Water-dispersible acrylic adhesive composition, water-dispersible acrylic adhesive, and surface protection film

The water-dispersible acrylic pressure-sensitive adhesive composition addresses the issues of high peeling forces and contamination in conventional films by using a specific adhesive composition, resulting in a film with low initial and stable peeling forces, effectively protecting device surfaces and offering impact resistance.

WO2024219073A1PCT designated stage expired Publication Date: 2024-10-24NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/005633
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-02-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional water-dispersed acrylic adhesives used in surface protection films for optical and electronic devices exhibit high trigger peeling forces, significant changes in peeling force over time, and contamination issues, which hinder their effectiveness as removable protective films.

Method used

A water-dispersible acrylic pressure-sensitive adhesive composition is developed, comprising an acrylic polymer emulsion and an oil-soluble crosslinking agent, formed by reacting (meth)acrylic acid alkyl esters, polar group-containing monomers, and trifunctional monomers, with a reactive emulsifier, to create a film with low trigger peeling force and minimal peeling force variation over time, while suppressing adherend contamination.

Benefits of technology

The solution results in a surface protection film with a low initial peeling force, stable peeling force over time, and reduced contamination, making it suitable for protecting sensitive device surfaces and providing impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention provides: a water-dispersible acrylic adhesive composition capable of forming a water-dispersible acrylic adhesive that has a low start peel force and undergoes small changes over time in the peel force, and that can suppress contamination of an adherend; the water-dispersible acrylic adhesive formed from the water-dispersible acrylic adhesive composition; and a surface protection film having an adhesive layer that is formed from the water-dispersible acrylic adhesive. A water-dispersible acrylic adhesive composition according to an embodiment of the present invention contains an acrylic polymer emulsion (A) and a crosslinking agent (B). The acrylic polymer emulsion (A) is obtained by, in the presence of a reactive emulsifier (component d), performing emulsion polymerization of a monomer composition containing a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a trifunctional or greater polyfunctional monomer (component c). The crosslinking agent (B) is oil soluble.
Need to check novelty before this filing date? Find Prior Art

Description

Water-dispersible acrylic pressure-sensitive adhesive composition, water-dispersible acrylic pressure-sensitive adhesive, and surface protection film

[0001] The present invention relates to a water-dispersible acrylic pressure-sensitive adhesive composition, a water-dispersible acrylic pressure-sensitive adhesive, and a surface protection film. Typically, the present invention relates to a water-dispersible acrylic pressure-sensitive adhesive composition, a water-dispersible acrylic pressure-sensitive adhesive formed from the water-dispersible acrylic pressure-sensitive adhesive composition, and a surface protection film having a pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive.

[0002] Surface protective films are provided on the surfaces of optical devices such as displays and imaging devices, electronic devices, and film and glass materials that are components of these devices, for the purpose of surface protection, imparting impact resistance, etc. A typical known surface protective film is a removable surface protective film that is temporarily attached during device assembly, processing, transportation, or other pre-use stages, and is then removed again before the device is used.

[0003] A removable surface protection film has a pressure-sensitive adhesive layer made of a removable pressure-sensitive adhesive on the main surface of a substrate, and is attached to the surface of an adherend to be protected via this pressure-sensitive adhesive layer.

[0004]

[0003] Conventionally, solvent-based acrylic pressure-sensitive adhesives have typically been used as removable pressure-sensitive adhesives. However, solvent-based acrylic pressure-sensitive adhesives contain organic solvents that have a large environmental impact. Therefore, against the backdrop of the recent global trend toward reducing environmental impact, a shift from solvent-based acrylic pressure-sensitive adhesives to water-dispersible acrylic pressure-sensitive adhesives that do not use organic solvents has been considered.

[0005] For example, a removable aqueous pressure-sensitive adhesive composition capable of forming a removable water-dispersible acrylic pressure-sensitive adhesive applicable to a surface protection film has been reported, which comprises an emulsion [A] obtained by emulsion polymerization, in the presence of an anionic reactive emulsifier, of a monomer mixture containing 50 to 99.8 wt % of a (meth)acrylic acid alkyl ester (a1) containing an alkyl group having 4 to 12 carbon atoms, 0.1 to 20 wt % of a carboxyl group-containing unsaturated monomer (a2), 0.1 to 20 wt % of a polyfunctional unsaturated monomer (a3), and 0 to 49.8 wt % of other unsaturated monomer (a4), and a crosslinking agent [B] (Patent Document 1).

[0006] Another surface protection sheet reported is one obtained by applying a water-based emulsion pressure-sensitive adhesive composition to one side of a soft polyvinyl chloride sheet and then drying the composition, the pressure-sensitive adhesive composition being an acrylic water-based emulsion adhesive composition in which the interiors of the polymer emulsion particles are crosslinked, the pressure-sensitive adhesive composition being obtained by emulsion polymerization of a monomer mixture comprising a main monomer whose main component is a (meth)acrylic acid alkyl ester having an alkyl group containing 1 to 8 carbon atoms and 0.1 to 10 parts by weight of a polyfunctional monomer having two or more ethylenic double bonds in the molecule, relative to 100 parts by weight of the main monomer (Patent Document 2).

[0007] However, surface protection films having a pressure-sensitive adhesive layer composed of a conventional water-dispersible acrylic pressure-sensitive adhesive have problems such as high initial peel strength, large changes in peel strength over time, contamination of the adherend, etc. For these reasons, surface protection films having a pressure-sensitive adhesive layer composed of a water-dispersible acrylic pressure-sensitive adhesive, particularly as surface protection films to be attached to the surfaces of optical devices, electronic devices, and component parts of these devices, have not been able to exhibit satisfactory performance.

[0008] Japanese Patent Application Laid-Open No. 2004-256789 Japanese Patent Application Laid-Open No. 61-268782

[0009] An object of the present invention is to provide a water-dispersible acrylic pressure-sensitive adhesive composition capable of forming a water-dispersible acrylic pressure-sensitive adhesive that has low initial peel strength, small change in peel strength over time, and is capable of suppressing contamination of adherends. Another object of the present invention is to provide a water-dispersible acrylic pressure-sensitive adhesive formed from such a water-dispersible acrylic pressure-sensitive adhesive composition. A further object of the present invention is to provide a surface protection film having a pressure-sensitive adhesive layer composed of such a water-dispersible acrylic pressure-sensitive adhesive.

[0010] [1] A water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention comprises an acrylic polymer emulsion (A) and a crosslinking agent (B), wherein the acrylic polymer emulsion (A) is obtained by emulsion polymerization of a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) in the presence of a reactive emulsifier (component d), and the crosslinking agent (B) is an oil-soluble crosslinking agent. [2] In the water-dispersible acrylic pressure-sensitive adhesive composition according to the above [1], the (meth)acrylic acid alkyl ester (component a) may be a combination of methyl (meth)acrylate and a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms. [3] In the water-dispersible acrylic pressure-sensitive adhesive composition according to the above [1] or [2], the polar group-containing monomer (component b) may be at least one selected from the group consisting of a hydroxyl group-containing monomer and a carboxyl group-containing monomer. [4] In the water-dispersible acrylic pressure-sensitive adhesive composition according to any one of [1] to [3] above, the reactive emulsifier (component d) may be an anionic reactive emulsifier. [5] In the water-dispersible acrylic pressure-sensitive adhesive composition according to any one of [1] to [4] above, the crosslinking agent (B) may be an oil-soluble epoxy crosslinking agent. [6] A water-dispersible acrylic pressure-sensitive adhesive according to an embodiment of the present invention is formed from the water-dispersible acrylic pressure-sensitive adhesive composition according to any one of [1] to [5] above. [7] A surface protection film according to an embodiment of the present invention has a pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive according to [6] above.

[0011] According to the present invention, it is possible to provide a water-dispersible acrylic pressure-sensitive adhesive composition capable of forming a water-dispersible acrylic pressure-sensitive adhesive that has low initial peel strength, small change in peel strength over time, and is capable of suppressing contamination of an adherend. According to the present invention, it is also possible to provide a water-dispersible acrylic pressure-sensitive adhesive formed from such a water-dispersible acrylic pressure-sensitive adhesive composition. According to the present invention, it is also possible to provide a surface protection film having a pressure-sensitive adhesive layer composed of such a water-dispersible acrylic pressure-sensitive adhesive.

[0012] When the expression "weight" appears in this specification, it may be read as "mass," which is commonly used as an SI unit indicating weight.

[0013] In this specification, the term "(meth)acrylic" means "acrylic and / or methacrylic", the term "(meth)acrylate" means "acrylate and / or methacrylate", the term "(meth)allyl" means "allyl and / or methallyl", and the term "(meth)acrolein" means "acrolein and / or methacrolein".

[0014] <Water-Dispersible Acrylic Pressure-Sensitive Adhesive Composition> The water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention contains an acrylic polymer emulsion (A) and a crosslinking agent (B).

[0015] The acrylic polymer emulsion (A) is obtained by emulsion polymerizing a monomer composition containing a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) in the presence of a reactive emulsifier (component d). That is, the acrylic polymer emulsion (A) contains an acrylic polymer obtained by emulsion polymerizing a monomer composition containing a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) in the presence of the reactive emulsifier (component d). The water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention uses a combination of three specific components as a monomer composition, namely, a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c), and emulsion-polymerizes the monomer composition in the presence of a reactive emulsifier (component d). This makes it possible to provide a water-dispersible acrylic pressure-sensitive adhesive composition capable of forming a water-dispersible acrylic pressure-sensitive adhesive that has low initial peel strength, small change in peel strength over time, and is capable of suppressing contamination of adherends.

[0016] Representative examples of the (meth)acrylic acid alkyl ester (component a) include (meth)acrylic acid alkyl esters having an alkyl group of 1 to 20 carbon atoms as the alkyl group of the alkyl ester moiety. Examples of such (meth)acrylic acid alkyl esters (component a) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and methyl (meth)acrylate. Examples of suitable acrylates include isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, isotridodecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0017] The (meth)acrylic acid alkyl ester (component a) may be of one type only, or of two or more types.

[0018] The alkyl group in the alkyl ester portion of the (meth)acrylic acid alkyl ester (component a) is typically, as described above, an alkyl group having 1 to 20 carbon atoms, preferably an alkyl group having 1 to 16 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, even more preferably an alkyl group having 1 to 10 carbon atoms, and particularly preferably an alkyl group having 1 to 8 carbon atoms.

[0019] One preferred embodiment of the (meth)acrylic acid alkyl ester (component a) is a combination of methyl (meth)acrylate and a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms, for example, a combination of methyl methacrylate (MMA) and 2-ethylhexyl acrylate (2EHA). In this embodiment, the content of the (meth)acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms in the total of methyl (meth)acrylate and the (meth)acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms is preferably 50% by weight to 99.9% by weight, more preferably 60% by weight to 99% by weight, even more preferably 70% by weight to 99% by weight, even more preferably 80% by weight to 98.5% by weight, particularly preferably 90% by weight to 98% by weight, and most preferably 93% by weight to 98% by weight, in order to further exhibit the effects of the present invention.

[0020] The (meth)acrylic acid alkyl ester (component a) can be selected so that the glass transition temperature Tg of the acrylic polymer obtained from component a falls within a predetermined range, in order to further enhance the effects of the present invention. The glass transition temperature Tg of the acrylic polymer formed from component a here refers to the glass transition temperature Tg of the acrylic polymer formed from component a as the sole monomer component, and refers to the value calculated from the Fox formula based on the glass transition temperatures Tg of the homopolymers of each monomer contained in component a and the weight fractions of the monomers (copolymerization ratios on a weight basis).

[0021] The Fox equation is a relational expression between the glass transition temperature Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below: 1 / Tg=Σ(Wi / Tgi)

[0022] In the Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio on a weight basis), and Tgi represents the glass transition temperature (unit: K) of a homopolymer of monomer i. As the glass transition temperature Tg of the homopolymer, a value described in a publicly available document is adopted.

[0023] As the glass transition temperature Tg of the homopolymer, for example, the following specific values ​​can be used: Homopolymer of n-butyl acrylate (BA): -55°C Homopolymer of lauryl acrylate (LA): -23°C Homopolymer of 2-ethylhexyl acrylate (2EHA): -70°C Homopolymer of methyl methacrylate (MMA): 105°C

[0024] For the glass transition temperature Tg of homopolymers other than those exemplified above, the values ​​described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) can be used. When multiple values ​​are described in the "Polymer Handbook," the conventional value is used. For monomers not described in the "Polymer Handbook," the value in the catalog of the monomer manufacturer is used. For the glass transition temperature Tg of homopolymers of monomers not described in the "Polymer Handbook" and for which no catalog value is provided by the monomer manufacturer, the value obtained by the measurement method described in JP 2007-51271 A is used.

[0025] In terms of being able to further exhibit the effects of the present invention, the glass transition temperature Tg of the acrylic polymer obtained from component a, calculated by the above Fox's formula, is preferably −100° C. to −10° C., more preferably −90° C. to −20° C., even more preferably −80° C. to −30° C., and particularly preferably −70° C. to −40° C.

[0026] The content of the (meth)acrylic acid alkyl ester (component a) in the monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the trifunctional or higher polyfunctional monomer (component c) is preferably 50 wt% to 99.9 wt%, more preferably 60 wt% to 99 wt%, even more preferably 70 wt% to 99 wt%, even more preferably 80 wt% to 98.5 wt%, even more preferably 90 wt% to 98 wt%, even more preferably 90 wt% to 97.5 wt%, even more preferably 90 wt% to 97 wt%, even more preferably 90 wt% to 96.5 wt%, even more preferably 90 wt% to 96 wt%, even more preferably 90 wt% to 95.5 wt%, even more preferably 90 wt% to 95 wt%, particularly preferably 90.5 wt% to 94.5 wt%, and most preferably 91 wt% to 94 wt%.

[0027] Any appropriate monomer having a polar group can be used as the polar group-containing monomer (component b) as long as it does not impair the effects of the present invention. In terms of further enhancing the effects of the present invention, the polar group-containing monomer (component b) is preferably at least one selected from the group consisting of hydroxyl group-containing monomers and carboxyl group-containing monomers. Note that the term "hydroxyl group" as used herein does not include the OH moiety of a carboxyl group (-COOH).

[0028] The polar group-containing monomer (component b) may be of only one type or two or more types. The hydroxyl group-containing monomer may be of only one type or two or more types. The carboxyl group-containing monomer may be of only one type or two types.

[0029] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0030] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, (meth)acrylic acid dimer, crotonic acid, itaconic acid, and maleic acid.

[0031] One preferred embodiment of the polar group-containing monomer (component b) is a carboxyl group-containing monomer, preferably (meth)acrylic acid, more preferably acrylic acid (AA).

[0032] The content of the polar group-containing monomer (component b) in a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) is preferably 0.01 wt% to 15 wt%, more preferably 0.1 wt% to 10 wt%, even more preferably 0.5 wt% to 6 wt%, particularly preferably 1 wt% to 4.5 wt%, and most preferably 2 wt% to 3.5 wt% in order to further exhibit the effects of the present invention. If the content of the polar group-containing monomer (component b) in a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) is too low outside the above range, the initial peel strength of the resulting aqueous dispersion-type acrylic pressure-sensitive adhesive may be excessively low, or the peel strength may be excessively low, resulting in excessive ease of peeling from the adherend. If the content of the polar group-containing monomer (component b) in the monomer composition comprising the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the tri- or higher functional monomer (component c) is too high and deviates from the above range, the initial peel strength of the resulting water-dispersible acrylic pressure-sensitive adhesive may be too high, the peel strength may be too high, or the change in peel strength over time may be significant.

[0033] Examples of tri- or higher functional monomers (component c) include trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, and tripentaerythritol penta(meth)acrylate.

[0034] By using a tri- or higher functional monomer (component c), the effects of the present invention can be significantly exhibited, and in particular, a water-dispersible acrylic pressure-sensitive adhesive composition can be provided which can form a water-dispersible acrylic pressure-sensitive adhesive having a low initial peel strength and little change in peel strength over time.Furthermore, compared to the case where a bifunctional polyfunctional monomer is used, the gel content of the acrylic polymer emulsion (A) can be appropriately increased.

[0035] The content of the tri- or higher functional monomer (component c) in a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) is preferably 0.01 wt% to 5 wt%, more preferably 0.1 wt% to 3.5 wt%, even more preferably 0.2 wt% to 3 wt%, particularly preferably 0.3 wt% to 2 wt%, and most preferably 0.4 wt% to 1.5 wt%, in order to further exhibit the effects of the present invention. If the content of the tri- or higher functional monomer (component c) in a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a tri- or higher functional monomer (component c) is too low outside the above range, the initial peel strength of the resulting aqueous dispersion-type acrylic pressure-sensitive adhesive may be increased, the peel strength may be increased, or the peel strength may change significantly over time. If the content of the tri- or higher functional monomer (component c) in the monomer composition comprising the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the tri- or higher functional monomer (component c) is too high and deviates from the above range, the acrylic polymer emulsion (A) may undergo excessive gelation, which may prevent polymerization, or may increase the initial peel strength of the resulting water-dispersible acrylic pressure-sensitive adhesive, or may result in significant change in the peel strength over time.

[0036] The monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the trifunctional or higher polyfunctional monomer (component c) may contain any appropriate other monomer within the range not impairing the effects of the present invention. Such other monomer may be one type only, or two or more types.

[0037] The content of other monomers in the monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the tri- or higher functional monomer (component c) is preferably 0% by weight to 10% by weight, more preferably 0% by weight to 5% by weight, even more preferably 0% by weight to 1% by weight, particularly preferably 0% by weight to 0.1% by weight, and most preferably 0% by weight to 0.05% by weight, in order to further exhibit the effects of the present invention.

[0038] The acrylic polymer emulsion (A) is obtained by emulsion polymerization of a monomer composition containing a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a trifunctional or higher polyfunctional monomer (component c) in the presence of a reactive emulsifier (component d).

[0039] As the reactive emulsifier (component d), any appropriate reactive emulsifier can be used as long as it is a reactive emulsifier and does not impair the effects of the present invention. The reactive emulsifier (component d) may be a single type or two or more types. Here, the reactive emulsifier refers to an emulsifier having a reactive group capable of undergoing a polymerization reaction with a monomer in the monomer composition. Examples of such reactive groups include alkenyl groups such as a vinyl group, an allyl group, and a 1-propenyl group, and a (meth)acryloyl group.

[0040] In an embodiment of the present invention, the use of a reactive emulsifier (component d) as an emulsifier can effectively suppress contamination of an adherend by the resulting water-dispersible acrylic pressure-sensitive adhesive. When a non-reactive emulsifier is used as the emulsifier, the non-reactive emulsifier is more likely to be liberated in the resulting water-dispersible acrylic pressure-sensitive adhesive, which may migrate to the adherend and cause contamination.

[0041] Examples of the reactive emulsifier (component d) include anionic reactive emulsifiers and nonionic reactive emulsifiers.

[0042] Examples of the anionic reactive emulsifier include polyoxyethylene alkyl ether sulfates ("Aqualon KH-05" series, "Aqualon KH-10" series, and "Aqualon KH-20" series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; "ADEKA REASOAP SR-10N" series and "ADEKA REASOAP SR-20N" series manufactured by ADEKA Corporation; and "LATEMUL PD-104" series manufactured by Kao Corporation); polyoxyethylene styrenated phenyl ether sulfates (Dai-ichi Kogyo Seiyaku Co., Ltd.'s "Aqualon AR-10" series, "Aqualon AR-20" series, etc.); sulfosuccinate esters (Kao Corporation's "Latemul S-120" series, "Latemul S-120A" series, "Latemul S-180P" series, "Latemul S-180A" series; Sanyo Chemical Co., Ltd.'s "Eleminol JS-2" series, etc.); polyoxyethylene nonyl flobenylphenyl ether sulfates (Dai-ichi Kogyo Seiyaku Co., Ltd.'s " "Aqualon HS-10" series, "Aqualon HS-20" series, "Aqualon HS-30" series, "Aqualon BC-10" series, "Aqualon BC-20" series; "ADEKA REASOAP SDX-222" series, "ADEKA REASOAP SDX-223" series, "ADEKA REASOAP SDX-232" series, "ADEKA REASOAP SDX-233" series, "ADEKA REASOAP SDX-259" series, and "ADEKA REASOAP SDX-259" series manufactured by ADEKA Corporation. SE-10N series, ADEKA REASOAP SE-20N series, etc.); (meth)acrylate sulfate esters (Antox MS-60 series, Antox MS-2N series manufactured by Nippon Nyukazai Co., Ltd.; Eleminol RS-30 series manufactured by Sanyo Chemical Industries, Ltd.; phosphate esters (H-3330PL series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; Adeka Reasop PP-70 series manufactured by ADEKA Corporation, etc.).

[0043] Examples of nonionic reactive emulsifiers include polyoxyethylene alkyl ethers ("ADEKA REASOAP ER-10" series, "ADEKA REASOAP ER-20" series, "ADEKA REASOAP ER-30" series, and "ADEKA REASOAP ER-40" series manufactured by ADEKA Corporation; "LATEMUL PD-420" series, "LATEMUL PD-430" series, and "LATEMUL PD-450" series manufactured by Kao Corporation); polyoxyalkylene styrenated phenyl ethers ("AQUALON AN-10" series and "AQUALON AN-20" series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.); polyoxyethylene alkyl phenyl ethers ("AQUALON AN-10" series and "AQUALON AN-20" series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.); Examples of such an alkyl ether-based or alkylphenyl ester-based surfactants include the "Aqualon RN-10" series, "Aqualon RN-20" series, "Aqualon RN-30" series, and "Aqualon RN-50" series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; the "ADEKA REASOAP NE-10" series, "ADEKA REASOAP NE-20" series, "ADEKA REASOAP NE-30" series, and "ADEKA REASOAP NE-40" series manufactured by ADEKA Corporation; and (meth)acrylate sulfate-based surfactants include the "RMA-564" series, "RMA-568" series, and "RMA-1114" series manufactured by Nippon Nyukazai Co., Ltd.

[0044] As the reactive emulsifier (component d), an anionic reactive emulsifier is preferred, as it can more effectively exhibit the effects of the present invention.

[0045] The amount of reactive emulsifier (component d) used is preferably 0.5 to 10 parts by weight, more preferably 1.0 to 8 parts by weight, even more preferably 1.2 to 6 parts by weight, and particularly preferably 1.5 to 5 parts by weight, per 100 parts by weight of the monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the trifunctional or higher polyfunctional monomer (component c). If the amount of reactive emulsifier (component d) used is too small outside the above range, the emulsion polymerization may become unstable. If the amount of reactive emulsifier (component d) used is too large outside the above range, the amount of unreacted reactive emulsifier (d) increases, which may migrate to the adherend and cause contamination.

[0046] The reactive emulsifier (component d) may be used in combination with a non-reactive anionic emulsifier or a non-reactive nonionic emulsifier, if necessary, within the range that does not impair the effects of the present invention.

[0047] Examples of non-reactive anionic emulsifiers include alkyl sulfates, alkylbenzene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, polyoxyethylene alkyl sulfates, and polyoxyethylene alkyl phosphates. Examples of non-reactive nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, oxyethylene-oxypropylene block polymers, sorbitan fatty acid esters, and polyoxyethylene fatty acids.

[0048] In the emulsion polymerization, a polymerization initiator is preferably used. The polymerization initiator may be one kind or two or more kinds.Examples of the polymerization initiator include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate; hydrogen peroxide; 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[N-(2-carboxyethyl)amidino]propane}n hydrate, and 2,2'-azobis(N,N'-dimethyleneisobutylamidine), dimethyl-2,2' -azobisisobutyrate, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), ammonium (amine) salt of 4,4'-azobis-4-cyanovaleric acid, 2,2'-azobis(2-methylamidoxime) dihydrochloride, 2,2'-azobis(2-methylbutanamidoxime) dihydrochloride tetrahydrate, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]-propionamide}, Azo initiators such as 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide]; alkyl peroxides, t-butyl hydroperoxide, cumene hydroperoxide, p-methane hydroperoxide, lauroyl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, t-butylcumyl peroxide, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, 1,1-bis(2-methyl-N-propionamide)- Examples of the peroxide include organic peroxides such as (t-butylperoxy)-3,3,5-trimethylcyclohexane, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, di-isobutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and t-butylperoxyisobutyrate; and redox polymerization initiators (for example, a combination of aqueous hydrogen peroxide and ascorbic acid, a combination of aqueous hydrogen peroxide and an iron (II) salt, or a combination of a persulfate and sodium hydrogen sulfite).

[0049] The amount of the polymerization initiator used is preferably 0.001 to 5 parts by weight, more preferably 0.01 to 4 parts by weight, still more preferably 0.03 to 3 parts by weight, and particularly preferably 0.05 to 2 parts by weight, relative to 100 parts by weight of the monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the tri- or higher functional monomer (component c).

[0050] The amount of water used in emulsion polymerization may be any appropriate amount as long as it does not impair the effects of the present invention. The amount of water used is preferably 25 to 900 parts by weight, more preferably 30 to 600 parts by weight, even more preferably 35 to 500 parts by weight, particularly preferably 40 to 450 parts by weight, and most preferably 43 to 400 parts by weight, relative to 100 parts by weight of the monomer composition containing the (meth)acrylic acid alkyl ester (component a), the polar group-containing monomer (component b), and the trifunctional or higher polyfunctional monomer (component c).

[0051] As the emulsion polymerization method, any suitable method can be adopted as long as it does not impair the effects of the present invention.As such a method, for example, a method can be mentioned in which a part of water and a polymerization initiator are charged into a reaction vessel, a monomer composition containing (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a trifunctional or higher polyfunctional monomer (component c), a reactive emulsifier (d), and the rest of the water are charged into a separate vessel, and stirred to prepare a monomer emulsion, and this monomer emulsion is added to the reaction vessel, heated, and polymerized.

[0052] The polymerization temperature for the emulsion polymerization may be any appropriate temperature within a range that does not impair the effects of the present invention, such as 50°C to 90°C.

[0053] The polymerization time for emulsion polymerization may be any appropriate time within the range that does not impair the effects of the present invention, for example, 0.5 to 10 hours.

[0054] During emulsion polymerization, any suitable additive may be added in any suitable amount depending on the purpose, as long as the effects of the present invention are not impaired. Examples of such additives include tackifiers, plasticizers, antiseptics / antifungals, rust inhibitors, freeze-thaw stabilizers, high-boiling solvents, pigments, colorants, fillers, metal powders, antifoaming agents, thickeners, adhesion control agents, and chain transfer agents.

[0055] After the emulsion polymerization, the pH may be adjusted using an alkaline compound (for example, aqueous ammonia).

[0056] The acrylic polymer emulsion (A) obtained by emulsion polymerization preferably has a gel fraction of 80% by weight or more, more preferably 85% by weight or more, even more preferably 90% by weight or more, particularly preferably 92% by weight or more, and most preferably 94% by weight or more, in order to further demonstrate the effects of the present invention. The upper limit of the gel fraction is preferably 99.9% by weight or less, more preferably 99.5% by weight or less, even more preferably 99% by weight or less, particularly preferably 98.7% by weight or less, and most preferably 98.5% by weight or less, in order to further demonstrate the effects of the present invention. If the gel fraction of the acrylic polymer emulsion (A) is too small and outside the above range, the initial peel strength of the resulting water-dispersible acrylic pressure-sensitive adhesive may be too high, the peel strength may be too high, or the peel strength may change significantly over time.

[0057] In this manner, an acrylic polymer emulsion (A) can be obtained which contains, as a solid content, an acrylic polymer obtained by emulsion polymerizing a monomer composition containing a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b), and a trifunctional or higher functional monomer (component c) in the presence of a reactive emulsifier (component d).

[0058] In an embodiment of the present invention, the crosslinking agent (B) is an oil-soluble crosslinking agent.

[0059] The oil-soluble crosslinking agent may also be referred to as a water-insoluble crosslinking agent, a non-hydrophilic crosslinking agent, or a hydrophobic crosslinking agent. The oil-soluble crosslinking agent may be one type only, or two or more types may be used.

[0060] Examples of oil-soluble crosslinking agents include oil-soluble epoxy-based crosslinking agents such as N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane, and 1,6-hexanediol diglycidyl ether; oil-soluble isocyanate-based crosslinking agents such as hexamethylene diisocyanate; and oil-soluble carbodiimide-based crosslinking agents. Among these, oil-soluble epoxy-based crosslinking agents are preferred in that they can better exhibit the effects of the present invention.

[0061] Specific examples of oil-soluble epoxy crosslinking agents include those manufactured by Nagase ChemteX Corporation under the trade names "Denacol EX-321", "Denacol EX-321L", "Denacol EX-622", "Denacol EX-201", "Denacol EX-201-IM", "Denacol EX-211", "Denacol EX-212", "Denacol EX-212L", "Denacol EX-252", and " Denacol EX-931, trade name "Denacol EX-991L", trade name "Denacol EX-121", trade name "Denacol EX-141", trade name "Denacol EX-142-IM", trade name "Denacol EX-146", trade name "Denacol EX-146P", trade name "Denacol EX-192", trade name "Denacol EX-731"; and trade names "TETRAD-C" and "TETRAD-X" manufactured by Mitsubishi Gas Chemical Company, Inc. can be used.

[0062] The content of the crosslinking agent (B) in the water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, even more preferably 0.1 to 5 parts by weight, even more preferably 0.2 to 4 parts by weight, particularly preferably 0.25 to 2.5 parts by weight, and most preferably 0.3 to 2.0 parts by weight, relative to 100 parts by weight of the acrylic polymer (solid content), in order to further exhibit the effects of the present invention. If the content of the crosslinking agent (B) relative to 100 parts by weight of the acrylic polymer (solid content) is too low, outside the above range, the initial peel strength of the resulting water-dispersible acrylic pressure-sensitive adhesive may be too high, the peel strength may be too high, or the peel strength may change significantly over time. If the content ratio of the crosslinking agent (B) relative to 100 parts by weight of the acrylic polymer (solid content) is too large and deviates from the above range, the initial peel strength of the resulting water-dispersible acrylic pressure-sensitive adhesive may become excessively small, or the peel strength may become excessively small, resulting in the adhesive being excessively prone to peeling from the adherend.

[0063] The water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention may contain any suitable additive in any suitable amount depending on the purpose, as long as the effects of the present invention are not impaired. Examples of such additives include tackifiers, plasticizers, antiseptics / antifungals, rust inhibitors, freeze-thaw stabilizers, high-boiling solvents, pigments, colorants, fillers, metal powders, antifoaming agents, thickeners, adhesion control agents, and chain transfer agents.

[0064] In this manner, the water-dispersible acrylic pressure-sensitive adhesive composition according to the embodiment of the present invention can be obtained.

[0065] <Water-Dispersible Acrylic Pressure-Sensitive Adhesive> The water-dispersible acrylic pressure-sensitive adhesive according to an embodiment of the present invention is formed from the water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention.

[0066] The water-dispersible acrylic pressure-sensitive adhesive according to an embodiment of the present invention may be a pressure-sensitive adhesive in any shape. Typically, the water-dispersible acrylic pressure-sensitive adhesive according to an embodiment of the present invention is a sheet-shaped water-dispersible acrylic pressure-sensitive adhesive. A sheet-shaped water-dispersible acrylic pressure-sensitive adhesive is typically recognized as one of the constituent members, such as a water-dispersible acrylic pressure-sensitive adhesive layer.

[0067] The water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention can be defined as one formed from a water-dispersible acrylic pressure-sensitive adhesive composition in this way. This is because a water-dispersible acrylic pressure-sensitive adhesive becomes a water-dispersible acrylic pressure-sensitive adhesive when a water-dispersible acrylic pressure-sensitive adhesive composition undergoes a crosslinking reaction, etc., upon heating, etc., and therefore, there are circumstances that make it impossible and almost impractical to directly identify a water-dispersible acrylic pressure-sensitive adhesive by its structure ("impossible / impractical circumstances"). Therefore, the definition of "something formed from a water-dispersible acrylic pressure-sensitive adhesive composition" appropriately identifies the water-dispersible acrylic pressure-sensitive adhesive as a "product."

[0068] Any appropriate method may be employed to form the water-dispersible acrylic pressure-sensitive adhesive according to an embodiment of the present invention, provided that it does not impair the effects of the present invention. Examples of methods for forming such water-dispersible acrylic pressure-sensitive adhesive include applying a water-dispersible acrylic pressure-sensitive adhesive composition to a suitable substrate, and optionally heating and drying the composition to form a sheet of the water-dispersible acrylic pressure-sensitive adhesive on the substrate. Any appropriate means may be employed for such application, provided that it does not impair the effects of the present invention. Examples of such application means include a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, an air knife coater, a spray coater, a comma coater, a direct coater, and a roll brush coater. Any appropriate means may be employed to heat and dry the water-dispersible acrylic pressure-sensitive adhesive composition, provided that it does not impair the effects of the present invention. Examples of such heating and drying means include heating to approximately 60°C to 180°C. If necessary, the curing may be accelerated by irradiation with ultraviolet rays, laser rays, α rays, β rays, γ rays, X rays, electron beams, or the like.

[0069] <Surface Protection Film> The surface protection film according to the embodiment of the present invention has a pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention.

[0070] The surface protection film according to the embodiment of the present invention typically has a pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention and a substrate layer. The surface protection film according to the embodiment of the present invention may have any appropriate other layer in addition to the pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention and the substrate layer, as long as the effects of the present invention are not impaired. The surface protection film according to the embodiment of the present invention typically has a pressure-sensitive adhesive layer composed of the water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention and a substrate layer.

[0071] The substrate layer may be one layer or two or more layers, but is preferably one layer in that the effects of the present invention can be more effectively exhibited.

[0072] The thickness of the substrate layer is preferably 1 μm to 500 μm, more preferably 5 μm to 300 μm, even more preferably 10 μm to 100 μm, particularly preferably 15 μm to 80 μm, and most preferably 20 μm to 60 μm. When the thickness of the substrate layer is within the above range, the effects of the present invention can be more effectively exhibited.

[0073] Any appropriate material can be used as the material for the substrate layer as long as it does not impair the effects of the present invention. A typical example of the material for such a substrate layer is a resin material.

[0074] Examples of resin materials for the substrate layer include acrylic resins such as polyimide (PI), polyether ether ketone (PEEK), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose (TAC), polysulfone, polyarylate, polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, ethylene-vinyl acetate copolymer (EVA), polyamide (nylon), wholly aromatic polyamide (aramid), polyvinyl chloride (PVC), polyvinyl acetate, polyphenylene sulfide (PPS), fluorine-based resins, and cyclic olefin polymers.

[0075] The pressure-sensitive adhesive layer may be one layer or two or more layers, but is preferably one layer in that the effects of the present invention can be more effectively exhibited.

[0076] The thickness of the pressure-sensitive adhesive layer is preferably 1 μm to 250 μm, more preferably 1 μm to 150 μm, even more preferably 2 μm to 100 μm, even more preferably 2 μm to 80 μm, still more preferably 2 μm to 50 μm, particularly preferably 3 μm to 40 μm, and most preferably 3 μm to 30 μm. When the thickness of the pressure-sensitive adhesive layer is within the above range, the effects of the present invention can be more effectively exhibited.

[0077] The surface protection film according to the embodiment of the present invention may be provided with any appropriate release liner on the surface of the pressure-sensitive adhesive layer opposite the substrate layer for protection until use.

[0078] Examples of release liners include release liners in which the surface of a substrate (liner substrate) such as paper or plastic film is silicone-treated, release liners in which the surface of a substrate (liner substrate) such as paper or plastic film is laminated with a polyolefin resin, etc. Examples of plastic films as liner substrates include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polybutylene terephthalate films, polyurethane films, ethylene-vinyl acetate copolymer films, etc.

[0079] The thickness of the release liner can be any appropriate thickness as long as it does not impair the effects of the present invention. In order to further exhibit the effects of the present invention, the thickness is preferably 3 μm to 200 μm, and more preferably 10 μm to 100 μm. Of the surfaces of the release liner, the surface that is bonded to the PSA layer may be subjected to a release treatment or an antifouling treatment using a conventionally known release agent (e.g., a silicone-based release agent, a fluorine-based release agent, a long-chain alkyl-based release agent, or a fatty acid amide-based release agent) or silica powder.

[0080] The thickness of the surface protection film according to the embodiment of the present invention is preferably 1 μm to 400 μm, more preferably 2 μm to 300 μm, even more preferably 5 μm to 300 μm, particularly preferably 10 μm to 200 μm, and most preferably 20 μm to 100 μm.

[0081] The surface protection film according to the embodiment of the present invention can be produced by employing the method for forming the water-dispersible acrylic pressure-sensitive adhesive according to the embodiment of the present invention described above, for example, by applying a water-dispersible acrylic pressure-sensitive adhesive composition to a material to be used as a substrate for the surface protection film, and optionally heating and drying the composition to form a sheet of the water-dispersible acrylic pressure-sensitive adhesive on the substrate.

[0082] The surface protection film according to an embodiment of the present invention preferably exhibits an initial peel strength of 0.01 N / 25 mm to 2 N / 25 mm, more preferably 0.05 N / 25 mm to 1.6 N / 25 mm, even more preferably 0.1 N / 25 mm to 1.4 N / 25 mm, particularly preferably 0.2 N / 25 mm to 1.2 N / 25 mm, and most preferably 0.2 N / 25 mm to 1 N / 25 mm, after being attached to a glass plate and left for 30 minutes in an environment of 23°C and 50% RH. If the initial peel strength is within the above range, the effects of the present invention can be more effectively exhibited. The initial peel strength is an indicator of the maximum stress applied at the beginning of peeling, and a specific measurement method will be described later.

[0083] The surface protection film according to an embodiment of the present invention preferably exhibits a peel strength after attachment to a glass plate, storage at 50°C for one week, and then storage at 23°C x 50% RH for two hours of aging, of 0.01 N / 25 mm to 2 N / 25 mm, more preferably 0.05 N / 25 mm to 1.6 N / 25 mm, even more preferably 0.1 N / 25 mm to 1.4 N / 25 mm, particularly preferably 0.2 N / 25 mm to 1.2 N / 25 mm, and most preferably 0.2 N / 25 mm to 1 N / 25 mm. When the peel strength is within the above range, the effects of the present invention can be more effectively exhibited. The peel strength after attachment is an index of the maximum stress applied at the beginning of peeling after storage at 50°C for one week, and a specific measurement method will be described later.

[0084] The surface protection film according to an embodiment of the present invention preferably exhibits an initial peel strength of 0.01 N / 25 mm to 1 N / 25 mm, more preferably 0.05 N / 25 mm to 0.8 N / 25 mm, even more preferably 0.07 N / 25 mm to 0.5 N / 25 mm, particularly preferably 0.09 N / 25 mm to 0.3 N / 25 mm, and most preferably 0.1 N / 25 mm to 0.28 N / 25 mm, after being attached to a glass plate and left in an environment of 23°C and 50% RH for 30 minutes. If the initial peel strength is within the above range, the effects of the present invention can be more effectively exhibited. The initial peel strength is an index of the peel strength in the range where the value stabilizes after peeling begins, and a specific measurement method will be described later.

[0085] The surface protection film according to an embodiment of the present invention preferably exhibits a peel strength over time of 0.01 N / 25 mm to 1 N / 25 mm, more preferably 0.05 N / 25 mm to 0.8 N / 25 mm, even more preferably 0.07 N / 25 mm to 0.5 N / 25 mm, particularly preferably 0.09 N / 25 mm to 0.3 N / 25 mm, and most preferably 0.1 N / 25 mm to 0.28 N / 25 mm, after being attached to a glass plate and stored in a 50°C environment for one week, followed by being left in a 23°C x 50% RH environment for two hours. When the peel strength over time is within the above range, the effects of the present invention can be more effectively exhibited. The peel strength over time is an index of the peel strength in the range where the value stabilizes after peeling begins after storage in a 50°C environment for one week, and a specific measurement method will be described later.

[0086] In the surface protection film according to an embodiment of the present invention, the rate of increase in peel strength over time, which indicates the degree of increase in peel strength over time relative to the initial peel strength ((peel strength over time / initial peel strength) x 100), is preferably 80% to 150%, more preferably 85% to 140%, even more preferably 90% to 135%, and particularly preferably 95% to 130%. When the rate of increase in peel strength over time is within the above range, the effects of the present invention can be more effectively exhibited.

[0087] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The test and evaluation methods used in the examples are as follows. The term "parts" means "parts by weight" unless otherwise specified, and the term "%" means "% by weight" unless otherwise specified.

[0088] <Measurement of gel fraction of emulsion> Approximately 0.1 g of the acrylic polymer in the acrylic polymer emulsion was collected and wrapped in a porous tetrafluoroethylene sheet (trade name "NTF1122", manufactured by Nitto Denko Corporation) with an average pore size of 0.2 μm, and then tied with kite string. The weight at this time was measured and recorded as the weight before immersion. The weight before immersion is the total weight of the acrylic polymer (collected above), the tetrafluoroethylene sheet, and the kite string. The total weight of the tetrafluoroethylene sheet and the kite string was also measured, and this total weight was recorded as the bag weight. Next, the acrylic polymer wrapped in the porous tetrafluoroethylene sheet and tied with kite string (hereinafter referred to as the "sample") was placed in a 50 ml container filled with ethyl acetate and allowed to stand at 23°C for 7 days. The sample (after ethyl acetate treatment) was then removed from the container, transferred to an aluminum cup, and dried in a dryer at 130°C for 2 hours to remove the ethyl acetate. The weight was then measured and used as the post-immersion weight. The gel fraction of the emulsion was calculated using the following formula (1). In the following formula (1), a is the post-immersion weight, b is the envelope weight, and c is the pre-immersion weight. Gel fraction (wt%) = (a - b) / (c - b) x 100 (1)

[0089] <Initial peel strength and initial peel strength> The prepared surface protection film was cut to a size of 25 mm wide and 100 mm long, and after peeling off the release liner, it was laminated to a glass plate using a 2 kg roller to prepare an evaluation sample. After lamination, the sample was left in an environment of 23 ° C. x 50% RH for 30 minutes. Then, a single-sided adhesive tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)") cut to a size of 25 mm wide and 50 mm long was pressed onto the substrate side of the evaluation sample (glass plate with surface protection film) so that the edge protruded 1 mm, and left for 10 seconds. Then, using a universal tensile tester, the single-sided adhesive tape was peeled from the edge protruding 1 mm at a peel speed of 0.3 m / min and a peel angle of 180°. The maximum stress applied at the beginning of peeling was recorded as the "initial peel strength (N / 25 mm)." The adhesive strength in the range where the value stabilized was measured and recorded as the "initial peel strength (N / 25 mm)." The measurement was carried out in an environment of 23°C and 50% RH.

[0090] <Temporal Peel Force and Time-Varying Peel Force> The evaluation sample (glass plate with surface protective film) was stored in a 50°C environment for one week, and then left in a 23°C x 50% RH environment for two hours. A single-sided adhesive tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)") cut to a size of 25 mm wide and 50 mm long was then pressed onto the substrate side of the evaluation sample (glass plate with surface protective film) so that the edge was 1 mm protruding, and the sample was left for 10 seconds. The single-sided adhesive tape was then peeled from the 1 mm protruding edge using a universal tensile tester at a peel speed of 0.3 m / min and a peel angle of 180°. The maximum stress applied at the beginning of peeling was recorded as the "temporal peel force (N / 25 mm)." The adhesive force in the range where the value stabilized was measured and recorded as the "time-varying peel force (N / 25 mm)." The measurement was performed in a 23°C x 50% RH environment.

[0091] <Contamination (Whitening)> The prepared surface protective film was cut to a size of 25 mm wide and 100 mm long, and the release liner was peeled off. Then, using a laminator (a small laminator manufactured by Tester Sangyo Co., Ltd.), the film was bonded to a polarizing plate (manufactured by Nitto Denko Corporation, product name "SEG1425DU", size: 70 mm wide x 120 mm long) under conditions of 0.25 MPa and 0.3 m / min. The polarizing plate to which the surface protective film was attached was left at 80°C for 4 hours, and then the surface protective film was peeled off. The polarizing plate from which the surface protective film had been peeled was then left in a humidified environment (23°C, 90% RH) for 12 hours, and the polarizing plate surface was visually observed. The low-contamination properties were evaluated according to the following criteria. If whitening occurs on the polarizing plate as an adherend under humidified conditions (high humidity conditions) after application and peeling of the surface protective film, this means that the low-contamination properties are insufficient for use as a surface protective film for optical components. ◯: Good low-staining properties (no difference was observed between the area where the surface protective film was attached and the area where it was not attached). ×: Poor low-staining properties (whitening was observed in the area where the surface protective film was attached).

[0092] Example 1 Preparation of Acrylic Polymer Emulsion 30 parts by weight of water, 95 parts by weight of 2-ethylhexyl acrylate (2EHA), 4 parts by weight of methyl methacrylate (MMA), 3 parts by weight of acrylic acid (AA), 0.3 parts by weight of trimethylolpropane triacrylate (TMPTA), and 12 parts by weight (3 parts by weight as solids) of a reactive anionic emulsifier (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., trade name "Aqualon KH-1025", solids concentration = 25 wt%) were blended in a vessel, and then stirred and mixed using a homomixer to prepare a monomer emulsion. Next, 50 parts by weight of water and 0.1 parts by weight of a polymerization initiator (ammonium persulfate (APS)) were added to a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and the monomer emulsion was added over 3 hours with stirring, followed by a reaction at 75°C for 3 hours. Next, the mixture was cooled to 30°C, and a 10 wt% aqueous ammonia solution was added to adjust the pH to 8, thereby preparing an acrylic polymer emulsion (1) containing the acrylic polymer (1) (concentration of the acrylic polymer (1) (solid content concentration) = 55 wt%).

[0093] <Preparation of Water-Dispersible Acrylic Pressure-Sensitive Adhesive Composition> To the acrylic polymer emulsion (1) prepared above, 0.5 parts by weight of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "TETRAD-C", 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, epoxy equivalent=110, number of functional groups=4), which is an oil-soluble crosslinking agent, was added per 100 parts by weight of the acrylic polymer (1) (solid content), and the mixture was stirred and mixed using a stirrer under stirring conditions of 23°C, 300 rpm, and 10 minutes, to prepare a water-dispersible acrylic pressure-sensitive adhesive composition (1).

[0094] <Preparation of Surface Protection Film> The water-dispersible acrylic pressure-sensitive adhesive composition (1) prepared above was applied (coated) onto the corona-treated surface of a PET film (manufactured by Toyobo Co., Ltd., trade name "E7415", thickness = 38 μm) using an applicator manufactured by Tester Sangyo Co., Ltd. so as to give a dried thickness of 5 μm, and then dried at 130°C for 1 minute in a hot air circulation oven to form an acrylic pressure-sensitive adhesive layer. The obtained acrylic pressure-sensitive adhesive layer was attached to a release liner and then aged at room temperature for 1 week to obtain a surface protection film (1). The results are shown in Table 1.

[0095] [Example 2] The same procedure as in Example 1 was carried out except that the amount of trimethylolpropane triacrylate (TMPTA) was changed to 0.5 parts by weight, to obtain an acrylic polymer emulsion (2) containing an acrylic polymer (2) (concentration of acrylic polymer (2) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (2), and a surface protection film (2). The results are shown in Table 1.

[0096] [Example 3] An acrylic polymer emulsion (3) containing the acrylic polymer (3) (concentration of the acrylic polymer (3) (solid content) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (3), and a surface protection film (3) were obtained in the same manner as in Example 1, except that the amount of trimethylolpropane triacrylate (TMPTA) was changed to 1 part by weight. The results are shown in Table 1.

[0097] [Example 4] The same procedure as in Example 2 was carried out except that the amount of acrylic acid (AA) was changed to 1 part by weight, to obtain an acrylic polymer emulsion (4) containing an acrylic polymer (4) (concentration of acrylic polymer (4) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (4), and a surface protection film (4). The results are shown in Table 1.

[0098] [Example 5] The same procedure as in Example 2 was carried out except that the amount of acrylic acid (AA) was changed to 4 parts by weight, to obtain an acrylic polymer emulsion (5) containing an acrylic polymer (5) (concentration of acrylic polymer (5) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (5), and a surface protection film (5). The results are shown in Table 1.

[0099] Example 6 An acrylic polymer emulsion (6) containing acrylic polymer (6) (concentration of acrylic polymer (6) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (6), and a surface protection film (6) were obtained in the same manner as in Example 2, except that the amount of the oil-soluble crosslinking agent TETRAD-C was changed to 0.2 parts by weight. The results are shown in Table 1.

[0100] Example 7 An acrylic polymer emulsion (7) containing acrylic polymer (7) (concentration of acrylic polymer (7) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (7), and a surface protection film (7) were obtained in the same manner as in Example 2, except that the amount of the oil-soluble crosslinking agent TETRAD-C was changed to 1.5 parts by weight. The results are shown in Table 1.

[0101] Example 8 An acrylic polymer emulsion (8) containing an acrylic polymer (8) (concentration of acrylic polymer (8) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (8), and a surface protection film (8) were obtained in the same manner as in Example 2, except that the amount of the oil-soluble crosslinking agent TETRAD-C was changed to 3 parts by weight. The results are shown in Table 1.

[0102] [Example 9] The same procedure as in Example 3 was carried out, except that in the preparation of the acrylic polymer emulsion, the amount of 2-ethylhexyl acrylate (2EHA) was changed to 80 parts by weight and the amount of methyl methacrylate (MMA) was changed to 20 parts by weight, to obtain an acrylic polymer emulsion (9) containing an acrylic polymer (9) (concentration of acrylic polymer (9) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (9), and a surface protection film (9). The results are shown in Table 1.

[0103] [Example 10] The same procedure as in Example 3 was carried out, except that in the preparation of the acrylic polymer emulsion, the amount of 2-ethylhexyl acrylate (2EHA) was changed to 70 parts by weight and the amount of methyl methacrylate (MMA) was changed to 30 parts by weight, to obtain an acrylic polymer emulsion (10) containing an acrylic polymer (10) (concentration of acrylic polymer (10) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (10), and a surface protection film (10). The results are shown in Table 1.

[0104] Comparative Example 1 An acrylic polymer emulsion (C1) containing the acrylic polymer (C1) (concentration of the acrylic polymer (C1) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (C1), and a surface protective film (C1) were obtained in the same manner as in Example 2, except that 1 part by weight of 1,6-hexanediol diacrylate (HDDA) was used instead of 0.5 parts by weight of trimethylolpropane triacrylate (TMPTA). The results are shown in Table 1.

[0105]

[0111] The same procedure as in Example 2 was carried out except that trimethylolpropane triacrylate (TMPTA) was not used, to obtain an acrylic polymer emulsion (C2) containing the acrylic polymer (C2) (concentration of the acrylic polymer (C2) (solids concentration) = 50 wt%), a water-dispersible acrylic pressure-sensitive adhesive composition (C2), and a surface protective film (C2). The results are shown in Table 1.

[0106] Comparative Example 3 The same procedure as in Example 2 was carried out except that the amount of trimethylolpropane triacrylate (TMPTA) was changed to 4 parts by weight. However, the reaction mixture in the reaction vessel gelled during polymerization, making it impossible to carry out polymerization. The results are shown in Table 1.

[0107] Comparative Example 4 An acrylic polymer emulsion (C4) containing the acrylic polymer (C4) (concentration of the acrylic polymer (C4) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (C4), and a surface protection film (C4) were obtained in the same manner as in Example 2, except that the oil-soluble crosslinking agent TETRAD-C was not used. The results are shown in Table 1.

[0108] Comparative Example 5 An acrylic polymer emulsion (C5) containing the acrylic polymer (C5) (concentration of the acrylic polymer (C5) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (C5), and a surface protection film (C5) were obtained in the same manner as in Example 2, except that 4 parts by weight of an oxazoline-based crosslinking agent (manufactured by Nippon Shokubai Co., Ltd., trade name "Epocross WS-500"), which is a hydrophilic crosslinking agent, was used instead of 0.5 parts by weight of the oil-soluble crosslinking agent TETRAD-C. The results are shown in Table 1.

[0109] Comparative Example 6 An acrylic polymer emulsion (C6) containing the acrylic polymer (C6) (concentration of the acrylic polymer (C6) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (C6), and a surface protection film (C6) were obtained in the same manner as in Example 2, except that 2 parts by weight of a water-soluble epoxy crosslinking agent (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-313") was used instead of 0.5 parts by weight of the oil-soluble crosslinking agent TETRAD-C. The results are shown in Table 1.

[0110] Comparative Example 7 An acrylic polymer emulsion (C7) containing the acrylic polymer (C7) (concentration of the acrylic polymer (C7) (solids concentration)=50 wt %), a water-dispersible acrylic pressure-sensitive adhesive composition (C7), and a surface protection film (C7) were obtained in the same manner as in Example 2, except that 2 parts by weight of a non-reactive emulsifier, sodium lauryl sulfate, was used instead of 12 parts by weight (3 parts by weight as solids) of the reactive anionic emulsifier (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., trade name "Aqualon KH-1025", solids concentration=25 wt %). The results are shown in Table 1.

[0111]

[0112] The water-dispersible acrylic pressure-sensitive adhesive composition according to an embodiment of the present invention can form a water-dispersible acrylic pressure-sensitive adhesive that has a low initial peel strength, small change in peel strength over time, and is capable of suppressing contamination of an adherend, and can provide a surface protection film having a pressure-sensitive adhesive layer composed of such a water-dispersible acrylic pressure-sensitive adhesive. Such a surface protection film can be suitably used as a removable surface protection film that is attached to the surfaces of optical devices such as displays and imaging devices, electronic devices, and films and glass materials that are components of these devices for the purposes of surface protection, imparting impact resistance, etc.

Claims

1. A water-dispersible acrylic pressure-sensitive adhesive composition comprising an acrylic polymer emulsion (A) and a crosslinking agent (B), wherein the acrylic polymer emulsion (A) is obtained by emulsion polymerization of a monomer composition comprising a (meth)acrylic acid alkyl ester (component a), a polar group-containing monomer (component b) and a trifunctional or higher polyfunctional monomer (component c) in the presence of a reactive emulsifier (component d), and the crosslinking agent (B) is an oil-soluble crosslinking agent.

2. The water-dispersible acrylic pressure-sensitive adhesive composition according to claim 1, wherein the (meth)acrylic acid alkyl ester (component a) is a combination of methyl (meth)acrylate and a (meth)acrylic acid alkyl ester having an alkyl group having 2 to 8 carbon atoms.

3. The water-dispersible acrylic pressure-sensitive adhesive composition according to claim 1, wherein the polar group-containing monomer (component b) is at least one monomer selected from the group consisting of hydroxyl group-containing monomers and carboxyl group-containing monomers.

4. The water-dispersible acrylic pressure-sensitive adhesive composition according to claim 1, wherein the reactive emulsifier (component d) is an anionic reactive emulsifier.

5. The water-dispersible acrylic pressure-sensitive adhesive composition according to claim 1, wherein the crosslinking agent (B) is an oil-soluble epoxy crosslinking agent.

6. A water-dispersible acrylic pressure-sensitive adhesive formed from the water-dispersible acrylic pressure-sensitive adhesive composition according to any one of claims 1 to 5.

7. A surface protection film having an adhesive layer composed of the water-dispersible acrylic adhesive according to claim 6.

Citation Information

Patent Citations

  • Water dispersion type acrylic adhesive composition for re-exfoliation and adhesive sheet

    JP2007177003A

  • Aqueous emulsion adhesive

    JP2011144316A

  • Removable water-dispersible acrylic-based adhesive composition and adhesive sheet

    JP2013241561A

  • Re-peelable sheet

    JP2019048974A

  • Optical member with adhesive layer, image display device and method for manufacturing optical member with adhesive layer

    JP2019077878A