Anode active material, method for preparing anode active material, anode composition, lithium secondary battery anode comprising same, and lithium secondary battery comprising anode
By controlling the grain size and high-angle grain boundary ratio of silicon-based active materials through a rapid cooling and pulverization process, the negative electrode active material in lithium secondary batteries improves cycle capacity retention and initial capacity efficiency, overcoming the challenges of volume expansion and conductive path damage.
Patent Information
- Application Number
- PCT/KR2024/001456
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-01-30
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-24
AI Technical Summary
Silicon-based compounds used as negative electrode active materials in lithium secondary batteries face challenges due to high volume expansion during charging and discharging, which can lead to conductive path damage and reduced battery performance, limiting the ability to achieve high capacity and cycle life.
A negative electrode active material is developed using silicon-based crystal grains with a high angle grain boundary ratio of 30% or more, where the crystal grain size is controlled between 2nm and 1μm through a rapid cooling process followed by pulverization of a plate-shaped silicon precursor, optimizing grain size and boundary ratio to prevent conductive path damage and enhance capacity retention.
The approach results in increased cycle capacity retention and initial capacity efficiency of lithium secondary batteries by controlling the grain size and high-angle grain boundary ratio, effectively addressing the issues of volume expansion and conductive path damage.
Smart Images

Figure KR2024001456_24102024_PF_FP_ABST
Abstract
Description
Negative electrode active material, method for producing negative electrode active material, negative electrode composition, negative electrode for lithium secondary battery including the same, and lithium secondary battery including the negative electrode
[0001] This application is based upon and claims priority to Korean Patent Application No. 10-2023-0052006, filed with the Korean Intellectual Property Office on April 20, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present application relates to a negative electrode active material, a method for producing a negative electrode active material, a negative electrode composition, a negative electrode for a lithium secondary battery including the same, and a lithium secondary battery including the negative electrode.
[0003] Due to the rapid increase in fossil fuel use, the demand for alternative or clean energy is increasing, and as part of this, the most actively researched field is power generation and storage using electrochemical reactions.
[0004] A representative example of an electrochemical device that currently utilizes this electrochemical energy is the secondary battery, and its application area is gradually expanding.
[0005] With the increasing technological development and demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used. Furthermore, active research is being conducted on methods for manufacturing high-density electrodes with even higher energy density per unit volume as electrodes for these high-capacity lithium secondary batteries.
[0006] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode contains a negative active material that inserts and desorbs lithium ions from the positive electrode. Silicon particles with high discharge capacity can be used as the negative active material. Therefore, active research is underway to improve the performance of negative active materials using silicon particles.
[0007] <Prior Art Literature>
[0008] (Patent Document 1) Japanese Patent Publication No. 2009-080971
[0009] As a result of research on reducing the grain size, it was confirmed through research that when a plate-shaped silicon precursor is formed and then crushed by controlling the cooling rate of the rapid cooling process prior to crushing the existing MG (Metallurgical Grade)-Si, the desired grain size can be reduced and the high-angle boundary ratio can be controlled.
[0010] The present application relates to a negative electrode active material, a method for producing a negative electrode active material, a negative electrode composition, a negative electrode for a lithium secondary battery including the same, and a lithium secondary battery including the negative electrode.
[0011] One embodiment of the present specification provides an anode active material including a silicon-based active material, wherein the silicon-based active material includes silicon-based crystal grains, a high angle grain boundary ratio within the silicon-based crystal grains is 30% or more, and the silicon-based active material satisfies the following equations 1 and 2.
[0012] [Formula 1] About 1 μm ≤ particle size (D50) of silicon-based active material ≤ about 10 μm
[0013] [Formula 2] About 2 nm ≤ Crystalline grain size of silicon-based active material ≤ about 1 μm
[0014] In another embodiment, a method for producing an anode active material is provided, comprising: a step of rapidly cooling metal silicon to form a silicon precursor; and a step of pulverizing the silicon precursor to form a silicon-based active material; wherein the step of rapidly cooling includes melt spinning, suction casting, or injection casting.
[0015] In another embodiment, an object of the present invention is to provide a negative electrode composition comprising a negative electrode active material according to the present application; a negative electrode conductive material; and a negative electrode binder.
[0016] In another embodiment, there is provided an anode for a lithium secondary battery, comprising: a negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, wherein the negative electrode active material layer comprises a negative electrode composition according to the present application or a cured product thereof.
[0017] In addition, a lithium secondary battery is provided, including: a positive electrode; an anode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.
[0018] In the case of a negative active material according to one embodiment of the present invention, unlike the existing pulverization processing method, a rapid cooling process is performed prior to MG (Metallurgical Grade)-Si pulverization to form a plate-shaped silicon precursor, and the crystal grain size and high angle grain boundary ratio of the produced silicon-based active material can be optimized by controlling the cooling rate.
[0019] As described above, a silicon-based active material having nano-sized crystal grains can be secured by grinding a plate-shaped silicon precursor having nano-sized crystal grains, and when manufacturing a negative electrode using this, the cycle capacity retention rate and initial capacity efficiency are increased.
[0020] The negative active material of the present invention is a silicon-based active material, including SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 약 70 중량부 이상 포함하는, 예를 들면 Pure Si 활물질을 가지면서 이에 따른 문제점인 충방전에 따른 부피 팽창의 문제를 결정립 사이즈 조절을 통하여 해결한다.
[0021] Figure 1 is a flowchart of a manufacturing process of a silicon-based active material according to one embodiment of the present application.
[0022] Figure 2 shows an enlarged view of a silicon-based active material according to one embodiment of the present application.
[0023] Figure 3 is a diagram showing a laminated structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application.
[0024] Fig. 4 is a diagram showing a laminated structure of a lithium secondary battery according to one embodiment of the present application.
[0025] Figure 5 is a diagram showing a method for calculating crystal grain size.
[0026] Figure 6 is a diagram showing the misorientation angle.
[0027] In some of the accompanying drawings, corresponding components are designated by the same reference numerals. Those skilled in the art will appreciate that the drawings illustrate elements simply and clearly and are not necessarily drawn to scale. For example, to facilitate understanding of various embodiments, the dimensions of some elements depicted in the drawings may be exaggerated relative to other elements. Furthermore, elements of known technology that are useful or essential in commercially feasible embodiments may often not be depicted so as not to obscure the spirit of various embodiments of the present invention.
[0028] <Explanation of symbols>
[0029] 1: Silicon-based active material
[0030] 2: Silicon-based crystal grains
[0031] 3: Grain boundary
[0032] 4: misorientation angle
[0033] 10: Negative current collector layer
[0034] 20: Negative active material layer
[0035] 30: Membrane
[0036] 40: Positive active material layer
[0037] 50: Positive current collector layer
[0038] 100: Cathode for lithium secondary batteries
[0039] 200: Cathode for lithium secondary batteries
[0040] Before explaining the present invention, some terms are first defined.
[0041] When a part of this specification is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise stated.
[0042] In this specification, ‘p to q’ means a range of ‘p or more and q or less.’
[0043] In this specification, "specific surface area" is measured by the BET method, and specifically, is calculated from the nitrogen gas adsorption amount at liquid nitrogen temperature (77K) using BELSORP-mino II of BEL Japan. That is, in this application, the BET specific surface area may mean the specific surface area measured by the above measurement method.
[0044] In this specification, "Dn" means particle size distribution, and means the particle size at the n% point of the cumulative distribution of particle numbers according to particle size. That is, D50 is the particle size (average particle size) at the 50% point of the cumulative distribution of particle numbers according to particle size, D90 is the particle size at the 90% point of the cumulative distribution of particle numbers according to particle size, and D10 is the particle size at the 10% point of the cumulative distribution of particle numbers according to particle size. Meanwhile, the average particle size can be measured using a laser diffraction method. For example, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction pattern according to particle size is measured when the particles pass through a laser beam, thereby calculating the particle size distribution.
[0045] In one embodiment of the present application, particle size or particle diameter may mean the average diameter or representative diameter of each grain forming the metal powder.
[0046] As used herein, the term "a polymer comprises a monomer as a monomer unit" means that the monomer participates in a polymerization reaction and is included as a repeating unit within the polymer. As used herein, "a polymer comprises a monomer" is interpreted to mean that the polymer comprises the monomer as a monomer unit.
[0047] In this specification, the term 'polymer' is understood to be used in a broad sense including copolymers unless 'homopolymer' is specified.
[0048] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-converted molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various degrees of polymerization commercially available for molecular weight measurement as standard materials. In this specification, molecular weight means weight average molecular weight unless otherwise specified.
[0049] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values provided to aid understanding of the present invention.
[0050] The limitations of numerical ranges used in this specification (e.g., ≤, parts by weight, thickness, more than, less than, etc.) are used to mean a range or approximation of the numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which mentions exact or absolute numbers provided to aid in the understanding of the present invention.
[0051] Recent demand for high-density energy batteries has led to research into ways to increase battery capacity by using silicon-based compounds, such as Si / C or SiOx, as anode active materials. These compounds have capacities more than 10 times greater than graphite-based materials. However, high-capacity silicon-based compounds, while offering greater capacity than conventional graphite, suffer from rapid volume expansion during the charging process, which disrupts conductive paths and degrades battery performance.
[0052] Accordingly, various studies are being conducted to address the challenges associated with using silicon-based compounds as anode active materials. For example, various methods are being discussed, including controlling the operating potential for silicon-based compounds as anode active materials, coating additional thin films on the active material layer, controlling the particle size of silicon-based compounds to suppress volume expansion itself, and preventing the interruption of conductive paths. However, each method has its own advantages and disadvantages.
[0053] Meanwhile, in the case of Si anode active materials, since the grain boundary acts as a diffusion path for lithium, it has been revealed through research that the wider the grain boundary, that is, the smaller the grain size, the more advantageous it is for the performance characteristics of secondary batteries. However, when manufacturing anode active materials by pulverizing Metallurgical Grade Si (MG-Si), there is a limit to reducing the grain size of the Si active material because the general grain size of MG-Si is several hundred millimeters to several millimeters, and thus there is still a limit to improving the performance characteristics of secondary batteries.
[0054] In the present invention, even when a silicon-based active material is used as an anode active material to improve the capacity performance of a secondary battery, a technique is provided for controlling the crystal grain size within Si particles, for example, by reducing the crystal grain size within Si particles to a size of several nm to several tens of nm, so as to prevent damage to a conductive path due to volume expansion of the silicon-based compound.
[0055] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice it. However, the present invention can be implemented in various different forms and is not limited to the following description.
[0056] One embodiment of the present specification provides an anode active material including a silicon-based active material, wherein the silicon-based active material includes silicon-based crystal grains, and a high angle grain boundary ratio (HAGB) within the silicon-based crystal grains is 30% or more, and the silicon-based active material satisfies the following equations 1 and 2.
[0057] [Formula 1] About 1 μm ≤ particle size (D50) of silicon-based active material ≤ about 10 μm
[0058] [Formula 2] About 2 nm ≤ Crystalline grain size of silicon-based active material ≤ about 1 μm
[0059] In the case of a negative active material according to one embodiment of the present invention, unlike the existing pulverization process, a rapid cooling process is performed prior to MG-Si pulverization to form a plate-shaped silicon precursor, and as a result, the plate-shaped silicon precursor produced by controlling the cooling rate is pulverized, thereby optimizing the crystal grain size and high angle boundary (HAGB) ratio of the silicon-based active material.
[0060] As described above, a silicon-based active material having nano-sized crystal grains can be secured by grinding a plate-shaped silicon precursor having nano-sized crystal grains, and when this is used to manufacture a negative electrode of a lithium secondary battery, the cycle capacity retention rate and initial capacity efficiency of the lithium secondary battery are increased.
[0061] In one embodiment of the present application, the silicon-based active material is SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 약 70 중량부 이상 포함할 수 있다.
[0062] In one embodiment of the present application, the silicon-based active material includes SiOx (x=0), and may include about 70 parts by weight or more of the SiOx (x=0) based on 100 parts by weight of the silicon-based active material.
[0063] In another embodiment, the silicon-based active material may include about 70 parts by weight or more, for example, about 80 parts by weight or more, or about 90 parts by weight or more, and may include about 100 parts by weight or less, for example, about 99 parts by weight or less, or about 95 parts by weight or less, of the SiOx (x=0) based on 100 parts by weight.
[0064] In one embodiment of the present application, pure silicon (Si) particles may be used as a silicon-based active material. Using pure silicon (Si) particles as a silicon-based active material may mean that, based on 100 parts by weight of the total silicon-based active material, pure Si particles (SiOx (x=0)) not combined with other particles or elements are included within the above range.
[0065] In one embodiment of the present application, the silicon-based active material may be formed of silicon-based particles having 100 parts by weight of SiOx (x=0) based on 100 parts by weight of the silicon-based active material.
[0066] In one embodiment of the present application, the silicon-based active material may include a metal impurity, and at this time, the impurity may be a metal that may be generally included in the silicon-based active material, and may include, for example, about 0.1 part by weight or less based on 100 parts by weight of the silicon-based active material.
[0067] In the case of silicon-based active materials used as negative electrode active materials in lithium secondary batteries, their capacity is significantly higher than that of graphite-based active materials used in the past, and attempts to apply them are increasing. However, due to the high volume expansion rate during the charge / discharge process, such attempts are limited to cases where a small amount of silicon-based active material is mixed with the graphite-based active material.
[0068] Therefore, in the case of the present invention, while using a silicon-based active material as an anode active material to improve capacity performance, in order to solve the problems of the silicon-based active material as described above, the existing problems were solved by controlling the crystal grain size of the silicon-based active material itself rather than controlling the composition of the conductive agent and binder.
[0069] In this application, in order to reduce the crystal grain size, a rapid cooling process is performed prior to MG-Si pulverization in the manufacturing process of a negative electrode active material to manufacture a plate-shaped silicon precursor, which is then pulverized to manufacture a silicon-based active material.
[0070] In one embodiment of the present application, the silicon precursor satisfies the following equations 3 and 4.
[0071] [Formula 3] Approximately 10 μm ≤ silicon precursor plate thickness ≤ approximately 2 mm
[0072] [Formula 4] About 2 nm ≤ Crystalline grain size in silicon precursor ≤ about 1 μm
[0073] In one embodiment of the present application, the above formula 3 satisfies about 10 μm ≤ plate thickness of silicon precursor ≤ 2 mm, or about 13 μm ≤ plate thickness of silicon precursor ≤ 1.5 mm, or about 15 μm ≤ plate thickness of silicon precursor ≤ 1 mm.
[0074] In one embodiment of the present application, the above formula 4 satisfies about 2 nm ≤ crystal grain size in the silicon precursor ≤ 1 μm, and may satisfy, for example, about 10 nm ≤ crystal grain size in the silicon precursor ≤ 1 μm, or about 40 nm ≤ crystal grain size in the silicon precursor ≤ 1 μm.
[0075] Referring to FIG. 1, according to one embodiment of the present invention, when forming a plate-shaped silicon precursor using melt spinning, first, MG silicon is placed in a graphite crucible and a current of about 10 kA is applied to a copper coil to manufacture silicon in a molten state of about 2000°C. (S1) Next, the molten silicon is injected at a pressure of 1.2 kPa into a copper wheel with a diameter of 25 cm that rotates at a speed of 3000 rpm to manufacture a plate-shaped silicon precursor. (S2) Meanwhile, it is checked whether the manufactured precursor satisfies Equations 3 and 4 (S3), and if so (S3, YES), the manufactured silicon precursor is pulverized using a method such as a ball mill, a pin mill, a disk mill, or a jet mill to form a silicon-based active material. (S4) If the precursor manufactured in S3 does not satisfy Equations 3 and 4, the process returns to step S1 to manufacture molten metal silicon. Or, return to step S2 and repeat the process of manufacturing plate-shaped metal silicon through rapid cooling of the molten metal silicon. Meanwhile, check whether the active material formed in step S5 satisfies Equations 1 and 2, and if so (YES, S5), secure the silicon-based active material in step S6 and complete the process. After this, the secured silicon-based active material can be used to manufacture, for example, a negative electrode of a lithium secondary battery. Meanwhile, if the active material formed in step S5 does not satisfy Equations 1 and 2 (S5, NO), return to step S4 and repeat the process.
[0076] The present application manufactures a plate-shaped silicon precursor by performing a rapid cooling process on molten MG-Si prior to MG-Si pulverization in the manufacturing process of a negative active material in order to reduce the crystal grain size, and manufactures a silicon precursor satisfying Equations 3 and 4 through this control.
[0077] By grinding a plate-shaped silicon precursor having nano-sized grains as described above, a silicon-based active material having nano-sized grains can be secured, and by using this to manufacture a negative electrode, for example, the cycle capacity retention rate and initial capacity efficiency of a secondary battery can be increased.
[0078] In one embodiment of the present application, a silicon-based active material can be formed by pulverizing a silicon precursor in the form of a plate as described above, and the silicon-based active material according to the present application satisfies the following equations 1 and 2.
[0079] [Formula 1] Approximately 1 μm ≤ particle size (D50) of silicon-based active material ≤ 10 μm
[0080] [Formula 2] About 2 nm ≤ Crystalline grain size of silicon-based active material ≤ 1 μm
[0081] The above formula 1 can satisfy, for example, a range of about 3 μm ≤ particle size (D50) of the silicon-based active material ≤ 9 μm, or about 3 μm ≤ particle size (D50) of the silicon-based active material ≤ 7 μm.
[0082] In addition, the above formula 2 can satisfy, for example, about 5 nm ≤ crystal grain size of silicon-based active material ≤ 700 nm, or about 20 nm ≤ crystal grain size of silicon-based active material ≤ 500 nm.
[0083] As described above, by controlling the crystal grain size during the formation of a silicon precursor and further performing a grinding process, the crystal grain size is finally satisfied in the range of the above formula 2, thereby increasing the cycle capacity retention rate and initial capacity efficiency of the secondary battery.
[0084] In one embodiment of the present application, the crystal grain size can be calculated as the FWHM (Full Width at Half Maximum) value through XRD analysis. For example, a method for calculating the crystal grain size can be seen in Fig. 5. In Fig. 5, the remaining values excluding L are measured through XRD analysis of a silicon-based active material, and the crystal grain size can be measured through the Debey-Scherrer equation, which shows that the FWHM and the crystal grain size are inversely proportional. In this case, the Debey-Scherrer equation is as shown in Equation 1-1 below.
[0085] [Equation 1-1] FWHM=Kλ / LCosθ
[0086] In the above formula 1-1,
[0087] L represents the grain size, K is a constant, θ is the bragg angle, and λ is the wavelength of the X-ray.
[0088] In addition, the shape of the crystal grains is diverse and can be measured three-dimensionally, and the size of the crystal grains can be measured using the commonly used circle method and diameter measurement method, but is not limited thereto.
[0089] The above diameter measurement method can be measured by drawing 5-10 equilibrium lines, each of which is L mm long, on a microscopic photograph of the target particle, counting the number of grains z on the lines, and averaging them. At this time, only those that are completely included are counted, and those that intersect are excluded. If the number of lines is P and the magnification is V, the average grain diameter can be calculated using the following equations 1-2.
[0090] [Formula 1-2] Dm = (L*P*10 3 ) / (zV) (um)
[0091] In addition, the above circle method is a method of calculating the average area of crystal grains by drawing a circle of a set diameter on a microscopic photograph of the target particle and calculating the number of crystal grains within the circle and the number of crystal grains that fall on the boundary line using the following equation 1-3.
[0092] [Formula 1-3] Fm = (Fk * 10 6 ) / ((0.67n + z) V 2 ) (um 2 )
[0093] In the above equation 1-3, Fm represents the average particle area, Fk represents the measured area on the photograph, z represents the number of particles inside the circle, n represents the number of particles in the circular arc, and V represents the magnification of the microscope.
[0094] In one embodiment of the present application, the silicon-based active material includes silicon-based crystal grains, and a negative electrode active material is provided in which the ratio of high-angle boundaries within the silicon-based crystal grains is about 30% or more.
[0095] In another embodiment, the silicon-based active material includes silicon-based crystal grains, and the ratio of high-angle boundaries within the silicon-based crystal grains may be about 30% or more, 35% or more, 40% or more, and about 80% or less, 75% or less, or 70% or less.
[0096] In the present application, a silicon-based crystal grain may mean an individual particle forming a silicon-based active material, and the silicon-based crystal grains come together to form a silicon-based active material, and a grain boundary may be defined as a defect between the corresponding crystal grains.
[0097] When manufactured using the above-described manufacturing method, many high angle grain boundaries (HAGBs) with high grain boundary energy are formed, and lithium ions can diffuse more easily in the high angle boundaries than in the low angle grain boundaries (LAGBs).
[0098] In the present application, the high-angle boundary ratio may mean the ratio of grain boundaries having a boundary angle of about 15° or more in the entire silicon-based active material.
[0099] In the present application, the high angle grain boundary may mean a misorientation angle > about 15°, and the low angle grain boundary may mean about 2° < misorientation angle <15°.
[0100] Figure 6 is a diagram showing a misorientation angle. The misorientation angle (4) can be defined as the angle of the difference in crystal orientation between two adjacent silicon-based crystal grains (2). In this case, a grain boundary can be defined as a crystal defect between different silicon-based crystal grains (2).
[0101] The silicon-based active material according to the present application can be formed with a relatively high ratio of high-angle boundaries among all grain boundaries, thereby improving the performance of the battery.
[0102] In one embodiment of the present application, a negative active material is provided in which the average misorientation angle of the silicon-based crystal grains is about 5° or more.
[0103] Figure 2 is an enlarged view of a silicon-based active material according to one embodiment of the present application. For example, the silicon-based active material (1) is composed of a plurality of silicon-based crystal grains (2), wherein the crystal grains have a crystal grain size as shown in the above formula 2. In addition, crystal defects between silicon-based crystal grains can be defined as grain boundaries.
[0104] In one embodiment of the present application, the silicon-based active material may include silicon-based particles having a particle size distribution of about 0.01 μm or more and 30 μm or less.
[0105] The above-mentioned silicon-based active material includes silicon-based particles having a particle size distribution of about 0.01 μm or more and 30 μm or less, which means that it includes a plurality of individual silicon-based particles having particle sizes within the above range, and the number of silicon-based particles included is not limited.
[0106] The particle size of the above silicon-based particles can be expressed by their diameter if they are spherical, but even if they are of a shape other than spherical, the particle size can be measured by comparing them to the spherical case, and the particle size of individual silicon-based particles can be measured by a method generally used in the art.
[0107] In one embodiment of the present application, the silicon-based active material may exist in a crystalline or amorphous form, for example, and may not be porous. The silicon particles may be spherical or fragment-shaped, for example. In one embodiment, the silicon particles may also have a fibrous structure or exist in the form of a silicon-containing film or coating.
[0108] In one embodiment of the present application, a negative electrode composition is provided, including the negative electrode active material; a negative electrode conductive material; and a negative electrode binder.
[0109] In one embodiment of the present application, a negative electrode composition is provided in which the negative electrode active material is at least about 40 parts by weight based on 100 parts by weight of the negative electrode composition.
[0110] In another embodiment, the negative electrode active material may be included in an amount of about 40 parts by weight or more, for example, 60 parts by weight or more, or 65 parts by weight or more, or 70 parts by weight or more, and may be 95 parts by weight or less, or 90 parts by weight or less, or 85 parts by weight or less, based on 100 parts by weight of the negative electrode composition.
[0111] The negative electrode composition according to the present application uses a negative electrode active material that satisfies a specific surface area size capable of controlling the volume expansion rate during the charge and discharge process even when a silicon-based active material with a significantly high capacity is used within the above range, so that the performance of the negative electrode is not deteriorated even within the above range, and has the characteristic of improved output characteristics during charge and discharge compared to conventional secondary batteries.
[0112] Graphite compounds were traditionally used as negative electrode active materials. However, with the increasing demand for high-capacity batteries, attempts to mix silicon-based active materials to increase capacity are increasing. However, in the case of silicon-based active materials, even if the properties of the silicon-based active material itself are adjusted as described above, the problem of rapid volume expansion during the charge / discharge process can occur, damaging the conductive path formed within the negative electrode active material layer.
[0113] In one embodiment of the present application, the negative electrode conductive material may include at least one selected from the group consisting of a dot-shaped conductive material, a planar conductive material, and a linear conductive material.
[0114] In one embodiment of the present application, the dot-shaped conductive material may be used to improve conductivity of the negative electrode, and refers to a dot-shaped or spherical conductive material that has conductivity without causing chemical change. For example, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, paneth black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and according to one embodiment, may include carbon black in terms of implementing high conductivity and improving dispersibility.
[0115] In one embodiment of the present application, the dot-shaped conductive material has a BET specific surface area of about 40 m 2 / g or more than 70 m 2 / g or less, for example 45 m 2 / g or more than 65 m 2 / g or less, or 50 m 2 / g or more than 60 m 2 / g can be less.
[0116] In one embodiment of the present application, the dot-shaped conductive material can satisfy a range in which the volatile matter content is about 0.01% or more and about 1% or less, for example, about 0.01% or more and about 0.3% or less, or about 0.01% or more and about 0.1% or less.
[0117] When the functional group content of the dot-shaped conductive material satisfies the above range, the functional groups present on the surface of the dot-shaped conductive material allow the dot-shaped conductive material to be smoothly dispersed within the solvent when water is used as the solvent. For example, in the present invention, the functional group content of the dot-shaped conductive material can be reduced by using a specific silicon-based active material, thereby achieving an enhanced effect in improving dispersibility.
[0118] In one embodiment of the present application, a dot-shaped conductive material having a functional group content within the above range is included together with a silicon-based active material, and the functional group content can be controlled by adjusting the degree of heat treatment of the dot-shaped conductive material.
[0119] In one embodiment of the present application, the particle size of the dot-shaped conductive material may be from about 10 nm to about 100 nm, for example, from about 20 nm to 90 nm, or from about 20 nm to 60 nm.
[0120] In one embodiment of the present application, the conductive material may include a planar conductive material.
[0121] The above-mentioned planar conductive material can improve conductivity by increasing planar contact between silicon particles within the cathode, and at the same time, suppress the disconnection of conductive paths due to volume expansion. The above-mentioned planar conductive material can be expressed as a plate-shaped conductive material or a bulk conductive material.
[0122] In one embodiment of the present application, the planar conductive material may include at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and may be plate-shaped graphite according to one embodiment.
[0123] In one embodiment of the present application, the average particle diameter (D50) of the surface-shaped conductive material may be about 2 μm to 7 μm, for example, about 3 μm to 6 μm, or about 3.5 μm to 5 μm. When the above range is satisfied, the sufficient particle size facilitates dispersion without causing excessive viscosity increase in the negative electrode slurry. Therefore, the dispersion effect is improved when dispersion is performed using the same equipment and time.
[0124] In one embodiment of the present application, the surface-shaped conductive material provides a negative electrode composition having a D10 of about 0.5 μm or more and 2.0 μm or less, a D50 of about 2.5 μm or more and 3.5 μm or less, and a D90 of about 6.5 μm or more and 15.0 μm or less.
[0125] In one embodiment of the present application, the planar conductive material may be a high-specific surface area planar conductive material having a high BET surface area; or a low-specific surface area planar conductive material.
[0126] In one embodiment of the present application, a high surface area surface conductive material or a low surface area surface conductive material may be used without limitation as the surface conductive material, but in one embodiment, a surface conductive material may be affected to some extent by dispersion influence on electrode performance, and thus a low surface area surface conductive material that does not cause dispersion problems may be used.
[0127] In one embodiment of the present application, the surface-shaped conductive material has a BET specific surface area of about 0.25 m 2 / g can be more than that.
[0128] In another embodiment, the surface-shaped conductive material has a BET surface area of about 1 m 2 / g or more than 500m 2 / g or less, for example, about 5m 2 / g or more than 300m 2 / g or less, or 5m 2 / g or more than 250m 2 / g can be less.
[0129] The planar conductive material according to the present application may be a planar conductive material with a high specific surface area; or a planar conductive material with a low specific surface area.
[0130] In another embodiment, the surface-shaped conductive material is a high surface area surface-shaped conductive material, and has a BET surface area of about 50 m 2 / g or more than 500m 2 / g or less, for example, about 80m 2 / g or more than 300m 2 / g or less, or 100m 2 / g or more than 300m 2 / g can satisfy the range below.
[0131] In another embodiment, the surface-shaped conductive material is a low surface area surface-shaped conductive material, and has a BET surface area of about 1 m 2 / g or more than 40m 2 / g or less, for example, about 5m 2 / g or more than 30m 2 / g or less, or 5m 2 / g or more than 25m 2 / g can satisfy the range below.
[0132] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundle-type carbon nanotubes. The bundle-type carbon nanotubes may include a plurality of carbon nanotube units. For example, the term "bundle type" herein, unless otherwise stated, refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged in a substantially identical orientation with their longitudinal axes aligned in parallel or entangled. The carbon nanotube units have a cylindrical graphite sheet with a nano-sized diameter and an sp2 bonding structure. At this time, the graphite sheets may exhibit conductor or semiconductor properties depending on the curling angle and structure. The above bundled carbon nanotubes can be uniformly dispersed during the manufacture of a cathode compared to entangled type carbon nanotubes, and can smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.
[0133] In one embodiment of the present application, a negative electrode composition is provided in which the negative electrode conductive material is present in an amount of about 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode composition.
[0134] In another embodiment, the negative electrode conductive material may be included in an amount of about 0.1 parts by weight or more and 40 parts by weight or less, for example, about 0.2 parts by weight or more and 30 parts by weight or less, or about 0.4 parts by weight or more and 25 parts by weight or less, or about 0.4 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of the negative electrode composition.
[0135] In one embodiment of the present application, a negative electrode composition is provided, wherein the negative electrode conductive material includes a planar conductive material and a linear conductive material.
[0136] In one embodiment of the present application, the negative electrode composition is provided, wherein the negative electrode conductive material comprises about 80 parts by weight or more and 99.9 parts by weight or less of the planar conductive material and about 0.1 parts by weight or more and 20 parts by weight or less of the linear conductive material, based on 100 parts by weight of the negative electrode conductive material.
[0137] In another embodiment, the negative electrode conductive material may include about 80 parts by weight or more and 99.9 parts by weight or less of the planar conductive material, for example, about 85 parts by weight or more to 99.9 parts by weight or less, or 95 parts by weight or more to 98 parts by weight or less, based on 100 parts by weight of the negative electrode conductive material.
[0138] In another embodiment, the cathode conductive material may include about 0.1 to 20 parts by weight of the linear conductive material, for example, 0.1 to 15 parts by weight, or 0.2 to 5 parts by weight, based on 100 parts by weight of the cathode conductive material.
[0139] In one embodiment of the present application, since the negative electrode conductive material includes a planar conductive material and a linear conductive material and satisfies the above composition and ratio, respectively, it does not have a significant effect on the life characteristics of an existing lithium secondary battery. For example, when a planar conductive material and a linear conductive material are included, the number of points at which charging and discharging are possible increases, thereby improving the output characteristics of the secondary battery at a high C-rate and reducing the amount of high-temperature gas generated.
[0140] In one embodiment of the present application, the negative electrode conductive material may be composed of a linear conductive material. When a linear conductive material is used alone, the electrode tortuosity, which is a problem with silicon-based negative electrodes, can be simplified, thereby improving the electrode structure and thereby reducing the resistance to lithium ion movement within the electrode.
[0141] In one embodiment of the present application, when the negative electrode conductive material comprises a linear conductive material alone, the negative electrode conductive material may comprise about 0.1 parts by weight or more and 5 parts by weight or less, for example, about 0.2 parts by weight or more and 3 parts by weight or less, or about 0.4 parts by weight or more and 1 part by weight or less, based on 100 parts by weight of the negative electrode composition.
[0142] The negative electrode conductive material according to the present application has a substantially separate composition from the positive electrode conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present application controls the contact between silicon-based active materials, which undergo a significant volume expansion of the electrode due to charging and discharging, and the positive electrode conductive material acts as a buffer when rolled and provides some conductivity, and thus is substantially different in composition and function from the negative electrode conductive material of the present invention.
[0143] In addition, the negative electrode conductive material according to the present application is applied to a silicon-based active material and has a substantially different composition from the conductive material applied to a graphite-based active material. For example, the conductive material used in an electrode having a graphite-based active material simply has smaller particles than the active material, and thus has the characteristics of improving output characteristics and imparting some conductivity, and is substantially different in composition and function from the negative electrode conductive material applied together with a silicon-based active material, as in the present invention.
[0144] In one embodiment of the present application, the planar conductive material used as the aforementioned negative electrode conductive material has a structure and function different from those of carbon-based active materials typically used as negative electrode active materials. For example, the carbon-based active material used as the negative electrode active material may be artificial graphite or natural graphite, and refers to a material processed into a spherical or dot-shaped form to facilitate the storage and release of lithium ions.
[0145] Meanwhile, the planar conductive material used as the negative electrode conductor is a material in the form of a plane or plate, and can be expressed as plate-shaped graphite. For example, it refers to a material included to maintain a conductive path within the negative electrode active material layer, not to store and release lithium, but to secure a conductive path in the form of a plane within the negative electrode active material layer.
[0146] That is, in the present application, the use of plate-shaped graphite as a conductive material means that it is processed into a planar or plate-shaped form and used as a material to secure a conductive path, rather than to store or release lithium. In this case, the included negative electrode active material has high capacity characteristics for lithium storage and release, and can store and release all lithium ions delivered from the positive electrode.
[0147] Meanwhile, in the present application, the use of a carbon-based active material as an active material means that it is processed into a dot or spherical shape and used as a material that plays a role in storing or releasing lithium.
[0148] For example, in one embodiment of the present application, the carbon-based active material, artificial graphite or natural graphite, is in a dot-like shape and has a BET specific surface area of 0.1 m 2 / g or more than 4.5 m 2 / g or less can be satisfied. In addition, the plate-shaped graphite, which is a planar conductive material, has a BET surface area of about 5 m in the form of a planar surface. 2 / g can be more than that.
[0149] In one embodiment of the present application, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and a material in which hydrogens thereof are substituted with Li, Na, Ca, or the like, and may also include various copolymers thereof.
[0150] The negative electrode binder according to one embodiment of the present application serves to hold the active material and conductive material in order to prevent distortion and structural deformation of the negative electrode structure when the volume of the silicon-based active material expands and relaxes. Any binder can be applied as long as it satisfies the above-mentioned role, and for example, an aqueous binder or a PAM-based binder can be used.
[0151] In one embodiment of the present application, the negative electrode binder may be about 30 parts by weight or less, for example, about 25 parts by weight or less, or about 20 parts by weight or less, or about 5 parts by weight or more, or about 10 parts by weight or more, based on 100 parts by weight of the negative electrode composition.
[0152] One embodiment of the present application provides a method for producing an anode active material, including a step of rapidly cooling metal silicon to form a silicon precursor; and a step of pulverizing the silicon precursor to form a silicon-based active material; wherein the step of rapidly cooling includes melt spinning, suction casting, or injection casting.
[0153] As described above, rather than directly crushing the metal silicon itself, the silicon precursor is formed by controlling the crystal grain size through a rapid cooling process and crushing the precursor to manufacture a silicon-based active material.
[0154] That is, when casting molten silicon, the shorter the solidification time (Ts), the faster the cooling rate, and as the plate thickness of the silicon precursor satisfies the range of the above equation 3 (e.g., approximately 10 μm-2 mm), the shorter the solidification time, so that the cooling rate can be quickly controlled. In addition, since the cooling rate is quickly controlled as described above, the time for grain growth is short, so that the above-mentioned grain size (e.g., approximately 2 nm-11 μm) can be satisfied.
[0155] In one embodiment of the present application, a method for producing a negative electrode active material is provided, which further includes a step of heating the metal silicon in an induction furnace before the step of rapidly cooling the metal silicon to form a silicon precursor.
[0156] As described above, the metal silicon is heated in an induction furnace to a molten state, and then rapidly cooled. The rapid cooling includes melt spinning, suction casting, or injection casting. Any method capable of rapidly cooling the molten metal silicon to form a plate-shaped silicon precursor in accordance with the purpose of the present invention can be applied.
[0157] Generally, melt spinning can refer to a process of rapidly cooling molten material by spraying it onto a rotating copper wheel. Suction casting can also refer to a process of casting molten material by sucking it out from under a mold using a vacuum, and injection casting can refer to a process of casting molten material by injecting it into a mold using high-pressure gas.
[0158] For the rapid cooling step described above, the melt spinning, suction casting or injection casting processes are each different and diverse, making it difficult to generally specify the conditions, but as a result, all silicon precursors can be manufactured in the form of plates.
[0159] In the present application, the cooling rate control during rapid cooling varies for each process, but in general, in melt spinning, the faster the wheel rotation speed, the faster the cooling rate, and in the case of suction casting or injection casting, the thinner the mold, the faster the cooling rate. In addition, the cooling rate can be controlled through external temperature control, such as by flowing cooling water into the mold or cooling the wheel or mold with liquid nitrogen, etc. Meanwhile, rapid cooling is a type of cooling method that rapidly cools MG silicon to form a plate-shaped silicon precursor. The rapid cooling is a cooling method that suppresses reactions such as phase transformation or grain coarsening that occur in an equilibrium state, and refers to a type of non-equilibrium solidification. For example, when metal silicon is rapidly cooled using melt spinning, the cooling rate can be controlled by controlling the rotation speed of the Cu wheel, and it takes approximately less than 1 second to cool from approximately 1,500°C, which is a temperature in a molten state, to approximately 25°C, which is a room temperature.
[0160] In one embodiment of the present application, a method for producing a negative electrode active material is provided, wherein after the step of rapidly cooling metal silicon to form a silicon precursor, the silicon precursor satisfies the above-described equations 3 and 4.
[0161] A silicon precursor is formed through a rapid cooling process, which may mean that equations 3 and 4 are satisfied.
[0162] In the present application, a method for producing a negative electrode active material is provided, comprising the steps of: pulverizing the silicon precursor to form a silicon-based active material; and then, the silicon-based active material satisfies the above-described formulas 1 and 2.
[0163] A silicon-based active material satisfying the ranges of the above-described formulas 1 and 2 can be manufactured through a process of forming a silicon precursor satisfying specific formulas 3 and 4 through a rapid cooling process and pulverizing the same.
[0164] In one embodiment of the present application, the pulverizing process may include, but is not limited to, one or more processes selected from the group consisting of a ball mill, a pin mill, a disk mill, and a jet mill, and any pulverizing process that can pulverize a plate-shaped metal silicon precursor to produce a silicon-based active material satisfying the ranges of the above-described formulas 1 and 2 may be applied.
[0165] Through the above-described grinding process, a silicon-based active material satisfying the ranges of the above-described formulas 1 and 2 can be manufactured.
[0166] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, including: a negative electrode current collector layer; and a negative electrode active material layer including a negative electrode composition according to the present application or a cured product thereof formed on one or both sides of the negative electrode current collector layer.
[0167] Fig. 3 is a diagram showing a laminated structure of an anode for a lithium secondary battery according to one embodiment of the present application. For example, a lithium secondary battery anode (100) including an anode active material layer (20) on one surface of an anode current collector layer (10) can be confirmed, and although Fig. 3 shows that the anode active material layer (20) is formed on one surface, it can be included on both surfaces of the anode current collector layer.
[0168] In one embodiment of the present application, the negative electrode for the lithium secondary battery can be formed by applying and drying a negative electrode slurry containing the negative electrode composition to one or both sides of a negative electrode current collector layer.
[0169] At this time, the cathode slurry may include the above-described cathode composition; and a slurry solvent.
[0170] In one embodiment of the present application, the solid content of the cathode slurry can satisfy a range of about 5% to 40%.
[0171] In another embodiment, the solid content of the cathode slurry can satisfy a range of about 5% to 40%, for example, about 7% to 35%, or about 10% to 30%.
[0172] The solid content of the above cathode slurry may mean the content of the cathode composition included in the cathode slurry, and may mean the content of the cathode composition based on 100 parts by weight of the cathode slurry.
[0173] When the solid content of the above negative electrode slurry satisfies the above range, the viscosity is appropriate when forming the negative electrode active material layer, so that the particle agglomeration phenomenon of the negative electrode composition is minimized, thereby efficiently forming the negative electrode active material layer.
[0174] In one embodiment of the present application, the slurry solvent can be used without limitation as long as it can dissolve the negative electrode composition, and for example, water or NMP can be used.
[0175] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of about 1 μm to 100 μm. The negative electrode current collector layer is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the bonding strength of the negative electrode active material can be strengthened by forming fine unevenness on the surface, and can be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc.
[0176] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, wherein the thickness of the negative electrode current collector layer is about 1 μm or more and 100 μm or less, and the thickness of the negative electrode active material layer is about 5 μm or more and 500 μm or less.
[0177] However, the thickness can be varied depending on the type and purpose of the cathode used.
[0178] In one embodiment of the present application, the porosity of the negative electrode active material layer can satisfy a range of about 10% or more and 60% or less.
[0179] In another embodiment, the porosity of the negative electrode active material layer can satisfy a range of about 10% to 60%, for example, about 20% to 50%, or about 30% to 45%.
[0180] The above porosity varies depending on the composition and content of the silicon-based active material, conductive material, and binder included in the negative electrode active material layer. For example, the above range is satisfied by including a specific composition and content of the silicon-based active material and conductive material according to the present application, and accordingly, the electrical conductivity and resistance of the electrode have an appropriate range.
[0181] In one embodiment of the present application, a lithium secondary battery is provided, including: a positive electrode; an anode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.
[0182] FIG. 4 is a diagram showing a laminated structure of a lithium secondary battery according to one embodiment of the present application. For example, a lithium secondary battery negative electrode (100) including a negative electrode active material layer (20) on one surface of a negative electrode current collector layer (10) can be confirmed, and a lithium secondary battery positive electrode (200) including a positive electrode active material layer (40) on one surface of a positive electrode current collector layer (50) can be confirmed, and it is shown that the lithium secondary battery negative electrode (100) and the lithium secondary battery positive electrode (200) are formed in a laminated structure with a separator (30) interposed therebetween.
[0183] A secondary battery according to one embodiment of the present specification may include the negative electrode for a lithium secondary battery described above. For example, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the negative electrode is identical to the negative electrode described above. Since the negative electrode has been described above, a detailed description thereof will be omitted.
[0184] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and including the positive electrode active material.
[0185] In the above positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 ㎛, and fine unevenness may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0186] The above positive electrode active material may be a commonly used positive electrode active material. For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound having the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4(0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein, M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3Lithium manganese composite oxide represented by O2 (wherein, M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein, M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn2O4, etc., in which a part of Li in the chemical formula is replaced with an alkaline earth metal ion, but is not limited thereto. The positive electrode may be Li-metal.
[0187] The above-described positive electrode active material layer may include a positive electrode conductive material and a positive electrode binder together with the positive electrode active material described above.
[0188] The above-mentioned positive electrode conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.
[0189] In addition, the positive electrode binder plays a role of improving the adhesion between positive electrode active material particles and the adhesiveness between the positive electrode active material and the positive electrode current collector. Examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof.
[0190] The separator above separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in secondary batteries can be used without any particular restrictions. For example, any separator that has low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity can be used. For example, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof can be used. In addition, a conventional porous non-woven fabric, for example, a non-woven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.
[0191] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0192] For example, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0193] As the above non-aqueous organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethylsulfoxide, 1,3-dioxolan, formamide, dimethylformamide, dioxolan, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolan derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used.
[0194] Among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants and thus can be used because they easily dissociate lithium salts. By mixing and using low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate in an appropriate ratio with these cyclic carbonates, an electrolyte with high electrical conductivity can be produced and used.
[0195] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, for example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 -, BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.
[0196] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as, for example, a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, a cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery.
[0197] One embodiment of the present invention provides a battery module including the secondary battery as a unit cell and a battery pack including the same. The battery module and battery pack include the secondary battery having high capacity, high rate characteristics, and cycle characteristics, and thus can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0198] Hereinafter, examples are presented to help understand the present invention, but the examples are only illustrative of the present disclosure, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended patent claims.
[0199] <Manufacturing Example>
[0200] <Manufacturing of silicon precursors>
[0201] <Example 1>
[0202] MG silicon was placed in a graphite crucible and melted using an induction furnace, and a plate-shaped silicon precursor was manufactured through a melt spinning process.
[0203] For example, by applying a current of 10 kA to a copper coil, molten silicon at 2000°C was produced, and the molten silicon was injected at a pressure of 1.2 kPa onto a copper wheel with a diameter of 25 cm rotating at a speed of 3000 rpm to obtain a plate-shaped silicon precursor. At this time, the plate thickness of the silicon precursor was approximately 20 μm, and the crystal grain size was approximately 50 nm, which can be seen to satisfy the aforementioned equations 3 and 4, respectively.
[0204] Silicon precursors of Examples 2, 3 and Comparative Example 3 were manufactured in the same manner as in Example 1, except that the rotation speed was changed to the conditions in Table 1 below to control the cooling rate during rapid cooling by melt spinning in Example 1.
[0205] Rapid cooling rotation speed pressure type 3 type 4 Example 1 Melt spinning 3000 rpm 1.2 kPa 20 μm 50 nm Example 2 Melt spinning 4000 rpm 1.2 kPa 15 μm 40 nm Example 3 Melt spinning 1000 rpm 1.2 kPa 100 μm 300 nm Comparative example 1 XXXXX Comparative example 2 XXXXX Comparative example 3 Melt spinning 100 rpm 1.2 kPa 3 mm 2.5 μm
[0206] In the case of the above Example 2, when the rotation speed of the copper wheel in the melt spinning process is 4000 rpm, which is higher than 3000 rpm in Example 1, the plate thickness of the silicon-based precursor is about 15 μm, and the crystal grain size is about 40 nm, which can be seen to satisfy the above-described Equations 3 and 4, respectively. In addition, in the case of Example 3, when the rotation speed of the copper wheel in the melt spinning process is 1000 rpm, in this case as well, the plate thickness of the silicon-based precursor is about 100 μm, and the crystal grain size is about 300 nm, which can be seen to satisfy the above-described Equations 3 and 4, respectively.
[0207] In the case of the above Comparative Examples 1 and 2, the MG silicon was put into a graphite crucible and melted using an induction furnace, and instead of manufacturing a plate-shaped silicon precursor through a melt spinning process, the MG silicon itself was used as is and the milling process described below was performed. Meanwhile, in the case of Comparative Example 3, when the rotation speed of the copper wheel in the melt spinning process was 100 rpm, the plate thickness of the silicon precursor was about 3 mm, which was thicker than the examples of the present invention, and the crystal grain size was 2.5 μm, which was larger than the examples of the present invention, and it can be seen that the above-described equations 3 and 4 were not satisfied.
[0208] <Example 4>
[0209] In Example 4, unlike Examples 1, 2, and 3 described above, MG silicon was made into a molten state through arc melting, and then a plate-shaped silicon precursor was manufactured through a suction casting process.
[0210] For example, vacuum 10 -6 A high-purity argon atmosphere was created by filling the inside of the torr chamber with argon at a pressure of 0.5 kPa, and silicon in a molten state of 2000°C was manufactured using arc plasma. Afterwards, the vacuum level at the bottom of the mold was increased to 10 -5 After maintaining the pressure above 10 torr, the valve between the bottom of the mold and the chamber was opened to suck the molten silicon into the mold, thereby manufacturing a plate-shaped silicon precursor. A mold measuring 0.5 mm in thickness, 10 mm in width, and 50 mm in length was used, and the crystal grain size was 50 nm.
[0211] A silicon precursor was manufactured in the same manner as in Example 4, except that the thickness of the mold, which determines the cooling rate during rapid cooling by suction casting in Example 4, was changed to the conditions in Table 2 below.
[0212] Rapid cooling plate mold thickness formula 3 formula 4 (nm) Example 4 Suction casting 0.5 mm 500 μm 400 nm Example 5 Suction casting 0.4 mm 400 μm 500 nm Example 6 Suction casting 1 mm 100 μm 1000 nm Comparative example 4 XXXX Comparative example 5 XXXX Comparative example 6 Suction casting 3 mm 3 mm 2.5 μm
[0213] For Examples 4, 5, and 6, it can be seen that the plate thicknesses of the silicon precursor are 500 μm, 400 μm, and 100 μm, respectively, satisfying the condition of Equation 3, and the crystal grain sizes within the silicon precursor are 400 nm, 500 nm, and 1,000 nm, respectively, satisfying Equation 4.
[0214] In the case of the above comparative examples 4 and 5, rather than making the MG silicon into a molten state through arc melting and then manufacturing a plate-shaped silicon precursor through a suction casting process, the MG silicon itself was used as is and the milling process described below was performed.
[0215] Meanwhile, in the case of comparative example 6 where the plate mold thickness is 3 mm, the plate thickness of the silicon precursor is 3 mm, which does not satisfy the condition of Equation 3, and the crystal grain size within the silicon precursor is 2.510 μm, which does not satisfy Equation 4.
[0216] As confirmed from the values in Tables 1 and 2 above, it was confirmed that the melt spinning process is generally easier to manufacture a thinner silicon precursor than the suction casting process.
[0217] <Manufacturing of silicon-based active materials>
[0218] For the silicon precursor manufactured above, a silicon active material was manufactured through ball milling.
[0219] For example, a wet grinding method using n-hexane as a medium was used, and zirconia (ZrO2) was used as the ball. At this time, the mass ratio of the silicon precursor and the ball was approximately 1:40, and the grinding was performed for 30 minutes. The particle size of the manufactured negative active material was 5 μm, and the crystal grain size was 50 nm, satisfying Equations 1 and 2, respectively.
[0220] The silicon precursors of the above-described examples and comparative examples were pulverized in the same manner as above, and the results are shown in Table 3.
[0221] Equation 1 Equation 2 Elevation boundary ratio Example 15 μm 50 nm 45% Example 25 μm 250 nm 34% Example 33 μm 40 nm 55% Example 43 μm 200 nm 38% Example 57 μm 100 nm 40% Example 67 μm 500 nm 30% Comparative Example 15 μm 5 μm - Comparative Example 23 μm 3 μm - Comparative Example 37 μm 7 μm - Comparative Example 411 μm 1.2 μm 18% Comparative Example 513 μm 1.5 μm 15% Comparative Example 615 μm 2.0 μm 10%
[0222] According to Table 3, it can be seen that the particle size (D50) of the silicon-based active material of all Examples 1-6 satisfies Equation 1, while Comparative Examples 5 and 6 do not satisfy Equation 1. In addition, it can be seen that the crystal grain size of the silicon-based active material of all Examples 1-6 satisfies Equation 2, but none of Comparative Examples 1-6 satisfies Equation 2. In addition, it can be seen that all of Examples 1-6 have a high-angle boundary ratio of 30% or more, but in the case of Comparative Examples 4-6, the high-angle boundary ratio is less than 30%.
[0223] <Manufacturing of the cathode>
[0224] According to one embodiment, a negative electrode slurry was prepared by adding a negative electrode active material including the silicon-based active material of Table 3, a first conductive material, a second conductive material, and polyacrylamide as a binder in a weight ratio of 80:9.6:0.4:10 to distilled water as a solvent for forming a negative electrode slurry (solid content concentration 25 wt%).
[0225] For example, the first challenge material is a plate-shaped graphite (specific surface area: 17 m 2 / g, average particle diameter (D50): about 3.5 μm), and the second conductive material was SWCNT.
[0226] As a mixing method, the first and second conductive materials, binder and water were dispersed using a homogenous mixer at about 2500 rpm for 30 minutes, and then the silicon-based active material was added and dispersed at about 2500 rpm for 30 minutes to produce a negative electrode slurry.
[0227] The negative electrode slurry is applied to both sides of a copper current collector (thickness: 8㎛) as a negative electrode current collector layer at a concentration of about 85mg / 25cm. 2 The coating was carried out with a loading amount of , rolled (roll pressed), and dried in a vacuum oven at 130°C for 10 hours to form a negative electrode active material layer (thickness: 33 μm), which was used as a negative electrode (thickness of negative electrode: 41 μm, porosity of negative electrode: 40.0%).
[0228] <Manufacturing of secondary batteries>
[0229] According to one embodiment, LiNi as a positive electrode active material 0.6 Co 0.2 Mn 0.2 O2 (average particle size (D50): 15㎛), carbon black (product name: Super C65, manufacturer: Timcal) as a conductive agent, and polyvinylidene fluoride (PVdF) as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent for forming a cathode slurry at a weight ratio of about 97:1.5:1.5 to prepare a cathode slurry (solid content concentration: about 78 wt%).
[0230] The positive electrode slurry is applied to both sides of an aluminum current collector (thickness: 12㎛) as a positive electrode collector at a density of about 537mg / 25cm. 2 A positive electrode was manufactured by coating with a loading amount, rolling (roll pressing), and drying in a vacuum oven at 130°C for 10 hours to form a positive electrode active material layer (thickness: 65 μm) (positive electrode thickness: approximately 77 μm, porosity: approximately 26%).
[0231] A lithium secondary battery was manufactured by interposing a polyethylene separator between the positive electrode and the negative electrode of the above examples and comparative examples and injecting an electrolyte.
[0232] The above electrolyte was an organic solvent containing fluoroethylene carbonate (FEC) and diethyl carbonate (DMC) mixed in a volume ratio of 10:90, vinylene carbonate added at approximately 3 wt% based on the total weight of the electrolyte, and LiPF6 added as a lithium salt at a concentration of approximately 1 M.
[0233] <Experimental Example>
[0234] Experimental Example 1: Monocell Life Performance Results
[0235] The secondary batteries containing the negative electrodes manufactured in the above examples and comparative examples were subjected to a life evaluation using an electrochemical charger / discharger, and the capacity retention rate was evaluated. The secondary batteries were subjected to an in-situ cycle test at 4.2-3.0 V 1C / 0.5C, and the capacity retention rate was measured by charging / discharging at 0.33C / 0.33C (4.2-3.0 V) every 50 cycles during the test.
[0236] Life retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at 1st cycle)} Х 100
[0237] Lifespan after 200 cycles (%) Example 191 Example 288 Example 389 Example 486 Example 587 Example 684 Comparative Example 172 Comparative Example 270 Comparative Example 369 Comparative Example 468 Comparative Example 566 Comparative Example 665
[0238] As can be seen in Table 4, when the capacity retention rate according to the cycle of Examples 1 to 6 and Comparative Examples 1 to 6 to which the present invention was applied was confirmed, it was confirmed that the capacity retention rate of the Comparative Examples to which the present invention was not applied was lower than that of the Examples. This corresponds to the result that when the crystal grain size of the silicon-based active material satisfies the range according to the present invention, the insertion and de-insertion of lithium during charge and discharge can react uniformly, and the stress applied to the silicon-based active material can be reduced to alleviate the breakage of the particles, thereby improving the life retention rate of the electrode.
[0239] Experimental Example 2: Changes in Monocell Resistance
[0240] In the above experimental example 1, the capacity retention rate was measured by performing 0.33C / 0.33C charge / discharge (4.2-3.0V) every 50 cycles during the test, and then the resistance was measured by discharging with 2.5C pulse at SOC50 to compare and analyze the resistance increase rate.
[0241] For the above resistance increase rate measurement evaluation, data at 200 cycles were calculated, and the results were as shown in Table 5 below.
[0242] Resistance increase rate (%) after 200 cycles Example 116 Example 219 Example 318 Example 422 Example 517 Example 625 Comparative Example 148 Comparative Example 250 Comparative Example 351 Comparative Example 454 Comparative Example 556 Comparative Example 657
[0243] According to Tables 4 and 5, it was confirmed that the life characteristics and resistance change of the battery using the silicon manufactured in Examples 1 to 6 as the negative electrode active material were excellent. In the case of the negative electrode active material according to one embodiment of the present invention, unlike the existing pulverization processing method, a plate-shaped silicon precursor was formed by prioritizing a rapid cooling process prior to MG-Si pulverization, and the crystal grain size was optimized by controlling the cooling rate, and as in the example, a silicon-based active material satisfying nano-sized crystal grains and a specific high-angle boundary ratio can be secured by pulverizing a plate-shaped silicon precursor having nano-sized crystal grains, and it was confirmed that when manufacturing an negative electrode using the same, the cycle capacity retention rate and the initial capacity efficiency were increased.
[0244] For reference, in the case of Comparative Examples 1 to 3, the particle size (Formula 1) and the crystal grain size (Formula 2) of the silicon-based active material are the same, that is, there is no grain boundary inside the particle of the silicon-based active material in the form of a single crystal, and thus, a high-angle boundary cannot exist. In the case of Comparative Examples 4 to 6, the value of Formula 1 is larger than the value of Formula 2, so that a grain boundary exists inside the particle, but the high-angle boundary ratio does not fall within the scope of the present application. In the case of Examples 1 to 6 of the present application, a high-angle grain boundary (HAGB) with high grain boundary energy was formed at the ratio of Table 3 by manufacturing using the above-described manufacturing method, and in the case of a high-angle grain boundary, lithium ions are easily diffused compared to a low-angle grain boundary (LAGB), so it was confirmed that it was superior to the Comparative Example in terms of life characteristics and resistance increase rate.
[0245] Although the present invention has been described above with reference to embodiments thereof, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes may be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. A negative electrode active material containing a silicon-based active material, The above silicon-based active material includes silicon-based crystal grains, The ratio of high angle grain boundaries within the above silicon-based crystal grains is 30% or more, The above silicon-based active material is a negative electrode active material having a chemical composition satisfying the following formulas 1 and 2: [Formula 1] 1 μm ≤ particle size (D50) of silicon-based active material ≤ 10 μm [Formula 2] 2 nm ≤ crystal grain size of silicon-based active material ≤ 1 μm 2. In claim 1, The above silicon-based active material comprises a pulverized product of a silicon precursor, The above silicon precursor is a negative electrode active material having a chemical composition satisfying the following formulas 3 and 4: [Formula 3] 10 μm ≤ silicon precursor plate thickness ≤ 2 mm [Formula 4] 2 nm ≤ crystal grain size in silicon precursor ≤ 1 μm 3. In claim 1, A negative active material having an average grain misorientation angle of the above silicon-based crystal grains of 5° or more.
4. In claim 1, the silicon-based active material is SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함하는 것인 음극 활물질.
5. A silicon precursor having a chemical composition satisfying the following equations 3 and 4: [Formula 3] 10 μm ≤ silicon precursor plate thickness ≤ 2 mm [Formula 4] 2 nm ≤ crystal grain size in silicon precursor ≤ 1 μm 6. A step of forming a silicon precursor by performing a rapid cooling process on metal silicon; and A step of forming a silicon-based active material by crushing the silicon precursor; A method for manufacturing a negative electrode active material including: A method for manufacturing a negative electrode active material, wherein the above rapid cooling step is performed by any one of melt spinning, suction casting, or injection casting.
7. In claim 6, Before the rapid cooling step of metal silicon, A method for producing a negative active material, further comprising a step of heating the metal silicon in an induction furnace.
8. In claim 6, After the step of rapidly cooling the metal silicon to form a silicon precursor, A method for manufacturing a negative electrode active material, wherein the silicon precursor comprises a chemical composition satisfying the following formulas 3 and 4: [Formula 3] 10 μm ≤ silicon precursor plate thickness ≤ 2 mm [Formula 4] 2 nm ≤ crystal grain size in silicon precursor ≤ 1 μm 9. In claim 6, A step of forming a silicon-based active material by crushing the above silicon precursor; thereafter, A method for manufacturing a negative electrode active material, wherein the silicon-based active material comprises a chemical composition satisfying the following formulas 1 and 2: [Formula 1] 1 μm ≤ particle size (D50) of silicon-based active material ≤ 10 μm [Formula 2] 2 nm ≤ crystal grain size of silicon-based active material ≤ 100 nm 10. A negative electrode composition comprising a negative electrode active material according to any one of claims 1 to 4; a negative electrode conductive material; and a negative electrode binder.
11. In claim 10, A negative electrode composition in which the negative electrode active material is at least 40 parts by weight based on 100 parts by weight of the negative electrode composition.
12. In claim 10, A cathode composition comprising the above cathode conductive material, a planar conductive material, and a linear conductive material.
13. A negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, A negative electrode for a lithium secondary battery, wherein the negative electrode active material layer comprises the negative electrode composition according to claim 10 or a cured product thereof.
14. In claim 13, The thickness of the above negative electrode current collector layer is 1 μm or more and 100 μm or less, A negative electrode for a lithium secondary battery, wherein the thickness of the negative electrode active material layer is 5 μm or more and 500 μm or less.
15. Bipolar; A negative electrode for a lithium secondary battery according to claim 13; A separator provided between the anode and the cathode; and A lithium secondary battery comprising an electrolyte.
16. Step of manufacturing metal silicon in a molten state; A step of forming a plate-shaped metal silicon precursor by performing a rapid cooling process on the molten metal silicon; A step of determining whether the plate thickness of the formed metal silicon precursor is 10 μm or more and 2 mm or less and whether the size of crystal grains in the metal silicon precursor is 2 nm or more and 1 μm or less; A step of producing a silicon-based active material by crushing the metal silicon precursor when the plate thickness and crystal grain size of the metal silicon precursor are determined to be 10 μm or more and 2 mm or less and 2 nm or more and 1 μm or less, respectively; A step of determining whether the particle size (D50) of the manufactured silicon-based active material is 1 μm or more and 10 μm or less, and whether the crystal grain size of the manufactured silicon-based active material is 2 nm or more and 1 μm or less; A method for manufacturing an anode active material, comprising a step of classifying the silicon-based active material as an active material for manufacturing an anode of a lithium secondary battery, when the particle size (D50) and crystal grain size of the silicon-based active material manufactured above are respectively 1 μm or more and 10 μm or less and 2 nm or more and 1 μm or less.
17. In paragraph 16, A method for manufacturing a negative electrode active material, wherein the above rapid cooling step is performed by any one of melt spinning, suction casting, or injection casting.
Citation Information
Patent Citations
Anode for lithium ion battery
JP2009080971A
Preparation method of amorphous silicon powder body, amorphous silicon powder body and lithium ion battery
CN107572529A
Negative active material, lithium battery including the material, and method for manufacturing the material
KR101749506B1
Negative electrode active material for secondary battery and manufacturing method thereof
KR1020150018337A
Manufcturing method for amorphous silicon composite and manufacturing apparatus for amorphous silicon composite
KR102136820B1