Solar cell and manufacturing method therefor

By performing multiple doping treatments and oxide layer etching on the silicon wafer, the problem of high difficulty in the boron expansion SE process was solved, light doping and heavy doping were achieved, improving solar cell performance and reducing costs.

WO2024217501A1PCT designated stage expired Publication Date: 2024-10-24TONGWEI SOLAR ENERGY (MEISHAN) CO LTD

Patent Information

Application Number
PCT/CN2024/088592
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

In the existing technology, the boron SE expansion process is difficult. The traditional laser propulsion method cannot effectively achieve light doping and heavy doping of boron, and it is easy to damage the surface morphology of the silicon wafer and the p-n junction in the lightly expanded area.

Method used

By making a textured surface on the front side of the silicon wafer, performing the first and second doping treatments to form an oxide layer, and using a semi-solid fluid material that can etch silicon oxide for etching, the oxide layer in the predetermined area is removed. Lightly doped and heavily doped, avoiding the use of lasers, controlling the size of the oxide layer, and using existing equipment for the process.

Benefits of technology

It effectively realizes light doping and heavy doping of silicon wafers, avoids damage to surface morphology and p-n junctions in lightly expanded areas, improves solar cell performance, reduces process costs, and eliminates the need to develop new equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024088592_24102024_PF_FP_ABST
    Figure CN2024088592_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a manufacturing method for a solar cell. The manufacturing method for the solar cell comprises: manufacturing a textured structure on a front surface of a silicon wafer; performing first doping treatment on the silicon wafer on the textured surface side, and forming an oxide layer on the textured surface; forming an etching material in a predetermined region of the surface of the oxide layer distant from the silicon wafer, and etching and removing the oxide layer at the predetermined region; cleaning and removing the etching material; performing second doping treatment on the silicon wafer corresponding to the predetermined region, so as to obtain a heavily doped region p-n junction and a lightly doped region p-n junction having a doping difference.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and manufacturing method thereof

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 18, 2023, with application number 202310417906.2 and invention name “Solar Cell and Its Manufacturing Method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the technical field of batteries, and in particular to a solar cell and a manufacturing method thereof. Background Art

[0003] TOPCon (Tunnel Oxide Passivated Contact) is a tunnel oxide passivated contact solar cell technology based on the principle of selective carriers. Compared to other traditional solar cells, TOPCon solar cell technology can significantly improve the photoelectric conversion efficiency of solar cells. Currently, TOPCon solar cells have a certain market share in the domestic market. Therefore, TOPCon cell technology has extremely high industrial value. Currently, the key technology for further improving the efficiency of TOPCon cells is the boron diffusion SE (selective emitter) process. Through the SE process, there is still significant room for improvement in the passivation and metallization of the cell front.

[0004] However, due to the high difficulty of the boron diffusion SE process, the traditional "diffusion-laser propulsion" method cannot achieve SE. This is because the BSG (borosilicate glass) is very thick after boron diffusion, and the boron in the BSG is mainly distributed on the top surface, with the boron content of the BSG near the silicon wafer being very low. If a laser is used, the boron on the top surface of the BSG must be pushed through the thicker BSG at the junction depth and then into the silicon wafer to achieve the purpose of re-doping, which is very difficult.

[0005] Summary of the Invention

[0006] The present invention aims to at least partially address one of the technical problems in the related art. To this end, one object of the present invention is to provide a method for manufacturing solar cells that can effectively achieve light and heavy doping of the textured surface of a silicon wafer without damaging the surface morphology of the silicon wafer or the pn junction in the lightly expanded region.

[0007] In one aspect of the present invention, the present invention provides a method for manufacturing a solar cell. According to an embodiment of the present invention, the method for manufacturing a solar cell includes: manufacturing a velvet surface on the front side of a silicon wafer; performing a first doping treatment on the silicon wafer on one side of the velvet surface, and forming an oxide layer on the velvet surface; coating an etching material on a predetermined area of ​​the oxide layer away from the surface of the silicon wafer, and etching away the oxide layer at the predetermined area; cleaning and removing the etching material; performing a second doping treatment on the silicon wafer corresponding to the predetermined area, thereby obtaining a heavy expansion area pn junction and a light expansion area pn junction. Therefore, compared with the laser boost doping in the prior art, the present invention removes the oxide layer in the predetermined area by etching the material, which can not only effectively achieve light doping and heavy doping of the doping element, but also avoids the use of laser and does not cause damage to the surface morphology of the silicon wafer and the light expansion area pn junction; at the same time, by etching the oxide layer by coating the etching material, it is easy to control the size of the oxide layer to be removed; in addition, there is no need to develop new equipment, and existing conventional equipment can be used, that is, the production cost of the manufacturing process will not be increased.

[0008] According to an embodiment of the present invention, both the first doping process and the second doping process are boron diffusion processes.

[0009] According to an embodiment of the present invention, the etching material is a semi-solid fluid material capable of etching silicon oxide.

[0010] According to an embodiment of the present invention, the etching material is coated by screen printing or spraying.

[0011] According to an embodiment of the present invention, the sheet resistance of the first doped pn junction is 100-300Ω.

[0012] According to an embodiment of the present invention, the pn junction in the re-expanded region satisfies at least one of the following conditions: the square resistance of the pn junction in the re-expanded region is 25 to 70 Ω; the junction depth of the pn junction in the re-expanded region is 1.1 to 1.8 microns; the surface doping concentration of the pn junction in the re-expanded region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 The metal composite of the pn junction in the re-expanded area is 300fA / cm 2 ~350fA / cm 2 ; The metal contact resistivity of the pn junction in the re-expanded region is 0.5~1mΩ*cm2.

[0013] According to an embodiment of the present invention, before coating the etching material, the method further comprises: performing laser propulsion in the predetermined area to obtain a pre-reexpanded region pn junction.

[0014] According to an embodiment of the present invention, the laser used for the laser propulsion is a microsecond laser. Optionally, the external frequency of the microsecond laser is 1000KHZ to 3000KHZ, and the power of the laser propulsion is 50 to 100W.

[0015] According to an embodiment of the present invention, at least one of the following conditions is met: the junction depth of the pn junction in the pre-reexpansion region can reach 1.8 to 2.5 μm; the junction depth of the pn junction in the re-expansion region can reach 2.0 to 2.8 μm; the surface doping concentration of the pn junction in the re-expansion region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 The square resistance of the pn junction in the re-expansion area is 15 to 40Ω; the metal composite of the pn junction in the re-expansion area is 280fA / cm 2 ~310fA / cm 2 The metal contact resistivity of the pn junction in the re-expansion area is 0.6 mΩ*cm 2 ~0.85mΩ*cm 2 .

[0016] According to an embodiment of the present invention, the lightly expanded area pn junction satisfies at least one of the following conditions: a sheet resistance of the lightly expanded area pn junction is 150-250Ω; and a junction depth of the lightly expanded area pn junction is 0.6-0.9 micrometers.

[0017] According to an embodiment of the present invention, the temperature of the first doping treatment is 800-1030°C, and the temperature of the second doping treatment is 800-1080°C.

[0018] According to an embodiment of the present invention, the temperature of the first doping process is lower than the temperature of the second doping process.

[0019] According to an embodiment of the present invention, the method for manufacturing a solar cell also includes: removing the pn junction on the back and edge of the silicon wafer, and polishing the back and the edge; sequentially forming a tunneling oxide layer, an in-situ phosphorus-doped n-poly layer and a silicon oxide mask layer on the back; crystallizing and activating the in-situ phosphorus-doped n-poly layer to obtain a doped polysilicon layer; removing the n-poly layer on the front and edge and the oxide layer on the surface; passivating and anti-reflective coating the front to form a first passivation layer, and passivating the back to form a second passivation layer; silk-screening and metallizing the front and back to form a front electrode and a back electrode, wherein the metallized area of ​​the front corresponds to the pn junction of the re-expanded region, the front electrode is arranged in contact with the pn junction of the re-expanded region through a through hole penetrating the first passivation layer, and the back electrode is arranged in contact with the doped polysilicon layer through a through hole penetrating the second passivation layer.

[0020] In another aspect, the present invention provides a solar cell, which is manufactured by the method described above according to an embodiment of the present invention. The solar cell has all the features and advantages of the solar cell described above, and no further details will be given here. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:

[0022] FIG1 is a flow chart showing the structure of manufacturing a solar cell according to an embodiment of the present invention;

[0023] FIG2 is a flow chart showing the structure of manufacturing a solar cell in another embodiment of the present invention;

[0024] FIG3 is a structural flow chart of manufacturing a solar cell in another embodiment of the present invention. DETAILED DESCRIPTION

[0025] The scheme of the present invention will be explained below with reference to the examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. Where specific techniques or conditions are not specified in the examples, the techniques or conditions described in the literature in this field or the product specifications are used. Where the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0026] The present invention is described below with reference to specific examples. It should be noted that these examples are merely illustrative and do not limit the present invention in any way.

[0027] In one aspect of the present invention, the present invention provides a method for manufacturing a solar cell. According to an embodiment of the present invention, referring to FIG1 , the method for manufacturing a solar cell includes:

[0028] S100: forming a velvet surface 110 on the front side of the silicon wafer 100.

[0029] In the above steps, before forming the velvet surface 110, the silicon wafer may be further cleaned in advance to remove stains on the surface of the silicon wafer and ensure the quality of the velvet surface. After the velvet surface is formed, the silicon wafer needs to be further cleaned to ensure the subsequent steps.

[0030] Further, there is no special requirement for the specific method of making the suede, and those skilled in the art can flexibly select according to actual conditions. In some embodiments, the suede can be made with alkali solution to form a pyramid-shaped suede, which is simple and easy to control.

[0031] S200: Performing a first doping treatment on the silicon wafer 100 on one side of the textured surface 110, and forming an oxide layer 200 on the textured surface. In the above steps, the first doping treatment is used to achieve a light expansion treatment on the silicon wafer, thereby obtaining a light expansion region pn junction 320.

[0032] According to an embodiment of the present invention, the temperature of the first doping treatment is 800-1030°C. The first doping treatment can be performed in multiple doping stages, with the doping temperature gradually increasing from a low temperature to a high temperature. That is, in the multiple doping stages, the doping temperature gradually increases from about 800°C (e.g., 810°C, 820°C, 830°C, 840°C, 850°C) to about 1030°C. That is, the highest doping temperature can be 980°C, 1000°C, or 1030°C. Within this temperature range, light expansion treatment of the silicon wafer can be effectively achieved to obtain a lightly expanded region pn junction 320. Moreover, the above treatment temperature can be lower than that of the subsequent second doping treatment. In this way, the effect of the first doping treatment will not be affected, energy consumption can be reduced, and the adverse effects of high temperature on the silicon wafer can be avoided.

[0033] According to an embodiment of the present invention, the first doping treatment is a boron diffusion treatment. Thus, a light boron diffusion treatment is achieved on the silicon wafer, and the oxide layer formed on the textured surface is borosilicate glass (BSG). In other embodiments, the first doping treatment is a phosphorus diffusion treatment. Thus, a light phosphorus diffusion treatment is achieved on the silicon wafer, and the oxide layer formed on the textured surface is phosphorus silicon glass (PSG).

[0034] Furthermore, the sheet resistance of the first doped pn junction is 100-300Ω, such as 100Ω, 150Ω, 160Ω, 180Ω, 190Ω, 200Ω, 220Ω, 240Ω, 250Ω, 300Ω, etc. This helps to obtain a lightly expanded region pn junction with appropriate sheet resistance.

[0035] S300: An etching material 300 is applied to a predetermined area of ​​the oxide layer 200 away from the surface of the silicon wafer 100, and the oxide layer 200 in the predetermined area is etched away. In this way, the oxide layer in the predetermined area is etched away by the etching material, while the etching material does not damage the surface morphology of the silicon wafer or the pn junction of the lightly extended region.

[0036] In the above steps, the etching material is a semi-solid fluid material capable of etching silicon oxide. Thus, the etching material is a semi-solid fluid, which allows it to adhere well to the surface of the silicon wafer 100, preventing it from flowing to other areas other than the intended area. The etching material is a material capable of etching silicon oxide, which allows it to effectively etch away the oxide layer without etching the silicon wafer, thereby protecting the silicon wafer from damage during the etching process.

[0037] In the above steps, the specific method of coating the etching material is screen printing or spraying. This method has a mature process, is easy to operate and industrially mass-produced, and can coat the etching material in a precise predetermined area.

[0038] S400: cleaning and removing the etching material 300.

[0039] There are no special requirements for the specific method of cleaning and removing the etching material 300. Those skilled in the art can flexibly choose according to actual needs. In some embodiments, a tank cleaning machine can be used to clean and remove the etching material 300.

[0040] S500: performing a second doping treatment on the silicon wafer 100 corresponding to the predetermined area, thereby obtaining the heavily expanded area pn junction 310 and the lightly expanded area pn junction 320.

[0041] According to an embodiment of the present invention, the second doping treatment is a boron diffusion treatment. Thus, a second boron re-diffusion treatment of the silicon wafer is achieved, and a pn junction 310 in the re-diffusion area is obtained. At the same time, a layer of oxide layer is formed on the surface, which is borosilicate glass (BSG). In the current prior art, since boron is more difficult to dope into silicon wafers than phosphorus, the process of using a laser to perform boron diffusion on silicon wafers is still relatively difficult. However, the method of the present invention is used to remove the oxide layer in a predetermined area on the surface of the silicon wafer by forming an etching material, and the silicon wafer is directly subjected to boron diffusion. In this way, not only can the boron diffusion treatment of the silicon wafer be achieved more effectively, but also the use of lasers to avoid damage and destruction to the surface morphology of the silicon wafer and the pn junction in the lightly expanded area can be avoided. In other embodiments, the second doping treatment is a phosphorus diffusion treatment. Thus, a phosphorus re-diffusion treatment of the silicon wafer is achieved, and at the same time, the oxide layer formed on the velvet surface is phosphorus silicon glass (PSG).

[0042] According to an embodiment of the present invention, the square resistance of the pn junction in the heavily expanded region is 25 to 70Ω, such as 25Ω, 30Ω, 40Ω, 50Ω, 60Ω, and 70Ω. It can be seen that the above-mentioned manufacturing method of the present invention can obtain a heavily expanded region pn junction with a lower square resistance, which greatly improves the performance of the solar cell compared to the existing technology using laser doping. In some embodiments of the present invention, the square resistance of the pn junction in the heavily expanded region is 30 to 70Ω. In this way, the lower square resistance can better improve the performance of the solar cell. According to an embodiment of the present invention, the square resistance of the pn junction in the heavily expanded region in this application will not be restricted by the square resistance of the pn junction in the light expanded region, and the two can independently achieve control of the size of their square resistances. In the prior art method of using laser for boron expansion, the square resistance of the pn junction in the heavily expanded region is usually restricted by the square resistance of the pn junction in the light expanded region, and it is difficult to achieve independent control of the square resistances of the two.

[0043] According to an embodiment of the present invention, the junction depth of the re-expanded region pn junction is 1.1 to 1.8 microns, for example, 1.1 microns, 1.2 microns, 1.3 microns, 1.4 microns, 1.54 microns, 1.6 microns, 1.7 microns, or 1.8 microns. Thus, a re-expanded region pn junction with a deeper doping junction depth can be obtained. Furthermore, compared to the prior art process using laser boron diffusion, the method of the present invention eliminates the constraints of the oxide layer, thereby increasing the doping rate per unit time, that is, increasing the doping junction depth per unit time.

[0044] According to an embodiment of the present invention, the surface doping concentration of the pn junction in the re-expansion region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 , for example, the surface doping concentration is 1.0*10 19 cm -3 , 1.5*10 19 cm -3 , 2.0*10 19 cm -3 , 2.5*10 19 cm -3 、3.0*10 19 cm -3 Therefore, the high surface doping concentration of the re-expansion region will be beneficial to reducing metal recombination and contact resistance.

[0045] According to an embodiment of the present invention, the metal composite (J0 metal) of the re-expansion region pn junction is 300fA / cm 2 ~350fA / cm 2 , which is significantly lower than that of metal composite without SE process (about 600fA / cm 2 ). The metal contact resistivity of the pn junction in the re-expansion area is 0.5mΩ*cm2 ~1mΩ*cm 2 , which is also lower than the metal contact resistivity without SE process (about 1~2mΩ*cm 2 ).

[0046] According to an embodiment of the present invention, the sheet resistance of the lightly expanded region pn junction is 150 to 250 Ω, such as 150 Ω, 160 Ω, 180 Ω, 190 Ω, 200 Ω, 220 Ω, 240 Ω, and 250 Ω. The junction depth of the lightly expanded region pn junction is 0.6 to 0.9 microns, such as 0.6 microns, 0.7 microns, 0.8 microns, and 0.9 microns. Thus, the lightly expanded region pn junction has good operating performance, helping to ensure good performance of the solar cell.

[0047] According to an embodiment of the present invention, the temperature of the second doping treatment is 800-1080°C. The second doping treatment can be performed in multiple doping stages, with the doping temperature gradually increasing from a low temperature to a high temperature. That is, in the multiple doping stages, the doping temperature gradually increases from approximately 800°C (e.g., 810°C, 820°C, 830°C, 840°C, 850°C) to approximately 1080°C. That is, the maximum doping temperature can be 1000°C, 1050°C, or 1080°C. Within this temperature range, the silicon wafer can be effectively re-expanded to obtain the pn junction 310 in the re-expanded region.

[0048] Furthermore, the temperature of the first doping treatment is lower than that of the second doping treatment. In this way, the lower temperature will not affect the effect of the first doping treatment, but can also reduce energy consumption and avoid the adverse effects of high temperature on the silicon wafer.

[0049] According to an embodiment of the present invention, both the first doping process and the second doping process can be performed using a BC13 diffusion furnace.

[0050] According to an embodiment of the present invention, in the above-mentioned manufacturing method, compared with the laser-assisted doping in the prior art, the present invention removes the oxide layer in a predetermined area by etching the material, which can not only effectively realize light doping and heavy doping of the doping element, but also avoids the use of laser without causing damage to the surface morphology of the silicon wafer and the pn junction of the light expansion area; at the same time, by etching the oxide layer by coating the etching material, it is convenient to control the size of the oxide layer to be removed; in addition, there is no need to develop new equipment, and existing conventional equipment can be used, that is, the production cost of the manufacturing process will not be increased.

[0051] In some specific embodiments, the first doping treatment is light boron diffusion, and the second doping treatment is heavy boron diffusion. The above-mentioned manufacturing method effectively realizes the boron diffusion SE process of the TOPCon battery, thereby greatly improving the passivation and metallization of the front of the TOPCon battery.

[0052] According to an embodiment of the present invention, referring to FIG2 , before applying the etching material, the process further includes S210: performing laser propulsion in a predetermined area to obtain a pre-reexpanded region pn junction 330. Thus, after the first doping treatment and before the second doping treatment, laser propulsion is performed in the predetermined area in advance, thereby further reducing the sheet resistance and metal recombination of the re-expanded region pn junction and further increasing the junction depth of the re-expanded region pn junction.

[0053] According to an embodiment of the present invention, the laser used for laser propulsion is a microsecond laser with an external frequency of 1000kHz to 3000kHz (e.g., 1000kHz, 1100kHz, 1300kHz, 1500kHz, 1800kHz, 2000kHz, 2200kHz, 2500kHz, 2700kHz, or 3000kHz), and a power of 50 to 100W (e.g., 50W, 60W, 70W, 80W, 90W, or 100W). Therefore, laser propulsion under the above conditions can effectively achieve the desired effect in a short period of time without adversely affecting the pn junction in non-predetermined areas (or the lightly expanded area pn junction 320).

[0054] According to an embodiment of the present invention, the junction depth of the pre-reexpanded region pn junction 330 can reach 1.8-2.5 μm. This shows that laser propulsion can further deepen the junction depth of the predetermined region, thereby facilitating obtaining a reexpanded region pn junction with better performance.

[0055] According to an embodiment of the present invention, the steps of manufacturing a solar cell include laser propulsion, wherein the junction depth of the re-expanded region pn junction can reach 2.0 to 2.8 μm, such as 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, and 2.8 μm. In this way, a re-expanded region pn junction with a deeper doping junction depth can be further obtained.

[0056] The surface doping concentration of the pn junction in the re-expanded region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 , for example, the surface doping concentration is 1.0*10 19 cm -3 , 1.5*10 19 cm -3 , 2.0*10 19 cm -3 , 2.5*10 19 cm -3 、3.0*10 19 cm -3Therefore, the high surface doping concentration of the re-expansion region will be beneficial to reducing metal recombination and contact resistance.

[0057] The square resistance of the pn junction in the heavily expanded area is 15 to 40Ω, such as 15Ω, 18Ω, 20Ω, 23Ω, 25Ω, 28Ω, 30Ω, 33Ω, 35Ω, 38Ω, 40Ω, 50Ω, 60Ω, and 70Ω. It can be seen that by implementing laser propulsion, a heavily expanded area pn junction with lower square resistance can be obtained, and lower square resistance can better improve the performance of solar cells. According to the embodiments of the present invention, the square resistance of the pn junction in the heavily expanded area in this application will not be restricted by the square resistance of the pn junction in the light expanded area, and the two can independently achieve control of the size of their square resistances. In the prior art, the square resistance of the pn junction in the heavily expanded area is usually restricted by the square resistance of the pn junction in the light expanded area, and it is difficult to achieve independent control of the square resistances of the two.

[0058] The metal recombination of the pn junction in the re-expanded area is 280fA / cm 2 ~310fA / cm 2 The metal contact resistance of the pn junction in the re-expansion area is 0.6mΩ*cm 2 ~0.85mΩ*cm 2 It can be seen that the implementation of laser propulsion can further reduce the metal composite and metal contact resistivity of the re-expansion area pn junction.

[0059] According to an embodiment of the present invention, when the steps of manufacturing solar cells include laser propulsion, any requirements of the remaining steps are completely consistent with the requirements of the steps in the manufacturing method when laser propulsion is not included, and will not be elaborated on here.

[0060] According to an embodiment of the present invention, referring to FIG3 , the method for manufacturing a solar cell further includes:

[0061] S500: removing the pn junction (not shown in the figure) plated on the back and edge of the silicon wafer, and polishing the back and edge.

[0062] After the silicon wafer is doped, an oxide layer with a certain junction depth is usually formed on the back of the silicon wafer. Doping may also be performed on the edge area of ​​the back silicon wafer. Therefore, before forming the tunneling oxide layer 410, the back of the silicon wafer needs to be pre-treated to remove the oxide layer on the back (for example, HF can be used to remove the oxide layer) and the doped pn junction on the edge to form a polished structure on the back.

[0063] S600: forming a tunneling oxide layer 410, an in-situ phosphorus-doped n-poly layer, and a silicon oxide mask layer 430 in sequence on the back side, and crystallizing and activating the in-situ phosphorus-doped n-poly layer to obtain a doped polysilicon layer 420;

[0064] Among them, the tunneling oxide layer 410 can be a tunneling silicon dioxide layer, and the tunneling silicon dioxide layer can be formed by plasma enhanced chemical vapor deposition; the doped polysilicon layer 420 is an N-type doped polysilicon layer, and the method for forming the N-type doped polysilicon layer is: after forming amorphous silicon by plasma enhanced chemical vapor deposition, the amorphous silicon is converted into polysilicon by high-temperature annealing treatment, and doped with phosphorus to obtain an N-type doped polysilicon layer; the silicon oxide mask layer 430 can be formed by plasma enhanced chemical vapor deposition.

[0065] S700: removing the n-poly layer on the front and edge and the oxide layer 200 on the surface.

[0066] When forming the doped polysilicon layer 420 on the back side, a doped polysilicon layer with a certain junction depth is usually formed on the front side and the edges. Therefore, it needs to be removed before forming the passivation layer on the front side. HF removal, NaOH, H2O2 and other chemicals can be used to remove the front polysilicon wrap-around and surface oxide layers.

[0067] S800 : performing passivation and anti-reflection coating on the front surface to form a first passivation layer 510 , and performing passivation coating on the back surface to form a second passivation layer 430 .

[0068] In the above steps, the second passivation layer 510 can be a double-layer structure of an aluminum oxide layer 511 and a silicon nitride layer 512. The aluminum oxide layer 511 is first formed as a bottom layer on the front side by atomic deposition (ALD), and then the silicon nitride layer 512 is formed on the surface of the oxide layer. The silicon nitride layer 512 can serve as both a passivation and an anti-reflection film. The silicon nitride layer 512 can be formed by plasma enhanced chemical vapor deposition.

[0069] In addition, the second passivation layer 430 on the back side may be a silicon nitride layer, which may be formed by plasma enhanced chemical vapor deposition.

[0070] S900: Silk screen printing and metallization are performed on the front and back sides to form a front electrode 520 and a back electrode 440. The metallized area on the front side corresponds to the pn junction of the re-expanded region. The front electrode 520 is in contact with the pn junction 310 of the re-expanded region through a through hole penetrating the first passivation layer 510. The back electrode 440 is in contact with the doped polysilicon layer 420 through a through hole penetrating the second passivation layer 430.

[0071] The front electrode and the back electrode can be obtained by printing silver paste by screen printing and sintering metallization.

[0072] It should be noted that the above steps can be performed in a different order, and do not have to be performed in the same order, as long as the final structure and performance of the product are not affected.

[0073] In another aspect, the present invention provides a solar cell. According to an embodiment of the present invention, the solar cell is manufactured using the aforementioned method. As a result, the solar cell exhibits high performance and a high battery utilization rate. Those skilled in the art will appreciate that the solar cell possesses all the features and advantages of the aforementioned solar cell manufacturing method, and further elaboration is omitted here.

[0074] According to an embodiment of the present invention, the solar cell may be a TOPCon cell, which can effectively implement the boron diffusion SE process of the TOPCon cell and improve the front passivation and metallization of the TOPCon cell.

[0075] Example

[0076] Example 1

[0077] The method of making solar cells is:

[0078] Use alkali solution to create a velvet surface on the front side of the silicon wafer and then clean it;

[0079] A boron diffusion treatment is performed on one side of the velvet surface to form an oxide layer on the velvet surface. The boron diffusion treatment temperature is between 800 and 1030°C.

[0080] forming an etching material in a predetermined area of ​​the oxide layer away from the surface of the silicon wafer, and etching away the oxide layer in the predetermined area;

[0081] Cleaning and removing the etched material;

[0082] The silicon wafer corresponding to the predetermined area is subjected to a boron re-expansion process at a temperature of up to 1050°C, thereby obtaining a pn junction in the lightly expanded area and a pn junction in the heavily expanded area. The pn junction in the lightly expanded area has a square resistance of 200Ω and a depth of 0.6 microns, while the pn junction in the heavily expanded area has a square resistance of 45Ω and a junction depth of 1.6 microns.

[0083] HF is used to remove the oxide layer on the back side and the doped pn junction at the edge, forming a polished structure on the back side;

[0084] forming a tunneling silicon dioxide layer, a phosphorus-doped polysilicon layer, and a silicon oxide mask layer in sequence on the back side of the silicon wafer;

[0085] Use HF, NaOH, H2O2 and other chemicals to remove the front polysilicon wrap-around and surface oxide layers;

[0086] Forming aluminum oxide and silicon nitride passivation layers on the surfaces of the heavy expansion area pn junction and the light expansion area pn junction on the front side of the battery;

[0087] forming a silicon nitride layer on the back of the cell;

[0088] A front electrode and a back electrode are sequentially formed on the front and back sides by screen printing to obtain a TOPCon battery, wherein the front electrode corresponds to the pn junction of the re-expansion region.

[0089] Example 2

[0090] Use alkali solution to create a velvet surface on the front side of the silicon wafer and then clean it;

[0091] A boron diffusion treatment is performed on one side of the velvet surface to form an oxide layer on the velvet surface. The boron diffusion treatment temperature is between 800 and 1030°C.

[0092] Using a microsecond laser with a high external frequency (2000KHZ) to process the predetermined area, the square resistance of the predetermined area after processing is reduced to 100Ω, and the pn junction depth is deepened to 2.0 microns (i.e., the junction depth of the pn junction in the pre-reexpansion area is 2.0 microns);

[0093] forming an etching material in a predetermined area of ​​the oxide layer away from the surface of the silicon wafer, and etching away the oxide layer in the predetermined area;

[0094] Cleaning and removing the etched material;

[0095] The silicon wafer corresponding to the predetermined area is subjected to a boron re-expansion process at a temperature of up to 1050°C, thereby forming a pn junction in the lightly expanded area and a pn junction in the heavily expanded area. The pn junction in the lightly expanded area has a square resistance of 180Ω and a depth of 0.8 microns, while the pn junction in the heavily expanded area has a square resistance of 30Ω and a junction depth of 2.2 microns.

[0096] HF is used to remove the oxide layer on the back side and the doped pn junction at the edge, forming a polished structure on the back side;

[0097] forming a tunneling silicon dioxide layer, a phosphorus-doped polysilicon layer, and a silicon oxide mask layer in sequence on the back side of the silicon wafer;

[0098] Use HF, NaOH, H2O2 and other chemicals to remove the front polysilicon wrap-around and surface oxide layers;

[0099] Forming aluminum oxide and silicon nitride passivation layers on the surfaces of the heavy expansion area pn junction and the light expansion area pn junction on the front side of the battery;

[0100] forming a silicon nitride layer on the back of the cell;

[0101] A front electrode and a back electrode are sequentially formed on the front and back sides by screen printing to obtain a TOPCon battery, wherein the front electrode corresponds to the pn junction of the re-expansion region.

[0102] Comparative Example 1

[0103] The method of making solar cells is:

[0104] Use alkali solution to create a velvet surface on the front side of the silicon wafer and then clean it;

[0105] On one side of the textured surface, a silicon wafer is subjected to a boron diffusion process using a laser, and an oxide layer is formed on the textured surface. The boron diffusion process is performed at a temperature of up to 1050°C. The resulting pn junction has a square resistance of 100Ω and a depth of 1.1 microns.

[0106] HF is used to remove the oxide layer on the back side and the doped pn junction at the edge, forming a polished structure on the back side;

[0107] A tunneling silicon dioxide layer, a phosphorus-doped polysilicon layer, and a silicon oxide mask layer are sequentially formed on the back of the cell;

[0108] Use HF, NaOH, H2O2 and other chemicals to remove the front polysilicon wrap-around and surface oxide layers;

[0109] Forming aluminum oxide and silicon nitride passivation layers on the front of the cell;

[0110] forming a silicon nitride layer on the back of the cell;

[0111] The front electrode and the back electrode are sequentially formed on the front and back sides by screen printing to obtain a TOPCon battery.

[0112] The solar cells obtained in Example 1, Example 2, and Comparative Example 1 were subjected to performance tests (using a Sinton tester, the testing equipment being a Sinton WCT-120, with Lifetime (minority carrier lifetime), J0 (surface recombination density), iVoc (open circuit voltage), and iFF (fill factor) all tested five times). The results are shown in Table 1 below:

[0113] Table 1

[0114] The above test results show that the solar cells in Examples 1 and 2 have a longer lifetime, lower J0, higher iVoc, higher iFF, and higher conversion efficiency, indicating that the solar cell in Example 1 has excellent passivation. Furthermore, compared to Example 1, the pn junction in the heavily expanded region in Example 2 has a lower junction depth and lower sheet resistance.

[0115] The terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature specified as "first" or "second" may explicitly or implicitly include one or more of the features. Throughout the description of this application, "plurality" means two or more, unless otherwise specifically defined.

[0116] In the description of this specification, the reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.

[0117] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for manufacturing a solar cell, characterized in that: The following steps are involved: Making a velvet surface on the front side of the silicon wafer; Performing a first doping treatment on the silicon wafer on one side of the velvet surface, and forming an oxide layer on the velvet surface; Coating an etching material on a predetermined area of ​​the oxide layer away from the surface of the silicon wafer, and etching away the oxide layer at the predetermined area; Cleaning and removing the etching material; The silicon wafer corresponding to the predetermined area is subjected to a second doping treatment, thereby obtaining a heavily expanded area pn junction and a lightly expanded area pn junction.

2. The method according to claim 1, characterized in that The first doping treatment and the second doping treatment are both boron diffusion treatments.

3. The method according to claim 1, characterized in that The etching material is a semi-solid fluid material capable of etching silicon oxide.

4. The method according to claim 1, characterized in that The method of coating the etching material is screen printing or spraying.

5. The method according to claim 1, characterized in that The square resistance of the first doped pn junction is 100-300Ω.

6. The method according to claim 2, characterized in that The square resistance of the pn junction in the re-expanded region is 25-70Ω.

7. The method according to claim 2, characterized in that: The junction depth of the pn junction in the re-expanded region is 1.1 to 1.8 microns.

8. The method according to claim 2, characterized in that: The surface doping concentration of the pn junction in the re-expanded region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 .

9. The method according to claim 2, characterized in that: The metal recombination of the pn junction in the re-expanded area is 300fA / cm 2 ~350fA / cm 2 .

10. The method according to claim 2, characterized in that The metal contact resistivity of the pn junction in the re-expansion region is 0.5 mΩ*cm 2 ~1mΩ*cm 2 .

11. The method according to claim 2, characterized in that Before coating the etching material, the method further includes: performing laser propulsion in the predetermined area to obtain a pre-reexpanded area pn junction.

12. The method according to claim 11, characterized in that The laser used in the laser propulsion is a microsecond laser.

13. The method according to claim 12, characterized in that The external frequency of the microsecond laser is 1000KHZ to 3000KHZ.

14. The method according to claim 11, characterized in that The power of the laser propulsion is 50-100W.

15. The method according to claim 11, characterized in that The junction depth of the pn junction in the pre-reexpansion region can reach 1.8 to 2.5 μm.

16. The method according to claim 11, characterized in that The junction depth of the pn junction in the re-expanded region can reach 2.0-2.8 μm.

17. The method according to claim 11, characterized in that The surface doping concentration of the pn junction in the re-expanded region is 1.0*10 19 cm -3 ~3.0*10 19 cm -3 .

18. The method according to claim 11, characterized in that The square resistance of the pn junction in the re-expanded region is 15-40Ω.

19. The method according to claim 11, characterized in that The metal recombination of the pn junction in the re-expanded area is 280 fA / cm 2 ~310fA / cm 2 .

20. The method according to claim 11, characterized in that The metal contact resistivity of the pn junction in the re-expansion region is 0.6 mΩ*cm 2 ~0.85mΩ*cm 2 .

21. The method according to any one of claims 1 to 20, characterized in that The square resistance of the pn junction in the lightly expanded area is 150-250Ω.

22. The method according to any one of claims 1 to 20, characterized in that: The junction depth of the lightly expanded region pn junction is 0.6-0.9 microns.

23. The method according to any one of claims 1 to 20, characterized in that The temperature of the first doping treatment is 800-1030°C, and the temperature of the second doping treatment is 800-1080°C.

24. The method according to claim 23, characterized in that The temperature of the first doping process is lower than the temperature of the second doping process.

25. The method according to any one of claims 1 to 20, characterized in that Also includes: Removing the pn junction plated on the back and edge of the silicon wafer, and polishing the back and edge; A tunneling oxide layer, an in-situ phosphorus-doped n-poly layer, and a silicon oxide mask layer are sequentially formed on the back side, and the in-situ phosphorus-doped n-poly layer is crystallized and activated to obtain a doped polysilicon layer; Removing the n-poly layer coating on the front and edge and the oxide layer on the surface; Passivation and anti-reflection coating are performed on the front surface to form a first passivation layer, and passivation coating is performed on the back surface to form a second passivation layer; The front side and the back side are screen printed and metallized to form a front electrode and a back side electrode, wherein the metallized area of ​​the front side corresponds to the pn junction of the re-expanded region, the front side electrode is contacted with the pn junction of the re-expanded region via a through hole penetrating the first passivation layer, and the back side electrode is contacted with the doped polysilicon layer via a through hole penetrating the second passivation layer.

26. A solar cell, characterized in that: Produced by the method according to any one of claims 1 to 25.

Citation Information

Patent Citations

  • Selective doping method and manufacturing method of solar cell

    CN115148856A

  • Solar cell and manufacturing method thereof

    CN116454167A

  • Full back electrode solar battery structure of passivation contact

    CN206595264U

Cited By

  • Solar cell and preparation method thereof

    CN120187111A

  • Photovoltaic cell, preparation method thereof and photovoltaic module

    CN121531791A