gas to the etching solution to generate bubbles, and the second gas volume is not less than a critical gas flow rate, which refers to the minimum gas flow rate to avoid backflow to the gas nozzle.
9. The substrate etching method according to claim 1, characterized in that: The gas supply period is 10ms to 1s.
10. The substrate etching method according to claim 1, characterized in that: The number of bubbles generated during the gas supply period is N, where N is a natural number and N≤10.
11. The substrate etching method according to claim 10, characterized in that: The interval time T between adjacent bubbles generated during the gas supply period g Less than the diffusion time T required for the key components in the deep structure to reach diffusion equilibrium after the previous bubble disturbance in the adjacent bubble d1 .
12. The substrate etching method according to claim 11, characterized in that: The T g =k1*T d1 , k1∈(0,0.5).
13. The substrate etching method according to claim 10, characterized in that: The gas supply period continuously supplies gas to the etching solution.
14. The substrate etching method according to claim 13, characterized in that: The flow rate of the gas continuously supplied to the etching solution is 0.5L / min to 2L / min.
15. The substrate etching method according to claim 10, characterized in that: The gas supply period intermittently supplies gas to the etching solution based on N sub-pulse signals, each sub-pulse signal generates a bubble, N is a natural number and N≤10.
16. The substrate etching method according to claim 15, characterized in that: The pulse time of each sub-pulse signal is 10ms to 100ms.
17. The substrate etching method according to claim 15, characterized in that: The gas flow rate supplied to the etching solution by the sub-pulse signal is not less than 2 L / min.
18. The substrate etching method according to claim 17, characterized in that: The gas flow rate supplied by the sub-pulse signal to the etching solution is 2L / min to 30L / min.
19. The substrate etching method according to claim 1, characterized in that: The pulse signal is periodic or non-periodic.
20. A substrate etching device, comprising: a processing tank for containing an etching solution; A holding mechanism, used for holding a substrate and immersing the substrate in an etching solution, wherein a deep structure is formed on a surface of the substrate; A gas supply part, used for supplying gas into the etching solution to generate bubbles to disturb the etching solution; as well as The controller is configured to control the gas supply part to provide gas to the etching solution based on a pulse signal, wherein a pulse time of the pulse signal includes a gas supply period and an intermittent period, and the intermittent period depends on the diffusion time required for the key components in the deep structure to reach diffusion equilibrium after the gas supply period ends.
Citation Information
Patent Citations
Apparatus for manufacturing semiconductor device, wet etching process device and wet etching process method
CN101154581A
Manufacture method of roughened silicon substrate, process device thereof and manufacture method of solar cell element
CN103377878A
Technique for BOE corrosion
CN110600374A
Systems and methods for manufacturing elements of photonic devices
CN114223051A
Acid etching method for controlling morphology of silicon wafer
CN114420554A