Solar cell

By stacking the first silicon oxide layer and the first wide bandgap metal oxide layer on the crystalline silicon absorption layer of the solar cell, the problems of high front surface recombination rate and large interface contact resistance are solved, the charge transfer efficiency is improved and the light emission is reduced. Parasitic absorption improves the overall efficiency of solar cells.

WO2024217475A1PCT designated stage expired Publication Date: 2024-10-24LONGI GREEN ENERGY TECH CO LTD

Patent Information

Application Number
PCT/CN2024/088443
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-23
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing solar cells have a high surface recombination rate on the front surface, which limits the improvement of cell efficiency. When using wide bandgap materials as passivation layers, there are problems such as high interface contact resistance or serious light parasitic absorption.

Method used

The first silicon oxide layer, the first wide band gap metal oxide layer and the first protective layer are sequentially stacked on the light receiving surface of the crystalline silicon absorption layer. The first wide band gap metal oxide layer is formed of doped metal oxide. Impurity elements diffuse into the silicon absorption layer through the silicon oxide layer to form a doped region, optimizing interface contact and carrier transport.

Benefits of technology

It effectively reduces the surface recombination rate, improves charge transfer efficiency, reduces light parasitic absorption, and improves the overall efficiency of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024088443_24102024_PF_FP_ABST
    Figure CN2024088443_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A solar cell, comprising a crystalline silicon absorption layer and, successively stacked on a light-receiving surface of the crystalline silicon absorption layer, a first silicon oxide layer, a first broad band gap metal oxide layer, a first protection layer and a front surface electrode, the first broad band gap metal oxide layer being formed by doped metal oxide, and elements with which the first broad band gap metal oxide layer is doped diffusing to the crystalline silicon absorption layer via the first silicon oxide layer so as to form a first doped region. A multilayer silicon oxide / broad band gap oxide structure is used as a selective contact and transport layer of the silicon solar cell, and a high-temperature process is used for forming a hole structure in the silicon oxide, such that the elements with which the broad band gap oxide is doped further diffuse to the surface of the crystalline silicon, thereby avoiding great photo-parasitic absorption, obtaining a better field passivation effect, and improving the efficiency of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

solar cells

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the Patent Office of China on April 17, 2023, with application number 202310411689.6 and invention name “Solar cell with a wide band gap oxide structure on the front surface”, and the priority to the Chinese patent application filed with the Patent Office of China on April 23, 2023, with application number 202310444710.2 and invention name “Solar cell with a multilayer zinc oxide structure on the front surface”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application belongs to the technical field of solar cells, and in particular, relates to a solar cell. Background Art

[0004] The current front structure of the tunneling oxide passivated contact (TOPCon) cell still uses the same structure as the emitter rear passivated (PERC) cell. This structure has direct contact between the metal grid and the silicon absorption layer, resulting in a relatively high surface recombination rate on the front surface of the cell, limiting the further improvement of the TOPCon cell efficiency.

[0005] The POLO structure can improve these issues, but the introduction of a doped polysilicon transport layer on the front of the crystalline silicon cell results in strong parasitic absorption, which also limits the improvement of cell efficiency. Currently, many studies use wide-bandgap materials as passivation contact layers, generally using low-temperature processes and a complete silicon oxide layer as the passivation layer, resulting in high interface contact resistance and severe efficiency loss. Alternatively, amorphous silicon passivation is used, resulting in severe parasitic absorption losses.

[0006] Current heterojunction (HJT) cells use materials such as TCO as the transmission layer, which also causes strong optical parasitic absorption and leads to loss of cell efficiency.

[0007] Summary of the Invention

[0008] In response to the problems existing in the prior art, the present application provides a solar cell having a wide bandgap oxide structure on the front surface.

[0009] Specifically, this application involves the following aspects:

[0010] A solar cell comprises a crystalline silicon absorption layer, and a first silicon oxide layer, a first wide bandgap metal oxide layer, a first protective layer and a front surface electrode stacked in sequence on a light-receiving surface of the crystalline silicon absorption layer.

[0011] The first wide band gap metal oxide layer is formed of doped metal oxide, and the doped elements in the first wide band gap metal oxide layer diffuse into the crystalline silicon absorption layer through the first silicon oxide layer to form a first doped region.

[0012] Optionally, the thickness of the first silicon oxide layer is 0.5-4 nm.

[0013] Optionally, the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers, and preferably, the thickness of the first silicon oxide layer is less than or equal to 8 atomic layers.

[0014] Optionally, the first silicon oxide layer has pores formed by calcination.

[0015] Optionally, the first wide band gap metal oxide layer includes a first zinc oxide layer and a second zinc oxide layer, the thickness of the first zinc oxide layer is 3-10 nm, and the thickness of the second zinc oxide layer is 10-200 nm;

[0016] Or, the second zinc oxide layer is a doped zinc oxide layer, and the doping concentration of the second zinc oxide layer is greater than the doping concentration of the first zinc oxide layer;

[0017] Alternatively, the sheet resistance of the second zinc oxide layer is smaller than the sheet resistance of the first zinc oxide layer.

[0018] Optionally, the second zinc oxide layer has a columnar crystal structure.

[0019] Optionally, a front surface anti-reflection layer is further provided on a side of the second zinc oxide layer away from the crystalline silicon absorption layer, and the front surface electrode penetrates the front surface anti-reflection layer and contacts the second zinc oxide layer.

[0020] Optionally, the polycrystallization degree of the first wide band gap metal oxide layer increases gradually from a side close to the first oxide layer to a side far away from the first oxide layer.

[0021] Optionally, the material of the first protective layer is selected from one or more of silicon nitride, titanium oxide, zinc sulfide, aluminum oxide, aluminum nitride, silicon oxide, etc.

[0022] Optionally, the thickness of the first protective layer is 10-100 nm.

[0023] Optionally, the front surface electrode penetrates the first protective layer and contacts the first wide band gap metal oxide layer.

[0024] Optionally, a front surface anti-reflection layer is further provided on a side of the first protective layer away from the crystalline silicon absorption layer, and the front surface electrode penetrates the front surface anti-reflection layer and the first protective layer and contacts the first wide bandgap metal oxide layer.

[0025] Optionally, the solar cell further comprises a second silicon oxide layer, a second wide bandgap metal oxide layer, a second protective layer, and a back surface electrode stacked in sequence on the backlight side of the crystalline silicon absorption layer, wherein the back surface electrode penetrates the second protective layer and contacts the second wide bandgap metal oxide layer.

[0026] The second wide band gap metal oxide layer is formed of a doped metal oxide, and the doped elements in the second wide band gap metal oxide layer diffuse into the crystalline silicon absorption layer through the second silicon oxide layer to form a second doped region.

[0027] The second wide band gap metal oxide layer and the first wide band gap metal oxide layer have opposite charge transport properties.

[0028] Optionally, the thickness of the second silicon oxide layer is 0.5-4 nm.

[0029] Optionally, the second silicon oxide layer has pores formed by calcination.

[0030] Optionally, the metal oxide used in the first wide band gap metal oxide layer or the second wide band gap metal oxide layer is selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, rhenium oxide, etc.

[0031] Optionally, the thickness of the first wide band gap metal oxide layer or the second wide band gap metal oxide layer is 10-200 nm.

[0032] Optionally, the polycrystallization degree of the second wide band gap metal oxide layer increases gradually from a side close to the second oxide layer to a side far from the second oxide layer.

[0033] Optionally, the material of the second protective layer is selected from silicon nitride or aluminum nitride.

[0034] Optionally, the thickness of the second protective layer is 10-100 nm.

[0035] Optionally, a back anti-reflection layer is further provided on a side of the second protective layer away from the crystalline silicon absorption layer, and the back surface electrode penetrates the back anti-reflection layer and the second protective layer and contacts the second wide bandgap metal oxide layer.

[0036] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are specifically listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0038] FIG1 is a schematic structural diagram of a solar cell according to an embodiment of the present application;

[0039] FIG2 is a schematic structural diagram of a solar cell according to another embodiment of the present application;

[0040] FIG3 is a schematic structural diagram of a solar cell according to another embodiment of the present application;

[0041] FIG4 is a schematic structural diagram of a solar cell according to another embodiment of the present application;

[0042] FIG5 is a schematic structural diagram of a solar cell according to an embodiment of the present application;

[0043] FIG6 is a schematic structural diagram of a solar cell according to another embodiment of the present application;

[0044] FIG7 is a schematic structural diagram of a solar cell according to another embodiment of the present application.

[0045] Reference numerals:

[0046] Figures 1 to 4, 1 crystalline silicon absorption layer, 21 first silicon oxide layer, 22 first wide bandgap metal oxide layer, 23 first protective layer, 24 first doped region, 31 back passivation layer, 32 back anti-reflection layer; 4 front surface electrode, 5 back surface electrode, 61 back tunneling passivation layer, 62 first back transmission layer, 63 back anti-reflection layer, 71 amorphous silicon passivation layer, 72 second back transmission layer, 73 third back transmission layer, 81 second silicon oxide layer, 82 second wide bandgap metal oxide layer, 83 second protective layer, 84 second doped region;

[0047] Figures 5 to 7, 1 crystalline silicon absorption layer, 21 first zinc oxide layer, 22 second zinc oxide layer, 31 back passivation layer, 32 back anti-reflection layer; 4 front surface electrode, 5 back surface electrode, 61 back tunneling passivation layer, 62 first back transmission layer, 71 amorphous silicon passivation layer, 72 second back transmission layer, 73 third back transmission layer. Specific embodiments

[0048] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0049] The present application is further described below with reference to examples. It should be understood that the examples are only used to further illustrate and explain the present application and are not intended to limit the present application.

[0050] Unless otherwise defined, technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art. Although methods and materials similar or identical to those described herein may be used in experiments or practical applications, the materials and methods are described herein below. In the event of a conflict, the present specification, including definitions, will prevail. In addition, the materials, methods, and examples are provided for illustrative purposes only and are not intended to be limiting. The present application is further described below with reference to specific examples, which are not intended to limit the scope of this application.

[0051] The present application provides a solar cell, as shown in Figures 1 to 4, comprising a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide, and the doped element in the first wide-bandgap metal oxide layer 22 diffuses into the crystalline silicon absorber layer 1 through the first silicon oxide layer 21, forming a first doped region 24.

[0052] The first silicon oxide layer 21 is formed of silicon oxide and serves as a chemical passivation layer. In one embodiment, the thickness of the first silicon oxide layer 21 is 0.5-4 nm, for example, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, or any range therebetween. This ultra-thin structure of the first silicon oxide layer 21 serves two primary functions: 1. It chemically passivates the crystalline silicon surface, reducing surface recombination; and 2. It acts as a tunneling agent during charge transport, facilitating charge transport and improving battery efficiency.

[0053] In a specific embodiment, the first silicon oxide layer 21 has pores formed by calcination. The presence of the pores allows the doped elements in the first wide bandgap metal oxide layer 22 to diffuse into the crystalline silicon absorption layer 1 to form the first doped region 24 .

[0054] A first wide-bandgap metal oxide layer 22 overlies the first silicon oxide layer 21, i.e., on the side of the first silicon oxide layer 21 facing away from the crystalline silicon absorber layer 1. The first wide-bandgap metal oxide layer 22 provides field effects, selective contact, and carrier transport. The first wide-bandgap metal oxide layer 22 is formed from a doped metal oxide. The dopants that can be doped are commonly known in the art, such as aluminum, gallium, indium, and trace amounts of transition metals or rare earth elements, such as nickel, copper, lanthanum, iridium, and actinium.

[0055] The wide bandgap material in the first wide bandgap metal oxide layer 22 can reduce the optical parasitic absorption caused by doped amorphous silicon and TCO. If this structure is used on the front surface of PERC and TOPCon cells, the interface contact between the electrode and crystalline silicon can also be optimized to reduce contact recombination.

[0056] In a specific embodiment, the metal oxide used in the first wide bandgap metal oxide layer 22 is selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, and rhenium oxide.

[0057] In a specific embodiment, the thickness of the first wide band gap metal oxide layer 22 is 10-200 nm, for example, it can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or any range therebetween.

[0058] In a specific embodiment, the polycrystallization degree of the first wide bandgap metal oxide layer 22 increases gradually from the side close to the first oxide layer 21 to the side far from the first oxide layer 21 (ie, the side close to the first protective layer 23 ).

[0059] In a specific embodiment, the first wide band gap metal oxide layer 22 gradually transitions from an amorphous structure to a polycrystalline structure from a side close to the first oxide layer 21 to a side far from the first oxide layer 21 .

[0060] The material of the first protective layer 23 can be selected from one or more of silicon nitride, titanium oxide, zinc sulfide, aluminum oxide, and aluminum nitride, providing stability and anti-reflection properties. The first protective layer 23 may include dopants such as aluminum, gallium, and indium, as well as trace amounts of transition metals or rare earth elements such as nickel, copper, lanthanum, iridium, and actinium.

[0061] In a specific embodiment, the thickness of the first protective layer 23 is 10-100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, or any range therebetween.

[0062] First doped region 24 is formed by the element doped in first wide-bandgap metal oxide layer 22, diffused through first silicon oxide layer 21 toward crystalline silicon absorber layer 1. It extends from the side of first wide-bandgap metal oxide layer 22 closest to crystalline silicon absorber layer 1 to crystalline silicon absorber layer 1. First doped region 24 optimizes interface resistance, passivates crystalline silicon, and reduces interface recombination.

[0063] The crystalline silicon absorption layer 1 may be an n-type or p-type silicon wafer known in the art, with a thickness of 60-150 μm.

[0064] The front surface electrode 4 is disposed on the light-receiving surface of the solar cell and penetrates the first protective layer 23 to contact the first wide bandgap metal oxide layer 22 .

[0065] Those skilled in the art will appreciate that, according to actual needs, a front surface anti-reflection layer may be provided on the side of the wide bandgap metal oxide layer 22 away from the crystalline silicon absorption layer 1 , and the front surface electrode 4 passes through the front surface anti-reflection layer and the first protective layer 23 and contacts the wide bandgap metal oxide layer 22 .

[0066] The solar cell of the present application can be any type of solar cell including the above-mentioned structure on the light-receiving surface, for example, an emitter back-side passivation cell, a tunneling oxide layer passivation contact cell, a heterojunction cell, etc. Those skilled in the art can select the corresponding back-side structure according to different solar cell types.

[0067] In a specific embodiment, the solar cell structure is shown in Figure 1, and the solar cell is an emitter back passivation cell. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide bandgap metal oxide layer 22. The first wide bandgap metal oxide layer 22 is formed of a doped metal oxide, and the doped elements in the first wide bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the back-light side of the crystalline silicon absorption layer 1 with a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorption layer 1.

[0068] The back passivation layer 31 may be a single layer of aluminum oxide or a stacked structure of aluminum oxide and silicon oxide.

[0069] In one specific embodiment, the solar cell structure is shown in FIG1 , and the solar cell is an emitter back passivation cell. The solar cell includes a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped element in the first wide-bandgap metal oxide layer 22 diffuses through the first silicon oxide layer 21 into the crystalline silicon absorber layer 1, forming a first doped region 24. The first silicon oxide layer 21 has a thickness of 0.5-4 nm and has pores formed by calcination. The first wide-bandgap metal oxide layer 22 is made of a metal oxide selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, and rhenium oxide, and has a thickness of 10-200 nm. The polycrystallization degree of the first wide-bandgap metal oxide layer 22 increases from the side closest to the first oxide layer 21 to the side farther away from the first oxide layer 21. The first protective layer 23 is made of silicon nitride or aluminum nitride and has a thickness of 10-100 nm. The solar cell is provided with a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5 stacked in sequence on the backlight side of the crystalline silicon absorber layer 1. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorber layer 1.

[0070] In a specific embodiment, the solar cell structure is shown in Figure 2, and the solar cell is a tunneling oxide layer passivation contact cell. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide bandgap metal oxide layer 22, a first protective layer 23 and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide bandgap metal oxide layer 22. The first wide bandgap metal oxide layer 22 is formed by doping metal oxide, and the doped elements in the first wide bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorption layer 1 with a back tunneling passivation layer 61, a first back transmission layer 62 and a back surface electrode 5.

[0071] The back tunneling passivation layer 61 is a silicon oxide layer, and the first back transmission layer 62 is a p-type doped polysilicon layer.

[0072] Those skilled in the art will understand that, according to actual needs, a back anti-reflection layer 63 is further provided on the side of the first back transmission layer 62 away from the crystalline silicon absorption layer 1 , and the back surface electrode 5 passes through the back anti-reflection layer 63 and contacts the first back transmission layer 62 .

[0073] In one specific embodiment, the solar cell structure is shown in FIG2 , and the solar cell is a tunneling oxide layer passivated contact cell. The solar cell includes a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped element in the first wide-bandgap metal oxide layer 22 diffuses through the first silicon oxide layer 21 into the crystalline silicon absorber layer 1, forming a first doped region 24. The first silicon oxide layer 21 has a thickness of 0.5-4 nm and has pores formed by calcination. The first wide-bandgap metal oxide layer 22 is made of a metal oxide selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, and rhenium oxide, and has a thickness of 10-200 nm. The polycrystallization degree of the first wide-bandgap metal oxide layer 22 increases from the side closest to the first oxide layer 21 to the side farther away from the first oxide layer 21. The first protective layer 23 is made of silicon nitride or aluminum nitride and has a thickness of 10-100 nm. The solar cell is sequentially stacked on the backlight side of the crystalline silicon absorption layer 1 with a back tunneling passivation layer 61, a first back transport layer 62, a back anti-reflection layer, and a back surface electrode 5. The back surface electrode 5 penetrates the back anti-reflection layer and contacts the first back transport layer 62.

[0074] In a specific embodiment, the solar cell structure is shown in Figure 3, and the solar cell is a heterojunction cell. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide bandgap metal oxide layer 22. The first wide bandgap metal oxide layer 22 is formed by doping metal oxides, and the doped elements in the first wide bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorption layer 1 with an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, and a back surface electrode 5.

[0075] The amorphous silicon passivation layer 71 is formed of amorphous silicon, the second back transmission layer 72 is formed of p-type doped amorphous silicon, and the third back transmission layer 73 can be a silver electrode.

[0076] Those skilled in the art will understand that, according to actual needs, a back anti-reflection layer is further provided on the side of the third back transmission layer 73 away from the crystalline silicon absorption layer 1 , and the back surface electrode 5 penetrates the back anti-reflection layer and contacts the third back transmission layer 73 .

[0077] In one specific embodiment, the solar cell structure is shown in FIG3 , and the solar cell is a heterojunction cell. The solar cell includes a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped element in the first wide-bandgap metal oxide layer 22 diffuses through the first silicon oxide layer 21 into the crystalline silicon absorber layer 1, forming a first doped region 24. The first silicon oxide layer 21 has a thickness of 0.5-4 nm and has pores formed by calcination. The first wide-bandgap metal oxide layer 22 is made of a metal oxide selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, and rhenium oxide, and has a thickness of 10-200 nm. The polycrystallization degree of the first wide-bandgap metal oxide layer 22 increases from the side closest to the first oxide layer 21 to the side farther away from the first oxide layer 21. The first protective layer 23 is made of silicon nitride or aluminum nitride and has a thickness of 10-100 nm. The solar cell is sequentially stacked on the backlight side of the crystalline silicon absorption layer 1 with an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, a back anti-reflection layer, and a back surface electrode 5. The back surface electrode 5 penetrates the back anti-reflection layer and contacts the third back transmission layer 73.

[0078] In a specific embodiment, the solar cell structure is shown in FIG4 , and the solar cell is a double-sided wide-bandgap oxide tunneling structure. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide, and the doped elements in the first wide-bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorption layer 1 with a second silicon oxide layer 81, a second wide-bandgap metal oxide layer 82, a second protective layer 83, and a back surface electrode 5. The back surface electrode 5 penetrates the second protective layer 83 and contacts the second wide-bandgap metal oxide layer 82. The second wide-bandgap metal oxide layer 82 is formed of a doped metal oxide. The doped element in the second wide-bandgap metal oxide layer 82 diffuses through the second silicon oxide layer 81 into the crystalline silicon absorption layer 1, forming a second doped region 84. The second wide-bandgap metal oxide layer 82 has opposite charge transport properties to the first wide-bandgap metal oxide layer 22.

[0079] The function, material, thickness range, and morphology of the second silicon oxide layer 81 are the same as those of the first silicon oxide layer 21. The function, material, thickness range, and degree of polycrystallization of the second wide-bandgap metal oxide layer 82 are the same as those of the first wide-bandgap metal oxide layer 22. The function, material, and thickness range of the second protective layer 83 are the same as those of the first protective layer 83. The function and selection of doping elements of the second doping region 84 are the same as those of the first doping region 24. The opposite charge transport properties of the second wide-bandgap metal oxide layer 82 and the first wide-bandgap metal oxide layer 22 mean that if the first wide-bandgap metal oxide layer 22 is an electron-selective contact layer, the second wide-bandgap metal oxide layer 82 is a hole-selective contact layer; and if the first wide-bandgap metal oxide layer 22 is a hole-selective contact layer, the second wide-bandgap metal oxide layer 82 is an electron-selective contact layer.

[0080] In a specific embodiment, the solar cell structure is shown in FIG4 , and the solar cell is a double-sided wide-bandgap oxide tunneling structure. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide, and the doped elements in the first wide-bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorption layer 1 with a second silicon oxide layer 81, a second wide-bandgap metal oxide layer 82, a second protective layer 83, and a back surface electrode 5. The back surface electrode 5 penetrates the second protective layer 83 and contacts the second wide-bandgap metal oxide layer 82. The second wide-bandgap metal oxide layer 82 is formed of a doped metal oxide. The doped element in the second wide-bandgap metal oxide layer 82 diffuses through the second silicon oxide layer 81 into the crystalline silicon absorption layer 1, forming a second doped region 84. The second wide-bandgap metal oxide layer 82 has opposite charge transport properties to the first wide-bandgap metal oxide layer 22. The first silicon oxide layer 21 and the second oxide layer 81 have a thickness of 0.5-4 nm and contain pores formed by calcination. The metal oxide used in the first wide-bandgap metal oxide layer 22 and the second wide-bandgap metal oxide layer 82 is selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, and rhenium oxide, and has a thickness of 10-200 nm. The first protective layer 23 and the second protective layer 83 are selected from silicon nitride or aluminum nitride, and have a thickness of 10-100 nm.

[0081] Example

[0082] Example 1

[0083] The solar cell structure is shown in Figure 1. The solar cell is an emitter back-passivated cell. The solar cell comprises a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed from a doped metal oxide. The doped elements in the first wide-bandgap metal oxide layer 22 diffuse into the crystalline silicon absorber layer 1 through the first silicon oxide layer 21, forming a first doped region 24. The solar cell comprises a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5, which are sequentially stacked on the back-light-receiving surface of the crystalline silicon absorber layer 1. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorber layer 1.

[0084] Specifically, the steps for preparing a solar cell are as follows:

[0085] 1. Silicon wafer cleaning

[0086] The sample substrate is a single crystal silicon wafer (n-type) with a textured front surface. The substrate is cleaned using a standard RCA (Radio Corporation of America) cleaning process, then repeatedly rinsed with deionized water, and blown dry with nitrogen gas for use.

[0087] 2. Silicon oxide film preparation

[0088] A SiO2 passivation layer 21 is oxidized on the front surface of the silicon wafer using thermal oxidation method, and its thickness is about 1.7nm. 3. Preparation of zinc oxide film

[0089] A phosphorus-doped zinc oxide film 22 with a thickness of approximately 40 nm was prepared using an ALD method at a temperature of 160 degrees Celsius. The gas sources used were diethyl zinc, deionized water, and diborane. The cycle steps were: diethyl zinc pulse for 0.1 second, nitrogen purge for 10 seconds, deionized water pulse for 0.1 second, and nitrogen purge for 10 seconds. During the above cycle, diborane was introduced into the reaction chamber light, and the cycle ratio of diborane to diethyl zinc was 1:2.

[0090] 4. Front silicon nitride preparation

[0091] A 60 nm thick silicon nitride layer 23 is deposited on the layer 22 to form a silicon nitride capping layer on the front side of the silicon wafer.

[0092] 5. Backside aluminum oxide / silicon nitride preparation

[0093] A 15 nm thick aluminum oxide layer 31 is first deposited on the back of the silicon wafer by PECVD; an 80 nm thick silicon nitride layer 32 is deposited thereon to form an aluminum oxide / silicon nitride stacked passivation film on the back of the silicon wafer.

[0094] 6. Laser grooving on the aluminum oxide film on both sides

[0095] A pulsed laser is used to create grooves on the front side of the silicon wafer, partially penetrating the silicon nitride film layer 23 to expose layer 22. The metal electrode then contacts layer 22 through the grooves in the film. A laser is used on the back side to partially penetrate the aluminum oxide film layer to expose the silicon body layer 1. The metal electrode then contacts layer 1 through the grooves in the film.

[0096] 7. Electrode Preparation

[0097] The back silver electrode, back aluminum paste, and front silver electrode are screen-printed and dried. Finally, the silicon wafer is sent to a sintering furnace for sintering and calcining at 930°C. During this process, the dopant elements in the 22 layers diffuse through the 21st layer to the 1st layer, forming the 24th layer, completing the solar cell fabrication.

[0098] Example 2

[0099] The solar cell structure is shown in Figure 2. The solar cell is a tunneling oxide layer passivation contact cell. The solar cell includes a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide bandgap metal oxide layer 22. The first wide bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped elements in the first wide bandgap metal oxide layer 22 diffuse into the crystalline silicon absorber layer 1 through the first silicon oxide layer 21, forming a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorber layer 1 with a back tunneling passivation layer 61, a first back transmission layer 62, a back anti-reflection layer 63, and a back surface electrode 5.

[0100] Specifically, the steps for preparing a solar cell are as follows:

[0101] 1. Silicon wafer cleaning

[0102] The sample substrate is a single crystal silicon wafer (p-type) with a textured front surface. The substrate is cleaned using a standard RCA (Radio Corporation of America) cleaning process, then repeatedly rinsed with deionized water, and blown dry with nitrogen gas for use.

[0103] 2. Silicon oxide film preparation

[0104] The SiO2 tunnel passivation layers 21 and 61 are oxidized on the front and back surfaces of the silicon wafer by ultraviolet ozone oxidation method, and the thickness of each layer is 1.8 nm.

[0105] 3. Preparation of Nickel Oxide Thin Film

[0106] A boron-doped nickel oxide film 22 with a thickness of approximately 35 nm was deposited using an ALD method at 150°C. The nickel, boron, and oxygen sources used were bis-(N,N'-di-tert-butylacetamido) nickel (II), a diborane / hydrogen mixture, and deionized water. The cycle consisted of a 0.1-second pulse of bis-(N,N'-di-tert-butylacetamido) nickel (II), a 10-second nitrogen purge, a 0.1-second pulse of deionized water, and a 10-second nitrogen purge. During this process, a hexahydroboron / hydrogen mixture was introduced into the reaction chamber, with a 1:3 ratio of bis-(N,N'-di-tert-butylacetamido) nickel (II) to the bis-(N,N'-di-tert-butylacetamido) nickel (II).

[0107] 4. Preparation of back-side amorphous silicon

[0108] The polysilicon film 62 is directly prepared by introducing hydrogen-diluted silane through the PECVD method, and its thickness is about 100 nm.

[0109] 5. Silicon Nitride Film Preparation

[0110] Silicon nitride layers 23 and 63 are deposited on layers 22 and 62 respectively, with a thickness of about 80 nm, to form silicon nitride capping layers on the front and back sides of the silicon wafer.

[0111] 6. Electrode Preparation

[0112] The back silver electrode, back aluminum paste, and front silver electrode are screen-printed and dried, and finally the silicon wafer is sent to a sintering furnace for sintering and calcining at 900°C. During this process, the dopant elements in the 22 layers diffuse through the 21st layer to the 1st layer, forming the 24th layer, completing the solar cell production.

[0113] Example 3

[0114] The solar cell structure is shown in Figure 3. The solar cell is a heterojunction cell. The solar cell includes a crystalline silicon absorption layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped elements in the first wide-bandgap metal oxide layer 22 diffuse into the crystalline silicon absorption layer 1 through the first silicon oxide layer 21 to form a first doped region 24. The solar cell is stacked in sequence on the backlight side of the crystalline silicon absorption layer 1 with an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, and a back surface electrode 5.

[0115] Specifically, the steps for preparing a solar cell are as follows:

[0116] 1. Silicon wafer cleaning

[0117] The sample substrate is a double-sided textured single crystal silicon wafer (n-type). The substrate is cleaned using a standard RCA (Radio Corporation of America) cleaning process, then repeatedly rinsed with deionized water, and blown dry with nitrogen before use.

[0118] 2. Silicon oxide film preparation

[0119] The SiO2 tunnel passivation layer 21 is oxidized on the front surface of the silicon wafer by ultraviolet ozone oxidation method, and the thickness of the layer is about 1.8 nm.

[0120] 3. Preparation of zinc oxide thin films

[0121] A phosphorus-doped zinc oxide film 22 with a thickness of approximately 40 nm was prepared using an ALD method at a temperature of 160 degrees Celsius. The gas sources used were diethyl zinc, deionized water, and diborane. The cycle steps were: diethyl zinc pulse for 0.1 second, nitrogen purge for 10 seconds, deionized water pulse for 0.1 second, and nitrogen purge for 10 seconds. During the above cycle, diborane was introduced into the reaction chamber light, and the cycle ratio of diborane to diethyl zinc was 1:2.

[0122] 4. Alumina Layer Preparation

[0123] An aluminum oxide thin film layer 23 is deposited on the front surface using an ALD process. A high-temperature calcination process is used, calcined at 930°C. During this process, the doping elements in the 22nd layer diffuse through the 21st layer to the 1st layer to form the 24th layer.

[0124] 5. Amorphous silicon deposition

[0125] The intrinsic amorphous silicon thin film layer 71 and the doped amorphous silicon thin film layer 72 are prepared by ion implantation, wherein the thickness of layer 71 is about 3 nm and the thickness of layer 72 is about 30 nm, and an annealing method is used for activation process.

[0126] 6.TCO deposition

[0127] A transparent conductive thin film layer 73 is prepared on the surface of the silicon wafer by reactive plasma deposition or magnetron sputtering, and the thickness of the transparent conductive thin film layer 73 is about 40 nm.

[0128] 7. Laser grooving on the front aluminum oxide film

[0129] A pulsed laser is used to create grooves on the front side of the silicon wafer, partially penetrating the aluminum oxide film layer 23 to expose the 22 layer, and the metal electrode contacts the 22 layer through the grooves on the film.

[0130] 8. Electrode Preparation

[0131] The back silver electrode, back aluminum paste, and front silver electrode are screen-printed and dried, and finally the silicon wafer is sent to a sintering furnace for sintering to complete the preparation of the solar cell.

[0132] Example 4

[0133] The solar cell structure is shown in Figure 4. The solar cell is a double-sided wide-bandgap oxide tunneling structure. The solar cell includes a crystalline silicon absorber layer 1, and a first silicon oxide layer 21, a first wide-bandgap metal oxide layer 22, a first protective layer 23, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. The front surface electrode 4 penetrates the first protective layer 23 and contacts the first wide-bandgap metal oxide layer 22. The first wide-bandgap metal oxide layer 22 is formed of a doped metal oxide. The doped elements in the first wide-bandgap metal oxide layer 22 diffuse into the crystalline silicon absorber layer 1 through the first silicon oxide layer 21, forming a first doped region 24. The solar cell includes a second silicon oxide layer 81, a second wide-bandgap metal oxide layer 82, a second protective layer 83, and a back surface electrode 5, which are sequentially stacked on the backlight side of the crystalline silicon absorber layer 1. The back surface electrode 5 penetrates the second protective layer 83 and contacts the second wide-bandgap metal oxide layer 82. The second wide-bandgap metal oxide layer 82 is formed of a doped metal oxide. The doped element in the second wide-bandgap metal oxide layer 82 diffuses through the second silicon oxide layer 81 into the crystalline silicon absorption layer 1, forming a second doped region 84. The second wide-bandgap metal oxide layer 82 has opposite charge transport properties to the first wide-bandgap metal oxide layer 22.

[0134] Specifically, the steps for preparing a solar cell are as follows:

[0135] 1. Silicon wafer cleaning

[0136] The sample substrate is a double-sided textured single crystal silicon wafer (n-type, resistivity 0.5-2.0Ω.cm, thickness 0.15-0.2mm). The substrate is cleaned using a standard RCA (Radio Corporation of America) cleaning process, then repeatedly rinsed with deionized water and blown dry with nitrogen for use.

[0137] 2. Silicon oxide film preparation

[0138] The SiO2 tunnel passivation layers 21 and 81 are oxidized on both sides of the silicon wafer by thermal oxidation method, with a thickness of 1.7 nm.

[0139] 3. Preparation of Nickel Oxide Thin Film

[0140] A boron-doped nickel oxide film 22 with a thickness of approximately 30 nm was deposited using an ALD method at 150°C. The nickel, boron, and oxygen sources used were bis-(N,N'-di-tert-butylacetamido) nickel (II), a diborane / hydrogen mixture, and deionized water. The cycle consisted of a 0.1-second pulse of bis-(N,N'-di-tert-butylacetamido) nickel (II), a 10-second nitrogen purge, a 0.1-second pulse of deionized water, and a 10-second nitrogen purge. During this process, a hexahydroboron / hydrogen mixture was introduced into the reaction chamber, with a 1:3 ratio of bis-(N,N'-di-tert-butylacetamido) nickel (II) to the bis-(N,N'-di-tert-butylacetamido) nickel (II).

[0141] 4. Preparation of zinc oxide thin films

[0142] A fluorine-doped zinc oxide film 82 with a thickness of approximately 40 nm was prepared by the ALD method at a temperature of 160 degrees Celsius. The zinc, fluorine, and oxygen sources used were a mixture of diethyl zinc, deionized water, and hydrofluoric acid (v:v = 200:1). The cycle steps were: diethyl zinc pulse for 0.1 second, nitrogen purge for 10 seconds, deionized water / hydrofluoric acid mixture pulse for 0.1 second, and nitrogen purge for 10 seconds.

[0143] 5. Alumina Layer Preparation

[0144] The PECVD process is used to deposit Al2O3 passivation layers 23 and 83 on both sides. A high-temperature calcination process is used, calcined at 950°C. During this process, the doping elements in the 22 layer will diffuse through the 21 layer to the 1 layer to form the 24 layer.

[0145] 6. Laser grooving on the aluminum oxide film on both sides

[0146] A pulsed laser is used to create grooves on both sides of the silicon wafer, partially breaking through the aluminum oxide film layer to expose the aluminum oxide layers 23 and 83. The metal electrode contacts the doped oxide layers 22 and 82 through the grooves on the film.

[0147] 7. Preparation of positive and negative electrodes

[0148] The back silver electrode and the front silver electrode are screen-printed and dried, and finally the silicon wafer is sent to the sintering furnace for sintering to complete the preparation of the solar cell.

[0149] The present application provides a solar cell, as shown in Figures 5-7, comprising a crystalline silicon absorption layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. A first silicon oxide layer (not shown) is provided between the crystalline silicon absorption layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers.

[0150] Those skilled in the art will understand that when thickness is mentioned in this application, it refers to the average thickness of the corresponding film layer. For the thickness of the first silicon oxide layer to be less than or equal to 20 atomic layers, it means that the average thickness of the first silicon oxide layer is less than or equal to 20 atomic layers, for example, it can be 20 atomic layers, 19 atomic layers, 18 atomic layers, 17 atomic layers, 16 atomic layers, 15 atomic layers, 14 atomic layers, 13 atomic layers, 12 atomic layers, 11 atomic layers, 10 atomic layers, 9 atomic layers, 8 atomic layers, 7 atomic layers, 6 atomic layers, 5 atomic layers, 4 atomic layers, 3 atomic layers, 2 atomic layers, etc., or any range therebetween.

[0151] In a specific embodiment, the thickness of the first silicon oxide layer is less than or equal to 8 atomic layers.

[0152] An excessively thick first silicon oxide layer creates a high interface resistance, hindering the selective contact of carriers. The interface silicon oxide or interface silicon-oxygen bond eliminates the dangling bonds of silicon atoms on the surface of single-crystal silicon by forming bonds, thereby passivating the strong recombination centers formed by the dangling bonds. The silicon oxide or silicon-oxygen bond layer itself is a dielectric, an insulating material, which hinders the transport of carriers. When this layer is thin, electrons can tunnel through it, achieving carrier transport. The thinner the layer, the higher the tunneling efficiency and the stronger the conductivity.

[0153] The thickness of the first silicon oxide layer can be measured by characterization methods known in the art, such as transmission electron microscopy, deep etching secondary ion mass spectrometry, deep etching ultraviolet photoelectron spectroscopy and other high-precision interface characterization techniques.

[0154] The zinc oxide layer of the present application is composed of a first zinc oxide layer 21 and a second zinc oxide layer 22. The first zinc oxide layer 21 and the second zinc oxide layer 22 are prepared by a discontinuous process. Through characterization methods known in the art, such as transmission electron microscopy, it can be observed that the first zinc oxide layer 21 and the second zinc oxide layer 22 are two different layers.

[0155] The first zinc oxide layer 21 performs chemical passivation, field effect, and selective contact functions. The first zinc oxide layer 21 can be formed of undoped zinc oxide or doped zinc oxide, for example, including dopant components such as aluminum, gallium, indium, and trace amounts of transition metals or rare earth elements such as nickel, copper, lanthanum, iridium, and actinium.

[0156] In a specific embodiment, the thickness of the first zinc oxide layer 21 is 3-10 nm, for example, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any range therebetween.

[0157] In a specific embodiment, the first zinc oxide layer 21 is formed by atomic layer deposition (ALD).

[0158] In a specific embodiment, in the ALD method, an oxygen-containing metal source is used instead of an independent oxygen source such as water or ozone. The oxygen-containing metal source includes one or both of zinc ethoxide and zinc isopropoxide. Oxygen elements tend to combine with silicon elements, so controlling the oxygen content at the interface during the process is a key control point of the process. The process using an independent oxygen source is prone to excessive oxygen content at the interface, forming a thicker interface oxide layer; the use of an oxygen-containing metal source can effectively control the oxygen concentration at the interface during the process. This avoids the first silicon oxide layer obtained in the process of preparing the first zinc oxide layer 21 from being too thick, and the thickness of the interface zinc oxide layer can be controlled within 20 atomic layers.

[0159] In a specific embodiment, in the ALD method, the temperature used is 150-400°C, for example, it can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, or any range therebetween.

[0160] In the ALD method, metal sources known in the art, such as ZnCl2, Zn(CH3)2, Zn(C2H5)2, ZnCHCl, etc., can be used.

[0161] In one embodiment, the first zinc oxide layer 21 is deposited by atomic layer deposition (ALD). In the ALD method, an oxygen-containing metal source is used instead of an independent oxygen source. The oxygen-containing metal source includes one or both of zinc ethoxide and zinc isopropoxide. The metal source used is ZnCl2, Zn(CH3)2, Zn(C2H5)2, or ZnCHCl. ​​The temperature used is 150-400°C.

[0162] The second zinc oxide layer 22 overlies the first zinc oxide layer 21, i.e., on the side of the first zinc oxide layer 21 away from the crystalline silicon absorber layer 1. The second zinc oxide layer 22 performs selectivity regulation and carrier transport functions. The second zinc oxide layer 22 can be formed of undoped zinc oxide or doped zinc oxide, for example, including dopants such as aluminum, gallium, indium, and trace amounts of transition metals or rare earth elements such as nickel, copper, lanthanum, iridium, and actinium.

[0163] In a specific embodiment, the thickness of the second zinc oxide layer 22 is 10-200 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or any range therebetween.

[0164] In one specific embodiment, the second zinc oxide layer 22 has a columnar crystal structure. This columnar crystal structure facilitates vertical carrier transport, specifically, the transport process from the interior of the crystalline silicon to the exterior. The electron mobility within the zinc oxide crystal is high, meaning the electrons are small. The presence of grain boundaries between the crystals hinders electron migration, creating resistance. Columnar crystals have small electrons in the vertical direction and slightly higher, but controllable, resistance in the lateral direction. Therefore, columnar crystals facilitate the outward electron transport function of the second zinc oxide layer.

[0165] In a specific embodiment, the second zinc oxide layer 22 is a doped zinc oxide layer, and the doping concentration of the second zinc oxide layer 22 is greater than the doping concentration of the first zinc oxide layer 21 .

[0166] In a specific embodiment, the sheet resistance of the second zinc oxide layer 22 is smaller than the sheet resistance of the first zinc oxide layer 21 .

[0167] The crystalline silicon absorption layer 1 may be an n-type or p-type silicon wafer known in the art, with a thickness of 60-150 μm.

[0168] The front surface electrode 5 is provided on the light-receiving surface of the solar cell and is in contact with the second zinc oxide layer 22 .

[0169] Those skilled in the art will appreciate that, according to actual needs, a front surface anti-reflection layer may be provided on the side of the second zinc oxide layer 22 away from the crystalline silicon absorption layer 1 , and the front surface electrode 5 passes through the front surface anti-reflection layer and contacts the second zinc oxide layer 22 .

[0170] The solar cell of the present application can be any type of solar cell including the above-mentioned structure on the light-receiving surface, for example, an emitter back-side passivation cell, a tunneling oxide layer passivation contact cell, a heterojunction cell, etc. Those skilled in the art can select the corresponding back-side structure according to different solar cell types.

[0171] In one specific embodiment, the solar cell structure is shown in FIG5 . The solar cell is an emitter back passivation cell, comprising a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. A first silicon oxide layer is provided between the crystalline silicon absorber layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers. The solar cell is sequentially stacked on the backlight side of the crystalline silicon absorber layer 1 with a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorber layer 1.

[0172] The back passivation layer 31 may be a single layer of aluminum oxide or a stacked structure of aluminum oxide and silicon oxide.

[0173] In one specific embodiment, the solar cell structure is shown in Figure 5. The solar cell is an emitter back passivation cell, comprising a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. A first silicon oxide layer is located between the crystalline silicon absorber layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers. The first zinc oxide layer 21 has a thickness of 3-10 nm; the second zinc oxide layer 22 has a thickness of 10-200 nm, and the second zinc oxide layer 22 has a columnar crystal structure. The second zinc oxide layer 22 is a doped zinc oxide layer. The solar cell comprises a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5, which are sequentially stacked on the backlight surface of the crystalline silicon absorber layer 1. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorber layer 1.

[0174] In one specific embodiment, the solar cell structure is shown in FIG6 . The solar cell is a tunneling oxide layer passivated contact cell, comprising a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. A first silicon oxide layer is provided between the crystalline silicon absorber layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers. The solar cell is sequentially stacked on the backlight side of the crystalline silicon absorber layer 1 with a back tunneling passivation layer 61, a first back transmission layer 62, and a back surface electrode 5.

[0175] The back tunneling passivation layer 61 is a silicon oxide layer, and the first back transmission layer 62 is a p-type doped polysilicon layer.

[0176] Those skilled in the art will understand that, according to actual needs, a back anti-reflection layer is further provided on the side of the first back transmission layer 62 away from the crystalline silicon absorption layer 1 , and the back surface electrode 5 passes through the back anti-reflection layer and contacts the first back transmission layer 62 .

[0177] In one specific embodiment, the solar cell structure is shown in FIG6 . The solar cell is a tunneling oxide passivation contact cell, comprising a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. A first silicon oxide layer is disposed between the crystalline silicon absorber layer 1 and the first zinc oxide layer 21, with the thickness of the first silicon oxide layer being less than or equal to 20 atomic layers. The first zinc oxide layer 21 has a thickness of 3-10 nm; the second zinc oxide layer 22 has a thickness of 10-200 nm, has a columnar crystal structure, and is a doped zinc oxide layer. The solar cell comprises a back tunneling passivation layer 61, a first back transmission layer 62, a back anti-reflection layer, and a back surface electrode 5, stacked sequentially on the backlight side of the crystalline silicon absorber layer 1. The back surface electrode 5 penetrates the back anti-reflection layer and contacts the first back transmission layer 62.

[0178] In one specific embodiment, the solar cell structure is shown in FIG7 . The solar cell is a heterojunction cell and includes a crystalline silicon absorption layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4 stacked in sequence on the light-receiving surface of the crystalline silicon absorption layer 1. A first silicon oxide layer is provided between the crystalline silicon absorption layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers. The solar cell includes an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, and a back surface electrode 5 stacked in sequence on the backlight side of the crystalline silicon absorption layer 1.

[0179] The amorphous silicon passivation layer 71 is formed of amorphous silicon, the second back transmission layer 72 is formed of p-type doped amorphous silicon, and the third back transmission layer 73 can be made of ITO material or other transparent conductive film materials used as back transmission layers in the art.

[0180] Those skilled in the art will understand that, according to actual needs, a back anti-reflection layer is further provided on the side of the third back transmission layer 73 away from the crystalline silicon absorption layer 1 , and the back surface electrode 5 penetrates the back anti-reflection layer and contacts the third back transmission layer 73 .

[0181] In one specific embodiment, the solar cell structure is shown in Figure 7. The solar cell is a heterojunction cell and includes a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, which are sequentially stacked on the light-receiving surface of the crystalline silicon absorber layer 1. A first silicon oxide layer is located between the crystalline silicon absorber layer 1 and the first zinc oxide layer 21, and the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers. The thickness of the first zinc oxide layer 21 is 3-10 nm, and the thickness of the second zinc oxide layer 22 is 10-200 nm. The second zinc oxide layer 22 has a columnar crystal structure and is a doped zinc oxide layer. On the backlight side of the crystalline silicon absorber layer 1, the solar cell includes an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, a back anti-reflection layer, and a back surface electrode 5, which are sequentially stacked. The back surface electrode 5 extends through the back anti-reflection layer and contacts the third back transmission layer 73.

[0182] Example

[0183] Example 1

[0184] The solar cell structure is shown in Figure 5. The solar cell is an emitter back-passivated cell. The solar cell comprises a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, stacked sequentially on the light-receiving surface of the crystalline silicon absorber layer 1. On the back-light-reflecting surface of the crystalline silicon absorber layer 1, the solar cell comprises a back passivation layer 31, a back anti-reflection layer 32, and a back surface electrode 5, stacked sequentially. The back surface electrode 5 penetrates the back passivation layer 31 and the back anti-reflection layer 32 and contacts the crystalline silicon absorber layer 1.

[0185] Specifically, the steps for preparing a solar cell are as follows:

[0186] After conventional cell-electrochemical texturing and diffusion, a pn junction is formed on the front surface of the p-type silicon wafer, forming an n-type surface. A first zinc oxide layer 21 is deposited on the n-type surface using an ALD process. Zinc ethoxide is used as the oxygen-containing metal source during the deposition process at a temperature of 250°C. The resulting first zinc oxide layer 21 is 5 nm thick.

[0187] This process can obtain a first zinc oxide layer with almost no interfacial silicon oxide. The first silicon oxide layer is thickened during the subsequent process, and the overall thickness does not exceed 20 atomic layers.

[0188] The second zinc oxide layer 22 is prepared by remote plasma magnetron sputtering. The thickness of the second zinc oxide layer is 30 nm. A gradient doping scheme is adopted, and the doping concentration gradually increases from the side close to the first zinc oxide layer 21 to the side away from the first zinc oxide layer 21.

[0189] The other parts of the solar cell are prepared using the general process of PERC cells.

[0190] Example 2

[0191] The solar cell structure is shown in Figure 6. The solar cell is a tunneling oxide passivation contact cell. The solar cell comprises a crystalline silicon absorber layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, stacked sequentially on the light-receiving surface of the crystalline silicon absorber layer 1. On the backlight-reflecting surface of the crystalline silicon absorber layer 1, the solar cell comprises a back tunneling passivation layer 61, a first back transmission layer 62, a back anti-reflection layer, and a back surface electrode 5, which penetrates the back anti-reflection layer and contacts the first back transmission layer 62.

[0192] Specifically, the steps for preparing a solar cell are as follows:

[0193] After conventional battery cleaning and texturing of the n-type silicon wafer, the pn junction is not diffused. A first zinc oxide layer 21 is deposited on the n-type surface using an ALD process. Zn(CH3)2 is used as the oxygen-containing metal source during the deposition process at a temperature of 200°C. The resulting first zinc oxide layer 21 is 5nm thick.

[0194] This process can obtain a first zinc oxide layer with almost no interfacial silicon oxide. The first silicon oxide layer is thickened during the subsequent process, and the overall thickness does not exceed 20 atomic layers.

[0195] The second zinc oxide layer 22 is prepared by remote plasma magnetron sputtering. The thickness of the second zinc oxide layer is 30 nm. A gradient doping scheme is adopted, and the doping concentration gradually increases from the side close to the first zinc oxide layer 21 to the side far from the first zinc oxide layer 21.

[0196] The other parts of the solar cell are prepared using the general process of back-junction TOPCon cells.

[0197] Example 3

[0198] The solar cell structure is shown in Figure 7. The solar cell is a heterojunction cell. It includes a crystalline silicon absorption layer 1, and a first zinc oxide layer 21, a second zinc oxide layer 22, and a front surface electrode 4, stacked sequentially on the light-receiving surface of the crystalline silicon absorption layer 1. On the backlight side of the crystalline silicon absorption layer 1, the solar cell includes an amorphous silicon passivation layer 71, a second back transmission layer 72, a third back transmission layer 73, a back anti-reflection layer, and a back surface electrode 5, which extends through the back anti-reflection layer and contacts the third back transmission layer 73.

[0199] Specifically, the steps for preparing a solar cell are as follows:

[0200] After conventional battery cleaning, the n-type silicon wafer is cleaned, and the pn junction is not diffused. A first zinc oxide layer 21 is deposited on the n-type surface using an ALD process. Zinc ethoxide is used as the oxygen-containing metal source during the deposition process, and the temperature employed is 350°C. The resulting first zinc oxide layer 21 has a thickness of 5 nm.

[0201] This process can obtain a first silicon oxide layer with a thickness of about 8 atomic layers. Since other processes do not involve high-temperature processes, the first silicon oxide layer will not change during subsequent processes.

[0202] The second zinc oxide layer 22 is prepared by remote plasma magnetron sputtering. The thickness of the second zinc oxide layer is 30 nm. A gradient doping scheme is adopted, and the doping concentration gradually increases from the side close to the first zinc oxide layer 21 to the side far from the first zinc oxide layer 21.

[0203] The other parts of the solar cell are prepared using the general process of back-junction HJT cells.

[0204] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0205] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.

Claims

1. A solar cell comprising a crystalline silicon absorption layer, and a first silicon oxide layer, a first wide bandgap metal oxide layer, a first protective layer and a front surface electrode sequentially stacked on a light-receiving surface of the crystalline silicon absorption layer, in, The first wide band gap metal oxide layer is formed of doped metal oxide, and the doped elements in the first wide band gap metal oxide layer diffuse into the crystalline silicon absorption layer through the first silicon oxide layer to form a first doped region. 2 . The solar cell according to claim 1 , wherein the thickness of the first silicon oxide layer is 0.5-4 nm. 3 . The solar cell according to claim 1 , wherein the thickness of the first silicon oxide layer is less than or equal to 20 atomic layers, and preferably, the thickness of the first silicon oxide layer is less than or equal to 8 atomic layers. 4 . The solar cell according to claim 1 , wherein the first silicon oxide layer has holes formed by calcination.

5. The solar cell according to any one of claims 1 to 4, wherein the first wide bandgap metal oxide layer comprises a first zinc oxide layer and a second zinc oxide layer, the first zinc oxide layer has a thickness of 3-10 nm, and the second zinc oxide layer has a thickness of 10-200 nm; Or, the second zinc oxide layer is a doped zinc oxide layer, and the doping concentration of the second zinc oxide layer is greater than the doping concentration of the first zinc oxide layer; Alternatively, the sheet resistance of the second zinc oxide layer is smaller than the sheet resistance of the first zinc oxide layer. The solar cell according to claim 5 , wherein the second zinc oxide layer has a columnar crystal structure.

7. According to the solar cell of claim 6, a front surface anti-reflection layer is further provided on a side of the second zinc oxide layer away from the crystalline silicon absorption layer, and the front surface electrode penetrates the front surface anti-reflection layer and contacts the second zinc oxide layer. 8 . The solar cell according to claim 1 , wherein a degree of polycrystallization of the first wide bandgap metal oxide layer increases gradually from a side close to the first oxide layer to a side far from the first oxide layer. 9 . The solar cell according to claim 1 , wherein the material of the first protective layer is selected from one or more of silicon nitride, titanium oxide, zinc sulfide, aluminum oxide, aluminum nitride, silicon oxide, and the like. 10 . The solar cell according to claim 1 , wherein the first protective layer has a thickness of 10-100 nm. 11 . The solar cell according to claim 1 , wherein the front surface electrode penetrates the first protective layer and contacts the first wide band gap metal oxide layer.

12. The solar cell according to any one of claims 1 to 11, wherein a front surface anti-reflection layer is further provided on a side of the first protective layer away from the crystalline silicon absorption layer, and the front surface electrode penetrates the front surface anti-reflection layer and the first protective layer and contacts the first wide bandgap metal oxide layer.

13. The solar cell according to any one of claims 1 to 12, wherein the solar cell further comprises a second silicon oxide layer, a second wide bandgap metal oxide layer, a second protective layer and a back surface electrode stacked in sequence on the backlight side of the crystalline silicon absorption layer, the back surface electrode penetrating the second protective layer and contacting the second wide bandgap metal oxide layer, in, The second wide band gap metal oxide layer is formed of doped metal oxide, and the doped element in the second wide band gap metal oxide layer diffuses into the crystalline silicon absorption layer through the second silicon oxide layer to form a second doped region. The second wide band gap metal oxide layer has opposite charge transport properties to the first wide band gap metal oxide layer. The solar cell according to claim 13 , wherein the second silicon oxide layer has a thickness of 0.5-4 nm. 15 . The solar cell according to claim 13 , wherein the second silicon oxide layer has holes formed by calcination.

16. The solar cell according to any one of claims 13 to 15, wherein the metal oxide used in the first wide band gap metal oxide layer or the second wide band gap metal oxide layer is selected from one or more of zinc oxide, tin oxide, molybdenum oxide, titanium oxide, nickel oxide, gallium oxide, indium oxide, copper oxide, magnesium oxide, aluminum oxide, tungsten oxide, cerium oxide, manganese oxide, vanadium oxide, chromium oxide, cobalt oxide, germanium oxide, cadmium oxide, rhenium oxide, and the like. 17 . The solar cell according to claim 13 , wherein the first wide band gap metal oxide layer or the second wide band gap metal oxide layer has a thickness of 10-200 nm. 18 . The solar cell according to claim 13 , wherein a degree of polycrystallization of the second wide bandgap metal oxide layer increases gradually from a side close to the second oxide layer to a side far from the second oxide layer.

19. The solar cell according to any one of claims 13 to 18, wherein the material of the second protective layer is selected from silicon nitride or aluminum nitride.

20. The solar cell according to any one of claims 13 to 19, wherein the second protective layer has a thickness of 10 to 100 nm.

21. The solar cell according to any one of claims 13 to 20, wherein a back anti-reflection layer is further provided on a side of the second protective layer away from the crystalline silicon absorption layer, and the back surface electrode penetrates the back anti-reflection layer and the second protective layer and contacts the second wide bandgap metal oxide layer.

Citation Information

Patent Citations

  • Crystalline silicon solar cell and preparation method thereof

    CN108336154A

  • Laminated photovoltaic device and productionmethod thereof

    CN113471322A

  • Solar cell, preparation method thereof and photovoltaic module

    CN114709294A

  • Silicon-based heterojunction solar cell and preparation method thereof

    CN114759100A

  • Metal oxide-doped composite layer structure

    CN115172602A

Cited By

  • Solar cell, manufacturing method thereof and photovoltaic module

    CN121057354A