Method for preparing regenerated polycaprolactone with high molecular weight and mechanical property by polymerizing depolymerized product through two-step method

Through the two-step polymerization and depolymerization product method, metal catalysts are used to promote the ring-opening polymerization and esterification polycondensation of the depolymerization product, solving the problem of low regeneration polycaprolactone performance in the prior art, and achieving high molecular weight and high mechanical properties The production of regenerated PCL improves the chemical recycling cycle rate and performance.

CN119019653APending Publication Date: 2024-11-26SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411183904.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to obtain regenerated polycaprolactone with high molecular weight and high mechanical properties through chemical depolymerization recovery, and the complex structure and low purity of the depolymerization products lead to deterioration of repolymerization performance, affecting their application and recycling recycle.

Method used

The two-step polymerization and depolymerization product method are used to perform ring-opening polymerization and esterification polycondensation in an inert atmosphere. The chain oligomers of the depolymerization product are catalyzed by metal catalysts to form high molecular weight regenerated polycaprolactone, through coordination bonds and Hydrogen bonds promote esterification and polycondensation reaction to form high-performance regenerated PCL.

Benefits of technology

The production of regenerated PCL with high molecular weight and high mechanical properties has been achieved, the tensile strength and elongation of break are significantly improved, the chemical recycling cycle rate has reached 99%, and the performance of regenerated PCL is similar to that of commercial PCL, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012985380000041
    Figure BDA0005012985380000041
  • Figure BDA0005012985380000081
    Figure BDA0005012985380000081
  • Figure BDA0005012985380000091
    Figure BDA0005012985380000091
Patent Text Reader

Abstract

The invention belongs to the field of polymer chemical recovery, and discloses a method for preparing regenerated polycaprolactone with high molecular weight and mechanical property by polymerizing a depolymerization product through a two-step method. The method comprises the following steps: in an inert atmosphere, carrying out ring opening polymerization on a depolymerization product at 120-160 DEG C to obtain a pre-polymerization product p-PCL, then carrying out esterification polycondensation at 140-270 DEG C to obtain regenerated polycaprolactone pc-PCL, and the reaction system contains a metal catalyst. The weight-average molecular weight of the obtained polycondensation PCL (pc-PCL) reaches up to 5.06 * 10 < 4 > g / mol, the tensile strength and the elongation at break of the polycondensation PCL are 35.5 Mpa and 1400% respectively, and the structure and the performance of the polycondensation PCL are similar to those of commercial PCL.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer chemical recovery, and particularly relates to a method for preparing regenerated polycaprolactone with high molecular weight and mechanical properties by polymerizing and depolymerizing products in two steps. Background Art

[0002] Polyester materials such as polycaprolactone (PCL), polylactic acid (PLLA), and polyethylene terephthalate (PET) are biodegradable, and the use of such materials can effectively reduce the threat of waste plastics to the ecological environment. However, the biodegradation of waste polyester can neither achieve efficient treatment of waste polyester nor cause serious waste of natural resources. Chemical depolymerization and recycling can quickly depolymerize polyester materials into small molecule chemicals or low molecular weight polyesters through chemical reactions, but the secondary use of these products is often low-value and high-loss, and it is impossible to achieve economical recovery and industrialization of waste polyester.

[0003] In the process of chemical depolymerization and recovery of PCL, due to the breakage of the ester bond with low bond energy in the main chain, the products obtained by depolymerization are usually hydroxy acids with carboxyl and hydroxyl ends, chain oligomers or cyclic monomers, cyclic oligomers, etc., and the depolymerization products are relatively complex. In addition, the small amount of carboxyl products present in the depolymerization products will further acidify PCL during its repolymerization process, reduce the molecular weight of the product of the traditional ε-CL monomer ring-opening polymerization reaction, and deteriorate the performance of the repolymerized PCL. If a single ring-opening polymerization method is used for the chemical depolymerization product, it will not be possible to prepare high-molecular-weight regenerated PCL, and the deterioration of the performance of the regenerated PCL will affect its application and recycling, and its chemical recycling recovery rate will be significantly reduced, resulting in a waste of resources.

[0004] Zhang et al. used a direct two-step method to melt polycondense lactic acid monomers, and completed the prepolymerization and final polymerization processes at 130°C and 165°C respectively while vacuuming to separate water molecules. They successfully prepared polylactic acid with a molecular weight of 37,000 under the catalysis of tin chloride dihydrate (Plastic Industry, 2023, 51(9): 60-64). Chinese patent publication CN107286697A introduces a method that first removes impurities from waste plastics and then adds a viscosity-enhancing chain extender, polyethylene oxide, and ethylene vinyl acetate copolymer. After mixing and mixing, these materials are homogenized and chain extended at a pressure of 1.5MPa in a twin-screw extruder to finally obtain composite plastic particles. This treatment method significantly increases the tensile strength of plastic particles from the original 16MPa to 31MPa. Chinese patent publication CN109749070A provides a method for recycling polyester bottle flakes and improving their viscosity. This method uses a compound of triphenyl phosphite and epoxy chain extender as a chain extender, and the polyester bottle flakes are reacted in a torque rheometer at a temperature of 250°C and a speed of 40r / min for 10 minutes. After such treatment, a high-viscosity polyester is obtained, and its characteristic viscosity reaches 1.1029dL / g, and the viscosity-average molecular weight increases to 47813g / mol. In these patents, the two-step method for preparing PLA allows its cyclization and chain growth processes to proceed step by step, and its polymerization process is more controllable, which effectively increases the molecular weight of PLA, but it is aimed at high-purity lactic acid monomers. In chain extension recovery technology, polyester materials with complex structures and uneven molecular weight distribution can be chain extended to prepare high-molecular-weight polyesters, but the addition of chain extenders destroys the regularity of the original structure of the polyester. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a two-step method for polymerizing and depolymerizing products to prepare regenerated polycaprolactone.

[0006] The purpose of the present invention is achieved through the following solutions:

[0007] A method for preparing regenerated polycaprolactone by polymerizing a depolymerization product in two steps comprises the following steps: in an inert atmosphere, subjecting the depolymerization product to ring-opening polymerization at 120-160° C. to obtain a prepolymerization product p-PCL, and then subjecting the prepolymerization product to esterification and polycondensation at 140-270° C. to obtain regenerated polycaprolactone pc-PCL, wherein the reaction system contains a metal catalyst.

[0008] The inert atmosphere includes at least one of nitrogen, argon and helium.

[0009] The depolymerization product is a product obtained by depolymerizing and degrading polycaprolactone, and includes cyclic monomers, cyclic oligomers, 6-hydroxycaproic acid and chain oligomers with carboxyl and hydroxyl ends.

[0010] The metal catalyst includes at least one of a metal ion salt and a metal oxide.

[0011] When the metal catalyst is a single catalyst, the metal catalyst is added in the ring-opening polymerization reaction; when the metal catalyst is a mixed catalyst, it is added in the ring-opening polymerization reaction and the esterification polycondensation reaction respectively.

[0012] When the metal catalyst is a mixed catalyst, a metal ion salt is added to the ring-opening polymerization reaction, and a metal oxide is added to the esterification polycondensation reaction; wherein the molar ratio of the metal ion salt to the metal oxide is 1:1-4.

[0013] The metal is a main group metal element or a transition metal element having Lewis acidity.

[0014] The metal ions in the metal ion salt are stannous ions and zinc ions; the anion groups are carboxylic acid ion groups or alcohol ion groups.

[0015] The carboxylic acid ion group is acetate (CH3COO - ) or isooctanoate (CH3(CH2)5CH2COO - ); the alcohol group is butanol (CH3CH2CH2CH2O - ) or isopropanol ((CH3)2CHO - ).

[0016] The metal element in the metal oxide is aluminum, iron or zinc.

[0017] The metal ion salt includes at least one of stannous acetate (Sn(CH3COO)2), zinc acetate (Zn(CH3COO)2), stannous isooctanoate (Sn(Oct)2), and zinc isooctanoate (Zn(Oct)2).

[0018] The metal oxide includes at least one of aluminum oxide (Al2O3), iron oxide (Fe2O3), and zinc oxide (ZnO).

[0019] The usage ratio of the metal catalyst to the depolymerization product is 0.05-5 mmol:114 g, preferably 0.05-1 mmol:114 g.

[0020] The temperature of the ring-opening polymerization is 120-140° C. and the time is 6-12 hours, preferably 8-12 hours.

[0021] The esterification polycondensation is carried out under a pressure of 0.01 to 0.05 MPa, at a temperature of 140 to 250° C., for a time of 3 to 24 hours.

[0022] The esterification polycondensation is carried out under a pressure of 0.01 to 0.02 MPa, at a temperature of 140 to 230° C., for a time of 3 to 12 hours.

[0023] After the esterification and polycondensation, the product is dissolved, added into methanol for precipitation, and separated to obtain regenerated polycaprolactone pc-PCL.

[0024] The concentration of the esterification polycondensation product in the solution after dissolution is 5-10 wt %.

[0025] The mechanism of the present invention is:

[0026] The cyclic product (including caprolactone monomer and cyclic oligomer) obtained after depolymerization is subjected to ring-opening polymerization to form low molecular weight p-PCL, and the chain oligomers in the depolymerization product, the terminal carboxyl group and the terminal hydroxyl group of p-PCL are catalyzed by a metal catalyst with controllable coordination bond strength to esterify and polycondense to prepare high-performance pc-PCL. The metal catalyst in the system forms coordination with the carbonyl oxygen atom with high electronegativity on the terminal carboxyl group of p-PCL at an appropriate temperature, and the hydrogen atom in the carboxyl group forms a hydrogen bond with the oxygen atom adjacent to the metal atom in the catalyst, thereby quickly generating an intermediate (I). In the intermediate (I), the electronegativity of the carbonyl carbon is reduced due to the electrophilic effect of coordination. At this time, the terminal hydroxyl group of another PCL chain nucleophilically attacks the carbonyl group, and coordination occurs between the hydroxyl oxygen and the carbonyl carbon. The hydroxyl oxygen in the terminal carboxyl group forms a hydrogen bond with the hydrogen of the terminal hydroxyl group, and a new intermediate (II) is formed due to the coordination and hydrogen bonding. Subsequently, the coordination bonds and hydrogen bonds in the intermediate (II) are rearranged, and a new PCL chain is formed with the release of water molecules. In this process, the metal atom reduces the electronegativity of the carbonyl carbon through coordination, promoting proton transfer during the esterification reaction. At the same time, the metal atom may also coordinate with the terminal hydroxyl group to enhance its nucleophilic attack ability. The general reaction formula is as follows:

[0027]

[0028] After the polycondensation reaction, the low / medium molecular weight p-PCL molecular chains are "reconnected" together to form higher molecular weight PCL molecular chains, achieving the goal of esterification polycondensation of p-PCL to form high-performance pc-PCL, where the reactivity of the polycondensation reaction is related to the number of free carboxyl and hydroxyl ends in p-PCL. The polycondensation reaction of terminal hydroxyl and carboxyl groups is a reversible reaction, and the introduction of catalysts and the generation of water may lead to further hydrolysis and acidolysis of PCL, so strict control of the amount of catalyst and timely removal of water in the system are the key to the polycondensation reaction.

[0029] Two chain-like PCL molecular chains are connected by ester bonds formed by esterification and polycondensation as a "bridge" to form high-molecular-weight PCL molecular chains, thereby preparing high-molecular-weight, high-performance recycled PCL by polymerizing complex depolymerization products in a two-step process of prepolymerization and polycondensation. Its mechanical properties are better than those of commercial PCL, and the recycled PCL can still be recycled in this way after being degraded. This two-step polymerization and depolymerization product preparation of high-performance PCL is extremely efficient, with a chemical recovery rate of up to 99%, which provides a new strategy for the chemical recycling of polyester.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) In the present invention, the depolymerization products containing various structures are polymerized in a one-pot manner using a two-step method to obtain high-molecular-weight and high-performance regenerated PCL, thereby solving the problems of low purity and complex structure of the depolymerization products, which lead to difficult polymerization of the products and low molecular weight of the polymerization products, and effectively improving the utilization rate of the products recovered by chemical depolymerization.

[0032] (2) In the present invention, the ring-opening polymerization of caprolactone and cyclic oligomers in the depolymerization product is first catalyzed to form chain PCL with terminal hydroxyl groups and terminal carboxyl groups, which is then mixed with carboxylic acids and chain oligomers in the depolymerization product that cannot be ring-opened, and high-performance PCL is prepared in a one-pot method through an esterification polycondensation reaction. The metal atom in the catalyst coordinates with the terminal carboxyl group in the chain PCL, and the terminal hydroxyl group of the other PCL chain nucleophilically attacks the carbonyl carbon in the carboxyl group, resulting in further esterification polycondensation reaction. With the release of water molecules and the formation of new ester bonds, the chain PCL with terminal hydroxyl groups and terminal carboxyl groups are connected to form a high molecular weight pc-PCL chain. The weight average molecular weight of the polycondensation PCL (pc-PCL) in the present invention is as high as 5.06×10 4 g / mol, its tensile strength and elongation at break are 35.5 MPa and 1400% respectively, and its structure and performance are similar to those of commercial PCL.

[0033] (3) In the present invention, a suitable catalyst and its ratio are selected to achieve asymmetric coordination catalysis for prepolymerization of the depolymerization product and esterification polycondensation of the prepolymer, effectively upgrading low / medium molecular weight p-PCL to pc-PCL with similar structure and performance to commercial PCL. Under the action of a metal catalyst, the depolymerization product is polymerized in a two-step method to form high-performance PCL, thereby achieving the reuse of the depolymerization product.

[0034] (4) Based on the thermodynamic and kinetic principles of mass transfer and heat transfer in the polycondensation process, the present invention optimizes the process parameters such as temperature, pressure and stirring, and obtains pc-PCL with high molecular weight and mechanical properties through efficient prepolymerization and polycondensation under relatively mild process parameters, including relatively low temperature, low pressure and low reaction time. In the present invention, the water molecules generated by the esterification polycondensation are separated in time by vacuum distillation during the esterification polycondensation process, which inhibits the hydrolysis of PCL and is more conducive to the formation of high molecular weight PCL.

[0035] (5) The present invention achieves the goal of preparing PCL with high chemical recycling rate, high molecular weight and mechanical properties by two-step polymerization and depolymerization products. The method is simple to operate, the reaction conditions are mild and controllable, it is convenient for industrial production, and it can efficiently complete the chemical recycling purpose of PCL whose performance has been reduced due to biodegradation. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The NMR spectrum and mass spectrum of the depolymerization product used in the present invention.

[0037] Figure 2 The stress-strain curve (a) and mechanical property comparison diagram (b) of pc-PCL11 obtained in Example 9 and commercial PCL. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0039] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0040] Preparation of depolymerization products:

[0041] Take 1000g of commercial PCL (purchased from Shenzhen Guanghua Weiye Co., Ltd.), add 0.5mol.% (accounting for the caprolactone unit in PCL) of stannous isooctanoate, depolymerize and separate after reduced pressure distillation at 220°C and 0.02MPa. After 8h of reaction, the depolymerization is complete, and the yield is 91.05wt.%.

[0042] like Figure 1 The depolymerization products include caprolactone monomers, cyclic oligomers, 6-hydroxycaproic acid and chain oligomers with carboxyl and hydroxyl ends.

[0043] Comparative Example 1

[0044] (1) 570 g of the depolymerization product and 0.5 mmol Ti(OCH2CH2CH2CH3)4 were added to a 1000 mL reaction bottle, and nitrogen was continuously passed at room temperature for 2 h. After the nitrogen was turned off, the temperature was raised to 140 °C and the reaction was carried out for 12 h. After the reaction was completed, the product was placed in a 40 °C forced air drying oven and dried to constant weight to obtain a prepolymerized product p-PCL.

[0045] (2) Esterification and polycondensation of p-PCL by melt polymerization: 114 g of dried p-PCL was added to a 500 mL reaction bottle, and the system was subjected to reduced pressure distillation at a pressure of 0.01 MPa. The oil bath temperature was raised to 220°C, and p-PCL was subjected to esterification and polycondensation for 12 h under mechanical stirring at 100 r / min.

[0046] (3) The polymer was completely dissolved in CH2Cl2 at a concentration of 5 wt%, and the polymer solution was added dropwise into high-speed rotating methanol (the volume of methanol was about 5 times the volume of chloroform). After the polymer was precipitated, the mixed solution was filtered and placed in a forced air drying oven at 40°C to dry to constant weight to obtain pc-PCL1.

[0047] pc-PCL1 was brittle and could not be processed and used for tensile testing.

[0048] Comparative Example 2

[0049] The difference from Comparative Example 1 is that the catalyst used is Ti(OCH(CH3)2)4, and pc-PCL2 is obtained.

[0050] pc-PCL2 is brittle and cannot be molded and used for tensile testing.

[0051] Example 1

[0052] The difference from Comparative Example 1 is that the catalyst used is Sn(CH3COO)2, and pc-PCL3 is obtained.

[0053] Example 2

[0054] The difference from Comparative Example 1 is that the catalyst used is Sn(Oct)2, and pc-PCL4 is obtained.

[0055] Example 3

[0056] The difference from Comparative Example 1 is that the catalyst used is Zn(CH3COO)2, and pc-PCL5 is obtained.

[0057] Example 4

[0058] The difference from Comparative Example 1 is that the catalyst used is Zn(Oct)2, the esterification polycondensation time is 6h, and pc-PCL6 is obtained.

[0059] Example 5

[0060] The difference from Comparative Example 1 is that the catalyst used is Al2O3, and pc-PCL7 is obtained.

[0061] Example 6

[0062] The difference from Comparative Example 1 is that the catalyst used is Fe2O3, the esterification polycondensation time is 6h, and pc-PCL8 is obtained.

[0063] Example 7

[0064] The difference from Comparative Example 1 is that the catalyst used is ZnO, the temperature of esterification polycondensation is 180°C, and pc-PCL9 is obtained.

[0065] Example 8

[0066] The difference from Comparative Example 1 is that the catalysts are Zn(Oct)2 and ZnO, 0.25 mmol Zn(Oct)2 is added in step (1), and 0.05 mmol ZnO is added in step (2), the temperature of esterification polycondensation is 160°C, and the time is 6 hours to obtain pc-PCL10.

[0067] Example 9

[0068] The difference from Comparative Example 1 is that the catalysts are Zn(Oct)2 and ZnO, 0.125 mmol Zn(Oct)2 is added in step (1), and 0.075 mmol ZnO is added in step (2). The temperature of esterification polycondensation is 140°C and the time is 8 hours to obtain pc-PCL11.

[0069] Example 10

[0070] The difference from Comparative Example 1 is that the catalysts are Zn(Oct)2 and ZnO, 0.1 mmol Zn(Oct)2 is added in step (1), and 0.08 mmol ZnO is added in step (2), and the temperature of esterification and polycondensation is 140°C to obtain pc-PCL12.

[0071] Table 1 Statistics of weight average molecular weight and reaction time of pc-PCL in various examples and comparative examples

[0072]

[0073] As shown in Table 1, the Zn-containing 2+ The metal catalyst can obtain higher molecular weight pc-PCL when preparing PCL by catalytic ring-opening polymerization and esterification polycondensation, and effectively shorten the polycondensation reaction time. 2+In the process of coordination with the terminal hydroxyl group, a stronger coordination effect can be achieved, which effectively reduces the activation energy of the reaction and avoids side reactions such as random rupture of the main chain and carbonization. Since the anionic groups in the ionic catalyst may form acids, the presence of acids will lead to acid hydrolysis or rupture of the main chain, competing with the polycondensation reaction, thereby reducing the polycondensation efficiency. Therefore, metal oxides are introduced in Examples 5-7. It is found from the table that compared with the catalysts without Zn 2+ The molecular weight of pc-PCL obtained by polycondensation of Al2O3 and Fe2O3 is significantly higher than that of ionic catalysts. Among them, the weight average molecular weight of pc-PCL9 obtained by polycondensation catalyzed by ZnO is the highest, which is 4.26×10 4 g / mol, indicating that ZnO can effectively increase the molecular weight growth of PCL short chains. In Table 1 Examples 8-10, it was found that the molecular weight of the polymer product can be effectively increased by using different catalysts for prepolymerization and polycondensation. The possible reason is that Zn(Oct)2 is more conducive to the ring-opening polymerization of caprolactone in the prepolymerization stage, while the addition of ZnO is more conducive to the esterification polycondensation reaction of p-PCL short chains. A relatively uniform prepolymer product can be obtained under catalysis, thereby further improving the polycondensation effect of ZnO on p-PCL short chains, among which Zn(Oct)2 / ZnO=1:3 can achieve efficient polymerization and generate high molecular weight pc-PCL11. Under this condition, the molecular weight of pc-PCL is increased, and the energy loss in the esterification polycondensation process is effectively reduced. When the Zn(Oct)2 participating in the prepolymerization has a stronger synergistic coordination ability with ZnO, it can affect the polarity of the carbonyl oxygen to a greater extent when coordinating with the main chain, which can effectively improve its condensation efficiency during the condensation process and avoid the occurrence of side reactions, thereby obtaining pc-PCL with a higher molecular weight.

[0074] Table 2 Mechanical properties of pc-PCL in various embodiments and comparative examples

[0075]

[0076] The pc-PCL in the above Examples 1-10 was subjected to tensile tests, and the mechanical properties are shown in Table 2. It can be seen from Table 2 that with the increase of molecular weight, the increase of pc-PCL molecular weight leads to the enhancement of the intermolecular force of the polymer chain, and the molecular chain structure is more stable when subjected to external force, thus showing stronger mechanical properties. Comparative Example 9, the stress-strain curve of the commercial PCL of pc-PCL11 is shown in Table 2. Figure 2. From the data in the figure, it can be seen that the tensile strength and elongation at break of commercial PCL are 29.9MPa and 1204%, respectively. At a catalyst addition ratio of Zn(Oct)2 / ZnO=1:3, the depolymerization product was subjected to a two-step prepolymerization and polycondensation method to prepare a regenerated PCL with mechanical properties equivalent to those of commercial PCL, and its tensile strength and elongation at break were 35.5Mpa and 1400%, respectively. That is, at a catalyst addition amount of Zn(Oct)2 / ZnO=1:3, the depolymerization product was subjected to a two-step prepolymerization and polycondensation method to prepare a regenerated PCL with mechanical properties equivalent to those of commercial PCL.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps, It is characterized in that The following steps are involved: In an inert atmosphere, the depolymerization product is subjected to ring-opening polymerization at 120-160° C. to obtain a prepolymer product p-PCL, and then esterified and polycondensed at 140-270° C. to obtain a regenerated polycaprolactone pc-PCL, and the reaction system contains a metal catalyst.

2. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: The inert atmosphere includes at least one of nitrogen, argon and helium; The depolymerization product is a product obtained by depolymerizing and degrading polycaprolactone, including cyclic monomers, cyclic oligomers, 6-hydroxycaproic acid and chain oligomers with carboxyl and hydroxyl ends; The metal catalyst includes at least one of a metal ion salt and a metal oxide; wherein the metal is a main group metal element or a transition metal element having Lewis acidity.

3. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: When the metal catalyst is a single catalyst, the metal catalyst is added in the ring-opening polymerization reaction; when the metal catalyst is a mixed catalyst, it is added in the ring-opening polymerization reaction and the esterification polycondensation reaction respectively.

4. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: When the metal catalyst is a mixed catalyst, a metal ion salt is added to the ring-opening polymerization reaction, and a metal oxide is added to the esterification polycondensation reaction; wherein the molar ratio of the metal ion salt to the metal oxide is 1:1-4.

5. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 2, Features: The metal ion salt contains stannous ions and zinc ions; the anion group contains carboxylic acid ion groups or alcohol ion groups; The carboxylic acid ion group is acetate or isooctanoate; the alcohol group is butanol or isopropanol; The metal element in the metal oxide is aluminum, iron or zinc.

6. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 2, Features: The metal ion salt comprises at least one of stannous acetate, zinc acetate, stannous isooctanoate and zinc isooctanoate; The metal oxide includes at least one of aluminum oxide, iron oxide and zinc oxide.

7. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: The usage ratio of the metal catalyst to the depolymerization product is 0.05-5 mmol:114 g, preferably 0.05-1 mmol:114 g.

8. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: The temperature of the ring-opening polymerization is 120-140° C. and the time is 6-12 hours, preferably 8-12 hours.

9. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: The esterification polycondensation is carried out under a pressure of 0.01 to 0.05 MPa, at a temperature of 140 to 250° C., for a time of 3 to 24 hours.

10. The method for preparing regenerated polycaprolactone by polymerizing the depolymerization product in two steps according to claim 1, Features: The esterification polycondensation is carried out under a pressure of 0.01 to 0.02 MPa, at a temperature of 140 to 230° C., for a time of 3 to 12 hours.

Citation Information

Patent Citations

  • A method for recycling and regenerating plastic through homogenization and chain extending

    CN107286697A

  • Method for tackifying recycled polyester bottle flake by using chain extender and application thereof

    CN109749070A

Cited By

  • Method for preparing high-molecular-weight and mechanical-property PCL (polycaprolactone) through efficient polycondensation of low / medium-molecular-weight PCL

    CN121064450A

  • Method for recycling waste chinlon textile

    CN121698794A

  • Method for recycling waste nylon textile

    CN121698794B