Lithium metal composite oxide powder, positive electrode active material for solid secondary battery, positive electrode for solid secondary battery, and solid secondary battery

The lithium metal composite oxide powder with a layered structure and optimized particle characteristics addresses the interfacial resistance issue in solid secondary batteries, ensuring low resistance and extended lifespan by enhancing the contact area with the solid electrolyte.

WO2024218923A1PCT designated stage expired Publication Date: 2024-10-24SUMITOMO CHEM CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/015677
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Solid secondary batteries face increased interfacial resistance between the electrode active material and solid electrolyte, which affects their performance, particularly due to the particle shape of the electrode active material used, leading to interrupted conductive paths and decreased output during charge/discharge cycles.

Method used

A lithium metal composite oxide powder with a layered structure, containing at least Li, Mn, and element M1, is developed, with specific particle size distribution and surface characteristics to enhance the contact area with the solid electrolyte, maintaining a low resistance even after charge/discharge cycles. The powder has a controlled number average degree of envelopment and BET specific surface area, optimizing the interfacial bond and contact area.

Benefits of technology

The lithium metal composite oxide powder ensures a solid secondary battery with low resistance and improved lifespan by maintaining a stable interface with the solid electrolyte, even after repeated charge/discharge cycles, as measured by AC impedance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023015677_24102024_PF_FP_ABST
    Figure JP2023015677_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A lithium metal composite oxide powder having a layered structure and to be used in a solid secondary battery containing at least Li, Mn, and an element M1, wherein, in a volume-based cumulative particle size distribution of the projection area equivalent circle diameter of the lithium metal composite oxide powder measured by static image analysis, when equivalent circle diameters (μm) at which the cumulative percentages from the small particle side are 50% and 90% are respectively defined as CD50 and CD90, the number average envelope degree of particles satisfying the range from CD50 to CD90 is 0.860-0.980, and the composition formula (1) is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium metal composite oxide powder, positive electrode active material for solid secondary battery, positive electrode for solid secondary battery, and solid secondary battery

[0001] The present invention relates to a lithium metal composite oxide powder, a positive electrode active material for a solid secondary battery, a positive electrode for a solid secondary battery, and a solid secondary battery.

[0002] There are two types of lithium secondary batteries: liquid secondary batteries, which use an electrolyte solution made by dissolving an electrolyte in an organic solvent, and solid secondary batteries, which use a solid electrolyte. Development of solid secondary batteries is progressing due to their advantages such as improved energy density and greater design freedom.

[0003] On the other hand, solid-state secondary batteries have the disadvantage that the interfacial resistance between the electrode active material and the solid electrolyte is more likely to increase than in liquid-based secondary batteries. Therefore, the particle shape of the electrode active material used in solid-state secondary batteries affects the performance of the solid-state secondary battery.

[0004] For example, Patent Document 1 discloses a positive electrode active material for all-solid-state lithium-ion batteries that contains high-strength single particles that are less likely to break during pressing, because if the positive electrode active material breaks during pressing in the battery manufacturing process, the conductive path will be interrupted, resulting in a decrease in output. Patent Document 1 discloses that the shape of the single particles is defined based on the degree of particle envelopment.

[0005] Japanese Patent Application Laid-Open No. 2021-22547

[0006] There is room for further improvement in the performance of solid secondary batteries by controlling the particle shape of the lithium metal composite oxide powder used in solid secondary batteries from another aspect.

[0007] The present invention has been made in view of the above circumstances, and aims to provide a lithium metal composite oxide powder for a solid secondary battery, a positive electrode active material for a solid secondary battery, a positive electrode for a solid battery, and a solid secondary battery, which are capable of obtaining a low-resistance solid secondary battery in which interfacial bonding between the positive electrode active material and the solid electrolyte is well maintained even after a charge-discharge cycle test.

[0008] The present invention encompasses the following aspects: [1] A lithium metal composite oxide powder for use in a solid secondary battery, having a layered structure and containing at least Li, Mn, and an element M1, wherein, in a cumulative particle size distribution based on the volume of the projected area equivalent circle diameter of the lithium metal composite oxide powder measured by static image analysis, when the circle equivalent diameters (μm) at which the cumulative proportions from the small particle side are 50% and 90% are defined as CD50 and CD90, respectively, the number average envelopment degree of particles satisfying the range of CD50 or more and CD90 or less is 0.860 or more and 0.980 or less, and the lithium metal composite oxide powder satisfies the following composition formula (1): aLi 2 MnO 3 ・(1-a) LiM1O 2 ... (1) (In formula (1), 0.1<a<1, and M1 is one or more elements selected from the group consisting of Ni, Co, Mn, Fe, Cu, Ti, V, Na, Mg, Ca, Sr, Ba, B, Al, Si, P, W, Mo, Nb, Zn, Sn, Zr, Cr, Ga, Ge, Pd, Ag, Cd, In, and V.) [2] The lithium metal composite oxide powder according to [1], wherein, when CD10 is the circle equivalent diameter (μm) at which a cumulative proportion from the small particle side becomes 10% in the cumulative particle size distribution, the number average envelopment degree of particles satisfying the range of CD10 or more and CD50 or less is 0.950 or more and less than 1. [3] The lithium metal composite oxide powder according to [1] or [2], wherein CD90 is more than 7.0 μm and 20.0 μm or less. [4] The lithium metal composite oxide powder according to [2] or [3], wherein the CD10 is 3.0 μm or more and 7.0 μm or less. [5] The BET specific surface area is 0.3 m 2 / g or more 2.0m 2 / g or less. [6] The lithium metal composite oxide powder according to any one of [1] to [5], wherein the element M1 essentially contains Ni, and the proportion of Ni in the total amount of element M1 is 20 mol% or more. [7] A positive electrode active material for a solid secondary battery, comprising the lithium metal composite oxide powder according to any one of [1] to [6]. [8] A positive electrode for a solid secondary battery, comprising the positive electrode active material for a solid secondary battery according to [7]. [9] A solid secondary battery, comprising the positive electrode for a solid secondary battery according to [8].

[0009] According to the present invention, it is possible to provide a lithium metal composite oxide powder that can provide a solid secondary battery in which the resistance is less likely to increase during charging and discharging, a positive electrode active material for a solid secondary battery, a positive electrode for a solid secondary battery, and a solid secondary battery.

[0010] In this specification, whether or not a solid secondary battery has low resistance even after a charge-discharge cycle test is determined from the impedance value |Z| at a frequency of 0.1 Hz, which is determined by measuring the AC impedance of the solid secondary battery after the charge-discharge cycle test.

[0011] If |Z| is 200Ω or less, the solid secondary battery is evaluated as having low resistance even after the charge-discharge cycle test. Such a solid secondary battery means a battery with a longer life. Details of the manufacturing conditions of the solid secondary battery for calculating the resistance after the charge-discharge cycle test will be described later.

[0012] Fig. 1 is a schematic diagram showing the overall configuration of a solid secondary battery. Fig. 2 is an electron microscope photograph of the lithium metal composite oxide produced in Example 1. Fig. 3 is a schematic diagram for explaining how the lithium metal composite oxide powder for a solid secondary battery of the present embodiment contacts with a solid electrolyte. Fig. 4 is a schematic diagram for explaining how the lithium metal composite oxide powder for a solid secondary battery other than the present embodiment contacts with a solid electrolyte. Fig. 5 is a schematic diagram for explaining how the lithium metal composite oxide powder for a solid secondary battery other than the present embodiment contacts with a solid electrolyte.

[0013] In this specification, when a numerical range is described as, for example, "1-10 μm" or "1 to 10 μm," it means a range from 1 μm to 10 μm, and means a numerical range including a lower limit of 1 μm and an upper limit of 10 μm.

[0014] <Lithium Metal Composite Oxide Powder> This embodiment relates to a lithium metal composite oxide powder that can be suitably used as a positive electrode active material for a solid secondary battery.

[0015] The lithium metal composite oxide powder has a layered structure, contains at least Li, Mn, and an element M1, and satisfies the composition formula (1) described below.

[0016] The lithium metal composite oxide powder is an aggregate of a plurality of particles. The aggregate of a plurality of particles includes secondary particles, which are aggregates of primary particles. The aggregate of a plurality of particles may include only secondary particles, or may be a mixture of primary particles and secondary particles. When the lithium metal composite oxide powder is a mixture of primary particles and secondary particles, the ratio of the number of secondary particles to the total number of particles is 90% or more.

[0017] The term "primary particles" refers to particles that do not appear to have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope or the like.

[0018] The "secondary particles" are particles formed by agglomeration of the primary particles. In other words, the secondary particles are agglomerates of the primary particles.

[0019] <<Number-average envelopment degree>> The envelopment degree of the lithium metal composite oxide powder is the ratio of the envelope length to the perimeter of one particle measured in a planar image of the lithium metal composite oxide powder, i.e., the perimeter envelopment degree. Hereinafter, the perimeter envelopment degree will be abbreviated to the envelopment degree. In this specification, the number-average envelopment degree is an index showing the degree of contact of the lithium metal composite oxide powder with the solid electrolyte.

[0020] The degree of envelopment is calculated for a single particle using the concept known as the enveloping perimeter and the actual perimeter using the following formula: Enveloping degree = enveloping perimeter / actual perimeter The enveloping perimeter is calculated from a virtual rubber band wrapped around the outline of a single particle. The number-average degree of envelopment of the lithium metal composite oxide powder is measured by the following method.

[0021] [Method for measuring number average envelopment degree] The number average envelopment degree of the lithium metal composite oxide powder is measured by static image analysis. The static image analysis can be performed using a static automatic image analyzer. As the static automatic image analyzer, for example, Morphologi 4 manufactured by Malvern Panalytical can be used. The static automatic image analyzer automatically measures the envelopment degree and projected area circle equivalent diameter of each particle.

[0022] Here, the projected area equivalent diameter is the diameter of a circle having the same area as the projected area of ​​one particle of the lithium metal composite oxide powder.

[0023] First, a cumulative particle size distribution based on the volume of the diameter of a circle equivalent to the projected area of ​​the lithium metal composite oxide powder is obtained by static image analysis.

[0024] Specifically, static image analysis is performed by the following method. First, 0.5 mg of lithium metal composite oxide powder is introduced into the supply unit of the analytical device and sprayed onto a preparation to fix it. Next, the fixed particles are observed under an optical microscope and images are acquired. The acquired images are analyzed to calculate the projected area circle equivalent diameter of the lithium metal composite oxide powder. From the obtained projected area circle equivalent diameter, a volume-based cumulative particle size distribution is obtained.

[0025] The lithium metal composite oxide powder introduced into the supply unit of the analytical device may be either a lithium metal composite oxide powder with a coating layer or a lithium metal composite oxide powder without a coating layer. Because the coating layer is very thin, having a thickness of about 1 to 20 nm, even when the coating layer is present, the measured value of the degree of envelopment is approximately the same as when the coating layer is not present.

[0026] In the obtained cumulative particle size distribution, the circle-equivalent diameters (μm) at which the cumulative proportions from the small particle diameter side are 10%, 50%, and 90%, respectively, are defined as CD10, CD50, and CD90.

[0027] At least 100 particles whose equivalent circle diameter (μm) falls within the range of CD50 or more and CD90 or less are selected from a static image of the lithium metal composite oxide powder, and the number average degree of envelopment is automatically measured. Hereinafter, the range of "CD50 or more and CD90 or less" is referred to as "CD50-CD90". The number average degree of envelopment in the range of equivalent circle diameter CD50-CD90 is referred to as "number average degree of envelopment 1".

[0028] The lithium metal composite oxide powder has a number average degree of envelopment 1 of 0.860 to 0.980. The number average degree of envelopment 1 is preferably 0.880 or more, more preferably 0.900 or more, and even more preferably 0.910 or more. The number average degree of envelopment 1 is also preferably 0.970 or less, more preferably 0.965 or less, and even more preferably 0.960 or less.

[0029] The upper and lower limits can be arbitrarily combined. As an example of a combination, the number average envelopment index 1 is preferably 0.880 to 0.970, more preferably 0.900 to 0.990, and even more preferably 0.910 to 0.960.

[0030] The number average envelopment degree 1 is an index showing the degree to which particles having a circle equivalent diameter (μm) that falls within the range of CD50-CD90, i.e., particles having a large particle diameter among the particles contained in the lithium metal composite oxide powder, come into contact with the solid electrolyte.

[0031] When the number average degree of envelopment 1 is equal to or greater than the lower limit, the solid electrolyte easily enters the recesses on the surface of each particle of the lithium metal composite oxide, and the contact area between the lithium metal composite oxide powder and the solid electrolyte easily increases.

[0032] Furthermore, by having the solid electrolyte fill the recesses, contact between the lithium metal composite oxide powder and the solid electrolyte is easily maintained even when the lithium metal composite oxide particles repeatedly expand and contract during charge-discharge cycle testing, resulting in a solid secondary battery with low resistance even after charge-discharge cycle testing.

[0033] 3 has protrusions 1a and recesses 1b on its surface. When the number average degree of envelopment 1 satisfies the range of the present invention, the solid electrolyte 2 easily enters the recesses 1b on the surface of the lithium metal composite oxide particle 1, and the contact area between the lithium metal composite oxide particle 1 and the solid electrolyte 2 easily increases.

[0034] The larger the contact area between one particle of the lithium metal composite oxide powder and the solid electrolyte, the more easily a good interface is formed between the lithium metal composite oxide powder and the solid electrolyte.

[0035] When the solid electrolyte fills the recesses in the particles of the lithium metal composite oxide powder and a good interface is formed between the lithium metal composite oxide powder and the solid electrolyte, contact between the lithium metal composite oxide powder and the solid electrolyte is easily maintained when the solid secondary battery is repeatedly charged and discharged, and a solid secondary battery with low resistance even after a charge-discharge cycle test is obtained.

[0036] For example, lithium metal composite oxide particle 3 shown in Fig. 4 has convex portions 3a and concave portions 3b on its surface. If the number average envelopment degree 1 is less than the lower limit of the present invention, solid electrolyte 2 cannot enter concave portions 3b on the surface of lithium metal composite oxide particle 3, and point contact occurs at convex portions 3a of lithium metal composite oxide particle 3, making it difficult to increase the contact area with solid electrolyte 2. When charge and discharge are repeated in this state, expansion and contraction of the lithium metal composite oxide particles occurs, causing the contact points with the solid electrolyte to be broken, resulting in high resistance.

[0037] Furthermore, the solid electrolyte 2 cannot sufficiently fill the recesses 3b, and for example, on the surface indicated by the reference numeral 5, the lithium metal composite oxide particles 3 do not come into contact with the solid electrolyte 2, which tends to reduce the utilization rate of the lithium metal composite oxide particles.

[0038] If the number average degree of envelopment 1 exceeds the upper limit of the present invention and is too close to 1, the lithium metal oxide particles 4 will have a smooth surface without irregularities, as shown in Figure 5. In this case, the lithium metal oxide particles 4 and the solid electrolyte 2 will also be in point contact, making it difficult to increase the contact area with the solid electrolyte 2. If charge and discharge are repeated in this state, as the lithium metal composite oxide particles expand and contract, the contact points with the solid electrolyte will be broken, resulting in high resistance.

[0039] In a static image of the lithium metal composite oxide powder, at least 100 particles whose equivalent circle diameter (μm) falls within the range of CD10-CD50 are selected, and the number average degree of envelopment is automatically measured. The number average degree of envelopment for particle diameters in the range of CD10-CD50 is defined as "number average degree of envelopment 2."

[0040] The number average degree of envelopment 2 is preferably 0.950 or more and less than 1. The number average degree of envelopment 2 is more preferably 0.960 or more, and even more preferably 0.960 or more. The number average degree of envelopment 2 is more preferably 0.995 or less, and even more preferably 0.990 or less. The above upper and lower limit values ​​can be combined arbitrarily. As an example of a combination, the number average degree of envelopment 2 is preferably 0.960-0.995, and more preferably 0.960-0.990.

[0041] The number average envelopment degree 2 is an index that indicates the degree to which particles having a particle diameter that falls within the range of CD10-CD50, i.e., particles having a small particle diameter among the particles contained in the lithium metal composite oxide powder, come into contact with the solid electrolyte.

[0042] When the number average envelopment degree 2 is within the above range, the surface of each particle of the lithium metal composite oxide has moderate irregularities, and the contact area between the lithium metal composite oxide powder and the solid electrolyte increases, making it easier to form an interface.

[0043] CD90 is preferably greater than 7.0 μm and equal to or less than 20.0 μm. CD90 is more preferably equal to or greater than 8.0 μm, and even more preferably equal to or greater than 8.5 μm. CD90 is more preferably equal to or less than 16.0 μm, even more preferably equal to or less than 14.0 μm, even more preferably equal to or less than 13.0 μm, and particularly preferably equal to or less than 12.0 μm.

[0044] The above upper and lower limits can be combined arbitrarily. As an example of a combination, CD90 is preferably 8.0 to 16.0 μm, more preferably 8.5 to 14.0 μm, even more preferably 8.5 to 13.0 μm, and particularly preferably 8.5 to 12.0 μm. When CD90 satisfies the above range, the proportion of coarse lithium metal composite oxide particles with a long lithium ion diffusion distance is low, which is preferable because the discharge rate characteristics are excellent.

[0045] CD10 is preferably 3.0 to 7.0 μm, more preferably 4.0 μm or more, and even more preferably 4.5 μm or more, and more preferably 6.5 μm or less, and even more preferably 6.0 μm or less.

[0046] The upper and lower limits can be combined arbitrarily. As an example of such a combination, CD10 is preferably 4.0-6.5 μm, more preferably 4.5-6.0 μm. When CD10 satisfies the above range, the proportion of fine lithium metal composite oxide powder that is electrically isolated without being able to contact the conductive material or solid electrolyte in the positive electrode can be reduced, which is preferable because a high charge / discharge capacity can be obtained.

[0047] The lithium metal composite oxide powder has a BET specific surface area of ​​0.3-2.0 m 2 / g, and 0.4-1.6m 2 / g is more preferable, and 0.5-1.4m 2 / g is more preferred.

[0048] When the BET specific surface area is within the above range, the contact area between the lithium metal composite oxide powder and the solid electrolyte increases, making it easier to form an interface.

[0049] [Method for Measuring BET Specific Surface Area] The "BET specific surface area" is a value measured by the BET (Brunauer, Emmett, Teller) method. In measuring the BET specific surface area, nitrogen gas is used as the adsorption gas. For example, 1 g of the powder to be measured is dried in a nitrogen atmosphere at 105°C for 30 minutes, and then the BET specific surface area can be measured using a BET specific surface area meter (for example, Macsorb (registered trademark) manufactured by Mountec Co., Ltd.) (unit: m 2 / g).

[0050] The lithium metal composite oxide powder satisfies the following composition formula (1): 2 MnO 3 ・(1-a) LiM1O 2 ... (1) (In formula (1), 0.1<a<1, and M1 is one or more elements selected from the group consisting of Ni, Co, Mn, Fe, Cu, Ti, V, Na, Mg, Ca, Sr, Ba, B, Al, Si, P, W, Mo, Nb, Zn, Sn, Zr, Cr, Ga, Ge, Pd, Ag, Cd, In, and V.)

[0051] In formula (1), from the viewpoint of obtaining a solid secondary battery with a higher capacity, a is preferably 0.25 or more, more preferably 0.35 or more, and even more preferably 0.45 or more, and is preferably 0.90 or less, more preferably 0.80 or less, and even more preferably 0.75 or less.

[0052] The upper and lower limits can be arbitrarily combined. As an example of a combination, a is preferably 0.25 to 0.90, more preferably 0.35 to 0.80, and even more preferably 0.45 to 0.75.

[0053] In formula (1), when a is in the above range, it is easy to obtain a lithium composite metal oxide powder with a stabilized crystal structure. The stabilized crystal plane and the solid electrolyte are bonded to form a good interface, so that the bond at the interface between the lithium metal composite oxide powder and the solid electrolyte is easily maintained good even when the solid secondary battery is repeatedly charged and discharged, and a solid secondary battery with low resistance even after charge-discharge cycle testing is obtained.

[0054] In formula (1), element M1 preferably contains Ni. The proportion of Ni contained in the total amount of element M1 is preferably 20 mol% or more, more preferably 25 mol% or more, and even more preferably 30 mol% or more. The proportion of Ni contained in the total amount of element M1 is preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less.

[0055] The upper and lower limits can be arbitrarily combined. As an example of such a combination, the proportion of Ni contained in the total amount of element M1 is preferably 20 to 90 mol %, more preferably 25 to 80 mol %, and even more preferably 30 to 70 mol %.

[0056] In formula (1), the element M1 preferably contains Mn. The proportion of Mn contained in the total amount of the element M1 is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more. The proportion of Mn contained in the total amount of the element M1 is preferably 50 mol% or less, more preferably 40 mol% or less, and even more preferably 35 mol% or less.

[0057] In formula (1), element M1 is preferably one or more elements selected from the group consisting of Ni, Co, Mn, Fe, Cu, Ti, Mg, Ca, Ba, B, Al, Si, P, W, Mo, Nb, Zn, Sn, and Zr, and more preferably one or more elements selected from the group consisting of Ni, Co, Mn, Mg, Ba, B, Al, Si, P, W, Mo, Nb, and Zr.

[0058] The upper and lower limits can be arbitrarily combined. As an example of a combination, the proportion of Mn contained in the total amount of element M1 is preferably 5 to 50 mol %, more preferably 10 to 40 mol %, and even more preferably 15 to 35 mol %.

[0059] [Composition Analysis] The composition of the lithium metal composite oxide powder can be analyzed, for example, by dissolving the lithium metal composite oxide powder in hydrochloric acid and then using an inductively coupled plasma emission spectrometer (for example, SPS3000, manufactured by SII NanoTechnology Inc.).

[0060] The lithium metal composite oxide powder has a layered crystal structure, and more preferably has a hexagonal crystal structure or a monoclinic crystal structure.

[0061] The hexagonal crystal structure is P3, P3 1 , P3 2 , R3, P-3, R-3, P312, P321, P3 1 12. P3 1 21, P3 2 12. P3 2 21, R32, P3m1, P31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P6 1 , P6 5 , P6 2 , P6 4 , P6 3 , P-6, P6 / m, P6 3 / m, P622, P6 1 22, P6 5 22, P6 2 22, P6 4 22, P6 3 22, P6mm, P6cc, P6 3 cm, P6 3 mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P6 3 / mcm, and P6 3 / mmc.

[0062] In addition, the monoclinic crystal structure is P2, P2 1 , C2, Pm, Pc, Cm, Cc, P2 / m, P2 1 / m, C2 / m, P2 / c, P2 1 It is assigned to any one space group selected from the group consisting of C1 / c, C2 / c, and C3 / c.

[0063] Among these, from the viewpoint of obtaining a solid secondary battery with a high discharge capacity, the crystal structure is particularly preferably a hexagonal crystal structure belonging to the space group R-3m and a monoclinic crystal structure belonging to the space group C2 / m.

[0064] Li in formula (1) 2 MnO 3 has a monoclinic crystal structure belonging to the space group C2 / m. By making the composition contain Mn, Li 2 MnO 3 A lithium metal composite oxide having the above crystal structure can be obtained, and high capacity can be easily achieved.

[0065] The crystal structure of the lithium metal composite oxide can be calculated by powder X-ray diffraction measurement of the lithium metal composite oxide using CuKα as a radiation source and a measurement range of the diffraction angle 2θ of 10 to 90°. Specifically, it can be confirmed by observation using a powder X-ray diffraction measurement device (for example, Ultima IV manufactured by Rigaku Corporation).

[0066] [Coating Layer] A coating layer made of a metal composite oxide having lithium ion conductivity may be formed on the surface of the lithium metal composite oxide particles. By forming a coating layer on the surface of the lithium metal composite oxide particles, the decomposition reaction of the solid electrolyte occurring between the lithium metal composite oxide and the solid electrolyte is suppressed, thereby improving the charge / discharge efficiency of the solid secondary battery. For example, when an argyrodite-type sulfide solid electrolyte or a sulfide solid electrolyte described below is used as the solid electrolyte, forming a coating layer on the surface of the lithium metal composite oxide suppresses the decomposition reaction of the solid electrolyte, enabling stable battery operation.

[0067] The thickness of the coating layer may be adjusted within a range that does not impair the effects of the present invention. Specifically, the thickness is preferably about 1 to 20 nm.

[0068] The thickness of the coating layer is determined from the results of analysis using a scanning transmission electron microscope (STEM)-energy dispersive X-ray spectroscopy (EDX). A line profile of elements specific to the coating layer is created, and based on the obtained line profile, the range in which the specific elements are detected is defined as the range in which the coating layer exists. The thickness of the coating layer can be determined.

[0069] Examples of such metal composite oxides include metal composite oxides of Li and at least one element selected from the group consisting of Nb, Si, P, Al, W, Ta, Ti, Zr, Mo, and B.

[0070] Examples of methods for forming the coating layer include a method of adding and mixing a compound containing the elements contained in the coating layer to a lithium metal composite oxide and then heat-treating the mixture, a method of spraying a solution containing the elements contained in the coating layer onto a lithium metal composite oxide and then heat-treating the mixture, and a method of immersing a lithium metal composite oxide in a solution containing the elements contained in the coating layer and then heat-treating the mixture.

[0071] <Method for producing lithium metal composite oxide powder> Next, a method for producing lithium metal composite oxide powder will be described. The method for producing lithium metal composite oxide powder includes at least a step of producing a hydroxide precursor, a step of calcining a mixture of the hydroxide precursor and a lithium compound, and a step of crushing the calcined product obtained in the calcination step.

[0072] [Hydroxide precursor production process] The hydroxide precursor can be produced by a commonly known semi-continuous method (semi-batch method). Preferred reaction vessels include a reaction vessel without an overflow pipe, and an apparatus equipped with a concentration tank connected to an overflow pipe, in which the overflowed product is concentrated in the concentration tank and circulated back to the reaction vessel. Hereinafter, the production method will be described in detail using as an example a method for producing a hydroxide precursor containing Ni, Co, and Mn as metals by a semi-continuous method.

[0073] Specifically, first, nuclei of hydroxide precursor particles are generated, and then the nuclei are grown. The hydroxide precursor may be a metal composite hydroxide containing Ni, Co, and Mn.

[0074] Examples of metal source liquids for producing hydroxide precursors containing Ni, Co, and Mn include nickel salt solutions, cobalt salt solutions, and manganese salt solutions.

[0075] The nickel salt that is the solute of the nickel salt solution is not particularly limited, but for example, any one or more of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate can be used.

[0076] As the cobalt salt that is the solute of the cobalt salt solution, for example, any one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate can be used.

[0077] As the manganese salt that is the solute of the manganese salt solution, for example, any one or more of manganese sulfate, manganese nitrate, manganese chloride, and manganese acetate can be used.

[0078] Nucleation step: A metal raw material mixture, a complexing agent, and an alkaline aqueous solution are reacted to form Ni 1-x-y Co x Mn y O w (OH) 2-w Nuclei of metal composite hydroxides expressed as (0<1-xy, 0<x, 0<y, 0<w<1) are generated. The mixed metal raw material solution is a mixed solution of a nickel salt solution, a cobalt salt solution, and a manganese salt solution.

[0079] The metal raw material mixture, the complexing agent, and the alkaline aqueous solution are simultaneously and continuously fed into a reaction vessel equipped with a stirrer, whereby nuclei are formed.

[0080] In the semi-continuous process, an alkaline aqueous solution such as sodium hydroxide or potassium hydroxide is added to the mixed solution before the pH of the mixed solution changes from alkaline to neutral in order to adjust the pH of the mixed solution containing the metal raw material and the complexing agent.

[0081] The complexing agent is a compound capable of forming a complex with nickel ions and cobalt ions in an aqueous solution. Examples of the complexing agent include ammonium ion donors, hydrazine, ethylenediaminetetraacetic acid, nitrilotriacetic acid, uracildiacetic acid, and glycine. Examples of the ammonium ion donor that can be used include ammonium salts such as ammonium hydroxide, ammonium sulfate, ammonium chloride, ammonium carbonate, and ammonium fluoride.

[0082] The complexing agent is preferably an ammonium ion donor.

[0083] In the nucleation step, the number average degree of envelopment 1 can be controlled within the range of the present invention by controlling the concentration of the complexing agent in the reaction tank so that the ratio of the molar concentration of the manganese salt contained in the metal raw material liquid to the molar concentration of ammonium in the reaction tank is in the range of 1.0 to 2.0.

[0084] The pH value in this specification is defined as the value measured when the temperature of the mixed solution is 40° C. The pH of the mixed solution is measured when the temperature of the mixed solution sampled from the reaction vessel reaches 40° C.

[0085] If the temperature of the sampled mixed liquid is lower than 40° C., the mixed liquid is heated and the pH is measured when it reaches 40° C. If the temperature of the sampled mixed liquid is higher than 40° C., the mixed liquid is cooled and the pH is measured when it reaches 40° C.

[0086] During the reaction, the temperature of the reaction vessel is controlled within a range of, for example, 20°C or higher and 80°C or lower, preferably 30°C or higher and 70°C or lower.

[0087] In the nucleation step, the pH value in the reaction vessel is controlled within the range of, for example, pH 10 to pH 13, preferably pH 11 to pH 13.

[0088] In the nucleation step, the materials in the reaction vessel are mixed by stirring. For example, the stirring rotation speed is preferably more than 1000 rpm, more preferably 1100 rpm or more, and even more preferably 1500 rpm or more. By stirring under such stirring conditions, the supplied raw material solutions are easily mixed uniformly.

[0089] After a certain time has elapsed since the start of the nucleation step, the generated nuclei overflow from the reaction tank and are precipitated and concentrated in a concentration tank connected to the overflow pipe. The certain time is preferably adjusted appropriately depending on the amount of raw material liquid fed and the slurry concentration in the reaction tank. Generally, 0.1 to 10 hours is preferred.

[0090] [Nucleus Growth Step] The concentrated nucleus-containing slurry is returned to the reaction vessel, where the nuclei are grown again.

[0091] It is preferable to supply nitrogen gas or argon gas into the reaction tank and the concentration tank. By supplying these gases, Mn, which is easily oxidized, can be prevented from being oxidized and changing into oxide particles of irregular shape. By using a precursor obtained by suppressing the oxidation of Mn, the number average envelopment degree 1 can be controlled within the range of the present invention.

[0092] The concentration of the complexing agent in the reaction tank in the nucleus growth step is controlled so that the ratio of the molar concentration of the manganese salt contained in the metal raw material liquid to the molar concentration of ammonium in the reaction tank is in the range of 1.0 to 2.0, thereby controlling the number average degree of envelopment 1 within the range of the present invention.

[0093] The pH in the nucleus growth step is controlled within the range of, for example, pH 9 to pH 12, preferably pH 9 to pH 11.5.

[0094] By the above-mentioned steps, a slurry containing nickel-cobalt-manganese metal composite hydroxide is obtained as a metal composite hydroxide-containing slurry. When isolating the nickel-cobalt-manganese metal composite hydroxide, a method of dehydrating the metal composite hydroxide-containing slurry by centrifugation, suction filtration, or the like is preferred.

[0095] After the above reaction, the mixture is dehydrated, dried and sieved to obtain a hydroxide precursor containing Ni, Co and Mn.

[0096] [Step of Calcining a Mixture of a Hydroxide Precursor and a Lithium Compound] This step is a step of calcining a mixture obtained by mixing a lithium compound and a hydroxide precursor.

[0097] The hydroxide precursor is dried and then mixed with a lithium compound. After drying, the hydroxide precursor may be appropriately classified.

[0098] The lithium compound may be at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxide, lithium chloride, and lithium fluoride. Among these, either lithium hydroxide or lithium carbonate, or a mixture thereof, is preferred. When the lithium hydroxide contains lithium carbonate, the content of lithium carbonate in the lithium hydroxide is preferably 5 mass% or less.

[0099] A mixture is obtained by mixing a lithium compound and a hydroxide precursor in consideration of the composition ratio of the final target product. Specifically, the lithium compound and the hydroxide precursor are mixed in a ratio corresponding to the composition ratio of the above composition formula (1). The amount (molar ratio) of lithium atoms relative to the total amount of metal atoms contained in the hydroxide precursor (1) is preferably 1.10 or more, more preferably 1.12 or more, and even more preferably 1.15 or more.

[0100] A calcined product is obtained by calcining the mixture of the lithium compound and the hydroxide precursor.

[0101] The resulting mixture is fired, for example, in an oxygen-containing atmosphere at a firing temperature of 500-1050° C. By firing the mixture, crystals of the lithium metal composite oxide grow.

[0102] In this specification, the firing temperature refers to the temperature of the atmosphere in the firing furnace, and means the highest temperature of the holding temperature (maximum holding temperature). When the firing process includes multiple heating steps, the firing temperature refers to the temperature when heated at the highest holding temperature in each heating step.

[0103] Specifically, the holding temperature is preferably 550 to 1000°C, more preferably 600 to 1000°C.

[0104] The time for maintaining the temperature may be 0.1 to 20 hours, preferably 0.5 to 10 hours.

[0105] It is also preferable to carry out the firing in an oxygen-containing atmosphere, specifically, by introducing an oxygen-containing gas into the firing furnace to create an oxygen-containing atmosphere.

[0106] The temperature rise rate is calculated from the time from when the temperature rise starts in the firing device until the maximum holding temperature is reached, and the temperature difference from the temperature at the start of the temperature rise in the firing furnace of the firing device to the maximum holding temperature.

[0107] By firing the mixture under the firing conditions as described above, it becomes easier to control the number average envelopment degrees 1 and 2, CD10 and CD90 of the lithium metal composite oxide powder within the above ranges.

[0108] After the firing step, the fired product obtained by firing is weakly crushed under conditions of weak crushing force or using a device with weak crushing force.

[0109] The calcined product can be crushed, for example, by a disc mill, etc. The conditions for crushing the reaction product by a disc mill include operating the disc mill at a rotation speed of 500 to 2000 rpm.

[0110] By crushing the fired product under such conditions, the number average envelopment degrees 1 and 2, CD10 and CD90 of the lithium metal composite oxide powder can be controlled within the above-mentioned ranges.

[0111] <Solid State Secondary Battery> Next, while explaining the configuration of a solid state secondary battery, a positive electrode using the lithium metal composite oxide powder according to one embodiment of the present invention as a positive electrode active material of the solid state secondary battery, and a solid state secondary battery having this positive electrode will be described.

[0112] The solid secondary battery may be an all-solid secondary battery having a solid electrolyte layer made of a solid electrolyte, or may be a solid secondary battery in which the solid electrolyte layer contains a trace amount of an organic solvent or an ionic liquid.

[0113] FIG. 1 is a schematic diagram showing an example of a solid secondary battery. The solid secondary battery 1000 shown in FIG. 1 includes a laminate 100 having a positive electrode 110, a negative electrode 120, and a solid electrolyte layer 130, and an exterior body 200 that houses the laminate 100. The solid secondary battery 1000 may also have a bipolar structure in which a positive electrode active material and a negative electrode active material are disposed on both sides of a current collector. A specific example of a bipolar structure is the structure described in JP-A-2004-95400. The materials constituting each component will be described later.

[0114] The laminate 100 may have an external terminal 113 connected to the positive electrode current collector 112 and an external terminal 123 connected to the negative electrode current collector 122. In addition, the solid secondary battery 1000 may have a separator between the positive electrode 110 and the negative electrode 120.

[0115] The solid secondary battery 1000 further includes an insulator (not shown) that insulates the laminate 100 from the exterior body 200 , and a sealing body (not shown) that seals the opening 200 a of the exterior body 200 .

[0116] The exterior body 200 may be a container molded from a highly corrosion-resistant metal material such as aluminum, stainless steel, or nickel-plated steel. Alternatively, the exterior body 200 may be a bag-shaped container made of a laminate film having corrosion resistance on at least one surface.

[0117] The shape of the solid secondary battery 1000 may be, for example, a coin type, a button type, a paper type (or a sheet type), a cylindrical type, a square type, or a laminate type (pouch type).

[0118] Although the solid state secondary battery 1000 is illustrated as having one laminate 100 as an example, the present embodiment is not limited to this. The solid state secondary battery 1000 may have a configuration in which the laminate 100 is used as a unit cell, and a plurality of unit cells (laminated bodies 100) are sealed inside an exterior body 200.

[0119] Each component will be described below in order.

[0120] (Positive Electrode) The positive electrode 110 includes a positive electrode active material layer 111 and a positive electrode current collector 112 .

[0121] The positive electrode active material layer 111 includes the lithium metal composite oxide powder according to one embodiment of the present invention and a solid electrolyte. The positive electrode active material layer 111 may also include a conductive material and a binder.

[0122] (Solid Electrolyte) A solid electrolyte having lithium ion conductivity and used in known solid secondary batteries can be used as the solid electrolyte contained in the positive electrode active material layer 111. Examples of such a solid electrolyte include inorganic electrolytes and organic electrolytes.

[0123] Examples of inorganic electrolytes include argyrodide-type sulfide solid electrolytes, oxide-based solid electrolytes, sulfide-based solid electrolytes, and hydride-based solid electrolytes. Examples of organic electrolytes include polymer-based solid electrolytes. Examples of each electrolyte include compounds described in WO2020 / 208872A1, US2016 / 0233510A1, US2012 / 0251871A1, and US2018 / 0159169A1, such as the following compounds:

[0124] (Argyridide-type sulfide solid electrolyte) Examples of the argyrodide-type sulfide solid electrolyte include Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br and Li 6 P.S. 5 I can be mentioned.

[0125] (Oxide-based solid electrolyte) Examples of oxide-based solid electrolytes include perovskite-type oxides, NASICON-type oxides, LISICON-type oxides, and garnet-type oxides. Specific examples of each oxide include the compounds described in WO2020 / 208872A1, US2016 / 0233510A1, and US2020 / 0259213A1, such as the following compounds:

[0126] As the perovskite oxide, Li a La 1-a TiO 3 (0<a<1) and other Li-La-Ti oxides, Li b La1-b TaO 3 (0<b<1) and Li-La-Ta oxides c La 1-c NbO 3 Examples include Li-La-Nb oxides such as (0<c<1).

[0127] As the NASICON type oxide, Li 1+d Al d Ti 2-d (P.O. 4 ) 3 (0≦d≦1) and the like. NASICON type oxides are Li m M 1 n M 2 o P p O q (In the formula, M 1 is one or more elements selected from the group consisting of B, Al, Ga, In, C, Si, Ge, Sn, Sb, and Se. 2 is one or more elements selected from the group consisting of Ti, Zr, Ge, In, Ga, Sn, and Al. m, n, o, p, and q are any positive numbers.

[0128] As the LISICON type oxide, Li 4 M 3 O 4 -Li 3 M 4 O 4 (M 3 is one or more elements selected from the group consisting of Si, Ge, and Ti. 4 is one or more elements selected from the group consisting of P, As and V.

[0129] Garnet-type oxides include Li 7 La 3 Zr 2 O 12 Examples of suitable oxides include Li-La-Zr oxides such as Li-La-Zr (also called LLZ).

[0130] The oxide-based solid electrolyte may be a crystalline material or an amorphous material.

[0131] (Sulfide-based solid electrolyte) As the sulfide-based solid electrolyte, Li 2 S-P 2 S 5 based compound, Li 2 S-SiS 2 based compound, Li 2 S-GeS 2 based compound, Li 2 S-B 2 S 3 system compound, LiI-Si 2 S-P 2 S 5 system compound, LiI-Li 2 S-P 2 O 5 system compound, LiI-Li 3 P.O. 4 -P 2 S 5 Compounds based on Li 10 GeP 2 S 12 compounds based on the above.

[0132] In this specification, the expression "sulfide-based compound" referring to a sulfide-based solid electrolyte is the same as the expression "Li 2 S" "P" 2 S 5 " is used as a general term for solid electrolytes that mainly contain raw materials such as Li. 2 S-P 2 S 5 The compounds include Li 2 S and P 2 S 5 and further includes other raw materials. 2 S-P 2 S 5 Li contained in the compound 2 The ratio of S is, for example, Li 2 S-P 2 S 5 It is 50 to 90% by mass based on the entire system compound. 2 S-P 2 S 5 P contained in the compound 2 S 5 The ratio of Li 2 S-P2 S 5 It is 10 to 50 mass% based on the entire system compound. 2 S-P 2 S 5 The ratio of other raw materials contained in the system compound is, for example, Li 2 S-P 2 S 5 It is 0 to 30 mass% based on the entire system compound. 2 S-P 2 S 5 The compounds include Li 2 S and P 2 S 5 The solid electrolyte also includes a mixture ratio of different.

[0133] Li 2 S-P 2 S 5 Li-based compounds include 2 S-P 2 S 5 , Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P 2 S 5 - LiBr, Li 2 S-P 2 S 5 -LiI-LiBr, Li 2 S-P 2 S 5 -Li 2 O, Li 2 S-P 2 S 5 -Li 2 O-LiI and Li 2 S-P 2 S 5 -Z m S n (m and n are positive numbers, and Z is Ge, Zn, or Ga).

[0134] Li 2 S-SiS 2 Li-based compounds include 2 S-SiS 2 , Li2 S-SiS 2 - LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S-SiS 2 -P 2 S 5 -LiCl, Li 2 S-SiS 2 -Li 3 P.O. 4 , Li 2 S-SiS 2 -Li 2 SO 4 and Li 2 S-SiS 2 -Li x MO y (x and y are positive numbers. M is P, Si, Ge, B, Al, Ga, or In.)

[0135] Li 2 S-GeS 2 Li-based compounds include 2 S-GeS 2 and Li 2 S-GeS 2 -P 2 S 5 Examples include:

[0136] The sulfide-based solid electrolyte may be a crystalline material or an amorphous material.

[0137] (Hydride-based solid electrolyte) As the hydride-based solid electrolyte material, LiBH 4 , LiBH 4 -3KI, LiBH 4 -PI 2 , LiBH 4 -P 2 S 5 , LiBH 4-LiNH 2 , 3LiBH 4 - LiI, LiNH 2 , Li 2 AlH 6 , Li(NH 2 ) 2 I, Li 2 NH, LiGd(BH 4 ) 3 Cl, Li 2 (BH 4 ) (NH 2 ), Li 3 (NH 2 ) I and Li 4 (BH 4 ) (NH 2 ) 3 Examples include:

[0138] (Polymer-Based Solid Electrolyte) Examples of the polymer-based solid electrolyte include organic polymer electrolytes such as polyethylene oxide-based polymer compounds and polymer compounds containing at least one selected from the group consisting of polyorganosiloxane chains and polyoxyalkylene chains. Also, so-called gel-type solid electrolytes in which a non-aqueous electrolyte solution is held in a polymer compound can be used.

[0139] Two or more solid electrolytes can be used in combination as long as the effects of the invention are not impaired.

[0140] The average particle size of the solid electrolyte powder is preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 1 μm or less.

[0141] (Conductive Material) A carbon material can be used as the conductive material contained in the positive electrode active material layer 111. Examples of the carbon material include graphite powder, carbon black (for example, acetylene black), and fibrous carbon materials.

[0142] The proportion of the conductive material in the positive electrode active material layer 111 is preferably 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the positive electrode active material.

[0143] (Binder) The binder of the positive electrode can be a thermoplastic resin. Examples of the thermoplastic resin include polyimide resin, fluororesin such as polyvinylidene fluoride (hereinafter sometimes referred to as PVdF) and polytetrafluoroethylene, polyolefin resin such as polyethylene and polypropylene, and resins described in WO2019 / 098384A1 or US2020 / 0274158A1.

[0144] (Positive Electrode Current Collector) The positive electrode current collector 112 of the positive electrode 110 may be a strip-shaped member made of a metal material such as Al, Ni, or stainless steel.

[0145] A method for supporting the positive electrode active material layer 111 on the positive electrode current collector 112 includes a method of pressure molding the positive electrode active material layer 111 on the positive electrode current collector 112. Cold pressing or hot pressing can be used for pressure molding.

[0146] Alternatively, a mixture of the positive electrode active material, the solid electrolyte, the conductive material, and the binder may be made into a paste using an organic solvent to form a positive electrode mixture, and the obtained positive electrode mixture may be applied to at least one surface of the positive electrode current collector 112, dried, and pressed to adhere the mixture, thereby causing the positive electrode active material layer 111 to be supported on the positive electrode current collector 112.

[0147] Alternatively, a mixture of the positive electrode active material, the solid electrolyte, and the conductive material may be made into a paste using an organic solvent to form a positive electrode mixture, and the obtained positive electrode mixture may be applied to at least one surface of the positive electrode current collector 112, dried, and sintered, thereby causing the positive electrode active material layer 111 to be supported on the positive electrode current collector 112.

[0148] An example of an organic solvent that can be used in the positive electrode mixture is N-methyl-2-pyrrolidone (hereinafter sometimes referred to as NMP).

[0149] Examples of methods for applying the positive electrode mixture to the positive electrode current collector 112 include slit die coating, screen coating, curtain coating, knife coating, gravure coating, and electrostatic spraying. A positive electrode can be manufactured by any of the methods listed above.

[0150] The positive electrode 110 can be manufactured by the method described above. Specific combinations of materials used for the positive electrode 110 include the positive electrode active material of this embodiment and the combinations shown in Table 1.

[0151]

[0152]

[0153]

[0154] (Negative Electrode) The negative electrode 120 has a negative electrode active material layer 121 and a negative electrode current collector 122. The negative electrode active material layer 121 contains a negative electrode active material. The negative electrode active material layer 121 may also contain a solid electrolyte and a conductive material. The negative electrode active material, the negative electrode current collector, the solid electrolyte, the conductive material, and the binder may be those described above.

[0155] As in the case of the positive electrode 110, methods for supporting the negative electrode active material layer 121 on the negative electrode current collector 122 include a pressure molding method, a method in which a paste-like negative electrode mixture containing a negative electrode active material is applied to the negative electrode current collector 122, dried, and then pressed and compressed, and a method in which a paste-like negative electrode mixture containing a negative electrode active material is applied to the negative electrode current collector 122, dried, and then sintered.

[0156] (Solid Electrolyte Layer) The solid electrolyte layer 130 has the above-described solid electrolyte. In one embodiment of the present invention, the solid electrolyte layer 130 is made of a solid electrolyte. In one embodiment of the present invention, the solid electrolyte layer 130 may contain a solid electrolyte and a trace amount of either or both of an organic solvent and an ionic liquid.

[0157] Examples of organic solvents that may be contained in the solid electrolyte layer 130 include ethylene carbonate, propylene carbonate, and ethyl methyl carbonate. Examples of ionic liquids that may be contained in the solid electrolyte 130 include anions such as triflate and bis(trifluoromethanesulfonyl)imide and cations such as ammonium, imidazolium, and pyridinium. Either one or both of the organic solvent and the ionic liquid preferably accounts for a weight ratio of 0.1 to 1.0 with respect to the total weight of the solid electrolyte contained in the solid electrolyte layer 130.

[0158] The solid electrolyte layer 130 can be formed by depositing an inorganic solid electrolyte on the surface of the positive electrode active material layer 111 of the above-described positive electrode 110 by a sputtering method.

[0159] The solid electrolyte layer 130 can be formed by applying a paste mixture containing a solid electrolyte to the surface of the positive electrode active material layer 111 of the above-described positive electrode 110 and drying the mixture. After drying, the mixture may be press-molded and further pressed by cold isostatic pressing (CIP) to form the solid electrolyte layer 130.

[0160] The laminate 100 can be produced by stacking the negative electrode 120 on the solid electrolyte layer 130 provided on the positive electrode 110 as described above, using a known method, in such a manner that the negative electrode active material layer 121 contacts the surface of the solid electrolyte layer 130.

[0161] In the solid secondary battery having the above-described configuration, the positive electrode active material layer uses the lithium metal composite oxide powder of the present embodiment described above, and therefore the resistance is low even when the solid secondary battery is repeatedly charged and discharged.

[0162] [Resistance Measurement After Charge-Discharge Cycle Test] (Production of Solid Secondary Battery) The following operations are carried out in a glove box under an argon atmosphere.

[0163] (Preparation of positive electrode and solid secondary battery) A solid electrolyte (MSE, 75Li) was placed in a φ10 mm pellet molding die (Hosen Co., Ltd.). 2 S・25P 2 S 5 0.16 g of powder (average particle size 1 μm or less) is placed in the mold, and the upper and lower punches are pressed into the mold. The mold is then pressurized to 10 MPa with a uniaxial press to produce a solid electrolyte layer.

[0164] Next, 1.000 g of coated lithium metal composite oxide powder as a positive electrode active material, 0.0543 g of a conductive material (acetylene black), and a solid electrolyte (MSE, Li 6 P.S. 5 Weigh out 8.6 mg of HCl.

[0165] The positive electrode active material, conductive material, and solid electrolyte were mixed in a mortar for 15 minutes to prepare a positive electrode composite, and 15 mg of the positive electrode composite was placed on the solid electrolyte layer formed in a mold. The upper punch was then inserted again, and the mixture was pressurized to 10 MPa using a uniaxial press to prepare a positive electrode on the solid electrolyte layer.

[0166] Next, the lower punch is removed, and a lithium metal foil (manufactured by Honjo Chemical Co., Ltd.) and an indium metal foil (manufactured by Nilaco Corporation) are placed on the solid electrolyte on the side opposite to the side to which the positive electrode mixture has been added. The lower punch is then reinserted, and the solid electrolyte is pressurized to 14 MPa using a uniaxial press and restrained from the outside to produce a solid secondary battery.

[0167] <Charge / Discharge Test> A charge / discharge test is carried out under the following conditions using the solid secondary battery prepared by the above method.

[0168] (Charge / Discharge Conditions) Test Temperature: 60°C (First Charge / Discharge (Initial)) Maximum charge voltage 3.98V, charge current density 0.1C, cutoff current density 0.02C, constant current-constant voltage charge Minimum discharge voltage 1.38V, discharge current density 0.1C, constant current discharge (Charge / Discharge Cycle Test) Maximum charge voltage 3.88V, charge current density 0.2C, cutoff current density 0.02C, constant current-constant voltage charge Minimum discharge voltage 1.38V, discharge current density 0.2C, constant current discharge The above charge and discharge constitute one cycle, and a total of 20 cycles were performed. (AC Impedance Measurement) After constant current-constant voltage charge with a maximum charge voltage of 3.98V, charge current density 0.1C, cutoff current density 0.02C, AC impedance measurement was performed at 25°C with a voltage amplitude of 10mV and a frequency range of 1 to 10MHz.

[0169] The impedance value |Z| at a frequency of 0.1 Hz obtained by measuring the AC impedance of the solid secondary battery using the above method is calculated and used as the resistance value after the charge-discharge cycle test. If the resistance value after the charge-discharge cycle test is 200 Ω or less, it is determined that the resistance remains low even after the charge-discharge cycle test.

[0170] Next, the present invention will be described in more detail with reference to examples.

[0171] <Composition Analysis> The composition of the lithium metal composite oxide powder produced by the method described below was analyzed by the method described above in [Composition Analysis].

[0172] <Measurement of Number Average Envelopment Degree> The number average envelopment degree 1 and number average envelopment degree 2 of the lithium metal composite oxide powder produced by the method described below were measured by the method described in the above [Method for measuring number average envelopment degree].

[0173] <Measurement of CD90 and CD10> CD90 and CD10 of the lithium metal composite oxide powder produced by the method described below were measured by the method described in the above [Method for measuring number average envelopment degree].

[0174] <Measurement of BET Specific Surface Area> The BET specific surface area of ​​the lithium metal composite oxide powder produced by the method described below was measured by the method described above in [Method for measuring BET specific surface area].

[0175] <Observation by electron microscope> A lithium metal composite oxide powder produced by the method described below was placed on a conductive sheet attached to a sample stage. Next, using a scanning electron microscope, the lithium metal composite oxide powder was irradiated with an electron beam at an acceleration voltage of 15 kV, and SEM observation (magnification: 10,000 times) was performed. The scanning electron microscope used was a JSM-5510 manufactured by JEOL Ltd.

[0176] <Resistance Measurement After Charge-Discharge Cycle Test> The resistance value after a charge-discharge cycle test of a solid secondary battery using a positive electrode active material produced by the method described below was measured by the method described in [Resistance Measurement After Charge-Discharge Cycle Test] above.

[0177] <Coating Treatment of Lithium Metal Composite Oxide> In producing and evaluating a solid secondary battery by the above method, H was applied to the lithium metal composite oxide powder produced in the examples and comparative examples described later. 3 BO 3A lithium-boron composite oxide layer with a thickness of approximately 5 nm was formed on the surface of the lithium metal composite oxide by adding and mixing 1% by weight of WAKO (manufactured by Wako Co., Ltd.) and heat-treating it at 300°C. This layer was used as a positive electrode active material. Because the coating layer was very thin at approximately 5 nm, the positive electrode active material had the same number average envelopment index of 1, number average envelopment index of 2, CD10, and CD90 as the lithium metal composite oxide.

[0178] Example 1 Production of Lithium Metal Composite Oxide E1 [Nucleation Step] Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was placed in the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0179] A nickel sulfate aqueous solution and a manganese sulfate aqueous solution were mixed in such a ratio that the atomic ratio of Ni to Mn was 0.35:0.65 to prepare a metal raw material mixture.

[0180] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel, and nitrogen gas was continuously supplied to the reaction vessel and the concentration vessel. While stirring, the metal source liquid mixture was continuously added at a flow rate of 10 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source liquid to the molar concentration of ammonium in the reaction vessel was 1.6. Furthermore, an aqueous sodium hydroxide solution was added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 11.7 (set temperature: 40°C).

[0181] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0182] [Nucleus Growth Step] Next, with nitrogen gas continuously supplied to the reaction tank and the concentration tank, the metal raw material mixture was added to the reaction tank where the nucleation step was performed at a rate of 8 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction tank at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction tank was 1.6. Furthermore, an aqueous sodium hydroxide solution was added dropwise at appropriate times so that the pH of the solution in the reaction tank was 11.0 (measurement temperature: 40°C). After 94 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0183] The obtained nickel-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried and sieved at 105°C for 20 hours to obtain nickel-manganese metal composite hydroxide E1. Nickel-manganese metal composite hydroxide E1 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder relative to Ni and Mn in the precursor was Li / (Ni + Mn) = 1.30 to obtain a mixed raw material. The resulting mixed raw material was then fired at 1000°C for 10 hours in an air atmosphere and crushed using a disk mill at a rotation speed of 1200 rpm to obtain lithium metal composite oxide E1. Composition analysis was performed and the results were compared with the composition formula (1), revealing a = 0.34 and M1 = Ni and Mn. The proportion of Ni contained in M1 was 54.7 mol%.

[0184] The lithium metal composite oxide E1 has a layered structure and a specific surface area of ​​0.6 m 2 / g.

[0185] Table 4 shows the measurement results of the number average envelopment degree 1, number average envelopment degree 2, CD10, CD90, and BET specific surface area of ​​the lithium metal composite oxide E1. The same applies to the subsequent examples and comparative examples. Figure 2 shows a scanning electron microscope photograph of the lithium metal composite oxide E1.

[0186] Example 2 Production of Lithium Metal Composite Oxide E2 [Nucleation Step] Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was charged into the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0187] A metal raw material mixture was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of manganese sulfate in such a ratio that the atomic ratio of Ni, Co, and Mn was 0.34:0.14:0.52.

[0188] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel, and nitrogen gas was continuously supplied to the reaction vessel and the concentration vessel. While stirring, the metal source liquid mixture was continuously added at a liquid feed rate of 10 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source liquid to the molar concentration of ammonium in the reaction vessel was 1.2. Furthermore, an aqueous sodium hydroxide solution was added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 11.7 (set temperature: 40°C).

[0189] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0190] [Nucleus Growth Step] Next, with nitrogen gas continuously supplied to the reaction tank and the concentration tank, the metal raw material mixture was added to the reaction tank where the nucleation step was performed at a rate of 8 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction tank at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction tank was 1.2. Furthermore, an aqueous sodium hydroxide solution was added dropwise at appropriate times so that the pH of the solution in the reaction tank was 11.0 (measurement temperature: 40°C). After 44 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0191] The obtained nickel-cobalt-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried at 105°C for 20 hours and sieved to obtain nickel-cobalt-manganese metal composite hydroxide E2. Nickel-cobalt-manganese metal composite hydroxide E2 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder to Ni, Co, and Mn in the precursor was Li / (Ni + Co + Mn) = 1.30, to obtain a mixed raw material.

[0192] The resulting mixed raw material was then fired at 900°C for 10 hours in an air atmosphere and crushed using a disk mill at 1200 rpm to obtain lithium metal composite oxide E2. Composition analysis was performed and the results, corresponding to composition formula (1), showed a = 0.27, M1 = Ni, Co, and Mn. The proportion of Ni contained in M1 was 47.3 mol%.

[0193] The lithium metal composite oxide E2 has a layered structure and a specific surface area of ​​0.9 m 2 / g.

[0194] Example 3 Production of Lithium Metal Composite Oxide E3 Nucleation Step Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was placed in the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0195] A metal raw material mixture was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of manganese sulfate in such a ratio that the atomic ratio of Ni, Co, and Mn was 0.17:0.17:0.66.

[0196] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel, and nitrogen gas was continuously supplied to the reaction vessel and the concentration vessel. While stirring, the metal source liquid mixture was continuously added at a flow rate of 10 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source liquid to the molar concentration of ammonium in the reaction vessel was 1.6. Furthermore, an aqueous sodium hydroxide solution was added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 11.7 (set temperature: 40°C).

[0197] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0198] [Nucleus Growth Step] Next, with nitrogen gas continuously supplied to the reaction tank and the concentration tank, the metal raw material mixture was added to the reaction tank where the nucleation step was performed at a rate of 8 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction tank at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction tank was 1.2. Furthermore, an aqueous sodium hydroxide solution was added dropwise at appropriate times so that the pH of the solution in the reaction tank was 11.0 (measurement temperature: 40°C). After 91 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0199] The obtained nickel-cobalt-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried at 105°C for 20 hours and sieved to obtain nickel-cobalt-manganese metal composite hydroxide E3. Nickel-cobalt-manganese metal composite hydroxide E3 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder to Ni, Co, and Mn in the precursor was Li / (Ni + Co + Mn) = 1.50, to obtain a mixed raw material.

[0200] The resulting mixed material was then fired at 900°C for 10 hours in an air atmosphere and crushed using a disk mill at 1200 rpm to obtain lithium metal composite oxide E3. Composition analysis was performed and the results, corresponding to composition formula (1), showed a = 0.47, M1 = Ni, Co, and Mn. The proportion of Ni contained in M1 was 32.5 mol%.

[0201] The lithium metal composite oxide E3 has a layered structure and a specific surface area of ​​0.9 m 2 / g.

[0202] Example 4 Production of Lithium Metal Composite Oxide E4 Nucleation Step Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was placed in the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0203] A metal raw material mixture was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of manganese sulfate in such a ratio that the atomic ratio of Ni, Co, and Mn was 0.23:0.23:0.54.

[0204] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel, and nitrogen gas was continuously supplied to the reaction vessel and the concentration vessel. While stirring, the metal source liquid mixture was continuously added at a liquid feed rate of 10 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source liquid to the molar concentration of ammonium in the reaction vessel was 1.3. Furthermore, an aqueous sodium hydroxide solution was added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 12.5 (set temperature: 40°C).

[0205] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0206] [Nucleus Growth Step] Next, with nitrogen gas continuously supplied to the reaction tank and the concentration tank, the metal raw material mixture was added to the reaction tank where the nucleation step was performed at a rate of 8 mL / min, and an aqueous ammonium sulfate solution was continuously added to the reaction tank at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction tank was 1.3. Furthermore, an aqueous sodium hydroxide solution was added dropwise at appropriate times so that the pH of the solution in the reaction tank was 11.0 (measurement temperature: 40°C). After 47 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0207] The obtained nickel-cobalt-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried at 105°C for 20 hours and sieved to obtain nickel-cobalt-manganese metal composite hydroxide E4. Nickel-cobalt-manganese metal composite hydroxide E4 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder to Ni, Co, and Mn in the precursor was Li / (Ni + Co + Mn) = 1.30, to obtain a mixed raw material.

[0208] The resulting mixed material was then fired at 900°C for 10 hours in an air atmosphere and crushed using a disk mill at 1200 rpm to obtain lithium metal composite oxide E4. Composition analysis was performed and the results were compared with composition formula (1), revealing a = 0.28 and M1 = Ni, Co, and Mn. The proportion of Ni contained in M1 was 32.5 mol%.

[0209] The lithium metal composite oxide E4 has a layered structure and a specific surface area of ​​0.9 m 2 / g.

[0210] Comparative Example 1 Production of Lithium Metal Composite Oxide C1 [Nucleation Step] Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was charged into the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0211] A metal raw material mixture was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of manganese sulfate in such a ratio that the atomic ratio of Ni, Co, and Mn was 0.23:0.23:0.54.

[0212] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel. Nitrogen gas was continuously supplied to the reaction vessel, and the concentration vessel was kept under atmospheric pressure. Under stirring, the metal source mixture was continuously added at a flow rate of 10 mL / min. An aqueous solution of ammonium sulfate was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source solution to the molar concentration of ammonium in the reaction vessel was 1.3. An aqueous solution of sodium hydroxide was also added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 11.7 (set temperature: 40°C).

[0213] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0214] [Nucleus Growth Step] Next, nitrogen gas was continuously supplied to the reaction vessel, and the concentration vessel was kept in an air atmosphere. The metal raw material mixture was added to the reaction vessel where the nucleation step was performed at a rate of 8 mL / min. An aqueous solution of ammonium sulfate was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction vessel was 1.3. A sodium hydroxide aqueous solution was also added dropwise at appropriate times to adjust the pH of the solution in the reaction vessel to 11.0 (measurement temperature: 40°C). After 27 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0215] The obtained nickel-cobalt-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried at 105°C for 20 hours and sieved to obtain nickel-cobalt-manganese metal composite hydroxide C1. Nickel-cobalt-manganese metal composite hydroxide C1 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder to Ni, Co, and Mn in the precursor was Li / (Ni + Co + Mn) = 1.30, to obtain a mixed raw material.

[0216] The resulting mixed raw material was then fired in an air atmosphere at 1100°C for 10 hours, crushed using a disk mill at 1200 rpm, and crushed in an agate mortar to obtain lithium metal composite oxide C1. Composition analysis was performed, and the results were compared with composition formula (1). The results showed a = 0.29, and M1 = Ni, Co, and Mn. The proportion of Ni contained in M1 was 33.2 mol%.

[0217] The lithium metal composite oxide C1 has a layered structure and a specific surface area of ​​0.6 m 2 / g.

[0218] Comparative Example 2 Production of Lithium Metal Composite Oxide C2 Nucleation Step Using an apparatus having a reaction tank equipped with a stirrer and an overflow pipe, a concentration tank connected to the overflow pipe, and a mechanism for circulating the water from the concentration tank to the reaction tank, water was placed in the reaction tank, and then an aqueous sodium hydroxide solution was added and the liquid temperature was maintained at 30°C.

[0219] A metal raw material mixture was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of manganese sulfate in such a ratio that the atomic ratio of Ni, Co, and Mn was 0.34:0.33:0.33.

[0220] Next, ammonium sulfate crystals, a complexing agent, were added to the reaction vessel. Nitrogen gas was continuously supplied to the reaction vessel, and the concentration vessel was kept under atmospheric pressure. Under stirring, the metal source mixture was continuously added at a flow rate of 10 mL / min. An aqueous solution of ammonium sulfate was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal source solution to the molar concentration of ammonium in the reaction vessel was 0.8. An aqueous solution of sodium hydroxide was also added dropwise from time to time to adjust the pH of the solution in the reaction vessel to 11.7 (set temperature: 40°C).

[0221] After 2 hours had passed since the start of the nucleation step, all liquid transfer was stopped.

[0222] [Nucleus Growth Step] Next, nitrogen gas was continuously supplied to the reaction vessel, and the concentration vessel was kept in an air atmosphere. The metal raw material mixture was added to the reaction vessel where the nucleation step was performed at a rate of 8 mL / min. An aqueous solution of ammonium sulfate was continuously added to the reaction vessel at a rate such that the ratio of the molar concentration of manganese salt contained in the metal raw material solution to the molar concentration of ammonium in the reaction vessel was 0.8. A sodium hydroxide aqueous solution was also added dropwise at appropriate times to adjust the pH of the solution in the reaction vessel to 11.0 (measurement temperature: 40°C). After 18 hours had elapsed since the start of the nucleus growth step, all liquid transfer was stopped, and the crystallization reaction was terminated.

[0223] The obtained nickel-cobalt-manganese metal composite hydroxide-containing slurry was washed and dehydrated, then dried at 105°C for 20 hours and sieved to obtain nickel-cobalt-manganese metal composite hydroxide C2. Nickel-cobalt-manganese metal composite hydroxide C2 and lithium hydroxide powder were weighed and mixed in a ratio such that the molar ratio of Li in the lithium hydroxide powder to Ni, Co, and Mn in the precursor was Li / (Ni + Co + Mn) = 1.03, to obtain a mixed raw material.

[0224] The resulting mixed raw material was then fired in an air atmosphere at 950°C for 10 hours and crushed using a disk mill at 1200 rpm to obtain lithium metal composite oxide C2. Composition analysis was performed and the results, corresponding to composition formula (1), showed a = 0.03 and M1 = Ni, Co, and Mn. The proportion of Ni contained in M1 was 34.9 mol%.

[0225] The lithium metal composite oxide C2 has a layered structure and a specific surface area of ​​1.0 m 2 / g.

[0226]

[0227] In Examples 1 to 4, where CD50-CD90 satisfied the range of 0.860-0.980, the resistance after the charge-discharge cycle test was less than 200 Ω, and a low-resistance solid secondary battery was obtained. This is presumably because in Examples 1 to 4, the contact area between the lithium metal composite oxide powder and the solid electrolyte increased and the contact was maintained.

[0228] In Comparative Example 1, in which CD50 - CD90 was less than 0.860, it is presumed that the solid electrolyte did not easily penetrate into the recesses on the surface of one particle of the lithium metal composite oxide, and the contact area between the lithium metal composite oxide powder and the solid electrolyte was small, resulting in an increase in resistance after the charge-discharge cycle test.

[0229] In Comparative Example 2, where a is less than 0.1, it is presumed that the crystal plane of the lithium metal composite oxide is unstable, resulting in poor interfacial bonding with the solid electrolyte, resulting in increased resistance after the charge-discharge cycle test.

[0230] 100: laminate, 110: positive electrode, 111: positive electrode active material layer, 112: positive electrode current collector, 113: external terminal, 120: negative electrode, 121: negative electrode active material layer, 122: negative electrode current collector, 123: external terminal, 130: solid electrolyte layer, 200: exterior body, 200a: opening, 1000: solid secondary battery

Claims

1. A lithium metal composite oxide powder for use in a solid secondary battery having a layered structure and containing at least Li, Mn, and an element M1, wherein, in a cumulative particle size distribution based on the volume of the projected area equivalent circle diameter of the lithium metal composite oxide powder measured by static image analysis, when the circle equivalent diameters (μm) at which the cumulative ratios from the small particle side are 50% and 90% are respectively CD50 and CD90, the number average envelopment degree of particles satisfying the range of CD50 or more and CD90 or less is 0.860 or more and 0.980 or less, and the lithium metal composite oxide powder satisfies the following composition formula (1). 2 MnO 3 ・(1-a) LiM1O 2 ... (1) (In formula (1), 0.1<a<1, and M1 is one or more elements selected from the group consisting of Ni, Co, Mn, Fe, Cu, Ti, V, Na, Mg, Ca, Sr, Ba, B, Al, Si, P, W, Mo, Nb, Zn, Sn, Zr, Cr, Ga, Ge, Pd, Ag, Cd, In, and V.) 2. The lithium metal composite oxide powder according to claim 1, wherein, in the cumulative particle size distribution, when CD10 is the circle equivalent diameter (μm) at which the cumulative proportion from the small particle side is 10%, the number average envelopment degree of particles that satisfy the range of CD10 or more and CD50 or less is 0.950 or more and less than 1.

3. The lithium metal composite oxide powder according to claim 1 or 2, wherein the CD90 is greater than 7.0 μm and not greater than 20.0 μm.

4. The lithium metal composite oxide powder according to claim 2 or 3, wherein the CD10 is 3.0 μm or more and 7.0 μm or less.

5. BET specific surface area is 0.3m 2 / g or more 2.0m 2 The lithium metal composite oxide powder according to any one of claims 1 to 4, wherein the lithium metal composite oxide powder has a molecular weight of 1000 or less.

6. The lithium metal composite oxide powder according to any one of claims 1 to 5, wherein the element M1 essentially contains Ni, and the proportion of Ni in the total amount of element M1 is 20 mol % or more.

7. A positive electrode active material for a solid secondary battery, comprising the lithium metal composite oxide powder according to any one of claims 1 to 6.

8. A positive electrode for a solid secondary battery comprising the positive electrode active material for a solid secondary battery according to claim 7.

9. A solid secondary battery comprising the positive electrode for a solid secondary battery according to claim 8.

Citation Information

Patent Citations

  • Bipolar battery and its control method

    JP2004095400A

  • All-solid-state battery

    US20120251871A1

  • All-solid state battery, electrode for all-solid state battery, and method of manufacturing the same

    US20160233510A1

  • Polymer electrolyte having multi-layer structure, and all-solid battery comprising same

    US20180159169A1

  • All-solid-state battery

    US20200259213A1