Aluminum alloy sheet for can lids
The aluminum alloy plate with tailored composition effectively addresses the strength and toughness issues of conventional can lid alloys by incorporating scrap materials, reducing new metal use, and enhancing formability, thus addressing the challenges of recycling and emissions while meeting the demands of positive pressure can lids.
Patent Information
- Application Number
- PCT/JP2024/015126
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional aluminum alloy plates for can lids, with compositions similar to 3104 aluminum alloy, face challenges in achieving both high strength and toughness, leading to reduced pressure resistance and increased risk of leakage, especially in positive pressure cans, while also requiring more new metal and resulting in low recycling rates and high CO2 emissions.
An aluminum alloy plate with specific composition ranges of Si (0.20-0.47%), Fe (0.30-0.70%), Cu (0.11-0.40%), Mn (0.70-1.20%), and Mg (1.1-3.7%), where the solidus temperature is higher than the solid solution temperature of Si, allowing for effective blending of scrap materials and reducing new metal usage, enhancing both strength and toughness without heat treatment, and improving formability.
The solution achieves high strength and toughness in aluminum alloy plates, enabling the use of more 3104 aluminum alloy scrap, reducing new metal consumption, lowering CO2 emissions, and providing high formability suitable for positive pressure can lids with improved pressure resistance and reduced risk of leakage.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Aluminum alloy plate for can lids CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This international application claims the benefit of Japanese Patent Application No. 2023-067373, filed with the Japan Patent Office on April 17, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present disclosure relates to an aluminum alloy sheet for can ends.
[0003] In recent years, with the rise of environmental awareness, CO 2 There is a demand for aluminum alloy sheets with low CO emissions. 2 The compounding of new aluminum ingots in the casting process indirectly contributes significantly to these emissions.
[0004] The production of primary aluminum ingots uses a large amount of electricity during the refining process and produces a large amount of CO 2 Therefore, reducing the amount of virgin aluminum used and increasing the horizontal recycling rate will reduce CO emissions in the manufacture of aluminum alloy sheets. 2 This will lead to reduced emissions.
[0005] Generally, CO generated when aluminum scrap is remelted and cast 2 It is said that waste emissions can be reduced to about one-thirtieth of that when producing virgin aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used worldwide is extremely large, and further improving the horizontal recycling rate for these cans will have a significant impact on reducing the environmental impact.
[0006] Among these, can ends made of 5182 aluminum alloy (AA5182 alloy) have lower upper limits for the compositional specifications of Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to incorporate scrap derived from can stock containing 3104 aluminum alloy.
[0007] For example, if can scrap (UBC: Used Beverage Can) generated in the market is blended as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will likely exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.
[0008] Therefore, compared with the aluminum alloy sheet for can bodies, the aluminum alloy sheet for can ends uses a larger amount of virgin metal to adjust the composition to that of 5182 aluminum alloy, resulting in a low recyclability. Therefore, by changing the can ends to an alloy whose composition is easily blended with 3104 aluminum alloy, the virgin metal usage rate for can ends can be significantly reduced.
[0009] Patent Documents 1 to 5 disclose aluminum alloy sheets for can lids that have compositions relatively close to those of 3104 aluminum alloy, which has excellent recyclability.
[0010] Japanese Patent Application Laid-Open No. 2001-73106 Japanese Patent Application Laid-Open No. 9-070925 Japanese Patent Application Laid-Open No. 11-269594 Japanese Patent Application Laid-Open No. 2000-160273 Japanese Patent Application Laid-Open No. 2016-160511
[0011] The problem of using an alloy for can lids with a composition similar to that of 3104 aluminum alloy is that it reduces the pressure resistance of the can lid and the toughness of the material. The pressure resistance of a can lid is the internal pressure value when the can lid is inverted against the pressure inside the can, and is the resistance value when the internal pressure of the can increases unexpectedly due to a change in the external environment.
[0012] In particular, positive pressure cans for beer and carbonated beverages require high pressure resistance. Generally, the stronger the material and the thicker the plate, the greater the pressure resistance. For this reason, the high-strength 5182 aluminum alloy, which contains a large amount of magnesium, is used for the lids of positive pressure cans.
[0013] In contrast, if conventional 3104 aluminum alloy is used for can lids, the pressure resistance is significantly reduced, and there is a high risk that the lid will invert and leak contents if the internal pressure of the can suddenly increases. Furthermore, if the plate thickness is increased to increase the pressure resistance, this will result in an increase in the weight and cost of the lid.
[0014] Furthermore, the toughness of the material affects the formability and openability of the lid. If the material has low toughness, cracks may occur during molding, especially at the rivet and countersink areas of the lid. Also, if the internal pressure of the can suddenly increases, cracks may occur at the score area, increasing the risk of the can contents leaking. These cracks occur particularly along the rolling direction. Therefore, the material must have toughness against tensile stress and bending stress in directions perpendicular to the rolling direction.
[0015] However, aluminum alloy sheets for can lids, which have chemical compositions relatively close to those of the conventional 3104 aluminum alloy, do not satisfy either or both of the above-mentioned two problems, i.e., material strength (i.e., pressure resistance of the lid) and toughness (i.e., formability and openability).
[0016] One aspect of the present disclosure is to provide an aluminum alloy sheet for can ends that can achieve both high strength and high toughness while incorporating scrap raw materials derived from can stock.
[0017] One aspect of the present disclosure is a steel sheet having a silicon (Si) content of 0.20% by mass or more and 0.47% by mass or less, an iron (Fe) content of 0.30% by mass or more and 0.70% by mass or less, a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less, a manganese (Mn) content of 0.70% by mass or more and 1.20% by mass or less, a magnesium (Mg) content of 1.1% by mass or more and 3.7% by mass or less, and the balance consisting of aluminum (Al) and unavoidable impurities or containing aluminum (Al) and unavoidable impurities, and a solidus temperature of Mg 2 The aluminum alloy sheet for can lids has a temperature higher than the solid solution temperature of Si.
[0018] According to this configuration, the solidus temperature of the aluminum alloy is 2 Therefore, by subjecting an aluminum alloy ingot to soaking treatment within this temperature range, the Mg content, which can cause cracks and unexpected openings during molding, can be reduced. 2 It is expected that the formation of Si crystals can be suppressed.
[0019] As a result, it is possible to achieve both high strength and high toughness in the aluminum alloy sheet while blending scrap raw materials derived from can stock. That is, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, reduce the rate of virgin metal usage, and reduce CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends that has high formability and can be used for positive pressure can ends, which require high pressure resistance.
[0020] Hereinafter, embodiments to which the present disclosure is applied will be described.
[0021] [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for can lids of the present disclosure (hereinafter also simply referred to as "alloy sheet") contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).
[0022] The lower limit of the Si content is 0.20% by mass. The average Si content standard for 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30% by mass, and the average Si content standard for 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10% by mass. Therefore, by setting the Si content to 0.20% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0023] The upper limit of the Si content is 0.47 mass%, preferably 0.39 mass%. If the Si content exceeds 0.47 mass%, Mg 2 The difference between the solid solution temperature of Si and the solidus temperature of the Al matrix becomes small, and the Mg 2 It becomes difficult to dissolve Si in the homogenization process. 2 New Si precipitates, resulting in a decrease in the strength and toughness of the alloy.
[0024] In addition, by setting the Si content to 0.39 mass% or less, Mg 2 Si can be easily dissolved in the homogenization process. 2The precipitation of Si is suppressed, and good strength and toughness can be obtained without carrying out a heat treatment step after hot rolling.
[0025] The lower limit of the Fe content is 0.30% by mass. The average Fe content of the 3104 aluminum alloy is 0.40% by mass, and the average Fe content of the 5182 aluminum alloy is 0.18% by mass. Therefore, by setting the Fe content to 0.30% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0026] The upper limit of the Fe content is 0.70% by mass, preferably 0.59% by mass, and more preferably 0.51% by mass. If the Fe content exceeds 0.70% by mass, abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., giant compounds) increase. As a result, crack propagation paths are generated, and the toughness of the alloy plate decreases. Furthermore, if the Fe content is 0.51% by mass or less, adding a large amount of Mg can compensate for strength and toughness while suppressing the crystallization of the above-mentioned coarse intermetallic compounds.
[0027] The lower limit of the Cu content is 0.11% by mass, preferably 0.17% by mass, and more preferably 0.20% by mass. If the Cu content is less than 0.11% by mass, the amount of Cu that increases strength through solid solution or precipitation is insufficient, resulting in a decrease in the strength of the alloy sheet. The average Cu content standard for 3104 aluminum alloy is 0.15% by mass, and the average Cu content standard for 5182 aluminum alloy is 0.075% by mass. Therefore, by setting the Cu content to 0.11% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0028] The upper limit of the Cu content is 0.40 mass%, preferably 0.25 mass%. If the Cu content exceeds 4.0 mass%, coarse precipitates increase, and the toughness of the alloy plate decreases. Furthermore, by setting the Cu content to 0.25 mass% or less, the strength can be increased without significantly impairing the toughness.
[0029] The lower limit of the Mn content is 0.70% by mass. If the Mn content is less than 0.70% by mass, the Mn that increases strength through solid solution or precipitation will be insufficient, resulting in a decrease in the average strength of the alloy sheet. The average Mn content standard for the 3104 aluminum alloy is 1.1% by mass, while the average Mn content standard for the 5182 aluminum alloy is 0.35% by mass. Therefore, by setting the Mn content to 0.70% by mass or more, it is possible to incorporate more 3104 aluminum alloy scrap than in the conventional 5182 aluminum alloy.
[0030] The upper limit of the Mn content is 1.20% by mass, preferably 0.98% by mass, and more preferably 0.92% by mass. If the Mn content exceeds 1.20% by mass, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds increases. As a result, crack propagation paths are formed, and the toughness of the alloy plate decreases.
[0031] The lower limit of the Mg content is 1.1% by mass. If the Mg content is less than 1.1% by mass, there will be insufficient Mg, which increases strength through solid solution, and the average strength of the alloy sheet will decrease. Note that the strength of the alloy sheet will be significantly increased by precipitating Mg during hot rolling and cold rolling after solution treatment.
[0032] The upper limit of the Mg content is 3.7 mass%, preferably 3.3 mass%, more preferably 3.1 mass%, and even more preferably 2.9 mass%. If the Mg content exceeds 3.7 mass%, the solidus temperature of the Al matrix decreases and the Mg content decreases. 2 The solution temperature of Si increases, so the Mg 2 It becomes difficult to dissolve Si in the homogenization process. In addition, the solidus temperature of the Al matrix decreases, increasing the amount of coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds. This reduces strength and toughness.
[0033] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. The inclusion of Ti refines the ingot structure of the alloy plate. On the other hand, if the Ti content is too high, it causes inclusions and impairs toughness. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may also contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.
[0034] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the respective ranges described above, with the balance consisting of Al and unavoidable impurities or including Al and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%. The balance may contain substances other than Al and unavoidable impurities.
[0035] <Calculation of phase diagram by computer software> In the alloy plate of the present disclosure, in order to increase the toughness of the material, Mg, which becomes the initiation point and propagation path of cracks and affects the decrease in toughness, is used. 2 It is preferable to redissolve the Si particles in the ingot during a homogenization heat treatment step.
[0036] While avoiding local melting of the Al matrix, Mg 2 In order to redissolve Si, the solidus temperature must be higher than Mg 2 The temperature must be higher than the solid solution temperature of Si. 2 It is preferable that the temperature difference minus the solid solution temperature of Si is 30°C or more. 2 The low dissolution temperature of Si prevents the formation of coarse crystals during casting, thereby avoiding the performance degradation caused by the coarse crystals.
[0037] Also, Al 6 In materials where the crystallization temperature of (Mn, Fe) is higher than the solidification start temperature of Al, Al is 6 The formation of coarse crystals of (Mn, Fe) leads to molding defects such as pinholes. 6It is preferable that the temperature is higher than the crystallization temperature of (Mn, Fe), and more preferably the temperature difference obtained by subtracting the crystallization temperature of the primary crystal from the solidification start temperature of Al is 1° C. or more.
[0038] Al 6 When (Mn, Fe) crystallizes, Al is formed when the surrounding area is liquid Al. 6 (Mn, Fe) tend to grow into giant crystals. Such giant crystals can be the starting point for crack propagation in the alloy, leading to a decrease in toughness. 6 When the crystallization temperature is higher than that of (Mn, Fe), Al 6 When (Mn, Fe) crystallizes, the surrounding Al has already begun to solidify, so the generation of large crystallized particles is suppressed, and an aluminum alloy sheet for can lids having higher toughness can be obtained.
[0039] The Mg mentioned here 2 The solid solution temperature of Si is the same as that of Mg in the equilibrium diagram. 2 The temperature at which Si can exist is the highest temperature at which it can be in a liquid phase, and the temperature at which it can be in a liquid phase is the lowest temperature at which it can be in a liquid phase. The solidification temperature of Al is the highest temperature at which solid Al can exist in the equilibrium diagram, and the crystallization temperature of the primary crystal is the highest temperature at which Al can be in a liquid phase. 6 This is the highest temperature at which (Mn, Fe) can exist.
[0040] Mg 2 The solution temperature of Si, the solidus temperature of the aluminum alloy, the solidification start temperature of Al, and the crystallization temperature of the primary crystal can be obtained from an equilibrium phase diagram of the aluminum alloy calculated using thermodynamic calculation software.
[0041] Mg 2 The solution temperature of Si, the solidus temperature of the aluminum alloy, the solidification start temperature of Al, and the crystallization temperature of the primary crystal are uniquely determined by the composition of the aluminum alloy. As a method for determining these boundary temperatures from the alloy composition, there is a method for calculating the thermodynamic quantities required for each calculation using the CALPHAD method.
[0042] Such thermodynamic calculations for multi-component alloys can be performed using commercially available system software (e.g., "JMatPro" developed by Sente Software) that combines the thermodynamic database, interface, and phase diagram creation functions required for the calculations.
[0043] <Method for producing aluminum alloy sheet> The aluminum alloy sheet of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy sheet of the present disclosure is subjected to a semi-continuous casting method (i.e., DC casting) according to a conventional method to produce an ingot.
[0044] Next, the four sides of the ingot, excluding the front and rear ends, are chamfered. The ingot is then placed in a soaking furnace for homogenization. The temperature in the homogenization is preferably, for example, 470°C or higher and 620°C or lower. The time for the homogenization is preferably, for example, 1 hour or higher and 20 hours or lower.
[0045] When the homogenization temperature is 400°C or higher, segregation of the ingot structure is easily eliminated. Furthermore, when the homogenization temperature is 450°C or higher, Mg 2 The homogenization temperature is 490°C or higher, preferably 550°C or higher, and more preferably Mg 2 When the temperature is higher than the solid solution temperature of Si, Mg 2 The re-dissolution of Si particles is promoted, and the strength and toughness of the alloy sheet can be further improved. On the other hand, when the temperature in the homogenization treatment is 620°C or lower, more preferably the solidus temperature or lower, local melting of the aluminum alloy is unlikely to occur.
[0046] When the homogenization treatment time is 1 hour or more, the temperature of the entire ingot becomes uniform, segregation of the ingot structure is easily eliminated, and Mg 2 The longer the homogenization time, the easier it is to redissolve the Si particles. 2 The Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.
[0047] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot-rolled coil.
[0048] When the total reduction rate of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the isotropic Cube orientation can be increased. When the coiling temperature of the finish rolling is high, a recrystallized structure is formed after coiling, and the concentration of the Cube orientation can be increased. By increasing the concentration of the Cube orientation of the aluminum alloy sheet, the toughness is improved.
[0049] Following the hot rolling, the plate material is cold rolled. In the cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. The cold rolling may be either single rolling or tandem rolling. In the cold rolling by single rolling, it is preferable to perform the rolling in two or more passes.
[0050] By setting the finishing temperature of cold rolling in intermediate passes other than the final pass to 120°C or higher, Si, Cu, Mg, etc. are finely precipitated and age hardened, thereby increasing the strength of the alloy sheet. Furthermore, by setting the finishing temperature to 130°C or higher, the strength of the alloy sheet can be further increased.
[0051] The cold rolling reduction (i.e., the target total reduction) is preferably 80% or more. When the cold rolling reduction is 80% or more, the strength of the alloy sheet can be increased. On the other hand, the cold rolling reduction is preferably 92% or less. By setting the cold rolling reduction to 92% or less, the anisotropy of the crystal grain structure is reduced, and the toughness against tensile stress and bending stress in a direction perpendicular to the rolling direction is improved.
[0052] The cold rolling reduction ratio R (%) is the thickness t of the hot rolled sheet after hot finish rolling. 0 (mm), product thickness after cold rolling t 1 (mm) is calculated using the following formula (1).
[0053] R = (t 0 -t 1 ) / t 0× 100 (1) The product plate thickness can be appropriately selected so as to obtain a desired pressure resistance. Although the pressure resistance improves as the plate thickness increases, the aluminum alloy plate of the present disclosure can suppress an increase in plate thickness in order to maintain a high pressure resistance.
[0054] Furthermore, in the above-described method for producing an aluminum alloy sheet, annealing may be performed, for example, before or after cold rolling or between passes, as long as the effects of the aluminum alloy sheet of the present disclosure are exhibited.
[0055] Coils that have been cold-rolled to the product thickness are pre-coated on a painting line, etc. The surface of the cold-rolled coil is degreased, cleaned, and chemically treated, and then painted, followed by a paint baking process.
[0056] Chemical solutions such as chromate-based and zirconium-based solutions are used in chemical conversion treatments. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the recovery of the material is suppressed, and the higher the strength of the alloy plate can be maintained.
[0057] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained.
[0058] (1a) The solidus temperature of an aluminum alloy is Mg 2 Therefore, by subjecting an aluminum alloy ingot to soaking treatment within this temperature range, the Mg content, which can cause cracks and unexpected openings during molding, can be reduced. 2 It is expected that the formation of Si crystals can be suppressed.
[0059] As a result, it is possible to achieve both high strength and high toughness in the aluminum alloy sheet while blending scrap raw materials derived from can stock. That is, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, reduce the rate of virgin metal usage, and reduce CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends that has high formability and can be used for positive pressure can ends, which require high pressure resistance.
[0060] [2. Other Embodiments] Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take on various forms.
[0061] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments such as a member made of this aluminum alloy sheet and a method for manufacturing this aluminum alloy sheet.
[0062] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. Also, part of the configuration of the above embodiments may be omitted. Furthermore, at least part of the configuration of the above embodiments may be added to, replaced with, or the like, the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified by the wording of the claims are embodiments of the present disclosure.
[0063] 3. Examples The following describes the details of tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.
[0064] <Calculation of Equilibrium Diagram> As examples and comparative examples, the equilibrium diagrams of the aluminum alloys S1-S14 shown in Table 1 were calculated using "JMatPro" by the calculation method described in the embodiment. The results are shown in Table 1.
[0065]
[0066] <Evaluation of Aluminum Alloy Sheets> (Various Temperatures) In S2-S9 and S11-S14, the solidus temperature is Mg 2 The temperature is higher than the solid solution temperature of Si. Therefore, these alloys 2 Soaking can be performed at a temperature at which Si can be dissolved.
[0067] In S1, the amount of Si is relatively large, so Mg 2 The Si solid solution temperature is higher than the solidus temperature. As a result, Si becomes more soluble in Mg as the temperature rises. 2 Since Al melts locally before Si dissolves, Mg 2Soaking to dissolve Si is difficult.
[0068] On the other hand, in S2, the amount of Si is less than that in S1, so Mg 2 Even if Si is dissolved in the solid solution, there is a temperature range in which the liquid phase does not appear. In addition, since the amount of Si in S3 is even less than that in S2, the solidus temperature and the Mg 2 The temperature difference from the Si solid solution temperature is large, at least 30° C. As a result, in S3, there is a temperature range in which soaking is possible even taking into account manufacturing variations.
[0069] In S4, the amount of Fe is relatively large, so Al 6 The crystallization temperature of (Mn, Fe) is higher than the solidification start temperature of Al. Therefore, in S4, Al is dissolved in the Al liquid phase as it is cooled. 6 (Mn, Fe) may crystallize and become large crystals.
[0070] On the other hand, in S5, the Fe content is less than that in F4, so the Al solidification start temperature is higher than that of Al. 6 The crystallization temperature of S5 is higher than that of (Mn, Fe). Therefore, the generation of large crystals is suppressed in S5. In addition, in S6, the amount of Fe is even less than that in F5, so the Al solidification start temperature and the Al 6 The difference in temperature between the crystallization temperature of (Mn, Fe) becomes large. Therefore, in S6, the decrease in strength and toughness due to the formation of large crystals is less likely to occur.
[0071] In S7, the amount of Mn is relatively large, so Al 6 The crystallization temperature of (Mn, Fe) is higher than the solidification start temperature of Al. Therefore, in S7, Al is added to the Al liquid phase as it is cooled. 6 (Mn, Fe) may crystallize and form large crystals.
[0072] On the other hand, in S8, the Mn content is less than that in S7, so the Al solidification start temperature is higher than that of Al. 6 The crystallization temperature of S8 is higher than that of S8 (Mn, Fe). Therefore, the generation of large crystals is suppressed. In S9, the Mn content is even lower than that of S8, so the Al solidification start temperature and Al 6 The difference in temperature between the crystallization temperature of (Mn, Fe) becomes large. Therefore, in S9, the decrease in strength and toughness due to large crystallized particles is less likely to occur.
[0073] In S10, the amount of Mg is relatively large, so Mg 2 The Si solid solution temperature is higher than the solidus temperature. Therefore, in S10, as the temperature rises, Mg 2 Al melts locally before Si dissolves, and Mg 2 It is difficult to perform the soaking homogenization treatment to dissolve Si. 6 The crystallization temperature of (Mn, Fe) is higher than the solidification start temperature of Al. Therefore, in S10, Al is added to the Al liquid phase as it is cooled. 6 (Mn, Fe) crystallizes to form large crystals, which causes a decrease in strength and toughness.
[0074] On the other hand, in S11, the amount of Mg is less than that in S10, so Mg 2 Even if Si is dissolved in the solution, there is a temperature range in which the liquid phase does not appear. In addition, in S12, the amount of Mg is even less than in S11, so the solidification temperature of Al is higher than that of Al. 6 The crystallization temperature of (Mn, Fe) is higher than that of S12. Therefore, in S12, the formation of large crystals is suppressed.
[0075] In S13, the amount of Mg is even less than that in S12, so the solidus temperature and Mg 2 The temperature difference from the Si solid solution temperature is large, at least 30° C. As a result, in S13, there is a temperature range in which soaking is possible even taking into account manufacturing variations.
[0076] In addition, in S14, the Mg content is even less than in S13, so the Al solidification start temperature and Al 6 The difference in temperature between the crystallization temperature of (Mn, Fe) becomes larger. Therefore, in S14, the decrease in strength and toughness due to the formation of large crystals is less likely to occur.
[0077] (Scrap Blending Ratio) Table 2 shows the blending ratio of 3104 aluminum alloy to 5182 aluminum alloy and the corresponding average values of the component specifications. The first row of Table 2 shows the average values of the component specifications of 3104 aluminum alloy, and the second row shows the average values of the component specifications of 5182 aluminum alloy.
[0078] For example, when the compounding ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.
[0079] Therefore, when the proportions of each component in the aluminum alloy sheet are equal to or greater than the above-mentioned values of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of 3104 aluminum alloy sheet is 50% by mass or more. As the blending ratio of 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy sheets S1-S14 can be blended with 50% by mass or more of 3104 aluminum alloy scrap.
[0080]
Claims
1. A steel having a silicon (Si) content of 0.20% by mass or more and 0.47% by mass or less, an iron (Fe) content of 0.30% by mass or more and 0.70% by mass or less, a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less, a manganese (Mn) content of 0.70% by mass or more and 1.20% by mass or less, a magnesium (Mg) content of 1.1% by mass or more and 3.7% by mass or less, and the remainder consisting of aluminum (Al) and unavoidable impurities or containing aluminum (Al) and unavoidable impurities, and a solidus temperature of Mg 2 Aluminum alloy sheet for can lids, with a temperature higher than the solid solution temperature of Si.
2. An aluminum alloy sheet for can ends according to claim 1, comprising: a silicon (Si) content of 0.20% by mass or more and 0.47% by mass or less; an iron (Fe) content of 0.30% by mass or more and 0.59% by mass or less; a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less; a manganese (Mn) content of 0.70% by mass or more and 0.98% by mass or less; a magnesium (Mg) content of 1.1% by mass or more and 3.3% by mass or less; and a solidification start temperature of Al is higher than a crystallization temperature of the primary crystal.
3. The aluminum alloy sheet for can lids according to claim 2, wherein the silicon (Si) content is 0.20% by mass or more and 0.39% by mass or less, the iron (Fe) content is 0.30% by mass or more and 0.59% by mass or less, the copper (Cu) content is 0.11% by mass or more and 0.40% by mass or less, the manganese (Mn) content is 0.70% by mass or more and 0.98% by mass or less, the magnesium (Mg) content is 1.1% by mass or more and 3.1% by mass or less, and the solidus temperature is 0.01 to 0.03%, and the Mg content ... 2 An aluminum alloy sheet for can ends, having a temperature difference of 30°C or more minus the solid solution temperature of Si.
4. An aluminum alloy sheet for can lids according to claim 3, comprising: a silicon (Si) content of 0.20% by mass or more and 0.39% by mass or less; an iron (Fe) content of 0.30% by mass or more and 0.51% by mass or less; a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less; a manganese (Mn) content of 0.70% by mass or more and 0.92% by mass or less; a magnesium (Mg) content of 1.1% by mass or more and 2.9% by mass or less; and a temperature difference obtained by subtracting the crystallization temperature of the primary crystal from the solidification start temperature of Al is 1°C or more.
Citation Information
Patent Citations
Aluminum alloy sheet for can end
JP2000160273A
Manufacture of aluminum alloy hard sheet for can-top
JP2001073106A
Aluminum alloy sheet for negative pressure can-top
JP2016160511A
3104 Aluminum alloy can lid material and production method thereof
CN105568085A
Aluminum alloy plate as well as production method and applications thereof
CN107058823A
Cited By
Aluminum alloy plate for can lids
JP7914315B1
Aluminum alloy plate for can lids
JP7914316B1
Aluminum alloy sheet for can lids
WO2026095012A1