Plastic depolymerization method
The mechanochemical method using ball milling for plastic depolymerization addresses the inefficiencies of existing chemical recycling by applying mechanical energy to convert plastics into valuable monomers without solvents or catalysts, achieving efficient and environmentally friendly recycling of plastics like PET and PLA.
Patent Information
- Application Number
- PCT/KR2023/018625
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-09
- Filing Date
- 2023-11-20
- Publication Date
- 2024-10-24
AI Technical Summary
Current plastic recycling methods, particularly chemical recycling, require solvents and catalysts, leading to complex processes and high energy consumption, and struggle with low solubility of plastics like PET, resulting in inefficient depolymerization and environmental concerns such as microplastics from slow decomposition of bio-based plastics like PLA.
A mechanochemical method that applies mechanical energy through ball milling to depolymerize plastics without the need for solvents or catalysts, simplifying the process and reducing energy requirements, while promoting efficient conversion of ester and carbonate plastics into monomers or high-value chemicals.
This method enables effective depolymerization of plastics like PET and PLA, producing high-demand monomers like bisphenol A and dimethyl carbonate, with simplified product separation and purification, reducing environmental impact and operational costs, and achieving high conversion rates without the need for harsh conditions.
Smart Images

Figure KR2023018625_24102024_PF_FP_ABST
Abstract
Description
Depolymerization method of plastic
[0001] The present invention relates to a method for decomposing a feedstock containing plastic, and more particularly, to a method for depolymerizing plastic using mechanical energy.
[0002] Plastics are widely used in a wide range of fields due to their low cost, ease of production, and durability, and their use has increased rapidly over the past several decades. Consequently, the resulting plastic waste has become a serious environmental problem, prompting various solutions to address it.
[0003] Plastic waste recycling encompasses mechanical recycling, chemical recycling, and energy-recovery combustion. Chemical recycling involves chemically depolymerizing plastic waste, converting it into monomers and repolymerizing it, or converting it into high-value-added chemicals. This process preserves the benefits of plastic while preserving the environment. Accordingly, significant investment and research has been devoted to the chemical decomposition of plastics.
[0004] Representative examples of plastics include carbonate and ester polymers such as poly(bisphenol-A carbonate) (BPA-PC), poly(ethylene terephthalate) (PET), and polylactic acid (PLA).
[0005] BPA-PC waste can pose a risk of releasing the environmental hormone bisphenol A. While efficient mechanical recycling methods for PET have been developed, they are not sufficient to handle the volume of PET being discharged. Despite being a representative bio-based, eco-friendly plastic, PLA is slow to decompose in nature, consistently causing problems like microplastics.
[0006] For these materials to become sustainable plastics, practical and fully circular chemical recycling processes are needed. Technologies that efficiently convert ester and carbonate functional groups into monomers or high-value-added chemical products through chemical reactions will drive the future plastics industry.
[0007] Ester substitution and amidation reactions, based on alcohols and amines, are widely used for the degradation of ester and carbonate plastics. Conventionally, these reactions required homogeneous conditions using solvents and activating reagents (e.g., catalysts). This complicates the process configuration and, consequently, incurs significant additional costs. In the case of PET, its very low solubility in common solvents often necessitates high-temperature, energy-intensive processes.
[0008]
[0009] (Patent Document 0001) Republic of Korea Patent Publication No. 10-2023-0006233
[0010] The present invention addresses the problems of the prior art by devising a mechanical energy input chemical process, a mechanochemical method, that does not require solvents or activating catalysts for dissolution. This method enables effective depolymerization of plastics in an environment that does not use reaction-promoting compounds or large quantities of solvents.
[0011] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.
[0012] In order to achieve the above technical task, one embodiment of the present invention provides a plastic depolymerization method.
[0013] A plastic depolymerization method according to one embodiment of the present invention is characterized by including the steps of: mixing a feedstock containing plastic with alcohol to obtain a reaction mixture; and applying mechanical energy to the reaction mixture to cause a depolymerization reaction to obtain a product.
[0014] In an embodiment of the present invention, the feedstock including the plastic may be a plastic depolymerization method characterized in that it includes polyester or polycarbonate.
[0015] In an embodiment of the present invention, in the step of applying mechanical energy to the reaction mixture to depolymerize and obtain a product, it may be a plastic depolymerization method characterized in that the mechanical energy is applied through a ball milling method.
[0016] In an embodiment of the present invention, the depolymerization reaction may be a plastic depolymerization method characterized in that it is performed without the addition of a separate catalyst or activator.
[0017] In an embodiment of the present invention, it may be a product depolymerized according to the above-described plastic depolymerization method.
[0018] According to an embodiment of the present invention, since there is no problem of solubility compared to conventional depolymerization through depolymerization using a mechanochemical method such as a ball milling method, it is easy and environmentally friendly because it does not require a solvent or catalyst as well as a high temperature condition required in conventional research, and at the time of completion of the reaction, the simplest combination of products is produced, so that separation and purification can be easily performed.
[0019] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.
[0020] Figure 1 is a flow chart schematically showing a method for depolymerizing plastic according to one embodiment of the present invention.
[0021] Figure 2 is an image showing a product obtained by depolymerizing a plastic using a mechanochemical method according to one embodiment of the present invention.
[0022] Figure 3 is a chemical reaction diagram showing the depolymerization reaction of BPA-PC according to one embodiment of the present invention.
[0023] Figure 4 is a graph showing the conversion rate and product amount of the BPA-PC ball milling depolymerization reaction performed through the above manufacturing example and comparative example of the present invention.
[0024] Figure 5 shows the H of the reactants and products according to the degree of depolymerization carried out through one manufacturing example of the present invention. 1 -This is a graph showing NMR data.
[0025] Figure 6 is an image showing the conversion rate of a ball milling depolymerization reaction with different shapes of BPA-PC according to one embodiment of the present invention.
[0026] Figure 7 is an image showing the conversion rate of the ball milling depolymerization reaction of PLA and PET according to one embodiment of the present invention.
[0027] Hereinafter, the present invention will be described with reference to the attached drawings. However, the present invention can be implemented in various different forms and is therefore not limited to the embodiments described herein. In the drawings, irrelevant parts have been omitted for clarity of description, and similar parts have been designated with similar reference numerals throughout the specification.
[0028] Throughout the specification, when a part is said to be "connected (connected, contacted, or coupled)" to another part, this includes not only cases where it is "directly connected," but also cases where it is "indirectly connected" with another part in between. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that it may include other components, unless otherwise specifically stated.
[0029] The terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0030] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.
[0031]
[0032] A plastic depolymerization method according to one embodiment of the present invention is described.
[0033] Figure 1 is a flow chart schematically showing a method for depolymerizing plastic according to one embodiment of the present invention.
[0034] A plastic depolymerization method according to one embodiment of the present invention is characterized by including a step (S100) of mixing a feedstock containing plastic with alcohol to obtain a reaction mixture, and a step (S200) of applying mechanical energy to the reaction mixture to cause a depolymerization reaction to obtain a product.
[0035] Initially, a feedstock containing plastic can be mixed with alcohol to obtain a reaction mixture (S100).
[0036] Figure 2 is an image showing a product obtained by depolymerizing a plastic using a mechanochemical method according to one embodiment of the present invention.
[0037] The plastic may include polyester or polycarbonate, more specifically, polyethylene terephthalate (PET), polylactic acid (PLA), or polybisphenol-A carbonate (BPA-PC). However, the present invention is not limited thereto, and other plastic materials capable of undergoing ester exchange may also be included.
[0038] At this time, in the step of mixing a feedstock containing plastic with alcohol to obtain a reaction mixture, the form of the feedstock containing plastic is not limited, but it may be efficient to provide plastic in powder form to promote depolymerization.
[0039] At this time, the alcohol may be methanol.
[0040] A product can be obtained by applying mechanical energy to the above reaction mixture to cause a depolymerization reaction (S200).
[0041] The above mechanical energy includes the use of physical processes such as collision, shearing and grinding for chemical reactions.
[0042] In this case, mechanical forces on the polymer chains may result in chain fragmentation, which may aid in the PC depolymerization process.
[0043] At this time, ball milling may be proposed as a means of applying the mechanical energy. However, the present invention is not limited thereto, and any means capable of applying mechanical energy sufficient to induce a chemical depolymerization reaction may be included.
[0044] The ball milling method at this time is generally used by placing the feedstock in a container containing metal beads and rotating the container or a similar method.
[0045] The above depolymerization reaction can be performed without the addition of a separate catalyst or activator.
[0046] At this time, the catalyst or activator may mean a hydrolytic enzyme such as Humicola insolens (HiC) and Thermobita fusca (TfH), which have been suggested for the depolymerization of PET in the past, Ideonella sakaiensis (Is) bacteria, or PETase enzyme using these.
[0047] At this time, the above depolymerization reaction does not require the high temperature, strong acid, or strong alkali conditions required in conventional plastic depolymerization reactions. However, these factors can be controlled to ensure an effective depolymerization reaction.
[0048] In order to achieve the above technical task, another embodiment of the present invention provides a product depolymerized according to the above plastic depolymerization method.
[0049] At this time, the depolymerized product may include bisphenol A (BPA), dimethyl carbonate (DMC), dimethyl terephthalate (DMT), and methyl lactate, depending on the type of plastic supplied.
[0050]
[0051] Previous studies have required homogeneous conditions and activating agents (e.g., catalysts) for the chemical recycling of plastics using alcohol. However, this process is complex and requires significant costs. Furthermore, the low solubility of PET and other materials in common solvents can pose challenges in achieving homogeneous conditions.
[0052] The method for depolymerizing plastic according to one embodiment of the present invention proposes a practical and sustainable plastic recycling method that is different from existing research in that it does not require a large amount of solvent, does not require a catalyst, and does not require high temperature and strong acid or strong base conditions by promoting efficient mixing and energy transfer using a mechanochemical method, such as a ball milling method.
[0053] Furthermore, existing plastic depolymerization technologies rarely occur in non-catalytic environments, and even when depolymerization occurs, the resulting products are often diol products not desired by the market. However, the present invention utilizes a mechanochemical depolymerization process using minimal chemical inputs, resulting in a very simple plastic monomer mixture. This product is in high demand and is environmentally friendly, as it can be used in the remanufacturing of BPA-PC and PET, as well as in other applications.
[0054] Hereinafter, the present invention will be described in more detail through manufacturing examples, comparative examples, and experimental examples. However, the present invention is not limited to the following manufacturing examples and experimental examples.
[0055] [Experimental Example 1]
[0056] Figure 3 is a chemical reaction diagram showing the depolymerization reaction of BPA-PC according to one embodiment of the present invention.
[0057] In order to investigate the effect of mechanical energy applied through ball milling on plastic depolymerization according to one embodiment of the present invention, BPA-PC was depolymerized under various conditions.
[0058] Figure 4 is a graph showing the conversion rate and product amount of the BPA-PC ball milling depolymerization reaction carried out under various conditions.
[0059] Referring to FIGS. 3 and 4, the effect of mechanical energy applied through ball milling in the above-described plastic depolymerization method is explained.
[0060]
[0061] Comparative Example 1: Depolymerization of non-ball milled BPA-PC powder
[0062] Commercial BPA-PC powder with a number-average molecular weight (Mn) of 16.4 kg / mol and a polydispersity of 2.15 was reacted with 70 mmol of methanol (MeOH), but it was insoluble even at 100°C and did not promote depolymerization. The number-average molecular weight decreased slightly to 14.3 kg / mol. After methanol treatment, a unimodal polydispersity similar to that of the initial BPA-PC was maintained (2.04), and no oligomer or monomer was detected.
[0063]
[0064] Manufacturing Example 1: Depolymerization of BPA-PC powder ball-milled in a 12ML container
[0065] Additional mechanistic conditions were applied to the same mixture. A heterogeneous mixture of BPA-PC (powder, 1 mmol) and methanol (MeOH, 70 mmol) was planetarily ball-milled at 600 rpm with 50 SS balls (5 mm in diameter) in a 12-mL stainless steel (SS) vessel. Quantitative depolymerization occurred after 6 h (97%).
[0066]
[0067] Manufacturing Example 2: Depolymerization of BPA-PC powder ball-milled in a 25 ML container
[0068] As a result of depolymerization in a 25 mL container of a composition applying mechanochemical conditions as described above, the BPA-PC powder was completely converted into BPA and DMC.
[0069] Referring to Comparative Example 1 and Manufacturing Examples 1 to 2, Comparative Example 1 did not promote depolymerization. This ruled out non-catalytic solution-phase methanol decomposition as a depolymerization mechanism.
[0070] On the other hand, quantitative depolymerization occurred when the planetary ball milling method was applied. In the reaction conducted in a 12 mL vessel, 97% of BPA-PC was depolymerized, and 78% was converted to BPA. Meanwhile, in the reaction conducted in a 25 mL vessel, 99% of BPA-PC was completely depolymerized to BPA (99%). This may be because the increased volume promoted additional ball movement and mixing.
[0071]
[0072] Manufacturing Example 3
[0073] When the amount of methanol was reduced to 30 mmol, BPA and DMC were quantitatively produced, maintaining the depolymerization efficiency.
[0074]
[0075] Manufacturing Example 4
[0076] On the other hand, further reducing the amount of methanol to less than 30 mmol (10 mmol) resulted in a decrease in reactivity.
[0077]
[0078] ClassificationMeOH(mmol)Conversion(%)BPA(%)BPAMC(%)BPADC(%)CommentsComparative Example 1700Non-catalytic solution-phase ethanol decompositionManufacturing Example 170977818112mL containerManufacturing Example 2709999Manufacturing Example 3309999Manufacturing Example 41055141031
[0079] [Experimental Example 2]
[0080] Figure 5 is a graph showing H-NMR data of reactants and products according to the degree of depolymerization carried out through the above-described manufacturing example 2 of the present invention.
[0081] Referring to Figure 5, after one hour, the BPA-PC and methanol mixture (1 hr-Heterogeneous) remained heterogeneous. The NMR spectrum includes the polymer BPA-PC (yellow region), monomer BPAMC (blue region), and BPA (green region).
[0082] Meanwhile, after three hours, a homogeneous mixture (3hr-Homogeneous) without polymer BPA-PC was formed. The reaction continued homogeneously, and after five hours, only BPA was detected (5hr).
[0083] In this case, DMC evaporated during the post-processing process because its boiling point is 90°C. The presence of DMC was confirmed through separate measurements using NMR spectroscopy.
[0084]
[0085] [Experimental Example 3]
[0086] Figure 6 is an image showing the conversion rate of a ball milling depolymerization reaction with different shapes of BPA-PC according to one embodiment of the present invention.
[0087] Referring to Fig. 6, BPA-PC (5 g, 20 mmol) was treated with DMC (3.4 mL, 40 mmol) in a 125 mL SS bottle containing 500 balls (diameter 5 mm), and then the crushed BPA-PC was mixed with methanol (24 mL, 600 mmol). As a result of ball milling at 600 rpm for 6 hours, it was depolymerized into BPA and DMC.
[0088] Meanwhile, compact discs (CDs, Mn = 16.4 kg / mol, polydispersity = 2.15) and safety glasses (Mn = 21.1 kg / mol, polydispersity = 2.55) were used to demonstrate the chemical recycling of waste polycarbonate. These contain additives such as UV stabilizers and release agents, which can interfere with the depolymerization process.
[0089] Following the same mechanochemical process, polycarbonate was completely decomposed into BPA. Following a subsequent purification process, 3.6 g of BPA was obtained from CD and 4.1 g from safety glasses. The complete conversion to BPA and DMC demonstrates the potential of mechanochemical processes.
[0090]
[0091] Planetary Milling By 500 SS Balls (5mm), 125mL SS, DMC (3.4mL, 40mmol) followed by MeOH (24mL, 600mmol) Ball Milling (600rpm, 6hour) Classification BPAIsolation yield (%) Pellet (5.0g, 20mmol) 3.9g85%Lab Safety Goggles (Mn = 21.1kg / mol, dispersion 2.55)4.1g90%Compact Disc (Mn = 16.4kg / mol, dispersion 2.15)3.6g80%
[0092] [Experimental Example 4]
[0093] Figure 7 is an image showing the conversion rate of the ball milling depolymerization reaction of PLA and PET according to one embodiment of the present invention.
[0094] PET and PLA obtained from beverage containers were chopped into small pieces and placed in a ball milling container containing methanol.
[0095] PLA chunks (2.2 g, 30 mmol) and methanol (20 equiv) were ball milled (SS125 mL, 600 rpm, 6 h, SS Balls 300ea 5mm) to obtain quantitative methanol decomposition and depolymerization (3.1 g methyl lactate, 98% purification yield).
[0096] PET (2.8 g, 15 mmol) was briefly milled (6 min) below the brittle-to-ductile transition temperature (-40°C) to obtain a powder. The resulting PET powder was depolymerized with methanol (70 equiv) using ball milling (SS125 mL, 650 rpm, 6 h, SS Balls 300ea 5mm), producing a mixture of methanol, dimethyl tert-butyl ether (DMT), and ethylene glycol. After purification, 2.4 g of DMT was obtained.
[0097]
[0098] ClassificationProductIsolation yield (%)PLA (2.2g, 30mmol)MeOH(20equiv), Planetary Milling SS125mL 600rpm, 6h, SS Balls 250ea (5mm)3.1g Methyl Lactate98%PET (2.8g, 15mmol)At -40℃ 6 minutes Milling,MeOH(70equiv), Planetary Milling SS125mL 650rpm, 6h, SS Balls 300ea (5mm) 2.4g Dimethyl Terephthalate82%
[0099]
[0100] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0101] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
Claims
1. A step of obtaining a reaction mixture by mixing a feedstock containing plastic with alcohol; and A plastic depolymerization method characterized by including a step of applying mechanical energy to the above reaction mixture to cause a depolymerization reaction and obtain a product.
2. In paragraph 1, A plastic depolymerization method, characterized in that the feedstock containing the above plastic contains polyester or polycarbonate.
3. In paragraph 1, A plastic depolymerization method characterized in that, in the step of applying mechanical energy to the above reaction mixture to cause a depolymerization reaction and obtain a product, mechanical energy is applied through a ball milling method.
4. In paragraph 1, A plastic depolymerization method characterized in that the above depolymerization reaction is performed without the addition of a separate catalyst or activator.
5. A product depolymerized according to the plastic depolymerization method of paragraph 1.
Citation Information
Patent Citations
Recycling technology of waste crosslinked polycarbonate
CN106432797A
Apparatus and method for forming 3D realistic stereoscopic projection mapping
KR1020240111547A
Method for depolymerising polysaccharides by means of mechanical milling
US20130032650A1
Mechanocatalytic Depolymerization of Plastics
US20230107759A1
KR20230039099A