Lithium-ion battery positive electrode material precursor and preparation method therefor, lithium-ion battery positive electrode material, lithium-ion battery and electric device
By preparing lithium-ion battery cathode material precursors with high regularity and integrity, the problems of structural damage and performance degradation of high-nickel cathode materials are solved, and the cycle performance and capacity retention rate of lithium-ion batteries are improved.
Patent Information
- Application Number
- PCT/CN2024/087550
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-24
AI Technical Summary
High-nickel cathode materials suffer structural damage and performance degradation due to phase changes during the charge and discharge process, resulting in poor cycle performance of lithium-ion batteries, and the poor regularity of existing precursor particles affects battery performance.
A lithium-ion battery cathode material precursor is used, which is a primary particle composed of multiple neatly stacked monolithic layers. By controlling the reaction conditions such as pH and ammonia concentration, a precursor with high regularity and integrity is prepared, reducing the crystal defects and improve cycle performance.
It improves the cycle performance and capacity retention rate of lithium-ion battery cathode materials, reduces side reactions, and enhances the stability and safety of the battery.
Smart Images

Figure CN2024087550_24102024_PF_FP_ABST
Abstract
Description
Lithium-ion battery positive electrode material precursor and preparation method thereof, lithium-ion battery positive electrode material, lithium-ion battery and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 202310429383.3 filed with the State Intellectual Property Office of China on April 20, 2023, entitled “Lithium-ion battery positive electrode material precursor and preparation method thereof, lithium-ion battery positive electrode material, lithium-ion battery and electrical-related equipment,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of lithium-ion batteries, and in particular to a lithium-ion battery positive electrode material precursor and a preparation method thereof, a lithium-ion battery positive electrode material, a lithium-ion battery, and electrical equipment. Background Art
[0004] With the development of energy storage technology, the threshold requirements and cost requirements for energy density per unit volume of lithium battery materials are rapidly increasing. Against this background, positive electrode materials are gradually developing towards high nickel. Although high nickel positive electrode materials have advantages in cost and capacity, high nickel materials also have poor cycle performance and are accompanied by serious performance degradation.
[0005] Studies have shown that the phase change of high-nickel positive electrode materials during the charging and discharging process will cause the volume of the positive electrode material crystal to change, generating anisotropic stress, which is prone to primary cracks within and between crystals and triggering a vicious cycle of diffuse cracks, triggering more side reactions, and finally causing the entire positive electrode material structure to collapse and break, causing serious degradation of battery performance.
[0006] Cathode material precursors are highly customized standard products and are key materials in their production. The characteristics of these precursors directly determine the cathode material's primary physical and chemical properties, including particle size, particle size distribution, the ratio of metal elements other than lithium, and impurity content. These characteristics, in turn, influence the lithium battery's core electrochemical properties, including rate capability, energy density, and cycle life.
[0007] The multiple monolithic layers in the primary particles of high-nickel precursors currently on the market vary widely in shape and size, often fragmented or misplaced, resulting in poor primary particle regularity and a wide distribution of length and width. After sintering into cathode materials, electron micrographs of the secondary particles reveal poor primary particle regularity. While this allows for high capacity due to the high nickel content, the poor primary particle regularity, poor crystallinity, and numerous crystal defects inherent in the material result in poor cycling performance for the sintered cathode material, limiting its full application in lithium-ion batteries.
[0008] Summary of the Invention
[0009] The purpose of this application is to provide a lithium-ion battery positive electrode material precursor and a preparation method thereof, a lithium-ion battery positive electrode material, a lithium-ion battery and electrical equipment to solve the above problems.
[0010] To achieve the above objectives, this application adopts the following technical solutions:
[0011] A lithium-ion battery cathode material precursor, wherein one precursor secondary particle comprises N primary particles, and one primary particle comprises N neatly stacked single sheets with smooth edges.
[0012] Wherein, N is a positive integer and N≥2.
[0013] Preferably, in a precursor secondary particle, at least 60% of the primary particles meet requirement ①: the primary particle length is not less than 200 nm, the primary particle width is not less than 50 nm, and the primary particle aspect ratio is not less than 1.2;
[0014] Preferably, in a precursor secondary particle, at least 70% of the primary particles meet requirement ②: the primary particle length is 200-3000 nm, the primary particle width is 50-300 nm, and the primary particle aspect ratio is not less than 1.2.
[0015] The length, width, and aspect ratio of the primary particles of the precursor must be within a certain range, otherwise the regularity and integrity of the primary particles will be poor, thereby affecting the electrochemical performance of the battery made from the positive electrode material after sintering. Specifically, if the width of the primary particles is too narrow and the length is too short, the pores inside the corresponding secondary particles of the precursor are too small, and the specific surface area BET value is too small, resulting in a low porosity of the positive electrode material after sintering, causing the Li ion transmission path to be too long, thereby affecting the capacity performance; if the width of the primary particles is too wide and the length is too long, the pores inside the corresponding secondary particles of the precursor are too large, and the specific surface area BET value is too large, resulting in a high porosity of the positive electrode material after sintering, causing its secondary particles to easily crack, thereby affecting the cycle performance.
[0016] Preferably, in a precursor secondary particle, at least 20% of the primary particles meet requirement ③:
[0017] The single layer includes a broken single layer and / or an unbroken single layer, and the broken single layer is in a straight line or a bent shape;
[0018] When the broken single layer is bent, the minimum angle γ between the extension line of the straight portion and the bent portion is less than or equal to 30°.
[0019] Preferably, in one precursor secondary particle, at least 20% of the primary particles meet at least one of the following requirements:
[0020] Requirement ④: In a primary particle, the monolithic layer includes broken monolithic layers and / or unbroken monolithic layers, and the number of fractures of each broken monolithic layer is less than or equal to 2;
[0021] Requirement ⑤: In a primary particle, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the length of the longest fragment in each broken monolithic layer accounts for no less than 50% of the total length of the monolithic layer in which it is located;
[0022] Requirement 6: In a primary particle, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the sum of the total length of all unbroken monolithic layers and the total length of the longest fragment of all broken monolithic layers accounts for no less than 60% of the total length of all monolithic layers. Preferably, the lithium-ion battery positive electrode material precursor meets at least one of the following conditions:
[0023] A. Precursor particle size D50 is 4-20 μm;
[0024] B. The half maximum width (FWHM) (001) of the precursor corresponding to the diffraction angle 2θ = 19.2 ± 1° and the half maximum width (FWHM) (101) of the precursor corresponding to the diffraction angle 2θ = 38.5 ± 1° are both less than 0.550°;
[0025] C. The BET surface area of the precursor is 3-20m 2 / g;
[0026] D. The precursor chemical formula is Ni x M 1-x (OH)2, wherein 0.6≤x<1, and M is at least one of Co, Mn, Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr;
[0027] E. The precursor chemical formula is Ni x Co y Mn z M 1 1-x-y-z (OH)2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 1-xy≥0; M 1 It is at least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr.
[0028] The present application also provides a method for preparing a lithium-ion battery positive electrode material precursor, comprising:
[0029] Raw materials including nickel metal salt solution, precipitant and complexing agent are introduced into the bottom liquid for reaction. During the reaction, the pH is controlled at 9.8-11.3, the ammonia concentration is controlled at 2-12 g / L and the nickel concentration in the supernatant is controlled at 70-350 ppm. After the reaction, solid-liquid separation, drying and sieving for demagnetization are performed to obtain a precursor of the positive electrode material for lithium-ion batteries.
[0030] The above preparation method satisfies at least one of the following conditions:
[0031] a. The nickel-containing metal salt solution contains nickel metal Ni and at least one of Co and Mn;
[0032] b. The nickel-containing metal salt solution contains only Ni;
[0033] c. The raw materials introduced into the bottom liquid further include a doping metal salt solution, wherein the doping metal in the doping metal salt solution includes at least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr;
[0034] d. The precipitant includes sodium hydroxide solution, and the complexing agent includes aqueous ammonia;
[0035] e. The flow rate of the nickel metal salt solution is 2-10% of the available volume of the reactor / h, the flow rate of the precipitant is 0.5-3.5% of the available volume of the reactor / h, and the flow rate of the complexing agent is 0.01-1% of the available volume of the reactor / h;
[0036] f. The base liquid includes sodium hydroxide solution, ammonia water and water;
[0037] g. The pH of the bottom solution is 10.5-12.3, and the ammonia concentration of the bottom solution is 3.4-6 g / L; optionally, the pH of the bottom solution is 10.5-11.90;
[0038] h. The mother liquor is discharged during the reaction. The total liquid inlet rate is the sum of the flow rates of the raw materials introduced into the bottom liquid at the same time. The mother liquor discharge rate is consistent with the total liquid inlet rate.
[0039] The present application also provides a lithium-ion battery positive electrode material, the raw materials of which include a lithium-ion battery positive electrode material precursor.
[0040] The present application also provides a lithium-ion battery, including a lithium-ion battery positive electrode material.
[0041] The present application also provides an electrical device including a lithium-ion battery.
[0042] Compared with the prior art, the advantages of this application include:
[0043] The lithium-ion battery positive electrode material precursor provided in the present application is composed of primary particles, and one primary particle includes multiple neatly stacked single layers with smooth edges. The multiple single layers that make up the primary particle have the characteristics of high regularity and high integrity, which means that the half-peak width on the (001) crystal plane and the (101) crystal plane is narrow, with high crystallinity and fewer crystal defects, which can effectively reduce side reactions during battery use, inhibit damage to the secondary particle structure during repeated charging and discharging, and improve the capacity retention rate after cycling.
[0044] High lamellar regularity means that the shapes and sizes of the multiple lamellars within a primary particle are relatively uniform, their edges are flat, and they are neatly stacked. High lamellar integrity means that within a primary particle, there are few broken lamellars, the number of broken lamellars is small, and the proportion of long fragments is high. The broken lamellars also show little bending deformation, and the minimum angle γ between the extension of the straight line and the bend is small.
[0045] The preparation method of the lithium-ion battery positive electrode material precursor provided in the present application obtains the precursor secondary particles formed by the above-mentioned primary particles including multiple monolithic layers by controlling the pH, ammonia concentration and nickel content of the supernatant during the reaction. The process is simple and the product quality stability between batches is good.
[0046] The lithium-ion battery positive electrode material provided in this application has higher capacity and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0048] FIG1 is a schematic diagram of a primary particle and a single layer constituting the primary particle;
[0049] Figure 2 is a schematic diagram of the length and width of primary particles;
[0050] FIG3 is a schematic diagram of the minimum angle γ between the extension line of the straight portion and the bent portion of the broken single sheet in requirement ③;
[0051] FIG4 is a schematic diagram of a fractured monolithic layer that meets requirements ④ and ⑤;
[0052] FIG5 is a schematic diagram of a fractured monolithic layer that does not meet requirement ⑤;
[0053] FIG6 is a schematic diagram of N broken monolithic layers in a primary particle meeting requirement ⑥;
[0054] FIG7 is a schematic diagram of multiple broken monolithic layers in a primary particle that does not meet requirement ⑥;
[0055] Figure 8 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 1 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0056] Figure 9 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 1 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0057] Figure 10 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 2 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0058] Figure 11 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 2 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0059] Figure 12 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 3 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0060] Figure 13 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Example 3 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0061] Figure 14 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 1 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0062] Figure 15 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 1 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0063] Figure 16 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 2 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0064] Figure 17 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 2 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0065] Figure 18 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 3 0.95 Co 0.04 Mn 0.01 Local surface SEM photos of (OH)2 secondary particles;
[0066] Figure 19 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 4 0.95 Co 0.04 Mn 0.01 XRD pattern of (OH)2;
[0067] Figure 20 is the lithium ion battery ternary positive electrode material precursor Ni obtained in Comparative Example 2 0.95 Co 0.04 Mn 0.01 SEM image of the surface of (OH)2 secondary particles with squares. DETAILED DESCRIPTION
[0068] As used herein:
[0069] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0070] The conjunction "consisting of" excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed, excluding materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim, rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0071] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed alone. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0072] In these examples, parts and percentages are by mass unless otherwise indicated.
[0073] "Parts by mass" refers to the basic unit of measurement used to express the mass ratio of multiple components. One part can represent any unit of mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, this means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, we could say that the mass of component A is aK and the mass of component B is bK (where K is an arbitrary number representing a multiplication factor). It's important to note that, unlike parts by mass, the sum of the mass of all components is not limited to 100 parts.
[0074] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0075] A lithium-ion battery positive electrode material precursor is composed of primary particles. Each primary particle includes a plurality of neatly stacked single layers with smooth edges.
[0076] A schematic diagram of a primary particle and a monolithic layer constituting the primary particle is shown in Figure 1. It should be noted that each primary particle is formed by stacking N monolithic layers, where N is a positive integer and N≥2. The "smooth edge" referred to in this application refers to that the monolithic layer has a smooth edge and does not have obvious concavo-convex shapes. In the surface local SEM photo, the smooth edge of the monolithic layer in the primary particle refers to that the monolithic layer is stacked neatly, so that the side of the primary particle is a plurality of long straight strips parallel to each other (similar to the stacking state of each page in a book), and the side of the primary particle does not have obvious concavo-convex shapes (as shown in Figure 10). If the monolithic layer in the primary particle is not neatly stacked, in some cases, as shown in Figure 20, the side of its primary particle is uneven, and multiple non-linear multi-section strips can be seen in the surface local SEM image, which seem to be composed of multiple fragments, and the part of each fragment is a section (as shown in the part in the box in Figure 20), and the length of one section for the entire monolithic layer is shorter, so it is believed that the monolithic layer has an uneven edge. For example, the magnification of the local surface SEM photograph may be 40.0K, 45.0K, 50.0K, 60.0K, etc. The specific magnification is preferably such that the single layer morphology can be clearly displayed in the SEM field of view.
[0077] The term "neatly stacked" as used herein means that each monolithic layer is stacked in a parallel or substantially parallel state, with no significant displacement of the monolithic layers along one edge in the stacking direction (width direction), similar to the stacking of pages in a closed book. For example, in a localized surface SEM photograph taken at a magnification of 50.0K, neatly stacked monolithic layers means that the visible dimensions (length, width, and height) of the multiple monolithic layers within a primary particle are not significantly different, and that, after the monolithic layers are stacked, no significant displacement of the monolithic layers along one edge in the stacking direction (width direction) occurs, similar to the stacking of pages in a closed book.
[0078] The lithium-ion battery positive electrode material precursor provided in the present application is composed of primary particles, and one primary particle includes multiple neatly stacked single layers with flat edges. After the positive electrode material inheriting the precursor structure is prepared into a battery, it can inhibit the secondary particles from cracking or breaking due to multiple expansion and contraction during repeated charging and discharging, thereby improving the capacity retention rate after cycling.
[0079] In an optional embodiment, in a precursor secondary particle, at least 60% of the primary particles meet requirement ①: the primary particle length is not less than 200 nm, the primary particle width is not less than 50 nm, and the primary particle aspect ratio is not less than 1.2;
[0080] Optionally, in a precursor secondary particle, at least 60% of the primary particles meet requirement ①: the primary particle length can be not less than 200nm, not less than 400nm, not less than 600nm, not less than 800nm, not less than 1000nm, not less than 1200nm, not less than 1400nm, not less than 1600nm, not less than 1800nm, not less than 2000nm, not less than 2200nm, not less than 2400nm, not less than 2600nm, not less than 2800nm, not less than 3000nm, not less than 4000nm m, not less than 5000 nm, not less than 6000 nm or not less than 2000 nm; the primary particle width may be not less than 50 nm, not less than 80 nm, not less than 100 nm, not less than 120 nm, not less than 140 nm, not less than 160 nm, not less than 180 nm, not less than 200 nm, not less than 220 nm, not less than 240 nm, not less than 260 nm, not less than 280 nm, not less than 300 nm, not less than 400 nm, not less than 500 nm or any value between 50 nm and 500 nm;
[0081] In an optional embodiment, in a precursor secondary particle, at least 70% of the primary particles meet requirement ②: the primary particle length is 200-3000 nm, the primary particle width is 50-300 nm, and the primary particle aspect ratio is not less than 1.2;
[0082] Alternatively, in an optional embodiment, in a precursor secondary particle, at least 70% of the primary particles meet requirement ②: the primary particle length can be 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, 210 0nm, 2200nm, 2300nm, 2400nm, 2500nm, 2600nm, 2700nm, 2800nm, 2900nm, 3000nm or any value or any interval between 200-3000nm such as 200nm-2000nm, 300nm-1200nm, 600nm-3000nm, 600nm-3000nm, 1500nm-2500nm, etc.; the primary particle width can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 1500nm, 2500nm, etc. 0nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, 300nm or any value or any interval between 50-300nm such as 50-100nm, 100-200nm, 200-300 The aspect ratio of the primary particle may be not less than 1.2, not less than 2.0, not less than 3.0, not less than 4.0, not less than 5.0, not less than 6.0, not less than 7.0, not less than 8.0, not less than 9.0, not less than 10.0, not less than 11.0, not less than 12.0, not less than 13.0, not less than 14.0, not less than 15.0 or any range such as 2.0-5.0, 4.0-8.5, 2.5-6.5, 7.5-13.0, 6.0-11.0, etc.
[0083] A schematic diagram of the width and length of a primary particle is shown in FIG2 , that is, the width direction is along the stacking direction of the monolithic layers, and the length direction is along the extending direction of the monolithic layers.
[0084] The length of a primary particle involved in this application refers to the average value of multiple length data obtained by measuring multiple primary particles; the width of a primary particle refers to the average value of multiple width data obtained by measuring multiple primary particles.
[0085] The testing method for primary particles is as follows: first adjust the magnification of the scanning electron microscope (SEM) and take a photo to obtain a local SEM photo of the surface. Then, as shown in Figure 2, use the electronic ruler software Ruler to measure the primary particles selected in the photo separately to obtain the length and width of the primary particles, and then calculate the aspect ratio of the primary particles.
[0086] The surface local SEM photo refers to a surface local photo of the precursor secondary particles of the lithium-ion battery positive electrode material precursor obtained by scanning electron microscope (SEM) at a certain magnification. For example, the magnification of the SEM photo can be 40.0K, 45.0K, 50.0K, 60.0K, etc. The specific magnification is preferably such that the single layer morphology can be clearly displayed in the SEM field of view. In the above measurement, if there is a situation where the primary particle is blocked, the unblocked part is assumed to be a complete primary particle for measurement.
[0087] In an optional embodiment, in a precursor secondary particle, at least 20% of the primary particles meet requirement ③:
[0088] The single layer includes a broken single layer and / or an unbroken single layer, and the broken single layer is in a straight line or a bent shape;
[0089] When the broken single layer is bent, the minimum angle γ between the extension line of the straight part and the bent part is less than or equal to 30°.
[0090] Optionally, when the broken single layer is bent, the minimum angle γ between the extension line of its straight part and the bent part can be less than or equal to 30°, less than or equal to 25°, less than or equal to 20°, less than or equal to 15°, less than or equal to 10°, less than or equal to 5°, etc.
[0091] As shown in FIG3 , the minimum angle γ between the extension line of the straight portion of the broken single layer in ③ and the bent portion is required to be ≤30°.
[0092] The relevant test method is: in the local surface SEM photo, select the broken monolithic layer in the primary particle, and then use the electronic ruler software ruler to measure the minimum angle γ between the extension line of the straight part of the broken monolithic layer and the bent part as shown in Figure 3.
[0093] In an optional embodiment, in a precursor secondary particle, at least 20% of the primary particles meet at least one of the following requirements:
[0094] Requirement ④: In a primary particle, the monolithic layer includes broken monolithic layers and / or unbroken monolithic layers, and the number of fractures of each broken monolithic layer is less than or equal to 2;
[0095] Requirement ⑤: In one of the primary particles, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the length of the longest fragment in each broken monolithic layer accounts for no less than 50% of the total length of the monolithic layer in which it is located;
[0096] Optionally, in one of the primary particles, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the length of the longest fragment in each broken monolithic layer may account for no less than 50%, no less than 55%, no less than 60%, no less than 65%, no less than 70%, no less than 75%, no less than 80%, no less than 85%, no less than 90%, etc. of the total length of the monolithic layer.
[0097] For example, as shown in FIG4 and FIG5 , FIG4 is a schematic diagram of a broken single-piece layer that meets the requirement ⑤, and FIG5 is a schematic diagram of a broken single-piece layer that does not meet the requirement ⑤.
[0098] Requirement ⑥: In a primary particle, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the sum of the total length of all unbroken monolithic layers and the total length of the longest fragments of all broken monolithic layers accounts for no less than 60% of the total length of all monolithic layers.
[0099] For example, as shown in Figures 6 and 7 , assuming that all monoliths in the same primary particle are of the same length and the fracture positions in the fractured monoliths are consistent, the total length of the longest fragment of all fractured monoliths shown in Figure 6 accounts for 70% of the total length of all monoliths in the primary particle in which they are located, meeting requirement ⑥;
[0100] As shown in FIG7 , the total length of the longest fragment in all the broken monoliths accounts for 59.4% of the total length of all the monoliths in the primary particle in which it is located, which does not meet requirement ⑥.
[0101] The relevant testing method is as follows: In the local surface SEM photograph, select a broken monolith in the primary particle, first observe the number of monolith fractures, then use the electronic ruler software Ruler to measure the length of each fragment in the broken monolith, as shown in Figure 5, and then calculate the ratio of the length of the longest fragment in each broken monolith to the total length of the monolith in which it is located; finally, refer to Figures 6 and 7 to calculate the ratio of the total length of the longest fragments of all broken monoliths in the primary particle to the total length of all monoliths. In the above measurement, if a monolith is obscured, the unobstructed portion is assumed to be a complete monolith for measurement.
[0102] The provided lithium-ion battery positive electrode material precursor is composed of primary particles, each of which includes multiple neatly stacked single layers with smooth edges. The multiple single layers that make up the primary particles have the characteristics of high regularity and high integrity, which means that they have narrow half-peak widths on the (001) crystal plane and the (101) crystal plane, high crystallinity and fewer crystal defects, which can effectively reduce side reactions during battery use, inhibit damage to the secondary particle structure during repeated charging and discharging, and improve the capacity retention rate after cycling.
[0103] High lamellar regularity means that the shapes and sizes of the multiple lamellars within a primary particle are relatively uniform, their edges are flat, and they are neatly stacked. High lamellar integrity means that within a primary particle, there are few broken lamellars, the number of broken lamellars is small, and the proportion of long fragments is high. The broken lamellars also show little bending deformation, and the minimum angle γ between the extension of the straight line and the bend is small.
[0104] In an optional embodiment, the lithium-ion battery positive electrode material precursor satisfies at least one of the following conditions:
[0105] A. Precursor particle size D50 is 4-20 μm;
[0106] Optionally, the precursor particle size D50 may be 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or any value between 4 and 20 μm, or any interval such as 4-8 μm, 8-20 μm, 8-15 μm, 12-20 μm, 5-10 μm, etc.;
[0107] B. The half maximum width (FWHM) (001) of the precursor corresponding to the diffraction angle 2θ = 19.2 ± 1° and the half maximum width (FWHM) (101) of the precursor corresponding to the diffraction angle 2θ = 38.5 ± 1° are both less than 0.550°;
[0108] Optionally, the half maximum width FWHM (001) of the (001) crystal plane corresponding to the diffraction angle 2θ = 19.2 ± 1° and the half maximum width FWHM (101) of the (101) crystal plane corresponding to the diffraction angle 2θ = 38.5 ± 1° in the precursor can be both less than 0.550°, both less than 0.500°, both less than 0.450°, both less than 0.400°, both less than 0.350°, both less than 0.300°, both less than 0.250°, both less than 0.200°, both less than 0.150°, etc.;
[0109] C. The BET surface area of the precursor is 3-20m 2 / g;
[0110] Optionally, the precursor surface area BET can be 3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g、9m 2 / g、10m 2 / g、11m 2 / g、12m 2 / g、13m 2 / g、14m 2 / g、15m 2 / g、16m 2 / g、17m 2 / g、18m 2 / g、19m 2 / g, 20m 2 / g、12m 2 / g、22m 2 / g, 23m 2 / g、24m 2 / g, 25m 2 / g, 26m 2 / g、27m 2 / g、28m 2 / g、29m 2 / g、30m 2 / g or 3-20m 2 Any value or any interval between 3-8m / g 2 / g, 8-17m 2 / g, 15-20m 2 / g, 5-10m 2 / g, 6-16m 2 / g etc.;
[0111] D. The precursor chemical formula is Ni x M 1-x (OH)2, wherein 0.6≤x<1, and M is at least one of Co, Mn, Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr;
[0112] Optionally, in the precursor chemical formula, x can be 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99 or any value between 0.6≤x<1 or any interval such as 0.6≤x<0.8, 0.8≤x<1, 0.75≤x≤0.95, 0.9≤x<1, 0.95≤x<1, etc.;
[0113] E. Its chemical formula is Ni x Co y Mn z M 1 1-x-y-z (OH)2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 1-xy≥0; M 1 At least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr;
[0114] Optionally, in the precursor chemical formula, y can be 0, 0.005, 0.01, 0.015, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, or 0≤y ≤0.4, such as 0≤y≤0.05, 0≤y≤0.2, 0≤y≤0.3, 0<y<0.4, 0≤y≤0.1, 0.1≤y≤0.3, 0.2≤y≤0.4, etc.; z can be 0, 0.005, 0.01, 0.015, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 or any value between 0≤y≤0.4 or any interval such as 0≤z≤0.05, 0≤z≤0.2, 0≤z≤0.3, 0<z<0.4, 0≤z≤0.1, 0.1≤z≤0.3, 0.2≤z≤0.4, etc.; 1-xy can be 0, 0.005, 0.01, 0.015, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0. 1-xy≥0, such as 0≤1-xy≤0.05, 0≤1-xy≤0.2, 0≤1-xy≤0.3, 0<1-xy<0.4, 0≤1-xy≤0.1, 0.1≤1-xy≤0.3, 0.2≤1-xy≤0.4, etc.
[0115] The present application also provides a method for preparing a lithium-ion battery positive electrode material precursor, comprising:
[0116] The raw materials including nickel metal salt solution, precipitant, and complexing agent are introduced into the bottom liquid for reaction, wherein the pH is controlled at 9.8-11.3, the ammonia concentration is controlled at 2-12 g / L, and the nickel concentration in the supernatant is controlled at 70-350 ppm. After the reaction, the precursor is separated from the solid and liquid, dried, and sieved for demagnetization to obtain a positive electrode material precursor for a lithium ion battery.
[0117] Optionally, the pH during the reaction can be controlled to be 9.8, 9.9, 10.0, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3 or any value between 9.8 and 11.3 or any interval such as 9.8-10.4, 10.4-11.0, 11.0-11. 3, 11.00-11.20, etc.; the ammonia concentration can be 2g / L, 3g / L, 4g / L, 5g / L, 6g / L, 7g / L, 8g / L, 9g / L, 10g / L, 11g / L, 12g / L or any value between 2-12g / L or any interval such as 2-8g / L, 3-7g / L, 8-12g / L, 4-10g / L, 5-12g / L, etc.; nickel in the supernatant The concentration can be 70ppm, 80ppm, 90ppm, 100ppm, 110ppm, 120ppm, 130ppm, 140ppm, 150ppm, 160ppm, 170ppm, 180ppm, 190ppm, 210ppm, 220ppm, 230ppm, 240ppm, 250ppm, 260ppm, 270ppm, 280ppm, 290ppm, 300ppm, 310ppm, 320ppm, 330ppm, 340ppm, 350ppm or any value between 70-350ppm or any interval such as 70-250ppm, 250-350ppm, 70-150ppm, 150-300ppm, 200-350ppm, 100-300ppm, etc.
[0118] In an optional embodiment, the above preparation method satisfies at least one of the following conditions:
[0119] a. The nickel-containing metal salt solution contains nickel metal Ni and at least one of Co and Mn;
[0120] b. The nickel-containing metal salt solution contains only Ni;
[0121] c. The raw materials introduced into the bottom liquid further include a doping metal salt solution, wherein the doping metal in the doping metal salt solution includes at least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr;
[0122] It should be noted that the doping metal salt can be prepared together with the nickel-containing metal salt to form a mixed solution for use, or it can be prepared separately into a doping metal salt solution and then flowed into the reactor together with the nickel-containing metal salt solution. The expression herein should not be understood as simply "the doping metal salt must be prepared separately from the nickel-containing metal salt for use."
[0123] d. The precipitant includes sodium hydroxide solution, and the complexing agent includes aqueous ammonia;
[0124] e. The flow rate of the nickel metal salt solution is 2-10% of the available volume of the reactor / h, the flow rate of the precipitant is 0.5-3.5% of the available volume of the reactor / h, and the flow rate of the complexing agent is 0.01-1% of the available volume of the reactor / h;
[0125] Optionally, the flow rate of the nickel-containing metal salt solution can be 2% / h, 3% / h, 4% / h, 5% / h, 6% / h, 7% / h, 8% / h, 9% / h, 10% / h or any value between 2-10% / h or any interval such as 2-8% / h, 4-10% / h, 6-10% / h, 3-7% / h, 5-9% / h, etc. of the available volume of the reactor, and the flow rate of the precipitant can be 0.5% / h, 1.0% / h, 1.5% / h, 2.0% / h, 2.5% / h, 3.0% / h. h, 3.5% / h reactor available volume or any value between 0.5-3.5% / h or any interval such as 0.5-1.5% / h, 1.5-2.5% / h, 2.5-3.5% / h, 1.0-2.5% / h, 1.5-3.0% / h, 0.8-1.5% / h, 0.9-1.4% / h, 1.4% / h ~ 1.5% / h, etc. The flow rate of the complexing agent can be 0.01% / h, 0.05% / h, 0.1% / h, 0.2% / h, 0.3% / h, 0.4% / h, 0.5% / h, 0.6% / h, 0.7% / h, 0.8% / h, 0.9% / h, 1% / h of the available volume of the reactor or any value or any interval between 0.01-1% / h such as 0.08% / h to 0.16% / h, 0.01-0.3% / h, 0.3-0.6% / h, 0.6-1% / h, 0.05-0.20% / h, 0.2-0.7% / h, 0.3-0.8% / h, etc.;
[0126] f. The base liquid includes sodium hydroxide solution, ammonia water and water;
[0127] g. The pH of the bottom solution is 10.5-12.3, and the ammonia concentration of the bottom solution is 3.4-6 g / L; optionally, the pH of the bottom solution is 10.5-11.90;
[0128] Optionally, the pH of the base solution may be 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12.0, 12.1, 12.1, 12.2, 12.3 or any value between 10.5 and 12.3 or any range such as 10.5-11.8, 11.8-12.3, 11. 0-12.0, 10.8-11.8, etc. The ammonia concentration of the base solution can be 3.4g / L, 3.5g / L, 3.6g / L, 3.7g / L, 3.8g / L, 3.9g / L, 4.0g / L, 4.5g / L, 5g / L, 5.5g / L, 6.0g / L or any value between 3.4-6g / L or any interval such as 3.4-4.5g / L, 4.5-6.0g / L, 4.0-5.0g / L, etc.;
[0129] h. During the reaction, the mother liquor is discharged. The total liquid inlet rate is the sum of the flow rates of the raw materials simultaneously introduced into the bottom liquid. The mother liquor discharge rate is consistent with the total liquid inlet rate.
[0130] The present application also provides a lithium-ion battery positive electrode material, the raw materials of which include a lithium-ion battery positive electrode material precursor.
[0131] The present application also provides a lithium-ion battery, including a lithium-ion battery positive electrode material.
[0132] The present application also provides an electrical device including a lithium-ion battery.
[0133] The electrical equipment referred to in this application includes electric vehicles, electric bicycles, mobile phones, tablet computers, power banks, energy storage stations and other equipment that directly or indirectly use lithium-ion batteries.
[0134] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be understood by those skilled in the art that the following examples are merely illustrative of the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, the conditions are carried out according to conventional conditions or manufacturer recommendations. The reagents or instruments used are not specified by the manufacturer and are conventional products that can be purchased commercially.
[0135] First of all, it should be noted that primary particles with high regularity and integrity represent a material with high crystallinity, and the corresponding XRD half-peak width is significantly narrower than that of similar products. At the same time, due to the reduction in the gaps between multiple monolithic layers in the primary particles, the cross-sectional structure has a lower BET when the porosity is the same, indicating that its crystal defects are reduced, reducing side reactions during circulation.
[0136] Example 1 (ternary precursor: Ni 0.95 Co0.04 Mn 0.01 (OH)2)
[0137] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0138] Step 1: Solution Preparation
[0139] According to the metal molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0140] Step 2: Primer Preparation
[0141] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 65°C to obtain a base solution with a pH of 11.75 and an ammonia concentration of 4 g / L.
[0142] Step 3: Material preparation
[0143] Under stirring, constant temperature of 65° C., and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentrator, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0144] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 10.4-10.7 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 170-230 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.04 Mn 0.01 (OH)2.
[0145] The obtained lithium-ion battery ternary cathode material precursor Ni 0.95 Co 0.04 Mn 0.01 A local SEM photograph of the secondary particles of (OH)2 is shown in FIG8 , and its XRD spectrum is shown in FIG9 .
[0146] Example 2 (ternary precursor: Ni 0.95 Co 0.04 Mn0.01 (OH)2)
[0147] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0148] Step 1: Solution Preparation
[0149] According to the metal molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0150] Step 2: Primer Preparation
[0151] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred uniformly at a constant temperature of 60°C to obtain a base solution with a pH of 11.85 and an ammonia concentration within the range of 5 g / L;
[0152] Step 3: Material preparation
[0153] Under stirring, constant temperature of 60° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0154] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to the range of 10.20-10.70 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 250-330 ppm, and finally a metal hydroxide reaction precipitation slurry with a diameter D50 of 14 μm was obtained.
[0155] The reaction precipitate slurry is washed, centrifuged, dried, sieved and demagnetized to obtain the precursor Ni for the lithium-ion battery ternary positive electrode material. 0.95 Co 0.04 Mn 0.01 (OH)2.
[0156] The obtained lithium-ion battery ternary cathode material precursor Ni 0.95 Co 0.04 Mn 0.01 A local SEM photograph of the secondary particles of (OH)2 is shown in FIG10 , and its XRD spectrum is shown in FIG11 .
[0157] Example 3 (ternary precursor: Ni 0.95 Co0.04 Mn 0.01 (OH)2)
[0158] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0159] Step 1: Solution Preparation
[0160] According to the metal molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0161] Step 2: Primer Preparation
[0162] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 55°C to obtain a base solution with a pH of 11.60 and an ammonia concentration of 6 g / L.
[0163] Step 3: Material preparation
[0164] Under stirring, constant temperature of 55° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0165] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.00-11.20 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 80-150 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.04 Mn 0.01 (OH)2.
[0166] The obtained lithium-ion battery ternary cathode material precursor Ni 0.95 Co 0.04 Mn 0.01 A local SEM photograph of the secondary particles of (OH)2 is shown in FIG12 , and its XRD spectrum is shown in FIG13 .
[0167] Example 4 (binary precursor: Ni 0.95 Mn 0.05 (OH)2)
[0168] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0169] Step 1: Solution Preparation
[0170] According to the nickel and manganese metal molar ratio of 95:5, nickel sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0171] Step 2: Primer Preparation
[0172] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 60°C to obtain a base solution with a pH of 11.90 and an ammonia concentration of 6 g / L.
[0173] Step 3: Material preparation
[0174] Under stirring, constant temperature of 60° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0175] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.00-11.20 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 80-150 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Mn 0.05 (OH)2.
[0176] Example 5 (ternary precursor: Ni 0.7 Co 0.1 Mn 0.2 (OH)2)
[0177] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0178] Step 1: Solution Preparation
[0179] According to the molar ratio of nickel, cobalt and manganese of 70:10:20, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0180] Step 2: Primer Preparation
[0181] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 50°C to obtain a base solution with a pH of 11.40 and an ammonia concentration of 3.4 g / L.
[0182] Step 3: Material preparation
[0183] Under stirring, constant temperature of 50° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentrating device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0184] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.00-11.20 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 70-100 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 10 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.7 Co 0.1 Mn 0.2 (OH)2.
[0185] Example 6 (Quaternary Precursor: Ni 0.95 Co 0.03 Mn 0.015 Al 0.005 (OH)2)
[0186] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0187] Step 1: Solution Preparation
[0188] According to the molar ratio of nickel, cobalt, manganese and aluminum of 95:3:1.5:0.5, nickel sulfate, cobalt sulfate, manganese sulfate and aluminum sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0189] Step 2: Primer Preparation
[0190] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred uniformly at a constant temperature of 65°C to obtain a base solution with a pH of 11.40 and an ammonia concentration of 3.4 g / L;
[0191] Step 3: Material preparation
[0192] Under stirring, constant temperature of 65° C., and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentrator, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0193] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.00-11.20 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 100-150 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.03 Mn 0.015 Al 0.005 (OH)2.
[0194] Example 7 (Quaternary Precursor: Ni 0.95 Co 0.03 Mn 0.015 Zr 0.005 (OH)2)
[0195] This embodiment provides a lithium-ion battery positive electrode material precursor, and the preparation method thereof is as follows:
[0196] Step 1: Solution Preparation
[0197] According to the molar ratio of nickel, cobalt, manganese and zirconium of 95:3:1.5:0.5, nickel sulfate, cobalt sulfate, manganese sulfate and zirconium sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0198] Step 2: Primer Preparation
[0199] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 55°C to obtain a base solution with a pH of 11.40 and an ammonia concentration of 3.4 g / L.
[0200] Step 3: Material preparation
[0201] Under stirring, constant temperature of 55° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0202] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.00-11.20 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 250-300 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.03 Mn 0.015 Zr 0.005 (OH)2.
[0203] Example 8 (ternary precursor: Ni 0.95 Co 0.04 Mn 0.01 (OH)2)
[0204] Step 1: Solution Preparation
[0205] According to the molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0206] Step 2: Primer Preparation
[0207] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 55°C to obtain a base solution with a pH of 11.00 and an ammonia concentration of 3.4 g / L.
[0208] Step 3: Material preparation
[0209] Under stirring, constant temperature of 65° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 3% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.05% / h to 1.15% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.06% / h to 0.12% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing a bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0210] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 10.30-10.50 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 100-150 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 4 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.04 Mn 0.01 (OH)2.
[0211] Example 9 (ternary precursor: Ni 0.83 Co 0.11 Mn 0.06 (OH)2)
[0212] Step 1: Solution Preparation
[0213] According to the metal molar ratio of nickel, cobalt and manganese of 83:11:6, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0214] Step 2: Primer Preparation
[0215] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 60°C to obtain a base solution with a pH of 11.30 and an ammonia concentration of 3.0 g / L.
[0216] Step 3: Material preparation
[0217] Under stirring, constant temperature of 60° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0218] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 10.50-10.70 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 3-7 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 150-250 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 8 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.83 Co 0.11 Mn 0.06 (OH)2. Comparative Example 1 (ternary precursor: Ni 0.95 Co 0.04 Mn 0.01 (OH)2)
[0219] This comparative example provides a lithium-ion battery positive electrode material precursor, and its preparation method is as follows:
[0220] Step 1: Solution Preparation
[0221] According to the metal molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0222] Step 2: Primer Preparation
[0223] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred at a constant temperature of 65°C to obtain a base solution with a pH of 12.25 and an ammonia concentration of 6 g / L.
[0224] Step 3: Material preparation
[0225] Under stirring, constant temperature of 65° C. and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into the reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentration device, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0226] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 11.60-11.80 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 5-8 g / L. The nickel concentration in the supernatant was changed and maintained within the range of ≤10 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material.0.95 Co 0.04 Mn 0.01 (OH)2.
[0227] The obtained lithium-ion battery ternary cathode material precursor Ni 0.95 Co 0.04 Mn 0.01 A local SEM photograph of the secondary particles of (OH)2 is shown in FIG14 , and its XRD spectrum is shown in FIG15 .
[0228] Comparative Example 2 (ternary precursor: Ni 0.95 Co 0.04 Mn 0.01 (OH)2)
[0229] This comparative example provides a lithium-ion battery positive electrode material precursor, and its preparation method is as follows:
[0230] Step 1: Solution Preparation
[0231] According to the metal molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate crystals were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0232] Step 2: Primer Preparation
[0233] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred uniformly at a constant temperature of 65°C to obtain a base solution with a pH of 12.15 and an ammonia concentration fluctuating within the range of 5 g / L;
[0234] Step 3: Material preparation
[0235] Under stirring, constant temperature of 65° C., and nitrogen protection, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing the bottom liquid; during the reaction process, the mother liquor is discharged through a concentrator, and the discharge rate of the mother liquor is consistent with the total liquid inlet rate;
[0236] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 9.30-9.50 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 5-8 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 400-500 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 14 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co0.04 Mn 0.01 (OH)2.
[0237] The obtained lithium-ion battery ternary cathode material precursor Ni 0.95 Co 0.04 Mn 0.01 A local SEM photograph of the secondary particles of (OH)2 is shown in FIG16 , and its XRD spectrum is shown in FIG17 .
[0238] Comparative Example 3 (ternary precursor: Ni 0.95 Co 0.04 Mn 0.01 (OH)2)
[0239] This comparative example provides a lithium-ion battery positive electrode material precursor, and its preparation method is as follows:
[0240] Step 1: Solution Preparation
[0241] According to the molar ratio of nickel, cobalt and manganese of 95:4:1, nickel sulfate, cobalt sulfate and manganese sulfate were weighed and calculated to prepare a nickel-containing metal salt solution with a total metal content of 2 mol / L.
[0242] Step 2: Primer Preparation
[0243] Pure water, NaOH solution (concentration 32 wt%), and ammonia water (concentration 21 wt%) were added to a reactor and stirred evenly at a constant temperature of 35° C. to obtain a base solution with a pH of 10.80 and an ammonia concentration of 3.4 g / L.
[0244] Step 3: Material preparation
[0245] Under stirring, a constant temperature of 35° C., and an air environment, a nickel-containing metal salt solution (flow rate: 4% / h of the available volume of the reactor), a NaOH solution (flow rate: 1.4% / h to 1.5% / h of the available volume of the reactor), and aqueous ammonia (flow rate: 0.08% / h to 0.16% / h of the available volume of the reactor) are simultaneously introduced into a reactor containing a base liquid; during the reaction process, the mother liquor is discharged through a concentrator, and the discharge rate of the mother liquor is kept consistent with the total liquid inlet rate;
[0246] During the reaction, by fine-tuning the flow rate of NaOH solution and ammonia water, the pH was adjusted to 9.30-9.50 within 4 hours of feeding, and the ammonia concentration fluctuated within the range of 5-8 g / L. The nickel concentration in the supernatant was changed and maintained within the range of 400-500 ppm, and finally a metal hydroxide reaction precipitate slurry with a diameter D50 of 4 μm was obtained. The reaction precipitate slurry was washed, centrifuged, dried, sieved and demagnetized to obtain Ni, a precursor of the lithium-ion battery ternary positive electrode material. 0.95 Co 0.04 Mn0.01 (OH)2. The measurement data and related parameters of the local SEM photos of the precursor secondary particles obtained in Examples 1-9 and Comparative Examples 1-3 are shown in Tables 1, 2 and 3 below:
[0247] Table 1 Parameters of at least 60% of the primary particles in the precursor
[0248] Table 2 Fracture parameters of preferably at least 20% of the primary particles in the precursor
[0249] Table 3 Precursor parameters
[0250] 2000 g of the precursors prepared in Examples 1-7 and Comparative Examples 1-2 and LiOH·H2O were weighed respectively in a molar ratio of 1:1.03, mixed evenly by a high-speed mixer, and sintered in a box furnace under an air atmosphere at a sintering temperature of 780°C for 12 h. After cooling to room temperature, the mixture was crushed and sieved to obtain a positive electrode material.
[0251] Electrochemical performance testing was conducted using a button-type semi-battery: The aforementioned positive electrode material, conductive carbon black, and binder PVDF (polyvinylidene fluoride) were mixed into a slurry at a ratio of 8:1:1 and coated onto aluminum foil to form the positive electrode sheet. A metallic lithium sheet was used as the negative electrode, and the electrolyte was a 1 mol / L LiPF6 / EC:DMC (volume ratio 1:1). In a vacuum glove box, the battery case, positive and negative electrode sheets, separator, spring, and gasket were assembled into a button-type cell. Electrochemical performance testing was conducted using a Blue Electric test system.
[0252] The test results are shown in Table 4:
[0253] Table 4 Electrochemical test results
[0254] As can be seen from Table 4, the precursors prepared in Comparative Examples 1 and 2 do not have the high regularity and integrity possessed by the precursors in this application, and the edges of the monolithic layers that make up the primary particles are uneven and more easily broken, making it impossible to take into account capacity, rate performance, and cycle performance at the same time. The samples of Examples 1-3 have capacity and rate performance close to those of Comparative Examples 1-2, and their cycle performance is significantly better than that of Comparative Examples 1 and 2; this performance advantage stems from the fact that, based on a similar porous, radially grown structure, the regularity and integrity of the primary particles are further optimized, the XRD half-peak width is greatly narrowed, the crystal defects of the secondary particles as a whole are reduced, the crystallinity is further improved, thereby reducing the occurrence of side reactions and improving the cycle performance. In addition, the precursors prepared in Example 8 and Comparative Example 3 are both small particle products. Compared with Example 8, the edges of the monolithic layers of Comparative Example 3 are concave and convex, the edges are uneven, and the monolithic layers are staggered and not neatly stacked. Even if the characteristics of less primary particle breakage are met and the initial capacity is high, the cycle decay is too fast, so it is difficult to actually have application value.
[0255] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
[0256] Furthermore, those skilled in the art will appreciate that although some embodiments herein include certain features included in other embodiments but not others, combinations of features from different embodiments are intended to be within the scope of this application and to form distinct embodiments. For example, in the claims above, any of the claimed embodiments may be used in any combination. The information disclosed in this background section is intended solely to enhance understanding of the overall background of this application and should not be construed as an admission or any implication that such information constitutes prior art known to those skilled in the art. Industrial Applicability
[0257] The present application provides a lithium-ion battery positive electrode material precursor and its preparation method, lithium-ion battery positive electrode material, lithium-ion battery and electrical equipment, and relates to the field of lithium-ion batteries. The lithium-ion battery positive electrode material precursor, the precursor of which includes a plurality of primary particles, and one primary particle includes a plurality of neatly stacked monolithic layers, and the edges of the monolithic layers are flat. The preparation method includes: introducing raw materials including a nickel-containing metal salt solution, a precipitant, and a complexing agent into a base liquid for reaction, controlling the pH to 9.8-11.3, the ammonia concentration to 2-12 g / L, and the nickel concentration in the supernatant to 70-350 ppm during the reaction; after the reaction, solid-liquid separation, drying, sieving and demagnetization are performed to obtain a lithium-ion battery positive electrode material precursor. In the lithium-ion battery positive electrode material precursor, the multiple monolithic layers constituting the primary particles have the characteristics of high regularity and integrity, and the prepared positive electrode material has higher cycle, capacity and safety.
[0258] Furthermore, it is understood that the lithium-ion battery cathode material precursor and preparation method thereof, lithium-ion battery cathode material, lithium-ion battery, and electrical equipment of the present application are reproducible and can be used in a variety of industrial applications. For example, the lithium-ion battery cathode material precursor and preparation method thereof, lithium-ion battery cathode material, lithium-ion battery, and electrical equipment of the present application can be used in the field of lithium-ion batteries.
Claims
1. A lithium-ion battery positive electrode material precursor, characterized in that: One of the precursor secondary particles includes N primary particles, and one of the primary particles includes N neatly stacked monolayers, and the edges of the monolayers are flat; Wherein, N is a positive integer and N≥2.
2. The lithium-ion battery positive electrode material precursor according to claim 1, characterized in that: In one of the precursor secondary particles, at least 60% of the primary particles meet requirement ①: the length of the primary particle is not less than 200 nm, the width of the primary particle is not less than 50 nm, and the aspect ratio of the primary particle is not less than 1.2; Preferably, in one of the precursor secondary particles, at least 70% of the primary particles meet requirement ②: the length of the primary particles is 200-3000nm, the width of the primary particles is 50-300nm, and the aspect ratio of the primary particles is not less than 1.
2.
3. The lithium-ion battery positive electrode material precursor according to claim 1, characterized in that: In one of the precursor secondary particles, at least 20% of the primary particles meet requirement ③: The monolithic layer includes a broken monolithic layer and / or an unbroken monolithic layer, and the broken monolithic layer is in a straight line or a bent shape; When the broken single layer is bent, the minimum angle γ between the extension line of the straight part and the bent part is less than or equal to 30 o .
4. The lithium-ion battery positive electrode material precursor according to claim 1, characterized in that: In one of the precursor secondary particles, at least 20% of the primary particles meet at least one of the following requirements: Requirement ④: In one of the primary particles, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the number of fractures of each of the broken monolithic layers is less than or equal to 2; Requirement ⑤: In one of the primary particles, the monolithic layers include broken monolithic layers and / or unbroken monolithic layers, and the length of the longest fragment in each of the broken monolithic layers accounts for no less than 50% of the total length of the monolithic layer in which it is located; Requirement ⑥: In one of the primary particles, the monolayers include broken monolayers and / or unbroken monolayers, and the sum of the total length of all the unbroken monolayers and the total length of the longest fragments of all the broken monolayers accounts for no less than 60% of the total length of all the monolayers.
5. The lithium-ion battery positive electrode material precursor according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: A. The precursor particle size D50 is 4-20 μm; B. The precursor has a half-peak width FWHM (001) of the (001) crystal plane corresponding to a diffraction angle of 2θ = 19.2 ± 1° and a half-peak width FWHM (101) of the (101) crystal plane corresponding to a diffraction angle of 2θ = 38.5 ± 1°, both of which are less than 0.550°; C. The precursor has a BET specific surface area of 3-20 m 2 / g; D. The precursor chemical formula is Ni x M 1-x (OH)2, wherein 0.6≤x<1, and M is at least one of Co, Mn, Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr; E. The precursor chemical formula is Ni x Co y Mn z M 1 1-x-y-z (OH)2, where 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 1-xy≥0; M 1 It is at least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr.
6. A method for preparing a lithium-ion battery positive electrode material precursor according to any one of claims 1 to 5, characterized in that: include: The raw materials including nickel metal salt solution, precipitant and complexing agent are introduced into the bottom liquid for reaction. During the reaction, the pH is controlled to be 9.8-11.3, the ammonia concentration is 2-12 g / L, and the nickel concentration in the supernatant is 70-350 ppm; after the reaction is completed, the positive electrode material precursor of the lithium ion battery is obtained after solid-liquid separation, drying, and sieving and demagnetization.
7. The preparation method according to claim 6, characterized in that: At least one of the following conditions is met: a. The nickel-containing metal salt solution contains nickel metal Ni and at least one of Co and Mn; b. The nickel-containing metal salt solution contains only Ni; c. The raw material introduced into the bottom solution further comprises a doped metal salt solution, wherein the doped metal in the doped metal salt solution comprises at least one of Al, Fe, Ti, Zr, Mo, Cr, W, B, Mg, Ba, Nb and Sr; d. the precipitating agent comprises sodium hydroxide solution, and the complexing agent comprises aqueous ammonia; e. The flow rate of the nickel-containing metal salt solution is 2-10% / h of the available volume of the reactor, the flow rate of the precipitant is 0.5-3.5% / h of the available volume of the reactor, and the flow rate of the complexing agent is 0.01-1% / h of the available volume of the reactor; f. The base liquid comprises sodium hydroxide solution, ammonia and water; g. The pH of the base solution is 10.5-12.3, and the ammonia concentration of the base solution is 3.4-6g / L; h. The mother liquor is discharged during the reaction process. The total liquid inlet rate is the sum of the flow rates of the raw materials simultaneously introduced into the bottom liquid. The discharge rate of the mother liquor is consistent with the total liquid inlet rate.
8. A positive electrode material for a lithium ion battery, characterized in that: The raw materials include the lithium ion battery positive electrode material precursor according to any one of claims 1 to 5.
9. A lithium ion battery, characterized in that: The lithium-ion battery positive electrode material comprises the positive electrode material of claim 8.
10. An electrical equipment, characterized in that: Includes the lithium ion battery as claimed in claim 9.
Citation Information
Patent Citations
Nickel-containing hydroxide precursor, preparation method thereof and positive electrode material
CN112978813A
Positive electrode material precursor and preparation method thereof, lithium ion battery positive electrode material and lithium ion battery
CN115771916A
Lithium ion battery positive electrode material precursor and preparation method thereof, lithium ion battery positive electrode material, lithium ion battery and electric equipment
CN116425219A
Lithium ion battery positive electrode material, preparation method therefor, and lithium ion battery
US20220246978A1
Lithium battery positive electrode material precursor, preparation method therefor and application thereof
WO2022242596A1