Self-supporting ceramic separator for electrochemical device and electrochemical device comprising same

The self-supporting ceramic separator, composed of plate-shaped and zeolite-based inorganic particles, addresses the heat-induced issues of conventional separators by forming a dense structure that prevents transition metal elution and enhances battery stability and life.

WO2024219773A1PCT designated stage expired Publication Date: 2024-10-24LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005029
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional electrochemical device separators, particularly those using polyolefin resin, suffer from heat-induced shrinkage leading to electrical short circuits and reduced battery life due to thermal contraction, and lack sufficient heat resistance and durability.

Method used

A self-supporting ceramic separator is developed without a porous polymer substrate, utilizing plate-shaped first inorganic particles and zeolite-based second inorganic particles with specific pore sizes and a polymer binder to form a dense laminated structure, enhancing heat resistance and preventing transition metal elution from the anode to the cathode.

Benefits of technology

The solution effectively suppresses thermal contraction, improves battery stability, and extends battery life by preventing electrical short circuits and enhancing gas and transition metal adsorption, thereby maintaining battery performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005029_24102024_PF_FP_ABST
    Figure KR2024005029_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a self-supporting ceramic separator for an electrochemical device and an electrochemical device comprising same and, more specifically, to a self-supporting ceramic separator for an electrochemical device and an electrochemical device comprising same, wherein the self-supporting ceramic separator for an electrochemical device appropriately controls the quantity and arrangement of first inorganic particles which are flat and second inorganic particles which are a zeolite-based inorganic material so as to improve the heat resistance of the separator, prevents an electrical short circuit between electrodes so as to improve the safety of a battery, and exhibits excellent cell life characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Self-supporting ceramic separator for electrochemical devices and electrochemical devices including the same

[0001] This invention claims the benefit of patent application No. 10-2023-0051554 filed with the Korean Intellectual Property Office on April 19, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a self-supporting ceramic separator for an electrochemical device and an electrochemical device including the same, and more particularly, to a self-supporting ceramic separator for an electrochemical device including first inorganic particles and second inorganic particles, which has improved heat resistance and exhibits high cell life characteristics, and an electrochemical device including the same.

[0003] Among the components of electrochemical devices, the separator comprises a porous polymer substrate located between the anode and cathode. It isolates the anode and cathode, prevents electrical short-circuiting between the two electrodes, and allows the passage of electrolytes and ions. While the separator itself does not participate in electrochemical reactions, its physical properties, such as wettability with electrolyte, degree of porosity, and thermal shrinkage, influence the performance and safety of the electrochemical device.

[0004] Accordingly, various methods have been attempted to enhance the physical properties of membranes by adding a coating layer to a porous polymer substrate and by adding various substances to the coating layer to change the properties of the coating layer. For example, inorganic substances may be added to the coating layer to enhance the mechanical strength of the membrane, or inorganic substances or hydrates may be added to the coating layer to enhance the flame retardancy and heat resistance of the polymer substrate.

[0005] The separator can be bonded to the electrode through a lamination process, and a polymer binder can be added to the coating layer composition of the separator to secure adhesion between the electrode and the separator.

[0006] Meanwhile, polyolefin resins, which are widely used as porous polymer substrates for electrochemical devices, have a problem in that they shrink when exposed to high temperatures, causing the positive and negative electrodes to come into contact, resulting in an electrical short circuit between the two electrodes, and causing heat generation, which in turn causes thermal runaway due to a decomposition reaction of the electrolyte and active material.

[0007] Therefore, research was needed on a self-supporting ceramic separator that could improve heat resistance and durability by appropriately combining inorganic particles without a polyolefin resin, which is a porous polymer substrate, and prevent electrical short-circuiting between electrodes, thereby improving the safety and lifespan of the battery.

[0008] The technical problem to be achieved by the present invention is to provide a self-supporting ceramic separator for an electrochemical device, which comprises first inorganic particles capable of forming a dense laminated structure in a plate shape to prevent transition metals eluted from an anode from moving to the cathode surface, and second inorganic particles capable of adsorbing gases and transition metals with a high specific surface area, but which has improved heat resistance and durability and can improve the stability and lifespan characteristics of a battery by having a configuration without a porous polymer substrate, and an electrochemical device including the same.

[0009] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.

[0010] One embodiment of the present invention provides a self-supporting ceramic separator for an electrochemical device, comprising first inorganic particles, second inorganic particles, and a polymer binder, wherein the first inorganic particles are plate-shaped, and the aspect ratio of the first inorganic particles is 10 or more and 300 or less.

[0011] According to one embodiment of the present invention, one side of the first inorganic particle and one side of the separation membrane may be arranged to face each other.

[0012] According to one embodiment of the present invention, the first layer may include a first layer having a weight greater than that of the second inorganic particles; and a second layer provided on one surface of the first layer, the second layer having a weight greater than that of the first inorganic particles.

[0013] According to one embodiment of the present invention, the opposite side of one side of the first layer may be provided to face the cathode.

[0014] According to one embodiment of the present invention, the first inorganic particle may include one selected from the group consisting of boron nitride, boehmite, kaolin, and combinations thereof.

[0015] According to one embodiment of the present invention, the second inorganic particle is a zeolite-based inorganic particle, the second inorganic particle includes pores having a diameter of 0.5 nm or more and 0.9 nm or less, and the pores of the second inorganic particle may be substituted with metal ions.

[0016] According to one embodiment of the present invention, the average particle diameter (D50) of the second inorganic particles may be 1 ㎛ or less.

[0017] According to one embodiment of the present invention, the thickness of the second layer may be 1 ㎛ or more and 3 ㎛ or less.

[0018] According to one embodiment of the present invention, the content of the first inorganic particles may be 5 parts by weight or more and 10 parts by weight or less with respect to 100 parts by weight of the coating layer.

[0019] According to one embodiment of the present invention, the polymer binder may be an acrylic binder, a polyvinylidene binder, or a combination thereof.

[0020] According to one embodiment of the present invention, the thickness of the separation membrane may be 7 ㎛ or more and 15 ㎛ or less.

[0021] According to one embodiment of the present invention, the air permeability of the separation membrane may be 170 sec / 100cc or less.

[0022] According to one embodiment of the present invention, the resistance of the separator may be 0.6 Ω or more and 1.2 Ω or less.

[0023] One embodiment of the present invention provides an electrochemical device including: an anode; a cathode; and a separator interposed between the anode and the cathode.

[0024] A self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention can suppress thermal shrinkage at high temperatures.

[0025] A self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention can improve the stability and life characteristics of a battery by preventing a transition metal eluted from an anode from moving to the cathode surface.

[0026] Figure 1 is a schematic diagram of a self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention.

[0027] Figure 2 is a schematic diagram of an electrochemical device according to one embodiment of the present invention.

[0028] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0029] In this specification, “A and / or B” means “A and B, or A or B.”

[0030] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, and it means that other components may be further placed.

[0031] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.

[0032] In this specification, the separator has a porous characteristic including a large number of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.

[0033] Hereinafter, the present invention will be described in more detail.

[0034]

[0035] One embodiment of the present invention provides a self-supporting ceramic separator for an electrochemical device, comprising first inorganic particles, second inorganic particles, and a polymer binder, wherein the first inorganic particles are plate-shaped, and the aspect ratio of the first inorganic particles is 10 or more and 300 or less.

[0036] A self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention can suppress thermal shrinkage at high temperatures. Furthermore, the self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention can prevent transition metals eluted from the anode from moving toward the cathode surface, thereby improving battery stability and battery life characteristics.

[0037] FIG. 1 is a schematic diagram of a self-supporting ceramic separator for an electrochemical device according to an embodiment of the present invention. Referring to FIG. 1, the self-supporting ceramic separator for an electrochemical device according to an embodiment of the present invention will be described in detail. FIG. 2 is a schematic diagram of an electrochemical device according to an embodiment of the present invention. Referring to FIG. 2, the electrochemical device according to an embodiment of the present invention will be described in detail.

[0038] According to one embodiment of the present invention, the self-supporting ceramic separator (100) for an electrochemical device does not include a porous polymer substrate. Since the self-supporting ceramic separator for an electrochemical device does not include the porous polymer substrate, the heat resistance of the separator is improved, and the shrinkage of the separator at high temperatures can be prevented, thereby preventing an electrical short circuit of the electrode.

[0039] According to one embodiment of the present invention, the separator (100) includes first inorganic particles, second inorganic particles, and a polymer binder. As described above, by including the first inorganic particles, second inorganic particles, and a polymer binder, the heat resistance of the separator can be improved, and the separator can be prevented from shrinking at high temperatures, resulting in an electrical short circuit of the electrode. Furthermore, pores can be formed within the separator.

[0040] According to one embodiment of the present invention, the separator (100) may include a plurality of pores. Specifically, the separator may be a porous separator including a plurality of pores within it. As described above, by including a plurality of pores, the separator can physically block the negative and positive electrodes while allowing lithium ions to pass through and current to flow.

[0041] According to one embodiment of the present invention, the separator (100) may be formed by inorganic particles being bound by a polymer binder and accumulated within the side. The pores within the separator may be derived from an interstitial volume, which is an empty space between the inorganic particles. Specifically, as described below, there may be differences in the structure and size of the pores depending on differences in the shape and combination of the first and second inorganic particles. Furthermore, depending on the differences in the structure and size of the pores, it is possible to prevent transition metals eluted from the anode from moving toward the cathode surface.

[0042] According to one embodiment of the present invention, the inorganic particles may include first inorganic particles and second inorganic particles. Non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), zeolite A, zeolite X, zeolite Y, etc., and may include one or more of these. Meanwhile, in addition, it may include plate-like inorganic particles of one or more of boron nitride (BN), boehmite, and kaolin.

[0043] According to one embodiment of the present invention, the first inorganic particles are plate-shaped. As described above, since the first inorganic particles are plate-shaped, a densely laminated structure can be formed, thereby improving the durability of the separation membrane.

[0044] According to one embodiment of the present invention, the aspect ratio of the first inorganic particle is 10 or more and 300 or less. As described above, the first inorganic particle may be a plate-shaped inorganic particle and the aspect ratio may be 10 or more and 300 or less. More specifically, the first inorganic particle may be a plate-shaped inorganic particle having an aspect ratio of 20 to 290, 30 to 280, 40 to 270, 50 to 260, 60 to 250, 70 to 240, 80 to 230, 90 to 220, 100 to 210, 110 to 200, 120 to 190, 130 to 180, 140 to 170, or 150 to 160. In the present specification, the aspect ratio may be defined as [length in the major axis direction] / [width in the direction orthogonal to the major axis direction] of the plate-shaped inorganic particle. By controlling the aspect ratio of the first inorganic particles within the above-described range, the thickness of the coating layer can be made thin, and a dense laminated structure can be formed, thereby improving the durability of the separation membrane.

[0045] According to one embodiment of the present invention, one side of the first inorganic particle may be arranged to face one side of the separator. As described above, the first inorganic particle is a plate-shaped inorganic particle and has an elongated shape in the longitudinal direction, so that the longitudinal direction is arranged to face one side of the separator, thereby forming a dense laminated structure, thereby improving the durability of the separator. In addition, by forming a complex pore structure, the transition metal eluted from the anode can be suppressed from moving to the cathode surface.

[0046] According to one embodiment of the present invention, it may include a first layer (110) having a weight including the first inorganic particles greater than a weight including the second inorganic particles; and a second layer (130) provided on one surface of the first layer and having a weight including the second inorganic particles greater than a weight including the first inorganic particles. Specifically, the first layer and the second layer may contain a mixture of the first inorganic particles and the second inorganic particles, but may be laminated separately as a first layer including a greater weight of the first inorganic particles and a second layer including a greater weight of the second inorganic particles. By laminating the first layer and the second layer separately as described above, the second layer can adsorb gases and transition metals, and the first layer can prevent transition metals adsorbed in the second layer from moving toward the negative electrode surface, thereby suppressing the occurrence of a battery short circuit.

[0047] According to one embodiment of the present invention, the opposite side of one side of the first layer may be provided to face the negative electrode (300). Fig. 2 is a schematic diagram of an electrochemical device according to one embodiment of the present invention. Referring to Fig. 2, the first layer including an excessive amount of first inorganic particles or including only the first inorganic particles may be formed by contacting the negative electrode. As described above, the second layer is provided on one side of the first layer, and the opposite side of one side of the first layer is provided to face the negative electrode, so that when a transition metal eluted from the positive electrode passes through without being adsorbed by the second layer, the first layer can prevent the occurrence of a battery short circuit by preventing the transition metal from flowing to the negative electrode surface.

[0048] According to one embodiment of the present invention, the first inorganic particle may include one selected from the group consisting of boron nitride, boehmite, kaolin, and combinations thereof. As described above, the first inorganic particle may be a plate-shaped inorganic particle. Specifically, boron nitride (BN) having a hexagonal crystal structure, boehmite (AlOOH) having a hexagonal crystal structure, and kaolin (Al2O 3· 2SiO 2· By including a plate-like clay powder such as 2H2O), the first layer containing a greater weight of the first inorganic particles can be arranged to face one side of the separator, thereby forming a dense laminated structure. Furthermore, by forming a complex pore structure between the plate-like inorganic particles through the dense laminated structure, the transition metal eluted from the anode can be suppressed from passing through the separator to the cathode surface.

[0049] According to one embodiment of the present invention, the second inorganic particle may be a zeolite-based inorganic particle. Specifically, the zeolite-based inorganic particle may include one selected from the group consisting of zeolite A, zeolite X, zeolite Y, zeolite L, ZSM-5, beta-zeolite, ZSM-8, ZSM-11, and combinations thereof. The zeolite-based inorganic particle may have a high specific surface area, and preferably, the zeolite-based inorganic particle may be zeolite Y. As described above, by using a zeolite-based inorganic particle as the second inorganic particle, the ability to adsorb gases and transition metals may be improved.

[0050] According to one embodiment of the present invention, the second inorganic particle may include a pore having a diameter of 0.5 nm to 0.9 nm. Specifically, the second inorganic particle may include a space inside the particle, and the internal space may have a diameter of 0.5 nm to 0.9 nm. Furthermore, the diameter of the pore may mean the longest of the lengths of two points where a straight line passing through the inside of the pore meets the surface of the pore. More specifically, the pore of the second inorganic particle may have a diameter of 0.55 nm to 0.85 nm, 0.6 nm to 0.8 nm, or 0.65 nm to 0.75 nm. By controlling the diameter of the pore within the above-described range, the ability to adsorb gases generated in a lithium ion battery, such as carbon monoxide (CO) or carbon dioxide (CO2), may be improved.

[0051] According to one embodiment of the present invention, the pores of the second inorganic particles may be substituted with metal ions. Specifically, the metal ions may be metal ions having the same or lower electronegativity as lithium ions. More specifically, the metal ions may be alkali metal ions. Preferably, the metal ions may be one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and combinations thereof. By substituting the metal ions selected from the above into the pores of the second inorganic particles, manganese ions included in excess as a cathode active material are adsorbed, and the substituted lithium ions are dissolved into the electrolyte, thereby maintaining the electrical conductivity of the battery, and reducing lithium tendrite generated when manganese, a transition metal that moves from the cathode to the anode, accumulates on the cathode.

[0052] According to one embodiment of the present invention, the average particle diameter (D50) of the second inorganic particles may be 0.3 ㎛ or more and 1 ㎛ or less. Specifically, the average particle diameter (D50) of the second inorganic particles may be 0.4 ㎛ or more and 0.9 ㎛ or less, 0.5 ㎛ or more and 0.8 ㎛ or less, or 0.6 ㎛ or more and 0.7 ㎛ or less. By controlling the average particle diameter (D50) of the second inorganic particles within the above-described range, the phase separation speed and phase separation efficiency between the polymer binder and the second inorganic particles in the slurry for a coating layer, which is an emulsion in which the polymer binder is dispersed in water, can be improved. Furthermore, when it is less than 0.3 ㎛, the dispersibility of the second inorganic particles in the slurry prepared for manufacturing a separation membrane may be reduced, and when it exceeds 1 ㎛, the thickness of the formed separation membrane may be increased.

[0053] In this specification, "D50 particle size" means the particle size at the 50% point of the cumulative distribution of particle numbers according to particle size. The particle size can be measured using a laser diffraction method. Specifically, after the powder to be measured is dispersed in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through the laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. By calculating the particle diameter at the point where the cumulative distribution of particle numbers according to particle size in the measuring device becomes 50%, the D50 particle size can be measured.

[0054] According to one embodiment of the present invention, the inorganic particles usable in the separator may be electrochemically stable. That is, the inorganic particles usable in one embodiment of the present invention may be stable within the operating voltage range of the applied electrochemical device (e.g., Li / Li). + It may be that no oxidation and / or reduction reaction occurs at a voltage of 0 V to 5 V as a reference.

[0055] According to one embodiment of the present invention, the second layer may have a thickness of 1 ㎛ or more and 3 ㎛ or less. Specifically, the thickness of the second layer may be 1.1 ㎛ or more and 2.9 ㎛ or less, 1.2 ㎛ or more and 2.8 ㎛ or less, 1.3 ㎛ or more and 2.7 ㎛ or less, 1.4 ㎛ or more and 2.6 ㎛ or less, 1.5 ㎛ or more and 2.5 ㎛ or less, 1.6 ㎛ or more and 2.4 ㎛ or less, 1.7 ㎛ or more and 2.3 ㎛ or less, 1.8 ㎛ or more and 2.2 ㎛ or less, or 1.9 ㎛ or more and 2.1 ㎛ or less. As described above, since the average particle diameter (D50) of the second inorganic particles constituting the second layer is 1 ㎛ or less, the thickness of the second layer can be controlled within the above-described range.

[0056] According to one embodiment of the present invention, the content of the first inorganic particles may be 5 parts by weight or more and 10 parts by weight or less with respect to 100 parts by weight of the separator. Specifically, the content of the first inorganic particles may be 6 parts by weight or more and 9 parts by weight or less or 7 parts by weight or more and 8 parts by weight or less with respect to 100 parts by weight of the separator. By adjusting the content of the first inorganic particles within the above-described range, the heat resistance of the separator can be improved, and the durability of the coating layer can be improved.

[0057] According to one embodiment of the present invention, the content of the second inorganic particles may be 5 parts by weight or more and 10 parts by weight or less with respect to 100 parts by weight of the separator. Specifically, the content of the second inorganic particles may be 6 parts by weight or more and 9 parts by weight or less or 7 parts by weight or more and 8 parts by weight or less with respect to 100 parts by weight of the separator. By controlling the content of the second inorganic particles within the above-described range, the heat resistance of the separator can be improved, and the adsorption rate of gases and transition metals can be improved.

[0058] According to one embodiment of the present invention, the content of the polymer binder may be 5 parts by weight or more and 10 parts by weight or less with respect to 100 parts by weight of the separator. Specifically, the content of the polymer binder may be 6 parts by weight or more and 9 parts by weight or less or 7 parts by weight or more and 8 parts by weight or less with respect to 100 parts by weight of the separator. By controlling the content of the polymer binder within the above-described range, the porosity of the separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained.

[0059] According to one embodiment of the present invention, the polymer binder may be in the form of particles or non-particulates. Specifically, as described below, the polymer binder may be one that does not dissolve in a dispersion medium or solvent and maintains a particle shape, or the polymer binder may be one that dissolves in a dispersion medium or solvent and does not maintain a particle shape. As described above, by selecting the polymer binder as being in the form of particles or non-particulates, the mechanical properties and porosity of the coating layer can be controlled.

[0060] According to one embodiment of the present invention, the average particle diameter (D50) of the particulate polymer binder is 1.0 ㎛ or less. Specifically, the average particle diameter (D50) of the particulate polymer binder particles may be 0.10 ㎛ or more and 0.90 ㎛ or less, 0.15 ㎛ or more and 0.85 ㎛ or less, 0.20 ㎛ or more and 0.70 ㎛ or less, 0.25 ㎛ or more and 0.65 ㎛ or less, 0.30 ㎛ or more and 0.60 ㎛ or less, 0.35 ㎛ or more and 0.55 ㎛ or less, or 0.40 ㎛ or more and 0.50 ㎛ or less. By controlling the average particle diameter (D50) of the particulate polymer binder within the above-described range, the phase separation speed and phase separation efficiency between the particulate polymer binder and the inorganic particles in an inorganic slurry, which is an emulsion in which the particulate polymer binder is dispersed in water, can be improved.

[0061] According to one embodiment of the present invention, the polymer binder may be an acrylic binder, a polyvinylidene binder, or a combination thereof.

[0062] According to one embodiment of the present invention, the polymer binder may include two or more types of polymer binders. As described above, by including two or more types of polymer binders, the adhesive strength of the separator can be improved, the porosity of the separator can be improved, and the dry adhesive strength before injecting the electrolyte and the wet adhesive strength after injecting the electrolyte can be improved at the same time.

[0063] According to one embodiment of the present invention, the polymer binder may include an acrylic binder. By using the acrylic binder, the porosity of the separator can be maintained, the adhesive strength between the electrode and the separator can be improved during the battery lamination process, thereby improving the ease of battery manufacturing, and the stacking process can be stably implemented.

[0064] According to one embodiment of the present invention, the acrylic binder is a polymer containing a carboxylic acid ester as a repeating unit, and may preferably be a (meth)acrylic acid ester or an acrylic-styrene copolymer.

[0065] According to one embodiment of the present invention, specific examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-amyl (meth)acrylate, i-amyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene glycol (meth)acrylate, di(meth)acrylate, propylene glycol (meth)acrylate, Examples thereof include trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate, and the like may be at least one selected from these. Among these, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate is preferable, and methyl (meth)acrylate is particularly preferable.

[0066] According to one embodiment of the present invention, the acrylic-styrene copolymer may include an acrylic binder, and the acrylic binder may be a polyacrylate. For example, the binder may be at least one selected from the group consisting of styrenebutadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, and acrylate polymers, and more specifically, may be a copolymer including acrylate.

[0067] According to one embodiment of the present invention, the polymer binder may include a polyvinylidene-based binder. Specifically, according to one embodiment of the present invention, the polyvinylidene-based binder may be a copolymer of polyvinylidene fluoride and hexafluoropropylene. As described above, by selecting the polymer binder as a polyvinylidene-based binder, the porosity of the separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained. Furthermore, the stiffness of the battery can be improved, and bending of the separator can be prevented.

[0068] According to one embodiment of the present invention, the polyvinylidene-based binder may be an aqueous binder. Specifically, by selecting the polyvinylidene-based binder as an aqueous binder, pollutants emitted during the manufacturing process of the separator can be minimized, thereby reducing the manufacturing cost of the battery.

[0069] According to one embodiment of the present invention, the polyvinylidene-based binder may be a polyvinylidene-based binder having a hexafluoropropylene content of 1 wt% or more and 50 wt% or less. As described above, by selecting the second polymer binder particle as a polyvinylidene-based binder having a hexafluoropropylene content of 1 wt% or more and 50 wt% or less, the porosity of the separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained.

[0070] According to one embodiment of the present invention, the thickness of the separator may be 7 ㎛ or more and 15 ㎛ or less, but is not particularly limited thereto. Specifically, the thickness of the separator may be 8 ㎛ or more and 14 ㎛ or less, 9 ㎛ or more and 13 ㎛ or less, or 10 ㎛ or more and 12 ㎛ or less. The thickness can be adjusted to an appropriate range by a person skilled in the art in terms of heat resistance or electrical resistance. As described above, the plate-shaped first inorganic particles constituting the separator are arranged to face one surface of the separator to form a dense laminated structure, and since the average particle diameter (D50) of the second inorganic particles is 1 ㎛ or less, the thickness of the separator can be adjusted to an appropriate range within the above-described range.

[0071] According to one embodiment of the present invention, the thickness of the second layer and / or the separator, etc., can be measured using a contact thickness measuring device. The contact thickness measuring device can be, for example, VL-50S-B from Mitutoyo.

[0072] According to one embodiment of the present invention, the air permeability of the separation membrane may be 170 sec / 100cc or less. Specifically, the air permeability of the separation membrane may be 100 sec / 100cc or more and 170 sec / 100cc or less, 110 sec / 100cc or more and 160 sec / 100cc or less, 120 sec / 100cc or more and 150 sec / 100cc or less, or 130 sec / 100cc or more and 140 sec / 100cc or less. As described above, since the inorganic particles are plate-shaped or have a small average particle diameter (D50), the air permeability may be excellent.

[0073] According to one embodiment of the present invention, the resistance of the separator may be 0.6 Ω or more and 1.2 Ω or less. Specifically, the resistance of the separator may be 0.7 Ω or more and 1.1 Ω or less or 0.8 Ω or more and 1.0 Ω or less. As described above, it is believed that the resistance value of the separator is low because the inorganic particles are plate-shaped or have a small average particle diameter (D50).

[0074] According to one embodiment of the present invention, the breakdown voltage of the separator may be 3700 V or more. Specifically, the breakdown voltage of the separator may be 3700 V or more and 5000 V or less, 3800 V or more and 4900 V or less, 3900 V or more and 4800 V or less, 4000 V or more and 4700 V or less, 4100 V or more and 4600 V or less, 4200 V or more and 4500 V or less, or 4300 V or more and 4400 V or less. As described above, since the inorganic particles are plate-shaped or have a small average particle diameter (D50), the breakdown voltage of the separator is high, and it can be seen that the withstand voltage characteristics are excellent.

[0075] According to one embodiment of the present invention, the porosity of the separator may be 30% by volume or more. Specifically, the porosity of the separator may be 30% by volume or more and 70% by volume or less, 32% by volume or more and 68% by volume or less, 34% by volume or more and 66% by volume or less, 36% by volume or more and 64% by volume or less, 38% by volume or more and 62% by volume or less, 40% by volume or more and 60% by volume or less, 42% by volume or more and 58% by volume or less, 44% by volume or more and 56% by volume or less, 46% by volume or more and 54% by volume or 48% by volume or more and 52% by volume. By controlling the porosity of the separator within the above-described range, it is possible to maintain the movement of ions in the separator and prevent an increase in resistance of the separator. Specifically, if the porosity is 70% by volume or less, mechanical properties that can withstand the pressing process for bonding with the electrode can be secured, and the surface opening ratio is not too high, making it suitable for securing adhesive strength. On the other hand, if the porosity is 30% by volume or more, it is advantageous from the perspective of ion permeability.

[0076] In this specification, “porosity” means the ratio of the volume occupied by pores to the total volume, and uses volume % as its unit, and can be used interchangeably with terms such as void ratio and porosity.

[0077] In this specification, porosity corresponds to a value obtained by subtracting the volume converted to the weight and density of each component of the membrane from the volume calculated by the thickness, width, and length of the membrane.

[0078] In one embodiment of the present invention, the porosity and pore size of the membrane can be measured by the BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) through a nitrogen gas adsorption flow method. In this case, it may be advantageous to use a capillary flow porometer.

[0079] According to one embodiment of the present invention, the method for forming the separation membrane is as follows, for example. First, a polymer solution or polymer emulsion is prepared by dissolving a polymer binder in an appropriate solvent or dispersing it in a dispersion medium. The solvent or dispersion medium preferably has a solubility index similar to that of the polymer binder to be used and a low boiling point. This is to facilitate uniform mixing and subsequent removal of the solvent or dispersion medium. Non-limiting examples of solvents or dispersion mediums that can be used include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or mixtures thereof.

[0080] Next, first inorganic particles are added and dispersed in the first polymer solution or first polymer emulsion thus manufactured to manufacture a first inorganic slurry. According to one embodiment of the present invention, the content ratio of the first inorganic particles and the polymer binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the final manufactured separation membrane of the present invention.

[0081] Next, the first inorganic slurry prepared above is applied to at least one side of the prepared PET release film and dried. The method for applying the first inorganic slurry to the surface of the PET release film is not particularly limited to any one method, and any conventional method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a mixture thereof can be used.

[0082] Next, second inorganic particles are added and dispersed in the second polymer solution or second polymer emulsion manufactured in the same manner to manufacture a second inorganic slurry. According to one embodiment of the present invention, the content ratio of the second inorganic particles and the polymer binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the final separation membrane of the present invention.

[0083] Next, the second inorganic slurry prepared above is applied onto the first layer including the first inorganic particles applied above and dried. The method for applying the second inorganic slurry onto the surface of the first layer is not particularly limited to any one method, and any conventional method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a mixture thereof can be used.

[0084] The above drying process is performed under appropriate temperature and time conditions to minimize the occurrence of surface defects in the membrane. The drying may be performed using a drying oven or a drying auxiliary device, such as hot air, within an appropriate range.

[0085] After the above drying process, the PET release film can be removed to manufacture the separator.

[0086] According to one embodiment of the present invention, a polymer emulsion may be prepared by dispersing a polymer binder, i.e., a first polymer binder and a second polymer binder, in a suitable dispersion medium, water, together with a wetting agent, to thereby prepare a first and / or second inorganic slurry. The wetting agent may be present in the first and / or second inorganic slurry as one or more wetting agents, at 0 to 5 parts, preferably 0 to 3 parts, per 100 parts of water. A surfactant may be provided as the wetting agent, but the wetting agent may also include a non-surfactant. In some embodiments, the wetting agent may be an organic solvent. The presence of any wetting agent allows the powder material(s) to be uniformly dispersed in the aqueous dispersion of the polyvinylidene-based binder. Useful wetting agents include, but are not limited to, ionic and nonionic surfactants such as the TRITON series (Dow) and the PLURONIC series (BASF), BYK-346 (BYK Additives), and organic liquids compatible with aqueous dispersions, such as NMP, DMSO, and acetone. As described above, by dispersing the polymer binder together with the wetting agent in a suitable dispersion medium, water, to prepare a polymer emulsion to provide the first and / or second inorganic slurry, contaminants generated during the manufacturing process can be minimized.

[0087] According to one embodiment of the present invention, the separator (100) is interposed between the negative electrode (300) and the positive electrode (500) and is manufactured into an electrochemical device through a lamination process in which heat and / or pressure are applied to bond the separator. In one embodiment of the present invention, the lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode are sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot press method.

[0088] One embodiment of the present invention provides an electrochemical device including an anode (300); a cathode (500); and a separator (100) interposed between the anode and the cathode.

[0089] An electrochemical device according to one embodiment of the present invention comprises first inorganic particles capable of preventing transition metals eluted from an anode from moving toward a cathode by forming a dense, plate-like laminated structure, and second inorganic particles capable of gas adsorption and transition metal adsorption with a high specific surface area, and a separator without a porous polymer substrate, thereby improving heat resistance and durability, and enhancing battery stability and battery life characteristics.

[0090] In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction, and is a concept encompassing a primary battery and a secondary battery. In the present specification, the secondary battery is capable of charging and discharging, and refers to a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery uses lithium ions as an ion conductor, and examples thereof include, but are not limited to, a non-aqueous electrolyte secondary battery including a liquid electrolyte, an all-solid-state battery including a solid electrolyte, a lithium polymer battery including a gel polymer electrolyte, and a lithium metal battery using lithium metal as an anode.

[0091] According to one embodiment of the present invention, the positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-xLithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x A lithium manganese composite oxide represented by MxO2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.

[0092] According to one embodiment of the present invention, the negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.

[0093] According to one embodiment of the present invention, the conductive material may be, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials among these. More specifically, the conductive material may be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.

[0094] According to one embodiment of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used.

[0095] According to one embodiment of the present invention, the binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0096] According to one embodiment of the present invention, the positive electrode slurry for manufacturing the positive electrode active material layer may include a dispersant, and the dispersant may be a pyrrolidone-based compound. Specifically, it may be N-methylpyrrolidone (ADC-01, LG Chemical).

[0097] According to one embodiment of the present invention, the content of the dispersant included in the positive electrode slurry may be more than 0 part by weight and less than or equal to 0.5 part by weight with respect to 100 parts by weight of the positive electrode slurry. Specifically, the content of the dispersant included in the positive electrode slurry may be more than 0.05 part by weight and less than or equal to 0.4 part by weight with respect to 100 parts by weight of the positive electrode slurry.

[0098] According to one embodiment of the present invention, the negative electrode slurry for producing the negative electrode active material layer may include a dispersant, and the dispersant may be a polypyrrolidone-based compound. Specifically, the dispersant may be polyvinylpyrrolidone (Polyvinylpyrrolidone, Junsei, Japan).

[0099] According to one embodiment of the present invention, the content of the dispersant included in the cathode slurry may be more than 0 part by weight and less than or equal to 0.5 part by weight with respect to 100 parts by weight of the cathode slurry. Specifically, the content of the dispersant included in the cathode slurry may be more than 0.05 part by weight and less than or equal to 0.4 part by weight with respect to 100 parts by weight of the cathode slurry.

[0100] According to one embodiment of the present invention, an electrochemical device prepared as described above can be placed in an appropriate case and an electrolyte solution is injected to manufacture a battery.

[0101] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure as A + is Li + , Na + , K +B containing ions composed of alkali metal cations or combinations thereof; - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2) 2- , C(CF2SO2) 3- Salts containing anions such as or combinations thereof are dissolved or dissociated in organic solvents such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or mixtures thereof, but are not limited thereto.

[0102] One embodiment of the present invention provides a battery module including a battery including the electrochemical element as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.

[0103] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.

[0104]

[0105] <Example 1>

[0106] Hexagonal boron nitride (hBN) synthesized as a plate-shaped first inorganic particle with an aspect ratio of 50 and polyacrylic acid (PAA) as a dispersant were added to NMP (N-Methyl-2-pyrrolidone) as a solvent and dispersed using a sonicator for about 30 minutes to prepare an oil-based slurry.

[0107] A first polymer binder solution containing an acrylic water-dispersed emulsion (Toyo ink, CSB130) and a surfactant (FC-4430, Kemis) as a polymer binder was added to the oil-based slurry and dispersed using a sonicator for about 30 minutes to prepare a first inorganic slurry.

[0108] Thereafter, the first inorganic slurry was applied to one side of a PET release film and dried. The weight ratio of the first inorganic particles and the polymer binder was 9:1.

[0109] Zeolite Y (SAR, Silicon Aluminum ratio 1.5 or higher) as a second inorganic particle was added to water and dispersed, and basket milling was performed at 1400 rpm and 1800 rpm for 10 minutes and 50 minutes, respectively, to prepare an aqueous slurry with a reduced particle size (D50: 1 μm or less).

[0110] A second polymer binder solution containing an acrylic water-dispersed emulsion (Toyo ink, CSB140) and a surfactant (BYK, BYK348) as a polymer binder was added to the aqueous slurry 1 hour before coating, and a second inorganic slurry was prepared after sonication for 30 minutes.

[0111] Thereafter, the second inorganic slurry was applied to the surface of the first layer including the first inorganic particles and dried. The weight ratio of the second inorganic particles and the polymer binder was 92:8.

[0112] The dispersion was applied to the surface of the second layer containing the second inorganic particles by bar coating using a doctor blade and dried with air at 50°C using a heat gun.

[0113] Afterwards, the PET release film was removed to manufacture a separator with a total thickness of 13 ㎛.

[0114]

[0115] <Example 2>

[0116] A separation membrane was manufactured in the same manner as in Example 1, except that the aspect ratio of the first inorganic particle in the plate shape was 200.

[0117]

[0118] <Comparative Example 1>

[0119] A separation membrane having a thickness of 14 μm was manufactured in the same manner as in Example 1, except that the first layer including the plate-shaped first inorganic particles was omitted and the second inorganic particle, zeolite Y, was added to manufacture the membrane as a single layer.

[0120]

[0121] <Comparative Example 2>

[0122] A separation membrane having a thickness of 11 μm was manufactured in the same manner as in Example 1, except that the first inorganic particle, hexagonal boron nitride (hBN), which is a plate-shaped first inorganic particle, was added without a second layer including the second inorganic particle in Example 1, and manufactured as a single layer.

[0123]

[0124] <Comparative Example 3>

[0125] A 14 μm thick separation membrane was manufactured in the same manner as in Example 1, except that the aspect ratio of the first inorganic particle in the plate shape was less than 10.

[0126]

[0127] <Comparative Example 4>

[0128] A 12 μm thick separation membrane was manufactured in the same manner as in Example 1, except that the aspect ratio of the first inorganic particle in the plate shape was greater than 300.

[0129]

[0130] <Manufacturing of electrochemical devices>

[0131] 1) Manufacturing of the anode

[0132] Cathode active material (LiNi) 0.8 Mn 0.1 Co 0.1 O2), a conductive agent (carbon black), a dispersant (N-methylpyrrolidone, ADC-01, LG Chemical), and a binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a cathode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to manufacture a cathode having a cathode active material layer (thickness 120 μm).

[0133] 2) Manufacturing of cathode

[0134] Graphite (natural graphite and artificial graphite blend), conductive agent (carbon black), dispersant (polyvinylpyrrolidone, Junsei, Japan), and binder resin (PVDF-HFP and PVDF blend) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for an anode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (thickness 10 μm) and dried to manufacture an anode having an anode active material layer (thickness 120 μm).

[0135] 3) Lamination process

[0136] The separators of the examples and comparative examples were interposed between the manufactured cathodes and anodes, and a lamination process was performed to obtain an electrode assembly. The lamination process was performed using a hot press at 70°C and 5.2 MPa for 10 seconds.

[0137]

[0138] <Experimental Example 1: Membrane Permeability>

[0139] The air permeability (air permeability time, Gurley) of the membranes of the examples and comparative examples was measured by the ASTM D-2873 method. The Gurley value was measured using a Gurley type densometer (No. 158) from Toyoseiki according to the Gurley (JIS) measurement method of the Japanese Industrial Standard. The air permeability value was measured when 100 ml of air was blown through 1 in of the membrane under a pressure of 12.2 in H2O. 2 The time (in seconds) it takes to pass through the cross section is expressed as the ventilation time.

[0140]

[0141] <Experimental Example 2: Membrane Resistance>

[0142] Coin cells were manufactured by sandwiching the separators of the examples and comparative examples between SUS. The electrolyte of the coin cells was a mixture of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 1:2, and LiPF6 was added at a concentration of 1 M. For each coin cell, the resistance was measured through electrochemical impedance spectroscopy analysis results using an analysis device (VMP3, Bio logic science instrument) at 25°C with an amplitude of 10 mV and a scan range of 0.1 Hz to 1 MHz.

[0143]

[0144] <Experimental Example 3: Breakdown Voltage of the Separator>

[0145] The membrane samples of the examples and comparative examples prepared between aluminum jigs (upper jig diameter 30 mm, lower jig diameter 50 x 100 mm) were placed and the voltage at which a short circuit occurs was measured using a Hi-pot tester. At this time, the measurement conditions were set to DC, current 0.5 mA, and voltage increase 100 V / s (up to 3 kV).

[0146]

[0147] <Experimental Example 4: Performance Maintenance Rate of Electrochemical Devices>

[0148] In order to evaluate the lifespan of electrochemical devices manufactured including the separators of the examples and comparative examples, each electrochemical device was charged to 4.35 V at 0.33 C and discharged to 2.0 V at 0.33 C for 500 cycles, and the initial capacity and residual capacity were measured.

[0149]

[0150] <Experimental Example 5: Gas Generation from an Electrochemical Device>

[0151] In order to measure the amount of gas generated from the electrochemical devices manufactured including the separators of the examples and comparative examples, each electrochemical device was charged and discharged once at 25°C under 0.1C / 0.1C conditions to proceed with formation, and the amount of gas generated was measured. In order to measure the amount of gas generated from a degraded cell, a cell evaluated for up to 500 cycles as in Experimental Example 4 was completely discharged to 2.0 V at 0.33C, and then the amount of gas was measured.

[0152]

[0153] <Experimental Example 6: Transition Metal Elution Amount from an Electrochemical Device>

[0154] In order to measure the amount of cathode transition metal eluted from electrochemical devices manufactured including the separators of Examples and Comparative Examples, a charge-discharge test was performed 500 times, in which the cells were formed at SOC 30%, discharged under the conditions of a discharge current density of 0.33 C and a discharge voltage of 2.0 V, and then charged under the conditions of a charge current density of 0.33 C and a charge voltage of 4.35 V and CC-CV (Constant Current-Constant Voltage). After 500 cycles of testing, the amount of transition metal eluted from the cathode surface was measured.

[0155]

[0156] Membrane properties Electrochemical device evaluation Thickness (μm) Air permeability (sec / 100cc) Resistance (Ω) Breakdown voltage (V) Performance retention (% / 0.33C 500 cycle) Gas generation (μl) Cathode-faced ICP Analysis (ppm / 500 cycles) NiCoMn Comparative Example 1 141200.936508512070<5510 Comparative Example 2 111401.4167073550170<5860 Comparative Example 3 141251.0343080230100<5680 Comparative Example 4 121401.721507421035<5290 Example 1 131301.043608322053<5460 Example 2 131331.141208921542<5340

[0157]

[0158] Referring to Table 1 above, in Examples 1 and 2 according to an embodiment of the present invention, the number of cases in which by-products that were not adsorbed by the functional inorganic particles of the second layer did not reach the cathode surface as they passed through the plate-shaped inorganic layer, which is the first layer, increased, and it was confirmed that the amount of transition metal elution was significantly reduced at the cathode surface of the electrochemical device deteriorated by 500 cycles of discharge. With the same effect, the performance maintenance rate of the electrochemical device was improved and the amount of gas generated was also confirmed to be reduced.

[0159]

[0160] In this regard, Comparative Example 1 is a self-supporting ceramic separator composed only of second inorganic particles capable of adsorbing by-products generated during the degradation of electrochemical devices. It shows that the amount of transition metal elution from the cathode surface of the degraded electrochemical device is reduced compared to a general separator after 500 cycles of discharge. Comparative Example 2 is a separator composed only of plate-shaped inorganic particles as the first inorganic particles. It is expected that denser inorganic assembly will make the path of transition metal ions complicated and the by-products accumulating on the cathode surface will be reduced, but it is inferior to Comparative Example 1. In cases where the aspect ratio value of the plate-shaped inorganic particles is too low (AR<10), as in Comparative Example 3, the expected effect by using plate-shaped inorganic particles is insufficient, showing inferior properties in the amount of transition metal elution from the cathode surface, the performance maintenance rate of the electrochemical device, and the amount of gas generated. As in Comparative Example 4, when the aspect ratio value of the plate-shaped inorganic particles is too large (AR>300), the plate-shaped inorganic particles have a strong property of interfering with the durability of the separator, so the insulation breakdown voltage is significantly lowered and the performance maintenance rate of the electrochemical device is also confirmed to be low.

[0161]

[0162] A self-supporting ceramic separator for an electrochemical device according to one embodiment of the present invention includes a functional inorganic material and a plate-shaped inorganic material, thereby preventing gas adsorption and accumulation of byproducts on the cathode surface during deterioration of the electrochemical device, thereby enabling improvement in the performance of the electrochemical device.

[0163]

[0164] <Explanation of symbols>

[0165] 100: Self-supporting ceramic separator for electrochemical devices

[0166] 110: 1st floor

[0167] 130: 2nd floor

[0168] 300: Cathode

[0169] 500: Bipolar

Claims

1. Containing first inorganic particles, second inorganic particles and a polymer binder, The above first inorganic particle is plate-shaped, A self-supporting ceramic separator for an electrochemical device, wherein the aspect ratio of the first inorganic particle is 10 or more and 300 or less.

2. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein one side of the first inorganic particle and one side of the separator are arranged to face each other.

3. In claim 1, A first layer having a weight containing the first inorganic particles greater than a weight containing the second inorganic particles; and A self-supporting ceramic separator for an electrochemical device, comprising a second layer provided on one side of the first layer, the second layer including the second inorganic particles having a weight greater than the weight including the first inorganic particles.

4. In claim 3, A self-supporting ceramic separator for an electrochemical device, wherein the opposite side of one side of the first layer is provided to face the cathode.

5. In claim 1, The above first inorganic particle, A self-supporting ceramic separator for an electrochemical device, comprising one selected from the group consisting of boron nitride, boehmite, kaolin, and combinations thereof.

6. In claim 1, The above second inorganic particle is a zeolite-based inorganic material, The second inorganic particle includes pores having a diameter of 0.5 nm or more and 0.9 nm or less, A self-supporting ceramic separator for an electrochemical device, wherein the pores of the second inorganic particles are replaced with metal ions.

7. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein the average particle diameter (D50) of the second inorganic particles is 1 ㎛ or less.

8. In claim 3, A self-supporting ceramic separator for an electrochemical device, wherein the thickness of the second layer is 1 ㎛ or more and 3 ㎛ or less.

9. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein the content of the first inorganic particles is 5 parts by weight or more and 10 parts by weight or less with respect to 100 parts by weight of the separator.

10. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein the polymer binder is an acrylic binder, a polyvinylidene binder, or a combination thereof.

11. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein the thickness of the separator is 7 ㎛ or more and 15 ㎛ or less.

12. In claim 1, A self-standing ceramic separator for an electrochemical device, wherein the air permeability of the above separator is 170 sec / 100cc or less.

13. In claim 1, A self-supporting ceramic separator for an electrochemical device, wherein the resistance of the separator is 0.6 Ω or more and 1.2 Ω or less.

14. An electrochemical device comprising: a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode, the separator of claim 1.

Citation Information

Patent Citations

  • A self-supporting ceramic seperator for an electrochemical device and an electrochemical device comprising the same

    KR1020240154961A

  • Sensing data processing method and sensor hub using the same

    KR1020210123893A

  • Driving roller for conveyor

    KR1020220114393A

  • Magnetic nail clippers

    KR1020230016840A

  • Opening and closing system for valve

    KR1020230024769A