Linear friction welding method and welding joint
The linear friction welding method addresses the challenge of joint reliability by increasing the toe radius and angle through pressure deformation, enhancing fatigue life and mechanical properties in metal structures.
Patent Information
- Application Number
- PCT/JP2024/013489
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-24
AI Technical Summary
Ensuring the strength and long-term reliability of joints in metal structures, particularly in infrastructure and architectural applications, where conventional welding methods fail to adequately address stress concentration and fatigue life due to heat softening and notch formation.
A linear friction welding method that involves applying a first pressure to remove burrs and then increasing the pressure to deform the base material portions of the joint, thereby increasing the toe radius and angle, reducing stress concentration, and promoting martensite generation for improved mechanical properties.
The method enhances the fatigue life and mechanical properties of the joint by alleviating stress concentration and increasing the toe radius and angle, while also improving hardness, thus addressing the limitations of conventional welding techniques.
Smart Images

Figure JP2024013489_24102024_PF_FP_ABST
Abstract
Description
Linear friction joining method and joined joint
[0001] The present disclosure relates to linear friction joining methods and joined joints.
[0002] As the strength of metal materials such as steel and aluminum alloys increases, ensuring the strength of the joints in welded joints has become an important issue. In response to this issue, solid-state joining has recently attracted attention as a technology that can ensure the strength of the joints compared to conventional fusion welding by preventing the temperature reached during joining from reaching the melting point of the joined materials.
[0003] Among the solid-state joining methods, linear friction joining in particular is a joining method that is expected to be put to practical use in various industries. Linear friction joining is a solid-state joining method that uses the frictional heat generated when the workpieces to be joined are rubbed together in a linear motion as a heat source. It has the positive aspects of not requiring tools like friction stir welding and being able to join in a short time.
[0004] For example, in the linear friction joining method described in Patent Document 1, the pressure applied to the joining interface when the workpieces are rubbed together by linear motion is set to be equal to or greater than the yield stress and equal to or less than the tensile strength of one or both of the workpieces at the desired joining temperature. This method makes it possible to accurately control the joining temperature by the pressure applied during joining, thereby enabling the joining temperature to be lowered, and is expected to promote the practical application of linear friction joining.
[0005] Japanese Patent Application Laid-Open No. 2018-122344
[0006] Linear friction welding is applied to various infrastructure and architectural structures, for example. In these structures, the long-term reliability of the joint between the joined components is extremely important. From the perspective of ensuring the long-term reliability of the joint, it is considered necessary to alleviate stress concentrations caused by, for example, softening due to thermal effects on the joint and the formation of sharp notches. For this reason, there is a demand for technology that can control the inherent properties of the joint in-process and improve the fatigue life of welded joints.
[0007] The present disclosure has been made to solve the above-mentioned problems, and aims to provide a linear friction joining method that can control the inherent properties of the joint in-process and improve the fatigue life of the joined joint, and a joined joint made by this method.
[0008] A linear friction welding method according to one aspect of the present disclosure comprises a first step of bringing a first member to be welded and a second member to be welded together to form a weld interface; a second step of repeatedly sliding the first member to be welded and the second member to be welded together in a linear manner while applying a first pressure to the weld interface to remove burrs from the weld interface; and a third step of stopping the sliding between the first member to be welded and the second member to be welded together to form a weld; in the third step, at the timing when the newly formed surfaces of the first member to be welded and the newly formed surfaces of the second member to be welded come into contact due to the removal of burrs, a second pressure greater than the first pressure is applied to the weld interface so that the base material portions of the first member to be welded and the second member to be welded that are continuous with the weld interface undergo plastic deformation in a flared manner toward the weld interface.
[0009] In this linear friction welding method, at the end of the joining of the first and second workpieces, i.e., when the newly formed surfaces of the first and second workpieces come into contact due to the removal of flash, the pressure applied to the weld interface is increased from the first pressure to the second pressure, causing the base material portions of the first and second workpieces connected to the weld interface to plastically deform in a flared manner toward the weld interface. This allows the toe radius and toe angle of the resulting welded joint to be increased in the vicinity of the weld, compared to when the pressure is kept constant during the process. The increased toe radius and toe angle near the weld reduce stress concentration at the toe and improve the fatigue life of the welded joint. Furthermore, increasing the pressure from the first pressure to the second pressure at the aforementioned timing promotes the formation of martensite in the weld, thereby improving the mechanical properties of the weld.
[0010] The sliding between the first and second workpieces may be stopped at the timing when the second pressure is applied to the weld interface. In this case, plastic deformation of the base material occurs before cooling of the weld progresses, so that the toe radius and toe angle in the vicinity of the weld can be sufficiently increased.
[0011] The second pressure may be set to 250 MPa or more. In this case, plastic deformation of the base metal occurs more reliably, and the toe radius and toe angle in the vicinity of the weld can be sufficiently increased. In addition, the hardness of the weld can be improved.
[0012] The contact margin between the first and second workpieces may be set to 3 mm or more and 5 mm or less. By setting the contact margin at or above the lower limit of the above range, plastic deformation of the base material portion occurs more reliably, and the toe radius and toe angle near the weld can be sufficiently increased. By setting the contact margin at or below the upper limit of the above range, excessive reduction in the length in the pressure direction of the obtained welded joint can be suppressed.
[0013] The first pressure may be set so as to be equal to or greater than the yield stress and equal to or less than the tensile strength at a desired joining temperature of at least one of the first member to be joined and the second member to be joined.
[0014] A welded joint according to one aspect of the present disclosure is formed by joining a first workpiece and a second workpiece by the linear friction joining method.
[0015] This welded joint ensures a sufficient toe radius and toe angle near the welded joint. This reduces stress concentration at the toe, improving fatigue life. It also promotes martensite formation in the welded joint, improving the mechanical properties of the welded joint.
[0016] According to the present disclosure, the shape of the welded portion can be controlled in-process, thereby improving the fatigue life of the welded joint.
[0017] 1 is a schematic perspective view showing a linear friction welding method according to an embodiment of the present disclosure; FIG. 2 is a schematic side view showing a welded joint obtained by the linear friction welding method shown in FIG. 1; FIG. 3 is a schematic diagram showing the toe radius and toe angle; FIG. 4 is a diagram showing the conditions for implementing the friction welding method; (a) is a diagram showing sampling for microstructure observation and hardness testing, and (b) is a diagram showing the shape and dimensions of the test piece used in the fatigue test; FIG. 5 is a diagram showing the results of the hardness test; FIG. 6 is a diagram showing the results of observation of the microstructure of the joint, where (a) is the observation result for the Comparative Example, (b) is the observation result for Example 1, and (c) is the observation result for Example 2; FIG. 7 is a diagram showing the results of a fatigue life test; FIG. 8 is a diagram showing the results of toe shape measurement, where (a) is the measurement position, and (b) to (d) are the toe shape measurement results at each measurement position; (a) is a diagram showing the relationship between the second pressure and the toe radius, and (b) is a diagram showing the relationship between the second pressure and the toe angle; and FIG. 9 is a diagram showing the relationship between the second pressure and the stress concentration factor at the toe.
[0018] Hereinafter, preferred embodiments of a linear friction joining method and a joined joint formed by this method according to one aspect of the present disclosure will be described in detail with reference to the drawings.
[0019] Fig. 1 is a schematic perspective view showing a linear friction welding method according to an embodiment of the present disclosure. Fig. 2 is a schematic side view showing a welded joint obtained by the linear friction welding method shown in Fig. 1. The linear friction welding method is a type of solid-state welding method that uses frictional heat generated when welded members are rubbed together by linear motion as a heat source. In the linear friction welding method, pressure is applied to an area softened by frictional heat, and a weld is formed by expelling flash from the system.
[0020] 1 and 2, the linear friction welding method according to this embodiment includes a first step S01 in which a first workpiece 11A and a second workpiece 11B are brought into contact with each other to form a welded interface M, a second step S02 in which the first workpiece 11A and the second workpiece 11B are repeatedly slid linearly together while applying a first pressure P1 to the welded interface M to remove burrs 12 (see FIG. 2) from the welded interface M, and a third step S03 in which the sliding between the first workpiece 11A and the second workpiece 11B is stopped to form a weld 13. Each step will be described in detail below.
[0021] The first step S01 is a step (initial step) of preparing for linear friction welding. In the first step S01, one surface of the first workpiece 11A and one surface of the second workpiece 11B are brought into contact with each other to form a weld interface M. The materials of the first workpiece 11A and the second workpiece 11B are not particularly limited as long as they have a metallic phase that can be welded by linear friction welding. Examples include iron-based metals, titanium, and titanium alloys. The materials of the first workpiece 11A and the second workpiece 11B may be the same or different. The shapes and sizes of the first workpiece 11A and the second workpiece 11B are not particularly limited as long as they can realize the pressure and sliding required for linear friction welding. However, it is preferable that the weld interface M be rectangular. In the example shown in FIG. 1, the first workpiece 11A and the second workpiece 11B are rectangular parallelepiped-shaped, and the weld interface M is rectangular. By forming the welded interface M in a rectangular shape, the timing for stopping the welding (sliding) can be determined using the discharge status of the burrs 12 as an indicator.
[0022] The second step S02 is a step (transition step) of raising the temperature by friction and a step (steady-state step) of generating a new surface by expelling burrs 12. In the second step S02, the first workpiece 11A and the second workpiece 11B are repeatedly slid linearly along the same trajectory, expelling burrs 12 from the workpiece interface M in the surface direction of the workpiece interface M. When the first workpiece 11A and the second workpiece 11B slide against each other, either one of the first workpiece 11A and the second workpiece 11B may be vibrated, or both may be vibrated. In the example shown in FIG. 1, the first workpiece 11A is fixed, and the second workpiece 11B is vibrated in the vertical direction.
[0023] In the second step S02, from the viewpoint of controlling the joining temperature, a first pressure P1 is applied to the joining interface M when the first and second members 11A and 11B slide against each other. The first pressure P1 may be applied from only one of the first and second members 11A and 11B, or from both. In the example of FIG. 1, the first pressure P1 is applied from both the first and second members 11A and 11B.
[0024] The first pressure P1 is set to be equal to or greater than the yield stress and equal to or less than the tensile strength at a desired joining temperature of at least one of the first and second members to be joined 11A and 11B. By setting the first pressure P1 equal to or greater than the yield stress at a desired joining temperature of at least one of the first and second members to be joined 11A and 11B, the removal of burrs 12 from the joining interface M begins, and by setting the first pressure P1 in a range equal to or less than the tensile strength, the removal of burrs 12 can be accelerated.
[0025] Since the tensile strength at a specific temperature is approximately constant depending on the material of the workpieces, just like the yield stress, it is possible to control the joining temperature by setting the first pressure P1. That is, by setting the first pressure P1 high, it is possible to remove non-joined materials with higher yield temperatures and tensile strengths as burrs, and it is possible to reduce the joining temperature.
[0026] From the viewpoint of controlling the joining temperature more precisely, the first pressure P may be set to the yield stress of at least one of the first workpieces 11A and the second workpieces 11B at the desired joining temperature. In linear friction joining, the timing at which the discharge of flash 12 begins is the moment when the first pressure P1 reaches the yield stress. Therefore, the joining temperature can be controlled more precisely compared to when the first pressure P1 is set to a value greater than the yield stress.
[0027] The third step S03 is a step (cooling step) in which the sliding is stopped and a welded portion 13 is formed. In the third step S03, after burrs 12 are expelled from the welded interface M, the sliding of the first welded member 11A and the second welded member 11B is stopped and the region softened by frictional heat is cooled. As a result, a welded portion 13 is formed in the region including the welded interface M, and the welded joint 1 shown in FIG. 2 is obtained.
[0028] The timing of stopping the sliding is not particularly limited as long as it is after the burrs 12 are discharged from the bonded interface M, but it may be the timing when the burrs 12 start to be discharged evenly or approximately evenly from the periphery of the bonded interface M (here, each of a pair of long sides and a pair of short sides of the rectangular bonded interface M). In this case, it is possible to minimize the amount of discharge of the burrs 12, and to reduce the consumption of the bonded materials.
[0029] In the third step S03, when the newly formed surfaces of the first and second workpieces 11A and 11B come into contact with each other due to the removal of the burrs 12, the pressure applied to the workpiece interface M is increased from the first pressure P1 to a second pressure P2. The second pressure P2 is greater than the first pressure P1 and is set to a pressure at which the base material portions of the first and second workpieces 11A and 11B that are continuous with the joint 13 undergo plastic deformation in a manner that widens toward the workpiece interface M.
[0030] A second pressure P2 greater than the first pressure P1 is applied at the end of the second step S02. This causes the base material portions (non-bonded portions) of the first and second workpieces 11A and 11B, which are continuous with the bonded portion 13, to slightly collapse and undergo plastic deformation so as to expand outward in the in-plane direction of the bonded interface M. As a result, in the resulting bonded joint 1, the base material portions adjacent to the burr 12 bulge, forming a plastically deformed portion 14 that is gently concavely curved in side view and connects the base material sides of the first and second workpieces 11A and 11B to the base end portions of the burr 12 protruding from the base material sides, as shown in FIG. 2 . Note that, even in conventional linear friction welding, the applied pressure may be increased at the end of the joining process. However, this increase in pressure is intended to expel the burr and is different from the second pressure P2, which is intended to form the plastically deformed portion 14.
[0031] The second pressure P2 may be set so that the gap between the first and second workpieces 11A, 11B is 3 mm or more and 5 mm or less. The gap is the amount of change in the dimensions of the workpieces before and after joining. Here, the gap is the sum of the lengths of the first and second workpieces 11A, 11B in the pressure direction before joining minus the sum of the lengths of the first and second workpieces 11A, 11B (joint 1) in the pressure direction after joining.
[0032] As an example, when the first pressure P1 is set to 50 MPa, the second pressure P2 is set to 250 MPa or more. The second pressure P2 may be set to 350 Pa or less. By setting the second pressure P2 to 250 MPa or more, sufficient plastic deformation of the base material portion can be generated. On the other hand, by setting the second pressure P2 to 350 MPa or less, an increase in the contact allowance can be avoided, and an excessive decrease in the length of the obtained welded joint 1 in the pressure direction can be suppressed.
[0033] The timing at which the newly formed surfaces of the first and second workpieces 11A and 11B come into contact with each other due to the discharge of the burrs 12 can be determined by the state of discharge of the burrs 12 from the welded interface M. For example, the timing at which the sliding movement is stopped, i.e., the timing at which the burrs 12 begin to be discharged evenly or approximately evenly from the periphery of the welded interface M (here, each of the pair of long sides and the pair of short sides of the rectangular welded interface M), may be considered to be the timing at which the newly formed surfaces of the first and second workpieces 11A and 11B come into contact with each other. In this case, the pressure applied to the welded interface M may be increased from the first pressure P1 to the second pressure P2 simultaneously with the cessation of the sliding movement. The duration for which the second pressure P2 is maintained is not particularly limited and may be set within a range of, for example, several to several tens of seconds.
[0034] Frictional heat generated during welding is conducted to the base metal sides of the first and second welded members 11A and 11B, so a temperature distribution is formed from the welded interface M, where burrs 12 are discharged, to the base metal side. By forming this temperature distribution and forming plastically deformed portions 14 in the base metal parts of the first and second welded members 11A and 11B as the sliding stops, the shape of the toe 15 near the weld can be controlled. The temperature distribution from the welded interface M to the base metal side can be controlled by the welding temperature, and the welding temperature can be accurately determined by the welding pressure.
[0035] As evaluation parameters for the shape of the toe 15, for example, the toe radius ρ and the toe angle α can be used. The toe radius ρ corresponds to the radius of curvature of the plastically deformed portion 14, which has a gently curved shape, as shown in Figure 3. The toe angle α corresponds to the angle formed by the base end of the burr 12 and the side surface of the first welded member 11A or the second welded member 11B. By increasing the toe radius ρ and the toe angle α for the same contact allowance, stress concentration at the toe 15 can be alleviated, and the fatigue life of the welded joint can be improved. [Example]
[0036] The present disclosure will be described in further detail below with reference to examples.
[0037] Two low-carbon steels, SM490A, with a yield stress of 393 MPa and a tensile strength of 530 MPa, were prepared as the welded components used to form the welded joints. The chemical composition of the low-carbon steel SM490A was 0.10 wt% C, 0.29 wt% Si, 1.32 wt% Mn, 0.01 wt% P, 0.002 wt% S, 0.012 wt% Nb, and 0.003 wt% V. Each low-carbon steel SM490A was a rectangular parallelepiped measuring 54 mm x 40 mm x 9 mm. The 40 mm x 9 mm surface was the welded interface, and the black oxide layer at this interface was removed by milling.
[0038] The conditions for performing the linear friction welding method are shown in Figure 4. Here, the welding conditions were a vibration of ±1.5 mm, a frequency of 50 Hz, and a joining allowance of 3.4 mm. The first pressure P1 in the second step was set to 50 MPa, and the second pressure P2 in the third step was set to 50 MPa (maintaining the first pressure P1) in the comparative example, 250 MPa in Example 1, and 300 MPa in Example 2.
[0039] The welded joints according to the comparative example and examples 1 and 2 were cut using an electric discharge machine, and the microstructure of the cross section (see FIG. 5(a)) near the center in the thickness direction of the weld was observed using a scanning electron microscope, and a Vickers hardness test was also performed. In the Vickers hardness test, a load of 100 gf was applied at intervals of 200 μm along the pressure direction. The holding time was 15 seconds.
[0040] Furthermore, fatigue tests were conducted on the test pieces of the bonded joints and base metals according to the comparative example, examples 1 and 2. The shape and dimensions of the test pieces used in the fatigue tests are shown in Figure 5(b). For the fatigue tests, a hydraulic pressure testing machine was used, and the test pieces were subjected to a load frequency of 7 Hz, a stress ratio R of 0.05, and a load cycle of 2 x 10 6 After exceeding this limit, the fracture surface was observed using a shape scanning machine.
[0041] Furthermore, the toe radius ρ and toe angle α of the welded joints according to the comparative example and examples 1 and 2 were measured using a three-dimensional microscope. Then, based on the measured toe radius ρ and toe angle α, the stress concentration factor Kt of the welded joints according to the comparative example and examples 1 and 2 was evaluated.
[0042] Figure 6 shows the results of the hardness test. In Figure 6, the horizontal axis represents the distance from the welded interface, and the vertical axis represents Vickers hardness. As shown in the figure, there was no clear difference in hardness between the vibration-side and pressure-side welded members. The hardness of the base material (BM) was approximately 184 HV, but a hardness peak was observed near the welded interface in all of the comparative example and examples 1 and 2. The peak hardness value was approximately 300 HV in the comparative example, increased to approximately 450 HV in example 1, and increased to approximately 470 HV in example 2. In neither the comparative example nor examples 1 and 2 did a clear softened region occur compared to the base material, suggesting improved mechanical properties in linear friction welding. The increased hardness improves yield stress and contributes to suppressing the initiation and progression of cracks near the weld.
[0043] 7A to 7C show the results of observation of the microstructure of the welded portion. FIG. 7A shows the results of the comparative example, FIG. 7B shows the results of Example 1, and FIG. 7C shows the results of Example 2. Each figure shows the results of observation of the microstructure near the edge and near the center of the welded interface, respectively. In the figures, F represents ferrite, B represents bainite, and M represents martensite. As shown in FIGS. 7A to 7C, it can be seen that bainite and martensite are formed in all of the comparative example and Examples 1 and 2.
[0044] As shown in Figure 7(a), in the comparative example, ferrite is predominantly formed near the center compared to near the edges. This suggests that there is a difference in cooling rate between near the edges and near the center. Because the cooling rate is higher near the edges compared to near the center, it can be seen that bainite and martensite are predominantly formed. The appearance of bainite and martensite is thought to be the cause of the hardness peak shown in Figure 6.
[0045] As shown in Figure 7(b), in Example 1, the proportions of bainite and martensite increased both near the edge and near the center compared to the comparative example. Furthermore, a small amount of ferrite was generated, and due to the transformation of the microstructure into a large amount of bainite and martensite, it was confirmed that there was a slight difference in the proportion of ferrite between near the edge and near the center. As shown in Figure 7(c), in Example 2, it was confirmed that lath martensite accounted for a large portion of the microstructure compared to Example 1. In Example 2, almost no ferrite was observed.
[0046] FIG. 8 shows the results of fatigue life tests. In FIG. 8 , the horizontal axis represents fatigue life, and the vertical axis represents stress range. In addition to the test results for the Comparative Example and Examples 1 and 2, FIG. 8 also plots the fatigue life of the base metal and the FAT90 design curve proposed by the International Institute of Welding (IIW). As shown in FIG. 8 , in the fatigue life test conducted at a maximum stress of 350 MPa, Example 1 exhibited a fatigue life increase of approximately 30% compared to the Comparative Example, and Example 2 exhibited a fatigue life increase of approximately 87% compared to Example 1. Furthermore, in the fatigue life test conducted at a maximum stress of 400 MPa, Example 1 exhibited a fatigue life increase of approximately 47% compared to the Comparative Example, and Example 2 exhibited a fatigue life increase of approximately 50% compared to Example 1. The fatigue life of the base metal was longer than that of Examples 1 and 2. This is thought to be because the base metal test specimens had no burrs, which prevented stress concentration at the toes.
[0047] Figure 9 shows the results of measuring the shape of the toe of the weld. As shown in Figure 9(a), measurements of the shape of the toe of the weld were carried out near the center and near both ends of the weld. Figure 9(b) shows the measurement results near the center, and Figure 9(c) shows the measurement results at one end (Side 1). Figure 9(d) shows the measurement results at the other end (Side 2). In Figures 9(b) to 9(d), the horizontal axis shows the distance from the weld interface, and the vertical axis shows the height (height from the base material surface).
[0048] 9(b) to 9(d), the burrs in the comparative example and examples 1 and 2 are mountain-shaped, but the height of the burrs near both ends is slightly lower than the height of the burrs near the center. The height of the burrs near the center is greater in example 2, which has a higher second pressure P2, than in comparative example 1 and example 1 (see FIG. 9(b)).
[0049] 9(b) to 9(d) also confirm that the shape of the weld toe changes when the second pressure P2 is increased. For example, it can be seen that in Example 2, the height of the weld toe near the center increases from approximately 0 mm to 0.8 mm compared to Comparative Example 1. It is thought that the increase in the second pressure P2 causes widespread plastic deformation, resulting in a larger weld toe height.
[0050] To quantitatively evaluate the shape of the toe, the toe radius ρ and toe angle α (see Figure 3) were measured. Figure 10(a) shows the measurement results for the toe radius ρ, and Figure 10(b) shows the measurement results for the toe angle α. As Figures 10(a) and 10(b) show, both near the center and near both ends, the toe radius ρ and toe angle α increase as the second pressure P2 increases. It can also be seen that when the second pressure P2 is 250 MPa or higher, the slope of the increase in the toe radius ρ and toe angle α with respect to the magnitude of the pressure becomes significantly larger.
[0051] As shown in Figure 10(a), for example, near the center, the toe radius ρ was 0.36 mm when the second pressure P2 was 50 MPa, while the toe radius ρ was 2.07 mm when the second pressure P2 was 300 MPa. Also, as shown in Figure 10(b), for example, near the center, the toe angle α was 92.7° when the second pressure P2 was 50 MPa, while the toe angle α was 103° when the second pressure P2 was 300 MPa.
[0052] Figure 11 is a diagram showing the relationship between the second pressure P2 and the stress concentration factor at the toe. In Figure 11, the horizontal axis shows the second pressure P2, and the vertical axis shows the stress concentration factor Kt. The stress concentration factor Kt was calculated using the toe radius ρ and toe angle α using the following formula (1). In formula (1), ts is the plate thickness, δ is the burr height, P 1 ~P 8 is the calculated coefficient value. 1 is 1.398, P 2 is -0.144, P 3 is 0.715, P 4 is 1.650, P 5 is 0.322, P 6 is -2.233, P 7 is 2.319, P 8 is 0.526.
[0053] As shown in Figure 11, it can be seen that the stress concentration factor Kt at the toe decreases both near the center and near both ends as the second pressure P2 increases and the toe radius ρ and toe angle α increase. For example, near the center, the stress concentration factor Kt at the toe was 3.0 when the second pressure P2 was 50 MPa, but decreased to 1.8 when the second pressure P2 was 300 MPa.
[0054] The formation of a toe by increasing the pressure applied to the weld interface when the newly formed surfaces of the welded parts come into contact can be explained as follows: In linear friction welding, as the temperature rises due to frictional heat, the base material parts that can no longer withstand the applied pressure deform and are expelled from the weld interface as burrs. At this time, if the pressure is increased to a large value immediately after the sliding stops, the base material parts that did not deform with the small pressure undergo plastic deformation, resulting in an increase in the toe radius ρ and toe angle α. By increasing the toe radius and toe angle near the weld, the shape of the toe becomes smoother and stress concentration at the toe is alleviated, thereby improving the fatigue life of the welded joint.
[0055] Furthermore, as suggested by the microstructure observation results shown in Figure 7, the cooling rate at the center of the weld is slower than that at both ends, so the temperature immediately after sliding stops is higher at the center than at both ends. Therefore, plastic deformation of the base material due to increased pressure tends to occur more significantly at the center than at both ends. In fatigue tests, fracture usually occurs at the point with the highest stress concentration factor Kt. Therefore, in welded joints obtained by linear friction welding according to the present disclosure, it is believed that sufficiently increasing the toe radius ρ and toe angle α at both ends of the weld and providing sufficient hardness will greatly contribute to improving the fatigue life.
[0056] 1... welded joint, 11A... first welded member, 11B... second welded member, M... welded interface.
Claims
1. A linear friction joining method comprising: a first step of bringing a first member to be joined and a second member to be joined together to form a joining interface; a second step of repeatedly sliding the first member to be joined and the second member to be joined in a linear manner while applying a first pressure to the joining interface to remove burrs from the joining interface; and a third step of stopping the sliding between the first member to be joined and the second member to be joined to form a joint, wherein in the third step, at the timing when the newly formed surfaces of the first member to be joined and the newly formed surfaces of the second member to be joined come into contact due to the removal of the burrs, a second pressure greater than the first pressure is applied to the joining interface so that base material portions of the first member to be joined and the second member to be joined which are continuous with the joint are plastically deformed so as to flare out toward the joining interface.
2. A linear friction joining method according to claim 1, wherein the sliding between said first workpiece and said second workpiece is stopped at the timing when said second pressure is applied to said weld interface.
3. The linear friction joining method according to claim 1 or 2, wherein the second pressure is set to 250 MPa or more.
4. A linear friction joining method according to any one of claims 1 to 3, wherein the contact between the first workpiece and the second workpiece is set to 3 mm or more and 5 mm or less.
5. A linear friction joining method according to any one of claims 1 to 4, wherein the first pressure is set so as to be equal to or greater than the yield stress and equal to or less than the tensile strength at a desired joining temperature of at least one of the first workpiece and the second workpiece.
6. A welded joint obtained by joining the first workpiece and the second workpiece by the linear friction joining method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Friction welding method of metal member and member for power generation facility
JP2018015776A
Friction welding method and friction welding part
US20100047606A1
Dissimilar material solid phase bonding method, and dissimilar material solid phase bonded structure
WO2021024687A1
Cited By
Tailored blank material, method for manufacturing same, and press-molded article